Thermoelectric conversion module

By integrating thermally conductive interface members with specific properties and high thermal conductivity layers, the thermoelectric performance and reliability of in-plane thermoelectric conversion modules are enhanced, addressing thermal resistance and shear stress challenges.

WO2024204850A1PCT designated stage expired Publication Date: 2024-10-03LINTEC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013524
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-04-01
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In-plane thermoelectric conversion modules face challenges in improving thermoelectric performance, reducing thickness, and enhancing reliability, with existing insulating layers not adequately addressing thermal resistance and shear stress issues at interfaces.

Method used

Incorporating thermally conductive interface members with specific thermal resistance ratios and adhesive properties on both surfaces of the module, along with high thermal conductivity layers, to enhance heat conductivity and adhesion, thereby improving thermoelectric performance.

Benefits of technology

The solution significantly improves heat conductivity at interfaces, leading to higher thermoelectric performance and reliability by optimizing thermal resistance and adhesive properties within the module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013524_03102024_PF_FP_ABST
    Figure JP2024013524_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a thermoelectric conversion module having high thermoelectric performance in which the heat conductivity of the interface between members is improved. The thermoelectric conversion module comprises: a thermally conductive interface member A and a heat-dissipating member on one surface of an in-plane thermoelectric conversion module; and a thermally conductive interface member B on the other surface of the in-plane thermoelectric conversion module. When the thermal resistance value of the thermally conductive interface member A is RA (mK / W), the thermal resistance value of the thermally conductive interface member B is RB (mK / W), and the total thermal resistance value that is the sum thereof is RAB (mK / W), and when the total thermal resistance value of the in-plane thermoelectric conversion module is RM (mK / W), the ratio of the RAB to the RM, i.e., (RAB / RM), is 1.40 or less.
Need to check novelty before this filing date? Find Prior Art

Description

thermoelectric conversion module

[0001] The present invention relates to a thermoelectric conversion module.

[0002] Conventionally, as one of the means for effectively utilizing energy, there has been a device that directly converts thermal energy into electrical energy and vice versa using a thermoelectric conversion module having a thermoelectric effect such as the Seebeck effect or the Peltier effect. As a thermoelectric conversion module, a so-called in-plane type thermoelectric conversion element configuration is known. From the viewpoint of thermoelectric performance, an in-plane type thermoelectric conversion element is typically configured by alternately arranging P-type thermoelectric elements and N-type thermoelectric elements in the in-plane direction of a substrate, for example, by connecting the upper or lower portions of adjacent or abutting P-type and N-type thermoelectric elements in series via electrodes. Under these circumstances, various demands remain for in-plane type thermoelectric conversion modules, such as further improvement in thermoelectric performance, thinner design, improved reliability, and improved mass productivity. For example, in Patent Document 1, an insulating layer is provided between a thermoelectric element layer and a heat dissipation layer in the configuration of an in-plane type thermoelectric conversion module.

[0003] International Publication No. 2018 / 179544

[0004] However, in Patent Document 1, the insulating layer is used for the purpose of preventing short circuits, such as between a heat source and a thermoelectric element layer or between a heat dissipation layer and a thermoelectric element layer, from the viewpoint of improving the reliability of the in-plane thermoelectric conversion module. However, Patent Document 1 does not consider the placement of another specific insulating layer on the in-plane thermoelectric conversion module from the viewpoint of improving thermoelectric performance, or the relationship between the thermal resistance of the other specific insulating layer and the thermal resistance of the components constituting the in-plane thermoelectric conversion module. Furthermore, Patent Document 1 does not consider the placement of another specific insulating layer on the in-plane thermoelectric conversion module from the viewpoint of improving thermoelectric performance, or the effects resulting from the shear stress and adhesive strength of the other specific insulating layer. Furthermore, Patent Document 1 does not consider the placement of another specific insulating layer on the in-plane thermoelectric conversion module or the π-type thermoelectric conversion module from the viewpoint of improving thermoelectric performance, or the relationship between the thermal resistance of the other specific insulating layer and the thermal resistance of the components constituting the in-plane thermoelectric conversion module or the π-type thermoelectric conversion module. In addition, the effects and advantages resulting from the shear stress and adhesive strength of the other specific insulating layer are not considered.

[0005] In view of the above, an object of the present invention is to provide a thermoelectric conversion module having high thermoelectric performance with improved heat conductivity at the interfaces between members.

[0006] As a result of extensive research to solve the above problems, the present inventors have found that providing a thermally conductive interface member (hereinafter, sometimes simply referred to as "TIM") having a thermal resistance value at a specific ratio to a total thermal resistance value, which is the sum of the thermal resistance values ​​of the components constituting the in-plane thermoelectric conversion module, on the top and bottom surfaces of the in-plane thermoelectric conversion module, can further improve the heat transfer at the interface between the components constituting the in-plane thermoelectric conversion module, and have completed the invention according to a first embodiment of the present invention. That is, the invention according to the first embodiment of the present invention provides the following [1] to [5]. [1] A thermoelectric conversion module comprising a thermally conductive interface member A and a heat dissipation member on one surface of the in-plane thermoelectric conversion module, and further comprising a thermally conductive interface member B on the other surface of the in-plane thermoelectric conversion module, wherein the thermal resistance value of the thermally conductive interface member A is set to R A (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is R AB (mK / W), and the total thermal resistance of the in-plane thermoelectric conversion module is R M (mK / W), the R M The R AB The ratio (R AB / R M) is 1.40 or less. [2] The thermoelectric conversion module according to [1] above, wherein the in-plane type thermoelectric conversion module further includes a high thermal conductivity layer A and a high thermal conductivity layer B, the high thermal conductivity layer A constituting the outermost layer of the in-plane type thermoelectric conversion module on the thermally conductive interface member A side, and the high thermal conductivity layer B constituting the outermost layer of the in-plane type thermoelectric conversion module on the thermally conductive interface member B side. [3] The thermoelectric conversion module according to [2] above, wherein the high thermal conductivity layer A is made of a plurality of high thermal conductivity layers a arranged at intervals, with parts of the thermally conductive interface member A embedded in the gaps between adjacent high thermal conductivity layers a, and the high thermal conductivity layer B is made of a plurality of high thermal conductivity layers b arranged at intervals, with parts of the thermally conductive interface member B embedded in the gaps between adjacent high thermal conductivity layers b. [4] The thermoelectric conversion module according to [2] or [3] above, wherein a ratio M of the embedding depth of a portion of the thermally conductive interface member A to the thickness of the high thermal conductivity layer A is 0.01 to 1.00, and a ratio N of the embedding depth of a portion of the thermally conductive interface member B to the thickness of the high thermal conductivity layer B is 0.01 to 1.00. [5] The thermoelectric conversion module according to any of [1] to [4] above, wherein the thermally conductive interface member A and the thermally conductive interface member B are each independently a resin layer or an organic layer.

[0007] In another aspect, the present inventors have found that providing a thermally conductive interface member (hereinafter, sometimes simply referred to as "TIM") having a specific shear stress and adhesive property on the top and bottom surfaces of an in-plane thermoelectric conversion module can further improve the heat transfer at the interface between the components constituting the in-plane thermoelectric conversion module, and have completed the invention according to a second embodiment of the present invention. That is, the invention according to the second embodiment of the present invention provides the following [6] to [8]. [6] A thermoelectric conversion module including a thermally conductive interface member A having adhesive property on one surface of the in-plane thermoelectric conversion module, and a heat dissipation member, and further including a thermally conductive interface member B having adhesive property on the other surface of the in-plane thermoelectric conversion module, wherein the shear stress τ applied to the thermally conductive interface member A when the thermally conductive interface member A is adhered to one surface of the in-plane thermoelectric conversion module is A (N / mm 2 ) and the shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the in-plane type thermoelectric conversion module. B (N / mm 2 ) and each independently 0.001 (N / mm 2 ) or more. [7] The thermoelectric conversion module according to [6] above, wherein the in-plane type thermoelectric conversion module further includes a high thermal conductivity layer A and a high thermal conductivity layer B, the high thermal conductivity layer A constituting the outermost layer of the in-plane type thermoelectric conversion module on the thermally conductive interface member A side, and the high thermal conductivity layer B constituting the outermost layer of the in-plane type thermoelectric conversion module on the thermally conductive interface member B side. [8] The thermoelectric conversion module according to [7] above, wherein the adhesive strength (N / cm) of the thermally conductive interface member A to the high thermal conductivity layer A and the adhesive strength (N / cm) of the thermally conductive interface member B to the high thermal conductivity layer B are each independently 0.01 (N / cm) or more.

[0008] In yet another aspect, the present inventors have found that by providing adhesive thermally conductive interface members (hereinafter sometimes simply referred to as "TIM") on the upper and lower surfaces of a thermoelectric conversion element, and by setting the ratio of the total thermal resistance value of the adhesive thermally conductive interface members to the total thermal resistance value of the thermoelectric conversion module within a specific range, and by setting the shear stress applied to the adhesive thermally conductive interface members within a specific range, it is possible to further improve the heat transfer at the interfaces between the members constituting the thermoelectric conversion module, and have completed the invention according to a third embodiment of the present invention. That is, the invention according to the third embodiment of the present invention provides the following [9]. [9] A thermoelectric conversion module including an adhesive thermally conductive interface member A and a heat dissipation member, in this order, on one surface of a thermoelectric conversion element, and an adhesive thermally conductive interface member B on the other surface of the thermoelectric conversion element, wherein the thermal resistance value of the thermally conductive interface member A is set to R A (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is R AB (mK / W), and the total thermal resistance of the thermoelectric conversion module is R M (mK / W), the R M The R AB The ratio (R AB / R M ) is 1.40 or less, and the shear stress τ applied to the thermally conductive interface member A when the thermally conductive interface member A is bonded to one surface of the thermoelectric conversion element A (N / mm 2 ) and the shear stress τ applied to the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the thermoelectric conversion element. B (N / mm 2 ) and each independently 0.001 (N / mm 2 ) or more.

[0009] According to the present invention, it is possible to provide a thermoelectric conversion module having high thermoelectric performance with improved heat transfer at the interface between members.

[0010] FIG. 1 is a cross-sectional configuration diagram showing an embodiment of a thermoelectric conversion module according to a first embodiment of the present invention. FIG. 2 is a plan view showing an example of an arrangement of electrodes and thermoelectric element layers on a substrate constituting a part of a thermoelectric conversion module used in examples according to the first and second embodiments of the present invention. FIG. 3 is a cross-sectional configuration diagram showing an example of an evaluation configuration of a thermoelectric conversion module used in examples according to the first embodiment of the present invention. FIG. 4 is a cross-sectional configuration diagram showing an embodiment of a thermoelectric conversion module according to a second embodiment of the present invention. FIG. 5 is a cross-sectional configuration diagram showing an embodiment of a thermoelectric conversion module according to a third embodiment of the present invention. FIG. 6 is a cross-sectional configuration diagram showing an example of an evaluation configuration of a thermoelectric conversion module used in examples according to the third embodiment of the present invention.

[0011] [Thermoelectric Conversion Module] A thermoelectric conversion module according to a first embodiment of the present invention is a thermoelectric conversion module including a thermally conductive interface member A and a heat dissipation member on one surface of an in-plane type thermoelectric conversion module, and further including a thermally conductive interface member B on the other surface of the in-plane type thermoelectric conversion module, wherein the thermal resistance value of the thermally conductive interface member A is R A (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is R AB (mK / W), and the total thermal resistance of the in-plane thermoelectric conversion module is R M (mK / W), the R M The R AB The ratio (R AB / R MThe thermoelectric conversion module according to the first embodiment of the present invention has a configuration including a thermally conductive interface member A (hereinafter, sometimes simply referred to as "TIMA") and a heat dissipation member on one surface of the in-plane type thermoelectric conversion module, and further including a thermally conductive interface member B (hereinafter, sometimes simply referred to as "TIMB") on the other surface of the in-plane type thermoelectric conversion module, and has a total thermal resistance value R M The thermal resistance value R of TIMA A and the thermal resistance value R of TIMB B The total thermal resistance value R AB The ratio (R AB / R M By making the ratio 1.40 or less, the heat transfer properties at the interfaces between the members constituting the in-plane type thermoelectric conversion module can be further improved, resulting in higher thermoelectric performance.

[0012] In this specification, the "thermoelectric conversion module" according to the first embodiment of the present invention is composed of an "in-plane type thermoelectric conversion module", "thermally conductive interface members A and B", and a "heat dissipation member".

[0013] In this specification, preferred definitions can be selected arbitrarily, and it can be said that a combination of preferred definitions is more preferable. In this specification, the expression "XX to YY" means "XX or more and YY or less." In this specification, for preferred numerical ranges (for example, ranges of content, etc.), lower and upper limits described in stages can be independently combined. For example, from the description "preferably 10 to 90, more preferably 30 to 60," the "preferable lower limit (10)" and the "more preferable upper limit (60)" can be combined to form "10 to 60."

[0014] A thermoelectric conversion module according to a first embodiment of the present invention will be described below with reference to the drawings.

[0015] 1 is a cross-sectional view showing an embodiment of a thermoelectric conversion module according to a first embodiment of the present invention. The thermoelectric conversion module 1A includes a thermally conductive interface member A10a and a heat dissipation member 11 on one surface of an in-plane thermoelectric conversion module 9, and further includes a thermally conductive interface member B10b on the other surface of the in-plane thermoelectric conversion module 9. The in-plane thermoelectric conversion module 9 includes a thermoelectric element layer 6 formed by P-type thermoelectric element layers 4 and N-type thermoelectric element layers 5 arranged in series, alternately adjacent (abutting) in the in-plane direction of a substrate 2 and with a common electrode 3 interposed therebetween. The in-plane thermoelectric conversion module 9 includes a high-thermal-conductivity layer A8A on one surface of the thermoelectric element layer 6, the high-thermal-conductivity layer A8A being made up of a plurality of high-thermal-conductivity layers a8a arranged at intervals with a coating layer 7 interposed therebetween. The other surface of the thermoelectric element layer 6 includes a high-thermal-conductivity layer B8B made up of a plurality of high-thermal-conductivity layers b8b arranged at intervals with the electrode 3 and the substrate 2 interposed therebetween. By providing a thermally conductive interface member A10a between the high thermal conductivity layer a8a on the upper surface of the in-plane type thermoelectric conversion module 9 and the heat dissipation member 11, it is possible to reduce the contact thermal resistance that occurs therebetween. Similarly, by providing a thermally conductive interface member B10b between the high thermal conductivity layer b8b on the lower surface of the in-plane type thermoelectric conversion module 9 and, for example, a heat source (not shown), it is possible to reduce the contact thermal resistance that occurs therebetween. By using the thermally conductive interface members A and B having such effects, and by using the thermally conductive interface members A and B, it is possible to reduce the total thermal resistance R M The thermal resistance value R of the thermally conductive interface member A A and the thermal resistance value R of the thermally conductive interface member B. B The total thermal resistance value R AB The ratio (R AB / R M By making the ratio 1.40 or less, the heat transfer properties at the interfaces between the members constituting the in-plane type thermoelectric conversion module can be further improved, resulting in higher thermoelectric performance.

[0016] The total thermal resistance R is the sum of the thermal resistances of the components that make up the in-plane thermoelectric conversion module. M The thermal resistance value R of TIMA Aand the thermal resistance value R of TIMB B The total thermal resistance value R AB The ratio (R AB / R M ) is 1.40 or less. AB / R M ) is preferably 0.01 to 1.00, more preferably 0.03 to 0.50, and even more preferably 0.05 to 0.10. AB / R M When the temperature sintering ratio ) is within this range, the heat transfer at the interface between the members is more likely to be improved, and the thermoelectric performance is improved.

[0017] <Thermal Conductive Interface Member A and the Thermal Conductive Interface Member B> In the thermoelectric conversion module according to the first embodiment of the present invention, a thermal conductive interface member A is provided between the upper surface of the in-plane thermoelectric conversion module and the heat dissipation member, and a thermal conductive interface member B is provided on the lower surface of the in-plane thermoelectric conversion module. By providing the thermal conductive interface member A between the upper surface of the in-plane thermoelectric conversion module and the heat dissipation member, the contact thermal resistance generated therebetween can be reduced. Similarly, by providing the thermal conductive interface member B between the lower surface of the in-plane thermoelectric conversion module and, for example, a heat source, the contact thermal resistance generated therebetween can be reduced. In this way, the use of the thermal conductive interface member A and the thermal conductive interface member B facilitates improvement in thermal conduction within the in-plane thermoelectric conversion module, leading to improved thermoelectric performance of the thermoelectric conversion module.

[0018] It is preferable that the thermally conductive interface member A and the thermally conductive interface member B are each independently a resin layer or an organic layer. Hereinafter, "thermally conductive interface member A and the thermally conductive interface member B" may be simply referred to as "thermally conductive interface member".

