Solid electrolyte and all-solid-state battery comprising same

The development of a sulfide-based solid electrolyte with an argyrodite-type crystal structure and a Li2CO3 buffer layer addresses moisture stability and interfacial reaction issues, improving battery performance by maintaining a stable phase and high ionic conductivity.

WO2024205304A1PCT designated stage expired Publication Date: 2024-10-03LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004034
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Sulfide-based solid electrolytes in all-solid-state batteries face issues with moisture stability and interfacial side reactions with electrode materials, leading to performance deterioration over time.

Method used

A sulfide-based solid electrolyte with an argyrodite-type crystal structure and a Li2CO3 buffer layer, formulated as Li(a)(P1-bMb)S6-cXc, where M is Sb, Sn, Ge, Si, Nb, Ni, Ga, and X is F, Cl, Br, I, with specific ionic conductivity and band integral value ranges, is developed to enhance moisture stability and suppress side reactions.

Benefits of technology

The solid electrolyte maintains a stable phase and improves battery characteristics by reducing interfacial side reactions and maintaining high ionic conductivity, leading to enhanced lifespan and rate characteristics of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004034_03102024_PF_FP_ABST
    Figure KR2024004034_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a solid electrolyte and an all-solid-state battery comprising same, the solid electrolyte comprising: a sulfide-based solid electrolyte particle; and a buffer layer comprising Li2CO3, formed on the sulfide-based solid electrolyte particle, wherein, on an NIR spectrum, a Li2CO3 band integral value existing in the region between 5200 cm-1 and 4725 cm-1 is at least 2.0 and at most 8.0.
Need to check novelty before this filing date? Find Prior Art

Description

Solid electrolyte and all-solid-state battery containing the same

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0042176, filed March 30, 2023, the entire contents of which are incorporated herein by reference.

[0003] Technology field

[0004] The present invention relates to a solid electrolyte and an all-solid-state battery including the same.

[0005]

[0006] All-solid-state batteries replace the liquid electrolyte that fills the space between the positive and negative electrodes of conventional lithium secondary batteries with a solid electrolyte. They are safe because they eliminate the risk of explosion, and they boast a higher energy density than conventional batteries, making them a promising next-generation battery option. The solid electrolyte used in all-solid-state batteries is a solid material capable of conducting lithium ions within the battery, boasting ionic conductivity comparable to that of the electrolytes currently used in lithium secondary batteries. Key materials for solid electrolytes include polymers, sulfides, and oxides, but among them, sulfide-based solid electrolytes, which are highly flexible and highly conductive, are considered suitable for manufacturing high-capacity, large-scale batteries.

[0007] However, sulfide-based solid electrolytes have a problem in that they decompose by reacting with moisture in the air and generating hydrogen sulfide gas, and there is a problem in that battery performance deteriorates during long-term operation due to decomposition products generated by interfacial side reactions with electrode materials.

[0008] Accordingly, there is a need to develop a sulfide-based solid electrolyte that can suppress reactions with moisture in the air and interfacial side reactions with electrode materials.

[0009]

[0010] The problem to be solved by the present invention is to provide a solid electrolyte having improved moisture stability and capable of suppressing interfacial side reactions with electrode materials, and an all-solid-state battery including the same.

[0011] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.

[0012]

[0013] To solve the above problem, the present invention provides a solid electrolyte and an all-solid-state battery including the same.

[0014]

[0015] (1) The present invention comprises a sulfide-based solid electrolyte particle; and a buffer layer comprising Li2CO3 formed on the sulfide-based solid electrolyte particle; and in the NIR spectrum, 5200 cm -1 Height 4725cm -1 A solid electrolyte having a Li2CO3 band integral value existing in a region of 2.0 or more and 8.0 or less is provided.

[0016] (2) The present invention provides a solid electrolyte in the above (1), wherein the sulfide-based solid electrolyte has an argyrodite-type crystal structure.

[0017] (3) The present invention provides a solid electrolyte in (1) or (2) above, wherein the sulfide-based solid electrolyte has a composition represented by the following chemical formula 1.

[0018] [Chemical Formula 1]

[0019] Li a (P 1-b M b )S 6-c X c

[0020] In the above chemical formula 1,

[0021] M is at least one selected from Sb, Sn, Ge, Si, Nb, Ni, Ga, and Al,

[0022] X is one or more selected from F, Cl, Br, and I,

[0023] 5.0 <a<7.5, 0≤b≤0.7, 0<c≤2.0이다.

[0024] (4) The present invention provides a solid electrolyte having an ionic conductivity of 3 mS / cm to 12 mS / cm in any one of the above (1) to (3).

[0025] (5) The present invention, in any one of the above (1) to (4), in the NIR spectrum, 7200 cm -1 Height 7140cm -1 A solid electrolyte having a LiOH band integral value of less than 0.1 existing in the region is provided.

[0026] (6) The present invention, in any one of the above (1) to (5), PS4 in the 2p spectrum of phosphorus (P) obtained by XPS analysis 3- Peak area (A1) and PO x S 4-x 3- PO for the sum of peak areas (A2) x S 4-x 3- A solid electrolyte is provided having a ratio of peak areas (A2) (A2 / (A1+A2)) of less than 0.1.

[0027] (7) The present invention provides an all-solid-state battery comprising a solid electrolyte according to any one of (1) to (6).

