Silicon nitride-silicon composite powder and manufacturing method therefor
The silicon nitride-silicon composite powder with a core-shell structure and metal-doped silicon layer addresses the limitations of existing heat dissipation and battery materials by enhancing thermal conductivity and mechanical stability, suitable for high-frequency applications and lithium secondary batteries.
Patent Information
- Application Number
- PCT/KR2024/002814
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
Current heat dissipation materials, such as aluminum nitride, lack sufficient mechanical properties and exhibit high dielectric loss, while silicon nitride has lower thermal conductivity but excellent mechanical properties and low dielectric loss, making them unsuitable for high-frequency applications. Additionally, silicon anode active materials for lithium secondary batteries face volume expansion issues and require complex processing.
A silicon nitride-silicon composite powder with a core-shell structure is developed, where a silicon layer forms the shell and the silicon nitride core, with the silicon layer thickness controlled between 2 to 100 nm, and doped with metals like Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, and W, using a heat treatment process in a vacuum at 1000 to 1500°C to enhance thermal conductivity and mechanical stability.
The composite powder achieves improved thermal conductivity and mechanical stability, suitable for high-frequency applications, and addresses the volume expansion issue in silicon anode active materials, offering a promising solution for next-generation heat dissipation and battery technologies.
Smart Images

Figure KR2024002814_03102024_PF_FP_ABST
Abstract
Description
Silicon nitride-silicon composite powder and its manufacturing method
[0001] The present invention relates to a silicon nitride-silicon composite powder and a method for producing the same, and more particularly, to a silicon nitride-silicon composite powder having a silicon layer (Si layer) formed on the surface to form a core-shell structure, and a method for producing the same.
[0002] Alumina (Al2O3), aluminum nitride (AlN), and silicon nitride (Si3N4) have been actively studied as materials for heat sink substrates for power devices.
[0003] Aluminum nitride (AlN) has been reported to possess high thermal conductivity, but its low mechanical properties (strength and fracture toughness) make it unsuitable as a heat sink substrate material. Furthermore, aluminum nitride has been found to have high dielectric loss in the GHz frequency range.
[0004] Silicon nitride has excellent mechanical properties, but its thermal conductivity is lower than that of aluminum nitride (AlN), making it unsuitable as a heat-dissipating material. However, recent research has shown that the theoretical thermal conductivity of silicon nitride can surpass that of aluminum nitride, revitalizing its appeal as a heat-dissipating material. In particular, silicon nitride is known to have low dielectric loss and stability even in the high-frequency range. Therefore, it is expected to be practically used as a heat-dissipating substrate material for central processing units (CPUs) in computers operating at GHz frequencies and power transistors in smartphones. Silicon nitride exhibits both excellent mechanical properties and high thermal conductivity, and is expected to be a stable, next-generation heat-dissipating substrate material even in the high-frequency range.
[0005] The inventor of the present invention studied a method for utilizing silicon nitride as a negative electrode active material, and proposed a silicon nitride-silicon composite powder having a structure suitable for use as a negative electrode active material and a method for producing the same.
[0006] [Prior Art Literature]
[0007] Republic of Korea Patent Publication No. 10-1999-0066754
[0008] The problem to be solved by the present invention is to provide a silicon nitride-silicon composite powder having a silicon layer (Si layer) formed on the surface to form a core-shell structure, and a method for manufacturing the same.
[0009] The present invention provides a silicon nitride-silicon composite powder having a core-shell structure, wherein Si3N4 forms a core and a silicon (Si) layer forms a shell.
[0010] The thickness of the silicon layer forming the above shell may be approximately 2 to 100 nm.
[0011] The silicon layer forming the above shell may be a layer doped with a metal.
[0012] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0013] The surface of Si3N4 forming the above core may be doped with metal.
[0014] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0015] In addition, the present invention provides a method for producing a silicon nitride-silicon composite powder, comprising the steps of (a) preparing Si3N4 powder as a starting material; and (b) heat-treating the Si3N4 powder in a vacuum to form a silicon layer, wherein Si3N4 forms a core and the silicon (Si) layer forms a shell.
[0016] By controlling the above heat treatment conditions, the thickness of the silicon layer forming the shell can be made to be 2 to 100 nm.
[0017] Before the above step (b), a step of surface-treating the Si3N4 powder with a solution in which a metal salt is dissolved may be further included, and the silicon layer forming the shell may be a layer doped with a metal that is a component of the metal salt.
[0018] The above metal salt may include one or more salts selected from the group consisting of metal nitrates and metal sulfates.
[0019] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0020] The surface of Si3N4 forming the above core may be doped with metal.
[0021] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0022] It is preferable to perform the above heat treatment at a temperature of 1000 to 1500 ℃.
[0023] The above heat treatment is carried out at 10 below atmospheric pressure. -13 10 inland -2 It is desirable to perform the operation in a vacuum of MPa.
[0024] The above heat treatment can be performed in an inert gas atmosphere.
