Lithium metal battery and preparation method therefor

The lithium metal battery design with a nitrile-based compound and specific lithium salts in the electrolyte layer addresses dendrite growth and capacity issues, enhancing performance and lifespan while reducing costs.

WO2024205169A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003726
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium metal batteries face challenges with dendrite growth and capacity degradation due to side reactions with the electrolyte, leading to reduced lifespan and energy density, and existing solutions do not adequately address these issues while increasing manufacturing costs.

Method used

A lithium metal battery design incorporating a nitrile-based compound and lithium salts like lithium difluorodioxalatoborate and lithium tetrafluoroborate in the electrolyte layer, which forms a robust Solid Electrolyte Interphase (SEI) film to inhibit dendrite growth and enhance lithium ion interaction, improving cycle performance and initial capacity.

Benefits of technology

The proposed battery structure and manufacturing method result in improved initial capacity and cycle performance by suppressing dendrite growth and enhancing lithium ion transfer, leading to a longer lifespan and reduced manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003726_03102024_PF_FP_ABST
    Figure KR2024003726_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a lithium metal battery and a preparation method therefor, the lithium metal battery comprising an anode, a cathode, and an electrolyte arranged between the anode and the cathode, wherein, in an X-ray photoelectron spectroscopy (XPS) analysis spectrum obtained for the surface of the anode, the ratio of an area (A1) for an Li1s peak to the total area (B1+B2) of an area (B1) for an F1s peak and an area (B2) for a B1s peak is 1:0.7 to 1:1.2, and the electrolyte comprises a nitrile-based compound, a lithium salt, and a carbonate-based compound, wherein the lithium salt comprises lithium difluoro(oxalato)borate (LiDFOB) and lithium tetrafluoroborate (LiBF4), and the amount of the nitrile-based compound is 3 wt% to 45 wt%, based on 100 wt% of the total weight of the electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium metal battery and manufacturing method thereof

[0001] It relates to a lithium metal battery and a method for manufacturing the same.

[0002] Lithium metal batteries primarily use carbon-based anode materials, such as graphite. Carbon-based anode materials exhibit no volume change during charge / discharge, contributing to the stability of lithium metal batteries. However, their low capacity necessitates the use of higher-capacity anode materials.

[0003] Lithium metal, which has a much larger theoretical electric capacity than carbon-based negative electrode materials, can be used as a negative electrode material.

[0004] When lithium metal is charged and discharged, dendrites are formed on the surface of the lithium metal due to a side reaction with the electrolyte, and the growth of the dendrites can cause a short circuit between the positive and negative electrodes, which can reduce the life characteristics of a lithium metal battery containing lithium metal.

[0005] Furthermore, despite their high energy density, lithium metal batteries suffer from rapid declines in battery capacity due to the difficulty in controlling dendritic lithium growth when lithium ions are electroplated onto the anode surface. To address this issue, the formation of a coating layer that inhibits lithium growth has been proposed. However, this method fails to provide satisfactory improvements in battery capacity and lifespan, and increases battery manufacturing costs, leaving room for improvement.

[0006] One aspect is to provide a lithium metal battery with a new structure.

[0007] Another aspect is to provide a method for manufacturing the above-described lithium metal battery.

[0008] In a lithium metal battery comprising a cathode, an anode, and an electrolyte layer disposed between the cathode and the anode according to one aspect,

[0009] In the X-ray photoelectron spectroscopy (XPS) analysis obtained for the above cathode surface, the ratio of the total area (B1+B2) of the area of ​​the Li1s peak (A1), the area of ​​the F1s peak (B1), and the area of ​​the B1s peak (B2) is 1:0.7 to 1:1.2.

[0010] The above electrolyte layer includes a nitrile compound, a lithium salt, and a carbonate compound,

[0011] The above lithium salts include lithium difluoro(oxalato)borate (LiDFOB) and lithium tetrafluoroborate (LiBF4).

[0012] A lithium metal battery is provided in which the content of the nitrile compound is 3 wt% to 45 wt% based on 100 wt% of the total weight of the electrolyte layer.

[0013] The above nitrile compound is butyronitrile, valeronitrile, propionitrile, acetonitrile, or a combination thereof.

[0014] The concentration of the lithium salt is 1 to 5 M. And the mixing weight ratio of LiDFOB and LiBF4 is 1:2 to 1:0.5.

[0015] The above carbonate compound is fluoroethylene carbonate (FEC), dimethyl carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, or a combination thereof.

[0016] In the Raman analysis spectrum obtained for the above cathode surface, the area (Ac) of the peak at wavenumbers 695 to 725 eV is 25 to 40%, or 27 to 40%, based on the total Raman analysis area of ​​the electrolyte layer.

[0017] The peak at wavenumbers 695 to 725 eV is a Li coordinated DFOB related peak.

[0018] Here, the total concentration of the lithium salt is 1.0 to 2.4 M, 1.0 to 1.6 M, for example, 1.2 M. The concentration of LiDFOB salt in the lithium salt is, for example, 0.6 M. And as the concentration of the lithium salt increases, the above area can increase proportionally.

[0019] In the Raman analysis spectrum obtained for the above cathode surface, the ratio of the area of ​​the peak at wavenumbers 695 to 725 eV (Ac) to the area of ​​the peak at wavenumbers 715 to 745 eV (Ad) (Ac / A) d ) is 0.4 to 1. The peak at wavenumber 715 to 745 eV is a free FEC related peak. Here, the total concentration of lithium salt is 1.0 to 2.4 M, 1.0 to 1.6 M, for example, 1.2 M. The concentration of LiDFOB salt in lithium salt is, for example, 0.6 M. The concentration of LiDFOB salt in lithium salt is, for example, 0.6 M. And as the concentration of lithium salt increases, the area can increase proportionally.

[0020] The above carbonate compound includes FEC and DEC, and the mixing weight ratio of FEC and DEC is 1:10 to 1:1.

[0021] The above negative electrode may include a negative electrode collector.

[0022] The above negative electrode further includes a lithium metal layer disposed on the negative electrode current collector,

[0023] The lithium metal layer may include a lithium metal foil, a lithium metal powder, a lithium alloy foil, a lithium alloy powder, or a combination thereof.

[0024] The above negative electrode may further include a protective layer disposed on the lithium metal layer.

[0025] The above electrolyte layer is a liquid electrolyte, a gel electrolyte, a solid electrolyte, or a combination thereof. The solid electrolyte may further include an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.

[0026] The lithium alloy contains lithium and a first metal, wherein the first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

[0027] The above negative electrode may include a negative electrode active material layer between a lithium metal layer and an electrolyte layer.

[0028] The positive electrode includes a positive electrode current collector and a positive electrode active material layer, and at least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one or both sides of the base film, and the base film includes a polymer, and the polymer includes polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof.

[0029] The above metal layer includes indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0030] The above lithium metal battery may further include a separator.

[0031] Steps for preparing the cathode according to other aspects;

[0032] Steps to prepare the anode;

[0033] A step of preparing an assembly using the above positive and negative electrodes; and

[0034] A step of providing an electrolyte layer to the above assembly is included,

[0035] The above electrolyte layer includes a nitrile compound, a lithium salt, and a carbonate compound,

[0036] The above lithium salts include lithium difluorodioxalatoborate (LiDFOB) and lithium tetrafluoroborate (LiBF4).

[0037] A method for manufacturing a lithium metal battery is provided, which manufactures the above-described lithium metal battery in which the content of the nitrile compound is 3 wt% to 45 wt% based on 100 wt% of the total weight of the electrolyte layer.

[0038] In the step of preparing the above assembly, a separator can be placed between the positive and negative electrodes.

[0039] According to one aspect, a lithium metal battery with improved initial capacity and cycle performance is provided by using an electrolyte layer containing a nitrile compound and a carbonate compound having strong interactions between cations and anions.

[0040] Figure 1a schematically illustrates the laminated structure of a lithium metal battery according to an embodiment.

[0041] Figure 1b schematically illustrates a laminated structure of a lithium metal battery according to another embodiment.

[0042] Figures 2a to 2f show XPS analysis spectra of the lithium metal surface of the lithium metal batteries of Example 1 and Comparative Example 1.

[0043] Figure 3a is a Raman analysis spectrum of F1s on the lithium metal surface in the lithium metal battery of Example 1.

[0044] Figure 3b is a Raman analysis spectrum of F1s on the lithium metal surface in the lithium metal battery of Comparative Example 1.

[0045] Figure 4 is a graph showing charge / discharge characteristics of the lithium metal battery of Example 9 and the lithium ion battery of Comparative Example 4.

[0046] Figure 5 is a schematic diagram of a lithium metal battery according to an embodiment.

[0047] Figure 6 is a schematic diagram of a lithium metal battery according to another embodiment.

[0048] Figure 7 is a schematic diagram of a lithium metal battery according to another embodiment.

[0049] <Explanation of key symbols in the drawing>

[0050] 1: Lithium metal battery 2, 20: Cathode

[0051] 3, 10: Anode 4: Separator

[0052] 5: Battery case 6: Cap assembly

[0053] 7: Battery structure 8: Electrode tab

[0054] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present inventive concept to specific embodiments, but rather to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.

[0055] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. Hereinafter, the terms "comprises" or "has" and the like are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below may be interpreted as "and" or "or" depending on the context.

[0056] In order to clearly express various layers and regions in the drawings, the thickness is shown enlarged or reduced. Similar parts are designated by the same drawing reference numerals throughout the specification. When a part such as a layer, film, region, or plate is said to be "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals, and redundant descriptions are omitted.

[0057] In the present disclosure, the "particle diameter" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter of a particle can be measured using a particle size analyzer (PSA). The "particle diameter" of a particle is, for example, the average particle diameter. The average particle diameter is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of a particle corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, laser diffraction. The average particle diameter and average major axis length of a particle can be measured using a scanning electron microscope. When the particle size is measured using a scanning electron microscope, it is determined as the average value of 30 or more randomly selected particles having a size of 1 μm or more, excluding fine particles.

[0058] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.

[0059] In this disclosure, “alloy” means a mixture of two or more metals.

[0060] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.

[0061] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.

[0062] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.

[0063] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.

[0064] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.

[0065] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.

[0066] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.

[0067] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.

