Thermoplastic resin composition and molded articled manufactured therefrom

The thermoplastic resin composition, combining polycarbonate resin with specific additives, addresses the challenges of flame retardancy and physical property maintenance, achieving enhanced dimensional stability, impact resistance, and appearance in molded articles.

WO2024205350A1PCT designated stage expired Publication Date: 2024-10-03LOTTE CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/095031
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-01-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Thermoplastic resin compositions face challenges in achieving excellent flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, and appearance properties, particularly when fillers like glass fiber, talc, and mica are used, as their excessive content can lead to deterioration of physical properties.

Method used

A thermoplastic resin composition comprising polycarbonate resin, polyester resin, phosphate compounds, phosphazene compounds, talc, and mica, with specific weight ratios and particle sizes, which enhances flame retardancy, dimensional stability, isotropy, impact resistance, and rigidity while maintaining appearance properties.

Benefits of technology

The composition achieves V-0 or higher flame resistance, linear expansion coefficients between 15 to 36 μm/m·°C, isotropy of 1.1 to 1.3, notched Izod impact strength of 5 to 20 kgf·cm/cm, and flexural modulus of 70,000 to 140,000 kgf/cm², ensuring superior physical properties and appearance characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024095031_03102024_PF_FP_ABST
    Figure KR2024095031_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A thermoplastic resin composition of the present invention comprises: about 100 parts by weight of a polycarbonate resin; about 0.5 to 15 parts by weight of a polyester resin; about 1 to 20 parts by weight of a phosphate compound; about 1 to 15 parts by weight of a phosphazene compound; about 1 to 15 parts by weight of talc having an average particle size (D50) of about 7 to 20 μm; about 10 to 40 parts by weight of flat plate-shaped glass fiber; and about 1 to 20 parts by weight of mica having an average particle size (D50) of about 250 to 450 μm. The thermoplastic resin composition has excellent flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, exterior characteristics, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic resin composition and molded article manufactured therefrom

[0001] The present invention relates to a thermoplastic resin composition and a molded article manufactured therefrom. More specifically, the present invention relates to a thermoplastic resin composition exhibiting excellent flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, and appearance properties, and a molded article manufactured therefrom.

[0002]

[0003] As an engineering plastic, polycarbonate resin boasts excellent impact resistance, heat resistance, dimensional stability, weather resistance, flame retardancy, electrical properties, and transparency, making it useful for housing electrical and electronic products and interior and exterior materials for other office equipment. Furthermore, it has the ability to enhance various physical properties through the application of various fillers.

[0004] However, fillers such as glass fiber, talc, mica, and wollastonite applied to improve the dimensional stability and rigidity of polycarbonate resin may have differences in physical properties depending on the type, and there is a concern that the appearance characteristics may be deteriorated due to filler protrusion, etc., and when a certain amount is added, the physical properties may actually be deteriorated.

[0005] Therefore, there is a need to develop a thermoplastic resin composition that has excellent flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, and appearance properties without these problems.

[0006] The background technology of the present invention is disclosed in Korean Patent Publication No. 10-2011-0059886, etc.

[0007]

[0008] The purpose of the present invention is to provide a thermoplastic resin composition having excellent flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance properties, etc.

[0009] Another object of the present invention is to provide a molded article formed from the thermoplastic resin composition.

[0010] The above and other objects of the present invention can all be achieved by the present invention described below.

[0011]

[0012] 1. One aspect of the present invention relates to a thermoplastic resin composition. The thermoplastic resin composition comprises: about 100 parts by weight of a polycarbonate resin; about 0.5 to about 15 parts by weight of a polyester resin; about 1 to about 20 parts by weight of a phosphate compound; about 1 to about 15 parts by weight of a phosphazene compound; about 1 to about 15 parts by weight of talc having an average particle size (D50) of about 7 to about 20 μm; about 10 to about 40 parts by weight of flat glass fibers; and about 1 to about 20 parts by weight of mica having an average particle size (D50) of about 250 to about 450 μm.

[0013] 2. In the above 1 specific example, the polyester resin may include at least one of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polytrimethylene terephthalate, and polycyclohexylene terephthalate.

[0014] 3. In the above 1 or 2 specific examples, the flat glass fiber may have an aspect ratio of a cross section (major axis of the cross section / minor axis of the cross section) of about 1.5 to about 10, a minor axis of the cross section of about 2 to about 10 ㎛, and a length before processing of about 1 to about 30 mm.

[0015] 4. In the above specific examples 1 to 3, the weight ratio of the phosphate compound and the phosphazene compound may be about 1:0.3 to about 1:2.

[0016] 5. In the above specific examples 1 to 4, the weight ratio of the talc and the flat glass fiber may be about 1:2 to about 1:8.

[0017] 6. In the above 1 to 5 specific examples, the weight ratio of the talc and the mica may be about 1: about 0.5 to about 1:2.

[0018] 7. In the above 1 to 6 specific examples, the weight ratio of the flat glass fiber and the mica may be about 1:0.1 to about 1:0.6.

[0019] 8. In the above 1 to 7 specific examples, the thermoplastic resin composition may have a flame retardancy of V-0 or higher in a 1.5 mm thick injection molded specimen measured by the UL-94 vertical test method.

[0020] 9. In the above 1 to 8 specific examples, the thermoplastic resin composition may have a linear expansion coefficient of about 15 to about 36 ㎛ / m·℃ of an injection molded specimen measuring 10 mm × 10 mm × 3.2 mm, measured while heating at a rate of 5°C / min from -20°C to 100°C according to ASTM D696.