[0028]

[0029] The solid electrolyte according to the present invention comprises a buffer layer comprising Li2CO3 formed on sulfide-based solid electrolyte particles, and in the NIR spectrum, 5200 cm -1 Height 4725cm -1Since the Li2CO3 band integral value existing in the region satisfies a value of 2.0 or more and 8.0 or less, a stable phase is maintained when exposed to moisture in the battery manufacturing process, and an interfacial side reaction between the solid electrolyte and the electrode material can be suppressed, which has the advantage of improving battery characteristics.

[0030]

[0031] Figure 1 is an XRD peak of the solid electrolyte of Example 5.

[0032] Figure 2 shows XPS data of the solid electrolytes of Examples 1 to 3 and Comparative Examples 3 and 6.

[0033] Figure 3 shows rate characteristic evaluation data of an all-solid-state battery including the solid electrolytes of Example 1 and Comparative Example 1.

[0034]

[0035] Hereinafter, the present invention will be described in more detail to help understand the present invention.

[0036]

[0037] The terms and words used in this specification should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0038] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0039] In this specification, it should be understood that terms such as “include,” “comprising,” or “having” are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0040] In this specification, room temperature means 20°C to 25°C.

[0041]

[0042] solid electrolyte

[0043] The solid electrolyte according to the present invention comprises: sulfide-based solid electrolyte particles; and a buffer layer comprising Li2CO3 formed on the sulfide-based solid electrolyte particles; and in the NIR spectrum, 5200 cm -1 Height 4725cm -1 The Li2CO3 band integral value existing in the region is 2.0 or more and 8.0 or less.

[0044]

[0045] The present inventors have developed a solid electrolyte comprising sulfide-based solid electrolyte particles; and a buffer layer comprising Li2CO3 formed on the sulfide-based solid electrolyte particles; and in the NIR spectrum, 5200 cm -1 Height 4725cm -1 When the Li2CO3 band integral value existing in the region satisfies the condition of 2.0 or more and 8.0 or less, the moisture stability of the solid electrolyte is improved, so that a stable phase of the solid electrolyte is maintained in the battery manufacturing process, and as a result, the lifespan and rate characteristics of the battery can be improved, thereby completing the present invention.

[0046]

[0047] According to the present invention, the sulfide-based solid electrolyte may have an argyrodite-type crystal structure in terms of high ionic conductivity and low reactivity with a lithium negative electrode.

[0048] The above sulfide-based solid electrolyte may be a sulfide-based solid electrolyte containing Li, P, and S.

[0049] According to the present invention, the sulfide-based solid electrolyte may have a composition represented by the following chemical formula 1. In this case, the ionic conductivity may be excellent even after the buffer layer is formed.

[0050] [Chemical Formula 1]

[0051] Li a (P 1-b M b )S 6-c X c

[0052] In the above chemical formula 1,

[0053] M is at least one selected from Sb, Sn, Ge, Si, Nb, Ni, Ga, and Al,

[0054] X is one or more selected from F, Cl, Br, and I,

[0055] 5.0 <a<7.5, 0≤b≤0.7, 0<c≤2.0이다.

[0056]

[0057] The above M is a cation doped at the position of P, and specifically, it may be at least one selected from Sb, Sn, Ge, and Si. In this case, since it has a similar oxidation number to P, it may be easily doped (substituted) at the P position.

[0058] The above X can be specifically Cl, Br, or a combination thereof. In this case, the degree of disorder of the anion arrangement increases, thereby changing the lithium ion conduction path, and consequently, the ion conductivity can be further increased.

[0059] The above a may be greater than 5.0, 5.1, 5.2, 5.3, 5.4, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4 or less, or less than 7.5. More specifically, the above a may be greater than 5.4 and less than 6.6. In this case, formation of an argyrodite phase having an appropriate lithium concentration is possible, so that ionic conductivity may be higher.

[0060] The above b may be 0 or more and 0.3, 0.4, 0.5, 0.6, or 0.7 or less. More specifically, the above b may be 0 or more and 0.3 or less. In this case, since the amount of cation doping (substitution amount) is appropriate, the amount of impurities may be reduced.

[0061] The above c may be greater than 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 or more, 1.6, 1.7, 1.8, 1.9, or 2.0 or less. In this case, the formation of an argyrodite phase is possible, and the degree of disorder of the anion arrangement increases, so the ionic conductivity may be higher.

[0062]

[0063] The above buffer layer may be a mixture of Li2CO3 and argyrodite-type crystal structures.

[0064]

[0065] According to the present invention, the solid electrolyte has an NIR spectrum at 5200 cm -1 Height 4725cm -1 The Li2CO3 band integral value existing in the region may be 2.0 or more and 8.0 or less. Specifically, in the NIR spectrum, 5200 cm -1 Height 4725cm -1The Li2CO3 band integral value present in the region may be 2.0 or more, 2.1 or more, 2.2 or more, 2.3 or more, 2.4 or more, 2.5 or more, 2.6 or more, 2.7 or more, 2.8 or more, 2.9 or more, 3.0 or more, 3.1 or more, 3.2 or more, or 3.3 or more, 6.6 or less, 6.7 or less, 6.8 or less, 6.9 or less, 7.0 or less, 7.1 or less, 7.2 or less, 7.3 or less, 7.4 or less, 7.5 or less, 7.6 or less, 7.7 or less, 7.8 or less, 7.9 or less, or 8.0 or less. In this case, an appropriate amount of buffer layer is created, which is effective in blocking side reactions and has the advantage of higher ionic conductivity performance.

