Solid oxide fuel cell
A laminated anode support structure with specific yttria-stabilized zirconia and alumina layers in solid oxide fuel cells addresses strength and durability issues, enabling reduced thickness while maintaining performance and preventing redox-induced damage.
Patent Information
- Application Number
- PCT/KR2024/001128
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-01-24
- Publication Date
- 2024-10-03
AI Technical Summary
Anode-supported solid oxide fuel cells face challenges in maintaining mechanical strength and long-term performance due to reduced anode support thickness, which can lead to breakage and electrolyte damage from nickel particle growth during redox reactions.
A laminated anode support structure comprising a first support layer of yttria-stabilized zirconia with low yttria content and a second support layer of higher yttria-stabilized zirconia and alumina, both with porous structures, to enhance strength and suppress nickel particle growth, allowing for reduced anode thickness while maintaining performance.
The solution provides sufficient mechanical strength and improved long-term performance by reducing anode support thickness, preventing damage from redox reactions and enhancing fuel cell durability.
Smart Images

Figure KR2024001128_03102024_PF_FP_ABST
Abstract
Description
solid oxide fuel cell
[0001] The present invention relates to a fuel cell that generates electrical energy by a reaction of hydrogen and oxygen, and more particularly, to an anode-supported solid oxide fuel cell.
[0002] Solid oxide fuel cells are fuel cells that operate at high temperatures of approximately 600 to 1000°C. They are the most efficient and pollutant-free of all existing fuel cells, and have several advantages, including the ability to generate combined power without requiring a fuel reformer.
[0003] The solid oxide fuel cells described above can be broadly classified into planar, cylindrical, and tubular types. Planar solid oxide fuel cells have the advantage of higher power density of the stack itself compared to cylindrical or tubular solid oxide fuel cells, and cylindrical or tubular solid oxide fuel cells have the advantage of easier gas sealing and greater resistance to thermal shock due to differences in thermal equilibrium coefficients between materials compared to planar solid oxide fuel cells. Therefore, planar solid oxide fuel cells, cylindrical solid oxide fuel cells, and tubular solid oxide fuel cells are all currently being actively researched.
[0004] All types of solid oxide fuel cells generally use a support to improve durability, and can be classified into anode-supported single cells, electrolyte-supported single cells, and metal-supported single cells depending on the support. Electrolyte-supported single cells have the problem of operating only at temperatures above 900°C, and metal-supported single cells have the problem of operating temperatures being limited to 600°C or lower due to the thermal expansion of the metal. Therefore, most companies are developing and commercializing anode-supported single cells.
[0005] In anode-supported single-cell batteries, the thickness of the anode support significantly influences the diffusion of fuel and generated water, thus significantly impacting the performance of the single-cell. To improve single-cell performance and lower operating temperatures, extensive research is being conducted to reduce the thickness of the anode support. However, reducing the thickness of the anode support reduces its mechanical strength, making handling difficult and prone to breakage during the manufacturing process, thereby lowering yield.
[0006] Meanwhile, in the case of an anode-supported single cell, problems such as damage to the electrolyte due to volume expansion of the anode support caused by nickel particle growth due to redox reaction may occur.
[0007] Therefore, there is a need for the development of a solid oxide fuel cell that can secure sufficient strength even when the thickness of the anode support is reduced, and can also improve the long-term performance of the solid oxide fuel cell.
[0008] An object of the present invention is to provide a solid oxide fuel cell capable of securing sufficient strength even when the thickness of the anode support is reduced, and also improving the long-term performance of the solid oxide fuel cell.
[0009] According to one embodiment of the present invention, a solid oxide fuel cell comprises: an anode support electrode; a solid oxide electrolyte disposed on the anode support electrode; and a cathode electrode disposed on the solid oxide electrolyte; wherein the anode support electrode comprises: a first support layer comprising a cermet of first yttria-stabilized zirconia containing nickel and yttria in a ratio of 1 to 5 mol% and having a porous structure; a second support layer formed of a cermet of nickel, second yttria-stabilized zirconia having a higher yttria content than the first yttria-stabilized zirconia, and alumina and having a porous structure; and an anode functional layer formed of a cermet of yttria-stabilized zirconia and nickel and disposed on the second support layer so as to be in contact with the solid oxide electrolyte.