[0021] 10. In the above 1 to 9 specific examples, the thermoplastic resin composition may have an isotropy of about 1.1 to about 1.3 calculated according to the following formula 1:

[0022] [Formula 1]

[0023] Isotropy = TD coefficient of linear expansion / MD coefficient of linear expansion

[0024] In the above equation 1, the TD coefficient of linear expansion is the coefficient of linear expansion in the vertical direction (TD: transverse direction) of an injection molded specimen measuring 10 mm × 10 mm × 3.2 mm, measured while heating from -20°C to 100°C at a rate of 5°C / min according to ASTM D696, and the MD coefficient of linear expansion is the coefficient of linear expansion in the flow direction (MD: machine direction) of the injection molded specimen.

[0025] 11. In the above 1 to 10 specific examples, the thermoplastic resin composition may have a notched Izod impact strength of about 5 to about 20 kgf·cm / cm for a 1 / 8" thick specimen measured according to ASTM D256.

[0026] 12. In the above 1 to 11 specific examples, the thermoplastic resin composition has a flexural modulus of about 70,000 to about 140,000 kgf / cm of a 6.4 mm thick specimen measured under 2.8 mm / min conditions according to ASTM D790. 2 It could be.

[0027] 13. Another aspect of the present invention relates to a molded article. The molded article is characterized in that it is formed from a thermoplastic resin composition according to any one of 1 to 12.

[0028] 14. In the above 13 specific examples, the molded product may be a plastic member of an electronic device housing including a metal frame and a plastic member in contact with at least one surface of the metal frame.

[0029]

[0030] The present invention has the effect of providing a thermoplastic resin composition having excellent flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, etc., and a molded article formed therefrom.

[0031]

[0032] FIG. 1 schematically illustrates a cross-section of an electronic device housing according to one specific example of the present invention.

[0033]

[0034] Hereinafter, the present invention will be described in detail as follows.

[0035] A thermoplastic resin composition according to the present invention comprises (A) a polycarbonate resin; (B) a polyester resin; (C) a phosphate compound; (D) a phosphazene compound; (E) talc; (F) flat glass fibers; and (G) mica.

[0036] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.

[0037]

[0038] (A) Polycarbonate resin

[0039] As a polycarbonate resin according to one specific example of the present invention, a polycarbonate resin used in a conventional thermoplastic resin composition can be used. For example, an aromatic polycarbonate resin produced by reacting a diphenol (aromatic diol compound) with a precursor such as phosgene, halogen formate, or carbonic diester can be used.

[0040] In specific examples, the diphenols include, but are not limited to, 4,4'-biphenol, 2,2-bis(4-hydroxyphenyl)propane, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(3-chloro-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, etc. For example, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, or 1,1-bis(4-hydroxyphenyl)cyclohexane can be used, and specifically, 2,2-bis(4-hydroxyphenyl)propane, also called bisphenol-A, can be used.

[0041] In a specific example, the polycarbonate resin may be one having a branched chain, and for example, a branched polycarbonate resin may be used that is prepared by adding 0.05 to 2 mol% of a trivalent or higher polyfunctional compound, specifically, a compound having a trivalent or higher phenol group, to the total diphenols used in the polymerization.

[0042] In specific examples, the polycarbonate resin may be used in the form of a homopolycarbonate resin, a copolycarbonate resin, or a blend thereof. In addition, the polycarbonate resin may be partially or entirely replaced with an aromatic polyester-carbonate resin obtained by polymerization in the presence of an ester precursor, such as a difunctional carboxylic acid.

[0043] In a specific example, the polycarbonate resin may have a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) of about 10,000 to about 200,000 g / mol, for example, about 15,000 to about 80,000 g / mol. Within this range, the thermoplastic resin composition may have excellent fluidity (processability), etc.

[0044]

[0045] (B) Polyester resin

[0046] According to one specific example of the present invention, a polyester resin can be applied to a polycarbonate resin together with a phosphate compound, a phosphazene compound, talc, flat glass fiber, mica, etc., to improve the flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, and the balance of these physical properties, etc. of a thermoplastic resin composition. A polyester resin used in a typical thermoplastic resin composition can be used. For example, the polyester resin may include, as a dicarboxylic acid component, aromatic dicarboxylic acids such as terephthalic acid (TPA), isophthalic acid (IPA), 1,2-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, and 2,7-naphthalene dicarboxylic acid, dimethyl terephthalate (DMT), dimethyl isophthalate, dimethyl-1,2-naphthalate, Aromatic dicarboxylates such as dimethyl-1,5-naphthalate, dimethyl-1,7-naphthalate, dimethyl-1,8-naphthalate, dimethyl-2,3-naphthalate, dimethyl-2,6-naphthalate, and dimethyl-2,7-naphthalate can be obtained by polycondensation with diol components such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2,2-dimethyl-1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and cyclic alkylenediol.

[0047] In a specific example, the polyester resin may include one or more of polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT), and polycyclohexylene terephthalate. For example, the polyester resin may be polyethylene terephthalate, polybutylene terephthalate, or a combination thereof.

[0048] In a specific example, the polyester resin of the present invention may be dissolved in an o-chlorophenol solution (concentration: 0.5 g / dl) and have an intrinsic viscosity measured at 25°C using an Ubbelohde viscometer (capillary viscometer) of about 0.6 to about 1.5 dl / g, for example, about 0.7 to about 1.3 dl / g. Within this range, the thermoplastic resin composition may have excellent processability, dimensional stability, and the like.

