Composite cathode active material, preparation method therefor, cathode comprising same, and solid-state secondary battery

The composite cathode active material with a lithium sulfide core and carbon-based shell enhances the performance and safety of all-solid-state batteries by mitigating polysulfide reactions and eliminating flammable solvent risks, improving lifespan and capacity.

WO2024205085A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD

Patent Information

Application Number
PCT/KR2024/003342
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-26
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium sulfur batteries face challenges with polysulfide side reactions during charging and discharging, leading to reduced lifespan and capacity due to the use of sulfur-based materials, and safety concerns arise from flammable organic solvents in traditional lithium batteries.

Method used

A composite cathode active material is developed, comprising a lithium-containing sulfide-based core coated with a shell of metal oxides and carbon-based materials, including fibrous carbon, to suppress polysulfide side reactions and enhance electrical conductivity, integrated into an all-solid-state battery with a solid electrolyte.

Benefits of technology

The composite cathode active material improves the lifespan and capacity characteristics of all-solid-state secondary batteries by reducing internal resistance and preventing polysulfide-related degradation, while eliminating the risk of fires associated with flammable solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003342_03102024_PF_FP_ABST
    Figure KR2024003342_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a composite cathode active material, a preparation method therefor, a cathode comprising same, and a solid-state secondary battery, the composite cathode active material comprising: a core comprising a lithium-containing sulfide-based cathode active material; and a shell disposed along the surface of the core, wherein the shell comprises at least one first metal oxide represented by chemical formula MaOb (0<a≤3, 0<b<4, and if a is 1, 2 or 3, b is not an integer), a first carbon-based material and a second carbon-based material, the first metal oxide is disposed inside a first carbon-based material matrix, M is at least one metal selected from the elements of groups 2-16 on the periodic table, and the second carbon-based material comprises a fibrous carbon having an aspect ratio of 10 or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Composite cathode active material, method for manufacturing the same, cathode and all-solid-state secondary battery containing the same

[0001] The present invention relates to a composite cathode active material, a method for manufacturing the same, a cathode including the same, and an all-solid-state secondary battery.

[0002] Recent industrial demands have led to the active development of batteries with high energy density and safety. For example, lithium batteries are being used not only in information and communication devices, but also in the automotive sector. Safety is particularly important in the automotive sector, as it is directly related to life.

[0003] Because lithium batteries use an electrolyte containing a flammable organic solvent, there is a risk of overheating and fire if a short circuit occurs.

[0004] All-solid-state batteries using solid electrolytes instead of electrolytes are being proposed.

[0005] All-solid-state batteries do not use flammable organic solvents, significantly reducing the risk of fire or explosion in the event of a short circuit. These all-solid-state batteries significantly improve safety compared to lithium batteries that use electrolytes.

[0006] Secondary batteries use sulfur-based materials as cathode active materials to increase capacity. The use of sulfur-based materials increases the theoretical energy capacity of secondary batteries compared to lithium-ion batteries, and their low cost reduces the manufacturing cost of secondary batteries.

[0007] During the charge / discharge process of a secondary battery, polysulfides are generated from sulfur-based materials. These polysulfides migrate to the cathode and react with it. This side reaction degrades the life and capacity characteristics of the secondary battery.

[0008] One aspect is to provide a composite cathode active material and a method for manufacturing the same with improved capacity by suppressing side reactions caused by polysulfide.

[0009] Another aspect is to provide a positive electrode comprising the composite positive electrode active material described above.

[0010] Another aspect is to provide an all-solid-state secondary battery with improved life characteristics, including the above-described positive electrode.

[0011] Depending on one aspect

[0012] A core comprising a lithium-containing sulfide-based positive electrode active material; and a shell disposed along the surface of the core;

[0013] The above shell has the chemical formula MaOb (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되는 1종 이상의 제1 금속산화물; 제1탄소계 재료 및 제2탄소계 재료를 포함하며, 상기 제1 금속산화물이 제1탄소계 재료 메트릭스 내에 배치되며, 상기 M은 원소주기율표 2족 내지 16족 중에서 선택된 하나 이상의 금속이며,

[0014] A composite cathode active material is provided, wherein the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more.

[0015] According to another aspect, an all-solid-state battery comprising a positive electrode layer; a negative electrode layer; and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer,

[0016] An all-solid-state battery is provided, wherein the positive electrode layer includes the positive electrode described above.

[0017] According to another aspect, a step of providing a lithium-containing sulfide compound; a step of providing a composite; a first step of providing a second carbon-based material; and

[0018] i) a second step including a step of mechanically milling the lithium-containing sulfide compound, composite and second carbon-based material; or

[0019] ii) a step of mechanically milling the lithium-containing sulfide compound and the composite; and a second step of mixing a second carbon-based material into the milled product,

[0020] The above-described composite cathode active material is manufactured,

[0021] The above complex has the chemical formula M a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되는 1종 이상의 제1 금속산화물, 제1 탄소계 재료 및 제2탄소계 재료를 포함하며,

[0022] The first metal oxide is arranged in a first carbon-based material matrix, and M is at least one metal selected from groups 2 to 13, 15, and 16 of the periodic table of elements.

[0023] A method for manufacturing a composite cathode active material is provided, wherein the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more.

[0024] According to one aspect, it is possible to provide an all-solid-state secondary battery with improved capacity and lifespan characteristics by using a composite cathode active material according to an embodiment.

[0025] Figure 1 schematically illustrates the structure of a composite positive electrode active material according to an embodiment.

[0026] Figure 2 is a cross-sectional view of an all-solid-state secondary battery according to an embodiment.

[0027] Figure 3 is a cross-sectional view of an all-solid-state secondary battery according to another embodiment.

[0028] <Explanation of symbols for major parts of the drawing>

[0029] 1 All-solid-state secondary battery 10 Cathode layer

[0030] 11. Cathode current collector 12. Cathode active material layer

[0031] 20 Cathode layer 21 Cathode current collector

[0032] 22 First negative electrode active material layer 30 Solid electrolyte layer

[0033] Various embodiments are illustrated in the accompanying drawings. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Like reference numerals in the drawings indicate like elements.

[0034] When a component is referred to as being "on" another component, it can be understood that it is either directly on top of the other component or that other components may be intervening between them. Conversely, when a component is referred to as being "directly on" another component, no intervening components are present.

[0035] Although the terms "first," "second," "third," etc. may be used herein to describe various components, elements, regions, layers, and / or zones, these components, elements, regions, layers, and / or zones should not be limited by these terms. These terms are used only to distinguish one component, element, region, layer, or zone from another component, element, region, layer, or zone. Thus, a first component, element, region, layer, or zone described below may be referred to as a second component, element, region, layer, or zone without departing from the teachings of this specification.

[0036] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms including "at least one," unless the content clearly dictates otherwise. "At least one" should not be construed as limiting to the singular. As used herein, the term "and / or" includes any and all combinations of one or more of the listed items. The terms "comprises" and / or "comprising" as used in the detailed description specify the presence of stated features, regions, integers, steps, operations, components, and / or ingredients, but do not preclude the presence or addition of one or more other features, regions, integers, steps, operations, components, ingredients, and / or groups thereof.

[0037] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Furthermore, it will be understood that terms defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning within the context of the relevant art and the present disclosure, and not in an idealized or overly formal sense.

[0038] "Group" means a group in the periodic table of elements according to the International Union of Pure and Applied Chemistry ("IUPAC") Group 1-18 classification system.

[0039] In this specification, "particle size" refers to the average diameter when the particle is spherical, and the average major axis length when the particle is non-spherical. Particle size can be measured using a particle size analyzer (PSA). "Particle size" refers to the average particle diameter, for example. "Average particle size" refers to the median particle diameter, D50, for example.

[0040] D50 is the size of the particle corresponding to 50% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.

[0041] D90 is the size of the particle corresponding to 90% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.

[0042] D10 is the size of the particle corresponding to 10% of the cumulative volume, calculated from the particle side with a small particle size in the particle size distribution measured by laser diffraction.

[0043] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.

[0044] In this disclosure, “alloy” means a mixture of two or more metals.

[0045] While specific implementations have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently anticipated or unforeseen may occur to the applicant or those skilled in the art. Accordingly, the appended claims, as filed and as amended, are intended to encompass all such alternatives, modifications, variations, improvements, and substantial equivalents.

[0046] Hereinafter, composite cathode active materials, cathodes including the same, and all-solid-state secondary batteries according to exemplary embodiments will be described in more detail.

[0047] The composite cathode active material comprises a core including a lithium-containing sulfide-based cathode active material; and a shell disposed along the surface of the core, wherein the shell has the chemical formula MaOb (0 <a≤3, 0<b<4, a가 1, 2, 또는 3이면, b는 정수가 아님)로 표시되는 1종 이상의 제1 금속산화물; 제1탄소계 재료 및 제2탄소계 재료를 포함하며, 상기 제1 금속산화물이 제1 탄소계 재료 메트릭스 내에 배치되며, 상기 M은 원소주기율표 2족 내지 16족중에서 선택된 하나 이상의 금속이며, 상기 제2탄소계 재료가 종횡비 10 이상의 섬유상 탄소를 포함한다.

[0048] Referring to FIG. 1, the composite cathode active material (100) includes a core (110) and a shell (220) that is continuously or discontinuously arranged along the surface of the core (110). The shell (220) may cover all or part of the core (110). The core (110) includes a lithium-containing sulfide-based cathode active material, and the shell (220) includes a first metal oxide (221), a first carbon-based material (222), and a second carbon-based material (223).

[0049] Lithium-containing sulfide-based cathode active materials are insulators with virtually no electrical conductivity, but the aforementioned shell forms an effective conductive network. Consequently, a cathode comprising this composite cathode active material can produce an all-solid-state secondary battery with improved cycle life and high-rate characteristics, reduced volume expansion of the electrode terminals, increased composite density, and high-energy density.

[0050] The second carbon-based material (223) includes fibrous carbon having an aspect ratio of 10 or more. When manufacturing a composite cathode active material (100), a shell (20) may be disposed on a lithium-containing sulfide-based cathode active material core (10) using a composite including a plurality of first metal oxides (221) disposed in a matrix of a first carbon-based material (222). Accordingly, the shell (220) may be uniformly disposed on the core (110) while preventing agglomeration of the first carbon-based material (222). The shell (220) disposed on the core (110) may effectively block contact between the core (110) and the electrolyte. By effectively blocking contact between the core (110) and the electrolyte, a side reaction due to contact between the core (110) and the electrolyte may be prevented. In addition, by arranging the shell (220) on the core (110), cation mixing due to contact between the core (110) and the electrolyte can be suppressed. By suppressing cation mixing due to contact between the core (110) and the electrolyte, the formation of a resistance layer inside and / or on the surface of the composite cathode active material (100) can be suppressed. The first carbon-based material may be, for example, a crystalline carbon-based material. The first carbon-based material may be, for example, a carbon-based nanostructure. The first carbon-based material may be, for example, a carbon-based two-dimensional nanostructure. The first carbon-based material may be, for example, graphene. In this case, the shell including graphene and / or its matrix has flexibility, so that it can easily accommodate a change in the volume of the composite cathode active material during charge and discharge, thereby suppressing the occurrence of cracks inside the composite cathode active material. Graphene possesses high electronic conductivity, which can reduce the interfacial resistance between the composite cathode active material and the electrolyte. Therefore, the internal resistance of a lithium battery can be maintained or reduced even when a shell containing graphene is introduced. In contrast, conventional carbon-based materials readily aggregate, making it difficult to uniformly coat the lithium transition metal oxide core.

[0051] As described above, the shell includes a second carbon-based material that is fibrous carbon having 10 or more particles. Therefore, the conductive path of the composite cathode active material can be further lengthened. The second carbon-based material can form a three-dimensional conductive network between a plurality of composite cathode active materials, thereby reducing the internal resistance of the cathode including the composite cathode active material. By fixing the fibrous carbon on the composite cathode active material, a uniform and stable three-dimensional conductive network can be formed between the plurality of composite cathode active materials. Therefore, since the composite cathode active material includes the second carbon-based material, the high-rate characteristics of a lithium battery including the composite cathode active material can be improved. In contrast, a simple mixture of the core and the second carbon-based material, fibrous carbon, has difficulty forming a uniform three-dimensional conductive network between a plurality of particles due to aggregation of the fibrous carbon, etc. As shown in FIG. 1, the second carbon-based material (223) can be disposed on the surface of the composite cathode active material (100). In addition, the second carbon-based material (223) may protrude from the surface of the composite cathode active material (100). Therefore, the second carbon-based material (223) may effectively provide a conductive network between the plurality of composite cathode active materials (100). The second carbon-based material (223) may be easily coated on the core (110) by being disposed within the matrix of the first carbon-based material (222). The matrix of the first carbon-based material (222) may act as a binder that binds the core and the second carbon-based material (223). Therefore, when the matrix of the first carbon-based material (222) is absent, it may be difficult for the second carbon-based material (223) to be easily attached to the core (110) or the second carbon-based material (223) may be easily detached from the core (110) during the process of manufacturing a slurry for the cathode. When a binder is added to bond the core (220) and the second carbon-based material (223), the internal resistance of the composite cathode active material (100) may increase as the core (110) is covered with the insulating binder.When the core coated with the second carbon-based material and the binder is subjected to high-temperature heat treatment to carbonize the binder, the core (110) and the second carbon-based material (223) may deteriorate during the heat treatment process.

[0052] The aspect ratio of the second carbon-based material may be 10 or greater or 20 or greater. The aspect ratio of the second carbon-based material may be, for example, 10 to 100,000, 10 to 80,000, 10 to 50,000, 10 to 10,000, 10 to 5000, 10 to 1000, 10 to 500, 10 to 100, or 10 to 50. The aspect ratio of the second carbon-based material is, for example, a ratio of the length of a major axis passing through the center of the second carbon-based material, i.e., the second carbon-based material, to the length of a minor axis passing through the center of the second carbon-based material and perpendicular to the major axis, i.e., the diameter of the second carbon-based material.

[0053] The diameter of the second carbon-based material may be, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the second carbon-based material may be, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. If the diameter of the second carbon-based material is excessively large, the absolute number of strands per volume may decrease, resulting in a minimal effect in reducing internal resistance. If the diameter of the second carbon-based material is excessively small, uniform dispersion may be difficult.

[0054] The length of the second carbon-based material may be, for example, 1000 μm or less, 100 μm or less, 50 μm or less, 10 μm or less, 5 μm or less, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the second carbon-based material may be, for example, 100 nm to 1000 μm, 100 nm to 500 μm, 100 nm to 100 μm, 100 nm to 50 μm, 100 nm to 10 μm, 100 nm to 5 μm, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, or 100 nm to 300 nm. The length of the second carbon-based material may be, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 100 μm, 500 nm to 50 μm, 500 nm to 10 μm, 500 nm to 5 μm, or 500 nm to 2 μm. As the length of the second carbon-based material increases, the internal resistance of the electrode may decrease. If the length of the second carbon-based material is too short, it may be difficult to provide an effective conductive path.

[0055] The second carbon-based material may include, for example, carbon nanofibers, carbon nanotubes, or a combination thereof.