[0019] The resin material used for the resin layer is not particularly limited, and any resin can be appropriately selected from those used in the field of electronic components, etc. Examples of the resin material include thermosetting resins, thermoplastic resins, and photocurable resins. Examples include polyolefin resins such as polyethylene and polypropylene; styrene resins such as polystyrene; acrylic resins such as polymethyl methacrylate; polyamide resins such as polyamide (nylon 6, nylon 66, etc.), poly-m-phenylene isophthalamide, and poly-p-phenylene terephthalamide; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polyarylate; cycloolefin polymers such as norbornene polymers, monocyclic olefin polymers, cyclic conjugated diene polymers, vinyl alicyclic hydrocarbon polymers, and hydrogenated versions thereof; vinyl chloride; polyimide; polyamideimide; polyphenylene ether; polyether ketone; polyether ether ketone; polycarbonate; polysulfone resins such as polysulfone and polyethersulfone; polyphenylene sulfide; silicone resins; and combinations of two or more of these polymers. Among these, polyamide resins, polyimide, polyamideimide, and silicone resins are preferred from the viewpoint of excellent heat resistance and resistance to deterioration in heat dissipation properties.

[0020] Examples of the organic layer include an adhesive layer, a pressure-sensitive adhesive layer, a gel layer, a grease layer, a clay layer, etc. Among these, from the viewpoints of workability and conformability to irregularities, an adhesive layer and a pressure-sensitive adhesive layer are preferred.

[0021] The adhesive used in the adhesive layer is not particularly limited, and may be a two-component curing adhesive, a thermosetting adhesive, a moisture-curing adhesive, or a hot-melt adhesive. Examples of the adhesive include an acrylic adhesive, a urethane adhesive, a silicone adhesive, a rubber adhesive, an olefin adhesive, and an epoxy adhesive.

[0022] The adhesive used in the adhesive layer is not particularly limited and may be any of an acrylic adhesive, a silicone adhesive, a polyester adhesive, a polyurethane adhesive, a rubber adhesive, etc. The adhesive may be an emulsion type, a solvent type, or a solventless type, and may be a crosslinked type or a non-crosslinked type. Among them, an acrylic adhesive or a silicone adhesive is preferred.

[0023] To improve thermal conductivity, the resin layer may be filled with a thermally conductive filler. The thermally conductive filler is not particularly limited, but may be, for example, at least one selected from silica, alumina, magnesium oxide, silicon nitride, aluminum nitride, magnesium nitride, boron nitride, copper, and aluminum. These thermally conductive fillers may be used alone or in combination of two or more. The thermally conductive filler preferably has an average particle size of 0.1 to 200 μm, more preferably 1 to 100 μm, even more preferably 5 to 50 μm, and particularly preferably 10 to 30 μm. The average particle size can be measured, for example, by the Coulter counter method. The content of the thermally conductive filler is adjusted appropriately depending on the desired thermal conductivity, and is preferably 40 to 99% by mass, more preferably 50 to 95% by mass, and particularly preferably 50 to 80% by mass in the resin composition. If the content of the thermally conductive filler is within this range, the thermally conductive interface member will have excellent heat dissipation properties, folding resistance, and flex resistance, and will maintain its strength.

[0024] The thickness of the thermally conductive interface member is preferably 0.05 to 1.50 mm, more preferably 0.08 to 1.20 mm, and even more preferably 0.10 to 1.00 mm. If the thickness of the thermally conductive interface member is within this range, the thermal resistance of the thermally conductive interface member can be maintained low, and the contact thermal resistance generated between the heat source and the heat dissipation member can be efficiently reduced.

[0025] Examples of commercially available thermally conductive interface members include the following: high thermal conductive heat dissipation sheet (manufactured by Sekisui Polymatech Co., Ltd., product number: Manion50α, thickness: 0.50 mm, thermal conductivity: 17 W / (m·K)), heat dissipation sheet TIMLIGHT (manufactured by Sekisui Polymatech Co., Ltd., product number: PT-V, thickness: 0.50 mm, thermal conductivity: 12 W / (m·K)), thermally conductive double-sided tape (manufactured by 3M Co., Ltd., product number: 8926, thickness: 0.20 mm, thermal conductivity: 1.5 W / (m·K)), and thermally conductive double-sided tape (manufactured by 3M Co., Ltd., product number: VHR0601, thickness: 0.30 mm, thermal conductivity: 0.6 W / (m·K)).

[0026] <Heat Dissipation Member> The heat dissipation member may be any member that conducts generated heat and dissipates it to the outside, and is not particularly limited, but examples thereof include a heat sink and a heat spreader. Examples of materials for heat sinks and heat spreaders include copper and aluminum. In addition to heat spreaders and heat sinks, examples of materials include radiators, coolers, cooling fans, heat pipes, vapor chambers, metal covers, and housings. A heat pipe is, for example, a hollow structure that is cylindrical, approximately cylindrical, or flattened.

[0027] (High thermal conductivity layer A and high thermal conductivity layer B) From the viewpoint of efficiently applying a temperature difference to the thermoelectric element layer, the in-plane type thermoelectric conversion module further includes a high thermal conductivity layer A and a high thermal conductivity layer B, and it is preferable that the high thermal conductivity layer A constitutes the outermost layer of the in-plane type thermoelectric conversion module on the thermal conductive interface member A side, and the high thermal conductivity layer B constitutes the outermost layer of the in-plane type thermoelectric conversion module on the thermal conductive interface member B side.

[0028] From the viewpoint of suppressing the contact thermal resistance at the interfaces between the components of the in-plane thermoelectric conversion module and further improving heat transfer, it is preferable that the high thermal conductivity layer A is made up of a plurality of high thermal conductivity layers a arranged at intervals, with part of the thermally conductive interface member A embedded in the gaps between adjacent high thermal conductivity layers a. Similarly, it is preferable that the high thermal conductivity layer B is made up of a plurality of high thermal conductivity layers b arranged at intervals, with part of the thermally conductive interface member B embedded in the gaps between adjacent high thermal conductivity layers b.

[0029] The ratio M of the embedding depth of the portion of the thermally conductive interface member A to the thickness of the high thermal conductivity layer A is preferably 0.01 to 1.00, more preferably 0.10 to 0.95, and even more preferably 0.60 to 0.90. The ratio N of the embedding depth of the portion of the thermally conductive interface member B to the thickness of the high thermal conductivity layer B is preferably 0.01 to 1.00, more preferably 0.10 to 0.95, and even more preferably 0.60 to 0.90. When the ratios M and N are within these ranges, the thermal conductivity of the interfaces between the respective members is more likely to be improved, and thermoelectric performance is further improved. Here, the "embedding depth of the portion of the thermally conductive interface member A" refers to, for example, the maximum distance in the thickness direction, starting from the top surface of the high thermal conductivity layer a8a, when a portion of the thermally conductive interface member A10a in contact with the top surface of the high thermal conductivity layer a8a in FIG. 1 partially penetrates into the gap between the high thermal conductivity layers a8a. Similarly, the "embedding depth of a portion of the thermally conductive interface member B" refers to, for example, in FIG. 1, the maximum distance in the thickness direction from the lower surface of the high thermal conductivity layer b8b when a portion of the thermally conductive interface member B10b in contact with the lower surface of the high thermal conductivity layer b8b partially enters a gap between the high thermal conductivity layers b8b.

[0030] The high thermal conductivity layers A and B used in the first embodiment of the present invention can efficiently create a temperature difference between the thermoelectric element layers arranged in the in-plane direction. Hereinafter, the high thermal conductivity layers A, a, B, and b may be simply referred to as "high thermal conductivity layers."

[0031] The arrangement of the high thermal conductivity layers used in the first embodiment of the present invention is not particularly limited, but should be appropriately adjusted depending on the arrangement and shape of the thermoelectric element layers of the thermoelectric conversion module used, i.e., the P-type thermoelectric element layer and the N-type thermoelectric element layer. In the invention according to the first embodiment of the present invention, it is preferable that the high thermal conductivity layers b8b and a8a are repeatedly arranged at predetermined intervals on the surface of the substrate 2 or the covering layer 7 opposite the thermoelectric element layer 6, so as to straddle the extension of the boundary surface joining the P-type thermoelectric element layer 4 and the N-type thermoelectric element layer 5. Furthermore, it is preferable that the high thermal conductivity layers a8a and b8b straddle only one extension of the boundary surface, and that the high thermal conductivity layers a and b are arranged alternately when viewed in a cross section in the thickness direction as shown in FIG. By arranging the high thermal conductivity layers a and b in this manner, high temperature and low temperature regions are formed continuously and sequentially within the thermoelectric element layer 6 in a direction parallel to the plane of the substrate 2 and the plane of the covering layer 7, presumably improving power generation efficiency. For example, as shown in FIG. 1 , high thermal conductivity layers a 8a and b 8b are alternately arranged in the in-plane direction of the covering layer 7 and the substrate 2 across the electrodes 3 connecting the P-type thermoelectric element layer 4 and the N-type thermoelectric element layer 5, which are alternately adjacent (abutting) in the in-plane direction of the substrate 2. In this case, a temperature difference can be applied in the in-plane direction of the thermoelectric element layer 6. The ratio of the high thermal conductivity layers to the total width in the series direction consisting of a pair of P-type thermoelectric element layer 4 and N-type thermoelectric element layer 5 is preferably 0.30 to 0.70, more preferably 0.40 to 0.60, even more preferably 0.48 to 0.52, and particularly preferably 0.50. When the proportion of the high thermal conductivity layers is within this range, heat can be selectively dissipated in a specific direction, and a temperature difference can be efficiently created in the in-plane direction of the thermoelectric element layer 6. Furthermore, it is preferable that the high thermal conductivity layers are arranged symmetrically at the contact portion consisting of a pair of P-type thermoelectric element layers 4 and N-type thermoelectric element layers 5 in the series direction while satisfying the above conditions.

[0032] The highly thermally conductive layer used in the first embodiment of the present invention is formed using a highly thermally conductive material from the viewpoint of thermoelectric performance. The method for forming the highly thermally conductive layer is not particularly limited, but may include a method in which a sheet-shaped highly thermally conductive material is processed into a predetermined pattern shape in advance by a known physical or chemical treatment, mainly based on photolithography, or a combination of these.

[0033] Examples of materials for the high thermal conductivity layer include metal materials, ceramic materials, carbon-based materials such as carbon fiber, and mixtures of these materials with resin. Among these, the high thermal conductivity layer is preferably at least one selected from the group consisting of metal materials, ceramic materials, mixtures of metal materials and resins, and mixtures of ceramic materials and resins, and more preferably at least one selected from the group consisting of metal materials and ceramic materials. Metal materials include single metals such as gold, silver, copper, nickel, tin, iron, chromium, platinum, palladium, rhodium, iridium, ruthenium, osmium, indium, zinc, molybdenum, manganese, titanium, and aluminum, as well as alloys containing two or more metals such as stainless steel and brass. Examples of ceramic materials include barium titanate, aluminum nitride, boron nitride, aluminum oxide, silicon carbide, and silicon nitride. Among these, metal materials are preferred from the viewpoints of high thermal conductivity, processability, and flexibility. Among metal materials, copper (including oxygen-free copper) and stainless steel are preferred, with copper being more preferred due to its high thermal conductivity and ease of processing. The resins mentioned above can be used as the resin. Representative metal materials with high thermal conductivity that can be used in the first embodiment of the present invention are listed below. Oxygen-free copper: Oxygen-free copper (OFC) generally refers to high-purity copper with a purity of 99.95% (3N) or higher that does not contain oxides. The Japanese Industrial Standards specify oxygen-free copper (JIS H 3100, C1020) and oxygen-free copper for electron tubes (JIS H 3510, C1011). Stainless steel (JIS) SUS304: 18Cr-8Ni (containing 18% Cr and 8% Ni) SUS316: 18Cr-12Ni (containing 18% Cr, 12% Ni, and molybdenum (Mo)) stainless steel)

[0034] The thermal conductivity of the high thermal conductive layer is preferably 5 to 500 W / (m K), more preferably 12 to 450 W / (m K), and even more preferably 15 to 420 W / (m K). When the thermal conductivity of the high thermal conductive layer is within the above range, a temperature difference can be efficiently created.

[0035] The thickness of the high thermal conductivity layer is preferably 40 to 550 μm, more preferably 60 to 530 μm, and even more preferably 80 to 510 μm. If the thickness of the high thermal conductivity layer is within this range, heat can be selectively dissipated in a specific direction, and a temperature difference can be efficiently created in the in-plane direction of the thermoelectric element layer in which P-type thermoelectric element layers and N-type thermoelectric element layers are alternately adjacent to each other in the in-plane direction and arranged in series with electrodes interposed therebetween.

[0036] <Substrate> The substrate of the thermoelectric conversion module used in the first embodiment of the present invention is not particularly limited, but it is preferable to use a film substrate that does not affect the decrease in electrical conductivity or the increase in thermal conductivity of the thermoelectric element layer. Among them, polyimide films, polyamide films, polyetherimide films, polyaramid films, and polyamideimide films are preferred because they have excellent flexibility, can maintain the performance of the thermoelectric element layer without thermal deformation even when a thin film made of a thermoelectric semiconductor composition described below is annealed, and have high heat resistance and dimensional stability. Furthermore, polyimide films are particularly preferred because of their high versatility.

[0037] From the viewpoints of flexibility, heat resistance, and dimensional stability, the thickness of the substrate is preferably 1 μm to 1000 μm, more preferably 10 μm to 500 μm, and even more preferably 20 μm to 100 μm. Furthermore, the decomposition temperature of the film is preferably 300° C. or higher.

[0038] <Electrode Layer> The electrode layer used in the first embodiment of the present invention is provided to electrically connect the P-type thermoelectric element layer and the N-type thermoelectric element layer that constitute the thermoelectric element layer described below. Examples of electrode materials include gold, silver, nickel, copper, and alloys thereof. The thickness of the electrode layer is preferably 10 nm to 200 μm, more preferably 30 nm to 150 μm, and even more preferably 50 nm to 120 μm. When the electrode layer thickness is within the above range, the electrical conductivity is high and the resistance is low, thereby keeping the total electrical resistance of the thermoelectric element layer low. Furthermore, sufficient strength as an electrode can be obtained. Examples of methods for forming an electrode on a film substrate include a method in which an unpatterned electrode layer is provided on the film substrate, and then processed into a predetermined pattern shape by known physical or chemical treatments, primarily photolithography, or a combination of these, or a method in which a pattern of the electrode layer is directly formed by screen printing, inkjet printing, or the like. Examples of methods for forming an electrode layer on which no pattern is formed include dry processes such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), or wet processes such as various coating methods and electrodeposition methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade methods, silver halide plating, electrolytic plating, electroless plating, and lamination of metal foil, and are appropriately selected depending on the material of the electrode layer.

[0039] <Thermoelectric Element Layer> As described above, the thermoelectric element layer of the thermoelectric conversion module used in the first embodiment of the present invention includes a P-type thermoelectric element layer and an N-type thermoelectric element layer, and the P-type thermoelectric element layers and the N-type thermoelectric element layers are alternately arranged adjacent to each other in the in-plane direction and are electrically connected in series. Furthermore, the connection between the P-type thermoelectric element layer and the N-type thermoelectric element layer may be via the above-mentioned electrode layer made of a highly conductive metal material or the like from the viewpoints of connection stability and thermoelectric performance.

[0040] The thermoelectric element layer used in the first embodiment of the present invention is preferably a layer formed on a substrate and comprising thermoelectric semiconductor particles, a heat-resistant resin, and a thermoelectric semiconductor composition containing one or both of an ionic liquid and an inorganic ionic compound.

[0041] (Thermoelectric Semiconductor Particles) The thermoelectric semiconductor particles used in the thermoelectric element layer are preferably prepared by pulverizing a thermoelectric semiconductor material to a predetermined size using a fine pulverizer or the like.

[0042] The materials constituting the P-type thermoelectric element layer and the N-type thermoelectric element layer used in the first embodiment of the present invention are not particularly limited as long as they are materials that can generate thermoelectric power by applying a temperature difference, and examples thereof include bismuth-tellurium-based thermoelectric semiconductor materials such as P-type bismuth telluride and N-type bismuth telluride; telluride-based thermoelectric semiconductor materials such as GeTe and PbTe; antimony-tellurium-based thermoelectric semiconductor materials; ZnSb, Zn 3 Sb 2、 Zn 4 Sb 3 Zinc-antimony based thermoelectric semiconductor materials such as silicon-germanium based thermoelectric semiconductor materials such as silicon germanium; Bi 2 Se 3 Bismuth selenide-based thermoelectric semiconductor materials such as β-FeSi 2 , CrSi 2 , MnSi 1.73 , Mg 2 Silicide-based thermoelectric semiconductor materials such as Si; oxide-based thermoelectric semiconductor materials; Heusler materials such as FeVAl, FeVAlSi, and FeVTiAl; TiS 2 Sulfide-based thermoelectric semiconductor materials such as the above are used.

[0043] Among these, the thermoelectric semiconductor material used in the first embodiment of the present invention is preferably a bismuth-tellurium-based thermoelectric semiconductor material such as P-type bismuth telluride or N-type bismuth telluride. The P-type bismuth telluride has positive holes as carriers and a positive Seebeck coefficient, for example, Bi X Te 3 Sb 2-XIn this case, X is preferably 0<X≦0.8, and more preferably 0.4≦X≦0.6. When X is greater than 0 and not greater than 0.8, the Seebeck coefficient and electrical conductivity are increased, and the properties as a P-type thermoelectric conversion material are maintained, which is preferable. In addition, the N-type bismuth telluride has electrons as carriers and a negative Seebeck coefficient, for example, Bi 2 Te 3-Y Se Y In this case, Y is preferably 0≦Y≦3 (when Y=0: Bi 2 Te 3 ), and more preferably 0<Y≦2.7. When Y is 0 to 3, the Seebeck coefficient and electrical conductivity become large, and the properties as an N-type thermoelectric conversion material are maintained, which is preferable.