[0049] In a specific example, the polyester resin may be included in an amount of about 0.5 to about 15 parts by weight, for example, about 1 to about 10 parts by weight, based on about 100 parts by weight of the polycarbonate resin. If the content of the polyester resin is less than about 0.5 parts by weight based on about 100 parts by weight of the polycarbonate resin, there is a concern that the dimensional stability, isotropy, etc. of the thermoplastic resin composition may deteriorate, and if it exceeds about 15 parts by weight, there is a concern that the flame retardancy, isotropy, impact resistance, etc. of the thermoplastic resin composition may deteriorate.

[0050]

[0051] (C) Phosphate compound

[0052] A phosphate compound according to one specific example of the present invention can be applied to a polycarbonate resin together with a polyester resin, a phosphazene compound, talc, flat glass fiber, mica, etc., to improve the flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, and physical property balance thereof of a thermoplastic resin composition. Phosphate compounds used in conventional flame retardant thermoplastic resin compositions can be used.

[0053] In specific examples, the phosphate compound may be exemplified by diaryl phosphates such as diphenyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, tri(2,6-dimethylphenyl)phosphate, tri(2,4,6-trimethylphenyl)phosphate, tri(2,4-ditertiarybutylphenyl)phosphate, tri(2,6-dimethylphenyl)phosphate, etc., and may be exemplified by bisphenol-A bis(diphenylphosphate), resorcinol bis(diphenylphosphate), resorcinol bis[bis(2,6-dimethylphenyl)phosphate], resorcinol bis[bis(2,4-ditertiarybutylphenyl)phosphate], hydroquinone bis[bis(2,6-dimethylphenyl)phosphate], hydroquinone bis[bis(2,4-ditertiarybutylphenyl)phosphate], etc. However, this is not limited thereto. These may be applied singly or in the form of a mixture of two or more. For example, the phosphate compound may be oligomeric bisphenol-A diphosphate, etc.

[0054] In a specific example, the phosphate compound may be included in an amount of about 1 to about 20 parts by weight, for example, about 5 to about 15 parts by weight, based on about 100 parts by weight of the polycarbonate resin. If the content of the phosphate compound is less than about 1 part by weight based on about 100 parts by weight of the polycarbonate resin, there is a concern that the flame retardancy, appearance characteristics (injection moldability), etc. of the thermoplastic resin composition may deteriorate, and if it exceeds about 20 parts by weight, there is a concern that the isotropy, impact resistance, etc. of the thermoplastic resin composition may deteriorate.

[0055]

[0056] (D) Phosphazene compound

[0057] A phosphazene compound according to one specific example of the present invention can be applied to a polycarbonate resin together with a polyester resin, a phosphate compound, a phosphazene compound, talc, flat glass fiber, mica, etc., to improve the flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, and the balance of these physical properties of a thermoplastic resin composition. A phosphazene compound used in a typical flame retardant thermoplastic resin composition can be used.

[0058] In a specific example, the phosphazene compound may include a phosphazene compound represented by the following chemical formula 1.

[0059] [Chemical Formula 1]

[0060]

[0061] In the above chemical formula 1, R1, R2, R3, R4, R5 and R6 are each independently a hydrogen atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 7 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted heterocycloalkyl group having 2 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an aryl group or aryloxy group having 6 to 20 carbon atoms, a heteroaryl group having about 5 to about 20 carbon atoms, a substituted or unsubstituted alkoxycarbonylalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted carbonylalkyl group having about 2 to about 10 carbon atoms, an amino group or a hydroxy group.

[0062] Here, the above “substitution” means that a hydrogen atom is replaced with a substituent such as an alkyl group having 1 to 10 carbon atoms, a halogen atom, a nitro group, a cyano group, a hydroxy group, an amino group, an aryl group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a heterocycloalkyl group having 3 to 10 carbon atoms, a heteroaryl group having 4 to 10 carbon atoms, or a combination thereof.

[0063] In addition, the substituents including the above "alkyl", "alkoxy" and other "alkyl" moieties include both straight-chain and branched forms, "alkenyl" includes both straight-chain and branched forms having 2 to 8 carbon atoms and containing at least one double bond, and the above "cycloalkyl" includes all saturated monocyclic or saturated bicyclic ring structures having 3 to 20 carbon atoms. The above "aryl" is an organic radical derived from an aromatic hydrocarbon by removal of one hydrogen atom, and includes a single or fused ring system, suitably containing 4 to 7, preferably 5 or 6 ring atoms in each ring. Specifically, phenyl, naphthyl, biphenyl, tolyl, etc. can be exemplified.

[0064] The above "heterocycloalkyl" means a cycloalkyl group containing 1 to 3 heteroatoms selected from N, O, and S as saturated cyclic hydrocarbon skeletal atoms, and the remaining saturated monocyclic or bicyclic ring skeletal atoms are carbon, and is selected from pyrrolidinyl, azetidinyl, pyrazolidinyl, oxazolidinyl, piperidinyl, piperazinyl, morpholinyl, thiomorpholinyl, thiazolidinyl, hydantoinyl, valerolactamyl, oxiranyl, oxetanyl, dioxolanyl, dioxanyl, oxathiolanyl, oxathianyl, dithianyl, dihydrofuranyl, tetrahydrofuranyl, dihydropyranyl, tetrahydropyranyl, tetrahydropyridinyl, tetrahydropyrimidinyl, tetrahydrothiophenyl, tetrahydrothiopyranyl, diazepanyl, Examples include azepanil.

