Photosensitive resin composition, dry film, cured product, printed wiring board, and laminate
The photosensitive resin composition, featuring a carboxyl group-containing resin, inorganic filler, and trimethylbenzoylphosphine oxide initiator, addresses reflectance and yellowing issues in dry films for printed wiring boards by reducing outgassing and improving encapsulant reaction rates, resulting in enhanced reliability and performance.
Patent Information
- Application Number
- PCT/KR2024/003983
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-27
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Current photosensitive dry films for printed wiring boards face issues with high reflectance, yellowing resistance, and outgassing problems, leading to reduced reflectance and long-term reliability, especially when used with silicone encapsulants and under high temperature/high humidity conditions.
A photosensitive resin composition containing a carboxyl group-containing resin without aromatic rings, an inorganic filler, and a photopolymerization initiator with a trimethylbenzoylphosphine oxide group, which reduces outgassing and enhances the reaction rate of silicone encapsulants, allowing for higher reflectance and improved HAST resistance.
The solution significantly reduces outgassing, improves yellowing resistance, and maintains high reflectance even under challenging conditions, enhancing the reliability and performance of solder resist layers in printed wiring boards.
Smart Images

Figure KR2024003983_03102024_PF_FP_ABST
Abstract
Description
Photosensitive resin composition, dry film, cured product, printed wiring board and laminate
[0001] The present invention relates to a photosensitive resin composition, a dry film, a cured product, a printed wiring board, and a laminate. Specifically, the dry film has a photosensitive resin layer formed by applying and drying the photosensitive resin composition on a first film, the cured product is obtained by curing the photosensitive resin layer of the dry film, and the printed wiring board and the laminate include the cured product.
[0002] In general, in printed wiring boards used in electronic devices, etc., when mounting electronic components on a printed wiring board, a solder resist layer is formed in areas other than the connection holes on the board where the circuit pattern is formed, in order to prevent solder from being attached to unnecessary areas and to prevent the conductors of the circuit from being exposed and corroded by oxidation or humidity.
[0003] Recently, with the advancement in the precision and density of printed wiring boards due to the miniaturization and thinning of electronic devices, the solder resist layer is currently formed mainly by so-called photo solder resist, which is formed by applying a photosensitive resin composition to a board, forming a pattern through exposure and development, and then curing the patterned resin by heating or light irradiation.
[0004] The liquid photosensitive resin composition as described above contains a solvent in the composition, so the printing and composition drying processes must be repeated during manufacturing, which has the problem of requiring a long working time and being unfriendly to the environment.
[0005] Accordingly, it has been proposed to form a solder resist layer using a so-called photosensitive dry film, which, instead of a liquid photosensitive resin composition, allows for the omission of a drying process after applying the composition. Using a dry film for lamination shortens the working time, significantly shortening the manufacturing process and achieving excellent productivity. Furthermore, the solder resist layer can be efficiently used even on thin-film substrates.
[0006] These dry films generally have a laminated structure in which a photosensitive resin layer, i.e., a solder resist layer, is formed on a first film, which is a substrate, and a second film is bonded to the layer for purposes such as protection. When in use, the second film is peeled off, heat-pressed onto a wiring board, exposed from above the first film, and then the first film is peeled off and developed, thereby forming a patterned solder resist layer. When a solder resist layer is formed using a dry film, compared to a case in which a liquid photosensitive resin composition as described above is used, not only can the composition drying step be omitted, but also, since the dry film is pressed onto the circuit board, it is difficult for air bubbles to be mixed between the substrate and the solder resist layer, so that the hole-filling performance of the concave portion of the substrate surface is improved. In addition, when a solder resist layer is formed using a dry film, the flatness of the film is excellent, so that chips can be mounted efficiently and the resolution is high.
[0007] However, in the case of a white solder resist layer, since the reflectivity is higher than that of a colored solder resist layer, when a solder resist layer is formed using a dry film in the above manner, there is a problem in that when exposed, light is reflected from the surface of the solder resist layer, making it difficult for the light to penetrate to the lower part, and a phenomenon (halation) in which the upper part of the surface becomes larger than the lower part occurs, making it difficult to implement a pattern (see, for example, Patent Document 1, etc.).
[0008] Meanwhile, since the solder resist layer also functions as a permanent protective film for the circuit board, the solder resist composition is required to have various performances such as alkaline development properties and solder heat resistance.
[0009] In addition, for the white solder resist layer, in addition to the required characteristics as a general solder resist layer, it is also important to have high reflectivity, little decrease in reflectivity due to the manufacturing process, and no yellowing of the cured product when exposed to heat or light.
[0010] In addition to the basic properties required for a solder resist layer, there is a need for a photosensitive resin composition that satisfies additional properties required for a white solder resist layer, has a higher reflectivity than conventional ones and has excellent yellowing resistance, and a method for manufacturing a dry film and a printed wiring board including a solder resist layer that can solve unique problems that occur during the manufacturing process of the solder resist layer.
[0011] (Patent Document 1) Korean Patent Publication No. 10-2022-0086524
[0012] Conventionally, photopolymerization initiators (e.g., 2,4,6-trimethylbenzoyldiphenyl phosphine oxide (TPO)) included in photosensitive resin compositions forming solder resists generate a large amount of outgas. If this outgas diffuses into an adjacent silicone encapsulant, yellowing may occur in the transparent silicone encapsulant, reducing reflectivity and preventing proper curing of the silicone encapsulant. Due to these problems, there have been problems with the long-term reliability of the substrate. In addition, the photopolymerization initiator may be transferred not only to the silicone encapsulant but also to an adjacent substrate, etc.
[0013] Accordingly, in order to remove outgassing of the photopolymerization initiator, it was considered to add a baking process (e.g., curing at 150°C for 6 hours) after a reflow process (e.g., performing at 260°C for 10 seconds), but there was a problem that the reflectivity was significantly reduced by this baking process, and thus, when used in a backlight unit, etc., there was an increase in power consumption to increase the reflectivity after the chip was mounted. In other words, as the process lengthens, the reflectivity may also decrease.
[0014] Additionally, a protective film (PF) may be placed on the solder resist layer prior to the firing process to remove the photopolymerization initiator. The protective film is a film that removes the outgassing of the photopolymerization initiator as much as possible before the subsequent firing process after the solder resist is manufactured. It is peeled and removed before the firing process, and because it has a high affinity for the photopolymerization initiator, it can efficiently remove the photopolymerization initiator, so it was used for the purpose of removing the photopolymerization initiator. However, in the end, two additional processes, the use of this protective film and the firing process, were required, and the problem of reduced reflectivity still existed.
[0015] The present invention is intended to solve the above problems, and provides a technique for a photosensitive resin composition comprising (A) a carboxyl group-containing resin not containing an aromatic ring, (B) an inorganic filler or (C) a mercapto-modified (meth)acrylate, and (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond.
[0016] The photosensitive resin composition of the present invention significantly reduces outgassing of a photopolymerization initiator, thereby improving yellowing and non-curing problems of silicone encapsulating materials, and enhancing the reaction rate of the silicone encapsulating materials. In addition, by suppressing the amount of outgassing generated by the photopolymerization initiator, the amount of outgassing transferred to a protective film can be reduced, and since the baking process after the reflow process can be omitted, the power consumption problem can be improved by increasing reflectivity. In addition, the photosensitive resin composition of the present invention has high HAST (Highly Accelerated Stress Test) resistance, high reflectivity after reflow, UV test, or HAST test, excellent HAST resistance, and can suppress the decrease in reflectivity under high temperature / high humidity conditions. Due to these characteristics, the solder resist manufactured using the photosensitive resin composition of the present invention exhibits excellent effects.
[0017] In addition, the present invention provides a dry film, a cured product, a printed wiring board, and a laminate using the photosensitive resin composition.
[0018] One embodiment of the present invention relates to a photosensitive resin composition.
[0019] In one aspect, the photosensitive resin composition may include (A) a carboxyl group-containing resin that does not contain an aromatic ring, (B) an inorganic filler, and (E) a photopolymerization initiator that is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond.
[0020] In one aspect, the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), may include a *-C(=O)-P(=O)R1-O-*' moiety (wherein R1 is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a cyclic group having 5 to 20 carbon atoms).
[0021] In one aspect, the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), may be a trimethylbenzoylphosphine oxide group-containing polymer.
[0022] In one aspect, the trimethylbenzoylphosphine oxide group-containing polymer has a weight average molecular weight (M n ) can be greater than 900 g / mol.
[0023] In one aspect, the trimethylbenzoylphosphine oxide group-containing polymer may be represented by the following chemical formula 1.
[0024] <Chemical Formula 1>
[0025]
[0026] a= 0~100, b= 0~100, c=0~100
[0027] In one aspect, the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), may include an alkoxy group.
[0028] In one aspect, the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), may include an ethoxy group.
[0029] In one aspect, the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), may be represented by the following chemical formula 2.
[0030] <Chemical Formula 2>
[0031]
[0032] In one aspect, the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), may be 0.01 to 10 wt% based on the total weight of the composition.
[0033] In one aspect, the carboxyl group-containing resin not containing the aromatic ring (A) may contain an unsaturated double bond.
[0034] In one aspect, the photosensitive resin composition may further include (D) a resin containing an aromatic ring.
[0035] In one aspect, the resin containing the aromatic ring (D) may be a melamine resin, a silicone resin, or a resin having a styrene skeleton.
[0036] In one aspect, the photosensitive resin composition may further comprise (C) a mercapto-modified (meth)acrylate.
[0037] In one aspect, the photosensitive resin composition may additionally include (F) a silane coupling agent.
[0038] In one aspect, the photosensitive resin composition may further include a resin having a (G) urethane bond.
[0039] In one aspect, the content of outgas measured by thermal desorption spectroscopy (TDS) and gas chromatography-mass spectrometry (GC-MS) for the photosensitive resin composition may be 1,000 ppm or less with respect to the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including (E) one or more PO bonds.
[0040] In one aspect, the photosensitive resin composition may have a phosphorus content of 500 to 5000 ppm.
[0041] Another embodiment of the present invention relates to a photosensitive resin composition comprising (A) a carboxyl group-containing resin not containing an aromatic ring, (C) a mercapto-modified (meth)acrylate, and (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond.
[0042] In one aspect, the photosensitive resin composition may further include (D) a resin containing an aromatic ring.
[0043] In one aspect, the photosensitive resin composition may additionally include (F) a silane coupling agent.
[0044] In one aspect, the photosensitive resin composition may further include a resin having a (G) urethane bond.
[0045] Another embodiment of the present invention relates to a dry film having a photosensitive resin layer formed by applying and drying the photosensitive resin composition described above on a first film.
[0046] Another embodiment of the present invention relates to a cured product obtained by curing the photosensitive resin layer of the photosensitive resin composition described above or a dry film obtained through the same.
[0047] Another embodiment of the present invention relates to a printed wiring board comprising the above-described cured product as a solder resist.
[0048] In one aspect, the printed wiring board may further include a silicone encapsulant layer disposed on the solder resist.
[0049] In one aspect, the silicone encapsulating material layer includes an upper encapsulating material region and a lower encapsulating material region, and the content of the (E) photopolymerization initiator included in at least one of the upper encapsulating material region or the lower encapsulating material region may be 1,000 ppm or less relative to the content of the (E) photopolymerization initiator included in the solder resist.
[0050] Another embodiment of the present invention relates to a laminate comprising the above-described cured product and a protective film.
[0051] In one aspect, the content of the (E) photopolymerization initiator included in the protective film may be 1,000 ppm or less with respect to the content of the (E) photopolymerization initiator included in the solder resist.
[0052] A photosensitive resin composition according to one embodiment of the present invention can significantly reduce outgassing of a photopolymerization initiator, thereby improving yellowing and uncured problems of silicone encapsulating materials, and enhancing the reaction rate of the silicone encapsulating materials. In addition, the amount of outgassing of the photopolymerization initiator transferred to a protective film can be reduced, and the baking process after the reflow process can be omitted, thereby improving the power consumption problem through increased reflectance. In addition, the photosensitive resin composition has high HAST resistance and reflectance after a HAST test, and the decrease in reflectance under high temperature / high humidity conditions can be suppressed. Due to these characteristics, a solder resist manufactured using the photosensitive resin composition of the present invention can exhibit excellent effects.
[0053] For example, a photosensitive resin composition according to one aspect of the present invention can obtain an excellent reflectivity maintenance effect by further including titanium oxide as an inorganic filler.
[0054] In addition, the present invention can provide a dry film, a cured product, and a printed wiring board using the photosensitive resin composition.
[0055] Figures 1a and 1b are images showing the BHAST test results of dry films using the photosensitive resin compositions of Comparative Example 1 and Example 3, respectively.
[0056] Various embodiments of the present invention are described below.
[0057] [Photosensitive resin composition]
[0058] One embodiment of the present invention relates to a photosensitive resin composition comprising (A) a carboxyl group-containing resin not containing an aromatic ring, (B) an inorganic filler, and (E) at least one photopolymerization initiator selected from a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond.
[0059] Another embodiment of the present invention relates to a photosensitive resin composition comprising (A) a carboxyl group-containing resin not containing an aromatic ring, (C) a mercapto-modified (meth)acrylate, and (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond.
[0060] The above photosensitive resin composition can suppress outgassing and exhibit excellent silicone encapsulating material reaction rate, reflectivity, and HAST resistance.
[0061] For example, the photosensitive resin composition may be a composition that is cured to form a solder resist.
[0062] Below, each component of the photosensitive resin composition is described in detail.
[0063] [(A) Carboxyl group-containing resin not containing an aromatic ring]
[0064] In a photosensitive resin composition according to one embodiment of the present invention, (A) a carboxyl group-containing resin that does not contain an aromatic ring (hereinafter, “resin (A)”) may be a resin that exhibits electrical insulation properties by being cured by irradiation with active energy rays. Examples of the aromatic ring include a benzene ring, a pyridine ring, a pyrimidine ring, a triazine ring, and the like.
[0065] Resin (A) contains a carboxyl group, which enables alkaline development, and since it does not contain an aromatic ring, it has excellent resistance to discoloration and yellowing when exposed to heat or UV energy. In addition, due to the combination of the (B) inorganic filler described below, high reflectivity can be realized, the reflectivity decreases less after the reflow process, and the reflectivity decreases less after a 3,000-hour blue light test. Therefore, the composition including resin (A) has less reflectivity decrease due to discoloration and yellowing and excellent yellowing resistance compared to other white ink compositions. For example, a carboxyl group-containing resin including an aromatic ring has a relatively low initial reflectivity of a cured product compared to resin (A) that does not contain an aromatic ring, and the decrease in reflectivity may be very high when performing heat, UV, BHAST, and 85℃ / 85% tests. This is because the aromatic ring is deformed by heat, UV, BHAST, and 85℃ / 85% tests, which greatly contributes to the decrease in reflectivity.