[0056] The carbon nanotube may include, for example, a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof.

[0057] The primary structure of a carbon nanotube is a single carbon nanotube unit. A carbon nanotube unit has a graphite sheet in the shape of a cylinder with a nano-sized diameter and an sp2 bonding structure. Depending on the angle and structure of the graphite sheet, it can exhibit the properties of a conductor or a semiconductor. Carbon nanotube units can be classified into single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNTs) depending on the number of bonds forming the wall. The thinner the wall of a carbon nanotube unit, the lower the resistance.

[0058] The carbon nanotube primary structure may include, for example, a single-walled carbon nanotube (SWCNT), a double-walled carbon nanotube (DWCNT), a multi-walled carbon nanotube (MWCNT), or a combination thereof. The diameter of the carbon nanotube primary structure may be, for example, 1 nm or more or 2 nm or more. The diameter of the carbon nanotube primary structure may be, for example, 20 nm or less or 10 nm or less. The diameter of the carbon nanotube primary structure may be, for example, 1 nm to 20 nm, 1 nm to 15 nm, or 1 nm to 10 nm. The length of the carbon nanotube primary structure may be, for example, 100 nm or more or 200 nm or more. The length of the carbon nanotube primary structure can be, for example, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the carbon nanotube primary structure can be, for example, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 300 nm, or 200 nm to 300 nm. The diameter and length of the carbon nanotube primary structure can be measured from scanning electron microscope (SEM) or transmission electron microscope (TEM) images.

[0059] Alternatively, the diameter and / or length of the carbon nanotube primary structure can be measured by laser diffraction.

[0060] A carbon nanotube secondary structure is a structure formed by assembling carbon nanotube primary structures, wholly or partially, into a bundle-type or bundle-type structure. The carbon nanotube secondary structure may include, for example, a bundle-type carbon nanotube, a rope-type carbon nanotube, or a combination thereof. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm or more, or 3 nm or more. The diameter of the carbon nanotube secondary structure may be, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm to 50 nm, 2 nm to 30 nm, or 2 nm to 20 nm. The length of the carbon nanotube secondary structure can be, for example, 500 nm or more, 700 nm or more, 1 μm or more, or 10 μm or more. The length of the carbon nanotube secondary structure can be, for example, 1000 μm or less, 500 μm or less, or 100 μm or less. The length of the carbon nanotube secondary structure can be, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 200 μm, 500 nm to 100 μm, or 500 nm to 50 μm. The diameter and length of the carbon nanotube secondary structure can be measured from a scanning electron microscope (SEM) image or an optical microscope. Alternatively, the diameter and / or length of the carbon nanotube secondary structure can be measured by laser diffraction.

[0061] Carbon nanotube secondary structures can be converted into carbon nanotube primary structures by dispersing them in a solvent, etc., and then used to manufacture composite cathode active materials.

[0062] According to an embodiment, when carbon nanofibers are used as the second carbon-based material, the diameter is 100 to 500 nm, or 200 to 400 nm, and the length is 10 to 100 um, 12 to 80 um, or 15 to 50 um. In addition, the aspect ratio of the carbon nanofibers is 30 to 100, 40 to 80, or 45 to 60.

[0063] According to another embodiment, when carbon nanotubes (CNTs) are used as the second carbon-based material, the diameter is 5 to 7 um, 5 to 6.5 um, or 5.5 to 6.5 nm, and the length is 50 to 150 um, 70 to 130 um, or 80 to 110 um.

[0064] The content of the second carbon-based material may be, for example, 0.1 wt % to 50 wt %, 1 wt % to 40 wt %, or 5 wt % to 30 wt % based on the total weight of the first carbon-based material and the second carbon-based material. When the composite cathode active material includes the first carbon-based material and the second carbon-based material in this range, a conduction path is more effectively secured within the composite cathode active material, so that the internal resistance of the composite cathode active material can be further reduced. As a result, the cycle characteristics of a lithium battery including the composite cathode active material can be further improved. The content of the second carbon-based material is 5 wt % to 20 wt %, 6 wt % to 19 wt %, 8 wt % to 19 wt %, or 9 wt % to 19 wt % based on 100 wt % of the total weight of the composite cathode active material. By including a second carbon-based material within this range, a conductive path is secured within the composite cathode active material, further reducing its internal resistance. Consequently, the cycle characteristics of a lithium battery containing the composite cathode active material can be further improved.

[0065] Below, the theoretical basis for the superior effect of the composite bipolar active material according to the embodiment is explained, but this is only to help understand the creative idea and is not intended to limit the creative idea in any way.

[0066] The composite cathode active material includes a first carbon-based material, and by using a composite including a plurality of first metal oxides arranged within the matrix, a uniform shell is arranged on the core while preventing agglomeration of the first carbon-based material. Accordingly, contact between the core and the electrolyte is effectively blocked, thereby effectively preventing side reactions due to contact between the core and the electrolyte. The first carbon-based material may be, for example, a crystalline carbon-based material. The first carbon-based material may be, for example, a carbon-based nanostructure. The first carbon-based material may be, for example, a carbon-based two-dimensional nanostructure. The first carbon-based material may be, for example, a carbon-based flake. The first carbon-based material may be, for example, graphene.

[0067] A shell including graphene and / or its matrix is ​​flexible and can easily accommodate changes in the volume of the core during charge and discharge. Therefore, the occurrence of cracks on the surface and / or inside of the composite cathode active material during charge and discharge is suppressed, thereby suppressing the formation of a solid electrolyte membrane (SEI) on the surface and / or inside of the composite cathode active material. Consequently, deterioration of a lithium battery including the composite cathode active material is suppressed. In contrast, in the case of conventional lithium-containing sulfide compounds, lithium polysulfides generated by the reaction between lithium ions and sulfur are dissolved in the electrolyte, resulting in a decrease in the capacity and life characteristics of the battery.

[0068] Lithium sulfide (Li2S) is an insulator with virtually no electrical conductivity. Therefore, to use it as a cathode active material, it must be composited with a highly conductive carbon material to overcome its low electrical conductivity. Furthermore, in all-solid-state lithium-sulfur batteries, the solid electrolyte layer, cathode, and anode composite layers contain virtually no solvent, resulting in low electronic and lithium ion conductivity, making it difficult to secure sufficient capacity during charge and discharge. Therefore, it is crucial to form an interface between the cathode active material and the solid electrolyte to facilitate electrochemical reactions.

[0069] Accordingly, the inventors of the present invention provide a composite cathode active material that can solve the problem of low electrical conductivity of lithium-containing sulfide compounds.

[0070] An all-solid-state secondary battery with improved life characteristics can be manufactured by coating a lithium-containing sulfide-based compound with a composite cathode active material according to an embodiment of the present invention and introducing a second carbon-based material between the lithium-containing sulfide-based compound particles coated with the composite to impart conductivity.

[0071] The composite cathode active material includes a matrix of a first carbon-based material, and when the first metal oxide is Al2O3 in the composite including a plurality of first metal oxides disposed within the matrix, Al2O3 reacts with Li of Li2S to form a lithium ion conductive compound such as LiAlO2, LiAlO4, etc., thereby imparting lithium ion conductivity to the composite cathode active material, thereby reducing the interfacial resistance between the composite cathode active material and the sulfide-based solid electrolyte at the cathode, thereby improving the cycle characteristics of the all-solid-state secondary battery. In addition, Al2O3 can improve the cycle characteristics by adsorbing lithium polysulfide and suppressing side reactions. In this way, Al2O3 has the effect of suppressing the dissolution of lithium polysulfide generated during battery operation. The matrix of the first carbon-based material (e.g., graphene matrix) imparts electronic conductivity to the composite cathode active material and buffers changes in the volume of the core, thereby improving the cycle characteristics of the all-solid-state secondary battery.

[0072] In the shell, the composite enables CNT anchoring through pi-pi bonding with fibrous carbons such as carbon nanotubes (CNTs). Since the CB and CNT coatings are manufactured dry, CNT separation, as in wet coating, is suppressed, and CNT separation from the composite cathode active material is not observed during the subsequent electrode slurry manufacturing process.

[0073] The content of the second carbon-based material in the shell is 5 to 20 wt%, 8 to 18 wt%, or 9 to 17 wt% based on 100 wt% of the total weight of the composite cathode active material. When within this range, the workability of the electrode slurry is excellent without increasing the viscosity.

[0074] Since the shell of the composite cathode active material includes a second carbon-based material, the composite cathode active material can additionally perform the role of a conductive material. Therefore, the content of the conductive material used in the cathode can be reduced. The conductive material is necessary to improve the conductivity of the battery, but if the content of the conductive material increases, the composite density of the cathode decreases, resulting in a decrease in the energy density of the lithium battery. In contrast, the cathode of the present invention can reduce the content of the conductive material without increasing the internal resistance by using the composite cathode active material described above. Therefore, the composite density of the cathode increases, resulting in an improvement in the energy density of the lithium battery. In particular, in a high-capacity lithium battery, the energy density of the lithium battery can be significantly increased by increasing the content of the composite cathode active material while reducing the content of the conductive material.

[0075] The first carbon-based material included in the shell of the composite cathode active material is derived from a graphene matrix, and therefore has a relatively low density and high porosity compared to conventional first carbon-based materials derived from graphite-based materials. The d002 interplanar distance of the first carbon-based material included in the shell of the composite cathode active material may be, for example, 3.38 Å or more, 3.40 Å or more, 3.45 Å or more, 3.50 Å or more, 3.60 Å or more, 3.80 Å or more, or 4.00 Å or more. The d002 interplanar distance of the first carbon-based material included in the shell of the composite cathode active material may be, for example, 3.38 to 4.0 Å, 3.38 to 3.8 Å, 3.38 to 3.6 Å, 3.38 to 3.5 Å, or 3.38 to 3.45 Å. In contrast, the d002 interplanar distance of a conventional carbon-based material derived from a graphite-based material may be, for example, 3.38 Å or less, or 3.35 to 3.38 Å.

[0076] The shell may comprise, for example, one kind of first metal oxide or two or more different kinds of first metal oxides.

[0077] As a result, the increase in internal resistance of a lithium battery including the composite cathode active material described above is suppressed, and high-temperature and high-voltage cycle characteristics are improved.

[0078] In the composite cathode active material, the content of the composite including the first metal oxide and the first carbon-based material is 25 to 40 wt%, or 27 to 40 wt%, based on 100 wt% of the total weight of the composite cathode active material. And the content of the first metal oxide in the composite is 60 to 80 wt%, 65 to 80 wt%, or 70 to 75 wt%, based on 100 wt% of the total weight of the composite. When the content of the first metal oxide in the composite is within the above range, the life characteristics and capacity characteristics of the all-solid-state secondary battery are further improved.

[0079] In the composite cathode active material, the content of the lithium-containing sulfide-based cathode active material is 40 to 65 parts by weight, 45 to 60 parts by weight, or 48 to 55 parts by weight based on 100% by weight of the total weight of the composite cathode active material. When the content of the lithium-containing sulfide-based cathode active material is within the above range, the life characteristics and capacity characteristics of the all-solid-state secondary battery are further improved.

[0080] The shell may further comprise a solid electrolyte, wherein the solid electrolyte is a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0081] The thickness of the shell is 10 nm to 2 ㎛, the shell has a single-layer structure or a multi-layer structure, the shell is a dry coating layer, and the content of the shell is 5 wt% or less with respect to the total weight of the composite positive electrode active material.

[0082] The content of the first metal included in the shell may be, for example, 0 to 10 at%, 0.1 to 9.5 at%, 1 to 9 at%, 2 to 9 at%, 3 to 9 at%, 3 to 8 at%, or 4 to 8 at%, based on the total number of atoms in the shell. By including the first metal in the shell having this content range, the cycle characteristics of the all-solid-state secondary battery including the composite cathode active material may be further improved. The content of the first metal element included in the shell may be obtained, for example, from a peak obtained by measuring an XPS spectrum on the surface of the composite cathode active material.

[0083] The content of carbon included in the shell may be, for example, 80 to 99 at%, 80 to 95 at%, 80 to 93 at%, 80 to 91 at%, or 83 to 90 at% based on the total number of atoms in the shell. By including carbon in the shell having this content range, the cycle characteristics of a lithium battery including the composite cathode active material may be further improved. The content of carbon included in the shell may be obtained, for example, from a peak obtained by measuring an XPS spectrum on the surface of the composite cathode active material.

[0084] The metal included in the first metal oxide may be, for example, one or more selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide may be, for example, Al2O z (0 <z<3), NbO x (0 <x<2.5), MgO x (0 <x<1), Sc2O z (0 <z<3), TiO y (0 <y<2), ZrO y (0 <y<2), V2O z (0 <z<3), WO y (0 <y<2), MnO y (0 <y<2), Fe2O z (0 <z<3), Co3O w(0 <w<4), PdO x (0 <x<1), CuO x (0 <x<1), AgO x (0 <x<1), ZnO x (0 <x<1), Sb2O z (0 <z<3), 및 SeO y (0 <y<2) 중에서 선택된 하나 이상일 수 있다. 제1 탄소계 재료 메트릭스 내에 이러한 제1 금속산화물이 배치됨에 의하여 코어 상에 배치된 쉘의 균일성이 향상되고, 복합양극활물질의 내전압성이 더욱 향상된다. 예를 들어, 쉘은 제1 금속산화물로서 Al2O x (0 <x<3)를 포함한다.

[0085] The shell has the chemical formula M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 1종 이상의 제2 금속산화물을 더 포함할 수 있다. 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이다. 예를 들어, 제2 금속산화물은 상기 제1 금속산화물과 동일한 금속을 포함하며, 제2 금속산화물의 a 와 c의 비율인 c / a가 상기 제1 금속산화물의 a 와 b의 비율인 b / a에 비하여 더 큰 값을 가진다. 예를 들어, c / a > b / a. The second metal oxide is selected from, for example, Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide is a reduction product of the second metal oxide. The first metal oxide is obtained by reducing part or all of the second metal oxide. Therefore, the first metal oxide has a lower oxygen content and a higher oxidation number of the metal than the second metal oxide. For example, the shell is the first metal oxide Al2O x (0 <x<3) 및 제2 금속산화물인 Al2O3를 포함한다.

[0086] In a composite cathode active material, for example, a first carbon-based material included in a shell and a transition metal of a lithium transition metal oxide included in a core are chemically bound through a chemical bond. The carbon atoms (C) of the first carbon-based material included in the shell and the transition metal (Me) of the lithium transition metal oxide are chemically bound through, for example, a CO-Me bond (e.g., a CO-Ni bond or a CO-Co bond) mediated by an oxygen atom. The core and the shell are composited by the chemical bonding of the first carbon-based material included in the shell and the lithium transition metal oxide included in the core. Therefore, it is distinguished from a simple physical mixture of the first carbon-based material and the lithium transition metal oxide.

[0087] In addition, the first metal oxide and the first carbon-based material included in the shell are chemically bonded through a chemical bond. Here, the chemical bond is, for example, a covalent bond or an ionic bond. The covalent bond is, for example, a bond containing at least one of an ester group, an ether group, a carbonyl group, an amide group, a carbonate anhydride group, and an acid anhydride group. The ionic bond is, for example, a bond containing a carboxylic acid ion, an ammonium ion, an acyl cation group, etc.

