Optical laminate and image display device comprising same
The optical laminate with a hard coating film bonded to ultra-thin glass through a high-strength adhesive layer addresses the bending strength and hardness challenges in flexible displays, providing enhanced durability and resistance for flexible displays.
Patent Information
- Application Number
- PCT/KR2024/003382
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Ultra-thin glass used in flexible displays requires improved bending strength and pencil hardness to prevent scratches and damage, while existing chemical strengthening methods compromise on hardness due to the use of protective films.
An optical laminate is created with a glass substrate and a hard coating film bonded through an adhesive layer with a storage modulus of 10 MPa or more and adhesive force of 600gf/25mm or more, using an acrylic random copolymer and tackifier composition to ensure high pencil hardness and bending resistance.
The optical laminate achieves a pencil hardness of H or higher, preventing marks from pens and ensuring excellent bending resistance, antifouling, wear resistance, and chemical resistance without curling issues, suitable for flexible displays.
Smart Images

Figure KR2024003382_03102024_PF_FP_ABST
Abstract
Description
Optical laminate and image display device having the same
[0001] The present invention relates to an optical laminate and an image display device having the same, and more particularly, to an optical laminate made of a glass substrate that has excellent pencil hardness characteristics while ensuring bending resistance, and an image display device having the same.
[0002] Recent advancements in display technology have led to the development of foldable, rollable, and stretchable displays. To protect these diverse display formats, active research is underway on ultra-thin glass (UTG) with improved flexibility.
[0003] These ultra-thin glasses, with their flexible properties, require excellent flexural strength for use in various display formats. Furthermore, improved surface roughness is required to enhance display quality.
[0004] In general, in order to reduce the possibility of scratches on the glass surface of the window glass when using the display and the possibility of breakage due to dropping during use, the strength of the window glass used in mobile displays is improved by using ion substitution chemical strengthening.
[0005] For example, Republic of Korea Patent Publication No. 10-1999-0042313 discloses a method for strengthening glass for display.
[0006] However, ultra-thin glass, despite this chemical strengthening treatment, is still too thin. To prevent scattering, a protective film is applied using a soft adhesive. However, this reduces pencil hardness, leading to problems such as marks when using a pen.
[0007] One object of the present invention is to provide an optical laminate of a glass substrate that has excellent pencil hardness characteristics while ensuring bending resistance.
[0008] Another object of the present invention is to provide an image display device equipped with the optical laminate.
[0009] On the one hand, the present invention
[0010] glass substrate,
[0011] A first adhesive layer formed on one surface of the glass substrate, and
[0012] An optical laminate comprising a hard coating film formed on the first adhesive layer,
[0013] The above first adhesive layer has a storage modulus of 10 MPa or more at 25°C and an adhesive strength of 600 gf / 25 mm or more at 25°C,
[0014] The above glass substrate is an ultra-thin glass having a thickness of less than 100 ㎛,
[0015] An optical laminate is provided in which the pencil hardness of the entire optical laminate is H or higher.
[0016]
[0017] In one embodiment of the present invention, the first adhesive layer is formed from an adhesive composition comprising an acrylic random copolymer and a tackifier, and the acrylic random copolymer may be polymerized by including 5 to 30 wt% of a first monomer having a glass transition temperature of a homopolymer of -40°C or lower, 60 to 90 wt% of a second monomer having a glass transition temperature of a homopolymer of 80°C or higher, and 3 to 20 wt% of a third monomer having at least one of a hydroxyl group and a carboxylic acid group in the molecule.
[0018] In one embodiment of the present invention, the acrylic random copolymer may have a glass transition temperature of 0°C or higher.
[0019] In one embodiment of the present invention, the acrylic random copolymer may have an acid value of 0.1 or less.
[0020] In one embodiment of the present invention, the tackifier may include at least one selected from the group consisting of isocyanate compounds, aziridine compounds, epoxy compounds, melamine compounds, peroxide compounds, metal chelate compounds, and oxazoline compounds.
[0021] In one embodiment of the present invention, the hard coating film may include a base film and a hard coating layer formed on the base film.
[0022] In one embodiment of the present invention, the substrate film may be a film composed of one or more resins selected from the group consisting of polyester resin and polyamideimide resin.
[0023] In one embodiment of the present invention, the hard coating layer can be formed from a hard coating composition including a light-transmitting resin, a fluorine-based UV-curable functional group-containing compound, a photoinitiator, and a solvent.
[0024] An optical laminate according to one embodiment of the present invention may further include a second adhesive layer formed on the other side of the glass substrate, and a substrate film formed on the second adhesive layer.
[0025]
[0026] On the other hand, the present invention provides an image display device equipped with the optical laminate.
[0027] On the other hand, the present invention provides a window of a flexible display device having the optical laminate.
[0028] On the other hand, the present invention provides a polarizing plate having the optical laminate.
[0029] On the other hand, the present invention provides a touch sensor equipped with the optical laminate.
[0030] The optical laminate according to the present invention has a laminated structure in which a hard coating film is bonded to an ultra-thin glass via an adhesive layer whose storage modulus and adhesive strength are controlled under specific conditions, thereby ensuring excellent pencil hardness characteristics and bending resistance. In particular, the optical laminate according to one embodiment of the present invention exhibits a pencil hardness of H or higher, so that no marks are left when using a pen.
[0031] FIG. 1 and FIG. 2 are schematic cross-sectional views of an optical laminate according to one embodiment of the present invention.
[0032] Hereinafter, the present invention will be described in more detail.
[0033]
[0034] One embodiment of the present invention
[0035] glass substrate,
[0036] A first adhesive layer formed on one surface of the glass substrate, and
[0037] An optical laminate comprising a hard coating film formed on the first adhesive layer,
[0038] The above first adhesive layer has a storage modulus of 10 MPa or more at 25°C and an adhesive strength of 600 gf / 25 mm or more at 25°C,
[0039] The above glass substrate is an ultra-thin glass having a thickness of less than 100 ㎛,
[0040] It relates to an optical laminate having a pencil hardness of H or higher throughout the optical laminate.
[0041]
[0042] An optical laminate according to one embodiment of the present invention has a pencil hardness of H or higher throughout the entire optical laminate.
[0043] The above pencil hardness is determined by fixing the optical laminate so that the hard coating film is on top, and then repeating the pencil hardness test operation 5 times with a load of 750 gf at a length of 2 cm from the surface of the hard coating film. If no external abnormalities such as scratches are observed 4 or more times during the measurement, the hardness of the pencil used in the test is taken as the pencil hardness. For example, if the test operation is performed 5 times using a pencil H and no external abnormalities occur 4 or more times, the pencil hardness of the material is H or higher.
[0044] If the pencil hardness of the entire optical laminate is less than H, a pressure mark may remain when using the pen, or it may take a long time for the pressure mark to recover.
[0045]
[0046] An optical laminate according to one embodiment of the present invention has a laminated structure in which a hard coating film is bonded to an ultra-thin glass via an adhesive layer whose storage modulus and adhesive strength are controlled under specific conditions, thereby ensuring excellent pencil hardness characteristics and bending resistance. In particular, the optical laminate according to one embodiment of the present invention exhibits a pencil hardness of H or higher, so that no marks are left when using a pen. In addition, since the optical laminate according to one embodiment of the present invention is manufactured by curing and then laminating the adhesive layer, curing shrinkage due to the use of an adhesive does not occur, so curling does not occur, and thus the processability is excellent. In addition, the optical laminate according to one embodiment of the present invention exhibits antifouling properties, wear resistance, and chemical resistance.
[0047]
[0048] Figure 1 is a cross-sectional view of the structure of an optical laminate according to one embodiment of the present invention.
[0049] Referring to FIG. 1, an optical laminate (100) according to one embodiment of the present invention includes a sequentially laminated glass substrate (110), a first adhesive layer (120), and a hard coating film (130).
[0050]
[0051] Below, each component of the optical laminate is described in detail.
[0052]
[0053] The above glass substrate (110) is an ultra-thin glass (UTG) having a thickness of less than 100 μm. For example, the thickness of the glass substrate (110) is 10 μm or more and less than 100 μm, preferably 20 to 95 μm, and more preferably 30 to 90 μm.