[0068] In the present disclosure, thickness means average thickness.

[0069]

[0070] Hereinafter, a lithium metal battery and a manufacturing method thereof according to embodiments will be described in more detail.

[0071] A non-cathode lithium metal battery is a battery that uses only a cathode current collector without a cathode active material layer. When charging, lithium ions transferred from the cathode are deposited / electrodeposited on the surface of the cathode current collector, and when discharging, the lithium deposited / electrodeposited on the cathode current collector is eluted again and inserted into the cathode, thereby operating the battery.

[0072] In a cathode-free lithium metal battery, lithium metal is not added during battery assembly. However, as lithium ions generated at the anode transform into lithium during the process of transitioning to the anode, they are converted into lithium and attached to the anode through electroplating, minimizing unused space and significantly improving the battery's energy density. However, if the growth method of lithium metal is not controlled, precipitation or dendrite growth toward the anode can occur, leading to irreversible reactions within the battery or increased current.

[0073] The present inventors have solved the above-described problem and provided a lithium metal battery using an electrolyte layer containing a solvent designed to form clusters having a coordination structure with a solvent that is a component of an SEI (Solid Electrolyte Interphase) film existing on the surface of an anode, so as to suppress dendrite growth on a lithium metal, wherein the components constituting the film are the same, but can move more to the surface of the anode or can form a film earlier than when formed as a single substance during film formation. As a result, a more solid SEI film is formed on the surface of the lithium anode.

[0074] A lithium metal battery according to an embodiment includes an anode, an anode, and an electrolyte layer disposed between the anode and the cathode, and in an X-ray photoelectron spectroscopy (XPS) analysis obtained for the surface of the anode, a ratio of the total area (B1+B2) of the area of ​​the Li1s peak (A1), the area of ​​the F1s peak (B1), and the area of ​​the B1s peak (B2) of the Li1s peak is 1:0.7 to 1:1.2, and the electrolyte layer includes a nitrile compound, a lithium salt, and a carbonate compound, and the lithium salt includes lithium difluoro(oxalato)borate (LiDFOB) and lithium tetrafluoroborate (LiBF4), and the content of the nitrile compound is 3 wt% to 45 wt% based on 100 wt% of the total weight of the electrolyte layer.

[0075] In the XPS analysis spectrum obtained for the above cathode surface, the ratio of the total area (B1+B2) of the area of ​​the F1s peak (B1) and the area of ​​the B1s peak (B2) and the area of ​​the O1s peak (C1) is in the range of 1:0.6 to 1:1.3.

[0076] In the above XPS analysis spectrum, the ratio of the area of ​​the Li1s peak (A1) originating from the cation and the area of ​​the F1s peak (B1) originating from the anion and the total area (B1+B2) of the B1s peak has a range of, for example, 1:0.75 to 1:2, 1:0.8 to 1:2, 1:0.85 to 1:2, 1:0.9 to 1:2, or 1:0.95 to 1:2.

[0077] In the XPS analysis spectrum obtained for the above cathode surface, the ratio of the total area (B1+B2) of the area of ​​the F1s peak (B1) and the area of ​​the B1s peak (B2) originating from the anion, and the area of ​​the O1s peak originating from the anion (C1) is, for example, in the range of 1:0.6 to 1:1.25, 1:0.6 to 1:1.2, 1:0.6 to 1:1.1, 1:0.7 to 1:1.1, 1:0.75 to 1:1.1, 1:0.8 to 1:1.1, 1:0.85 to 1:1.1, or 1:0.9 to 1:1.1.

[0078] The XPS analysis spectrum obtained for the above negative electrode is an XPS analysis spectrum obtained for the lithium metal surface. In the XPS spectrum, the Li1s peak is related to cations, the F1s peak and B1s peak are related to anions, and the O1s peak is related to solvents and anions.

[0079] The electrolyte layer includes a nitrile compound, a lithium salt, and a carbonate compound, and the lithium salt includes lithium difluorodioxalatoborate (LiDFOB) and lithium tetrafluoroborate (LiBF4). A lithium metal battery is provided in which the content of the nitrile compound is 3 wt% to 45 wt% based on 100 wt% of the total weight of the electrolyte layer.

[0080] The above negative electrode may include a negative electrode current collector and lithium metal.

[0081] The concentration of the lithium salt is 1 to 5 M, 1 to 3 M, 1.0 to 2.4 M, 1.0 to 1.6 M. The mixing weight ratio of the LiDFOB and LiBF4 is 1:2 to 1:0.3, or 1:1.5 to 1:0.5. When the concentration of the lithium salt and the mixing weight ratio of LiDFOB and LiBF4 are within the above ranges, a lithium metal battery having improved performance can be manufactured. If the content of LiBF4 is greater than the above range, the nitrile-based compound exhibits better interaction with LiDFOB, but the probability of encountering LiDFOB is greatly reduced, which may be disadvantageous for film formation, and if the content of LiDFOB is greater than the above range, the viscosity of the electrolyte layer increases, which may lower the mobility, thereby reducing the initial capacity of the lithium metal battery.

[0082] In lithium metal batteries, the control of lithium ion deposition and desorption directly impacts their lifespan. Therefore, it is common to use large quantities of salts that impair lithium dissociation properties to improve their performance.

[0083] However, in a lithium metal battery according to an embodiment, the inorganic component of the cathode film is strengthened through the use of a nitrile compound, which is a medium that enables the movement of anions to the cathode along with lithium.

[0084] In lithium metal batteries, two types of salts are used as the electrolyte layer to ensure the long cycle life of lithium deposition. One of the two salts is a film-forming salt to form a robust film, while the other is a lithium salt that facilitates lithium ion transport during continuous charge and discharge. In this case, the two salts have different affinities for lithium cations, which results in a failure of lithium salt dissociation. This necessitates the use of a solvent that can aid dissociation, in addition to the solvents used in conventional lithium-ion batteries. Therefore, in a lithium metal battery according to one embodiment, a nitrile-based compound, such as butyronitrile, with improved anion interaction can be applied, thereby improving the long cycle life and resistance characteristics.

[0085] Nitrile compounds utilize neutral molecules with enhanced anion interactions in addition to lithium cation interactions. Using an electrolyte layer containing these nitrile compounds can provide lithium metal batteries with improved lifespan and reduced resistance.

[0086] The composition of the SEI layer present on the lithium metal surface can be analyzed through the XPS analysis spectrum obtained for the lithium metal surface. The XPS analysis spectrum obtained for the lithium metal surface is for the lithium metal surface charged at a current corresponding to 0.05 to 0.2 of the capacity, and in the case of the second cycle or less after formation of the lithium metal battery, which is involved in the film formation.

[0087] In a lithium metal battery according to one embodiment, if a nitrile compound such as butyronitrile (BN), which has excellent affinity for both cations and anions, is used on the negative electrode surface, cations and anions (difluorooxalateborate anions or tetrafluoroborate anions) are bonded to BN, so that when Li cations move from the positive electrode to the anions, the content of anions on the negative electrode surface increases, and when lithium cations are electrodeposited, the effect of forming a film including a performing anion on the surface is obtained. In the existing electrolyte layer, the structure of lithium metal surface / cation / solvent is obtained, and the solvent is decomposed to form an SEI, and the formation of an organic SEI may deteriorate the performance of the lithium metal battery.

[0088] However, in a lithium metal battery according to an embodiment, the use of a nitrile compound such as BN can form an SEI with an increased inorganic (anion) content on the lithium metal surface. As a result, the performance of the lithium metal battery is improved.

[0089] If a nitrile compound is not added to the electrolyte layer, electrons are supplied to lithium ions on the negative electrode current collector, forming a lithium electrodeposited layer. The solvent components surrounding the lithium ions decompose, forming an SEI layer containing organic substances on the lithium metal surface. However, if the SEI layer contains organic substances, the lifespan characteristics of the lithium metal battery may be reduced.

[0090] Nitrile compounds are neutral molecules with very strong lithium cation and anion interactions. Their use can induce anions to migrate along with the initial charge of lithium ions from the positive to negative electrodes. This, in turn, induces the presence of more anions at the negative electrode, resulting in an abundance of clustered solvation structures, thereby forming a robust film rich in boron and fluorine anions.

[0091] When the content of the nitrile compound is within the above range, the ions are not completely dissociated, and clusters in which three or more ions exist simultaneously increase, and these clusters have different configurations even though the constituent materials themselves are the same, so they form a film before other structures. These nitrile compounds have excellent cation and anion interactions, and thus have excellent affinity for cations and anions. Therefore, when this is used, anions increase in addition to cations around lithium, so that an SEI layer with an increased inorganic content can be formed on the lithium metal surface. At this time, the thickness of the SEI layer is 50 nm or less, 30 nm or less, or 1 to 25 nm. When an SEI layer with an increased inorganic content exists on the lithium metal surface in this way, a lithium metal battery with improved life characteristics can be manufactured.

[0092] Nitrile compounds have the property of bringing in anions, and thus the performance of lithium metal batteries is improved due to the film that increases the anions. If the content of the nitrile compound is less than 3 wt% based on 100 wt% of the total weight of the electrolyte layer, the effect of the existence of anions other than the solvent around the lithium is minimal, and if it exceeds 45 wt%, solvents such as VC, VEC, and FEC are not contained in the cluster containing the lithium salt and solvent, and thus hardly participate in the formation of the SEI film. As a result, the SEI film is formed only with salts and nitrile compounds such as BN, which may deteriorate the performance of the lithium metal battery.

[0093] Nitrile compounds include, for example, butyronitrile, valeronitrile, propionitrile, acetonitrile, or combinations thereof. The dipole moments, lithium cation interaction energies, and dipole moments of butyronitrile, valeronitrile, fluoroethylene, and dimethyl carbonate are shown in Table 1 below. Table 2 also shows the dipole moments, lithium cation interaction energies, and dipole moments for solvents.