[0088] The thickness of the shell is, for example, 1 nm to 5 um, 1 nm to 1 um, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 90 nm, 1 nm to 80 nm, 1 nm to 70 nm, 1 nm to 60 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, 1 nm to 20 nm. When the shell has a thickness in this range, an increase in the internal resistance of a lithium battery including a composite positive electrode active material is suppressed.

[0089] In the composite cathode active material, for example, a third metal doped on the core or a third metal oxide coated on the core may be further included. In addition, the shell may be disposed on the doped third metal or the coated third metal oxide. For example, after the surface of a lithium transition metal oxide included in the core is doped with the third metal or the surface of the lithium transition metal oxide is coated with the third metal oxide, the shell may be disposed on the third metal and / or the third metal oxide. For example, the composite cathode active material includes a core; an intermediate layer disposed on the core; and a shell disposed on the intermediate layer, and the intermediate layer may include a third metal or a third metal oxide. The third metal may be one or more metals selected from Al, Zr, W, and Co, and the third metal oxide may be Al2O3, Li2O-ZrO2, WO2, CoO, Co2O3, Co3O4, etc.

[0090] The shell included in the composite cathode active material includes, for example, at least one selected from a composite including a first metal oxide, a first carbon-based material such as graphene, and a milling result of the composite, wherein the first metal oxide is disposed within a matrix of the first carbon-based material, for example, a graphene matrix. The shell is manufactured from, for example, a composite including a first metal oxide, a first carbon-based material such as graphene. The composite may further include a second metal oxide in addition to the first metal oxide. The composite may include, for example, two or more types of the first metal oxide. The composite may include, for example, two or more types of the first metal oxide and two or more types of the second metal oxide.

[0091] The content of at least one of the composite and the milling result thereof included in the composite cathode active material may be 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, or 0.2 wt% or less of the total weight of the composite cathode active material. The content of at least one of the composite and the milling result thereof may be 0.01 wt% to 3 wt%, 0.01 wt% to 1 wt%, 0.01 wt% to 0.7 wt%, 0.01 wt% to 0.5 wt%, 0.01 wt% to 0.2 wt%, 0.01 wt% to 0.1 wt%, or 0.03 wt% to 0.07 wt% of the total weight of the composite cathode active material. When the composite cathode active material includes at least one of the composite and the milling result thereof in these ranges, the cycle characteristics of a lithium battery including the composite cathode active material are further improved.

[0092] The average particle size of at least one selected from the first metal oxide and the second metal oxide included in the composite may be 1 nm to 1 um, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 70 nm, 1 nm to 50 nm, 1 nm to 30 nm, 3 nm to 30 nm, 3 nm to 25 nm, 5 nm to 25 nm, 5 nm to 20 nm, or 7 nm to 20 nm. Since the first metal oxide and / or the second metal oxide have particle sizes in this nano-range, they can be more uniformly distributed within the first carbon-based material matrix of the composite. Therefore, the composite can be uniformly coated on the core without aggregation to form a shell. In addition, since the first metal oxide and / or the second metal oxide have particle sizes in this range, they can be more uniformly arranged on the core. Therefore, the voltage resistance characteristics can be more effectively exhibited by uniformly disposing the first metal oxide and / or the second metal oxide on the core.

[0093] The average particle diameter of the first metal oxide and the second metal oxide is measured using a measuring device such as a laser diffraction method or a dynamic light scattering method. The average particle diameter is measured using a laser scattering particle size distribution meter (e.g., Horiba LA-920), and is the value of the median particle diameter (D50) when 50% of the small particles are accumulated in volume conversion.

[0094] The uniformity deviation of at least one selected from among the first metal oxide and the second metal oxide included in the composite may be 3% or less, 2% or less, or 1% or less. The uniformity may be determined, for example, by XPS. Accordingly, at least one selected from among the first metal oxide and the second metal oxide within the composite may be uniformly distributed with a deviation of 3% or less, 2% or less, or 1% or less.

[0095] The first carbon-based material included in the composite has, for example, a branched structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide can be distributed within the branched structure of the first carbon-based material. The branched structure of the first carbon-based material includes, for example, a plurality of first carbon-based material particles that are in contact with each other. Since the first carbon-based material has a branched structure, it can provide various conductive paths.

[0096] The first carbon-based material included in the composite may be, for example, graphene. The graphene may have, for example, a branched structure, and one or more metal oxides selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the graphene. The branched structure of the graphene may include, for example, a plurality of graphene particles in contact with each other. By having a branched structure, the graphene may provide various conductive paths.

[0097] The first carbon-based material included in the composite has, for example, a spherical structure, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the first carbon-based material may be 50 nm to 300 nm. There may be a plurality of first carbon-based materials having a spherical structure. Since the first carbon-based material has a spherical structure, the composite may have a rigid structure.

[0098] The first carbon-based material included in the composite may be, for example, graphene. The graphene may have, for example, a spherical structure, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the graphene may be 50 nm to 300 nm. There may be a plurality of graphenes having a spherical structure. Since the graphene has a spherical structure, the composite may have a rigid structure.

[0099] The first carbon-based material included in the composite has, for example, a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the spiral structure. The size of the spiral structure of the first carbon-based material may be 500 nm to 100 um. Since the first carbon-based material has a spiral structure, the composite may have a rigid structure.

[0100] The first carbon-based material included in the composite may be, for example, graphene. The graphene may have, for example, a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the spiral structure. The size of the spiral structure of the graphene may be from 500 nm to 100 um. Since the graphene has a spiral structure, the composite may have a rigid structure.

[0101] The first carbon-based material included in the composite has, for example, a cluster structure in which a plurality of spherical structures are aggregated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the cluster structure. The size of the cluster structure of the first carbon-based material may be from 0.5 mm to 10 cm. Since the first carbon-based material has a cluster structure, the composite may have a rigid structure.

[0102] The first carbon-based material included in the composite may be, for example, graphene. The graphene may have, for example, a cluster structure in which a plurality of spherical structures are aggregated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the cluster structure. The size of the graphene cluster structure may be from 0.5 mm to 10 cm. Since the graphene has a cluster structure, the composite may have a rigid structure.

[0103] The composite may be, for example, a faceted-ball structure, and at least one selected from a first metal oxide and a second metal oxide may be distributed within or on the surface of the structure. Since the composite is a faceted-ball structure, the composite can be easily coated on the irregular surface unevenness of the core.

[0104] The composite may be, for example, a planar structure, and at least one selected from a first metal oxide and a second metal oxide may be distributed within or on the surface of the structure. Since the composite is such a two-dimensional planar structure, the composite can be easily coated on the irregular surface unevenness of the core.

[0105] The first carbon-based material included in the composite extends from the first metal oxide by a distance of 10 nm or less and may include at least 1 to 20 layers of the first carbon-based material. For example, a first carbon-based material having a total thickness of 12 nm or less may be disposed on the first metal oxide by stacking a plurality of layers of the first carbon-based material. For example, the total thickness of the first carbon-based material may be 0.6 to 12 nm.

[0106] The first carbon-based material included in the composite may be, for example, graphene. The graphene may extend from the first metal oxide by a distance of 10 nm or less and may include at least 1 to 20 graphene layers. For example, by stacking multiple graphene layers, graphene having a total thickness of 12 nm or less may be disposed on the first metal oxide. For example, the total thickness of the graphene may be 0.6 to 12 nm.

[0107] According to another embodiment, a positive electrode comprises the composite positive electrode active material described above. By comprising the composite positive electrode active material described above, the positive electrode provides improved cycle characteristics and reduced internal resistance.

[0108] The anode is manufactured by, for example, the following exemplary method, but is not limited to this method and is adjusted according to the required conditions.

[0109] First, a positive electrode active material composition is prepared by mixing the above-described composite positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.

[0110] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used.

[0111] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.

[0112] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.

[0113] The content of the composite cathode active material, conductive agent, binder, and solvent used in the positive electrode is at the level typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, binder, and solvent may be omitted.

[0114] The binder content included in the positive electrode may be 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the positive electrode active material layer. The composite positive electrode active material content included in the positive electrode may be 90 to 99 wt% or 95 to 99 wt% of the total weight of the positive electrode active material layer.

[0115] , the positive electrode according to the embodiment further includes a third carbon-based material, and the third carbon-based material

[0116] The material may include carbon nanofibers, carbon nanotubes, or a combination thereof.

[0117] The positive electrode may further include a solid electrolyte. The solid electrolyte may be an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer-based solid electrolyte, or a combination thereof. The content of the solid electrolyte is 80 to 120 parts by weight based on 100 parts by weight of the composite positive electrode active material.

[0118] In addition, the positive electrode may additionally include other general positive electrode active materials in addition to the composite positive electrode active materials described above.

[0119] The general cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c(In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G dO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:

[0120] In the chemical formula representing the compound described above, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.

[0121] It is also possible to use a compound having a coating layer added to the surface of the above-mentioned compound, or it is also possible to use a mixture of the above-mentioned compound and a compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes, for example, a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since specific coating methods are well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0122] A lithium battery according to another embodiment employs a positive electrode including the composite positive electrode active material described above.

[0123] An all-solid-state secondary battery with improved life characteristics and capacity characteristics is provided by employing a positive electrode including the composite positive electrode active material described above.

[0124] Below, all-solid-state secondary batteries according to embodiments are described in more detail.

[0125] [All-solid-state secondary battery]

[0126] An all-solid-state secondary battery according to one embodiment includes a cathode layer; a cathode layer; and a solid electrolyte layer disposed between the cathode layer and the cathode layer, wherein the cathode layer includes a cathode current collector and a cathode active material layer disposed on one or both surfaces of the cathode current collector, wherein the cathode active material layer includes a lithium sulfide-based cathode active material, and the lithium-containing sulfide-based cathode active material is Li2S. n (n≥1), Li2S n (n≥1) containing complexes or combinations thereof. Li2S n (n≥1) contains, for example, Li2S. The negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on one surface of the negative electrode current collector, and a ratio (B / A) of an initial charge capacity (B) of the first negative electrode active material layer and an initial charge capacity (A) of the positive electrode active material layer is 0.005 to 0.45, and the initial charge capacity of the positive electrode active material layer is a first open circuit voltage (1 st Li / Li from open circuit voltage) + The initial charge capacity of the negative electrode active material layer is determined at the maximum charging voltage, and the initial charge capacity of the negative electrode active material layer is determined at the second open circuit voltage (2 nd Li / Li from open circuit voltage) + It is determined at 0.01 V.

[0127] All-solid-state secondary batteries incorporate a lithium-containing sulfide-based cathode active material instead of lithium metal as a lithium source. This allows for the omission of a lithium source, such as lithium metal, from the cathode layer. This reduction in cathode layer volume improves the energy density of the all-solid-state secondary battery.

[0128] An all-solid-state secondary battery includes a lithium-containing sulfide-based cathode active material as a cathode active material. Therefore, the interruption of ion and / or electron transfer pathways due to volume increase during initial discharge of a lithium-free sulfide-based cathode active material, such as sulfur (S), is prevented. By preventing such interruption of ion and / or electron transfer pathways, the cycle characteristics of the all-solid-state secondary battery are improved. In contrast, an all-solid-state secondary battery according to one embodiment does not cause the problem of lithium polysulfide dissolving in the electrolyte and does not contain a flammable organic solvent, thereby ensuring safety.

[0129] An all-solid-state secondary battery includes a first negative electrode active material layer having an initial charge capacity in the range of 0.005 to 0.45 compared to the initial charge capacity of the positive electrode active material layer. Since the first negative electrode active material layer has a small initial charge capacity in this range, the negative electrode layer can effectively compensate for the volume change of the positive electrode layer during charge and discharge. Consequently, the overall volume change of the all-solid-state secondary battery is suppressed during charge and discharge. Since deterioration, such as crack formation due to rapid volume change during charge and discharge of the all-solid-state secondary battery, is prevented, short-circuiting of the all-solid-state secondary battery is prevented and cycle characteristics are improved.

[0130] Since the all-solid-state secondary battery includes a solid electrolyte layer, the migration of polysulfides generated during charging and discharging of the lithium-containing sulfide-based positive electrode active material to the negative electrode layer is blocked. Consequently, side reactions between polysulfides and the negative electrode active material are suppressed.

[0131] By arranging an inert member on one side of the cathode layer, cracking of the solid electrolyte layer that occurs during pressurization and / or charging / discharging of the all-solid-state secondary battery is suppressed. Accordingly, cracking of the solid electrolyte layer is suppressed during the manufacturing and / or charging / discharging of the all-solid-state secondary battery, thereby suppressing short circuits in the all-solid-state secondary battery. Consequently, short circuits of the all-solid-state secondary battery are prevented and the life characteristics are improved.

[0132] Referring to FIGS. 2 and 3, an all-solid-state secondary battery (1) includes a positive electrode layer (10); a negative electrode layer (20); and a solid electrolyte layer (30) disposed between the positive electrode layer (10) and the negative electrode layer (20), wherein the positive electrode layer (10) includes a positive electrode current collector (11) and a positive electrode active material layer (12) disposed on one or both surfaces of the positive electrode current collector, and the positive electrode active material layer (12) includes a composite positive electrode active material according to one embodiment.

[0133] According to an embodiment, a composite cathode active material includes a sulfide-based cathode active material including Li2S, a Li2S-containing composite, or a combination thereof.

[0134] [Anode layer]

[0135] [Anode layer: cathode active material]

[0136] Referring to FIGS. 2 and 3, the positive electrode active material layer (12) includes, for example, a positive electrode active material and a solid electrolyte. The solid electrolyte included in the positive electrode active material layer (12) is similar to or different from the solid electrolyte included in the solid electrolyte layer (30). For more information on the solid electrolyte, refer to the section on the solid electrolyte layer (30).

[0137] The cathode active material includes a lithium-containing sulfide-based cathode active material. A lithium-containing sulfide-based cathode active material is, for example, an electrode material in which lithium is added to a sulfur-based cathode active material. A sulfur-based cathode active material includes, for example, a sulfur-based material, a composite containing a sulfur-based material, or a combination thereof. The sulfur-based material includes, for example, inorganic sulfur, Li2S. n (n≥1), a disulfide compound, an organic sulfur compound, a carbon-sulfur polymer, or a combination thereof. The sulfur-containing composite may be an inorganic sulfur, Li2S n(n≥1), a disulfide compound, an organic sulfur compound, a carbon-sulfur polymer, or a combination thereof. The sulfur-containing composite may include, for example, a composite of a sulfur-containing material and carbon, a composite of a sulfur-containing material and carbon and a solid electrolyte, a composite of a sulfur-containing material and a solid electrolyte, a composite of a sulfur-containing material and a metal carbide, a composite of a sulfur-containing material and carbon and a metal carbide, a composite of a sulfur-containing material and a metal nitride, a composite of a sulfur-containing material and carbon and a metal nitride, or a combination thereof. Since a lithium-containing sulfide-based cathode active material provides a higher discharge capacity per unit weight than an oxide-based cathode active material, the energy density per unit weight of an all-solid-state secondary battery including a lithium-containing sulfide-based cathode active material can be improved.

