Low-temperature deposition material, method for forming low-temperature deposition film, and semiconductor substrate and semiconductor device manufactured therefrom

The use of low-temperature deposition materials with lower binding energies addresses thermal decomposition and impurity issues in semiconductor manufacturing, enabling the formation of high-quality, low-resistance metal films on complex substrates without high heat, effectively improving film quality and electrical properties.

WO2024205314A1PCT designated stage expired Publication Date: 2024-10-03SOULBRAIN CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004062
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-29
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current semiconductor manufacturing processes require high thermal energy for deposition, leading to thermal decomposition of precursor compounds, voids, and impurities like carbon, which affect film quality and electrical conductivity, especially in complex substrates with high aspect ratios.

Method used

A low-temperature deposition material with a lower binding energy than H2 is used, featuring direct bonds between hydrogen, iodine, carbon, and halogen elements, to form metal films and nitride films with reduced impurities and improved crystallinity, eliminating the need for high heat and separate reduction gases.

Benefits of technology

This method enables the formation of uniform, low-resistance metal films with reduced impurities, enhancing film quality and electrical properties, even at low temperatures, suitable for complex substrate structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004062_03102024_PF_FP_ABST
    Figure KR2024004062_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a low-temperature deposition material, a method for forming a low-temperature deposition film, and a semiconductor substrate and semiconductor device manufactured therefrom, and has the effects of providing a low-temperature deposition material, a method for forming a low-temperature deposition film, and a semiconductor substrate and a semiconductor device manufactured therefrom, in which by applying a predetermined material that can perform the role as a strong reducing agent even in a low-temperature process, it is possible to effectively manufacture a thin film and / or a metal nitride film with low resistance in a low-temperature process, and to reduce film impurities caused by ligands such as carbon and to improve physical properties such as specific resistivity and crystallinity.
Need to check novelty before this filing date? Find Prior Art

Description

Low-temperature deposition material, low-temperature deposition film forming method, semiconductor substrate and semiconductor device manufactured therefrom

[0001] The present invention relates to a low-temperature deposition material, a method for forming a low-temperature deposition film, a semiconductor substrate and a semiconductor device manufactured therefrom, and more particularly, to a low-temperature deposition material, a method for forming a low-temperature deposition film, a semiconductor substrate and a semiconductor device manufactured therefrom, which can effectively manufacture a deposition film with low resistance in a low-temperature process by applying a predetermined substance that can perform the role of a strong reducing agent even in a low-temperature process, and can reduce impurities in the deposition film caused by ligands such as carbon and improve physical properties such as roughness and crystallinity.

[0002] As the performance of semiconductor devices improves and higher integration is required, electrode materials or diffusion barrier materials with low resistivity are required.

[0003] These materials are provided in the form of metal films and / or metal nitride films through the ALD (atomic layer deposition) process, and the reduction process requires the use of extremely strong reducing agents or high thermal energy.

[0004] However, since the binding energy of H2 used for the above deposition is 467.7 kJ / mol, high heat energy is required during reduction. If high heat energy is applied, the precursor compound is thermally decomposed, which may result in deterioration of step coverage or occurrence of voids or seams on highly integrated or complex substrates with high aspect ratios.

[0005] Additionally, impurities (C, Cl) in the low-temperature deposition film derived from the ligand of the precursor compound in the metal film and / or metal nitride film - , F - ) are introduced and contaminated, and the crystal arrangement is disturbed, lowering the density of the formed film, which may cause problems with electrical conductivity due to low density.

[0006] Therefore, there is a need for the development of low-temperature deposition materials that can form uniform metal films and / or metal nitride films of complex structures, have excellent physical properties such as crystallinity, and provide deposition films with low resistance even under low-temperature process conditions due to low residual film impurities caused by ligands such as carbon, a method for forming low-temperature deposition films using the materials, and semiconductor substrates.

[0007] [Patent Number]

[0008] Korean Patent Publication No. 2019-0141071

[0009] In order to solve the problems of the prior art as described above, the present invention provides a method for forming a low-temperature deposition film, which can provide a deposition film with uniform thickness uniformity and low resistance even in a low-temperature process, by applying a material having a low binding energy compared to H2 as a low-temperature deposition material to effectively improve impurities, resistivity, and deposition characteristics, even when forming a metal film on a substrate having a complex structure, and a semiconductor substrate manufactured thereby.

[0010] That is, the purpose of the present invention is to provide a method for performing a reduction reaction in a low-temperature process by applying a novel low-temperature deposition material.

[0011] Furthermore, the present invention aims to provide a deposition film having low resistance while improving film properties such as electrical characteristics and density by applying a novel material that forms a metal film and / or a metal nitride film by performing a reduction reaction as a low-temperature deposition material.

[0012] The above and other objects of the present invention can all be achieved by the present invention described below.

[0013] In order to achieve the above object, the present invention provides a low-temperature deposition material for a wiring metal, a metal having a melting point of 350°C or lower, or a wiring metal diffusion barrier film, characterized in that it includes at least one selected from a compound having a direct bond between hydrogen (H) and iodine, a compound having a direct bond between carbon (C) and iodine, and a compound having a direct bond between a halogen element (F, Cl, Br) and iodine.

[0014] The above wiring metal or metal having a melting point of 350°C or lower may be selected from Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, and Ga.

[0015] The above wiring metal diffusion barrier film may be a transition metal nitride film of Ti, Ta, Ni, Mo, Nb, Zr, V, W, or a combination of two or more metals.

[0016] The compound having the direct bond between hydrogen (H) and iodine may have a total binding energy of 305 to 325 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP).

[0017] The compound having the direct bond between the above carbon (C) and iodine may have a total binding energy of 165 to 242 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen elements: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP).

[0018] Compounds having a direct bond between the above halogen elements (F, Cl, Br) and iodine may have a total binding energy of 50 to 160 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen elements: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP).

[0019] The above low-temperature deposition material may be at least one selected from compounds represented by the following chemical formulas 1-1 to 1-11.

[0020] [Chemical Formulas 1-1 to 1-11]

[0021] [Correction pursuant to Rule 91, May 31, 2024]

[0022] In addition, the present invention can provide a method for forming a low-temperature deposition film, characterized in that it includes a step of depositing a deposition film using the above-described low-temperature deposition material.

[0023] The above deposition film may be a metal film and / or a metal nitride film.

[0024] The above low-temperature deposition film forming method may include a step of forming a deposition film through a reduction reaction while injecting a precursor compound and the low-temperature deposition material into a chamber and adsorbing them onto a substrate surface.

[0025] The above low-temperature deposition film forming method can omit the step of injecting hydrogen as a reaction gas to perform a reduction reaction.

[0026] The above low-temperature deposition film forming method may include a post-treatment step of purging the inside of the chamber with a purge gas.

[0027] The chamber may be an ALD chamber, a CVD chamber, a PEALD chamber, or a PECVD chamber.

[0028] The above low-temperature deposition film may be one or more laminated films selected from the group consisting of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, and Ga.

[0029] The above metal nitride film may be a transition metal nitride film of Ti, Ta, Ni, Mo, Nb, Zr, V, W, or a nitride film in which a combination of two or more metals is selected.

[0030] The above low-temperature deposition film may be a wiring metal film, a wiring diffusion barrier film, or a low-resistance metal film.

[0031] The above wiring metal film may be a metal film of Mo, W, Ru, Cu, or Rh.

[0032] The above wiring metal diffusion barrier film may be a transition metal nitride film of Ti, Ta, Ni, Mo, Nb, Zr, V, W, or a nitride film in which a combination of two or more metals is selected.

[0033] The above low-resistance metal film may be a metal film having a melting point of 350°C or lower.

[0034] The above low resistance metal film may be a metal film of Pb, Cd, Sn, Bi, In or Ga.

[0035] The above low-temperature deposition film can be provided as a precursor compound for a low-resistance metal film.

[0036] The precursor compound for the above low-resistance metal film is a molecule having at least one selected from the group consisting of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, Ti, Ta, Ni, Mo, Nb, Zr, V, and Ga as a central metal atom (M) and at least one ligand composed of C, N, O, H, X (halogen), and in order to reduce the central metal atom at a low process temperature of 400 degrees or less, the compound may have a bond dissociation energy between the central metal atom and the ligand calculated using the basis set of the Gaussian 16 program (DFT-D3 / B3LYP (central metal, iodine: LanL2DZ, C, N, O, H, X: 6-31+G(dp)) of less than 350 kJ / mol.

[0037] The above precursor compound may be a molecule composed of at least one selected from the group consisting of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, Ti, Ta, Ni, Mo, Nb, Zr, V, and Ga as a central metal atom (M), and may be a compound having a vapor pressure of more than 0.01 mTorr and less than 100 Torr at 25°C.

[0038] The substrate loaded into the chamber may be heated to 100 to 700°C.

[0039] In the present invention, not only can the reaction gases commonly used in this technical field, such as ammonia, hydrogen, and oxygen, be omitted, but the process of separately injecting the reaction gas and performing reduction treatment can also be omitted.

