Polymer composite, use of the composite in the production of beams, pre-molded parts and interlocking floors, and production process
The polymeric composite material addresses the environmental and performance limitations of Portland cement in civil construction by providing high-strength, eco-friendly beams and interlocking floors with enhanced mechanical properties, suitable for heavy traffic areas without the need for internal reinforcement.
Patent Information
- Application Number
- PCT/BR2023/050110
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-10
AI Technical Summary
Current civil construction methods, particularly in producing beams and interlocking floors, rely heavily on Portland cement, which generates significant environmental impact due to high carbon dioxide emissions, resource consumption, and waste generation, and lacks materials with improved mechanical properties for heavy traffic areas.
A polymeric composite material composed of sand, organic or inorganic filler, dicyclopentadiene-based polyester resin, and organic peroxide initiator, combined with flexibilizing additives, is used to produce beams and interlocking floors without internal reinforcement, offering enhanced mechanical properties and reduced environmental footprint.
The polymeric composite achieves mechanical properties comparable to or exceeding those of traditional Portland cement-based materials, with improved resistance to compression, flexure, water absorption, and abrasion, while reducing environmental impact by utilizing recycled materials and eliminating the need for metal frames.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Patent Descriptive Report for “POLYMERIC COMPOSITE, USE OF THE COMPOSITE IN THE PRODUCTION OF BEAMS, PRE-CAST PARTS AND INTERLOCKING FLOORS AND PRODUCTION PROCESS” FIELD OF INVENTION
[0001] , The present invention relates to a polymer composite and its use in the production of beams, precast parts and interlocking floors with high resistance to compression and flexure.
[0002] , Additionally, the present invention also relates to the production process of the polymer composite and beams, precast parts and interlocking floors.
[0003] , The area of application of the present invention belongs to the field of civil construction, more specifically, in applications aimed at large structures that support large loads and apply pre-molded parts such as beams, in addition to paving areas that require high resistance for traffic and storage of heavy loads, such as containers in ports, airports and industrial areas. BACKGROUND OF THE INVENTION
[0004] , Currently, several types of beams, precast pieces and interlocking floors are known, as highlights, it is possible to mention rectangular interlocking floors, sixteen faces, racket, directional podotactile, alert, hollow, among others.
[0005] , The beams, precast pieces and interlocking flooring can be used in road works, walkways, sidewalks, squares, cycle paths, common areas in clubs, parking lots, external areas of shopping centers, industrial floors, airport yards, container terminal yards, among other places.
[0006] , Current estimates place global concrete production at around 10 km 3 per year, and this number continues to increase due to the massive development of urban infrastructure worldwide. Therefore, new materials emerge to balance the exploitation of input sources in construction and to minimize environmental impacts. This is the case of interlocking blocks are being produced with new materials, in addition to concrete, for the same functionality.
[0007] The beams, precast pieces, and interlocking flooring are environmentally friendly, more durable than other types, and offer high drainage capacity, low maintenance, and reduced costs. In the interlocking system, the pieces fit together like a puzzle, enabling customization and quick replacement, drainage, and return of water to the ground through their cracks, all while saving material.
[0008] Construction is one of the activities with the greatest environmental impact, as it consumes significant natural resources. This sector utilizes 40 to 75% of natural resources, generating a considerable amount of waste. In Brazil alone, approximately 25% of industrial waste is generated by construction. Furthermore, there is the impact of the cement industry. Although the cement manufacturing process does not directly produce solid waste, since the ash from the combustion of fuel in the rotary kiln is typically incorporated into the clinker itself, it still emits high amounts of gaseous pollutants and particulate matter. Thus, the main impacts are caused by the emission of polluting gases from this combustion. One example is the high emission of carbon dioxide (CO2), one of the main greenhouse gases.Cement plants are responsible for approximately 5% of global carbon dioxide (CO2) emissions from anthropogenic sources, released annually into the atmosphere. This equates to approximately 2.8 billion tons of CO2 released into the atmosphere annually. It is estimated that the production of one ton of clinker produces one ton of CO2, contributing significantly to the greenhouse effect. The cement manufacturing process can also release sulfur oxide, nitrogen oxide, carbon monoxide, and lead compounds, all of which are pollutants. Furthermore, cement plants are one of the largest anthropogenic sources of mercury (Hg) emissions, accounting for approximately 1.71 tons of mercury released into the atmosphere annually, without treatment or control.
[0009] , Polymer concrete, which has a polymeric resin as a binder, has become a good option for civil construction in applications where high mechanical performance, durability and fast curing are required, important properties for materials aimed at the sustainability of buildings.
[0010] , The beams, precast pieces and conventional interlocking paving are produced from raw materials extracted from nature - river sand, stone sand, stone dust, additives, pigments, gravel and high-strength, immediate-curing cement. The materials used in the production of interlocking paving, or as they are also known, blocks or simply interlocking paving, must comply with the parameters of the Brazilian standards ABNT NBR 9781: 2013 Concrete paving pieces > Specifications and Test Methods and ABNT NBR 15953: 2011 Interlocking paving with concrete pieces > Execution.
