Separator for secondary battery, and secondary battery comprising same

The use of a separator with an inorganic layer and a specific adhesive layer composition addresses the interface resistance issues in lithium batteries, enhancing their capacity, lifespan, and safety by maintaining strong adhesion and stable performance.

WO2024205129A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003562
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium batteries face challenges in achieving high discharge capacity, energy density, and cycle characteristics due to increased interface resistance between electrodes and separators during the rolling process, leading to deteriorated capacity and safety issues over cycles.

Method used

A separator with an improved adhesive layer, comprising a porous substrate, an inorganic layer, and an adhesive layer containing first and second organic binder particles with specific size ratios, enhancing adhesion and reducing interface resistance.

Benefits of technology

The solution results in lithium batteries with improved capacity, lifespan, and safety by maintaining strong adhesion between electrodes and the separator, suppressing volume changes during charging and discharging, and maintaining stable cell performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003562_03102024_PF_FP_ABST
    Figure KR2024003562_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a separator for a secondary battery, and a secondary battery comprising same, the separator comprising a porous substrate, an inorganic layer positioned on at least one surface of the porous substrate, and an adhesive layer positioned on the inorganic layer, wherein the adhesive layer contains first particles and second particles which are an organic binder of different particle sizes, and the mixing volume ratio of the first particles and the second particles is 1:5 to 1:35.
Need to check novelty before this filing date? Find Prior Art

Description

Separator for secondary batteries and secondary batteries containing the same

[0001] It relates to a separator for a secondary battery and a secondary battery including the same.

[0002] To meet the miniaturization and high-performance demands of various devices, miniaturization and lightweight lithium batteries are becoming increasingly important. Furthermore, for applications in fields such as electric vehicles, the discharge capacity, energy density, and cycle characteristics of lithium batteries are becoming increasingly important. To meet these needs, lithium batteries with high discharge capacity per unit volume, high energy density, and high capacity, along with excellent cycle life and safety, are in demand.

[0003] In a lithium battery, a separator is placed between the positive electrode and the negative electrode to prevent short circuits. An electrode assembly including a positive electrode, a negative electrode, and a separator placed between the positive electrode and the negative electrode is rolled into a jelly roll shape, and the jelly roll is rolled to improve the adhesion between the positive electrode / negative electrode and the separator in the electrode assembly. During this rolling process, the interfacial resistance between the positive electrode and the separator, and the negative electrode and the separator increases, and as the charge / discharge cycle of the lithium battery is repeated, the capacity and high-rate charge / discharge characteristics may deteriorate.

[0004] Therefore, in order to manufacture lithium batteries with high capacity, excellent lifespan characteristics, and safety, a separator with improved adhesion and safety is required.

[0005] One aspect is to provide a separator for secondary batteries with improved adhesion and safety.

[0006] Another aspect is to provide a secondary battery having excellent capacity and lifespan characteristics and improved safety, including the above-described separator.

[0007] According to one aspect,

[0008] A porous substrate, comprising an inorganic layer positioned on at least one surface of the porous substrate, and an adhesive layer positioned on the inorganic layer,

[0009] The above adhesive layer contains first and second particles which are organic binders having different particle sizes,

[0010] A secondary battery separator is provided in which the mixing volume ratio of the first and second particles is 1:5 to 1:35.

[0011] According to another aspect, a secondary battery is provided, which includes a positive electrode, a negative electrode, and a separator interposed therebetween and described above.

[0012] A secondary battery separator according to one embodiment of the present invention contains an adhesive layer with improved adhesive strength, thereby exhibiting good air permeability and excellent adhesion between the separator and electrodes after charge and discharge, thereby preventing deformation of the battery. Therefore, its use can provide a secondary battery with improved capacity, lifespan, and safety.

[0013] Figure 1 is a schematic diagram showing a cross-section of a separator of a lithium battery according to an embodiment.

[0014] Figure 2 is a schematic diagram showing a cross-section of a separator of a lithium battery according to another embodiment.

[0015] Figure 3 is a schematic diagram showing a cross-section of a separator of a lithium battery according to another embodiment.

[0016] Figure 4 is a schematic diagram of a lithium battery according to an embodiment.

[0017] <Brief explanation of the main symbols in the drawing>

[0018] 10: Separator 20: Porous substrate

[0019] 30: Inorganic layer 40: Adhesive layer

[0020] 140: positive pole 150: negative pole

[0021] 160: Electrode assembly 170: Case

[0022] Hereinafter, a secondary battery separator and a secondary battery including the same according to exemplary implementation examples will be described in more detail.

[0023] Lithium secondary batteries typically have a separator positioned between the positive and negative electrodes, and then undergo a hot press process at a specific temperature and pressure. This hot press process increases the adhesive strength between the positive and negative electrode / separator interfaces, thereby maintaining the battery's shape. However, if this adhesive strength is insufficient, the interface between the electrodes becomes loose, which fundamentally causes a continuous decrease in capacity over the cycle of lithium polymer batteries and deteriorates high-rate charge and discharge characteristics. Furthermore, this also compromises battery safety, necessitating improvements.

[0024] Accordingly, the inventors of the present invention have provided a porous substrate comprising: a porous substrate; an inorganic layer positioned on at least one surface of the porous substrate; and an adhesive layer positioned on the inorganic layer.

[0025] The invention has been completed for a secondary battery separator, wherein the adhesive layer contains first and second particles, which are organic binders with different particle sizes, and the volume ratio of the first and second particles is 1:5 to 1:35.

[0026] According to an embodiment, the adhesive layer provides a separator with improved adhesion to an inorganic layer by using two types of organic binders with different particle sizes, thereby more strongly controlling the bonding force between an electrode and a separator, thereby manufacturing a lithium secondary battery having stable cell performance without abnormal behavior such as cell swelling during charge and discharge.

[0027] The volume ratio of the first particle to the second particle is 1:5 to 1:35, 1:8 to 1:30, for example, 1:20. If the volume ratio of the second particle is greater than the above-mentioned range of the volume ratio of the first particle to the second particle, the resistance increases, and if the volume ratio of the second particle is smaller than the above-mentioned range, the cell life is reduced due to a decrease in the bending strength.

[0028] The volume ratio of the first particle to the second particle is related to the diameter ratio of the first particle to the second particle, and the diameter ratio of the first particle to the second particle is, for example, 1:1.25 to 1:3.5, 1:2 to 1:3.5, 1:2.5 to 1:3.5, or 1:2.5 to 1:3.0.

[0029] According to one embodiment, the mixing weight ratio of the first particle and the second particle contained in the adhesive layer is 1:99 to 99:1, 1:90 to 90:1, 1:80 to 80:1, 70:1 to 1:70, 50:1 to 1:50, 30:1 to 1:30, 20:1 to 1:1, 10:1 to 1:1, or 5:1 to 1:1. According to another embodiment, the mixing weight ratio of the first particle to the second particle is 20:1 to 1:1, 10:1 to 1:1, 10:1 to 1.5:1, 8:1 to 1.5:1, 7:1 to 1.5:1, 6:1 to 1.5:1, 6:1 to 1.5:1, 5.5:1 to 1.5:1, 5.5:1 to 1.7:1, 5.3:1 to 1.9:1, 5.13:1 to 1.97:1, or 5:1 to 2:1. According to another embodiment, the weight ratio of the first particle to the second particle contained in the adhesive layer is 5:1 to 1:1, 4:1 to 1:1, or 3:1 to 1:1.

[0030] When the diameter ratio and weight ratio of the first and second particles are within the above-described ranges, a separator having improved adhesiveness can be manufactured while reducing the interfacial resistance between the separator and the electrode.

[0031] The first particle has a smaller size than the second particle.

[0032] The size of the first particle is 100 to 300 nm, or 150 nm to 250 nm, and the size of the second particle is 500 nm to 900 nm, or 500 nm to 870 nm.

[0033] In this specification, "size" refers to the particle diameter when the particle to be measured is spherical, and refers to the major axis length when the particle is non-spherical. The particle diameter is, for example, the average particle diameter, and the major axis length is, for example, the average major axis length. The average particle diameter and the average major axis length represent the average values ​​of the measured particle diameters and measured major axis lengths, respectively. In the present disclosure, the particle size refers to the average size of the particles.

[0034] In this specification, the size of particles can be evaluated using a particle size analyzer, a scanning electron microscope, or a transmission electron microscope. For example, a HORIBA LA-950 laser particle size analyzer can be used as a particle size analyzer. The average particle diameter is, for example, the average particle diameter observed using a scanning electron microscope (SEM), and can be calculated as the average value of the particle diameters of about 10-30 particles using SEM images.

[0035] When particle size is measured using a particle size analyzer, the average particle diameter is represented by D50. D50 refers to the average diameter of particles that account for 50% of the cumulative volume in the particle size distribution, and in a distribution curve where particle sizes are accumulated from the smallest to the largest, it refers to the value of the particle diameter corresponding to 50% of the smallest particle when the total number of particles is 100%.

[0036] D50 can be measured using a particle size analyzer. Alternatively, D50 can be easily obtained by counting the number of particles in each particle size range using a dynamic light scattering (DLS) measuring device, analyzing the data, and calculating the number of particles.

[0037] The glass transition temperature of the first particle is not indicated. And the thermal decomposition temperature of the first particle is 200°C or higher, 220°C or higher, 250°C or higher, for example, 250 to 300°C. When the glass transition temperature or thermal decomposition temperature of the first particle is within the above range, the first particle can function as a filler and exhibit high heat-resistant particle characteristics.

[0038] The glass transition temperature of the second particle is 40°C to 80°C, 42°C to 78°C, 45°C to 75°C, 48°C to 73°C, or 50°C to 70°C. When the second particle has the above-described glass transition temperature, the bonding force between the electrode and the adhesive layer becomes stronger.

[0039] The total content of the first and second particles is 60 to 98 parts by weight, 62 to 98 parts by weight, 63 to 98 parts by weight, 64 to 98 parts by weight, for example, 65 to 98 parts by weight, based on 100 parts by weight of the total weight of the adhesive layer. When the total content of the first and second particles is within the above range, the adhesive strength between the electrode and the separator is excellent.

