Magnetocaloric alloy having wide phase transition temperature range, and manufacturing method therefor
The development of a magnetocaloric alloy with specific composition and manufacturing process expands its phase transition temperature range and refrigeration capacity, addressing the limitations of general magnetocaloric alloys and improving magnetic cooling system efficiency.
Patent Information
- Application Number
- PCT/KR2024/004041
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
General magnetocaloric alloys exhibit a narrow usable temperature range and refrigeration capacity due to rapid decreases in magnetocaloric characteristics with changes in system temperature, limiting their application in thermomagnetic devices and refrigeration systems.
A magnetocaloric alloy with the composition MnFe0.95-xNi xP0.6-ySi0.4+y, where x is between 0.01 and 0.05, and y is between -0.05 and 0.05, is developed, which is manufactured through an arc melting process followed by heat-treatment in a vacuum, enhancing the alloy's phase transition temperature range and refrigeration capacity.
The alloy achieves a wider phase transition temperature range and improved refrigeration capacity, enabling more efficient magnetic cooling systems with enhanced usability and productivity compared to conventional methods.
Smart Images

Figure KR2024004041_03102024_PF_FP_ABST
Abstract
Description
Magnetocaloric alloy having a wide phase transition temperature range and method for manufacturing the same
[0001] This specification claims the benefit of Korean Patent Application No. 10-2023-0041036, filed with the Korean Intellectual Property Office on March 29, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a magnetocaloric alloy having a wide phase transition temperature range and a method for manufacturing the same.
[0003] Magnetocaloric alloys are materials that utilize the magnetocaloric effect (MCE), which heats when magnetized and cools when demagnetized, to provide cooling without gaseous refrigerants such as CFCs (chlorofluorocarbons) used in existing refrigerators and air conditioners, and are environmentally friendly and exhibit high energy efficiency.
[0004] Systems utilizing the magnetocaloric effect can range from thermomagnetic devices, which convert thermal energy into magnetic work, to heat pumps, where magnetic work is used to transfer thermal energy from a low-temperature source to a high-temperature sink (or vice versa). Typical applications include thermomagnetic, thermoelectric, and thermomagnetic generators, magnetic refrigerators, heat exchangers, heat pumps, and air conditioning systems.
[0005] The operating method of a system utilizing the magnetocaloric effect is a repetitive process in which the temperature of the system changes due to the magnetocaloric effect of the magnetocaloric alloy in response to a change in the magnetic field, and then the temperature of the system changes due to the magnetocaloric effect of the magnetocaloric alloy in response to a change in the magnetic field at the changed temperature. Therefore, the wider the magnetocaloric properties of the magnetocaloric alloy over a wide temperature range, the more advantageous it is.
[0006] However, as shown in Fig. 1, typical magnetocaloric alloys exhibit a rapid decline in magnetocaloric properties as system temperature changes, resulting in a narrow usable temperature range. Therefore, there is a need for magnetocaloric alloys with improved usable temperature range and refrigeration capacity.
[0007] The problem to be solved by the present invention is to provide a magnetocaloric alloy with improved usable temperature range and refrigeration capacity by controlling the composition of the magnetocaloric alloy.
[0008] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0009] According to one aspect of the present invention, the chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+y A magnetocaloric alloy having a composition of, in the chemical formula, x is 0.01 or more and 0.05 or less, and y is -0.05 or more and less than 0.05 is provided.
[0010] In addition, according to another aspect of the present invention, there is provided a method for manufacturing a magnetocaloric alloy, comprising the steps of: manufacturing an alloy ingot by arc-melting Mn, Fe, Ni, P and Si raw materials; and heat-treating the alloy ingot in a vacuum; wherein the magnetocaloric alloy has the chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+y The present invention provides a method for manufacturing a magnetocaloric alloy having a composition of, in the chemical formula, x is 0.01 or more and 0.05 or less, and y is -0.05 or more and less than 0.05.
[0011] A magnetocaloric alloy according to one embodiment of the present invention can provide a magnetocaloric alloy with improved usable temperature range and refrigeration capacity.
[0012] The effects of the present invention are not limited to the effects described above, and effects not mentioned will be clearly understood by those skilled in the art from the specification herein.
[0013] Figure 1 shows a ΔS-T graph of a typical magnetocaloric alloy.
[0014] Figure 2 shows a ΔS-T graph of a magnetocaloric alloy showing a tabletop-shaped graph trend.
[0015] Figure 3a shows the MT graph of the magnetocaloric alloy of Example 1.