[0011] As an alternative to this conventional block, there are recycled interlocking blocks, which are manufactured from Construction Waste (RCC) and Demolition Waste (RCD).
[0012] , Additionally, as can be seen in the state of the art, several researchers have been working on the development of alternative floors.
[0013] , EP2758353A1 protects a mixture for obtaining polymer concrete, which mixture is comprised of a part by volume of a filler or filler and the other part of a resin mixture, which may be a resin plus a hardening agent and an accelerator agent. Among the examples of resins claimed is the use of polyester or acrylic resin. However, it does not provide for the use of DCPD (dicyclopentadiene) or the use of chemical additives to improve mechanical properties.
[0014] , Document US9,885,157 describes a method for installing paving tiles on a concrete base without causing them to break under future vehicular traffic. To achieve this, a binder (a binding agent) is used to fix the tiles to the concrete. This mixture may include latex polymer, cement, sand, and hydrating agents. This composition will create a permanent bond between the tiles and the cement base.
[0015] Portland cement is the worldwide conventional name for the material commonly known in construction as cement. Portland cement is a fine powder with binding, agglutinating, or binding properties. that hardens under the action of water. Once hardened, even if it is subjected to water again, Portland cement does not decompose any further.
[0016] Portland cement was created by an English builder, Joseph Aspdin, who patented it in 1824. At that time, it was common in England to build with stone from Portland, an island located in the south of that country. Because the result of Aspdin's invention resembled Portland stone in color and hardness, he registered this name in his patent. This is why the cement is called Portland cement.
[0017] Most types of Portland cement on the market today are suitable for general use. Some, however, have specific characteristics and properties that make them more suitable for specific uses, allowing for concrete or mortar with the desired strength and durability.
[0018] Portland cement is composed of clinker and additives. Clinker's raw materials are limestone and clay. The limestone is first crushed, then ground, and then mixed in appropriate proportions with ground clay. This mixture undergoes several processes and ultimately forms a powder.
[0019] , Additions are other raw materials that, mixed with clinker during the grinding phase, allow for the production of the various types of Portland cement currently available on the market. These other raw materials include gypsum, blast furnace slag, pozzolanic materials, and carbonate materials.
[0020] Clinker is the main component and is present in all types of Portland cement. The additions can vary from one type of cement to another and are primarily what define the different types of cement.
[0021] Precast beams are frequently used in the construction of bridges and viaducts, buildings, commercial warehouses, and other structures, aiming to reduce construction time and costs through a streamlined construction process. Prestressed beams allow them to be adapted to a variety of projects due to their ability to span spans of varying sizes. Another advantage is the reduced consumption of concrete and steel due to the use of higher-strength materials.
[0022] Beams are manufactured either in segments (called staves) or in one piece, depending on the project's design. Generally, the first option is recommended for bridges and projects with large spans. On the other hand, whole pieces are used in spans of up to 40 meters. The design must follow the slab-beam-column order to transfer vertical forces. Rectangular in shape, beams can be manufactured in varying cross-sections and sizes, depending on the construction's specificities. All these precast pieces have a metal frame inside, often prestressed.
[0023] Reinforced concrete beams and columns offer many advantages to a project, as they are the concrete beams that tie the vertical columns together, and most importantly, they are robust beams. Concrete beams are widely used in slab-beam-column systems to transfer vertical forces from the slab to the column, or to transmit a concentrated load if supporting a column. Concrete beams transfer the weight of the slabs and other elements to the columns. The use of concrete beams allows for the use of formwork of a wide variety of designs on the project, thus perfectly enabling a well-planned project built with concrete columns, beams, and slabs.
[0024] , In view of the state of the art scenario and seeking alternatives for new materials applied in the production of beams, precast parts and high-resistance interlocking floors, which could be compared to traditional Portland cement, with or without metal reinforcement, the researchers of the present invention developed a polymer composite that can be used in the production of beams, precast parts without the use of metal reinforcement and high-resistance interlocking floors for use in heavy traffic paving, and the polymer composite comprises as materials sand, inorganic or organic filler, at least one dicyclopentadiene-based polyester resin (DCPD), combined or not with virgin terephthalic resin (PET) or neopentyl glycol (NPG) and at least one phase compatibilizing or flexibilizing additive,allowing the production of beams and precast parts with mechanical properties achieved without the use of internal reinforcement in the artifacts and interlocking floors with mechanical properties of high-resistance floors (heavy traffic) using dimensions of light traffic floors.,
[0025] , Therefore, there is no solution in the state of the art equivalent to that presented here in the present invention that combines technical differences, economic advantages, safety and reliability. SUMMARY OF THE INVENTION
[0026] , The present invention relates to a polymer composite, composed of sand, organic or inorganic filler, sand, inorganic or organic filler, polyester resin, organic peroxide initiator and additive or flexible agents of the polymer structure.
[0027] , The present invention also relates to the use of the polymer composite in the production of beams, precast parts and high-strength interlocking flooring with equal or improved mechanical properties, such as axial compression resistance, 4-point flexural strength, water absorption and resistance to abrasion wear, when compared to the same artifacts produced from Portland cement under the same conditions and dimensions.
[0028] , The present invention also relates to the method of producing the polymer composite and the beams, precast parts and interlocking floors.
