Resin composition, transparent material, transparent film, plate material for screen printing, stencil for screen printing, and photosensitive resist film
The aqueous emulsion-type photosensitive resin compositions with specific epoxy compounds and viscosity ranges address the limitations of conventional screen printing materials by enhancing film transparency and resolution, enabling high-definition images with improved chemical resistance.
Patent Information
- Application Number
- PCT/JP2024/013005
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional screen printing sensitive materials face limitations in increasing film thickness and improving resolution due to light scattering, which reduces the transparency and effectiveness of photosensitive films, especially in the ultraviolet region.
Aqueous emulsion-type photosensitive resin compositions are developed, incorporating a water-soluble polymer and an epoxy compound with specific viscosity ranges, along with a photoacid generator and sensitizer, to enhance the transparency and resolution of photosensitive films by optimizing the monomer viscosity and compatibility, resulting in high transmittance and reduced haze values.
The resin composition achieves high transparency and improved resolution in thick photosensitive films, allowing for high-definition relief images without the need for oxygen barrier films and with excellent chemical and solvent resistance.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Resin composition, transparent material, transparent film, screen printing plate material, screen printing stencil, and photosensitive resist film REFERENCE TO RELATED APPLICATIONS
[0001] This patent application claims priority based on Japanese Patent Application No. 2023-058908 filed on March 31, 2023, the entire disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a resin composition. More specifically, the present invention relates to an aqueous emulsion resin composition and a photosensitive resin composition comprising a water-soluble polymer and an epoxy compound, and a photosensitive film obtained therefrom. These compositions can be suitably used as screen printing plates and etching resist films.
[0003] Photosensitive polymers for pattern formation, such as those used as photoresists, are available in negative and positive types. A film-forming solution containing either type is uniformly applied to a substrate and dried, and the resulting film is then subjected to pattern exposure. For both negative and positive types, organic solvents are used for film formation, and alkaline aqueous solutions are generally used as developers. On the other hand, for aqueous emulsion-type photosensitive photopolymers used in screen printing plates, neutral water is used as the film-forming and developing solvent. Neutral water is also used as the film-forming and developing solvent for some resin relief printing plates. These water-developable photopolymers are classified as negative types.
[0004] Aqueous emulsion-type photosensitive resin compositions containing water-developable photopolymers, protective colloids, and photocrosslinkable polymers are widely used as screen printing sensitive materials. Originating from the blending of a polymer emulsion with a dichromate or diazo resin, examples of such compositions include emulsion-type photosensitive materials using polyvinyl alcohol bonded with a photodimerization-type photosensitive residue as a photocrosslinking agent, compositions in which a (meth)acrylic compound and a photoradical polymerization initiator are emulsified in an aqueous polyvinyl alcohol solution and then blended with a dichromate or diazo resin as a photocrosslinking agent, and aqueous emulsion-type compositions in which a photodimerization-type crosslinking group is introduced into polyvinyl alcohol.
[0005] In aqueous emulsion-type photosensitive materials using a water-soluble polymer such as polyvinyl alcohol as a protective colloid, the dispersed phase is a (meth)acrylic monomer. Generally, in radical polymerization of (meth)acrylic compounds, chain transfer to polyvinyl alcohol does not substantially occur. Therefore, the incorporation of a photocrosslinker for polyvinyl alcohol is essential for the above-mentioned radical emulsion photosensitive materials. In contrast, cationic polymerizable monomers undergo chain transfer to polyvinyl alcohol, making photoinsolubilization possible without a photocrosslinker. Patent Document 1 proposes a dry film resist made of an emulsion photosensitive material consisting of polyvinyl alcohol, a polymethylol compound, and a photoacid generator. However, this requires heating to 150°C after pattern exposure.
[0006] Patent Documents 2 and 3 propose photosensitive compositions in which an epoxy compound and a photoacid generator are emulsified using a water-soluble protective colloid. Patent Document 4 also proposes a composition in which a photocrosslinkable polyvinyl alcohol is used as a protective colloid. Patent Document 5 proposes a composition in which a photoacid generator and a sensitizer are dissolved or dispersed in an emulsion of an epoxy and an oxetane compound. Meanwhile, Patent Document 6 proposes a hybrid emulsion photosensitive material composed of a radically polymerizable monomer and a cationically polymerizable monomer. The above emulsion-type photosensitive compositions are primarily intended for use as screen printing photosensitive materials, and therefore, transparency of the films obtained from these compositions is not an essential requirement.
[0007] However, in photopatterning of screen printing sensitive films, even if the resolution on the incident surface is good, the effect of scattering of excitation light becomes significant as the film thickness increases, resulting in a significant deterioration of the resolution on the exit side. As a result, conventional screen printing sensitive films have limitations not only on the thickness of stencils but also on the improvement of resolution. To overcome these problems, it is necessary to significantly improve the transmittance of excitation light through films prepared from emulsion-type photosensitive compositions.
[0008] Regarding transparent photosensitive films, Patent Document 7 proposes a transparent photosensitive film using a composition in which a photoacid generator and an epoxy monomer or an acid-catalyzed condensation monomer are dissolved or dispersed in an aqueous solution of partially saponified polyvinyl alcohol. Note that transparency here is defined by the haze value, which corresponds to the transmittance in the visible wavelength region.
[0009] Patent Document 7 proposes transparent photosensitive films using not only epoxy monomers alone, but also mixtures of epoxy monomers and oxetane monomers, and compositions in which these cationic ring-opening polymerizable monomers are blended with acid-catalyzed condensation monomers such as N-methylolated or N-alkoxymethylated nitrogen-containing compounds, hydroxymethylated phenol derivatives, or resol resins. Thus, the monomers constituting the compositions in this patent cover a very wide range.
[0010] The transparency of a material refers to the absence of absorption or scattering of visible light passing through the material, and is quantified by its visible light transmittance. When the material does not absorb or scatter visible light, it is colorless and transparent; when it absorbs visible light but does not scatter it, it is colored and transparent. Patent Document 7 lists a wide variety of sensitizers that absorb visible light, along with photoacid generators, as essential components for producing a transparent photosensitive film. Therefore, the films covered by Patent Document 7 are both colorless and transparent, as well as colored and transparent. Meanwhile, the examples of photosensitive films for which haze values, an indicator of colorless transparency, are given are limited to three types composed of cationically polymerizable monomers.
[0011] Patent Document 7 posits that the transparency of films obtained from the three emulsion-type photosensitive compositions containing the above-mentioned cationic photopolymerizable monomers is due to the relatively small difference in refractive index between polyvinyl alcohol and the cationic photopolymerizable monomers, as well as their partial compatibility. Furthermore, it speculates that the improved transparency is due to the smaller particle size of the cationic polymerizable monomer dispersed in water compared to the radical polymerizable monomer. However, no experimental data supporting this assertion is presented. Furthermore, the photosensitive compositions described in Patent Document 7 include a wide variety of monomers, photoacid generators, and sensitizers, making it difficult to find evidence that all cationic polymerizable monomers and acid-catalyzed condensation monomers with diverse refractive indices produce transparent films. Therefore, in order to explore the physical properties of the monomers that affect film transparency, we systematically investigated the factors that contribute to the transparency of photosensitive resin compositions prepared from cationic polymerizable monomers.
[0012] The refractive index of photo- or thermally polymerizable cationically polymerizable monomers varies significantly depending on, for example, the presence or absence of aromatic rings or halogen atoms. Therefore, it is clearly beyond the scope of the present invention to expect that the refractive index of partially saponified polyvinyl alcohol, which has a constant refractive index, will match that of all the monomers exemplified in Patent Document 1. Next, we hypothesized that the transparency of the film is due to at least partial compatibility between partially saponified polyvinyl alcohol and epoxy compounds, and focused on the I / O value in the organic conceptual diagram as a parameter reflecting the degree of compatibility. In other words, we hypothesized that an epoxy monomer with an I / O value similar to that of partially saponified polyvinyl alcohol would yield a transparent emulsion-type composition. We investigated the transparency of polyvinyl alcohol emulsion films using epoxy monomers with various I / O values, but were unable to find any correlation between the haze value, an indicator of transparency, and the I / O value of the monomer.
[0013] Through these investigations, we discovered that films prepared from emulsions containing epoxy monomers and aqueous polyvinyl alcohol solutions maintain high transparency when the monomer viscosity is within a specific range. Therefore, we selected transmittance at 405 nm as an indicator of emulsion film transparency, taking into account the predominant wavelength of light sources commonly used in screen printing sensitive materials, and systematically investigated the correlation between monomer viscosity and film transmittance. As a result, we found that emulsion films prepared from monomers with viscosities ranging from approximately 300 mPa·s to 12,000 mPa·s maintain high transmittance. The present invention is based on this newly discovered finding.