[0010] According to another embodiment of the present invention, a solid oxide fuel cell comprises: an anode support electrode; a solid oxide electrolyte disposed on the anode support electrode; and a cathode electrode disposed on the solid oxide electrolyte; wherein the anode support electrode comprises: a first support layer comprising a cermet of first yttria-stabilized zirconia containing nickel and yttria in a ratio of 1 to 5 mol% and having a porous structure; a second support layer disposed under the first support layer and formed of a cermet of nickel, second yttria-stabilized zirconia having a higher yttria content than the first yttria-stabilized zirconia, and alumina and having a porous structure; and an anode functional layer disposed on the first support layer so as to be in contact with the solid oxide electrolyte, and formed of a cermet of yttria-stabilized zirconia and nickel.
[0011] In one embodiment, the second yttria-stabilized zirconia may contain yttria in a proportion of 5 to 10 mol%.
[0012] In one embodiment, the second support layer may include the alumina in a ratio of 0.1 to 1.0 wt.%.
[0013] In one embodiment, the first support layer may be formed of a first raw material powder including x to y parts by weight of the first itzri-stabilized zirconia powder relative to 100 parts by weight of the nickel oxide powder, and the second support layer may be formed of a second raw material powder including a to b parts by weight of the second itzri-stabilized zirconia powder relative to 100 parts by weight of the nickel oxide powder, and including 0.1 to 1.0 wt.% of the alumina powder.
[0014] In one embodiment, the thickness of the first support layer may be 1 to 3 times the thickness of the second support layer. For example, the thickness of the first support layer may be 200 to 300 μm, and the thickness of the second support layer may be 100 to 200 μm.
[0015] According to the solid oxide fuel cell of the present invention, since the anode support has a laminated structure in which a first support layer contributing to strength improvement is manufactured using nickel oxide powder and YSZ powder containing 5 mol% or less of yttria, and a second support layer contributing to suppressing metal particle growth due to redox reaction is manufactured using nickel oxide powder, YSZ powder, and alumina powder, sufficient strength can be secured even if the thickness of the anode support is reduced, and the long-term performance of the solid oxide fuel cell can be improved.
[0016] FIG. 1 is a cross-sectional view illustrating a solid oxide fuel cell according to one embodiment of the present invention.
[0017] FIG. 2 is a cross-sectional view illustrating a solid oxide fuel cell according to another embodiment of the present invention.
[0018] Figure 3 shows the results of a three-point bending strength evaluation of a support sheet (8YSZ) according to Comparative Example 1 and a support sheet (3YSZ) according to Example 1.
[0019] Figure 4 shows the results of repeated redox evaluations measured for a single cell according to Comparative Example 2 and a single cell according to Example 2.
[0020] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. The present invention can be modified in various ways and can take various forms, and thus specific embodiments are illustrated in the drawings and described in detail in the text. However, this is not intended to limit the present invention to a specific disclosed form, but it should be understood that all modifications, equivalents, and substitutes included in the spirit and technical scope of the present invention are included. In describing each drawing, similar reference numerals are used to indicate similar components. In the attached drawings, the dimensions of structures are shown larger than actual size to ensure clarity of the present invention.
[0021] While terms like "first" and "second" may be used to describe various components, these components should not be limited by these terms. These terms are used solely to distinguish one component from another. For example, without departing from the scope of the present invention, a first component could be referred to as a "second component," and similarly, a second component could also be referred to as a "first component."
[0022] The terminology used in this application is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this application, it should be understood that the terms "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0023] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and will not be interpreted in an idealized or overly formal sense unless explicitly defined herein.
[0024]
[0025] FIG. 1 is a cross-sectional view illustrating a solid oxide fuel cell according to one embodiment of the present invention.
[0026] Referring to FIG. 1, a solid oxide fuel cell (100) according to one embodiment of the present invention may include an anode support electrode (110); a solid oxide electrolyte (120); and a cathode electrode (130).
[0027] The above anode support electrode (110) may include a first support layer (111), a second support layer (112), and an anode functional layer (113).
[0028] The first support layer (111) is a configuration for improving the strength of the anode support electrode (110), has a porous structure so that hydrogen-containing fuel gas can move inside, and may be formed of a cermet of first yttria-stabilized zirconia (YSZ) having a relatively low content of nickel and yttria. In one embodiment, the first yttria-stabilized zirconia powder may contain yttria in a ratio of about 1 to 5 mol%.
[0029] In one embodiment, the first support layer (111) may be manufactured from a first raw material powder including a nickel oxide powder and the first yttria-stabilized zirconia (YSZ) powder. For example, the first support layer (111) may be formed from a first raw material powder including about 30 to 60 parts by weight of the first yttria-stabilized zirconia powder and about 40 to 70 parts by weight of the nickel oxide powder.