[0044] The amount of thermoelectric semiconductor particles in the thermoelectric semiconductor composition is preferably 30 to 99% by mass, and more preferably 70 to 95% by mass. When the amount of thermoelectric semiconductor particles is within this range, the Seebeck coefficient (absolute value of the Peltier coefficient) is large, and the decrease in electrical conductivity is suppressed, with only the thermal conductivity decreasing, so that a film exhibiting high thermoelectric performance and having sufficient film strength and flexibility is obtained, which is preferable.

[0045] The average particle size of the thermoelectric semiconductor particles is preferably 10 nm to 200 μm, more preferably 50 nm to 10 μm. Within this range, uniform dispersion is facilitated, and electrical conductivity can be increased. The method for pulverizing the thermoelectric semiconductor material to obtain thermoelectric semiconductor particles is not particularly limited, and the material may be pulverized to a predetermined size using a known fine pulverizing device such as a jet mill, ball mill, bead mill, colloid mill, conical mill, disk mill, edge mill, flour mill, hammer mill, pellet mill, Willy mill, or roller mill. The average particle size of the thermoelectric semiconductor particles was measured using a laser diffraction particle size analyzer (Model 1064, manufactured by CILAS) and was taken as the median of the particle size distribution.

[0046] Furthermore, the thermoelectric semiconductor particles are preferably annealed (hereinafter, sometimes referred to as "annealing treatment A"). Annealing treatment A improves the crystallinity of the thermoelectric semiconductor particles and removes the surface oxide film of the thermoelectric semiconductor particles, thereby increasing the Seebeck coefficient (absolute value of the Peltier coefficient) of the thermoelectric conversion material and further improving the thermoelectric figure of merit. Annealing treatment A is not particularly limited, but is preferably performed before preparing the thermoelectric semiconductor composition in an inert gas atmosphere such as nitrogen or argon, a reducing gas atmosphere such as hydrogen, or a vacuum condition with a controlled gas flow rate, so as not to adversely affect the thermoelectric semiconductor particles. Annealing treatment A is more preferably performed in a mixed gas atmosphere of an inert gas and a reducing gas. The specific temperature conditions depend on the thermoelectric semiconductor particles used, but it is typically performed at a temperature below the melting point of the particles, at 100 to 1500°C, for several minutes to several tens of hours.

[0047] (Heat-Resistant Resin) The heat-resistant resin used in the first embodiment of the present invention functions as a binder between thermoelectric semiconductor particles and enhances the flexibility of the thermoelectric conversion material. The heat-resistant resin is not particularly limited, but is preferably one that maintains its physical properties, such as mechanical strength and thermal conductivity, when the thermoelectric semiconductor particles are crystallized by annealing a thin film made of the thermoelectric semiconductor composition. Examples of heat-resistant resins include polyamide resins, polyamideimide resins, polyimide resins, polyetherimide resins, polybenzoxazole resins, polybenzimidazole resins, epoxy resins, and copolymers having the chemical structures of these resins. The heat-resistant resins may be used alone or in combination. Among these, polyamide resins, polyamideimide resins, polyimide resins, and epoxy resins are preferred because of their high heat resistance and the fact that they do not adversely affect the crystal growth of the thermoelectric semiconductor particles in the thin film. Polyamide resins, polyamideimide resins, and polyimide resins are more preferred because of their excellent flexibility. When a polyimide film is used as the substrate, a polyimide resin is more preferable as the heat-resistant resin in terms of adhesion to the polyimide film, etc. In the first embodiment of the present invention, the polyimide resin collectively refers to polyimide and its precursor.

[0048] The heat-resistant resin preferably has a decomposition temperature of 300° C. or higher. If the decomposition temperature is within the above range, the resin will not lose its function as a binder and the flexibility of the thermoelectric element layer can be maintained even when a thin film made of the thermoelectric semiconductor composition is annealed, as will be described later.

[0049] The heat-resistant resin preferably has a mass loss rate of 10% or less, more preferably 5% or less, and even more preferably 1% or less, at 300° C. as measured by thermogravimetry (TG). If the mass loss rate is within the above range, the resin will not lose its function as a binder and the flexibility of the thermoelectric element layer can be maintained, even when a thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0050] The amount of the heat-resistant resin in the thermoelectric semiconductor composition is preferably 0.1 to 40% by mass, more preferably 1 to 20% by mass. When the amount of the heat-resistant resin in the thermoelectric semiconductor composition is within the above range, a film having both high thermoelectric performance and high film strength can be obtained.

[0051] (Ionic Liquid) The ionic liquid used in the first embodiment of the present invention is a molten salt formed by combining a cation and an anion, and refers to a salt that can exist in liquid form at any temperature range from -50°C to less than 400°C. In other words, an ionic liquid is an ionic compound having a melting point in the range of -50°C to less than 400°C. The melting point of the ionic liquid is more preferably 0°C to 150°C. Ionic liquids have characteristics such as extremely low vapor pressure and nonvolatility, excellent thermal stability and electrochemical stability, low viscosity, and high ionic conductivity. Therefore, as a conductive additive, they can effectively suppress a decrease in electrical conductivity between thermoelectric semiconductor particles. Furthermore, ionic liquids exhibit high polarity due to their aprotic ionic structure and excellent compatibility with heat-resistant resins, thereby enabling the electrical conductivity of the thermoelectric element layer to be uniform.

[0052] The ionic liquid may be a known or commercially available one. For example, a nitrogen-containing cyclic cationic compound such as pyridinium, pyrimidinium, pyrazolium, pyrrolidinium, piperidinium, or imidazolium, or a derivative thereof; a tetraalkylammonium-based amine-based cation and a derivative thereof; a phosphine-based cation such as phosphonium, trialkylsulfonium, or tetraalkylphosphonium, or a derivative thereof; a lithium cation and a derivative thereof; or a mixture of a cation component and Cl - ,Br - , I - , AlCl 4 - , Al 2 Cl 7 - , B.F. 4 - , P.F. 6 - , ClO 4 - , NO 3 - , C.H. 3 COO- , C.F. 3 COO - , C.H. 3 SO 3 - , C.F. 3 SO 3 - , (FSO 2 ) 2 N - , (CF 3 SO 2 ) 2 N - , (CF 3 SO 2 ) 3 C - , AsF 6 - , SbF 6 - , NbF 6 - , TaF 6 - , F(HF)n - , (CN) 2 N - , C 4 F 9 SO 3 - , (C 2 F 5 SO 2 ) 2 N - , C 3 F 7 COO - , (CF 3 SO 2 ) (CF 3 CO)N - and an anion component such as the above.

[0053] The electrical conductivity of the ionic liquid is preferably 10 -7 S / cm or more, more preferably 10 -6 If the electrical conductivity is in the above range, the conductive additive can effectively suppress a decrease in electrical conductivity between thermoelectric semiconductor particles.

[0054] The ionic liquid preferably has a decomposition temperature of 300° C. or higher. If the decomposition temperature is within the above range, the effect as a conductive additive can be maintained even when a thin film made of the thermoelectric semiconductor composition is annealed, as will be described later.

[0055] Furthermore, the ionic liquid preferably has a mass loss rate of 10% or less, more preferably 5% or less, and even more preferably 1% or less at 300° C. as measured by thermogravimetry (TG). If the mass loss rate is within the above range, the ionic liquid can maintain its effectiveness as a conductive additive even when a thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0056] The amount of the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50% by mass, more preferably 1.0 to 20% by mass. When the amount of the ionic liquid is within this range, a decrease in electrical conductivity is effectively suppressed, and a film having high thermoelectric performance is obtained.

[0057] (Inorganic Ionic Compound) The inorganic ionic compound used in the first embodiment of the present invention is a compound composed of at least a cation and an anion. The inorganic ionic compound is solid at room temperature, has a melting point somewhere in the temperature range of 400 to 900°C, and has characteristics such as high ionic conductivity, so that as a conductive additive, it can suppress a decrease in electrical conductivity between thermoelectric semiconductor particles.

[0058] As the cation, a metal cation is used. Examples of the metal cation include an alkali metal cation, an alkaline earth metal cation, a typical metal cation, and a transition metal cation, and an alkali metal cation or an alkaline earth metal cation is more preferred. Examples of the alkali metal cation include Li + , Na + , K. + , Rb + , Cs + and Fr + Examples of alkaline earth metal cations include Mg 2+ , Ca 2+ , Sr 2+ and Ba2+ etc.

[0059] Examples of anions include F - , Cl - ,Br - , I - , O.H. - , C.N. - , NO 3- , NO 2- , ClO - , ClO 2- , ClO 3- , ClO 4- , CrO 4 2- , HSO 4 - , SCN - , B.F. 4 - , P.F. 6 - etc.

[0060] The inorganic ionic compound may be a known or commercially available one. For example, a compound containing a cationic component such as potassium cation, sodium cation, or lithium cation and Cl - , AlCl 4 - , Al 2 Cl 7 - , ClO 4 - chloride ions such as Br - bromide ions such as I - Iodide ions such as BF 4 - , P.F. 6 - Fluoride ions such as F(HF) n - Halide anions such as NO 3 - , O.H. - , C.N. - and an anion component such as the above.

[0061] Among the inorganic ionic compounds described above, from the viewpoints of high-temperature stability, compatibility with thermoelectric semiconductor particles and resin, and suppression of a decrease in the electrical conductivity of the gaps between thermoelectric semiconductor particles, it is preferred that the cation component of the inorganic ionic compound contains at least one selected from potassium, sodium, and lithium. Also, it is preferred that the anion component of the inorganic ionic compound contains a halide anion, and Cl - ,Br - , and I - It is more preferable that the composition contains at least one selected from the following:

[0062] The inorganic ionic compound has an electrical conductivity of 10 -7 S / cm or more, and -6 If the electrical conductivity is in the above range, the conductive additive can effectively suppress a decrease in electrical conductivity between thermoelectric semiconductor particles.

[0063] The inorganic ionic compound preferably has a decomposition temperature of 400° C. or higher. If the decomposition temperature is within the above range, the effect as a conductive additive can be maintained even when a thin film made of the thermoelectric semiconductor composition is annealed, as will be described later.

[0064] Furthermore, the inorganic ionic compound preferably exhibits a mass loss rate of 10% or less, more preferably 5% or less, and even more preferably 1% or less at 400° C. as measured by thermogravimetry (TG). If the mass loss rate is within the above range, the compound can maintain its effectiveness as a conductive additive even when a thin film made of the thermoelectric semiconductor composition is annealed, as described below.

[0065] The amount of the inorganic ionic compound in the thermoelectric semiconductor composition is preferably 0.01 to 50% by mass, more preferably 1.0 to 10% by mass. When the amount of the inorganic ionic compound is within the above range, a decrease in electrical conductivity can be effectively suppressed, resulting in a film with improved thermoelectric performance. When an inorganic ionic compound and an ionic liquid are used in combination, the total content of the inorganic ionic compound and the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50% by mass, more preferably 1.0 to 10% by mass.

[0066] The thickness of the thermoelectric element layer consisting of the P-type thermoelectric element layer and the N-type thermoelectric element layer is not particularly limited, and may be the same thickness or different thicknesses (a step is generated at the connection portion). From the viewpoints of flexibility and material cost, the thickness of the P-type thermoelectric element and the N-type thermoelectric element is preferably 0.1 μm to 300 μm, more preferably 1 μm to 140 μm, and particularly preferably 30 μm to 100 μm.

[0067] The thermoelectric element layer used in the first embodiment of the present invention is preferably formed from the thermoelectric semiconductor composition on one surface of the substrate. Methods for applying the thermoelectric semiconductor composition to the substrate include, but are not limited to, well-known methods such as screen printing, flexographic printing, gravure printing, spin coating, dip coating, die coating, spray coating, bar coating, and doctor blade coating. When forming a patterned coating, screen printing and slot die coating are preferably used, as they allow for easy pattern formation using a screen plate with the desired pattern. The resulting coating is then dried to form a thin film. Conventional drying methods, such as hot air drying, hot roll drying, and infrared irradiation, can be used. The heating temperature is typically 80 to 150°C, and the heating time varies depending on the heating method, but is typically several seconds to several tens of minutes. Furthermore, when a solvent is used in preparing the thermoelectric semiconductor composition, the heating temperature is not particularly limited as long as it is within a temperature range that can dry the solvent used. After forming the thin film, an annealing treatment (hereinafter sometimes referred to as annealing treatment B) is preferably performed. By performing the annealing treatment B, the thermoelectric performance can be stabilized and the thermoelectric semiconductor particles in the thin film can undergo crystal growth, thereby further improving the thermoelectric performance. Although there are no particular limitations on the annealing treatment B, it is usually performed in an inert gas atmosphere such as nitrogen or argon, in a reducing gas atmosphere, or under vacuum conditions with a controlled gas flow rate, at 100 to 500°C for several minutes to several tens of hours, depending on the heat resistance temperature of the resin and ionic liquid used, etc.

[0068] <Insulating Layer> The thermoelectric conversion module according to the first embodiment of the present invention may include an insulating layer. The insulating layer is not particularly limited, but is preferably made of a resin or an inorganic material, and is more preferably made of a resin from the viewpoint of flexibility.

[0069] The resin is not particularly limited, and examples thereof include resin films. The inorganic material is not particularly limited, and examples thereof include silicon oxide, aluminum oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, barium oxide, boron nitride, aluminum nitride, and silicon carbide. Among these, silicon oxide and aluminum oxide are preferred from the viewpoints of cost, stability, and ease of availability. The thickness of the insulating layer is preferably 1 to 150 μm, and particularly preferably 5 to 100 μm. The insulating layer can be formed by a known method. For example, the insulating layer may be formed directly on the surface of the thermoelectric element layer, or may be bonded via an adhesive layer or the like. Alternatively, the insulating layer may be formed by bonding an insulating layer previously formed on a release sheet to the thermoelectric element layer and transferring the insulating layer to the thermoelectric element layer. Furthermore, two or more types of insulating layers may be laminated, or a coating layer may be interposed.

[0070] <Coating Layer> The thermoelectric conversion module according to the first embodiment of the present invention may include a coating layer. Examples of the coating layer include, but are not limited to, a sealing layer and a gas barrier layer.

[0071] The sealing layer may be laminated directly on the thermoelectric element layer, or via a substrate, or via a gas barrier layer or insulating layer (described later). The main component of the sealing layer used in the present invention is preferably a polyolefin resin, an epoxy resin, or an acrylic resin. Furthermore, the sealing layer preferably comprises a sealant (hereinafter sometimes referred to as a "sealant composition") having adhesive properties. As used herein, "adhesive" means that the sealant has adhesive properties, such as tackiness, adhesion, or stickiness in the normal state when applied, and subsequently adheres and hardens upon application of energy. The use of a sealing layer facilitates lamination onto the thermoelectric element layer. It also facilitates application to the insulating layer, the high thermal conductivity layer, the gas barrier layer (described later), and the like. The sealing layer may consist of one layer or two or more layers. When two or more layers are laminated, they may be the same or different. The thickness of the sealing layer is preferably 0.5 to 300 μm, more preferably 10 to 100 μm, and even more preferably 30 to 80 μm. Within this range, when laminated on the surface of the thermoelectric element layer of the thermoelectric conversion module, the water vapor permeability can be reduced, improving the durability of the thermoelectric conversion module. Furthermore, as described above, it is preferable that the thermoelectric element layer and the sealing layer are in direct contact with each other. Direct contact between the thermoelectric element layer and the sealing layer prevents atmospheric water vapor from being directly present between the thermoelectric element layer and the sealing layer, thereby preventing water vapor from penetrating into the thermoelectric element layer and improving the sealing properties of the sealing layer. The sealing layer can be formed by a known method. For example, the sealing layer may be formed directly on the surface of the thermoelectric element layer and / or on a substrate, or a sealing layer previously formed on a release sheet may be attached to the thermoelectric element layer and transferred to the thermoelectric element layer. Furthermore, two or more sealing layers may be laminated, and an insulating layer or other covering layer may be interposed between them.

[0072] The gas barrier layer may be laminated directly on the thermoelectric element layer, or may be composed of a layer containing the main component described below on a substrate, with either side of the layer laminated directly on the thermoelectric element layer, or may be laminated via a sealing layer or an insulating layer. The gas barrier layer used in the first embodiment of the present invention is mainly composed of one or more compounds selected from the group consisting of metals, inorganic compounds, and polymer compounds. The gas barrier layer can improve the durability of the thermoelectric conversion module. Examples of metals include aluminum, magnesium, nickel, zinc, gold, silver, copper, and tin, and these are preferably used as a vapor-deposited film. Examples of inorganic compounds include inorganic oxides (MO). x ), inorganic nitrides (MN y ), inorganic carbide (MC z ), inorganic oxide carbide (MO x C z ), inorganic carbide nitrides (MN y C z ), inorganic oxide nitrides (MO x N y ), and inorganic oxynitride carbide (MO x N y C z ) and the like. Here, x, y, and z represent the composition ratio of each compound. Examples of M include metal elements such as silicon, zinc, aluminum, magnesium, indium, calcium, zirconium, titanium, boron, hafnium, and barium. Examples of polymer compounds include silicon-containing polymer compounds such as polyorganosiloxane and polysilazane compounds, polyimide, polyamide, polyamideimide, polyphenylene ether, polyether ketone, polyether ether ketone, polyolefin, and polyester. These polymer compounds can be used alone or in combination of two or more. The thickness of the layer containing the metal, inorganic compound, and polymer compound varies depending on the compounds used, but is typically 0.01 to 50 μm, preferably 0.03 to 10 μm. If the thickness of the layer containing the metal, inorganic compound, and resin is within this range, the water vapor permeability can be effectively suppressed.