[0029] Finally, the present invention provides for the production of precast beams and parts, without the use of internal reinforcement, that present mechanical properties equal to or superior to those obtained for these precast artifacts in traditional Portland cement reinforced concrete. Furthermore, in the case of interlocking floors, it is possible to achieve high-strength flooring values—that is, floors applied to heavy-traffic areas or storage of heavy loads, such as containers—using floors with light-traffic floor dimensions. DETAILED DESCRIPTION OF THE INVENTION
[0030] , The present invention relates to a polymer composite, composed of sand, organic or inorganic filler, sand, inorganic or organic filler, polyester resin, organic peroxide initiator and additive or flexible agents of the polymer structure
[0031] , The present invention also relates to the use of the polymer composite in the production of beams, precast parts and high-resistance interlocking flooring that can be used in civil construction.
[0032] , More specifically, the present invention relates to beams, precast parts and interlocking floors for use in civil construction, which present mechanical properties, such as resistance to axial compression, resistance to 4-point bending, water absorption and resistance to abrasion wear, equal or improved when compared to the same artifacts produced under the same conditions and dimensions made of Portland cement.
[0033] , The present invention also relates to the method of producing the polymer composite and the beams, precast parts and interlocking floors.
[0034] , Another aspect of the present invention relates to obtaining precast beams and parts, without the use of internal reinforcement, which present mechanical properties equal to or superior to those obtained for these precast artifacts in traditional Portland cement reinforced concrete.
[0035] , The present invention also relates to obtaining high-resistance interlocking floors, that is, floors that can be applied to heavy traffic areas or storage areas for heavy loads, such as containers, using floors with dimensions of light traffic floors.
[0036] , Finally, the present invention refers to products defined as beams, precast parts and interlocking floors, obtained with composite, for application in civil construction.
[0037] , According to the present invention, the composite material used to obtain the beams, precast parts and interlocking floors comprises: (a) sand; (b) at least one inorganic or organic filler or mixture thereof; (c) at least one polyester resin; (c) at least one organic peroxide initiator and (d) at least one additive.
[0038] , In a first aspect, sand is understood to be any type of sand known in the state of the art, including sand defined as construction sand, washed sand (also known as natural sand), mine sand, and quarry sand. Washed sand can be defined as fine, medium, and coarse sand.
[0039] , According to the present invention, organic load is understood to be all residues that can be used to give a specific property or reduce the cost of the product, such as, but not limited to, fly ash, sugarcane bagasse or eucalyptus root and other vegetable or mineral residue.
[0040] , According to the present invention, inorganic filler is understood to mean all residues that can be used to give a specific property or reduce the cost of the product, such as, but not limited to, silica, alumina, limestone, foundry sand, talc, crushed stone powder, plaster, lime, dolomite, bentoite, barite, attapulgite, sepiolite, vermiculite, porous magnetite, calcium carbonate, magnesium carbonate, mica, graphite, gypsum and gilsonite, among others.
[0041] , Polyester resin are synthetic resins formed by the reaction of dibasic organic acids and polyhydric alcohols, and according to the present invention are selected from the group consisting of: orthophthalic, isophthalic and / or terephthalic unsaturated polyester resin, PET monomers, associated with each other or with other components such as dicyclopentadiene (DCPD) or neopentyl glycol (NPG). Preferably dicyclopentadiene (DCPD), PET monomers, neopentyl glycol (NPG) or a combination thereof.
[0042] , The organic peroxide initiator is defined among the selected group of benzoyl peroxide, methyl ethyl ketone peroxide, tert-butyl peroxide, tert-butyl benzoate peroxide, di tert-butyl peroxide dicumyl peroxide, being preferably defined as methyl ethyl ketone peroxide, of medium reactivity, desensitized with dimethyl phthalate.
[0043] Finally, the additive is defined as a phase compatibilizing agent, also called coupling agents or flexibilizing agent. The phase compatibilizing agent is selected from the group consisting of: vinyl trimethoxysilane, methacryltrimethoxysilane, methacryloxypropyltrimethoxysilane, vinyl triethoxysilane, calcium diacrylate, zinc diacrylate, and combinations thereof; and the flexibilizing agent is selected from butylacrylate, butylmethylacrylate, methylmethacrylate, triethylene glycolmethacrylate, ethylhexylmethacrylate, acrylic acid, methacrylic acid, and combinations thereof.
[0044] , As mentioned, the present invention has as its main objective a polymeric composite useful in obtaining products applied to construction civil, which are defined as beams, precast parts and interlocking floors.
[0045] , A second objective of the present invention is to obtain products applied to civil construction, which are defined as beams, precast parts and interlocking floors using the polymer composite in their production.
[0046] Precast beams and parts are prepared without the use of internal reinforcement and have mechanical properties equal to or superior to those obtained for these precast artifacts made with traditional Portland cement reinforced concrete. Interlocking floors achieve mechanical properties, water absorption, and abrasion resistance similar to those of high-strength floors—i.e., floors used in heavy-traffic areas or for storing heavy loads, such as containers, using light-traffic flooring dimensions.