[0065] The above "heteroaryl" refers to an aryl group having 1 to 3 heteroatoms selected from N, O, and S as aromatic ring skeletal atoms, and the remaining aromatic ring skeletal atoms are carbon, and the heteroaryl group includes a divalent aryl group in which the heteroatoms in the ring are oxidized or quaternized to form, for example, an N-oxide or a quaternary salt. Specifically, examples thereof include furyl, thienyl, pyrrolyl, pyranyl, imidazolyl, pyrazolyl, thiazolyl, thiadiazolyl, isothiazolyl, isoxazolyl, oxazolyl, oxadiazolyl, triazinyl, tetrazinyl, triazolyl, tetrazolyl, furazanyl, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, and the like.

[0066] In a specific example, the phosphazene compound may be included in an amount of about 1 to about 15 parts by weight, for example, about 5 to about 10 parts by weight, relative to about 100 parts by weight of the polycarbonate resin. If the content of the phosphazene compound is less than about 1 part by weight relative to about 100 parts by weight of the polycarbonate resin, there is a concern that the flame retardancy, etc. of the thermoplastic resin composition may be reduced, and if it exceeds about 15 parts by weight, there is a concern that the isotropy, impact resistance, etc. of the thermoplastic resin composition may be reduced.

[0067] In a specific example, the weight ratio of the phosphate compound and the phosphazene compound (phosphate compound: phosphazene compound) may be from about 1:0.3 to about 1:2, for example from about 1:0.4 to about 1:1.7. In this range, the flame retardancy, etc. of the thermoplastic resin composition may be more excellent.

[0068]

[0069] (E) Talk

[0070] According to one specific example of the present invention, talc can be applied to a polycarbonate resin together with a polyester resin, a phosphate compound, a phosphazene compound, a phosphazene compound, a flat glass fiber, and mica, thereby improving the flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, and balance of these physical properties of a thermoplastic resin composition. Talc having an average particle size (D50) of about 7 to about 20 ㎛ can be used.

[0071] In a specific example, the talc is a plate-shaped filler and may have an average particle size (D50) of about 7 to about 20 μm, for example, about 8 to about 14 μm, as measured by a laser particle size analyzer (manufacturer: Beckman Coulter, device name: LS 13 320). When the average particle size (D50) of the talc is less than about 7 μm, there is a concern that the dimensional stability, impact resistance, etc. of the thermoplastic resin composition may deteriorate, and when it exceeds about 20 μm, there is a concern that the impact resistance, appearance characteristics, etc. of the thermoplastic resin composition may deteriorate.

[0072] In a specific example, the talc may be included in an amount of about 1 to about 15 parts by weight, for example, about 5 to about 10 parts by weight, based on about 100 parts by weight of the polycarbonate resin. If the amount of the talc is less than about 1 part by weight based on about 100 parts by weight of the polycarbonate resin, there is a concern that the isotropy, etc. of the thermoplastic resin composition may be reduced, and if it exceeds about 15 parts by weight, there is a concern that the flame retardancy, impact resistance, etc. of the thermoplastic resin composition may be reduced.

[0073]

[0074] (F) Flat glass fiber

[0075] According to one specific example of the present invention, a flat type glass fiber can be applied to a polycarbonate resin together with a polyester resin, a phosphate compound, a phosphazene compound, a phosphazene compound, talc, mica, etc., thereby improving the flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, and the balance of these physical properties, etc. of a thermoplastic resin composition.

[0076] In a specific example, the flat glass fiber may have a rectangular cross-section. For example, the flat glass fiber may have an aspect ratio (major axis of the cross-section / minor axis of the cross-section) of the cross-section measured by a scanning electron microscope (manufacturer: JEOL, device name: JSM-6390A) of about 1.5 to about 10, for example, about 2 to about 8, the minor axis of the cross-section may be about 2 to about 10 ㎛, for example, about 4 to about 8 ㎛, and the length before processing may be about 1 to about 5 mm, for example, about 2 to about 4 mm. In the above range, the rigidity, appearance characteristics, etc. of the thermoplastic resin composition may be excellent.

[0077] In a specific example, the flat glass fiber may be treated with a conventional surface treatment agent.

[0078] In a specific example, the flat glass fiber may be included in an amount of about 10 to about 40 parts by weight, for example, about 20 to about 40 parts by weight, relative to about 100 parts by weight of the polycarbonate resin. If the content of the flat glass fiber is less than about 10 parts by weight relative to about 100 parts by weight of the polycarbonate resin, there is a concern that the dimensional stability, isotropy, rigidity, etc. of the thermoplastic resin composition may be deteriorated, and if it exceeds about 40 parts by weight, there is a concern that the flame retardancy, dimensional stability, isotropy, etc. of the thermoplastic resin composition may be deteriorated.

[0079] In a specific example, the weight ratio of the talc and the flat glass fiber (talc: flat glass fiber) may be from about 1:2 to about 1:8, for example, from about 1:2.5 to about 1:7. In this range, the dimensional stability, appearance properties, etc. of the thermoplastic resin composition may be better.