[0040] The above low-temperature deposition film may be a metal film such as a molybdenum metal film, a tungsten metal film, a ruthenium metal film, a copper metal film, a rhodium metal film, a lead metal film, a cadmium metal film, a tin metal film, a bismuth metal film, an indium metal film, or a gallium metal film.

[0041] The above low-temperature deposition film may be a titanium nitride film, a tantalum nitride film, a vanadium nitride film, a tungsten nitride film, a nickel nitride film, a zirconium nitride film, a molybdenum nitride film, etc., and may be a metal nitride film in which two or more types are combined for the purpose of a diffusion barrier film, such as a titanium niobium nitride film and a titanium nickel nitride film.

[0042] The above metal film and / or metal nitride film is characterized by having a low resistivity of 5 μΩ·cm to 1000 μΩ·cm.

[0043] The above metal film and / or metal nitride film is characterized in that the content of ligand-derived film impurities, such as carbon, is 1% or less when measured by XPS or SIMS.

[0044] The above metal film and / or metal nitride film is characterized in that the crystallinity measured by XRD is improved due to the effect of reducing impurities inside the film through stronger reduction of the metal precursor.

[0045] In addition, the present invention provides a semiconductor substrate characterized by being manufactured by the low-temperature deposition film forming method described above.

[0046] The above low-temperature deposition film may be a metal film and / or a metal nitride film.

[0047] The above low-temperature deposition film may have a multi-layer structure of two or three layers.

[0048]

[0049] In addition, the present invention provides a semiconductor device characterized by including the semiconductor substrate described above.

[0050] According to the present invention, by applying a predetermined substance that can act as a strong reducing agent even in a low-temperature process, a reduction reaction (reduction of reaction activation energy with a reaction gas) can be provided at a process temperature at which the precursor is not thermally decomposed, thereby providing a method for forming a uniform metal film and / or metal nitride film even when forming a metal film and / or metal nitride film on a substrate having a highly integrated or complex structure.

[0051] In addition, it has the effect of more effectively reducing impurities and process byproducts of the metal film and / or metal nitride film caused by ligands such as carbon that cause deterioration of film properties such as crystallinity and electrical properties during formation of the metal film and / or metal nitride film, and improving the crystallinity and resistivity of the metal film and / or metal nitride film by modifying the film quality, thereby improving the electrical properties of the metal film and / or metal nitride film.

[0052] Furthermore, there is an effect of providing a method for forming a high-quality low-temperature deposition film by improving impurities and film quality, and a semiconductor substrate manufactured thereby.

[0053] Figure 1 is a graph showing the AES analysis results by temperature of Example 5 according to the present invention.

[0054] Figure 2 is an XRD analysis graph according to process temperature of Example 5 according to the present invention and Comparative Example 3.

[0055] Figure 3 is an XRD analysis graph between Example 6 according to the present invention and Comparative Example 4.

[0056] FIG. 4 and FIG. 5 are diagrams showing the reaction activation energy required to reduce the CO ligand and NO ligand of the Mo(CO)6 precursor and the (EtCp)Mo(CO)2(NO) precursor in Example 8 and Comparative Example 5, respectively, in terms of H2 and HI.

[0057]

[0058] Hereinafter, the low-temperature deposition film forming method of the present invention and the semiconductor substrate manufactured therefrom are described in detail.

[0059] The term “low-temperature deposition material” in this description refers to a novel material capable of forming a metal film and / or a metal nitride film through deposition by a reduction reaction in a low-temperature process of, for example, 600°C or less, preferably 550°C or less, and more preferably 500°C or less.

[0060] In this description, unless otherwise specified, the term “reduction reaction” refers to a reaction that not only displaces the ligand of a precursor compound but also reduces it to the extent that a reduction reaction provided using a conventional reaction gas is omitted.

[0061] In this description, unless otherwise specified, the term “modification” means that a substance other than a precursor and a reactant positively interacts with the reaction surface to improve film quality, such as reducing resistivity of the deposited film, increasing density, or reducing impurities.

[0062] Unless otherwise stated herein, % refers to weight %.

[0063] The present inventors have confirmed that the film quality, such as electrical characteristics and crystallinity, can be improved while preventing and inhibiting the inflow of film impurities caused by ligands such as carbon by using a predetermined low-temperature deposition material capable of performing a reduction reaction at a relatively low process temperature so that the precursor compound adsorbed on the surface of a substrate loaded inside a chamber is not thermally decomposed, and have dedicated themselves to related research to complete the present invention.

[0064] The above low-temperature deposition film can provide a metal film by providing one or more precursors selected from the group consisting of, for example, Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, and Ga, and in this case, the effect to be achieved in the present invention can be sufficiently obtained.

[0065] The above-mentioned wiring metal diffusion barrier film can be provided with one or more precursors selected from the group consisting of, for example, Ti, Ta, Ni, Mo, Nb, Zr, V, and W, and can provide a metal nitride film, and in this case, the effect to be achieved in the present invention can be sufficiently obtained.

[0066] The above low-temperature deposition film may have a film composition such as a molybdenum metal film, a tungsten metal film, a ruthenium metal film, a copper metal film, a rhodium metal film, a lead metal film, a cadmium metal film, a tin metal film, a bismuth metal film, an indium metal film, or a gallium metal film, as a specific example.

[0067] The above low-temperature deposition film may include the above-described film composition alone or in a selective area, but is not limited thereto, and may also include SiH, SiOH, etc.

[0068] The above low-temperature deposition film may be one or more laminated films selected from the group consisting of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, and Ga.

[0069] The above metal nitride film may be a laminated film of one or more types selected from the group consisting of Ti, Ta, Ni, Mo, Nb, Zr, V, and W.

[0070] The above low-temperature deposition film can be used in semiconductor devices as a commonly used wiring metal film or low-resistance metal film.

[0071] The above metal nitride film can be used in semiconductor devices as a commonly used wiring metal diffusion barrier film or for low resistance purposes.

[0072] The resistivity of the metal film and / or metal nitride film may be in the range of 5 μΩ·cm to 1000 μΩ·cm.

[0073] The above wiring metal film may be a metal film of Mo, W, Ru, Cu, or Rh.

[0074] The above low-resistance metal film may be a metal film having a melting point of 350°C or lower.

[0075] The above low resistance metal film may be a metal film of Pb, Cd, Sn, Bi, In or Ga.

[0076] The above low-temperature deposition film can be provided as a precursor compound for a low-resistance metal film.

[0077] The above precursor compound may have a structure in which ligands (L1, L2, L3, L4, L5, L6, etc.) are bonded to a central metal atom (M) such as Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, Ti, Ta, Ni, Mo, Nb, Zr, V, and Ga, for example.

[0078] The above precursor compound is a molecule having a central metal atom (M) of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, Ti, Ta, Ni, Mo, Nb, Zr, V and Ga and one or more ligands composed of C, N, O, H and X (halogen), and in the case of a precursor having a vapor pressure of 0.01 mTorr to 100 Torr at 25°C, the effect of using the low-temperature deposition material can be maximized.

[0079] The precursor compound may be, as another specific example, a molecule having at least one selected from the group consisting of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, Ti, Ta, Ni, Mo, Nb, Zr, V, and Ga as a central metal atom (M) and at least one ligand composed of C, N, O, H, X (halogen), and in order to reduce the central metal atom at a low process temperature of 400 degrees or less, the compound may have a bond dissociation energy between the central metal atom and the ligand calculated using the basis set of the Gaussian 16 program (DFT-D3 / B3LYP (central metal, iodine: LanL2DZ, C, N, O, H, X: 6-31+G(dp)) of less than 350 kJ / mol.

[0080] For example, when the central metal is divalent, L1 and L2 may be attached to the central metal as ligands, and when the central metal is hexavalent, L1, L2, L3, L4, L5, and L6 may be attached to the central metal, and the ligands corresponding to L1 to L6 may be the same or different.

[0081] For example, L1, L2, L3, L4, L5 and L6 may be the same or different as -H or -R, wherein -R may be linear or cyclic as C1-C10 alkyl, C1-C10 alkene, or C1-C10 alkane, and L1, L2, L3 and L4 may be formed such that the n number of L is from 2 to 6 depending on the oxidation state of the central metal.

[0082] For example, if the central metal is divalent, L1 and L2 may be attached to the central metal as ligands, and if the central metal is hexavalent, L1, L2, L3, L4, L5, and L6 may be attached to the central metal, and the ligands corresponding to L1 to L6 may be the same or different.)

[0083] As a specific example, L1, L2, L3, L4, L5 and L6 may be the same or different as -H, -OR, or -NR2, where -R may be H, C1-C10 alkyl, C1-C10 alkene, C1-C10 alkane, iPr, or TBu, in which case it has a reaction energy suitable for being replaced by the reaction gas described below.

[0084] As a specific example, L1, L2, L3, L4, L5 and L6 may be the same or different as -H or -X, where -X may be F, Cl, Br or I, and in this case have a reaction energy suitable for being replaced by the reaction gas described below.