[0040] The above first and second particles are organic polymers. The weight average molecular weight of the organic polymer is 50,000 to 500,000, 100,000 to 480,000, 120,000 to 470,000, 150,000 to 450,000, 200,000 to 450,000, for example, 300,000 to 450,000. When the weight average molecular weight of the organic polymer is within the above range, the adhesive strength of the separation membrane is improved.

[0041] The first particle and the second particle are, for example, butyl methacrylate-ethylene glycol dimethacrylate copolymer, butyl methacrylate-ethylene glycol dimethacrylate-acrylonitrile copolymer, styrene-ethylhexylacrylate copolymer, styrene-ethylhexylacrylate-acrylonitrile copolymer, styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, acrylic rubber, butyl rubber, fluoroelastomer, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylate, polyacrylonitrile, polystyrene, ethylene propylene diene copolymer, It may include polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol, carboxymethylcellulose, hydroxypropylmethylcellulose, hydroxypropylcellulose, diacetylcellulose, or a combination thereof.

[0042] The first particle is, for example, a polymer obtained by a polymerization reaction of a polymerizable monomer having a crosslinking functional group, wherein the crosslinking functional group is, for example, a glycidyl group, an amino group, an N-methylol group, or a vinyl group.

[0043] The polymerizable monomer having the above crosslinking functional group is, for example, a hydroxy ester of an ethylenically unsaturated carboxylic acid, a glycidyl ester of an ethylenically unsaturated carboxylic acid, an amino ester of an ethylenically unsaturated carboxylic acid, an ethylenically unsaturated amide containing a methylol group, a monomer having two or more vinyl groups, or a combination thereof.

[0044] The hydroxy ester of the ethylenically unsaturated carboxylic acid includes (meth)acrylate hydroxypropyl, (meth)acrylate hydroxyethyl or a combination thereof, the glycidyl ester of the ethylenically unsaturated carboxylic acid includes glycidyl(meth)acrylate, and the amino ester of the ethylenically unsaturated carboxylic acid includes dimethylaminoethyl(meth)acrylate, the methylol group-containing ethylenically unsaturated amide includes N-methylol(meth)acrylamide, N,N-dimethylol(meth)acrylamide or a combination thereof, and the monomer having two or more vinyl groups may include ethylene di(meth)acrylate, divinylbenzene or a combination thereof.

[0045] In one embodiment, the first particle is, for example, a butyl methacrylate-ethylene glycol dimethacrylate copolymer, a butyl methacrylate-ethylene glycol dimethacrylate-acrylonitrile copolymer, or a combination thereof.

[0046] The second particle is, for example, a styrene-ethylhexylacrylate copolymer, a styrene-ethylhexylacrylate-acrylonitrile copolymer, or a combination thereof.

[0047] In a secondary battery separator according to an embodiment, the adhesive layer may further contain an additional binder, such as a fluorine-based resin, a polyacrylic acid-based compound, or a combination thereof. The content of such additional binder is 1 to 3 parts by weight based on the total weight of the adhesive layer.

[0048] When the total content of the additional binder is within the above range, the bonding force between the electrode and the separator can be more effectively controlled.

[0049] The weight average molecular weight of the polyacrylic acid compound is 50,000 to 500,000, for example, 150,000 to 450,000, for example, 300,000 to 450,000. When the weight average molecular weight of the (meth)acrylic polymer is within the above range, the adhesive strength of the separation membrane is improved. In the present disclosure, the weight average molecular weight can be evaluated by gel permeation chromatography.

[0050] Polyacrylic acid compounds include, for example, polyacrylic acid, polymethylacrylic acid, polyethylacrylic acid, polybutylacrylic acid, polyhexylacrylic acid, polyhydroxyethylmethacrylic acid, polyaminoacrylic acid, or combinations thereof.

[0051] The fluorinated resin acts as a binder to fix inorganic particles onto the porous substrate, while also providing excellent adhesion so that one side of the adhesive layer adheres well to the porous substrate and the other side adheres well to the electrode. The average particle size of the fluorinated resin, which is the binder, is 100 to 300 nm. When the fluorinated resin has the above-described average particle size, the adhesive layer exhibits excellent adhesion to the porous substrate. Even when the separator is exposed to high temperatures, the binder has high heat resistance and can maintain the matrix form of the network structure.

[0052] The glass transition temperature (Tg) of the fluorinated resin is 50°C or higher, and the weight average molecular weight is 200,000 to 3,000,000 g / mol, 200,000 to 2,500,000 g / mol, 200,000 to 2,000,000 g / mol, 300,000 to 1,500,000 g / mol, or 300,000 to 1,200,000 g / mol. In the present specification, the weight average molecular weight may be a polystyrene-converted average molecular weight measured using gel permeation chromatography. When the weight average molecular weight of the fluorinated resin is within the above range, the separator may have excellent adhesive strength.

[0053] The fluorinated resin is polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trichloroethylene copolymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer, or a combination thereof. And the methacrylic binder is polyacrylate, polymethacrylate, polybutylacrylate, polyacrylonitrile, or a combination thereof.

[0054] In the above vinylidene fluoride-hexafluoropropylene copolymer, the vinylidene fluoride repeating unit may be included in an amount of 90 mol% to 99.5 mol%, 93 mol% to 99 mol%, or 95 mol% to 99 mol%. When the vinylidene fluoride repeating unit is included in the above range, the vinylidene fluoride-hexafluoropropylene copolymer can secure excellent adhesive strength and electrolyte impregnation property, etc.

[0055] The crystallinity of the above fluorinated resin may be 35% to 45%, for example, 38% to 45%, or 40% to 45%. A separator having adhesive strength and containing a fluorinated resin having such a crystallinity exhibits excellent adhesive strength to a substrate.

[0056] When the adhesive layer further includes a (meth)acrylic binder, the mixing weight ratio of the total weight of the first particle and the second particle to the (meth)acrylic binder can be controlled to a weight ratio of 0.01:1 to 1:1, a weight ratio of 0.05:1 to 1:1, a weight ratio of 0.1:1 to 1:1, a weight ratio of 0.2:1 to 1:1, or a weight ratio of 0.25:1 to 0.75:1.

[0057] In another embodiment, the adhesive layer may further include at least one selected from the group consisting of, for example, polyvinylpyrrolidone, polyvinyl acetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, cyanoethylpolyvinyl alcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxyl methyl cellulose, and acrylonitrile-styrene-butadiene copolymer.

[0058] Hereinafter, with reference to Fig. 1, a secondary battery separator according to an embodiment will be examined in detail.

[0059] Secondary batteries include, for example, lithium secondary batteries.

[0060] Referring to FIG. 1, a secondary battery separator (10) according to an embodiment comprises a porous substrate (20) and an inorganic layer (30) positioned on both sides of the porous substrate (20).

[0061] The separator of Fig. 1 has an inorganic layer (30) positioned on both sides of a porous substrate (20), but the inorganic layer (30) may be positioned on one side of the porous substrate as shown in Fig. 3. In the separator of Fig. 3, an adhesive layer (40) is positioned on top of the inorganic layer (30).

[0062] The above adhesive layer (40) contains first and second particles having different particle sizes, and the volume ratio of the first and second particles is 1:8 to 1:40. By including the above-described adhesive layer (40), the separator (10) can exhibit improved heat resistance, stability, and adhesive strength.

[0063] The thickness of the adhesive layer (40) is 0.01 µm to 10 µm, 0.01 µm to 8 µm, 0.01 µm to 6 µm, 0.01 µm to 4 µm, or 0.04 µm to 1 µm. When the thickness of the adhesive is within the above range, excellent adhesive strength is exhibited. The thickness of the adhesive layer is measured using a film thickness measuring device. In the present disclosure, the thickness represents an average thickness.

[0064] According to another embodiment, a separation membrane may further include an inorganic layer (30) formed on the other side of the porous substrate (20) as shown in FIG. 2. The inorganic layer (30) disposed on the other side of the porous substrate (20) may have the same or different composition as the inorganic layer (40) disposed on the other side of the porous substrate (20).

[0065] According to another embodiment, a separator may have a laminated structure in which an adhesive layer (40) is arranged on the other side of a porous substrate (20), although this is not shown in the drawing.

[0066] The inorganic particles contained in the inorganic layer (40) are not particularly limited, and inorganic particles commonly used in the relevant technical field can be used. Specific examples of inorganic particles that can be used in the present invention include at least one selected from Al2O3, SiO2, B2O3, Ga2O3, TiO2, SnO2, boehmite, BaSO4, MgO, Mg(OH)2, clay, ZnO, CaO, CeO2, NiO, GaO, ZrO2, Y2O3, SrTiO3, and BaTiO3. The inorganic particles can be used alone or in combination of two or more of the above-described materials. More specifically, the inorganic particles can be used as Al2O3 (alumina).

[0067] The size of the inorganic particles is, for example, 1 ㎛ to 20 ㎛, 2 to 15 ㎛, or 3 to 12 ㎛. In this specification, “size” refers to the average size, and when the particles are spherical, it refers to the average particle diameter, and when the particles are non-spherical, it refers to the average major axis length. The average particle diameter refers to the volume-based D50. The average particle diameter is measured using a measuring device such as a laser diffraction method or a dynamic light scattering method. The average particle diameter is measured using, for example, a laser scattering particle size distribution meter (e.g., Horiba LA-920), and is the value of the median particle diameter (D50) when 50% is accumulated from the small particle side in volume conversion.

[0068] When using inorganic particles having the sizes described above, the dispersibility and coating processability of the inorganic particles within the inorganic layer can be prevented from deteriorating, and the thickness of the inorganic layer can be appropriately controlled to enhance mechanical properties. Furthermore, the size of the pores created in the separator can be appropriately controlled to reduce the likelihood of internal short circuits occurring during battery charging and discharging.

[0069] In the inorganic layer, the inorganic particles are contained in an amount of 50 to 95 parts by weight, 55 to 95 parts by weight, 58 to 95 parts by weight, 60 to 95 parts by weight, 62 to 95 parts by weight, 65 to 95 parts by weight, 68 to 95 parts by weight, 70 to 95 parts by weight, 72 to 95 parts by weight, or 75 to 95 parts by weight, based on 100 parts by weight of the total weight of the inorganic layer. When the content of the inorganic particles is within the above range, the thermal shrinkage of the separator can be effectively suppressed. When the inorganic particles are contained within the above range, the heat dissipation properties of the inorganic particles can be sufficiently exhibited, and the thermal shrinkage of the separator can be effectively suppressed.