[0016] Figure 3b shows the MT graph of the magnetocaloric alloy of Example 2.
[0017] Figure 3c shows the MT graph of the magnetocaloric alloy of Example 3-1.
[0018] Figure 4 shows the MH graph of the magnetocaloric alloy of Example 3-1.
[0019] Figure 5 shows a ΔS-T graph of the magnetocaloric alloy of Example 3-1.
[0020] Figure 6 shows the ΔS-T graphs during cooling and heating of the magnetocaloric alloys of Examples 1, 2, and 3-1.
[0021] Figure 7 shows the ΔS-T graph of the magnetocaloric alloys of Examples 3-1 to 3-3 in a 1T or 2T magnetic field.
[0022] Figure 8 shows the ΔS-T graph of the magnetocaloric alloys of Example 3-1 and Comparative Example 1 in a 2T magnetic field.
[0023] Figure 9 shows the XRD pattern according to temperature of Example 3-1.
[0024] Figure 10 shows the XRD pattern according to temperature of Comparative Example 1.
[0025] When a part in this specification is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0026] Throughout this specification, the unit “parts by weight” or “wt%” means the weight ratio between each component.
[0027] Throughout this specification, “thermal hysteresis change (ΔT thermal hysteresis , ΔT hys ) refers to the temperature difference between the heating curve and the cooling curve in the MT graph.
[0028] Throughout the specification, “Refrigeration Capacity (RC)” means the ability of a magnetocaloric alloy to supply or remove heat according to a change in a magnetic field, and can be specifically obtained using the following mathematical expression 1.
[0029] [Mathematical Formula 1]
[0030]
[0031] In the above mathematical expression 1, RC is the refrigeration capacity, ΔS is the change in magnetic entropy, and T hot and T cold are the half-widths of the maximum change in self-entropy (T FWHM ) means the highest and lowest temperatures.
[0032] Throughout this specification, “Maxwell’s equations” means the following mathematical equation 2, and the ΔS-T graph can be derived from the MH graph using Maxwell’s equations.
[0033] [Equation 2]
[0034]
[0035] In the above mathematical expression 2, ΔS mwhere T represents temperature, H represents magnetic field, and M represents magnetization.
[0036] Throughout the present specification, “tabletop” means a graph that exhibits a tabletop-shaped trend in the ΔS-T graph as in Fig. 2, and a magnetocaloric alloy exhibiting a tabletop-shaped graph trend can have a wide phase transition temperature range. In addition, compared to the general magnetocaloric alloy of Fig. 1, the maximum magnetic entropy change value (│ΔS max │) half-width (T FWHM ) values can be larger, and the available temperature range and refrigeration capacity can be improved.
[0037] Hereinafter, the present invention will be described in more detail.
[0038] One embodiment of the present invention is a chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+y A magnetocaloric alloy having a composition of, in the chemical formula, x is 0.01 or more and 0.05 or less, and y is -0.05 or more and less than 0.05 is provided.
[0039] The above magnetocaloric alloy is a quintuple magnetocaloric alloy containing Mn (manganese), Fe (iron), Ni (nickel), P (phosphorus), and Si (silicon). Since it has a wide phase transition temperature range by adjusting the contents of Fe, Ni, P, and Si within an appropriate range, the usable temperature range and refrigeration capacity can be improved. Therefore, the magnetocaloric alloy can improve the efficiency of a magnetic refrigeration system.
[0040] According to one embodiment of the present invention, the magnetocaloric alloy has the chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+yIt has a composition of. At this time, the x is 0.01 or more and 0.05 or less, and specifically, it may be 0.01 or more and 0.05 or less, 0.01 or more and 0.045 or less, 0.01 or more and 0.04 or less, 0.015 or more and 0.045 or less, 0.015 or more and 0.04 or less, 0.02 or more and 0.045 or less, or 0.02 or more and 0.04 or less. When the range of the x is within the above-mentioned range, the magnetocaloric alloy has a wide phase transition temperature range, so that the usable temperature range and the refrigeration capacity can be improved.
[0041] Also, the chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+y In , y is -0.05 or more and less than 0.05, and specifically, -0.05 or more and less than 0.05, -0.04 or more and 0.04 or less, -0.03 or more and 0.03 or less, -0.025 or more and 0.025 or less, -0.02 or more and 0.02 or less, -0.01 or more and 0.01 or less, or 0. When the range of y is within the above-mentioned range, the magnetocaloric alloy has a wide phase transition temperature range, so that the usable temperature range and the refrigeration capacity can be improved.