[0073] The thickness of the gas barrier layer having a base material made of a metal, inorganic compound, or polymer compound is preferably 10 to 80 μm, more preferably 15 to 50 μm. When the thickness of the gas barrier layer is within this range, excellent gas barrier properties can be obtained, while also achieving both flexibility and film strength. The gas barrier layer may be a single layer or a laminate of two or more layers. Furthermore, when two or more layers are laminated, the layers may be the same or different. The gas barrier layer can be formed by a known method. It may be formed directly on the surface of the thermoelectric element layer and / or on a substrate. Alternatively, a gas barrier layer previously formed on a release sheet may be attached to the thermoelectric element layer and the gas barrier layer transferred to the thermoelectric element layer. Alternatively, a base material having a gas barrier layer may be laminated opposite the thermoelectric element layer. Furthermore, two or more types of gas barrier layers may be laminated, and an insulating layer or other coating layer may be interposed between them.

[0074] A thermoelectric conversion module according to a second embodiment of the present invention will now be described.

[0075] [Thermoelectric Conversion Module] A thermoelectric conversion module according to a second embodiment of the present invention includes a thermally conductive interface member A having adhesive properties on one surface of an in-plane type thermoelectric conversion module, a heat dissipation member, and further includes a thermally conductive interface member B having adhesive properties on the other surface of the in-plane type thermoelectric conversion module. When the thermally conductive interface member A is adhered to one surface of the in-plane type thermoelectric conversion module, the shear stress τ applied to the thermally conductive interface member A is A (N / mm 2 ) and the shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the in-plane type thermoelectric conversion module. B (N / mm 2 ) and each independently 0.001 (N / mm 2The thermoelectric conversion module according to the second embodiment of the present invention is configured to include a thermally conductive interface member A (hereinafter, sometimes simply referred to as "TIMA") having adhesive properties on one surface of the in-plane type thermoelectric conversion module, a heat dissipation member, and further includes a thermally conductive interface member B (hereinafter, sometimes simply referred to as "TIMB") having adhesive properties on the other surface of the in-plane type thermoelectric conversion module, and further includes a shear stress τ A and the shear stress τ of the TIMB B Each of these is independently 0.001 (N / mm 2 ) or more, the heat transfer properties at the interfaces between the members constituting the in-plane type thermoelectric conversion module can be further improved, resulting in higher thermoelectric performance.

[0076] In this specification, the configuration of the "thermoelectric conversion module" according to the second embodiment of the present invention includes an "in-plane type thermoelectric conversion module", "an adhesive thermally conductive interface member A and an adhesive thermally conductive interface member B", and a "heat dissipation member".

[0077] A thermoelectric conversion module according to a second embodiment of the present invention will be described below with reference to the drawings.

[0078] 4 is a cross-sectional view showing an embodiment of a thermoelectric conversion module according to a second embodiment of the present invention. The thermoelectric conversion module 1B includes an adhesive thermally conductive interface member A10c and a heat dissipation member 11 on one surface of an in-plane thermoelectric conversion module 9, and further includes an adhesive thermally conductive interface member B10d on the other surface of the in-plane thermoelectric conversion module 9. The in-plane thermoelectric conversion module 9 includes a thermoelectric element layer 6 formed by P-type thermoelectric element layers 4 and N-type thermoelectric element layers 5 arranged in series and alternately adjacent (abutting) in the in-plane direction of a substrate 2 with a common electrode 3 interposed therebetween. The in-plane thermoelectric conversion module 9 includes a high thermal conductivity layer A8A on one surface of the thermoelectric element layer 6, the high thermal conductivity layer A8A being made up of a plurality of high thermal conductivity layers a8a arranged at intervals with a coating layer 7 interposed therebetween. The high thermal conductivity layer B8B on the other surface of the thermoelectric element layer 6 includes the electrode 3 and a plurality of high thermal conductivity layers b8b arranged at intervals with the substrate 2 interposed therebetween. By providing an adhesive thermally conductive interface member A10c between the heat dissipation member 11 and the outermost high thermal conductivity layer a8a on one surface of the in-plane type thermoelectric conversion module 9, it is possible to reduce the contact thermal resistance that occurs therebetween. Similarly, by providing an adhesive thermally conductive interface member B10d between the outermost high thermal conductivity layer b8b on the other surface of the in-plane type thermoelectric conversion module 9 and, for example, a heat source (not shown), it is possible to reduce the contact thermal resistance that occurs therebetween. The adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B having such effects are used, and the shear stress τ of the adhesive thermally conductive interface member A is A and shear stress τ of adhesive thermally conductive interface member B B Each of these is independently 0.001 (N / mm 2 ) or more, the heat transfer properties at the interfaces between the members constituting the in-plane type thermoelectric conversion module can be further improved, resulting in higher thermoelectric performance.

[0079] When a thermally conductive interface member A having adhesiveness is bonded to one surface of an in-plane type thermoelectric conversion module, the shear stress τ applied to the thermally conductive interface member A is Aand shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the in-plane type thermoelectric conversion module. B are each independently 0.001 (N / mm 2 ) or more. The shear stress τ applied to the thermally conductive interface member A A and shear stress τ applied to the thermally conductive interface member B B are preferably 0.001 (N / mm 2 ) ~ 5.00 (N / mm 2 ), and more preferably 0.01 (N / mm 2 ) ~ 3.00 (N / mm 2 ), and more preferably 0.02 (N / mm 2 ) ~ 2.00 (N / mm 2 ) Shear stress τ A and shear stress τ B When the thickness is within this range, the adhesion between the components constituting the in-plane type thermoelectric conversion module is improved, and the thermoelectric performance is easily improved without causing physical damage to the P-type thermoelectric element layer and the N-type thermoelectric element layer.

[0080] The total thermal resistance R is the sum of the thermal resistances of the components that make up the in-plane thermoelectric conversion module. M The thermal resistance value R of TIMA A and the thermal resistance value R of TIMB B The total thermal resistance value R AB The ratio (R AB / R M ) is preferably 0.01 to 2.00, more preferably 0.05 to 1.50, and even more preferably 0.10 to 1.30. AB / R M When the shear stress is within this range, the heat transfer at the interface between the members is more likely to be improved while the shear stress is maintained within the appropriate range, and the thermoelectric performance is improved.

[0081] <Thermal Conductive Interface Member A and Thermal Conductive Interface Member B> The thermoelectric conversion module according to the second embodiment of the present invention includes an adhesive thermal conductive interface member A and a heat dissipation member on one surface of the in-plane thermoelectric conversion module, and further includes an adhesive thermal conductive interface member B on the other surface of the in-plane thermoelectric conversion module. By providing the adhesive thermal conductive interface member A between one surface of the in-plane thermoelectric conversion module and the heat dissipation member, the contact thermal resistance generated therebetween can be reduced. Similarly, by providing the adhesive thermal conductive interface member B between the other surface of the in-plane thermoelectric conversion module and, for example, a heat source, the contact thermal resistance generated therebetween can be reduced. In this way, the use of the adhesive thermal conductive interface member A and the adhesive thermal conductive interface member B facilitates improved thermal conductivity within the in-plane thermoelectric conversion module, leading to improved thermoelectric performance of the thermoelectric conversion module.

[0082] The adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B are preferably pressure-sensitive adhesive layers. Hereinafter, the "adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B" may be collectively referred to simply as the "thermal conductive interface member."

[0083] The adhesive used in the adhesive layer can be the same as that in the first embodiment.

[0084] To improve thermal conductivity, the pressure-sensitive adhesive layer may be filled with a thermally conductive filler. The thermally conductive filler is not particularly limited, but may be, for example, at least one selected from carbon fiber, graphite, silica, alumina, magnesium oxide, silicon nitride, aluminum nitride, magnesium nitride, boron nitride, copper, and aluminum. These thermally conductive fillers may be used alone or in combination of two or more. The thermally conductive filler preferably has an average particle size of 0.01 to 200 μm. The average particle size can be measured, for example, by the Coulter Counter method. The content of the thermally conductive filler is adjusted appropriately depending on the desired thermal conductivity, and is preferably 40 to 99 mass% in the composition. When the content of the thermally conductive filler is within this range, the thermally conductive interface member exhibits excellent heat dissipation properties, folding resistance, and flex resistance, and maintains its strength.

[0085] The thickness of the thermally conductive interface member is preferably 0.05 to 1.50 mm, more preferably 0.08 to 1.20 mm, and even more preferably 0.10 to 1.00 mm. If the thickness of the thermally conductive interface member is within this range, the thermal resistance of the thermally conductive interface member can be maintained low, and the contact thermal resistance generated between the heat source and the heat dissipation member can be efficiently reduced.

[0086] Examples of commercially available thermally conductive interface members include the following: High thermal conductivity heat dissipation sheet (manufactured by Sekisui Polymatech Co., Ltd., product number: Manion50α, thickness: 0.50 mm, thermal conductivity: 17 W / (m·K)), heat dissipation sheet TIMLIGHT (manufactured by Sekisui Polymatech Co., Ltd., product number: PT-V, thickness: 0.50 mm, thermal conductivity: 12 W / (m·K)), heat dissipation sheet TIMLIGHT (manufactured by Sekisui Polymatech Co., Ltd., product number: PT-UT, thickness: 0.50 mm, thermal conductivity: 6.0 W / (m·K)), thermally conductive double-sided tape (manufactured by 3M Co., Ltd., product number: 8926, thickness: 0.20 mm, thermal conductivity: 1.5 W / (m·K)), thermally conductive double-sided tape (manufactured by 3M Co., Ltd., product number: VHR0601, thickness: 0.30 mm, thermal conductivity: 0.6 W / (m·K)).

[0087] <Heat Dissipation Member> The heat dissipation member may be the same as that in the first embodiment.

[0088] (High Thermal Conductivity Layer A and High Thermal Conductivity Layer B) From the viewpoint of efficiently applying a temperature difference to the thermoelectric element layer, the in-plane type thermoelectric conversion module may further include a high thermal conductivity layer A and a high thermal conductivity layer B. It is preferable that the high thermal conductivity layer A constitutes the outermost layer of the in-plane type thermoelectric conversion module on the side of the thermally conductive interface member A having adhesive properties, and the high thermal conductivity layer B constitutes the outermost layer of the in-plane type thermoelectric conversion module on the side of the thermally conductive interface member B having adhesive properties. It is also preferable that the high thermal conductivity layer A is made up of a plurality of high thermal conductivity layers a arranged at intervals, and the high thermal conductivity layer B is made up of a plurality of high thermal conductivity layers b arranged at intervals.

[0089] The high thermal conductivity layers A and B used in the second embodiment of the present invention can efficiently create a temperature difference between the thermoelectric element layers arranged in the in-plane direction. Hereinafter, the high thermal conductivity layers A, a, B, and b may be simply referred to as "high thermal conductivity layers."

[0090] The arrangement of the high thermal conductivity layer used in the second embodiment of the present invention is not particularly limited, but should be appropriately adjusted depending on the arrangement and shape of the thermoelectric element layers of the thermoelectric conversion module used, i.e., the P-type thermoelectric element layer and the N-type thermoelectric element layer. In the second embodiment of the present invention, for example, as shown in FIG. 4 , high thermal conductivity layers a8a and a8b are alternately arranged in the in-plane direction of the covering layer 7 and the substrate 2, straddling the electrodes 3 that connect the P-type thermoelectric element layer 4 and the N-type thermoelectric element layer 5 that are alternately adjacent (abutting) in the in-plane direction of the substrate 2. In this case, a temperature difference can be applied in the in-plane direction of the thermoelectric element layer 6. The ratio of the high thermal conductivity layer to the total width of a pair of P-type thermoelectric element layer 4 and N-type thermoelectric element layer 5 in the series direction is preferably 0.30 to 0.70, more preferably 0.40 to 0.60, and even more preferably 0.48 to 0.52. When the proportion of the high thermal conductivity layers is within this range, heat can be selectively dissipated in a specific direction, and a temperature difference can be efficiently created in the in-plane direction of the thermoelectric element layer 6. Furthermore, it is preferable that the high thermal conductivity layers are arranged symmetrically at the contact portion consisting of a pair of P-type thermoelectric element layers 4 and N-type thermoelectric element layers 5 in the series direction while satisfying the above conditions.

[0091] The high thermal conductive layer used in the second embodiment of the present invention, the material forming the layer, the thermal conductivity of the high thermal conductive layer, and the thickness of the high thermal conductive layer can be the same as those in the first embodiment.

[0092] The adhesive strength of the thermally conductive interface member A to the high thermal conductivity layer A and the adhesive strength of the thermally conductive interface member B to the high thermal conductivity layer B are each independently preferably 0.01 (N / cm) to 50.0 (N / cm), more preferably 0.05 (N / cm) to 25.0 (N / cm), and even more preferably 0.10 (N / cm) to 10.0 (N / cm). When the adhesive strength of the thermally conductive interface member A to the high thermal conductivity layer A and the adhesive strength of the thermally conductive interface member B to the high thermal conductivity layer B are within these ranges, the adhesion between the components constituting the in-plane thermoelectric conversion module is improved while maintaining the desired thermal conductivity, and thermoelectric performance is easily improved without physically damaging the P-type thermoelectric element layer and the N-type thermoelectric element layer.

[0093] <Substrate> The substrate of the thermoelectric conversion module according to the second embodiment of the present invention can be the same as the substrate used in the first embodiment of the present invention described above, including details such as the material and thickness of the substrate.

[0094] <Electrode Layer> The electrode layer used in the second embodiment of the present invention can be the same as the electrode layer used in the first embodiment of the present invention described above, including details such as the electrode material constituting the electrode layer, the thickness of the electrode layer, and the method of forming the electrode.

[0095] <Thermoelectric Element Layer> The thermoelectric element layer used in the second embodiment of the present invention may be the same as the thermoelectric element layer used in the first embodiment of the present invention described above. Specifically, the thermoelectric element layer is the same in all respects, including the materials of the thermoelectric semiconductor particles, heat-resistant resin, ionic liquid, and inorganic ionic compound that constitute the thermoelectric element layer, the amounts of each compound in the thermoelectric semiconductor composition, the thickness of the thermoelectric element layer, and the method for forming the thermoelectric element layer.

[0096] <Insulating Layer> The thermoelectric conversion module according to the second embodiment of the present invention may include an insulating layer. The insulating layer used in the second embodiment may be the same as the insulating layer used in the first embodiment of the present invention. Specifically, the material used for the insulating layer, the thickness, the method for forming the insulating layer, and other details are all the same.

[0097] <Coating Layer> The thermoelectric conversion module according to the second embodiment of the present invention may include a coating layer. The coating layer used in the second embodiment may be the same as the coating layer used in the first embodiment of the present invention described above. Examples of coating layers include, but are not limited to, a sealing layer, a gas barrier layer, etc. Details of the sealing layer, including the main components constituting the sealing layer, the thickness of the sealing layer, and the method for forming the sealing layer, are all the same. Details of the gas barrier layer, including the main components constituting the gas barrier layer, the thickness of the gas barrier layer, and the method for forming the gas barrier layer, are also the same.

[0098] A thermoelectric conversion module according to a third embodiment of the present invention will be described.

[0099] [Thermoelectric Conversion Module] A thermoelectric conversion module according to a third embodiment of the present invention is a thermoelectric conversion module including a thermally conductive interface member A having adhesive properties on one surface of a thermoelectric conversion element and a heat dissipation member in this order, and a thermally conductive interface member B having adhesive properties on the other surface of the thermoelectric conversion element, wherein the thermal resistance value of the thermally conductive interface member A is R A (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is R AB (mK / W), and the total thermal resistance of the thermoelectric conversion module is R M (mK / W), the R M The R AB The ratio (R AB / R M ) is 1.40 or less, and when the thermally conductive interface member A is bonded to one surface of the thermoelectric conversion element, the shear stress τ applied to the thermally conductive interface member A A (N / mm 2) and the shear stress τ applied to the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the thermoelectric conversion element. B (N / mm 2 ) and each independently 0.001 (N / mm 2 ) or more. The thermoelectric conversion module according to the third embodiment of the present invention is configured to include a thermally conductive interface member A (hereinafter, sometimes simply referred to as "TIMA") having adhesive properties on one surface of a thermoelectric conversion element, a heat dissipation member, and further includes a thermally conductive interface member B (hereinafter, sometimes simply referred to as "TIMB") having adhesive properties on the other surface of the thermoelectric conversion module. In this configuration, the shear stress τ of TIMA A and the shear stress τ of the TIMB B Each of these is independently 0.001 (N / mm 2 ) or more, and the total thermal resistance value R M The total thermal resistance value R of the thermally conductive interface member AB By setting the ratio to 1.40 or less, it is possible to further improve the heat transfer at the interfaces between the members that make up the thermoelectric conversion module, resulting in higher thermoelectric performance.