[0085] As a specific example, L1, L2, L3, L4, L5 and L6 may be the same or different as -H or -R, where -R is C1-C10 alkyl, C1-C10 alkene, or C1-C10 alkane, and may have a linear or cyclic structure, and in this case, has a reaction energy appropriate for being replaced by a reaction gas described below.

[0086] As a specific example, L1, L2, L3, L4, L5 and L6 may be the same or different as -H, -OR, or -NR2, where -R may be H, C1-C10 alkyl, C1-C10 alkene, C1-C10 alkane, iPr, or tBu, in which case it has a reaction energy suitable for being replaced by a reaction gas described below.

[0087] As a specific example, L1, L2, L3, L4, L5 and L6 may be the same or different as -H or -X, where -X may be F, Cl, Br or I, and in this case have a reaction energy suitable for being replaced by the reaction gas described below.

[0088]

[0089] For example, the precursor compound having molybdenum (Mo) as a central metal may be at least one selected from compounds having a structure represented by the following chemical formulas 2 to 3, and may include, but is not limited to, trimethylene methane ligands and derivatives thereof.

[0090] [Chemical Formula 2]

[0091]

[0092]

[0093] (In the above chemical formula 2, R1 to R5 are independently selected from hydrogen, an amino group, a silyl group, an alkyl group having 1 to 8 carbon atoms, and an aryl group having 6 to 8 carbon atoms, and the case where R1 to R5 are both hydrogen is not included.)

[0094] [Chemical Formula 3]

[0095]

[0096] (In the above chemical formula 3, X is a linear and branched cyclic, saturated or unsaturated hydrocarbon substituted with H; F; Cl; Br; I; NO; CN; amidinate; guadiinate; ethylenediamine; propylenediamine; -NR6R7; -OR8; R9Cp and one or more carbon (C), nitrogen (N), oxygen (O), phosphorus (P), sulfur (S), and R6, R7, R8, R9 are independently selected from hydrogen, an alkyl group having 1 to 12 carbon atoms, and an aryl group having 6 to 12 carbon atoms, and n is an integer of 0 to 2.)

[0097] Derivatives of the above trimethylene methane ligand may include structures having, for example, a tribenzylidene methane ligand, a dibenzylidene methane ligand, etc.

[0098] Examples of precursor compounds with molybdenum (Mo) as the central metal include Mo(CO)6, (Ethylbenzene)2Mo, (2,6-diisopropylaniline)Mo(CO)3, (1,4-diisopropyl-1,4-diazabutadiene)Mo(CO), Mo(CO)5PCl2Me, Molybdenum Acetate Dimer, (Ethylbenzene)Mo(allyl)2, MeCpMo(CO)2(allyl), iprCpMo(CO)2(allyl), Mo(thd)3, (MeCp)Mo(EMA)3, (tert-butylimido)Mo (MeCp)2, TDMAMo,Cp2MoH2, Mo(Dithiocabate)4, (tert-butylimido)2MoCl(aminothiolate), (tert-butylimido)2Mo(tert-butylthiol)(aminothiolate), (tertbutylimido)2Mo(aminothiolate)2, (tert-butylimido)2Mo(tert-butylthiol)2 , (tert-butylimido)2Mo(tert-butylamine)2 , (tert-butylimido)2Mo(CpEMA) , MoO2(ipr-amidinate)2 , (tert-butylimido)2Mo(ipr-amidinate)2 , (tert-butylimido)2Mo(tert-butoxy)2 , (tert-butylimido)2Mo(hydrazido)Cl, MoO2(Dithiocarbamate)2, (1,4-di-tert-butyl-1,4,diazabutadiene)Mo(tert-butylimido)2, MoO2Cl2등일 수실다.

[0099] Here, the above MoO2Cl2, (Ethylbenzene)2Mo, (2,6-diisopropylaniline)Mo(CO)3, (benzene)Mo(CO)3, and 1,4-diisopropyl-1,4-diazabutaiene)Mo(CO)3 may be compounds represented by the following chemical formulas 4-1 to 4-5, respectively.

[0100] [Chemical Formulae 4-1 to 4-5]

[0101] [Correction pursuant to Rule 91, May 31, 2024]

[0102] Here, Mo(CO)5PCl2Me, Molybdenum Acetate Dimer, (Ethylbenzene)Mo(allyl)2, MeCpMo(CO)2(allyl) , i prCpMo(CO)2(allyl) may be a compound represented by the following chemical formulas 4-6 to 4-10, respectively.

[0103] [Chemical Formula 4-6 to 4-10]

[0104] [Correction pursuant to Rule 91, May 31, 2024]

[0105] Here, the above Mo(thd)3, (MeCp)Mo(EMA)3, (tert-butylimido)Mo(MeCp) 2, TDMAMo , Cp2MoH2 may be compounds represented by the following chemical formulas 4-11 to 4-15, respectively.

[0106] [Chemical Formula 4-11 to 4-15]

[0107] [Correction pursuant to Rule 91, May 31, 2024]

[0108] Here, the above Mo(Dithiocabate)4 , ( tert-butylimido )2MoCl (aminothiolate) , (tert-butylimido)2Mo(tert-butylthiol)(aminothiolate), (tertbutylimido)2Mo(aminothiolate)2, (tert-butylimido)2Mo(tert-butylthiol)2 may be compounds represented by the following chemical formulae 4-16 to 4-20, respectively.

[0109] [Chemical Formula 4-16 to 4-20]

[0110]

[0111] Here, the above (tert-butylimido)2Mo(tert-butylamine)2, (tert-butylimido)2Mo(CpEMA), MoO2(ipr-amidinate)2, and (tert-butylimido)2Mo(ipr-amidinate)2 may be compounds represented by the following chemical formulas 4-21 to 4-24, respectively.

[0112] [Chemical Formulas 4-21 to 4-24]

[0113]

[0114] Here, the (tert-butylimido)2Mo(tert-butoxy)2, (tert-butylimido)2Mo(N,N-dimethyldiethylene triamine), (tert-butylimido)2Mo(hydrazido)Cl, MoO2(Dithiocarbamate)2, 1,4-ditert-butyl-1,4,diazabutadiene)Mo(tert-butylimido)2, MoO2Cl2, (tert-butylimido)2Mo(dimethylamide)2, (Methylbenzene)2Mo may be compounds represented by the following chemical formulae 4-25 to 4-31, respectively.

[0115] [Chemical Formula 4-25 to 4-31]

[0116]

[0117] The above precursor compound can be used, for example, by mixing it with a non-polar solvent, in which case there is an advantage in that the viscosity or vapor pressure of the precursor compound can be easily controlled.

[0118]

[0119] The low-temperature deposition material of the present invention not only effectively substitutes ligands by lowering the activation energy of a precursor compound adsorbed on a substrate, but also has reducing power and performs a reduction reaction, thereby eliminating the need for a reduction process using a reaction gas required in the process.

[0120] The substitution for the above ligand can be formed, for example, on the entire substrate or a portion of the substrate on which the low-temperature deposition film is formed.

[0121] The above low-temperature deposition material is characterized by including at least one selected from, for example, a compound having a direct bond between hydrogen (H) and iodine, a compound having a direct bond between carbon (C) and iodine, and a compound having a direct bond between a halogen element (F, Cl, Br) and iodine.

[0122] The above low-temperature deposition material can form a film by performing a reduction reaction on its own without a separate reaction gas such as H2.

[0123] The compound having the direct bond between hydrogen (H) and iodine may have a total binding energy of 305 to 325 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP), and in this case, a thin film with low resistance can be effectively provided.

[0124] The compound having the direct bond between the above carbon (C) and iodine may have a total binding energy of 165 to 242 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP), and in this case, the content of film impurities caused by ligands such as carbon can be reduced and a thin film with low resistance can be effectively provided.

[0125] The compound having a direct bond between the above halogen element (F, Cl, Br) and iodine may have a total binding energy of 50 to 160 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP), and in this case, a thin film with low resistance can be effectively provided.

[0126] The above low-temperature deposition material is a compound having a direct bond between hydrogen (H) and iodine, and the total binding energy of the compound calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP) can be 305 to 325 kJ / mol. In this case, the content of film impurities caused by ligands such as carbon can be reduced and a thin film with low resistance can be effectively provided.

[0127] The above low-temperature deposition material may be at least one selected from compounds represented by the following chemical formulas 1-1 to 1-11.

[0128] [Chemical Formulas 1-1 to 1-11]

[0129] [Correction pursuant to Rule 91, May 31, 2024]

[0130] The low-temperature deposition material is, for example, a single hydrogen iodide of 3N to 15N, a gas mixture of 1 to 99 wt% of hydrogen iodide of 3N to 15N and the remainder of an inert gas so that the total amount becomes 100 wt%, or an aqueous solution mixture of 0.5 to 70 wt% of hydrogen iodide of 3N to 15N and the remainder of water so that the total amount becomes 100 wt%, wherein the inert gas may be nitrogen, helium or argon having a purity of 4N to 9N, in which case a reduction reaction is performed to reduce impurities and effectively form a thin film or a metal nitride film having low resistance.

