Binder, and anode and lithium battery comprising same

A cross-linked polymer binder addresses the challenges of dendrite formation and ion flux in lithium batteries by enhancing electrode stability and energy density, maintaining efficient ion flux and reducing volume changes in lithium batteries with a thin protective film.

WO2024205171A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003728
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium batteries employing a negative electrode with lithium metal or without a negative electrode active material face challenges in dendrite formation and uniform ion flux, leading to reduced current density and stability due to the thickness requirements of protective films, which also hinder initial efficiency and lifespan characteristics.

Method used

A hybrid binder composed of a cross-linked polymer of fluorine-substituted polyamic acid or polyimide and polyvinyl alcohol is used to form a protective film on the negative electrode, enhancing electrode stability and suppressing volume changes while maintaining thin film thickness for improved ion conductivity.

Benefits of technology

The binder improves the initial capacity, lifespan, and stability of lithium batteries by preventing dendrite growth and maintaining high energy density, while the thin protective film ensures efficient ion flux and reduced volume changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003728_03102024_PF_FP_ABST
    Figure KR2024003728_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a binder, an anode comprising a protective layer including the binder, and a lithium battery comprising the anode, wherein the binder comprises a third polymer that is a product of a cross-linking reaction between one or more first polymers comprising a first functional group and being selected from among fluorine-substituted poly(amic acid) and fluorine-substituted polyimide and a second polymer comprising a second functional group and being water soluble, wherein the first polymer and the second polymer are cross-linked by forming an ester bond through a reaction between the first functional group and the second functional group.
Need to check novelty before this filing date? Find Prior Art

Description

Binder, cathode and lithium battery containing the same

[0001] It relates to a binder, an electrode containing the same, and a lithium battery.

[0002] In a lithium battery employing a cathode containing lithium metal or a non-cathode containing no cathode active material, a protective film is applied to prevent dendrite formation and ensure uniform ion flux when dendrites are formed.

[0003] Protective films can be polymeric, inorganic, or organic / inorganic composite. Most protective films require a thickness of at least 10 μm to ensure sufficient ionic conductivity. However, thicker protective films lead to lower current densities in lithium batteries employing them.

[0004] To solve these problems, a hybrid binder of polyimide and polyvinyl alcohol was applied to the protective film, but it was not easy to form a stable SEI during the initial deposition.

[0005] Therefore, in a lithium battery employing a cathode including lithium metal or a cathode without a cathode active material, a protective film capable of suppressing volume change of the electrode and a binder forming the protective film are required, which provides high initial efficiency and life characteristics, and improved electrode stability.

[0006] One aspect is to provide a binder that forms a protective film capable of suppressing volume change of the electrode and having improved initial capacity, life characteristics and electrode stability.

[0007] Another aspect is to provide a cathode comprising a protective film comprising the above binder.

[0008] Another aspect is to provide a lithium battery employing the above negative electrode.

[0009] According to one implementation example,

[0010] A third polymer comprising a crosslinking reaction product of at least one first polymer selected from among polyamic acid and polyimide having a first functional group and substituted with fluorine and a water-soluble second polymer having a second functional group,

[0011] A binder is provided in which the first polymer and the second polymer are crosslinked by the reaction of the first functional group and the second functional group to form an ester bond.

[0012] According to another implementation example,

[0013] A negative electrode is provided, comprising: a negative electrode current collector; and a protective layer disposed on the negative electrode current collector and including the binder.

[0014] According to another implementation example,

[0015] A lithium battery is provided, comprising: a positive electrode; the negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode.

[0016] According to one aspect, the initial efficiency, cycle life, and electrode stability of a lithium battery can be improved by using a binder comprising a crosslinked polymer crosslinked with a fluorine-substituted polyamic acid or polyimide and a water-soluble binder. In addition, volume changes in the lithium battery can be suppressed.

[0017] Figure 1 is a cross-sectional view of a cathode according to an exemplary embodiment.

[0018] Figure 2 is a cross-sectional view of a cathode according to another exemplary embodiment.

[0019] Figure 3 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0020] Figure 4 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0021] Figure 5 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0022] Below, the binder, the negative electrode including the binder, and the lithium battery according to exemplary embodiments are described in more detail.

[0023] As used herein, "cross-link" means a bond that connects one polymer chain to another polymer chain. As used herein, a cross-link is a covalent bond. As used herein, a "linker" or "cross-linker" means a functional group that connects one polymer chain to another polymer chain. As used herein, a "cross-linked polymer" means a polymer in which one polymer chain and another polymer chain are connected by one or more linkers. Furthermore, a cross-linked polymer is a product of a cross-linking reaction of one or more polymers.

[0024] As used herein, “fluorine-substituted” means that any hydrogen contained in the polymer is replaced with fluorine or an alkyl group having 1 to 5 carbon atoms substituted with fluorine.

[0025] According to one embodiment, a binder includes a third polymer which is a crosslinking reaction product of at least one first polymer selected from among polyamic acid and polyimide substituted with fluorine and a water-soluble second polymer having a second functional group, wherein the first polymer and the second polymer are crosslinked by forming an ester bond through a reaction between the first functional group and the second functional group. The third polymer is a crosslinked polymer of the first polymer and the second polymer. Since the binder includes the third binder which is a crosslinked polymer in which the first polymer containing fluorine and the second polymer are crosslinked by an ester bond, a lithium battery employing an anode having a protective film including the binder can simultaneously provide excellent anode stability derived from a polyimide containing fluorine, suppression of volume expansion of the anode, and improved initial charge / discharge efficiency and cycle life characteristics due to fluorine.

[0026] In the binder, the first functional group and the second functional group included in the first polymer and the second polymer may be independently selected from a carboxyl group, a hydroxyl group, an amide group, and an aldehyde group, but are not necessarily limited thereto, and any functional group that can react with the first functional group and the second functional group to form a cross-linking bond including an ester bond is possible. For example, the first functional group may be a carboxyl group (-COOH), and the second functional group may be a hydroxyl group (-OH). The carboxyl group and the hydroxyl group may react to form an ester cross-linking bond. In the first polymer, the first functional group may not be connected to a trivalent aromatic group included in the polyamic acid and the polyimide, but may be connected to a divalent aromatic group as a side chain.

[0027] In the binder, the first polymer may include an alkali metal. The alkali metal may be sodium, lithium, or the like. The first polymer may be substituted or doped with the alkali metal. For example, in polyamic acid, the hydrogen of the carboxyl group connected to the trivalent aromatic group contained in the polyamic acid may be substituted with an alkali metal ion. For example, in polyimide, an alkali metal ion may be doped and coordinated to an amide group. The initial charge / discharge efficiency may be improved by the first polymer including the alkali metal in advance (pre-lithiation).

[0028] The content of the alkali metal included in the first polymer may be 0.2 to 1.0 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.2 to 0.8 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.3 to 0.7 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.4 to 0.6 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.45 to 0.55 in terms of an equivalent ratio to the carboxyl group or the amide group. In the above alkali metal content range, further improved binder properties may be provided.

[0029] If the lithium content of the polyamic acid, i.e., the degree of substitution of lithium ions, is lower than 0.2 in terms of the equivalent ratio to the carboxylic acid, the prelithiation rate is low, so the effect of suppressing irreversible occurrence in the first cycle is not significant. In addition, if the lithium content of the polyamic acid, i.e., the degree of substitution of lithium ions, is higher than 1.0 in terms of the equivalent ratio to the carboxylic acid, the imidization rate is significantly reduced, which may lower the life characteristics. The lithium content, i.e., the degree of substitution of lithium ions, in the above range can be obtained by adding the content of LiOH used to lithiate the polyamic acid in the range of 0.2 to 1.0 in terms of the equivalent ratio to the carboxylic acid of the polyamic acid.

[0030] For example, the polyimide may be represented by the following chemical formula 1 or chemical formula 2:

[0031] <Chemical Formula 1>

[0032]

[0033] <Chemical Formula 2>

[0034]

[0035] Among the above chemical formulas 1 and 2,

[0036] M is an alkali metal,

[0037] Ar1, Ar2, Ar4 and Ar5 are each independently a trivalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; or a trivalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; An aromatic ring group selected from among, wherein the aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-O,

[0038] Ar3 and Ar6 are each independently a divalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; or a divalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; An aromatic ring group selected from among, wherein the aromatic ring group is one aromatic ring, a fused ring of two or more aromatic rings, or a ring of two or more aromatic rings connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-, X1 is -COOH, -OH, -CO-NH2, or -COH, Y1 and Y2 are each independently an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction in a repeating unit, 0 <n<1, 0<m<1, n+m=1이다.