[0014] Japanese Patent Laid-Open No. 57-84451 Japanese Patent Laid-Open No. 59-184220 Japanese Patent Laid-Open No. 10-62990 Japanese Patent Laid-Open No. 2004-37955 Japanese Patent Laid-Open No. 2004-325810 Japanese Patent Laid-Open No. 2005-208070 Japanese Patent Laid-Open No. 2005-351979
[0015] Photosensitive compositions containing a photocrosslinker in an aqueous emulsion of a photopolymerizable acrylic monomer prepared using partially saponified polyvinyl alcohol are widely used as photosensitive materials for screen printing. On the other hand, as mentioned above, photosensitive films prepared from aqueous emulsion compositions of epoxy monomers containing a photoacid generator facilitate pattern formation through cationic polymerization of the epoxy monomer and crosslinking via chain transfer to polyvinyl alcohol, and are used as photosensitive compositions for screen printing. Generally, the thickness of photosensitive films for screen printing is large, significantly degrading the resolution on the backside of the stencil. Therefore, to minimize light scattering in these thick emulsion-type photosensitive films, it is essential to improve the transmittance of actinic light in the ultraviolet region, which excites the photoacid generator or sensitizer, within the film. The present invention focuses on improving the transmittance of actinic light in the ultraviolet region and relates to improving the transparency of photosensitive films obtained from cationically polymerizable monomers. Therefore, we prepared aqueous emulsion films of a wide variety of cationically polymerizable monomers and measured their transmittance at 405 nm. Based on these results, we succeeded in improving the transparency of emulsion-type photosensitive films. Based on these results, we aim to provide these as screen printing plates, screen printing stencils, and further photosensitive films and film resists.
[0016] Generally, photosensitive films for screen printing, which are prepared from a heterogeneous system called an emulsion, are thick and lack transparency. Therefore, the resolution at the exit surface of the patterning light irradiated thereon is significantly deteriorated due to light scattering. Therefore, a significant suppression of light scattering is required, especially for thick photosensitive films.
[0017] What needs to be confirmed here is the definition of film transparency. Transparency is a visual characteristic, and as a physical property it is quantified by the haze value. In short, transparency is recognized by the amount of diffused transmitted light in the visible light range. On the other hand, in photosensitive films, the ultraviolet transmittance of the photosensitive compound that induces patterning in the photosensitive film is essentially important. This is because improving transmittance in the ultraviolet range inevitably increases the transparency of the film.
[0018] Therefore, as described above, we selected 405 nm as the wavelength for transmittance measurement and conducted extensive research into the relationship between transmittance at this wavelength and the properties of emulsion films prepared from cationically polymerizable monomers. Commonly used epoxy monomers and oxetane monomers themselves are transparent at 405 nm. Therefore, the decrease in transmittance of emulsion films prepared from them is due to light scattering, and the transmittance of emulsion films at 405 nm serves as an indicator of transparency. After extensive measurements of many emulsion films, we confirmed that the viscosity of the cationically polymerizable monomers used in these films plays an important role in determining UV transmittance, and that dissolving a photoacid generator and a sensitizer in the concentration range that imparts photosensitivity has little effect on the monomer viscosity, leading to the completion of the present invention.
[0019] That is, according to the present invention, there are provided the following resin composition, a photosensitive resin composition developable with neutral water, and a screen printing plate, a screen printing stencil, a photosensitive transparent film, and a dry film resist each using the photosensitive resin composition.
[0020] [1] A resin composition comprising an aqueous solution of the following component (A) and the following component (B) emulsified and dispersed in the aqueous solution: Component (A): at least one water-soluble polymer selected from the group consisting of polyvinyl alcohol polymers, ethylene-vinyl alcohol copolymers, hydroxyethyl cellulose, and hydroxypropyl cellulose; Component (B): a cationically polymerizable monomer comprising, as an essential component, an epoxy compound having at least one epoxy group (component (b1)), and having a viscosity of 300 mPa·s or more and 12,000 mPa·s or less. [2] The resin composition according to [1], further comprising a photoacid generator (component (C)). [3] The resin composition according to [2], further comprising a sensitizer (component (D)). [4] The resin composition according to any one of [1] to [3], wherein the component (A) is polyvinyl alcohol having a saponification rate of 60% or more and a sodium acetate content of 5% by weight or less.
[0021] [5] The resin composition according to any one of [1] to [4], wherein the component (B) comprises the epoxy compound (component (b1)) and a compound having an oxetane group (component (b2)). [6] The resin composition according to any one of [1] to [5], wherein the resin composition comprises a dispersion medium comprising an aqueous solution of the component (A) and a dispersoid comprising the component (B) emulsified and dispersed in the dispersion medium, and the dispersoid has a particle size (median size (D50)) measured by a laser diffraction / scattering method of 0.1 μm to 3.0 μm. [7] A transparent material comprising a dried product of the resin composition according to any one of [1] to [6]. [8] The transparent material according to [7], wherein the transmittance of light at a wavelength of 405 nm in the form of a 30 μm-thick film is 60% or more and 100% or less. [9] The transparent material according to [7] or [8], which has a haze value of 20 or less in a film form with a thickness of 30 μm.
[10] A transparent film comprising a transparent film-like supporting substrate and the transparent material according to any one of [7] to [9].
[11] A screen printing plate comprising the transparent material according to any one of [7] to [9] and a screen printing mesh.
[12] A method for producing the screen printing plate according to
[11] , comprising applying the resin composition according to any one of [1] to [6] to a screen printing mesh, and then subjecting the mesh to a drying treatment.
[13] A method for producing a screen printing plate using the transparent film according to
[10] , comprising wetting the surface of the transparent material of the transparent film with water or an aqueous medium, attaching the wetted transparent material to the screen printing mesh, and then removing the transparent film-like supporting substrate.
[14] A screen printing stencil comprising a cured product of the transparent material in the screen printing plate material according to
[11] .
[15] A method for producing the screen printing stencil according to
[14] , comprising: irradiating the transparent material of the screen printing plate with light to harden and insolubilize the transparent material; and then subjecting the transparent material to a water development treatment and a drying treatment to form a hardened product of the transparent material.
[16] A photosensitive resist film, characterized in that it is made of the transparent film according to
[10] .
[0022] The resin composition of the present invention and the transparent material obtained from this resin composition have the great advantage of being highly transparent, and in particular highly transparent to visible light and ultraviolet light.
[0023] For this reason, when a photoreactive material such as a photoacid generator or a sensitizer is present in the resin composition, the amount of light reaching the photoreactive material increases. Therefore, the photosensitive resin composition of the present invention containing the photoreactive material can achieve the following effects, for example: (1) By applying the photosensitive resin composition of the present invention to a substrate such as a film or a screen mesh and drying it to form a photosensitive transparent material film, a photosensitive transparent film, a screen printing plate, a screen printing stencil, and a photosensitive resist film can be provided. (2) The photosensitive resin composition, photosensitive transparent material, photosensitive transparent film, screen printing plate, and screen printing stencil of the present invention use only water as a solvent in their production and development processes, which is suitable for ensuring a safe working environment, preventing fires, and preventing pollution. (3) The photosensitive transparent material obtained from the photosensitive resin composition of the present invention has high transmittance for visible light and ultraviolet light and significantly reduced scattering of these rays. This allows high-resolution relief images to be obtained by light irradiation. The improvement in resolution is particularly remarkable in photosensitive films with large thicknesses. (4) The photoinsolubilization of the photosensitive transparent material according to the present invention is not inhibited by oxygen in the air, so a barrier film is not required. Therefore, there is no reduction in resolution due to the barrier film. (5) By wet laminating the photosensitive transparent film according to the present invention onto an etching substrate, a dry film resist that is not inhibited by oxygen can be obtained. (6) The epoxy compound of component (B) not only undergoes cationic polymerization but also forms a high-density crosslinked structure through an acid-catalyzed addition reaction with the hydroxyl groups of polyvinyl alcohol, so the photoinsolubilized relief pattern has excellent chemical resistance, water resistance, and solvent resistance.
[0024] [Resin Composition] The resin composition according to the present invention is characterized by comprising an aqueous solution of the following component (A) and the following component (B) emulsified and dispersed in the aqueous solution: Component (A): at least one water-soluble polymer selected from the group consisting of a polyvinyl alcohol polymer, an ethylene-vinyl alcohol copolymer, hydroxyethyl cellulose, and hydroxypropyl cellulose, Component (B): a cationically polymerizable monomer comprising, as an essential component, an epoxy compound having at least one epoxy group (component (b1)), and having a viscosity of 300 mPa·s or more and 12,000 mPa·s or less.
[0025] The resin composition according to the present invention essentially contains a specific component (A) and a specific component (B), but may contain other components (i.e., components other than component (A) and components other than component (B)). Specific examples of such other components include a photoacid generator and a sensitizer.
[0026] In this specification, "resin compositions containing specific component (A) and specific component (B) as essential components" are collectively referred to as "resin compositions." The resin composition according to the present invention and a transparent material obtained from this resin composition may be characterized by excellent long-term storage stability and transparency.