[0025] The above step (a) may include a step of synthesizing Si3N4 powder by nitriding Si powder in a gas atmosphere containing a nitrogen component.
[0026] According to the silicon nitride-silicon composite powder of the present invention, a silicon layer (Si layer) is formed on the surface to form a core-shell structure, with Si3N4 forming the core and a silicon (Si) layer forming the shell.
[0027] According to the present invention, it is possible to form a Si layer (Si film) on the surface with a thickness precisely controlled from several to several tens of nanometers, and it can be utilized as an anode active material for secondary batteries utilizing a Si structure with a thickness in the nanometer range. It is expected that the silicon (Si) forming the shell will be able to bond well with Li and thus be utilized as an anode active material.
[0028] FIG. 1 is a drawing illustrating the structure of a silicon nitride-silicon composite powder according to a preferred embodiment of the present invention.
[0029] Figure 2 is a schematic diagram showing how N2 on the surface is volatilized and Si is generated when Si3N4 powder is heat treated.
[0030] Figure 3 is a diagram showing the decomposition region of Si3N4 and the melting temperature of silicon according to temperature and pressure.
[0031] Figures 4 and 5 are photographs showing silicon nitride-silicon composite powder manufactured according to Experimental Example 1 observed using a transmission electron microscope.
[0032] Figures 6 and 7 are photographs showing silicon nitride-silicon composite powder manufactured according to Experimental Example 2 observed using a transmission electron microscope.
[0033] A silicon nitride-silicon composite powder according to a preferred embodiment of the present invention has a core-shell structure, with Si3N4 forming the core and a silicon (Si) layer forming the shell.
[0034] A method for producing silicon nitride according to a preferred embodiment of the present invention comprises the steps of (a) preparing Si3N4 powder as a starting material; and (b) heat-treating the Si3N4 powder in a vacuum to form a silicon layer, wherein Si3N4 forms a core and the silicon (Si) layer forms a shell.
[0035] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the following embodiments are provided to enable those of ordinary skill in the art to fully understand the present invention, and may be modified in various other forms, and the scope of the present invention is not limited to the embodiments described below.
[0036] When it is said in the detailed description or claims of an invention that one component "includes" another component, this is not to be construed as being limited to that component alone, unless specifically stated to the contrary, and should be understood to mean that it may further include other components.
[0037] A silicon nitride-silicon composite powder according to a preferred embodiment of the present invention has a core-shell structure, with Si3N4 forming the core and a silicon (Si) layer forming the shell.
[0038] The thickness of the silicon layer forming the above shell may be approximately 2 to 100 nm.
[0039] The silicon layer forming the above shell may be a layer doped with a metal.
[0040] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0041] The surface of Si3N4 forming the above core may be doped with metal.
[0042] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0043] A method for producing silicon nitride according to a preferred embodiment of the present invention comprises the steps of (a) preparing Si3N4 powder as a starting material; and (b) heat-treating the Si3N4 powder in a vacuum to form a silicon layer, wherein Si3N4 forms a core and the silicon (Si) layer forms a shell.
[0044] By controlling the above heat treatment conditions, the thickness of the silicon layer forming the shell can be made to be 2 to 100 nm.
[0045] Before the above step (b), a step of surface-treating the Si3N4 powder with a solution in which a metal salt is dissolved may be further included, and the silicon layer forming the shell may be a layer doped with a metal that is a component of the metal salt.
[0046] The above metal salt may include one or more salts selected from the group consisting of metal nitrates and metal sulfates.
[0047] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0048] The surface of Si3N4 forming the above core may be doped with metal.
[0049] The above metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
[0050] It is preferable to perform the above heat treatment at a temperature of 1000 to 1500 ℃.
[0051] The above heat treatment is carried out at 10 below atmospheric pressure. -13 10 inland -2 It is desirable to perform the operation in a vacuum of MPa.
[0052] The above heat treatment can be performed in an inert gas atmosphere.
[0053] The above step (a) may include a step of synthesizing Si3N4 powder by nitriding Si powder in a gas atmosphere containing a nitrogen component.
[0054] Hereinafter, a silicon nitride-silicon composite powder according to a preferred embodiment of the present invention is described in more detail.
[0055] Some ceramics exhibit relatively high thermal conductivity. The thermal conductivity of these ceramics is closely related to their crystal structure. Ceramics with high thermal conductivity are composed of light elements with strong interatomic bonds, resulting in highly symmetrical crystal structures. This facilitates the transfer of lattice vibrations, resulting in high thermal conductivity. Silicon nitride (Si3N4) crystals also exhibit these characteristics, and the thermal conductivity of pure Si3N4 crystals is expected to exceed 200 W / mK.
[0056] Silicon nitride, represented by the chemical formula Si3N4, is an inorganic compound formed by combining silicic acid and nitrogen. Silicon nitride possesses physical properties such as high strength, high heat resistance, and insulation, and is utilized in various industrial fields. For example, silicon nitride is used as an additive to enhance the strength of rubber and plastics, as well as in high-strength ceramics, and in automotive and aircraft engine parts. Because of its high strength and excellent heat resistance, silicon nitride is also used in the military and defense industries. For example, it can be used as a radiation shielding material in radioactively contaminated areas.