[0039] For example, the polyimide may be represented by the following chemical formula 3 or chemical formula 4:

[0040] <Chemical Formula 3>

[0041]

[0042] <Chemical Formula 4>

[0043]

[0044] Among the above chemical formulas 3 and 4,

[0045] M is lithium or sodium,

[0046] R1 to R 20are independently a halogen; -COOH; -OH; -CO-NH2; -COH; a C1 to C10 alkyl group substituted or unsubstituted with a halogen; a C6 to C20 aryl group substituted or unsubstituted with a halogen; or a C2 to C20 heteroaryl group substituted or unsubstituted with a halogen; wherein at least one of R5 to R8 is -COOH, -OH, -CO-NH2, or -COH, and R 13 Inland R 20 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, Y1 to Y3 are each independently a single bond or an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.

[0047] For example, the polyamic acid may be represented by the following chemical formula 7 or chemical formula 8:

[0048] <Chemical Formula 7>

[0049]

[0050] <Chemical Formula 8>

[0051]

[0052] Among the above chemical formulas 7 and 8,

[0053] M is an alkali metal,

[0054] Ar1, Ar2, Ar4 and Ar5 are each independently a trivalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; or a trivalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; An aromatic ring group selected from among, wherein the aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-O,

[0055] Ar3 and Ar6 are each independently a divalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; or a divalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; An aromatic ring group selected from among, wherein the aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-.

[0056] X1 is -COOH, -OH, -CO-NH2, or -COH, Y1 is an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.

[0057] For example, the polyamic acid may be represented by the following chemical formula 9 or chemical formula 10:

[0058] <Chemical Formula 9>

[0059]

[0060] <Chemical Formula 10>

[0061]

[0062] Among the above chemical formulas 9 and 10,

[0063] M is lithium or sodium,

[0064] R1 to R 20 are independently hydrogen; halogen; -COOH; -OH; -CO-NH2; -COH; a C1 to C10 alkyl group substituted or unsubstituted with a halogen; a C6 to C20 aryl group substituted or unsubstituted with a halogen; or a C2 to C20 heteroaryl group substituted or unsubstituted with a halogen; wherein at least one of R5 to R8 is -COOH, -OH, -CO-NH2, or -COH, and R 13 Inland R 20 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, Y1 to Y3 are each independently a single bond or an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.

[0065] For example, in the binder, the polyimide may be represented by the following chemical formula 5 or chemical formula 6, and the polyamic acid may be represented by the following chemical formula 11 or chemical formula 12:

[0066] <Chemical Formula 5>

[0067]

[0068] <Chemical Formula 6>

[0069]

[0070] <Chemical Formula 11>

[0071]

[0072] <Chemical Formula 12>

[0073]

[0074] Among the above chemical formulas 5, 6, 11 and 12,

[0075] R 51 Inland R 58 are independently an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine (F), R 51 Inland R 58 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, and n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.

[0076] For example, in the first polymer represented by the above chemical formulas 1 to 12, the mole fractions of repeating units including a crosslinking group and repeating units not including a crosslinking group are each 0. <m<0.5, 0.5<n<1 및 m+n=1일 수 있다. 예를 들어, 상기 화학식 1 내지 12로 표시되는 제1 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.1<m<0.4, 0.6<n<0.9 및 m+n=1일 수 있다. 예를 들어, 상기 화학식 1 내지 12로 표시되는 제1 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.15<m<0.35, 0.65<n<0.85 및 m+n=1일 수 있다. 예를 들어, 상기 화학식 1 내지 12로 표시되는 제1 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.2<m<0.3, 0.7<n<0.8 및 m+n=1일 수 있다. 상기 몰분율 범위에서 바인더가 더욱 향상된 물성을 제공할 수 있다.

[0077] For example, the first polymer represented by the chemical formulas 1 to 12 may be a random copolymer. For example, the first polymer represented by the chemical formulas 1 to 12 may be a block copolymer.

[0078] The weight average molecular weight of the first polymer may be 10,000 to 1,200,000 Daltons. For example, the weight average molecular weight of the first polymer in the binder may be 10,000 to 1,100,000 Daltons. For example, the weight average molecular weight of the first polymer in the binder may be 10,000 to 1,000,000 Daltons. For example, the weight average molecular weight of the first polymer may be 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the first polymer may be 100,000 to 500,000 Daltons. For example, the weight average molecular weight of the first polymer may be 100,000 to 400,000 Daltons. For example, the weight average molecular weight of the first polymer may be 100,000 to 300,000 Dalton. The properties of the binder may be further improved within the weight average molecular weight range of the first polymer.

[0079] In the binder, the second polymer may be a polymerization reaction product of one or more monomers selected from a vinyl monomer, an acetate monomer, an alcohol monomer, an acrylic monomer, a methacrylic monomer, an acrylamide monomer, and a methacrylamide monomer, or a hydrolyzate thereof.

[0080] For example, the second polymer may be vinyl acetate, vinyl alcohol, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxyethylene glycol (meth)acrylate, 2-hydroxypropylene glycol (meth)acrylate, acrylic acid, methacrylic acid, 2-(meth)acryloyloxy acetic acid, 3-(meth)acryloyloxy propyl acid, 4-(meth)acryloyloxy butyric acid, itaconic acid, maleic acid, 2-isocyanatoethyl (meth)acrylate, 3-isocyanatopropyl It may be a polymerization reaction product of one or more monomers selected from (meth)acrylate, 4-isocyanatobutyl (meth)acrylate, (meth)acrylamide, ethylenedi(meth)acrylate, diethyleneglycol(meth)acrylate, triethyleneglycoldi(meth)acrylate, trimethylenepropanetri(meth)acrylate, trimethylenepropanetriacrylate, 1,3-butanediol(meth)acrylate, 1,6-hexanedioldi(meth)acrylate, allyl acrylate, and N-vinyl caprolactam, or a hydrolyzate thereof.

[0081] In particular, the second polymer may be polyvinyl alcohol (PVA). For example, polyvinyl alcohol may be a hydrolyzate obtained by hydrolyzing polyvinyl acetate with an alkali.

[0082] The degree of saponification of the polyvinyl alcohol may be 60 to 99%. For example, the degree of saponification of the polyvinyl alcohol may be 70 to 95%. For example, the degree of saponification of the polyvinyl alcohol may be 75 to 90%. For example, the degree of saponification of the polyvinyl alcohol may be 80 to 90%. For example, the degree of saponification of the polyvinyl alcohol may be 85 to 90%. In the above saponification range, the binder can provide further improved physical properties.

[0083] The weight average molecular weight of the polyvinyl alcohol may be 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 400,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 300,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 200,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 50,000 to 150,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 70,000 to 100,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 80,000 to 100,000 Daltons. The physical properties of the binder may be further improved within the weight average molecular weight range of the polyvinyl alcohol.

[0084] The weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 1:99 to 50:50. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 5:95 to 45:55. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 5:95 to 40:60. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 5:95 to 35:65. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 10:90 to 30:70. The physical properties of the binder may be further improved within the above range of the weight ratio of the first polymer to the second polymer.

[0085] The crosslinking reaction in the binder may be performed at a temperature of 100°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 100°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 120°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 140°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 160°C or higher. The crosslinking reaction may proceed within the above temperature range to produce a crosslinked polymer.

[0086] In addition, by performing the crosslinking reaction in the binder at a temperature of 100°C or higher, the polyamic acid can be cured into polyimide. For example, the imidization rate of the polyamic acid can be 60% or higher. For example, the imidization rate of the polyamic acid can be 70% or higher. For example, the imidization rate of the polyamic acid can be 80% or higher. For example, the imidization rate of the polyamic acid can be 90% or higher. The imidization rate of the polyamic acid 1 It can be obtained using H-NMR. The mechanical properties of the binder can be further improved by curing the polyamic acid in the binder into polyimide.