[0027] In addition, "a resin composition containing a specific component (A) and a specific component (B) and further containing a photoacid generator (component (C))" and "a resin composition containing a specific component (A) and a specific component (B) and further containing a photoacid generator (component (C)) and a sensitizer (component (D))" may be referred to as "photosensitive resin composition" according to the present invention.
[0028] A preferred example of the resin composition according to the present invention comprises a dispersion medium comprising an aqueous solution of component (A) and a dispersoid containing component (B) emulsified and dispersed in the dispersion medium, the dispersoid having a particle size (median size (D50)) measured by a laser diffraction / scattering method of 0.1 μm to 3.0 μm, preferably 0.1 μm to 2.0 μm. Here, the particle size (median size (D50)) measured by a laser diffraction / scattering method is defined by JIS Z8825:2013, and specifically, is determined using an MT3000II (Microtrac Bell Corporation).
[0029] In the present invention, regardless of the type of cationically polymerizable epoxy monomer and oxetane monomer in component (B) or the ratio of their mixture, when their viscosities are within a specific range, the films prepared from their aqueous emulsions have excellent transparency. Each component in the present invention is shown below.
[0030] <Component (A)> The component (A) used in the present invention is at least one water-soluble polymer selected from the group consisting of polyvinyl alcohol polymers, ethylene-vinyl alcohol copolymers, hydroxyethyl cellulose, and hydroxypropyl cellulose.
[0031] Component (A) is preferably polyvinyl alcohol. Polyvinyl alcohol with a saponification rate of 60% or more, particularly polyvinyl alcohol with a saponification rate of 80% or more, is preferred. A saponification rate of 60% or more improves water resistance and the emulsion dispersion state. The upper limit of the saponification rate is 99%.
[0032] Furthermore, the amount of sodium acetate produced by saponification is preferably 5% by weight or less, and particularly preferably 0.04 to 3% by weight. Polyvinyl alcohol having a sodium acetate content within the above range is preferred from the viewpoints of sensitivity and resolution.
[0033] The polyvinyl alcohol preferably has a degree of polymerization of 300 to 4500, particularly preferably 1000 to 4000. A polyvinyl alcohol-based polymer having a degree of polymerization within the above range is preferable in terms of, for example, water resistance, film strength, and image reproducibility, and can also achieve a high level of balance among these.
[0034] In place of partially saponified polyvinyl acetate, an ethylene-vinyl alcohol copolymer can be suitably used, in which the ethylene unit content is preferably 2 to 15 mol %, more preferably 3 to 10 mol %.
[0035] Also preferably used are water-soluble polyvinyl alcohols partially acetalized with butylaldehyde, acrolein, etc., or polyvinyl alcohols modified by copolymerization with a monomer having a cationic group. In such modified polyvinyl alcohols, the proportion of unmodified vinyl alcohol components in the main chain is at least 60 mol %, preferably 70 mol % or more.
[0036] <Component (B)> Component (B) is a cationically polymerizable monomer that contains, as an essential component, an epoxy compound (component (b1)) having at least one epoxy group, and has a viscosity of 300 mPa s or more and 12,000 mPa s or less. Here, the viscosity of component (B) is specified in accordance with JIS Z8803, and specifically, the viscosity at a liquid temperature of 25°C was determined using TVB-10 (Toki Sangyo Co., Ltd.).
[0037] It is worth noting here that, regardless of the type and blending ratio of the cationically polymerizable monomer of component (B), an emulsion film with excellent transparency can be obtained as long as the monomer viscosity is in the range of 300 mPa·s or more and 12,000 mPa·s or less.
[0038] The upper and lower limits of the monomer viscosity were determined through the following procedure.
[0039] The viscosities of numerous single cationically polymerizable monomers and various mixtures of cationically polymerizable monomers were measured. Films were then prepared from emulsions of each monomer prepared using an aqueous solution of partially saponified polyvinyl alcohol, and the transmittance at 405 nm was measured. Based on these measured values, the logarithm of viscosity was plotted on the horizontal axis and the haze value on the vertical axis. It was found that high transmittance at 405 nm was achieved when the viscosity of the monomer was in the range of 300 mPa·s or more and 12,000 mPa·s or less. On the other hand, at viscosities below approximately 300 mPa·s, the transmittance significantly decreased discontinuously. That is, the lower limit of 300 mPa·s of the monomer viscosity required to ensure high transmittance was determined based on the experimental results described above. Meanwhile, the upper limit of 12,000 mPa·s was determined based on the viscosity of EX-622. This result was determined taking into account the upper limit of the monomer viscosity when preparing aqueous emulsions at room temperature.
[0040] The preferred photoacid generator (component (C)) and sensitizer (component (D)) of the present invention described below, as well as their photodecomposition products, have no absorption band in the visible light region, and the viscosity hardly changes even when the photoacid generator and sensitizer are dissolved in the monomer within a concentration range that imparts photosensitivity. Therefore, the above-mentioned upper and lower limits of the monomer viscosity serve as the criteria for obtaining a transparent photosensitive film.
[0041] The viscosity of component (B) is preferably 1000 mPa·s or more and 12000 mPa·s or less.
[0042] Component (B) of the present invention requires component (b1), and such component (B) may be any of the following: (I) when a single type of component (b1) alone (i.e., when only one type of component (b1)) provides a viscosity within the above-mentioned specified range; (II) when a combination of multiple types of components (b1) (i.e., when two or more types of components (b1)) provides a viscosity within the above-mentioned specified range; or (III) when a combination of one or more types of component (b1) with one or more types of other cationically polymerizable monomer components other than component (b1) (e.g., component (b2) described below), or other components, provides a viscosity within the above-mentioned specified range.
[0043] When multiple components are used in combination as in (II) and (III) above, the requirement of "a viscosity of 300 mPa s or more and 12,000 mPa s or less" for component (B) can be satisfied by appropriately selecting each component and the proportions of each component used.
[0044] As in the case of (I) above, when a single component (b1) is used to achieve the viscosity within the specified range, the selection of component (b1) tends to be limited. However, when multiple components are used in combination, as in the cases of (II) and (III) above, the selection of component (b1) and other cationically polymerizable monomer components is greatly expanded. For example, even if component (b1) alone cannot achieve the viscosity within the specified range, the viscosity of component (B) can be adjusted by appropriately combining it with other cationically polymerizable monomer components, etc., thereby easily achieving the specified viscosity. Furthermore, more desirable viscosities can be easily obtained. Furthermore, component (B) and resin compositions with properties or characteristics that are difficult to achieve with component (b1) alone can be easily obtained. This allows more desirable component (B) and resin compositions suitable for specific applications to be obtained easily and at low cost.
[0045] <<Component (b1)>> Component (B) of the present invention comprises, as an essential component, an epoxy compound having at least one epoxy group (component (b1)). Specific examples of such component (b1) include the following (A) to (C).
[0046] In the present invention, the compounds exemplified in (A) to (C) can be used alone or in combination, provided that the component (B) satisfies the requirement that the viscosity be 300 mPa s or more and 12,000 mPa s or less.
[0047] (A) Examples of reactive diluents include, but are not limited to, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, phenol (EO) 5 glycidyl ether, p-tert-butylphenyl glycidyl ether, dibromophenyl glycidyl ether, lauryl alcohol (EO) 15 glycidyl ether, and C12 / C13 mixed alcohol glycidyl ether. Specific examples include Denacol EX-121, EX-141, EX-145, EX-146, EX-147, EX-171, EX-192, and EX-731 manufactured by Nagase ChemteX Corporation, and Epolite 100MF manufactured by Kyoeisha Chemical Co., Ltd. The use of these as reactive diluents allows the use of high-viscosity or solid epoxy resins.
[0048] (b) Examples of polyfunctional glycidyl epoxy monomers include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, diglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether), ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, glycerin diglycidyl ether, terephthalic acid diglycidyl ester, phthalic acid diglycidyl ester, and hydrogenated phthalic acid diglycidyl ester. Specific examples include Denacol EX-201, EX-211, EX-212, EX-252, EX-411, EX-622, and EX-711 manufactured by Nagase ChemteX Corporation; YD-115, YD-115G, YD-115CA, YD-118T, YD-127, and YD-128 manufactured by Nippon Steel Chemical & Material Co., Ltd.; 40E, 100E, 200E, 400E, 70P, 200P, 400P, 1500NP, 1600, 80MF, 4000, and 3002(N) of the Epolite series manufactured by Kyoeisha Chemical Co., Ltd.; and jER epoxy resin series 825, 827, 828, 828EL, 828US, 828XA, and 834 manufactured by Mitsubishi Chemical Corporation.