[0100] In this specification, the configuration of the "thermoelectric conversion module" according to the third embodiment of the present invention includes a "thermoelectric conversion element," an "adhesive thermally conductive interface member A and an adhesive thermally conductive interface member B," and a "heat dissipation member."

[0101] A thermoelectric conversion module according to a third embodiment of the present invention will be described below with reference to the drawings.

[0102] 6 is a cross-sectional view showing an embodiment of a thermoelectric conversion module according to a third embodiment of the present invention. The thermoelectric conversion module 1C includes a thermally conductive interface member A 50a having adhesive properties on one surface of a thermoelectric conversion element 49, a heat dissipation member 51, and a thermally conductive interface member B 50b having adhesive properties on the other surface of the thermoelectric conversion element 49. The thermoelectric conversion element 49 includes chips 44 made of P-type thermoelectric conversion material and chips 45 made of N-type thermoelectric conversion material, which are alternately arranged in series in the in-plane direction of the first substrate 42a and the second substrate 42b, with common first electrodes 43a and second electrodes 43b interposed therebetween. The chips 44 made of P-type thermoelectric material and the chips 45 made of N-type thermoelectric material are bonded to a common first electrode 43a and a common second electrode 43b via a solder-receiving layer 47 and a solder material layer 46, respectively. Furthermore, a heat dissipation layer A 48a and a heat dissipation layer B 48b are provided on the first substrate 42a and the second substrate 42b, in this order. By providing an adhesive thermally conductive interface member A 50a between the outermost heat dissipation layer A 48a on one side of the thermoelectric conversion element 49 and the heat dissipation member 51, the contact thermal resistance generated therebetween can be reduced. Similarly, by providing an adhesive thermally conductive interface member B 50b between the outermost heat dissipation layer B 48b on the other side of the thermoelectric conversion element 49 and, for example, a heat source (not shown), the contact thermal resistance generated therebetween can be reduced. The adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B having such effects are used, and the shear stress τ applied to the adhesive thermally conductive interface member A is A and shear stress τ applied to the adhesive thermally conductive interface member B B Each of these is independently 0.001 (N / mm 2 ) or more, and further, the total thermal resistance value R M The total thermal resistance value R of the thermally conductive interface member having adhesive properties to AB By setting the ratio to 1.40 or less, it is possible to further improve the heat transfer at the interfaces between the members that make up the thermoelectric conversion module, resulting in higher thermoelectric performance.

[0103] When the thermally conductive interface member A is bonded to one surface of the thermoelectric conversion element, the shear stress τ applied to the thermally conductive interface member A is A and shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the thermoelectric conversion element. B are each independently 0.001 (N / mm 2 ) or more. The shear stress τ applied to the thermally conductive interface member A A and shear stress τ applied to the thermally conductive interface member B B are preferably 0.001 (N / mm 2 ) ~ 5.00 (N / mm 2 ), and more preferably 0.01 (N / mm 2 ) ~ 3.00 (N / mm 2 ), and more preferably 0.02 (N / mm 2 ) ~ 1.00 (N / mm 2 ) Shear stress τ A and shear stress τ B When the temperature is within this range, the adhesion between the components constituting the thermoelectric conversion module is improved, and the thermoelectric performance is easily improved without causing physical damage to the chips of P-type thermoelectric conversion material and the chips of N-type thermoelectric conversion material.

[0104] The total thermal resistance value R is the sum of the thermal resistance values ​​of the components that make up the thermoelectric conversion module. M The thermal resistance value R of TIMA A and the thermal resistance value R of TIMB B The total thermal resistance value R AB The ratio (R AB / R M ) is 1.40 or less. AB / R M ) is preferably 0.01 to 1.00, more preferably 0.05 to 0.80, and even more preferably 0.10 to 0.40. AB / R M When the temperature sintering ratio ) is within this range, the heat transfer at the interface between the members is more likely to be improved, and the thermoelectric performance is improved.

[0105] <Thermal Conductive Interface Member A and Thermal Conductive Interface Member B> A thermoelectric conversion module according to a third embodiment of the present invention includes an adhesive thermal conductive interface member A and a heat dissipation member on one surface of a thermoelectric conversion element, and further includes an adhesive thermal conductive interface member B on the other surface of the thermoelectric conversion element. By providing the adhesive thermal conductive interface member A between one surface of the thermoelectric conversion element and the heat dissipation member, the contact thermal resistance generated therebetween can be reduced. Similarly, by providing the adhesive thermal conductive interface member B between the other surface of the thermoelectric conversion element and, for example, a heat source, the contact thermal resistance generated therebetween can be reduced. In this way, the use of the adhesive thermal conductive interface member A and the adhesive thermal conductive interface member B facilitates improved thermal conduction within the thermoelectric conversion element, leading to improved thermoelectric performance of the thermoelectric conversion module.

[0106] The adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B are preferably pressure-sensitive adhesive layers. Hereinafter, the "adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B" may be collectively referred to simply as the "thermal conductive interface member."

[0107] The adhesive used in the adhesive layer can be the same as that in the first embodiment.

[0108] In order to improve the thermal conductivity, the adhesive layer may be filled with a thermally conductive filler, which may be the same as that used in the second embodiment.

[0109] The thickness of the thermally conductive interface member is the same as in the second embodiment.

[0110] Examples of commercially available thermally conductive interface members include those similar to those in the second embodiment.

[0111] <Heat Dissipation Member> As the heat dissipation member, the same member as in the first embodiment can be used.

[0112] <Heat Dissipation Layer> In the thermoelectric conversion element, from the viewpoint of efficiently applying a temperature difference to the chip of the thermoelectric conversion material, it is preferable to further provide a heat dissipation layer on at least one surface of the substrate. The material used for the heat dissipation layer is not particularly limited, and known materials can be used. Preferably, the material is selected from gold, silver, copper, nickel, tin, iron, chromium, platinum, palladium, rhodium, iridium, ruthenium, osmium, indium, zinc, molybdenum, manganese, titanium, aluminum, stainless steel, and brass.

[0113] The method for laminating the heat dissipation layer is not particularly limited, but includes dry processes such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), or various coating methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade, as well as wet processes such as electrodeposition, silver halide plating, electroplating, and electroless plating. Furthermore, patterning of the heat dissipation layer can be performed using known physical or chemical processes, primarily photolithography, or a combination of these. The thermal conductivity of each heat dissipation layer is preferably 5 to 500 W / (m·K), more preferably 8 to 500 W / (m·K), even more preferably 10 to 450 W / (m·K), particularly preferably 12 to 420 W / (m·K), and most preferably 15 to 400 W / (m·K).

[0114] The thickness of the heat dissipation layer is determined appropriately from the viewpoint of thermoelectric performance, but is preferably 1 to 550 μm, more preferably 10 to 400 μm, and even more preferably 30 to 200 μm.

[0115] The adhesive strength of the thermally conductive interface member A to the heat dissipation layer and the adhesive strength of the thermally conductive interface member B to the heat dissipation layer are each independently preferably 0.01 (N / cm) to 50.0 (N / cm), more preferably 0.05 (N / cm) to 25.0 (N / cm), and even more preferably 0.10 (N / cm) to 10.0 (N / cm). When the adhesive strength of the thermally conductive interface member A to the heat dissipation layer and the adhesive strength of the thermally conductive interface member B to the heat dissipation layer are within these ranges, the desired thermal conductivity is maintained while the adhesion between the components constituting the thermoelectric conversion module is improved, and thermoelectric performance is easily improved without causing physical damage to the P-type thermoelectric conversion material chips and the N-type thermoelectric conversion material chips.

[0116] (Thermoelectric Conversion Material Chip) The thermoelectric conversion material chip used in the third embodiment of the present invention is preferably formed by dividing a thermoelectric conversion material layer made of a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (hereinafter sometimes referred to as "thermoelectric semiconductor particles"), a binder resin, and an ionic compound (ionic liquid, inorganic ionic compound).

[0117] (Thermoelectric Semiconductor Material) As the thermoelectric semiconductor material used in the third embodiment of the present invention, the same material as the thermoelectric semiconductor material used in the first embodiment of the present invention described above can be used, and the content (blending amount) in the thermoelectric semiconductor composition is also the same.

[0118] (Binder Resin) The binder resin used in the third embodiment of the present invention has the effect of physically bonding thermoelectric semiconductor materials (thermoelectric semiconductor particles) together, and can increase the flexibility of the thermoelectric conversion module and facilitate the formation of a thin film by coating or the like.

[0119] The binder resin is appropriately selected depending on the heat treatment temperature and the baking (annealing) temperature of the thermoelectric semiconductor material. It is preferable to heat-treat the binder resin at a temperature higher than its decomposition temperature. Furthermore, a resin that maintains its physical properties, such as mechanical strength and thermal conductivity, without being impaired when a coating film made of a thermoelectric semiconductor composition is subjected to heat treatment or the like to cause crystal growth of thermoelectric semiconductor particles is more preferable. In this specification, the "decomposition temperature" refers to the temperature at which the mass loss rate measured by thermogravimetry (TG) is 100% (the mass after decomposition is less than 1% of the mass before decomposition). The decomposition temperature of the binder resin is preferably 150 to 400°C, and it is preferable that 90% or more by mass is decomposed and vaporized.

[0120] Thermoplastic resins and curable resins can be used as such binder resins. Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, polyisobutylene, and polymethylpentene; polycarbonate; thermoplastic polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyvinyl polymers such as polystyrene, acrylonitrile-styrene copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, vinyl chloride, polyvinylpyridine, polyvinyl alcohol, and polyvinylpyrrolidone; polyurethane; and cellulose derivatives such as ethyl cellulose. Examples of curable resins include thermosetting resins and photocurable resins. Examples of thermosetting resins include epoxy resins and phenolic resins. Examples of photocurable resins include photocurable acrylic resins, photocurable urethane resins, and photocurable epoxy resins. These resins may be used alone or in combination of two or more. Among these, thermoplastic resins are preferred, with polycarbonate and cellulose derivatives such as ethyl cellulose being more preferred, and polycarbonate being particularly preferred.

[0121] The content of the binder resin in the thermoelectric semiconductor composition is preferably 0.1 to 20% by mass, more preferably 0.5 to 15% by mass, and even more preferably 1.0 to 10% by mass.

[0122] <Ionic Compound> (Ionic Liquid) As the ionic liquid used in the third embodiment of the present invention, the same ionic liquid as the ionic liquid used in the first embodiment of the present invention described above can be used, and the content (blending amount) in the thermoelectric semiconductor composition is also the same.

[0123] (Inorganic ionic compound) As the inorganic ionic compound used in the third embodiment of the present invention, the same inorganic ionic compound as used in the first embodiment of the present invention described above can be used, and the content (blending amount) in the thermoelectric semiconductor composition is also the same.

[0124] (Other Additives) The thermoelectric semiconductor composition used in the third embodiment of the present invention may further contain, as necessary, other additives other than those described above, such as dispersants, film-forming aids, light stabilizers, antioxidants, tackifiers, plasticizers, colorants, resin stabilizers, fillers, pigments, conductive fillers, conductive polymers, curing agents, etc. These additives may be used alone or in combination of two or more.

[0125] (Method for Preparing Thermoelectric Semiconductor Composition) The method for preparing the thermoelectric semiconductor composition is not particularly limited. For example, the thermoelectric semiconductor particles, the binder resin, the ionic compound, and optionally the other additives, as well as a solvent, may be mixed and dispersed by a known method such as an ultrasonic homogenizer, a spiral mixer, a planetary mixer, a disperser, or a hybrid mixer to prepare the thermoelectric semiconductor composition. Examples of the solvent include toluene, ethyl acetate, methyl ethyl ketone, alcohol, tetrahydrofuran, methylpyrrolidone, and ethyl cellosolve. These solvents may be used alone or in combination of two or more. The solids concentration of the thermoelectric semiconductor composition is not particularly limited as long as the composition has a viscosity suitable for coating.

[0126] The coating film made of the thermoelectric semiconductor composition is not particularly limited, but can be formed, for example, by applying the thermoelectric semiconductor composition to a substrate such as glass, alumina, silicon, or resin to obtain a coating film and drying it. Methods for applying the thermoelectric semiconductor composition to obtain a coating film include known methods such as screen printing, flexographic printing, gravure printing, spin coating, dip coating, die coating, spray coating, bar coating, and doctor blade coating, and are not particularly limited. When forming a patterned coating film, preferred methods include screen printing and slot die coating, which allow for easy pattern formation using a screen plate with a desired pattern. The resulting coating film is then dried to form a coating film. Conventional drying methods, such as hot air drying, hot roll drying, and infrared irradiation, can be used. The heating temperature is typically 80 to 150°C, and the heating time varies depending on the heating method, but is typically several seconds to several tens of minutes. Furthermore, when a solvent is used in preparing the thermoelectric semiconductor composition, the heating temperature is not particularly limited as long as it is within a temperature range that can dry the solvent used. Furthermore, the dried coating film may be subjected to a hot press (heat and pressure) treatment to form a thermoelectric conversion material layer precursor for purposes such as suppressing voids in the thermoelectric conversion material chip and improving electrical conductivity. The hot press (heat and pressure) treatment can be performed, for example, using a device such as a hydraulic press to apply pressure to the entire upper surface of the coating film at a predetermined temperature and in an atmospheric atmosphere for a predetermined time. The temperature of the hot press (heat and pressure) treatment is not particularly limited, but is typically 100 to 300°C, preferably 200 to 300°C. The pressure of the hot press (heat and pressure) treatment is not particularly limited, but is typically 20 to 200 MPa, preferably 50 to 150 MPa. The duration of the hot press (heat and pressure) treatment is not particularly limited, but is typically several seconds to several tens of minutes, preferably several tens of seconds to several tens of minutes.

[0127] The obtained thermoelectric conversion material layer precursor is preferably subjected to a firing (annealing) treatment to stabilize the thermoelectric performance and promote crystal growth of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition, thereby forming a thermoelectric conversion material layer. The firing (annealing) treatment is not particularly limited, but is typically carried out under an inert gas atmosphere such as nitrogen or argon, a reducing gas atmosphere, or vacuum conditions with a controlled gas flow rate. The firing (annealing) temperature depends on the thermoelectric semiconductor particles, binder resin, ionic liquid, inorganic ionic compound, etc. used in the thermoelectric semiconductor composition and is adjusted as appropriate; however, it is typically carried out at 260 to 600°C, preferably 280 to 550°C. The firing (annealing) treatment time is not particularly limited, but is typically from several minutes to several tens of hours, preferably from several minutes to several hours.

[0128] The thermoelectric conversion material chips used in the third embodiment of the present invention are obtained by dicing the thermoelectric conversion material layer. There are no particular limitations on the method of dicing, but from the viewpoints of processing accuracy and process stability, it is preferable to attach a dicing tape and use a dicing blade.

[0129] <Substrate> As the substrate of the thermoelectric conversion module used in the third embodiment of the present invention, for example, the first substrate 2 a and the second substrate 2 b are preferably made of a plastic film that does not affect the decrease in electrical conductivity or the increase in thermal conductivity of the thermoelectric conversion material chip. Even when the thermoelectric conversion material layer is annealed, the substrate does not thermally deform, and the performance of the thermoelectric conversion module can be maintained. In view of high heat resistance and dimensional stability, the plastic film is preferably a polyimide film, a polyamide film, a polyetherimide film, a polyaramid film, a polyamideimide film, or a glass-epoxy sheet.

[0130] The thickness of the plastic film used for the substrate is preferably 1 to 1000 μm, more preferably 10 to 500 μm, and even more preferably 20 to 100 μm, from the viewpoints of flexibility, heat resistance, and dimensional stability.

[0131] <Electrodes> There are no particular limitations on the metal material used as the electrodes of the thermoelectric conversion module used in the third embodiment of the present invention. For example, examples of the metal material for the first electrode 3a and the second electrode 3b include gold, nickel, aluminum, rhodium, platinum, chromium, palladium, stainless steel, molybdenum, and alloys containing any of these metals. Furthermore, the electrodes may be formed using a paste material containing a solvent and a resin component in addition to the metal material. When using a paste material, it is preferable to remove the solvent and resin component by firing or the like. Examples of paste materials include silver paste and aluminum paste. The thickness of the electrode layer is preferably 10 nm to 200 μm, more preferably 30 nm to 150 μm, and even more preferably 50 nm to 120 μm. When the thickness of the electrode layer is within the above range, the electrical conductivity is high and the resistance is low, resulting in sufficient strength as an electrode.

[0132] Examples of methods for forming electrodes include methods of processing into a predetermined pattern shape by known physical or chemical treatments, mainly photolithography, or a combination of these, or methods of forming an electrode pattern by screen printing, stencil printing, inkjet printing, etc. Examples of methods for forming electrodes without a pattern include vacuum film formation methods such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), various coating methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade methods, wet processes such as electrodeposition, silver halide plating, electrolytic plating, electroless plating, and metal foil lamination, and the like, and these methods are appropriately selected depending on the metal material. The electrodes used in the third embodiment of the present invention are required to have high conductivity. Since electrodes formed by plating or vacuum deposition can easily achieve high conductivity, vacuum deposition methods such as vacuum deposition and sputtering, as well as electroplating and electroless plating are preferred. Depending on the dimensions and dimensional accuracy of the formed pattern, a hard mask such as a metal mask may be used to easily form a pattern. Furthermore, when forming a film by vacuum deposition, the substrate may be heated to a temperature within a range that does not impair the properties of the substrate, for the purposes of improving adhesion to the substrate and removing moisture. When forming a film by plating, electroplating may be performed on a film formed by electroless plating.