[0138] The lithium-containing sulfide-based cathode active material includes, for example, Li2S, a Li2S-containing composite, or a combination thereof. By including Li2S, a Li2S-containing composite, or a combination thereof as the lithium-containing sulfide-based cathode active material having a high capacity, the use of lithium metal can be omitted when manufacturing an all-solid-state secondary battery. Lithium metal has high reactivity and great ductility, which can reduce mass productivity during battery manufacturing. Therefore, the mass productivity of the all-solid-state secondary battery can be improved. Since lithium metal is omitted from the negative electrode layer, the volume of the negative electrode layer is reduced, thereby improving the energy density per unit volume of the all-solid-state secondary battery and allowing for a simpler structure of the all-solid-state secondary battery.

[0139] Lithium-containing sulfide-based cathode active materials (e.g., Li2S) undergo delithiation during initial charging, for example, which reduces in volume, and then increases again due to lithiation during subsequent discharge. Therefore, since the volume of the lithium-containing sulfide-based cathode active material changes while maintaining the ion and / or electron transfer pathways established by conductive materials, etc., around the lithium-containing sulfide-based cathode active material, the ion and / or electron transfer pathways are less likely to be interrupted. In contrast, sulfur-based cathode active materials (e.g., S) undergo lithiation during initial discharge, for example, which increases in volume, and then decreases again due to delithiation during subsequent charge. Therefore, since the initial ion and / or electron transfer pathways established by conductive materials, etc., around the sulfur-based cathode active material may be disrupted by the initial volume increase of the sulfur-based cathode active material, the ion and / or electron transfer pathways are more likely to be interrupted.

[0140] The average particle diameter (D50) of the lithium-containing sulfide-based cathode active material may be, for example, 0.1 nm to 10 um, 1 nm to 50 um, 10 nm to 50 um, or 10 nm to 1 um. When the lithium-containing sulfide-based cathode active material has an average particle diameter in this range, the cycle characteristics of an all-solid-state secondary battery including the lithium sulfide-based cathode active material can be further improved. The Li2S-containing composite is, for example, a composite of Li2S and a conductive material. The conductive material is, for example, an ion-conducting material, an electron-conducting material, or a combination thereof.

[0141] When the composite cathode active material includes a solid electrolyte (e.g., a sulfide-based solid electrolyte), the average particle size of the solid electrolyte is 0.1 nm to 10 um, 1 nm to 8 um, 10 nm to 5 um, or 100 nm to 3 um.

[0142] The average particle diameter of a composite including a lithium-containing sulfide-based positive electrode active material and a first carbon-based material according to an embodiment of the present invention, or including a lithium-containing sulfide-based positive electrode active material, a first carbon-based material, and a solid electrolyte, is 0.1 to 50 um or 1 to 10 um.

[0143] The electronic conductivity of an electronically conductive material is, for example, 1.0×10 3 S / m, 1.0×10 4 S / m, or 1.0×10 5 S / m or more. The form of the electron-conducting material may be, for example, a particle-like electron-conducting material, a plate-like electron-conducting material, a rod-like electron-conducting material, or a combination thereof, but is not necessarily limited thereto. The electron-conducting material may be, for example, carbon, metal powder, a metal compound, etc. When carbon is included as the electron-conducting material, since carbon has high electron conductivity and is light, an all-solid-state secondary battery having a high energy density per unit mass can be implemented. The electron-conducting material may have pores. Since the electron-conducting material has pores, Li2S can be included in the pores, thereby increasing the contact area between Li2S and the electron-conducting material and increasing the specific surface area of ​​Li2S. The pore capacity is, for example, 0.1 cc / g to 20.0 cc / g, 0.5 cc / g to 10 cc / g, or 0.5 cc / g to 5 cc / g. The average pore diameter is, for example, 1 nm to 100 nm, 1 nm to 50 nm, or 1 nm to 20 nm. The BET specific surface area of ​​an electron-conducting material having pores is 200 m when the average pore diameter is 15 nm or less. 2 / g to 4500 m 2 / g, and if the average pore diameter exceeds 15 nm, 100 m 2 / g to 2500 m 2 / g. The BET surface area, pore diameter, pore volume and average pore diameter can be obtained, for example, using the nitrogen adsorption method.

[0144] The ionic conductivity of an ionic conductive material is, for example, 1.0×10 -5 S / m or more, 1.0×10 -4 S / m or more, or 1.0×10 -3 S / m or more. The ion-conducting material may have pores. By having pores, Li2S can be included in the pores, thereby increasing the contact area between Li2S and the ion-conducting material and increasing the specific surface area of ​​Li2S. The form of the ion-conducting material may be, for example, a particle-shaped ion-conducting material, a plate-shaped electron-conducting material, a rod-shaped electron-conducting material, or a combination thereof, but is not necessarily limited thereto. The ion-conducting material may be, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, etc. When a sulfide-based solid electrolyte is included as the ion-conducting material, the sulfide-based solid electrolyte has high ion conductivity and can be formed into various shapes, so that an all-solid-state secondary battery having a large capacity can be implemented.

[0145] The Li2S-containing complex includes, for example, a complex of Li2S and carbon, a complex of Li2S and carbon and a solid electrolyte, a complex of Li2S and a solid electrolyte, a complex of Li2S and a metal carbide, a complex of Li2S and carbon and a metal carbide, a complex of Li2S and a metal nitride, a complex of Li2S and carbon and a metal nitride, or a combination thereof.

[0146] The Li2S and carbon composite comprises carbon. The carbon may be any material containing carbon atoms used as a conductive material in the art. The carbon may be, for example, crystalline carbon, amorphous carbon, or a combination thereof. The carbon may be, for example, a sintered product of a carbon precursor. The carbon may be, for example, a carbon nanostructure. The carbon nanostructure may be, for example, a one-dimensional carbon nanostructure, a two-dimensional carbon nanostructure, a three-dimensional carbon nanostructure, or a combination thereof. The carbon nanostructure may be, for example, a carbon nanotube, a carbon nanofiber, a carbon nanobelt, a carbon nanorod, graphene, or a combination thereof. The carbon may be, for example, porous carbon or non-porous carbon. The porous carbon may include, for example, periodic and regular two-dimensional or three-dimensional pores. The porous carbon may be, for example, carbon black such as Ketjen Black, acetylene black, Denka Black, thermal black, channel black, or the like; graphite, activated carbon, or a combination thereof. The form of carbon may be, for example, particle form, sheet form, flake form, etc., but is not limited thereto, and any method used as carbon in the relevant technical field may be used. The method for producing a composite of Li2S and carbon may be, but is not limited to, a dry method, a wet method, or a combination thereof, and the method for producing a composite of Li2S and carbon in the relevant technical field may be, for example, milling, heat treatment, deposition, etc., but is not necessarily limited thereto, and any method used in the relevant technical field may be used.

[0147] The composite of Li2S, carbon, and a solid electrolyte comprises carbon and a solid electrolyte. Carbon refers to the composite of Li2S and carbon described above. The solid electrolyte can be any material used as an ion-conducting material in the relevant technical field, for example. The solid electrolyte is, for example, an inorganic solid electrolyte. The solid electrolyte is, for example, a crystalline solid electrolyte, an amorphous solid electrolyte, or a combination thereof. The solid electrolyte is, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a combination thereof. The sulfide-based solid electrolyte comprises, for example, Li, S, and P, and may optionally further comprise a halogen element. The sulfide-based solid electrolyte can be selected from among the sulfide-based solid electrolytes used in the solid electrolyte layer. The sulfide-based solid electrolyte has, for example, a density of 1×10 -5 It can have an ionic conductivity of S / cm or more. The oxide-based solid electrolyte contains, for example, Li, O, and transition metal elements, and may optionally contain other elements. The oxide-based solid electrolyte has, for example, an ionic conductivity of 1×10 at room temperature. -5 It may be a solid electrolyte having an ionic conductivity of S / cm or more. The oxide-based solid electrolyte may be selected from among oxide-based solid electrolytes used in the solid electrolyte layer.

[0148] The composite of Li2S and a solid electrolyte includes a solid electrolyte. The solid electrolyte refers to the composite of Li2S, carbon, and a solid electrolyte described above.

[0149] The composite of Li2S and metal carbide includes metal carbide. The metal carbide is, for example, a two-dimensional metal carbide. The two-dimensional metal carbide is, for example, M n+1 C n T x (M is a transition metal, T is a terminal group, T is O, OH and / or F, n=1, 2, or 3, and x is the number of terminal groups) is expressed as 2D metal carbides, for example, Ti2CT x , (Ti 0.5 , Nb 0.5)2CT x , Nb2CT x , V2CT x , Ti3C2T x , (V 0.5 , Cr 0.5 )3C2T x , Ti3CNT x , Ta4C3T x , Nb4C3T x or a combination thereof. The surface of the two-dimensional metal carbide is terminated with O, OH and / or F.

[0150] The complex of Li2S, carbon, and metal carbide includes carbon and metal carbide. Carbon refers to the complex of Li2S and carbon described above. Metal carbide refers to the complex of Li2S and metal carbide described above.

[0151] The complex of Li2S and metal nitride includes a metal nitride. The metal nitride is, for example, a two-dimensional metal nitride. The two-dimensional metal nitride is, for example, M n+1 N n T x (M is a transition metal, T is a terminal group, T is O, OH and / or F, n=1, 2, or 3, and x is the number of terminal groups) is expressed as The surface of the two-dimensional metal nitride is terminated with O, OH and / or F.

[0152] A complex of Li2S, carbon, and a metal nitride includes carbon and a metal nitride. Carbon refers to the complex of Li2S and carbon described above. Metal carbide refers to the complex of Li2S and a metal nitride described above.

[0153] The content of the sulfide-based positive electrode active material included in the positive electrode active material layer (12) may be, for example, 10 wt% to 90 wt%, 10 wt% to 80 wt%, 10 wt% to 70 wt%, 10 wt% to 60 wt%, or 10 wt% to 50 wt% of the total weight of the positive electrode active material layer (12).

[0154] The cathode active material layer (12) may additionally include, for example, a sulfide-based compound that is distinct from Li2S. The sulfide-based compound may be, for example, a compound containing a metal element other than Li and the element sulfur. The sulfide-based compound may be, for example, a compound containing a metal element belonging to Groups 1 to 14 of the Periodic Table of Elements having an atomic weight of 10 or more and the element sulfur. The sulfide-based compound may be, for example, FeS2, VS2, NaS, MnS, FeS, NiS, CuS, or a combination thereof. By additionally including a sulfide-based compound in the cathode active material layer, the cycle characteristics of the all-solid-state secondary battery may be further improved. The content of the sulfide-based compound that is distinct from Li2S included in the cathode active material layer (12) may be 10 wt% or less, 5 wt% or less, 3 wt% or less, or 1 wt% or less of the total weight of the cathode active material layer (12).

[0155] [Anode layer: solid electrolyte]

[0156] The cathode active material layer (12) may further include, for example, a solid electrolyte. The solid electrolyte may be, for example, a sulfide-based solid electrolyte. The solid electrolyte included in the cathode layer (10) may be the same as or different from the solid electrolyte included in the solid electrolyte layer (30). For details on the solid electrolyte, refer to the section on the solid electrolyte layer (30).

[0157] The solid electrolyte included in the positive electrode active material layer (12) may have a smaller average D50 particle diameter than the solid electrolyte included in the solid electrolyte layer (30). For example, the average D50 particle diameter of the solid electrolyte included in the positive electrode active material layer (12) may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the average D50 particle diameter of the solid electrolyte included in the solid electrolyte layer (30). The average D50 particle diameter is, for example, a median particle diameter (D50). The median particle diameter (D50) is, for example, the size of particles corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by laser diffraction.

[0158] The solid electrolyte content included in the positive electrode active material layer (12) may be, for example, 1 wt% to 40 wt%, 1 wt% to 30 wt%, 1 wt% to 20 wt%, or 1 wt% to 10 wt% of the total weight of the positive electrode active material layer (12).

[0159] [Anode layer: conductive material]

[0160] The cathode active material layer (12) may further include a conductive material. The conductive material may be, for example, a carbon-based conductive material, a metal-based conductive material, or a combination thereof. The carbon-based conductive material may be, for example, graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or a combination thereof, but is not limited thereto, and any material used as a carbon-based conductive material in the art may be used. The metal-based conductive material may be, for example, metal powder, metal fiber, or a combination thereof, but is not limited thereto, and any material used as a metal-based conductive material in the art may be used. The content of the conductive material included in the cathode active material layer (12) may be, for example, 1 wt% to 30 wt%, 1 wt% to 20 wt%, or 1 wt% to 10 wt% of the total weight of the cathode active material layer (12).

[0161] [Anode layer: binder]

[0162] The positive electrode active material layer (12) may further include a binder. The binder may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used in the relevant technical field may be used. The binder content included in the positive electrode active material layer (12) may be, for example, 1 wt% to 10 wt% of the total weight of the positive electrode active material layer (12). The binder may be omitted.

[0163] [Anode layer: Other additives]

[0164] The cathode active material layer (12) may further include additives such as fillers, coating agents, dispersants, and ion conductive aids in addition to the cathode active material, solid electrolyte, binder, and conductive agent described above.

[0165] As fillers, coating agents, dispersants, ion conductivity aids, etc. that can be included in the positive electrode active material layer (12), known materials generally used in electrodes of all-solid-state secondary batteries can be used.

[0166] [Anode layer: Anode current collector]

[0167] The positive electrode collector (11) uses a plate or foil made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode collector (11) may be omitted. The thickness of the positive electrode collector (11) is, for example, 1 µm to 100 µm, 1 µm to 50 µm, 5 µm to 25 µm, or 10 µm to 20 µm.

[0168] In one embodiment of the present invention, the positive electrode current collector (11) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The positive electrode current collector (11) may additionally include a metal piece and / or a lead tab. For more specific details regarding the base film, metal layer, metal piece, and lead tab of the positive electrode current collector (11), refer to the negative electrode current collector (21) described below. By having such a structure, the positive electrode current collector (11) can reduce the weight of the electrode and consequently improve the energy density.

[0169] [Cathode layer]

[0170] [Cathode layer: Cathode active material]

[0171] Referring to FIGS. 2 and 3, the negative electrode layer (20) includes a first negative electrode active material layer (22). The first negative electrode active material layer (22) includes, for example, a negative electrode active material and a binder.

[0172] The negative electrode active material included in the first negative electrode active material layer (22) is, for example, a negative electrode material that can form an alloy or compound with lithium.

[0173] The negative electrode active material included in the first negative electrode active material layer (22) has, for example, a particle form. The average particle diameter of the negative electrode active material having a particle form is, for example, 4 ㎛ or less, 3 ㎛ or less, 2 ㎛ or less, 1 ㎛ or less, 500 nm or less, 300 nm or less, or 100 nm or less. The average particle diameter of the negative electrode active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 3 ㎛, 10 nm to 2 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 300 nm, or 10 nm to 100 nm. When the negative electrode active material has an average particle diameter in this range, reversible absorption and / or desorption of lithium can be facilitated during charge and discharge. The average particle size of the negative electrode active material is, for example, the median diameter (D50) measured using a laser particle size distribution meter.