[0049] (c) Examples of alicyclic epoxy monomers include 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate (Celloxide 2021P), an adduct of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate and ε-caprolactone (Celloxide 2081), 1,2,8,9-diepoxylimonene (Celloxide 3000), (3,3'4,4'-diepoxy)bicyclohexyl (Celloxide 8000), 1,2-epoxy-4-vinylcyclohexane (Celloxide 2000), 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (EHPE3150, 3150CE), and butanetetracarboxylic acid. Examples of the component (b1) include, but are not limited to, tetra(3,4-epoxycyclohexylmethyl)-modified ε-caprolactone (Epolead GT401) and 3,4-epoxycyclohexylmethyl methacrylate (Cyclomer M100). Specific examples include Celloxide 2021P, Celloxide 2081, Celloxide 3000, Celloxide 8000, Celloxide 2000, EHPE3150, 3150CE, Epolead GT401, and Cyclomer M100, all manufactured by Daicel Corporation. In the present invention, a particularly preferred example of the component (b1) is hydrogenated bisphenol A diglycidyl ether.
[0050] <<Component (b2)>> Component (B) of the present invention can optionally contain other cationically polymerizable monomer components in addition to the above-described component (b1). Examples of such other cationically polymerizable monomers include oxetane monomers (component (b2)). The incorporation of the oxetane monomers (component (b2)) can adjust the viscosity of component (B) and significantly improve the cationic polymerization rate.
[0051] Preferred examples of the oxetane monomer (component (b2)) that can be used in the present invention include the following. These can be used alone or in combination of two or more types.
[0052] For example, (a) monofunctional ones include 3-ethyl-3-hydroxymethyloxetane (oxetane alcohol) (OXT-101, EHO), 2-ethylhexyloxetane (OXT-212), (3-ethyloxetan-3-yl)methyl methacrylate (OXE-30), (3-ethyloxetan-3-yl)methyl acrylate (OXE-10), 3-ethyl-3-(4-hydroxybutyloxymethyl)oxetane (HBOX), and the like. Specific examples include EHO and HBOX manufactured by Ube Industries, Ltd., OXT-101 and 212 manufactured by Toagosei Co., Ltd., and OXE-10 and OXE-30 manufactured by Osaka Organic Chemical Industry Ltd.
[0053] (ii) Examples of bifunctional compounds include xylylene bisoxetane (OXT-121, XDO), 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane (OXT-221, DOX), 4,4'-bis[(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl) (OXBP), bis[(3-ethyl-3-oxetanyl)methyl]isophthalate (OXIPA), and the like. Specific examples include OXBP and OXIPA manufactured by Ube Industries, Ltd., and OXT-121 and OXT-221 manufactured by Toagosei Co., Ltd.
[0054] These oxetane monomers can be used in combination with the above-mentioned epoxy monomers.
[0055] In the present invention, a particularly preferred example of the component (b2) is 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.
[0056] <Breakdown of Components and Preparation of Resin Composition> The blending ratio of each component in the present invention is as follows. The ratio of parts by mass of component (B) to 1 part by mass of component (A) is preferably 1 to 15 parts by mass, and particularly preferably 1 to 10 parts by mass. If the blending ratio is below this range, photocrosslinking does not occur sufficiently, and resolution may decrease significantly. On the other hand, if the blending ratio exceeds this range, resolution also decreases significantly, and the water resistance of the insolubilized pattern tends to deteriorate.
[0057] The resin composition according to the present invention is in the form of an aqueous emulsion comprising an aqueous solution in which component (A) is dissolved in an aqueous medium (preferably water) and a dispersoid emulsified and dispersed in this aqueous solution.
[0058] In this case, the proportion of component (A) in the aqueous solution is preferably 5 to 50% by mass, and particularly preferably 10 to 30% by mass, based on 100% by mass of the entire aqueous solution. If the concentration of component (A) is less than 5% by mass, the viscosity of the aqueous solution decreases and the aqueous solution may not form an aqueous emulsion. On the other hand, if the concentration exceeds 50% by mass, the aqueous emulsion tends to gel, which is undesirable. The water content in the resin composition of the present invention in the form of an aqueous emulsion does not need to be constant at a predetermined value and can fluctuate. For example, emulsions with a reduced water content due to drying are also included in the resin composition of the present invention. Incidentally, the transparent material of the present invention is derived from a dried product of the resin composition in the form of the aforementioned aqueous emulsion.
[0059] The resin composition of the present invention may contain, as needed, existing additives such as emulsifiers, antifoaming agents, leveling agents, colorants, ultraviolet absorbers, polymer emulsions, etc., within the range that does not impair transparency. The resin composition of the present invention may also contain a photoacid generator and a sensitizer (preferable photoacid generators and sensitizers in the present invention will be described later).
[0060] To prepare the resin composition of the present invention, polyvinyl alcohol, component (A), is dissolved in water to prepare an aqueous polyvinyl alcohol solution of a predetermined concentration, and a cationically polymerizable monomer, component (B), is added to this aqueous solution of component (A), followed by emulsification and dispersion by stirring in a conventional manner to prepare an aqueous emulsion.
[0061] When component (b1) and an oxetane monomer (component (b2)) are used in combination as component (B), it is preferable to premix component (b1) and component (b2) and then add this mixture to the aqueous solution of component (A).
[0062] [Transparent Material] The transparent material according to the present invention is formed from the resin composition described above and is characterized by comprising a dried product thereof. Here, "drying" refers to removing volatile components from the resin composition in the form of an aqueous emulsion to reduce its mass, and "dried product" refers to a product obtained by the drying (however, this is not limited to products from which substantially all of the volatile components have been removed, but also includes products from which some of the volatile components remain).
[0063] In the present invention, volatile components (mainly the water or aqueous medium that formed the aqueous solution of component (A)) are removed from a resin composition in the form of an aqueous emulsion, and a transparent material containing the dried product can be obtained. The opaque aqueous emulsion gradually becomes transparent as drying progresses, resulting in the transparent material of the present invention. The amount of water or aqueous medium in the transparent material of the present invention is preferably 50% by mass or more, and particularly preferably 60 to 80% by mass, when the total amount of the transparent material before drying is taken as 100% by mass.
[0064] The drying method is not particularly limited as long as the object of the present invention is achieved, and can be any method, such as (a) leaving it at room temperature under atmospheric pressure, (b) heating it under atmospheric pressure (e.g., drying by far-infrared irradiation), (c) leaving it at room temperature under reduced pressure, (d) heating it under reduced pressure, (e) blowing air or an inert gas onto it (e.g., hot air drying), or (f) using a desiccant. In the present invention, for example, hot air drying and far-infrared drying are preferred.
[0065] The transparent material according to the present invention has high transparency to light having wavelengths in the visible to ultraviolet regions, and has a particularly high transmittance for light having a wavelength of 405 nm and an excellent haze value. For example, it is a preferred transparent material having a haze value of 20 or less in the form of a 30 μm-thick film and / or a transmittance of 60% or more and 100% or less for light having a wavelength of 405 nm in the form of a 30 μm-thick film.
[0066] The transparent material according to the present invention in such a film form can be easily obtained, for example, by applying it to another film (support film) or the like and drying it, as described below.
[0067] The transparent material of the present invention also has excellent transparency, which prevents a decrease in resolution due to light scattering.Furthermore, since the epoxy compound can form a high-density crosslinked structure not only by cationic polymerization but also by an acid-catalyzed addition reaction with the hydroxyl groups of polyvinyl alcohol, the transparent material has excellent chemical resistance, water resistance, and solvent resistance.
[0068] [Transparent Film and Manufacturing Method Thereof] The transparent film according to the present invention is characterized by comprising a transparent film-like support substrate (also referred to as a support film) and the above-described transparent material. Such a transparent film can be obtained by applying the above-described resin composition of the present invention to the support film and drying it. Examples of the support film in this case include various conventionally known polymer films, preferably polyester, polyolefin, cellulose acetate, polyimide, etc. The thickness (after drying) of such a film is 5 to 500 μm, preferably 10 to 200 μm.
[0069] The resin composition can be applied to the surface of a substrate or a support film by any known method that forms a uniform film, such as spin coating, brushing, spraying, reverse roll coating, dip coating, doctor knife coating, and curtain coating.
[0070] The film thickness depends on the purpose and the type of substrate, but is 0.1 μm to 2000 μm, preferably 1.0 to 1000 μm, in average. The resin layer coated on the support film can be dried by a conventionally known method to obtain a transparent film. Examples of drying methods include hot air drying and far-infrared drying.
[0071] In this way, a transparent film (two-layer film) according to the present invention can be obtained, which consists of a support film and a transparent material formed on this support film. Since this transparent film (two-layer film) according to the present invention contains a transparent film-like support substrate and a transparent material, it is usually self-supporting. If necessary, a surface protective film can be provided on the surface of the transparent material of such a transparent film. Here, preferred examples of the surface protective film include polyethylene film, polypropylene film, and polyethylene terephthalate film.
[0072] [Photosensitive Resin Composition] The resin composition according to the present invention may further contain, in addition to the above-described components (A) and (B), component (C): a photoacid generator. By forming the resin composition into one that further contains, in addition to the above-described components (A) and (B), a photoacid generator, the resin composition can be suitably used, for example, as a photosensitive resin composition.