[0042] According to one embodiment of the present invention, the magnetocaloric alloy may have a Curie temperature of 245 K to 290 K when heated. Specifically, the magnetocaloric alloy may have a Curie temperature of 245 K to 290 K, 245 K to 285 K, 245 K to 280 K, 245 K to 275 K, or 245 K to 270 K when heated. At this time, the Curie temperature of the magnetocaloric alloy is the maximum value of the entropy change. ( │ΔS max │ ) The Curie temperature (T) at this peak appears c) and may be measured under an external magnetic field of 2 T. The heating may be from 100 K to 375 K, and may vary depending on the magnetocaloric alloy being measured.
[0043] According to one embodiment of the present invention, the magnetocaloric alloy may have a Curie temperature of 190 K to 240 K when cooled. Specifically, the magnetocaloric alloy may have a Curie temperature of 190 K to 240 K, 195 K to 240 K, 200 K to 240 K, 205 K to 240 K, 210 K to 240 K, 215 K to 240 K, or 220 K to 240 K when cooled, and may be measured under an externally applied magnetic field of 2 T. The cooling may be heating from 375 K to 100 K, and may vary depending on the magnetocaloric alloy being measured.
[0044] In addition, a typical magnetocaloric alloy having a narrow phase transition temperature range shows one peak in a graph that differentiates the MT graph (dM / dT-T graph), and the graphs overlap when heated and cooled, but the magnetocaloric alloy having a wide phase transition temperature range according to the present invention shows more than one peak in the dM / dT-T graph, and the dM / dT-T graphs may be different when heated and cooled. Therefore, the magnetocaloric alloy having a wide phase transition temperature range according to the present invention may have different Curie temperatures when heated or cooled.
[0045] Specifically, the magnetocaloric alloy having a wide phase transition temperature range according to the present invention exhibits a magnetocaloric effect due to a structural phase transition in which a change in the positions of atoms occurs while maintaining the same hexagonal structure at the Curie temperature, and is accompanied by a change in volume due to a change in the lattice constant. In this case, the graphs may differ during heating and cooling due to the difference in the heating process in which volume expansion occurs and the cooling process in which a transition occurs due to volume contraction.
[0046] In addition, in the case of a magnetocaloric alloy that shows multiple peaks in the dM / dT-T graph, the phase transition occurs over a wide temperature range due to the characteristic of coexistence of more than one phase with different phase transition temperatures, as shown in the XRD pattern of Fig. 9, and a table-top graph trend can be shown in the ΔS-T graph.
[0047] According to one embodiment of the present invention, the magnetocaloric alloy may have a refrigeration capacity of 150 J / kg to 250 J / kg in a 2T magnetic field. Specifically, the refrigeration capacity may be 150 J / kg to 250 J / kg, 150 J / kg to 240 J / kg, 150 J / kg to 230 J / kg, 150 J / kg to 220 J / kg, 150 J / kg to 215 J / kg, 160 J / kg to 250 J / kg, 160 J / kg to 240 J / kg, 160 J / kg to 230 J / kg, 160 J / kg to 220 J / kg, or 160 J / kg to 215 J / kg. When the refrigeration capacity of the above magnetocaloric alloy is within the above-mentioned range, products and systems to which magnetic cooling technology can be applied can operate effectively.
[0048] According to one embodiment of the present invention, the magnetocaloric alloy has a maximum value (│ΔS) of magnetic entropy change in a 2T magnetic field. max │) may be 3 J / kg·K to 13 J / kg·K. Specifically, the maximum value of the magnetic entropy change may be 3 J / kg·K to 13 J / kg·K, 3 J / kg·K to 12 J / kg·K, 3 J / kg·K to 11 J / kg·K, or 3 J / kg·K to 10 J / kg·K.
[0049] In addition, the maximum value of the magnetic entropy change may be different during heating and cooling. Specifically, the maximum value of the magnetic entropy change during heating may be 6 J / kg·K to 13 J / kg·K, 6 J / kg·K to 12 J / kg·K, 6 J / kg·K to 11 J / kg·K, 6 J / kg·K to 10 J / kg·K, 7 J / kg·K to 13 J / kg·K, 7 J / kg·K to 12 J / kg·K, 7 J / kg·K to 11 J / kg·K, 7 J / kg·K to 10 J / kg·K, 8 J / kg·K to 13 J / kg·K, 8 J / kg·K to 12 J / kg·K, 8 J / kg·K to 11 J / kg·K, or 8 J / kg·K to 10 J / kg·K. Furthermore, the maximum value of the magnetic entropy change during cooling may be 3 J / kg·K to 6 J / kg·K, 3 J / kg·K to 5.5 J / kg·K, 3 J / kg·K to 5 J / kg·K, 3 J / kg·K to 4.5 J / kg·K, or 3 J / kg·K to 4 J / kg·K. When the maximum value of the magnetic entropy change during heating or cooling is within the above-mentioned range, the refrigeration capacity may be excellent.