[0057] Meanwhile, lithium secondary batteries are rechargeable and dischargeable secondary batteries composed of positive and negative electrode active materials, a separator, and an electrolyte. These batteries generate electrical energy through changes in chemical potential during the intercalation and deintercalation of lithium ions. These lithium secondary batteries boast high energy density, high electromotive force, and high capacity, and are therefore widely used in various fields.
[0058] Carbon-based materials, such as graphite and activated carbon, are primarily used as anode materials in lithium secondary batteries. However, carbon-based materials have a low theoretical capacity of approximately 400 mAh / g. To address this, extensive research is being conducted on high-capacity anode materials. Among these, silicon, with its high theoretical capacity, is attracting attention.
[0059] Silicon negative electrode materials have a theoretical capacity of approximately 4,200 mAh / g, which is nearly 10 times higher than that of graphite, and are being actively researched to overcome the limitations of lithium secondary batteries.
[0060] However, silicon anode materials experience high volume expansion of 300% during lithium insertion and de-insertion, which leads to pulverization and the formation of an unstable solid electrolyte interphase, resulting in reduced life characteristics.
[0061] To solve the problem of silicon, various studies are being conducted on silicon nanostructuring, porous silicon, silicon-carbon composites, silicon-metal oxide composites, etc., but there are limitations in effectively controlling the volume expansion problem of silicon, and most of them have the disadvantage of requiring the use of expensive chemical vapor deposition processes and complex processes.
[0062] The inventor of the present invention studied a method for utilizing silicon nitride as a negative electrode active material, and proposed a silicon nitride-silicon composite powder having a structure suitable for use as a negative electrode active material and a method for producing the same.
[0063] FIG. 1 is a drawing illustrating the structure of a silicon nitride-silicon composite powder according to a preferred embodiment of the present invention.
[0064] Referring to FIG. 1, a silicon nitride-silicon composite powder according to a preferred embodiment of the present invention has a core-shell structure. The core-shell structure is a structure in which a core (10) is surrounded by a shell (20). The core-shell structure is a particle composed of a core and a shell, where the core is a small particle and the shell is a layer of material surrounding the core. The silicon nitride-silicon composite powder according to a preferred embodiment of the present invention has a core-shell structure in which Si3N4 forms the core (10) and a silicon (Si) layer forms the shell (20).
[0065] The thickness of the silicon layer forming the shell (20) may be 2 to 100 nm, specifically 2 to 20 nm.
[0066] The silicon layer (Si layer) forming the shell (20) may be a layer doped with a metal. The metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti.
[0067] The surface of Si3N4 forming the core (10) may also be doped with a metal. The metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti.
[0068] The silicon nitride-silicon composite powder according to a preferred embodiment of the present invention can be utilized as a negative electrode active material by utilizing a Si structure with a nano-unit thickness.
[0069] Hereinafter, a method for manufacturing a silicon nitride-silicon composite powder according to a preferred embodiment of the present invention will be described in more detail.
[0070] <Example 1>
[0071] Prepare Si3N4 powder as a starting material. The particle size of the Si3N4 powder is not particularly limited, but it may preferably be a powder having a particle size of approximately 1 nm to 500 μm. Considering that the Si3N4 powder is to be used as a negative electrode active material, it is preferable that it be a powder having a spherical shape.
[0072] The above Si3N4 powder is heat-treated in a vacuum state to form a silicon layer (Si layer). The heat treatment is preferably performed at a temperature of about 1000 to 1500°C. The vacuum state is a state in which there is almost no air and the pressure is lower than atmospheric pressure (1013 millibars, about 760 mmHg). The heat treatment is performed at 10 -13 10 inland -2 MPa or so, more specifically 10 -11 10 inland -3 It is desirable to perform the operation in a vacuum of about MPa.
[0073] Below, the heat treatment process is described in more detail.
[0074] Si3N4 powder is placed in a crucible and placed in a heat treatment device.
[0075] The above crucible is installed inside the chamber, and Si3N4 powder is contained inside the crucible. The Si3N4 powder contained inside the crucible is heated by a heating source. The crucible itself acts as a heating source and may be made of graphite material having a high melting point. The crucible may be provided in a form including a main body and a cover.
[0076] The above heat treatment device includes a chamber in which a crucible is accommodated and a heating source for heating the interior of the chamber.
[0077] A chamber is required to block the heat of a heated crucible from escaping to the outside and to create a vacuum state. The chamber provides a sealed space so that heating can be performed in a vacuum state. The crucible is accommodated inside the chamber. The chamber may be provided with a gas exhaust port (not shown), and an exhaust device (not shown) such as a pump may be installed in the gas exhaust port. The pressure inside the chamber can be controlled by the exhaust device. The exhaust device may include a vacuum pump for creating a vacuum state inside the chamber or exhausting gas, valves for blocking or controlling exhaust of gas by the vacuum pump, and a vacuum gauge for measuring the vacuum level inside the chamber.