[0054] If the thickness of the above glass substrate is 100 ㎛ or more, the bending resistance may be reduced.
[0055]
[0056] The above ultra-thin glass may include at least one selected from the group consisting of aluminoborosilicate, borosilicate, alkali lead silicate, soda lime, lithium aluminosilicate and aluminosilicate, and preferably may include at least one selected from the group consisting of soda lime, lithium aluminosilicate and aluminosilicate.
[0057] The above ultra-thin glass is obtained by cutting a plate into cell units, and the cut surface, i.e. the side surface of the ultra-thin glass, may be vertical without any curves and may be polished to have a uniform side roughness. The ultra-thin glass polished in this way may have an edge portion formed at the point where the top surface and the side surface connect due to the polished portion. The edge portion may be slanted or curved.
[0058] The above ultra-thin glass can be manufactured by the manufacturing method described below, but is not limited thereto.
[0059]
[0060] The method for manufacturing the above ultra-thin glass may include a step of cutting a glass plate into cell units; a step of polishing a cut surface of the cell; a step of etching the polished cell; and a step of healing the polished cut surface of the cell.
[0061] In addition, the method for manufacturing ultra-thin glass may further include, after the healing step, a cleaning step; a chemical strengthening step; and / or a chemical polishing step.
[0062]
[0063] Steps for cutting the original glass into cell units
[0064] First, the original glass is cut into cell units to prepare multiple cells.
[0065] The step of cutting the original glass into cell units is a step for forming a shape according to the design of a device that intends to use the original glass, and may be a step of cutting the original glass to form a plurality of cells. This step may be a step performed without laminating the original glass into multiple layers. This allows for cell tracking in the event of a defect, simplifies the manufacturing process by omitting the lamination process, reduces the defect rate due to residue that may occur during the lamination process, and allows for free selection of the shape of the glass side.
[0066] The above cutting step is not particularly limited as long as it can form a plurality of cells by cutting the original glass, and in one embodiment, the cutting step may form a plurality of cells having a certain shape using a diamond cutting wheel or a CNC cutting machine equipped with a laser.
[0067]
[0068] Step of polishing the cross-section of the unit cell
[0069] Next, the method for manufacturing the ultra-thin glass includes a step of polishing the cut surface of the cell.
[0070] The above polishing is preferably physical polishing, and most preferably, it may be physically polished so that the cut surface of the cell becomes round. The cut surface of the cell refers to the side surface of the cell. In this case, the thickness of the cut cell may be the same as the thickness of the original glass.
[0071] The above physical polishing includes physically polishing the chipping of the cut surface after the cutting step, while simultaneously processing the cell side surface into a desired shape. At this time, the thickness of the cut cell may be the same as the thickness of the original glass before cutting.
[0072] The above polished cut surface, i.e. the side surface of the cell, may have a gentle round shape with a predetermined curvature in terms of stability to reduce the possibility of breakage during post-processing.
[0073] The above physical polishing step is not particularly limited as long as it is a method capable of physically polishing chipping that occurs during cutting, and in one embodiment, it may be performed including a roughing step of polishing the cut surface of a cut cell using a chamfering tool of 400 mesh or less; a semi-finishing step of polishing the cut surface of a cell that has undergone the roughing step using a chamfering tool of about 500 to 800 mesh; and a finishing step of polishing the cross-section of a cell that has undergone the semi-finishing step using a chamfering tool of 1200 mesh or more.
[0074]
[0075] Etching of polished cells and healing of polished cut surfaces of polished cells
[0076] Next, the process may include etching the polished cell and healing the polished cut surface of the polished cell. The process includes simultaneously performing the etching of the polished cell and the healing of the polished cut surface of the polished cell. In addition, the healed cut surface refers to the side surface of the ultra-thin glass cell that is ultimately manufactured.
[0077] In the above healing step, the polished cell can be etched without a protective material such as resin or film to prevent impact on the glass during the process or to mask the etchant.
[0078] The above polished cell can be made ultra-thin through a chemical etching process, and at the same time, the polished cut surface of the cell can be healed to obtain an ultra-thin glass in cell units.
[0079] Specifically, the etching step of the polished cell includes, but is not limited to, chemical etching. The etching step of the polished cell can make the cell ultra-thin.
[0080] The above ultra-thinning refers to a process of making glass thinner to a thickness of less than 100 ㎛.
[0081] Although the etching of the polished cell and the healing of the polished cut surface of the polished cell may be performed separately, it is more preferable in terms of process simplification that the healing of the cut surface of the polished cell is performed simultaneously with the etching of the polished cell by the same method.
[0082] When the above etching and healing steps are performed simultaneously, it is performed to thin the thick-film state cell while improving the edge strength of the cut cell, and the healed cut surface may be processed into a round shape that is smoother than the shape of the polished cut surface. Defects such as chipping of the cut surface due to physical polishing are removed by healing, and the roughness is reduced, so that destruction due to bending can be suppressed. It is preferable that the rounded surface has a gentle curve.
[0083] The chemical etching step may be performed by using a dipping method of dipping the cell in an etchant, and in one embodiment, the chemical etching step may be performed by including at least one of a cell jig fixing step of fixing the cell to a jig for handling the cell; a jig dipping step of allowing the cell to be dipped in an etchant bath filled with the etchant by using the jig; a chemical etching step of uniformly chemically etching the thickness and cross-section at a constant etching rate in the dipped state; a jig discharge step of discharging the jig from the etchant bath when the chemical etching is completed; and a cell separation step of separating the cell, which has been chemically etched, from the jig.
[0084] The etching can be further aided by using a side spray or top spray method in addition to the dipping method in which the above cells are completely immersed in the etchant. The process can also be performed using only the side spray or top spray method, without the dipping method in which the above cells are completely immersed in the etchant. In this case, since the glass is cut into individual cells, the surface tension of the sprayed etchant allows the etchant to be absorbed onto the surface of the glass cells, enabling etching and side healing.
[0085] In the above etching and healing step, etching and healing can be performed while moving a plurality of glass cells through upper and lower jigs, respectively, so that contact between each glass cell can be minimized.
[0086] The above etchant may, in one or more embodiments, contain at least one selected from the group consisting of hydrofluoric acid (HF), ammonium fluoride (NH4F), ammonium hydrogen fluoride (NH4HF2), sodium fluoride (NaF), sodium hydrogen fluoride (NaHF2), lithium fluoride (LiF), potassium fluoride (KF), and calcium fluoride (CaF2).
[0087] When the etching of the polished cell and the healing step of the polished cut surface of the polished cell are each performed as separate steps, after etching the cell through the chemical etching step as described above, the healing step of the polished cut surface of the polished cell can be further performed by applying the same method as the chemical etching step described above.
[0088]
[0089] Cleaning, chemical strengthening and / or chemical polishing steps
[0090] Additionally, the method for manufacturing the ultra-thin glass may further include a cleaning step, a chemical strengthening step, and / or a chemical polishing step. The cleaning step, the chemical strengthening step, and the chemical polishing step may be changed in order, added, or omitted as needed.
[0091] The above cleaning step may be for removing residual foreign substances and etching solution from the previous process. The cleaning process for removing residual foreign substances and etching solution may be a commonly used process. In one embodiment, cleaning may be performed using a cleaning solution, and a spray method for spraying the cleaning solution or a dipping method for immersing the material in the cleaning solution may be used.
[0092] The cleaning solution is not particularly limited as long as it serves to clean the ultra-thin glass surface, and in one or more embodiments, it may be pure water (DI water), or an alkaline cleaning solution containing potassium hydroxide (KOH) or sodium hydroxide (NaOH).
[0093] The chemical strengthening step is for strengthening the ultra-thin glass by immersing the ultra-thin glass in a molten salt to exchange alkali ions within the ultra-thin glass with alkali ions in the molten salt. In one embodiment, the chemical strengthening step may be performed by including a preheating step of gradually increasing the temperature of the ultra-thin glass; a chemical strengthening step of the preheated ultra-thin glass by ion substitution; and a step of slowly cooling the strengthened ultra-thin glass to room temperature.