[0066] For example, the resin (A) may contain an unsaturated double bond. By containing an unsaturated double bond, the resin (A) is capable of radical curing by ultraviolet rays, electron beams, or heat.
[0067] The resin (A) is not particularly limited as long as it does not contain an aromatic ring and contains a carboxyl group, but may be, for example, a photosensitive carboxyl group-containing resin having at least one photosensitive unsaturated double bond therein or a carboxyl group-containing resin without a photosensitive unsaturated double bond.
[0068] For example, as the resin (A), any of the resins listed below that do not have an aromatic ring (either an oligomer or a polymer is preferable) can be suitably used:
[0069] (1) A carboxyl group-containing resin obtained by copolymerization of an unsaturated carboxylic acid and a compound having an unsaturated double bond;
[0070] (2) A photosensitive carboxyl group-containing resin obtained by reacting a carboxyl group-containing (meth)acrylic copolymer resin with a compound having an oxirane ring and an ethylenically unsaturated group in one molecule.
[0071] (3) A photosensitive carboxyl group-containing resin obtained by reacting a copolymer of a compound having one epoxy group and an unsaturated double bond in each molecule and a compound having an unsaturated double bond with an unsaturated monocarboxylic acid, and reacting the secondary hydroxyl group-saturated or unsaturated polybasic acid anhydride produced by the reaction.
[0072] (4) A resin containing photosensitive hydroxyl and carboxyl groups, obtained by reacting a saturated or unsaturated polybasic acid anhydride with a hydroxyl group-containing polymer, and then reacting a compound having one epoxy group and one unsaturated double bond in each of the carboxylic acid molecules produced by the reaction.
[0073] For example, the resin (A) may be a (a) carboxyl group-containing (meth)acrylic copolymer resin, which is a resin containing a photosensitive carboxyl group of (2), and (b) a copolymer resin having a carboxyl group obtained by the reaction of a compound having an oxirane ring and an ethylenically unsaturated group in one molecule.
[0074] For example, (a) a carboxyl group-containing (meth)acrylic copolymer resin can be obtained by copolymerizing a (meth)acrylic acid ester and a compound having one unsaturated group and at least one carboxyl group per molecule, but is not limited thereto. The (meth)acrylic acid esters constituting the copolymer resin (a) include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate, hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and caprolactone-modified 2-hydroxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, and isooctyloxyethylene glycol (meth)acrylate, Examples of glycol-modified (meth)acrylates include phenoxytriethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate. These may be used alone, or two or more types may be mixed and used. In addition, in this specification, (meth)acrylate is a general term for acrylate and methacrylate, and the same applies to other similar expressions.
[0075] In addition, compounds having one unsaturated group and at least one carboxyl group in one molecule include acrylic acid, methacrylic acid, modified unsaturated monocarboxylic acids with an extended chain between the unsaturated group and the carboxylic acid, such as β-carboxyethyl (meth)acrylate, 2-acryloyloxyethyl cohaxic acid, 2-acryloyloxyethyl hexahydrophthalic acid, unsaturated monocarboxylic acids having an ester bond through lactone modification, modified unsaturated monocarboxylic acids having an ether bond, and maleic acid, which contain two or more carboxyl groups in the molecule. These may be used alone or as a mixture of two or more.
[0076] (b) The compound having an oxirane ring and an ethylenically unsaturated group in one molecule may be any compound having an oxirane ring and an ethylenically unsaturated group in one molecule, and examples thereof include glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylbutyl (meth)acrylate, and 3,4-epoxycyclohexylmethylaminoacrylate. These may be used alone, or two or more types may be mixed and used. For example, (b) the compound having an oxirane ring and an ethylenically unsaturated group in one molecule may be 3,4-epoxycyclohexylmethyl (meth)acrylate.
[0077] For example, the acid value of the resin (A) may be 30 to 200 mgKOH / g. When the acid value of the resin (A) is 30 mgKOH / g or more, the unexposed portion of the solder resist composition film in a weakly alkaline aqueous solution can be easily removed. When the acid value of the resin (A) is 200 mgKOH / g or less, the water resistance and electrical properties of the cured film can be improved.
[0078] For example, the weight average molecular weight of the resin (A) may be 5,000 to 100,000 g / mol. When the weight average molecular weight of the resin (A) is 5,000 g / mol or more, the deterioration of the touch-drying property of the solder resist composition film can be suppressed. When the weight average molecular weight of the resin (A) is 100,000 g / mol or less, the deterioration of the developability and storage stability of the solder resist composition can be suppressed.
[0079] In the photosensitive resin composition of the present invention, the content of the resin (A) may be 5 to 40 wt%, 10 to 35 wt%, or 12 to 33 wt% based on the total composition. The composition includes a solid content and a solvent. The content of the resin (A) may be calculated based on the solid content conversion standard.
[0080] When the content of resin (A) is within the above range, the yellowing resistance is excellent, high reflectivity can be achieved, a solder resist film can be formed well, excellent pencil hardness and adhesion can be exhibited, and the touch dryness of the film and undercutting can be suppressed.
[0081] [(B) Weapon Filler]
[0082] A photosensitive resin composition according to one embodiment of the present invention can obtain high reflectance by including an inorganic filler.
[0083] Inorganic fillers include, for example, titanium oxide, zinc oxide, basic carbonate, basic sulfate, sulfate, zinc sulfide, antimony oxide, aluminum hydroxide, silica, barium sulfate, etc. For example, when a composition is implemented by mixing barium sulfate and silica and using them as an inorganic filler, the L value is 80 or more, the a value is -5 or more, and the b value is -5 or more. The L value may be measured by Hunter 1948. For example, when a composition is implemented by using a high content of titanium oxide and silica as inorganic fillers, the cured product of the composition has an L value of 90 or more, an a value of -3 or more, and a b value of -3 or more, thereby exhibiting high whiteness and reflectance. For example, when a composition is implemented by using at least one of titanium oxide and silica as an inorganic filler, the L value may be 95 or more, an a value of -2 or more, and a b value of -1 or more, thereby exhibiting the highest whiteness and reflectance.
[0084] For example, the manufacturing method of titanium oxide can be either the sulfuric acid method or the chlorine method, and for example, the chlorine method may be used. For example, sulfuric acid may not be used in the manufacturing process. Furthermore, the surface treatment of titanium oxide is not particularly limited, but may be titanium oxide treated with an acid other than sulfuric acid, such as hydrochloric acid, nitric acid, phosphoric acid, or acetic acid, during neutralization.
[0085] Titanium oxide may be of any structure, including rutile, anatase, and Ramsdelight types, and may be used alone or in combination of two or more types. Among these, Ramsdelight type titanium oxide is Ramsdelight type Li. 0.5 TiO2 can be obtained by performing chemical lithium oxide removal treatment.
[0086] Among the above, the use of rutile-type titanium oxide can further improve heat resistance, make it difficult for discoloration due to light irradiation to occur, and make it difficult for quality to deteriorate even in a strict usage environment. In particular, the heat resistance can be improved by using rutile-type titanium oxide surface-treated with aluminum oxide such as alumina. The content of rutile-type titanium oxide surface-treated with aluminum oxide in the total titanium oxide is, for example, 35 mass% or more, for example, 55 mass% or more, and the upper limit is 100 mass% or less, that is, the entire amount of titanium oxide may be rutile-type titanium oxide surface-treated with the above aluminum oxide. In addition, since anatase-type titanium oxide has a lower hardness than rutile-type titanium oxide, the formability of the composition is further improved when anatase-type titanium oxide is used.
[0087] In the photosensitive resin composition of the present invention, the blending amount of the (B) inorganic filler may be in the range of 30 to 70 mass%, for example, in the range of 40 to 70 mass%, for example, in the range of 45 to 70 mass%, based on the entire resin composition. The content of the (B) inorganic filler may be calculated based on the solid content conversion standard. If the content of the (B) inorganic filler is within the above range, it is advantageous for high reflection, and if it is less than the above range, the reflectivity decreases, and if it exceeds the above range, cracks may occur.
[0088] (B) Among the inorganic fillers, the sulfur concentration of titanium oxide may be 100 ppm or less, or 50 ppm or less. In addition, commercially available titanium oxide having a sulfur concentration of 100 ppm or less may be used, or commercially available titanium oxide having a sulfur concentration of 100 ppm or more may be mixed and lowered by performing a purification process such as heat treatment or chemical treatment, washing, or calcination. Here, the sulfur contained in the titanium oxide refers to all sulfur detected by analysis. It includes sulfur adsorbed on the titanium oxide and sulfur coated on the titanium oxide as an impurity. In addition, the sodium concentration of the titanium oxide may be 100 ppm or less, or 50 ppm or less. The lower the sodium concentration, the better. If the sodium concentration is too high, corrosion or oxidation may be promoted when the copper substrate is exposed to moisture due to sodium ions. For this reason, the concentration of sodium ions may be less than 100 ppm.
[0089] In addition, the photosensitive resin composition of the present invention may contain titanium oxide having a sulfur concentration of 100 ppm or more, as long as the effects of the present invention are not impaired. Titanium oxide having a sulfur concentration of 100 ppm or more includes CR-58, CR-90, and R-630 manufactured by Isahara Sangyo Co., Ltd., and R-21 manufactured by Sakai-chem Co., Ltd.
[0090] In addition, rutile type chlorinated titanium dioxide such as T-550, T-580, R-630, R-820, CR-50, CR-60, R-90, CR-97 manufactured by Ishihara Sangyo Co., Ltd., Ti PURE R-706, R-902+, R931 manufactured by DuPont, TR-600, TR-700, TR-840 manufactured by Fuji Titanium Industry Co., Ltd., and KR-270, KR-310, KR-380 manufactured by Titanium Industry Co., Ltd. can be used.
[0091] If the particle size of titanium oxide is too small, the fluidity may be poor, and conversely, if it is too large, the insertability into small diameter substrates may be poor. Considering these, the median particle size of titanium oxide is in the range of 0.1 to 5 ㎛, for example, in the range of 0.1 to 1 ㎛, for example, in the range of 0.1 to 0.5 ㎛, and may be 0.36 ㎛. When the particle size of titanium oxide is within the above range, high reflectivity can be exhibited. The above particle size was measured using a laser diffraction method.
[0092] (B) Among inorganic fillers, barium sulfate includes precipitated barium sulfate #100, precipitated barium sulfate #300, precipitated barium sulfate SS-50, BARIACE B-30, BARIACE B-31, BARIACE B-32, BARIACE B-33, BARIACE B-34, BARIFINE BF-1, BARIFINE BF-10, BARIFINE BF-20, BARIFINE BF-40 (manufactured by Sakai Kagaku Kogyo Co., Ltd.), W-1, W-6, W-10, C300 (manufactured by Takehara Kagaku Kogyo Co., Ltd.), etc.
[0093] (B) Among inorganic fillers, silica particles are not particularly limited and can be obtained by a method known to those skilled in the art. For example, they can be manufactured by burning silicon powder using the VMC (Vaporized Metal Combustion) method. The VMC method is a method in which a chemical flame is formed by a burner in an atmosphere containing oxygen, and a metal powder constituting a portion of the target oxide particle is injected into the chemical flame in an amount that forms a dust cloud, thereby causing knocking to obtain oxide particles. Examples of commercially available silica include the SO series manufactured by Admatex Co., Ltd. and the HPS series manufactured by Toagosei Co., Ltd. (HPS-0500, HPS-1000, HPS3500, etc.).
[0094] [(C) Mercapto-modified (meth)acrylate]
[0095] The photosensitive resin composition according to one embodiment of the present invention can enhance surface hardening, improve gloss, and achieve high reflectivity by using (C) mercapto-modified (meth)acrylate.
[0096] In addition, when the (C) mercapto-modified (meth)acrylate of the present invention is used in a photosensitive resin composition together with the (B) inorganic filler described above, the surface curing of the photosensitive resin layer is improved, and the improvement in surface curing enables implementation of higher reflectivity and higher gloss.
[0097] The (C) mercapto-modified (meth)acrylate of the present invention is a compound modified by introducing a mercapto group into an acrylate compound, wherein the acrylate compound may be a monofunctional or polyfunctional acrylate compound, and may be an aliphatic compound having 1 to 15 carbon atoms substituted with at least one functional group selected from the group consisting of an acryloyl group, an acryloyloxy group, and an acryloyloxyalkyl group, and examples thereof include pentane triacrylate.
[0098] The (C) mercapto-modified (meth)acrylate of the present invention may be curable or may be active energy ray-curable, and the (C) mercapto-modified (meth)acrylate of the present invention can be obtained by Michael addition reaction of a mercapto-modified (meth)acrylate polyfunctional thiol compound and a stoichiometrically excessive bifunctional or higher polyfunctional (meth)acrylate compound. As polyfunctional thiol compounds, for example, polyisocyanates such as pentaerythritol tetrakis(3-mercaptopropionate) (molecular weight 489 g / mol), trimethylolpropane tris(3-mercaptopropionate) (molecular weight 399 g / mol), 1,3-bis(2-isocyanato-2-propyl)benzene tetrathiol (thiol) and polyfunctional thiol compounds such as trimethylolpropane tris(3-mercaptopropionate) are reaction products, polyisocyanates such as isophorone diisocyanate are reaction products, polyfunctional thiol compounds such as trimethylolpropane tris(3-mercaptopropionate) are reaction products, polyisocyanates such as hexamethylene diisocyanate are reaction products, polyfunctional thiols such as trimethylolpropane tris(3-mercaptopropionate) are reaction products. Polyfunctional thiol compounds of reaction products with compounds include 1,6-hexanedithiol (molecular weight 150 g / mol), ethylene glycol di-2-mercaptoacetate (molecular weight 210 g / mol), pentaerythritol tetrakis(2-mercaptoacetate) (molecular weight 433 g / mol), trimethylolpropane tris(2-mercaptoacetate), ethylene glycol bis(3-mercaptopropionate) (molecular weight 238 g / mol), etc. For example, the (C) mercapto-modified (meth)acrylate may include two or more mercapto groups, or may include three or more mercapto groups.