[0174] The negative electrode active material included in the first negative electrode active material layer (22) includes, for example, at least one selected from among a carbon-based negative electrode active material and a metal or metalloid negative electrode active material.

[0175] Carbon-based negative electrode materials include, for example, amorphous carbon, crystalline carbon, porous carbon, or a combination thereof.

[0176] The carbon-based negative electrode material is, in particular, amorphous carbon. Amorphous carbon includes, but is not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), and graphene, and any material classified as amorphous carbon in the relevant technical field is acceptable. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon.

[0177] The carbon-based negative electrode active material may be, for example, porous carbon. The porous carbon has a pore volume of, for example, 0.1 cc / g to 10.0 cc / g, 0.5 cc / g to 5 cc / g, or 0.1 cc / g to 1 cc / g. The porous carbon has an average pore diameter of, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. The porous carbon has a BET surface area of, for example, 100 m 2 / g to 3000 m 2 / g is.

[0178] The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), indium (In), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium and therefore is not a metal negative electrode active material.

[0179] The first negative electrode active material layer (22) includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the first negative electrode active material layer (22) includes only amorphous carbon, or includes at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the first negative electrode active material layer (22) includes a mixture of amorphous carbon and at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture of amorphous carbon and gold, etc., is a weight ratio, for example, 99:1 to 1:99, 10:1 to 1:2, 5:1 to 1:1, or 4:1 to 2:1, but is not necessarily limited to this range and is selected according to the required characteristics of the all-solid-state secondary battery (1). When the negative electrode active material has this composition, the cycle characteristics of the all-solid-state secondary battery (1) are further improved.

[0180] The negative electrode active material included in the first negative electrode active material layer (22) includes, for example, a mixture of first particles made of amorphous carbon and second particles made of a metal or a metalloid. The metal or metalloid includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the metalloid is a semiconductor. The content of the second particles is 1 to 99 wt%, 1 to 60 wt%, 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, an all-solid-state secondary battery (1) are further improved.

[0181] [Cathode layer: binder]

[0182] The binder included in the first negative electrode active material layer (22) is, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders.

[0183] Since the first negative electrode active material layer (22) includes a binder, the first negative electrode active material layer (22) is stabilized on the negative electrode current collector (21). In addition, cracking of the first negative electrode active material layer (22) is suppressed despite changes in the volume and / or relative position of the first negative electrode active material layer (22) during the charge and discharge process. For example, if the first negative electrode active material layer (22) does not include a binder, the first negative electrode active material layer (22) can be easily separated from the negative electrode current collector (21). As the first negative electrode active material layer (22) is detached from the negative electrode current collector (21), the possibility of a short circuit occurring increases at the exposed portion of the negative electrode current collector (21) due to the negative electrode current collector (21) coming into contact with the solid electrolyte layer (30). The first negative electrode active material layer (22) is manufactured by, for example, applying a slurry in which the material constituting the first negative electrode active material layer (22) is dispersed onto the negative electrode current collector (21) and drying the slurry. By including a binder in the first negative electrode active material layer (22), stable dispersion of the negative electrode active material in the slurry is possible. For example, when applying the slurry onto the negative electrode current collector (21) by screen printing, it is possible to suppress clogging of the screen (for example, clogging by aggregates of the negative electrode active material).

[0184] [Cathode layer: Other additives]

[0185] The first negative electrode active material layer (22) may further include additives used in a conventional all-solid-state secondary battery (1), such as fillers, coating agents, dispersants, and ion conductive aids.

[0186] [Cathode layer: solid electrolyte]

[0187] The first negative electrode active material layer (22) may further include a solid electrolyte. The solid electrolyte may be, for example, a material selected from among the solid electrolytes included in the solid electrolyte layer (30). The solid electrolyte included in the first negative electrode active material layer (22) may act as a reaction site where lithium metal formation begins within the first negative electrode active material layer (22), as a space where the formed lithium metal is stored, or as a path for transferring lithium ions. The solid electrolyte may be omitted.

[0188] In the first negative electrode active material layer (22), the content of the solid electrolyte may be high, for example, in an area adjacent to the solid electrolyte layer (30), and low, for example, in an area adjacent to the negative electrode current collector (21). In the first negative electrode active material layer (22), the solid electrolyte may have a concentration gradient in which the concentration decreases, for example, from an area adjacent to the solid electrolyte layer (30) to an area adjacent to the negative electrode current collector (21).

[0189] [Cathode layer: first cathode active material layer]

[0190] The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer (22) and the initial charge capacity (A) of the positive electrode active material layer is 0.005 to 0.45. The initial charge capacity of the positive electrode active material layer (12) is the first open circuit voltage (1 st Li / Li from open circuit voltage) + The initial charge capacity of the first negative electrode active material layer (22) is determined at the maximum charging voltage. The initial charge capacity of the first negative electrode active material layer (22) is determined at the second open circuit voltage (2 nd Li / Li from open circuit voltage) + It is determined at 0.01 V.

[0191] The maximum charging voltage is determined by the type of cathode active material. The maximum charging voltage can be, for example, 1.5 V, 2.0 V, 2.5 V, 3.0 V, 3.5 V, 4.0 V, 4.2 V, or 4.3 V. For example, the maximum charging voltage of Li2S or Li2S composite is Li / Li + can be 2.5 V for Li2S or Li2S complex. For example, the maximum charging voltage of Li / Li + It can be 3.0 V for. The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer (22) and the initial charge capacity (A) of the positive electrode active material layer is, for example, 0.01 to 0.3, 0.01 to 0.2, or 0.05 to 0.1.

[0192] The initial charge capacity (mAh) of the positive electrode active material layer (12) is obtained by multiplying the charge capacity density (charge specific capacity) (mAh / g) of the positive electrode active material by the mass (g) of the positive electrode active material in the positive electrode active material layer (12). When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values ​​is the initial charge capacity of the positive electrode active material layer (12). The initial charge capacity of the first negative electrode active material layer (22) is also calculated in the same way. The initial charge capacity of the first negative electrode active material layer (22) is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the first negative electrode active material layer (22). When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values ​​is the initial charge capacity of the first negative electrode active material layer (22). The charge capacity density of each of the positive electrode active material and the negative electrode active material can be measured using an all-solid-state half-cell using lithium metal as a counter electrode. The initial charge capacity of each of the positive electrode active material layer (12) and the first negative electrode active material layer (22) is measured at a constant current density, for example, 0.1 mA / cm 2can be directly measured using an all-solid-state half-cell. For the positive electrode, the measurement is made from the first open circuit voltage (OCV) to the maximum charge voltage, for example, 3.0 V (vs. Li / Li + ) can be performed for an operating voltage of up to 0.01 V for the cathode, for example, lithium metal, from the second open circuit voltage (OCV). For example, an all-solid-state half-cell having a cathode active material layer can measure a current of 0.1 mA / cm from the first open circuit voltage to 3.0 V. 2 The all-solid-state half-cell having the first negative active material layer is charged with a constant current of 0.1 mA / cm from the second open circuit voltage to 0.01 V. 2 It can be charged with a constant current. The current density during constant current charging is, for example, 0.2 mA / cm 2 , or 0.5 mA / cm 2 The all-solid-state half-cell having the positive electrode active material layer can be charged from the first open circuit voltage to, for example, 2.5 V, 2.0 V, 3.5 V, or 4.0 V. The maximum charge voltage of the positive electrode active material layer can be determined by the maximum voltage of the battery that satisfies the safety conditions according to JISC8712:2015 of the Japanese Standards Association.

[0193] If the initial charge capacity of the first negative electrode active material layer (22) is too small, the thickness of the first negative electrode active material layer (22) becomes very thin, so that lithium dendrites formed between the first negative electrode active material layer (22) and the negative electrode current collector (21) during repeated charge and discharge processes collapse the first negative electrode active material layer (22), making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the charge capacity of the first negative electrode active material layer (22) increases excessively, the energy density of the all-solid-state secondary battery (1) decreases and the internal resistance of the all-solid-state secondary battery (1) due to the first negative electrode active material layer (22) increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1).

[0194] The thickness of the first negative electrode active material layer (22) is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer (12). The thickness of the first negative electrode active material layer (22) is, for example, 1 to 50%, 1 to 40%, 1 to 30%, 1 to 20%, 1 to 10%, or 1 to 5% of the thickness of the positive electrode active material layer (12). The thickness of the first negative electrode active material layer (22) is, for example, 1 µm to 20 µm, 2 µm to 15 µm, or 3 µm to 10 µm. If the thickness of the first negative electrode active material layer (22) is too thin, lithium dendrites formed between the first negative electrode active material layer (22) and the negative electrode current collector (21) collapse the first negative electrode active material layer (22), making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the thickness of the first negative electrode active material layer (22) increases excessively, the energy density of the all-solid-state secondary battery (1) decreases and the internal resistance of the all-solid-state secondary battery (1) due to the first negative electrode active material layer (22) increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the thickness of the first negative electrode active material layer (22) decreases, for example, the initial charge capacity of the first negative electrode active material layer (22) also decreases.

[0195] [Cathode layer: second cathode active material layer]

[0196] Although not shown in the drawing, the all-solid-state secondary battery (1) further includes, after being charged, a second negative electrode active material layer disposed, for example, between the negative electrode current collector (21) and the first negative electrode active material layer (22). The second negative electrode active material layer is a metal layer containing lithium or a lithium alloy. The metal layer contains lithium or a lithium alloy. Therefore, since the second negative electrode active material layer is a metal layer containing lithium, it functions as, for example, a lithium reservoir. The lithium alloy is, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., but is not limited thereto, and any lithium alloy used in the art may be used. The second negative electrode active material layer may be made of one of these alloys or lithium, or may be made of several types of alloys. The second negative electrode active material layer is, for example, a plated layer. The second negative electrode active material layer is deposited between the first negative electrode active material layer (22) and the negative electrode current collector (21), for example, during the charging process of an all-solid-state secondary battery (1).

[0197] The thickness of the second negative electrode active material layer is not particularly limited, but is, for example, 1 ㎛ to 500 ㎛, 1 ㎛ to 200 ㎛, 1 ㎛ to 150 ㎛, 1 ㎛ to 100 ㎛, or 1 ㎛ to 50 ㎛. If the thickness of the second negative electrode active material layer is too thin, it is difficult for the second negative electrode active material layer to perform the role of a lithium reservoir. If the thickness of the second negative electrode active material layer is too thick, the mass and volume of the all-solid-state secondary battery (1) may increase, and the cycle characteristics of the all-solid-state secondary battery (1) may rather deteriorate.

[0198] Alternatively, in the all-solid-state secondary battery (1), the second negative electrode active material layer may be disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22), for example, before assembling the all-solid-state secondary battery (1). As shown in Fig. 3, when the second negative electrode active material layer (23) is disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22) before assembling the all-solid-state secondary battery (1), the second negative electrode active material layer acts as a lithium reservoir because it is a metal layer containing lithium. For example, a lithium foil may be disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22) before assembling the all-solid-state secondary battery (1).

[0199] When the second negative electrode active material layer is precipitated by charging after assembling the all-solid-state secondary battery (1), the energy density of the all-solid-state secondary battery (1) increases because the second negative electrode active material layer is not included when assembling the all-solid-state secondary battery (1). When charging the all-solid-state secondary battery (1), the charging is performed in excess of the charging capacity of the first negative electrode active material layer (22). That is, the first negative electrode active material layer (22) is overcharged. At the beginning of charging, lithium is absorbed into the first negative electrode active material layer (22). The negative electrode active material included in the first negative electrode active material layer (22) forms an alloy or compound with the lithium ions that have moved from the positive electrode layer (10). When charging exceeds the capacity of the first negative electrode active material layer (22), for example, lithium is deposited on the back surface of the first negative electrode active material layer (22), that is, between the negative electrode current collector (21) and the first negative electrode active material layer (22), and a metal layer corresponding to the second negative electrode active material layer is formed by the deposited lithium. The second negative electrode active material layer is a metal layer mainly composed of lithium (i.e., metallic lithium). This result is obtained, for example, by the negative electrode active material included in the first negative electrode active material layer (22) including a material that forms an alloy or compound with lithium. During discharge, lithium in the first negative electrode active material layer (22) and the second negative electrode active material layer, that is, the metal layer, is ionized and moves toward the positive electrode layer (10). Therefore, it is possible to use lithium as the negative electrode active material in an all-solid-state secondary battery (1). In addition, since the first negative electrode active material layer (22) covers the second negative electrode active material layer, it functions as a protective layer for the second negative electrode active material layer, i.e., the metal layer, and at the same time, it suppresses the precipitation and growth of lithium dendrites. Accordingly, it suppresses short circuits and capacity reduction of the all-solid-state secondary battery (1), and consequently improves the cycle characteristics of the all-solid-state secondary battery (1).In addition, when the second negative electrode active material layer is disposed by charging after assembling the all-solid-state secondary battery (1), the negative electrode layer (20), i.e., the negative electrode current collector (21) and the first negative electrode active material layer (22) and the region between them are Li-free regions that do not contain lithium (Li) in the initial state or the state after complete discharge of the all-solid-state secondary battery (1).

[0200] [Cathode layer: negative electrode collector]

[0201] The negative electrode current collector (21) is composed of, for example, a material that does not react with lithium, i.e., does not form an alloy or a compound. The material constituting the negative electrode current collector (21) is, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), but is not necessarily limited thereto, and any material that can be used as an electrode current collector in the relevant technical field can be used. The negative electrode current collector (21) may be composed of one type of the above-described metal, or may be composed of an alloy or a coating material of two or more types of metals. The negative electrode current collector (21) is, for example, in the form of a plate or foil.

[0202] In one embodiment of the present invention, the negative electrode current collector (21) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse and cut off in the event of an overcurrent, thereby performing a short circuit prevention function. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer may be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the negative electrode current collector (521b, 522b) decrease, thereby improving the stability of the lithium battery in the event of a short circuit. A lead tab may be added on the metal layer for external connection. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the base film and / or the metal layer may be melted, electrically connecting the metal layer to the lead tab. In order to strengthen the welding of the metal layer and the lead tab, a metal piece may be added between the metal layer and the lead tab. The metal piece may be a thin piece of the same material as the metal of the metal layer.The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, an aluminum foil, a copper foil, a SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate by welding the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the welding process of the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to μm. Since the metal layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the electrode assembly. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the negative electrode current collector (521b, 522b) can reduce the weight of the electrode and consequently improve the energy density.The all-solid-state secondary battery (1) may further include, for example, a thin film containing an element capable of forming an alloy with lithium on one surface of the negative electrode current collector (21), although not shown in the drawing. The thin film is disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22). The thin film contains, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By placing the thin film on one surface of the negative electrode current collector (21), for example, the deposition shape of the second negative electrode active material layer deposited between the thin film (24) and the first negative electrode active material layer (22) becomes flatter, and the cycle characteristics of the all-solid-state secondary battery (1) can be further improved.