[0131] The above low-temperature deposition material is preferably a single hydrogen iodide of 5N to 6N, a gas mixture of 1 to 99 wt% of hydrogen iodide of 5N to 6N and the balance of an inert gas so that the total amount becomes 100 wt%, or an aqueous solution mixture of 0.5 to 70 wt% of hydrogen iodide of 5N to 6N and the balance of water so that the total amount becomes 100 wt%, wherein the inert gas may be nitrogen, helium or argon having a purity of 4N to 9N, and in this case, when forming a low-temperature deposition film, side reactions are suppressed and a film growth rate is controlled, so that process byproducts in the low-temperature deposition film are reduced, corrosion or deterioration is reduced, and film quality improvement such as improved film crystallinity is provided, and film thickness uniformity can be greatly improved even when forming a thin film on a substrate having a highly integrated or complex structure.

[0132] In such cases, when forming a thin film on a substrate having a highly integrated or complex structure, the film thickness uniformity is greatly improved by sufficiently providing the effect of a reduction reaction to the precursor compound adsorbed on the substrate at a relatively low process temperature at which the precursor is not thermally decomposed, and not only the precursor but also the process by-products are effectively protected by preventing adsorption, and the reaction speed is reduced, but there is also the advantage of effectively removing the process by-products.

[0133] The above low-temperature deposition material may preferably be a compound having a purity of 99.9% or higher, a compound having a purity of 99.95% or higher, or a compound having a purity of 99.99% or higher. Note that when using a compound having a purity of less than 99%, impurities may remain in the thin film or cause a side reaction with the precursor or reactant, so it is recommended to use a material having a purity of 99% or higher if possible.

[0134] The above low-temperature deposition film may, for example, contain halogen compounds at 100 ppm or less. For reference, if the halogen remains excessively, for example, when using a nitriding agent described below under temperature conditions of 200 to 300°C, chlorides such as NH4Cl are generated and remain in the low-temperature deposition film, which is not desirable.

[0135] The above low-temperature deposition film can be used for purposes such as a wiring metal film or a low-resistance metal film, but is not limited thereto.

[0136] In particular, since the film growth rate is significantly reduced while forming a relatively thick film, uniformity is secured even when applied to a substrate with a complex structure, and deposition is possible with a particularly thin thickness, and it can provide the effect of improving the amount of O, Si, metal, metal oxide remaining as process byproducts, and even carbon residue that was difficult to reduce in the past.

[0137]

[0138] A method for forming a low-temperature deposition film according to one embodiment of the present invention is characterized by including a step of forming a deposition film through a reduction reaction while injecting a precursor compound and the low-temperature deposition material into a chamber and adsorbing them onto a substrate surface, wherein the reduction of the precursor adsorbed on the substrate can be effectively performed at a relatively low process temperature at which the precursor is not thermally decomposed, and the film growth rate is appropriately lowered to greatly improve film uniformity even when deposited on a substrate having a highly integrated or complex structure, and there is an effect of providing a deposition film with low resistance.

[0139] The above low-temperature deposition material and precursor compound can be transferred into the chamber by the VFC method, the DLI method, or the LDS method.

[0140] The ratio of the amount (mg / cycle) of the precursor compound and the low-temperature deposition material injected into the chamber may be 1:1 to 1:20.

[0141] The step of injecting the low-temperature deposition material onto the substrate surface has a feeding time (second) of the low-temperature deposition material onto the substrate surface of preferably 0.01 to 10 seconds per cycle, more preferably 0.02 to 8 seconds, even more preferably 0.04 to 6 seconds, and even more preferably 0.05 to 4 seconds, and within this range, there is an advantage of a low film growth rate, excellent step coverage, and economic efficiency.

[0142] In this description, the feeding time of the low-temperature deposition material is based on a flow rate of 0.1 to 8,000 mg / cycle for a chamber volume of 15 to 20 L, and more specifically, based on a flow rate of 10 to 5,000 mg / cycle for a chamber volume of 18 L.

[0143]

[0144] As a specific example, the method for forming a low-temperature deposition film may include a step of forming a deposition film through a reduction reaction by injecting a precursor compound and the low-temperature deposition material into a chamber and adsorbing them onto a substrate surface; and a step of purging the inside of the chamber with a purge gas.

[0145] The entire steps described above can be repeated as a unit cycle until a low-temperature deposition film of the desired thickness is obtained, and when the low-temperature deposition material is simultaneously introduced with a precursor compound within one cycle to improve the film quality, the process by-products generated are effectively removed, thereby reducing the resistivity, greatly improving the step coverage, improving the uniformity, and improving the film quality such as electrical characteristics, dielectric characteristics, and density, and providing a low-resistance deposition film.

[0146] The chamber may be an ALD chamber, a CVD chamber, a PEALD chamber, or a PECVD chamber.

[0147] The substrate loaded into the chamber may be heated to 100 to 700°C.

[0148] The above low temperature deposition material or precursor compound may be vaporized and injected, followed by a plasma post-treatment step, which may improve film growth rate while reducing process byproducts.

[0149] In the purging step, the amount of purge gas injected into the ALD chamber is not particularly limited as long as it is an amount sufficient to remove the unabsorbed precursor compound. However, for example, it may be 10 to 10,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times, based on the volume of the precursor compound injected into the ALD chamber. Within this range, the unabsorbed precursor compound is sufficiently removed to form a thin film evenly and prevent deterioration of the film quality. Here, the amounts of the purge gas and the precursor compound injected are each based on one cycle, and the volume of the precursor compound means the volume of the vapor of the precursor compound injected.

[0150]

[0151] The above low-temperature deposition material and precursor compound can be preferably transferred into the ALD chamber by the VFC method, the DLI method or the LDS method, and more preferably, they are transferred into the chamber by the VFC method.

[0152] The substrate loaded in the chamber can be heated, for example, to 100 to 700°C, specifically, to 300 to 600°C, and the low-temperature deposition material or precursor compound can be injected onto the substrate in an unheated or heated state, and depending on the deposition efficiency, it may be injected in an unheated state and then the heating conditions may be adjusted during the deposition process. For example, it can be injected onto the substrate at 50 to 400°C for 1 to 20 seconds.

[0153]

[0154] The ratio of the precursor compound and the low-temperature deposition material injected into the chamber (mg / cycle) may be preferably 1:1 to 1:400, more preferably 1:2 to 1:350, still more preferably 1:2 to 1:300, and still more preferably 1:2.5 to 1:200, and within this range, the effect of improving the step coverage and reducing the process by-products is significant.

[0155]

[0156] The above low-temperature deposition film formation method can be performed at a deposition temperature in the range of, for example, 100 to 600°C, preferably at a deposition temperature in the range of 300 to 500°C, and more preferably at a deposition temperature in the range of 300 to 400°C, and has the effect of growing an excellent film quality while providing ALD process characteristics within this range.

[0157] The above low-temperature deposition film forming method can be performed at a deposition pressure in the range of, for example, 0.01 to 20 Torr, preferably at a deposition pressure in the range of 0.1 to 20 Torr, more preferably at a deposition pressure in the range of 0.1 to 10 Torr, and most preferably at a deposition pressure in the range of 0.3 to 7 Torr, and within this range, there is an effect of obtaining a low-temperature deposition film of uniform thickness.

[0158] In this description, the deposition temperature and deposition pressure can be measured as the temperature and pressure formed within the deposition chamber, or as the temperature and pressure applied to the substrate within the deposition chamber.

[0159] The above low-temperature deposition film forming method may preferably include a step of raising the temperature inside the chamber to a deposition temperature before introducing the precursor compound into the chamber; and / or a step of purging the chamber by injecting an inert gas into the chamber before introducing the precursor compound into the chamber.

[0160]

[0161] The low-temperature deposition film forming method is such that the residual impurity (carbon or halogen element) intensity (c / s) in the low-temperature deposition film, measured based on SIMS, based on a low-temperature deposition film thickness of 100 Å, may be preferably 100,000 or less, more preferably 70,000 or less, even more preferably 50,000 or less, and even more preferably 10,000 or less, and in a preferred embodiment, 5,000 or less, more preferably 10 to 4,000, and even more preferably 10 to 3,000, and within this range, the effect of preventing deterioration of crystallinity and electrical characteristics is excellent.

[0162] In the present invention, purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the film growth rate per cycle is appropriately controlled, and deposition is performed as or close to a single atomic mono-layer, which is advantageous in terms of film quality.

[0163]

[0164] In addition, the present invention provides a manufacturing device capable of providing the low-temperature deposition film manufacturing method, which may include an ALD chamber, a first vaporizer for vaporizing a precursor compound, a first transfer means for transferring the vaporized precursor compound into the ALD chamber, a second vaporizer for vaporizing a low-temperature deposition material, and a second transfer means for transferring the vaporized low-temperature deposition material into the ALD chamber. Here, the vaporizer and the transfer means are not particularly limited as long as they are vaporizers and transfer means commonly used in the technical field to which the present invention belongs.

[0165] As a specific example, regarding the method for forming the above low-temperature deposition film, first, a substrate on which a deposition film is to be formed is placed in a deposition chamber capable of atomic layer deposition.