[0087] In one embodiment, the acid equivalent of the polyamic acid may be less than 300 g / eq. For example, the acid equivalent of the polyamic acid may be in the range of 50 g / eq to 250 g / eq. When the acid equivalent of the polyamic acid is lowered to less than 300 g / eq, the amount of carboxyl groups and / or carboxylates per unit mass may increase. When the amount of carboxyl groups and / or carboxylates per unit mass increases, for example, when a silicon-based negative electrode active material is used as the negative electrode material, the interaction between the negative electrode active material having a hydroxyl group on the surface and the binder may increase, thereby improving the bonding strength with the negative electrode active material. When the acid equivalent is 300 g / eq or more, the initial efficiency and life characteristics of the lithium battery may decrease.

[0088] In the binder, the modulus of the third polymer may have a value greater than the modulus of the first polymer and the modulus of the second polymer, respectively. Since the third polymer is a cross-linked polymer formed by cross-linking the first and second polymers, the modulus may increase, thereby increasing the stiffness of the polymer. For example, the modulus of the third polymer may be 5 GPa or more. For example, the modulus of the third polymer may be 6 GPa or more. For example, the modulus of the third polymer may be 7 GPa or more. The modulus may be an indentation modulus.

[0089] The hardness (indentation hardness) of the third polymer in the binder may be greater than the hardness of the first polymer and the hardness of the second polymer, respectively. For example, since the third polymer is a cross-linked polymer formed by cross-linking the first and second polymers, the surface hardness (surface indentation hardness) may increase.

[0090] The third polymer, which is a cross-linked polymer in the binder, may have a three-dimensional network structure in which a plurality of first polymer chains and a plurality of second polymer chains are cross-linked with each other by a linker or a cross-linker. Since the third polymer has a network structure, volume change during charge and discharge of an electrode including the binder can be suppressed.

[0091] The weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,500,000 Daltons. For example, the weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,200,000 Daltons. For example, the weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,100,000 Daltons. For example, the weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,000,000 Daltons. For example, the weight average molecular weight of the third polymer may be from 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the third polymer may be from 100,000 to 500,000 Daltons. For example, the weight average molecular weight of the third polymer may be 100,000 to 400,000 Daltons. For example, the weight average molecular weight of the third polymer may be 100,000 to 300,000 Daltons. The physical properties of the binder may be further improved within the weight average molecular weight range of the third polymer.

[0092] For example, the third polymer in the binder may be represented by one or more of the following chemical formulae 13 to 16:

[0093] <Chemical Formula 13>

[0094]

[0095] <Chemical Formula 14>

[0096]

[0097] <Chemical Formula 15>

[0098]

[0099] <Chemical Formula 16>

[0100]

[0101] In the above equations, n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이며, p는 중합도로서 250 내지 12500다.

[0102] The binder may additionally include a water-soluble fourth polymer selected from cellulose hydroxyethyl ether, dextran, carboxymethylcellulose (CMC), alginate, cellulose nanofiber, xanthan gum, and guar gum. By additionally including the fourth polymer in the binder, the physical properties of the binder can be variously controlled.

[0103] The above binder can be used, for example, in an electrochemical cell. The binder can be used, for example, in a protective film included in an electrochemical cell. The type of electrochemical cell is not particularly limited as long as it is a device that can store energy through an electrochemical reaction, and includes both primary and secondary batteries. The electrochemical cell can be, for example, an alkali metal battery such as a lithium battery or a sodium battery, an alkaline earth metal battery such as a magnesium battery, a metal-air battery, a supercapacitor, a fuel cell, etc.

[0104]

[0105] According to another embodiment, a negative electrode may include a negative current collector; and a protective layer disposed on the negative current collector and including the binder described above.

[0106] Hereinafter, a negative electrode including a protective layer including the binder according to exemplary embodiments and a lithium battery including the same will be described in more detail.

[0107] [cathode]

[0108] According to one embodiment, a negative electrode for a lithium battery includes: a negative electrode current collector; and a protective layer disposed on one surface of the negative electrode current collector; wherein the protective layer may include the binder described above. Since the negative electrode includes the protective layer including the binder, the initial efficiency, life characteristics, and electrode stability of a lithium battery including the negative electrode may be improved. In addition, volume change of the lithium battery may be suppressed.

[0109] Referring to FIG. 1, the negative electrode (20) includes a negative electrode current collector (21); and a protective layer (24) disposed on the negative electrode current collector (21); wherein the protective layer (24) includes the binder described above.

[0110] According to one embodiment, the negative electrode (20) may further include a negative electrode intermediate layer (22) disposed between the negative electrode current collector (21) and the protective layer (24).

[0111] Referring to FIG. 2, the negative electrode (20) may further include a negative electrode active material layer (23) disposed between the protective layer (24) and the negative electrode current collector (21).

[0112]

[0113] [Cathode: Protective layer]

[0114] Referring to FIGS. 1 and 2, the negative electrode (20) includes a negative electrode current collector (21); and a protective layer (24) disposed on the negative electrode current collector (21). The protective layer (24) includes the binder described above.

[0115] According to one embodiment, the thickness of the protective layer (24) may be 5 μm or less. The thickness of the protective layer (24) may be, for example, 0.1 μm to 5 μm, 0.1 μm to 3 μm, 0.1 μm to 2 μm, 0.1 μm to 1.5 μm, 0.1 μm to 1.2 μm, 0.1 μm to 1.2 μm, or 0.2 to 1 μm. When the protective layer (24) has a thickness in this range, the decomposition of the electrolyte can be effectively suppressed and the imbalance of local current density can be effectively prevented, thereby effectively preventing the generation and / or growth of lithium dendrites. Accordingly, the cycle characteristics of the lithium battery including the protective layer (24) can be further improved. If the thickness of the protective layer (24) is excessively increased, the energy density of the lithium metal battery may be reduced. If the thickness of the protective layer (24) is excessively decreased, the improvement in the cycle characteristics of the lithium metal battery may be minimal.

[0116] According to one embodiment, the modulus of the protective layer (24) may be 5 GPa or greater. For example, the modulus of the third polymer may be 6 GPa or greater. For example, the modulus of the third polymer may be 7 GPa or greater. The modulus may be an indentation modulus.

[0117] According to one embodiment, the recovery rate of the protective layer (24) may be 50% or more. For example, the recovery rate of the protective layer (24) may be 55% or more. For example, the recovery rate of the protective layer (24) may be 60% or more. For example, the recovery rate of the protective layer (24) may be 65% or more.

[0118] According to one implementation example, the hardness (indentation hardness) of the protective layer (24) is 1200 N / mm 2 It may be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1300 N / mm 2It may be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1400 N / mm 2 It may be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1450 N / mm 2 It may be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1500 N / mm 2 It may be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1550 N / mm 2 It could be strange.

[0119] According to one embodiment, the protective layer (24) can be manufactured by curing the protective film-forming composition described below. The protective film-forming composition can include the first polymer described above and the second polymer described above. The protective layer (24) can be formed, for example, by applying the protective film-forming composition on a negative electrode current collector (21) and then curing it at a temperature of 100°C or higher.

[0120] The protective layer (24) can be formed, for example, by applying the composition for forming a protective film on the negative electrode current collector (21) and then heat-treating at a temperature of 100°C or higher for 1 to 10 hours. The protective layer (24) can be formed, for example, by applying the composition for forming a protective film on the negative electrode current collector (21) and then heat-treating at a temperature of 160°C or higher for 1 to 10 hours.

[0121] According to one embodiment, the protective layer (24) may further include a conductive material.

[0122] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used.

[0123]

[0124] [Cathode: Negative current collector]

[0125] Referring to FIGS. 1 and 2, the negative electrode (20) includes a negative electrode collector (21).

[0126] The negative electrode current collector (21) includes, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or an alloy thereof.

[0127] The negative electrode current collector (21) includes, for example, a first metal substrate. The first metal substrate includes, as a main component, the first metal, or is made of the first metal. The content of the first metal included in the first metal substrate is, for example, 90 wt% or more, 95 wt% or more, 99 wt% or more, or 99.9 wt% or more, based on the total weight of the first metal substrate. The first metal substrate may be composed of, for example, a material that does not react with lithium, i.e., does not form an alloy and / or compound with lithium. The first metal includes, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The first metal substrate may be composed of, for example, one of the above-described metals, or may be composed of an alloy of two or more metals. The first metal substrate is, for example, in the form of a sheet or foil. The thickness of the negative electrode current collector (21) may be, for example, 5 μm to 50 μm, 10 μm to 50 μm, 10 μm to 40 μm, or 10 μm to 30 μm, but is not necessarily limited to this range and may be selected depending on the characteristics of the required lithium battery.

