Sealant for new energy battery and preparation method thereof

By using bisphenol A type epoxy resin and bisphenol F type epoxy resin, along with epoxy silane coupling agent to modify boron nitride and nano-alumina, a thermally conductive network is constructed, solving the problem of poor sealant compatibility and achieving high strength and high thermal conductivity.

CN118879256APending Publication Date: 2024-11-01JIANGSU ZHIXIN NEW MATERIALS CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411106969.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing sealants used in new energy batteries have poor compatibility issues in terms of improving strength and thermal conductivity, resulting in poor sealing and inability to effectively protect the battery.

Method used

Bisphenol A type epoxy resin and bisphenol F type epoxy resin are used in combination, and boron nitride and nano-alumina are modified by epoxy silane coupling agent to construct a thermally conductive network, reduce interfacial thermal resistance, and improve compatibility and wettability.

Benefits of technology

The prepared sealant has high strength and good thermal conductivity, which can effectively protect new energy batteries and ensure the stability and safety of batteries under long-distance bumps and unexpected conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a sealant for a new energy battery and a preparation method thereof.The sealant for the new energy battery is prepared from, by weight, an agent A and an agent B. The agent A is prepared from, by mass, 25-27 parts of bisphenol A type epoxy resin, 5-8 parts of bisphenol F type epoxy resin, 15-20 parts of heat conduction filler and 5-8 parts of reactive diluent; the heat-conducting filler comprises epoxy silane coupling agent modified boron nitride; the agent B comprises the following raw materials in parts by mass: 18-21 parts of a polyamide curing agent, 10-11 parts of a fatty amine curing agent, 1-2 parts of a silane coupling agent and 1-3 parts of a reactive diluent. The sealant for the new energy battery is high in strength, good in heat conduction effect and suitable for bonding of various materials, and is particularly used as the sealant for the new energy battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a sealant, and more specifically, to a sealant for new energy batteries and a preparation method thereof. Background Art

[0002] At present, new energy batteries are increasingly being used in all walks of life, especially new energy battery vehicles, which are a key link in solving energy security and are developing more and more rapidly. As one of the most important components in new energy vehicles, the safety and stability of batteries cannot be ignored.

[0003] The current causes of battery failure are battery damage, leakage and local short circuit. Therefore, the sealant used for new energy batteries needs to have higher strength and better thermal conductivity. The higher strength of the sealant can provide more adequate protection for the battery, and it is still stable after the car has been running for a long time and bumpy. It is not easy for the battery to be damaged in the event of an accident. High thermal conductivity can dissipate heat for the battery in time to further improve the reliability of the battery and make the vehicle safer. The existing technology generally improves the performance of the sealant by adding reinforcing fillers, but the reinforcing fillers are generally not compatible with the sealant, and are prone to agglomeration or precipitation, which also causes the sealant to have poor sealing. How to provide a sealant with both high strength and high thermal conductivity that can meet the bonding and protection needs of various materials such as new energy batteries is a problem to be solved. Summary of the invention

[0004] In order to solve the problem of high bonding strength and hardness of sealants, the present application provides a sealant for new energy batteries and a preparation method thereof.

[0005] In a first aspect, the present application provides a sealant for new energy batteries, comprising agent A and agent B, wherein agent A comprises the following raw materials in parts by mass: 25-27 parts of bisphenol A epoxy resin, 5-8 parts of bisphenol F epoxy resin, 15-20 parts of thermally conductive filler, and 5-8 parts of active diluent, wherein the thermally conductive filler comprises boron nitride modified with an epoxy silane coupling agent; agent B comprises the following raw materials in parts by mass: 18-21 parts of a polyamide curing agent, 10-11 parts of a fatty amine curing agent, 1-2 parts of a silane coupling agent, and 1-3 parts of an active diluent.