[0047] , According to the present invention, the composite material used in the production of beams, precast parts and interlocking floors is composed of sand, organic or inorganic filler, polyester resin, organic peroxide indicator and an additive defined as a phase compatibilizing agent or flexibilizing agent.
[0048] The sand used in composite production has a predominant composition of silica particles, but may also contain other minerals such as feldspar, mica, zircon, magnetite, ilmenite, monazite, and cassiterite. Commercial sand typically contains moisture. Regarding particle size, the preferred composite material is prepared using medium-sized sand (0.2 mm to 0.6 mm), previously washed to remove most of the organic impurities, and dried to a moisture content below 1% by mass.
[0049] , The sand used is in the proportion of 30% to 97%, by mass, based on the total mass of the composite composition. Preferably, the proportion is 47% to 94%, by mass, based on the total mass of the composite composition, and more preferably, 55% to 85%, by mass, based on the total mass of the composite composition.
[0050] , The composite material, used in the production of the artifacts of the present invention, including beams, pre-molded parts and interlocking floors, also comprises the use of at least one organic or inorganic filler, which functions as a filler for the potential empty spaces generated between the grains of sand.
[0051] , Organic loads are selected from the group consisting of: fly ash, sugarcane bagasse, eucalyptus root or other vegetable or mineral residue and inorganic loads selected from the group consisting of: silica, alumina, limestone, foundry sand, crushed stone powder, plaster, lime, dolomite, bentonite, barite, attapulgite, sepiolite, vermiculite, porous magnetite, calcium carbonate, magnesium carbonate, mica, graphite, gypsum, gilsonite or a mixture of these.
[0052] Fly ash, which consists of solidified material from the exhaust gas suspension in burners, is collected by electrostatic precipitators or extracted by mechanical filtration. Due to solidification in suspension under gas flow, the particles obtained are preferably spherical and often hollow or highly porous, with dimensions ranging from 0.5 pm to 100 pm.
[0053] Due to the mineral impurities present in coal, the ash is composed primarily of silicon dioxide (SiO2), aluminum oxide (AI2O3), and iron oxide (Fe2Ü3). The ash possesses pozzolanic activity, which means it can react, at normal temperatures and in the presence of water, with calcium hydroxide and alkalis to form calcium silicate hydrates, which are compounds capable of setting Portland cement. In other words, these compounds maintain cohesion between the particulate aggregates and the cementitious matrix.
[0054] , In the pavements of the present invention, the pozzolanic activity is not relevant, since the matrix is not composed of Portland cement, but of polymeric resin, whose curing reactions are crosslinking reactions of the polymeric chains, not involving the formation of hydrated calcium silicate.
[0055] , Gypsum, also called plaster stone, is composed of calcium sulfate dihydrate, that is, it is a calcium ore whose chemical composition corresponds to the formula Ca(SO4). 2H2O. It is a mineral, generally, of Its color ranges from white to translucent, with a micaceous, lamellar appearance, a pearly luster, an unctuous (or fibrous) feel, and a low hardness of around 2.0. It is the most abundant sulfate in the Earth's crust, occurring in evaporites or in the form of interstratified layers of shales, limestone, and clay, and can also be found in meteorites. Through calcination, gypsum loses its water of crystallization and can then be transformed into plaster when it retains crystallized water (CaSO4.1 / 2H2O), or calcium sulfate (anhydrite) when it completely loses its crystallized water (CaSCM).
[0056] Gypsum's primary application is in cement manufacturing, but it is also used in the production of sulfuric acid, chalk, glass, enamels, plaster, and beer production. Gypsum, or calcium sulfate, is also used as a casting mold material; as a dehydrator; as a binder and soil conditioner (supplying calcium and sulfur); and as a metallurgical slag producer.
[0057] , The fillers are present in the proportion of 4% to 38%, by mass, based on the total mass of the composite composition, preferably from 6% to 30%, by mass, based on the total mass of the composite composition and more preferably from 7% to 25%, by mass, based on the total mass of the composite composition.
[0058] , More specifically, the composite of the present invention comprises ash, gypsum or plaster in an amount that can vary from 4% to 38%, by mass, based on the total mass of the composite composition, preferably from 6% to 30%, by mass based on the total mass of the composite composition and more preferably still from 7% to 25%, by mass, based on the total mass of the composite composition.
[0059] , The polyester resin present in the composite of the present invention is selected from the group consisting of: orthophthalic, isophthalic and / or terephthalic unsaturated polyester resin, polyethylene terephthalate (PET) associated with each other or with other components such as dicyclopentadiene (DCPD) or neopentyl glycol.
[0060] , Resins, these are present in the proportion of 4% to 44%, by mass, based on the total mass of the composite composition, preferably from 6% to 38%, by mass, based on the total mass of the composite composition and more preferably 8 to 32% by mass, based on the total mass of the composite composition.
[0061] , Resins are the most widely used, mainly unsaturated polyester resins, which are also used in paints and adhesives. In the artifacts of the present invention, including beams, precast parts, and interlocking flooring, DCPD is used in an amount that can vary from 4% to 44% by mass, preferably from 6% to 38% by mass, and most preferably from 8% to 32% by mass, based on the total mass of the composite material composition.