[0094] The preheating step of gradually increasing the temperature of the ultra-thin glass may be performed to gradually increase the temperature before immersing the ultra-thin glass in an ion exchange solution in order to prevent breakage of the ultra-thin glass due to rapid temperature changes during the chemical strengthening step that is performed at a high temperature of 350 to 500°C.
[0095] The chemical strengthening step is Na + Glass containing K + When contacted with a salt containing ions, the surface Na + and K + Ion exchange proceeds inward, in this case Na among the ultra-thin glass structures. + K in the position occupied by + Ions enter, and Na + K is greater than the ionic radius of + Because the ionic radius is large, a compressive force may be generated around the mesh structure, which may strengthen the glass.
[0096] K by the above chemical strengthening + The depth at which ions are substituted is not particularly limited, but may be 5% to 40% of the cell thickness in terms of improving bending resistance, and specifically, it is preferably 10% to 35%, and more preferably 15% to 30%.
[0097] Additionally, the depth of chemical strengthening targeted may vary depending on the glass thickness, and for example, the depth (thickness) of chemical strengthening may vary depending on the glass thickness, as shown in Table 1 below.
[0098]
[0099]
[0100] The ion substitution solution used for the above chemical strengthening may be a commonly used ion substitution solution, and in one embodiment, may contain potassium nitrate (KNO3).
[0101] After the above chemical strengthening process, a slow cooling step and a process for removing impurities may be additionally performed. The slow cooling and impurity removal process may be any commonly used process. In one embodiment, after the process of naturally slow cooling through contact with the outside air, a washing process may be included to remove impurities, such as potassium nitrate.
[0102] The above chemical polishing step is to polish the ultra-thin glass using a chemical polishing solution, and the chemical polishing thickness may be such that, in terms of improving bending resistance, the thickness of the ultra-thin glass after chemical polishing is 80% or more and less than 100% of the thickness of the ultra-thin glass before chemical polishing, and preferably, it may be 90% or more and less than 100%.
[0103] The above chemical polishing solution is not particularly limited as long as it is one commonly used in a process of polishing ultra-thin glass, but may contain at least one of hydrofluoric acid (HF) and ammonium fluoride (NH4F).
[0104] Additionally, a cleaning step may be additionally performed after the chemical polishing step, if necessary.
[0105]
[0106] A hard coating film (130) is formed on the above glass substrate (110) via a first adhesive layer (120).
[0107] The above first adhesive layer (120) serves to attach the hard coating film (130) onto the glass substrate (110) and also serves to control the pencil hardness of the entire optical laminate.
[0108] The above first adhesive layer has a storage modulus of 10 MPa or more at 25°C and an adhesive strength of 600 gf / 25 mm or more at 25°C.
[0109] If the storage elastic modulus of the first adhesive layer at 25°C is less than 10 MPa, the pencil hardness of the entire optical laminate is less than H, so marks may remain when using a pen, and when applied to a flexible or foldable display, the adhesive layer may be damaged or lifted, causing a problem of wrinkles being formed.
[0110] If the adhesive strength of the first adhesive layer at 25°C is less than 600 gf / 25 mm, the adhesive strength is not secured, and the adhesive strength may not be maintained when the display is used in a harsh environment.
[0111] The first adhesive layer is formed from an adhesive composition including an acrylic random copolymer and an adhesive agent.
[0112] The above acrylic random copolymer may be polymerized by including 5 to 30 wt% of a first monomer having a glass transition temperature of a homopolymer of -40°C or lower, 60 to 90 wt% of a second monomer having a glass transition temperature of a homopolymer of 80°C or higher, and 3 to 20 wt% of a third monomer having at least one of a hydroxyl group and a carboxylic acid group in the molecule, in order to secure high elasticity properties.
[0113] The above acrylic random copolymer preferably has a glass transition temperature of 0°C or higher, and more preferably 0 to 25°C. In this case, there is an advantage in that the elasticity of the adhesive layer formed from the adhesive composition can be improved while also providing excellent adhesive properties.
[0114] If the glass transition temperature of the above acrylic random copolymer is less than 0°C, the elasticity is insufficient, so that the pencil hardness of the entire optical laminate is less than H, and thus marks may remain when using the pen.
[0115] Meanwhile, when the glass transition temperature of the acrylic random copolymer is 25°C or lower, the adhesive composition containing the acrylic random copolymer has excellent spreadability when applied to a substrate, and can exhibit even better effects in both elasticity and adhesiveness, which is preferable.
[0116]
[0117] Meanwhile, the acrylic random copolymer may have an acid value of 0.1 or less. If the acid value of the acrylic random copolymer exceeds 0.1, the tackifier described below acts as a crosslinking agent for each monomer included in the polymerization of the acrylic random copolymer and oligomers during the polymerization reaction, rather than improving the adhesiveness of the adhesive composition, thereby increasing the crosslinking degree of the copolymer, and thus may cause the adhesiveness of the adhesive layer to decrease.
[0118]
[0119] The first monomer having a glass transition temperature of -40°C or lower of the above homopolymer is not particularly limited, but may include, for example, at least one selected from the group consisting of n-butyl acrylate, t-butyl acrylate, sec-butyl acrylate, pentyl acrylate, 2-ethylbutyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl diglycol acrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, lauryl acrylate, and tetradecyl acrylate.
[0120] The first monomer may be included in an amount of 5 to 30 wt%, preferably 10 to 30 wt%, and more preferably 15 to 20 wt%, based on the total weight of monomers used in the polymerization of the acrylic random copolymer. If the first monomer is included in an amount of less than 5 wt% during the polymerization of the acrylic random copolymer, there is a problem that film formation occurs during curing of the adhesive composition, making it difficult to function as an adhesive layer. If the first monomer is included in an amount exceeding 30 wt%, there is a problem that the glass transition temperature of the copolymer becomes too low, making it difficult to exhibit high elasticity characteristics.
[0121]
[0122] In addition, the second monomer having a glass transition temperature of 80°C or higher of the homopolymer is not particularly limited, but may include, for example, at least one selected from the group consisting of (meth)acryloylmorpholine, N-vinylpyrrolidone, isobornyl(meth)acrylate, methacrylate, carbazole acrylate, dihydrodicyclopentadienyl acrylate, and potassium acrylate.
[0123] The second monomer may be included in an amount of 60 to 90 wt%, preferably 65 to 80 wt%, and more preferably 70 to 80 wt%, based on the total weight of monomers used in the polymerization of the acrylic random copolymer. If the second monomer is included in an amount of less than 60 wt% during the polymerization of the acrylic random copolymer, there is a problem that the glass transition temperature of the adhesive composition becomes too low, making it difficult to exhibit high elasticity characteristics, and if it is included in an amount exceeding 90 wt%, there is a problem that the adhesive composition forms a film during curing, making it difficult to function as an adhesive layer.
[0124]
[0125] In addition, the third monomer having at least one of a hydroxyl group and a carboxylic acid group in the molecule may include at least one selected from the group consisting of a (meth)acrylic monomer having a hydroxyl group in the molecule and a (meth)acrylic monomer having a carboxylic acid group in the molecule.
[0126] The (meth)acrylic monomer having the above hydroxyl group is not particularly limited, but may include, for example, at least one selected from the group consisting of 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxyethylene glycol (meth)acrylate, and 2-hydroxypropylene glycol (meth)acrylate.
[0127] The (meth)acrylic monomer having the above carboxylic acid group is not particularly limited, but may include, for example, at least one selected from the group consisting of (meth)acrylic acid, 2-(meth)acryloyloxyacetic acid, 3-(meth)acryloyloxypropyl acid, 4-(meth)acryloyloxybutyric acid, acrylic acid dimer, itaconic acid, maleic acid, and maleic anhydride.
[0128] The third monomer may be included in an amount of 3 to 20 wt%, preferably 4 to 15 wt%, and more preferably 5 to 10 wt%, based on the total weight of monomers used in the polymerization of the acrylic random copolymer. If the third monomer is included in an amount of less than 3 wt% during the polymerization of the acrylic random copolymer, the degree of crosslinking of the adhesive layer formed from the adhesive composition may be too low, resulting in problems of insufficient durability and adhesiveness. If the third monomer is included in an amount exceeding 20 wt%, the glass transition temperature of the copolymer may be too low, resulting in problems of difficulty in exhibiting high elasticity characteristics.