[0094] Distinction Li+ Interaction Energy (eV) Anion Interaction Energy (eV) Dipole Moment (eV) Valeronitrile-1.71-0.154.09 Butyronitrile-1.69-0.164.12 Propionitrile-1.65-0.094.14 Acetonitrile-1.61-0.114.03

[0095] DistinctionLi+ Interaction Energy (eV)Anion Interaction Energy (eV)Dipole Moment (eV)EC-1.86-0.365.63FEC-1.65-0.435.05DMC-1.70.160.19DEC-1.920.120.35

[0096] As shown in Table 1, for nitrile compounds, the solvent must have Li as compared to low-viscosity commercial solvents such as DMC or DEC. +Although the interaction energy is relatively weak, it was confirmed that the anion interaction energy and dipole moment were greatly improved while securing the FEC level, so it was found that it was greatly improved as a low-viscosity solvent compared to other commercial solvents. However, since solvents also interact with each other, the presence or absence of aggregate structure formation and resistance characteristics in the mixture state must be considered.

[0097] When the formation of the aggregate structure and the dissociation equilibrium constant were confirmed, it was found that the characteristics were the best when BN was maintained at 3 wt% to 45 wt%.

[0098] The content of the above carbonate compound is 30 to 95 wt%, or 40 to 90 wt%, based on 100 wt% of the total weight of the nitrile compound and the carbonate compound.

[0099] When the content of the carbonate compound is within the above range, the properties of the salt and organic matter within the lithium salt coordination cluster are appropriately controlled, thereby improving lithium mobility and manufacturing a lithium metal battery with improved initial capacity and lifespan characteristics. If the content of the carbonate compound exceeds 90 wt%, the proportion of clusters of an appropriate size decreases, thereby changing the SEI film composition, which can be confirmed by complex system calculations utilizing equilibrium energy.

[0100] The above carbonate compound includes FEC and DEC, and the mixing weight ratio of FEC and DEC is 1:10 to 1:1, 1:8 to 1:1, 1:5 to 1:1, or 1:3 to 1:1.

[0101] In the above Raman analysis spectrum, wave numbers 695 to 725 cm -1The peak area (Ac) is 25 to 40%, or 27 to 40%, of the total Raman analysis area of ​​the electrolyte layer. The total concentration of the lithium salt during the Raman analysis spectrum investigation is 1.0 to 2.4 M, 1.0 to 1.6 M, for example, 1.2 M. The concentration of LiDFOB salt in the lithium salt is, for example, 0.6 M. The area increases proportionally as the lithium salt concentration in the electrolyte layer increases.

[0102] In the above Raman analysis spectrum, wave numbers 695 to 725 cm -1 The ratio of the area of ​​the peak (Ac) to the area of ​​the peak at wavenumbers 715 to 745 eV (Ac / A) d ) is 0.4 to 1. When examining this Raman analysis spectrum, the total concentration of lithium salt here is 1.0 to 2.4 M, 1.0 to 1.6 M, for example, 1.2 M. The concentration of LiDFOB salt in the lithium salt is, for example, 0.6 M.

[0103] The ratio of the above areas (Ad) (Ac / A) d ) increases proportionally as the lithium salt concentration in the electrolyte layer increases.

[0104] Here, the peak (peak c) at wavenumbers 695 to 725 eV is the Li coordinated DFOB-peak, the peak (peak d) at wavenumbers 715 to 745 eV is for free FEC, and the peak (peak e) at wavenumbers 735 to 750 eV is for Li+ coordinated FEC peak.

[0105] The electrolyte layer according to the present invention may further contain a non-aqueous organic solvent in addition to the above-described carbonate compound.

[0106] Non-aqueous organic solvents that can be used include carbonate, ester, ether, ketone, alcohol, or aprotic solvents.

[0107] Examples of the carbonate solvent that can be used include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethylmethyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylethylene carbonate, etc. Examples of the ester solvent that can be used include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methylpropionate, ethylpropionate, decanolide, mevalonolactone, caprolactone, etc. Examples of the ether solvents that can be used include diethyl ether, dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, and tetrahydrofuran. Examples of the ketone solvents that can be used include cyclohexanone. Examples of the alcohol solvents that can be used include ethyl alcohol, isopropyl alcohol, and the like, and examples of the aprotic solvents that can be used include amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, 1,4-dioxolane, sulfolanes, and sulfoxides.

[0108] In terms of cell performance, a lithium metal battery according to an embodiment of the present invention can improve the initial capacity by increasing the total amount of lithium salt that can be dissolved or increasing the number of available Li ions in an electrolyte layer with the same salt concentration if the cation affinity of the solvent is strong, and the cycle performance of the lithium metal battery can be improved if the anion affinity of the molecule is strong.

[0109] In a lithium metal battery according to an embodiment, the negative electrode includes a negative electrode current collector.

[0110] The above negative electrode further includes a lithium metal layer disposed on the negative electrode current collector,

[0111] The above lithium metal layer includes a lithium metal foil, a lithium metal powder, a lithium alloy foil, a lithium alloy powder, or a combination thereof.

[0112] The lithium alloy contains lithium and a first metal, wherein the first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

[0113] The above negative electrode contains a negative electrode active material layer between a lithium metal layer and an electrolyte layer, and the negative electrode active material layer contains a carbon-based material; a mixture of a carbon-based material and at least one selected from a metal and a metalloid; a composite of a carbon-based material and at least one selected from a metal and a metalloid; or a combination thereof.

[0114] The above carbon-based material includes amorphous carbon, and the average particle diameter of the amorphous carbon is 10 nm to 100 nm, and the carbon-based material includes carbon black, carbon nanotubes, carbon nanofibers, fullerene, activated carbon, carbon fibers, or a combination thereof.

[0115] The above negative electrode further includes a protective layer disposed on the lithium metal layer.

[0116] The electrolyte of the above electrolyte layer includes a liquid electrolyte, a gel electrolyte, a solid electrolyte, or a combination thereof, and the solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0117] By using a lithium metal battery according to one embodiment, a method of increasing the participation of a lithium salt, which is expensive compared to a solvent, in the SEI film can reduce the battery manufacturing cost. In addition, it is known that forming a solvation structure that does not completely dissociate significantly reduces ionic conductivity and shortens the lifespan of a lithium ion battery. However, in a lithium metal battery according to one embodiment, by using an electrolyte layer having an incompletely dissociated solvation structure, side reactions occurring during the process of lithium electrodeposition on a negative electrode current collector can be effectively suppressed, thereby improving the lifespan.

[0118] According to one embodiment, when a lithium metal battery uses an electrolyte layer containing a nitrile compound such as butyronitrile, when neutral molecules are coordinated around Li during the formation of a solvation structure of Li ions, more of the electrolyte layer is located inside the first shell during the solvation process, and since the lithium metal battery electrolyte layer is friendly to cations and anions, anions are also located. In the case of a lithium ion battery solvent used for complete dissociation of lithium ions, it is advantageous to induce complete solvation, so a substance that is friendly to lithium cations but relatively less friendly to anions is used. When such a solvent is used, the lithium transfer characteristics are rather poor in general lithium ion batteries, so it is not used. However, when applied to a lithium metal battery according to one embodiment, a strong film is unexpectedly formed on the surface of the negative electrode, which can effectively improve the growth of lithium metal.

[0119] When a cation, anion, and electrolyte layer by a single embodiment exist inside the first solvation shell, one or more ions already exist, and this can form a structure in which three or more cations and anions can exist due to reasons such as the balance of attractive forces between them.

[0120] During the first charge, anions move to the lithium surface along with the movement of lithium ions. At this time, as lithium ions are deposited and converted into lithium metal, a SEI film is formed on the surface. This film usually contains organic substances containing cations and some anions, but according to one embodiment, since more anions move along the lithium, the amount of anion components increases, and this film improves the performance of the lithium metal battery.

[0121] Referring to Fig. 1a, an electrolyte layer (30) is laminated on a negative electrode current collector (21). The negative electrode (20) contains the negative electrode current collector (21), and the negative electrode active material layer is absent. The electrolyte layer (30) may contain a separator.

[0122] The membrane contains a porous substrate, wherein the porous substrate contains polypropylene, polyethylene, or a combination thereof.

[0123] The electrolyte layer may contain an electrolyte, which may be a solid electrolyte, a gel electrolyte, a liquid electrolyte, or a combination thereof.

[0124] A positive electrode (10) is placed on top of the electrolyte layer (30). The positive electrode (10) contains a positive electrode active material layer (12) and a positive electrode current collector (11).

[0125] An electrolyte may be further included between the separator (30) and the anode (10). The electrolyte may be a gel electrolyte, a solid electrolyte, a liquid electrolyte, or a combination thereof.

[0126] A protective layer may be further disposed on the negative electrode collector (21).

[0127] The electrolyte layer (30) is, for example, a separator containing a porous substrate. The pores of the separator may contain a liquid electrolyte or a gel-type polymer electrolyte containing a liquid electrolyte and a crosslinked polymer.

[0128] The pore diameter of the separator is generally 0.01 to 10 μm, and the thickness can generally be 5 to 20 μm. Examples of such separators include sheets or non-woven fabrics made of olefin-based polymers such as polypropylene, glass fiber, or polyethylene. When a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte may also function as the separator.

[0129] Among the above separation membranes, specific examples of olefin-based polymers include polyethylene, polypropylene, or a multilayer membrane of two or more layers thereof, and mixed multilayer membranes such as a polyethylene / polypropylene two-layer separation membrane, a polyethylene / polypropylene / polyethylene three-layer separation membrane, and a polypropylene / polyethylene / polypropylene three-layer separation membrane may be used.

[0130] According to another embodiment, a ceramic coating layer can be formed on both sides of a porous substrate constituting a separator.

[0131] Forming a ceramic coating layer can improve cell performance in lithium batteries by suppressing lithium dendrite formation through the rigidity of the ceramic coating layer without significantly increasing cell resistance. Furthermore, employing a separator with the aforementioned ceramic coating layer ensures heat resistance, improving heat shrinkage characteristics and reducing the separator margin for safety during cell design, thereby reducing the material cost of lithium batteries. Furthermore, by physically inhibiting dendrite growth on the anode, long-term lifespan at both room and high temperatures can be improved.

[0132] The ceramic coating layer includes inorganic particles and a binder.

[0133] Any inorganic particle that can be used when forming a coating layer of a separation membrane can be used, and for example, any one of the inorganic oxides of SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZnO2, Mg(OH)2, AIN(Aluminum Nitride), SiC(Silicon Carbide), BoN(Boron Nitride), or a combination thereof can be used.