[0099] The above (C) mercapto-modified (meth)acrylate may have a weight average molecular weight of 5,000 g / mol or less, 3,000 g / mol or less, or 2,000 g / mol or less. Since the weight average molecular weight is 5,000 g / mol or less, the mobility of the mercapto-modified (meth)acrylate molecules is reduced, so that the reduction in the reactivity of the active energy ray-curable coating film formation of the present invention can be suppressed. For example, if the reactivity is reduced, when the coating film is cured with UV-LED, the tackiness of the surface of the cured coating film increases, and the possibility of the problem of the cured coating film sticking to the printed matter when the printed matter is placed may increase.
[0100] In the photosensitive resin composition of the present invention, the content of the (C) mercapto-modified (meth)acrylate may be 1 to 20 parts by weight, 1 to 10 parts by weight, or 1 to 7 parts by weight based on 100 parts by weight of the entire composition.
[0101] (C) When the content of mercapto-modified (meth)acrylate is within the above range, surface hardening is enhanced, resulting in improved gloss, high reflectivity, less reduction in reflectivity after the manufacturing process, and superior crack resistance. In addition, gloss reduction due to reduced surface hardening can be suppressed, high reflectivity can be achieved, and the surface can be appropriately hardened to reduce brittleness of the coating, and improve resolution.
[0102] [(D) Resin containing an aromatic ring]
[0103] The photosensitive resin composition of the present invention includes (A) a carboxyl group-containing resin that does not contain an aromatic ring, but may additionally include (D) a resin containing an aromatic ring in addition to the (A) resin.
[0104] (D) A resin containing an aromatic ring can exhibit excellent yellowing resistance when combined with (A) resin. The photosensitive resin composition according to one embodiment of the present invention can exhibit excellent yellowing resistance by including (D) an aromatic ring-containing resin in a smaller amount than the (A) resin.
[0105] The resin containing the (D) aromatic ring of the present invention may be, for example, a resin that exhibits electrical insulation properties by being cured by heating.
[0106] The above aromatic ring may be a benzene ring, a pyridine ring, a pyrimidine ring, a triazine ring, etc., and as the resin containing the (D) aromatic ring of the present invention, for example, a melamine resin, a silicone resin, a resin having a styrene skeleton, etc., and for example, a resin having a styrene skeleton may be used.
[0107] In addition, (D) the resin containing an aromatic ring may contain a carboxyl group, and may be, for example, a carboxyl group-containing resin having a styrene skeleton. For example, (D) the resin containing an aromatic ring may be a mixture of a carboxyl group-containing resin having a styrene skeleton and a carboxyl group-containing resin other than a carboxyl group-containing resin having a styrene skeleton.
[0108] For example, if the resin containing (D) an aromatic ring is a carboxyl group-containing resin having a styrene skeleton, it may not have a photosensitive group such as an ethylenically unsaturated bond having a carboxyl group in the molecule, may have a styrene skeleton in the molecule, have an average molecular weight of 10,000 to 50,000 g / mol, and may have an acid value of 80 to 200 mgKOH / g. Such a carboxyl group-containing resin having a styrene skeleton can be synthesized by copolymerizing styrene as an essential monomer. By using a carboxyl group-containing resin having the properties in the above-described range, excellent touch-drying properties and flow-prevention effects of a cured film can be achieved.
[0109] Examples of carboxyl group-containing resins having a styrene skeleton include carboxyl group-containing resins (regardless of oligomers and polymers) that can be obtained by copolymerization with an unsaturated carboxylic acid such as (meth)acrylic acid and a compound containing an unsaturated group selected from styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc. Here, lower alkyl can mean an alkyl group having 1 to 5 carbon atoms.
[0110] In the photosensitive resin composition of the present invention, the weight average molecular weight of the carboxyl group-containing resin having a styrene skeleton varies depending on the resin skeleton, but may be 10,000 g / mol to 50,000 g / mol, 10,000 g / mol to 25,000 g / mol, 10,000 g / mol to 20,000 g / mol, or 10,000 g / mol to 17,000 g / mol. By setting the weight average molecular weight to 10,000 g / mol or more, not only is the flow prevention effect improved, but also the tackiness is further improved, the moisture resistance of the exposed film is improved, and the film reduction during development can be suppressed and the deterioration of the resolution can be suppressed. In addition, by setting the weight average molecular weight to 50,000 g / mol or less, not only the flow prevention effect but also the developability and storage stability can be improved.
[0111] In the photosensitive resin composition of the present invention, the acid value of the carboxyl group-containing resin having a styrene skeleton may be 80 to 200 mgKOH / g, or 100 to 180 mgKOH / g. By setting the acid value of the carboxyl group-containing resin having a styrene skeleton to 80 mgKOH / g or more, the softening point may be increased, thereby improving tackiness and developability. On the other hand, by setting the acid value of the carboxyl group-containing resin having a styrene skeleton to 200 mgKOH / g or less, a suitable crosslinking density may be achieved so that stress is not generated during curing and a good coating film can be obtained.
[0112] In the photosensitive resin composition of the present invention, the carboxyl group-containing resin having a styrene skeleton has an aromatic ring because it has a styrene skeleton, and thus suppresses a decrease in reflectance and discoloration due to light irradiation and heat of the cured product, and can have excellent developability and touch-drying properties. The ratio of the styrene skeleton can be 10 to 80 mol%, 10 to 60 mol%, or 10 to 50 mol% based on the molecule. That is, when synthesizing the carboxyl group-containing resin having a styrene skeleton, 30 to 60 mol% of styrene can be used based on the total amount of monomers. When the ratio of the styrene skeleton of the carboxyl group-containing resin having a styrene skeleton is 10 mol% or more based on the molecule, compatibility with other components becomes good, and when it is 80 mol% or less based on the molecule, developability can become good.
[0113] A carboxyl group-containing resin having a styrene backbone can be manufactured by suspension polymerization to become a high molecular weight resin. As a result, a photosensitive resin composition using the resin can have an excellent tacky effect. Generally, when a carboxyl group-containing resin having a styrene backbone is manufactured by suspension polymerization, it becomes a high molecular weight resin. However, considering characteristics such as screen printing suitability, tackiness, and developability, the weight average molecular weight can be limited to the range of 10,000 to 50,000 g / mol. Therefore, in order to control the molecular weight, a chain transfer agent can be used when synthesizing a carboxyl group-containing resin having a styrene backbone.
[0114] In addition, a polymerization initiator can be used when synthesizing a carboxyl group-containing resin having a styrene backbone to promote polymerization. Examples of the polymerization initiator include BPO (benzoyl peroxide), t-butylperoxy-2-ethylhexanonate, AMBN (2,2'-azobis(2-methylbutyronitrile)), and the like, and for example, BPO (benzoyl peroxide) can be used. The blending amount of the polymerization initiator can be 0.1 to 10 wt%, or 0.1 to 6 wt%, in terms of solid content, based on 100 wt% of the carboxyl group-containing resin having a styrene backbone.
[0115] In the photosensitive resin composition of the present invention, the content of the resin containing (D) an aromatic ring may be 0.1 to 15 wt%, 1 to 10 wt%, or 2 to 6 wt% based on the total weight of the composition. The photosensitive resin composition includes a solid content and a solvent.
[0116] (D) If the content of the resin containing an aromatic ring is within the above range, the decrease in reflectivity and discoloration are suppressed, and the developability and touch-drying properties are excellent, so that the effect of improving reflectivity and the effect of preventing yellowing can be improved.
[0117] [(E) Photopolymerization initiator]
[0118] A photosensitive resin composition according to one embodiment of the present invention may include a photopolymerization initiator (E) which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (hereinafter, “photopolymerization initiator (E)”).
[0119] In the case of 2,4,6-trimethylbenzoyldiphenyl phosphine oxide (TPO), which is widely used as a conventional photopolymerization initiator, a large amount of outgas is generated during the curing process, and these outgases diffuse into the silicone encapsulant layer or protective film, causing yellowing of the silicone encapsulant, reducing reflectivity and making curing of the silicone encapsulant difficult. This caused problems with the long-term reliability of the product.
[0120] As a photopolymerization initiator, a polymer containing a trimethylbenzoylphosphine oxide group has a high molecular structure and a large molecular weight, so the amount of outgassing due to heat is small even in the final curing stage where heat is applied, or in the reflow and firing processes.
[0121] Meanwhile, it is presumed that even in a trimethylbenzoylphosphine oxide group-containing compound having a lower molecular weight than TPO, by including one or more PO bonds, the outgassing of the photopolymerization initiator can be significantly suppressed by improving the bonding strength between molecules (e.g., stronger hydrogen bonding with OH groups or COOH groups that remain unreacted in the composition).
[0122] For example, the trimethylbenzoylphosphine oxide group-containing compound may include three or more hydrogen bonding sites. This enhances the intermolecular bonding strength, thereby significantly suppressing outgassing of the photopolymerization initiator.
[0123] Accordingly, the yellowing and non-curing problems of the silicone encapsulating material can be improved, the amount of outgas of the photopolymerization initiator transferred to the protective film can be reduced, and the reaction rate of the silicone encapsulating material can be significantly increased.
[0124] In addition, when using a photopolymerization initiator such as TPO, a separate firing process (e.g., curing at 150°C for 6 hours) was added after the reflow process to efficiently remove the resulting outgassing. However, this firing process significantly lowered the reflectivity, which resulted in an increase in power consumption when the chip was mounted.
[0125] However, by using the photopolymerization initiator (E) of the present invention described above, the baking process is omitted, so that the working time is reduced, the yield is increased, the cost is reduced, the reflectivity can be increased, the power consumption due to the decrease in reflectivity can be prevented, the outgassing content of the photopolymerization initiator is very low without using a protective film for removing the photopolymerization initiator, etc., the degree of curing of the silicone is greatly increased, the long-term reliability is improved, and excellent HAST resistance and reflectivity after the HAST test can be exhibited. In addition, the decrease in reflectivity under high temperature / high humidity conditions can be suppressed.
[0126] The above photopolymerization initiator (E) may be liquid at room temperature (20°C) and 1 atm.
[0127] The above photopolymerization initiator (E) may contain a PO bond.
[0128] The above photopolymerization initiator (E) may include a *-C(=O)-P(=O)R1-O-*' moiety (wherein R1 is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a cyclic group having 5 to 20 carbon atoms).
[0129] When the above photopolymerization initiator (E) is a polymer containing a trimethylbenzoylphosphine oxide group, the polymer containing a trimethylbenzoylphosphine oxide group has a weight average molecular weight (M n ) may be about 1,000 g / mol or more. For example, the trimethylbenzoylphosphine oxide group-containing polymer may have a weight average molecular weight (M n) can be from 1,000 g / mol to 100,000 g / mol.
[0130] The above trimethylbenzoylphosphine oxide group-containing polymer can be represented by the following chemical formula 1.
[0131] <Chemical Formula 1>
[0132]
[0133] a= 0~100, b= 0~100, c= 0~100
[0134] When the above photopolymerization initiator (E) is a trimethylbenzoylphosphine oxide group-containing compound including a PO bond, the trimethylbenzoylphosphine oxide group-containing compound including a PO bond may include an alkoxy group.
[0135] For example, in the above chemical formula 1, a+b+c>0 may be true.
[0136] For example, a trimethylbenzoylphosphine oxide group-containing compound including the PO bond may include an ethoxy group.
[0137] A compound containing a trimethylbenzoylphosphine oxide group including the above PO bond can be represented by the following chemical formula 2.
[0138] <Chemical Formula 2>
[0139]
[0140] For example, the photopolymerization initiator (E) may further include one or more selected from the group consisting of benzoin and its alkyl ethers, acetophenones, anthraquinones, thioxanthones, ketals, benzophenones, α-aminoacetophenones, acylphosphine oxides, acylphosphinates, and oxime esters.
[0141] In the photosensitive resin composition of the present invention, the content of the photopolymerization initiator (E) may be 0.01 to 10 wt%, 0.01 to 7 wt%, or 0.01 to 5 wt% based on the total composition. By including the photopolymerization initiator (E) within this range, photocurability on copper is sufficient, so that the curability of the coating film is improved, and coating film properties such as chemical resistance are improved, and deep curability can also be improved.
[0142] In addition, when the content of the photopolymerization initiator (E) is within the above range, the undercut is not severe, the upper growth phenomenon (halation) is not large, so the resolution is excellent and a large number of solder resist openings can be formed. In addition, a high reflectivity can be maintained.
[0143] [(F) Silane coupling agent]
[0144] The photosensitive resin composition according to one embodiment of the present invention may further contain (F) a silane coupling agent. By containing (F) a silane coupling agent, the photosensitive resin composition can exhibit improved crack resistance, improved reflectivity compared to conventional compositions, and excellent gloss.
[0145] The (F) silane coupling agent of the present invention may have an organic group such as a vinyl group, a styryl group, an acrylic group, a methacryl group, an isocyanurate group, an acid anhydride group, a ureide group, an epoxy group, an amino group, a methacryloxy group, a mercapto group, an isocyanate group, or an isocyanurate group.
[0146] Examples of silane coupling agents having a vinyl group include vinyltrimethoxysilane and vinyltriethoxysilane. Examples of silane coupling agents having a styryl group include p-styrylmethoxysilane. Examples of silane coupling agents having a methacryl group include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, etc. Examples of silane coupling agents having an acrylic group include 3-acryloxypropyltrimethoxysilane, etc. Silane coupling agents having an amino group include N-2-(aminoethyl)-3-aminopropyl methyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyl triethoxysilane, 3-triethoxy-silyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyl trimethoxysilane, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane, etc. Silane coupling agents having a methacryloxy group include 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, etc. Silane coupling agents having a mercapto group include 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, etc. Examples of silane coupling agents having an isocyanate group include 3-isocyanate propyltriethoxysilane. Examples of silane coupling agents having an isocyanurate group include tris-(trimethoxysilylpropyl)isocyanurate. Examples of silane coupling agents having a ureide group include 3-ureidopropyltrialkoxysilane. Examples of silane coupling agents having an acid anhydride group include 3-(trimethoxysilyl)propylsuccinic anhydride.
[0147] The above silane coupling agent may be a silane coupling agent having an epoxy group, and may be, for example, 2-(3,4-epoxycyclohexyl) ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane, and the like, and may be, for example, 3-glycidoxypropyltriethoxysilane.