[0128] The negative electrode current collector (21) may include, for example, a first metal substrate; and a coating layer (not shown) disposed on the first metal substrate and including a second metal. The second metal has a higher Mohs hardness than the first metal. That is, since the coating layer including the second metal is harder than the substrate including the first metal, deterioration of the first metal substrate can be prevented. The Mohs hardness of the material constituting the first metal substrate is, for example, 5.5 or less. The Mohs hardness of the first metal is, for example, 5.5 or less, 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, or 3.0 or less. The Mohs hardness of the first metal may be, for example, 2.0 to 6.0. The coating layer includes the second metal. The coating layer includes, for example, the second metal as a main component or is made of the second metal. The content of the second metal included in the coating layer is, for example, 90 wt% or more, 95 wt% or more, 99 wt% or more, or 99.9 wt% or more based on the total weight of the coating layer. The coating layer may be composed of, for example, a material that does not react with lithium, i.e., does not form an alloy and / or compound with lithium. The Mohs hardness of the material constituting the coating layer is, for example, 6.0 or more. For example, the Mohs hardness of the second metal is 6.0 or more, 6.5 or less, 7.0 or more, 7.5 or more, 8.0 or more, 8.5 or more, or 9.0 or more. The Mohs hardness of the second metal may be, for example, 6.0 to 12. If the Mohs hardness of the second metal is excessively low, it may be difficult to suppress deterioration of the negative electrode current collector. If the Mohs hardness of the second metal is excessively high, processing may not be easy. The second metal is, for example, one or more selected from titanium (Ti), manganese (Mn), niobium (Nb), tantalum (Ta), iridium (Ir), vanadium (V), rhenium (Re), osmium (Os), tungsten (W), chromium (Cr), boron (B), ruthenium (Ru), and rhodium (Rh).The coating layer may be composed of, for example, one of the above-described metals, or may be composed of an alloy of two or more metals. The difference in Mohs hardness between the first metal included in the first metal substrate and the second metal included in the coating layer may be, for example, 2 or more, 2.5 or more, 3 or more, 3.5 or more, or 4 or more. Since the first metal and the second metal have such a difference in Mohs hardness, deterioration of the negative electrode current collector can be more effectively suppressed. The coating layer may have a single-layer structure or a multi-layer structure of two or more layers. The coating layer may have a two-layer structure including, for example, a first coating layer and a second coating layer. The coating layer may have a three-layer structure including, for example, a first coating layer, a second coating layer, and a third coating layer. The thickness of the coating layer may be, for example, 10 nm to 1 ㎛, 50 nm to 500 nm, 50 nm to 200 nm, or 50 nm to 150 nm. If the thickness of the coating layer is too thin, it may be difficult to suppress the uneven growth of the lithium-containing metal layer. As the thickness of the coating layer increases, the cycle characteristics of the lithium battery improve. However, if the thickness of the coating layer is too thick, the energy density of the lithium battery decreases and the formation of the coating layer may not be easy. The coating layer may be formed on the first metal substrate by, for example, a vacuum deposition method, a sputtering method, a plating method, etc., but is not necessarily limited to these methods, and any method capable of forming a coating layer in the relevant technical field may be used.

[0129] The negative electrode current collector (21) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. Since the positive electrode current collector has such a structure, the weight of the electrode can be reduced, and consequently, the energy density of the all-solid-state secondary battery can be improved.

[0130]

[0131] [Cathode: Anode interlayer]

[0132] Referring to FIG. 1, the negative electrode (20) may include an anode interlayer (22) disposed between the negative electrode current collector (21) and the protective layer (24). Since the negative electrode (20) includes the anode interlayer (22), the generation and / or growth of lithium dendrites in the negative electrode (20) can be more effectively suppressed.

[0133] The negative electrode intermediate layer (22) may include, for example, a lithium-affinity metal. The negative electrode intermediate layer (22) may include, for example, a lithium-affinity metal and a carbon material.

[0134] The above lithium-compatible metal is a material that can be lithiated and delithiated. The negative electrode intermediate layer (22) can be formed by introducing the lithium-compatible metal onto the negative electrode current collector (21) through nanoparticle casting. When the negative electrode intermediate layer (22) is introduced onto the negative electrode current collector (21) through nanoparticle casting, lithium ions can penetrate the negative electrode intermediate layer (22), so that lithium metal can be formed between the negative electrode intermediate layer (22) and the negative electrode current collector (21).

[0135] The lithium-affinity metal included in the negative electrode intermediate layer (22) may be nanoparticles of the lithium-affinity metal. The average particle diameter of the lithium-affinity metal may be, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 100 nm, or 20 nm to 80 nm. Since the lithium-affinity metal has an average particle diameter in this range, reversible plating and / or dissolution of lithium may be facilitated during charge and discharge. In addition, since the lithium-affinity metal has a nano-sized size, lithium ions may penetrate the negative electrode intermediate layer (22) including the lithium-affinity metal, so that lithium metal may be precipitated between the negative electrode current collector (21) and the negative electrode intermediate layer (21). The average particle diameter of the above lithium-affinity metal is, for example, the median diameter (D50) measured using a laser particle size distribution meter.

[0136] The lithium-affinity metal may include, for example, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The lithium-affinity metal may include, for example, silver (Ag).

[0137] The carbon material can uniformly coat the lithium-affinity metal on the negative electrode current collector (21). The carbon material can uniformly coat the lithium-affinity metal on the negative electrode current collector (21) by uniformly applying the lithium-affinity metal on the negative electrode current collector (21). The uniformly coated first particles can uniformly precipitate lithium metal on the negative electrode current collector (21) to prevent the formation of lithium dendrites.

[0138] The carbon material may include, for example, amorphous carbon, crystalline carbon, or any combination thereof. The carbon material may include, for example, amorphous carbon.

[0139] The amorphous carbon may include, for example, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, or any combination thereof. The amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphitic carbon.

[0140] The negative electrode intermediate layer (22) may include, for example, a lithium-affinity metal and / or a carbon material, and uniformly apply the lithium-affinity metal onto the negative electrode current collector (21) through the carbon material, and the lithium-affinity metal may uniformly deposit lithium metal between the negative electrode intermediate layer (22) and the negative electrode current collector (21). Accordingly, the formation of lithium dendrites may be suppressed, and the life characteristics of a lithium battery including the negative electrode (20) may be improved. In addition, the negative electrode intermediate layer (22) may firmly attach the lithium metal to the protective layer (24) described below, thereby preventing deformation and perforation of the protective layer (24) due to uneven deposition of lithium metal.

[0141] The mixing ratio of the lithium-affinity metal and the carbon material included in the negative electrode intermediate layer (22) may be, for example, 10:1 to 1:10, 10:1 to 1:1, 10:1 to 2:1, 5:1 to 1:1, or 5:1 to 2:1 in weight ratio.

[0142] The negative electrode intermediate layer (22) may further include a binder. The binder included in the negative electrode intermediate layer (22) may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the art may be used. The binder may be composed of a single binder or a plurality of different binders. When the negative electrode intermediate layer (22) does not include a binder, the negative electrode intermediate layer (22) can be easily separated from the protective layer (24) or the negative electrode current collector (21). The content of the binder included in the negative electrode intermediate layer (22) may be, for example, 5 wt% or less, 0.1 to 5 wt%, 0.1 to 3 wt%, or 0.1 to 1 wt% relative to the total weight of the negative electrode (22) intermediate layer.

[0143] The thickness of the negative electrode intermediate layer may be, for example, 0.1 ㎛ to 5 ㎛, 0.1 ㎛ to 3 ㎛, or 0.5 ㎛ to 5 ㎛, 0.5 ㎛ to 3 ㎛, or 0.5 ㎛ to 2 ㎛. If the thickness of the negative electrode intermediate layer is too thin, lithium dendrites formed between the negative electrode intermediate layer and the negative electrode current collector may cause the negative electrode intermediate layer to collapse, making it difficult to improve the cycle characteristics of the lithium battery. If the thickness of the negative electrode intermediate layer increases excessively, the energy density of the lithium battery employing the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics. If the thickness of the negative electrode intermediate layer decreases, for example, the charge capacity of the negative electrode intermediate layer also decreases.