[0134] Inorganic particles include BaTiO3, BaTiO3, Pb(Zr,Ti)O3 (PZT), and Pb with a dielectric constant of 5 or higher. 1-a La a Zr 1-b Ti b O3 (PLZT, where, 0 <a<1, 0<b<1임), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC or a combination thereof can be used.

[0135] In addition to the ceramic coating layer, the inorganic particles having lithium ion transfer capability, i.e. lithium phosphate (Li3PO4), lithium titanium phosphate (Li c Ti d (PO4)3, 0 <d<2, 0<d<3), 리튬알루미늄티타늄포스페이트 (Li a1 Al b1 Ti c1 (PO4)3, 0 <a1<2, 0<b1<1, 0<c1<3), 14Li2O-9Al2O3-38TiO2-39P2O5 등과 같은 (LiAlTiP) a2 O b2 Series Glass (0) <a2<4, 0<b2<13), 리튬란탄티타네이트 (Li a3 La b3 TiO3, 0 <a3<2, 0<b3<3), Li 3.25 Ge 0.25 P 0.75Lithium germanium thiophosphate (Li) such as S4 a4 Ge b4 P c2 S d , 0 <a4<4, 0<b4<1, 0<c2<1, 0<d<5), Li3N 등과 같은 리튬나이트라이드 (Li a5 N b5 , 0 <a5<4, 0<b5<2), Li3PO4-Li2S-SiS2 등과 같은 SiS2 계열 글래스 (Li a6 Si b6 S c3 , 0 <a6<3, 0<b6<2, 0<c4<4), LiI-Li2S-P2S5 등과 같은 P2S5 계열 글래스 (Li a7 P b7 S c5 , 0 <a7<3, 0<b7<3, 0<c5<7) 또는 이들의 혼합물 등이 더 함유될 수 있다.

[0136] The above liquid electrolyte contains a lithium salt and an organic solvent.

[0137] As the organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxy franc, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyrropionate, ethyl propionate, etc. can be used. Carbonate solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, and diethyl carbonate can be used.

[0138] The above lithium salt can be any one that is commonly used in lithium secondary batteries, and as a material that is easily dissolved in the non-aqueous solvent, for example, one or more of the following materials can be used: LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2)3, LiC(FSO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, and LiB(C2O4)2.

[0139] The concentration of the lithium salt may be, for example, 1 to 5 M, 1 to 3 M, 1 to 2.5 M, 1.0 to 2.4 M, or 1.0 to 1.6 M in the liquid electrolyte. In the above range, a sufficient amount of lithium ions required for charging and discharging a lithium metal battery can be generated.

[0140] As shown in Fig. 1b, a negative electrode active material layer (22) can be placed between the negative electrode current collector (21) and the separator (30).

[0141] According to one embodiment, the negative electrode active material layer (22) can be arranged during the assembly of the lithium metal battery. According to another embodiment, the negative electrode active material layer can include a negative electrode active material layer by plating lithium metal after charging. The negative electrode active material layer can be a lithium plating layer (plated lithium layer).

[0142] The above negative electrode active material layer (22) includes lithium metal or a lithium alloy.

[0143] The thickness of the above-mentioned negative electrode active material layer is 1 to 500 um or 10 to 500 um. When the thickness of the negative electrode active material layer is within the above range, the cycle characteristics of the lithium metal battery are improved without reducing the energy density.

[0144] When the negative electrode active material layer is placed at the time of assembly, it may include only a carbon-based material, a carbon-based material, and at least one selected from metals and metalloids.

[0145] The carbon-based material includes amorphous carbon, and the average particle diameter of the amorphous carbon is 10 nm to 100 nm, and the carbon-based material includes carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, or a combination thereof.

[0146] The above negative active material layer includes a lithium metal foil, a lithium metal powder, a lithium alloy foil, a lithium alloy powder, or a combination thereof, wherein the lithium alloy contains lithium and a first metal.

[0147] The first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

[0148] The negative electrode active material layer (22) may include, for example, lithium foil, lithium powder, or a combination thereof. The lithium foil may include, for example, lithium metal foil, lithium alloy foil, or a combination thereof. The lithium powder may include lithium metal powder, lithium alloy powder, or a combination thereof. A lithium alloy is an alloy of lithium and another metal that can be alloyed with lithium, such as a lithium-silver alloy, a lithium-zinc alloy, a lithium-magnesium alloy, or a lithium-tin alloy. The negative electrode active material layer including a lithium metal foil may be, for example, a lithium metal layer. The negative electrode active material layer including a lithium alloy foil may be, for example, a lithium alloy layer. The negative electrode active material layer including a lithium metal powder and / or a lithium alloy powder may be introduced by coating a slurry including lithium powder and a binder, etc., on a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer can be made of a metal-based negative electrode active material.

[0149] The negative electrode current collector is composed of a material that does not react with lithium, i.e., does not form an alloy or compound. The material constituting the negative electrode current collector includes, but is not limited to, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), and any material that is used as an electrode current collector in the relevant technical field may be used. The negative electrode current collector may be composed of one of the above-mentioned metals, or may be composed of an alloy or a coating material of two or more metals. The negative electrode current collector is, for example, in the form of a plate or foil.

[0150] In a lithium metal battery according to an embodiment, a protective layer may be further introduced between the negative electrode current collector and the separator. It is also possible to introduce a protective layer further between the negative electrode active material layer and the separator.

[0151] The protective layer contains a polymer such as polyvinyl alcohol, polyimide, vinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride, carboxymethyl cellulose, styrene butylene rubber, or a polymer and an inorganic filler. Inorganic fillers include, for example, SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZnO2, Mg(OH)2, Aluminum Nitride (AlN), Silicon Carbide (SiC), Boron Nitride (BoN), or a combination thereof. Introducing an additional protective layer in this way can minimize contact between lithium and the electrolyte, thereby reducing side reactions, and can suppress lithium dendrite growth by creating a uniform flow of lithium ions throughout the electrode.

[0152] The thickness of the protective layer is, for example, 1 to 20 um.

[0153] In one embodiment of the present invention, the positive electrode current collector (11) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film can be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse, which may be cut in the event of an overcurrent to prevent a short circuit. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer may be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the negative electrode current collector (521b, 522b) decrease, thereby improving the stability of the lithium battery in the event of a short circuit. A lead tab may be added on the metal layer for external connection. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the base film and / or the metal layer may be melted, electrically connecting the metal layer to the lead tab. In order to strengthen the welding of the metal layer and the lead tab, a metal piece may be added between the metal layer and the lead tab. The metal piece may be a thin piece of the same material as the metal of the metal layer.The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, an aluminum foil, a copper foil, a SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate by welding the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the welding process. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to ㎛. Since the metal layer has a thickness within this range, the stability of the electrode assembly can be secured while maintaining conductivity. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure as the negative electrode collector, the weight of the electrode can be reduced, and as a result, the energy density can be improved.

[0154] In one embodiment of the present invention, the positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may additionally include a metal piece and / or a lead tab. For more specific details regarding the base film, metal layer, metal strip, and lead tab of the positive electrode current collector, refer to the negative electrode current collector described above. By having this structure, the positive electrode current collector can reduce the weight of the electrode, thereby improving energy density.

[0155] The negative electrode active material layer may contain a negative electrode active material and a binder.

[0156] The negative active material has, for example, a particle form. The average particle diameter of the negative active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the negative active material has an average particle diameter in this range, reversible plating and / or dissolution of lithium can be facilitated during charge and discharge. The average particle diameter of the negative active material is, for example, a median diameter (D50) measured using a laser particle size distribution analyzer.

[0157] The negative electrode active material may include, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material. The carbon-based negative electrode active material may be, for example, amorphous carbon. Examples of the carbon-based negative electrode active material include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., and any material classified as amorphous carbon in the relevant technical field may be used. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon. The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium, and therefore is not a metal negative electrode active material in the present specification. The negative electrode active material layer includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture may be, for example, 10:1 to 1:2, 10:1 to 1:1, 7:1 to 1:1, 5:1 to 1:1, or 4:1 to 2:1 by weight.The negative electrode active material included in the negative electrode active material layer may include a mixture of first particles made of, for example, amorphous carbon and second particles made of a metal or a metalloid. The metal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, a lithium metal battery are further improved.

[0158] The binder included in the negative electrode active material layer may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders. When the negative electrode active material layer does not include a binder, the negative electrode active material layer can be easily separated from the ceramic coating layer (21) or the negative electrode current collector (21). The content of the binder included in the negative electrode active material layer may be, for example, 1 to 20 wt% based on the total weight of the negative electrode active material layer.

[0159] When the negative electrode active material layer is present, the thickness of the negative electrode active material layer may be, for example, 1% to 50%, 1% to 30%, 1% to 10%, or 1% to 5% of the thickness of the positive electrode active material layer. If the thickness of the negative electrode active material layer is too thin, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the thickness of the negative electrode active material layer increases excessively, the energy density of the lithium metal battery employing the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics.

[0160] When the thickness of the negative electrode active material layer decreases, the charge capacity of the negative electrode active material layer also decreases, for example. The charge capacity of the negative electrode active material layer may be, for example, 0.1% to 50%, 1% to 30%, 1% to 10%, 1% to 5%, or 1% to 2% of the charge capacity. If the charge capacity of the negative electrode active material layer is too small, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the charge capacity of the negative electrode active material layer increases excessively, the energy density of the lithium metal battery using the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics. The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the positive electrode active material layer. The charge capacity of the negative electrode active material layer is also calculated in the same way. That is, the charge capacity of the negative electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer. When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values ​​is the capacity of the negative electrode active material layer. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is the estimated capacity using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the negative electrode active material layer are directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the negative electrode active material layer may be the initial charge capacity measured at the first charge cycle.

[0161] [Lithium metal battery]

[0162] According to one embodiment, a lithium metal battery includes a positive electrode; a negative electrode; and a separator disposed between the positive electrode and the negative electrode. Such a lithium metal battery can simultaneously provide excellent life characteristics. The lithium metal battery may be, but is not limited to, a lithium primary battery, a lithium secondary battery, a lithium-sulfur battery, a lithium-air battery, etc., and any lithium metal battery used in the relevant technical field may be used.

[0163] Lithium metal batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.