[0050] According to one embodiment of the present invention, the magnetocaloric alloy has a half-width (T) of the maximum value of the magnetic entropy change in a 2T magnetic field. FWHM ) may be 10 K to 100 K. Specifically, the half-width of the maximum magnetic entropy change amount may be 10 K to 100 K, 10 K to 90 K, 10 K to 80 K, 10 K to 70 K, 10 K to 65 K, 15 K to 100 K, 15 K to 95 K, 15 K to 85 K, 15 K to 75 K, 15 K to 65 K, 20 K to 100 K, 20 K to 90 K, 20 K to 80 K, 20 K to 70 K, or 20 K to 65 K.
[0051] In addition, the half-width of the maximum magnetic entropy change amount may be different during heating and cooling. Specifically, the half-width of the maximum magnetic entropy change amount during heating may be 10 K to 50 K, 10 K to 45 K, 10 K to 40 K, 10 K to 35 K, 10 K to 30 K, 15 K to 50 K, 15 K to 45 K, 15 K to 40 K, 15 K to 35 K, 15 K to 30 K, 20 K to 50 K, 20 K to 45 K, 20 K to 40 K, 20 K to 35 K, or 20 K to 30 K. Furthermore, the half-width of the maximum magnetic entropy change amount during cooling may be 50 K to 100 K, 50 K to 90 K, 50 K to 80 K, 50 K to 70 K, 50 K to 65 K, 55 K to 100 K, 55 K to 95 K, 55 K to 85 K, 55 K to 75 K, or 55 K to 65 K. When the half-width of the maximum magnetic entropy change amount during heating or cooling is within the above-mentioned range, the available temperature range and the refrigeration capacity may be improved.
[0052] One embodiment of the present invention is a method for manufacturing a magnetocaloric alloy, including the steps of manufacturing an alloy ingot by arc-melting raw materials of Mn, Fe, Ni, P and Si; and the step of heat-treating the alloy ingot in a vacuum; wherein the magnetocaloric alloy has the chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+y The present invention provides a method for manufacturing a magnetocaloric alloy having a composition of, in the chemical formula, x is 0.01 or more and 0.05 or less, and y is -0.05 or more and less than 0.05.
[0053] The above method for manufacturing a magnetocaloric alloy can easily manufacture a magnetocaloric alloy having a uniform composition and excellent usable temperature range and refrigeration capacity.
[0054] Previously, when manufacturing the magnetocaloric alloy MnFePSi, P had a significantly lower boiling point than other elements and was hazardous, so a solid-state reaction synthesis method using Fe powder, Mn powder, Si powder, and red phosphorus (Red P) powder was used. However, the metal powders were highly susceptible to oxidation, and red phosphorus also had flammability and hazardous properties, requiring the entire manufacturing process to be performed in a glove box. Consequently, the conventional method had problems such as high process costs, compositional imbalances in the manufactured alloy, and low productivity.
[0055] On the other hand, the method for manufacturing a magnetocaloric alloy according to one embodiment of the present invention can simplify the manufacturing process through an arc-melting process, compared to a conventional solid-state reaction synthesis method, can effectively homogenize the composition of the magnetocaloric alloy manufactured, and can realize high productivity according to the melting process.
[0056] The above Mn, Fe, Ni, P and Si raw materials can be used in the form of Mn-based, Fe-based, Ni-based, Si-based and Fe-P-based chips or bulk pieces. Using the Mn, Fe, Ni, P and Si raw materials in the form of chips or bulk pieces can effectively prevent the raw materials from being oxidized and increase the productivity of the magnetocaloric alloy.
[0057] In addition, the above Mn, Fe, Ni, P and Si raw materials are MnFe 0.95-x Ni x P 0.6-y Si 0.4+y It is weighed and used so that an ingot having the composition of MnFe can be manufactured, and ultimately 0.95-x Ni x P 0.6-y Si 0.4+y A magnetocaloric alloy having the composition of can be manufactured.
