Photosensitive thermosetting resin composition, dry film, cured product, and electronic component

The photosensitive thermosetting resin composition, incorporating a carboxyl group-containing resin and a combination of oxime ester and titanocene initiators, addresses the challenge of achieving high reflectance and heat resistance at low exposure doses, providing enhanced curing properties and stability for electronic components.

WO2024204759A1PCT designated stage expired Publication Date: 2024-10-03TAIYO HOLDINGS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013155
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing photosensitive thermosetting resin compositions struggle to achieve excellent surface curability and heat resistance at low exposure doses while maintaining high reflectance, which is essential for forming effective solder resist films in electronic components.

Method used

A photosensitive thermosetting resin composition is developed, comprising a carboxyl group-containing resin, an oxime ester photopolymerization initiator, a titanocene photopolymerization initiator, and a white pigment, specifically optimized to provide high reflectance and heat resistance, with a synergistic effect between the initiators enhancing curing properties and reducing discoloration.

Benefits of technology

The composition achieves excellent surface curability, heat resistance, and high reflectance, even at low exposure doses, with minimal discoloration due to the synergistic effect of the oxime ester and titanocene initiators, ensuring effective light utilization and stability in electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a photosensitive thermosetting resin composition from which it is possible to form a solder resist film that has high reflectance and excellent heat resistance and surface curability even with a low exposure amount. The photosensitive thermosetting resin composition contains a carboxy group-containing resin, a photoinitiator, a white pigment, and a thermosetting resin. The photoinitiator contains an oxime ester-based photoinitiator and a titanocene-based photoinitiator. The thermosetting resin contains an epoxy resin. A cured product obtained through thermosetting the photosensitive thermosetting resin composition has a b* value in the L*a*b* color system of 2.0 or less, and has a reflectance of 85% or more at a wavelength of 450 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Photosensitive thermosetting resin composition, dry film, cured product, and electronic component

[0001] The present invention relates to a photosensitive thermosetting resin composition, a dry film, a cured product, and an electronic component.

[0002] Light-emitting devices are known in which light-emitting diodes (hereinafter sometimes abbreviated as LEDs) are mounted on a printed wiring board. To efficiently utilize the light from the LEDs mounted on the printed wiring board, a highly reflective white solder resist film may be formed on the printed wiring board (see, for example, International Publication No. 2008 / 050768, Japanese Patent Application Laid-Open No. 2008-134621, Japanese Patent Application Laid-Open No. 2011-017010, and International Publication No. 2012 / 141124). Furthermore, Japanese Patent Application Laid-Open No. 2013-210443 proposes a photocurable thermosetting resin composition containing a photopolymerization initiator that does not contain a phosphorus atom in its molecular structure.

[0003] An object of one aspect of the present invention is to provide a photosensitive thermosetting resin composition that is excellent in surface curability and heat resistance even at a low exposure dose and that can form a solder resist film with high reflectivity.

[0004] The present invention encompasses the following aspects: [1] A photosensitive thermosetting resin composition comprising a carboxyl group-containing resin, a photopolymerization initiator, a white pigment, and a thermosetting resin, wherein the photopolymerization initiator comprises an oxime ester-based photopolymerization initiator and a titanocene-based photopolymerization initiator, the thermosetting resin comprises an epoxy resin, and a cured product of the photosensitive thermosetting resin composition after thermal curing is L. * a * b * b in the color system * A photosensitive thermosetting resin composition having a reflectance of 85% or more at a wavelength of 450 nm and a value of 2.0 or less.

[0005] [2] The photosensitive thermosetting resin composition according to [1], wherein the photopolymerization initiator contains an oxime ester photopolymerization initiator and a titanocene photopolymerization initiator in a mass ratio ranging from 1:10 to 10:1.

[0006] [3] A dry film having a resin layer obtained by applying the photosensitive thermosetting resin composition according to [1] or [2] to a first film and drying the applied resin layer.

[0007] [4] A cured product obtained by curing the photosensitive thermosetting resin composition according to [1] or [2].

[0008] [5] An electronic component comprising the cured product according to [4].

[0009] According to one aspect of the present invention, it is possible to provide a photosensitive thermosetting resin composition that is excellent in surface curability and heat resistance even at a low exposure dose and that can form a solder resist film with high reflectivity.

[0010] As used herein, the term "process" refers not only to an independent process, but also to processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Furthermore, the content of each component in a composition refers to the total amount of the components present in the composition, unless otherwise specified, when multiple substances corresponding to each component are present in the composition. Furthermore, the solid content refers to the substance remaining after removing volatile components (e.g., organic solvents). Furthermore, the upper and lower limits of the numerical ranges described herein can be arbitrarily selected and combined from the numerical values ​​exemplified as numerical ranges. Below, embodiments of the present invention are described in detail. However, the embodiments described below exemplify photosensitive thermosetting resin compositions, dry films, cured products, and electronic components intended to embody the technical concept of the present invention. The present invention is not limited to the photosensitive thermosetting resin compositions, dry films, cured products, and electronic components shown below.

[0011] Photosensitive thermosetting resin composition The photosensitive thermosetting resin composition comprises a carboxyl group-containing resin, a photopolymerization initiator, a white pigment, and a thermosetting resin. The photopolymerization initiator comprises at least an oxime ester-based photopolymerization initiator and a titanocene-based photopolymerization initiator. The thermosetting resin comprises at least an epoxy resin. The cured product of the photosensitive thermosetting resin composition after thermal curing is L * a * b * b in the color system * The reflectance at a wavelength of 450 nm is 85% or more.

[0012] By including a photopolymerization initiator having a specific structure in combination as a photopolymerization initiator, the photosensitive thermosetting resin composition can form a cured product with excellent surface curability and heat resistance and high reflectivity even at a low exposure dose. It can also suppress discoloration of the cured product due to heat, light, etc. Furthermore, it can form a latent image with high sensitivity and excellent resolution. This can be attributed to, for example, the synergistic effect of the oxime ester photopolymerization initiator and the titanocene photopolymerization initiator. The low exposure dose in the present invention specifically refers to 600 mJ / cm. 2 This refers to the following:

[0013] Carboxy Group-Containing Resin The carboxy group-containing resin may be any resin having a carboxy group in the molecule, and may or may not have a photosensitive functional group in the molecule. By including a carboxy group-containing resin in the photosensitive thermosetting resin composition, alkali developability can be imparted to the photocured product of the photosensitive thermosetting resin composition obtained by irradiating it with active energy rays. It is preferable that the carboxy group-containing resin have an ethylenically unsaturated double bond as a photosensitive functional group in the molecule in terms of photocurability, development resistance, etc. The ethylenically unsaturated double bond in the molecule may be derived from acrylic acid, methacrylic acid, or a derivative thereof. The photosensitive thermosetting resin composition may contain one carboxy group-containing resin alone, or two or more carboxy group-containing resins in combination. When the photosensitive thermosetting resin composition contains only a carboxy group-containing resin without an ethylenically unsaturated double bond as the carboxy group-containing resin, the photosensitive thermosetting resin composition can be made photocurable by using a compound having multiple ethylenically unsaturated groups in the molecule, i.e., a photopolymerizable monomer, as described below. Specific examples of the carboxyl group-containing resin include the following compounds (which may be either oligomers or polymers): Note that, hereinafter, the term "(meth)acrylate" is a general term for acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.

[0014] (1) Carboxy group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, or isobutylene.