[0129]
[0130] The first monomer and the second monomer, and the third monomer may be distinct from each other, and the first monomer and the second monomer may not have a hydroxyl group and a carboxylic acid group in the molecule.
[0131]
[0132] The above acrylic random copolymer may further include other monomers commonly used in the technical field to which the present invention pertains, in addition to the above monomers, within a range that does not reduce elasticity and adhesiveness.
[0133] The above-mentioned acrylic random copolymer may have a weight average molecular weight (polystyrene equivalent; Mw) of 300,000 to 2,000,000 as measured by gel permeation chromatography (GPC), more preferably 500,000 to 1,200,000. When the weight average molecular weight of the acrylic random copolymer is less than 300,000, the chain structure within the structure of the adhesive sheet after ultraviolet polymerization and curing is simple and the length is short, which is disadvantageous in terms of reliability, such as the generation of bubbles, and a decrease in durability due to discoloration, etc. may occur. When the weight average molecular weight exceeds 2,000,000, the viscosity of the adhesive resin composition is too high during the manufacture of the adhesive film, so that a large amount of monomer dilution is required to adjust the appropriate viscosity required for manufacture, and accordingly, high energy may be required during ultraviolet polymerization and curing, or unreacted monomers may remain.
[0134] The method for producing the above-mentioned acrylic random copolymer is not particularly limited. For example, methods commonly used in the technical field to which the present invention pertains, such as bulk polymerization, solution polymerization, emulsion polymerization, suspension polymerization, and UV polymerization, may be used, and solution polymerization or UV polymerization may be preferably used.
[0135]
[0136] The above-mentioned adhesive agent may be included together with the acrylic random copolymer to improve the adhesiveness and tackiness of the adhesive layer formed from the adhesive composition.
[0137] The above-mentioned adhesive agent may have a weight average molecular weight of 1,000 or less. When an adhesive agent having a weight average molecular weight of 1,000 or less is used, uniform wettability and adhesive strength can be secured.
[0138] The above-mentioned adhesive agent is not particularly limited as long as it can improve the adhesiveness and / or tackiness of the adhesive layer formed from the adhesive composition, but may include, for example, at least one selected from the group consisting of isocyanate compounds, aziridine compounds, epoxy compounds, melamine compounds, peroxide compounds, metal chelate compounds, and oxazoline compounds.
[0139]
[0140] The above isocyanate compound may include at least one selected from the group consisting of diisocyanate compounds such as xylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and tetramethylxylene diisocyanate; addition polymers prepared by reacting 3 moles of diisocyanate compounds with 1 mole of a polyhydric alcohol compound such as trimethylolpropane; isocyanurate polymers prepared by self-condensation of 3 moles of diisocyanate compounds; biuret polymers prepared by condensing 1 mole of the remaining 1 mole of diisocyanate onto urea diisocyanate obtained from 2 moles of 3 moles of diisocyanate compounds; and polyfunctional isocyanate compounds containing three functional groups such as triphenylmethane triisocyanate and methylene bis triisocyanate.
[0141] The above aziridine compound may include at least one selected from the group consisting of pentaerythol-tris-(beta-(N-aziridinyl)propionate, trimethylolpropane-tris(beta-N-aziridinyl)propionate, trimethylolpropane tris(2-methyl-1-aziridinepropionate), N,N'-toluene-2,4-bis(1-aziridinecarboxamide), N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), triethylene melamine, bisisopropylaloyl-1-(2-methylaziridine), and tri-1-aziridinylphosphineoxide.
[0142] The above epoxy compound may include at least one selected from the group consisting of ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, and pentaerythritol polyglycidyl erythritol.
[0143] The above melamine-based compound may include at least one selected from the group consisting of hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexabutoxymethylmelamine, hexapentyloxymethylmelamine, and hexahexyloxymethylmelamine.
[0144] The above peroxide compound may include at least one selected from the group consisting of di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butylperoxyisobutyrate, and 1,1-di(t-hexylperoxy)cyclohexane.
[0145] The above metal chelate compound may be exemplified by a compound in which at least one ligand of a compound in which a polyvalent metal is covalently bonded or coordinated with an organic compound is substituted with an alkoxy group. The polyvalent metal may be one selected from the group consisting of titanium, zirconium, aluminum, zinc, iron, and tin, and is preferably one selected from the group consisting of titanium, zirconium, and aluminum. Examples of the atom in the organic compound forming the covalent or coordinated bond include an oxygen atom, and the organic compound may be one selected from the group consisting of an alkyl ester, an alcohol compound, a carboxylic acid compound, an ether compound, and a ketone compound.
[0146] The above oxazoline compound may include at least one selected from the group consisting of 2-isopropyl-2-oxazoline, 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline.
[0147]
[0148] The above tackifier may be included in an amount of 2 parts by weight or more, and preferably 2 to 20 parts by weight, based on 100 parts by weight of the acrylic random copolymer. When the tackifier satisfies the above content range, the adhesiveness and tackiness of the adhesive composition can be further improved.
[0149] If the above-mentioned adhesive agent is included in an amount of less than 2 parts by weight based on 100 parts by weight of the acrylic random copolymer, the adhesion and tackiness to the substrate may be reduced, and if it is included in an amount of more than 20 parts by weight, the elasticity may be reduced due to the remaining compound.
[0150]
[0151] In addition to the aforementioned components, the adhesive composition may further include additives to enhance coating properties, adhesion, etc., as required by those skilled in the art, within a range that does not impair the purpose of the present invention. For this purpose, the adhesive composition may further include components commonly used in the art, such as surfactants, silane coupling agents, antioxidants, ultraviolet absorbers, and / or anti-coagulants. These may be used singly, or two or more may be used in any combination and ratio.
[0152]
[0153] The thickness of the first adhesive layer (120) may be 5 to 80 μm. When the thickness of the first adhesive layer is within the above range, the adhesive strength is excellent and there are advantages in terms of light transmittance, reliability, and step absorption.
[0154]
[0155] The above hard coating film (130) serves as a protective film to prevent scattering of the glass substrate (110), and also serves to improve surface hardness.
[0156] In one embodiment of the present invention, the hard coating film (130) may include a base film (131) and a hard coating layer (132) formed on the base film (131).
[0157] The above-mentioned substrate film (131) is intended to support the hard coating layer and serves as a protective film to prevent the glass substrate (110) from scattering.
[0158] The above-mentioned substrate film is a transparent film, and any transparent polymer film can be used as the transparent film.
[0159] For example, the base film may be a film formed of a polymer such as triacetyl cellulose, acetyl cellulose butyrate, ethylene-vinyl acetate copolymer, propionyl cellulose, butyryl cellulose, acetyl propionyl cellulose, polyester, polystyrene, polyamide, polyetherimide, polyacrylic, polyimide, polyamideimide, polyethersulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyether ketone, polyether ether ketone, polyether sulfone, polymethyl methacrylate, polybutylene terephthalate, polyethylene naphthalate, or polycarbonate. These polymers may be used alone or in combination of two or more.
[0160] Preferably, the above-mentioned base film may be a film composed of one or more resins among polyester resin and polyamide-imide resin, and in particular, may be a film composed of polyester resin, in that it has excellent durability against repeated bending, making it easier to apply to a flexible display, and also ensuring pencil hardness.
[0161] The thickness of the above-mentioned substrate film is not particularly limited, but may be 5 to 100 μm, preferably 5 to 80 μm. If the thickness of the above-mentioned substrate is less than 5 μm, it may be difficult to ensure uniformity of thickness, making it difficult to secure reproducible physical properties. If the thickness exceeds 100 μm, the bending resistance may be reduced.
[0162]
[0163] The above hard coating layer (132) plays a role in improving surface hardness.
[0164] In addition, the hard coating layer (132) exhibits antifouling performance and excellent wear resistance, and has excellent elastic recovery rate, so it not only has excellent pen pressure suppression properties, but also can provide excellent effects in durability such as scratch resistance, chemical resistance, and bending resistance.