[0006] By adopting the above scheme, boron nitride is an efficient thermal conductive material with a two-dimensional sheet structure, good insulation performance and chemical stability, and is suitable for use in new energy battery sealants. However, the compatibility of boron nitride with the sealant system is poor. The gap between boron nitride and the sealant may be due to the presence of a small air gap, which makes the interface thermal resistance large. The thermal conductivity of the obtained sealant does not reach the expected level, and it will also produce a certain amount of sedimentation, further affecting the structure of the thermal conductive network. Bisphenol A epoxy resin has a high bonding strength after curing, and bisphenol F epoxy resin has good wettability to boron nitride. By using bisphenol A epoxy resin and bisphenol F epoxy resin together, the sealant obtained has both certain strength and wettability to boron nitride, reducing the interface thermal resistance of the thermal conductive filler network in the sealant. By modifying boron nitride with an epoxy silane coupling agent, its compatibility and wettability in the sealant are further improved, reducing the interface thermal resistance. By adding a certain mass of active diluent to agent A and agent B and a certain mass of silane coupling agent to agent B, the viscosity of the sealant is reduced, the sealant system has a better effect on coating the thermally conductive filler, the prepared sealant is uniform and stable after curing, the thermally conductive filler is tightly connected to the sealant system, and the strength performance and thermal conductivity effect are good.

[0007] In a specific embodiment, the mass ratio of the thermal conductive filler to the bisphenol F epoxy resin is 3:(1-1.1).

[0008] By adopting the above scheme, the quality of the thermally conductive filler and the bisphenol F epoxy resin with good wetting effect is limited. On the one hand, the sealant has the excellent properties of both bisphenol A epoxy resin and bisphenol F epoxy resin. On the other hand, it also ensures that the sealant system has good wettability for the thermally conductive filler, small interface thermal resistance, and good thermal conductivity of the obtained sealant.

[0009] In a specific embodiment, the thermal conductive filler also includes nano-alumina modified with an epoxy silane coupling agent.

[0010] By adopting the above solution, the two-dimensional boron nitride gaps are filled with zero-dimensional modified nano-alumina powder with good thermal conductivity, which not only reduces the interfacial thermal resistance in the system, but also better connects the thermal conduction pathway, further improving the thermal conductivity performance of the new energy battery sealant.

[0011] In a specific embodiment, the mass ratio of epoxy silane coupling agent modified boron nitride to epoxy silane coupling agent modified nano alumina is (2.9-3.1):1.

[0012] By adopting the above scheme, the mass ratio of two-dimensional boron nitride and zero-dimensional nano-aluminum oxide is appropriate, and they are mixed by point-to-surface coating, surface-to-surface connection, etc. The filler is not easy to precipitate and is evenly distributed in the sealant, so that the obtained sealant has good thermal conductivity.

[0013] In a specific embodiment, the preparation steps of epoxysilane coupling agent modified boron nitride include: adding boron nitride to an ethanol aqueous solution, then ultrasonically dispersing, adding an epoxysilane coupling agent, stirring and reacting at 80-85°C, filtering, washing, and drying to obtain epoxysilane coupling agent modified boron nitride.

[0014] By adopting the above scheme, the steps of boron nitride modification are relatively simple, the modified product is relatively stable and has good effect, the obtained silane-modified boron nitride is not easy to precipitate in the sealant, the distribution is relatively uniform and stable, the compatibility is good, the modified boron nitride is more tightly connected to the sealant system, the interface thermal resistance is low, and the strength and thermal conductivity of the obtained sealant are good.

[0015] In one specific embodiment, the boron nitride is plasma treated.

[0016] By adopting the above scheme, the hydroxyl content on the surface of the boron nitride after plasma treatment is higher, which further improves the modification effect of the epoxysilane-modified boron nitride, reduces the interface thermal resistance and improves the thermal conductivity.

[0017] In a specific implementation scheme, the plasma treatment step includes: placing boron nitride on the lower plate, introducing protective gas, and then plasma treating, the distance between boron nitride and the plate is 2-3 mm, the plasma treatment voltage is 4-5 kV, the frequency is 2-2.5 kHz, and the time is 20-30 s.