[0073] A preferred example of the photosensitive resin composition comprises a dispersion medium consisting of an aqueous solution of the component (A) and a dispersoid containing the components (B) and (C) emulsified and dispersed in the dispersion medium, wherein the dispersoid has a particle size (median size (D50)) measured by a laser diffraction / scattering method of 0.1 μm to 3.0 μm, preferably 0.1 μm to 2.0 μm. Here, the particle size (median size (D50)) measured by the laser diffraction / scattering method is defined in JIS Z8825:2013, and specifically, is determined using an MT3000II (Microtrac Bell Corporation).
[0074] In the present invention, regardless of the type of cationically polymerizable epoxy monomer and oxetane monomer in component (B) or the ratio of their mixture, when their viscosities are within a specific range, the films prepared from their aqueous emulsions have excellent transparency. Each component in the present invention is shown below.
[0075] <Component (A)> Component (A) of the photosensitive resin composition according to the present invention is at least one water-soluble polymer selected from the group consisting of polyvinyl alcohol polymers, ethylene-vinyl alcohol copolymers, hydroxyethyl cellulose, and hydroxypropyl cellulose. As component (A) of the photosensitive resin composition according to the present invention, those described in detail in the section [Resin Composition] of this specification can be used. The aqueous solution of component (A) is also as described in detail in [Resin Composition].
[0076] <Component (B)> Component (B) of the photosensitive resin composition according to the present invention is a cationically polymerizable monomer that contains, as an essential component, an epoxy compound having at least one epoxy group (component (b1)) and has a viscosity of 300 mPa·s or more and 12,000 mPa·s or less. As component (B) of the photosensitive resin composition according to the present invention, those described in detail in the section [Resin Composition] of this specification can be used. For example, components (b1) and (b2) are also as described in detail in [Resin Composition].
[0077] <Component (C)> As described above, the resin composition according to the present invention can be suitably used as a photosensitive resin composition by including a photoacid generator (component (C)). The photoacid generator of component (C) in the present invention is a conventionally known compound having cationic polymerization initiation ability, and compounds used in chemically amplified photoresists and photocationic polymerization systems are used. Examples of photoacid generators used in the present invention include onium cationic compounds that have no absorption band in the visible light region of approximately 500 nm or more and sulfonated compounds that generate sulfonic acid, but photocationic polymerization initiators that generate strong acids that initiate cationic polymerization are particularly preferred. Examples of suitable compounds are as follows:
[0078] That is, the ionic photoacid generator includes onium cations such as diazonium, ammonium, iodonium, sulfonium, phosphonium, and ferrocenium, such as BF 4 - , P.F. 6 - , AsF 6 - , SbF6 - , (C 6 F 5 ) 4 B - , (C 4 H 9 ) 4 B - Examples of salts include:
[0079] Specific examples of the onium cation include 1-methoxyquinolinium, 1-ethoxyisoquinolinium, 1-phenacylpyridinium, 1-benzyl-4-benzoylpyridinium, 1-benzylquinolinium, and N-substituted benzothiazolium.
[0080] Further, benzyltriphenylsulfonium, p-methoxyphenyldiphenylsulfonium, bis(p-methoxyphenyl)phenylsulfonium, tris(p-methoxyphenyl)sulfonium, p-phenylthiophenyldiphenylsulfonium, benzyltetramethylenesulfonium, phenacyltetramethylenesulfonium, phenacyldimethylsulfonium, p-methoxyphenyldiethylsulfonium, naphthyldialkylsulfonium, (2-naphthylcarbonylmethyl)tetramethylenesulfonium, (p-hydroxyphenyl)dimethylsulfonium, (4-hydroxynaphthyl)diethylsulfonium, (4,7-dihydroxynaphthyl)-1-dimethylsulfonium, (4,8-dihydroxynaphthyl)-1-dimethylsulfonium, diphenyliodonium, phenyl(4-methoxyphenyl)iodonium, phenyl{4-(tert-butyl)phenyl}iodonium, (4-bis{4-(tert-butyl)phenyl}iodonium, bis(4-dodecylphenyl)iodonium, (4-methoxyphenyl)(4-octyloxyphenyl)iodonium, phenacyltriphenylphosphonium, and cyanomethyltriphenylphosphonium.
[0081] These may be used alone or in combination of two or more. In the present invention, a particularly preferred example of the component (C) is p-phenylthiophenyldiphenylsulfonium.
[0082] <Component (D)> When the resin composition according to the present invention is used as a photosensitive resin composition, a sensitizer (component (D)) can be further contained, if necessary, in addition to the above-mentioned component (C). That is, the photoacid generators exemplified above generate the corresponding Bronsted acid or Lewis acid by themselves under the action of light. For example, if the absorption wavelength of the photoacid generator is biased toward the short wavelength side of near-ultraviolet light, in the present invention, it becomes easy to use a commonly used exposure device by coexisting various sensitizers as necessary. In order to obtain a transparent photosensitive film, it is required that the sensitizer has no absorption band in the visible light region of approximately 500 nm or more.
[0083] Examples of aromatic polycyclic compounds having a sensitizing function that satisfy these conditions include those having a basic skeleton composed of a hydrocarbon, such as naphthalene, phenanthrene, pyrene, anthracene, tetracene, chrysene, pentacene, picene, coronene, hexacene, and ovalene. Other examples include five-membered aromatic heterocyclic polycyclic compounds containing oxygen, nitrogen, and sulfur atoms as constituent atoms, such as benzofuran, dibenzofuran, indole, carbazole, benzothiophene, and dibenzothiophene. Furthermore, examples of six-membered aromatic heterocyclic polycyclic compounds include α-benzopyrone, β-benzopyrone, α-thiabenzopyrone, β-thiabenzopyrone, flavone, xanthone, thioxanthone, phenoxazine, and phenothiazine. These basic skeletons may be substituted with at least one electron-donating group, such as an alkyl group, a hydroxy group, an alkoxy group, or an alkylthio group. Examples of sensitizers composed of substituted aromatic polycyclic compounds include 1-methoxynaphthalene, 1,4-dimethylnaphthalene, 1,8-dimethylnaphthalene, 9,10-dimethylphenanthrene, 9-methylanthracene, 9,10-dimethylanthracene, 9,10-diphenylanthracene, 9,10-bis(phenylethynyl)anthracene, 1,8-dimethyl-9,10-bis(phenylethynyl)anthracene, 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, 9,10-dibutoxyanthracene, 2-ethyl-9,10-diethoxyanthracene, 1-methylpyrene, etc. Examples of substituted polycyclic heterocyclic compounds include N-methylcarbazole, N-ethylcarbazole, thioxanthone, chlorothioxanthone, isopropylthioxanthone, diethylthioxanthone, etc. Among these sensitizers, compounds having an anthracene or thioxanthone skeleton are particularly preferred. A particularly preferred example of component (D) is 9,10-dibutoxyanthracene. These can be used alone or in combination.
[0084] <Breakdown of Components and Preparation of Resin Composition> The blending ratio of each component in the present invention is as follows: The ratio of the total parts by weight of components (B) and (C) (and, when a sensitizer (component (D)) is used, the total of components (B) to (D)) to 1 part by weight of component (A) is preferably 1 to 15 parts by weight, and particularly preferably 1 to 10 parts by weight. If the blending ratio is below this range, photocrosslinking may not occur sufficiently, resulting in a significant decrease in resolution. On the other hand, if the blending ratio exceeds this range, there is also a tendency for the resolution to decrease significantly and for the water resistance of the insolubilized pattern to deteriorate.
[0085] In one embodiment, the resin composition according to the present invention is in the form of an aqueous emulsion comprising an aqueous solution in which component (A) is dissolved in an aqueous medium (preferably water) and a dispersoid emulsified and dispersed in this aqueous solution.
[0086] In this case, the proportion of component (A) in the aqueous solution is preferably 5 to 50% by mass, and particularly preferably 10 to 30% by mass, based on 100% by mass of the entire aqueous solution. If the concentration of component (A) is less than 5% by mass, the viscosity of the aqueous solution decreases and the aqueous solution may not form an aqueous emulsion. On the other hand, if the concentration exceeds 50% by mass, the aqueous emulsion tends to gel, which is undesirable. The water content of the photosensitive resin composition of the present invention in the form of an aqueous emulsion does not need to be constant at a predetermined value and can fluctuate. For example, emulsions with reduced water content due to drying are also included in the photosensitive resin composition of the present invention. Incidentally, the photosensitive transparent material of the present invention is derived from a dried product of the photosensitive resin composition in the form of the aqueous emulsion described above.
[0087] Regarding the blending ratio of component (B) as a monomer to component (C) as a photoacid generator, the amount of component (C) per 1 part by weight of component (B) is preferably 0.01 to 0.5 parts by weight, and particularly preferably 0.05 to 0.3 parts by weight. On the other hand, if the concentration is less than this range, sufficient photoimage formation cannot be achieved, and even if the concentration exceeds this range, there is almost no change in sensitivity. The parts by weight of component (D) as a sensitizer per 1 part by weight of component (C) as a photoacid generator are preferably 0.05 to 2, and particularly preferably 0.1 to 1. Below this range, relief image formation becomes insufficient. On the other hand, even if the concentration exceeds this range, there is almost no change in sensitivity.