[0165] In one embodiment of the present invention, the hard coating layer can be formed from a hard coating composition including a light-transmitting resin, a fluorine-based UV-curable functional group-containing compound, a photoinitiator, and a solvent.
[0166] The above-mentioned transparent resin is a photocurable resin, and the photocurable resin may include, but is not limited to, a photocurable (meth)acrylate oligomer and / or monomer.
[0167] As the photocurable (meth)acrylate oligomer, epoxy (meth)acrylate, urethane (meth)acrylate, polyhedral oligomeric silsesquioxane (meth)acrylate, dendritic (meth)acrylate, etc. can be used, and at least one of urethane (meth)acrylate and dendritic (meth)acrylate is preferred.
[0168] The above urethane (meth)acrylate can be produced by reacting a (meth)acrylate having a hydroxy group in the molecule with a compound having an isocyanate group in the presence of a catalyst. Specific examples of the (meth)acrylate having a hydroxy group in the molecule include 2-hydroxyethyl (meth)acrylate, 2-hydroxyisopropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone ring-opening hydroxyacrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc. In addition, specific examples of compounds having the above isocyanate group include 1,4-diisocyanatobutane, 1,6-diisocyanatohexane, 1,8-diisocyanatooctane, 1,12-diisocyanatododecane, 1,5-diisocyanato-2-methylpentane, trimethyl-1,6-diisocyanatohexane, 1,3-bis(isocyanatomethyl)cyclohexane, trans-1,4-cyclohexenediisocyanate, 4,4'-methylenebis(cyclohexylisocyanate), isophoronediisocyanate, toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, xylene-1,4-diisocyanate, tetramethylxylene-1,3-diisocyanate, There are trifunctional isocyanates derived from 1-chloromethyl-2,4-diisocyanate, 4,4'-methylenebis(2,6-dimethylphenylisocyanate), 4,4'-oxybis(phenylisocyanate), hexamethylene diisocyanate, and trimethylolpropane adducttoluene diisocyanate.
[0169] The above dendritic (meth)acrylate refers to a (meth)acrylate oligomer having a dendritic structure, wherein the 'dendritic structure' refers to a shape in which monomers branch radially from one nucleus and polymerize, and spread radially. The dendritic (meth)acrylate can be used without being limited thereto as long as it corresponds to the form described above.
[0170] Commercially available products of the above dendritic (meth)acrylate include Miramer SP1106 from Miwon, Viscoat 1000, Viscoat 1020, and Viscoat 1080 from Osaka Yuki.
[0171] The above monomer can be used without limitation as a conventional monomer, and a monomer having an unsaturated group such as a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group in the molecule as a photocurable functional group is preferable, and among these, a monomer having a (meth)acryloyl group is preferable.
[0172] Specific examples of the monomer having the above (meth)acryloyl group include neopentyl glycol acrylate, 1,6-hexanediol di(meth)acrylate, propylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, 1,2,4-cyclohexane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, isooctyl(meth)acrylate, isodexyl(meth)acrylate, stearyl(meth)acrylate, At least one may be selected from the group consisting of tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, and isoborneol (meth)acrylate.
[0173] The photocurable (meth)acrylate oligomers and monomers exemplified above may be used alone or in combination of two or more.
[0174] The above-mentioned light-transmitting resin may be included in an amount of 1 to 80 wt% based on 100 wt% of the total hard coating composition. If the content of the light-transmitting resin is less than 1 wt%, it is difficult to achieve sufficient hardness improvement, and if it exceeds 80 wt%, curling becomes severe.
[0175]
[0176] The above fluorine-based UV-curable functional group-containing compound is a component that provides antifouling properties, wear resistance, and chemical resistance. The above fluorine-based UV-curable functional group-containing compound is not particularly limited as long as it contains fluorine and has a UV-curable functional group that can chemically bond with the light-transmitting resin forming the matrix of the hard coating layer.
[0177] The above fluorine-based UV-curable functional group-containing compound may be at least one selected from the group consisting of a (meth)acrylate containing a perfluoroalkyl group, a (meth)acrylate containing a perfluoropolyether group, a (meth)acrylate containing a perfluorocyclic aliphatic group, and a (meth)acrylate containing a perfluoroaromatic group. In this case, it is preferable because it exhibits excellent antifouling performance and has the advantage of excellent durability in that it forms a chemical bond with the hard coating layer to maintain the antifouling performance for a long time even after repeated use.
[0178] It is preferable that the above fluorine-based UV-curable functional group-containing compound has 1 to 6 UV-curable functional groups.
[0179] Examples of the above fluorine-based UV-curable functional group-containing compounds include 2,2,2-trifluoroethyl acrylate, 2,2,3,3,3-pentafluoropropyl acrylate, 2-perfluorobutyl ethyl acrylate, 3-perfluorobutyl-2-hydroxypropyl acrylate, 2-perfluorohexyl ethyl acrylate, 3-perfluorohexyl-2-hydroxypropyl acrylate, 2-perfluorooctyl ethyl acrylate, 3-perfluorooctyl-2-hydroxypropyl acrylate, 2-perfluorodecyl ethyl acrylate, 2-perfluoro-3-methylbutyl ethyl acrylate, 3-perfluoro-3-methoxybutyl-2-hydroxypropyl acrylate, 2-perfluoro-5-methylhexyl ethyl acrylate, 3-Perfluoro-5-methylhexyl-2-hydroxypropyl acrylate, 2-perfluoro-7-methyloctyl-2-hydroxypropyl acrylate, tetrafluoropropyl acrylate, octafluoropentylacrylate, dodecafluoroheptylacrylate, hexadecafluorononylacrylate, hexafluorobutylacrylate, 2,2,2-trifluoroethyl methacrylate, 2,2,3,3,3-pentafluoropropyl methacrylate, 2-perfluorobutylethyl methacrylate, 3-perfluorobutyl-2-hydroxypropyl methacrylate, 2-perfluorooctylethyl methacrylate, 3-perfluorooctyl-2-hydroxypropyl methacrylate, 2-perfluorodecylethyl methacrylate, 2-perfluoro-3-methylbutylethyl methacrylate, Examples thereof include 3-perfluoro-3-methylbutyl-2-hydroxypropyl methacrylate, 2-perfluoro-5-methylhexylethyl methacrylate, 3-perfluoro-5-methylhexyl-2-hydroxypropyl methacrylate, 2-perfluoro-7-methyloctylethyl methacrylate, 3-perfluoro-6-methyloctyl methacrylate, tetrafluoropropyl methacrylate, octafluoropentyl methacrylate, octafluoropentyl methacrylate, dodecafluoroheptyl methacrylate, hexadecafluorononyl methacrylate, 1-trifluoromethyltrifluoroethyl methacrylate, hexafluorobutyl methacrylate, and triacryloyl-heptadecafluorononenyl-pentaerythritol.
[0180] Commercial examples of the above fluorine-based UV-curable functional group-containing compound include KY-1203 (Shin-Etsu Silicone Co., Ltd.), OPTOOL DAC-HP (Daikin Co., Ltd.), and UVAS-2003 (Suyang Chemtech).
[0181] The above fluorine-based UV-curable functional group-containing compound may be included in an amount of more than 0.01 wt% and less than 10 wt% based on 100 wt% of the total hard coating composition. When the fluorine-based UV-curable functional group-containing compound is included within the above range, it is preferable because it can provide excellent wear resistance and antifouling effects. When the content of the fluorine-based UV-curable functional group-containing compound is less than the above range, it may be difficult to sufficiently achieve wear resistance or antifouling properties, and when it exceeds the above range, hardness and / or scratch resistance characteristics may deteriorate.
[0182]
[0183] In one embodiment of the present invention, the photoinitiator is included to induce photocuring of the hard coating composition, and may include, for example, a photoradical initiator capable of forming radicals upon light irradiation.
[0184] Examples of the above photoinitiators include Type 1 initiators that generate radicals by decomposition of molecules due to differences in chemical structure or molecular bond energy, and Type 2 initiators that coexist with tertiary amines to induce hydrogen recapture.