[0164] (anode)

[0165] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.

[0166] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c Dc (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G dO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.

[0167] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0168] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO 4-b X b (Here, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).

[0169] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.

[0170] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.

[0171] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.

[0172] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium metal battery, one or more of the conductive agent, binder, and solvent may be omitted.

[0173] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.

[0174] The positive electrode current collector is, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may be omitted. The positive electrode current collector (11) may further include a carbon layer disposed on one or both sides of the metal substrate. By additionally disposing the carbon layer on the metal substrate, the metal of the metal substrate is prevented from being corroded by the solid electrolyte included in the positive electrode layer, and the interface resistance between the positive electrode active material layer (12) and the positive electrode current collector (11) can be reduced. The thickness of the carbon layer may be, for example, 1 ㎛ to 5 ㎛, 1 ㎛ to 4 ㎛, or 1 ㎛ to 3 ㎛. If the thickness of the carbon layer is too thin, it may be difficult to completely block contact between the metal substrate and the solid electrolyte. If the carbon layer is too thick, the energy density of the all-solid-state secondary battery may be reduced. The carbon layer may include amorphous carbon, crystalline carbon, etc.

[0175] The thickness of the positive electrode current collector is, for example, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 25 μm, or 10 μm to 20 μm. The thickness of the positive electrode current collector is not necessarily limited to the above-described thickness range and may be selected depending on the required characteristics of the lithium metal battery.

[0176] The cathode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. By having such a structure, the cathode current collector can reduce the weight of the electrode and consequently improve the energy density of a lithium metal battery.

[0177] (Separator)

[0178] Next, a separator to be inserted between the anode and cathode is prepared.

[0179] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion transport and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in nonwoven or woven form. For lithium-ion batteries, rollable separators, such as polyethylene or polypropylene, are used, while for lithium-ion polymer batteries, separators with excellent organic electrolyte absorption capacity are used.

[0180] The membrane is manufactured by the following exemplary method, but is not limited to this method and may be adjusted according to required conditions.

[0181] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast onto a support and dried, and then a separator film peeled from the support is laminated onto the electrode to form a separator.

[0182] The polymer used in membrane manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.

[0183] (cathode)

[0184] The cathode contains a cathode current collector.

[0185] In one embodiment of the present invention, the negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film can be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse, which may be cut in the event of an overcurrent to prevent a short circuit. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer may be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the negative electrode current collector (521b, 522b) decrease, thereby improving the stability of the lithium battery in the event of a short circuit. A lead tab may be added on the metal layer for external connection. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the base film and / or the metal layer may be melted, electrically connecting the metal layer to the lead tab. In order to strengthen the welding of the metal layer and the lead tab, a metal piece may be added between the metal layer and the lead tab. The metal piece may be a thin piece of the same material as the metal of the metal layer.The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, an aluminum foil, a copper foil, a SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate by welding the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 μm to 3 μm, 0.1 μm to 3 μm, 0.1 μm to 2 μm, or 0.1 to 1 μm. Since the metal layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the electrode assembly. The thickness of the metal piece may be, for example, 2 μm to 10 μm, 2 μm to 7 μm, or 4 μm to 6 μm. By having a metal layer with this thickness range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure for the negative electrode current collector, the weight of the electrode can be reduced, resulting in an increase in energy density.

[0186] A negative electrode active material layer may be formed on the negative electrode current collector. The negative electrode active material layer may be formed as a lithium deposition layer after charging. Alternatively, the negative electrode active material layer may be formed using a negative electrode active material during battery assembly.

[0187] The method of forming a negative electrode active material layer using a negative electrode active material can be manufactured in the same manner as described above, except that the negative electrode active material is used instead of the positive electrode active material when forming the positive electrode active material layer.

[0188] A lithium metal battery may further include, for example, a thin film comprising an element capable of forming an alloy with lithium on one surface of an anode current collector. The thin film is disposed between the anode current collector and the anode active material layer. The thin film includes, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By disposing the thin film on one surface of the anode current collector, for example, the deposition shape of the first anode active material layer deposited between the thin film and the anode active material layer becomes flatter, and the cycle characteristics of the lithium metal battery may be further improved.

[0189] (Separator)

[0190] A separation membrane according to the embodiment is used.

[0191] Organic electrolytes are manufactured, for example, by dissolving lithium salts in organic solvents.

[0192] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0193] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof, etc. The concentration of the lithium salt is 0.1 M to 5.0 M, 0.1 M to 3.0 M, 1.0 to 2.4 M, 1.0 to 1.6 M, for example, 1.2 M.

[0194] A lithium metal battery according to one embodiment may further include a solid electrolyte, a gel electrolyte, a liquid electrolyte, or a combination thereof. The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0195] A gel electrolyte is an electrolyte that contains a crosslinked polymer and a liquid electrolyte and has a gel form.

[0196] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.

[0197] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x ("LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 An inorganic solid electrolyte prepared by adding S4 ("ThioLISICON"), Li2O-Al2O3-TiO2-P2O5 ("LATP"), etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.

[0198] The above sulfide-based solid electrolyte is, for example, Li2S-P2S5, Li2S-P2S5-LiX, X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x (0 <x<2), Li 7-x PS 6-x Br x (0 <x<2), 및 Li 7-x PS 6-x I x (0 <x<2) 중에서 선택된 하나 이상을 들 수 있다.

[0199] . A sulfide-based solid electrolyte is manufactured by treating starting materials such as Li2S and P2S5 by a melting rapid cooling method or a mechanical milling method. In addition, a heat treatment may be performed after the treatment. The solid electrolyte may be amorphous, crystalline, or a mixture thereof. In addition, the solid electrolyte may be, for example, a material containing sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-described sulfide-based solid electrolyte materials. For example, the solid electrolyte may be a material containing Li2S-P2S5. When using a material containing Li2S-P2S5 as a sulfide-based solid electrolyte material forming the solid electrolyte, the mixing molar ratio of Li2S and P2S5 is, for example, in the range of Li2S: P2S5= 50:50 to 90:10.

[0200] The sulfide-based solid electrolyte may include, for example, an argyrodite type solid electrolyte represented by the following chemical formula 1:

[0201] <Chemical Formula 1>

[0202] Li + 12-n-x A n+ X 2- 6-x Y - x

[0203] In the above formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta, X is S, Se or Te, Y is Cl, Br, I, F, CN, OCN, SCN or N3, and 1(n(5, 0(x(2). The sulfide-based solid electrolyte is, for example, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-xI x , may be an argyrodite-type compound including at least one selected from 0≤x≤2. The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.

[0204] The density of the argyrodite-type solid electrolyte may be 1.5 to 2.0 g / cc. Since the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and penetration of the solid electrolyte layer by Li can be effectively suppressed.

[0205] The elastic modulus, i.e., Young's modulus, of the sulfide-based solid electrolyte may be, for example, 35 GPa or less, 30 GPa or less, 27 GPa or less, 25 GPa or less, or 23 GPa or less. The elastic modulus, i.e., Young's modulus, of the sulfide-based solid electrolyte may be, for example, 10 to 35 GPa, 10 to 30 GPa, 10 to 27 GPa, 10 to 25 GPa, or 10 to 23 GPa. Since the sulfide-based solid electrolyte has an elastic modulus in this range, the temperature and / or pressure required for sintering, etc. is reduced, and thus sintering of the solid electrolyte can be performed more easily.

[0206] A polymer solid electrolyte is an electrolyte that includes, for example, a mixture of a lithium salt and a polymer, or a polymer having an ion-conducting functional group. A polymer solid electrolyte is, for example, a polymer electrolyte that does not include a liquid electrolyte.Polymers included in the polymer solid electrolyte include, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA), poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), Polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-Diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi. +) or a combination thereof, but is not limited thereto, and any polymer electrolyte used in the art may be used. The lithium salt may be any lithium salt that can be used in the art. The lithium salt may be, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(x and y are each 1 to 20), LiCl, LiI or a mixture thereof.

[0207] A gel electrolyte is, for example, a gel polymer electrolyte. A gel polymer electrolyte is, for example, an electrolyte that includes a liquid electrolyte and a polymer, or an organic solvent and a polymer having an ion-conducting functional group. The liquid electrolyte can be, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent, a mixture of an ionic liquid and an organic solvent, or a mixture of a lithium salt, an ionic liquid, and an organic solvent. The polymer can be selected from the polymers used in solid polymer electrolytes. The organic solvent can be selected from the organic solvents used in liquid electrolytes. The lithium salt can be selected from the lithium salts used in solid polymer electrolytes. An ionic liquid refers to a salt that is liquid at room temperature or a room-temperature molten salt that has a melting point below room temperature and is composed only of ions. The ionic liquid may comprise at least one selected from compounds comprising, for example, a) at least one cation selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof, and b) at least one anion selected from BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-. A gel polymer electrolyte can be formed by impregnating a polymer solid electrolyte into an electrolyte solution within a lithium battery. The gel electrolyte may further include inorganic particles.

[0208] (lithium metal battery)

[0209] Referring to Fig. 5, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2), and an electrolyte layer (4). The electrolyte layer may contain a separator.

[0210] According to one embodiment, a separator can be used as an electrolyte layer (4).

[0211] An electrolyte (not shown) may be placed between the separator and the anode. The anode (3), the cathode (2), and the electrolyte layer (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium metal battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.

[0212] Referring to FIG. 6, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2), and an electrolyte layer (4). The electrolyte layer may contain a separator. According to one embodiment, a separator may be used as the electrolyte layer (4).

[0213] An electrolyte layer (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the electrolyte layer (4) are wound or folded to form a battery structure (7). According to one embodiment, a separator may be used as the electrolyte layer (4). The battery structure (7) formed in this way is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium metal battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.

[0214] An electrolyte (not shown) may be placed between the separator and the anode.

[0215] Referring to Fig. 7, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2), and an electrolyte layer (4). An electrolyte layer (4) is disposed between the positive electrode (3) and the negative electrode (2), thereby forming a battery structure. The electrolyte layer may include a separator containing a porous substrate.

[0216] A gel-type polymer electrolyte can be placed between the separator and the anode.