[0070] The inorganic layer (30) constituting the separator (10) is a heat-resistant layer, and the shrinkage and rupture characteristics are not reduced at high temperatures and the adhesion to the substrate is improved.

[0071] The thickness of the inorganic layer (30) is 0.01 µm to 20 µm, 0.1 µm to 20 µm, 1 µm to 20 µm, 1 µm to 15 µm, 1 µm to 13 µm, 1 µm to 10 µm, 1 µm to 8 µm, 1 µm to 6 µm, or 1 µm to 5 µm.

[0072] The inorganic layer (30) contains inorganic particles and a binder. The binder may be a crosslinkable binder, a non-crosslinkable binder, or a combination thereof.

[0073] A crosslinkable binder refers to a material capable of generating a crosslinked structure binder by inducing a crosslinking reaction. The crosslinkable binder may be selected from a monomer, oligomer, polymer, or mixture thereof having one or more crosslinking functional groups. By curing the crosslinkable binder, not only physical and chemical bonds are formed between the monomers, oligomers, or polymers, but also physical and chemical bonds between the crosslinked binder and surface-treated inorganic particles enhance adhesion to the substrate and increase the coating density, thereby enabling the thin film formation of the separator.

[0074] The monomer, oligomer or polymer having one or more functional groups has one or more functional groups selected from the group consisting of, for example, an acrylate group, a vinyl group, a hydroxyl group, an epoxy group, an oxane group, an oxetane group, a carboxyl group, an amine group, an oxazoline group, an ester group and an isocyanate group. The number of functional groups is two or more, three or more, or four or more.

[0075] Crosslinking binders include, for example, alkyl (meth)acrylates such as methyl methacrylate, methyl acrylate; bifunctional (meth)acrylates such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, di(meth)acrylate of polyoxyethylene / polyoxypropylene copolymer, butanediol di(meth)acrylate, hexamethylene glycol di(meth)acrylate; Examples thereof include at least one acrylate selected from the group consisting of trifunctional (meth)acrylates such as trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, tri(meth)acrylate of an ethylene oxide adduct of glycerin, tri(meth)acrylate of a propylene oxide adduct of glycerin, tri(meth)acrylate of an ethylene oxide or propylene oxide adduct of glycerin, and the like; tetrafunctional or more polyfunctional (meth)acrylates such as diglycerin hexa(meth)acrylate; polyfunctional urethane acrylate; polyfunctional epoxy acrylate; and polyester acrylate.

[0076] Examples of crosslinking binders include vinylpyrrolidone, vinylcaprolactam, vinylimidazole, vinylmethylacetamide, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, pentyl vinyl ether, hexyl vinyl ether, heptyl vinyl ether, octyl vinyl ether, nonyl vinyl ether, decyl vinyl ether, cyclohexyl vinyl ether, ethylhexyl vinyl ether, dodecyl vinyl ether, and octadecyl vinyl ether.

[0077] Crosslinking binders include, for example, biphenol, bisphenol A, methanediol, ethanediol, propanediol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, and decanediol. Examples of monomers, oligomers, or polymers having one or more epoxy groups include diepoxyalkanes such as diepoxyethane, diepoxypropane, diepoxybutane, diepoxypentane, diepoxyhexane, diepoxyheptane, diepoxyoctane, diepoxynonane, and diepoxydodecane; glycidyl ethers such as bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, brominated bisphenol A diglycidyl ether, phenol novolac glycidyl ether, and cresol novolac glycidyl ether; Examples thereof include glycidyl esters such as hexahydrophthalic acid glycidyl ester and dimer acid glycidyl ester; glycidyl amines such as glycidyl isocyanurate and tetraglycidyl diamino phenylmethane; linear aliphatic epoxides such as epoxidized polybutadiene; and alicyclic epoxides such as 3,4-epoxy-6-methylcyclohexyl methyl carboxylate and 3,4-epoxycyclohexyl methyl carboxylate.

[0078] Crosslinking binders include, for example, 4,4'-diphenylenemethane diisocyanate, toluene diisocyanate, tolylene diisocyanate, naphthylene diisocyanate, 4,4'-dicyclohexylenemethane diisocyanate, cyclohexylene diisocyanate, 3,3'-dimethylphenylene diisocyanate, diphenylmethane diisocyanate, 3,3'-dimethyldiphenylenemethane diisocyanate, 4,6'-xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 3,5,5-trimethylcyclohexylene diisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, m-xylene diisocyanate, trimethylxylene diisocyanate, p-phenylene diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, trans-1,4-cyclohexyl diisocyanate, or combinations thereof.

[0079] Additionally, a compound represented by the following chemical formula 1 can be used as a crosslinking binder.

[0080] [Chemical Formula 1]

[0081]

[0082] In chemical formula 1, X 1 Inland X 3 are each an oxyethylene group, and X 4 is an oxyethylene group or an alkyl group having 1 to 10 carbon atoms, and R 1 Inland R 4 is independently any one selected from the group consisting of a (meth)acrylate group, a hydroxyl group, a carboxyl group, an ester group, a cyanate group, an isocyanate group, an amino group, a thiol group, an alkoxy group having 1 to 10 carbon atoms, a vinyl group, and a heterocyclic group, and a 1 Inland a 4 are integers from 1 to 10, respectively, and n 1 Inland n 3 are integers from 0 to 10, respectively, and n 1 Inland n 4 At least one of them is an integer from 1 to 10, provided that X 4 If the above oxyethylene group is n 4 is an integer from 1 to 10, m is 1, and X 4 If the above carbon number is an alkyl group having 1 to 10, n 4 is 1 and m is 0.

[0083] The above ester group can be represented as -COOR, and the amino group can be represented as -NR a R b It can be expressed as R, R a and R bEach of may be independently any one selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkenyl group having 3 to 20 carbon atoms, a cycloalkynyl group having 4 to 20 carbon atoms, and an aryl group having 6 to 30 carbon atoms. In addition, the heterocyclic group may be any one selected from the group consisting of a heterocycloalkyl group having 2 to 20 carbon atoms, a heterocycloalkenyl group having 3 to 20 carbon atoms, a heterocycloalkynyl group having 3 to 20 carbon atoms, and a heteroaryl group having 6 to 20 carbon atoms, and may include a heteroatom selected from N, O, and S. Examples thereof include an epoxy group or an oxetane group.

[0084] The compound of the above chemical formula 1 may be, for example, a compound of the following chemical formula 2 or 3.

[0085] [Chemical Formula 2]

[0086]

[0087] [Chemical Formula 3]

[0088]

[0089] In chemical formulas 2 and 3, R 5 may be an alkyl group having 1 to 10 carbon atoms, and n 5 Inland n 7 can be integers from 1 to 5, and a 5 Inland a 12 Each can be an integer from 1 to 10.

[0090] Compounds of formula 1 include, for example, ethoxylated pentaerythritol tetraacrylate or ethoxylated trimethylolpropane triacrylate.

[0091] The crosslinking binder is present in an amount of 1 to 10 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the total weight of the inorganic layer. Within the above range, the heat shrinkage resistance and fracture properties are excellent.

[0092] The inorganic particles contained in the inorganic layer may be surface-treated to be able to react with the crosslinking binder. The inorganic particles may be surface-treated with, for example, functional groups capable of reacting with functional groups of the crosslinking binder. When surface-treated, a crosslinking reaction occurs due to the reaction between the functional groups of the inorganic particles and the functional groups of the crosslinking binder, and a crosslinking reaction of the functional groups of the inorganic particles also occurs, thereby enhancing the bonding strength between the inorganic particles and the crosslinking binder, and improving the adhesion to the substrate or the coating density. For example, when the crosslinking binder has an acrylate functional group, the inorganic particles may be surface-treated to have an acrylate group.

[0093] A binder comprising an aqueous cross-linking reactive acrylamide copolymer can be used as a cross-linking binder contained in the inorganic layer. The aqueous cross-linking reactive acrylamide copolymer contains two or more types of cross-linkable reactive groups. It can be used in a single-component form without a cross-linking agent, and the two or more types of cross-linking reactive groups can cross-link with each other through a self-condensation reaction. Through this, a separator inorganic layer can be formed, thereby providing a separator having high heat resistance properties.

[0094] The crosslinking reactive group may include at least one first functional group selected from a carboxyl group, an amine group, and an isocyanate group; and at least one second functional group selected from a hydroxyl group, an epoxy group, and an oxazoline group; and a crosslinking reaction may occur between the first functional group and the second functional group to form a bond. For example, the crosslinking reactive group may include a carboxyl group and a hydroxyl group.

[0095] According to one embodiment, the equivalent ratio of the first functional group and the second functional group may be in the range of 30:70 to 70:30. The equivalent ratio of the first functional group and the second functional group may be, for example, in the range of 35:65 to 65:35, in the range of 40:60 to 60:40, or in the range of 45:55 to 55:45, and may be, for example, in the range of about 50:50. In the above range, a crosslinking reaction may smoothly occur between the first functional group and the second functional group.

[0096] According to one embodiment, the acrylamide copolymer includes an (N-substituted) amide monomer, and the (N-substituted) amide monomer is N,N-dialkyl (meth)acrylamide such as (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di (n-butyl) (meth)acrylamide, N,N-di (t-butyl) (meth)acrylamide, N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, Nn-butyl (meth)acrylamide, N-methylol (meth)acrylamide, It may include at least one selected from the group consisting of N-ethylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-methoxyethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, and N-acryloylmorpholine.

[0097] The content of the above (N-substituted) amide monomer is 30 to 90 mol%, 40 to 80 mol%, or 50 to 70 mol% based on the total mol of monomer components constituting the acrylamide copolymer. By using an acrylamide copolymer having an (N-substituted) amide monomer in the above range, a decomposition temperature characteristic of 200°C or higher can be exhibited.