[0058] The above Mn-based raw material may further include a step of removing an oxide film. Specifically, the oxide film of the Mn-based chip may be removed using an acid, and the acid may include one or more of nitric acid, sulfuric acid, phosphoric acid, and hydrochloric acid. By performing the step of removing the oxide film of the Mn-based raw material, the inclusion of impurities in the magnetocaloric alloy can be effectively suppressed.
[0059] According to one embodiment of the present invention, the step of manufacturing an alloy ingot by arc melting includes a first arc melting step of arc melting the raw material under a first current condition; and a second arc melting step of arc melting the alloy ingot formed by the first arc melting under a second current condition; wherein the second arc melting step may be performed under a higher current condition than the first arc melting step.
[0060] In the step of manufacturing an alloy ingot by arc melting, by first performing a first arc melting step with low current conditions and sequentially performing a second arc melting step with higher current conditions, it is possible to effectively suppress the loss of phosphorus (P) during the manufacturing of a magnetocaloric alloy, and to effectively manufacture a magnetocaloric alloy having a homogeneous composition.
[0061] The step of manufacturing an alloy ingot by arc melting may further include, between the first arc melting step and the second arc melting step, a step of cooling the alloy ingot formed by the first arc melting; and a step of preparing the second arc melting step by reversing the vertical position of the cooled alloy ingot. Specifically, after manufacturing an alloy ingot by arc melting the raw material mixture under a first current condition, the alloy ingot may be cooled. The alloy ingot may be cooled under room temperature or cold water conditions. Thereafter, after reversing the vertical position of the cooled alloy ingot, arc melting may be performed under a second current condition. That is, the upper side of the first arc melted alloy ingot may be positioned lower in the second arc melting step, and the lower side of the first arc melted alloy ingot may be positioned upper in the second arc melting step. By cooling the alloy ingot and changing the upper and lower positions of the alloy ingot between the first and second arc melting steps, the composition of the magnetocaloric alloy produced can be made more homogeneous.
[0062] According to one embodiment of the present invention, the first current condition may be 40 A to 50 A, and the second current condition may be 70 A to 80 A.
[0063] According to one embodiment of the present invention, the current ratio of the first current condition and the second current condition may be 1:1.4 to 1:2.0. Specifically, the current ratio of the first current condition and the second current condition may be 1:1.4 to 1:2.0, 1:1.4 to 1:1.8, 1:1.4 to 1:1.6, 1:1.4 to 1:1.5, 1:1.5 to 1:2.0, 1:1.5 to 1:1.9, 1:1.5 to 1:1.7, or 1:1.5 to 1:1.6. By controlling the current ratio of the first current condition applied in the first arc melting step and the second current condition applied in the second arc melting step within the aforementioned range, loss of phosphorus (P) during the manufacturing process of the magnetocaloric alloy can be effectively suppressed, and a magnetocaloric alloy having a homogeneous composition and a desired composition can be effectively manufactured.
[0064] The step of manufacturing an alloy ingot by arc melting may be performed repeatedly two or more times. Specifically, the arc melting step including the first arc melting step and the second arc melting step may be performed two or more times, three or more times, or four or more times. By repeatedly performing the step of manufacturing an alloy ingot by arc melting within the above-described range, the manufactured magnetocaloric alloy can be effectively homogenized.
[0065] The above heat treatment step may be performed at a temperature of 1200 K or more and 1600 K or less. Specifically, the temperature at which the heat treatment step is performed may be 1200 K or more and 1600 K or less, 1200 K or more and 1500 K or less, 1200 K or more and 1450 K or less, 1300 K or more and 1600 K or less, 1300 K or more and 1500 K or less, 1300 K or more and 1450 K or less, 1400 K or more and 1600 K or less, 1400 K or more and 1500 K or less, or 1400 K or more and 1450 K or less. In addition, the heat treatment step may be performed for 72 hours to 120 hours. By controlling the temperature and time of the heat treatment step within the above-mentioned range, the manufactured magnetocaloric alloy can be effectively homogenized.
[0066] According to one embodiment of the present invention, after the step of heat-treating the alloy ingot in a vacuum, the method may further include a step of rapidly cooling the heat-treated alloy ingot. The method of rapidly cooling may use any method used in the art without limitation, and for example, rapid cooling may be performed using cold water of 5°C to 20°C. By performing the rapid cooling step, the phase stability of the magnetocaloric alloy can be secured, and defects such as pores or dislocations that may exist inside can be reduced, thereby improving the magnetocaloric properties of the magnetocaloric alloy.