[0030] In one embodiment, the first support layer (111) may be manufactured by mixing the first raw material powder with a pore-forming agent, dispersing the mixture in a solvent, adding a binder thereto to manufacture a first molding paste, and then performing a compression molding process or a tape casting process using the first molding paste. In this case, the pore-forming agent may be a powder such as polymethyl methacrylate (PMMA), activated carbon, carbon black, graphite, starch, etc., and the first molding paste may include about 30 to 60 parts by weight of the first yttria-stabilized zirconia powder and about 40 to 70 parts by weight of the nickel oxide powder, along with about 1 to 20 parts by weight of the pore-forming agent. And as the binder, a polyvinyl alcohol (PVA)-based binder, a methylcellulose (MC)-based binder, a carboxycellulose (sodium carboxymethylcellulose (CMC)-based binder, etc. may be used alone or in a mixture of two or more thereof, and the binder may be mixed in an amount of about 10 vol.% to about 50 vol.% relative to the first raw material powder. In addition, water, for example, distilled water or deionized water, may be used as the solvent.
[0031] The second support layer (112) is a configuration for suppressing metal particle growth due to a redox reaction, is disposed on the upper portion of the first support layer (111), has a porous structure so that hydrogen-containing fuel gas can move inside, and may be formed of a cermet of nickel, second yttria-stabilized zirconia having a higher yttria content than the first yttria-stabilized zirconia, and alumina (Al2O3). For example, the second support layer (112) may be manufactured from a second raw material powder including a nickel oxide powder, a powder of the second yttria-stabilized zirconia, and a powder of alumina (Al2O3). In one embodiment, the second yttria-stabilized zirconia may contain yttria in a ratio of about 5 to 10 mol%. The above alumina can suppress the growth of particles such as nickel through a redox reaction, thereby suppressing the volume expansion of the entire first and second support layers (111, 112). In addition, in the second raw material powder, the alumina powder can act as a sintering aid in the sintering process.
[0032] In one embodiment, the second support layer (112) may be formed of a second raw material powder including about 40 to 70 parts by weight of the second yttria-stabilized zirconia powder and about 30 to 60 parts by weight of the nickel oxide powder. In addition, the second raw material powder may include the alumina powder in a ratio of about 0.1 to 1.0 wt.%.
[0033] In one embodiment, the second support layer (112) can be manufactured by mixing the second raw material powder with a pore-forming agent, dispersing it in a solvent, adding a binder thereto to manufacture a first molding paste, and then performing a compression molding process or a tape casting process using the second molding paste. The first and second support layers (111, 112) can be combined by laminating the green sheet of the second support layer (112) with the green sheet of the first support layer (111) and then sintering. In this case, the pore-forming agent may be a powder such as polymethyl methacrylate (PMMA), activated carbon, carbon black, graphite, starch, etc., and the second molding paste may include about 40 to 70 parts by weight of the second yttria-stabilized zirconia powder and about 30 to 60 parts by weight of the nickel oxide powder, along with about 1 to 30 parts by weight of the pore-forming agent. In addition, the binder may be a polyvinyl alcohol (PVA)-based binder, a methylcellulose (MC)-based binder, a carboxycellulose (sodium carboxymethylcellulose (CMC)-based binder, etc., which may be used alone or in a mixture of two or more, and the binder may be mixed in an amount of about 10 vol.% to about 50 vol.% relative to the second raw material powder. Additionally, water, for example, distilled water or deionized water, may be used as the solvent.
[0034] In one embodiment, the first support layer (111) and the second support layer (112) may have different porosities. For example, the second support layer (112) disposed closer to the anode functional layer (113) may have a greater porosity than the first support layer (111). The porosity of the first support layer (111) and the second support layer (112) may be controlled through the content, particle size, material, etc. of the pore-forming agent mixed in the process of manufacturing each layer.
[0035] In one embodiment, the thickness of the first support layer (111) may be greater than or equal to the thickness of the second support layer (112). In one embodiment, the thickness of the first support layer (111) may be about 1 to 3 times the thickness of the second support layer (112). For example, the thickness of the first support layer (111) may be about 200 to 300 μm, and the thickness of the second support layer (112) may be about 100 to 200 μm.