[0217] The battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). It may include an electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside. An organic electrolyte is injected into the battery case (5) and sealed, thereby completing the lithium metal battery (1). The battery case (5) is square, but is not necessarily limited to this shape, and may be, for example, cylindrical, thin-film, etc.

[0218] In Fig. 7, an electrolyte can be placed instead of the separator (4), and an electrolyte (not shown) can be placed between the separator and the anode.

[0219] A pouch-type lithium metal battery corresponds to the lithium metal batteries of FIGS. 6 and 7, each of which uses a pouch as a battery case. The pouch-type lithium metal battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium metal battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium metal battery.

[0220] The lithium metal battery of the present disclosure has excellent discharge capacity and cycle life characteristics, as well as high energy density, and is therefore used in, for example, electric vehicles (EVs). For example, it is used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). It is also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.

[0221] Lithium metal batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.

[0222] [Method for manufacturing lithium metal batteries]

[0223] According to one embodiment, a lithium metal battery comprises a step of preparing an anode; a step of preparing an anode; a step of preparing an assembly using the anode and the cathode; and a step of providing an electrolyte to the assembly, wherein the electrolyte comprises a nitrile-based compound, a lithium salt, and a carbonate-based compound, the lithium salt comprises lithium difluorodioxalatoborate (LiDFOB) and lithium tetrafluoroborate (LiBF4), and a content of the nitrile-based compound is 3 wt% to 45 wt% based on 100 wt% of the total weight of the electrolyte. A lithium metal battery can be manufactured.

[0224] An assembly can be prepared by interposing a separator between the positive and negative electrodes.

[0225] The above electrolyte may further include a solid electrolyte, a liquid electrolyte, a gel electrolyte, or a combination thereof. The solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

[0226] The above gel electrolyte can be formed by injecting and crosslinking a gel-type electrolyte composition comprising a polymerizable monomer, a liquid electrolyte, and an initiator into an assembly. The step of injecting the composition for forming a gel-type polymer electrolyte into the assembly can be performed as an impregnation step under vacuum so that the composition can sufficiently penetrate into the pores of the porous substrate.

[0227] Methods for forming a gel-type polymer electrolyte include curing using heat, UV, or high-energy radiation (electron beam, γ-ray). The curing reaction using heat can be carried out at a temperature of 40 to 120°C, for example, 50 to 90°C, for 30 to 120 minutes.

[0228] The above heat treatment varies depending on the type of polymerizable monomer, but is performed at, for example, 40 to 120°C.

[0229] The composition for forming the above gel-type polymer electrolyte may further include a crosslinking agent, a temperature-responsive initiator, etc. to assist in crosslinking of the crosslinkable monomer. The crosslinking agent, initiator, etc. are not particularly limited as long as they are commonly used in the relevant technical field.

[0230] Trimethylolpropane triacrylate, etc. can be used as a crosslinking monomer.

[0231] The initiator can be, for example, benzoin ethyl ether.

[0232] The content of the crosslinking agent, initiator, etc. may be within a conventional range. For example, the content of the initiator may be used in a range of 0.1 to 5 parts by weight, or 0.2 to 3 parts by weight, based on 100 parts by weight of the total content of the monomer for forming the crosslinking polymer. Using the gel polymer electrolyte formed in this way, the ionic conductivity can be maintained at a value close to that of the liquid electrolyte, and the gel polymer electrolyte inside the positive and negative electrodes can play a role in preventing leakage of the liquid electrolyte. The electrolyte can be trapped in the polymer matrix of the gel polymer electrolyte and maintained within the polymer matrix, thereby helping the smooth movement of lithium ions. In addition, the excellent electrochemical properties of the polymer can suppress the electrolyte decomposition reaction within the range of -1 V to 5 V.

[0233] The ionic conductivity of the gel polymer electrolyte is 0.26 mS / cm or more, for example, 0.26 to 1.0 mS / cm, or 0.3 to 1.0 mS / cm.

[0234] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0235] Example 1: 10% BN, 42:48 weight ratio of FEC and DEC, 0.6 M LiDFOB and 0.6 M LiBF4

[0236] A 20 μm thick polyethylene single film was laminated as a separator on a 10 μm thick copper foil as a negative current collector, and a positive electrode was laminated on the other side of the separator to manufacture a laminate. A liquid electrolyte was injected into the prepared laminate to manufacture a lithium metal battery.

[0237] Lithium metal batteries have a cathode / separator / negative current collector structure.

[0238] A liquid electrolyte was prepared by adding 0.6 M LiDFOB (lithium difluoro(oxalate)borate) and 0.6 M LiBF4 to a mixed solvent of fluoroethylene carbonate (FEC), diethyl carbonate (DEC), and butyronitrile (BN) in a weight ratio of 42:48:10. Here, the content of BN is 10 wt% based on 100 wt% of the total weight of the liquid electrolyte.

[0239] The above anode was manufactured according to the following method.

[0240] Li 1.04 Ni 0.88 Co 0.1 Al 0.02 O2 powder and carbon conductive material (Super-P; Timcal Ltd.) were uniformly mixed at a weight ratio of 90:5, and then a PVDF (polyvinylidene fluoride) binder solution was added to prepare a positive electrode active material slurry so that the weight ratio of active material:carbon conductive material:binder = 95.5:2:2.5.

[0241] The manufactured slurry was coated on a 15 ㎛ thick aluminum substrate using a coater, dried under reduced pressure at 120°C, and rolled using a roll press to form a sheet to manufacture a positive electrode.

[0242] Example 2: BN 25%, FEC and DEC in a weight ratio of 33:42, 0.6 M LiDFOB and 0.6 M LiBF4

[0243] A lithium metal battery was manufactured in the same manner as in Example 1, except that the content of BN, FEC, and DEC in the manufacture of the liquid electrolyte was changed to the conditions shown in Table 3 below.

[0244] Example 3: BN 43%, FEC and DEC in 19:38 weight ratio, 0.6 M LiDFOB and 0.6 M LiBF4

[0245] A lithium metal battery was manufactured in the same manner as in Example 1, except that the content of BN, FEC, and DEC in the manufacture of the liquid electrolyte was changed to the conditions shown in Table 3 below.

[0246] Example 4: BN 25%, FEC and DEC in a weight ratio of 33:41, 0.8 M LiDFOB and 0.8 M LiBF4

[0247] A lithium metal battery was manufactured in the same manner as in Example 1, except that the content of BN, FEC, and DEC in the manufacture of the liquid electrolyte was changed to the conditions shown in Table 3 below.

[0248] Example 5: 43% BN, 19:38 wt% FEC and DEC, 0.8 M LiDFOB and 0.8 M LiBF4

[0249] A lithium metal battery was manufactured in the same manner as in Example 1, except that the content of BN, FEC, and DEC in the manufacture of the liquid electrolyte was changed to the conditions shown in Table 3 below.

[0250] Example 6

[0251] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of 0.4 M LiDFOB and 0.6 M LiBF4 was changed to 2:3 (1:1.5).

[0252] Example 7

[0253] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of 0.9 M LiDFOB and 0.6 M LiBF4 was changed to 3:2 (1:0.67).

[0254] Example 8

[0255] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of 1.1 M LiDFOB and 0.6 M LiBF4 was changed to 1:0.55.

[0256] Example 9: Lithium metal battery

[0257] Li as a cathode active material in cathode manufacturing 1.04 Ni 0.88 Co 0.1 Al 0.02 A positive electrode was manufactured in the same manner as in Example 1, except that LiCoO2 was used instead of O2 powder.

[0258] Comparative Example 1: No BN used, 45:55 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF4

[0259] A lithium metal battery was manufactured by the same method as Example 1, except that the liquid electrolyte was obtained by the following process without adding butyronitrile as a liquid electrolyte.

[0260] A liquid electrolyte was prepared by adding 0.6 M LiDFOB (lithium difluoro(oxalate)borate) and 0.6 M LiBF4 to a mixed solvent of fluoroethylene carbonate (FEC) and diethyl carbonate (DEC) in a weight ratio of 45:55.

[0261] Comparative Example 2: 52% BN, 11:37 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF4

[0262] A lithium metal battery was manufactured in the same manner as in Example 1, except that the liquid electrolyte was manufactured by adding 0.6 M LiDFOB (lithium difluoro(oxalate)borate) and 0.6 M LiBF4 to a 2:1 volume ratio mixed solvent of fluoroethylene carbonate (FEC), diethyl carbonate (DEC), and butyronitrile (BN) in a weight ratio of 11:37:52 and mixing them.

[0263] Comparative Example 3: BN 52%, FEC and DEC with a weight ratio of 11:37, 0.8M LiDFOB and 0.8M LiBF4

[0264] When manufacturing a liquid electrolyte, 0.8 M LiDFOB (lithium difluoro(oxalate)borate) and 0.8 M LiBF4 were added to a mixed solvent of fluoroethylene carbonate (FEC), diethyl carbonate (DEC), and BN in a weight ratio of 11:37:52 to prepare a mixture.

[0265] Comparative Example 4: Graphite Anode Lithium Secondary Battery

[0266] On a 10 μm thick copper foil as a negative current collector, 9.51 g of graphite, 0.003 g of CNT as a conductive material, 0.05 g of carbon black, 0.20 g of aqueous styrene-butadiene rubber (SBR) as a binder, and 0.08 g of CMC as a thickener were mixed. These were added to water as a solvent and mixed to prepare a negative electrode slurry. The prepared negative electrode slurry was applied to one side of a copper current collector and dried at about 60°C for 24 hours to form a negative electrode active material layer. A 20 μm thick polyethylene single film was laminated as a separator thereon, and a positive electrode was laminated on the other side of the separator to prepare a laminate. A liquid electrolyte was injected into the prepared laminate to prepare a lithium metal battery.

[0267] Li as a cathode active material in cathode manufacturing 1.04 Ni 0.88 Co 0.1 Al 0.02 A positive electrode was manufactured in the same manner as in Example 1, except that LiCoO2 was used instead of O2 powder.

[0268] Lithium metal batteries have a structure of anode / separator / negative active material layer / negative current collector.

[0269] Table 3 below summarizes the composition of the electrolyte used in some of the above examples and comparative examples.