[0166] The above substrate may include a semiconductor substrate such as a silicon substrate or silicon oxide.

[0167] The above substrate may further have a conductive layer or an insulating layer formed on top thereof.

[0168] In order to deposit a deposition film on a substrate positioned in the above deposition chamber, the above-described low-temperature deposition material, precursor compound, or mixture thereof with a non-polar solvent are each prepared.

[0169] Afterwards, the prepared low-temperature deposition material, precursor compound or mixture thereof with a non-polar solvent (hereinafter referred to as “deposition film forming composition”) is injected into a vaporizer, changed into a vapor phase and transferred to a deposition chamber to be adsorbed on a substrate, and the unadsorbed material or mixture thereof with a non-polar solvent is purged.

[0170] The above non-polar solvent may preferably be at least one selected from the group consisting of alkanes and cycloalkanes, and in this case, there is an advantage in that the step coverage is improved even when the deposition temperature is increased during the formation of a low-temperature deposition film while containing an organic solvent that has low reactivity and solubility and is easy to manage moisture.

[0171] As a more preferred example, the non-polar solvent may include a C1 to C10 alkane or a C3 to C10 cycloalkane, preferably a C3 to C10 cycloalkane, in which case it has the advantages of low reactivity and solubility and easy moisture management.

[0172] In this description, C1, C3, etc. refer to the number of carbon atoms.

[0173] The above cycloalkane may preferably be a C3 to C10 monocycloalkane, and among the above monocycloalkanes, cyclopentane is liquid at room temperature and has the highest vapor pressure, so it is preferred in a vapor deposition process, but is not limited thereto.

[0174] The above nonpolar solvent has, for example, a solubility in water (25°C) of 200 mg / L or less, preferably 50 to 400 mg / L, more preferably 135 to 175 mg / L, and within this range has the advantage of low reactivity toward the precursor compound and easy moisture management.

[0175] In this description, solubility is not particularly limited if it is measured using a measurement method or standard commonly used in the technical field to which the present invention belongs, and for example, a saturated solution can be measured using the HPLC method.

[0176] The non-polar solvent may preferably comprise 5 to 95 wt%, more preferably 10 to 90 wt%, even more preferably 40 to 90 wt%, and most preferably 70 to 90 wt%, based on the total weight of the precursor compound and the non-polar solvent.

[0177] If the content of the nonpolar solvent is added in excess of the upper limit, impurities are generated, which increases resistance and film impurity levels. If the content of the organic solvent is added in excess of the lower limit, there is a disadvantage in that the effect of improving step coverage due to solvent addition and the effect of reducing impurities such as chloride (Cl) ions are small.

[0178]

[0179] As described above, the low-temperature deposition film forming method comprises, for example, a step of injecting a precursor compound and the low-temperature deposition material into a chamber and adsorbing them onto a substrate surface, and a step of purging the unadsorbed material as a unit cycle, and the unit cycle can be repeated to form a low-temperature deposition film of a desired thickness.

[0180] The above unit cycle can be repeated, for example, 1 to 99,999 times, preferably 10 to 1,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times, and within this range, there is an effect of well expressing the desired membrane characteristics.

[0181]

[0182] The present invention also provides a semiconductor substrate, characterized in that the semiconductor substrate is manufactured by the low-temperature deposition film forming method of the present invention, and in this case, the film thickness uniformity is greatly excellent and the density and electrical characteristics are excellent.

[0183]

[0184] The above low-temperature deposition film preferably has a thickness of 30 nm or less, a resistivity value of 5 to 2,000 μΩ·cm based on a low-temperature deposition film thickness of 10 nm, an impurity content of 10,000 ppm or less, a step coverage of 90% or more, and within this range, has excellent performance as a diffusion barrier film and excellent effect as a metal wiring material, but is not limited thereto.

[0185] The low-temperature deposition film may have a thickness of, for example, 0.1 to 30 nm, preferably 1 to 20 nm, and more preferably 2 to 10 nm, and within this range, the film has excellent film properties.

[0186] The low-temperature deposition film may have, for example, a resistivity value of 0.1 to 400 μΩ·cm, preferably 0.1 to 200 μΩ·cm, and more preferably 0.1 to 20 μΩ·cm based on a low-temperature deposition film thickness of 10 nm, and the film characteristics are excellent within this range.

[0187] The low-temperature deposition film may preferably have an impurity content of 10,000 ppm or less, or 1 to 9,000 ppm, more preferably 1 to 8,500 ppm, and even more preferably 1 to 1,000 ppm, and within this range, the film crystallinity is excellent while the resistivity is improved. Here, the impurities remaining in the low-temperature deposition film are impurities remaining due to insufficient reduction of the metal precursor ligand, and may be, for example, carbon, nitrogen, oxygen, or halogen elements, and the lower the impurity residue in the low-temperature deposition film, the better the film quality is, which is preferable.

[0188] The above low-temperature deposition film is characterized in that the content of ligand-derived film impurities, such as carbon, is reduced to 1% or less when measured by XPS.

[0189] Unless otherwise stated herein, percentages are by weight.

[0190] The above low-temperature deposition film has, for example, a step coverage of 90% or more, preferably 92% or more, and more preferably 95% or more, and within this range, even a complex structure can be easily deposited on a substrate, so it has the advantage of being applicable to next-generation semiconductor devices.

[0191] The low-temperature deposition film manufactured above preferably has a thickness of 20 nm or less, and has an impurity content of carbon, nitrogen, oxygen, halogen, etc. of 10,000 ppm or less based on a low-temperature deposition film thickness of 10 nm, and a step coverage of 90% or more, and has excellent performance as a dielectric film or blocking film within this range, but is not limited thereto.

[0192] The above low-temperature deposition film is characterized by improved crystallinity as measured by XRD.

[0193] The above low-temperature deposition film is characterized by improved resistivity.

[0194]

[0195] Hereinafter, preferred embodiments and drawings are presented to help understand the present invention, but the following embodiments and drawings are only illustrative of the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of ​​the present invention, and it is also natural that such changes and modifications fall within the scope of the appended patent claims.

[0196]

[0197] [Example]

[0198] Example 1

[0199] An ALD deposition process was performed using 5N HI as a low-temperature deposition material and a precursor compound having the following chemical formula BTBMMo as a precursor compound.

[0200]

[0201] First, the prepared precursor compound was placed in a separate canister and supplied to a separate vaporizer heated to 150°C at a flow rate of 0.1 g / min using a Liquid Mass Flow Controller (LMFC) at room temperature. The BTBMMo precursor vaporized in the vaporizer was introduced into the deposition chamber for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0202] Next, the prepared low-temperature deposition material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm using a mass flow controller (MFC) at room temperature. The low-temperature deposition material vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 350°C, and this process was repeated 200 to 400 times to form a self-limiting atomic layer metal film with a thickness of 10 nm.

[0203] The thickness of the metal film was measured using an ellipsometer, which is a device that can measure optical properties such as the thickness or refractive index of a metal film using the polarization characteristics of light for the manufactured low-temperature deposition film (MoN metal film). The thickness of the metal film was divided by the number of cycles to calculate the thickness of the metal film deposited per cycle, and the result was 10 nm. The metal film component analysis was performed using AES and SIMS analysis. In addition, the sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0204]

[0205] Example 2

[0206] An ALD deposition process was performed using 5N HI as a low-temperature deposition material, NH3 as a reaction gas, and a precursor compound having the following chemical formula BTBMMo.

[0207]

[0208] First, the prepared precursor compound was placed in a separate canister and supplied to a separate vaporizer heated to 150°C at a flow rate of 0.1 g / min using a Liquid Mass Flow Controller (LMFC) at room temperature. The BTBMMo precursor vaporized in the vaporizer was introduced into the deposition chamber for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0209] Next, the prepared HI low-temperature deposition material was placed in a canister and supplied to the chamber at room temperature using a mass flow controller (MFC). The low-temperature deposition material vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a catalytic reaction, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. Then, NH3 reaction gas was supplied to the chamber at a flow rate of 1000 sccm, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 350°C, and this process was repeated 200 to 400 times to form a self-limiting atomic layer metal film with a thickness of 10 nm.

[0210] The thickness of the metal film was measured using an ellipsometer, which is a device that can measure optical properties such as the thickness or refractive index of a metal film using the polarization characteristics of light for the manufactured low-temperature deposition film (MoN metal film). The thickness of the metal film was divided by the number of cycles to calculate the thickness of the metal film deposited per cycle, and the result was 10 nm. The metal film component analysis was performed using AES and SIMS analysis. In addition, the sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0211]

[0212] Example 3

[0213] An ALD deposition process was performed using 5N HI as a low-temperature deposition material and a precursor compound having the following chemical formula BTBTBMo as a precursor compound.