[0018] By adopting the above scheme, the steps of plasma treatment are relatively simple, the treatment effect is better, and the surface of the boron nitride after treatment has more active groups.

[0019] In a specific embodiment, the particle size of the boron nitride is 70-100 μm.

[0020] By adopting the above scheme, the effect of plasma modification is better, the active hydroxyl groups on the surface of boron nitride account for a larger proportion, the distribution of boron nitride in this system is further optimized, and the thermal conductive path structure in the prepared sealant is better.

[0021] In a second aspect, the present application provides a method for preparing a sealant for a new energy battery, comprising the following steps: S1: Preparation of Agent A: weighing and mixing bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to a mass ratio, stirring for 10-25 minutes, then adding a thermal conductive filler, and stirring for 20-30 minutes to obtain Agent A; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20-25 minutes to obtain Agent B; S3: Mix agent A and agent B evenly to obtain a sealant.

[0022] By adopting the above technical scheme, the sealant system is more uniform and the curing is more complete. The thermal conductive filler in the system is evenly distributed and not easy to precipitate, and the connection is tight. The prepared sealant has higher strength and toughness and is not easy to become brittle. The cured sealant shrinks less and is not easy to have structural defects.

[0023] In summary, this application has the following beneficial effects: Compared with the prior art, the present application adds a certain mass of epoxysilane coupling agent-modified boron nitride to sealant A agent, and matches it with bisphenol A epoxy resin and bisphenol F epoxy resin with certain strength and wettability, and further limits the mass ratio of thermal conductive filler to bisphenol F epoxy resin, the mass ratio of epoxysilane coupling agent-modified boron nitride and epoxysilane coupling agent-modified nano-alumina, and the obtained sealant internal two-dimensional thermal conductive filler and zero-dimensional thermal conductive filler cooperate to construct a thermal conductive network, and has good compatibility and wettability, the filler is tightly connected to the sealant system, the interface thermal resistance is small, and the strength is high. Further, the boron nitride is plasma treated before modification, which further increases its surface active groups, the silane modification effect is good, the distribution in the sealant is more uniform and stable, the constructed thermal conductive network structure is better, and the obtained sealant has good thermal conductivity. DETAILED DESCRIPTION

[0024] In the examples and comparative examples of the present application, the polyamide curing agent was purchased from Kain Chemical Co., Ltd., the fatty amine curing agent was H-55 from Chubu Chemical Co., Ltd., the active diluent was C12-14 alkyl glycidyl ether, the epoxy silane coupling agent was KH-172, the amino silane coupling agent was KH-540, and the remaining experimental reagents, unless otherwise specified, were conventional commercial brands or obtained through conventional preparation processes.

[0025] Preparation Example Preparation Example 1: Plasma-treated boron nitride: Boron nitride was placed on the lower electrode plate, and protective gas was introduced, followed by plasma treatment. The distance between the boron nitride and the electrode plate was 2 mm, the plasma treatment voltage was 5 kV, the frequency was 2 kHz, and the time was 20 s.

[0026] Preparation Example 2: Boron nitride modified with epoxy silane coupling agent: 75 g of boron nitride was added to 1700 ml of 50% wt ethanol aqueous solution, and then ultrasonically dispersed at a power of 300 W for 30 minutes, and then epoxy silane coupling agent was added, stirred and reacted at 85° C. for 3 hours, filtered, washed with pure water, and dried to obtain epoxy silane coupling agent-modified boron nitride.

[0027] Preparation Example 3: Plasma-treated boron nitride modified with epoxy silane coupling agent: 75 g of the plasma-treated boron nitride obtained in Preparation Example 1 was added to 1700 ml of a 50% wt ethanol aqueous solution, and then ultrasonically dispersed at a power of 300 W for 30 minutes, and then an epoxy silane coupling agent was added, stirred and reacted at 85° C. for 3 hours, filtered, washed with pure water, and dried to obtain epoxy silane coupling agent-modified boron nitride.