[0066] Meanwhile, in the NIR spectrum of the solid electrolyte, 5200 cm -1 Height 4725cm -1 If the Li2CO3 band integral value existing in the region is less than 2.0, the buffer layer is not sufficiently formed, so there is no side reaction blocking effect, and if it exceeds 8.0, there is a problem of low ionic conductivity due to excessive formation of impurity phases other than the argyrodite-type crystal structure.

[0067]

[0068] According to the present invention, the solid electrolyte may have an ionic conductivity of 3 mS / cm to 12 mS / cm.

[0069]

[0070] According to the present invention, the solid electrolyte has an NIR spectrum at 7200 cm -1 Height 7140cm -1 The LiOH band integral value existing in the region may be less than 0.1. That is, the buffer layer of the solid electrolyte may expose the electrolyte particles at a sufficiently low dew point so as to contain little lithium hydroxide. In this case, the amount of secondary phase generated is small, so there is an advantage of high ionic conductivity performance. Specifically, the solid electrolyte has an NIR spectrum of 7200 cm -17140cm in height -1 The LiOH band integral present in the region may be 0.

[0071]

[0072] According to the present invention, the solid electrolyte is PS4 in the 2p spectrum of phosphorus (P) obtained by XPS analysis. 3- Peak area (A1) and PO x S 4-x 3- PO for the sum of peak areas (A2) x S 4-x 3- The ratio of peak areas (A2) (A2 / (A1+A2)) may be less than 0.1, specifically 0.09 or less, and more specifically 0.085 or less (PO x S 4-x 3- In , x is 0 <x<4임). 즉, 상기 고체 전해질의 버퍼층은 PS4 3- Since the bond within the unit is not broken, PO x S 4-x 3- There may be no bonding. In this case, the amount of secondary phase produced is small, which has the advantage of high ionic conductivity.

[0073]

[0074] The solid electrolyte according to the present invention can be manufactured, for example, by exposing sulfide-based solid electrolyte particles to air having a dew point temperature of -40°C or higher and -20°C or lower, allowing trace amounts of moisture and carbon dioxide to react with the sulfide-based solid electrolyte particles, thereby forming a buffer layer containing Li2CO3 on the sulfide-based solid electrolyte particles, and then drying the sulfide-based solid electrolyte particles on which the buffer layer containing Li2CO3 has been formed, but is not limited thereto.

[0075] At this time, the exposure may be performed at room temperature to control extreme reactions with moisture. In the present invention, room temperature may mean 20°C to 25°C. Furthermore, the exposure may be performed for 1 to 10 hours. Specifically, the exposure may be performed for 1 hour, 2 hours, 3 hours or more, 4 hours, 5 hours, or 10 hours or less. In this case, there is an advantage in that a buffer layer with appropriate ionic conductivity is created.

[0076] Meanwhile, the drying may be vacuum drying performed in a vacuum to quickly remove residual moisture adsorbed on the surface. The drying may be performed at a temperature of 50°C to 150°C to sufficiently remove moisture while preventing particles from clumping together. Specifically, the drying may be performed at a temperature of 50°C, 55°C or higher, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or lower than 150°C. The drying may be performed for 5 to 24 hours to sufficiently remove moisture. Specifically, the drying may be performed for 5 hours, 7 hours, 9 hours, 10 hours, 12 hours, or lower than 24 hours.

[0077]

[0078] All-solid-state batteries

[0079] The present invention provides an all-solid-state battery comprising the above solid electrolyte.

[0080] Specifically, the all-solid-state battery comprises a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, and a solid electrolyte layer including a solid electrolyte according to the present invention disposed between the positive electrode and the negative electrode.

[0081] The all-solid-state battery according to the present invention has a small decrease in ionic conductivity due to moisture, and thus can have excellent initial efficiency, life characteristics, and output characteristics of the battery.

[0082]

[0083] At this time, the all-solid-state battery of the present invention can be manufactured according to a conventional method known in the art. For example, it can be manufactured by laminating and pressurizing so that a solid electrolyte layer exists between the positive and negative electrodes.

[0084]

[0085] (1) Bipolar

[0086] The above positive electrode can be manufactured by coating a positive electrode slurry containing a positive electrode active material, a binder, a conductive agent, a solvent, etc. on a positive electrode current collector.

[0087] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the bonding strength of the positive electrode active material may be strengthened by forming fine irregularities on the surface, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0088]

[0089] The above-mentioned positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically may include a lithium metal oxide containing lithium and one or more metals such as cobalt, manganese, nickel or aluminum. More specifically, the lithium metal oxide may be a lithium-manganese oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt oxide (e.g., LiCoO2, etc.), a lithium-nickel oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese oxide (e.g., LiNi 1-Y Mn Y O2 (here, 0 <Y<1), LiMn 2-z Ni zO4 (where 0<Z<2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 Co Y1 O2 (here, 0 <Y1<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y2 Mn Y2 O2 (here, 0 <Y2<1), LiMn 2-z1 Co z1 O4 (wherein, 0<Z1<2) etc.), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r1 )O2(wherein, 0<p<1, 0<q<1, 0<r1<1, p+q+r1=1) or Li(Ni p1 Co q1 Mn r2 )O4 (wherein, 0<p1<2, 0<q1<2, 0<r2<2, p1+q1+r2=2) etc.), or lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M S2 )O2 (wherein, M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r3 and s2 are atomic fractions of independent elements, respectively, 0<p2<1, 0<q2<1, 0<r3<1, 0<s2<1, p2+q2+r3+s2=1), etc.), and one or more compounds of these may be included.