[0078] The above heating source heats a crucible containing Si3N4 powder. The heating source may include a high-frequency induction coil or a heater, etc. The heating source is preferably installed around a portion where the crucible is seated so as to heat the crucible. When the heating source is a high-frequency induction coil, a magnetic field generated by flowing current through the high-frequency induction coil inductively heats the crucible. The heating source may be formed in the form of a cylindrical coil surrounding the crucible seated in the chamber. The high-frequency induction coil is connected to a high-frequency generator, and high-frequency power (RF power) generated from the high-frequency generator is applied through the high-frequency induction coil. The crucible can be heated to a target temperature through the heating source. Since the configuration and operation of such a heating source are already known, a detailed description thereof is omitted herein.
[0079] A cooling cylinder (not shown) may be provided around the above heating source, and the crucible may be cooled by cooling water (CW) flowing inside the cooling cylinder, thereby preventing the crucible from overheating and lowering the temperature inside the chamber. A cooling water inlet (CWI) is connected to the cooling cylinder to supply cooling water, and the supplied cooling water is discharged through a cooling water outlet (CWO), and the cooling water is circulated through the cooling cylinder so that the inside of the chamber can be evenly cooled as a whole.
[0080] The exterior of the chamber may be provided with insulation to suppress heat release, and the insulation may be provided in a form that wraps around the perimeter of the chamber. The insulation serves to block heat generated by the heating source from escaping to the outside.
[0081] Using the above-described heat treatment device, Si3N4 powder is heat-treated in a vacuum to form a silicon layer (Si layer). When Si3N4 powder is heat-treated, a decomposition reaction occurs on the Si3N4 surface, forming a silicon layer. Fig. 2 is a schematic diagram showing how N2 on the surface is volatilized and Si is generated when Si3N4 powder is heat-treated. It is preferable that the heat treatment be performed at a temperature of about 1000 to 1500°C, more preferably 1000°C or higher and lower than 1405°C. If the heat treatment temperature is high, bonding may occur between some powders due to melting of silicon. Taking this into consideration, it is preferable to perform the heat treatment at a temperature lower than the melting temperature of silicon (1405°C).
[0082] The above heat treatment is performed under vacuum conditions lower than atmospheric pressure, for example, 10 -13 10 inland -2 It is desirable to perform the operation in a vacuum of about MPa.
[0083] Figure 3 is a diagram showing the decomposition region of Si3N4 and the melting temperature of silicon according to temperature and pressure.
[0084] Referring to Fig. 3, as the vacuum pressure decreases, the decomposition temperature of Si3N4 decreases, and as the vacuum pressure increases, the decomposition temperature of Si3N4 increases. It is desirable to determine the heat treatment temperature and vacuum degree by considering the correlation between the vacuum pressure and the decomposition temperature of Si3N4.
[0085] The time for the above heat treatment is preferably 1 to 24 hours, more specifically 1 to 12 hours.
[0086] The above heat treatment may be performed in an inert gas atmosphere such as argon (Ar) or helium (He).
[0087] When the above heat treatment is completed, the crucible is unloaded.
[0088] Through the above heat treatment, a silicon layer (Si layer) is formed on the surface of the Si3N4 powder, forming a core-shell structure.
[0089] The silicon nitride-silicon composite powder thus manufactured has a core-shell structure, in which Si3N4 forms the core and a silicon (Si) layer forms the shell. The thickness of the silicon layer forming the shell may be 2 to 100 nm, specifically 2 to 20 nm. The thickness of the silicon layer can be controlled by heat treatment conditions, etc. For example, the thickness of the silicon layer can be adjusted by appropriately controlling the heat treatment temperature, heat treatment time, vacuum pressure, etc.
[0090] <Example 2>
[0091] Prepare Si3N4 powder as a starting material. The particle size of the Si3N4 powder is not particularly limited, but it may preferably be a powder having a particle size of approximately 1 nm to 500 μm. Considering that the Si3N4 powder is to be used as a negative electrode active material, it is preferable that it be a powder having a spherical shape.
[0092] The Si3N4 powder is surface-treated to dope a metal into the silicon layer formed after heat treatment. The surface treatment can be performed by a method such as immersing in a solution in which a metal salt is dissolved. The metal salt may be a salt containing at least one metal component selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti. More specifically, the metal salt may include at least one salt selected from the group consisting of metal nitrates and metal sulfates. More specifically, it may be a metal nitrate, a metal sulfate, a mixture thereof, etc. containing at least one metal component selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti. The solution is a solution in which a metal salt is dissolved in a solvent. The solvent described above is a substance capable of dissolving a metal salt, and may be a polar solvent such as water (H2O) or a non-polar solvent such as alcohol. The surface is treated by immersing Si3N4 powder in a solution containing a dissolved metal salt, and then drying. By performing surface treatment using a metal salt in this manner before heat treatment, the silicon layer formed after heat treatment can be doped with metal.