[0088] To the resin composition according to the present invention, additives such as existing emulsifiers, antifoaming agents, leveling agents, ultraviolet absorbers, polymer emulsions, etc. may be added as needed, provided that the transparency is not impaired.
[0089] To prepare the resin composition according to the present invention, a photoacid generator (component (C)) and a sensitizer (component (D)) are dissolved in a cationically polymerizable monomer (component (B)), and the solution is added to an aqueous solution of a water-soluble polymer (component (A)). The solution is emulsified and dispersed by stirring in a conventional manner to produce an aqueous emulsion. When component (b1) and an oxetane monomer (component (b2)) are used in combination as component (B), it is preferable to premix component (b1) and component (b2).
[0090] [Photosensitive Transparent Material] The resin composition according to the present invention is transparent after drying, making it suitable for use as a transparent material. According to one embodiment of the present invention, a transparent material containing a dried product of the resin composition is provided. In particular, a resin composition containing the above-described components (C) and (D) functions as a photosensitive resin composition, and a transparent material made from the dried product can be used as a photosensitive transparent material. Here, "drying" refers to removing volatile components from a photosensitive resin composition in the form of an aqueous emulsion to reduce its mass, and "dried product" refers to a product resulting from the drying process (however, this is not limited to products from which substantially all of the volatile components have been removed, but also includes products in which some of the volatile components remain). Furthermore, "transparent" refers to a material that has high transmittance at a wavelength of 405 nm and an excellent haze value, for example. For example, a haze value of 20 or less in a 30 μm-thick film form and / or a transmittance of 405 nm light in a 30 μm-thick film form of 60% or more and 100% or less can be used.
[0091] In the present invention, volatile components (mainly the water or aqueous medium that formed the aqueous solution of component (A)) are removed from a resin composition in the form of an aqueous emulsion, and a transparent material containing the dried product can be obtained. The opaque aqueous emulsion gradually becomes transparent as drying progresses, resulting in the transparent material of the present invention. The amount of water or aqueous medium in the transparent material of the present invention is preferably 50% by mass or less, and particularly preferably 60 to 80% by mass, when the total amount of the transparent material (i.e., the resin composition) before drying is taken as 100% by mass.
[0092] The drying method is not particularly limited as long as the object of the present invention is achieved, and can be any method, such as (a) leaving it at room temperature under atmospheric pressure, (b) heating it under atmospheric pressure (e.g., drying by far-infrared irradiation), (c) leaving it at room temperature under reduced pressure, (d) heating it under reduced pressure, (e) blowing air or an inert gas onto it (e.g., hot air drying), or (f) using a desiccant. In the present invention, for example, hot air drying and far-infrared drying are preferred.
[0093] The transparent material according to the present invention has high transparency to light having wavelengths in the visible to ultraviolet regions, for example, a particularly high transmittance of light having a wavelength of 405 nm, and an excellent haze value. For example, it is a preferred transparent material having a haze value of 20 or less in the form of a 30 μm thick film and / or a transmittance of 60% or more and 100% or less of light having a wavelength of 405 nm in the form of a 30 μm thick film. Therefore, the transparent material according to the present invention is particularly useful as a photosensitive transparent material for patterning by exposure.
[0094] The transparent material according to the present invention in such a film form can be easily obtained, for example, by applying it to another film (support film) or the like and drying it, as described below.
[0095] [Photosensitive Transparent Film and Manufacturing Method Thereof] The transparent film according to the present invention is characterized by comprising a transparent film-like support substrate and the aforementioned transparent material. According to one embodiment of the present invention, when the transparent material is a photosensitive transparent material comprising a dried product of a resin composition containing the aforementioned components (C) and (D), a transparent film comprising a transparent film-like support substrate and the aforementioned photosensitive transparent material can be used as a photosensitive transparent film. Such a transparent film can be obtained by applying the aforementioned resin composition of the present invention to a support film and drying it. Examples of the support film in this case include various conventionally known polymer films, preferably polyester, polyolefin, cellulose acetate, polyimide, etc. The thickness (after drying) of the film is 5 to 500 μm, preferably 10 to 200 μm.
[0096] The resin composition can be applied to the surface of a substrate or a support film by any known method that forms a uniform film, such as spin coating, brushing, spraying, reverse roll coating, dip coating, doctor knife coating, and curtain coating.
[0097] The film thickness depends on the purpose and the type of substrate, but is 0.1 μm to 2000 μm, preferably 1.0 to 1000 μm, in average. The resin layer coated on the support film can be dried by a conventionally known method to obtain a transparent film (preferably a photosensitive transparent film). Drying methods include hot air drying and far-infrared drying.
[0098] In this way, a transparent film (two-layer film) according to the present invention can be obtained, which consists of a support film and a transparent material formed on this support film. Since this transparent film (two-layer film) according to the present invention contains a transparent film-like support substrate and a transparent material, it is usually self-supporting. If necessary, a surface protective film can be provided on the surface of the transparent material of such a transparent film. Here, preferred examples of the surface protective film include polyethylene film, polypropylene film, and polyethylene terephthalate film.
[0099] The resist film of the present invention can be used as a screen printing plate by peeling off the surface protective film and then bonding another substrate (e.g., a screen printing mesh) to the exposed surface of the transparent material. According to one embodiment of the present invention, when a photosensitive transparent material consisting of a dried product of a resin composition containing the above-mentioned components (C) to (D) is used as the transparent material, the resist film can be used as a photosensitive resist film.
[0100] Furthermore, the transparent film (single-layer film) according to the present invention can be obtained by separating the support film from the transparent film (two-layer film) according to the present invention. According to one embodiment of the present invention, when a photosensitive transparent material comprising a dried product of a resin composition containing the above-mentioned components (C) to (D) is used as the transparent material, the transparent film can be used as a photosensitive transparent film.
[0101] [Screen printing plate] The screen printing plate according to the present invention is characterized by comprising the above-mentioned transparent material and a screen printing mesh. As the transparent material, it is preferable to use a photosensitive transparent material made of a dried resin composition containing the above-mentioned components (C) and (D). Here, as the screen printing mesh, a conventionally used screen printing mesh can be used as is, or a modified screen printing mesh can be used.
[0102] In the present invention, it is preferable to use a mesh for screen printing that is densely woven from stainless steel wires having a diameter of 25 μm or less.
[0103] Such a screen printing plate according to the present invention can be easily obtained, for example, by the following [Production method for a screen printing plate (first method)] or [Production method for a screen printing plate (second method)].
[0104] [Method for producing a screen printing plate (first method)] The method for producing a screen printing plate (first method) according to the present invention is characterized in that the aforementioned resin composition is applied to a screen printing mesh, followed by a drying treatment. According to one embodiment of the present invention, the resin composition can be a photosensitive resin composition containing the above-mentioned components (C) to (D).
[0105] The resin composition can be applied to the screen printing mesh by known methods. For example, methods such as spin coating, brushing, spraying, reverse roll coating, dip coating, doctor knife coating, and curtain coating can be used. The optimum film thickness varies depending on the purpose and application, but the average film thickness is 0.1 μm to 2000 μm, preferably 1.0 to 1000 μm. The resin layer applied to the screen printing mesh can be dried by a conventionally known method to obtain the screen printing plate material of the present invention. Hot air drying and far-infrared drying are particularly preferred drying methods.
[0106] [Second Method for Producing a Screen Printing Plate] The second method for producing a screen printing plate according to the present invention comprises wetting the surface of the transparent material of the transparent film with water or an aqueous medium, attaching the wetted transparent material to a screen printing mesh, and then removing the transparent film-like support substrate. According to one embodiment of the present invention, when a photosensitive transparent material comprising a dried product of a resin composition containing the above-mentioned components (C) and (D) is used as the transparent material, the transparent film can be used as a photosensitive transparent film.
[0107] The surface of the transparent material of the above-mentioned transparent film is moistened with water or an aqueous medium, and then the moistened transparent material is attached to a screen printing mesh to obtain a laminate (three-layer product) consisting of a "screen printing mesh," a "transparent material," and a "transparent film-like support substrate."Then, the "transparent film-like support substrate" is removed to obtain a screen printing plate material (two-layer product) according to the present invention.
[0108] [Screen printing stencil] The screen printing stencil according to the present invention is characterized in that it comprises a cured product of the transparent material in the screen printing plate described above. It is preferable to use a photosensitive transparent material consisting of a dried product of a resin composition containing the above-described components (C) and (D). A specific example of such a screen printing stencil according to the present invention is a screen printing plate comprising the above-described photosensitive transparent material and a screen printing mesh, in which the photosensitive transparent material has been cured into a water-insoluble product by light irradiation.