[0133] <Solder Material Layer> The solder material layer is used to join the thermoelectric conversion material chip and the electrode. The solder material constituting the solder material layer may be appropriately selected taking into consideration the heat resistance temperature and the like of the binder resin contained in the substrate and the thermoelectric conversion material chip, as well as electrical conductivity and thermal conductivity, and examples of known materials include Sn, Sn / Pb alloy, Sn / Ag alloy, Sn / Cu alloy, Sn / Sb alloy, Sn / In alloy, Sn / Zn alloy, Sn / In / Bi alloy, Sn / In / Bi / Zn alloy, Sn / Bi / Pb / Cd alloy, Sn / Bi / Pb alloy, Sn / Bi / Cd alloy, Bi / Pb alloy, Sn / Bi / Zn alloy, Sn / Bi alloy, Sn / Bi / Pb alloy, Sn / Pb / Cd alloy, and Sn / Cd alloy. From the viewpoints of lead-free and / or cadmium-free, melting point, electrical conductivity, and thermal conductivity, alloys such as 43Sn / 57Bi alloy, 42Sn / 58Bi alloy, 40Sn / 56Bi / 4Zn alloy, 48Sn / 52In alloy, and 39.8Sn / 52In / 7Bi / 1.2Zn alloy are preferred. Commercially available solder materials include the following: 42Sn / 58Bi alloy (manufactured by Tamura Corporation, product name: SAM10-401-27), 41Sn / 58Bi / Ag alloy (manufactured by Nippon Handa Co., Ltd., product name: PF141-LT7HO), and 96.5Sn3Ag0.5Cu alloy (manufactured by Nippon Handa Co., Ltd., product name: PF305-207BTO).

[0134] The thickness of the solder material layer (after heating and cooling) is preferably 10 to 200 μm, more preferably 20 to 150 μm, even more preferably 30 to 130 μm, and particularly preferably 40 to 120 μm. When the thickness of the solder material layer is within this range, adhesion between the thermoelectric conversion material chip and the electrode can be easily obtained.

[0135] Methods for applying the solder material onto the substrate include known methods such as stencil printing, screen printing, dispensing, etc. The heating temperature varies depending on the solder material, resin film, etc. used, but is usually 150 to 280°C for 3 to 20 minutes.

[0136] <Solder Receiving Layer> The solder receiving layer has the function of improving the bonding strength between the chip of thermoelectric conversion material containing resin and the solder material layer on the opposing electrode side that constitutes the thermoelectric conversion module, and is directly bonded to the chip of thermoelectric conversion material.

[0137] The solder-receiving layer preferably contains a metal material. The metal material is preferably at least one selected from gold, silver, nickel, aluminum, rhodium, platinum, chromium, palladium, tin, and an alloy containing any of these metal materials. Among these, a gold, silver, nickel, aluminum, or two-layer structure of tin and gold is preferred, and silver, nickel, and aluminum are more preferred from the viewpoints of material cost, high thermal conductivity, and bonding stability.

[0138] The thickness of the solder-receiving layer is preferably 10 nm to 50 μm, more preferably 200 nm to 10 μm, and particularly preferably 500 nm to 5 μm. When the solder-receiving layer is within this thickness range, it provides excellent adhesion to the surface of the thermoelectric conversion material chip and to the surface of the solder material layer on the electrode side that constitutes the thermoelectric conversion module, resulting in a highly reliable bond. Furthermore, high electrical conductivity as well as high thermal conductivity can be maintained, resulting in the thermoelectric performance of the thermoelectric conversion module being maintained without any degradation. The solder-receiving layer may be formed as a single layer using a metal material, or may be formed as a multilayer by laminating two or more metal materials.

[0139] The solder-receiving layer is preferably formed using the above-mentioned metal material. Since the solder-receiving layer is required to have high electrical conductivity and high thermal conductivity in order to maintain thermoelectric performance, it is preferable to use a solder-receiving layer formed by electroplating, electroless plating, or vacuum deposition.

[0140] The thermoelectric conversion module according to the third embodiment of the present invention has high thermoelectric performance with improved heat transfer effect at the interface between members.

[0141] Next, the first embodiment of the present invention will be described in more detail with reference to examples, but the first embodiment of the present invention is not limited to these examples in any way.

[0142] The electromotive force and the embedded amount of TIM of the thermoelectric conversion modules fabricated in the examples and comparative examples of the first embodiment of the present invention were evaluated by the following methods.

[0143] (a) Electromotive Force Evaluation (Output Evaluation) FIG. 3 is a cross-sectional view showing an example of an electromotive force evaluation configuration for a thermoelectric conversion module according to the first embodiment of the present invention. In the thermoelectric conversion module electromotive force evaluation configuration 31A, a heat dissipation member 35 [folding fin OPFF, manufactured by Mogami Inks Co., Ltd.] was installed on the surface of one thermally conductive interface member A 33a of an in-plane type thermoelectric conversion module 32 obtained in the examples and comparative examples. A temperature controller (heat source) 34 (product name: Peltier temperature controller set VTH1.8-70S, manufactured by Vicks Co., Ltd.) was installed on the surface of the other thermally conductive interface member B 33b. The temperature controller (heat source) 34 was set to 60°C to apply a temperature difference from the outside. To ensure close contact between the components, a heat insulating material 36 [polycarbonate hollow board, product number KTP4534W, manufactured by Hikarisha Co., Ltd.] was interposed on the heat dissipation member 35, and a load member 37 [precision weight, stainless steel, 27 gf / cm, manufactured by Murakami Scale Co., Ltd.] was installed on the heat dissipation member 35. 2 ] was used to apply a load. With a temperature difference applied, the electromotive force between the extraction electrodes was measured using a Digital HiTester (manufactured by Hioki E.E. Corporation, model number: 3801-50). (b) Evaluation of Thermal Resistance Value The thermal resistance value (K / W) of the TIM used in the examples and comparative examples was determined by the thermal conductivity [W / (m K)], thickness (m), and effective area [0.07 (m) × 0.065 (m) = 4.5 × 10 -3 (m 2 ) )] was used to calculate the thermal resistance value of the TIM from the following formula (1): Thermal resistance value of the TIM = Thickness of the TIM / (Thermal conductivity of the TIM × Effective area) (1) Similarly, the thermal conductivity, thickness, and effective area of ​​each of the following layers constituting the in-plane thermoelectric conversion module were calculated. Polyimide film substrate: Thermal conductivity 0.29 [W / (m K)]; Thickness 5.0 × 10 -5 (m); effective area 4.5 × 10 -3 (m 2 ) Electrode layer: Thermal conductivity 398 [W / (m K)]; Thickness 1.2 × 10 -5 (m); effective area 2.48 × 10 -3 (m 2) Thermoelectric element layer: thermal conductivity 0.5 [W / (m K)]; thickness 8.0 × 10 -5 (m); effective area 1.86 × 10 -3 (m 2 ) Adhesive layer: Thermal conductivity 0.17 [W / (m K)]; Thickness 5.0 × 10 -6 (m); effective area 4.5 × 10 -3 (m 2 ) Coating layer (Al / PET sealing layer): Thermal conductivity 0.3 [W / (m K)]; Thickness 1.2 × 10 -5 (m); effective area 4.5 × 10 -3 (m 2 High thermal conductivity layer: thermal conductivity 398 [W / (m·K)]; thickness 2.0×10 -4 (m); effective area 2.28 × 10 -3 (m 2 From the above, the thermal resistance value R of the thermally conductive interface member A A (mK / W), thermal resistance value R of thermally conductive interface member B B (mK / W) AB (mK / W) and the total thermal resistance R of the in-plane thermoelectric conversion module. M (mK / W) is calculated, and R M R against AB The ratio (R AB / R M (c) Evaluation of Embeddability The embedding depth of the thermally conductive interface member TIM embedded between the high thermal conductivity layers was measured by cross-sectional observation using a digital microscope (manufactured by Keyence Corporation, model name: VHX-5000), and the ratio of the embedding depth of the thermally conductive interface member TIM embedded between the high thermal conductivity layers to the thickness of the high thermal conductivity layers (embeddability) was calculated.

[0144] (Example 1) (Method of Producing Thermoelectric Semiconductor Particles) P-type bismuth telluride Bi, a bismuth-tellurium-based thermoelectric semiconductor material, was prepared. 0.4 Te 3 Sb 1.6(manufactured by Kojundo Chemical Laboratory, maximum particle size: 90 μm or less) was pulverized using a planetary ball mill (manufactured by Fritsch Japan, Premium Line P-7) to produce thermoelectric semiconductor particles T1 with an average particle size of 2.0 μm. 2 Te 3 (manufactured by Kojundo Chemical Laboratory, maximum particle size: 90 μm or less) was pulverized in the same manner as above to produce thermoelectric semiconductor particles T2 with an average particle size of 4.0 μm. The average particle sizes of thermoelectric semiconductor particles T1 and T2 were obtained by measuring the particle size distribution using a laser diffraction particle size analyzer (Malvern Mastersizer 3000).

[0145] (Preparation of Thermoelectric Semiconductor Composition) Coating Liquid (P) The P-type bismuth telluride Bi 0.4 Te 3 Sb 1.6 A coating liquid (P) consisting of a thermoelectric semiconductor composition was prepared by mixing and dispersing 75.7 parts by mass of the particles, 2.41 parts by mass of polyamideimide as a binder resin, 8.8 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 13.09 parts by mass of N-methylpyrrolidone as a solvent. 2 Te 3 A coating liquid (N) was prepared, which was a thermoelectric semiconductor composition obtained by mixing and dispersing 82.3 parts by mass of particles, 2.51 parts by mass of polyamideimide as a binder resin, 4.5 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 10.69 parts by mass of N-methylpyrrolidone as a solvent.

[0146] (Electrode Formation and Arrangement) Figure 2 is a plan view showing the configuration of the thermoelectric element layer used in the example. (a) shows a conceptual diagram of the arrangement of electrodes formed on a film substrate, and (b) shows a conceptual diagram of the arrangement of P-type and N-type thermoelectric element layers formed on the electrodes. A polyimide film substrate (manufactured by Ube Exsymo Co., Ltd., product name: Upicel N, polyimide substrate thickness: 50 μm, copper foil: 9 μm) with copper foil attached was prepared. The copper foil on the polyimide film substrate 22 was wet-etched using a ferric chloride solution to form an electrode pattern (single layer) 23P made of copper foil arranged corresponding to the arrangement of the P-type thermoelectric element layer 24 and the N-type thermoelectric element layer 25 described below. The main electrode 23a was formed with a size of 550 μm x 800 μm so as to straddle the boundaries of adjacent P-type thermoelectric element layer 24 and N-type thermoelectric element layer 25 in the arrangement of the thermoelectric element layer 26 described below. Here, 23b denotes an electrode portion (size: 3 mm × 5 mm) for extracting electromotive force, and 23c denotes a connecting electrode portion (size: 550 μm × 2.4 mm) for connecting each row of thermoelectric element layers 26. A nickel layer (thickness: 3 μm) was laminated on the patterned copper foil by electroless plating, and then a gold layer (thickness: 40 nm) was laminated on the nickel layer by electroless plating, thereby forming an electrode pattern (laminate) 23Q.

[0147] (Production of Thermoelectric Element Layer) The coating solution (N) prepared above was applied to the electrode pattern (laminate) 23Q on the polyimide film substrate 22 by screen printing using a printing plate with a thickness of 80 μm and an opening of 1 mm × 0.8 mm, and dried at a temperature of 125 ° C. for 10 minutes in air. Next, similarly, the coating solution (P) prepared above was applied to the electrode pattern (laminate) 23Q on the polyimide film substrate 22 using a printing plate with a thickness of 30 μm and an opening of 1 mm × 0.8 mm, and dried at a temperature of 125 ° C. for 10 minutes in air. Furthermore, each of the obtained thin films was heated at a heating rate of 5 K / min in an atmosphere of a hydrogen and argon mixed gas (hydrogen:argon = 3 vol%: 97 vol%), and held at 310 ° C. for 30 minutes, thereby performing an annealing treatment after thin film formation, thereby causing crystal growth of the particles of the thermoelectric semiconductor material, and a P-type thermoelectric element layer 24 and an N-type thermoelectric element layer 25 were produced. The resulting N-type thermoelectric element layer had a thickness of 80 μm, and the P-type thermoelectric element layer had a thickness of 90 μm.

[0148] (Arrangement of Thermoelectric Element Layer) The resulting P-type thermoelectric element layers 24, each measuring 1 mm x 0.8 mm x 80 μm, and N-type thermoelectric element layers 25, each measuring 1 mm x 0.8 mm x 90 μm, were alternately arranged, adjacent to each other along 0.8 mm sides, forming pairs. In the thermoelectric element layer 26, 408 pairs of P-type thermoelectric element layers 24 and N-type thermoelectric element layers 25 were formed, and were arranged electrically in series within the surface of the polyimide film substrate 22 to form the thermoelectric element layer 26. The P-type thermoelectric element layers 24 and N-type thermoelectric element layers 25 were electrically connected by main electrodes 23 a. The thermoelectric element layer 26 had a folded structure. Specifically, 24 rows were arranged, with 17 pairs of P-type thermoelectric element layers 24 and N-type thermoelectric element layers 25 connected to each other via connecting electrodes 23 c. It should be noted that FIG. 2 shows a conceptual arrangement of the electrodes and thermoelectric element layers, and the dimensions, number, etc. of the electrodes and thermoelectric element layers that are actually fabricated will differ.

[0149] (Arrangement of the coating layer and the high thermal conductivity layer) An aluminum vapor-deposited PET film (manufactured by BAX, thickness: 12 μm) was used as the insulating layer, and a coating layer was prepared by laminating an adhesive layer (manufactured by Somar, product name: EP-0002EF-01MB, thickness: 25 μm) on both sides of the insulating layer. The lamination was performed at a temperature of 80°C. The above-mentioned coating layer was interposed on the upper surface (surface of the thermoelectric element layer) of the prepared substrate with a thermoelectric element layer, and a coating layer consisting of a single layer of adhesive layer (manufactured by Somar, product name: EP-0002EF-01MB, thickness: 25 μm) was interposed on the lower surface (the surface of the substrate opposite to the surface on which the thermoelectric element layer was provided), and high thermal conductivity layers made of a high thermal conductivity material (copper foil) [C1020, thickness: 200 μm, width: 1 mm, length: 100 mm, spacing: 1 mm, thermal conductivity: 398 (W / (m·K))] were intermittently arranged above and below the area where the P-type thermoelectric element layer and the N-type thermoelectric element layer were adjacent, so as to be staggered. In this case, the coating layer provided on the upper surface of the substrate with a thermoelectric element layer was positioned so that the aluminum-deposited surface of the aluminum-deposited PET film was distal from the thermoelectric element layer. The coating layer was laminated onto the thermoelectric element layer and the adhesive layer was laminated onto the substrate under vacuum conditions at a temperature of 80°C and a pressure of 0.2 MPa for 10 seconds. The high thermal conductivity layer was laminated onto the coating layer and adhesive layer under vacuum conditions at a temperature of 80°C. The thermoelectric conversion module was then left to stand in an environment of 150°C for 30 minutes to cure the adhesive layer, thereby obtaining an in-plane type thermoelectric conversion module.

[0150] (Arrangement of TIM) The in-plane type thermoelectric conversion module was fabricated with R on the top and bottom surfaces. AB / R M A TIM [manufactured by Sekisui Polymatech Co., Ltd., product number: Manion 50α, thickness: 0.50 mm, thermal conductivity: 17 W / (m K)] satisfying a thermal conductivity of 0.08 was installed, and the electromotive force between the extraction electrodes of the obtained thermoelectric conversion module was measured based on the above-mentioned (a) electromotive force evaluation (output evaluation).

[0151] (Example 2) In Example 1, R AB / R MThe electromotive force between the extraction electrodes was measured in the same manner as in Example 1, except that a TIM [manufactured by Sekisui Polymatech Co., Ltd., product number: PT-V, thickness: 0.50 mm, thermal conductivity: 12 W / (m·K)] satisfying a thermal conductivity of 0.12 was installed.

[0152] (Example 3) In Example 1, R AB / R M The electromotive force between the extraction electrodes was measured in the same manner as in Example 1, except that a TIM [manufactured by 3M, product number: 8926, thickness: 0.20 mm, thermal conductivity: 1.5 W / (m·K)] satisfying a thermal conductivity of 0.38 was installed.

[0153] Comparative Example 1 The electromotive force between the extraction electrodes was measured in the same manner as in Example 1, except that no TIM was provided on the top and bottom surfaces of the in-plane type thermoelectric conversion module.

[0154] (Comparative Example 2) In Example 1, R AB / R M The electromotive force between the extraction electrodes was measured in the same manner as in Example 1, except that a TIM [manufactured by 3M, product number: VHR0601, thickness: 0.30 mm, thermal conductivity: 0.6 W / (m·K)] satisfying a thermal conductivity of 1.44 was installed.

[0155] Table 1 shows the evaluation results of the embeddability of the TIM and the electromotive force of the thermoelectric conversion modules obtained in Examples 1 to 3 and Comparative Examples 1 and 2.