[0214]

[0215] First, the prepared precursor compound was placed in a separate canister and supplied to a separate vaporizer heated to 150°C at a flow rate of 0.1 g / min using a Liquid Mass Flow Controller (LMFC) at room temperature. The BTBTBMo precursor vaporized in the vaporizer was introduced into the deposition chamber for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0216] Next, the prepared low-temperature deposition material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm using a mass flow controller (MFC) at room temperature. The low-temperature deposition material vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 350°C, and this process was repeated 200 to 400 times to form a self-limiting atomic layer metal film with a thickness of 10 nm.

[0217] The thickness of the metal film was measured using an ellipsometer, which is a device that can measure optical properties such as the thickness or refractive index of a metal film using the polarization characteristics of light for the manufactured low-temperature deposition film (MoN metal film). The thickness of the metal film was divided by the number of cycles to calculate the thickness of the metal film deposited per cycle, and the result was 10 nm. The metal film component analysis was performed using AES and SIMS analysis. In addition, the sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0218]

[0219] Example 4

[0220] An ALD deposition process was performed using 5N HI as a low-temperature deposition material, NH3 as a reaction gas, and a precursor compound having the following chemical formula BTBTBMo.

[0221]

[0222] First, the prepared precursor compound was placed in a separate canister and supplied to a separate vaporizer heated to 150°C at a flow rate of 0.1 g / min using a Liquid Mass Flow Controller (LMFC) at room temperature. The BTBTBMo precursor vaporized in the vaporizer was introduced into the deposition chamber for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0223] Next, the prepared HI low-temperature deposition material was placed in a canister and supplied to the chamber at room temperature using a mass flow controller (MFC). The low-temperature deposition material vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a catalytic reaction, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. Then, NH3 reaction gas was supplied to the chamber at a flow rate of 1000 sccm, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 350°C, and this process was repeated 200 to 400 times to form a self-limiting atomic layer metal film with a thickness of 10 nm.

[0224] The thickness of the metal film was measured using an ellipsometer, which is a device that can measure optical properties such as the thickness or refractive index of a metal film using the polarization characteristics of light for the manufactured low-temperature deposition film (MoN metal film). The thickness of the metal film deposited per cycle was calculated by dividing the thickness by the number of cycles, and the result was 10 nm. The metal film component analysis was performed using AES and SIMS analysis. In addition, the sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0225]

[0226] Example 5

[0227] An ALD deposition process was performed using 5N HI as a low-temperature deposition material and a precursor compound having the following chemical formula Mo(CO)6.

[0228]

[0229] First, the prepared precursor compound was placed in a separate canister and heated to 50°C. The Mo(CO)6 precursor was introduced into the deposition chamber using 50 sccm of Ar carrier for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0230] Next, the prepared low-temperature deposition material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm using a mass flow controller (MFC) at room temperature. The low-temperature deposition material vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 375°C, and this process was repeated 50 to 200 times to form a self-limiting atomic layer metal film with a thickness of 10 nm.

[0231] The thickness of the metal film was measured using an ellipsometer, which is a device that can measure optical properties such as the thickness or refractive index of a metal film using the polarization characteristics of light for the manufactured low-temperature deposition film (Mo metal film). The thickness of the metal film was divided by the number of cycles to calculate the thickness of the metal film deposited per cycle, and the result was 10 nm. The sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value. The crystallinity of the Mo metal film was confirmed through XRD analysis.

[0232]

[0233] Example 6

[0234] An ALD deposition process was performed using 5N HI as a low-temperature deposition material and a precursor compound having the following chemical formula Mo(tol)2.

[0235]

[0236] First, the prepared precursor compound was placed in a separate canister and heated to 130°C. The Mo(tol)2 precursor was introduced into the deposition chamber using 50 sccm of Ar carrier for 10 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0237] Next, the prepared low-temperature deposition material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm using a mass flow controller (MFC) at room temperature. The low-temperature deposition material vaporized in a vapor phase in the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 250°C, and this process was repeated 30 to 300 times to form a self-limiting atomic layer metal film with a thickness of 10 nm.

[0238] The thickness of the metal film was measured using an ellipsometer, a device that can measure optical properties such as the thickness or refractive index of a metal film using the polarization characteristics of light for the manufactured low-temperature deposition film (Mo metal film). The thickness of the metal film was divided by the number of cycles to calculate the thickness of the metal film deposited per cycle, which was 10 nm. The sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0239]

[0240] Example 7

[0241] The ALD deposition process was performed using 5N HI as a low-temperature deposition material, TiCl4 precursor as a precursor compound, and NH3 as a nitride film reducing agent.

[0242] First, the prepared precursor compound was placed in a separate canister and heated to 30℃. The TiCl4 precursor was introduced into the deposition chamber using an Ar carrier of 100 sccm for 3 seconds, and then purging was performed by supplying argon gas at 3000 sccm for 5 seconds. Afterwards, the prepared low-temperature deposition material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm for 5 seconds using an MFC (Mass Flow Controller) at room temperature. Afterwards, argon gas was supplied at 3000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.0 Torr. Afterwards, 1000 sccm of NH3 was supplied for 5 seconds to reduce the film and form a nitride thin film, followed by argon purging.

[0243] By repeating this process while maintaining the deposition temperature at 500 ℃, a self-limiting atomic layer metal nitride film with a thickness of 10 nm was formed.

[0244]

[0245] Example 8

[0246] The ALD deposition process was performed using 5N HI as a low-temperature deposition material, NbF5 precursor as a precursor compound, and NH3 as a nitride film reducing agent.

[0247] First, the prepared precursor compound was placed in a separate canister and heated to 50℃. The NbF5 precursor was introduced into the deposition chamber with an Ar carrier of 100 sccm for 3 seconds, and then purging was performed by supplying argon gas at 1000 sccm for 6 seconds. Afterwards, the prepared low-temperature deposition material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm for 5 seconds using an MFC (Mass Flow Controller) at room temperature. Afterwards, argon gas was supplied at 1000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.0 Torr. Afterwards, 1000 sccm of NH3 was supplied for 5 seconds to reduce the NbF5 precursor and form a nitride thin film, and then argon purging was performed.

[0248] By repeating this process while maintaining the deposition temperature at 450 ℃, a self-limiting atomic layer metal nitride film with a thickness of 10 nm was formed.

[0249]

[0250] Example 9

[0251] The ALD deposition process was performed using 3N tertiary-butyl iodide as a low-temperature deposition material, MoO2Cl2 precursor as a precursor compound, and NH3 as a nitride film reducing agent.

[0252] First, the prepared precursor compound was placed in a separate canister and heated to 120℃. The MoO2Cl2 precursor was introduced into the deposition chamber with an Ar carrier of 200 sccm for 5 seconds, and then purging was performed by supplying argon gas at 1000 sccm for 5 seconds. Afterwards, the prepared low-temperature deposition material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm for 5 seconds using an MFC (Mass Flow Controller) at room temperature. Afterwards, argon gas was supplied at 1000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 3.0 Torr. Afterwards, 1000 sccm of NH3 was supplied for 5 seconds to reduce the material and form a nitride thin film, and then argon purging was performed.

[0253] By repeating this process while maintaining the deposition temperature at 400 ℃, a self-limiting atomic layer metal nitride film with a thickness of 10 nm was formed.

[0254]

[0255] [Comparative example]

[0256] Comparative Example 1

[0257] An ALD deposition process was performed using NH3 as a thin film forming material and a precursor compound having the following chemical formula BTBMMo as a precursor compound.

[0258]

[0259] First, the prepared precursor compound was placed in a separate canister and supplied to a separate vaporizer heated to 150°C at a flow rate of 0.1 g / min using a Liquid Mass Flow Controller (LMFC) at room temperature. The BTBMMo precursor vaporized in the vaporizer was introduced into the deposition chamber for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0260] Next, the prepared thin film forming material, NH3, was supplied to the chamber at a flow rate of 1,000 sccm. The thin film forming material, vaporized in a vapor phase from the vaporizer, was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5,000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 350°C, and this process was repeated 200 to 400 times to form a self-limiting atomic layer thin film with a thickness of 10 nm.

[0261] The thickness of the thin film (MoN nitride film) was measured using an ellipsometer, a device that can measure optical properties such as the thickness or refractive index of a thin film using the polarization characteristics of light. The thickness of the thin film deposited per cycle was calculated by dividing the thickness by the number of cycles, and the result was 10 nm. The thin film component analysis was performed using AES and SIMS. In addition, the sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0262]

[0263] Comparative Example 2

[0264] An ALD deposition process was performed using NH3 as a reaction gas and a precursor compound having the following chemical formula BTBTBMo.

[0265]

[0266] First, the prepared precursor compound was placed in a separate canister and supplied to a separate vaporizer heated to 150°C at a flow rate of 0.1 g / min using a Liquid Mass Flow Controller (LMFC) at room temperature. The BTBTBMo precursor vaporized in the vaporizer was introduced into the deposition chamber for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0267] Next, the prepared reaction gas NH3 was supplied to the chamber at a flow rate of 1,000 sccm. The reaction gas vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5,000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 350°C, and this process was repeated 200 to 400 times to form a self-limiting atomic layer thin film with a thickness of 10 nm.