[0148] In the photosensitive resin composition of the present invention, the content of the (F) silane coupling agent may be 0.1 to 5 wt%, 0.3 to 3 wt%, or 0.4 to 2 wt% relative to the entire composition. The composition includes a solid content and a solvent.
[0149] (F) When the content of the silane coupling agent is within the above range, the composition may have excellent crack resistance, high reflectivity, excellent adhesion, and low tackiness, making it suitable for film formation.
[0150] (F) The silane coupling agent may be a commercially available product, and examples thereof include KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402 and KBE-403, KBM-1403, KBM-502, KBM-503, KBE-502, KBE-503, KBM5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103P, KBM-573, KBM-575, KBM-9659, KBM-585A, KBM-802, KBM-803, KBE-9007N, X-12-967C manufactured by Shin-Etsu Chemical Co., Ltd.
[0151] [(G) Resin having urethane bonds]
[0152] The photosensitive resin composition according to one embodiment of the present invention may further contain (G) a resin having a urethane bond. (G) The resin having a urethane bond may be a resin having excellent flexibility.
[0153] The photosensitive resin composition uses a resin having (G) urethane bonds, so that it can perform lamination work with a uniform thickness without breaking even on a flexible substrate or a thin-thickness sheet, and can have excellent resistance to cracking or breaking when subjected to external impact or when bent.
[0154] The resin having a (G) urethane bond of the present invention may include a modified urethane resin, and the resin having a urethane bond may be an ester type urethane, an ether type urethane, a modified urethane acrylate, a modified urethane epoxy, a silicone modified urethane, a fluorine-based modified urethane, etc., and may be, for example, a modified urethane epoxy acrylate containing an epoxy group.
[0155] As the resin having a (G) urethane bond of the present invention, a known compound having a urethane bond can be used. For example, a reaction product of an isocyanate compound (e.g., monoisocyanate, diisocyanate, polyisocyanate) and a compound having an OH group (e.g., polyhydric alcohols such as monohydric alcohols, polyester polyols, polyether polyols, epoxy (meth)acrylate), or a modified product thereof, may be mentioned.
[0156] The resin having a (G) urethane bond of the present invention may have a carboxyl group or an epoxy group, or a (meth)acryloyl group, and may be, for example, a carboxyl group-containing resin (1), an epoxy group-containing resin (2), a (meth)acryloyl group-containing resin (3), (4), (5), etc.
[0157] (1) A carboxyl group-containing photosensitive polyurethane resin obtained by a polyaddition reaction between a reaction product of a diisocyanate and a monocarboxylic acid compound having an ethylenically unsaturated double bond, such as a bifunctional epoxy resin (meth)acrylate, such as a biisocyanate and a bisphenol A type epoxy resin, a hydrogenated bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, a bixilenol epoxy resin, a phenol type epoxy resin, a partial anhydride thereof, or a modified product thereof, and a carboxyl group-containing dialcohol compound and a diol compound.
[0158] (2) A urethane-modified epoxy resin having a urethane bond and two or more epoxies in the molecule obtained by reacting a urethane bond-containing compound having an isocyanate group obtained by reacting a polyhydroxy compound and a polyisocyanate compound with an epoxy compound containing a hydroxy group.
[0159] (3) A urethane resin obtained by polyaddition reaction of a diisocyanate such as an aliphatic diisocyanate, a branched aliphatic diisocyanate, an alicyclic diisocyanate, an aromatic diisocyanate, and a diol compound such as a polycarbonate polyol, a polyether polyol, a polyester polyol, a polyolefin polyol, an acrylic polyol, an epoxy resin having a hydroxyl group (when this is used, a urethane resin having an epoxy group can be obtained), a bisphenol A-based alkylene oxide adduct diol, a compound having a phenolic hydroxyl group and an alcoholic hydroxyl group.
[0160] (4) A photosensitive polyurethane resin obtained by replacing part or all of the diisocyanate in the above (3) with a reaction product of isophorone diisocyanate and pentaerythritol triacrylate, and / or a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, and by a polyaddition reaction of such isocyanate and the diol compound.
[0161] (5) A terminal (meth)acrylated photosensitive polyurethane resin in which a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as hydroxyalkyl (meth)acrylate, is added during the synthesis of one of the resins (3) and (4) above.
[0162] Additionally, as described above, one resin may have at least two types of carboxyl groups, epoxy groups, or methacryloyl groups.
[0163] The resin having the above (G) urethane bond may be (1) among carboxyl group-containing resins, (2) among epoxy group-containing resins, and (5) among (meth)acryloyl group-containing resins.
[0164] The diisocyanate can be, for example, an aromatic polyisocyanate, an aliphatic polyisocyanate, or an alicyclic polyisocyanate. The aromatic polyisocyanates can be, for example, 4,4'-diphenylmethane diisocyanate, 2,4-diisocyanate-2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate-o-xylene diisocyanate, m-xylene diisocyanate, and 2,4-trilene dimer. The aliphatic polyisocyanates can be, for example, tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), and isophorone diisocyanate. The alicyclic polyisocyanate may be, for example, bicycloheptanetriisocyanate. The diisocyanate may be, for example, an aliphatic isocyanate.
[0165] (G) When the resin having a urethane bond is a carboxyl group-containing resin having a urethane bond, the acid value of the carboxyl group-containing resin may be 40 to 200 mgKOH / g, or 45 to 120 mgKOH / g. When the acid value of the carboxyl group-containing resin is in the range of 40 to 200 mgKOH / g, the adhesion of the cured film is obtained, and alkali development becomes easy, so dissolution of the exposed area by the developer is suppressed, so that the line does not become narrower than necessary, and a normal resist pattern can be easily drawn.
[0166] (G) When the resin having a urethane bond is a carboxyl group-containing resin having a urethane bond, the weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but may be 2,000 to 150,000 g / mol, 5,000 to 50,000 g / mol, or 2,000 to 50,000 g / mol. When the weight average molecular weight is within the above range, the tackiness is good, the moisture resistance of the cured film is good, and the occurrence of film reduction during development can be reduced. In addition, when the weight average molecular weight is within the above range, the resolution and developability are good, and the storage stability can be improved.
[0167] (G) Examples of commercially available products of resins having urethane bonds (e.g., carboxyl group-containing resins having urethane bonds) include UXE-3000 (Nippon Gunyaku Co., Ltd.), EPU-7N (urethane-modified epoxy resin; ADEKA Co., Ltd.), and Ebecryl 210 (aromatic urethane acrylate; Daicel Allnex Co., Ltd.).
[0168] In the photosensitive resin composition of the present invention, the content of the resin having (G) urethane bonds may be 0.1 to 15 wt%, 5 to 13 wt%, or 8 to 12 wt%, based on the total composition. The composition includes a solid content and a solvent. When the content of the resin having (G) urethane bonds is within the above range, the composition has excellent flexibility and crack resistance, and can exhibit appropriate tackiness, excellent printability, and excellent drying properties.
[0169] In the photosensitive resin composition of the present invention, the weight average molecular weight of the resin having (G) a urethane bond may be 2,000 to 150,000 g / mol, or may be 2,000 to 50,000 g / mol. When the weight average molecular weight of the resin having (G) a urethane bond is within the above range, excellent crack resistance and flexibility can be achieved.
[0170] [Other optional ingredients]
[0171] The photosensitive resin composition of the present invention may optionally contain various additives, as needed. Specifically, a thermosetting catalyst, a dispersant, an antioxidant, a colorant, an epoxy resin, an oxetane compound, a (meth)acrylic resin, various other additives, or a mixture of two or more thereof may be added. The optional components may contain one or more of the following materials.
[0172] Epoxy resin
[0173] The epoxy resin of the present invention may be a known, commonly used compound having one or more epoxy groups. For example, the epoxy resin may be one that does not overlap with the components (A) to (G) described above. For example, it may be a compound having two or more epoxy groups. For example, it may be a compound having two or more epoxy groups in one molecule, such as a monoepoxy compound such as butyl glycidyl ether, phenyl glycidyl ether, and glycidyl (meth)acrylate, bisphenol A type epoxy resin, bisphenol S type epoxy resin, bisphenol F type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, aliphatic ring epoxy resin, trimethylolpropane polyglycidyl ether, phenyl-1,3-diglycidyl ether, biphenyl-4,4'-diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ether of ethylene glycol or propylene glycol, sorbitol polyglycidyl ether, tris(2,3-epoxypropyl)isocyanurate, triglycidyltris(2-hydroxyethyl)isocyanurate. These can be used alone or in combination of two or more types to suit the required characteristics.
[0174] Examples of compounds having two or more epoxy groups include jER828, jER834, jER1001, jER1004 of Mitsubishi Chemical Co., Ltd., Epiclone 840, Epiclone 850, Epiclone 1050, Epiclone 2055 of DIC Co., Ltd., Epototo D-011, YD-013, YD127, YD-128 of Nittesu Chemical & Materials, DER317, DER331, DER661, DER664 of Dow Chemical Japan Co., Ltd., Sumiepoxy ESA-011, ESA-014, ELA-115, ELA128 of Sumitomo Chemical Co., Ltd., AER330, AER331, AER661, AER664 of Asahi Kasei Materials Co., Ltd. (all Bisphenol A type epoxy resin (trade name); jERYL903 of Mitsubishi Chemical Co., Ltd., Epichron 152, Epichron 165 of DIC Co., Ltd., Epototo YDE-400, YDE-500 of Nittesu Chemical & Materials Co., Ltd., DER542 of Dow Chemical Japan Co., Ltd., Sumiepokishi ESB-400, ESB-700 of Sumitomo Chemical Co., Ltd., AER711, AER714 of Asahi Kasei Materials Co., Ltd., etc. (all trade names); Mitsubishi Chemical Corporation's jER152, jER154, Dow Chemical Japan Co., Ltd.'s DEN431, DEN438, DIC Corporation's Epichron N-730, Epichron N-770, Epichron N-865, Nippon Chemical & Materials Co., Ltd.'s Epototo YDC-701, YDC-704, Nippon Chemical Co., Ltd.'s EPPN-201, EPPN-1025, EPPN-1020, EPPN-104S, RE-306, NC-3000, Sumitomo Chemical Co., Ltd.'s Sumiepoxy ESCN-195X, ESCN-220, Asahi Kasei Materials Co., Ltd.Noflak type epoxy resins such as ECN-235, ECN-299, YDCN-700-2, YDCN-700-3, YDCN-700-5, YDCN-700-7, YDCN-700-10, YDCN-704, YDCN-704A of Nittesu Chemical & Materials Co., Ltd., and Epichron N-680, N-690, N-695 of DIC Co., Ltd. (all trade names); Bisphenol F type epoxy resins such as Epichron 830 of DIC Co., Ltd., jER807 of Mitsubishi Chemical Co., Ltd., and Epitoto YDF-175, YDF-2004 of Nittesu Chemical & Materials Co., Ltd. (all trade names); Hydrogenated bisphenol A type epoxy resins such as Epototo ST-2004, ST-2007, and ST-3000 (trade names) of Nittesu Chemical & Materials Co., Ltd.; Glycidylamine type epoxy resins such as JER 604 of Mitsubishi Chemical Co., Ltd., Epototo YH-434 of Nittesu Chemical & Materials Co., Ltd., and Sumi Epoxy ELM-120 of Sumitomo Chemical Co., Ltd. (all trade names); Hydantoin type epoxy resins; Alicyclic epoxy resins such as Celoxide 2021 of Daicel Co., Ltd. (all trade names); YL-933 of Mitsubishi Chemical Co., Ltd., and TEN of Dow Chemical Japan Co., Ltd., EPPN-501, EPPN-502, etc. (all trade names); Bixilenol type or biphenol type epoxy resins or mixtures thereof, such as YL-6056, YX-4000, YL-6121 (all trade names) of Mitsubishi Chemical Co., Ltd.; Bisphenol S type epoxy resins, such as EBPS-200 of Nippon Kayaku Co., Ltd., EPX-30 of ADEKA Co., Ltd., EXA-1514 (trade names) of DIC Co., Ltd.; Bisphenol A novolac type epoxy resins, such as jER 157S (trade name) of Mitsubishi Chemical Co., Ltd.; Tetraphenylolethane type epoxy resins, such as jER YL-931 of Mitsubishi Chemical Co., Ltd. (all trade names); Heterocyclic epoxy resins, such as TEPIC of Nissan Chemical Industries, Ltd. (all trade names); Diglycidyl phthalate resins such as Brenmer DGT of Nichiyu Co., Ltd.; tetraglycyrrhizyl xylenol ethane resins such as ZX-1063 of Nittetsu Chemical & Materials Co., Ltd.; naphthalene group-containing epoxy resins such as ESN-190 and ESN-360 of Nittetsu Chemical & Materials Co., Ltd., and HP-4032, EXA-4750, and EXA-4700 of DIC Co., Ltd.; epoxy resins having a dicyclopentadiene skeleton such as HP-7200 and HP-7200H of DIC Co., Ltd.; glycidyl methacrylate copolymerization epoxy resins such as CP-50S and CP-50M of Nichiyu Co., Ltd.; and copolymerization epoxy resins of cyclohexylmaleimide and glycidyl methacrylate. Examples include, but are not limited to, CTBN-modified epoxy resins (e.g., YR-102 and YR-450 from Nittsu Chemical & Materials Co., Ltd.). Among these, for example, bisphenol A-type epoxy resins, heterocyclic epoxy resins, or mixtures thereof may be used, as they have superior discoloration resistance. These epoxy resins may be used singly, or two or more may be used in combination.
[0175] In the photosensitive resin composition of the present invention, the epoxy resin may be a bisphenol-based epoxy resin, for example, an epoxy resin having two or more epoxy groups in the bisphenol-based epoxy series. The blending amount of the bisphenol-based epoxy resin having two or more epoxy groups used in the present invention may be 1 to 15 wt%, may be in the range of 1 to 10 wt%, or may be in the range of 3 to 10 wt%, based on the total composition. The composition includes a solid content and a solvent.
[0176] When the content of the epoxy resin is within the above range, the coating film formed by the composition has excellent adhesion, heat resistance, and pencil hardness, is well cured, and the problems of yellowing and difficulty in implementing high reflectivity after processing can be solved.
[0177] In the photosensitive resin composition of the present invention, the weight average molecular weight of the epoxy resin may be 150 to 100,000 g / mol.