[0156]

[0157] High embeddability, R M R against AB The ratio (R AB / R M The electromotive force obtained from the thermoelectric conversion modules of Examples 1 to 3, in which the R M R against AB The ratio (R AB / R M ) is higher than the electromotive force obtained from the thermoelectric conversion modules of Comparative Examples 1 and 2 which do not satisfy the requirements according to the first embodiment of the present invention, and it can be seen that the thermoelectric performance is improved.

[0158] ​Next, the second embodiment of the present invention will be described in more detail with reference to examples, but the second embodiment of the present invention is not limited to these examples in any way.

[0159] (a) Shear Stress Evaluation The TIM (10 mm × 10 mm) used in the examples and comparative examples of the second embodiment of the present invention was attached to a copper plate (45 mm × 45 mm × 3 mm thick), and a copper chip (5 mm × 5 mm × 200 μm thick) was attached to the surface of the TIM opposite to the copper plate. Using a bond tester Dage Series 4000 (manufactured by Nordson Dage), a die shear test was performed at a test speed of 200 μm / s and a test height of 1 μm to measure the shear stress (N / mm 2) was measured. (b) Adhesion Strength Evaluation The TIM (25 mm × 40 mm) used in the Examples and Comparative Examples was attached to a copper plate (100 mm × 100 mm × 3.0 mm thick), and then bonded to the copper plate by rolling it back and forth once using a 2 kg roll (φ95 mm, material: rubber). After 24 hours, the 90-degree peel strength was measured at a peel rate of 300 mm / min using a universal tensile strength tester (manufactured by Shimadzu Corporation, model name: Autograph AG-X Plus) in an atmosphere of 23°C and 50% RH, and the result was taken as the adhesion strength (N / cm). (c) Electromotive Force Evaluation (Output Evaluation) FIG. 5 is a cross-sectional view showing an example of an electromotive force evaluation configuration for a thermoelectric conversion module according to a second embodiment of the present invention. In the thermoelectric conversion module electromotive force evaluation configuration 31B, a heat dissipation member 35 [folding fin OPFF, manufactured by Mogami Inks Co., Ltd.] was installed on one surface of the adhesive thermally conductive interface member A 33c on the in-plane type thermoelectric conversion module 32 obtained in the Examples and Comparative Examples, and a temperature controller (heat source) 34 (manufactured by Vicks Co., Ltd., product name: Peltier temperature controller set VTH1.8-70S) was installed on the other surface of the adhesive thermally conductive interface member B 33d. The temperature controller (heat source) 34 was set to 60°C, and a temperature difference was applied from the outside. With the temperature difference applied, the electromotive force between the extraction electrodes was measured using a Digital HiTester (manufactured by Hioki E.E. Corporation, model name: 3801-50). (d) Evaluation of Thermal Resistance Value The thermal resistance value (K / W) of the TIM used in the examples and comparative examples was determined by the thermal conductivity [W / (m K)], thickness (m), and effective area [0.07 (m) × 0.065 (m) = 4.5 × 10 -3 (m 2 ) )] was used to calculate the thermal resistance value of the TIM from the following formula (1): Thermal resistance value of the TIM = Thickness of the TIM / (Thermal conductivity of the TIM × Effective area) (1) Similarly, the thermal conductivity, thickness, and effective area of ​​each of the following layers constituting the in-plane thermoelectric conversion module were calculated. Polyimide film substrate: Thermal conductivity 0.29 [W / (m K)]; Thickness 5.0 × 10 -5 (m); effective area 4.5 × 10 -3 (m 2 ) Electrode layer: Thermal conductivity 398 [W / (m K)]; Thickness 1.2 × 10 -5 (m); effective area 2.48 × 10-3 (m 2 ) Thermoelectric element layer: thermal conductivity 0.5 [W / (m K)]; thickness 8.0 × 10 -5 (m); effective area 1.86 × 10 -3 (m 2 ) Adhesive layer: Thermal conductivity 0.17 [W / (m K)]; Thickness 5.0 × 10 -6 (m); effective area 4.5 × 10 -3 (m 2 ) Coating layer (Al / PET sealing layer): Thermal conductivity 0.3 [W / (m K)]; Thickness 1.2 × 10 -5 (m); effective area 4.5 × 10 -3 (m 2 High thermal conductivity layer: thermal conductivity 398 [W / (m·K)]; thickness 2.0×10 -4 (m); effective area 2.28 × 10 -3 (m 2 From the above, the thermal resistance value R of the thermally conductive interface member A A (mK / W), thermal resistance value R of thermally conductive interface member B B (mK / W) AB (mK / W) and the total thermal resistance R of the in-plane thermoelectric conversion module. M (mK / W) is calculated, and R M R against AB The ratio (R AB / R M ) was calculated.

[0160] (Example 4) (Method of Producing Thermoelectric Semiconductor Particles) P-type bismuth telluride Bi, a bismuth-tellurium-based thermoelectric semiconductor material, was prepared. 0.4 Te 3 Sb 1.6 (manufactured by Kojundo Chemical Laboratory, maximum particle size: 90 μm or less) was pulverized using a planetary ball mill (manufactured by Fritsch Japan, Premium Line P-7) to produce thermoelectric semiconductor particles T1 with an average particle size of 2.0 μm. 2 Te 3(manufactured by Kojundo Chemical Laboratory, maximum particle size: 90 μm or less) was pulverized in the same manner as above to produce thermoelectric semiconductor particles T2 with an average particle size of 4.0 μm. The average particle sizes of thermoelectric semiconductor particles T1 and T2 were obtained by measuring the particle size distribution using a laser diffraction particle size analyzer (Malvern Mastersizer 3000).

[0161] (Preparation of Thermoelectric Semiconductor Composition) Coating Liquid (P) The P-type bismuth telluride Bi 0.4 Te 3 Sb 1.6 A coating liquid (P) was prepared from a thermoelectric semiconductor composition in which 75.7 parts by mass of the particles, 2.41 parts by mass of polyamideimide as a binder resin, 8.8 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 13.09 parts by mass of N-methylpyrrolidone as a solvent were mixed and dispersed. 2 Te 3 A coating liquid (N) was prepared, which was a thermoelectric semiconductor composition obtained by mixing and dispersing 82.3 parts by mass of particles, 2.51 parts by mass of polyamideimide as a binder resin, 4.5 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 10.69 parts by mass of N-methylpyrrolidone as a solvent.

[0162] (Electrode Formation and Arrangement) Figure 2 is a plan view showing the configuration of the thermoelectric element layer used in the example. (a) shows a conceptual diagram of the arrangement of electrodes formed on a film substrate, and (b) shows a conceptual diagram of the arrangement of P-type and N-type thermoelectric element layers formed on the electrodes. A polyimide film substrate (manufactured by Ube Exsymo Co., Ltd., product name: Upicel N, polyimide substrate thickness: 50 μm, copper foil: 9 μm) with copper foil attached was prepared. The copper foil on the polyimide film substrate 22 was wet-etched using a ferric chloride solution to form an electrode pattern (single layer) 23P made of copper foil arranged corresponding to the arrangement of the P-type thermoelectric element layer 24 and the N-type thermoelectric element layer 25 described below. The main electrode 23a was formed with a size of 550 μm x 800 μm so as to straddle the boundaries of adjacent P-type thermoelectric element layer 24 and N-type thermoelectric element layer 25 in the arrangement of the thermoelectric element layer 26 described below. Here, 23b denotes an electrode portion (size: 3 mm × 5 mm) for extracting electromotive force, and 23c denotes a connecting electrode portion (size: 550 μm × 2.4 mm) for connecting each row of thermoelectric element layers 26. A nickel layer (thickness: 3 μm) was laminated on the patterned copper foil by electroless plating, and then a gold layer (thickness: 40 nm) was laminated on the nickel layer by electroless plating, thereby forming an electrode pattern (laminate) 23Q.

[0163] (Production of Thermoelectric Element Layer) The coating solution (N) prepared above was applied to the electrode pattern (laminate) 23Q on the polyimide film substrate 22 by screen printing using a printing plate with a thickness of 80 μm and an opening of 1 mm × 0.8 mm, and dried at a temperature of 125 ° C. for 10 minutes in air. Next, similarly, the coating solution (P) prepared above was applied to the electrode pattern (laminate) 23Q on the polyimide film substrate 22 using a printing plate with a thickness of 30 μm and an opening of 1 mm × 0.8 mm, and dried at a temperature of 125 ° C. for 10 minutes in air. Furthermore, each of the obtained thin films was heated at a heating rate of 5 K / min in an atmosphere of a hydrogen and argon mixed gas (hydrogen:argon = 3 vol%: 97 vol%), and held at 310 ° C. for 30 minutes, thereby performing an annealing treatment after thin film formation, thereby causing crystal growth of the particles of the thermoelectric semiconductor material, and a P-type thermoelectric element layer 24 and an N-type thermoelectric element layer 25 were produced. The resulting N-type thermoelectric element layer had a thickness of 80 μm, and the P-type thermoelectric element layer had a thickness of 90 μm.

[0164] (Arrangement of Thermoelectric Element Layer) The resulting P-type thermoelectric element layers 24, each measuring 1 mm x 0.8 mm x 80 μm, and N-type thermoelectric element layers 25, each measuring 1 mm x 0.8 mm x 90 μm, were alternately arranged, adjacent to each other along 0.8 mm sides, forming pairs. In the thermoelectric element layer 26, 408 pairs of P-type thermoelectric element layers 24 and N-type thermoelectric element layers 25 were formed, and were arranged electrically in series within the surface of the polyimide film substrate 22 to form the thermoelectric element layer 26. The P-type thermoelectric element layers 24 and N-type thermoelectric element layers 25 were electrically connected by main electrodes 23 a. The thermoelectric element layer 26 had a folded structure. Specifically, 24 rows were arranged, with 17 pairs of P-type thermoelectric element layers 24 and N-type thermoelectric element layers 25 connected to each other via connecting electrodes 23 c. It should be noted that FIG. 2 shows a conceptual arrangement of the electrodes and thermoelectric element layers, and the dimensions, number, etc. of the electrodes and thermoelectric element layers that are actually fabricated will differ.

[0165] (Arrangement of the coating layer and the high thermal conductivity layer) An aluminum vapor-deposited PET film (manufactured by BAX, thickness: 12 μm) was used as the insulating layer, and a coating layer was prepared by laminating an adhesive layer (manufactured by Somar, product name: EP-0002EF-01MB, thickness: 25 μm) on both sides of the insulating layer. The lamination was performed at a temperature of 80°C. The above-mentioned coating layer was interposed on the upper surface (surface of the thermoelectric element layer) of the prepared substrate with a thermoelectric element layer, and a coating layer consisting of a single layer of adhesive layer (manufactured by Somar, product name: EP-0002EF-01MB, thickness: 25 μm) was interposed on the lower surface (the surface of the substrate opposite to the surface on which the thermoelectric element layer was provided), and high thermal conductivity layers [C1020, thickness: 200 μm, width: 1 mm, length: 100 mm, spacing: 1 mm, thermal conductivity: 398 (W / (m·K))] made of a high thermal conductivity material (copper foil) were intermittently arranged above and below the area where the P-type thermoelectric element layer and the N-type thermoelectric element layer were adjacent, so as to be staggered. In this case, the coating layer provided on the upper surface of the substrate with a thermoelectric element layer was positioned so that the aluminum-deposited surface of the aluminum-deposited PET film was distal from the thermoelectric element layer. The coating layer was laminated onto the thermoelectric element layer and the adhesive layer was laminated onto the substrate under vacuum conditions at a temperature of 80°C and a pressure of 0.2 MPa for 10 seconds. The high thermal conductivity layer was laminated onto the coating layer and adhesive layer under vacuum conditions at a temperature of 80°C. The thermoelectric conversion module was then left to stand in an environment of 150°C for 30 minutes to cure the adhesive layer, thereby obtaining an in-plane type thermoelectric conversion module.

[0166] (Arrangement of TIM) The upper and lower surfaces of the fabricated in-plane type thermoelectric conversion module were coated with a TIM having an adhesive strength of 0.16 (N / cm) and a shear stress of 0.039 (N / mm 2 The thermoelectric conversion module was then subjected to measurement of the electromotive force between the extraction electrodes based on the above-mentioned (c) electromotive force evaluation (output evaluation). The adhesive strength, shear stress, and total thermal resistance value R of the TIM in the thermoelectric conversion module were also measured. AB , the total thermal resistance value R of each component of the in-plane thermoelectric conversion module M , total thermal resistance value R AB / Total thermal resistance value R M was evaluated.

[0167] (Example 5) In Example 4, the adhesive strength was 0.13 (N / cm), the shear stress was 0.042 (N / mm 2 The electromotive force between the extraction electrodes was measured in the same manner as in Example 4, except that a TIM having a thickness of 0.50 mm and a thermal conductivity of 6.0 W / (m·K) [manufactured by Sekisui Polymatech Co., Ltd.] was installed. The adhesive strength, shear stress, and total thermal resistance value R AB , the total thermal resistance value R of each component of the in-plane thermoelectric conversion module M , total thermal resistance value R AB / Total thermal resistance value R M was evaluated.

[0168] (Example 6) In Example 4, the adhesive strength was 8.00 (N / cm), the shear stress was 0.780 (N / mm 2 The electromotive force between the extraction electrodes was measured in the same manner as in Example 4, except that a TIM having a thickness of 0.20 mm and a thermal conductivity of 1.5 W / (m·K) [manufactured by 3M, product number: 8926, thickness: 0.20 mm] was installed. The adhesive strength, shear stress, and total thermal resistance value R AB , the total thermal resistance value R of each component of the in-plane thermoelectric conversion module M , total thermal resistance value R AB / Total thermal resistance value R M was evaluated.

[0169] (Example 7) In Example 4, the adhesive strength was 20.00 (N / cm), the shear stress was 1.210 (N / mm 2 The electromotive force between the extraction electrodes was measured in the same manner as in Example 4, except that a TIM having a thickness of 0.30 mm and a thermal conductivity of 0.6 W / (m·K) [manufactured by 3M Corporation, product number: VHR0601, thickness: 0.30 mm, thermal conductivity: 0.6 W / (m·K)] was installed. In addition, the adhesive strength, shear stress, and total thermal resistance value R AB , the total thermal resistance value R of each component of the in-plane thermoelectric conversion module M , total thermal resistance value R AB / Total thermal resistance value R M was evaluated.

[0170] Comparative Example 3: The electromotive force between the extraction electrodes was measured in the same manner as in Example 4, except that a TIM having zero adhesive strength and shear stress (manufactured by Sekisui Polymatech Co., Ltd., product name: Manion 50α, thickness: 0.5 mm, thermal conductivity: 17.0 W / (m·K)) was installed. In addition, the adhesive strength, shear stress, and total thermal resistance value R of the TIM in the thermoelectric conversion module were measured. AB , the total thermal resistance value R of each component of the in-plane thermoelectric conversion module M , total thermal resistance value R AB / Total thermal resistance value R M was evaluated.

[0171] The adhesive strength, shear stress, and total thermal resistance R of the TIM in the thermoelectric conversion modules obtained in Examples 4 to 7 and Comparative Example 3 AB , the total thermal resistance value R of each component of the in-plane thermoelectric conversion module M , total thermal resistance value R AB / Total thermal resistance value R M The evaluation results of the thermoelectric conversion module and the electromotive force are shown in Table 2.

[0172]

[0173] The electromotive forces obtained from the thermoelectric conversion modules of Examples 4 to 7, in which the specific shear stresses of the thermally conductive interface members A and B satisfy the requirements of the second embodiment of the present invention, are higher than the electromotive force obtained from Comparative Example 3, which does not satisfy the requirements of the second embodiment of the present invention, and it is clear that the thermoelectric performance is improved.

[0174] Next, the third embodiment of the present invention will be described in more detail with reference to examples, but the third embodiment of the present invention is not limited to these examples in any way.

[0175] The adhesive strength of the TIM, shear stress, thermal resistance value of each member, and electromotive force of the thermoelectric conversion modules fabricated in the examples and comparative examples of the third embodiment of the present invention were evaluated by the following methods.

[0176] (a) Shear Stress Evaluation The TIM (10 mm x 10 mm) used in the examples and comparative examples of the third embodiment of the present invention was attached to a copper plate (45 mm x 45 mm x 3 mm thick), and a gold-plated copper chip (5 mm x 5 mm x 200 μm thick) was attached to the surface of the TIM opposite to the copper plate. Using a Bond Tester Dage Series 4000 (manufactured by Nordson Dage), a die shear test was carried out at a test speed of 200 μm / s and a test height of 1 μm to measure the shear stress (N / mm 2 ) was measured.

[0177] (b) Adhesion Strength Evaluation The TIM (25 mm × 40 mm) used in the Examples and Comparative Examples was attached to a copper plate (100 mm × 100 mm × 3.0 mm thick) and then bonded to the copper plate by rolling it back and forth once using a 2 kg roll (φ95 mm, material: rubber). After 24 hours, the 90-degree peel strength was measured at a peel rate of 300 mm / min using a universal tensile strength tester (Shimadzu Corporation, model: Autograph AG-X Plus) in an atmosphere of 23 ° C. and 50% RH, and the resulting value was used as the adhesion strength (N / cm).