[0015] (2) Carboxy group-containing urethane resins obtained by polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxy group-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxy groups and alcoholic hydroxy groups.

[0016] (3) Carboxy group-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins, and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxy group-containing dialcohol compounds, and diol compounds.

[0017] (4) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3) described above.

[0018] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation, obtained by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3) described above.

[0019] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl group present in the side chain.

[0020] (7) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin in which the hydroxyl groups of a bifunctional (solid) epoxy resin are further epoxidized with epichlorohydrin with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.

[0021] (8) Carboxy group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin, and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.

[0022] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl groups of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, or adipic acid.

[0023] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.

[0024] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.

[0025] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins (1) to (11) above.

[0026] Among these, from the viewpoints of suppressing warpage in the cured product, heat resistance, reflectivity, and the like, the carboxyl group-containing resin preferably includes at least one carboxyl group-containing photosensitive urethane resin obtained by a polyaddition reaction between a diisocyanate such as an aliphatic diisocyanate, a branched aliphatic diisocyanate, an alicyclic diisocyanate, or an aromatic diisocyanate, a carboxyl group-containing dialcohol compound such as dimethylolpropionic acid or dimethylolbutanoic acid, and a diol compound such as a polycarbonate polyol, a polyether polyol, a polyester polyol, a polyolefin polyol, an acrylic polyol, a bisphenol A alkylene oxide adduct diol, or a compound having a phenolic hydroxy group and an alcoholic hydroxy group, and which is terminated (meth)acrylated by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the urethane resin. More preferably, the carboxy group-containing resin is a carboxy group-containing urethane resin obtained by a polyaddition reaction between an aliphatic diisocyanate such as an aliphatic diisocyanate, a branched aliphatic diisocyanate, or an alicyclic diisocyanate, a carboxy group-containing dialcohol compound, and a diol compound such as a polycarbonate polyol, a polyether polyol, a polyester polyol, a polyolefin polyol, or an acrylic polyol, and may include at least one carboxy group-containing photosensitive urethane resin that has been terminally (meth)acrylated by adding a hydroxyalkyl (meth)acrylate during the synthesis of the urethane resin.

[0027] From the viewpoint of heat resistance and reflectance of the cured product, it is also preferable that the carboxyl group-containing resin contains at least one type of carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.

[0028] The acid value of the carboxyl group-containing resin may be, for example, 10 mgKOH / g or more and 150 mgKOH / g or less, preferably 30 mgKOH / g or more and 120 mgKOH / g or less. When the acid value of the carboxyl group-containing resin is 10 mgKOH / g or more, the alkaline developability of the photosensitive resin composition is improved. Furthermore, when the acid value is 150 mgKOH / g or less, it is easy to draw a good resist pattern. The acid value of the carboxyl group-containing resin is a value measured in accordance with JIS K0070:1992.

[0029] The weight-average molecular weight of the carboxyl group-containing resin may vary depending on the resin skeleton, and may generally be 2,000 to 150,000, preferably 5,000 to 100,000. A weight-average molecular weight of 2,000 or more can improve tack-free performance, resolution, etc. Furthermore, a weight-average molecular weight of 150,000 or less can improve the developability, storage stability, etc. of the photosensitive resin composition. Here, the weight-average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography.

[0030] The content of the carboxyl group-containing resin in the photosensitive thermosetting resin composition may be, for example, 5% by mass or more and 40% by mass or less, preferably 10% by mass or more and 35% by mass or less, calculated as solid content. A carboxyl group-containing resin content of 5% by mass or more can improve the coating strength. Furthermore, a carboxyl group-containing resin content of 40% by mass or less can provide an appropriate viscosity of the photosensitive resin composition, improving processability.

[0031] Photosensitive Compound The photosensitive thermosetting resin composition may further contain at least one photosensitive compound that does not have a carboxy group. Examples of the photosensitive compound include a compound having an ethylenically unsaturated bond. The photosensitive compound may also be a compound having multiple ethylenically unsaturated bonds.

[0032] Specific examples of the compound having an ethylenically unsaturated bond include the following compounds: hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; acrylamides such as N,N-dimethyl (meth)acrylamide, N-methylol (meth)acrylamide and N,N-dimethylaminopropyl (meth)acrylamide; aminoalkyl (meth)acrylates such as N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate; di(meth)acrylates derived from alkylene glycols such as ethylene glycol, polyethylene glycol, propylene glycol and polypropylene glycol; hexanediol, trimethylolpropane, pentylene glycol, ethylene glycol, propylene ... Examples of suitable polyhydric (meth)acrylates include polyhydric alcohols such as pentaerythritol, dipentaerythritol, and tris-hydroxyethyl isocyanurate, or their ethylene oxide adducts, propylene oxide adducts, or ε-caprolactone adducts; aromatic group-containing polyhydric (meth)acrylates derived from bisphenol A, bisphenol F, and ethylene oxide adducts or propylene oxide adducts of these phenols; and polyhydric (meth)acrylates derived from glycidyl ethers such as glycerin diglycidyl ether, glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate. Furthermore, examples of suitable polyhydric (meth)acrylates include, but are not limited to, melamine (meth)acrylates obtained by directly (meth)acrylating polyols such as polyether polyols, polycarbonate diols, hydroxyl-terminated polybutadienes, and polyester polyols, or by urethane (meth)acrylating them via a diisocyanate compound.

[0033] Further examples include epoxy (meth)acrylate resins obtained by reacting a polyfunctional epoxy resin such as a cresol novolac epoxy resin with (meth)acrylic acid, and epoxy urethane (meth)acrylate compounds obtained by reacting the hydroxyl groups of the epoxy (meth)acrylate resin with a half-urethane compound of a hydroxyacrylate such as pentaerythritol tri(meth)acrylate and a diisocyanate such as isophorone diisocyanate. Such epoxy (meth)acrylate resins can improve photocurability without reducing dryness to touch.

[0034] The photosensitive compound may contain at least an aromatic group-containing polyvalent (meth)acrylate derived from bisphenol A, bisphenol F, or an ethylene oxide or propylene oxide adduct of these phenols. The photosensitive resin may contain one type of photosensitive compound alone or two or more types in combination.

[0035] When the photosensitive thermosetting resin composition contains a photosensitive compound, the content of the photosensitive compound may be, for example, 5 parts by mass or more and 100 parts by mass or less, preferably 10 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the carboxy group-containing resin, calculated as solid content. When the content is 5 parts by mass or more, the photocurability is improved, and the pattern formability by alkaline development after irradiation with active energy rays tends to be further improved. Furthermore, when the content is 100 parts by mass or less, sufficient solubility in an alkaline aqueous solution after irradiation with active energy rays tends to be obtained, and the strength of the formed coating film tends to be further improved.

[0036] Photopolymerization Initiator The photosensitive thermosetting resin composition contains at least an oxime ester-based photopolymerization initiator and a titanocene-based photopolymerization initiator as the photopolymerization initiator.