[0178] Oxetane compound
[0179] Next, we will explain oxetane compounds. General formula (I) below:
[0180]
[0181] (In the formula R 1Specific examples of oxetane compounds containing an oxetane ring represented by (wherein represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms) include 3-ethyl-3-hydroxymethyloxetane (Dong-A Synthetic Co., Ltd., trade name OXT-101), 3-ethyl-3-(phenoxymethyl)oxetane (Dong-A Synthetic Co., Ltd., trade name OXT-211), 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane (Dong-A Synthetic Co., Ltd., trade name OXT-212), 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene (Dong-A Synthetic Co., Ltd., trade name OXT-121), bis(3-ethyl-3-oxetanylmethyl)ether (Dong-A Synthetic Co., Ltd., trade name OXT-221), etc. In addition, phenol novolak type oxetane compounds, etc. are also included. These oxetane compounds may be used in combination with the above epoxy compounds or may be used alone.
[0182] <(Meta)Acrylic Resin>
[0183] (Meth)acrylic resin is a photocurable resin. The photocurable resin is not particularly limited as long as it is a resin that exhibits electrical insulation properties by being cured by irradiation with active energy rays. For example, it may be a compound having one or more ethylenically unsaturated bonds in its molecule. For example, the (meth)acrylic resin may not overlap with the components (A) to (G) described above.
[0184] The compound having the above-mentioned ethylenically unsaturated bond may be a known photopolymerizable oligomer, photopolymerizable monomer, photopolymerizable vinyl monomer, etc. The photopolymerizable oligomer may be an unsaturated polyester oligomer, a (meth)acrylate oligomer, etc. The (meth)acrylate oligomer may be an epoxy (meth)acrylate such as phenol novolac epoxy (meth)acrylate, cresol novolac epoxy (meth)acrylate, bisphenol type epoxy (meth)acrylate, urethane (meth)acrylate, epoxy urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, polybutadiene modified (meth)acrylate, etc.
[0185] Photopolymerizable monomers or photopolymerizable vinyl monomers include those known in the art, for example, styrene derivatives such as styrene, chlorostyrene, and α-methylstyrene; vinyl esters such as vinyl acetate, vinyl butyrate, and vinyl benzoate; ethers such as vinyl isobutyl ether, vinyl-n-butyl ether, vinyl-t-butyl ether, vinyl-n-amyl ether, vinyl isoamyl ether, vinyl-n-octadecyl ether, vinylcyclohexyl ether, ethylene glycol monobutyl ether, and triethylene glycol monomethyl ether; (meth)acrylamides such as acrylamide, methacrylamide, N-hydroxymethylacrylamide, N-hydroxymethylmethacrylamide, N-methoxymethylacrylamide, N-ethoxymethyl acrylamide, and N-butoxymethylacrylamide; Aryl compounds such as triallyl isocyanurate, diaryl phthalate, and diaryl isophthalate; (meth)acrylic acid esters such as 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and pentaerythritol tri(meth)acrylate; alkoxyalkylene glycol mono(meth)acrylates such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; Alkylene polyol poly(meth)acrylates such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; polyoxyalkylene glycol poly(meth)acrylates such as diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, ethoxylated trimethylolpropane triacrylate, and propoxylated trimethylolpropane tri(meth)acrylate; poly(meth)acrylates such as hydroxypivalic acid neopentyl glycol ester di(meth)acrylate;Examples include isonalate-type poly(meth)acrylates such as tris[(meth)acryloxyethyl]isocyanurate, and these can be used alone or in combination of two or more.;
[0186] In the photosensitive resin composition of the present invention, the (meth)acrylic resin may be an unsaturated polyester oligomer, a (meth)acrylate oligomer, or the like, and may be, for example, a 6-functional flexible acrylic oligomer. The blending amount of the (meth)acrylic resin may be 1 to 15 wt%, 1 to 10 wt%, or 5 to 10 wt% based on the total composition. The composition includes a solid content and a solvent. When the content of the (meth)acrylic resin is within the above range, the resolution and undercut are excellent, and the coating film can be cured to an appropriate level.
[0187] <Thermocuring catalyst>
[0188] In the composition of the present invention, at least one curing agent or curing catalyst may be further added as a thermosetting catalyst. For example, the thermosetting catalyst may not overlap with the components (A) to (G) described above.
[0189] The curing agent can be, for example, a polyfunctional phenol compound, a polycarboxylic acid and anhydride thereof, an aliphatic or aromatic primary or secondary amine, a polyamide resin, an isocyanate compound, a polymercapto compound, etc. The curing agent can be, for example, a polyfunctional phenol compound, a polycarboxylic acid and anhydride thereof, and excellent workability and insulation can be obtained by using such a curing agent. The polyfunctional phenol compound is not particularly limited as long as it is a compound having two or more phenolic hydroxyl groups in one molecule, and can be, for example, a known or commonly used one. For example, the polyfunctional phenol compound can be a phenol novolac resin, a cresol novolac resin, bisphenol A, allylated bisphenol A, bisphenol F, a novolac resin of bisphenol A, or a vinylphenol copolymer resin. The polyfunctional phenol compound can be, for example, bisphenol A, thereby providing high reactivity and enhancing heat resistance. A polyfunctional phenol compound can undergo an addition reaction with at least one of an epoxy compound or an oxytane compound in the presence of a suitable curing catalyst. The polycarboxylic acid and its acid anhydride can be, for example, a compound having two or more carboxyl groups in one molecule and its acid anhydride, and can be, for example, a copolymer of (meth)acrylic acid, a copolymer of maleic anhydride, a condensate of a dibasic acid, etc. Commercially available products include Joncryl (product group name) from BASF, SMA Resin (product group name) from Satoma, and polyazelaic anhydride from Shin Nippon Rika.
[0190] In addition, the curing catalyst may be a compound that can act as a curing catalyst in the reaction between a thermosetting resin such as an epoxy compound or an oxetane compound and a curing agent, or a compound that acts as a polymerization catalyst when a curing agent is not used. Specifically, the curing catalyst may be, for example, a tertiary amine, a tertiary amine salt, a quaternary ammonium salt, a tertiary phosphine, a crown ether compound, or a phosphonium ylide, and any of these may be used singly or in combination of two or more.
[0191] For example, imidazoles such as 2E4MZ, C11Z, C17Z, 2PZ with the trade names, imidazole AZINE compounds such as 2MZ-A, 2E4MZ-A with the trade names, isocyanurates of imidazoles such as 2MZ-OK, 2PZ-OK with the trade names, imidazole hydroxymethyl compounds such as 2PHZ, 2P4MHZ with the trade names (trade name; Shikoku Kasei Industry Co., Ltd.), dicyandiamide and its derivatives, melamine and its derivatives, diaminomaleonitrile and its derivatives, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, bis(hexamethylene)triamine, triethanolamine, diaminodiphenylmethane with the trade names, 1,8-diazabicyclo[5,4,0]undecene-7 (trade name DBU, San-Apro Co., Ltd.), It may be an organic phosphine compound such as 3.9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5,5]undecane (trade name ATU, Ajinomoto Co., Ltd.) or triphenylphosphine, tricyclohexylphosphine, tributylphosphine, or methyldiphenylphosphine.
[0192] In the photosensitive resin composition of the present invention, the curing catalyst may be an amine-based, phosphine-based, or imidazole-based curing catalyst, and for example, may be a melamine-based amine curing catalyst. The blending amount of the curing catalyst may be 0.1 to 10 wt%, 0.1 to 5 wt%, or 0.1 to 3 wt% relative to the entire composition.
[0193] When the content of the above curing catalyst is within the above range, the coating film is sufficiently cured, so that the adhesion, pencil hardness, and heat resistance are excellent, and the curing time is appropriately maintained, and the deterioration of the developability can be prevented.
[0194] Antioxidant
[0195] The photosensitive resin composition of the present invention may also contain an antioxidant. By containing an antioxidant, not only can the effect of suppressing discoloration by preventing oxidative deterioration of the curable resin, etc. be obtained, but also the effect of improving heat resistance and improving resolution (line width reproducibility) can be obtained. In other words, depending on the type of white colorant, there are cases where resolution is deteriorated by reflecting and absorbing light, but by containing an antioxidant, good resolution can be obtained regardless of the type of white colorant. The antioxidant may be a radical scavenger that neutralizes generated radicals, or a peroxide decomposition inhibitor that decomposes generated peroxides into harmless substances and prevents the generation of new radicals, and may be used alone or in combination of two or more.
[0196] Antioxidants that act as radical scavengers include, for example, phenolic compounds such as hydroquinone, 4-t-butylcatechol, 2-t-butylhydroquinone, hydroquinone monomethyl ether, 2,6-di-t-butyl-p-cresol, 2,2-methylene-bis(4-methyl-6-t-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3',5'-di-t-butyl-4-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione, and quinone compounds such as menaquinone and benzoquinone. It can be an amine compound such as a compound, bis(2,2,6,6-tetramethyl-4-piperidyl)-sebacate, phenothiazine, etc. As a commercially available product, for example, IRGANOX1010 (product name of BASF Japan Co., Ltd.) can be used.
[0197] In addition, antioxidants that act as peroxide decomposers include, for example, phosphorus compounds such as triphenyl phosphite, sulfur compounds such as pentaerythritol tetralauryl thiopropionate, dilauryl thiodipropionate, and distearyl-3,3'-thiodipropionate.
[0198] For example, the antioxidant may be a phenolic compound, and its use can produce an anti-discoloration effect, improved heat resistance, and better resolution.
[0199] Additionally, antioxidants, such as phenolic antioxidants, can be used in combination with heat stabilizers. When used in combination, they can exhibit even better effects.
[0200] The heat-resistant stabilizer may be, for example, a phosphorus-based, hydroxylamine-based, or sulfur-based heat-resistant stabilizer. The heat-resistant stabilizer may be used alone or in combination of two or more types.
[0201] For example, the antioxidant may be a hydroxylamine-based antioxidant, a sulfur-based antioxidant, or a phenol-based antioxidant. When a phenol-based antioxidant is used, the blending amount may be 0.01 to 5 wt%, or 0.03 to 3 wt%, based on the total composition. By setting the blending amount of the antioxidant to 0.01 to 1 wt% or more, the effect of adding the antioxidant can be reliably obtained, and when it is 1 wt% or less, a good alkaline development can be obtained without inhibiting the photoreaction, and the touch-drying property and the coating film properties can also be well secured.
[0202] Organic solvents
[0203] The photosensitive resin composition of the present invention may contain an organic solvent for purposes such as preparing the composition or adjusting viscosity when applying it to a substrate or base material. Examples of the organic solvent include known and commonly used organic solvents such as esters; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. These organic solvents may be used alone or in combination of two or more.
[0204] Other additives
[0205] In addition, the photosensitive resin composition of the present invention may contain other commonly known additives in the field of electronic materials. Examples of the other additives include thermal polymerization inhibitors, ultraviolet absorbers, plasticizers, flame retardants, antistatic agents, anti-aging agents, antibacterial and antifungal agents, antifoaming agents, leveling agents, thickeners, adhesion-imparting agents, thixotropic agents, photoinitiation aids, sensitizers, curing accelerators, release agents, surface treatment agents, dispersants, dispersing aids, surface modifiers, stabilizers, and the like.
[0206] The photosensitive resin composition of the present invention may have a phosphorus content of 500 to 5000 ppm.
[0207] When the phosphorus content of the photosensitive resin composition is 500 ppm or more, surface hardening can be improved and gold plating resistance and adhesion can be strengthened. When the phosphorus content is 5000 ppm or less, the reaction rate of the silicone sealant can be increased.
[0208] When the phosphorus content is less than 500 ppm, the pencil hardness may be 3H, adhesion after gold plating may be poor, gloss may be low, and solder resist aperture (SRO) formation may not be successful. On the other hand, when the phosphorus content exceeds 5,000 ppm, the reactivity of the silicone encapsulant may be very low, developability and reflectivity may be reduced, and SRO formation may also become difficult.
[0209] [Dry film and its manufacturing method]
[0210] Another embodiment of the present invention relates to a dry film having a photosensitive resin layer formed by applying and drying a photosensitive resin composition on a first film.
[0211] When forming a dry film, first, the composition of the present invention is diluted with an organic solvent to adjust the viscosity to an appropriate level, and then applied to a first film with a uniform thickness, for example, in the range of 40 to 60 μm, using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, micro gravure coater, spray coater, or the like. Thereafter, the applied composition is dried at a temperature typically in the range of 40 to 120°C for 1 to 30 minutes to form a photosensitive resin layer, thereby forming a dry film.
[0212] There is no particular limitation on the thickness of the coating film, but generally, the thickness after drying may be 10 to 150 ㎛, 10 to 80 ㎛, or 10 to 60 ㎛.
[0213] As the first film, a plastic film is used, and for example, a polyester film such as polyethylene terephthalate (PET), a polyimide film, a polyamide-imide film, a polypropylene film, a polystyrene film, etc. can be used, and for example, it can be polyethylene terephthalate. There is no particular limitation on the thickness of the first film, but it can generally be appropriately selected within the range of 10 to 150 ㎛. In addition, it can be applied to a metal foil such as a copper foil or an aluminum foil. In addition, the first film used can be subjected to a peeling treatment such as acrylic or silicone.
[0214] Since the dry film of the present invention is white, it can be used to reflect light generated from light-emitting diodes (LEDs) or electroluminescent (EL) used as light sources in backlights of liquid crystal displays of lighting devices, mobile terminals, notebook computers, tablet PCs, monitors, smartphones, personal computers, televisions, etc. The dry film of the present invention can be applied to LEDs and light-emitting PCBs, etc.
[0215] To create a cured film on a printed wiring board using a dry film, a second film, intended for the purpose of protecting the dry film, is peeled off, the exposed resin layer of the dry film is superimposed on the circuit-formed substrate and attached using a laminator or the like, thereby forming a resin layer on the circuit-formed substrate. The formed resin layer is then exposed, developed, heated, and then cured to form a cured film. The second film can be peeled off at any stage, either before or after exposure.
[0216] [Curing agent and its manufacturing method]
[0217] The cured product of the present invention can be formed by curing the photosensitive resin composition of the present invention or the solder resist layer of the dry film of the present invention.
[0218] The cured product of the present invention can be suitably used in printed wiring boards, electronic components, and the like. The cured product of the present invention can exhibit excellent dielectric properties, including high crack resistance, high resolution, and low dielectric constant and low dielectric loss tangent. In addition, the cured product of the present invention can exhibit excellent heat resistance and coefficient of linear expansion.
[0219] For example, the cured product of the present invention may be a solder resist.