[0090] Among these, the lithium metal oxides are LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (e.g., Li(Ni)) in that they can improve the capacity characteristics and stability of the battery. 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni) 0.5 Mn 0.3Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.), and considering the remarkable improvement effect according to the control of the type and content ratio of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni) 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc., and any one of these or a mixture of two or more of them may be used.

[0091] The above positive electrode active material may be included in an amount of 60 wt% to 99 wt%, preferably 70 wt% to 99 wt%, and more preferably 80 wt% to 98 wt%, based on the total weight of the solid content excluding the solvent in the positive electrode slurry.

[0092]

[0093] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0094] Typically, the binder may be included in an amount of 1 wt% to 20 wt%, preferably 1 wt% to 15 wt%, and more preferably 1 wt% to 10 wt%, based on the total weight of solids excluding the solvent in the positive electrode slurry.

[0095]

[0096] The above-mentioned conductive agent is a component for further improving the conductivity of the positive electrode active material.

[0097] The conductive material is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, carbon-based materials such as graphite; carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorinated carbon, aluminum, and nickel powders; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives can be used.

[0098] Typically, the conductive material may be included in an amount of 1 wt% to 20 wt%, preferably 1 wt% to 15 wt%, and more preferably 1 wt% to 10 wt%, based on the total weight of solids excluding the solvent in the positive electrode slurry.

[0099]

[0100] The solvent may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a desirable viscosity when including the positive electrode active material, and optionally a binder and a conductive material. For example, the positive electrode active material, and optionally a binder and a conductive material, may be included so that the solid concentration is 50 wt% to 95 wt%, preferably 70 wt% to 95 wt%, and more preferably 70 wt% to 90 wt%.

[0101]

[0102] (2) Cathode

[0103] The above-mentioned negative electrode can be manufactured, for example, by coating a negative electrode slurry containing a negative electrode active material, a binder, a conductive material, and a solvent on a negative electrode current collector, or a graphite electrode made of carbon (C) or the metal itself can be used as the negative electrode.

[0104] For example, when manufacturing a negative electrode by coating a negative electrode slurry on the negative electrode current collector, the negative electrode current collector generally has a thickness of 3 to 500 μm. The negative electrode current collector is not particularly limited as long as it has high conductivity without causing a chemical change in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, like the positive electrode current collector, the bonding strength of the negative electrode active material can be strengthened by forming fine unevenness on the surface, and can be used in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric, etc.

[0105] The above negative active materials include natural graphite, artificial graphite, carbonaceous materials; lithium-containing titanium composite oxide (LTO), Si, SiO x , Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; alloys composed of the above metals (Me); oxides (MeO) of the above metals (Me) x ); and one or more types of negative electrode active materials selected from the group consisting of complexes of the above metals (Me) and carbon. Specifically, the negative electrode active materials include silicon (Si), silicon oxide (SiO x) or a silicon alloy, etc., may be used. In this case, a thin and stable SEI layer containing a siloxane bond is formed, thereby further improving the high-temperature stability and lifespan characteristics of the battery.

[0106] The above negative electrode active material may be included in an amount of 60 wt% to 99 wt%, preferably 70 wt% to 99 wt%, and more preferably 80 wt% to 98 wt%, based on the total weight of solids excluding the solvent in the negative electrode slurry.

[0107]

[0108] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0109] Typically, the binder may be included in an amount of 1 wt% to 20 wt%, preferably 1 wt% to 15 wt%, and more preferably 1 wt% to 10 wt%, based on the total weight of solids excluding the solvent in the slurry for the negative electrode.

[0110]

[0111] The above conductive agent is a component for further improving the conductivity of the negative electrode active material. The conductive agent is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0112] The above-mentioned conductive agent may be included in an amount of 1 wt% to 20 wt%, preferably 1 wt% to 15 wt%, and more preferably 1 wt% to 10 wt%, based on the total weight of solids excluding the solvent in the negative electrode slurry.

[0113]

[0114] The solvent may include water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a desirable viscosity when including the negative electrode active material, and optionally a binder and a conductive material. For example, the concentration of the solid content including the negative electrode active material, and optionally a binder and a conductive material may be 50 wt% to 95 wt%, preferably 70 wt% to 90 wt%.

[0115]

[0116] When using the metal itself as the above-mentioned cathode, it can be manufactured by physically bonding, rolling, or depositing the metal onto the metal thin film itself or the cathode current collector. The deposition method can use an electrical deposition method or a chemical vapor deposition method.

[0117] For example, the metal to be bonded / rolled / deposited on the metal thin film itself or the negative electrode current collector may include one metal selected from the group consisting of lithium (Li), nickel (Ni), tin (Sn), copper (Cu), and indium (In), or an alloy of two metals.