[0144] The charge capacity of the negative electrode intermediate layer may be, for example, 0.1% to 50%, 1% to 30%, 1% to 10%, 1% to 5%, or 1% to 2% of the charge capacity. If the charge capacity of the negative electrode intermediate layer is too small, lithium dendrites formed between the negative electrode intermediate layer and the negative electrode current collector may collapse the negative electrode intermediate layer, making it difficult to improve the cycle characteristics of the lithium battery. If the charge capacity of the negative electrode intermediate layer increases excessively, the energy density of the lithium battery using the negative electrode (20) may decrease and it may be difficult to improve the cycle characteristics. The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the positive electrode active material layer. The charge capacity of the negative electrode intermediate layer is also calculated in the same way. That is, the charge capacity of the negative electrode intermediate layer is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode intermediate layer. When multiple types of negative electrode active materials are used, the charge capacity density Х mass value is calculated for each negative electrode active material, and the sum of these values ​​is the capacity of the negative electrode intermediate layer. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is the capacity estimated using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the negative electrode intermediate layer is directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the negative electrode intermediate layer may be the initial charge capacity measured at the time of the 1st charge cycle.

[0145]

[0146] [Cathode: Cathode active material layer]

[0147] Referring to FIG. 2, the negative electrode (20) further includes a negative electrode active material layer (23) disposed between the negative electrode current collector (21) and the protective layer (22). The negative electrode active material layer (23) may include, for example, lithium metal or a lithium alloy.

[0148] The negative electrode active material layer (23) may include, for example, lithium foil, lithium powder, plated lithium, a carbon-based material, or a combination thereof. The negative electrode active material layer including lithium foil may be, for example, a lithium metal layer. The negative electrode active material layer including lithium powder may be introduced by coating a slurry including lithium powder and a binder, etc., on a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer may be formed of a metal-based negative electrode active material. The negative electrode active material layer (23) may also be a plated lithium metal layer. After manufacturing a lithium battery by assembling a negative electrode (20), a positive electrode, and an electrolyte that do not include a negative electrode active material layer (22), a lithium metal layer deposited between a negative electrode current collector (21) and a protective layer (22) by charging may be further included as a negative electrode active material layer (23).

[0149] The thickness of the negative electrode active material layer (23) may be, for example, 0.1 ㎛ to 100 ㎛, 0.1 ㎛ to 80 ㎛, 1 ㎛ to 80 ㎛, or 10 ㎛ to 80 ㎛, but is not necessarily limited to this range and may be adjusted depending on the shape, capacity, etc. of the required lithium metal battery. If the thickness of the negative electrode active material layer (23) increases excessively, the structural stability of the lithium metal battery may deteriorate and side reactions may increase. If the thickness of the negative electrode active material layer (22) is excessively small, the energy density of the lithium metal battery may decrease. The thickness of the lithium foil may be, for example, 1 ㎛ to 50 ㎛, 1 ㎛ to 30 ㎛, or 10 ㎛ to 30 ㎛, or 10 ㎛ to 80 ㎛. When the lithium foil has a thickness in this range, the life characteristics of the lithium battery including the protective layer can be further improved. The particle size of the lithium powder may be, for example, 0.1 ㎛ to 3 ㎛, 0.1 ㎛ to 2 ㎛, or 0.1 ㎛ to 2 ㎛. When the lithium powder has a thickness in this range, the life characteristics of the lithium battery including the protective layer may be further improved. The thickness of the lithium precipitation layer may be, for example, 1 ㎛ to 80 ㎛, or 10 ㎛ to 80 ㎛.

[0150]

[0151] [Lithium battery]

[0152] A lithium battery according to one embodiment includes a positive electrode; the above-described negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode. By including the above-described negative electrode, the lithium battery can simultaneously provide improved capacity and excellent lifespan characteristics.

[0153] Lithium batteries may be, but are not limited to, lithium primary batteries, lithium secondary batteries, lithium-sulfur batteries, lithium-air batteries, etc., and any lithium battery used in the relevant technical field may be used.

[0154] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.

[0155] (cathode)

[0156] Prepare the cathode described above.

[0157] (anode)

[0158] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.

[0159] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α(In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn dGeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.

[0160] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0161] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO 4-b X b (In the above chemical formula, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).

[0162] Conductive materials include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.

[0163] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.

[0164] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.

[0165] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, binder, and solvent may be omitted.

[0166] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.

[0167] (Separator)

[0168] Next, a separator to be inserted between the positive and negative electrodes is prepared.

[0169] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion migration and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in the form of a nonwoven or woven fabric. For lithium-ion batteries, a rollable separator, such as polyethylene or polypropylene, is used, while for lithium-ion polymer batteries, a separator with excellent organic electrolyte absorption capacity is used.

[0170] The separator is manufactured by the following exemplary methods, but is not limited to these methods and may be adjusted according to required conditions.

[0171] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast on a support and dried, and then a separator film peeled from the support is laminated on the electrode to form a separator.

[0172] The polymer used in separator manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.

[0173] (electrolyte)

[0174] Next, the electrolyte is prepared.

[0175] The electrolyte may be, for example, a liquid electrolyte, a solid electrolyte, or a combination thereof.

[0176] The electrolyte is, for example, an organic electrolyte. An organic electrolyte is prepared by dissolving a lithium salt in an organic solvent, for example.

[0177] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0178] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.

[0179] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.

[0180] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12(0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.

[0181] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON" 0≤x<1), Li 3+y PO 4-x N x( "LIPON" 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("Thio-LISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.

[0182] (lithium battery)

[0183] Referring to FIG. 3, a lithium battery (1) according to an embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.

[0184] Referring to FIG. 4, a lithium battery (1) according to one embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.

[0185] Referring to FIG. 5, a lithium battery (1) according to an embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2) to form a battery structure. A battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding a current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.

[0186] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 3 to 5, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.

[0187] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life and high-rate characteristics. For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.

[0188] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.

[0189]

[0190] [Binder Manufacturing Method]

[0191] According to another embodiment, a method for manufacturing a binder includes: preparing a third composition by mixing a first composition comprising at least one first polymer selected from among polyamic acid and polyimide substituted with a first functional group and a non-aqueous solvent, and a second composition comprising a water-soluble second polymer having a second functional group and water; and preparing a third polymer by heat-treating the third composition at a temperature of 100°C or higher.

[0192] The first polymer, the second polymer, and the third polymer are the same as those described in the binder section described above. The non-aqueous solvent included in the first composition may be a polar solvent such as N-methylpyrrolidone (NMP) or alcohol. The first composition may additionally include water. The second composition may additionally include an aqueous solution containing water or a polar organic solvent such as alcohol that is miscible with water in addition to water. Therefore, the first composition and the second composition may be easily mixed. The time for heat-treating the third composition at a temperature of 100°C or higher is not particularly limited, but, for example, the time for heat-treating the third composition at a temperature of 100°C or higher may be 1 hour to 10 hours. For example, the time for heat-treating the third composition at a temperature of 160°C or higher may be 1 hour to 5 hours. For example, the time for heat-treating the third composition at a temperature of 100°C or higher may be 1 hour to 3 hours. If the heat treatment time is too short, crosslinking may not be sufficiently formed, and if the heat treatment time is too long, the difference in the degree of crosslinking may be minimal compared to the heat treatment time. However, if the heat treatment temperature is too low, the polyamic acid may not cure into polyimide.

[0193] In the above binder manufacturing method, the third composition may be a composition for forming a protective film. Accordingly, by applying the third composition onto the negative electrode current collector and then heat-treating at a temperature of 100°C or higher for 1 to 10 hours, a protective film can be formed simultaneously with the negative electrode manufacturing. For example, by applying the third composition onto the negative electrode current collector and then heat-treating at a temperature of 160°C or higher for 1 to 10 hours, a protective film can be formed simultaneously with the negative electrode manufacturing.

[0194] In the binder manufacturing method, the first polymer may include an alkali metal. The first polymer may be substituted or doped with the alkali metal. For more specific details regarding the first polymer substituted or doped with the alkali metal, refer to the binder section described above.

[0195]

[0196] [Cathode manufacturing method]

[0197] A method for manufacturing a negative electrode according to another embodiment includes the steps of providing a negative electrode current collector; and the step of providing the protective layer on the negative electrode current collector.