[0098] According to one embodiment, the acrylamide copolymer comprises: an (N-substituted) amide monomer; And a carboxyl group-containing monomer, a (meth)acrylic acid alkyl monomer, a hydroxyl group-containing monomer, an isocyanate group-containing monomer, an oxazoline group-containing monomer, a hydroxyl group-containing monomer, a polyfunctional (meth)acrylate-based monomer, an acid anhydride group-containing monomer, a sulfonic acid group-containing monomer, a phosphoric acid group-containing monomer, a succinimide-based monomer, a maleimide-based monomer, an itaconimide-based monomer, a cyano-containing monomer, an (meth)acrylic acid aminoalkyl-based monomer, an (meth)acrylic acid alkoxyalkyl-based monomer, an epoxy group-containing acrylic monomer, an acrylic acid ester-based monomer having a heterocycle, a halogen atom, a silicon atom, etc., acryloylmorpholine, a (meth)acrylic acid ester having an alicyclic hydrocarbon group, a (meth)acrylic acid ester having an aromatic hydrocarbon group, and a terpene compound derivative. It may include one or more acrylic monomers selected from the group consisting of (meth)acrylic acid esters obtained from alcohol.

[0099] Here, two or more cross-linkable functional groups may be present in the (N-substituted) amide monomer and the acrylic monomer, or may be present only in the acrylic monomer.

[0100] Specific examples of acrylic monomers include carboxyl group-containing monomers such as acrylic acid, (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid; (Meth)acrylic acid alkyl monomers having a straight or branched alkyl group having 1 to 20 carbon atoms in the ester moiety, specifically, for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, (Meth)acrylic acid alkyl monomers such as isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, nonadecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, stearyl (meth)acrylate, and n-tetradecyl (meth)acrylate; Hydroxyl group-containing monomers such as hydroxyalkyl (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl (meth)acrylate, etc.;Multifunctional (meth)acrylate monomers such as hexanediol diacrylate (HDDA), tripropylene glycol diacrylate (TPGDA), ethylene glycol diacrylate (EGDA), trimethylolpropane triacrylate (TMPTA), trimethylolpropane ethoxy triacrylate (TMPEOTA), glycerin propoxylated triacrylate (GPTA), pentaerythritol tetraacrylate (PETA), or dipentaerythritol hexaacrylate (DPHA); acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; sulfonic acid group-containing monomers such as 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; Phosphoric acid group-containing monomers such as [2-(2-hydroxyethyl)acryloyl] phosphate; succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyhexamethylenesuccinimide; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide; Cyano-containing monomers such as acrylonitrile and (meth)acrylonitrile; aminoalkyl (meth)acrylate monomers such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; alkoxyalkyl (meth)acrylate monomers such as methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; epoxy-group-containing acrylic monomers such as glycidyl (meth)acrylate;Examples thereof include acrylic acid ester monomers having a heterocycle, halogen atom, silicon atom, etc., such as (meth)acrylate tetrahydrofurfuryl, fluorine-containing (meth)acrylate, and silicone (meth)acrylate; acryloylmorpholine; (meth)acrylic acid esters having an alicyclic hydrocarbon group, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; (meth)acrylic acid esters having an aromatic hydrocarbon group, such as phenyl (meth)acrylate and phenoxyethyl (meth)acrylate; (meth)acrylic acid esters obtained from terpene compound derivative alcohols; and the like. The acrylamide copolymer may be used alone or in combination of two or more of the above-described acrylic monomers.

[0101] According to one embodiment, the molar ratio of the (N-substituted) amide monomer and the acrylic monomer may be in the range of 1:99 to 99:1, 20:80 to 80:20, 30:70 to 70:30, 40:60 to 60:40, or 50:50. In the above range, a separation membrane coating layer with improved heat resistance can be formed.

[0102] The weight average molecular weight of the acrylamide copolymer is 100,000 to 1,000,000 g / mol, 150,000 to 800,000 g / mol, 180,000 to 750,000 g / mol, 200,000 to 700,000 g / mol, 250,000 to 650,000 g / mol, or 300,000 to 600,000 g / mol. By using the acrylamide copolymer having the above-described weight average molecular weight range, a separator having a low shrinkage rate when stored at high temperatures can be manufactured.

[0103] The acrylamide-based copolymer may have a glass transition temperature of 150°C or higher, 150°C to 300°C, 170°C to 280°C, or 190°C to 250°C. By using the acrylamide-based copolymer having the above-described glass transition temperature, a highly heat-resistant inorganic membrane layer can be formed.

[0104] The acrylamide copolymer may be, for example, an acrylic acid-acrylamide-(2-acrylamido)-(2-methylpropanesulfonic acid) copolymer, an aqueous cross-linking reactive polyacrylamide-acrylic acid-hydroxyethylacrylate copolymer, or a combination thereof.

[0105] According to one embodiment, the acrylamide-based copolymer may further include one or more non-acrylic monomers. By further including one or more non-acrylic monomers, the acrylamide-based copolymer can further improve the heat resistance of the copolymer and the bonding strength to the porous substrate of the separation membrane.

[0106] Non-acrylic monomers may be used without particular limitation as long as they are copolymerizable monomers other than the above-mentioned acrylic monomers. Examples of copolymerizable non-acrylic monomers include vinyl esters, nitrogen-containing heterocyclic monomers, N-vinylcarboxylic acid amides, lactam monomers, olefin monomers, vinyl ether monomers, aromatic vinyl compounds, olefins or dienes, vinyl ethers, vinyl chloride, sulfonic acid group-containing monomers, imide group-containing monomers, isocyanate group-containing monomers, etc., and one or more of these may be selected.

[0107] Specific examples of non-acrylic monomers include vinyl esters such as vinyl acetate and vinyl propionate; N-Vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloyl piperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-2-piperidone, N-vinyl-3-morpholinone, N-vinyl2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, Examples thereof include nitrogen-containing heterocyclic monomers such as N-vinylisothiazole and N-vinylpyridazine; N-vinylcarboxylic acid amides; lactam monomers such as N-vinylcaprolactam; olefin monomers such as isoprene, butadiene, and isobutylene; vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether; aromatic vinyl compounds such as vinyltoluene and styrene; olefins or dienes such as ethylene, butadiene, isoprene, and isobutylene; vinyl ethers such as vinyl alkyl ether; vinyl chloride; sulfonic acid group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, and sodium vinylsulfonate; imide group-containing monomers such as cyclohexylmaleimide and isopropylmaleimide; and isocyanate group-containing monomers such as 2-isocyanateethyl(meth)acrylate. These non-acrylic monomers can be used alone or in combination of two or more.

[0108] The content of the non-acrylic monomer included in the acrylamide copolymer is not particularly limited and can be used within a range that does not impair the aqueous crosslinking reaction characteristics of the acrylamide copolymer and the high heat resistance characteristics of the membrane. For example, the non-acrylic monomer may be included in a range of 0.1 to 30 mol% based on the total molar basis of the monomer components constituting the acrylamide copolymer.

[0109] The content of the acrylamide-based copolymer is 10 to 100 wt%, 30 to 95 wt%, 50 to 90 wt%, or 60 to 80 wt% based on the total weight of the binder. Within the above range, a composition for forming an inorganic layer of a separation membrane with improved heat resistance and substrate bonding strength can be provided.

[0110] The inorganic layer may further include a non-crosslinking binder. By additionally including a non-crosslinking binder in the inorganic layer, the adhesion to the substrate or electrode and heat resistance can be further improved.

[0111] The non-crosslinking binder may be, for example, a single polymer selected from the group consisting of polyvinylidene fluoride (PVdF) polymers, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxyl methyl cellulose, and acrylonitrile-butadiene-styrene copolymers, or a mixture thereof. The non-crosslinking binder may be, for example, a vinylidene fluoride polymer.

[0112] The above vinylidene fluoride-based polymer may be, for example, polyvinylidene fluoride, a vinylidene fluoride copolymer, or a mixture thereof. The vinylidene fluoride copolymer refers to a polymer that contains 5 wt% or less of a type of repeating unit other than a vinylidene fluoride repeating unit. An example of the vinylidene fluoride copolymer is a vinylidene fluoride-hexafluoropropylene copolymer.

[0113] When the non-crosslinkable binder is included in addition to the crosslinkable binder, the weight ratio of the crosslinkable binder to the non-crosslinkable binder may be 8:2 to 2:8, specifically 3:7 to 7:3. When the non-crosslinkable binder is used in the above-described range, a separator with improved adhesive strength and heat resistance can be manufactured.

[0114] The thickness of the porous substrate is, for example, 1 μm to 100 μm, 1 μm to 40 μm, 1 μm to 30 μm, 5 μm to 20 μm, 5 μm to 15 μm, or 5 μm to 10 μm. In the present disclosure, the thickness represents an average thickness. When a porous substrate within the above thickness range is used, a separator having an appropriate thickness that is thick enough to prevent short circuiting between the positive and negative electrodes of the battery, but not so thick as to increase the internal resistance of the battery, can be manufactured.

[0115] The porosity of the porous substrate included in the separation membrane may be 5% to 95%, 30% to 80%, for example, 40% to 60%, and the air permeability may be 250 sec / 100cc or less, 230 sec / 100cc or less, 210 sec / 100cc or less, 200 sec / 100cc or less, 180 sec / 100cc or less, or 150 sec / 100cc or less. And the pore size of the porous substrate in the separation membrane may be 0.01 µm to 50 µm, 0.01 µm to 30 µm, 0.01 µm to 20 µm, or 0.01 µm to 10 µm. In the present disclosure, the pore size represents the average pore size. When the porosity, air permeability, and pore size of the porous substrate including the separator are within the above ranges, a porous substrate having excellent mechanical properties can be obtained without increasing the internal resistance of the lithium battery.

[0116] The porous substrate may be, but is not limited to, a polymer membrane formed of any one polymer selected from the group consisting of polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyacetal, polyamide, polyimide, polycarbonate, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene oxide, cyclic olefin copolymer, polyphenylene sulfide, and polyethylene naphthalate, or a mixture of two or more thereof.

[0117] In one example, the porous substrate may be a polyolefin-based substrate, and the polyolefin-based substrate may contribute to improving the safety of the battery by having an excellent shutdown function. The polyolefin-based substrate may be selected from the group consisting of, for example, a polyethylene single film, a polypropylene single film, a polyethylene / polypropylene bilayer, a polypropylene / polyethylene / polypropylene triple film, and a polyethylene / polypropylene / polyethylene triple film. In another example, the polyolefin-based resin may include a non-olefin resin in addition to an olefin resin, or a copolymer of an olefin and a non-olefin monomer.