[0109] [Method for manufacturing a screen printing stencil] The screen printing stencil according to the present invention can be manufactured by irradiating the transparent material in the screen printing plate with light to harden and insolubilize the material, followed by water development and drying. It is preferable to use a photosensitive transparent material comprising a dried product of a resin composition containing the above-mentioned components (C) and (D).
[0110] Specifically, in the method for producing a screen printing stencil according to the present invention (first production method), the aforementioned resin composition (preferably a photosensitive resin composition) is applied to a screen printing mesh and dried to form a resin composition layer, which is then exposed to light in a pattern and developed with neutral water to obtain a negative pattern. In this method, a screen printing plate is obtained by using a screen mesh as a substrate. This is then exposed to light in a pattern to harden and insolubilize the transparent material (preferably a photosensitive transparent material), followed by water development and drying to produce a negative screen printing stencil. Alternatively, a resin composition is applied to a smooth substrate and dried, and the resulting film is exposed to light in a pattern and developed with neutral water to form a negative pattern.
[0111] In a method for producing a screen printing stencil (second production method) according to the present invention, the surface of the transparent material (preferably a photosensitive transparent material) of the aforementioned transparent film (preferably a photosensitive transparent film) is wetted with water or an aqueous medium, followed by application of a screen printing mesh, drying, and then pattern exposure and water development. For example, a transparent material wetted with an aqueous medium is applied to a screen mesh by pressure bonding. Next, a resin composition layer (preferably a photosensitive resin composition layer) is dried, followed by pattern exposure and water development to produce a screen printing stencil.
[0112] When the resin composition of the present invention (preferably a photosensitive resin composition) is used as an etching film (preferably a photosensitive etching film) such as a dry film resist or a sandblasting film, a wet lamination method can be used in which the film is pressure-bonded to the surface of a substrate moistened with an aqueous medium. This allows a resist film that sufficiently conforms to the unevenness of the substrate surface to be provided, and the resulting resist film can be developed with water after pattern exposure.
[0113] Based on the above operations, the methods for producing a screen printing stencil according to the present invention (the first and second production methods) enable film formation and development using only neutral water. Water development is achieved by immersing a resin composition layer (preferably a photosensitive resin composition layer) in water to dissolve and remove the unexposed areas, or by removing the unexposed areas with a water jet from a spray gun.
[0114] In the above-described manufacturing method, the exposed portion of the resin composition (preferably a photosensitive resin composition) becomes insoluble in water, but to promote the insolubilization, a heat treatment can be carried out after exposure. The heating temperature depends on the type of screen and substrate, but is in the range of room temperature to 150°C, preferably room temperature to 100°C, and more preferably room temperature to 60°C. The heating time depends on the type of composition and the heating temperature, but is about 30 seconds to 60 minutes.
[0115] The photosensitive wavelength range of a photosensitive film provided on a substrate such as a screen mesh or polyester film can be determined by the type of photoacid generator or sensitizer. The transparency of the photosensitive film in the visible wavelength range of the present invention can be ensured by appropriately selecting a photoacid generator or sensitizer that does not absorb light in the visible wavelength range. Light sources that can be used include low-pressure water lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, mercury-xenon lamps, and fluorescent lamps, as well as LED light sources that emit ultraviolet light of specific wavelengths. Exposure can be carried out through a photomask or by directly writing a laser beam onto the photosensitive film. Alternatively, a colored image can be directly drawn onto the photosensitive film or ink-receiving film using an inkjet method or the like to form a negative image, which can then be exposed and developed. Highly transparent photosensitive films significantly reduce scattering of excitation light during pattern formation, thereby improving resolution, especially for thick films.
[0116] The photoinsolubilization of the photosensitive film of the present invention is not inhibited by oxygen in the air, so a barrier film is not required. Therefore, there is no reduction in resolution due to a barrier film. Furthermore, because of the excellent transparency, reduction in resolution due to light scattering is also suppressed. Furthermore, since the epoxy compound not only undergoes cationic polymerization but also forms a high-density crosslinked structure through an acid-catalyzed addition reaction with the hydroxyl groups of polyvinyl alcohol, the photoinsolubilized relief image has excellent chemical resistance, water resistance, and solvent resistance.
[0117] [Photosensitive Resist Film] The resist film according to the present invention is characterized by comprising the transparent film described above. According to one embodiment of the present invention, the transparent film can be a photosensitive transparent film obtained using a photosensitive transparent material comprising a dried product of a resin composition containing the components (C) and (D) described above. The resist film according to the present invention can be wet-laminated onto an etching substrate while maintaining the various excellent properties of the transparent material described above, and is a resist film that is not inhibited by oxygen.
[0118] The photoinsolubilization of the resist film (preferably a photosensitive resist film) of the present invention is not inhibited by oxygen in the air, and therefore does not require a barrier film. Therefore, there is no reduction in resolution due to a barrier film. Furthermore, because of its excellent transparency, reduction in resolution due to light scattering is also suppressed. Furthermore, since the epoxy compound not only undergoes cationic polymerization but also forms a high-density crosslinked structure through an acid-catalyzed addition reaction with the hydroxyl groups of polyvinyl alcohol, the photoinsolubilized relief image has excellent chemical resistance, water resistance, and solvent resistance.
[0119] According to another aspect of the present invention, there is provided a resin composition for use in a screen printing plate material, a screen printing stencil, or a photosensitive resist film, characterized by comprising an aqueous solution of the following component (A) and the following component (B) emulsified and dispersed in the aqueous solution: component (A): at least one water-soluble polymer selected from the group consisting of a polyvinyl alcohol polymer, an ethylene-vinyl alcohol copolymer, hydroxyethyl cellulose, and hydroxypropyl cellulose, and component (B): a cationically polymerizable monomer comprising, as an essential component, an epoxy compound having at least one epoxy group (component (b1)), and having a viscosity of 300 mPa s or more and 12,000 mPa s or less. According to another aspect of the present invention, the resin composition may further comprise a photoacid generator (component (C)), or the resin composition may further comprise a photoacid generator (component (C)) and a sensitizer (component (D)).
[0120] According to another aspect of the present invention, there is provided use of a resin composition as a screen printing plate material, a screen printing stencil, or a photosensitive resist film, the resin composition comprising an aqueous solution of the following component (A) and the following component (B) emulsified and dispersed in the aqueous solution: component (A): at least one water-soluble polymer selected from the group consisting of polyvinyl alcohol polymers, ethylene-vinyl alcohol copolymers, hydroxyethyl cellulose, and hydroxypropyl cellulose, component (B): a cationically polymerizable monomer comprising, as an essential component, an epoxy compound having at least one epoxy group (component (b1)), and having a viscosity of 300 mPa s or more and 12,000 mPa s or less. According to another aspect of the present invention, the resin composition may further comprise a photoacid generator (component (C)), or the resin composition may further comprise a photoacid generator (component (C)) and a sensitizer (component (D)).
[0121] The present invention will be described in further detail below with reference to the following examples. (Components) The polyvinyl alcohol used had a degree of polymerization of 1700, a degree of saponification of 88%, and a sodium acetate content of 2% by weight (22-88 manufactured by Kuraray Co., Ltd.), the photoacid generator used was a sulfonium salt-based photocationic polymerization initiator (AT-6992 manufactured by ACETO Co., Ltd.), and the sensitizers used were isopropylthioxanthone (ITX manufactured by Nippon Kayaku Co., Ltd.) and 9,10-dibutoxyanthracene (UVS-1331 manufactured by Air Water Performance Chemicals Inc.). Examples of epoxy compounds include sorbitol polyglycidyl ether (EX-622 manufactured by Nagase ChemteX), pentaerythritol polyglycidyl ether (EX-411 manufactured by Nagase ChemteX), glycerol polyglycidyl ether (EX-314, EX-313 manufactured by Nagase ChemteX), 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate (Celloxide 2021 manufactured by Daicel), and P), hydrogenated bisphenol A diglycidyl ether (Nippon Steel Chemical & Material Co., Ltd., ST-3000) and bisphenol A diglycidyl ether (Nippon Steel Chemical & Material Co., Ltd., YD-128), and as oxetane compounds, xylylene bisoxetane (Toagosei Co., Ltd., OXT-121) and 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane (Toagosei Co., Ltd., OXT-221) were used.
[0122] (Measurement of Monomer Viscosity) The viscosity of the monomer was measured at 25° C. using a Brookfield viscometer (TVB-25 manufactured by Toki Sangyo Co., Ltd.).
[0123] (Preparation of emulsion film for transmittance measurement at 405 nm) 105 parts by mass of a cationically polymerizable monomer was added to 350 parts of a 15% by mass aqueous solution of polyvinyl alcohol while stirring to prepare an emulsion dispersion of the monomer. The resulting emulsion dispersion was applied to a polyester film substrate to prepare a film with a thickness of 30 μm, which was then peeled off from the substrate to obtain a film for transmittance measurement at 405 nm.
[0124] (Measurement of transmittance at 405 nm) The transmittance of the obtained film at 405 nm was measured using an ultraviolet-visible-near infrared spectrophotometer (V-750 manufactured by JASCO Corporation), and the average value of the values obtained at three different points was taken as the transmittance.