[0220] The above solder resist can be manufactured by forming a pattern by applying the photosensitive resin composition of the present invention on a substrate to form a photosensitive resin layer, selectively exposing the photosensitive resin layer to an active energy ray through a photomask having a predetermined pattern formed thereon, and developing the unexposed portion with a dilute alkaline aqueous solution (e.g., 0.3 to 3 wt% sodium carbonate aqueous solution). Alternatively, in the case of a dry film, after exposure, the first film of the dry film is peeled off and then developed, thereby forming a patterned solder resist on the substrate. Additionally, as long as the properties are not impaired, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed.
[0221] [Printed wiring board and manufacturing method thereof]
[0222] The printed wiring board of the present invention may include a cured film formed by curing a cured product of the photosensitive resin composition of the present invention or a photosensitive resin layer of the dry film of the present invention.
[0223] The printed wiring board of the present invention may include a cured product obtained from the photosensitive resin composition of the present invention or the photosensitive resin layer of the dry film. The method for manufacturing the printed wiring board of the present invention includes, for example, adjusting the viscosity of the photosensitive resin composition of the present invention to a viscosity suitable for the coating method using the organic solvent, coating the composition on a substrate by a dip coating method, a flow coating method, a roll coating method, a bar coater method, a screen printing method, a curtain coating method, or the like, and then drying (temporarily drying) the organic solvent included in the composition at a temperature of 60 to 100°C to volatilize it, thereby forming a tacky-free resin layer. In addition, in the case of a dry film, the resin layer may be bonded to the substrate by a laminator or the like so that it comes into contact with the substrate, and then the first film may be removed to form a resin layer on the substrate.
[0224] The above-mentioned substrates include not only printed wiring boards and flexible printed wiring boards formed with copper or the like, but also copper-clad laminates for high-frequency circuits using materials such as paper phenol, paper epoxy, glass fiber epoxy, glass polyimide, glass fiber / epoxy, glass fiber / paper epoxy, synthetic fiber epoxy, fluororesin, polyethylene, polyphenylene ether, and polyphenylene oxide cyanate, and examples thereof include FR-4 substrates, copper-clad laminates of all grades (FR-4, etc.), other metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, and wafer substrates.
[0225] A method of laminating a dry film on a substrate can be performed by applying pressure and heating using a vacuum laminator or the like. By using such a vacuum laminator, even if the circuit board surface is uneven when a circuit-formed substrate is used, the dry film adheres closely to the circuit board, preventing the inclusion of air bubbles and improving the relief of undulating areas on the substrate surface. The pressure conditions can be approximately 0.1 to 2.0 MPa, and the temperature conditions can be 40 to 120°C.
[0226] In addition, a cured film having excellent properties such as adhesion and hardness can be formed by i) irradiating the cured product with an active energy ray and then heat-curing (e.g., 100 to 220°C), ii) irradiating the cured product with an active energy ray after heat-curing, iii) only irradiating the cured product with an active energy ray, or iv) final curing only by heat-curing.
[0227] The cured product of the present invention can form a cured film having excellent properties such as high reflectivity, excellent yellowing resistance, and excellent crack resistance by curing it by heating it at a temperature of, for example, 100 to 220°C.
[0228] The exposure device used for the above active energy ray irradiation may be a device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, etc., and may irradiate ultraviolet (UV) rays in the range of 350 to 450 nm, and may also be a direct drawing device (e.g., a laser direct imaging device that directly draws CAD data on a computer with a laser). The maximum wavelength of the direct drawing device lamp light source or laser light source may be in the range of 350 to 450 nm. The exposure for image formation varies depending on the thickness, etc., but is generally 10 to 1000 mJ / cm. 2 It can be 20~800mJ / cm 2 It could be.
[0229] The above-mentioned developing method may be a dipping method, a shower method, a spray method, a brush method, etc., and an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, or amines may be used as the developing solution.
[0230] The printed wiring board of the present invention may include a dry film including one or more layers formed from the photosensitive resin composition.
[0231] When forming a printed wiring board, a dry film can be placed on a test substrate and vacuum lamination can be performed to transfer the dry film onto the test substrate.
[0232] Thereafter, the first film is peeled off, and the substrate to which the dry film from which the first film is peeled is transferred can be exposed to UV light using an exposure device. When exposed in this manner, the exposed portion (the portion irradiated with light) can be cured. After exposure, the substrate is cooled to room temperature, then placed in a developer to develop the unexposed portion with an alkaline aqueous solution, so that the formation of the resist pattern can be completed. The substrate on which the pattern is formed through development can be finally cured (post-cured) in an oven at 150°C for 1 hour, thereby completing the production of the substrate. After the final curing, a reflow process is performed, followed by a chip mounting process. Thereafter, a process of producing a silicone encapsulant on the cured product of the photosensitive resin layer is performed, and an encapsulation process is performed. The photosensitive resin composition of the present invention can improve the problems of yellowing and non-curing of the silicone encapsulant formed on the cured product by reducing the outgassing of the photopolymerization initiator, and can improve the reaction rate of the silicone encapsulant.
[0233] The method for manufacturing a printed wiring board including the cured product of the present invention can peel off the first film after, for example, performing an exposure operation after a lamination process.
[0234] [Silicone encapsulating layer and its manufacturing method]
[0235] The printed wiring board of the present invention may further include a silicone encapsulating layer disposed on the cured product (obtained by curing the photosensitive resin layer). The silicone encapsulating layer may be formed by coating a composition containing silicone to encapsulate and protect the printed wiring board or the solder resist layer.
[0236] In order to protect the light-emitting chip portion and the photosensitive resin layer (or the cured product obtained by curing the same), coating of the silicone encapsulating layer described above can be performed.
[0237] The following describes an exemplary method for manufacturing a silicone encapsulating layer.
[0238] After creating a dam measuring 2.0 cm in width and 2.0 cm in height and 250 to 300 μm in thickness on a printed circuit board that has completed final curing or reflow, a 1:1 mixture of any silicone encapsulant A and B is added and a silicone encapsulant with a thickness of 250 to 300 μm is applied. After that, curing is performed in a 100°C oven for 2 hours to complete the primary curing, and curing is performed in a 150°C oven for 4 hours to complete the secondary curing of the silicone encapsulant, thereby creating a silicone encapsulant layer.
[0239] To measure the properties of the silicone encapsulant layer, after curing is complete, the silicone encapsulant layer can be peeled off and the reaction rate of the silicone encapsulant and the amount of photopolymerization initiator remaining within the silicone encapsulant layer can be analyzed. Furthermore, the degree of curing (reaction rate) of the silicone encapsulant can be measured to determine the extent of curing. Furthermore, the reflectivity of the silicone encapsulant layer can be measured.
[0240] For example, the silicone encapsulant layer may include a lower encapsulant region, which is a region close to the solder resist layer, and an upper encapsulant region, which is a region far from the solder resist layer.
[0241] For example, the content of the (E) photopolymerization initiator included in the upper encapsulating material region or the lower encapsulating material region may be 1,000 ppm or less, for example, 900 ppm or less, 800 ppm or less, 700 ppm or less, 600 ppm or less, or 500 ppm or less, relative to the content of the (E) photopolymerization initiator included in the solder resist layer.
[0242] The content of the photopolymerization initiator included in the upper encapsulating material region or the lower encapsulating material region is the photopolymerization initiator included in the solder resist layer that has been transferred. That is, by using the trimethylbenzoylphosphine oxide-based compound including at least one PO bond, which is the (E) photopolymerization initiator of the present invention, the content of the photopolymerization initiator transferred to the nearby upper encapsulating material region or the lower encapsulating material region can be reduced.
[0243] For example, if transfer occurs due to outgas diffusion of a photopolymerization initiator in a silicone encapsulating layer, there is a problem in that the silicone encapsulating material is not cured due to the inhibition reaction between the phosphorus (P) component of the photopolymerization initiator and the catalyst component (e.g., a platinum catalyst) of the silicone encapsulating material layer, thereby reducing the reaction rate of the silicone encapsulating material. There is a possibility that problems may arise in long-term reliability due to the reduced reaction rate of the silicone encapsulating material.
[0244] [Protective Film]
[0245] The laminate of the present invention may include the cured material and the protective film.
[0246] In the present invention, a protective film can be attached after the photosensitive resin layer is finally cured to form a cured product in order to remove the photopolymerization initiator. When the protective film is attached, the photopolymerization initiator remaining in the solder resist layer can be efficiently removed because the protective film has a high affinity for the photopolymerization initiator. By removing this remaining photopolymerization initiator, the content of the photopolymerization initiator remaining after the reflow and baking processes can be reduced. Due to this reduced content of the photopolymerization initiator, when the silicone encapsulant is coated on the cured product layer, the reaction rate of the silicone encapsulant increases, and due to this increased reaction rate, long-term reliability can be significantly improved.
[0247] As the protective film, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc. can be used. The thickness of the protective film is not particularly limited, but may be, for example, 10 to 150 μm.
[0248] For example, the content of the (E) photopolymerization initiator included in the above protective film may be 1000 ppm or less with respect to the content of the (E) photopolymerization initiator included in the solder resist layer.
[0249] The content of the photopolymerization initiator included in the above protective film is the photopolymerization initiator included in the solder resist layer that has been transferred. That is, by using a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond, which is the (E) photopolymerization initiator of the present invention, the content of the photopolymerization initiator transferred to the adjacent protective film can be reduced.
[0250] <Example>
[0251] Hereinafter, the present invention will be described in detail using examples. The present invention is not limited to the following examples.
[0252] <Synthesis Example 1 (Alkali-soluble resin A, copolymer resin)>
[0253] In a flask equipped with a thermometer, a stirrer, a dropping funnel, and a reflux condenser, 325.0 parts by weight of dipropylene glycol monomethyl ether as a solvent was heated to 110°C, and a mixture of 174.0 parts by weight of methacrylic acid, 174.0 parts by weight of ε-caprolactone-modified methacrylic acid (average molecular weight 314), 77.0 parts by weight of methyl methacrylate, 222.0 parts by weight of dipropylene glycol monomethyl ether, and 12.0 parts by weight of t-butylperoxy-2-ethylhexanoate (Perbutyl-O from Nichiyu Co., Ltd.) as a polymerization catalyst was added dropwise over 3 hours, stirred at 110°C for 3 hours, and then the polymerization catalyst was deactivated to obtain a resin solution. After cooling this resin solution, 289.0 parts by weight of Daicel's Cyclomer M100, 3.0 parts by weight of triphenylphosphine, and 1.3 parts by weight of hydroquinone monomethyl ether were added, the temperature was raised to 100°C, and stirring was performed to perform a ring-opening addition reaction of the epoxy group ring, thereby obtaining resin solution A. The solid content of the obtained resin solution A was 54.5 wt%, and the acid value of the solid content was 79.8 mgKOH / g.
[0254] <Synthesis Example 2, D Resin Solution>
[0255] 200 parts by weight of deionized water and 0.3 parts by weight of sodium sulfate were injected into a pressure vessel equipped with a thermometer, a cooling tube, and a stirrer, and their dissolution was confirmed. Thereafter, 5 parts by weight of BPO (benzoyl peroxide) as a polymerization initiator and 5 parts by weight of MSD (α-methylstyrene dimer) as a chain transfer agent were added to a monomer mixture consisting of 10.4 parts by weight of MMA (methyl methacrylate), 5 parts by weight of n-BA (n-butylacrylate), 24.6 parts by weight of MAA (methacrylic acid), and 60 parts by weight of Stylene (styrene), and sufficiently dissolved. Thereafter, a dispersant was added to a concentration of 300 ppm, and the mixture was sufficiently stirred. The inside of the kiln was replaced with nitrogen, and the temperature was raised to perform suspension polymerization. After completion of polymerization, the obtained suspension was filtered through a 30 μm mesh and dried with warm air at 40°C to obtain a resin in the form of particles. The granular resin (copolymer resin) thus obtained was sufficiently dissolved using an organic solvent DPM (dipropylene glycol methyl ether) to a solid concentration of 50 wt%, which is referred to as resin solution D. The solid acid value was 160 mgKOH / g.
[0256] <Synthesis Example 3, Carboxyl Group-Containing Cresol Novolac-Type Epoxy Acrylate Resin A-2>
[0257] 220 parts by mass of cresol novolac epoxy resin was placed in a four-necked flask equipped with a stirrer and a reflux condenser, 214 parts by mass of carbitol acetate was added, and the mixture was heated to dissolve. Next, 0.1 parts by mass of hydroquinone as a polymerization inhibitor and 2.0 parts by mass of dimethylbenzylamine as a reaction catalyst were added to prepare a mixture. The mixture was heated to 95-105°C, 72 parts by mass of acrylic acid was slowly added dropwise, and the mixture was reacted for 16 hours. The reaction product was cooled to 80-90°C, 106 parts by mass of tetrahydrophthalic anhydride was added, and the mixture was reacted for 8 hours, cooled, and then taken out.
[0258] The photosensitive resin having both ethylenically unsaturated bonds and carboxyl groups thus obtained had a non-volatile content of 64%, an acid value of 84.4 mg KOH / g of solids, and a weight-average molecular weight Mw of approximately 7,500. Hereinafter, this resin is referred to as (A-2). In addition, the weight-average molecular weight of the obtained resin was measured by GPC.
[0259] Preparation of photosensitive resin composition
[0260]
[0261]
[0262]
[0263]
[0264] Preparation of dry film of photosensitive resin composition
[0265] In a dust-free room, a comma coater was used to coat (1) a first film (PET film) (XD-500P manufactured by Toray Industries, Inc., film thickness: 25 μm) with a uniform thickness (50 μm) of the compositions of each example and comparative example. (2) The coated compositions were dried in four temperature chambers (Chamber 1: 60 °C, Chamber 2: 80 °C, Chamber 3: 100 °C, Chamber 4: 100 °C) in the range of 40 to 120 °C. (3) The appropriately dried coating film on the first film was laminated with a second film (Poly Propylene, PP film) to manufacture a dry film. At this time, the thickness of the dried coating film was set to be in the range of 60 μm.
[0266] Evaluation Example 1: Measurement of outgassing, silicone sealant reaction rate, and photopolymerization initiator content
[0267] 1. Measurement of outgas content
[0268] A photosensitive resin composition according to an example or comparative example was laminated on a PET film using a vacuum laminator (CVP-300: manufactured by Nichiko Moulton Co., Ltd.) in a first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds to produce a dry film, and the PET film was peeled off.