[0198] The above protective layer can be formed by applying a third composition including the first polymer and the second polymer described above onto the negative electrode current collector and then heat-treating at a temperature of 100°C or higher for 1 to 10 hours.

[0199] First, a negative electrode current collector is provided. The negative electrode current collector refers to the negative electrode portion described above. For example, copper foil is provided as the negative electrode current collector.

[0200] Next, a protective layer is provided on the negative electrode current collector. The protective layer includes the steps of: preparing a third composition by mixing a first composition including at least one first polymer selected from among polyamic acid and polyimide substituted with a first functional group and a non-aqueous solvent and a second composition including a water-soluble second polymer having a second functional group and water; applying the third composition on the negative electrode current collector and heat-treating at a temperature of 100° C. or higher to form a protective layer.

[0201] The first polymer, second polymer, and third polymer are the same as those described in the binder section above. The non-aqueous solvent included in the first composition may be a polar solvent such as N-methylpyrrolidone (NMP) or alcohol. The first composition may additionally include water. The second composition may additionally include an aqueous solution containing water or a polar organic solvent such as alcohol that is miscible with water in addition to water. Therefore, the first composition and the second composition can be easily mixed.

[0202] The time for applying the third composition on the negative electrode current collector and heat-treating at a temperature of 100°C or higher is not particularly limited, but for example, the time for applying the third composition on the negative electrode current collector and heat-treating at a temperature of 100°C or higher may be 1 to 10 hours. For example, the time for applying the third composition on the negative electrode current collector and heat-treating at a temperature of 100°C or higher may be 1 to 5 hours. For example, the time for applying the third composition on the negative electrode current collector and heat-treating at a temperature of 100°C or higher may be 1 to 3 hours. If the heat-treatment time is too short, cross-linking may not be sufficiently formed, and if the heat-treatment time is too long, the difference in the degree of cross-linking may be minimal compared to the heat-treatment time. However, if the heat-treatment temperature is too low, the polyamic acid may not be cured into polyimide.

[0203] The method for manufacturing an anode may further include a step of introducing an anode intermediate layer between the anode protective layer and the anode current collector. The anode intermediate layer may include a lithium-compatible metal. The anode intermediate layer may include a lithium-compatible metal and a carbon material. The lithium-compatible metal and the carbon material are the same as those described in the anode intermediate layer section described above. For example, the anode intermediate layer may be provided on the anode current collector by applying nanoparticles including the lithium-compatible metal through a nanoparticle casting method. The anode intermediate layer may be provided, for example, by mixing a lithium-compatible metal and a solvent to prepare a first slurry, and then coating and drying the first slurry on the anode current collector. The solvent may be an organic solvent. The solvent may be, for example, N,N-dimethylacetamide, N-methylpyrrolidone (NMP), etc., but is not necessarily limited thereto, and any solvent used in the art may be used. The first slurry may further include a carbon material.

[0204] The negative electrode manufacturing method may further include a step of introducing a negative electrode active material layer between the protective layer and the negative electrode current collector. The negative electrode active material layer may include, for example, lithium metal and / or a lithium alloy.

[0205] The method for introducing the negative electrode active material layer between the protective layer and the negative electrode current collector is not particularly limited. For example, the negative electrode active material layer may be disposed on the negative electrode current collector before providing the protective layer on the negative electrode current collector. The method for arranging the negative electrode active material layer on the negative electrode current collector is not particularly limited. For example, a lithium metal layer may be disposed on the negative electrode current collector by sputtering or the like. Alternatively, a lithium foil may be disposed on the negative electrode current collector and rolled to prepare the layer. Alternatively, a laminate in which a lithium metal layer is laminated on a copper foil may be commercially available and used. Alternatively, a laminate may be prepared by coating and drying a composition including lithium powder and a binder on a metal substrate. For the lithium powder and binder, refer to the negative electrode section described above. Alternatively, after the negative electrode including the negative electrode current collector and the protective layer is prepared, the negative electrode active material layer may be introduced between the negative electrode collector and the protective layer by charging. The negative electrode active material layer may be, for example, a plated lithium layer.

[0206]

[0207] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0208] (Manufacture of cross-linked polymers)

[0209] Manufacturing Example 1: PI-F

[0210] After filling a three-necked round-bottom flask with nitrogen, 9.9790 g (0.0498 mol) of 2,2'-Bis(trifluoromethyl)benzidine (TFMB) and 2.5275 g (0.0166 mol) of 1,3-diaminobenzoic acid (DABA) were added, and 153 g of N-methylpyrrolidone (NMP) was added and completely dissolved using a mechanical stirrer. Subsequently, 14.4935 g (0.0664 mol) of 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride (6FDA) was added, and the mixture was stirred at room temperature for 24 hours to produce a fluorine-substituted polyamic acid represented by the following chemical formula 17 (6FDA / TFMB / DABA, acid equivalent 210 g / eq, weight average molecular weight Mw = approximately 1,000,000). The fluorine-substituted polyamic acid is a random copolymer. The molar ratio of 6FDA:TFMB:DABA was 4:3:1. In chemical formulas 17 and 18, the molar ratio of m:n was 1:3.

[0211] Manufacturing Example 2: LiPI-F

[0212] After filling a three-necked round-bottom flask with nitrogen, 9.9790 g (0.0498 mol) of 2,2'-Bis(trifluoromethyl)benzidine (TFMB) and 2.5275 g (0.0166 mol) of 1,3-diaminobenzoic acid (DABA) were added, and 153 g of N-methylpyrrolidone (NMP) was added and completely dissolved using a mechanical stirrer. Subsequently, 14.4935 g (0.0664 mol) of 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride (6FDA) was added, and the mixture was stirred at room temperature for 24 hours to produce a fluorine-substituted polyamic acid represented by the following chemical formula 17 (6FDA / TFMB / DABA, acid equivalent 210 g / eq, weight average molecular weight Mw = approximately 1,000,000). The fluorine-substituted polyamic acid is a random copolymer. The molar ratio of 6FDA:TFMB:DABA was 4:3:1. In chemical formulas 17 and 18, the molar ratio of m:n was 1:3.

[0213] A fluorine-substituted water-soluble polyamic acid represented by the following chemical formula 18, in which 0.5 equivalents of COOH in the fluorine-substituted polyamic acid were replaced with COO-Li+, was prepared by adding 10 g of a LiOH aqueous solution having an equivalent ratio of 0.5 equivalents to the carboxylic acid to a fluorine-substituted polyamic acid represented by the following chemical formula 17 (6FDA / TFMB / DABA, acid equivalent weight 210 g / eq, weight average molecular weight Mw = approximately 1,000,000). The fluorine-substituted water-soluble polyamic acid represented by the following chemical formula 18 and polyvinyl alcohol (weight average molecular weight, Mw = 78,000, degree of saponification 88%, Polysciences, 15132) were mixed in a weight ratio of 20:80 and then heat-treated in a vacuum oven at 180°C for 2 hours to perform a crosslinking reaction, thereby preparing a crosslinked polymer. A cross-linked polymer of fluorine-substituted polyimide and polyvinyl alcohol was prepared by reacting the carboxyl group of fluorine-substituted polyamic acid with the hydroxyl group of polyvinyl alcohol to form an ester linker. The cross-linked polymer has a three-dimensional network structure in which the polyimide and polyvinyl alcohol are cross-linked at multiple points.

[0214] <Chemical Formula 17>

[0215]

[0216] <Chemical Formula 18>

[0217]

[0218] Comparative Manufacturing Example 1: PI

[0219] In comparison with Example 1, a polyamic acid represented by the following chemical formula 19 was manufactured in the same manner as in Example 1, except that 2,2'-dimethylbenzidine, which does not contain fluorine, was used instead of 2,2'-Bis(trifluoromethyl)benzidine, and 4,4'-(isopropylidene)diphthalic anhydride, which does not contain fluorine, was used instead of 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride.

[0220] <Chemical Formula 19>

[0221]

[0222] Comparative manufacturing example 2: PVA

[0223] The polyvinyl alcohol used in Example 1 was used as is.

[0224] Comparative Manufacturing Example 3: SBR / CMC

[0225] A 1:1 weight ratio mixture of styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) was prepared.