[0036] The anode functional layer (113) is disposed on the second support layer (112) and may be formed with a relatively dense structure compared to the first and second support layers (111, 112). In one embodiment, the anode functional layer (113) may be formed of a cermet of yttria-stabilized zirconia and nickel. For example, the anode functional layer (113) may be formed by forming a mixed slurry of nickel oxide powder and yttria-stabilized zirconia powder, forming a coating film on the second support layer (112) using a dip coating method, drying the slurry, and then sintering the slurry in an air atmosphere at about 900°C to about 1200°C. Alternatively, the anode functional layer (113) may also be manufactured into a green sheet through a tape casting process and then combined with the support (110) through sintering.
[0037] The above solid oxide electrolyte layer (120) may be disposed on the anode functional layer (113), may be formed of yttria-stabilized zirconia, and may be formed with a denser structure than the first and second support layers (111, 112). For example, the yttria-stabilized zirconia may contain about 5 to 10 mol% of yttria.
[0038] In one embodiment, the solid oxide electrolyte layer (120) may be formed by forming an yttria-stabilized zirconia slurry, manufacturing the slurry into a green sheet through a tape casting process, and then laminating and sintering the green sheets of the first and second support layers (111, 112) to form the solid oxide electrolyte layer (120) combined with the support (110). Alternatively, the solid oxide electrolyte layer (120) may be formed by forming an electrolyte coating film on the outer surface of the anode functional layer (113) by dip coating the yttria-stabilized zirconia slurry, and then sintering the same in an air atmosphere electric furnace at about 1300°C to about 1500°C.
[0039] The above cathode electrode (130) is placed on the solid oxide electrolyte layer (120) and LSM (La 1-x Sr x It can be formed of MnO3) and can have a porous structure to allow air to move inside.
[0040] In one embodiment, the cathode electrode (130) is LSM (La 1-x Sr x After forming the MnO3) slurry, a coating film is formed on the outer surface of the solid oxide electrolyte layer (120) by a dip coating method, and then it can be formed by sintering it in an air atmosphere electric furnace at about 900°C to about 1300°C.
[0041]
[0042] FIG. 2 is a cross-sectional view illustrating a solid oxide fuel cell according to another embodiment of the present invention.
[0043] Referring to FIG. 2, a solid oxide fuel cell (200) according to an embodiment of the present invention may include an anode support electrode (210); a solid oxide electrolyte (220); and a cathode electrode (230).
[0044] The above solid oxide electrolyte (220) and the above cathode electrode (230) are substantially the same as the solid oxide electrolyte (120) and the cathode electrode (130) of the solid oxide fuel cell (100) described with reference to FIG. 1, respectively, and therefore, redundant detailed descriptions thereof are omitted.
[0045] The above anode support electrode (210) may include a first support layer (211), a second support layer (212), and an anode functional layer (213).
[0046] Except that the first support layer (211) is disposed between the second support layer (212) and the anode functional layer (213), the first support layer (211), the second support layer (212) and the anode functional layer (213) are substantially the same as the first support layer (111), the second support layer (112) and the anode functional layer (113) of the anode support electrode (110) of the solid oxide fuel cell (100) described with reference to FIG. 1, and therefore, a detailed description thereof will be omitted.
[0047]
[0048] According to the solid oxide fuel cell of the present invention, since the anode support has a laminated structure in which a first support layer contributing to strength improvement is manufactured using nickel oxide powder and YSZ powder containing 5 mol% or less of yttria, and a second support layer contributing to suppressing metal particle growth due to redox reaction is manufactured using nickel oxide powder, YSZ powder, and alumina powder, sufficient strength can be secured even if the thickness of the anode support is reduced, and the long-term performance of the solid oxide fuel cell can be improved.
[0049]
[0050] Hereinafter, specific examples of the present invention will be described in detail. However, the following examples are merely some embodiments of the present invention, and the scope of the present invention is not limited to the following examples.
[0051]
[0052] [Comparative Example 1]
[0053] A support sheet having a thickness of 400 μm was manufactured using a raw material powder consisting of nickel oxide powder and YSZ (hereinafter referred to as '8YSZ') powder containing 8 mol% of yttria.
[0054]
[0055] [Example 1]
[0056] A support sheet having a thickness of 400 μm was manufactured using the same method as in the comparative example using a raw material powder containing nickel oxide powder and YSZ (hereinafter referred to as '3YSZ') powder containing 3 mol% of yttria in the same ratio as in the comparative example.
[0057]
[0058] Figure 3 shows the results of a three-point bending strength evaluation of a support sheet (8YSZ) according to Comparative Example 1 and a support sheet (3YSZ) according to Example 1.