[0118]

[0119] (3) Solid electrolyte layer

[0120] The solid electrolyte layer may further include a binder in addition to the solid electrolyte according to the present invention.

[0121] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0122] Typically, the binder may be included in an amount of 1 wt% to 20 wt%, preferably 1 wt% to 15 wt%, and more preferably 1 wt% to 10 wt%, based on the total weight of the solid electrolyte layer.

[0123]

[0124] The present invention provides a battery module including the above-described all-solid-state battery as a unit cell and a battery pack including the same. The battery module and battery pack include the above-described secondary battery having high capacity, high rate characteristics, and cycle characteristics, and thus can be used as a power source for medium- to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0125]

[0126] Hereinafter, preferred embodiments are presented to help understand the present invention, but the above embodiments are only illustrative of the present disclosure, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of ​​the present disclosure, and it is natural that such changes and modifications fall within the scope of the appended patent claims.

[0127]

[0128] Manufacturing example

[0129] Manufacturing Example 1

[0130] Four precursors, Li2S, P2S5, LiCl, and LiBr, were dry mixed (ball milled) in a molar ratio of 1.9:0.5:0.6:1.0. During dry mixing, a planetary ball mill equipped with zirconia balls was used, and the mixture was rotated at a speed of 300 rpm or more to ensure uniform mixing. Afterwards, the obtained mixed precursor was heat-treated at 400-550°C for 12 hours to crystallize, and then pulverized through ball milling again to obtain Li having an argyrodite-type crystal structure. 5.4 PS 4.4 Cl 0.6 Br 1.0 Particles were manufactured. All of the above processes were performed under an inert Ar atmosphere.

[0131]

[0132] Manufacturing Example 2

[0133] Four precursors, Li2S, P2S5, LiCl, and LiBr, were dry mixed (ball milled) at a molar ratio of 2.0:0.5:0.5:1.0. During dry mixing, a planetary ball mill equipped with zirconia balls was used, and the mixture was rotated at a speed of 300 rpm or more to ensure uniform mixing. Afterwards, the obtained mixed precursor was heat-treated at 400-550°C for 12 hours to crystallize, and then pulverized through ball milling again to obtain Li having an argyrodite-type crystal structure. 5.5 PS 4.5 Cl 0.5 Br 1.0Particles were manufactured. All of the above processes were performed under an inert Ar atmosphere.

[0134]

[0135] Manufacturing Example 3

[0136] Four precursors, Li2S, P2S5, LiCl, and LiBr, were dry mixed (ball milled) at a molar ratio of 1.9:0.5:1.0:0.6. During dry mixing, a planetary ball mill equipped with zirconia balls was used, and the mixture was rotated at a speed of 300 rpm or more to ensure uniform mixing. Afterwards, the obtained mixed precursor was heat-treated at 400-550°C for 12 hours to crystallize, and then pulverized through ball milling again to obtain Li having an argyrodite-type crystal structure. 5.4 PS 4.4 Cl 1.0 Br 0.6 Particles were manufactured. All of the above processes were performed under an inert Ar atmosphere.

[0137]

[0138] Manufacturing Example 4

[0139] Three precursors, Li2S, P2S5, and LiCl, were dry mixed (ball milled) in a molar ratio of 2:0.5:1.5. During dry mixing, a planetary ball mill equipped with zirconia balls was used, and the mixture was rotated at a speed of 300 rpm or more to ensure uniform mixing. Afterwards, the obtained mixed precursor was heat-treated at 400-550°C for 12 hours to crystallize, and then pulverized through ball milling again to obtain Li having an argyrodite-type crystal structure. 5.5 PS 4.5 Cl 1.5 Particles were manufactured. All of the above processes were performed under an inert Ar atmosphere.

[0140]

[0141] Manufacturing Example 5

[0142] Three precursors, Li2S, P2S5, and LiBr, were dry mixed (ball milled) at a molar ratio of 2.5:0.5:1.0. During the dry mixing, a planetary ball mill equipped with zirconia balls was used, and the mixture was rotated at a speed of 300 rpm or higher to ensure uniform mixing. The obtained mixed precursor was then heat-treated at 400-550°C for 12 hours to crystallize, and then ball milled again to produce Li6PS5Br particles having an argyrodite-type crystal structure. All of the above processes were performed under an inert Ar atmosphere.

[0143]

[0144] Manufacturing Example 6

[0145] Three precursors, Li2S, P2S5, and LiCl, were dry mixed (ball milled) at a molar ratio of 2.5:0.5:1.0. During dry mixing, a planetary ball mill equipped with zirconia balls was used, and the mixture was rotated at a speed of 300 rpm or higher to ensure uniform mixing. The obtained mixed precursor was then heat-treated at 400-550°C for 12 hours to crystallize, and then ball milled again to pulverize the precursor to produce Li6PS5Cl particles having an argyrodite-type crystal structure. All of the above processes were performed under an inert Ar atmosphere.

[0146]

[0147] Examples and Comparative Examples

[0148] Example 1

[0149] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 1 5.4 PS 4.4 Cl 0.6 Br 1.0 Solid electrolyte A was prepared by exposing the particles to an atmosphere controlled at a dew point temperature of -30°C at room temperature for 5 hours and then vacuum drying at 80°C for 12 hours.