[0226]

[0227] (Manufacturing of cathodes and lithium batteries)

[0228] Example 1: Cu substrate / PI-F:PVA=20:80 protective layer (1 μm)

[0229] (Cathode manufacturing)

[0230] The fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1 was added to N,N-dimethylacetamide (DMAc, 99%, Sigma-Aldrich) and stirred overnight at 60°C to prepare a first composition.

[0231] Polyvinyl alcohol (weight average molecular weight, Mw=78,000, degree of saponification 88%, Polysciences, 15132) was added to N,N-dimethylacetamide (DMAc, 99%, Sigma-Aldrich) and stirred overnight at 60°C to prepare a second composition.

[0232] The first composition and the second composition were mixed so that the fluorine-substituted polyamic acid and the polyvinyl alcohol had a weight ratio of 20:80 to prepare a third composition.

[0233] A crosslinking reaction was performed by heat treatment in a vacuum oven at 180°C for 2 hours to produce a crosslinked polymer. A crosslinked polymer of fluorine-substituted polyimide and polyvinyl alcohol was produced by the reaction of the carboxyl group of the fluorine-substituted polyamic acid and the hydroxyl group of polyvinyl alcohol to form an ester linker. The crosslinked polymer has a three-dimensional network structure in which the polyimide and polyvinyl alcohol are crosslinked at multiple points.

[0234] After coating the third composition on a copper (Cu) current collector having a thickness of 20 ㎛ using a doctor blade, a protective layer was introduced by removing the solvent at 140°C for 6 hours.

[0235] A negative electrode having a negative electrode collector / protective layer structure was manufactured. The thickness of the protective layer was 1 μm.

[0236] (Manufacturing of coin cells)

[0237] A coin cell was manufactured by using a lithium foil with a thickness of 20 μm as a counter electrode, placing a polypropylene separator (Celgard 3510) between the counter electrode and the cathode, and injecting an electrolyte.

[0238] As an electrolyte, a solution containing 1.15 M LiPF6 dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (2:4:4 volume ratio) was used.

[0239] Example 2: Cu substrate / PI-F:PVA=20:80 protective layer (0.5 μm)

[0240] Coin cells were manufactured in the same manner as in Example 1, except that the thickness of the protective layer was 0.5 μm.

[0241] Example 3: Cu substrate / PI-F:PVA=20:80 protective layer (0.3 μm)

[0242] Coin cells were manufactured in the same manner as in Example 1, except that the thickness of the protective layer was 0.3 μm.

[0243] Example 4: Cu substrate / PI-F:PVA=20:80 protective layer (1.5 μm)

[0244] Coin cells were manufactured in the same manner as in Example 1, except that the thickness of the protective layer was 1.5 μm.

[0245] Example 5: Cu substrate / PI-F:PVA=20:80 protective layer (3 μm)

[0246] Coin cells were manufactured in the same manner as in Example 1, except that the thickness of the protective layer was 3 μm.

[0247] Example 6: Cu substrate / PI-F:PVA=20:80 protective layer (5 μm)

[0248] Coin cells were manufactured in the same manner as in Example 1, except that the thickness of the protective layer was 5 μm.

[0249] Example 7: Cu substrate / LiPI-F:PVA=20:80 protective layer (1 μm)

[0250] A coin cell was manufactured in the same manner as in Example 1, except that a water-soluble polyamic acid substituted with fluorine represented by the chemical formula 18 manufactured in Manufacturing Example 2 was used instead of the polyamic acid substituted with fluorine represented by the chemical formula 17 manufactured in Manufacturing Example 1.

[0251] Comparative Example 1: Cu substrate / PI:PVA=20:80 protective layer (1㎛)

[0252] A coin cell was manufactured in the same manner as in Example 1, except that the polyamic acid represented by the chemical formula 19 manufactured in Comparative Manufacturing Example 1 was used instead of the fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1.

[0253] Comparative Example 2: Cu substrate / PVA protective layer (1 μm)

[0254] A coin cell was manufactured in the same manner as Example 1, except that polyvinyl alcohol manufactured in Comparative Manufacturing Example 2 was used instead of the fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1.

[0255] Comparative Example 3: Cu substrate / SBR-CMC protective layer (1 μm)

[0256] A coin cell was manufactured in the same manner as in Example 1, except that SBR-CMC manufactured in Comparative Manufacturing Example 3 was used instead of the fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1.

[0257] Comparative Example 4: Cu substrate / without protective film

[0258] Coin cells were manufactured in the same manner as in Example 1, except that the cathode did not include a protective film.

[0259]

[0260] Evaluation Example 1: Evaluation of the physical properties of the protective film

[0261] Using the protective film manufactured in Example 1 and Comparative Examples 1 to 3, a 5×5 cm size film was formed on a glass substrate.2 After manufacturing a polymer film with a thickness of 50 ㎛, the mechanical properties of the polymer were evaluated as follows.

[0262] The extension, recovery, modulus, and hardness of the protective films manufactured in Example 1 and Comparative Examples 1 to 3 were measured using a microindenter (DUH-211, Shimadzu). The force applied to the polymer film sample was 10 mN.

[0263] The measurement results are shown in Table 1 below. Extension is the distance that the tip of the microindenter moves into the sample until a certain force is applied to the tip, and recovery is the ratio of the distance that the tip moves toward the sample surface from the point where the tip moves the most into the sample to the point where the force applied to the tip becomes zero, to the distance that the tip has moved into the sample. Modulus is the indentation modulus, and hardness is the indentation hardness, and they are calculated from the force applied to the tip from the sample according to the movement distance of the microindenter tip.

[0264] TypeExtension[mm]Recovery[%]Modulus[GPa]Hardness[N / mm2]Example 1PI-F:PVA=20:800.3968.638.11578Comparative Example 1PI:PVA=20:800.3765.334.31754Comparative Example 2PI:PVA=0:1000.3366.529.51695Comparative Example 3SBR / CMC1.2353.94.2169

[0265] As shown in Table 1 above, the protective film of Example 1 had an increased modulus, i.e., elastic coefficient, compared to the protective films of Comparative Examples 1 to 3, thereby increasing the strength of the binder and suppressing expansion of the negative electrode.

[0266]

[0267] Evaluation Example 2: Charge / Discharge Characteristics Evaluation

[0268] The lithium batteries (coin cells) manufactured in Examples 1 to 7 and Comparative Examples 1 to 4 were charged at a constant current rate of 0.1 C at 25°C until the voltage reached 0.01 V (vs. Li), and then charged at a constant voltage rate until the current reached 0.01 C while maintaining 0.01 V. After charging, the lithium batteries were allowed to rest for 10 minutes, and then discharged at a constant current rate of 0.1 C until the voltage reached 1.5 V (vs. Li) (1 st cycle).

[0269] Then, the coin cell was charged at a constant current rate of 0.2C until the voltage reached 0.01 V (vs. Li), and then charged at a constant voltage rate until the current reached 0.01 C while maintaining 0.01 V. After the coin cell was rested for 10 minutes after charging, it was discharged at a constant current rate of 0.2C until the voltage reached 1.5 V (vs. Li) (2 nd cycle)(1st-2nd cycle is the Mars phase).

[0270] The coin cell that had undergone the above-mentioned Martian step was charged at a constant current rate of 1.0 C at 25°C until the voltage reached 0.01 V (vs. Li), and then charged at a constant voltage rate until the current reached 0.01 C while maintaining 0.01 V. After the coin cell was rested for 10 minutes, the discharge cycle was repeated 50 times at a constant current rate of 1.0 C until the voltage reached 1.5 V (vs. Li). Some of the results of the charge-discharge experiment are shown in Table 2 below.

[0271] The electrode thickness expansion rate, initial efficiency, and capacity retention rate were calculated from the following mathematical equations 1 to 3, respectively. In the electrode thickness expansion rate, the electrode is a cathode.

[0272] <Mathematical Formula 1>

[0273] Thickness expansion ratio (%) = [electrode thickness of the disassembled battery after the 2nd cycle charge / electrode thickness before battery assembly] × 100.