[0118] The method for manufacturing a membrane according to the present invention can be any method applicable to the relevant technical field. For example, the membrane can be manufactured by a process such as preparing a slurry comprising inorganic particles, a first binder, and optionally, inorganic particles, applying the slurry to a porous substrate, followed by drying and rolling.

[0119] The method for applying the above slurry is not particularly limited, and any method that can be used in the relevant technical field may be used. For example, the slurry may be formed by methods such as printing, compression, indentation, roller application, blade application, grinding application, dipping application, spray application, or flow application.

[0120] Before forming a porous adhesive layer on one or both sides of the membrane substrate, a pretreatment such as sulfonation treatment, grafting treatment, corona discharge treatment, ultraviolet irradiation treatment, plasma treatment, or sputter etching treatment may be optionally performed to improve adhesion with the adhesive layer.

[0121] In a secondary battery separator according to an embodiment, the adhesive strength with the porous substrate may be 0.5 N / mm or more, 0.7 N / mm or more, 0.8 N / mm or more, specifically 0.8 to 0.99 N / mm, for example 0.81 to 0.93 N / mm. When the substrate adhesive strength is in the above range, the adhesive strength between the adhesive layer and the porous substrate is excellent, so that the performance of the battery can be maintained for a long period of time. The method for measuring the substrate adhesive strength is not particularly limited, and a method commonly used in the technical field of the present invention can be used.

[0122] A non-limiting example of a method for measuring the substrate adhesion of the above separator is as follows: According to Korean Industrial Standard KS-A-01107 (Testing method for adhesive tapes and adhesive sheets), the separator is cut to 25 mm in width and 250 mm in length, and tape (nitto 31B) is attached to each side to make a specimen, and then the specimen is compressed by reciprocating once at a speed of 300 mm / min using a compression roller with a load of 2 kg. After 30 minutes of compression, the specimen is turned over 180° and approximately 25 mm is peeled off, and the separator and the tape attached to one side of the separator are fixed to the upper clip of a tensile strength tester (Instron Series 1X / s Automated Materials Tester-3343, Instron). The tape attached to the other side of the separator is fixed to the lower clip, and then pulled at a tensile speed of 60 mm / min to measure the pressure when the porous adhesive layer is peeled off from the porous substrate, thereby obtaining the substrate adhesion.

[0123] The above separator may have an anode adhesive strength of 0.5 gf / 5 mm or more and an anode adhesive strength of 0.1 gf / 5 mm or more. Specifically, the anode adhesive strength may be 0.8 gf / 5 mm or more and the cathode adhesive strength may be 0.2 gf / 5 mm or more. Within the above range, the separator is sufficiently adhered to the anode and the cathode, and thus, when the battery including the separator is repeatedly charged and discharged, changes in the shape of the battery can be minimized in an environment where the battery expands and contracts repeatedly, and a short ion transfer distance can be secured, thereby improving the output efficiency of the battery.

[0124] According to another embodiment of the present invention, a secondary battery is provided, which includes: a positive electrode; a negative electrode; a separator according to one embodiment positioned between the positive electrode and the negative electrode; and an electrolyte.

[0125] The secondary battery may be a lithium secondary battery, such as a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery, for example.

[0126] The method for manufacturing a secondary battery according to the present invention is not particularly limited, and a method commonly used in the technical field of the present invention can be used.

[0127] Below, we will examine a method for manufacturing a separation membrane according to an embodiment.

[0128] An inorganic layer is provided on top of a porous substrate. When forming the inorganic layer, coating methods, lamination, coextrusion, etc. can be used. Non-limiting examples of the coating methods include, but are not limited to, roll coating, spin coating, dip coating, flow coating, spray coating, etc.

[0129] The above inorganic layer can be cured by providing a composition for forming an inorganic layer on top of a porous substrate and then applying light or heat thereto. Specifically, the photocuring can be ultraviolet curing or far-infrared curing, and for example, ultraviolet curing. The photocuring can be performed at, for example, 500 mJ / cm 2 3000 mJ / cm 2 The amount of light, specifically 500 mJ / cm 2 Up to 2000 mJ / cm 2 It may include irradiating the amount of light to the porous heat-resistant layer. The irradiation time may be 1 minute to 15 hours. A homogeneous cured density may be obtained through a subsequent heat treatment after the photocuring, which may be performed at a temperature of about 50°C or higher and about 180°C or lower for 1 hour to 10 hours. In addition, in the case of heat curing, it may include curing at about 40°C to 120°C, 50°C to 100°C, or 60°C to 90°C for 1 hour to 36 hours, specifically, curing for about 5 hours to 24 hours.

[0130] The composition for forming the above inorganic layer may include a material for forming the crosslinking binder and / or a polymerization initiator for crosslinking the crosslinking binder and the surface-treated inorganic particles.

[0131] The above polymerization initiator acts as a curing agent that generates free radicals by heating or light, and can be appropriately selected depending on the type of functional group of the material and inorganic particles that produce the cross-linked structure binder. For example, the initiator may be a thermal polymerization initiator such as a peroxide-based, azo-based, amine-based, imidazole-based, or isocyanate-based initiator, or a photopolymerization initiator such as an onium salt or an organometallic salt.

[0132] Next, an adhesive layer composition containing first particles, second particles, and a solvent, which are organic binders, is coated and dried on the upper part of the inorganic layer to form an adhesive layer.

[0133] By including water as the solvent, it can be provided in the form of a slurry. The composition for forming the first coating layer may further include an organic solvent as long as the aqueous characteristics are not impaired. The organic solvent may be an alcohol-based organic solvent. For example, the organic solvent may include one or more alcohol-based organic solvents selected from the group consisting of methanol, ethanol, propanol, and butanol. By using an alcohol-based organic solvent, a composition for forming the first coating layer can be provided that is harmless to the body and has excellent drying characteristics, thereby ensuring mass production without reducing productivity. According to one embodiment, water and the organic solvent may be included in a volume ratio of 100:0 to 60:40, a volume ratio of 95:5 to 80:20, or a volume ratio of 85:15 to 70:30. In the above range, a composition for forming the first coating layer of a separator with improved drying characteristics can be provided.

[0134] The solvent is evaporated through drying after coating the composition for forming the first coating layer of the separator, and is not present in the coating layer of the final obtained separator.

[0135] The coating method is not particularly limited, and for example, one or more selected from a forward roll coating method, a reverse roll coating method, a microgravure coating method, and a direct metering coating method may be selected, but is not necessarily limited to these methods. The coating method may be, for example, a direct metering coating method.

[0136] The above drying can be carried out by hot air in a dryer. Drying can be carried out, for example, at a temperature of 30 to 80°C, 35 to 75°C, 40 to 70°C, or 45 to 65°C. By drying in these temperature ranges, a separator having improved bending strength and peel strength can be manufactured.

[0137] A secondary battery according to another embodiment includes a positive electrode, a negative electrode, and the above-described separator disposed between the positive electrode and the negative electrode. The secondary battery is, for example, a lithium secondary battery.

[0138] According to one embodiment, a secondary battery includes an electrode assembly including a positive electrode, a negative electrode, and the above-described separator disposed between the positive electrode and the negative electrode, and the electrode assembly may have a form in which the electrode assembly is wound in a jelly roll shape. Since the lithium battery includes the above-described separator, the adhesive force between the electrodes (positive electrode and negative electrode) and the separator increases, so that volume changes during charging and discharging of the lithium battery can be suppressed. Accordingly, deterioration of the lithium battery accompanying volume changes of the lithium secondary battery can be suppressed, so that the life characteristics of the lithium battery can be improved.

[0139] Lithium secondary batteries can be manufactured, for example, by the following methods.

[0140] First, a negative electrode active material composition is prepared by mixing a negative electrode active material, a conductive agent, a binder, and a solvent. The negative electrode active material composition is directly coated on a metal current collector to manufacture a negative electrode plate. Alternatively, the negative electrode active material composition may be cast on a separate support, and then a film peeled from the support may be laminated on a metal current collector to manufacture a negative electrode plate. The negative electrode is not limited to the forms listed above and may have forms other than those listed above.

[0141] The negative active material includes a carbon-based material.

[0142] The carbonaceous material may be crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon may be non-shaped, plate-shaped, flake-shaped, natural graphite, artificial graphite, graphene, carbon black, fullerene soot, or a combination thereof.

[0143] Natural graphite is naturally occurring graphite, and includes flake graphite, highly crystalline graphite, and microcrystalline or cryptocrystalline (amorphous) graphite. Artificial graphite is artificially synthesized graphite, made by heating amorphous carbon to high temperatures, and includes primary or electrographite, secondary graphite, and graphite fibers. Expanded graphite is made by intercalating chemicals such as acid or alkali between the layers of graphite and heating them to expand the vertical layers of the molecular structure. Graphene contains a single layer or multiple single layers of graphite. Carbon black is a crystalline material with less regularity than graphite, and can be converted to graphite when heated to about 3,000℃ for a long time. Fullerene soot is a carbon mixture containing at least 3% by weight of fullerene, a polyhedral bundle-shaped compound composed of 60 or more carbon atoms. The above crystalline carbon may have a spherical, plate-like, fibrous, tubular or powder form.

[0144] The amorphous carbon may be soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, calcined coke, polymer carbide, or a combination thereof.

[0145] The negative electrode active material may further include a non-carbonaceous material. For example, the negative electrode active material may include at least one selected from the group consisting of a metal capable of forming an alloy with lithium, an alloy of a metal capable of forming an alloy with lithium, and an oxide of a metal capable of forming an alloy with lithium.

[0146] For example, the metal that can be alloyed with the lithium may be Si, Sn, Al, Ge, Pb, Bi, Sb Si-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a group 13-16 element, a transition metal, a rare earth element, or a combination thereof, and is not Si), Sn-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a group 13-16 element, a transition metal, a rare earth element, or a combination thereof, and is not Sn), etc. The element Y may be Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.

[0147] For example, the transition metal oxide may be lithium titanium oxide, vanadium oxide, lithium vanadium oxide, or the like.

[0148] For example, the above non-transition metal oxides are SnO2, SiO x (0 <x<2) 등일 수 있다.

[0149] Specifically, the negative electrode active material is Si, Sn, Pb, Ge, Al, SiOx(0 <x≤2), SnOy(0<y≤2), Li4Ti5O 12 , TiO2, LiTiO3, Li2Ti3O7, but is not necessarily limited to these, and any non-carbon-based negative electrode active material used in the relevant technical field is possible.