[0150]

[0151] Example 2

[0152] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 1 5.4 PS 4.4 Cl 0.6 Br 1.0 Solid electrolyte B was prepared by exposing the particles to an atmosphere controlled at a dew point temperature of -35°C at room temperature for 5 hours and then vacuum drying at 80°C for 12 hours.

[0153]

[0154] Example 3

[0155] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 1 5.4 PS 4.4 Cl 0.6 Br 1.0 Solid electrolyte C was prepared by exposing the particles to an atmosphere controlled at a dew point temperature of -25°C at room temperature for 5 hours and then vacuum drying at 80°C for 12 hours.

[0156]

[0157] Example 4

[0158] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 2 5.5 PS 4.5 Cl 0.5 Br 1.0 Solid electrolyte D was prepared by exposing the particles to an atmosphere controlled at a dew point temperature of -30°C for 5 hours and then vacuum drying at 80°C for 12 hours.

[0159]

[0160] Example 5

[0161] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 3 5.4 PS 4.4 Cl 1.0 Br 0.6 Solid electrolyte E was prepared by exposing the particles to an atmosphere controlled at a dew point temperature of -30°C at room temperature for 5 hours and then vacuum drying at 80°C for 12 hours.

[0162]

[0163] Example 6

[0164] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 4 5.5 PS 4.5 Cl 1.5 Solid electrolyte F was prepared by exposing the particles to an atmosphere controlled at a dew point temperature of -30°C at room temperature for 5 hours and then vacuum drying at 80°C for 12 hours.

[0165]

[0166] Comparative Example 1

[0167] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 1 5.4 PS 4.4 Cl 0.6 Br 1.0 was used as the solid electrolyte G of Comparative Example 1.

[0168]

[0169] Comparative Example 2

[0170] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 3 5.4 PS 4.4 Cl 1.0 Br 0.6 was used as the solid electrolyte H of Comparative Example 1.

[0171]

[0172] Comparative Example 3

[0173] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 1 5.4 PS 4.4 Cl 0.6 Br 1.0 Solid electrolyte I was prepared by exposing the particles to an atmosphere controlled at a dew point temperature of -40°C at room temperature for 5 hours and then vacuum drying at 80°C for 12 hours.

[0174]

[0175] Comparative Example 4

[0176] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 1 5.4PS 4.4 Cl 0.6 Br 1.0 The solid electrolyte J was prepared by exposing the particles to an atmosphere controlled at room temperature and a dew point temperature of 10°C for 3 hours and then vacuum drying at 80°C for 12 hours.

[0177]

[0178] Comparative Example 5

[0179] Li having an argyrodite-type crystal structure manufactured in the above manufacturing example 4 5.5 PS 4.5 Cl 1.5 was used as the solid electrolyte K of Comparative Example 10.

[0180]

[0181] Comparative Example 6

[0182] Li6PS5Br particles having an argyrodite-type crystal structure manufactured in the above Manufacturing Example 5 were exposed to an atmosphere controlled to a dew point temperature of -30°C at room temperature for 5 hours, and then left for 7 weeks without drying treatment to manufacture a solid electrolyte L.

[0183]

[0184] Comparative Example 7

[0185] The Li6PS5Cl particles having an argyrodite-type crystal structure manufactured in the above Manufacturing Example 6 were exposed to an atmosphere controlled to a dew point temperature of 10°C at room temperature for 3 hours, and then vacuum-dried at 80°C for 12 hours to manufacture a solid electrolyte M.

[0186]

[0187] Experimental example

[0188] Experimental Example 1: Crystal Structure Analysis

[0189] The crystal morphology of the solid electrolyte manufactured in Example 5 was observed using X-ray diffraction analysis (XRD). Figure 1 shows the XRD peaks of the solid electrolyte of Example 5.

[0190] Referring to Figure 1, it can be confirmed that the solid electrolyte of Example 5 has an argyrodite-type crystal structure.

[0191]

[0192] Experimental Example 2: Solid Electrolyte Surface Analysis

[0193] (1) NIR analysis

[0194] Measuring equipment: ABB MB3600

[0195] Spec:

[0196] - Covering Range: 3,700 to 14,885cm -1 range

[0197] - Interferometer Mechanism: High-throughput double pivot Michelson

[0198] - NIR Source: Quartz-halogen (Elec. Controlled)

[0199] - Lase Source: Solid-state Laser (Long lifetime)

[0200] - Optics materials: Completely non-Hygroscopic optics (ZnSe)

[0201] - TE cooled InGaAs detector

[0202]

[0203] Each solid electrolyte powder manufactured in the examples and comparative examples was placed in a glass vial, and then an FT-NIR diffuse reflectance accessory was installed to obtain the NIR reflection spectrum of the solid electrolyte in the glass vial (8 cm -1 resolution, 32 scans). 5300cm -1 , 4685cm -1After baseline correction, in the NIR spectra of each of the solid electrolytes A to M, 5200 cm -1 Height 4725cm -1 The integral value of the Li2CO3 band existing in the region was confirmed. Under the same conditions, 7230 cm -1 , 7120cm -1 After baseline correction, 7200cm -1 Height 7140cm -1 The LiOH band integral values ​​existing in the region were confirmed and are shown in Table 1 below.

[0204]

[0205] (2) XPS analysis

[0206] Measurement equipment: K-Alpha+ from ThermoFisher Scientific Inc.