[0268] The thickness of the thin film (MoN nitride film) was measured using an ellipsometer, a device that can measure optical properties such as the thickness or refractive index of a thin film using the polarization characteristics of light. The thickness of the thin film deposited per cycle was calculated by dividing the thickness by the number of cycles, and the result was 10 nm. The thin film component analysis was performed using AES and SIMS. In addition, the sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0269]

[0270] Comparative Example 3

[0271] An ALD deposition process was performed using NH3 as a reaction gas and Mo(CO)6 precursor with the following chemical formula as a precursor compound.

[0272]

[0273] First, the prepared precursor compound was placed in a separate canister and heated to 50°C. The Mo(CO)6 precursor was introduced into the deposition chamber using 50 sccm of Ar carrier for 3 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0274] Next, the prepared reaction gas NH3 was supplied to the chamber at a flow rate of 1,000 sccm. The reaction gas vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5,000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 375°C, and this process was repeated 50 to 200 times to form a self-limiting atomic layer thin film with a thickness of 10 nm.

[0275] The thickness of the thin film (Mo nitride film) produced was measured using an ellipsometer, a device that can measure optical properties such as the thickness or refractive index of a thin film using the polarization characteristics of light. The thickness of the thin film deposited per cycle was calculated by dividing the thickness by the number of cycles, and the result was 10 nm. The sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value. The crystallinity of the Mo thin film was confirmed through XRD analysis.

[0276]

[0277] Comparative Example 4

[0278] An ALD deposition process was performed using NH3 as a reaction gas and Mo(tol)2 precursor with the following chemical formula as a precursor compound.

[0279]

[0280] First, the prepared precursor compound was placed in a separate canister and heated to 130°C. The Mo(tol)2 precursor was introduced into the deposition chamber using 50 sccm of Ar carrier for 10 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr.

[0281] Next, the prepared reaction gas NH3 was supplied to the chamber at a flow rate of 1,000 sccm. The reaction gas vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5,000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5 Torr. The deposition temperature was maintained at 250 and 300°C, respectively, and this process was repeated 30 to 300 times to form a self-limiting atomic layer thin film with a thickness of 10 nm.

[0282] The thickness of the thin film (Mo nitride film) produced was measured using an ellipsometer, a device that can measure optical properties such as the thickness or refractive index of a thin film using the polarization characteristics of light. The thickness of the thin film deposited per cycle was calculated by dividing the thickness by the number of cycles, and the result was 10 nm. The sheet resistance was measured using the 4-probe measurement method, and the measured thickness was used to calculate the resistivity value.

[0283]

[0284] Comparative Example 5

[0285] The bond dissociation energy of the thin film forming material and metal precursor of the present invention is an important factor in reducing the precursor at low temperatures. The computational simulation program used to calculate the bond dissociation energy is Gaussian 16, and the computational simulation method used here is DFT-D3 / B3LYP. The basis set is LanL2DZ for iodine and the central metal (e.g., Mo), and 6-31+G(d,p) for other elements.

[0286] In addition, the activation energy for the reaction between Mo(CO)6, (EtCp)Mo(CO)2(NO) precursor and H2 was calculated using the same method, where the transition state method was DFT / TS-Berny and the intrinsic reaction coordinate was 40 pts.

[0287]

[0288] Comparative Example 6

[0289] 99% CH3I was used as a thin film forming material, and the ALD deposition process was performed using a precursor compound having the following chemical formula MoCl5.

[0290]

[0291] First, the prepared precursor compound was placed in a separate canister and heated to 140°C. The MoCl5 precursor was introduced into the deposition chamber using 100 sccm of Ar carrier for 5 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 5.0 Torr.

[0292] Next, the prepared thin film forming material was placed in a canister and supplied to the chamber at a flow rate of 1000 sccm using a mass flow controller (MFC) at room temperature. The thin film forming material vaporized in a vapor phase from the vaporizer was introduced into the deposition chamber loaded with the substrate for 2 seconds to perform a reduction reaction, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled at 5.0 Torr. The deposition temperature was maintained at 400 to 600°C, and this process was repeated 30 to 300 times to form a self-limiting atomic layer thin film with a thickness of 10 nm.

[0293]

[0294] Comparative Example 7

[0295] NH3 was used as a reactant for the nitriding process, and the ALD deposition process was performed using TiCl4 precursor as a precursor compound.

[0296] First, the prepared precursor compound was placed in a separate canister and heated to 50°C. The TiCl4 precursor was introduced into the deposition chamber using an Ar carrier of 100 sccm for 3 seconds, and then argon gas was supplied at 3000 sccm for 5 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.0 Torr.

[0297] Next, 1000 sccm of NH3 was supplied to the chamber to inject the reaction gas. This process was repeated 50 to 150 times at a deposition temperature of 500 to 550°C to form a self-limiting atomic layer thin film with a thickness of 10 nm.

[0298]

[0299] Comparative Example 8

[0300] NH3 was used as a reactant for the nitriding process, and NbF5 precursor was used as a precursor compound to perform the ALD deposition process. The process was performed in the same manner as Example 8, except that the low-temperature deposition material was supplied.

[0301]

[0302] Comparative Example 9

[0303] NH3 was used as a reactant for the nitriding process, and MoO2Cl2 precursor was used as a precursor compound to perform the ALD deposition process. The process was performed in the same manner as Example 9, except that the low-temperature deposition material was supplied.

[0304]

[0305] Comparative Example 10

[0306] An ALD deposition process was performed using H2 as a reactant and a precursor compound having the following chemical formula MoCl5.

[0307]

[0308] First, the prepared precursor compound was placed in a separate canister and heated to 140°C. The MoCl5 precursor was introduced into the deposition chamber using 100 sccm of Ar carrier for 5 seconds, and then argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 5.0 Torr.

[0309] Next, H2 was used as a reactant, and a reduction reaction was performed by supplying 1000 sccm for 5 seconds, after which argon gas was supplied at 5000 sccm for 10 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 5.0 Torr. The deposition temperature was maintained at 400°C.

[0310]

[0311] [Example Exam]

[0312] For each of the obtained thin films of Examples 1 to 9 and Comparative Examples 1 to 10, the impurity content, the type and content of elements constituting the material surface, the deposition rate, the crystal structure, the directionality, etc. were analyzed in the following manner.

[0313] * SIMS (Secondary-ion mass spectrometry) C impurity: The C impurity value was confirmed in the SIMS graph by considering the C impurity content (counts) when the thin film was axially dug into with an ion sputter and the sputter time was 50 seconds, which is low in contamination on the substrate surface layer.

[0314] * AES (Auger electron spectroscopy): A focused electron beam is incident on the surface of a material, and the energy of the emitted Auger electrons is measured to analyze the type and content of elements constituting the surface of the material.

[0315] *Deposition rate (GPC) measurement: The deposition rate (GPC) was measured for each of the thin films obtained in Examples 1 to 9 and Comparative Examples 1 to 9 in the following manner. Specifically, the deposition rate of thin films with a thickness of 3 to 30 nm was measured using an ellipsometer, and the unit is Å / cycle.

[0316] * Grazing-incidence angle (incident angle, θ=3°) X-ray diffractometry: Surface diffraction analysis was performed using Cu-Kα X-ray to confirm information such as crystal structure and orientation.

[0317]

[0318] As shown in Table 1 above, it can be confirmed that when the HI thin film forming material process according to the present invention is used alone or the HI thin film forming material and NH3 reaction gas are used together, the amount of C impurities generated when the NH3 reaction gas is used alone is drastically reduced.

[0319] In addition, as seen in Examples 1 and 2, it was confirmed through AES analysis that C impurities were reduced to 0% during thin film formation, and according to SIMS results, it was confirmed that the number of C ions detected was reduced by more than 91%.

[0320] Furthermore, the increase in film density from 6.0 to 6.8 indicates that a very high-quality MoN film was formed.

[0321]

[0322] [Correction pursuant to Rule 91, May 31, 2024] [Table 2]

[0323] As shown in Table 2 above, when the HI thin film forming material process according to the present invention is used alone, or when the HI thin film forming material and NH3 reaction gas are used together, the resistivity of the formed thin film is drastically reduced compared to when the NH3 reaction gas is used alone, and it was shown that the C impurity was also most effectively reduced when the HI thin film forming material was used alone in the order of Comparative Example 2 > Example 4 > Example 3.

[0324]

[0325] [Correction pursuant to Rule 91, May 31, 2024] [Table 3]

[0326] As shown in Table 3 above, when the HI thin film forming material according to the present invention is used, the resistivity of the formed thin film is drastically reduced and the deposition rate is increased by more than three times compared to when NH3 reaction gas is used alone.

[0327] In particular, XRD analysis was performed according to process temperature and the results are shown in Figure 2 below. Figure 2 is a graph of XRD analysis according to process temperature between Example 5 of the present invention and Comparative Example 3.

[0328] As shown in Figure 2 below, Example 5 shows that a pure Mo metal thin film was formed.

[0329] Furthermore, the temperature-dependent AES analysis results of Example 5 are shown in Figure 1 below.

[0330] Figure 1 is a graph showing the AES analysis results according to temperature in Example 5 of the present invention. As shown in Figure 1 below, changes in the types and contents of constituent elements according to process temperature were confirmed.