[0150] According to one embodiment, the negative active material may be a mixture of the above-described carbonaceous material and non-carbonaceous material, or a composite containing the above-described carbonaceous material and non-carbonaceous material. As the conductive material, acetylene black, Ketjen black, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, metal powder such as copper, nickel, aluminum, silver, metal fiber, etc. may be used, and also, one or more types of conductive materials such as polyphenylene derivatives may be used in combination, but are not limited thereto, and any material that can be used as a conductive material in the relevant technical field may be used. In addition, the above-described crystalline carbonaceous material may be added as a conductive material.

[0151] As a binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene, styrene butadiene rubber-based polymer or a combination thereof may be used, but is not limited to these, and any binder that can be used in the art may be used.

[0152] The solvent may include, but is not limited to, N-methylpyrrolidone, acetone, or water, and any solvent that can be used in the relevant technical field may be used.

[0153] The contents of the negative electrode active material, conductive agent, binder, and solvent are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, binder, and solvent may be omitted.

[0154] Meanwhile, the binder used in manufacturing the cathode may be the same as the coating composition included in the adhesive layer of the separator.

[0155] Next, a cathode active material composition is prepared, comprising a mixture of a cathode active material, a conductive agent, a binder, and a solvent. The cathode active material composition is directly coated and dried on a metal current collector to produce a cathode plate. Alternatively, the cathode active material composition can be cast on a separate support, and then a film peeled from the support can be laminated onto a metal current collector to produce a cathode plate.

[0156] The cathode active material may include at least one selected from the group consisting of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, and lithium manganese oxide, but is not necessarily limited thereto, and any cathode active material available in the relevant technical field may be used.

[0157] For example, Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Lia Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG bO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:

[0158] In this chemical formula, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.

[0159] Of course, it is also possible to use a compound having a coating layer on the surface of the compound, or it is also possible to use a mixture of the compound and a compound having a coating layer. The coating layer may include a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compounds forming these coating layers may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the compound with these elements in a method that does not adversely affect the properties of the positive electrode active material (for example, spray coating, dipping, etc.), and since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0160] For example, LiNiO2, LiCoO2, LiMn x O 2x (x=1, or 2), LiNi 1-x Mn x O2(0 <x<1), LiNi 1-x-y Co x Mn y O2(0≤x≤0.5, 0≤y≤0.5), LiFeO2, V2O5, TiS, MoS, etc. can be used.

[0161] In the positive electrode active material composition, the conductive agent, binder, and solvent may be the same as those used in the negative electrode active material composition. Meanwhile, it is also possible to form pores inside the electrode plate by further adding a plasticizer to the positive electrode active material composition and / or the negative electrode active material composition.

[0162] The contents of the cathode active material, conductive agent, general binder, and solvent are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, general binder, and solvent may be omitted.

[0163] Meanwhile, the binder used in the manufacture of the anode may be the same as the adhesive layer composition included in the adhesive layer of the separator.

[0164] Next, the above-described separator is placed between the anode and the cathode.

[0165] In an electrode assembly including an anode / separator / cathode, the separator disposed between the anode and the cathode includes a porous substrate as described above; and an adhesive layer disposed on both sides of the porous substrate, wherein the adhesive layer includes the coating composition for the separator as described above.

[0166] The separator may be prepared separately and placed between the positive electrode and the negative electrode. Alternatively, the separator may be prepared by winding an electrode assembly including a positive electrode / separator / negative electrode into a jelly roll shape, housing the jelly roll in a battery case or pouch, thermally softening the jelly roll under pressure while being housed in the battery case or pouch, pre-charging, hot-rolling the charged jelly roll, cold-rolling the charged jelly roll, and charging / discharging the charged jelly roll under pressure.

[0167] Next, the electrolyte is prepared.

[0168] The electrolyte may be in a liquid or gel state.

[0169] For example, the electrolyte may be an organic electrolyte. Furthermore, the electrolyte may be a solid. For example, boron oxide, lithium oxynitride, etc. may be used, but are not limited thereto, and any solid electrolyte that can be used in the art may be used. The solid electrolyte may be formed on the cathode by a method such as sputtering.

[0170] For example, an organic electrolyte can be prepared. The organic electrolyte can be manufactured by dissolving a lithium salt in an organic solvent.

[0171] Any organic solvent that can be used as an organic solvent in the relevant technical field can be used. For example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, methyl propionate, ethyl propionate, propyl propionate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0172] Lithium salts can be used as long as they can be used as lithium salts in the relevant technical field. For example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(FSO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (where x and y are natural numbers), LiCl, LiI, or mixtures thereof.

[0173] As an example of a secondary battery, a square lithium secondary battery is exemplarily described. Fig. 4 is an exploded perspective view of a lithium battery according to one embodiment.

[0174] Referring to FIG. 4, a lithium secondary battery (100) according to an embodiment includes an electrode assembly (160) wound with a separator (110) according to an embodiment interposed between a positive electrode (140) and a negative electrode (150) and a case (170) in which the electrode assembly (160) is built.

[0175] The electrode assembly (160) may be, for example, in the form of a jelly roll formed by winding an anode (140) and a cathode (150) with a separator (110) in between.

[0176] The anode (140), cathode (150) and separator (110) are impregnated with an electrolyte (not shown).

[0177] The above lithium secondary battery may be a lithium ion battery. The above lithium battery may be a lithium polymer battery.

[0178] Lithium batteries are suitable for electric vehicles (EVs) due to their excellent high-rate and long-life characteristics. For example, they are suitable for hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs).

[0179] The present invention is further described in detail through the following examples and comparative examples. However, these examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0180] Manufacturing Example 1: Manufacturing of acrylic copolymer

[0181] In a 10 L four-necked flask equipped with a stirrer, thermometer and condenser, distilled water (6361 g), acrylic acid (72.06 g, 1.0 mol), acrylamide (604.1 g, 8.5 mol), potassium persulfate (2.7 g, 0.01 mol), 2-acrylamido-2-methylpropanesulfonic acid (103.6 g, 0.5 mol) and 5N lithium hydroxide aqueous solution (1.05 equivalents based on the total amount of 2-acrylamido-2-methylpropanesulfonic acid) were added, and then the internal pressure was reduced to 10 mmHg using a diaphragm pump, and the operation of returning the internal pressure to atmospheric pressure with nitrogen was repeated three times.

[0182] The reaction was carried out for 12 hours while controlling the temperature of the reaction solution to be stable between 65 ℃ and 70 ℃. After cooling to room temperature, the pH of the reaction solution was adjusted to 7 to 8 using a 25% ammonia aqueous solution. In this way, poly(acrylic acid-co-acrylamide-co-2-acrylamido-2-methylpropanesulfonic acid), an acrylic copolymer, was prepared. The molar ratio of acrylic acid, acrylamide, and 2-acrylamido-2-methylpropanesulfonic acid was 10:85:5. Approximately 10 mL of the reaction solution (reaction product) was taken, and the nonvolatile component was measured, and it was 9.5 wt% (theoretical value: 10 wt%).

[0183] (Manufacturing of membranes)

[0184] Example 1: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0185] First, boehmite (Nabaltec, Japan) having an average size of 300 nm was ground for 2 hours using a bead mill, and then an inorganic dispersion containing 40 wt% of the ground boehmite (70 wt% of water) was obtained. Here, an acrylic copolymer prepared according to Manufacturing Example 1 was mixed so that the boehmite weight ratio was 95%, and water was added so that the total solid content was 25 wt%, thereby forming a composition for forming an inorganic layer.

[0186] The above-mentioned manufactured inorganic layer composition was coated on the cross-section of a polyethylene single-layer substrate film having a thickness of 5.5 μm used as a porous substrate by a gravure coating method, and then dried for 10 seconds under conditions of a drying temperature of 70°C and a wind speed of 15 m / sec, thereby manufacturing a separation membrane having an inorganic layer having a coating thickness of 2 μm.

[0187] Separately, the first particle, poly(butylmethacrylate-co-ethyleneglycol dimethacrylate) copolymer (2550M, Zeon Co.), and the second particle, poly(styrene-co-ethylhexylacrylate-acrylonitrile) copolymer (SP-18 A, Zeon Co.), were mixed at a weight ratio of 5.13:1, and then a PAA compound (AQC, Sumitomo Co.) was added and mixed thereto to form a composition for forming an adhesive layer. The content of the PAA compound is about 2 wt% based on 100 wt% of the total weight of the composition for forming an adhesive layer.

[0188] In poly(butyl methacrylate-co-ethylene glycol dimethacrylate) copolymer, the mixing molar ratio of butyl methacrylate and ethylene glycol dimethacrylate is 8:2, and in poly(styrene-co-ethylhexylacrylate-acrylonitrile) copolymer, the mixing molar ratio of styrene, ethylhexylacrylate, and acrylonitrile is 8:5:0.1.

[0189] The coating composition for forming the adhesive layer is coated on the porous substrate of the separation membrane having the inorganic layer (thickness: 2 um) manufactured according to the above process using the gravure coating method, and dried for 10 seconds under the conditions of a drying temperature of 60°C and a wind speed of 15 m / sec, so that 1.0 g / m is applied on the upper part of the inorganic layer. 2 A separator was formed by forming an adhesive layer on both sides.

[0190] An inorganic layer and an adhesive layer were formed on the other side of the porous substrate according to the method described above, thereby manufacturing a separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer.

[0191] Example 2: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0192] The first particle, Poly(butylmethacrylate-co-ethyleneglycol dimethacrylate) copolymer (2550M, Zeon Co.), and the second particle, Poly(styrene-co-ethylhexylacrylate-acrylonitrile) structure copolymer (SP-18 B, Zeon Co.) with a size of 780 nm, were mixed in a weight ratio of 1.97:1, and then a PAA compound (AQC, Sumitomo Co.) was used at 2 wt% of the total weight ratio to form a composition for forming an adhesive layer. The adhesive layer coating layer was applied in the same manner as in Example 1 to manufacture a separator.