[0203] The thickness of the thin film is, for example, 1 nm to 800 nm, 10 nm to 700 nm, 50 nm to 600 nm, or 100 nm to 500 nm. If the thickness of the thin film is less than 1 nm, it may be difficult for the function of the thin film to be exerted. If the thickness of the thin film is excessively thick, the thin film itself may absorb lithium, which may reduce the amount of lithium precipitation from the negative electrode, thereby lowering the energy density of the all-solid-state battery and deteriorating the cycle characteristics of the all-solid-state secondary battery (1). The thin film may be disposed on the negative electrode current collector (21) by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like, but is not necessarily limited to these methods, and any method capable of forming a thin film in the relevant technical field may be used.

[0204] The ratio of the volume of the all-solid-state secondary battery (1) before charging to the volume of the all-solid-state secondary battery (1) after charging, the volume expansion rate, may be, for example, 15% or less, 10% or less, or 5% or less.

[0205] The increase in the volume of the negative electrode layer (20) during charging of the all-solid-state secondary battery (1) is offset by the decrease in the volume of the positive electrode layer (10), and the change in the volume of the all-solid-state secondary battery (1) before and after charging is alleviated by the second inert member (50) accommodating the change in the volume of the negative electrode layer (20).

[0206] The energy density per unit volume of the all-solid-state secondary battery (1) may be, for example, 500 to 900 Wh / L, 500 to 800 Wh / L, or 500 to 700 Wh / L. The energy density per unit weight of the all-solid-state secondary battery (1) may be, for example, 350 to 600 Wh / g, 350 to 580 Wh / g, 350 to 570 Wh / g, or 350 to 550 Wh / g. Since the all-solid-state secondary battery (1) has an energy density in this range, it can provide an improved energy density compared to conventional secondary batteries.

[0207]

[0208] [Solid electrolyte layer]

[0209] [Solid electrolyte layer: solid electrolyte]

[0210] Referring to FIGS. 2 and 3, the solid electrolyte layer (30) includes a solid electrolyte disposed between the positive electrode layer (10) and the negative electrode layer (20).

[0211] The solid electrolyte may include, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0212] The solid electrolyte is, for example, a sulfide-based solid electrolyte. The sulfide-based solid electrolyte is, for example, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0(x(2, Li 7-x PS 6-x Br x , 0(x(2, and Li 7-x PS 6-x I x, 0(x(2) or more. The sulfide-based solid electrolyte is manufactured by treating starting materials such as Li2S, P2S5, etc. by a melting rapid cooling method or a mechanical milling method. In addition, heat treatment may be performed after the treatment. The solid electrolyte may be amorphous, crystalline, or a mixture thereof. In addition, the solid electrolyte may be, for example, one containing sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-described sulfide-based solid electrolyte materials. For example, the solid electrolyte may be a material containing Li2S-P2S5. When using a sulfide-based solid electrolyte material containing Li2S-P2S5 to form the solid electrolyte, the mixing molar ratio of Li2S and P2S5 is, for example, Li2S: P2S5=20:80 to 90:10, 25:75 to 90:10, The range is about 30:70 to 70:30, 40:60 to 60:40.

[0213] The sulfide-based solid electrolyte may include, for example, an argyrodite type solid electrolyte represented by the following chemical formula 1:

[0214] <Chemical Formula 1>

[0215] Li + 12-n-x A n+ X 2- 6-x Y - x

[0216] In the above formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta, X is S, Se or Te, Y is Cl, Br, I, F, CN, OCN, SCN or N3, and 1(n(5, 0(x(2). The sulfide-based solid electrolyte is, for example, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-xPS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , may be an argyrodite-type compound including at least one selected from 0≤x≤2. The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.

[0217] The density of the argyrodite-type solid electrolyte may be 1.5 to 2.0 g / cc. Since the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and penetration of the solid electrolyte layer by Li can be effectively suppressed.

[0218] Oxide solid electrolytes include, for example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≤x<1, 0≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, 0≤x≤10), or a combination thereof. The oxide-based solid electrolyte is manufactured, for example, by a sintering method.

[0219] Oxide-based solid electrolytes include, for example, Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, 0 <a<2, 0≤x≤10) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.

[0220] The polymer solid electrolyte may include, for example, a dry polymer electrolyte, a gel polymer electrolyte, or a combination thereof.

[0221] A dry polymer electrolyte is an electrolyte that is, for example, a mixture of a lithium salt and a polymer. A dry polymer electrolyte is, for example, a polymer electrolyte that does not include a liquid electrolyte. The polymer included in the dry polymer electrolyte can be, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, or a combination thereof.

[0222] A gel polymer electrolyte is an electrolyte that contains a liquid electrolyte and a polymer. The liquid electrolyte is, for example, a mixture of a lithium salt and an organic solvent. The polymer contained in the gel polymer electrolyte can be selected from the polymers contained in the dry polymer electrolyte.

[0223] The solid electrolyte layer (30) may be impermeable to lithium polysulfide. Accordingly, side reactions between lithium polysulfide generated during charging and discharging of the sulfide-based positive electrode active material and the negative electrode layer can be prevented. Accordingly, the cycle characteristics of the all-solid-state secondary battery (1) including the solid electrolyte layer (30) can be improved.

[0224] [Solid electrolyte layer: binder]

[0225] The solid electrolyte layer (30) may include, for example, a binder. The binder included in the solid electrolyte layer (30) is not limited to, but may include, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., and any binder used in the relevant technical field may be used. The binder of the solid electrolyte layer (30) may be the same as or different from the binder included in the positive electrode active material layer (12) and the negative electrode active material layer (22). The binder may be omitted.

[0226] The binder content included in the solid electrolyte layer (30) is 0.1 to 10 wt%, 0.1 to 5 wt%, 0.1 to 3 wt%, 0.1 to 1 wt%, 0 to 0.5 wt%, or 0 to 0.1 wt% with respect to the total weight of the solid electrolyte layer (30).

[0227] A method for manufacturing a composite cathode active material according to an embodiment of the present invention is as follows:

[0228] A step of providing a lithium-containing sulfide compound; a step of providing a composite; a first step of providing a second carbon-based material; and

[0229] i) a second step including a step of mechanically milling the lithium-containing sulfide-based compound, the composite, and the second carbon-based material; or ii) a second step including a step of mechanically milling the lithium-containing sulfide-based compound and the composite; and mixing the second carbon-based material into the milled product.

[0230] When the second carbon-based material is CNF, the second step is performed by mechanically milling the lithium-containing sulfide-based compound and the composite; and mixing the second carbon-based material into the milled product.

[0231] When the second carbon-based material is CNT, the second step can be performed by: i) mechanically milling the lithium-containing sulfide-based compound, composite, and the second carbon-based material. In this way, when CNF is used, unlike CNT, a milling process is not required, and thus a lithium battery with improved capacity and capacity retention can be manufactured compared to CNF.

[0232] The mechanical milling step can be performed using a planetary ball mill at 300 to 1000 rpm, 400 to 800 rpm, or 450 to 600 rpm. The milling time can be, for example, 1 to 20 hours, or 5 to 15 hours. The mixing process can be performed using a mixer, pestle, etc.

[0233] The above complex has the chemical formula M a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되는 1종 이상의 제1 금속산화물, 제1 탄소계 재료 및 제2탄소계 재료를 포함하며, 상기 제1 금속산화물이 제1 탄소계 재료 메트릭스 내에 배치되며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이며, 상기 제2탄소계 재료가 종횡비 10 이상의 섬유상 탄소를 포함한다.

[0234] In the above mechanical milling step, the milling method is not particularly limited,

[0235] Any method available in the art can be used as a method for mechanically contacting a mixture of lithium-containing sulfide compounds and complexes or the mixture with a second carbon-based material.

[0236] A lithium-containing sulfide compound is provided.

[0237] Next, the complex is provided.

[0238] The step of providing a complex includes, for example, supplying a reaction gas comprising a carbon source gas to a structure including a metal oxide and heat treating the structure to provide an undoped complex.

[0239] The steps for providing the complex are, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2 또는 3인 경우, b가 정수임)로 표시되는 1종 이상의 제2 금속산화물에 탄소 공급원 기체로 이루어진 반응 가스를 공급하고 열처리하여 미도핑 복합체를 제조하는 단계를 포함하며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이다.

[0240] The carbon source gas is a compound represented by the following chemical formula 7, or at least one mixed gas selected from the group consisting of a compound represented by the following chemical formula 7, a compound represented by the following chemical formula 8, and an oxygen-containing gas represented by the following chemical formula 9.

[0241] <Chemical Formula 7>

[0242] CnH (2n+2-a) [OH] a

[0243] In the above chemical formula 7, n is 1 to 20, a is 0 or 1;

[0244] <Chemical Formula 8>

[0245] CnH 2n

[0246] In the above chemical formula 8, n is 2 to 6;

[0247] <Chemical Formula 9>

[0248] C x H y O z

[0249] In the above chemical formula 9, x is 0 or an integer from 1 to 20, y is 0 or an integer from 1 to 20, and z is 1 or 2.

[0250] The compound represented by chemical formula 7 and the compound represented by chemical formula 8 are at least one selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by chemical formula 9 includes, for example, carbon dioxide (CO2), carbon monoxide (CO), water vapor (H2O), or a mixture thereof.

[0251] M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물에 탄소 공급원 기체로 이루어진 반응 가스를 공급하고 열처리하는 단계 이후에 질소, 헬륨 및 아르곤으로 이루어진 군으로부터 선택된 하나 이상의 불활성 기체를 이용한 냉각 단계를 더 거칠 수 있다. 냉각 단계는 상온(20-25℃)으로 조절하는 단계를 말한다. 탄소 공급원 기체는 질소, 헬륨, 아르곤으로 이루어진 군으로부터 선택된 하나 이상의 불활성 기체를 포함할 수 있다.

[0252] In the manufacturing method of the composite, the process of growing carbon-based materials, such as graphene, depending on the gas phase reaction can be performed under various conditions.

[0253] According to the first condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 메탄을 공급하고 열처리온도(T)까지 승온처리한다. 열처리 온도(T)까지의 승온 시간은 10분 내지 4시간이고 열처리온도(T)는 700 내지 1100℃ 범위이다. 열처리온도(T)에서 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 내지 8시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 내지 5 시간이다.

[0254] According to the second condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 수소를 공급하고 열처리온도(T)까지 승온 처리한다. 열처리 온도(T)까지의 승온 시간은 10분 내지 4시간이고 열처리온도(T)는 700 내지 1100℃ 범위이다. 열처리온도(T)에서 일정 반응 시간 동안 열처리한 후 메탄 가스를 공급하고 잔여 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 내지 8시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 냉각하는 과정에서 질소를 공급한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 내지 5시간이다.

[0255] According to the third condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 수소를 공급하고 열처리온도(T)까지 승온 처리한다. 열처리 온도(T)까지의 승온 시간은 10분 내지 4시간이고 열처리온도(T)는 700 내지 1100℃ 범위이다. 열처리온도(T)에서 일정 반응 시간 동안 열처리한 후 메탄과 수소의 혼합 가스를 공급하고 잔여 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 내지 8시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 냉각하는 과정에서 질소를 공급한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 내지 5 시간이다.

[0256] In the process of manufacturing a composite, if the carbon source gas contains water vapor, a composite having excellent conductivity can be obtained. The content of water vapor in the gas mixture is not limited and is, for example, 0.01 to 10% by volume based on 100% by volume of the total carbon source gas. The carbon source gas is, for example, methane; a mixed gas containing methane and an inert gas; or a mixed gas containing methane and an oxygen-containing gas.

[0257] The carbon source gas can be, for example, methane; a mixture of methane and carbon dioxide; or a mixture of methane, carbon dioxide, and water vapor. In the mixture of methane and carbon dioxide, the molar ratio of methane to carbon dioxide is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. In the mixture of methane, carbon dioxide, and water vapor, the molar ratio of methane, carbon dioxide, and water vapor is about 1:0.20 to 0.50:0.01 to 1.45, about 1:0.25 to 0.45:0.10 to 1.35, or about 1:0.30 to 0.40:0.50 to 1.0.

[0258] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas may not include an inert gas such as nitrogen.

[0259] The heat treatment pressure can be selected based on factors such as the heat treatment temperature, the composition of the gas mixture, and the desired amount of carbon coating. The heat treatment pressure can be controlled by adjusting the amount of the incoming and outgoing gas mixtures. The heat treatment pressure can be, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more.

[0260] The heat treatment time is not particularly limited and can be appropriately adjusted depending on the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the desired amount of carbon coating. For example, the reaction time at the heat treatment temperature is, for example, 10 minutes to 100 hours, 30 minutes to 90 hours, or 50 minutes to 40 hours. For example, as the heat treatment time increases, the amount of carbon deposited, for example, the amount of graphene, increases, and thus the electrical properties of the composite may improve. However, this trend may not necessarily be directly proportional to time. For example, after a certain period of time, carbon deposition, for example, graphene deposition, may no longer occur or the deposition rate may decrease.

[0261] Through the gas phase reaction of the carbon source gas described above, M is produced even at relatively low temperatures. a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물 및 그 환원 생성물인 M a O b (0 <a≤3, 0<b<4, a는 1, 2, 또는 3이며, b 는 정수가 아님)로 표시되는 제1 금속산화물 중에서 선택된 하나 이상에 균일한 탄소계 재료의 코팅 예를 들어 그래핀 코팅을 제공함에 의하여 미도핑 복합체가 얻어진다.

[0262] The composite is a matrix of a carbon-based material having one or more structures selected from, for example, a spherical structure, a spiral structure in which multiple spherical structures are connected, a cluster structure in which multiple spherical structures are aggregated, and a sponge structure, for example, a graphene matrix and M disposed within the carbon-based material matrix. a O b (0 <a≤3, 0<b<4, a는 1, 2, 또는 3이며, b 는 정수가 아님)로 표시되는 제1 금속산화물 및 M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물 중에서 선택된 하나 이상을 포함한다.

[0263] Next, the mixture of the lithium-containing sulfide-based positive electrode active material and the composite or the mixture and the second carbon-based material are mechanically milled.

[0264] A Novilta mixer, a planetary mixer, etc. can be used during milling. The rotation speed of the mixer during milling varies depending on the milling equipment, but is, for example, 500 rpm to 2000 rpm. When the milling speed is within the above range, the shear force applied to the lithium-containing sulfide-based positive electrode active material and the composite is appropriate, so that the lithium-containing sulfide-based positive electrode active material and the composite form a good chemical bond, and the composite progresses smoothly, so that the composite is uniformly coated on the lithium-containing sulfide-based positive electrode active material to form a uniform and continuous shell. The milling time is, for example, 1 hour to 20 hours, or 10 to 20 hours. When the milling time is within the above range, the composite is uniformly coated on the lithium-containing sulfide-based positive electrode active material, so that a uniform and continuous shell can be easily formed, and the production efficiency is excellent.

[0265] The average particle size (D50) of the composite used for mechanical milling is, for example, 1 um to 20 um, 3 um to 15 um, or 5 um to 10 um.

[0266] According to another embodiment, a step of mixing a second carbon-based material into the milled product is performed.