[0067] Matters mentioned in the magnetocaloric alloy and the method for manufacturing the magnetocaloric alloy of the present invention are equally applicable unless they are contradictory.
[0068] Hereinafter, the present invention will be described in detail with examples and experimental examples to specifically explain the present invention. However, the examples and experimental examples according to the present invention may be modified in various different forms, and the scope of the present invention is not construed as being limited to the examples and experimental examples described below. The examples and experimental examples in this specification are provided to more fully explain the present invention to those of average skill in the art.
[0069] Example 1. Preparation of magnetocaloric alloy
[0070] As raw materials, Fe chips (>99.95 wt%), Mn chips (>99.9 wt%), Ni bulk pieces (>99.99 wt%), Si bulk pieces (>99.999 wt%), and Fe-P bulk pieces (>99.9 wt%) were prepared. At this time, the Mn chips were treated with nitric acid to remove the oxide film and then used.
[0071] Afterwards, Fe chips, Mn chips, Ni bulk pieces, Si bulk pieces and Fe-P bulk pieces were prepared, with the chemical formula MnFe 0.94 Ni 0.01 P 0.6 Si 0.4 The raw material mixture was prepared by weighing so that an ingot having the composition of could be manufactured.
[0072] Thereafter, the raw material mixture was placed in an arc melting device (arc suction melting system), and a first arc melting step was performed for 1 minute under current conditions of 40 A to 50 A to form an alloy ingot. Thereafter, the alloy ingot was cooled to room temperature, changed in vertical position, and placed again in the arc melting device. Thereafter, a second arc melting step was performed for 1 minute under current conditions of 70 A to 80 A. In order to secure the uniformity of the alloy ingot, the above-described method was repeated 3 times, and a total of 4 arc melting steps (first arc melting step + second arc melting step) were performed.
[0073] Afterwards, the alloy ingot was sealed in a quartz glass tube under a vacuum atmosphere, and 1×10 -2 Heat treatment under the conditions of Torr vacuum and 1150 ℃ (1423 K) for 96 hours, and then rapidly cooled with cold water (20 ℃, MnFe 0.93 Ni 0.02 P 0.6 Si 0.4 A magnetocaloric alloy having the composition of was manufactured.
[0074] Examples 2 to 3-3 and Comparative Example 1
[0075] Magnetocaloric alloys of Examples 2 to 3-3 and Comparative Example 1 were manufactured in the same manner as in Example 1, except that a raw material mixture was prepared so that a magnetocaloric alloy having a composition as shown in Table 1 below could be manufactured.
[0076] Example 1: Composition of a magnetocaloric alloy MnFe 0.93 Ni 0.02 P 0.6 Si 0.4 Example 2MnFe 0.92 Ni 0.03 P 0.6 Si 0.4 Example 3-1MnFe 0.91 Ni 0.04 P 0.6 Si 0.4 Example 3-2MnFe 0.91 Ni 0.04 P 0.6 Si 0.4 Example 3-3MnFe 0.91 Ni 0.04 P 0.6 Si 0.4 Comparative Example 1MnFe 0.91 Ni 0.04 P 0.5 Si 0.5
[0077] Experimental Example 1. MT Graph
[0078] The temperature of the magnetocaloric alloys of Examples 1 to 3-1 was increased to 350 K to 375 K, and then an external magnetic field of 1 T was applied. While the magnetic field was applied, the temperature was decreased to 100 K to 150 K (first cooling) and the magnetic moment (emu) of the magnetocaloric alloy was measured, and then the temperature was increased (first heating) and the magnetic moment of the magnetocaloric alloy was measured. After that, the temperature was decreased once again (second cooling) and the magnetic moment (emu) of the magnetocaloric alloy was measured. The measured magnetic moment was divided by the weight of the sample to calculate the magnetization (magnetization, emu / g), and the magnetization-temperature (MT) graph according to the temperature and the differentiated graph of the MT graph (dM / dT-T graph) are shown in FIGS. 3a to 3c.
[0079] In the case of a general magnetocaloric alloy, the graph in which the MT graph is differentiated shows one peak, but as shown in FIGS. 3a to 3c, the graphs in which the MT graphs of the magnetocaloric alloys of Examples 1 to 3-1 are differentiated all show two peaks, and it was confirmed that the graphs are different during heating and cooling.