[0037] Oxime ester photopolymerization initiator The oxime ester photopolymerization initiator may be any photopolymerization initiator having an O-acyloxime structure in the molecule, and may be, for example, a photopolymerization initiator containing a partial structure represented by the following formula (I):

[0038]

[0039] In the formula, R 1 represents a hydrogen atom, a phenyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 8 carbon atoms, an alkanoyl group having 2 to 20 carbon atoms, or a benzoyl group which may have a substituent. 2 represents an optionally substituted phenyl group, an optionally substituted alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkanoyl group having 2 to 20 carbon atoms, or an optionally substituted benzoyl group. 1 or R 2 Examples of the substituents in the phenyl group represented by the formula (I) include an alkyl group having 1 to 6 carbon atoms, a phenyl group, and a halogen atom. The number of substituents in the phenyl group may be 1 to 5. 1 or R 2 The alkyl group represented by R may be linear or branched and may be substituted with one or more hydroxyl groups. At least one of the methylene groups constituting the alkyl group may be substituted with an oxygen atom or a carbonyl group. 1 or R 2 Examples of the substituent in the benzoyl group represented by the formula (I) include an alkyl group having 1 to 6 carbon atoms, a phenyl group, etc. The number of substituents in the benzoyl group may be 1 to 5.

[0040] Examples of compounds that can be substituted with the partial structure represented by formula (I) include diarylsulfane, 9H-carbazole, thioxanthen-9-one, fluorene, and derivatives thereof. The partial structure represented by formula (I) may be bonded to these compounds by substituting a hydrogen atom therein, or may be bonded via a carbonyl group.

[0041] Specific examples of the oxime ester photopolymerization initiator containing the partial structure represented by formula (I) include compounds represented by the following formulas (I-1), (I-2), and (I-3).

[0042]

[0043] In formula (I-1), R 11is R in formula (I). 1 is synonymous with R 12 is R in formula (I). 2 It is synonymous with R 13 represents a hydrogen atom, a hydroxy group, a carboxy group, a hydroxyalkoxy group, a hydroxyalkoxycarbonyl group, or the like. 13 The number of carbon atoms in the hydroxyalkoxy group in the formula (I) may be 1 to 20. n represents 0 or 1.

[0044]

[0045] In formula (I-2), R 21 is R in formula (I). 1 is synonymous with R 22 and R 24 R each independently represents a phenyl group which may have a substituent, an alkyl group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 8 carbon atoms, an alkanoyl group having 2 to 20 carbon atoms, or a benzoyl group which may have a substituent. 24 Examples of the substituent on the phenyl group represented by the formula (I) include an alkyl group having 1 to 18 carbon atoms and an organic group having an acetal bond. The organic group having an acetal bond may be, for example, a (2,2-dimethyl-1,3-dioxolan-4-yl)methoxy group. R 23 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 5 to 12 carbon atoms including the substituent, a phenyl group, a benzyl group, a benzoyl group, an alkanoyl group having 2 to 12 carbon atoms, an alkoxycarbonyl group having 2 to 12 carbon atoms, or a phenoxycarbonyl group. 23 When the alkyl group constituting the alkoxycarbonyl group represented by the formula (I) has two or more carbon atoms, it may be substituted with at least one hydroxyl group, and at least one methylene group constituting the alkyl group may be substituted with an oxygen atom.

[0046]

[0047] In formula (I-3), R 31 is R in formula (I). 1 is synonymous with R 32is R in formula (I). 2 It is synonymous with R 33 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 5 to 12 carbon atoms including the substituent, or the like.

[0048] Specific examples of the oxime ester photopolymerization initiator containing the structural moiety represented by formula (I) include 1-[4-(phenylsulfanyl)phenyl]-1,2-octanedione 2-(O-benzoyloxime), 1-{4-[4-(2-hydroxyethoxy)phenylsulfanyl]phenyl}propane-1,2-dione 2-(O-acetyloxime), 2-(acetyloxyiminomethyl)thioxanthen-9-one, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime), 1-[9-ethyl-6-(2-methyl-

[0033] Examples of suitable oxime ester photopolymerization initiators include 1-[4-tetrahydrofuranylmethoxybenzoyl]-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime), 1-[9-ethyl-6-{2-methyl-4-(2,2-dimethyl-1,3-dioxolanyl)methoxybenzoyl}-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime), and 1-[4-[3-[4-[[2-(acetyloxy)ethyl]sulfonyl]-2-methylbenzoyl]-6-[1-[(acetyloxy)imino]ethyl]-9H-carbazol]-9-yl]phenyloctanone 1-(O-acetyloxime). These oxime ester photopolymerization initiators may be used alone or in combination of two or more.

[0049] Commercially available oxime ester photopolymerization initiators include ADEKA ARCLES NCI-700, ADEKA ARCLES NCI-730, ADEKA ARCLES NCI-831, and ADEKA ARCLES NCI-930; 1-4-[[4-(2-hydroxyethoxy)phenyl]thio]phenyl]-1,2-propanedione 2-(O-acetyloxime) (all manufactured by ADEKA Corporation), DFI-020, and DFI-091 (all manufactured by Daito ChemiX Co., Ltd.), CGI-325, Irgacure OXE01, and Irgacure OXE02; 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime), Irgacure OXE03, and Irgacure OXE04. OXE04 (all manufactured by BASF Japan Ltd.) and the like can also be used.

[0050] The content of the oxime ester photopolymerization initiator in the photosensitive thermosetting resin composition may be, for example, 0.01 to 10 parts by mass, preferably 0.02 to 8 parts by mass, and more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin, calculated as solid content. When the content of the oxime ester photopolymerization initiator is 0.01 parts by mass or more, sufficient photocuring can be achieved. Furthermore, when the content is 10 parts by mass or less, a good balance between surface curing and bottom curing tends to be achieved. In one embodiment, the content of the oxime ester photopolymerization initiator may be 3 parts by mass or less, 2 parts by mass or less, or 1 part by mass or less.

[0051] Titanocene Photopolymerization Initiator Examples of the titanocene photopolymerization initiator include compounds represented by the following formula (II).

[0052]

[0053] In the formula, R 9 and R 10 each independently represents a halogen atom, an aryl group, a halogenated aryl group, or a heterocycle-containing halogenated aryl group.

[0054] Examples of the titanocene photopolymerization initiator represented by formula (II) include di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1H-pyrrol-1-yl)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(3-(1H-pyrrol-1-yl)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((1H-pyrrol-1-yl)methyl)phenyl]titanium, and bis(methylcyclopentadienyl)-bis[2,6-difluoro-3-((1H-pyrro di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,5-dimethyl-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2-isopropyl-5-methyl-1H-pyrrol-1,6-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2-(2-methoxyethyl)-5-methyl-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2-(2-methoxyethyl)-5-methyl-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((3-trimethylsilyl-2,5-dimethyl-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,5-dimethyl-3-(bis(2-methoxyethyl)aminomethyl)-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,5-bis(morpholinomethyl)-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,5-bis(morpholinomethyl)-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,5-dimethyl-3-(1,3-dioxolan-2-yl)-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-4-((2,5-dimethyl-1H-pyrrol-1-yl)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-methyl-4-(2-(1H-pyrrol-1-yl)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,di(cyclopentadienyl)-bis[2,3,5,6-tetrafluoro-4-(3-(1H-pyrrol-1-yl)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1H-pyrrol-1-yl)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(1-methyl-2-(1H-pyrrol-1-yl)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(1-methyl-2-(1H-pyrrol-1-yl)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(3-(2-isoindol-2-yl)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(4,5,6,7-tetrahydro-isoindol-2-yl)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(6-(9-carbazol-9-yl)hexyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(3-(2,3,4,5,6,7,8,9-octahydro di(cyclopentadienyl)-bis[2,6-difluoro-3-(3-(4,5,6,7-tetrahydro-2-methyl-1-indol-1-yl)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((acetylamino)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(propionylamino)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(propionylamino)ethyl)phenyl]titanium Fluoro-3-(3-(acetylamino)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(4-(pivaloylamino)butyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(2,2-dimethylpentanoylamino)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(3-(benzoylamino)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(2,2-dimethyl-3-chloropropanoylamino)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((2,2-dimethyl-3-ethoxypropanoylamino)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(lauroylamino)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(N-allylmethylsulfonylamino)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(N-allylmethylsulfonylamino)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(3-(N-isobutylphenylsulfonylamino)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-((methylsulfonylamino)methyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(3-(ethylsulfonylamino)propyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(butylsulfonylamino)ethyl)phenyl]titanium, di(cyclopentadienyl)-bis[2,6-difluoro-3-(4-(trisulfonylamino)propyl)phenyl]titanium, bis(η, 5 1H-pyrrol-1-yl)phenyl)titanium, etc. These titanocene photopolymerization initiators may be used singly or in combination of two or more.