[0178] (c) Electromotive Force Evaluation (Output Evaluation) Figure 7 is a cross-sectional view showing an example of an electromotive force evaluation configuration for a thermoelectric conversion module according to a third embodiment of the present invention. In a thermoelectric conversion module electromotive force evaluation configuration 61, a heat dissipation member 64 (heat sink UB2040-25B, manufactured by Alpha Electronics) was installed on one surface of a thermally conductive interface member A 63a having adhesive properties on a thermoelectric conversion element 62 obtained in the examples and comparative examples. A temperature controller (heat source) 65 (product name: Peltier Temperature Controller Set VTH1.8-70S, manufactured by Vicks Electronics) was installed on the other surface of a thermally conductive interface member B 63b having adhesive properties. The temperature controller (heat source) 65 was set to 60°C, and a temperature difference was applied from the outside. With the temperature difference applied, the electromotive force between the extraction electrodes was measured using a Digital HiTester (model: 3801-50, manufactured by Hioki E.E. Corporation).

[0179] (d) Evaluation of Thermal Resistance Value The thermal resistance value (K / W) of the TIM used in the examples and comparative examples was calculated using the thermal conductivity [W / (m K)], thickness (m), and effective area [0.006 (m) × 0.021 (m) = 1.26 × 10 -4(m 2 ) )] was used to calculate the thermal resistance value of the TIM from the following formula (1): Thermal resistance value of the TIM = Thickness of the TIM / (Thermal conductivity of the TIM × Effective area) (1) Similarly, the thermal conductivity, thickness, and effective area of ​​each of the following layers constituting the thermoelectric conversion module were calculated. Glass-epoxy substrate: Thermal conductivity 3.0 [W / (m K)]; Thickness 6.0 × 10 -5 (m); effective area 1.26 × 10 -4 (m 2 ) Heat dissipation layer: Cu, thermal conductivity 398 [W / (m K)], thickness 3.5 × 10 -5 (m) Ni 90.9 [W / (m K)] Thickness 3.0 × 10 -6 (m); effective area 1.26 × 10 -4 (m 2 ) Electrode layer: Cu Thermal conductivity 398 [W / (m K)] Thickness 3.5 × 10 -5 (m) Ni 90.9 [W / (m K)] Thickness 3.0 × 10 -6 (m); effective area 1.02 × 10 -4 (m 2 ) Solder material layer: Thermal conductivity 20 [W / (m·K)] Thickness 5.0×10 -5 (m); effective area 1.02 × 10 -4 (m 2 ) Chip: Thermal conductivity 0.5 [W / (m K)] Thickness 2.85 x 10 -4 (m); effective area 1.02 × 10 -4 (m 2 From the above, the thermal resistance value R of the thermally conductive interface member A A (mK / W), thermal resistance value R of thermally conductive interface member B B (mK / W) AB (mK / W), and the total thermal resistance value R of the thermoelectric conversion module M (mK / W) is calculated, and R M R against AB The ratio (R AB / R M ) was calculated.

[0180] (Example 8) <Fabrication of Thermoelectric Conversion Module> (1) Preparation of Thermoelectric Semiconductor Particles P-type bismuth telluride Bi, a bismuth-tellurium-based thermoelectric semiconductor material, was used as the P-type thermoelectric semiconductor particles. 0.4 Te 3 Sb 1.6 (manufactured by Kojundo Chemical Laboratory, average particle size: 16 μm) was used. N-type thermoelectric semiconductor particles were prepared using N-type bismuth telluride Bi, a bismuth-tellurium-based thermoelectric semiconductor material. 2 Te 3 Thermoelectric semiconductor particles having an average particle size of 2.8 μm were prepared by using a planetary ball mill (Premium line P-7, manufactured by Fritsch Japan) and pulverizing the thermoelectric semiconductor particles in a nitrogen gas atmosphere using a 90 μm particle size analyzer (manufactured by Kojundo Chemical Laboratory Co., Ltd.). The particle size distribution of each thermoelectric semiconductor particle was measured using a laser diffraction particle size analyzer (Malvern Mastersizer 3000).

[0181] (2) Preparation of coating liquid for thermoelectric semiconductor composition Coating liquid (P) The P-type bismuth telluride Bi 0.4 Te 3 Sb 1.6 A coating liquid (P) consisting of a thermoelectric semiconductor composition was prepared by mixing and dispersing 78.5 parts by mass of the particles, 5.2 parts by mass of polyethylene carbonate as a binder resin, 0.8 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 15.5 parts by mass of N-methylpyrrolidone as a solvent. 2 Te 3 A coating liquid (N) was prepared, which consisted of a thermoelectric semiconductor composition in which 78.8 parts by mass of particles, 4.25 parts by mass of polyethylene carbonate as a binder resin, 4.2 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 12.75 parts by mass of N-methylpyrrolidone as a solvent were mixed and dispersed.

[0182] (3) Preparation of Thermoelectric Conversion Material Chip The coating solution (P) prepared in (2) was applied onto a polyimide film (Ube Industries, Ltd., trade name "Kapton 500H", 100 mm x 160 mm x thickness 125 μm) using a screen printer (Newlong Co., Ltd., model name: LS-34TVA), and heated and dried at 110 ° C for 20 minutes to form a coating film with a thickness of 600 μm. Next, the coating film was subjected to a heat press at 250 ° C and 50 MPa for 10 minutes to obtain a P-type thermoelectric conversion material layer precursor with a thickness of 285 μm. The obtained P-type thermoelectric conversion material layer precursor was subjected to a baking (annealing) treatment at 430 ° C for 30 minutes in an argon-hydrogen mixed gas atmosphere to obtain a P-type thermoelectric conversion material layer. Next, a solder-receiving layer [Ni (thickness: 4 μm) laminated with Au (thickness: 30 nm)] was formed on the entire surface of the P-type thermoelectric conversion material layer by electroless plating, and then the P-type thermoelectric conversion material layer was singulated into chips using a dicing machine (manufactured by Disco Corporation, model name: DFD6362), thereby producing 0.9 mm x 0.9 mm P-type thermoelectric conversion material chips. Similarly, the coating liquid (N) prepared in (2) was applied to a polyimide film (manufactured by Ube Industries, trade name "Kapton 500H", 100 mm x 160 mm x thickness 125 μm) using a screen printer (manufactured by Newlong, product name: LS-34TVA), and the film was dried by heating at 110 ° C. for 20 minutes to form a coating film with a film thickness of 540 μm. The coated film was then heat-pressed at 250°C and 30 MPa for 20 minutes to obtain an N-type thermoelectric conversion material layer precursor with a film thickness of 285 μm. The obtained N-type thermoelectric conversion material layer precursor was baked (annealed) at 370°C for 30 minutes in an argon-hydrogen mixed gas atmosphere to obtain an N-type thermoelectric conversion material layer. Next, a solder-receptive layer [Ni (thickness: 4 μm) laminated with Au (thickness: 30 nm)] was provided on the entire surface of the N-type thermoelectric conversion material layer by electroless plating. The layer was then attached to dicing tape and singulated into chips using a dicing machine (manufactured by Disco Corporation, model name: DFD6362), producing 0.9 mm x 0.9 mm N-type thermoelectric conversion material chips.

[0183] (4) Preparation of Electrode Substrate: First, a substrate was prepared by attaching 35 μm thick copper foil to each side of a 60 μm thick glass epoxy sheet. A nickel layer (3 μm thick) and a gold layer (40 nm thick) were laminated in this order on the copper foil of the substrate by electroless plating. An electrode pattern (0.9 × 0.9 mm, 126 pieces, distance between adjacent electrodes: 0.1 mm, 6 columns, 21 rows) was then formed on only one side to produce a substrate with an electrode on one side and a heat sink on the other side (first substrate with first electrode, hereinafter sometimes referred to as the "first electrode substrate"). Similarly, a substrate with a patterned electrode arrangement was prepared so that, when bonded to the first electrode substrate, a π-type thermoelectric conversion module was obtained (second substrate with second electrode, hereinafter sometimes referred to as the "second electrode substrate"). The substrate and electrode materials, dimensions, including thickness, were the same as those of the first electrode substrate.

[0184] (Fabrication of Thermoelectric Conversion Elements) Using the chips of P-type thermoelectric conversion material and N-type thermoelectric conversion material having solder-receiving layers only on the top and bottom surfaces fabricated in (3), a π-type Peltier-cooled thermoelectric conversion module consisting of 63 pairs of chips each of P-type and N-type thermoelectric conversion material was fabricated as follows.

[0185] A solder material layer having a thickness of 50 μm was formed by screen printing on the first electrode substrate prepared in (4) using solder paste (manufactured by Kokisha, product name: T4AB58-M742) as the solder material. Next, one side of the solder-receiving layer of each of the P-type and N-type thermoelectric conversion material chips prepared in (3) was placed on the solder material layer, and the chips were heated at 190°C for 1 minute and then cooled, thereby placing the P-type and N-type thermoelectric conversion material chips on the first electrode substrate, respectively. Furthermore, a solder material layer having a thickness of 50 μm was formed on the other side of the solder-receiving layer of each of the P-type and N-type thermoelectric conversion material chips using the solder paste in the same manner as above, and the resulting chips were bonded to the second electrode substrate prepared in (4) and heated at 190°C for 2 minutes to produce thermoelectric conversion elements each consisting of 63 pairs of P-type and N-type thermoelectric conversion material chips.

[0186] (Arrangement of TIM) R AB / R MA TIM (manufactured by Sekisui Polymatech Co., Ltd., product number: PT-V, thickness: 0.50 mm, thermal conductivity: 12 W / (m K)) having a shear stress of 0.039 and a viscosity of 0.12 was installed to obtain a thermoelectric conversion module. The electromotive force between the extraction electrodes of the obtained thermoelectric conversion module was measured based on the above-mentioned (c) electromotive force evaluation (output evaluation).

[0187] (Example 9) In Example 8, R AB / R M A thermoelectric conversion module was produced in the same manner as in Example 8, except that a TIM [manufactured by Sekisui Polymatech Co., Ltd., product number: PT-UT, thickness: 0.50 mm, thermal conductivity: 6 W / (m K)] satisfying the above condition of 0.23 and having a shear stress of 0.042 was installed, and the electromotive force between the extraction electrodes was measured.

[0188] (Example 10) In Example 8, R AB / R M A thermoelectric conversion module was produced in the same manner as in Example 8, except that a TIM [manufactured by 3M Corporation, product number: 8926, thickness: 0.20 mm, thermal conductivity: 1.5 W / (m K)] satisfying the above condition of 0.38 and having a shear stress of 0.780 was installed, and the electromotive force between the extraction electrodes was measured.

[0189] (Comparative Example 4) In Example 8, R AB / R M A thermoelectric conversion module was produced in the same manner as in Example 8, except that a TIM [manufactured by 3M Corporation, product number: VHR0601, thickness: 0.30 mm, thermal conductivity: 0.6 W / (m K)] having a shear stress of 1.41 and a shear stress of 1.210 was installed, and the electromotive force between the extraction electrodes was measured.

[0190] (Comparative Example 5) In Example 8, R AB / R M A thermoelectric conversion module was produced in the same manner as in Example 8, except that a TIM [manufactured by Sekisui Polymatech Co., Ltd., product number: Manion 50α, thickness: 0.50 mm, thermal conductivity: 17 W / (m K)] was installed, which had a shear stress of 0.083 and a shear stress of 0, and the electromotive force between the extraction electrodes was measured.

[0191] Comparative Example 6 A thermoelectric conversion module was fabricated in the same manner as in Example 8, except that no TIM was provided on the top and bottom surfaces of the thermoelectric conversion module, and the electromotive force between the extraction electrodes was measured.

[0192] The adhesive strength, shear stress, and total thermal resistance R of the TIM in the thermoelectric conversion modules obtained in Examples 8 to 10 and Comparative Examples 4 to 6 AB , the total thermal resistance value R of each component of the thermoelectric conversion module M , total thermal resistance value R AB / Total thermal resistance value R M The evaluation results of the thermoelectric conversion module and the electromotive force are shown in Table 3.

[0193]

[0194] R M R against AB The ratio (R AB / R M ), and the electromotive force obtained from the thermoelectric conversion modules of Examples 8 to 10 in which the specific shear stress applied to the thermally conductive interface member A and the thermally conductive interface member B satisfied the provisions according to the third embodiment of the present invention was higher than the electromotive force obtained from the thermoelectric conversion modules of Comparative Examples 4 to 6 in which the provisions according to the third embodiment of the present invention were not satisfied, and it can be seen that the thermoelectric performance was improved.

[0195] The thermoelectric conversion module of the present invention provides a thermoelectric conversion module with improved electromotive force, and is therefore expected to be applicable to power generation applications, such as converting exhaust heat from various combustion furnaces, such as factories, waste incineration furnaces, and cement combustion furnaces, exhaust heat from automobile combustion gases, and exhaust heat from electronic devices, into electricity. Cooling applications include, in the field of electronics, temperature control of various sensors, such as CPUs (Central Processing Units) used in smartphones and various computers, image sensors, such as CMOSs ​​(Complementary Metal Oxide Semiconductors) and CCDs (Charge Coupled Devices), and MEMS (Micro Electro Mechanical Systems), and light-receiving elements.

[0196] DESCRIPTION OF SYMBOLS 1A, 1B, 1C: Thermoelectric conversion module 2: Substrate 3: Electrode 4: P-type thermoelectric element layer 5: N-type thermoelectric element layer 6: Thermoelectric element layer 7: Covering layer 8A: High thermal conductivity layer A 8B: High thermal conductivity layer B 8a: High thermal conductivity layer a 8b: High thermal conductivity layer b 9: In-plane type thermoelectric conversion module 10a: Thermally conductive interface member A 10b: Thermally conductive interface member B 10c: Adhesive thermally conductive interface member A 10d: Adhesive thermally conductive interface member B 11: Heat dissipation member 22: Polyimide film substrate 23P: Electrode pattern (single layer) 23Q: Electrode pattern (laminated) 23a: Main electrode 23b: Electrode portion for extracting electromotive force 23c: Connection electrode portion 24: P-type thermoelectric element layer 25: N-type thermoelectric element layer 26: Thermoelectric element layer 31A, 31B: Thermoelectric conversion module electromotive force evaluation configuration 32: In-plane type thermoelectric conversion module 33a: Thermally conductive interface member A 33b: Thermally conductive interface member B 33c: Adhesive thermally conductive interface member A 33d: Adhesive thermally conductive interface member B 34: Temperature controller (heat source) 35: Heat dissipation member 36: Heat insulating member 37: Load member 42a: First substrate 42b: Second substrate 43a: First electrode 43b: Second electrode 44: P-type thermoelectric conversion material chip 45: N-type thermoelectric conversion material chip 46: Solder material layer 47: Solder acceptance layer 48a: Heat dissipation layer A 48b: Heat dissipation layer B 49: Thermoelectric conversion element 50a: Adhesive thermally conductive interface member A 50b: Adhesive thermally conductive interface member B 51: Heat dissipation member 61: Thermoelectric conversion module electromotive force evaluation configuration 62: Thermoelectric conversion element 63a: Adhesive thermally conductive interface member A 63b: Adhesive thermally conductive interface member B 64: Heat dissipation member 65: Temperature controller (heat source)

Claims

1. A thermoelectric conversion module comprising a thermally conductive interface member A and a heat dissipation member on one surface of an in-plane type thermoelectric conversion module, and further comprising a thermally conductive interface member B on the other surface of the in-plane type thermoelectric conversion module, wherein the thermal resistance value of the thermally conductive interface member A is R A (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is R AB (mK / W), and the total thermal resistance of the in-plane type thermoelectric conversion module is R M (mK / W), the R M The R AB The ratio (R AB / R M ) is 1.40 or less.

2. The thermoelectric conversion module according to claim 1, wherein the in-plane type thermoelectric conversion module further includes a high thermal conductivity layer A and a high thermal conductivity layer B, the high thermal conductivity layer A constituting the outermost layer on the thermally conductive interface member A side of the in-plane type thermoelectric conversion module, and the high thermal conductivity layer B constituting the outermost layer on the thermally conductive interface member B side of the in-plane type thermoelectric conversion module.

3. A thermoelectric conversion module as described in claim 2, wherein the high thermal conductivity layer A is composed of a plurality of high thermal conductivity layers a arranged at intervals, with a portion of the thermally conductive interface member A embedded in the gaps between adjacent high thermal conductivity layers a, and the high thermal conductivity layer B is composed of a plurality of high thermal conductivity layers b arranged at intervals, with a portion of the thermally conductive interface member B embedded in the gaps between adjacent high thermal conductivity layers b.

4. The thermoelectric conversion module according to claim 3, wherein a ratio M of an embedding depth of the portion of the thermally conductive interface member A to a thickness of the high thermal conductivity layer A is 0.01 to 1.00, and a ratio N of an embedding depth of the portion of the thermally conductive interface member B to a thickness of the high thermal conductivity layer B is 0.01 to 1.

00.

5. The thermoelectric conversion module according to claim 1, wherein the thermally conductive interface member A and the thermally conductive interface member B are each independently a resin layer or an organic layer.

Citation Information

Patent Citations

  • Thermoelectric conversion module and power generating system

    JP2019204926A

  • Wearable thermoelectric generator system

    US20130087180A1

  • Thermoelectric conversion device and electronic device

    WO2018042708A1