[0267] In this specification, a and b of "carbon atoms a to b" refer to the carbon atoms of a specific functional group. That is, the functional group may include carbon atoms from a to b. For example, "an alkyl group having 1 to 4 carbon atoms" refers to an alkyl group having 1 to 4 carbon atoms, i.e., CH3-, CH3CH2-, CH3CH2CH2-, (CH3)2CH-, CH3CH2CH2CH2-, CH3CH2CH(CH3)- and (CH3)3C-.

[0268] The nomenclature for a particular radical may include monoradical or diradical, depending on the context. For example, if a substituent requires two points of attachment to the rest of the molecule, the substituent should be understood as a diradical. For example, a substituent specified as an alkyl group requiring two points of attachment would be -CH 2- , -CH2CH 2- , -CH2CH(CH3)CH 2- , etc. Other radical nomenclatures, such as "acylene", clearly indicate that the radical is a diradical.

[0269] As used herein, the term "alkyl group" or "alkylene group" refers to a branched or unbranched aliphatic hydrocarbon group. In one embodiment, the alkyl group can be substituted or unsubstituted. The alkyl group includes, but is not necessarily limited to, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a hexyl group, a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and the like, each of which can be optionally substituted or unsubstituted. In one embodiment, the alkyl group can have 1 to 5 carbon atoms. For example, an alkyl group having 1 to 5 carbon atoms can be, but is not necessarily limited to, methyl, ethyl, propyl, isopropyl, butyl, iso-butyl, sec-butyl, pentyl, 3-pentyl, and the like.

[0270] As used herein, the term "cyanoalkyl group" means an alkyl group to which a cyano group is attached. Examples thereof include cyanomethyl, cyanobutyl, and cyanopentyl.

[0271] As used herein, the term "alkenyl group" refers to a hydrocarbon group having 2 to 20 carbon atoms, including at least one carbon-carbon double bond, including but not limited to an ethenyl group, a 1-propenyl group, a 2-propenyl group, a 2-methyl-1-propenyl group, a 1-butenyl group, a 2-butenyl group, a cyclopropenyl group, a cyclopentenyl group, a cyclohexenyl group, a cycloheptenyl group, and the like. In one embodiment, the alkenyl group can be substituted or unsubstituted. In one embodiment, the alkenyl group can have 2 to 40 carbon atoms.

[0272] As used herein, the term "aromatic" means a ring or ring system having a conjugated pi electron system, including carbocyclic aromatics (e.g., a phenyl group) and heterocyclic aromatics (e.g., pyridine). The term includes monocyclic rings or fused polycyclic rings (i.e., rings that share adjacent pairs of atoms) if the entire ring system is aromatic.

[0273] As used herein, the term "aryl group" means an aromatic ring or ring system (i.e., two or more fused rings that share two adjacent carbon atoms) whose ring skeleton contains only carbon. If the aryl group is a ring system, each ring in the system is aromatic. For example, aryl groups include, but are not limited to, phenyl, biphenyl, naphthyl, phenanthrenyl, naphthacenyl, and the like. The aryl group may be substituted or unsubstituted.

[0274] As used herein, the term "heteroaryl group" refers to an aromatic ring system having one ring or multiple fused rings, wherein one or more ring atoms are not carbon, i.e., heteroatoms. In a fused ring system, one or more heteroatoms can be present in only one ring. For example, heteroatoms include, but are not necessarily limited to, oxygen, sulfur, and nitrogen. For example, a heteroaryl group can be, but is not limited to, furanyl, thienyl, imidazolyl, quinazolinyl, quinolinyl, isoquinolinyl, quinoxalinyl, pyridinyl, pyrrolyl, oxazolyl, indolyl, and the like.

[0275] As used herein, “halogen” means a stable element belonging to group 17 of the periodic table of elements, for example, fluorine, chlorine, bromine or iodine, and in particular, fluorine and / or chlorine.

[0276] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0277] (Manufacture of composites)

[0278] Manufacturing Example 1: Al2O3@Gr composite

[0279] Al2O3 particles (average particle size: approximately 20 nm) were placed inside the reactor, and then CH4 was supplied into the reactor at approximately 300 sccm and 1 atm for approximately 30 minutes, and the temperature inside the reactor was raised to 1000°C.

[0280] Then, heat treatment was performed by maintaining the temperature for 7 hours. Then, the internal temperature of the reactor was adjusted to room temperature (20-25℃) to produce Al2O3 particles and its reduction product, Al2O z (0 <z<3) 입자가 그래핀에 매립된 복합체를 얻었다.

[0281] The alumina content of the composite was 75 wt%.

[0282] Manufacturing Example 2: Al2O3@Gr composite

[0283] A composite was manufactured in the same manner as in Manufacturing Example 1, except that Al2O3 particles (average particle diameter: approximately 200 nm) were used instead of Al2O3 particles (average particle diameter: approximately 20 nm).

[0284] Comparative Manufacturing Example 1: SiO2@Gr Composite

[0285] SiO2 particles (average particle diameter: approximately 15 nm) were placed inside the reactor, and then CH4 was supplied into the reactor at approximately 300 sccm and 1 atm for approximately 30 minutes, and the temperature inside the reactor was raised to 1000°C.

[0286] Then, heat treatment was performed by maintaining the temperature for 7 hours. Then, the internal temperature of the reactor was adjusted to room temperature (20 to 25 ℃) to produce SiO2 particles and its reduction product, SiO y (0 <y<2) 입자가 그래핀에 매립된 복합체를 얻었다.

[0287] (Manufacture of composite cathode active material)

[0288] Example 1: Li2S-GB + CNF composite cathode active material with Al2O3-GB coating and CNF blend, GB 33.3 wt% (alumina 25 wt%) coating, CNF 16.7 wt% blend (Li2S-GB+CNF)

[0289] Li2S having an average particle size of 10 μm and the composite (Al2O3-GB) prepared in Manufacturing Example 1 were milled using a planetary mixer at a rotation speed of about 500 rpm for about 10 hours to obtain a composite cathode active material precursor. Here, Li2S and the composite prepared in Manufacturing Example 1 were mixed at a weight ratio of 3:2.

[0290] Carbon nanofibers (hereinafter referred to as CNF) were added to the above composite cathode active material precursor and mixed using a mortar and pestle to obtain a composite cathode active material (Li2S-GB+CNF). The mixing weight ratio of the composite cathode active material precursor and CNF was 5:1, the length of the CNF was 16 μm, the diameter was 300 nm, and the aspect ratio was 53.

[0291] Li2S, the composite prepared in Preparation Example 1, and CNF are in a weight ratio of 30:20:10.

[0292] In the composite cathode active material, based on 100 wt% of the composite cathode active material, the content of lithium sulfide is 50 wt%, the content of the composite (Al2O3-GB) prepared in Manufacturing Example 1 is 33.3 wt%, and the content of CNF is 16.7 wt%.

[0293] Example 2: Al2O3-GB and CNT-coated Li2S-GB-CNT composite cathode active material, GB 33.3 wt% coating, CNT 16.7 wt% coating (Li2S-GB-CNT)

[0294] Li2S, CNT, and the composite (Al2O3-GB) prepared in Manufacturing Example 1 with an average particle size of 10 μm were milled using a ball mill at a rotation speed of about 500 rpm for about 10 hours to obtain a composite cathode active material (Li2S-GB-CNT). Li2S, the composite prepared in Manufacturing Example 1, and CNT were mixed in a weight ratio of 30:20:10.

[0295] In the composite cathode active material, based on 100 wt% of the composite cathode active material, the content of lithium sulfide is 50 wt%, the content of the composite (Al2O3-GB) prepared in Manufacturing Example 1 is 33.3 wt%, and the content of CNT is 16.7 wt%.

[0296] Scanning electron microscopy analysis of the composite cathode active material confirmed the presence of carbon nanotubes (CNTs) on its surface. The CNTs are 6 nm in diameter, 100 μm in length, and have an aspect ratio of approximately 1667.

[0297] Example 3: Al2O3-GB coating and CNF mixed (Li2S-GB) + CNF composite cathode active material, GB 20 wt% coating, CNF 9.1 wt% mixed (Li2S-GB+CNF)

[0298] A composite cathode active material was manufactured in the same manner as in Example 1, except that the content of CNF was changed to 9.1 wt% based on 100 wt% of the final composite cathode active material. The mixing weight ratio of the composite cathode active material precursor (Li2S-GB) and CNF was 10:1, the length of CNF was 16 μm, the diameter was 300 nm, and the aspect ratio was 53. In addition, the weight ratio of Li2S, the composite (GB) prepared in Manufacturing Example 1, and CNF was 30:20:5. In the composite cathode active material, the content of lithium sulfide was 54.5 wt%, the content of the composite (Al2O3-GB) prepared in Manufacturing Example 1 was 36.4 wt%, and the content of CNF was 9.1 wt%, based on 100 wt% of the composite cathode active material.

[0299] Example 4: Al2O3-GB coated and CNT coated Li2S-GB-CNT composite cathode active material, GB 36.4 wt% coated, CNT 9.1 wt% coated (Li2S-GB-CNT)

[0300] A composite cathode active material was manufactured in the same manner as in Example 2, except that the content of CNT was changed to 9.1 wt% based on 100 wt% of the composite cathode active material. Li2S, the composite prepared in Manufacturing Example 1, and CNT were mixed in a weight ratio of 30:20:5. In the composite cathode active material, the content of lithium sulfide was 54.5 wt%, the content of the composite (Al2O3-GB) prepared in Manufacturing Example 1 was 36.4 wt%, and the content of CNT was 9.1 wt% based on 100 wt% of the composite cathode active material.

[0301] Example 5: Li2S + CNF composite cathode active material with Al2O3-GB coating and CNF blend, GB 27.3 wt% (alumina 20.5 wt% coating, CNF 18.2 wt% blend (Li2S-GB+CNF)

[0302] A composite cathode active material was manufactured in the same manner as in Example 1, except that the content of Al2O3-GB was changed to 27.3 wt% based on 100 wt% of the composite cathode active material.

[0303] In the composite cathode active material, based on 100 wt% of the composite cathode active material, the content of lithium sulfide is 54.5 wt%, the content of the composite (Al2O3-GB) prepared in Manufacturing Example 1 is 27.3 wt%, and the content of CNF is 18.2 wt%.

[0304] Example 6: Al2O3-GB coated and CNT coated Li2S-CNT composite cathode active material, GB 27.3 wt% coated, CNT 18.2 wt% coated (Li2S-GB-CNT)

[0305] A composite cathode active material was manufactured in the same manner as in Example 2, except that the content of Al2O3-GB was changed to 27.3 wt% based on 100 wt% of the composite cathode active material.

[0306] In the composite cathode active material, based on 100 wt% of the composite cathode active material, the content of lithium sulfide is 54.5 wt%, the content of the composite (Al2O3-GB) prepared in Manufacturing Example 1 is 27.3 wt%, and the content of CNT is 18.2 wt%.

[0307] Comparative Example 1: Bare Li2S cathode active material

[0308] Li2S with an average particle size of 10 μm was used as the positive electrode active material.

[0309] Comparative Example 2: Li2S+CNF

[0310] Li2S having an average particle size of 10 μm was milled using a planetary mixer at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes, then CNF was added thereto and mixed using a mortar and pestle to obtain a composite cathode active material (Li2S+CNF). Li2S and CNF were mixed at a weight ratio of 30:10, and the length of CNF was 16 μm, the diameter was 300 nm, and the aspect ratio was 53.

[0311] Comparative Example 3: CNT-coated Li2S composite cathode active material (Li2S-CNT)

[0312] Li2S and CNT with an average particle size of 10 μm were milled using a ball mill at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to produce a composite cathode active material (Li 2S -CNT) was obtained. Li2S and CNT were mixed at a weight ratio of 30:10. Here, the same CNT as in Example 2 was used.

[0313] Comparative Example 4: Li2S composite cathode active material mixed with CNT and CNF, CNF 0.1 wt% mixed (Li2S-CNT+CNF)

[0314] Li2S and CNT with an average particle size of 10 μm were milled using a ball mill at a rotation speed of approximately 1,000 to 2,000 rpm for approximately 5 to 30 minutes to obtain a composite cathode active material precursor. Li2S and CNT were mixed at a weight ratio of 30:10.

[0315] CNF was added to the above-mentioned cathode active material precursor and mixed using a mortar and pestle to obtain a composite cathode active material (Li2S-CNT+CNF). The mixing weight ratio of Li2S, CNT, and CNF was 30:10:10. Here, the CNF and CNT were the same as those used in Examples 1 and 2, respectively.

[0316] Comparative Example 5: Li2S-GB

[0317] Li2S having an average particle size of 10 μm and the composite (Al2O3-GB) prepared in Manufacturing Example 1 were milled using a planetary mixer at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to obtain a composite cathode active material. Li2S and the composite prepared in Manufacturing Example 1 were mixed at a weight ratio of 30:20.

[0318] The composition of the starting materials used in the manufacture of the composite positive electrode active material manufactured in the above Example 1-6 and Comparative Example 1-5 is as shown in Table 1 below.

[0319] Composition of the cathode active material (weight parts) Li2SGBCNTCNFExample 1 (Li2S-GB+CNF) 30 20 10Example 2 (Li2S-GB-CNT) 30 20 10Example 3 (Li2S-GB+CNF) 30 20 5Example 4 (Li2S-GB-CNT) 30 20 5Example 5 (Li2S-GB+CNF) 30 15 10Example 6 (Li2S-GB-CNT) 30 15 10Comparative Example 1 Li2S 30Comparative Example 2 Li2S+CNF 30 10Comparative Example 3 Li2S-CNT 30 10Comparative Example 4 Li2S-CNT+CNF 30 10 10Comparative Example 5 Li2S-GB 30 20

[0320] In Table 1 above, the total weight of the composite cathode active material is the sum of the weights of lithium sulfide, GB, CNT, and CNF, and SE represents the content of the solid electrolyte used in the manufacture of the cathode.

[0321] Production Example 1: All-solid-state secondary battery

[0322] (Cathode layer manufacturing)

[0323] A 10 ㎛ thick SUS foil was prepared as a negative electrode current collector. In addition, carbon black (CB) particles with a primary particle diameter of approximately 30 nm and silver (Ag) particles with an average particle diameter of approximately 60 nm were prepared as negative electrode active materials.

[0324] 4 g of a mixed powder containing carbon black (CB) and silver (Ag) particles in a weight ratio of 3:1 was placed in a container, and 4 g of an NMP solution containing 7 wt% PVDF binder (Kureha #9300) was added thereto to prepare a mixed solution. Then, a slurry was prepared by stirring the mixed solution while adding NMP little by little to the mixed solution. The prepared slurry was applied to a SUS sheet using a bar coater and dried in the air at 80°C for 10 minutes. The laminate thus obtained was vacuum-dried at 40°C for 10 hours. The dried laminate was dried at 5 ton·f / cm 2The surface of the first negative electrode active material layer of the laminate was flattened by cold roll pressing at a pressure of 5 m / sec. The negative electrode layer was manufactured by the above process. The thickness of the first negative electrode active material layer included in the negative electrode layer was approximately 15 μm. The areas of the first negative electrode active material layer and the negative electrode current collector were the same.