[0062] Polyethylene terephthalate (PET), also commonly used, is a thermoplastic polymer developed in 1941. This polymer is formed by the reaction between terephthalic acid and ethylene glycol. This polymer is primarily used in weaving fibers and beverage packaging. It is a polyester and therefore has an ester functional group in its main chain, exhibiting thermoplastic properties, meaning it can be reprocessed countless times.
[0063] The industrial production of polyethylene terephthalate (PET) occurs in two stages: prepolymerization followed by polycondensation. During prepolymerization, the oligomer bis(2-hydroxyethylene) terephthalate (BHET) is generated, which can be obtained by two distinct chemical routes. In the second stage, polycondensation, the reaction to obtain PET occurs. The first chemical route to obtain BHET is through direct esterification between terephthalic acid and ethylene glycol. This route is characterized as heterogeneous and autocatalytic, meaning it does not require the use of catalysts. The reaction temperature in this route is in the range of 240–260°C. In the second chemical route to obtain BHET, terephthalic acid is replaced by dimethylene terephthalate ester, using catalysts in a temperature range of 170–210°C. During polycondensation reactions, water and methanol are eliminated as by-products.In the floors that make up the present invention, PET resin is used in the preparation of the composite material in the form of PET monomers, preferably virgin, with the function of crosslinking the polymeric matrix to provide mechanical resistance to the floor obtained.
[0064] , Few reports are found in the prior art on the use of PET as a filler in concrete for the production of artifacts. Some reports mention the use of crushed bottles and filaments in this application. In these cases, both the filaments and the particles obtained from the crushed bottles serve as fillers and do not act as a matrix in the final material, as is the case with the present invention. Furthermore, the PET used both in the form of filaments and in the crushed bottle particles are thermoplastic versions of this polymer, meaning they are sensitive to temperature variations, which could result in warping and deformation if used to produce the artifacts (beams, precast parts, and interlocking flooring) that are the subject of the present invention.The PET resin used in the composite of the present invention is a thermosetting resin that undergoes crosslinking during polymerization, ensuring that the final artifact will not deform or warp with temperature variations, maintaining its shape for long periods. This represents a completely new and inventive use of PET in composite materials for obtaining the artifacts of the present invention and / or for various purposes.
[0065] , The composite of the present invention, used in the production of artifacts, including beams, precast parts and interlocking floors, comprises PET monomers in an amount that can vary from 4% to 44%, by mass, preferably from 6% to 38%, by mass and more preferably from 8 to 32%, by mass, based on the total mass of the composition of the composite material.
[0066] Neopentyl glycol (NPG) is used in the synthesis of polyesters, paints, lubricants, and plasticizers. In the case of polyesters, NPG increases the polymer's stability to heat, light, and water. NPG is also used in the production of esters used in synthetic lubricants due to its lower tendency to undergo hydrolysis or oxidation compared to natural esters.
[0067] , NPG is obtained industrially through the aldol reaction of formaldehyde and isobutyraldehyde that results in the intermediate hydroxypivaldehyde, which can be converted to NPG in the presence of excess formaldehyde or by palladium-catalyzed carbon hydrogenation. Among the many In other applications, NPG can be used as a protecting group for ketones, for example, in the synthesis of gestodene, or in NPG organoboronic acid esters for Suzuki reactions, which are cross-coupling reactions widely used to obtain all-substituted polyolefins, polystyrenes, and biphenyls. In the composite of the present invention, NPG is used in combination with cross-linked polyester resins, so that the final composite material has high thermal and dimensional stability.
[0068] , The composite of the present invention, used to obtain beams, precast parts and interlocking floors, comprises polyester resins containing NPG in an amount that can vary from 4% to 44%, by mass, preferably from 6% to 38%, by mass and more preferably from 8 to 32%, by mass, based on the total mass of the composition of the composite material.
[0069] , The peroxide initiator used in the composition of the composite is selected from the group consisting of: benzoyl peroxide, methyl ethyl ketone peroxide, tert-butyl peroxide, tert-butyl benzoate peroxide, di tert-butyl peroxide, dicumyl peroxide, preferably being methyl ethyl ketone peroxide, of medium reactivity, desensitized with dimethyl phthalate and is in the proportion of 0.05% to 6.0%, by mass, based on the total mass of the composite, preferably being used between 0.075% and 1.5% by mass, based on the total mass of the composite composition and more preferably between 0.10% and 0.85% by mass of the composite.
[0070] Methyl ethyl ketone (MEKP) is an organic peroxide with an explosive potential similar to butanone peroxide. MEKP is a colorless, oily liquid, while butanone peroxide is a white powder at STP. MEKP is slightly less sensitive to shocks and temperature and is more stable in storage. Depending on the reaction conditions, several adducts, or direct addition products, of methyl ethyl ketone and hydrogen peroxide can be obtained. The first adduct reported was a cyclic dimer, CsH-ieC, in 1906. Later studies showed that a linear dimer is the most frequently obtained adduct in the product mixture, and this is the form generally available commercially. Dilute solutions of 30–40% MEKP are applied in industry and by general users, such as artisans, as a A catalyst to initiate the crosslinking of unsaturated polyester resins. For this application, MEKP is dissolved in dimethyl phthalate, cyclohexane peroxide, or diallyl phthalate to reduce shock sensitivity. Benzoyl peroxide can be used for the same purpose. MEKP is a serious skin irritant and can cause progressive corrosive damage or blindness.