[0193] Example 3: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0194] The first particle, Poly(butylmethacrylate-co-ethyleneglycol dimethacrylate) copolymer (2550M, Zeon Co.) and the second particle, Poly(styrene-co-ethylhexylacrylate-acrylonitrile) copolymer (SP-18 A, Zeon Co.) were mixed at a weight ratio of 1.97:1, and then a PAA compound (AQC, Sumitomo Co.) was used at 2 wt% of the total weight ratio to form a composition for forming an adhesive layer. The coating and application of the composition for forming an adhesive layer were performed in the same manner as in Example 1 to manufacture a separator.

[0195] Example 4: Separator having a laminated structure of adhesive layer / porous substrate / inorganic layer / adhesive layer

[0196] A separator was formed in the same manner as in Example 1, except that an adhesive layer-forming composition was prepared according to the conditions described in Table 1 below, and the adhesive layer-forming composition was coated and dried on the other side of a porous substrate on which an inorganic layer and an adhesive layer were sequentially formed, thereby forming an adhesive layer on the other side of the porous substrate. The laminated structure of this separator had a laminated structure of adhesive layer / porous substrate / inorganic layer / adhesive layer.

[0197] Comparative Example 1: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0198] A composition for forming an adhesive layer was formed using 2 wt% of a PAA compound (AQC, Sumitomo Co., Ltd.) based on the total weight of the first particle, Poly(butylmethacrylate-co-ethyleneglycol dimethacrylate) copolymer (2550M, Zeon Co., Ltd.). Coating and drying of the composition for forming an adhesive layer were performed in the same manner as in Example 1 to manufacture a separator.

[0199] Comparative Example 2: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0200] A composition for forming an adhesive layer was prepared by applying 2 wt% of a PAA compound (AQC, Sumitomo Co., Ltd.) to a copolymer (SP-18 A, Zeon Co., Ltd.) having a poly(styrene-co-ethylhexylacrylate) structure and a size of 500 nm as the second particle based on the total weight of the second particle. Coating and drying of the composition for forming an adhesive layer were performed in the same manner as in Example 1 to prepare a separator.

[0201] Comparative Example 3: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0202] The first particle, Poly(butylmethacrylate-co-ethyleneglycol dimethacrylate) copolymer (2550M, Zeon Co.) and the second particle, Poly(styrene-co-ethylhexylacrylate-acrylonitrile) copolymer (SP-18 C, Zeon Co.) with a size of 870 nm were mixed in a weight ratio of 1.97:1, and then a PAA compound (AQC, Sumitomo Co.) was used at 2 wt% of the total weight ratio to prepare a composition for forming an adhesive layer. The coating and drying of the composition for forming an adhesive layer were performed in the same manner as in Example 1 to prepare a separator.

[0203] Comparative Example 4: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0204] A separation membrane was manufactured in the same manner as in Example 1, except that the volume ratio of the first particle, the organic filler, and the second particle, the adhesive binder, was changed to 8:1.

[0205] Comparative Example 5: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0206] An adhesive layer and a separator including the same were manufactured in the same manner as in Example 1, except that the mixing volume ratio of the first and second particles was changed to 1:4 when manufacturing a composition for forming an adhesive layer.

[0207] Comparative Example 6: Separator having a laminated structure of adhesive layer / inorganic layer / porous substrate / inorganic layer / adhesive layer

[0208] An adhesive layer and a separator including the same were manufactured in the same manner as in Example 1, except that the mixing volume ratio of the first and second particles was changed to 9:1 when manufacturing a composition for forming an adhesive layer.

[0209] ClassificationExample 1Example 2Example 3Example 4Comparative Example 1Comparative Example 2Comparative Example 3Comparative Example 4Comparative Example 5Comparative Example 6Composition 1ParticleOrganic filler (250 nm)8265656598065336565Second particleAdhesive binder (500 nm)16-3333098-65Adhesive binder (780 nm)-33-----Adhesive binder (870 nm)-----33-Adhesive binder (410 nm)33Adhesive binder (525 nm)33OtherPAA compound22222222Mixing ratioFirst particle:Second particleVolume ratio1:81:301:81:8--1:428:11:49:1First particle:Second particle Diameter ratio 1:21:3.11:21:2--1:3.52:11:1.62.1:1

[0210] In Table 1, Poly(butylmethacrylate-co-ethyleneglycol dimethacryatel) is used as the organic filler (2550M, Zeon) (size: 250 nm).

[0211] SP-18 A (Zeon) is used as an organic adhesive binder (500 nm), and is a copolymer having a poly(styrene-co-ethylhexylacrylate-acrylonitrile) structure, and the mixed molar ratio of styrene, ethylhexylacrylate, and acrylonitrile is 8:2:0.5.

[0212] It is a copolymer having a poly(styrene-co-ethylhexylacrylate-acrylonitrile) structure using SP-18 B (Zeon) as an organic adhesive binder (780 nm), and the mixed molar ratio of styrene, ethylhexylacrylate, and acrylonitrile is 8:2:0.5.

[0213] SP-18 C (Zeon) is used as an organic adhesive binder (870 nm), and is a copolymer having a poly(styrene-co-ethylhexylacrylate-acrylonitrile) structure, and the mixed molar ratio of styrene, ethylhexylacrylate, and acrylonitrile is 8:2:0.5.

[0214] AQC (sumittomo) is used as a compound containing PAA, and its weight average molecular weight is approximately 450,000. In Table 1, the size of each particle represents D50. In addition, in the composition of Table 1, the numbers of the first particle, the second particle, and other numbers represent parts by weight.

[0215] (Manufacturing of lithium batteries)

[0216] Production example 1

[0217] (Manufacturing of cathode)

[0218] The cathode was manufactured according to the following process.

[0219] A slurry of a negative electrode active material was prepared by mixing 97 wt% of graphite particles with an average particle size of 25 μm, 1.5 wt% of styrene-butadiene rubber (SBR) binder, and 1.5 wt% of carboxymethyl cellulose (CMC), adding the mixture to distilled water, and stirring for 60 minutes using a mechanical stirrer. The slurry was applied onto a 10 μm thick copper current collector using a doctor blade, dried in a hot air dryer at 100°C for 0.5 hour, and then dried again under vacuum at 120°C for 4 hours, and then roll pressing was performed to prepare a negative electrode.

[0220] (Manufacturing of positive electrode)

[0221] Separately, the anode was manufactured according to the following process.

[0222] LiCoO2 97 wt%, carbon black powder 1.5 wt% as a conductive material, and polyvinylidene fluoride (PVdF) 1.5 wt% were mixed and placed in an N-methyl-2-pyrrolidone solvent, and stirred for 30 minutes using a mechanical stirrer to prepare a positive electrode active material slurry. The slurry was applied onto a 20 μm thick aluminum current collector using a doctor blade, dried in a hot air dryer at 100°C for 0.5 hour, dried again under vacuum at 120°C for 4 hours, and rolled to prepare a positive electrode.

[0223] (Electrode assembly jelly roll)

[0224] An electrode assembly jelly roll was prepared by interposing a separator obtained according to Example 1 between the positive and negative electrodes manufactured above and then winding the separator. The jelly roll was inserted into a pouch, an electrolyte was injected, and the pouch was vacuum-sealed.

[0225] The electrolyte used was 1.3 M LiPF6 dissolved in a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 3:5:2.

[0226] 11.7 kgf / cm in jelly roll inserted into pouch 2 A lithium battery was manufactured by pressing at a temperature of 80℃ for 3 minutes while applying pressure.

[0227] Production Example 2-4

[0228] A lithium battery was manufactured in the same manner as in Manufacturing Example 1, except that the separator of Examples 2-4 was used instead of the separator of Example 1.

[0229] Comparative Production Example 1-6

[0230] A lithium battery was manufactured in the same manner as in Manufacturing Example 1, except that the separator of Comparative Examples 1-6 was used instead of the separator of Example 1.

[0231] Evaluation Example 1: Ventilation

[0232] According to the above Examples 1 to 4 and Comparative Examples 1 to 6, the unit thickness of each membrane was measured using an air permeation tester (Asahi Seiko OKEN Type Air Permeation Tester: EGO1-55-1MR) according to the following method.

[0233] Ten specimens were cut from ten different points to a size that could accommodate a circle with a diameter of 1 inch, and then the time it took for 100 cc of air to pass through each specimen was measured using an air permeation measuring device, ASAHI SEIKO OKEN TYPE Air Permeation Tester EG01-55-1MR (Asahi Seiko Co., Ltd.). The time was measured five times for each specimen and the average value was calculated to measure the air permeability.

[0234] Looking at the conditions for setting the ventilation measuring device, measurement pressure: 0.05 mPa, cylinder pressure: 2.5 kg / ㎠, setting time: 10 seconds, measurements were made more than 10 times at 10 cm intervals for a 1 m specimen, and the average of the data was recorded.

[0235] In Table 2 below, △ air permeability (sec / 100cc) represents the change in air permeability, which is expressed by the following equation.

[0236] <Formula 1>

[0237] △ Air permeability = (membrane air permeability after test) - (initial membrane air permeability).

[0238] The ventilation test conditions are as follows.

[0239] - Heat Press (HP): 80 ℃ / 300 kgf / 1 hr

[0240] - Cold Press (CP): 25 ℃ / 300 kgf / 1 min

[0241] Evaluation Example 2: Resistance

[0242] The resistance of the membranes of Examples 1 to 4 and Comparative Examples 1 to 6 was evaluated by measuring AC impedance, and the evaluation results are shown in Table 2 below.

[0243] Evaluation Example 3: Bending Strength

[0244] Bending strength measurements were performed in lithium batteries manufactured according to Manufacturing Examples 1 to 5 and Comparative Manufacturing Examples 1 to 6 to investigate the bending strength of pouch-type batteries. The bending strength was measured using the 3-point bending method to measure the adhesive strength (bending strength) between the active material layer of the positive electrode and the separator in each lithium battery.

[0245] The results of the bending strength evaluation are shown in Table 2.

[0246] Evaluation Example 4: Life Characteristics

[0247] In the lithium secondary batteries manufactured according to Manufacturing Example 1-4 and Comparative Manufacturing Example 1-6, the charge and discharge characteristics were evaluated using a charger / discharger (Manufacturer: TOYO, Model: TOYO-3100).