[0093] The surface-treated Si3N4 powder is heat-treated in a vacuum. The heat treatment device has already been described in Example 1.
[0094] The above heat treatment is preferably performed at a temperature of about 1000 to 1500°C. When the heat treatment temperature is reached, a decomposition reaction occurs on the Si3N4 surface, and a silicon layer is formed. The above heat treatment is preferably performed at a temperature of about 1000 to 1500°C, more preferably at a temperature of 1000°C or higher and lower than 1405°C. If the heat treatment temperature is high, bonding may occur between some powders due to melting of silicon, and taking this into consideration, it is preferable to perform the heat treatment at a temperature lower than the melting temperature of silicon (1405°C).
[0095] The above heat treatment is performed under vacuum conditions lower than atmospheric pressure, for example, 10 -13 10 inland -2 MPa or so, more specifically 10 -11 10 inland -3 It is desirable to perform the operation in a vacuum of about MPa.
[0096] As the vacuum pressure decreases, the decomposition temperature of Si3N4 decreases, and as the vacuum pressure increases, the decomposition temperature of Si3N4 increases. It is desirable to determine the heat treatment temperature and vacuum degree by considering the correlation between the vacuum pressure and the decomposition temperature of Si3N4.
[0097] The time for the above heat treatment is preferably 1 to 24 hours, more specifically 1 to 12 hours.
[0098] The above heat treatment may be performed in an inert gas atmosphere such as argon (Ar) or helium (He).
[0099] When the above heat treatment is completed, the crucible is unloaded.
[0100] Through the above heat treatment, a silicon layer (Si layer) is formed on the surface of the Si3N4 powder, forming a core-shell structure.
[0101] The silicon nitride-silicon composite powder thus manufactured has a core-shell structure, in which Si3N4 forms the core and a silicon (Si) layer forms the shell. The thickness of the silicon layer forming the shell may be 2 to 100 nm, specifically 2 to 20 nm. The thickness of the silicon layer can be controlled by heat treatment conditions, etc. For example, the thickness of the silicon layer can be adjusted by appropriately controlling the heat treatment temperature, heat treatment time, vacuum pressure, etc.
[0102] The silicon layer (Si layer) forming the shell is doped with a metal. The metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti. During the heat treatment process, the solvent component used for surface treatment or the component of the metal salt other than the metal component volatilizes and disappears.
[0103] The surface of Si3N4 forming the core may also be doped with a metal. This is because the metal component may diffuse into the surface of Si3N4 during the heat treatment process. The metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti.
[0104] <Example 3>
[0105] Synthesize Si3N4 powder.
[0106] There is a method for synthesizing Si3N4 powder by directly nitriding silicon (Si). The direct nitriding method is a method for synthesizing Si3N4 powder by directly nitriding Si powder in a gas atmosphere containing a nitrogen component.
[0107] Silicon (Si) powder is prepared to synthesize Si3N4 powder. The quality of the synthesized silicon nitride powder may vary depending on the purity, particle size, shape, surface area, etc. of the raw material Si powder.
[0108] Si3N4 powder is synthesized by nitriding Si powder in a gas atmosphere containing a nitrogen component. The nitriding treatment of Si powder is preferably performed in a gas atmosphere containing a nitrogen component at a temperature of approximately 1200 to 1500°C. The nitriding time can be several hours to several days. Silicon nitride can be synthesized through heat treatment at a temperature below the melting temperature of Si (1405°C) with or without the addition of a catalyst in an atmosphere of NH3 gas, N2, and H2 gas containing a nitrogen component, or N2 gas. Examples of gases containing a nitrogen component include N2 and H2 gas. The reason for using H2 is that it not only promotes complete nitriding of Si but also controls the partial pressure of O2, which inhibits the nitriding reaction. The nitriding treatment of Si powder is preferably performed at a temperature of approximately 1200 to 1500°C, specifically, at a temperature of approximately 1200 to 1405°C. Since the direct nitridation of Si exhibits a highly exothermic reaction (e.g., about 725 kJ / mol at 1400°C), and theoretically, the temperature can rise to several hundred°C due to the reaction, it is desirable to perform the nitridation process below the melting point (melting temperature) of Si to avoid the phenomenon of Si melting and remaining unreacted in the reaction product. During the nitridation process, the silicon powder increases in weight (the theoretical weight increase rate is 66.7%) and is converted to silicon nitride (Si3N4), but the value may be about 60% lower than the theoretical value due to the evaporation of SiO(g) by the active oxidation reaction.
[0109] The synthesized silicon nitride (Si3N4) may be subjected to a pulverization process to obtain a target particle size. The pulverization may be performed using a ball mill, planetary mill, attrition mill, or the like.
[0110] Additionally, a process for removing impurity elements may be performed to increase the purity of the synthesized silicon nitride (Si3N4). Silicon (Si) can be dissolved in mixtures of hydrofluoric acid and nitric acid, alkaline hydroxide solutions, etc., and this characteristic can be utilized to selectively remove unreacted impurity elements, such as silicon (Si).