[0071] , The composite of the present invention, used to obtain beams, precast parts and interlocking floors, also comprises methyl ethyl ketone peroxide desensitized with dimethyl phthalate in an amount that can vary from 0.05% to 6.0%, by mass, preferably from 0.075% to 1.50%, by mass and more preferably still from 0.10% to 0.85%, by mass, based on the total mass of the composite composition.
[0072] , Finally, the composite of the present invention also comprises an additive defined as a phase compatibilizing agent or flexibilizing agent, which are selected from the group consisting of: vinyltrimethoxysilane, methacryltrimethoxysilane, methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, calcium diacrylate, zinc diacrylate, butylacrylate, butylmethylacrylate, methylmethacrylate, triethyleneglycolmethacrylate, ethylhexylmethacrylate, acrylic acid, methacrylic acid or combinations thereof and are present in proportions of 0.01 to 1.1% by weight of the composite. The additive can be partially or totally replaced by a flexibilizing agent of the polymeric structure.
[0073] Vinyltrimethoxysilane is a vinyl-functional silane with a reactive methoxy group. Its primary application is as a crosslinking and grafting agent for the manufacture of high-density polyethylene cables and pipes. However, vinyltrimethoxysilane can be grafted onto various polymers, such as various polyethylenes and polyesters. The presence of the methoxy group makes vinyltrimethoxysilane a water-scavenging agent in coatings and adhesives. Vinyltrimethoxysilane can also be used with amino silanes in the synthesis of polyethers. Vinyltriethoxysilane is also a vinyl-functional silane, but the reactive group has two carbons, an ethoxy group. It has also been used as a coupling agent in polyolefins, particularly in polypropylene composites containing glass fibers.
[0074] , The composite of the present invention contains vinyltrimethoxysilane or vinyltriethoxysilane in an amount that can vary from 0.01% to 1.1%, based on the total mass of the composite composition.
[0075] , According to the present invention, the composite material, which is the object of the present invention and used in the production of beams, precast parts and interlocking floors, is composed of: (a) sand; (b) at least one organic or inorganic filler; (c) at least one polyester resin; (d) at least one organic peroxide initiator; and (e) at least one additive.
[0076] , More specifically, the composite material, which is the object of the present invention and used in the production of beams, precast parts and interlocking floors, is composed of: (a) sand; (b) at least one organic filler selected from the group consisting of: fly ash, sugarcane bagasse, eucalyptus root or other vegetable or mineral residue or an inorganic filler selected from the group consisting of: silica, alumina, limestone, foundry sand, crushed stone powder, gypsum, lime, dolomite, bentonite, barite, attapulgite, sepiolite, vermiculite, porous magnetite, calcium carbonate, magnesium carbonate, mica, graphite, gypsum, gilsonite or a mixture thereof; (c) at least one polyester resin selected from the group consisting of: orthophthalic, isophthalic and / or terephthalic unsaturated polyester resin associated with each other or with other components such as dicyclopentadiene (DCPD) or neopentyl glycol; (d) at least one organic peroxide initiator selected from the group consisting of: benzoyl peroxide, methyl ethyl ketone peroxide, tert-butyl peroxide, tert-butyl benzoate peroxide, di tert-butyl peroxide, dicumyl peroxide, preferably methyl ethyl ketone peroxide, of medium reactivity, desensitized with dimethyl phthalate; and (e) at least one additive defined as a phase compatibilizing agent or flexibilizing agent, which are selected from the group consisting of: vinyltrimethoxysilane, methacryltrimethoxysilane, methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, calcium diacrylate, zinc diacrylate, butylacrylate, butylmethylacrylate, methylmethacrylate, triethyleneglycolmethacrylate, ethylhexylmethacrylate, acrylic acid, methacrylic acid or combinations thereof.
[0077] , Additionally, the composite, which is the object of the present invention, is useful in obtaining beams, pre-molded parts and interlocking floors, and may also contain: a reaction accelerator system; ground rubber, glass or metallic fibers, metallic or polymeric structures and finishes.
[0078] , The reaction accelerator system is defined from the group selected by: cobalt naphthenate, cobalt octoate, dimethylaniline (DMA), or a mixture of these.
[0079] , The accelerator system is mixed with the resin in an amount that can vary from 0.05% to 8.0% by mass, based on the total mass of the composite. Preferably, a proportion of 0.1 to 3.5% is used, and more preferably a proportion of 0.1 to 3.5% of cobalt naphthenate or cobalt octoate, alone or together with 0.002% to 0.150% of dimethylaniline (DMA) by mass, based on the total mass of the composite.
[0080] , Ground rubber comes from tires and can be present in an amount of 0% to 45% by mass, based on the total mass of the composite. Preferably, a proportion of 0% to 20% ground rubber by mass, based on the total mass of the composite, is used.