[0269] Using a DI exposure device manufactured by Screen, a Kodak Step Tablet N0.2 (41-stage) photomask was used to perform full-face exposure at 23 stages to obtain 300 mJ / cm2 as measured by an integrated irradiance meter. Subsequently, development was performed for 60 seconds with a 1.0% Na2CO3 aqueous solution at 30°C and a spray pressure of 0.2 MPa. Thereafter, the photosensitive resin layer was cured for 60 minutes in an oven at 150°C to obtain a cured product.
[0270] A powder sample was collected from the fabricated resist layer and placed in a thermal desorption unit (TDU) manufactured by GURSTEL. Specifically, the powder sample was heated at a rate of 30°C to 60°C / min using helium as a purge gas (50 ml / min), heated at 150°C for 60 minutes, and desorbed and collected at -50°C. The collected outgas components were separated and analyzed using a gas chromatography mass spectrometer (8890 / 5977B) manufactured by Agilent Technologies, quantified in n-dodecane conversion, and then the weight % was measured based on the weight of the photopolymerization initiator contained in the cured product of the photosensitive resin layer.
[0271] The measurement conditions for gas chromatography are as follows. Column: Agilent Technologies capillary column DB-1MS (length 30 m, inner diameter 0.25 mm, thickness 0.25 μm), detector: MS (ITQ900), carrier gas: helium, injector temperature: 300°C, detector temperature: 230°C, column temperature conditions: initial temperature 50°C, hold at 50°C for 2 minutes after sample injection, then increase to 300°C at 12°C / sec, hold for 10 minutes after reaching 300°C.
[0272] In addition, separately from this, as described later, a silicone encapsulant was formed on a substrate (a dry film of a photosensitive resin composition was laminated on an FR-4 Cu film and then PET was peeled off), and then cured by heating at 100°C for 2 hours and then heating at 150°C for 4 hours.
[0273] The outgas content, silicone reaction rate, and the content of photopolymerization initiator transferred to the silicone encapsulant and protective film for each example and comparative example were measured and are shown in Table 2 below. Each measurement method is described below.
[0274] [Method for measuring outgas content]
[0275] The peak of the photopolymerization initiator was identified by analyzing TD-GCMS. At this time, the unit of the peak is expressed as μg / g, which means how many μg of gas is generated per 1 g of sample when converted to n-dodecane, and the sum of the outgassing of the photopolymerization initiator peak was measured. At this time, the peak area ratio of the photopolymerization initiator to the area of n-dodacane, which is the REF of GC-MS, was calculated (calculation formula below).
[0276] Calculation formula: Area of the analysis peak of the photopolymerization initiator / Area of the measurement peak of n-dodecane
[0277] 2. Measurement of the reaction rate and photopolymerization initiator content of silicone encapsulating materials
[0278] [Calculation of the reaction rate and photopolymerization initiator content of silicone encapsulating materials]
[0279] (1) A dry film of each photosensitive resin composition (white solder resist composition) was laminated on an FR-4 Cu film using a vacuum laminator (CVP-300: manufactured by Nichiko Moulton Co., Ltd.) in a first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and the PET film was peeled off.
[0280] Using a DI exposure device manufactured by Screen, a Kodak Step Tablet N0.2 (41-stage) photomask was used to expose 23 stages to 300 mJ / cm2 using an integrated irradiance meter, and development was performed for 60 seconds with a 1.0% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa, followed by curing in an oven at 150°C for 60 minutes to obtain a cured product (solder resist layer) of the photosensitive resin layer.
[0281] After making a dam measuring 2.0 cm in width, 2.0 cm in height, and 250 to 300 μm in thickness, it was attached to both ends of the cured product of the photosensitive resin layer on the FR-4 Cu film, and a 1:1 mixture of silicone encapsulant A and B was added to the space formed by the dam to laminate a silicone encapsulant layer having a thickness of 250 to 300 μm. After that, curing was performed in an oven at 100°C for 2 hours to complete the first curing, and curing was performed in an oven at 150°C for 4 hours to complete the second curing of the encapsulant. After the second curing was completed, the interface between the cured product of the photosensitive resin layer and the silicone encapsulant layer was peeled with a knife, and then the reaction rate of the upper encapsulant region and the lower encapsulant region of the silicone encapsulant layer was measured on a ZnSe crystal plate using FT-IR equipment, and the degree of curing of the silicone encapsulant among the silicone encapsulant layers was measured.
[0282] [How to calculate the silicone reaction rate]
[0283] 1) Samples (upper and lower) of silicone that had not undergone the first and second curing and silicone that had undergone the second curing were prepared.
[0284] 2) Uncured and cured silicone were placed on a ZnSe crystal plate and FT-IR was measured.
[0285] 3) Using uncured silicone as REF, the Si-H peak of cured silicone (2160 cm -1 ) and calculated the reaction rate by comparing the surroundings (calculation formula below).
[0286] Calculation formula: Height of Si-H peak of cured silicon / Height of Si-H peak of uncured silicon × 100
[0287] (2) In addition, the content of the photopolymerization initiator was measured using the analysis method of gel permeation chromatography using a silicone sealant peeled with a knife.
[0288] Specifically, a 0.05 g sample of the second final cured silicone encapsulant was prepared by peeling off the silicone encapsulant layer formed on the cured product of the photosensitive resin layer with a knife. The 0.05 g sample was dissolved in 10.0 g of THF and then filled into a vial. An ultrasonic vibrator was used to dissolve the undissolved photosensitive resin composition in the solution for 5 minutes to prepare a sample. Afterwards, 100 μl of the sample was injected into a gel permeation chromatography (GPC) equipment and analysis was completed.
[0289] [Calculation of the content of photopolymerization initiator transferred to the protective film]
[0290] After attaching the PF protective film on the above-mentioned second-cured silicone encapsulating material, it was left at a temperature of 40℃ and a humidity of 90% for 24 hours. After that, the PF protective film was peeled off, and 0.05 g of the PF protective film analysis sample was prepared by peeling off the silicone encapsulating material layer formed on the cured product of the photosensitive resin layer with a knife. The 0.05 g analysis sample was dissolved in 5.0 g of tetrahydrofuran (THF) and then filled into a vial. An ultrasonic vibrator was used to dissolve the undissolved photosensitive resin composition in the solution for 5 minutes to prepare a sample. After that, 100 μL of the sample was injected into a gel permeation chromatography (GPC) equipment and analysis was completed.
[0291] [Measurement method and measurement conditions of gel permeation chromatography (GPC) for photopolymerization initiator content analysis]
[0292] Gel permeation chromatography equipment name: E2695 separation module by water, detector: 2998 PDA / 2414 RI, flow rate: 0.5 ml / min, column: HSP gel HR MB-L x 2, HSP gel HR x 1.0, measurement temperature: 4 o C. Mobile phase: THF, the sampled sample was injected into the GPC equipment, and the calculation method was analyzed by quantifying the peak coming from 382 nm, which is the absorption wavelength of TPO, a photopolymerization initiator. Using TPO as the sampled analysis sample and the REF photopolymerization initiator sample, the same operation was performed with samples containing 1, 10, and 100 ppm TPO to obtain a calibration curve, and the photopolymerization initiator contained in the sample was quantified using the calibration curve results obtained at each concentration.
[0293] (Outgas content evaluation)
[0294] ◎: Outgas content <500ppm
[0295] ○: 500ppm≤outgas content<1,000ppm
[0296] △: 1,000ppm≤outgas content<2,000ppm
[0297] X: 2,000ppm≤outgas content
[0298] (Evaluation of the reaction rate of the silicone upper sealant)
[0299] ◎: 70%≤Silicone upper sealing material reaction rate
[0300] ○: 55%≤Silicone upper sealing material reaction rate<70%
[0301] △: 40%≤Silicone upper sealing material reaction rate<55%
[0302] X: Silicone top sealant reaction rate <40%
[0303] (Evaluation of the reaction rate of the silicone lower sealant)
[0304] ◎: 50%≤Silicone upper sealing material reaction rate
[0305] ○: 40%≤Silicone lower sealing material reaction rate<50%
[0306] △: 30%≤Silicone upper sealing material reaction rate<40%
[0307] X: Silicone top sealant reaction rate <30%
[0308] (Content of photopolymerization initiator transferred to the packaging material)
[0309] ◎: Photopolymerization initiator content <300ppm
[0310] ○: 300ppm≤Photopolymerization initiator content<500ppm
[0311] △: 500ppm≤Photopolymerization initiator content<700ppm
[0312] X: 700ppm≤Photopolymerization initiator content
[0313]
[0314] Referring to Table 2, it can be seen that the outgassing content of Examples 1 to 10 including photopolymerization initiator 1 or 2 is significantly lower than that of Comparative Examples 1 to 4, 6, and 7. By significantly reducing the outgassing of the photopolymerization initiator, yellowing of the silicone encapsulant is improved, so that the reaction rate of the silicone encapsulant can be significantly increased, and by reducing the content of the photopolymerization initiator transferred to the silicone encapsulant, the long-term reliability and stability of the product can be improved.
[0315] As in Comparative Examples 1 to 4, 6 and 7, when TPO was used as a photopolymerization initiator, it was confirmed that the photopolymerization initiator TPO was transferred and remained on the silicone encapsulating material in a content of 700 ppm or more, and accordingly, as described in the present specification, the reflectivity and reactivity of the silicone encapsulating material were lowered, which could cause problems in the long-term reliability of the product.
[0316] Meanwhile, as in Examples 1 and 2, when only Omnipol TP is used as a photopolymerization initiator, the amount of outgassing of the photopolymerization initiator and the content of the photopolymerization initiator transferred to the silicone encapsulant are significantly reduced, thereby maintaining high reflectivity, increasing the reaction rate in the encapsulant area, and improving the long-term reliability and stability of the product.
[0317] In addition, as in Examples 3 to 10, even when Omnirad TPO L is used as a photopolymerization initiator, the amount of outgas and the content of the photopolymerization initiator transferred to the silicone encapsulant are significantly reduced, thereby maintaining high reflectivity, increasing the reaction rate in the encapsulant area, and improving the long-term reliability and stability of the product.
[0318] Next, a protective film (PF) was formed on the silicone sealant, and after maintaining it at 40°C temperature / 90% humidity for 24 hours, only the protective film was peeled off, and the content of the photopolymerization initiator transferred to the protective film was measured using gel permeation chromatography, and the results are shown in Table 3 below.
[0319] (Photopolymerization initiator content evaluation)
[0320] ◎: Photopolymerization initiator content <500ppm
[0321] ○: 500ppm≤Photopolymerization initiator content<2,000ppm
[0322] △: 2,000ppm≤Photopolymerization initiator content<4,000ppm
[0323] X: 4,000ppm≤Photopolymerization initiator content
[0324]
[0325] Referring to Table 3 together with Table 2, it can be seen that the outgassing content of Examples 1 to 10 containing photopolymerization initiator 1 or 2 is significantly less than that of Comparative Examples 1 to 4, 6, and 7 containing other photopolymerization initiators, and therefore, the content of the photopolymerization initiator transferred to the protective film as well as the silicone encapsulant is also significantly reduced. Specifically, compared to Comparative Examples 1 to 4, 6, and 7, in the case of Examples 1 to 10, the transfer of the photopolymerization initiator to the protective film (PF) is significantly reduced. This is because when the photopolymerization initiators represented by Chemical Formulas 1 and 2 are used, the outgassing is reduced, and this reduced outgassing prevents the photopolymerization initiator from being transferred to the silicone encapsulant and the protective film, and thus, when the photopolymerization initiator defined in the present invention is used, the reflectivity increases and the reaction rate and curing degree of the silicone encapsulant are increased, so that long-term reliability can be improved.
[0326] Evaluation Example 2: BHAST Test
[0327] The dry films produced in Examples 3 and 4 and Comparative Examples 1 to 4 were laminated on a substrate having comb-shaped electrodes (line / space = 50 μm / 50 μm) formed thereon using a vacuum laminator (CVP-300: manufactured by Nichiko Moulton Co., Ltd.) in a first chamber at 60°C under the conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then pressed under the conditions of a press pressure of 0.2 MPa and a press time of 10 seconds to obtain an evaluation substrate. After peeling off the PET film, exposure was performed at an exposure dose such that 23 stages were obtained from a step tablet (41 stages) using a DI exposure device (Screen Co.), and then development (1 mass% Na2CO3, 30°C, 0.2 MPa) was performed for 60 seconds, thereby completing the production of the substrate. After completing the substrate fabrication, BHAST was performed at 110℃, 85%, and 20V for 250 hours in a chamber to evaluate insulation reliability, BHAST resistance, reflectivity, etc.
[0328] The BHAST test results are shown in Figs. 1a and 1b.
[0329] Next, the reflectance was measured after the BHAST test, and is shown in Table 4 below. The reflectance was measured at a wavelength of 450 nm using a spectrophotometer (CM-2600d, Konica Minolta Sensing Co., Ltd.).
[0330] ◎: 90%≤reflectivity
[0331] ○: 87%≤reflectivity<90%
[0332] △: 84%≤reflectivity<87%
[0333] X: Reflectance <84%
[0334] Additionally, after conducting the HAST resistance test, the results are shown in Table 4 below.
[0335] On a substrate formed with comb-shaped electrodes (line / space = 50 μm / 50 μm), dry films produced in each example and comparative example were laminated using a vacuum laminator (CVP-300: manufactured by Nichiko Moulton Co., Ltd.) in a first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and pressing was performed under conditions of a press pressure of 0.2 MPa and a press time of 10 seconds to obtain an evaluation substrate.
[0336] After peeling the PET film, it was exposed to 300 mJ / cm2 with an integrated light meter, developed for 60 seconds with a 1% Na2CO3 aqueous solution at 30°C and a spray pressure of 0.2 MPa, and cured for 60 minutes in an oven at 150°C to form a dry film cured coating, thereby producing a HAST evaluation substrate. This evaluation substrate was placed in a high-temperature, high-humidity chamber under an atmosphere of 110°C and 85% humidity, charged with a voltage of 20 V, and subjected to a HAST (Highly Accelerated Stress Test) test in the chamber for 250 hours. After 250 hours, the discoloration and dissolution of the dry film cured coating were evaluated according to the following judgment criteria (Equipment manufacturer: Espec, Ion migration system, Equipment name: NY IM1064).
[0337] ○: No peeling, discoloration, or dissolution.
[0338] X: Peeling, discoloration, or dissolution are frequently observed with the naked eye.