[0080] Experimental Example 2. MH Graph
[0081] For the magnetocaloric alloy samples of Example 3-1 above, the temperature was fixed at 210 K, and the magnetic field was varied from 20000 Oe to 0 Oe, while measuring the magnetic moment of each sample. Subsequently, the same measurement was repeated while increasing the temperature by 2 K or 5 K increments until the final temperature was 290 K. Then, the measured magnetic moment was divided by the weight of the sample to calculate the magnetization (emu / g), and the magnetization-applied field (MH) graph according to the magnetic field is shown in Fig. 4.
[0082] Referring to Fig. 4, it was confirmed that the MH curve of Example 3-1 has the characteristics of ferromagnetism in which the magnetization value increases rapidly and saturates in a weak magnetic field when the temperature is lower than the Curie temperature. In addition, it was confirmed that the magnetization value increases gradually as the magnetic field increases at a temperature higher than the Curie temperature.
[0083] Experimental Example 3. ΔS-T Graph
[0084] Based on the MH graph obtained in the above Experimental Example 2, a graph (ΔS-T) of the change in entropy according to temperature of the magnetocaloric alloy of Example 3-1 was shown in Fig. 5 using Maxwell's equations.
[0085] In addition, the graphs (ΔS-T) of the entropy change amount according to temperature of the magnetocaloric alloys of Examples 1, 2, 3-2, 3-3 and Comparative Example 1 were obtained in the same manner as in Experimental Examples 2 and 3, and the results are shown in Figs. 5 to 8. Furthermore, T from Figs. 5 to 8 pk , │ΔS max │, T FWHM And the RC values were obtained and shown in Tables 2 and 3.
[0086] Heating T pk (K) @2T│ΔS max │(J / kg·K) @2TT FWHM (K) @2TRC(J / kg) @2TExample 12819.2022.0168.6Example 2264 / 2829.63 / 6.9627.6210.8Example 3-1256 / 2688.09 / 7.7630.0183.0Example 3-2254 / 2668.59 / 7.8026.9198.5Example 3-3248 / 2649.36 / 6.0227.6191.5Comparative Example 130412.6815.4152.9T pk (K) @1T│ΔS max │(J / kg·K) @1TT FWHM(K) @1TRC(J / kg) @1TExample 12813.9321.972.2Example 2264 / 2824.30 / 3.2329.196.1Example 3-1256 / 2683.46 / 3.4326.178.9Example 3-2254 / 2663.75 / 3.5327.488.7Example 3-3248 / 2644.05 / 2.7327.984.6Comparative Example 13045.7115.368.5
[0087] Cooling T pk (K) @2T│ΔS max │(J / kg·K) @2TT FWHM (K) @2TRC(J / kg) @2TExample 12383.9460.1205.0Example 2202 / 2323.89 / 3.9564.6218.1Example 3-1191 / 2233.40 / 3.5261.1201.5
[0088] Figure 5 shows the ΔS-T graph of the magnetocaloric alloy of Example 3-1. Referring to Figure 5 and Table 2, ΔS varies depending on the magnetic field. max Although there is a difference in the size of the magnetocaloric alloy of Example 3-1, the graph shows a table-top shape trend, and T FWHM It was confirmed that the value was large. Figure 6 shows the ΔS-T graph during cooling and heating of the magnetocaloric alloys of Examples 1, 2 and 3-1. Looking at Figure 6, Tables 2 and 3, all of the magnetocaloric alloys of Examples 1, 2 and 3-1 showed a table-top shaped graph trend, and T FWHM It was confirmed that the value was large. In addition, the table-top shape trend was more clearly observed in the graph when cooling than when heating, and T FWHM I confirmed that the value was larger.
[0089] Figure 7 shows the ΔS-T graphs of magnetocaloric alloys of Examples 3-1 to 3-3 in a 1T or 2T magnetic field. Referring to Figure 7 and Table 2, MnFe 0.91 Ni 0.04 P 0.6 Si 0.4In the magnetocaloric alloy reproduction experiment of the composition, all examples 3-1 to 3-3 showed a table-top shape graph trend, and T FWHM It was confirmed that the values showed the same trend.
[0090] Figure 8 shows the ΔS-T graph of the magnetocaloric alloys of Example 3-1 and Comparative Example 1 in a 2T magnetic field. Referring to Figure 8 and Table 2, MnFe 0.91 Ni 0.04 P 0.6 Si 0.4 The magnetocaloric alloy of Example 3-1 having the composition T FWHM The values are large and show a table-top graph trend, but MnFe 0.91 Ni 0.04 P 0.5 Si 0.5 The magnetocaloric alloy of comparative example 1 having the composition T FWHM We confirmed that the values are small and do not show a tabletop-shaped graph trend.