[0207] Spec:

[0208] - X-ray source: monochromatic Al Kα (1486.6 eV)

[0209] - Operating mode: CAE (Constant Analyzer Energy) mode

[0210] - Software: Avantage software (version 5.992)

[0211] - X-ray spot size: 400㎛

[0212] - Charge compensation: default FG03 mode (100㎂, 0.5V)

[0213] - Pass energy: 50 eV

[0214]

[0215] A pellet-shaped sample was attached to a sample holder in an argon-atmosphere glove box. After capping the holder with a Vacuum Transfer Module (VTM) to prevent exposure to the atmosphere, it was placed in the instrument chamber. The region corresponding to a binding energy of 120 eV to 140 eV was scanned at an energy step of 0.1 eV.

[0216] After fitting the 2p spectrum peak of phosphorus (P) obtained by XPS analysis of each of the above solid electrolytes A to M, PS4 corresponding to the binding energy of 131.63 eV 3- PO corresponding to the peak area (A1) and position 132.85 eV x S 4-x 3- The peak area (A2) was obtained, and the A2 / (A1+A2) value was calculated and shown in Table 1 below. The peak fitting conditions were L / G ratio: 0.3, FWHM: 0.9~1.2 eV, and energy difference: 1.3±0.1 eV.

[0217] Figure 2 shows XPS data of the solid electrolytes of Examples 1 to 3 and Comparative Examples 3 and 6.

[0218] ClassificationNIRXPSLi2CO3 band integralLiOH band integralA2 / (A1+A2)Example 15.6300.029Example 23.3700.000Example 36.600.083Example 44.6800.029Example 56.4200.038Example 65.3400.048Comparative Example 11.2500.020Comparative Example 21.400.010Comparative Example 31.9600.000Comparative Example 440.31.6-Comparative Example 51.0400.014Comparative Example 68.6900.167Comparative Example 732.11.32-

[0219]

[0220] Experimental Example 3: Evaluation of the ionic conductivity of solid electrolytes

[0221] Each of the solid electrolyte powders of Examples 1 to 6 and Comparative Examples 1 to 7 was taken in an amount of 150 mg and placed into a SUS mold with a diameter of 13 mm. The mold was mounted on a press together with an insulating PEEK, and a potentiostat was connected to the SUS mold. After sufficiently densifying the electrolyte structure by pressurizing to 370 MPa, the pressure was slowly reduced to maintain it at 100 MPa, and AC impedance measurements were performed at a measurement frequency of 1 Hz to 7 MHz. The ionic conductivity (initial ionic conductivity) was calculated from the measured resistance values ​​through a Nyquist plot, and is shown in Table 2 below. All measurements were performed in a drying room at a temperature of 22°C and a relative humidity of 0.7%.

[0222] Each of the solid electrolyte powders manufactured in Examples 1 to 6 and Comparative Examples 1 to 3 and 5 was exposed to an atmosphere with a relative humidity of 1.91% for 5 hours, and then 150 mg each was placed into a SUS mold with a diameter of 13 mm. The mold was mounted on a press together with an insulating PEEK, and a potentiostat was connected to the SUS mold. After pressurizing to 370 MPa to sufficiently densify the electrolyte structure, the pressure was slowly lowered and maintained at 100 MPa, and AC impedance measurements were performed at a measurement frequency of 1 Hz to 7 MHz. The ionic conductivity after moisture exposure was calculated from the measured resistance value through a Nyquist plot, and the ionic conductivity retention rate was calculated according to the following Equation 1, which is shown in Table 2 below. All measurements were performed in a drying room at a temperature of 22°C and a relative humidity of 0.7%. Meanwhile, the solid electrolyte powders of Comparative Examples 4, 6, and 7 had such low initial ionic conductivity that the ionic conductivity retention rate was not evaluated.

[0223] [Formula 1]

[0224]

[0225] Classification Initial ionic conductivity (mS / cm) Ionic conductivity retention rate (%) Example 16.0051 Example 26.1752 Example 35.5449 Example 45.1458 Example 54.6659 Example 63.2455 Comparative example 16.7744 Comparative example 27.1833 Comparative example 36.4943 Comparative example 40.00013- Comparative example 55.4124 Comparative example 61.01- Comparative example 70.00022-

[0226] Referring to Table 1, the solid electrolytes of Examples 1 to 6 not only include a buffer layer comprising Li2CO3 formed on the particles, but also have a wavelength of 5200 cm in the NIR spectrum. -1 Height 4725cm -1 It can be confirmed that the Li2CO3 band integral value existing in the region is 2.0 or more and 8.0 or less.

[0227] Meanwhile, in the case of Comparative Examples 1, 2, and 5, which did not undergo surface treatment, it can be confirmed that no buffer layer exists on the solid electrolyte particles from the detection of the Li2CO3 band integral value corresponding to an impurity in the NIR spectrum. In addition, in the case of Comparative Example 3, it can be confirmed that almost no buffer layer exists on the solid electrolyte particles from the detection of the Li2CO3 band integral value corresponding to an impurity in the NIR spectrum. Accordingly, it can be seen that the solid electrolytes of Comparative Examples 1, 2, 3, and 5 do not maintain a stable phase during the battery manufacturing process, and there is a problem of deteriorating the performance of the battery.