[0055] Commercially available titanocene photopolymerization initiators include JMT-784 (manufactured by Yueyang Jinmaotai Technology Co., Ltd.; di(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium), and the like.

[0056] The content of the titanocene photopolymerization initiator in the photosensitive thermosetting resin composition may be, for example, 0.01 parts by mass or more and 10 parts by mass or less, preferably 0.02 parts by mass or more and 8 parts by mass or less, and more preferably 0.05 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the carboxy group-containing resin, calculated as solid content. When the content of the titanocene photopolymerization initiator is 0.01 parts by mass or more, sufficient photocuring can be achieved. Furthermore, when the content is 10 parts by mass or less, uneven curing tends to be suppressed. In one embodiment, the content of the titanocene photopolymerization initiator may be 2 parts by mass or less, 1 part by mass or less, or 0.5 parts by mass or less.

[0057] The mass-based content ratio of the oxime ester photopolymerization initiator to the titanocene photopolymerization initiator in the photopolymerization initiator may be, for example, 1:10 to 10:1 (oxime ester photopolymerization initiator:titanocene photopolymerization initiator), preferably 1:8 to 8:1, more preferably 1:5 to 5:1, and even more preferably 1:2 to 2:1. Within the above range, a good balance between surface curability and deep curability can be achieved, enabling the formation of a good pattern.

[0058] The total content of the titanocene photopolymerization initiator and the oxime ester photopolymerization initiator in the photosensitive thermosetting resin composition may be, for example, 0.01 to 10 parts by mass, preferably 0.1 to 2 parts by mass, and more preferably 0.2 to 1 part by mass, in terms of solid content, relative to 100 parts by mass of the carboxy group-containing resin. When the total content of the titanocene photopolymerization initiator and the oxime ester photopolymerization initiator is 0.01 parts by mass or more, sufficient photocuring can be achieved. Furthermore, when it is 10 parts by mass or less, uneven curing tends to be suppressed.

[0059] The photopolymerization initiator may further include, in addition to the oxime ester-based photopolymerization initiator and the titanocene-based photopolymerization initiator, a photopolymerization initiator other than the oxime ester-based and titanocene-based photopolymerization initiators. Examples of the other photopolymerization initiator include a benzophenone-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an aminoacetophenone-based photopolymerization initiator, a benzoin ether-based photopolymerization initiator, a benzyl ketyl-based photopolymerization initiator, an oxime ether-based photopolymerization initiator, an alkylphenone-based photopolymerization initiator, and an acylphosphine oxide-based photopolymerization initiator.

[0060] When the photopolymerization initiator contains another photopolymerization initiator, the content thereof may be, for example, 80% by mass or more and 99% by mass or less, and preferably 90% by mass or less and 97% by mass or less, in terms of solid content, relative to the total mass of the photopolymerization initiator in one embodiment, and in another embodiment, for example, 10% by mass or less, preferably 1% by mass or less, and more preferably 0.1% by mass or less.

[0061] White Pigment The photosensitive thermosetting resin composition contains at least one white pigment. The inclusion of a white pigment can whiten the cured product. Examples of white pigments include zinc oxide, potassium titanate, zirconium oxide, antimony oxide, white lead, zinc sulfide, and lead titanate. From the viewpoints of reflectance and discoloration suppression, the white pigment preferably contains at least titanium oxide. Examples of titanium oxide that can be used include those produced by the sulfuric acid method, the chlorine method, rutile titanium oxide, anatase titanium oxide, and titanium oxide that has been surface-treated with a hydrous metal oxide or an organic compound. Among these titanium oxides, rutile titanium oxide is preferred from the viewpoint of photocatalytic activity. The use of rutile titanium oxide allows for the production of a more stable cured product (e.g., a solder resist film). Specific examples of rutile titanium oxide include TR-600, TR-700, TR-750, and TR-840 (all manufactured by Fuji Titanium Kogyo Co., Ltd.), R-550, R-580, R-630, R-820, CR-50, CR-60, and CR-90 (all manufactured by Ishihara Sangyo Kaisha, Ltd.), and KR-270, KR-310, and KR-380 (all manufactured by Titanium Kogyo Co., Ltd.). Among these rutile titanium oxides, titanium oxide whose surface is treated with hydrous alumina or aluminum hydroxide is particularly preferred from the viewpoints of dispersibility in the composition, storage stability, and flame retardancy. The white pigment may be used alone or in combination of two or more.

[0062] The volume average particle size of the white pigment may be, for example, 10 nm to 5 μm, and preferably 100 nm to 1 μm. The volume average particle size of the white pigment is measured as the particle size corresponding to 50% of the cumulative volume from the smallest diameter side in a volume-based cumulative particle size distribution measured, for example, using a laser diffraction particle size distribution analyzer.

[0063] The whiteness of the white pigment may be, for example, 80 or more, and preferably 85 or more. The whiteness is measured, for example, using a spectrophotometer (such as PF10 manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS P8148:2018 "Method for measuring ISO whiteness (diffuse blue light reflectance)."

[0064] The content of the white pigment in the photosensitive thermosetting resin composition may be, for example, 200 parts by mass or more and 1000 parts by mass or less, and preferably 250 parts by mass or more and 800 parts by mass or less, relative to 100 parts by mass of the carboxy group-containing resin, calculated as solid content. When the content of the white pigment is 200 parts by mass or more, sufficient reflectance can be achieved in the cured product. Furthermore, when the content is 1000 parts by mass or less, an increase in viscosity of the composition can be suppressed, and the coating and moldability are good, and the brittleness of the cured product tends to be suppressed.

[0065] Thermosetting Resin The photosensitive thermosetting resin composition contains at least one thermosetting resin. Examples of thermosetting resins that can be used include known and commonly used isocyanate compounds, blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy resins, polyfunctional oxetane compounds, and episulfide resins. Among these, it is preferable for the thermosetting resin to have at least one of a plurality of cyclic ether groups and a cyclic thioether group (hereinafter referred to as cyclic (thio)ether groups) in one molecule. Many types of thermosetting components having these cyclic (thio)ether groups are commercially available, and their structure can impart a variety of properties.

[0066] The thermosetting resin having a plurality of cyclic (thio)ether groups in the molecule is a compound having a plurality of at least one type of group, which is a 3-, 4-, or 5-membered cyclic ether group or a cyclic thioether group, in the molecule. Examples of such a thermosetting resin include a compound having a plurality of epoxy groups in the molecule, i.e., a polyfunctional epoxy compound; a compound having a plurality of oxetanyl groups in the molecule, i.e., a polyfunctional oxetane compound; and a compound having a plurality of thioether groups in the molecule, i.e., an episulfide compound.