[0028] Preparation Example 4: Epoxysilane coupling agent modified nano-alumina: 75 g of nano-alumina was added to 1700 ml of 50% wt ethanol aqueous solution, and then ultrasonically dispersed at a power of 300 W for 30 minutes, and then epoxy silane coupling agent was added, stirred and reacted at 85° C. for 3 hours, filtered, washed with pure water, and dried to obtain epoxy silane coupling agent modified nano-alumina.

[0029] Preparation Example 5: Aminosilane coupling agent modified boron nitride: 3g of silane coupling agent, 200ml of ethanol and 25g of pure water were mixed evenly, and then 100g of boron nitride was added, and the mixture was stirred at 5°C for 1 hour, and then ultrasonically dispersed at a power of 300W for 30 minutes, and stirred at 80°C for 3 hours, filtered, washed with pure water, and dried to obtain aminosilane coupling agent-modified boron nitride; Example

[0030] Example 1 The masses of the components in this embodiment are as follows: Agent A: 250 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, thermal conductive filler: 200 g of boron nitride modified with epoxy silane coupling agent obtained in Preparation Example 2, 80 g of active diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxy silane coupling agent, and 10 g of active diluent.

[0031] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0032] Example 2 The masses of the components in this embodiment are as follows: Agent A: 270 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, thermal conductive filler: 180 g of boron nitride modified with epoxy silane coupling agent obtained in Preparation Example 2, 70 g of reactive diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxy silane coupling agent, and 30 g of reactive diluent.

[0033] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0034] Example 3 The masses of the components in this embodiment are as follows: Agent A: 260 g of bisphenol A epoxy resin, 60 g of bisphenol F epoxy resin, thermal conductive filler: 150 g of boron nitride modified with epoxysilane coupling agent obtained in Preparation Example 2, 80 g of reactive diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxysilane coupling agent, and 10 g of reactive diluent.

[0035] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0036] Example 4 The masses of the components in this embodiment are as follows: Agent A: 250 g of bisphenol A epoxy resin, 73.3 g of bisphenol F epoxy resin, thermal conductive filler: 200 g of boron nitride modified with epoxy silane coupling agent obtained in Preparation Example 2, 80 g of reactive diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxy silane coupling agent, and 10 g of reactive diluent.

[0037] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0038] Example 5 The masses of the components in this embodiment are as follows: Agent A: 250 g of bisphenol A epoxy resin, 73.3 g of bisphenol F epoxy resin, thermal conductive filler: 150 g of boron nitride modified with epoxy silane coupling agent prepared in Preparation Example 2, 50 g of nano-alumina modified with epoxy silane coupling agent prepared in Preparation Example 4, and 80 g of reactive diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxy silane coupling agent, and 10 g of reactive diluent.

[0039] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0040] Example 6 The masses of the components in this embodiment are as follows: Agent A: 250 g of bisphenol A epoxy resin, 73.3 g of bisphenol F epoxy resin, thermal conductive filler: 155 g of boron nitride modified with epoxy silane coupling agent obtained in Preparation Example 2, 45 g of nano-alumina modified with epoxy silane coupling agent obtained in Preparation Example 4, and 80 g of reactive diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxy silane coupling agent, and 10 g of reactive diluent.

[0041] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0042] Example 7 The masses of the components in this embodiment are as follows: Agent A: 250 g of bisphenol A epoxy resin, 73.3 g of bisphenol F epoxy resin, thermal conductive filler: 200 g of plasma-treated boron nitride modified by epoxy silane coupling agent obtained in Preparation Example 3, 80 g of reactive diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxy silane coupling agent, and 10 g of reactive diluent.

[0043] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0044] Example 8 The masses of the components in this embodiment are as follows: Agent A: 250 g of bisphenol A epoxy resin, 73.3 g of bisphenol F epoxy resin, thermal conductive filler: 150 g of plasma-treated boron nitride modified by epoxy silane coupling agent obtained in Preparation Example 3, 50 g of nano-alumina modified by epoxy silane coupling agent obtained in Preparation Example 4, and 80 g of reactive diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxy silane coupling agent, and 10 g of reactive diluent.