[0331]

[0332]

[0333] As shown in Table 4 above, when the HI thin film forming material according to the present invention is used, the resistivity of the thin film formed is drastically reduced compared to when only NH3 reaction gas is used, and the deposition rate is also increased by more than twice.

[0334] In particular, XRD analysis was performed and the results are shown in Figure 3 below. Figure 3 is an XRD analysis graph between Example 6 of the present invention and Comparative Example 4.

[0335] As shown in Figure 3 below, it can be seen that a pure Mo metal thin film was partially formed in Example 6.

[0336]

[0337]

[0338] As shown in Table 5 above, it can be seen that when the HI thin film forming material according to the present invention is used, a Mo metal thin film with low resistivity is formed even at a low temperature of 400°C. In addition, it can be seen that in the case of iodine bonded to carbon, a Mo thin film is formed without carbon impurities when I-1 with low bond dissociation energy is utilized. However, in the case of CH3I with a strong carbon-iodine bond of 250 kJ / mol, not only did the resistivity increase by more than 10 times, but it was also found that carbon impurities were present within the thin film. The cause of the increase in resistivity is carbon, which acts as an impurity within the thin film.

[0339] The residual action mechanism of thin film impurities is that when the bond dissociation energy of carbon and iodine is large, the bond of iodine does not dissociate or the dissociated carbon molecules are strongly bound to the substrate surface and are not desorbed.

[0340] Meanwhile, in Comparative Example 10 using H2 with high binding energy, a Mo thin film was not formed at a low temperature of 400°C.

[0341]

[0342] Furthermore, the results of calculating the bond dissociation energy of the carbon or hydrogen compound combined with iodine in Example 8 are shown in Table 6 below.

[0343] [Correction pursuant to Rule 91, May 31, 2024] [Table 6]

[0344] Meanwhile, CH3I used in Comparative Example 6 had a bond dissociation energy of 250.15 kJ / mol.

[0345] The reaction activation energies required to reduce the CO ligand and NO ligand of the Mo(CO)6 precursor and (EtCp)Mo(CO)2(NO) precursor in Example 8 and Comparative Example 5, respectively, were compared in the case of H2 and HI, and are shown in Figures 4 and 5 below.

[0346] As shown in Figures 4 and 5 below, the energy required to reduce CO ligands using H2 material in Mo(CO)6 precursor is 341.67 KJ / mol, but when HI is used, it is 157.12 KJ / mol, which is an extremely low activation energy. This result shows that reduction is possible even at a lower process temperature without C and O impurities.

[0347] The energy required to reduce NO ligand using H2 material in (EtCp)Mo(CO)2(NO) precursor is 323.77 KJ / mol, but when HI is used, it is 82.91 KJ / mol, which is an extremely low activation energy. This result shows that reduction is possible even at lower process temperatures without N and O impurities.

[0348] The bond dissociation energies of Mo precursors suitable for low-temperature processes are shown in Table 7 below.

[0349]

[0350] [Correction pursuant to Rule 91, May 31, 2024] [Table 7]

[0351] As shown in Table 7 above, when the bond dissociation energy of the ligand bonded to Mo is 350 KJ / mol or less, it can be confirmed that reduction occurs at 400°C or less.

[0352]

[0353] Table 8 below shows the resistivity results according to the bond dissociation energy among the inventive materials used to reduce the reaction activation energy between TiCl4 and NH3 reaction gases during the formation of a TiN thin film.

[0354]

[0355] [Correction pursuant to Rule 91, May 31, 2024] [Table 8]

[0356] As shown in Table 8 above, except for CH3I2, which does not have a carbon-iodine bond, in the case of iodine bonded to carbon, only materials with iodine bonded to carbon of 242 kJ / mol or less showed an improvement in deposition rate as well as an improvement in resistivity.

[0357] In particular, it was confirmed that the range of resistivity degradation increases as the carbon and iodine bond dissociation energy increases.

[0358]

[0359] As shown in Table 9 above, in each low-temperature process, it was confirmed that the deposition rate and resistivity were improved according to the use of low-temperature deposition materials when forming a metal nitride film, and that the impurities remaining in the thin film were reduced due to insufficient reduction of the precursor ligand in the low-temperature process.

[0360] As a result, it was confirmed that it is suitable for improving the film quality of a low-temperature deposition film, such as electrical characteristics and crystallinity, while preventing and inhibiting the inflow of film impurities caused by ligands such as carbon by using a predetermined thin film forming material that can perform a catalytic reaction or reduction reaction at a relatively low process temperature so that the precursor compound adsorbed on the surface of a substrate loaded inside the chamber is not thermally decomposed.

Claims

1. As a low-temperature deposition material for wiring metal, metal with a melting point of 350 ℃ or lower, or wiring metal diffusion barrier film, A low-temperature deposition material characterized by comprising at least one selected from a compound having a direct bond between hydrogen (H) and iodine, a compound having a direct bond between carbon (C) and iodine, and a compound having a direct bond between a halogen element (F, Cl, Br) and iodine.

2. In paragraph 1, The above wiring metal or metal having a melting point of 350°C or lower is selected from Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In and Ga. The above wiring metal diffusion barrier film is a low-temperature deposition material characterized in that a transition metal nitride film of Ti, Ta, Ni, Mo, Nb, Zr, V, W or a combination of two or more metals is selected.

3. In paragraph 1, A low-temperature deposition material characterized in that the compound having a direct bond between hydrogen (H) and iodine has a total binding energy of 305 to 325 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP).

4. In paragraph 1, A low-temperature deposition material characterized in that the compound having a direct bond between carbon (C) and iodine has a total binding energy of 165 to 242 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP).

5. In paragraph 1, A low-temperature deposition material characterized in that the compound having a direct bond between the above halogen element (F, Cl, Br) and iodine has a total binding energy of 50 to 160 kJ / mol calculated using the basis set (iodine: LanL2DZ, carbon, hydrogen element: 6-31+G(dp)) of the Gaussian 16 program (DFT-D3 / B3LYP).

6. [Revised 31.05.2024 by Rule 91] In paragraph 1, the low-temperature deposition material is characterized by being at least one selected from compounds represented by the following chemical formulas 1-1 to 1-11. [Chemical formulas 1-1 to 1-11] 7. A method for forming a low-temperature deposition film, characterized by including a step of depositing a deposition film using a low-temperature deposition material of any one of claims 1 to 6.

8. In paragraph 7, A low-temperature deposition film forming method, characterized in that the above deposition film is a metal film and / or a metal nitride film.

9. In paragraph 7, A low-temperature deposition film forming method characterized in that the method comprises a step of forming a deposition film through a reduction reaction by injecting a precursor compound and the low-temperature deposition material into a chamber and adsorbing them onto a substrate surface.

10. In paragraph 7, A low-temperature deposition film forming method characterized by omitting the step of injecting hydrogen as a reaction gas and causing a reduction reaction.

11. In paragraph 7, A low-temperature deposition film forming method characterized in that the above low-temperature deposition film forming method includes a post-treatment step of purging the inside of the chamber with a purge gas.

12. In paragraph 9 or 11, A low-temperature deposition film forming method, characterized in that the chamber is an ALD chamber, a CVD chamber, a PEALD chamber, or a PECVD chamber.

13. In paragraph 7, A method for forming a low-temperature deposition film, characterized in that the low-temperature deposition film is a laminated film of at least one metal selected from the group consisting of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, and Ga.

14. In paragraph 7, A method for forming a low-temperature deposition film, characterized in that the low-temperature deposition film has a resistivity within a range of 5 μΩ·cm to 1000 μΩ·cm.

15. In paragraph 9, The above precursor compound is a molecule having at least one selected from the group consisting of Mo, W, Ru, Cu, Rh, Pb, Cd, Sn, Bi, In, and Ga as a central metal atom (M) and at least one ligand composed of C, N, O, H, X (halogen), and a method for forming a low-temperature deposition film, characterized in that the compound is a compound having a bond dissociation energy between the central metal atom and the ligand of 350 kJ / mol or less, calculated using the basis set of the Gaussian 16 program (DFT-D3 / B3LYP (central metal, iodine: LanL2DZ, C, N, O, H, X: 6-31+G(dp)) in order to reduce the central metal atom at a low process temperature of 400 degrees or less.

16. In paragraph 9, A low-temperature deposition film forming method characterized in that the substrate is heated to 100 to 700°C.

17. A semiconductor substrate characterized by including a low-temperature deposition film manufactured by the low-temperature deposition film forming method of Article 7.

18. A semiconductor device characterized by including a semiconductor substrate according to claim 17.

Citation Information

Patent Citations

  • Metal precursor for low temperature deposition, method of forming metal layer using the precursor and method of fabricating phase-change memory device using the precursor

    KR100871692B1

  • A microspeaker module

    KR1020230114816A

  • Apparatus and method for reading temperature with high accuracy using pseudo-random data

    KR102423479B1

  • Method for manufacturing hole transport layer of perovskite solar cell

    WO2021177800A2