[0274] <Mathematical Formula 2>

[0275] Initial efficiency [%] = [1 st Discharge capacity in cycles / 1 st Charging capacity in cycle] × 100

[0276] <Mathematical Formula 3>

[0277] Capacity retention rate [%] = [53 rd Discharge capacity of cycle / 3 rd Discharge capacity of cycle] × 100

[0278] Shield initial efficiency [%] 1 st Cycle discharge capacity [mAh / g] Capacity retention [%] Electrode thickness expansion rate [%] Type Thickness (㎛) Example 1 PI-F:PVA = 20:80 194.12 3.38 7.5240 Example 2 PI-F:PVA = 20:80 0.59 2.82 3.18 2.1250 Example 3 PI-F:PVA = 20:80 0.39 1.22 2.87 7.6260 Example 4 PI-F:PVA = 20:80 1.59 3.72 3.38 9.7235 Example 5 PI-F:PVA = 20:80 391.02 2.76 9.2260 Example 6 LiPI-F:PVA = 20:80 194.32 2.99 0.1240 Comparative example 1PI:PVA=20:80190.821.285.4330Comparative example 2PI:PVA=0:100110.55.3N / A350Comparative example 3SBR / CMC155.917.765.5410Comparative example 4No protective film-94.023.188.3450

[0279] As shown in Table 2, the lithium batteries of Examples 1 to 7 formed a stable SEI during the initial electrodeposition compared to the lithium batteries of Comparative Examples 1 to 4, resulting in an initial efficiency, 1 st The electrode thickness expansion rate was reduced while the cycle discharge capacity and capacity retention rate were maintained or improved.

[0280] [Explanation of symbols]

[0281] 1: Lithium battery 2: Cathode

[0282] 3: Anode 4: Separator

[0283] 5: Battery case 6: Cap assembly

Claims

1. A third polymer comprising a crosslinking reaction product of at least one first polymer selected from among polyamic acid and polyimide having a first functional group and substituted with fluorine and a water-soluble second polymer having a second functional group, A binder in which the first polymer and the second polymer are crosslinked by the reaction of the first functional group and the second functional group to form an ester bond.

2. In paragraph 1, A binder, wherein the first functional group and the second functional group are independently any one selected from the group consisting of a carboxyl group, an amide group, an aldehyde group, and a hydroxyl group.

3. In paragraph 1, A binder wherein the first polymer comprises an alkali metal.

4. In paragraph 3, A binder, wherein the alkali metal content of the first polymer is 0.2 to 1.0 in an equivalent ratio to the carboxyl group or amide group.

5. In paragraph 1, The above polyimide is a binder represented by the following chemical formula 1 or chemical formula 2: <Chemical Formula 1> <Chemical Formula 2> Among the above chemical formulas 1 and 2, M is an alkali metal, Ar1, Ar2, Ar4 and Ar5 are independently an aromatic ring group selected from a trivalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with a halogen or a halogen-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; or a trivalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with a halogen or a halogen-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; The above aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-O. Ar3 and Ar6 are independently an aromatic ring group selected from among a divalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with fluorine or a fluorine-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; or a divalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with fluorine or a fluorine-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; The above aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-. X1 is -COOH, -OH, -CO-NH2, or -COH, Y1 and Y2 are each independently an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이다.

6. In paragraph 1, The above polyimide is a binder represented by the following chemical formula 3 or chemical formula 4: <Chemical Formula 3> <Chemical Formula 4> Among the above chemical formulas 3 and 4, M is lithium or sodium, R1 to R 20 are independently a halogen; -COOH; -OH; -CO-NH2; -COH; an alkyl group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen; an aryl group having 6 to 20 carbon atoms substituted or unsubstituted with a halogen; or a heteroaryl group having 2 to 20 carbon atoms substituted or unsubstituted with a halogen; At least one of R5 to R8 is -COOH, -OH, -CO-NH2, or -COH, R 13 Inland R 20 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, Y1 to Y3 are each independently a single bond or an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이다.

7. In paragraph 1, The above polyamic acid is a binder represented by the following chemical formula 7 or chemical formula 8: <Chemical Formula 7> <Chemical Formula 8> Among the above chemical formulas 7 and 8, M is an alkali metal, Ar1, Ar2, Ar4 and Ar5 are independently an aromatic ring group selected from a trivalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with a halogen or a halogen-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; or a trivalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with a halogen or a halogen-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; The above aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-O. Ar3 and Ar6 are independently an aromatic ring group selected from among a divalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with fluorine or a fluorine-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; or a divalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with fluorine or a fluorine-substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; The above aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-. X1 is -COOH, -OH, -CO-NH2, or -COH, Y1 is an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이다.

8. In paragraph 1, The above polyamic acid is a binder represented by the following chemical formula 9 or chemical formula 10: <Chemical Formula 9> <Chemical Formula 10> Among the above chemical formulas 9 and 10, M is lithium or sodium, R1 to R 20 are independently hydrogen; halogen; -COOH; -OH; -CO-NH2; -COH; an alkyl group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen; an aryl group having 6 to 20 carbon atoms substituted or unsubstituted with a halogen; or a heteroaryl group having 2 to 20 carbon atoms substituted or unsubstituted with a halogen; At least one of R5 to R8 is -COOH, -OH, -CO-NH2, or -COH, R 13 Inland R 20 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, Y1 to Y3 are each independently a single bond or an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이다.

9. In paragraph 1, The polyimide is represented by the following chemical formula 5 or chemical formula 6, and the polyamic acid is represented by the following chemical formula 11 or chemical formula 12, the binder: <Chemical Formula 5> <Chemical Formula 6> <Chemical Formula 11> <Chemical Formula 12> Among the above chemical formulas 5, 6, 11 and 12, R 51 Inland R 58 are independently an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine (F), R 51 Inland R 58 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이다.

10. In paragraph 9, 0 <m<0.5, 0.5<n<1 및 n+m=1인 바인더.

11. In paragraph 1, A binder wherein the second polymer is a polymerization reaction product of one or more monomers selected from among a vinyl monomer, an acetate monomer, an alcohol monomer, an acrylic monomer, a methacrylic monomer, an acrylamide monomer, and a methacrylamide monomer, or a hydrolyzate thereof.

12. In paragraph 1, The second polymer is vinyl acetate, vinyl alcohol, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxyethylene glycol (meth)acrylate, 2-hydroxypropylene glycol (meth)acrylate, acrylic acid, methacrylic acid, 2-(meth)acryloyloxy acetic acid, 3-(meth)acryloyloxy propyl acid, 4-(meth)acryloyloxy butyric acid, itaconic acid, maleic acid, 2-isocyanatoethyl (meth)acrylate, 3-isocyanatopropyl A binder, which is a polymerization reaction product of one or more monomers selected from (meth)acrylate, 4-isocyanatobutyl (meth)acrylate, (meth)acrylamide, ethylenedi(meth)acrylate, diethyleneglycol(meth)acrylate, triethyleneglycoldi(meth)acrylate, trimethylenepropanetri(meth)acrylate, trimethylenepropanetriacrylate, 1,3-butanediol(meth)acrylate, 1,6-hexanedioldi(meth)acrylate, allyl acrylate, and N-vinyl caprolactam, or a hydrolyzate thereof.

13. In paragraph 1, A binder wherein the second polymer is polyvinyl alcohol.

14. In the first paragraph, a binder in which the weight ratio of the first polymer and the second polymer is 1:99 to 50:50 15. In the first paragraph, the third polymer is a binder represented by the following chemical formulas 13 to 16: <Chemical Formula 13> <Chemical Formula 14> <Chemical Formula 15> <Chemical Formula 16> In the above equations, n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이며, p는 중합도로서 250 내지 12500다.

16. Negative current collector; and A negative electrode comprising a protective layer disposed on the negative electrode current collector and including a binder according to claim 1.

17. In paragraph 16, The thickness of the above protective layer is 5㎛ or less, the cathode.

18. In paragraph 16, The above negative electrode collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A cathode, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

19. Bipolar; The cathode according to Article 16; and A lithium battery comprising an electrolyte disposed between the positive electrode and the negative electrode.

20. In paragraph 19, A lithium battery wherein the electrolyte is a liquid electrolyte, a solid electrolyte, or a combination thereof.

Citation Information

Patent Citations

  • Negative electrode of lithium metal battery andlithium metal battery comprisng same

    KR1020050041661A

  • Lithium electrode comprising polymer protecting layer and lithium secondary battery employing thereof

    KR1020170061866A

  • Memory controller and operating method thereof

    KR1020200114149A

  • Fixing Device for Building Exterior with Vibration Transmission Blocking Part

    KR102521346B1

  • Sloped mold prefabricated pedestal

    KR102521437B1