[0091] Experimental Example 4. XRD Pattern Analysis
[0092] X-ray diffraction analysis was performed on the magnetocaloric alloys of Example 3-1 and Comparative Example 1 to obtain XRD patterns, and the results are shown in FIGS. 9 and 10.
[0093] Figure 9 shows the XRD pattern of Example 3-1. Looking at Figure 9, it was confirmed that the phase transition does not occur immediately at 160 K to 200 K, and that there is a mixed area where the Fe2P-type paramagnetic peak and the Fe2P-type ferromagnetic peak exist together, so that it has a wide phase transition temperature range.
[0094] Figure 10 shows the XRD pattern of Comparative Example 1. As shown in Figure 10, the phase transition occurs immediately in the 304 K region, and since there is no region where the Fe2P-type paramagnetic peak and the Fe2P-type ferromagnetic peak exist mixed, it was confirmed that there is a narrow phase transition temperature range.
[0095] Although the present invention has been described above through limited embodiments, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical idea of the present invention and the equivalent scope of the patent claims to be described below by a person having ordinary skill in the art to which the present invention pertains.
Claims
1. Chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+y With the composition of In the above chemical formula, x is greater than or equal to 0.01 and less than or equal to 0.05, Magnetocaloric alloy, where y is greater than or equal to -0.05 and less than 0.
05.
2. In paragraph 1, The magnetocaloric alloy above is a magnetocaloric alloy having a Curie temperature of 245 K to 290 K when heated.
3. In paragraph 1, The magnetocaloric alloy above is a magnetocaloric alloy having a Curie temperature of 190 K to 240 K when cooled.
4. In paragraph 1, The magnetocaloric alloy above is a magnetocaloric alloy having a refrigeration capacity of 150 J / kg to 250 J / kg in a 2T magnetic field.
5. In paragraph 1, The above magnetocaloric alloy has the highest value of magnetic entropy change (│ΔS) in a 2T magnetic field. max │) A magnetocaloric alloy having a thermal conductivity of 3 J / kg·K to 13 J / kg·K.
6. In paragraph 1, The above magnetocaloric alloy has a half-width (T) of the maximum change in magnetic entropy in a 2T magnetic field. FWHM ) is a magnetocaloric alloy having a temperature of 10 K to 100 K.
7. A step of manufacturing an alloy ingot by arc-melting raw materials of Mn, Fe, Ni, P and Si; and A method for manufacturing a magnetocaloric alloy, comprising the step of heat treating the above alloy ingot in a vacuum; The above magnetocaloric alloy has the chemical formula MnFe 0.95-x Ni x P 0.6-y Si 0.4+y With the composition of A method for manufacturing a magnetocaloric alloy, wherein in the above chemical formula, x is 0.01 or more and 0.05 or less, and y is -0.05 or more and less than 0.
05.
8. In paragraph 7, The step of manufacturing an alloy ingot by arc melting is as follows: A first arc melting step of arc melting the above raw material under first current conditions; and A second arc melting step of arc melting an alloy ingot formed by first arc melting under second current conditions; A method for manufacturing a magnetocaloric alloy, wherein the second arc melting step is performed under higher current conditions than the first arc melting step.
9. In paragraph 8, A method for manufacturing a magnetocaloric alloy, wherein the current ratio of the first current condition and the second current condition is 1:1.4 to 1:2.
0.
10. In paragraph 7, A method for manufacturing a magnetocaloric alloy, wherein the above heat treatment step is performed at a temperature of 1200 K or more and 1600 K or less.
11. In paragraph 7, After the step of heat treating the above alloy ingot in a vacuum A method for manufacturing a magnetocaloric alloy, further comprising a step of rapidly cooling the heat-treated alloy ingot.
Citation Information
Patent Citations
Magnetocaloric materials containing manganese, iron, silicon, phosphorus and carbon
JP2019523826A
Working component for magnetic heat exchange and method of producing a working component for magnetic refrigeration
KR101829050B1
Apparatus and method for mobility and session management in different plmn(public land mobile network) through non-access stratum protocol processing in 5g environment
KR1020210050408A
Top-interconnection metal lines for a memory array device and methods for forming the same
KR102576500B1
Centimeter-level High-strength Iron-based Bulk Amorphous Alloy and Novel Copper Mold Casting Method Thereof