[0125] (Preparation of Photosensitive Composition) A mixture of 30 parts of a photoacid generator and 3 parts of a sensitizer dissolved in 210 parts of a cationically polymerizable monomer was added to 350 parts of a 15% by weight aqueous solution of polyvinyl alcohol while stirring, to obtain a photosensitive composition dispersion. The components used here are as described above.
[0126] (Preparation of emulsion film for haze measurement) The obtained photosensitive composition dispersion was applied to a polyester film substrate to prepare a film having a thickness of 30 μm, which was then peeled off from the substrate to obtain a film for haze measurement.
[0127] (Haze Measurement) The obtained film was measured using a haze meter (NDH8000 manufactured by Nippon Denshoku Industries Co., Ltd.), and the average value of values obtained at three different points was taken as the haze value.
[0128] <Examples 1 to 11 and Comparative Examples 1 to 8> Table 1 summarizes the viscosity, particle size in aqueous emulsion, and transmittance at 405 nm of films prepared from various cationically polymerizable monomers. Among the cationically polymerizable monomers used here, the EX series epoxy compounds, ST-3000, and YD-128 are glycidyl-type epoxy monomers, 2021P is a cycloaliphatic epoxy monomer, and OXT-221 is an oxetane monomer. Furthermore, Kuraray's 22-88 polyvinyl alcohol was used. The monomers are listed in descending order of viscosity in this table. Among the general-purpose monomers used here, YD-128 has the highest viscosity, yet the transmittance of the emulsion films obtained from it is unusually low. This is thought to be due to light scattering by crystalline fine particles. Meanwhile, as seen in Examples 1 to 11, the transmittance at 405 nm ranges from 71% to 85%, regardless of the type of cationically polymerizable monomer, whether single or a mixture. On the other hand, when we look at Example 11 and Comparative Example 2, the difference in monomer viscosity between them is relatively small at 30 mPa·s, yet the transmittance in Comparative Example 2 is significantly reduced to only 47%. A further decrease in viscosity leads to a further decrease in transmittance. This result suggests that the emulsion film will maintain high transmittance if the monomer viscosity is approximately 300 mPa·s or higher. This means that there is a lower limit to the monomer viscosity for maintaining high transmittance of the emulsion film, and that this value is approximately 300 mPa·s.
[0129] <Examples 12 to 21> Table 2 summarizes the sensitivity characteristics and haze values before and after exposure of photosensitive emulsions prepared from mixtures of epoxy monomer and oxetane monomer with a photoacid generator and sensitizer. Here, the photoacid generator and sensitizer were dissolved in a cationically polymerizable monomer, and a 15% by weight aqueous solution of polyvinyl alcohol was added to the resulting emulsion while stirring. The resulting emulsion was then uniformly applied to a polyester film and dried to produce a 30 μm thick film. The film was irradiated from a distance of 1 meter with a 3 kW halogen lamp and then developed by spraying water with a spray gun.
[0130] Examples 12 to 16 show the results of investigating the effect of adding OXT-221 on the photosensitivity of emulsion films containing EX-622, a photoacid generator, and a sensitizer. Sensitivity improved with increasing amounts of OXT-221 added. Examples 17 and 18 show the results of adding OXT-221 to ST-3000 emulsion films, and here too, the improvement in sensitivity due to the oxetane monomer was observed. Example 19 shows the results for a ternary monomer, and sensitivity was observed to be approximately the same as in the binary system. Example 20 shows the results of diluting YD-128 with OXT-221, and similar to the cases of EX-622 and ST-3000, the increased sensitivity due to OXT-221 was observed. Example 21 shows the results of using polyvinyl alcohol with a small amount of sodium acetate (degree of polymerization 1700, degree of saponification 88%, amount of sodium acetate 0.2% by weight (VP-18 manufactured by Nippon Vinegar Vipbal Co., Ltd.)), and it is observed that the amount of sodium acetate increases the sensitivity.
[0131] Next, we will focus on the haze values before and after exposure for the emulsion films based on EX-622 and ST-3000 in Examples 12 to 19. The haze values before and after exposure were 1.2 to 2.7, and all maintained high transparency while showing little change in haze value due to photocuring. On the other hand, Example 20 shows the results when YD-128 was diluted with OXT-221. As in Comparative Example 1, the transmittance of the emulsion film prepared from only YD-128 was extremely low. In contrast, dilution with OXT-221 ensured good transparency and a low haze value even after exposure.
[0132] Examples 22 to 31 (Preparation of Screen Printing Films and Photosensitivity Characteristics) Each of the photosensitive compositions obtained in Examples 12 to 21 was applied to a polyester film using a known coating method and dried to obtain a 30 μm screen printing film. A 250-mesh polyester screen was moistened with the composition, and the prepared film was attached by pressure and dried at 40°C to obtain a screen printing material. A 3 kW halogen lamp was used to irradiate the photosensitive layer from a distance of 1 meter through a photomask pattern attached to the screen, and the screen was then developed by spraying water with a spray gun. The photosensitivity characteristics were evaluated as follows: ∘ (a) if the 50 μm pattern was faithfully resolved; Δ (a) if partial defects were observed in the pattern; and × (b) if no pattern was formed. The results are shown in Table 3. Example 32 (Etching of Copper-Clad Laminate) A 25 μm photosensitive film prepared by applying the photosensitive composition obtained in Example 13 to a polyester film and drying it was pressed onto a copper-clad laminate having a substrate of glass epoxy resin moistened with water, and then dried at 70° C. for 30 minutes. After 4 minutes of exposure using a 3 kW halogen lamp through a photomask, the support film was peeled off, and the unexposed areas were removed by spraying water with a spray gun. Development yielded a relief pattern. The resulting film was immersed in a 5% aqueous solution of ferric chloride at room temperature for etching, rinsed with water, and then immersed in a 2% aqueous solution of sodium periodate for 3 minutes to remove the resist layer. As a result, a copper pattern faithful to the photomask was obtained.
Claims
1. A resin composition comprising an aqueous solution of the following component (A) and the following component (B) emulsified and dispersed in the aqueous solution: Component (A): at least one water-soluble polymer selected from the group consisting of polyvinyl alcohol polymers, ethylene-vinyl alcohol copolymers, hydroxyethyl cellulose, and hydroxypropyl cellulose, Component (B): a cationically polymerizable monomer having a viscosity of 300 mPa·s or more and 12,000 mPa·s or less, comprising, as an essential component, an epoxy compound having at least one epoxy group (component (b1)).
2. The resin composition according to claim 1, further comprising a photoacid generator (component (C)).
3. The resin composition according to claim 2, further comprising a sensitizer (component (D)).
4. The resin composition according to claim 1, wherein the component (A) is polyvinyl alcohol having a saponification rate of 60% or more and a sodium acetate content of 5% by weight or less.
5. The resin composition according to claim 1, wherein the component (B) contains the epoxy compound (component (b1)) and a compound having an oxetane group (component (b2)).
6. The resin composition according to claim 1, comprising a dispersion medium consisting of an aqueous solution of component (A) and a dispersoid containing component (B) emulsified and dispersed in the dispersion medium, wherein the dispersoid has a particle size (median size (D50)) measured by a laser diffraction / scattering method of 0.1 μm to 3.0 μm.
7. A transparent material comprising a dried product of the resin composition according to any one of claims 1 to 6.
8. The transparent material according to claim 7, which has a transmittance of light with a wavelength of 405 nm in the form of a film having a thickness of 30 μm of 60% or more and 100% or less.
9. The transparent material according to claim 7, which has a haze value of 20 or less in a film form having a thickness of 30 μm.
10. A transparent film comprising a transparent film-like supporting substrate and the transparent material according to claim 7.
11. A screen printing plate comprising the transparent material according to claim 7 and a screen printing mesh.
12. A method for producing the screen printing plate material according to claim 11, comprising applying the resin composition according to any one of claims 1 to 6 to a screen printing mesh, and then subjecting the mesh to a drying treatment.
13. A method for producing a screen printing plate using the transparent film described in claim 10, comprising wetting the surface of the transparent material of the transparent film with water or an aqueous medium, attaching the moistened transparent material to a screen printing mesh, and then removing the transparent film-like support substrate.
14. A stencil for screen printing, comprising a cured product of the transparent material in the screen printing plate material according to claim 11.
15. A method for producing a screen printing stencil as described in claim 14, comprising irradiating the transparent material in the screen printing plate with light to harden and insolubilize the transparent material, and then subjecting the transparent material to a water development process and a drying process to obtain a hardened transparent material.
16. A photosensitive resist film comprising the transparent film according to claim 10.
Citation Information
Patent Citations
Photosetting resin composition and screen printing plate
JP1998062990A
Active energy line sensitive resin composition, active energy line sensitive resin film and pattern forming method using the film
JP2004325810A
Active energy ray sensitive resin composition
JP2005208070A
Photosensitive film, screen printing plate, and photosensitive film for etching