[0248] The first charge / discharge cycle was performed by constant-current charging at a current of 0.1 C until the voltage reached 4.4 V, followed by constant-voltage charging at a current of 0.05 C. After the fully charged cell was rested for approximately 10 minutes, a constant-current discharge was performed at a current of 0.1 C until the voltage reached 3 V. The second charge / discharge cycle was performed by constant-current charging at a current of 0.2 C until the voltage reached 4.2 V, followed by constant-voltage charging at a current of 0.05 C. After the fully charged cell was rested for approximately 10 minutes, a constant-current discharge was performed at a current of 0.2 C until the voltage reached 3 V.

[0249] The life evaluation was performed by constant-current charging at a current of 1C until the voltage reached 4.4 V, followed by constant-voltage charging at a current of 0.05C. After the cell was fully charged, a rest period of approximately 10 minutes was followed by constant-current discharge at a current of 1C until the voltage reached 3 V. This cycle was repeated 500 times to evaluate the life characteristics.

[0250] The results of the life evaluation are shown in Table 2 below.

[0251] The lifespan is evaluated according to the following formula 2.

[0252] <Formula 2>

[0253] Lifespan = (500 discharge capacity / 1 discharge capacity) X 100

[0254] Evaluation Example 5: Bonding strength for porous substrate (hereinafter, substrate bonding strength)

[0255] The separators manufactured in the above examples and comparative examples were tested using an Instron universal testing machine according to Korean Industrial Standard KS-A-01107 (Testing method for adhesive tapes and adhesive sheets). Each separator was cut to a width of 25 mm and a length of 250 mm, and tape (nitto 31B) was attached to each side to make a specimen. Then, the specimen was compressed by reciprocating once at a speed of 300 mm / min using a compression roller with a load of 2 kg. After 30 minutes of compression, the specimen was flipped 180°, and approximately 25 mm was peeled off. The separator and the tape attached to one side of the separator were fixed to the upper clip of a tensile strength tester (Instron Series 1X / s Automated Materials Tester-3343, Instron). The tape attached to the other side of the separator was fixed to the lower clip, and then pulled at a tensile speed of 60 mm / min to measure the pressure when the porous adhesive layer was peeled off from the porous substrate.

[0256] ClassificationEmbodiment 1Embodiment 2Embodiment 3Embodiment 4Comparative Example 1Comparative Example 2Comparative Example 3Comparative Example 4Comparative Example 5Comparative Example 6Aeration (sec / 100cc) 142147147162140315201178167227Membrane resistance (Ω) 0.740.750.750.790.721.30.850.870.81.06Life (500cy) 95%96%96%94%30%34%81%68%84%1%Bending strength (N) 42545644142145445412217317398Material bonding strength (N / mm) 0.70.80.80.70.020.80.60.10.70.8△Aeration (sec / 100cc)1541671658949540298398315482

[0257] Referring to Table 2, it was found that the lithium batteries of Manufacturing Examples 1 to 4, each of which employed the separators of Examples 1 to 4, had greatly improved life characteristics compared to the lithium batteries of Comparative Manufacturing Examples 1 to 6, each of which employed the separators of Comparative Examples 1 to 6.

[0258] The separator of Comparative Example 1 has excellent membrane resistance, but its bending strength and substrate adhesion are poor, making it difficult to apply practically, and the life characteristics of a lithium battery employing such a separator are significantly reduced compared to Examples 1 to 4. The separator of Comparative Example 2 has excellent bending strength and substrate adhesion, but not only does it exhibit poor membrane resistance, but the life characteristics of a lithium battery employing such a separator are significantly reduced compared to Examples 1 to 4.

[0259] The separator of Comparative Example 3 has a lower lifespan and higher air permeability compared to the examples, and the separator of Comparative Example 4 has poor adhesion to the substrate, making it difficult to describe a strong bonding force between the electrode and the adhesive layer. In addition, the separator of Comparative Example 5 has a low bending strength, resulting in a lower lifespan and higher air permeability compared to the examples, and the separator of Comparative Example 6 has poor membrane resistance characteristics, and the lifespan characteristics of a lithium battery employing it are very poor, making it difficult to apply practically. From these results, it was found that by controlling the volume ratio of the first and second particles in the adhesive layer of the separators of Examples 1 to 4, the adhesive strength between the electrode and the separator can be strongly controlled, thereby manufacturing a lithium battery with improved lifespan characteristics.

[0260] While the above has been described with reference to drawings and examples, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent implementations are possible. Accordingly, the scope of protection of the present invention should be defined by the appended claims.

[0261] Although the above has been described with reference to a preferred manufacturing example, it will be understood by those skilled in the art that various modifications and changes can be made without departing from the spirit and scope of the claims set forth below.

Claims

1. A porous substrate, comprising an inorganic layer positioned on at least one surface of the porous substrate, and an adhesive layer positioned on the inorganic layer. The above adhesive layer contains first and second particles which are organic binders having different particle sizes, A separator for a secondary battery, wherein the mixing volume ratio of the first and second particles is 1:5 to 1:

35.

2. In the first paragraph, the first particle has a smaller size than the second particle, A secondary battery separator wherein the size of the first particle is 100 nm to 300 nm.

3. A secondary battery separator according to claim 1, wherein the size of the second particle is 500 nm to 900 nm.

4. A secondary battery separator in the first paragraph, wherein the thermal decomposition temperature of the first particle is 200°C or higher.

5. A secondary battery separator according to claim 1, wherein the glass transition temperature of the second particle is 40°C to 80°C.

6. A secondary battery separator in the first paragraph, wherein the total content of the first particle and the second particle is 60 to 98 parts by weight based on 100 parts by weight of the total weight of the adhesive layer.

7. In the first paragraph, the first particle and the second particle are independently selected from the group consisting of butyl methacrylate-ethylene glycol dimethacrylate copolymer, butyl methacrylate-ethylene glycol dimethacrylate-acrylonitrile copolymer, styrene-ethylhexylacrylate copolymer, styrene-ethylhexylacrylate-acrylonitrile copolymer, styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, acrylic rubber, butyl rubber, fluoroelastomer, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylate, polyacrylonitrile, polystyrene, A secondary battery separator comprising ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl cellulose, diacetyl cellulose or a combination thereof.

8. In the first paragraph, the first particle is a polymer obtained from a polymerizable monomer having a crosslinking functional group, A secondary battery separator wherein the crosslinkable functional group is a glycidyl group, an amino group, an N-methylol group, or a vinyl group.

9. A secondary battery separator according to claim 8, wherein the polymerizable monomer having a crosslinking functional group is a hydroxy ester of an ethylenically unsaturated carboxylic acid, a glycidyl ester of an ethylenically unsaturated carboxylic acid, an amino ester of an ethylenically unsaturated carboxylic acid, an ethylenically unsaturated amide containing a methylol group, a monomer having two or more vinyl groups, or a combination thereof.

10. In paragraph 9, The hydroxy ester of the above ethylenically unsaturated carboxylic acid includes (meth)acrylic acid hydroxypropyl, (meth)acrylic acid hydroxyethyl or a combination thereof, The glycidyl ester of the above ethylenically unsaturated carboxylic acid includes glycidyl (meth) acrylate, The amino ester of the above ethylenically unsaturated carboxylic acid includes dimethylamino ethyl (meth)acrylate, The above methylol group-containing ethylenically unsaturated amide includes N-methylol(meth)acrylamide, N,N-dimethylol(meth)acrylamide or a combination thereof, A secondary battery separator comprising a monomer having two or more vinyl groups, wherein the monomer comprises ethylene di(meth)acrylate, divinylbenzene or a combination thereof.

11. A secondary battery separator according to claim 1, wherein the separator comprises an adhesive layer or an inorganic layer disposed on the other side of the porous substrate.

12. A secondary battery separator in claim 11, wherein the volume ratio of the first particle and the second particle of the adhesive layer is 1:8 to 1:

40.

13. A separator for a secondary battery in the first paragraph, wherein the adhesive layer further comprises at least one adhesive binder selected from a fluorine-based resin, a polyacrylic acid-based compound, and a (meth)acrylic resin.

14. In the 13th paragraph, the fluorine-based resin is polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trichloroethylene copolymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer, or a combination thereof. The above polyacrylic acid compound is polyacrylic acid, polymethylacrylic acid, polyethylacrylic acid, polybutylacrylic acid, polyhexylacrylic acid, polyhydroxyethylmethacrylic acid, polyaminoacrylic acid or a combination thereof. The above (meth)acrylic resin is a secondary battery separator comprising polyacrylate, polymethacrylate, polybutylacrylate, polyacrylonitrile or a combination thereof.

15. In the first paragraph, an adhesive layer is disposed on the other side of the porous substrate, A separator for a secondary battery further comprising an inorganic layer between the adhesive layer and the porous substrate.

16. In the 15th paragraph, the inorganic layer includes inorganic particles and a binder, The above inorganic particles are Al2O3, SiO2, B2O3, Ga2O3, TiO2, SnO2, boehmite, BaSO4, MgO, Mg(OH)2, clay, ZnO, CaO, CeO2, NiO, GaO, ZrO2, Y2O3, SrTiO3, BaTiO3, or a combination thereof, a separator for a secondary battery.

17. A secondary battery separator in claim 16, wherein the content of the inorganic particles is 50 to 95 parts by weight based on 100 parts by weight of the total weight of the inorganic layer.

18. In paragraph 16, the binder is a crosslinkable binder, a non-crosslinkable binder, or a combination thereof, A secondary battery separator, wherein the non-crosslinkable binder is selected from the group consisting of polyvinylidene fluoride (PVdF) polymers, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxyl methyl cellulose, and acrylonitrile-butadiene-styrene copolymers, alone or in a mixture thereof.

19. In the 18th paragraph, the crosslinkable binder is a secondary battery separator which is poly(acrylic acid-co-acrylamide-co-2-acrylamido-2-methylpropanesulfonic acid), polyacrylamide-acrylic acid-hydroxyethyl acrylic copolymer, or a combination thereof.

20. A secondary battery comprising a positive electrode, a negative electrode, and a separator interposed between them and any one of claims 1 to 19.

Citation Information

Patent Citations

  • Separator for non-aqueous secondary battery and non-aqueous secondary battery

    JP2023040938A

  • Novel crispr associated protein and use thereof

    KR1020200018345A

  • System and method for ventilation of substation

    KR1020220081969A

  • Shoe member manufactured through graphene composite molded body

    KR1020230123046A

  • Life fuze