[0059] Referring to FIG. 3, it can be confirmed that the support sheet (3YSZ) according to Example 1 has a strength that is about 5 to 10% higher than that of the support sheet (8YSZ) according to Comparative Example 1.
[0060]
[0061] [Comparative Example 2]
[0062] A single cell was manufactured by forming an anode functional layer, an electrolyte layer, and a cathode electrode on a support sheet having a thickness of 600 μm using the same method as in Comparative Example 1.
[0063]
[0064] [Example 2]
[0065] A 200 μm thick layer was formed using raw material powders consisting of nickel oxide powder, 3YSZ powder, and alumina powder on a support sheet according to Example 1, and then an anode functional layer, an electrolyte layer, and a cathode electrode were formed thereon to manufacture a single cell.
[0066]
[0067] Figure 4 shows the results of repeated redox evaluations measured for a single cell according to Comparative Example 2 and a single cell according to Example 2.
[0068] Referring to Fig. 4, it was confirmed that the single cell according to Example 2 had improved performance compared to the single cell according to Comparative Example 2. In addition, as a result of microstructural confirmation, it was confirmed that the growth of nickel particles was suppressed in the single cell according to Example 2 compared to the single cell according to Comparative Example 2.
[0069]
[0070] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood by those skilled in the art that various modifications and changes may be made to the present invention without departing from the spirit and scope of the present invention as set forth in the claims below.
Claims
1. Anode support electrode; A solid oxide electrolyte disposed on the anode support electrode; and A cathode electrode disposed on the solid oxide electrolyte; The above anode support electrode is, A first support layer having a porous structure, comprising a cermet of a first yttria-stabilized zirconia containing nickel and yttria in a ratio of 1 to 5 mol%; A second support layer disposed on the first support layer, formed of a cermet of nickel, second yttria-stabilized zirconia having a higher yttria content than the first yttria-stabilized zirconia, and alumina, and having a porous structure; and A solid oxide fuel cell characterized by comprising an anode functional layer formed of a cermet of yttria-stabilized zirconia and nickel, and arranged to be in contact with the solid oxide electrolyte on the second support layer.
2. Anode support electrode; A solid oxide electrolyte disposed on the anode support electrode; and A cathode electrode disposed on the solid oxide electrolyte; The above anode support electrode is, A first support layer having a porous structure, comprising a cermet of a first yttria-stabilized zirconia containing nickel and yttria in a ratio of 1 to 5 mol%; A second support layer disposed under the first support layer, formed of a cermet of nickel, second yttria-stabilized zirconia having a higher yttria content than the first yttria-stabilized zirconia, and alumina, and having a porous structure; and A solid oxide fuel cell characterized by comprising an anode functional layer formed of a cermet of yttria-stabilized zirconia and nickel, and arranged to be in contact with the solid oxide electrolyte on the first support layer.
3. In paragraph 1 or 2, A solid oxide fuel cell, characterized in that the second yttria-stabilized zirconia contains yttria in a ratio of 5 to 10 mol%.
4. In paragraph 3, A solid oxide fuel cell, characterized in that the second support layer comprises alumina in a ratio of 0.1 to 1.0 wt.%.
5. In paragraph 3, The first support layer is formed of a first raw material powder including 30 to 60 parts by weight of the first yttria-stabilized zirconia powder and 40 to 70 parts by weight of the nickel oxide powder, A solid oxide fuel cell, characterized in that the second support layer is formed of a second raw material powder comprising 40 to 70 wt. parts of the second yttria-stabilized zirconia powder and 30 to 60 wt. parts of the nickel oxide powder, and 0.1 to 1.0 wt.% of the alumina powder.
6. In paragraph 3, A solid oxide fuel cell, characterized in that the thickness of the first support layer is 1 to 3 times the thickness of the second support layer.
7. In paragraph 6, The thickness of the first support layer is 200 to 300 μm, A solid oxide fuel cell, characterized in that the thickness of the second support layer is 100 to 200 ㎛.
Citation Information
Patent Citations
Fabrication Method for Anode of Solid Oxide Fuel Cell
KR100660218B1
Method of manufacturing interconnect coating layer and ceramic interconnects including the interconnect coating layer
KR1020170038553A
A method for improving long term stability of Ni-YSZ anode supporter using Al2O3
KR1020170087105A
Solid oxide fuel cells
KR102590588B1
KR20190017817A