[0081] Glass or metal fibers can be short and uniformly distributed throughout the matrix; or long and aligned in a single direction. The fiber content can range from 0% to 8% by mass, based on the total mass of the composite. Preferably, the fiber content should be 0% to 3% by mass, based on the total mass of the composite.
[0082] , Metallic or polymeric structures are wires or meshes, and may be present in an amount that can vary from 0% to 30% by mass, based on the total mass of the composite. Preferably, in the proportion of 0% to 20% by mass, based on the total mass of the composite;
[0083] , Finishes are fakes, polishing, among others related to aesthetic interest or the need for signaling, depending on the installation location of the products beams, precast parts and interlocking floors obtained, previously defined as beams, precast parts and interlocking floors, for a given application.
[0084] , The composite material described in the present invention is capable of replacing, totally or partially, the traditional Portland concrete used in civil construction, including in the production of beams, precast parts and interlocking floors.
[0085] , Composite material presents numerous technical and economic advantages when compared with the state of the art.
[0086] , Among the advantages, researchers highlight the enormous potential for use in a wide range of applications, such as for the production of panels, posts, crosses, poles, etc., due to its high mechanical strength, excellent dielectric properties and chemical resistance to corrosion, low porosity and water absorption, and, in addition, low weight.
[0087] Another advantage is that artifacts made with the composite of the present invention are not subject to fungal attack and consequent insect proliferation, as is the case with products made with Portland cement. The main fungi that attack Portland cement feed on the calcium and phosphate released during the aging of concrete, which are not present in the composite material of the present invention. Therefore, the composite of the present invention, in addition to maintaining the aesthetic characteristics of artifacts made with Portland cement, is capable of preserving the health of people present in the environments where these artifacts are installed.
[0088] , The low deterioration of the products (beams, precast pieces and interlocking flooring) over time when compared to products produced from traditional Portland cement, since the composite of the present invention is resistant to rot, insect attack and solar radiation, and any eventual absorption of water does not produce loss of hardness or other mechanical properties, since this absorption is due to the eventual porosity of the material, with no chemical reaction with water. In addition to presenting impermeability and electrical insulation when compared to reinforced concrete and does not contain toxic components after curing.
[0089] , The products (beams, precast parts and interlocking flooring) obtained with the composite of the present invention do not require a metal frame, as in the case of reinforced concrete, in their structure, and consequently, do not present problems of corrosion of the structure and the products obtained are parts with a high degree of homogeneity, guaranteeing great reliability to the product.
[0090] , Finally, the composite reduces environmental risks, since by preferentially using ash as a filler, it uses a liability of the steel, thermoelectric, agricultural, sugar and alcohol industries or any industrial process that burns biomass in boilers, reducing waste and the non-use of water in its manufacture does not generate the discharge of liquid effluents.
[0091] , The composite material is prepared comprising the steps of: (i) Drying the sand until it reaches a moisture content of less than or equal to 1%; (ii) Weighing of all components; (iii) Obtaining the dry mixture composed of sand and filler and homogenizing the components for approximately 20 minutes; (iv) Obtaining the liquid mixture composed of additive agent and resin and then adding the peroxide initiator to the liquid mixture and mixing until homogeneity is obtained. (vi) Insert the liquid mixture into the mechanical mixer that already contains the dry aggregate mixture and immediately mix for approximately 1 to 2 minutes or until a homogeneous appearance is obtained. (v) Obtaining composite material for use in the production of beams, precast parts and interlocking floors.
[0092] , According to the present invention, the composite material comprises: (a) 70 to 85% sand; (b) 8 to 20% resin; (c) 6 to 25% filler; (d) 0.1 to 0.85% peroxide initiator; and (e) 0.01 to 0.85% additive agent.
[0093] , More specifically, the composite material, object of the present invention, comprises: (a) 70 to 85% sand; (b) 8 to 20% resin; (c) 6 to 15% ash, gypsum or plaster; (d) 0.1 to 0.6% peroxide initiator; (e) 0.1% to 0.85% additive agent; and (f) 4 to 8% marble powder. Wherein the resin pre-accelerated may contain a reaction promoter, preferably 1% cobalt naphthenate;
[0094] The beams, precast pieces and interlocking floors developed were prepared comprising the following steps: (i) Production of the composite material consisting of the following steps: (a) Drying the sand until it reaches a moisture content of less than or equal to 1%; (b) Weighing all components; (c) Obtaining the dry mix; (d) Obtaining the liquid mix, (e) Inserting the liquid mix into the mechanical mixer that already contains the dry aggregate mix and immediately mixing for approximately 1 to 2 minutes or until a homogeneous appearance is obtained (described above). (ii) Molding of beams, precast parts or floors in molds with previously established shapes and prepared with the application of a layer of release agent, (iii) Pressing of around 20 tons of pressure for larger parts, such as beams and precast parts, and at least 4 tons of pressure for smaller parts such as interlocking flooring. (iv) pre-curing in an oven at atmospheric pressure at a temperature of approximately 60°C for a period of 120 minutes; (v) curing process for a minimum period of 7 days at room pressure and temperature at a temperature of approximately 25°C.