[0325] (Anode layer manufacturing)

[0326] The composite cathode active material manufactured in Example 1 was used as the cathode active material. Li6PS5Cl, an argyrodite-type crystal (D50=3.0 μm, crystalline), was prepared as the solid electrolyte. Ketjen black was prepared as the conductive agent. These materials were mixed in a weight ratio of composite cathode active material: solid electrolyte: conductive agent = 45:45:1 to prepare a cathode mixture. The cathode mixture was obtained by dry mixing using a ball mill. The cathode mixture obtained by the ball milling formed an ionic conductive and electronic conductive network.

[0327] The positive electrode mixture was placed on one side of a positive electrode current collector made of aluminum foil or SUS coated on one side, and plate pressed at a pressure of 200 MPa for 10 minutes to produce a positive electrode layer. The thickness of the positive electrode layer was approximately 120 μm. The thickness of the positive electrode active material layer was approximately 100 μm, and the thickness of the carbon-coated aluminum foil was approximately 20 μm. The areas of the positive electrode active material layer and the positive electrode current collector were the same.

[0328] (Manufacturing of solid electrolyte layer)

[0329] Li6PS5Cl solid electrolyte in the form of argyrodite crystals (D 50=3.0 (m, crystalline), a mixture was prepared by adding 1.5 parts by weight of an acrylic binder to 98.5 parts by weight of a solid electrolyte. Octyl acetate was added to the prepared mixture and stirred to prepare a slurry. The prepared slurry was applied using a bar coater onto a 15 (m thick nonwoven fabric placed on a 75 (m thick PET substrate), and dried in air at 80°C for 10 minutes to obtain a laminate. The obtained laminate was vacuum-dried at 80°C for 2 hours. A solid electrolyte layer was prepared by the above process.

[0330] (Manufacturing of all-solid-state secondary batteries)

[0331] A solid electrolyte layer was placed on the cathode layer so that the first cathode active material layer was in contact with the solid electrolyte layer, and a positive electrode layer was placed on the solid electrolyte layer to prepare a laminate.

[0332] 85 prepared laminates o The solid electrolyte layer was plate-pressed at 500 MPa for 30 min at C. This pressurization process sintered the solid electrolyte layer, thereby improving battery characteristics. The thickness of the sintered solid electrolyte layer was approximately 45 ㎛. The density of the Li6PS5Cl solid electrolyte, which was an argyrodite-type crystal contained in the sintered solid electrolyte layer, was 1.6 g / cc. The area of ​​the solid electrolyte layer was the same as that of the negative electrode layer.

[0333] The pressurized laminate was placed in a pouch and vacuum-sealed to manufacture an all-solid-state secondary battery. Portions of the positive and negative electrode collectors were extended outside the sealed battery to serve as positive and negative electrode terminals.

[0334] Production example 2

[0335] An all-solid-state secondary battery was manufactured according to the same method as in Manufacturing Example 1, except that the composite cathode active material manufactured in Example 2 was used instead of the composite cathode active material manufactured in Example 1 as the cathode active material when manufacturing the cathode layer.

[0336] Production Example 3-6

[0337] An all-solid-state secondary battery was manufactured according to the same method as Example 6, except that the composite cathode active material manufactured in Examples 3 to 6 was used instead of the composite cathode active material manufactured in Example 1 as the cathode active material in the manufacture of the cathode layer.

[0338] Comparative Production Example 1-5

[0339] An all-solid-state secondary battery was manufactured according to the same method as Manufacturing Example 1, except that the composite cathode active material manufactured in Comparative Examples 1 to 5 was used instead of the composite cathode active material manufactured in Example 1 as the cathode active material in manufacturing the cathode layer.

[0340] Evaluation Example 1: SEM, HR-TEM, and SEM-EDS Analysis

[0341] Scanning electron microscopy, high-resolution transmission electron microscopy, and SEM-EDS (energy-dispersive X-ray spectroscopy) analyses were performed on the composite cathode active material manufactured in Example 1. For the SEM-EDS analysis, Philips' FEI Titan 80-300 was used.

[0342] The composite manufactured in Manufacturing Example 1 comprises Al2O3 particles and its reduction product, Al2O z (0 <z<3) 입자가 그래핀에 매립된 구조를 가짐을 보여주었다. Al2O3입자 및 Al2O z (0 <z<3) 중에서 선택된 하나 이상의 입자의 외곽에 그래핀층이 배치됨을 확인하였다. Al2O3입자 및 Al2O z (0 <z<3) 중에서 선택된 하나 이상의 입자는 그래핀 메트릭스 내에 균일하게 분산되었다. Al2O3입자 및 Al2Oz (0 <z<3) 입자 중 하나 이상의 입경은 약 20nm 이었다. 제조예 1에서 제조된 복합체의 입경은 약 50nm 내지 200nm 이었다.

[0343] In the composite negative electrode material manufactured in Example 1, on the lithium sulfide core or SiOx (0 <x<2) 코어 상에, 그래핀을 포함하는 복합체에 의하여 형성된 쉘(shell)이 배치됨을 확인하였다.

[0344] SEM-EDS mapping analysis was performed on the composite cathode active material manufactured in Example 1.

[0345] As a result of the analysis, aluminum (Al) distributed on the surface of the composite cathode active material of Example 1 was confirmed. From this, it was confirmed that in the composite cathode active material, on the silicon composite structure core or SiOx (0 <x<2) 코어 상에, 제조예 1에서 제조된 복합체가 균일하게 코팅되어 쉘(shell)을 형성함을 확인하였다.

[0346] Evaluation Example 2: Life Characteristics Test

[0347] The charge / discharge characteristics of the all-solid-state secondary batteries manufactured in Manufacturing Examples 1-3, 5-6 and Comparative Manufacturing Example 1-3 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary batteries in a constant temperature bath at 45°C.

[0348] The first cycle is 0.6 mA / cm until the battery voltage is 2.5 V to 2.8 V. 2 The battery was charged for 12.5 hours at a constant current of 0.6 mA / cm until the battery voltage reached 0.3 V. 2 Discharge was performed for 12.5 hours at a constant current.

[0349] The charge / discharge characteristics of the all-solid-state secondary battery manufactured in Comparative Example 2 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary battery in a constant temperature bath at 45°C.

[0350] The first cycle is 0.6 mA / cm until the battery voltage reaches 2.8 V to 3.0 V. 2 The battery was charged for 12.5 hours at a constant current of 0.6 mA / cm until the battery voltage became 1.0 V. 2 Discharge was performed for 12.5 hours at a constant current.

[0351] The discharge capacity of the first cycle was used as the standard capacity. From the second cycle onward, charging and discharging were performed up to 150 cycles under the same conditions as the first cycle. The measurement results are shown in Table 1 below.

[0352] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 3 below. The initial efficiency is defined by Equation 1 below, and the capacity retention rate is defined by Equation 2 below.

[0353] <Mathematical Formula 1>

[0354] Initial efficiency [%] = [Discharge capacity in the Martian cycle / Charge capacity in the Martian cycle] ㅧ 100

[0355] <Mathematical Formula 2>

[0356] Capacity retention rate [%] = [50 th Discharge capacity in cycles / 1 st Discharge capacity in cycle] × 100

[0357] Partial distribution Cathode active material composition Capacity (mAh / g) Capacity retention rate [%] Manufacturing example 1 Example 1 (Li2S-GB+CNF) 101795.3 Manufacturing example 2 Example 2 (Li2S-GB-CNT) 42572.5 Manufacturing example 3 Example 3 (Li2S-GB+CNF) 83280.2 Manufacturing example 5 Example 5 (Li2S-GB+CNF) 78482.6 Manufacturing example 6 Example 6 (Li2S-GB-CNT) 71462.1 Comparative Manufacturing example 1 Comparative example 1 (Li2S alone) 00 Comparative Manufacturing example 2 Comparative example 2 (Li2S+CNF) 13935.5 Comparative Manufacturing example 3 Comparative example 3 (Li2S-CNT) 68655.2

[0358] As shown in Table 2, the composite cathode active materials of Examples 1, 3, and 5 using GB and CNF showed improved capacity and capacity retention rate compared to the cathode active material of Comparative Example 1 using only lithium sulfide, the cathode active material of Comparative Example 2 using lithium sulfide and CNF, and the cathode active material of Comparative Example 3 using lithium sulfide and CNT. The all-solid-state secondary battery of Comparative Manufacturing Example 1 using the cathode active material of Comparative Example 1 did not show capacity development. In addition, the composite cathode active materials of Examples 1, 3, and 5 using GB and CNF showed higher capacity and better capacity retention rate than the composite cathode active materials of Examples 2 and 6 using GB and CNT. From this, it was found that the composite cathode active material obtained by mixing CNF as a second carbon-based material is more advantageous in improving capacity and capacity retention rate than the composite cathode active material obtained by milling CNT as a second carbon-based material.

[0359] The composite cathode active material of Example 2 using GB and CNT had a smaller capacity than the composite cathode active material of Comparative Example 3, but the capacity retention rate was greatly improved.

[0360] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.

Claims

1. A core including a lithium-containing sulfide-based positive electrode active material; and A shell disposed along the surface of the core; The above shell has the chemical formula MaOb (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 At least one first metal oxide represented by (not); a first carbon-based material and a second carbon-based material, The above first metal oxide is arranged within the first carbon-based material matrix, and the M is One or more metals selected from groups 2 to 16 of the periodic table of elements, A composite cathode active material, wherein the second carbon-based material comprises fibrous carbon having an aspect ratio of 10 or more.

2. A composite cathode active material in the first paragraph, wherein the metal included in the first metal oxide is at least one metal selected from among Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, Si, and Se.

3. In the first paragraph, the first metal oxide is Al2Oz(0 <z<3), NbOx(0<x<2.5), MgOx(0 <x<1), Sc2Oz(0<z<3), TiOy(0<y<2), ZrOy(0<y<2), V2Oz(0<z<3), WOy(0<y<2), MnOy(0<y<2), Fe2Oz(0<z<3), Co3Ow(0<w<4), PdOx(0<x<1), CuOx(0<x<1), AgOx(0<x<1), ZnOx(0<x<1), Sb2Oz(0<z<3), SiOz(0<z<2), 및SeOy(0<y<2) 중에서 선택되는 하나 이상인, 복합양극활물질.

4. In the first paragraph, the shell has the chemical formula MaOc (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3 , and further includes a second metal oxide represented by (where c is an integer), The second metal oxide contains the same metal as the first metal oxide, The ratio of a and c of the second metal oxide, c / a, is the ratio of a and c of the first metal oxide. A composite cathode active material having a larger value than the b / a ratio.

5. A composite cathode active material in the fourth paragraph, wherein the second metal oxide is selected from Al2O3, NbO, NbO2, Nb2O5MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, SiO2, and SeO2.

6. In the fourth paragraph, the first metal oxide is reduced to the second metal oxide. The product is a composite cathode active material.

7. In the first paragraph, the first carbon-based material includes a carbon-based nanostructure, The above carbon nanostructure comprises a two-dimensional carbon nanostructure, A composite cathode active material, wherein the above two-dimensional carbon nanostructure comprises graphene.

8. In the first paragraph, the second carbon-based material is carbon nanofibers, carbon nanotubes or A composite cathode active material comprising a combination of these.

9. In the 8th paragraph, the carbon nanotube comprises a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof, and the carbon nanotube primary structure is one carbon nanotube unit. Composite cathode active material.

10. In the first paragraph, the lithium-containing sulfide-based positive electrode active material is Li2S. n (n≥1), Li2S n A composite cathode active material comprising a complex containing (n≥1) or a combination thereof.

11. In the 10th paragraph, the Li2S n (n≥1) containing complex is a complex of Li2S and carbon, A composite cathode active material comprising a composite of Li2S, carbon, and a solid electrolyte, a composite of Li2S and a solid electrolyte, or a combination thereof.

12. In the first paragraph, a composite cathode active material in which the content of the second carbon-based material in the shell is 5 to 20 wt% based on 100 wt% of the total weight of the composite cathode active material.

13. A cathode comprising a composite cathode active material according to Article 1.

14. In the 13th paragraph, the positive electrode further includes a solid electrolyte, The content of the above solid electrolyte is 80 to 120 parts by weight based on 100 parts by weight of the composite positive electrode active material.

15. An all-solid-state battery comprising a positive electrode layer; a negative electrode layer; and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, An all-solid-state battery comprising the positive electrode layer according to claim 13.

16. In the 15th paragraph, the solid electrolyte layer includes a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof, The above polymer solid electrolyte comprises a dry polymer electrolyte, a gel polymer electrolyte or a combination thereof, An all-solid-state secondary battery, wherein the solid electrolyte layer is impermeable to lithium polysulfide.

17. In the 15th paragraph, the negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on one surface of the negative electrode current collector, The first negative electrode active material layer includes a negative electrode active material and a binder, The above negative electrode active material includes at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material, The above carbon-based negative electrode active material includes amorphous carbon, crystalline carbon, porous carbon, or a combination thereof. An all-solid-state secondary battery, wherein the metal or metalloid negative electrode active material comprises gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), indium (In), zinc (Zn), or a combination thereof.

18. In the 15th paragraph, after the all-solid-state battery is charged, a second negative electrode active material layer is further included between the negative electrode current collector and the first negative electrode active material layer. An all-solid-state secondary battery, wherein the second negative electrode active material layer is a metal layer, and the metal layer includes lithium or a lithium alloy.

19. In paragraph 15, The positive electrode includes a positive current collector, the negative electrode includes a negative current collector, and at least one of the positive current collector and the negative current collector includes a base film and a metal layer disposed on one or both sides of the base film. The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, An all-solid-state secondary battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

20. A step of providing a lithium-containing sulfide compound; a step of providing a composite; a first step of providing a second carbon-based material; and i) a second step including a step of mechanically milling the lithium-containing sulfide compound, composite and second carbon-based material; or ii) a step of mechanically milling the lithium-containing sulfide compound and the composite; and a second step of mixing a second carbon-based material into the milled product, Manufacture the composite positive electrode active material of Article 1, The above complex has the chemical formula M a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되는 1종 이상의 제1 금속산화물, 제1 탄소계 재료 및 제2탄소계 재료를 포함하며, The first metal oxide is arranged in a first carbon-based material matrix, and M is at least one metal selected from groups 2 to 13, 15, and 16 of the periodic table of elements. A method for producing a composite cathode active material, wherein the second carbon-based material comprises fibrous carbon having an aspect ratio of 10 or more.

Citation Information

Patent Citations

  • Preparation method for shell-core structured positive electrode material doped with carbon and lithium sulfide

    CN105609738A

  • Composite anode active material, lithium battery including same, and method for producing same

    KR1020150017012A

  • Electrode composite and preparing method thereof

    KR1020170142344A

  • Road traffic safety marking system in school zone

    KR102507553B1

  • Composite cathode active materials, preparation methods thereof, and lithium batteries including the composite cathode active materials

    US20150349333A1

Cited By

  • Cathode active material, battery, and method for producing cathode active material

    EP4768430A1