[0185] For example, the Type 1 initiator may include acetophenones such as 4-phenoxydichloroacetophenone, 4-t-butyldichloroacetophenone, 4-t-butyltrichloroacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-l-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexylphenyl ketone; benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzyl dimethyl ketal; phosphine oxides; titanocene compounds, and the like.
[0186] For example, Type 2 initiators include benzophenones such as benzophenone, benzoylbenzoic acid, benzoylbenzoic acid methyl ether, 4-phenylbenzophenone, hydroxybenzophenone, 4-benzol-4'-methyldiphenylsulfide, and 3,3'-methyl-4-methoxybenzophenone; and thioxanthones such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, and isopropylthioxanthone.
[0187] The above-described photoinitiators may be used alone or in combination of two or more. In addition, the Type 1 and Type 2 initiators may be used alone or in combination.
[0188] The photoinitiator may be included in an amount of about 0.1 to 10 wt%, preferably about 1 to 5 wt%, based on 100 wt% of the total hard coating composition. If the content of the photoinitiator is less than 0.1 wt%, sufficient curing may not occur, and thus the mechanical properties and adhesiveness of the hard coating film or hard coating layer may not be secured. If the content of the photoinitiator exceeds 10 wt%, poor adhesion, cracking, and curling may occur due to curing shrinkage.
[0189]
[0190] The above solvent may be used without limitation as long as it is known in the art to be capable of dissolving or dispersing the composition mentioned above. In addition, the solvent simultaneously plays a role in providing time for the fluorine-based UV-curable functional group-containing compound to float to the outermost surface of the coating layer due to the difference in surface tension during the process of applying and drying the hard coating composition to a substrate.
[0191] Available solvents include alcohols (methanol, ethanol, isopropanol, butanol, methyl cellusob, ethylsolusob, etc.), ketones (methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, diethyl ketone, dipropyl ketone, cyclohexanone, etc.), acetates (ethyl acetate, propyl acetate, n-butyl acetate, t-butyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, methoxybutyl acetate, methoxypentyl acetate, etc.), hexane-based solvents (hexane, heptane, octane, etc.), benzene-based solvents (benzene, toluene, xylene, etc.), ether-based solvents (diethylene glycol dimethyl ether, diethylene glycol diethyl ether, Diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, etc.) can be preferably used. The solvents exemplified above can be used alone or in combination of two or more.
[0192] Preferably, a solvent consisting solely of a good solvent or a mixed solvent comprising a good solvent and a poor solvent is used. The good solvent and poor solvent can be appropriately selected depending on the material of the transparent film used as the base film.
[0193] The above solvent may be included in an amount of 10 to 95 wt% based on 100 wt% of the total hard coating composition. If the content of the solvent is less than the above content, the viscosity is high, which reduces workability and makes it difficult to sufficiently promote swelling of the substrate. Conversely, if the content exceeds the above range, the drying process takes a long time and is less economical, and the swelling of the substrate film may be severe, resulting in the occurrence of haze. Therefore, it is appropriately used within the above range.
[0194]
[0195] The above hard coating composition may further include inorganic particles.
[0196] The above inorganic particles may be inorganic nanoparticles and are a component added to improve the elastic recovery rate of the hard coating layer.
[0197] Specifically, the inclusion of the inorganic nanoparticles in the hard coating composition has the advantage of further improving mechanical properties. More specifically, the inorganic nanoparticles are uniformly distributed within the coating film, thereby improving mechanical properties such as pen pressure and pencil hardness.
[0198] The above-mentioned inorganic nanoparticles may be used having an average particle diameter of 1 to 100 nm, specifically 1 to 80 nm, and more specifically 5 to 50 nm. When the average particle diameter of the above-mentioned inorganic nanoparticles satisfies the above range, there is an advantage in that a uniform coating can be formed by preventing agglomeration within the composition. In addition, the problem of deterioration of the optical characteristics and mechanical properties of the coating can be prevented.
[0199] The above inorganic nanoparticles may include metal oxides commonly used in the art. For example, the above inorganic nanoparticles may include at least one selected from the group consisting of Al2O3, SiO2, ZnO, ZrO2, BaTiO3, TiO2, Ta2O5, Ti3O5, ITO, IZO, ATO, ZnO-Al, Nb2O3, SnO, and MgO, but are not limited thereto.
[0200] Specifically, the inorganic nanoparticles may be Al2O3, SiO2, and / or ZrO2. The inorganic nanoparticles may be manufactured directly or purchased commercially. In the case of commercially available products, the inorganic nanoparticles may be dispersed in an organic solvent at a concentration of 10 to 80 wt%.
[0201]
[0202] The above hard coating composition may further include a leveling agent to provide smoothness and coatability to the coating film when coating the composition.
[0203] Leveling agents can be selected from commercially available silicone type leveling agents, fluorine type leveling agents, and acrylic polymer type leveling agents, for example, BYK Chemie's BYK-323, BYK-331, BYK-333, BYK-337, BYK-373, BYK-375, BYK-377, BYK-378, Daegu Chemical's TEGO Glide 410, TEGO Glide 411, TEGO Glide 415, TEGOGlide 420, TEGO Glide 432, TEGO Glide 435, TEGO Glide 440, TEGO Glide 450, TEGO Glide 455, TEGO Rad 2100, TEGO Rad 2200N, TEGO Rad 2250, TEGO Rad 2300, TEGO Rad 2500, 3M's FC-4430, FC-4432, etc. can be used. The leveling agent can be included in the range of 0.1 to 1 wt% based on 100 wt% of the total hard coating composition.
[0204]
[0205] In addition to the above-described components, the above-described hard coating composition may additionally include components commonly used in the relevant technical field, such as ultraviolet stabilizers, heat stabilizers, antioxidants, lubricants, and antifouling agents.
[0206] The above UV stabilizer is an additive added to protect the coating film by blocking or absorbing UV rays, as the surface of the cured coating film decomposes due to continuous exposure to UV rays, causing discoloration and crumbling. The above UV stabilizer is classified into an absorbent, a quencher, and a hindered amine light stabilizer (HALS) according to its mechanism of action. In addition, it can be classified into a phenyl salicylate (absorbent), a benzophenone (absorbent), a benzotriazole (absorbent), a nickel derivative (quencher), and a radical scavenger according to its chemical structure. The above UV stabilizer is not particularly limited as long as it does not significantly change the initial color of the coating film.
[0207] In addition, the heat stabilizer is a commercially applicable product, and the primary heat stabilizer, polyphenol-based, and the secondary heat stabilizers, phosphite-based and lactone-based, can be used alone or in combination.
[0208] The above UV stabilizer and heat stabilizer can be used by appropriately adjusting the content at a level that does not affect UV curability.
[0209]
[0210] The above hard coating layer can be formed by applying the above hard coating composition to one surface of the base film, drying it, and then UV curing it.
[0211] The above hard coating composition can be applied to a substrate (coating process) by appropriately using a known method such as a die coater, air knife, reverse roll, spray, blade, casting, gravure, micro gravure, or spin coating.
[0212] After applying the above hard coating composition to the base film, the composition is dried by evaporating the volatile matter at a temperature of 30 to 150°C for 10 seconds to 1 hour, more specifically for 30 seconds to 30 minutes, and then cured by irradiation with UV light. The irradiation dose of the UV light may be specifically about 0.01 to 10 J / cm2, and more specifically, may be 0.1 to 2 J / cm2.
[0213] At this time, the thickness of the hard coating layer formed may be specifically 1 to 50 μm, more specifically 3 to 20 μm. When the thickness of the hard coating layer is within the above range, excellent hardness and bending resistance can be obtained.
[0214]
[0215] In addition, referring to FIG. 2, the optical laminate according to one embodiment of the present invention may further include a substrate film (150) laminated via a second adhesive layer (140) on the opposite side of the surface facing the first adhesive layer (120) of the glass substrate (110).
[0216] The above second adhesive layer (140) serves to attach the substrate film (150) onto the glass substrate (110).
[0217] The physical properties, components, thickness, etc. of the second adhesive layer (140) may be the same as those of the first adhesive layer (120) described above.
[0218] The above-mentioned substrate film (150) serves as a protective film to prevent the glass substrate (110) from scattering, etc.
[0219] The material and thickness of the above-described base film (150) may be the same as the base film (131) used in the above-described hard coating film (130).