[0111] The Si3N4 powder synthesized in this way is not particularly limited in particle size, but may preferably be a powder having a particle size of approximately 1 nm to 500 μm. Considering that the Si3N4 powder is to be used as a negative electrode active material, it is preferable that it be a powder having a spherical shape.
[0112] The Si3N4 powder is heat-treated in a vacuum state to form a silicon layer (Si layer). The heat-treatment device and method have been described in Example 1, so a detailed description thereof is omitted here. The heat-treatment is preferably performed at a temperature of about 1000 to 1500°C. When the heat-treatment temperature is reached, a decomposition reaction occurs on the Si3N4 surface, and a silicon layer is formed. The heat-treatment is preferably performed at a temperature of about 1000 to 1500°C, more preferably at a temperature of 1000°C or higher and lower than 1405°C. If the heat-treatment temperature is high, bonding may occur between some powders due to melting of silicon. Considering this, it is preferable to perform the heat-treatment at a temperature lower than the melting temperature of silicon (1405°C). The heat-treatment is performed in a vacuum state lower than atmospheric pressure, for example, at a temperature of 10 -13 10 inland -2 MPa or so, more specifically 10 -1110 inland -3 It is preferable to perform the heat treatment in a vacuum of about MPa. As the vacuum pressure decreases, the decomposition temperature of Si3N4 decreases, and as the vacuum pressure increases, the decomposition temperature of Si3N4 increases. It is preferable to determine the heat treatment temperature and vacuum degree by considering the correlation between the vacuum pressure and the decomposition temperature of Si3N4. The heat treatment time is preferably 1 to 24 hours, and more specifically, 1 to 12 hours. The heat treatment may also be performed in an inert gas atmosphere such as argon (Ar) or helium (He).
[0113] Through the above heat treatment, a silicon layer (Si layer) is formed on the surface of the Si3N4 powder, forming a core-shell structure.
[0114] The silicon nitride-silicon composite powder thus manufactured has a core-shell structure, in which Si3N4 forms the core and a silicon (Si) layer forms the shell. The thickness of the silicon layer forming the shell may be 2 to 100 nm, specifically 2 to 20 nm. The thickness of the silicon layer can be controlled by heat treatment conditions, etc. For example, the thickness of the silicon layer can be adjusted by appropriately controlling the heat treatment temperature, heat treatment time, vacuum pressure, etc.
[0115] <Example 4>
[0116] Synthesize Si3N4 powder.
[0117] There is a method for synthesizing Si3N4 powder by directly nitriding silicon (Si). The direct nitriding method is a method for synthesizing Si3N4 powder by directly nitriding Si powder in a gas atmosphere containing a nitrogen component.
[0118] Silicon (Si) powder is prepared to synthesize Si3N4 powder. The quality of the synthesized silicon nitride powder may vary depending on the purity, particle size, shape, surface area, etc. of the raw material Si powder.
[0119] Si3N4 powder is synthesized by nitriding Si powder in a gas atmosphere containing a nitrogen component. The nitriding treatment of Si powder is preferably performed in a gas atmosphere containing a nitrogen component at a temperature of approximately 1200 to 1500°C. The nitriding time can be several hours to several days. Silicon nitride can be synthesized through heat treatment at a temperature below the melting temperature of Si (1405°C) with or without the addition of a catalyst in an atmosphere of NH3 gas, N2, and H2 gas containing a nitrogen component, or N2 gas. Examples of gases containing a nitrogen component include N2 and H2 gas. The reason for using H2 is that it not only promotes complete nitriding of Si but also controls the partial pressure of O2, which inhibits the nitriding reaction. The nitriding treatment of Si powder is preferably performed at a temperature of approximately 1200 to 1500°C, specifically, at a temperature of approximately 1200 to 1405°C. Since the direct nitridation of Si exhibits a highly exothermic reaction (e.g., about 725 kJ / mol at 1400°C), and theoretically, the temperature can rise to several hundred°C due to the reaction, it is desirable to perform the nitridation process below the melting point (melting temperature) of Si to avoid the phenomenon of Si melting and remaining unreacted in the reaction product. During the nitridation process, the silicon powder increases in weight (the theoretical weight increase rate is 66.7%) and is converted to silicon nitride (Si3N4), but the value may be about 60% lower than the theoretical value due to the evaporation of SiO(g) by the active oxidation reaction.
[0120] The synthesized silicon nitride (Si3N4) may be subjected to a pulverization process to obtain a target particle size. The pulverization may be performed using a ball mill, planetary mill, attrition mill, or the like.
[0121] Additionally, a process for removing impurity elements may be performed to increase the purity of the synthesized silicon nitride (Si3N4). Silicon (Si) can be dissolved in mixtures of hydrofluoric acid and nitric acid, alkaline hydroxide solutions, etc., and this characteristic can be utilized to selectively remove unreacted impurity elements, such as silicon (Si).