[0067] Specific examples of polyfunctional epoxy compounds include bisphenol A epoxy resins, hydrogenated bisphenol A epoxy resins, brominated bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, novolac epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, N-glycidyl epoxy resins, bisphenol A novolac epoxy resins, bixylenol epoxy resins, biphenol epoxy resins, chelate epoxy resins, glyoxal epoxy resins, amino group-containing epoxy resins, rubber-modified epoxy resins, dicyclopentadiene phenolic epoxy resins, diglycidyl phthalate resins, heterocyclic epoxy resins, tetraglycidyl xylenoylethane resins, silicone-modified epoxy resins, and ε-caprolactone-modified epoxy resins. Polyfunctional epoxy resins may also be used that incorporate halogen atoms such as chlorine and bromine, or atoms such as phosphorus, into their structures. This can, for example, impart flame retardancy. The polyfunctional epoxy resins may be used alone or in combination of two or more.

[0068] Examples of the polyfunctional oxetane compound include polyfunctional oxetanes such as bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, (3-ethyl-3-oxetanyl)methyl acrylate, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and oligomers or copolymers thereof, as well as ethers of oxetane alcohols with novolak resins, poly(p-hydroxystyrene), cardo-type bisphenols, calixarenes, calixresorcinarenes, or resins having a hydroxyl group such as silsesquioxane. Other examples include copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates.

[0069] An example of the episulfide resin is YL7000 (bisphenol A episulfide resin) manufactured by Mitsubishi Chemical Corporation. Furthermore, using a similar synthesis method, an episulfide resin in which the oxygen atom of the epoxy group of a novolac epoxy resin is replaced with a sulfur atom can also be used.

[0070] The content of the thermosetting resin in the photosensitive thermosetting resin composition may be, for example, 10 parts by mass or more and 100 parts by mass or less, and preferably 20 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the carboxyl group-containing resin, calculated as solid content. When the content of the thermosetting resin is within the above range, the cured product of the photosensitive resin composition has good solder heat resistance, and also tends to have good properties, particularly electrical insulation, when used as an insulating protective film for a printed wiring board.

[0071] The photosensitive thermosetting resin composition may contain a thermosetting catalyst in addition to the thermosetting resin. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. Commercially available examples include 2MZ-A, 2MA-OK, 2PHZ-PW, and 2P4BHZ-PW (all manufactured by Shikoku Chemicals Corporation; all are trade names of imidazole-based compounds), and DBU, DBN, U-CATSA102, and U-CAT5002 (all manufactured by San-Apro Co., Ltd.; all are bicyclic amidine compounds and salts thereof).The curing catalyst is not particularly limited to these, and any curing catalyst that promotes the reaction of an epoxy resin, an oxetane compound, or at least one of an epoxy group and an oxetanyl group with a carboxy group may be used. Also usable are S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct. The single thermal curing catalyst may be used alone or in combination of two or more.

[0072] When the photosensitive thermosetting resin composition contains a thermosetting catalyst, the amount of the thermosetting catalyst may be, for example, 0.1 parts by mass or more and 20 parts by mass or less, and preferably 0.5 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the thermosetting resin, in terms of solid content.

[0073] The photosensitive thermosetting resin composition may further contain at least one filler selected from the group consisting of inorganic fillers and organic fillers, as needed, for the purpose of improving properties such as adhesion, hardness, and heat resistance. Examples of inorganic fillers include barium sulfate, calcium carbonate, silicon oxide, amorphous silica, talc, clay, hydrotalcite, and mica powder. Examples of organic fillers include silicon powder, nylon powder, and fluorine powder. Among the above fillers, silica is particularly excellent in terms of low moisture absorption and low volume expansion. Silica may be fused or crystalline, or a mixture thereof. However, silica surface-treated with a coupling agent or the like is particularly preferred, as it can improve electrical insulation. The average particle size of the filler is desirably 25 μm or less, more desirably 10 μm or less, and even more desirably 3 μm or less. When the photosensitive thermosetting resin composition contains a filler, the content of the filler may be, for example, 150 parts by mass or less, and preferably 50 parts by mass or less, per 100 parts by mass of the carboxyl group-containing resin, calculated as solid content. When the content of the filler is in this range, the folding resistance of the cured film is good.

[0074] The photosensitive thermosetting resin composition may contain additives other than the above components. Examples of additives include thickeners such as organic bentonite and montmorillonite, at least one of silicone-based, fluorine-based, and polymer-based antifoaming agents and leveling agents, and fiber reinforcements such as glass fiber, carbon fiber, and boron nitride fiber. Furthermore, if necessary, adhesion promoters, thermal polymerization inhibitors, peroxide decomposers, UV absorbers, thiazole-based, triazole-based, and other silane coupling agents, dispersants, antifoaming agents, plasticizers, foaming agents, flame retardants, antistatic agents, antioxidants, antibacterial and antifungal agents, and the like may be added.

[0075] The photosensitive thermosetting resin composition may further contain at least one of a radical scavenger and a peroxide decomposer, as needed. This can suppress functional degradation in the cured product. The radical scavenger and the peroxide decomposer may be so-called antioxidants.

[0076] Examples of radical scavengers include phenolic compounds such as hydroquinone, 4-t-butylcatechol, 2-t-butylhydroquinone, hydroquinone monomethyl ether, 2,6-di-t-butyl-p-cresol, 2,2-methylene-bis(4-methyl-6-t-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, and 1,3,5-tris(3',5'-di-t-butyl-4-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione; quinone compounds such as methaquinone and benzoquinone; and amine compounds such as bis(2,2,6,6-tetramethyl-4-piperidyl)-sebacate and phenothiazine.

[0077] The radical scavenger may be a commercially available product, and examples thereof include ADK STAB (registered trademark) AO-30, ADK STAB AO-330, ADK STAB AO-20, ADK STAB LA-77, ADK STAB LA-57, ADK STAB LA-67, ADK STAB LA-68, and ADK STAB LA-87 (all manufactured by ADEKA CORPORATION), Irganox (registered trademark) 1010, Irganox 1035, Irganox 1076, Irganox 1135, Tinuvin (registered trademark) 111FDL, Tinuvin 123, Tinuvin 144, Tinuvin 152, Tinuvin 292, and Tinuvin 5100 (all manufactured by BASF Japan Ltd.).

[0078] The ultraviolet absorber may be a commercially available product, and examples thereof include Tinuvin PS, Tinuvin 99-2, Tinuvin 109, Tinuvin 384-2, Tinuvin 900, Tinuvin 928, Tinuvin 1130, Tinuvin 400, Tinuvin 405, Tinuvin 460, and Tinuvin 479 (all manufactured by BASF Japan Ltd.).

[0079] The photosensitive thermosetting resin composition may further contain an organic solvent. By containing an organic solvent, each component can be easily dissolved or dispersed. In addition, the viscosity can be easily adjusted to a value suitable for the application method, such as coating. Examples of organic solvents include aromatic solvents such as toluene, xylene, ethylbenzene, and nitrobenzene; aliphatic hydrocarbon solvents such as cyclohexane; ether solvents such as diethylene glycol dimethyl ether and ethylene glycol diethyl ether; ester solvents such as carbitol acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, dipropylene glycol methyl ether acetate, methyl methoxypropionate, ethyl methoxypropionate, methyl ethoxypropionate, ethyl ethoxypropionate, ethyl ethylpropionate, ethyl acetate, n-butyl acetate, isoamyl acetate, ethyl lactate, and γ-butyrolactone; ketone solvents such as acetone, methyl ethyl ketone, cyclohexanone, and isophorone; amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; and halogenated hydrocarbon solvents such as chloroform and methylene chloride. The organic solvent may be used alone or in combination of two or more. The content of the organic solvent may be appropriately determined depending on the desired viscosity, etc.