[0220]
[0221] One embodiment of the present invention relates to an image display device comprising the optical laminate described above. For example, the optical laminate of the present invention can be used as a window for an image display device, particularly a flexible display, a foldable display, a rollable display, or a stretchable display. Furthermore, the optical laminate of the present invention can be used by attaching it to a polarizing plate, a touch sensor, or the like.
[0222] The optical laminate according to one embodiment of the present invention can be used in various types of LCDs, such as reflective, transmissive, and semi-transmissive LCDs, or LCDs of various drive methods, such as TN, STN, OCB, HAN, VA, and IPS. In addition, the optical laminate according to one embodiment of the present invention can be used in various types of image display devices, such as plasma displays, field emission displays, organic EL displays, inorganic EL displays, and electronic paper.
[0223]
[0224] Hereinafter, the present invention will be described in more detail through examples, comparative examples, and experimental examples. These examples, comparative examples, and experimental examples are intended solely to illustrate the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited thereto.
[0225]
[0226] Synthesis Example 1: Synthesis of an acrylic random copolymer
[0227] Synthesis Example 1-1
[0228] A monomer mixture containing 20 wt% of 2-ethylhexyl acrylate (2-EHA; first monomer), 60 wt% of isobornyl acrylate (IBOA; second monomer), 10 wt% of dihydrodicyclopentadienyl acrylate (DCPA; second monomer), and 10 wt% of 2-hydroxyethyl acrylate (2-HEA; third monomer) was added to a 1 L reactor to adjust the solid content to 20 wt%, and ethyl acetate (EA) was added as a solvent.
[0229] Nitrogen gas was purged for 1 hour to remove oxygen, and the temperature was maintained at 80°C. After the monomer mixture was uniformly mixed, azobisisobutyronitrile (AIBN) was added as a reaction initiator in an amount of 0.07 parts by weight per 100 parts by weight of the monomer mixture, and the mixture was reacted for 8 hours to produce an acrylic random copolymer (weight average molecular weight: 650,000, PDI 4.5).
[0230] The weight average molecular weight, glass transition temperature (DSC2500, TA Instruments Inc.) and acid value of the obtained acrylic random copolymer are shown in Table 2 below.
[0231]
[0232] Synthesis examples 1-2 to 1-4
[0233] In the above Synthesis Example 1-1, an acrylic random copolymer was prepared in the same manner as above, except that the first monomer, the second monomer, and the third monomer were prepared in the composition and content shown in Table 2 below.
[0234] 1st monomer system 2nd monomer system 3rd monomer molecular weight (Mw) glass transition temperature (℃) acid value 2-EHABAIBOADCPA2-HEA4-HBAAA Synthesis example 1-120-60 1010--650,000 23.10.0 15 Synthesis example 1-2-2070--10-890,000 23.70.0 1 Synthesis example 1-340-40 1010--1,140,000 34.20.0 4 Synthesis example 1-420-50 1019.5-0.5 1010,000 3.32.1
[0235]
[0236] 2-EHA: 2-ethylhexylacrylate (Tg of homopolymer: -70℃; Sigma-Aldrich)
[0237] BA: n-butylacrylate (Tg of homopolymer: -54℃; Sigma-Aldrich)
[0238] IBOA: Isobornyl acrylate (Tg of homopolymer: 94℃; Sigma-Aldrich)
[0239] DCPA: dihydrodicyclopentadienyl acrylate (Tg of homopolymer: 110℃; BASF)
[0240] 2-HEA: 2-hydroxyethyl acrylate (Tg of homopolymer: -15℃; Sigma-Aldrich)
[0241] 4-HBA: 4-hydroxybutylacrylate (Tg of homopolymer: -40℃; Sigma-Aldrich)
[0242] AA: Acrylic acid (Tg of homopolymer: 105℃; Sigma-Aldrich)
[0243]
[0244] Manufacturing Example 1: Manufacturing of an adhesive layer
[0245] Manufacturing Example 1-1
[0246] An adhesive composition was prepared by mixing 100 parts by weight of the acrylic random copolymer synthesized in Synthesis Example 1-1, 5 parts by weight of an isocyanate compound (D-110N, Mitsui Chemicals) as a tackifier, and 0.1 part by weight of a silane coupling agent (KBM-403, Shin-Etsu), and then applying the composition to a thickness of 5 μm on a 75 μm release film coated with a silicone release agent, and drying at 120°C for 5 minutes to prepare an adhesive layer. In order to protect the adhesive layer before use in a subsequent process, a release film coated with a silicone release agent was laminated on the adhesive layer to prepare an adhesive sheet.
[0247]
[0248] Manufacturing Examples 1-2 to 1-4
[0249] In the above Manufacturing Example 1-1, an adhesive layer was manufactured in the same manner as above, except that the acrylic random copolymer and the adhesive agent were used in the composition and content shown in Table 3 below.
[0250] (Weight) Acrylic random copolymer adhesive agent silane coupling agent Manufacturing example 1-1 Synthesis example 1-1 100A50.1 Manufacturing example 1-2 Synthesis example 1-2 100B150.1 Manufacturing example 1-3 Synthesis example 1-3 100B100.1 Manufacturing example 1-4 Synthesis example 1-4 100B100.1
[0251]
[0252] A: D-110N (TMP(Trimethylolpropane)-XDI(Xylene diisocyanate) addition polymer, Mitsui Chemicals; isocyanate compound)
[0253] B: CL-467 (trimethylolpropane tris(2-methyl-1-aziridinepropionate), menadione; aziridine compound)
[0254] Silane coupling agent: KBM-403 (3-glycidoxypropyltrimethoxysilane, Shin-Etsu)
[0255]
[0256] Experimental Example 1:
[0257] The physical properties of the adhesive layers manufactured in Manufacturing Examples 1-1 to 1-4 were measured by the following method, and the results are shown in Table 4 below.
[0258]
[0259] (1) Storage modulus
[0260] For each adhesive layer, the storage modulus at 25°C was measured using a viscoelasticity measuring device (MCR-301, Anton Paar). More specifically, the adhesive sheet was cut to a size of 30 mm in length × 30 mm in width, the release film attached to one side of the cut adhesive sheet was removed, and then it was bonded to a glass substrate. Then, while in contact with the measuring tip, the sheet was measured under the conditions of a frequency of 1.0 Hz, a strain of 2%, and a heating rate of 5°C / min in a temperature range of -20 to 100°C, and the measured value at 25°C was read. The storage modulus was evaluated according to the following evaluation criteria.
[0261] <Evaluation Criteria>
[0262] ◎: Storage modulus of 50 MPa or more at 25℃
[0263] ○: Storage elastic modulus at 25℃ 10MPa or more but less than 50MPa
[0264] △: Storage elastic modulus at 25℃ 8MPa or more but less than 10MPa
[0265] ×: Storage modulus at 25℃ less than 8 MPa
[0266]
[0267] (2) Adhesion
[0268] The manufactured adhesive sheet was cut to a size of 25 mm × 85 mm, the release film was peeled off, the adhesive surface was corona-treated, laminated to a glass substrate, and autoclaved to produce a specimen. The room temperature adhesive strength was measured by leaving the manufactured specimen under the conditions of 23°C and 50% RH for 24 hours, and then peeling the adhesive layer using a universal tensile tester (UTM, Instron) at a peel speed of 300 mm / min and a peel angle of 180°. The adhesive strength was evaluated according to the following evaluation criteria.
[0269] <Evaluation Criteria>
[0270] ○: 1000gf / 25mm or more
[0271] △: 600gf / 25mm or more and less than 1000gf / 25mm
[0272] ×: Less than 600gf / 25mm
[0273]
[0274] Storage elastic modulus Adhesive strength Manufacturing example 1-1○○ Manufacturing example 1-2◎○ Manufacturing example 1-3×○ Manufacturing example 1-4△×
[0275]
[0276] Manufacturing Example 2: Manufacturing of hard coating film
[0277] Manufacturing Example 2-1
[0278] 23 parts by weight of 6-functional urethane acrylate (Kongyoungsa, UA-306I), 23 parts by weight of dendritic acrylate (Miwon Specialty Chemical, Miramer SP1106), 50 parts by weight of methyl ethyl ketone, 3.5 parts by weight of 1-hydroxycyclohexyl phenyl ketone, and 0.5 parts by weight of a fluorine-based UV-curable functional group-containing compound (Shin-Etsu Silicone, KY-1203) were mixed using a stirrer and filtered using a PP material filter to prepare a hard coating composition.