[0122] The Si3N4 powder synthesized in this way is not particularly limited in particle size, but may preferably be a powder having a particle size of approximately 1 nm to 500 μm. Considering that the Si3N4 powder is to be used as a negative electrode active material, it is preferable that it be a powder having a spherical shape.
[0123] The synthesized Si3N4 powder is surface-treated. The surface treatment can be performed by a method such as immersing in a solution in which a metal salt is dissolved. The metal salt may be a salt containing at least one metal component selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti. More specifically, the metal salt may include at least one salt selected from the group consisting of metal nitrates and metal sulfates. More specifically, it may be a metal nitrate, a metal sulfate, a mixture thereof, etc. containing at least one metal component selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti. The solution is a solution in which a metal salt is dissolved in a solvent. The solvent described above is a substance capable of dissolving a metal salt, and may be a polar solvent such as water (H2O) or a non-polar solvent such as alcohol. The surface is treated by immersing Si3N4 powder in a solution containing a dissolved metal salt, and then drying. By performing surface treatment using a metal salt in this manner before heat treatment, the silicon layer formed after heat treatment can be doped with metal.
[0124] The surface-treated Si3N4 powder is heat-treated in a vacuum. The heat-treatment device and method have been described in Example 1, so a detailed description thereof is omitted here. The heat-treatment is preferably performed at a temperature of about 1000 to 1500°C. When the heat-treatment temperature is reached, a decomposition reaction occurs on the Si3N4 surface, and a silicon layer is formed. The heat-treatment is preferably performed at a temperature of about 1000 to 1500°C, more preferably at a temperature of 1000°C or higher and lower than 1405°C. If the heat-treatment temperature is high, bonding may occur between some powders due to melting of silicon. Considering this, it is preferable to perform the heat-treatment at a temperature lower than the melting temperature of silicon (1405°C). The heat-treatment is performed in a vacuum state lower than atmospheric pressure, for example, at 10 -13 10 inland -2 MPa or so, more specifically 10 -11 10 inland -3 It is preferable to perform the heat treatment in a vacuum of about MPa. As the vacuum pressure decreases, the decomposition temperature of Si3N4 decreases, and as the vacuum pressure increases, the decomposition temperature of Si3N4 increases. It is preferable to determine the heat treatment temperature and vacuum degree by considering the correlation between the vacuum pressure and the decomposition temperature of Si3N4. The heat treatment time is preferably 1 to 24 hours, and more specifically, 1 to 12 hours. The heat treatment may also be performed in an inert gas atmosphere such as argon (Ar) or helium (He).
[0125] Through the above heat treatment, a silicon layer (Si layer) is formed on the surface of the Si3N4 powder, forming a core-shell structure.
[0126] The silicon nitride-silicon composite powder thus manufactured has a core-shell structure, in which Si3N4 forms the core and a silicon (Si) layer forms the shell. The thickness of the silicon layer forming the shell may be 2 to 100 nm, specifically 2 to 20 nm. The thickness of the silicon layer can be controlled by heat treatment conditions, etc. For example, the thickness of the silicon layer can be adjusted by appropriately controlling the heat treatment temperature, heat treatment time, vacuum pressure, etc.
[0127] The silicon layer (Si layer) forming the shell is doped with a metal. The metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti. During the heat treatment process, the solvent component used for surface treatment or the component of the metal salt other than the metal component volatilizes and disappears.
[0128] The surface of Si3N4 forming the core may also be doped with a metal. This is because the metal component may diffuse into the surface of Si3N4 during the heat treatment process. The metal may include one or more metals selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti.
[0129] Hereinafter, experimental examples according to the present invention are specifically presented, and the present invention is not limited to the experimental examples presented below.
[0130] Experimental Example 1
[0131] Si3N4 powder was prepared as a starting material. The Si3N4 powder used had an average particle diameter of approximately 1 ㎛.
[0132] The above Si3N4 powder was placed in a graphite crucible, and the crucible was placed in a heat treatment device.
[0133] A silicon layer was formed on the surface of Si3N4 by heat treatment in a vacuum using the above heat treatment device. The heat treatment was performed at a temperature of 1350°C for 10 -9 It was performed under a vacuum of about MPa. The heat treatment was performed for 1 hour.
[0134] The silicon nitride-silicon composite powder thus manufactured was observed using a transmission electron microscope, and is shown in Figs. 4 and 5. Fig. 5 is an enlarged transmission electron microscope photograph of part 'A' of Fig. 4.
[0135] Referring to FIGS. 4 and 5, it was confirmed that the silicon nitride-silicon composite powder manufactured according to Experimental Example 1 had a core-shell structure. It has a core-shell structure in which Si3N4 forms the core and a silicon (Si) layer forms the shell. The thickness of the silicon layer forming the shell was approximately 4 to 5 nm.
[0136] Experimental Example 2
[0137] Si3N4 powder was prepared as a starting material. The Si3N4 powder used had an average particle diameter of approximately 1 ㎛.