[0080] The photosensitive thermosetting resin composition can be obtained by dissolving or dispersing the above-mentioned components using a mixer such as a disper, kneader, three-roll mill, or bead mill.

[0081] In one embodiment, the photosensitive thermosetting resin composition includes a photosensitive resin, a photopolymerization initiator, a white pigment, and an epoxy resin, wherein the photosensitive resin includes a carboxyl group-containing resin, and the photopolymerization initiator includes an oxime ester photopolymerization initiator and a titanocene photopolymerization initiator, and the mass ratio of the white pigment content to the photosensitive resin content may be 1.2 to 5, and the mass ratio of the total content of the oxime ester photopolymerization initiator and the titanocene photopolymerization initiator to the white pigment content may be 0.0004 to 0.002. By having the white pigment content within the above ranges and the photopolymerization initiator content within the above ranges, excellent whiteness and high reflectance at a wavelength of 450 nm can be achieved.

[0082] Cured Product The cured product of the photosensitive thermosetting resin composition can exhibit high whiteness and excellent reflectance at a wavelength of 450 nm. The cured product of the photosensitive thermosetting resin composition can be obtained, for example, under the following curing conditions.

[0083] Curing conditions: The photosensitive thermosetting resin composition is applied to a substrate so that the film thickness after thermal curing is 55 μm, and then dried at 80° C. for 30 minutes. 2 and developed (30°C, 0.2 MPa, 1 mass % Na 2 CO 3 Aqueous solution) is applied for 60 seconds, and then thermally cured at 150°C for 60 minutes to obtain a cured product.

[0084] The cured product after thermal curing of the photosensitive thermosetting resin composition is L * a * b * b in the color system * The value is 2.0 or less. * The value may be preferably 1.8 or less, more preferably 1.5 or less. * a * b * b in the color system * The b value is measured for a cured product having a thickness of 55 μm produced under the above-mentioned production conditions using a spectrophotometer (manufactured by Konica Minolta, Inc., model number: CM-5). *When the value is within the above range, yellowing due to heating tends to be suppressed.

[0085] The cured product also has a reflectance of 85% or more at a wavelength of 450 nm. The reflectance at a wavelength of 450 nm may preferably be 88% or more. The reflectance at a wavelength of 450 nm is measured using a spectrophotometer (manufactured by Konica Minolta, Inc., model number: CM-5) with an SCI method and a measuring diameter of 8 mm for a cured product having a thickness of 55 μm produced under the curing conditions described above. When the reflectance of the cured product is within the above range, the light extraction efficiency of the display improves, and reflected light tends to be more effectively utilized.

[0086] The cured product formed from the photosensitive thermosetting resin composition exhibits excellent heat resistance and can maintain whiteness and reflectance. Specifically, for example, after a single heat treatment (reflow process) at a maximum temperature of 260° C. for 10 seconds, the ΔEab * may be, for example, 2.0 or less, and preferably 1.0 or less. * is the L before heat treatment * , a * and b * and L after heat treatment * , a * and b * The difference between * , Δa * and Δb * ΔEab is a value calculated by the following formula (1) using the above formula, and is an index showing the degree of discoloration. * = ((ΔL * ) 2 + (Δa * ) 2 + (Δb * ) 2 ) (1/2) ...(1)

[0087] The decrease in reflectance at a wavelength of 450 nm may be, for example, 5% or less, and preferably 2% or less, where the decrease in reflectance is calculated by subtracting the reflectance (%) measured for the cured product after the heat treatment from the reflectance (%) measured for the cured product before the heat treatment.

[0088] The photosensitive thermosetting resin composition can be applied to a printed circuit board by a method selected from commonly used application methods to form a resin composition layer. It can also be used in various forms and applications, such as dry films and prepregs. Various solvents can be used depending on the application method and application, and in some cases, not only good solvents but also poor solvents can be used.

[0089] The photosensitive thermosetting resin composition can be adjusted to a viscosity suitable for the application method using, for example, the organic solvent, applied to a substrate, and then evaporated and dried (pre-dried) at a temperature of about 60°C to 100°C to remove the organic solvent contained in the composition. A tack-free resin composition layer can be formed. Examples of application methods include dip coating, flow coating, roll coating, bar coating, screen printing, curtain coating, and spray coating. Alternatively, the photosensitive thermosetting resin composition can be applied to a carrier film, dried, and wound up as a film, which is then laminated onto a substrate to form a resin composition layer. Subsequently, the photosensitive thermosetting resin composition is selectively exposed to active energy rays through a patterned photomask using a contact (or non-contact) method, or directly exposed to a pattern using a laser direct exposure device. The unexposed areas are developed with a dilute alkaline aqueous solution (e.g., a 0.3% to 3% by weight sodium carbonate aqueous solution) to form a resist pattern (pattern image). The exposure conditions are as follows: Furthermore, by heating to a temperature of, for example, about 140°C to 180°C to cause thermal curing, the carboxy groups (or further the phenolic hydroxy groups) of the carboxy group-containing resin react with the cyclic (thio)ether groups of the thermosetting resin, forming a white cured coating that not only exhibits properties such as adhesion to the substrate, folding resistance, low warpage, resistance to electroless gold plating, solder heat resistance, and electrical insulation, but also achieves a high level of flexibility and high reflectance in a well-balanced manner, and that suppresses deterioration in reflectance and whiteness over time.

[0090] Examples of substrates that can be used include printed wiring boards, flexible printed wiring boards, paper-phenolic resin, paper-epoxy resin, glass cloth-epoxy resin, glass-polyimide, glass cloth / nonwoven cloth-epoxy resin, glass cloth / paper-epoxy resin, synthetic fiber-epoxy resin, copper-clad laminates of all grades (such as FR-4) using composite materials such as fluororesin, polyethylene, PPO, and cyanate ester, polyimide films, PET films, glass substrates, ceramic substrates, and wafer plates. Circuits may be formed on the above-mentioned substrates, and configurations such as transistors may also be formed and mounted on them.

[0091] The volatilization drying carried out after the application of the photosensitive resin composition can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which hot air in a dryer equipped with a heat source of an air heating type using steam is brought into countercurrent contact with the support, or a method in which hot air is blown onto the support from a nozzle).

[0092] A photosensitive resin composition is applied to a substrate, and after volatilization and drying, the resulting resin composition layer is exposed to light (irradiated with active energy rays). The exposed portions of the resin composition layer (portions irradiated with active energy rays) are cured.

[0093] Examples of exposure devices used for the above-mentioned active energy ray irradiation include direct imaging devices (for example, laser direct imaging devices that directly draw images with a laser based on CAD data from a computer), exposure devices equipped with a metal halide lamp, exposure devices equipped with a (ultra) high-pressure mercury lamp, exposure devices equipped with a mercury short arc lamp, and direct imaging devices using an ultraviolet lamp such as a (ultra) high-pressure mercury lamp. The active energy ray may be a laser beam having a maximum wavelength in the range of 350 nm to 450 nm. The active energy ray can be irradiated using, for example, a gas laser, a solid-state laser, etc. The exposure dose may be selected appropriately depending on the film thickness, etc., and is generally 5 mJ / cm. 2 to 800 mJ / cm 2 , preferably 5 mJ / cm 2 to 500 mJ / cm 2As the direct imaging device, for example, a device manufactured by Orbotech Japan Co., Ltd. may be used, and any device may be used as long as it emits laser light with a maximum wavelength of 350 nm to 450 nm.