[0045] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0046] Comparative Example Comparative Example 1 The mass of each component in this comparative example is: Agent A: 250g of bisphenol A epoxy resin, 50g of bisphenol F epoxy resin, thermal conductive filler: 150g of boron nitride, 80g of active diluent; Agent B: 200g of polyamide curing agent, 100g of fatty amine curing agent, 10g of epoxy silane coupling agent, and 10g of active diluent.

[0047] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0048] Comparative Example 2 The masses of the components in this comparative example are as follows: Agent A: 300 g of bisphenol A epoxy resin, thermal conductive filler: 150 g of boron nitride modified with epoxysilane coupling agent obtained in Preparation Example 2, 80 g of active diluent; Agent B: 200 g of polyamide curing agent, 100 g of fatty amine curing agent, 10 g of epoxysilane coupling agent, and 10 g of active diluent.

[0049] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0050] Comparative Example 3: The mass of each component in this comparative example is: Agent A: 250g of bisphenol A epoxy resin, 50g of bisphenol F epoxy resin, thermal conductive filler: 200g of aminosilane coupling agent modified boron nitride obtained in Preparation Example 5, 80g of active diluent; Agent B: 200g of polyamide curing agent, 100g of fatty amine curing agent, 10g of epoxy silane coupling agent, and 10g of active diluent.

[0051] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0052] Comparative Example 4: The mass of each component in this comparative example is: Agent A: 250g of bisphenol A epoxy resin, 50g of bisphenol F epoxy resin, thermal conductive filler: 150g of boron nitride modified by aminosilane coupling agent prepared in Preparation Example 5, 50g of nano-alumina modified by epoxysilane coupling agent prepared in Preparation Example 4, 80g of active diluent; Agent B: 200g of polyamide curing agent, 100g of fatty amine curing agent, 10g of epoxysilane coupling agent, and 10g of active diluent.

[0053] S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin, and active diluent according to mass, stir for 15 minutes, then add thermal conductive filler, and stir for 20 minutes; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20 minutes; S3: Mix agent A and agent B evenly to obtain a sealant.

[0054] Performance test test 1: Referring to the standard ISO4587, the shear strength of the sealants prepared in each embodiment and comparative example was tested, and the test results are summarized in Table 1: Test 2: The thermal conductivity of the sealants prepared in each embodiment and comparative example was tested according to the standard ASTM D5470. The test results are summarized in Table 1: Table 1 Shear strength(MPa) Thermal conductivity (W / m×K) Example 1 14.8 3.88 Example 2 14.5 3.63 Example 3 14.3 3.62 Example 4 15.1 3.93 Example 5 15.6 4.33 Example 6 15.3 4.09 Example 7 15.4 4.18 Example 8 15.7 4.52 Comparative Example 1 10.2 2.79 Comparative Example 2 11.4 3.10 Comparative Example 3 11.8 3.15 Comparative Example 4 12.3 3.33 In combination with Examples 1-4, Comparative Examples 1-4 and Table 1, the present application adds a certain mass of epoxy silane coupling agent to the sealant to modify and limit the mass ratio of each component, and limit the mass ratio of bisphenol F epoxy resin and modified boron nitride, so that the obtained sealant has a certain strength, and the sealant system fully wets the thermal conductive filler, greatly reducing the interfacial thermal resistance, and the obtained sealant has high strength and high thermal conductivity. The present application realizes the dispersion and arrangement of particles in the system by epoxy silane coupling agent modified boron nitride and epoxy silane coupling agent modified nano alumina, which is conducive to forming a better heat conduction path. When only amino silane coupling agent modified boron nitride or a certain mass of amino silane coupling agent modified boron nitride and epoxy silane coupling agent modified nano alumina are added as fillers, it is easy to cause a faster curing rate or active groups based on different active cross-linking, which affects the cross arrangement and effective dispersion of boron nitride particles and nano alumina particles in the system, thereby affecting the thermal conductivity of the sealant.