[0270] Classification LiDFOB content (M) LiBF4 content (M) Weight ratio FEC DEC B N Example 10.6 0.6 4 2 4 8 10 Example 20.6 0.6 3 3 4 2 5 Example 30.6 0.6 1 9 3 8 4 3 Example 40.8 0.8 3 3 4 1 2 5 Example 50.8 0.8 1 9 3 8 4 3 Comparative Example 13 0.6 0.6 4 5 5 5 - Comparative Example 20.6 0.6 1 1 3 7 5 2 Comparative Example 30.8 0.8 1 1 3 7 5 2

[0271] Evaluation Example 1: XPS Analysis

[0272] The XPS analysis spectra of the lithium metal surfaces of the lithium metal batteries of Examples 1 to 5 and Comparative Examples 1 to 3 were evaluated. The XPS analysis was performed using ESCALAB250 (Thermofischer), X-ray source: Al Kα (1486.6 eV) mono 500 μm, pass energy: 30 eV, CAE mode, calibrated by C 248.8 eV.

[0273] The above evaluation results are shown in Table 4 and FIGS. 2a to 2f below. FIG. 2 shows the evaluation results for Example 1 and Comparative Example 1. In addition, Table 4 below shows the ratio of the elemental area of ​​B1s and F1s originating from anions to the elemental area of ​​Li 1s originating from lithium ions, which are cations, in the lithium metal batteries of Examples 1 to 5 and Comparative Examples 1 to 3.

[0274] In Table 4 below, the area for each element was calculated by summing the spectral areas of each element and setting the sum to 100, and then adding up the areas corresponding to each element. In addition, Table 5 below shows the atomic percentages of Example 1 and Comparative Example 1.

[0275] The area of ​​the Li1s peak refers to the total area of ​​Li-F, LiOH, Li2Co2, and LiBO2 peaks appearing at binding energies of 280 to 294 eV, the area of ​​the B1s peak refers to the total area of ​​BF, B=O, BO, BN, and LixBFy peaks appearing at binding energies of 186 to 200 eV, and the F1s peak refers to the total area of ​​BF, and Li-F peaks appearing at binding energies of 682 to 692 eV. And the O1s peak refers to the total area of ​​CO, B2O3, CO3, N-(C=O), LiB02, and Li-O peaks appearing at binding energies of 527 to 537 eV.

[0276] Area of ​​the Li1s peak (A1): Area of ​​the F1s peak (B1) and total area of ​​the B1s peak (B1+B2) Area of ​​the F1s peak (B1) and total area of ​​the B1s peak (B2) (B1+B2): Area of ​​the O1s peak (C1) Example 1 BN 10%, 42:48 wt% FEC and DEC, 0.6M LiDFOB and 0.6M LiBF 4 1:0.75 1:1.3 Example 2 BN 25%, 33:41 wt% FEC and DEC, 0.6M LiDFOB and 0.6M LiBF 4 1:0.86 1:1.17 Example 3 BN 43%, 19:38 wt% FEC and DEC, 0.6M LiDFOB and 0.6M LiBF4 1:0.99 1:0.97 Example 4 BN 25%, FEC and DEC in a weight ratio of 33:41, 0.8M LiDFOB and 0.8M LiBF4 1:1.03 1:0.79 Example 5 BN 43%, FEC and DEC in a weight ratio of 19:38, 0.8M LiDFOB and 0.8M LiBF4 1:1.19 1:0.65 Comparative Example 1 BN Unused, FEC and DEC in a weight ratio of 45:55, 0.6M LiDFOB and 0.6M LiBF4 1:0.68 1:1.51 Comparative Example 2 BN 52%, FEC and DEC in a weight ratio of 11:37, 0.6M LiDFOB and 0.6M LiBF4 1:1.27 1:0.88 Comparative Example 3BN52%, 11:37 weight ratio of FEC and DEC, 0.8M LiDFOB and 0.8M LiBF41:1.331:0.59

[0277] Referring to Table 4, when the component formed from anions in the film increases to form a film, and in the case of organic molecules participating in the film-forming reaction, when the film is formed through CO3-induced organic molecules, the lithium metal battery employing this has improved high-temperature charge-discharge characteristics and capacity retention rate, as can be seen from Evaluation Examples 3 and 4 below. In particular, as the BN content increases, the intensity and area of ​​the BF peak of F1s and the Li-F peak, and the BF peak of B1s continuously increased. However, when the CO3 peak of O1s is greatly reduced as in Comparative Examples 2 and 3, it can be confirmed that the high-temperature charge-discharge characteristics and capacity retention rate deteriorate due to the deterioration of the film characteristics in the part formed by the organic substance, as can be seen from Evaluation Examples 3 and 4 below.

[0278] In addition, referring to FIGS. 2a to 2f, it was found that the lithium metal battery of Example 1 had stronger intensities of BF peaks, CN, BO, and Li-F peaks and increased peak areas compared to the lithium metal battery of Comparative Example 1. These results indicate that, according to Example 1, Li + It was obtained by using BN, a neutral molecule with strong anion interaction in addition to interaction, to induce the movement of anions together with lithium ions moving from the positive electrode to the negative electrode during initial charging, thereby forming a strong film rich in B and F, which are rich in anions, on the negative electrode.

[0279] ClassificationLi1sC1sO1sF1sB1sN1sCop3Example125.928.625.211.38.10.60.2Comparative Example126.327.527.310.47.70.50.2

[0280] From Table 5, we can see the ratio of elements that contributed to the components of the organic and inorganic composite film formed on the lithium metal surface. Since the film components are mainly observed on the surface, each element originates from the liquid electrolyte, and from this, we can know the components of the substances that participated in the cluster participating in the film formation. By confirming the extent to which the sum of the B 1s peak area derived from the anion and the F1s peak area derived from the anion and FEC increased compared to the cation, we could determine whether the anion contained in the solvation cluster increased.

[0281] Evaluation Example 2: Raman Analysis

[0282] In the lithium metal batteries of Example 1 and Comparative Example 1, Raman analysis of F1s on the lithium metal surface was performed.

[0283] Raman analysis was performed using LabRAM HR Evolution (HORIBA) (laser system: 325, 532, 633, 785, 1064 nm, lowest Raman shift: approximately 50 cm-1, spatial resolution: approximately 200 nm).

[0284] The above Raman analysis results are shown in FIGS. 3a and 3b, through which the area (Ac) of the peak (peak c) at wavenumbers 695 to 725 eV and the area (Ad) of the peak (peak d) at wavenumbers 715 to 745 eV and their area ratio (Ac / A) are obtained. d ) were investigated and some of them are shown in Table 6 below. The wavenumbers 695 to 725 cm -1 The peak (peak c) is the Li coordinated DFOB-peak, with wavenumbers 715 to 745 cm -1 The peak (peak d) is for FreeFEC, and is at wavenumbers 735 to 750 cm -1 The peak (peak e) in is for the Li coordinated FEC peak.

[0285] Distinction LiDFOB:LiBF4 1:1 Area of ​​each peak (%) Area ratio (Ac / A d )Li coordinatedDFOB-peak c(695-725 cm -1 )Free FEC peak d(715-745 cm -1 )Li coordinatedFEC735-750 cm -1) Example 10.6M 0.6M 37.75% 57.5% 4.75% 0.7 Comparative Example 10.6M 0.6M 23.6% 69.8% 6.6% 0.3

[0286] Referring to Table 6, the area ratio (Ac / A) of peak c, which is a Li coordinated DFOB- peak, and peak d, which is a free FEC-related peak, in the lithium metal battery of Example 1 d ) is the area ratio (Ac / A) of the lithium metal battery of Comparative Example 1. d ) was found to increase compared to the previous year.

[0287] From this, it was found that the lithium metal battery using the electrolyte with 10 wt% BN added according to Example 1 had a higher concentration of anions around lithium compared to the lithium metal battery of Comparative Example 1 using the electrolyte not containing butyronitrile (BN), and thus an SEI film with a relatively high inorganic content was formed on the lithium metal surface.

[0288] Evaluation Example 3: High Temperature (45℃) Lifespan

[0289] The charge / discharge characteristics of the lithium metal batteries of Examples 1 to 5 and Comparative Examples 1 to 3 were evaluated under the following conditions.

[0290] The battery was charged at a constant current of 0.1 C rate at 45°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).

[0291] The lithium metal battery that had undergone the Mars cycle was charged at a constant current of 0.2 C rate at 45°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle). These cycles are 200 th The cycle was repeated under the same conditions.

[0292] In all charge / discharge cycles, a 10-minute pause was observed after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Figures 2a to 2c. The capacity retention rate is defined by Equation 1 below, and the results are shown in Table 7 below.

[0293] <Formula 1>

[0294] Capacity retention rate [%] = [200 th Discharge capacity in cycles / 2 nd Discharge capacity in cycle] × 100

[0295] Electrolyte Capacity Retention Rate (%)Example 1BN 10%, 42:48 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF484.8Example 2BN 25%, 33:41 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF483.0Example 3BN 43%, 19:38 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF484.2Example 4BN 25%, 33:41 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF484.1Example 5BN 43%, 19:38 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF485.6Comparative Example 1BN Unused, 45:55 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF479.3Comparative Example 2BN 52%, 11:37 weight ratio of FEC and DEC, 0.6M LiDFOB and 0.6M LiBF478.2Comparative Example 3BN 52%, 11:37 weight ratio of FEC and DEC, 0.8M LiDFOB and 0.8M LiBF481.6

[0296] As shown in Table 7, the capacity retention rate of the lithium metal batteries of Comparative Examples 1 to 3 was reduced due to side reactions between lithium and electrolyte resulting from dendrite growth.

[0297] In comparison, the lithium metal batteries of Examples 1 to 5 showed improved capacity retention rates, unlike the lithium metal batteries of Comparative Examples 1 to 3. This improved capacity retention rate is because the composition of the material initially arriving at the negative electrode was changed by changing the components within the Li solvation shell, and the high-temperature long-term life characteristics were improved because the liquid electrolyte physically suppressed dendrite growth compared to the case where BN was not used at the same molar concentration due to the effect of a film on the lithium metal formed robustly by the changed components. In addition, the lithium metal batteries of Examples 1 to 5 showed improved capacity retention rates because the anion interaction was improved, which improved the initial completeness of the film.