[0094] Examples of the developing method include dipping, showering, spraying, brushing, etc. As the developer, an aqueous alkali solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, or amines can be used.

[0095] The photosensitive thermosetting resin composition can be used not only by directly applying it to a substrate in liquid form, but also in the form of a dry film having a resin composition layer formed by applying the photosensitive thermosetting resin composition to a film such as polyethylene terephthalate and drying it in advance. An example of using the photosensitive resin composition as a dry film is shown below.

[0096] Dry Film The dry film has a resin composition layer obtained by applying the above-mentioned photosensitive thermosetting resin composition to a film and drying it. The dry film may have a structure in which a first film, a resin composition layer, and an optional peelable second film are laminated in this order. The resin composition layer is, for example, a layer obtained by applying and drying the photosensitive thermosetting resin composition to the first film or the second film. A dry film can be obtained by forming a resin composition layer on the first film and then laminating a second film thereon, or by forming a resin composition layer on the second film and laminating the resulting laminate on the first film.

[0097] The first film is a thermoplastic film such as a polyester film having a thickness of 2 μm to 150 μm. The resin composition layer is formed by uniformly applying a photosensitive thermosetting resin composition to the first film or the second film to a thickness of 10 μm to 150 μm using a blade coater, lip coater, comma coater, film coater, or the like, and then drying the applied composition. The second film can be a polyethylene film, a polypropylene film, or the like, but preferably has a lower adhesive strength with the resin composition layer than the first film.

[0098] To prepare a protective film (permanent protective film) on a substrate using a dry film, the second film is peeled off, and the resin composition layer and the substrate on which a circuit is formed are superimposed and laminated using a laminator or the like to form a resin composition layer on the substrate on which a circuit is formed. The formed resin composition layer can be exposed, developed, and heat-cured in the same manner as above to form a cured coating film. The first film can be peeled off either before or after exposure.

[0099] Electronic Components The electronic components include a cured product of the above-mentioned photosensitive thermosetting resin composition. Examples of electronic components include printed wiring boards and light source modules. The printed wiring board comprises a substrate having a pattern conductor and a cured product of the photosensitive thermosetting resin composition disposed on the substrate. The cured product disposed on the substrate may be patterned into a desired shape. The light source module comprises a printed wiring board and a semiconductor light-emitting element disposed on the printed wiring board and connected to the pattern conductor. In the light source module, the semiconductor light-emitting element may be coated with a cured resin layer. The cured resin layer coating the semiconductor light-emitting element may contain, for example, a silicone resin.

[0100] Other aspects of the present invention include the use of the photosensitive thermosetting resin composition in the production of a dry film or an electronic component, and the photosensitive thermosetting resin composition used in the production of a dry film or an electronic component.

[0101] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0102] The following materials were prepared for preparing a photosensitive thermosetting resin composition. Carboxy group-containing resin (Synthesis Example 1) Varnish A-1 2,400 g (3 mol) of a polycarbonate diol derived from 1,5-pentanediol and 1,6-hexanediol (TJ5650J, number average molecular weight 800, manufactured by Asahi Kasei Corporation), 603 g (4.5 mol) of dimethylolpropionic acid, and 238 g (2.6 mol) of 2-hydroxyethyl acrylate as a monohydroxy compound were added to a reaction vessel equipped with a stirrer, a thermometer, and a condenser. Next, 1,887 g (8.5 mol) of isophorone diisocyanate as a polyisocyanate was added, and the mixture was heated to 60°C with stirring and stopped. When the temperature inside the reaction vessel began to decrease, the mixture was heated again and continued stirring at 80°C. The absorption spectrum of the isocyanate group (2,280 cm) was measured by infrared absorption spectroscopy. -1 The reaction was terminated after confirming that the saturation gas had disappeared. Carbitol acetate was added so that the solid content was 50% by mass, and Varnish A-1 was obtained. The solid had an acid value of 50 mgKOH / g and a weight-average molecular weight Mw of approximately 17,000.

[0103] Synthesis Example 2 Varnish A-2 220 g of cresol novolac epoxy resin (EPICLON N-695, manufactured by DIC Corporation, epoxy equivalent: 220 g / eq.) was placed in a four-neck flask equipped with a stirrer and a reflux condenser, and 214 g of carbitol acetate was added and dissolved by heating. Next, 0.1 g of hydroquinone as a polymerization inhibitor and 2.0 g of dimethylbenzylamine as a reaction catalyst were added. This mixture was heated to 95 to 105°C, and 72 g of acrylic acid was slowly added dropwise, followed by a 16-hour reaction. The reaction product was cooled to 80 to 90°C, and 106 g of tetrahydrophthalic anhydride was added. The reaction was continued for 8 hours, cooled, and then discharged. The carboxyl group-containing resin varnish A-2 thus obtained had a solids content of 65%, an acid value of the solids of 100 mgKOH / g, and a weight-average molecular weight Mw of approximately 3,500.

[0104] Photosensitive compound BPE-900: manufactured by Shin-Nakamura Chemical Co., Ltd.; ethoxylated bisphenol A dimethacrylate

[0105] Photopolymerization initiators: Oxime esters: ADEKA ARCLES NCI-930: manufactured by ADEKA Corporation; 1-4-[[4-(2-hydroxyethoxy)phenyl]thio]phenyl]-1,2-propanedione 2-(O-acetyloxime); ADEKA ARCLES NCI-730: manufactured by ADEKA Corporation; Irgacure OXE04: manufactured by BASF Japan Ltd.; Irgacure OXE02: manufactured by BASF Japan Ltd.; 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime).

[0106] Titanocene series JMT-784: Manufactured by Yueyang Jin Maotai Technology Co., Ltd.; Screw (η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium)

[0107] Alkylphenone Omnirad 184: manufactured by IGM Japan LLC; 1-hydroxycyclohexyl phenyl ketone

[0108] α-Aminoacetophenones Omnirad 379: manufactured by IGM Japan LLC; 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one Omnirad 907: manufactured by IGM Japan LLC; 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one

[0109] White pigment CR-90: manufactured by Ishihara Sangyo Kaisha; rutile-type titanium dioxide

[0110] Thermosetting resin jER834: manufactured by Mitsubishi Chemical Corporation; bisphenol A type epoxy resin, epoxy equivalent 250 g / eq

[0111] Heat curing catalyst DICY7: manufactured by Mitsubishi Chemical Corporation; dicyandiamide Wetting and dispersing agent Disperbyk-111: manufactured by BYK Japan Co., Ltd. Defoaming agent KS-66: manufactured by Shin-Etsu Chemical Co., Ltd.; silicone-based oil compound type defoaming agent

[0112] Preparation of Photosensitive Resin Compositions Using each of the obtained varnishes A-1 and A-2, the various components shown in Table 1 were blended in the indicated proportions (parts by mass), premixed in a stirrer, and then kneaded in a three-roll mill to prepare the photosensitive thermosetting resin compositions of Examples 1 to 13 and Comparative Examples 1 to 5. Values ​​in the tables are parts by mass unless otherwise specified. In Tables 1 and 2, "-" indicates that the component was not added or was not evaluated (because evaluation was not possible).