[0228] And, in the case of comparative example 6, which was left without drying treatment (no removal of moisture adsorbed on the surface) after surface treatment, phase decomposition occurred due to changes over time, and in the NIR spectrum, 5200 cm -1 Height 4725cm -1 The Li2CO3 band integral value existing in the region exceeds 8.0, and PO measured by XPS x S 4-x 3-It can be seen that the binding peak increases. Accordingly, there is a problem of low ionic conductivity.

[0229] And, in the case of comparative examples 4 and 7, a buffer layer is formed, but not only is it formed too much, but an excessive amount of argyrodite decomposition phase is generated, so that in the NIR spectrum, 5200 cm -1 Height 4725cm -1 There is a problem that the Li2CO3 band integral value existing in the region is much larger than 8.0 and the ionic conductivity is low.

[0230]

[0231] Experimental Example 4: Rate Evaluation of All-Solid-State Batteries

[0232] LiNi as positive electrode active material 0.8 Co 0.1 Mn 0.1 O2 was prepared as a solid electrolyte, the solid electrolytes of each of Example 1 and Comparative Example 1, and carbon nanofibers (CNF) as a conductive material, and then mixed in a weight ratio of positive electrode active material: solid electrolyte: conductive material = 60:35:5 to prepare a positive electrode composition. The positive electrode composition was placed on a solid electrolyte filled in a load cell with a diameter of 13 mm at a density of 3 mAh / cm. 2 The positive electrode was manufactured by uniformly distributing the loading amount. Afterwards, the screw was fastened while the load cell was pressurized using a flat press. The measured pressing force of the load cell was 35 MPa. Lithium metal with a thickness of 100 μm was used as the negative electrode, and a load cell (all-solid-state battery) with a negative electrode / solid electrolyte / positive electrode structure was manufactured.

[0233] The manufactured all-solid-state battery was charged to an upper limit voltage of 4.25 V in constant current / constant voltage (CC / CV) mode at a rate of 0.05 C while maintaining a temperature of 60°C, and then discharged to a final voltage of 3 V at 0.05 C in CC mode to perform an initial two-cycle charge / discharge. Thereafter, charging was performed at a rate of 0.1 C, and discharge was performed at rates of 0.1 C, 0.2 C, 0.33 C, 0.5 C, 1.0 C, and 0.1 C in steps to evaluate the rate characteristics, and the results are shown in Fig. 3.

[0234] Figure 3 shows rate characteristic evaluation data of an all-solid-state battery including the solid electrolytes of Example 1 and Comparative Example 1.

[0235] Referring to FIG. 3, in the case of an all-solid-state battery including the solid electrolyte of Example 1 according to the present invention, 5200 cm in the NIR spectrum -1 Height 4725cm -1 It can be confirmed that the rate characteristics are superior to those of the all-solid-state battery including the solid electrolyte of Comparative Example 1, in which the Li2CO3 band integral value existing in the region is less than 0.2.

[0236]

[0237] In conclusion, the solid electrolyte according to the present invention not only includes a buffer layer containing Li2CO3 formed on particles, but also has a NIR spectrum of 5200 cm -1 Height 4725cm -1 It can be seen that the Li2CO3 band integral value existing in the region satisfies the requirement of 2.0 or more and 8.0 or less, so that a stable phase is maintained when exposed to moisture in the battery manufacturing process, and the interfacial side reaction between the solid electrolyte and the electrode material can be suppressed, thereby improving the battery characteristics.

Claims

1. Sulfide-based solid electrolyte particles; and A buffer layer including Li2CO3 formed on the above sulfide-based solid electrolyte particles; In the NIR spectrum, 5200 cm -1 Height 4725cm -1 A solid electrolyte having a Li2CO3 band integral value of 2.0 or more and 8.0 or less in the region.

2. In claim 1, The above sulfide-based solid electrolyte is a solid electrolyte having an argyrodite-type crystal structure.

3. In claim 1, The above sulfide-based solid electrolyte is a solid electrolyte having a composition represented by the following chemical formula 1: [Chemical Formula 1] Li a (P 1-b M b )S 6-c X c In the above chemical formula 1, M is at least one selected from Sb, Sn, Ge, Si, Nb, Ni, Ga, and Al, X is one or more selected from F, Cl, Br, and I, 5.0 <a<7.5, 0≤b≤0.7, 0<c≤2.0이다.

4. In claim 1, A solid electrolyte having an ionic conductivity of 3 mS / cm to 12 mS / cm.

5. In claim 1, In the NIR spectrum, 7200 cm -1 7140cm in height -1 A solid electrolyte having a LiOH band integral value of less than 0.1 in the region.

6. In claim 1, In the 2p spectrum of P obtained by XPS analysis, PS4 3- Peak area (A1) and PO x S 4-x 3- PO for the sum of peak areas (A2) x S 4-x 3- A solid electrolyte having a ratio of peak areas (A2) (A2 / (A1+A2)) of less than 0.

1.

7. An all-solid-state battery comprising a solid electrolyte according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Sulfide solid electrolyte with core-shell structure, preparation method and solid battery

    CN110459798A

  • Device for measuring an anaerobic exercise amount

    KR1020210046447A

  • Sulfide solid electrolyte particles, method for producing the same, and all-solid-state battery

    US20200235423A1

  • Method for producing sulfide solid electrolyte

    WO2022186156A1

  • KR20230042176A