[0080]

[0081] (G) Mica

[0082] According to one specific example of the present invention, mica is applied to a polycarbonate resin together with a polyester resin, a phosphate compound, a phosphazene compound, a phosphazene compound, talc, and flat glass fibers, thereby improving the flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, and balance of these physical properties of a thermoplastic resin composition. Mica having an average particle size (D50) of about 250 to about 450 ㎛ can be used.

[0083] In a specific example, the mica may have an average particle size (D50) of about 250 to about 450 μm, for example, about 300 to about 400 μm, as measured by a particle size measuring device (Malvern mastersizer 3000). If the average particle size (D50) of the mica is less than about 250 μm, there is a concern that the dimensional stability, isotropy, etc. of the thermoplastic resin composition may deteriorate, and if it exceeds about 450 μm, there is a concern that the impact resistance, etc. of the thermoplastic resin composition may deteriorate.

[0084] In a specific example, the mica may be included in an amount of about 1 to about 20 parts by weight, for example, about 5 to about 15 parts by weight, relative to about 100 parts by weight of the polycarbonate resin. If the content of the mica is less than about 1 part by weight relative to about 100 parts by weight of the polycarbonate resin, there is a concern that the isotropy, etc. of the thermoplastic resin composition may be reduced, and if it exceeds about 20 parts by weight, there is a concern that the flame retardancy, impact resistance, etc. of the thermoplastic resin composition may be reduced.

[0085] In a specific example, the weight ratio of the talc and the mica (talc: mica) may be from about 1:0.5 to about 1:2, for example from about 1:0.6 to about 1:1.9. In this range, the dimensional stability, isotropy, appearance characteristics, etc. of the thermoplastic resin composition may be more excellent.

[0086] In a specific example, the weight ratio of the flat glass fiber and the mica (flat glass fiber: mica) may be from about 1:0.1 to about 1:0.6, for example from about 1:0.1 to about 1:0.5. In this range, the dimensional stability, isotropy, rigidity, etc. of the thermoplastic resin composition may be more excellent.

[0087]

[0088] A thermoplastic resin composition according to one embodiment of the present invention may further include additives included in conventional thermoplastic resin compositions. Examples of the additives include, but are not limited to, antioxidants, anti-drip agents, lubricants, release agents, nucleating agents, antistatic agents, stabilizers, pigments, dyes, and mixtures thereof. When the additives are used, the content thereof may be about 0.001 to about 40 parts by weight, for example, about 0.1 to about 10 parts by weight, based on about 100 parts by weight of the polycarbonate resin.

[0089]

[0090] A thermoplastic resin composition according to one specific example of the present invention may be in the form of pellets obtained by mixing the above components and melt-extruding them at about 200 to about 300°C, for example, about 230 to about 290°C, using a conventional twin-screw extruder.

[0091] In a specific example, the thermoplastic resin composition may have a flame retardancy of V-0 or higher in a 1.5 mm thick injection molded specimen measured by the UL-94 vertical test method.

[0092] In a specific example, the thermoplastic resin composition may have a linear expansion coefficient of about 15 to about 36 µm / m·°C, for example, about 16 to about 35 µm / m·°C, of ​​an injection-molded specimen measuring 10 mm × 10 mm × 3.2 mm, measured while heating at a rate of 5°C / min from -20°C to 100°C according to ASTM D696.

[0093] In a specific example, the thermoplastic resin composition may have an isotropy of about 1.1 to about 1.3 calculated according to the following equation 1:

[0094] [Formula 1]

[0095] Isotropy = TD coefficient of linear expansion / MD coefficient of linear expansion

[0096] In the above equation 1, the TD coefficient of linear expansion is the coefficient of linear expansion in the vertical direction (TD: transverse direction) of an injection molded specimen measuring 10 mm × 10 mm × 3.2 mm, measured while heating from -20°C to 100°C at a rate of 5°C / min according to ASTM D696, and the MD coefficient of linear expansion is the coefficient of linear expansion in the flow direction (MD: machine direction) of the injection molded specimen.

[0097] In a specific example, the thermoplastic resin composition may have a notched Izod impact strength of about 5 to about 20 kgf·cm / cm, for example, about 6 to about 15 kgf·cm / cm, of a 1 / 8" thick specimen measured according to ASTM D256.

[0098] In a specific example, the thermoplastic resin composition has a flexural modulus of about 70,000 to about 140,000 kgf / cm of a 6.4 mm thick specimen measured under 2.8 mm / min conditions according to ASTM D790. 2 , for example, about 75,000 to about 130,000 kgf / cm 2 It could be.

[0099]

[0100] A molded article according to the present invention is formed from the thermoplastic resin composition. The antibacterial thermoplastic resin composition can be manufactured in the form of pellets, and the manufactured pellets can be manufactured into various molded articles (products) through various molding methods such as injection molding, extrusion molding, vacuum molding, and casting molding. Such molding methods are well known to those skilled in the art to which the present invention pertains. The molded article has excellent flame retardancy, dimensional stability, isotropy, impact resistance, rigidity, appearance characteristics, and a balance of these physical properties, and is therefore useful as an interior / exterior material for electrical and electronic products, a thin film sheet, and the like.

[0101] In a specific example, the molded product may be a plastic member of an electronic device housing including a metal frame and a plastic member in contact with at least one surface of the metal frame.

[0102] FIG. 1 schematically illustrates a cross-section of an electronic device housing according to one embodiment of the present invention. The sizes of components constituting the invention in the drawing are exaggerated for clarity of the specification and are not limited thereto. As illustrated in FIG. 1, an electronic device housing according to one embodiment of the present invention includes a metal frame (10); and at least one plastic member (20) in contact with at least one surface of the metal frame (10), wherein the plastic member is characterized in that it is formed from the thermoplastic resin composition.