[0138] For surface treatment, 1 g of magnesium nitrate (Mg nitrate) was dissolved in 100 ml of distilled water to form an aqueous solution. 20 g of Si3N4 powder was immersed in the aqueous solution and then dried to perform surface treatment.
[0139] The surface-treated Si3N4 powder was placed in a graphite crucible, and the crucible was placed in a heat treatment device.
[0140] Using the above heat treatment device, a silicon layer doped with Mg was formed on the surface of Si3N4 by heat treatment in a vacuum. The heat treatment was performed at a temperature of 1300°C for 10 -9It was performed under a vacuum of about MPa. The heat treatment was performed for 1 hour.
[0141] The silicon nitride-silicon composite powder thus manufactured was observed using a transmission electron microscope, and is shown in Figs. 6 and 7. Fig. 7 is a transmission electron microscope photograph enlarged from part 'B' of Fig. 6.
[0142] Referring to FIGS. 6 and 7, it was confirmed that the silicon nitride-silicon composite powder manufactured according to Experimental Example 2 had a core-shell structure. It has a core-shell structure in which Si3N4 forms the core and a Mg-doped silicon (Si) layer forms the shell. The thickness of the Mg-doped silicon layer was approximately 4 to 5 nm.
[0143] Above, the preferred embodiments of the present invention have been described in detail, but the present invention is not limited to the above embodiments, and various modifications are possible by those skilled in the art.
[0144] According to the present invention, it is possible to form a Si layer (Si film) on the surface whose thickness can be precisely controlled from several to several tens of nanometers, and it can be used as an anode active material of a secondary battery using a Si structure with a thickness in nanometer units, and has industrial applicability.
Claims
1. It has a core-shell structure, Silicon nitride-silicon composite powder in which Si3N4 forms the core and a silicon (Si) layer forms the shell.
2. A silicon nitride-silicon composite powder characterized in that the thickness of the silicon layer forming the shell in the first paragraph is 2 to 100 nm.
3. A silicon nitride-silicon composite powder, characterized in that the silicon layer forming the shell in the first paragraph is a layer doped with a metal.
4. In the third paragraph, a silicon nitride-silicon composite powder characterized in that the metal comprises at least one metal selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W, and Ti.
5. In the first paragraph, the surface of Si3N4 forming the core is doped with metal, A silicon nitride-silicon composite powder characterized in that the metal comprises at least one metal selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti. 6.(a) Step of preparing Si3N4 powder as a starting material; and (b) a step of heat-treating the Si3N4 powder in a vacuum to form a silicon layer; A method for manufacturing a silicon nitride-silicon composite powder in which Si3N4 forms a core and the silicon (Si) layer forms a shell.
7. A method for producing a silicon nitride-silicon composite powder, characterized in that in paragraph 6, the heat treatment conditions are adjusted so that the thickness of the silicon layer forming the shell is 2 to 100 nm.
8. In paragraph 6, before step (b), It further includes a step of surface-treating the above Si3N4 powder with a solution containing dissolved metal salt, A method for manufacturing a silicon nitride-silicon composite powder, characterized in that the silicon layer forming the shell is a layer doped with a metal that is a component of a metal salt.
9. A method for producing a silicon nitride-silicon composite powder, characterized in that in paragraph 8, the metal salt comprises at least one salt selected from the group consisting of metal nitrates and metal sulfates.
10. A method for producing a silicon nitride-silicon composite powder, characterized in that in paragraph 8, the metal comprises at least one metal selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
11. In the 6th paragraph, the surface of Si3N4 forming the core is doped with metal, A method for producing a silicon nitride-silicon composite powder, characterized in that the metal comprises at least one metal selected from the group consisting of Al, Mg, Ni, Co, Fe, Cr, V, Ti, Cu, B, Ca, Zn, Nb, Mo, Sr, Sb, W and Ti.
12. A method for producing a silicon nitride-silicon composite powder, characterized in that in paragraph 6, the heat treatment is performed at a temperature of 1000 to 1500°C.
13. In the 6th paragraph, the heat treatment is performed at a pressure 10 lower than atmospheric pressure. -13 10 inland -2 A method for producing a silicon nitride-silicon composite powder, characterized in that the method is performed in a vacuum state of MPa.
14. A method for producing a silicon nitride-silicon composite powder, characterized in that the heat treatment in paragraph 6 is performed in an inert gas atmosphere.
15. In paragraph 6, step (a) is, A method for producing a silicon nitride-silicon composite powder, characterized by including a step of synthesizing Si3N4 powder by nitriding Si powder in a gas atmosphere containing a nitrogen component.
Citation Information
Patent Citations
Negative electrode active material and lithium ion secondary battery
JP2014116201A
Si / Si3N4 type nanoparticles, biomaterial labeling agent using the nanoparticles, and method for producing the nanoparticles.
JP5082860B2
Anode active materials and lithium secondary battery comprising the same
KR1020150061695A
Negative eletrode active material, negative electrode comprising the negative electrode material and lithium secondarty battery comprising the negative electrode