[0339]
[0340] Referring to Table 4, it can be confirmed that Examples 3 and 4 have higher reflectivity after the HAST test than Comparative Examples 1 to 4. In addition, it can be confirmed that Examples 3 and 4 have higher reflectivity after the HAST test than Comparative Examples 1 to 4, the degree of copper oxidation and corrosion is very low, and there is no phenomenon of peeling, discoloration, or dissolution.
[0341] Evaluation Example 3: Reflectance Test (After Reflow and UV Treatment)
[0342] The dry films produced in Examples 1 to 4 and Comparative Examples 1 to 7 were laminated on a copper substrate using a vacuum laminator (CVP-300: manufactured by Nichiko Moulton Co., Ltd.) in a first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and pressing was performed under conditions of a press pressure of 0.2 MPa and a press time of 10 seconds.
[0343] After peeling off the PET film, the exposure was performed using a DI exposure device manufactured by Screen, with an integrated light meter to obtain 300 mJ / cm2, and a Kodak Step Tablet N0.2 (41-stage) photomask was used to obtain 23 stages, and development was performed for 60 seconds with a 1% Na2CO3 aqueous solution at 30°C and a spray pressure of 0.2 MPa, and curing was performed in an oven at 150°C for 60 minutes to obtain a substrate. The reflectance at a wavelength of 450 nm was measured for the surface of the coating film of the obtained substrate using a spectrophotometer (CM-2600d, Konica Minolta Sensing Co., Ltd.). The reflow was performed at 260 oThe process was repeated 1 to 3 times for 10 seconds under C conditions, and the reflectance was measured. The results are shown in Table 5. In addition, after the final curing, the UV was passed through a photometer at 500 mJ / cm2 for 3 times, and the reflectance was measured for each pass. The results are shown in Table 6.
[0344] ◎: 90%≤reflectivity
[0345] ○: 87%≤reflectivity<90%
[0346] △: 84%≤reflectivity<87%
[0347] X: Reflectance <84%
[0348]
[0349] In the case of Examples 1 to 4, not only the initial reflectance when reflow was not performed, but also the reflectance at 450 nm after reflow was performed 1, 2, and 3 times and after reflow was performed once and firing was performed, was higher than in Comparative Examples 1 to 7, confirming that the decrease in reflectance after reflow or firing was small.
[0350] In particular, Examples 1 to 4 use Omnipol TP or Omnirad TPO-L as the photopolymerization initiator, resulting in a small amount of outgassing and thus a minimal impact on the silicone encapsulant, thereby allowing the sintering process to be omitted. Accordingly, high reflectivity can be maintained even after reflow.
[0351] However, for Comparative Examples 1 to 7, a firing process to remove TPO must be performed after the reflow process in order to apply the TPO photopolymerization initiator to backlight unit products, as it affects the curing properties of the silicone encapsulant. Furthermore, it can be confirmed that the reflectivity is significantly reduced after the firing process.
[0352] In conclusion, compared to Comparative Examples 1 to 7, Examples 1 to 4 have excellent reflectivity applied to actual products at an equivalent or higher level, and as seen in Table 2 above, the reactivity and curing degree of the silicone encapsulant are excellent, so that the long-term reliability and stability of the product can be improved.
[0353]
[0354] The reflectance at 450 nm of Examples 1 to 4 showed a higher initial reflectance than that of Comparative Examples 1 to 6, and showed a similar tendency even after being treated three times with UV at 500 mJ. The reflectance of Examples 1 to 4 after being treated three times with UV was 90.2 to 90.6, but Comparative Examples 1 to 4 showed a reflectance of 73 to 89.7 after being treated three times with UV, which may be due to the severe yellowing.
[0355] Evaluation Example 4: Test in a chamber with a temperature of 85℃ and a humidity of 85%, reflectivity test in an HS chamber
[0356] The dry films produced in Examples 2 to 4 and Comparative Example 1 were laminated using a vacuum laminator (CVP-300: manufactured by Nichiko Moulton Co., Ltd.) in a first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then pressed under conditions of a press pressure of 0.2 MPa and a press time of 10 seconds to obtain an evaluation substrate.
[0357] After peeling off the PET film, it was exposed to 300 mJ / cm2 using an integrated light meter, developed with a 1% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa for 60 seconds, and cured in an oven at 150°C for 60 minutes to obtain a substrate. The obtained substrate was placed in a chamber (HIFLEX, Temperature and Humidity Chamber, ETAC) at a temperature of 85°C and a humidity of 85% and left for 1000 hours. The reflectance at a wavelength of 450 nm was measured for the substrate left in the HS chamber for 1000 hours using a spectrophotometer (CM-2600d, Konica Minolta Sensing Co., Ltd.). The results are shown in Table 7.
[0358] ◎: 90%≤reflectivity
[0359] ○: 87%≤reflectivity<90%
[0360] △: 84%≤reflectivity<87%
[0361] X: Reflectance <84%
[0362]
[0363] Examples 2 to 4 confirmed that the reflectance at 450 nm was not reduced much even under high temperature and humid conditions when evaluated for a long period of time.
[0364] Meanwhile, in the case of Examples 2 to 4, the b value after evaluation under high temperature and high humidity conditions was smaller than that of Comparative Example 1. This indicates that Examples 2 to 4 exhibited less yellowing than Comparative Example 1 under high temperature and high humidity conditions. Since Examples 2 to 4 exhibited less yellowing even under harsh conditions of high temperature and high humidity compared to Comparative Example 1, they can be more usefully used as materials for backlight units.
[0365] Evaluation Example 5: General Property Evaluation
[0366] <Production of the evaluation board>
[0367] The photosensitive resin compositions produced in each example and comparative example were laminated on a PET film substrate using a vacuum laminator (CVP-300: manufactured by Nichiko Moulton Co., Ltd.) in the first chamber at 60°C under the conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then pressed under the conditions of a press pressure of 0.2 MPa and a press time of 10 seconds to obtain an evaluation substrate. After peeling off the PET film, the exposure was performed to 23 stages using a Kodak Step Tablet N0.2 (41 stages) photomask so that the irradiance was 300 mJ / cm2 using a DI exposure device manufactured by Screen, and development was performed with a 1% Na2CO3 aqueous solution at 30°C under the conditions of a spray pressure of 0.2 MPa for 60 seconds, and final curing was performed in an oven at 150°C to produce a substrate.
[0368] Pencil Hardness
[0369] Using the above substrate, a pencil from B to 9H, polished to make the tip flat, was pressed at an angle of approximately 45°, and the hardness of the pencil at which peeling of the film did not occur was recorded.
[0370] <Adhesion>
[0371] A 1 mm checkerboard grid (10×10) was made on the above substrate, a transparent adhesive tape was completely attached to the checkerboard grid, and then one end of the tape was immediately removed while being held perpendicular to the substrate, and the number of checkerboard grids remaining without being completely peeled off was counted. The results were recorded with the number of remaining checkerboard grids as the numerator and the total number of checkerboard grids (100) as the denominator.
[0372] PASS: More than 95% of the board remains.
[0373] NG: Less than 95% of the board remains.
[0374] Gloss Evaluation
[0375] For the coating surface of the above substrate, the gloss at an angle of 60° was measured using a gloss spectrometer (BYK E-4430).
[0376] <Solder heat resistance>
[0377] After immersing the above substrate in a soldering bath at 288°C for 10 seconds, 1 mm checkerboard patterns (10×10) were created on the substrate, transparent adhesive tape was completely attached on the checkerboard patterns, and immediately, while maintaining one end of the tape perpendicular to the substrate, it was momentarily removed to determine the number of checkerboard patterns that remained without being completely peeled off. The results were recorded with the number of remaining checkerboard patterns as the numerator and the total number of checkerboard patterns (100) as the denominator.
[0378] PASS: More than 95% of the board remains.
[0379] NG: Less than 95% of the board remains.
[0380]
[0381] However, in the case of Comparative Example 5, the surface hardening was not done well because the content of the photopolymerization initiator was low, and as a result, the pencil hardness was low at 3H, the gloss was significantly reduced to 72, the adhesion and solder heat resistance were NG, and the developability was also poor. In addition, in the case of Comparative Example 6, the content of the photopolymerization initiator was too high, and as a result of good surface hardening, the adhesion and solder heat resistance were excellent, but the developability was poor due to the increased curing, and this may cause problems in forming SRO. In Example 7, the pencil hardness was improved to 6H, and the adhesion and solder heat resistance were greatly improved, and in Example 8, the pencil hardness was improved to 6H, and the adhesion and solder heat resistance were greatly improved.
[0382] Evaluation Example 6: Analysis of phosphorus content in photosensitive resin composition
[0383] 1) 0.1 g of the photosensitive resin compositions of Examples 1 to 8 and Comparative Examples 1 to 6 were accurately weighed in a beaker, 2 mL of nitric acid was added, and the mixture was heated on a hot plate to react. 2) The samples were temporarily removed from the hot plate, cooled to room temperature, and 0.03 mL of hydrochloric acid was added while hot to react. 3) Afterwards, the nitric acid solution of the samples was not completely evaporated, but a small amount remained, and after cooling to room temperature, 1 mL of concentrated nitric acid was added again to completely dissolve the samples. After the samples were completely dissolved, they were diluted with ultrapure water. 4) The concentration of phosphorus (P) in the examples and comparative examples was analyzed under conditions of wavelengths of 213.617 nm and 214.914 nm using an ICP-OES analyzer (Optima series, manufactured by Perkin Elmer).
[0384]
[0385] The compositions of Examples 1 to 8 and Comparative Examples 1 to 4 were detected to have phosphorus contents of approximately 3,000 ppm. Comparative Example 5 was detected to have a low phosphorus content of approximately 430 ppm because it did not use a phosphorus-containing photopolymerization initiator. In addition, the phosphorus content of Comparative Example 6 was detected to be 5,500 ppm in the composition.
Claims
1. (A) A carboxyl group-containing resin that does not contain an aromatic ring, (B) Weapon filler, and (E) A photopolymerization initiator comprising a trimethylbenzoylphosphine oxide group-containing compound including one or more PO bonds. A photosensitive resin composition comprising:
2. In paragraph 1, A photosensitive resin composition, wherein the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), comprises a *-C(=O)-P(=O)R1-O-*' moiety (wherein R1 is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a cyclic group having 5 to 20 carbon atoms).
3. In paragraph 1, A photosensitive resin composition, wherein the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), is a trimethylbenzoylphosphine oxide group-containing polymer.
4. In paragraph 3, The above trimethylbenzoylphosphine oxide group-containing polymer has a weight average molecular weight (M n ) is 900 g / mol or more, a photosensitive resin composition.
5. In paragraph 3, A photosensitive resin composition, wherein the above trimethylbenzoylphosphine oxide group-containing polymer is represented by the following chemical formula 1. <Chemical Formula 1> a= 0~100, b= 0~100, c=0~100 6. In paragraph 1, A photosensitive resin composition, wherein the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), includes an alkoxy group.
7. In paragraph 1, A photosensitive resin composition, wherein the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), includes an ethoxy group.
8. In paragraph 1, A photosensitive resin composition, wherein the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), is represented by the following chemical formula 2. <Chemical Formula 2> 9. In paragraph 1, A photosensitive resin composition, wherein the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including at least one PO bond (E), is 0.01 to 10 wt% based on the total weight of the composition.
10. In paragraph 1, A photosensitive resin composition in which the carboxyl group-containing resin that does not contain an aromatic ring (A) contains an unsaturated double bond.
11. In paragraph 1, (D) A photosensitive resin composition further comprising a resin containing an aromatic ring.
12. In paragraph 11, A photosensitive resin composition, wherein the resin containing the above (D) aromatic ring is a melamine resin, a silicone resin, or a resin having a styrene skeleton.
13. In paragraph 1, (C) A photosensitive resin composition further comprising a mercapto-modified (meth)acrylate.
14. In paragraph 1, (F) A photosensitive resin composition further comprising a silane coupling agent.
15. In paragraph 1, (G) A photosensitive resin composition further comprising a resin having a urethane bond.
16. In paragraph 1, A photosensitive resin composition, wherein the content of outgas measured by thermal desorption spectroscopy (TDS) and gas chromatography-mass spectrometry (GC-MS) for the photosensitive resin composition is 1,000 ppm or less with respect to the content of a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound including (E) one or more PO bonds.
17. In paragraph 1, A photosensitive resin composition having a phosphorus content of 500 to 5000 ppm. 18.(A) Carboxyl group-containing resin not containing an aromatic ring, (C) mercapto-modified (meth)acrylate, and (E) A photopolymerization initiator comprising a trimethylbenzoylphosphine oxide group-containing compound including one or more PO bonds. A photosensitive resin composition comprising:
19. In paragraph 18, (D) A photosensitive resin composition further comprising a resin containing an aromatic ring.
20. In paragraph 18, (F) A photosensitive resin composition further comprising a silane coupling agent.
21. In paragraph 18, (G) A photosensitive resin composition further comprising a resin having a urethane bond.
22. A dry film having a photosensitive resin layer formed by applying and drying a photosensitive resin composition according to any one of claims 1 to 21 on a first film.
23. A cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 21 or the photosensitive resin layer of a dry film obtained therefrom.
24. A printed wiring board comprising a cured product according to Article 23 as a solder resist.
25. In paragraph 24, A printed wiring board further comprising a silicone encapsulating layer disposed on the solder resist.
26. In paragraph 25, The above silicone encapsulating material layer includes an upper encapsulating material region and a lower encapsulating material region, A printed wiring board, wherein the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including (E) one or more PO bonds, contained in at least one of the upper encapsulating material region or the lower encapsulating material region, is 1,000 ppm or less relative to the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound including (E) one or more PO bonds, contained in the solder resist.
27. Hardened material according to Article 23; and, A laminate comprising a protective film.
28. In paragraph 27, A laminate, wherein the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound containing (E) one or more PO bonds included in the protective film, is 1,000 ppm or less relative to the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound containing (E) one or more PO bonds included in the solder resist.
Citation Information
Patent Citations
Flame-retardant photocurable resin composition, dry film and cured product of the same, and printed wiring board using the composition, dry film or cured product
KR1020110039452A
Photosensitive compositions, preparation methods thereof, and quantum dot polymer composite pattern produced therefrom
KR1020170073019A
Intelligent distribution box and controlling method of the same
KR102539823B1
Blue LED cure on demand compositions
US20200017623A1
Flame retardant photoimagable coverlay compositions
WO2007073498A2