[0055] In combination with Examples 4-6 and Table 1, the present application further adds modified nano-alumina to Agent A and limits its mass ratio to modified boron nitride, and the two-dimensional thermal conductive filler and the zero-dimensional thermal conductive filler cooperate with each other to further improve the thermal conductive network, so that the obtained sealant has a high thermal conductivity coefficient.

[0056] In combination with Example 4, Examples 7-8 and Table 1, the present application increases the number of surface active groups of boron nitride by first subjecting boron nitride to plasma treatment and then subjecting it to epoxy silane coupling agent modification, thereby improving the effect of subsequent epoxy silane coupling agent modification of boron nitride, and further improving the thermal conductivity of the prepared sealant.

[0057] This specific embodiment of the present application is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, a person skilled in the art may make modifications to the embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A sealant for new energy batteries, characterized in that: The invention comprises agent A and agent B, wherein agent A comprises the following raw materials in parts by mass: 25-27 parts of bisphenol A epoxy resin, 5-8 parts of bisphenol F epoxy resin, 15-20 parts of thermal conductive filler, and 5-8 parts of active diluent, wherein the thermal conductive filler comprises boron nitride modified by epoxy silane coupling agent; agent B comprises the following raw materials in parts by mass: 18-21 parts of polyamide curing agent, 10-11 parts of fatty amine curing agent, 1-2 parts of silane coupling agent, and 1-3 parts of active diluent.

2. The sealant for new energy batteries according to claim 1, characterized in that: The mass ratio of the thermal conductive filler to the bisphenol F epoxy resin is 3:(1-1.1).

3. The sealant for new energy batteries according to claim 1, characterized in that: The thermal conductive filler also includes epoxy silane coupling agent modified nano alumina.

4. The sealant for new energy batteries according to claim 3, characterized in that: The mass ratio of the epoxy silane coupling agent modified boron nitride to the epoxy silane coupling agent modified nano-alumina is (2.9-3.1):

1.

5. The sealant for new energy batteries according to claim 1, characterized in that: The preparation steps of the epoxysilane coupling agent modified boron nitride include: adding boron nitride to an ethanol aqueous solution, then ultrasonically dispersing, adding an epoxysilane coupling agent, stirring and reacting at 80-85° C., filtering, washing, and drying to obtain epoxysilane coupling agent modified boron nitride.

6. The sealant for new energy batteries according to claim 5, characterized in that: The boron nitride is plasma treated.

7. The sealant for new energy batteries according to claim 6, characterized in that: The plasma treatment step includes: placing boron nitride on the lower electrode plate, introducing protective gas, and then plasma treatment, the distance between boron nitride and the electrode plate is 2-3mm, the plasma treatment voltage is 4-5 kV, the frequency is 2-2.5kHz, and the time is 20-30s.

8. The sealant for new energy batteries according to claim 7, characterized in that: The particle size of the boron nitride is 70-100 μm.

9. A method for preparing a sealant for new energy batteries according to any one of claims 1 to 8, characterized in that: The steps include: S1: Preparation of Agent A: Weigh and mix bisphenol A epoxy resin, bisphenol F epoxy resin and active diluent according to mass ratio, stir for 10-25 minutes, then add thermal conductive filler, stir for 20-30 minutes to obtain Agent A; S2: Preparation of Agent B: weigh and mix the raw materials of Agent B according to the mass ratio, and stir for 20-25 minutes to obtain Agent B; S3: Mix agent A and agent B evenly to obtain a sealant.

Citation Information

Cited By

  • Battery shell, preparation method thereof and secondary battery

    CN119119832A

  • Battery casing, preparation method thereof, and secondary battery

    CN119119832B

  • High-heat-resistance epoxy resin curing agent and preparation method thereof

    CN120775160A

  • High heat resistant epoxy resin curing agent and preparation method thereof

    CN120775160B