[0103] In a specific example, the shape of the metal frame (10) and the plastic member (20) is not limited to the drawing and may have various shapes. However, the metal frame (10) and the plastic member (20) have a structure in which at least one surface is in contact with each other. The contact structure may be implemented by bonding or insertion, and the method of contact is not limited.

[0104] In a specific example, the metal frame (10) may be a stainless steel frame, a plastic member, or any other product commonly used in electronic device housings, and is readily available commercially.

[0105] In a specific example, the plastic member (20) may be formed from the polycarbonate resin composition through various molding methods such as injection molding, extrusion molding, vacuum molding, and casting molding. Specifically, the plastic member (20) may be molded by a hot water mold method or a steam mold method (such as a rapid heat cycle molding (RHCM) method), and may be a front cover, a rear cover, or the like of a 22 to 85 inch thin film television, thin film monitor, or the like. The plastic member (20) may also be applied to exterior specifications such as a hairline pattern and a corrosion pattern.

[0106]

[0107] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.

[0108]

[0109] Example

[0110] Below, the specifications of each component used in the examples and comparative examples are as follows.

[0111] (A) Polycarbonate resin

[0112] Bisphenol-A type polycarbonate resin having a weight average molecular weight (Mw) of approximately 25,000 g / mol was used.

[0113] (B) Polyester resin

[0114] Polyethylene terephthalate (PET, manufacturer: Lotte Chemical, intrinsic viscosity: approximately 0.765 dl / g) was used.

[0115] (C) Phosphate compound

[0116] Bisphenol-A diphosphate (manufacturer: Yoke Chemical, product name: YOKE BDP) was used.

[0117] (D) Phosphazene compound

[0118] Phosphazene compound (Manufacturer: Pharmicell, Product name: Phoretar) was used.

[0119] (E) Talk

[0120] Talc (manufacturer: KOCH, product name: KCP-04) with an average particle size (D50) of approximately 10 ㎛ was used.

[0121] (F) Glass fiber

[0122] (F1) A flat glass fiber (manufacturer: Nittobo, product name: CSG 3PA-832) with a rectangular cross-section having an aspect ratio (major axis of the cross-section / minor axis of the cross-section) of approximately 4, a minor axis of approximately 7 ㎛, and a length before processing of approximately 3 mm was used.

[0123] (F2) A circular glass fiber (manufacturer: KCC, product name: CS321-EC10-3) with a cross-section diameter of approximately 13 ㎛ and a length before processing of approximately 3 mm was used.

[0124] (G) Mica

[0125] (G1) Mica (manufacturer: Koch, product name: M-50) with an average particle size (D50) of approximately 350 ㎛ was used.

[0126] (G2) Mica (manufacturer: Koch, product name: M50-1) with an average particle size (D50) of approximately 200 ㎛ was used.

[0127] (G3) Mica (manufacturer: Koch, product name: M50-2) with an average particle size (D50) of approximately 500 ㎛ was used.

[0128]

[0129] Examples 1 to 13 and Comparative Examples 1 to 15

[0130] Each of the above components was added in the amounts shown in Tables 1, 2, 3, 4, and 5 below, and then extruded at about 260°C to produce pellets. The extrusion was performed using a twin-screw extruder with an L / D of 36 and a diameter of 45 mm. The manufactured pellets were dried at about 80°C for about 4 hours or more, and then injected using a 6 Oz injection molding machine (molding temperature: about 260°C, mold temperature: about 60°C) to produce specimens. The physical properties of the manufactured specimens were evaluated using the following methods, and the results are shown in Tables 1, 2, 3, 4, and 5 below.

[0131]

[0132] Method of measuring physical properties

[0133] (1) Flame retardancy evaluation: The flame retardancy of a 0.8 mm thick injection specimen was measured using the UL-94 vertical test method.

[0134] (2) Dimensional stability evaluation: According to ASTM D696, the temperature was increased from -20℃ to 100℃ at a rate of 5℃ / min using a thermo mechanical analyzer, and the linear expansion coefficient (unit: ㎛ / m·℃) of an injection molded specimen measuring 10 mm × 10 mm × 3.2 mm was measured.

[0135] (3) Isotropy evaluation: Isotropy was calculated according to Equation 1 below.

[0136] [Formula 1]

[0137] Isotropy = TD coefficient of linear expansion / MD coefficient of linear expansion

[0138] In the above equation 1, the TD coefficient of linear expansion is the coefficient of linear expansion in the vertical direction (TD: transverse direction) of an injection molded specimen measuring 10 mm × 10 mm × 3.2 mm, measured while heating from -20°C to 100°C at a rate of 5°C / min according to ASTM D696, and the MD coefficient of linear expansion is the coefficient of linear expansion in the flow direction (MD: machine direction) of the injection molded specimen.

[0139] (4) Impact resistance evaluation: The notched Izod impact strength (unit: kgf·cm / cm) of a 1 / 8" thick specimen was measured according to ASTM D256.

[0140] (5) Stiffness evaluation: Flexural modulus of 6.4 mm thick specimen at 2.8 mm / min according to ASTM D790 (unit: kgf / cm 2 ) was measured.