[0279] The above hard coating composition was coated on a polyethylene terephthalate film (PET, 50㎛) to a thickness of 7㎛ after curing, and the solvent was dried. Then, a UV accumulated light dose of 600 mJ / cm2 was irradiated under a nitrogen atmosphere to manufacture a hard coating film.
[0280]
[0281] Manufacturing Example 2-2
[0282] In the above manufacturing example 2-1, a hard coating film was manufactured using the same method as above, except that a polyamideimide film (PAI, 50 μm) was used instead of the polyethylene terephthalate film (PET, 50 μm).
[0283]
[0284] Example: Fabrication of optical laminates
[0285] Example 1
[0286] The adhesive sheet of Manufacturing Example 1-1 and the hard coating film of Manufacturing Example 2-1 were prepared. Ultra-thin glass having a thickness of 90 μm was prepared.
[0287] The release film attached to one side of the adhesive sheet was peeled off, the surface of the adhesive layer was subjected to corona treatment, and the substrate film side of the hard coating film (the side opposite the HC layer) was also subjected to corona treatment, and these were laminated to produce an intermediate laminate. Next, the remaining release film of the intermediate laminate was peeled off, the surface of the adhesive layer was subjected to corona treatment, and the surface of the ultra-thin glass was also subjected to corona treatment on the other side, and these were laminated. Finally, autoclave treatment was performed to produce the final optical laminate.
[0288]
[0289] Examples 2 to 6 and Comparative Examples 1 to 3
[0290] An optical laminate was manufactured in the same manner as described in Table 5, except that the adhesive sheet, hard coating film, and ultra-thin glass were used.
[0291] Classification Hard coating film First adhesive layer Thickness of ultra-thin glass (㎛) Second adhesive layer Base film type Base film type 25℃ Elasticity modulus Example 1 Manufacturing example 2-1 PET Manufacturing example 1-1○90 -- Example 2 Manufacturing example 2-2 PAI Manufacturing example 1-1○90 -- Example 3 Manufacturing example 2-1 PET Manufacturing example 1-1○30 -- Example 4 Manufacturing example 2-1 PET Manufacturing example 1-2◎90 -- Example 5 Manufacturing example 2-2 PAI Manufacturing example 1-2◎90 -- Example 6 Manufacturing example 2-1 PET Manufacturing example 1-2◎90 Manufacturing example 1-2 PET Comparative example 1 Manufacturing example 2-1 PET Manufacturing example 1-3×90 -- Comparative example 2 Manufacturing example 2-1PET Manufacturing Example 1-4△90--Comparative Example 3 Manufacturing Example 2-1PET Manufacturing Example 1-1○100--
[0292]
[0293] Experimental Example 2:
[0294] The physical properties of the optical laminates manufactured in the above examples and comparative examples were measured using the method described below, and the results are shown in Table 6 below.
[0295]
[0296] (1) Pencil hardness
[0297] After fixing the optical laminate so that the hard coating layer side faces upward, the pencil hardness was measured under a load of 750 gf. The test was performed five times with a 2 cm length using a pencil of the same hardness, and the hardness that was OK four or more times was designated as the pencil hardness.
[0298]
[0299] (2) Flexibility
[0300] The optical laminate was evaluated by mandrel with a radius of curvature of 4 mm so that the hard coating layer surface was folded inward, and the presence or absence of fracture was observed. The bending resistance was evaluated according to the following evaluation criteria.
[0301] <Evaluation Criteria>
[0302] ○: No breakage of optical laminate
[0303] X: Occurrence of optical laminate fracture
[0304]
[0305] Classification Pencil Hardness Flexibility Example 1H ○ Example 22H ○ Example 3H ○ Example 43H ○ Example 54H ○ Example 63H ○ Comparative Example 12B ○ Comparative Example 2F ○ Comparative Example 32H ×
[0306]
[0307] As shown in Table 6 above, it was confirmed that the optical laminates of Examples 1 to 6, in which a hard coating film is bonded to an ultra-thin glass having a thickness of less than 100 ㎛ according to the present invention via an adhesive layer having a storage modulus at 25°C of 10 MPa or more and an adhesive strength at 25°C of 600 gf / 25 mm or more, can secure bending resistance while having excellent pencil hardness characteristics.
[0308] On the other hand, it was found that the optical laminates of Comparative Examples 1 to 3, in which the thickness of the ultra-thin glass was 100 ㎛ or more or the storage elastic modulus of the adhesive layer was outside the above range, could not simultaneously secure pencil hardness characteristics and bending resistance.
[0309]
[0310] While specific aspects of the present invention have been described in detail above, it should be apparent to those skilled in the art that these specific descriptions are merely preferred embodiments and do not limit the scope of the present invention. Those skilled in the art will be able to make various applications and modifications within the scope of the present invention based on the above description.
[0311] Accordingly, the substantial scope of the present invention will be defined by the appended claims and their equivalents.
[0312] [Explanation of symbols]
[0313] 110: Glass substrate 120: First adhesive layer
[0314] 130: Hard coating film 131: Base film
[0315] 132: Hard coating layer 140: Second adhesive layer
[0316] 150: Base film
Claims
1. Glass substrate, A first adhesive layer formed on one surface of the glass substrate, and An optical laminate comprising a hard coating film formed on the first adhesive layer, The above first adhesive layer has a storage modulus of 10 MPa or more at 25°C and an adhesive strength of 600 gf / 25 mm or more at 25°C, The above glass substrate is an ultra-thin glass having a thickness of less than 100 ㎛, An optical laminate having a pencil hardness of H or higher throughout the entire optical laminate.
2. An optical laminate according to claim 1, wherein the first adhesive layer is formed from an adhesive composition comprising an acrylic random copolymer and a tackifier, and the acrylic random copolymer is polymerized by including 5 to 30 wt% of a first monomer having a glass transition temperature of a homopolymer of -40°C or lower, 60 to 90 wt% of a second monomer having a glass transition temperature of a homopolymer of 80°C or higher, and 3 to 20 wt% of a third monomer having at least one of a hydroxyl group and a carboxylic acid group in the molecule.
3. An optical laminate according to claim 2, wherein the acrylic random copolymer has a glass transition temperature of 0°C or higher.
4. An optical laminate according to claim 2, wherein the acrylic random copolymer has an acid value of 0.1 or less.
5. An optical laminate in the second paragraph, wherein the adhesive agent comprises at least one selected from the group consisting of isocyanate compounds, aziridine compounds, epoxy compounds, melamine compounds, peroxide compounds, metal chelate compounds, and oxazoline compounds.
6. In the first paragraph, the hard coating film is an optical laminate including a base film and a hard coating layer formed on the base film.
7. An optical laminate in the 6th paragraph, wherein the base film is a film composed of at least one resin among polyester resin and polyamideimide resin.
8. In the sixth paragraph, the hard coating layer is an optical laminate formed from a hard coating composition containing a light-transmitting resin, a fluorine-based UV-curable functional group-containing compound, a photoinitiator, and a solvent.
9. In paragraph 1, A second adhesive layer formed on the other side of the glass substrate, and An optical laminate further comprising a substrate film formed on the second adhesive layer.
10. An image display device having an optical laminate according to any one of claims 1 to 9.
11. A window of a flexible display device having an optical laminate according to any one of claims 1 to 9.
12. A polarizing plate having an optical laminate according to any one of claims 1 to 9.
13. A touch sensor having an optical laminate according to any one of claims 1 to 9.
Citation Information
Patent Citations
Laminate and display device
JP2022074108A
Optical Laminate and Flexible Display Comprising the Same
KR101903888B1
Laminate
KR1020170093623A
Pressure-sensitive adhesive tape, laminate, and image display device
WO2011007861A1
Display device member, optical laminate, and display device
WO2021177288A1