[0113] The photosensitive thermosetting resin compositions of Examples 1 to 13 and Comparative Examples 1 to 5 obtained in this manner were evaluated as follows. The results are shown in Tables 1 and 2.

[0114] Preparation of Evaluation Substrates The photosensitive thermosetting resin compositions of Examples 1 to 13 and Comparative Examples 1 to 5 were screen printed twice on a copper solid substrate to form a coating film with a total film thickness of 55 μm after thermal curing. Specifically, the composition was applied to the entire surface of the copper solid substrate by screen printing and dried for 10 minutes in a hot air circulation drying oven at 80°C to form a first layer, and the first layer was further applied to the entire surface by screen printing and dried for 20 minutes in a hot air circulation drying oven at 80°C to form a second layer. The formed coating film was exposed to an optimal exposure dose using an exposure device (Mms60: manufactured by Oak Manufacturing Co., Ltd.) equipped with a high-pressure mercury lamp, and developed (30°C, 0.2 MPa, 1 mass% Na 2 CO 3 Aqueous solution) was applied for 60 seconds. Thereafter, the resulting solution was thermally cured in a hot air circulation drying oven at 150°C for 60 minutes to form a resin layer, and a substrate for evaluation was prepared. The optimal exposure dose was determined by exposing the dried coating film to light through a Stouffer 41-step tablet using an exposure device (Mms60: manufactured by Oak Manufacturing Co., Ltd.) equipped with a high-pressure mercury lamp, and by spraying a 1% by mass Na solution at a spray pressure of 0.2 MPa and a liquid temperature of 30°C. 2 CO 3 The exposure dose was set so that the remaining step tablet pattern had 15 to 20 steps when developed with an aqueous solution for 60 seconds.

[0115] Evaluation of surface curability The exposure amount was changed from "optimum exposure amount" to "400 mJ / cm 2" was prepared in the same manner as in the preparation of the evaluation substrate, except that " after development and before thermal curing " was used, and the surface of the substrate was visually observed. The evaluation criteria for surface curability were as follows: a: The surface was not rough and was in good condition. b: Roughness was observed in part of the surface. c: Roughness was observed on the entire surface.

[0116] Evaluation of reflectance The reflectance at 450 nm and b of the resin layer formed on each evaluation substrate obtained by the above-mentioned evaluation substrate production were measured. * was measured using a spectrophotometer (manufactured by Konica Minolta, Inc., model number: CM-5) with a measuring diameter of 8 mm using the SCI method. The measurement results are shown in Table 1 under "Reflectance" and b * is shown in the row.

[0117] The evaluation substrate was subjected to a reflow process once using a reflow machine (NIS-20-82C manufactured by Atec Techtron Co., Ltd.) at a maximum temperature of 260°C for 10 seconds. Thereafter, the reflectance and b * The measurement results were recorded as reflectance after heat resistance test and b * The values ​​are shown in Table 1.

[0118] ΔEab * Evaluation of ΔEab * is the L before reflow * , a * , b * and L after reflow * , a * , b * The value was measured using a spectrophotometer (manufactured by Konica Minolta, Inc., model number: CM-5). The calculation results are shown in ΔEab in Table 1. * ΔEab * = ((ΔL * ) 2 + (Δa * ) 2 + (Δb * ) 2 ) (1/2) ...(1)

[0119] Evaluation of solder heat resistance A rosin-based flux was applied to each evaluation board obtained above, and the board was immersed in a solder bath previously set to 260°C for 10 seconds. Next, the flux was washed off with denatured alcohol, and the resin layer was visually evaluated for swelling and peeling. The heat resistance evaluation criteria were as follows: a: No swelling or peeling of the resin layer after immersion for 10 seconds. b: No swelling or peeling of the resin layer after immersion for 5 seconds. c: Clear swelling and peeling of the resin layer after immersion for 5 seconds.

[0120] Evaluation of deep curing (undercut) The photosensitive thermosetting resin compositions of Examples 1 to 13 and Comparative Examples 1 to 5 were screen printed twice on a copper solid substrate to form a coating film with a total film thickness of 55 μm after thermal curing. Specifically, the coating was applied to the entire surface of the copper solid substrate by screen printing and dried for 10 minutes in a hot air circulation drying oven at 80°C to form a first layer, and the first layer was further screen printed on the entire surface and dried for 20 minutes in a hot air circulation drying oven at 80°C to form a second layer. The formed coating film was exposed to 400 mJ / cm using an exposure device equipped with a high-pressure mercury lamp (Mms60: manufactured by Oak Manufacturing Co., Ltd.). 2 and developed (30°C, 0.2 MPa, 1 mass % Na 2 CO 3 The cross section of the opening of the pattern obtained was observed, and the lengths of the upper part (air side) and lower part (substrate side) were measured. The undercut was calculated using the following formula to evaluate the deep curing property: Undercut = (upper length - lower length) / 2

[0121]

[0122]

[0123] As described above, it can be seen that the present invention can provide a photosensitive resin composition that is less likely to discolor after a heating step and can maintain a high reflectance. In particular, Examples 2 and 4, which contain a small amount of oxime ester photopolymerization initiator and titanocene photopolymerization initiator and a larger amount of white pigment than Example 3, have high reflectance, but b *This is thought to be due to the synergistic effect of the oxime ester photopolymerization initiator and the titanocene photopolymerization initiator, which allows the desired properties to be achieved even with a small amount of initiator.

[0124] In Comparative Example 1, a coating film was formed, but a pattern strong enough to evaluate undercutting was not left after development, so deep curing properties could not be evaluated. In Comparative Example 2, a coating film could not be formed, so all evaluation items could not be evaluated. In Comparative Examples 4 and 5, a resin layer could not be formed at the exposure dose used to evaluate surface curing properties and deep curing properties, so evaluation was not possible.

[0125] The disclosure of Japanese Patent Application No. 2023-055267 (filing date: March 30, 2023) is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A photosensitive thermosetting resin composition comprising a carboxyl group-containing resin, a photopolymerization initiator, a white pigment, and a thermosetting resin, wherein the photopolymerization initiator comprises an oxime ester-based photopolymerization initiator and a titanocene-based photopolymerization initiator, the thermosetting resin comprises an epoxy resin, and the photosensitive thermosetting resin composition is thermally cured to have a cured product having a L * a * b * b in color system * The photosensitive thermosetting resin composition has a reflectance of 85% or more at a wavelength of 450 nm.

2. The photosensitive thermosetting resin composition according to claim 1, wherein the photopolymerization initiator is an oxime ester-based photopolymerization initiator and a titanocene-based photopolymerization initiator in a mass ratio within the range of 1:10 to 10:

1.

3. A dry film having a resin layer obtained by applying the photosensitive thermosetting resin composition according to claim 1 or 2 to a first film and drying it.

4. A cured product obtained by curing the photosensitive thermosetting resin composition according to claim 1 or 2.

5. An electronic part comprising the cured product according to claim 4.

Citation Information

Patent Citations

  • Photosetting and thermosetting solder resist composition, and printed wiring board using the same

    JP2007322546A

  • Curable resin composition, dry film, cured product, and printed wiring board

    JP2016035042A

  • Negative-type photosensitive white composition for touch panel, touch panel, and production method for touch panel

    WO2015012228A1