[0141]

[0142] Example 1234567 (A) (parts by weight) 100100100100100100100 (B) (parts by weight) 13103333 (C) (parts by weight) 1212125151212 (D) (parts by weight) 88888510 (E) (parts by weight) 8888888 (F1) (parts by weight) 35353535353535 (F2) (parts by weight)------- (G1) (parts by weight) 7777777 (G2) (parts by weight)------- (G3) (parts by weight)------- Flame retardancy V-0 V-0 V-0 V-0 V-0 V-0 Coefficient of linear expansion 30253025313025 Isotropic (TD / MD)1.21.21.31.21.31.21.3 Notch Izod Impact Strength9116136128 Flexural Modulus100,000110,000110,000120,00095,000110,000100,000

[0143]

[0144] Example 8910111213(A) (parts by weight)100100100100100100(B) (parts by weight)333333(C) (parts by weight)121212121212(D) (parts by weight)888888(E) (parts by weight)5108888(F1) (parts by weight)353520403535(F2) (parts by weight)------(G1) (parts by weight)7777515(G2) (parts by weight)------(G3) (parts by weight)------Flame retardancyV-0V-0V-0V-0V-0V-0Coefficient of linear expansion312535183018Isotropy (TD / MD)1.21.21.31.31.31.2Notched Izod Impact strength 136 12 12 12 12 Flexural modulus 100,000 120,000 75,000 130,000 115,000 125,000

[0145]

[0146] Comparative Example 123456 (A) (parts by weight) 100 100 100 100 100 100 (B) (parts by weight) 0.1 20 3333 (C) (parts by weight) 12 12 12 0 12 12 (D) (parts by weight) 88 88 0.520 (E) (parts by weight) 88 88 88 (F1) (parts by weight) 35 35 35 35 35 35 (F2) (parts by weight)------ (G1) (parts by weight) 77 77 77 (G2) (parts by weight)------ (G3) (parts by weight)------ Flame retardancy V-0 V-2 V-2 V-0 V-2 V-0 Coefficient of linear expansion 40 35 25 35 25 35 Isotropy (TD / MD) 1.4 1.9 1.2 1.7 1.2 1.6 Notched Izod Impact strength 123134124 Flexural modulus 100,000120,000120,00080,000110,00080,000

[0147]

[0148] Comparative Example 7891011(A) (parts by weight)100100100100100(B) (parts by weight)33333(C) (parts by weight)1212121212(D) (parts by weight)88888(E) (parts by weight)0.520888(F1) (parts by weight)3535545-(F2) (parts by weight)--35(G1) (parts by weight)77777(G2) (parts by weight)---(G3) (parts by weight)---FlammabilityV-0V-2V-0V-1V-0Coefficient of linear expansion3222551312Isotropy (TD / MD)1.71.32.11.41.5Notched Izod Impact strength 1132099 Flexural modulus 99,000115,00035,000140,000120,000

[0149]

[0150] Comparative Example 12131415(A) (parts by weight) 100100100100(B) (parts by weight) 3333(C) (parts by weight) 12121212(D) (parts by weight) 8888(E) (parts by weight) 8888(F1) (parts by weight) 35353535(F2) (parts by weight)----(G1) (parts by weight) 0.120--(G2) (parts by weight)--7-(G3) (parts by weight)---7Flammability V-0 V-1 V-0 V-0Coefficient of linear expansion 35203725Isotropy (TD / MD) 1.61.21.41.2Notched Izod impact strength 124144Flexural modulus 100,000120,000110,000110,000

[0151]

[0152] From the above results, it can be seen that the thermoplastic resin composition of the present invention is excellent in flame retardancy, dimensional stability (coefficient of linear expansion), isotropy (TD coefficient of linear expansion / MD coefficient of linear expansion), impact resistance (notched Izod impact strength), rigidity (flexural modulus), etc., and it was confirmed that the appearance characteristics are excellent.

[0153] On the other hand, when the polyester resin is applied in an amount less than the content range of the present invention (Comparative Example 1), it can be seen that the dimensional stability, isotropy, etc. of the thermoplastic resin composition are deteriorated, and when the polyester resin is applied in an amount exceeding the content range of the present invention (Comparative Example 2), it can be seen that the flame retardancy, isotropy, impact resistance, etc. of the thermoplastic resin composition are deteriorated. When the phosphate compound is applied in an amount less than the content range of the present invention (Comparative Example 3), it can be seen that the flame retardancy, etc. of the thermoplastic resin composition are deteriorated, and when the phosphate compound is applied in an amount exceeding the content range of the present invention (Comparative Example 4), it can be seen that the isotropy, impact resistance, etc. of the thermoplastic resin composition are deteriorated. When the phosphazene compound is applied in an amount less than the content range of the present invention (Comparative Example 5), it can be seen that the flame retardancy, etc. of the thermoplastic resin composition is lowered, and when the phosphazene compound is applied in an amount exceeding the content range of the present invention (Comparative Example 6), it can be seen that the isotropy, impact resistance, etc. of the thermoplastic resin composition are lowered. When talc is applied in an amount less than the content range of the present invention (Comparative Example 7), it can be seen that the isotropy, etc. of the thermoplastic resin composition are lowered, and when talc is applied in an amount exceeding the content range of the present invention (Comparative Example 8), it can be seen that the flame retardancy, impact resistance, etc. of the thermoplastic resin composition are lowered. When the flat glass fiber is applied in an amount less than the content range of the present invention (Comparative Example 9), it can be seen that the dimensional stability, isotropy, rigidity, etc. of the thermoplastic resin composition are deteriorated. When the flat glass fiber is applied in an amount exceeding the content range of the present invention (Comparative Example 10), it can be seen that the flame retardancy, dimensional stability, isotropy, etc. of the thermoplastic resin composition are deteriorated. When the glass fiber (F2) having a circular cross-section is applied instead of the flat glass fiber of the present invention (Comparative Example 11), it can be seen that the dimensional stability, isotropy, etc. of the thermoplastic resin composition are deteriorated.In addition, when mica is applied in an amount less than the content range of the present invention (Comparative Example 12), it can be seen that the isotropy, etc. of the thermoplastic resin composition is lowered, and when mica is applied in an amount exceeding the content range of the present invention (Comparative Example 13), it can be seen that the flame retardancy, impact resistance, etc. of the thermoplastic resin composition are lowered, and when mica (G2) is applied instead of the mica of the present invention (Comparative Example 14), it can be seen that the dimensional stability, isotropy, etc. of the thermoplastic resin composition are lowered, and when mica (G3) is applied (Comparative Example 15), it can be seen that the impact resistance, etc. of the thermoplastic resin composition are lowered.