[0298] Evaluation Example 4: Viscosity, initial capacity, and capacity retention rate

[0299] The conductivity, viscosity, initial capacity and capacity retention rate of the electrolyte of the lithium metal battery manufactured according to Examples 1, 6 and 7 were investigated and are shown in Table 7 below.

[0300] In Table 7 below, the initial capacity and capacity retention rate were analyzed according to the following conditions.

[0301] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) (formation cycle).

[0302] The lithium metal battery that had undergone the Mars cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle). These cycles are 60 th The cycle was repeated under the same conditions.

[0303] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. The initial capacity is defined by Equation 2 below, and the capacity retention rate is defined by Equation 3 below, and the results are shown in Table 8 below.

[0304] <Formula 2>

[0305] Initial capacity (%) = (discharge capacity in the 1st cycle / charge capacity in the 1st cycle) × 100

[0306] <Formula 3>

[0307] Capacity retention rate [%] = [60 th Discharge capacity in cycles / 2 nd Discharge capacity in cycle] × 100

[0308] Classification Salt ratio (LiDFOB:LiBF4) Viscosity Initial capacity (%) Capacity retention (%) @ 60 cycle Example 11:14.84 100% 91 Example 62:3 (1:1.5) 3.83 100% 82 Example 73:2 (1:0.67) 5.32 97% 85

[0309] Referring to Table 8, it was found that the lithium metal batteries of Examples 1, 6, and 7 had excellent capacities due to reduced resistance because the movement of Li ions was improved. In addition, when the mixing weight ratio of LiDFOB and LiBF4 was between 2:3 or 3:2 (Examples 6 and 7), it was confirmed that BN had better interaction with LiDFOB, but when the content of LiBF4 was more than the above range (Example 6), the probability of encountering LiDFOB decreased, resulting in a decrease in capacity retention compared to the lithium metal battery of Example 1, and when the content of LiDFOB was more than the above range (Example 7), the salt ratio relative to the total weight increased, resulting in a decrease in mobility due to increased viscosity, resulting in a decrease in initial capacity compared to Example 1.

[0310] Evaluation Example 5: Charge / Discharge Characteristics

[0311] The charge / discharge characteristics of the lithium metal battery of Example 9 and the lithium ion battery of Comparative Example 5 were evaluated as follows.

[0312] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.48 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.48 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).

[0313] The lithium metal battery that had undergone the Mars cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle).

[0314] The lithium metal battery that had undergone the first cycle was charged at a constant current of 0.33 C rate at 25°C until the voltage reached 4.48 V (vs. Li), and then cut-off was achieved at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 1.0 C rate until the voltage reached 3.0 V (vs. Li) (2 nd cycle). These cycles are 120 th The cycle was repeated under the same conditions.

[0315] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. The results of the charge / discharge characteristic evaluation are shown in Fig. 4.

[0316] As shown in Fig. 4, the lithium metal battery of Example 9 showed significantly improved life characteristics compared to Comparative Example 5. These results indicate that the lithium metal battery of Example 9 showed improved lifespan due to improved anion interaction and improved initial film completion in Comparative Example 1.

[0317] Evaluation Example 6: High-rate characteristics

[0318] The high-rate characteristics of the lithium metal batteries of Example 1 and Comparative Example 1 were evaluated according to the following method.

[0319] The lithium metal batteries manufactured in Example 1 and Comparative Example 1 were charged at a constant current of 0.1 C at 45°C until the voltage reached 4.3 V (vs. Li), and then cut-off was performed at a current of 0.05 C while maintaining 4.3 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C until the voltage reached 2.8 V (vs. Li) (1 st cycle, Mars (formation) cycle).

[0320] 1 st The cycled lithium battery was charged at a constant current of 0.2 C at 45°C until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C until the voltage reached 2.8 V (vs. Li) (2 nd cycle).

[0321] 2 nd Cycle 11 th The cycle was repeated under the same conditions.

[0322] 11 thThe cycled lithium battery was charged at a constant current of 0.2 C at 25°C until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C until the voltage reached 2.8 V (vs. Li) (12 nd cycle).

[0323] 12th cycle 21 th The cycle was repeated under the same conditions.

[0324] 21 th The cycled lithium battery was charged at a constant current of 0.2 C at 45°C until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 1 C until the voltage reached 2.8 V (vs. Li) (22 nd cycle).

[0325] 22 nd Cycle 31 th The cycle was repeated under the same conditions.

[0326] 31 st The cycled lithium battery was charged at a constant current of 0.2 C at 45°C until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 2 C until the voltage reached 2.8 V (vs. Li) (32 nd cycle).

[0327] 32nd cycle 41 th The cycle was repeated under the same conditions.

[0328] This cycle is 50 thThe cycle was repeated under the same conditions (50 repetitions).

[0329] In all the above charge / discharge cycles, a pause of 10 minutes was allowed after each charge / discharge cycle.

[0330] Some of the results of the above charge-discharge experiment are shown in Table 9 below. The high-rate characteristics are defined by Equation 5 below.

[0331] <Formula 5>

[0332] High rate characteristic [%] = [32 nd Discharge capacity in cycle (2C rate) / 2 nd Discharge capacity in cycle (0.2C rate)] × 100

[0333] Classification rate characteristics (%) Example 191.6 Comparative example 190.4

[0334] Referring to Table 9, it was found that the lithium metal battery of Example 1 had improved high-rate characteristics because the movement of lithium (Li) ions was improved in the case of Comparative Example 1.

[0335] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.

Claims

1. In a lithium metal battery including a cathode, an anode, and an electrolyte layer disposed between the anode and the cathode, In the X-ray photoelectron spectroscopy (XPS) analysis spectrum obtained for the above cathode surface, The ratio of the total area (B1+B2) of the area of ​​the Li1s peak (A1), the area of ​​the F1s peak (B1), and the area of ​​the B1s peak (B2) is 1:0.7 to 1:1.2, The above electrolyte layer includes a nitrile compound, a lithium salt, and a carbonate compound, The above lithium salts include lithium difluoro(oxalato)borate (LiDFOB) and lithium tetrafluoroborate (LiBF4). A lithium metal battery in which the content of the nitrile compound is 3 wt% to 45 wt% based on 100 wt% of the total weight of the electrolyte layer.

2. In paragraph 1, A lithium metal battery, wherein the ratio of the total area (B1+B2) of the area of ​​the F1s peak (B1) and the area of ​​the B1s peak (B2) and the area of ​​the O1s peak (C1) in the XPS analysis spectrum obtained for the above-mentioned cathode surface is in the range of 1:0.6 to 1:1.

3.

3. In paragraph 1, A lithium metal battery wherein the nitrile compound is butyronitrile, valeronitrile, propionitrile, acetonitrile, or a combination thereof.

4. In paragraph 1, A lithium metal battery wherein the concentration of the lithium salt is 1 to 5 M.

5. In paragraph 1, A lithium metal battery wherein the mixing weight ratio of lithium difluorodioxalatoborate (LiDFOB) and lithium tetrafluoroborate (LiBF4) is 1:2 to 1:0.

3.

6. In paragraph 1, A lithium metal battery, wherein the carbonate compound is fluoroethylene carbonate, dimethyl carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, or a combination thereof.

7. In paragraph 1, In the Raman analysis spectrum obtained for the above cathode surface, wave number 695 cm -1 725 cm inland -1 A lithium metal battery, wherein the peak area (Ac) is 25% to 40% of the total Raman analysis area of ​​the electrolyte layer.

8. In paragraph 1, In the Raman analysis spectrum obtained for the above cathode surface, wave number 695 cm -1 725 cm inland -1 The ratio of the area of ​​the peak (Ac) to the area of ​​the peak at wavenumbers 715 to 745 eV (Ac / A) d ) is 0.4 to 1, lithium metal battery.

9. In paragraph 1, The above carbonate compounds include fluoroethylene carbonate (FEC) and diethyl carbonate (DEC), A lithium metal battery in which the mixing weight ratio of the above FEC and DEC is 1:10 to 1:

1.

10. In paragraph 1, A lithium metal battery, wherein the negative electrode includes a negative electrode collector.

11. In paragraph 10, The above negative electrode further includes a lithium metal layer disposed on the negative electrode current collector, A lithium metal battery, wherein the lithium metal layer comprises lithium metal foil, lithium metal powder, lithium alloy foil, lithium alloy powder, or a combination thereof.

12. In paragraph 11, A lithium metal battery further comprising a protective layer disposed on the lithium metal layer.

13. In paragraph 1, The above electrolyte layer includes a liquid electrolyte, a gel electrolyte, a solid electrolyte or a combination thereof, A lithium metal battery, wherein the solid electrolyte comprises an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.

14. In paragraph 13, A lithium metal battery wherein the solid electrolyte further comprises an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.

15. In paragraph 11, The above lithium alloy contains lithium and a first metal, A lithium metal battery wherein the first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.

16. In paragraph 11, The above negative electrode is a lithium metal battery including a negative electrode active material layer between a lithium metal layer and an electrolyte layer.

17. In paragraph 1, The above positive electrode includes a positive electrode current collector and a positive electrode active material layer, At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film contains a polymer, The above polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium metal battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

18. In paragraph 1, The above lithium metal battery is a lithium metal battery further comprising a separator.

19. In paragraph 18, The above separator comprises a porous substrate, The above porous substrate is a lithium metal battery comprising polypropylene, polyethylene, or a combination thereof.

20. Step of preparing the cathode; Steps to prepare the anode; A step of preparing an assembly using the above positive and negative electrodes; and A step of providing an electrolyte layer to the above assembly is included, The above electrolyte layer includes a nitrile compound, a lithium salt, and a carbonate compound, The above lithium salts include lithium difluorodioxalatoborate (LiDFOB) and lithium tetrafluoroborate (LiBF4). A method for manufacturing a lithium metal battery, wherein the content of the nitrile compound is 3 wt% to 45 wt% based on 100 wt% of the total weight of the electrolyte.

Citation Information

Patent Citations

  • Electrolyte and lithium secondary battery with the same

    KR102291944B1

  • Anode-free rechargeable battery

    US10367189B2

  • Electrolyte additive and lithium secondary battery comprising same

    US20190207258A1

  • Flame-resistant bipolar electrodes, bipolar lithium batteries, and manufacturing method

    WO2022198241A1