[0154]

[0155] The present invention has been described above, focusing on specific embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.

Claims

1. About 100 parts by weight of polycarbonate resin; About 0.5 to about 15 parts by weight of polyester resin; About 1 to about 20 parts by weight of a phosphate compound; About 1 to about 15 parts by weight of a phosphazene compound; About 1 to about 15 parts by weight of talc having an average particle size (D50) of about 7 to about 20 μm; about 10 to about 40 parts by weight of flat glass fibers; and A thermoplastic resin composition comprising about 1 to about 20 parts by weight of mica having an average particle size (D50) of about 250 to about 450 μm.

2. A thermoplastic resin composition according to claim 1, characterized in that the polyester resin comprises at least one of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polytrimethylene terephthalate, and polycyclohexylene terephthalate.

3. A thermoplastic resin composition according to claim 1 or 2, wherein the flat glass fiber has an aspect ratio of a cross section (major axis of the cross section / minor axis of the cross section) of about 1.5 to about 10, a minor axis of the cross section of about 2 to about 10 ㎛, and a length before processing of about 1 to about 30 mm.

4. A thermoplastic resin composition according to any one of claims 1 to 3, characterized in that the weight ratio of the phosphate compound and the phosphazene compound is about 1:0.3 to about 1:

2.

5. A thermoplastic resin composition according to any one of claims 1 to 4, characterized in that the weight ratio of the talc and the flat glass fiber is about 1:2 to about 1:

8.

6. A thermoplastic resin composition according to any one of claims 1 to 5, wherein the weight ratio of the talc and the mica is about 1: about 0.5 to about 1:

2.

7. A thermoplastic resin composition according to any one of claims 1 to 6, characterized in that the weight ratio of the flat glass fiber and the mica is about 1:0.1 to about 1:0.

6.

8. A thermoplastic resin composition according to any one of claims 1 to 7, characterized in that the thermoplastic resin composition has a flame retardancy of V-0 or higher in a 1.5 mm thick injection molded specimen measured by the UL-94 vertical test method.

9. A thermoplastic resin composition according to any one of claims 1 to 8, characterized in that the thermoplastic resin composition has a linear expansion coefficient of about 15 to about 36 ㎛ / m·℃ of an injection molded specimen measuring 10 mm × 10 mm × 3.2 mm in size, measured while heating from -20°C to 100°C at a rate of 5°C / min according to ASTM D696.

10. A thermoplastic resin composition according to any one of claims 1 to 9, characterized in that the thermoplastic resin composition has an isotropy of about 1.1 to about 1.3 calculated according to the following formula 1: [Formula 1] Isotropy = TD coefficient of linear expansion / MD coefficient of linear expansion In the above equation 1, the TD coefficient of linear expansion is the coefficient of linear expansion in the vertical direction (TD: transverse direction) of an injection molded specimen measuring 10 mm × 10 mm × 3.2 mm, measured while heating from -20°C to 100°C at a rate of 5°C / min according to ASTM D696, and the MD coefficient of linear expansion is the coefficient of linear expansion in the flow direction (MD: machine direction) of the injection molded specimen.

11. A thermoplastic resin composition according to any one of claims 1 to 10, characterized in that the thermoplastic resin composition has a notched Izod impact strength of about 5 to about 20 kgf·cm / cm of a 1 / 8" thick specimen measured according to ASTM D256.

12. In any one of claims 1 to 11, the thermoplastic resin composition has a flexural modulus of about 70,000 to about 140,000 kgf / cm of a 6.4 mm thick specimen measured under 2.8 mm / min conditions according to ASTM D790. 2 A thermoplastic resin composition characterized by:

13. A molded product characterized by being formed from a thermoplastic resin composition according to any one of claims 1 to 12.

14. A molded product according to claim 13, characterized in that the molded product is a plastic member of an electronic device housing including a metal frame and a plastic member in contact with at least one surface of the metal frame.

Citation Information

Patent Citations

  • Stress cracking-resistant and low-warpage two-component molded parts comprising talcum

    KR1020110059886A

  • Polycarbonate resin composition and molding of the same

    JP2020172635A

  • Flame retardant thermoplastic resin composition and article prepared using the same

    KR1020110068682A

  • Glass-fiber-reinforced polycarbonate resin composition

    KR1020150132087A

  • Reinforced flame retardant polycarbonate composition and molded article comprising same

    KR1020180081834A