[0095] , The molding of the products takes place for 12 minutes with a pressure of 4 t for small parts (interlocking flooring) and 20 t for large parts (beams and precast parts). The specification of the aggregates must not exceed 1% moisture; the specific mass of the sand must be 2.65 g / cm 3; the specific mass of fly ash must be 2.16 g / cm 3 ; the specific mass of gypsum must be 2.32 g / cm 3 ; and the specific mass of plaster can vary from 1.80 to 2.60 g / cm 3 .
[0096] , Estimated elemental chemical composition and Morphology.
[0097] , To define the morphology and estimated elemental chemical composition of the product of the preferred embodiment described above, tests were carried out using a scanning electron microscope (SEM) model Inspect S50 FEI with EDS. The sample of the preferred embodiment used received a gold coating approximately 10 to 20 nm thick. Analyses were conducted with a secondary electron beam for morphology analysis and emitted X-rays for elemental chemical composition estimation by EDS.
[0098] The micrographs show a material with low porosity, with uniformly distributed aggregate phases and excellent adhesion of the aggregates to the polymer matrix. This condition differs from that observed in traditional Portland concrete, which has many internal phases generated during its curing reactions and the insertion of aggregates into it during its preparation process. During the preparation process of traditional Portland concrete, high porosity, both open and closed, is generated due to the release of gases during curing. The EDS analysis revealed that this preferred embodiment has an elemental chemical composition of 45.36% carbon atoms, 25.73% oxygen atoms, 21.79% silicon atoms, 5.35% aluminum atoms, and 1.77% potassium atoms.
[0099] , Thermal properties of the composite
[0100] , To define the thermal properties, the composite, obtained by using dicyclopentadiene resin (DCPD), was tested in its thermal properties to determine both its thermal stability and its degradation profile. The sample of the present invention was analyzed using the techniques of differential scanning calorimetry (DSC) and thermogravimetric analysis (TGA), carried out in the certified laboratory of the Center for Characterization and Development of Materials (CCDM / DEMA / UFSCar).
[0101] , In the differential scanning calorimetry (DSC) technique, the difference in energy supplied to a substance (sample) and a reference material (standard) is determined as a function of temperature, with both simultaneously subjected to a controlled temperature variation program. Considering that the phase transitions of materials occur under heat flow, with the release (in the case of exothermic events) or absorption (in the case of endothermic events), phenomena such as solidification, melting, glass transition, oxidation, and curing can be monitored. The DSC curves of the same preferred embodiment were acquired on a device Netzsch brand model DSC 214 Polyma, under nitrogen gas flow of 50ml / min, using a sealed aluminum pan, following the heating / cooling program described here: (a) Heating from 23°C to 300°C using a rate of 20°C / min; (b) Isotherm at 300°C for 5 minutes; (c) Cooling from 300°C to 23°C using a rate of 20°C / min; (c) Isotherm at 23°C for 5 minutes; and (d) Heating from 23°C to 300°C using a rate of 20°C / min.
[0102] The results of the analysis of the sample of the preferred embodiment, obtained using the dicyclopentadiene (DCPD) resin of the present invention, showed that after 14 days of curing, a slight residual curing occurs in two endothermic events of 10 and 20 J / g at temperatures of 114°C and 230°C, respectively, and the curing of the material can be considered virtually complete during this period. In conventional Portland cement concrete, there is a more intense curing process in the first 7 days, and the curing process can be considered virtually complete after 28 days. However, the curing of conventional Portland cement concrete can take up to 2 years to be completely completed, depending on the application.
[0103] Thermogravimetric analysis is an analytical technique that monitors the variation in sample mass as a function of temperature variation. Thermogravimetric analysis of the same preferred embodiment was conducted on a TA Instruments TA Q500 thermogravimetric analyzer, using a heating rate of 20°C / min, an alumina pan, and a temperature range of 30 to 850°C. In the first stage of the analysis, with temperatures ranging from 30°C to 550°C, an inert nitrogen gas atmosphere was used at a flow rate of 50 mL / min. In the second stage of the analysis, with a temperature range of 550°C to 850°C, an oxidative oxygen gas atmosphere was used at a flow rate of 50 mL / min.
[0104] , The results of the thermogravimetric analysis of the preferred embodiment using dicyclopentadiene resin (DCPD) showed that up to 230°C there was a slight elimination of residual monomers and water, originating from residual curing of the material, in the order of 0.79% m / m. From 230°C to 550°C, a mass loss of 8.11% m / m was recorded corresponding to the degraded organic matter, from the polymer chains with the lowest molar mass. At 850°C, a mass of 90.44% w / w of residual ash was obtained. This result demonstrates that the material from a preferred embodiment using DCPD resin exhibits high thermal stability.
[0105] , Flammability Test
[0106] , Considering further the characterization of the thermal properties and fire susceptibility of the material of the present invention, a flammability test was performed on the same preferred embodiment. The flammability test was performed by the CCDM certified laboratory, in accordance with IEC 60695-11-20:2015 Fire Hazard Testing Part 11-20: Test Flames. The results demonstrated that the material produced by a preferred embodiment with DCPD resin is flame resistant, with no visible flame being observed on the opposite face of the test specimen, nor was there any formation of a hole larger than 3 mm in the test specimen after cooling.
[0107] , Mechanical Properties
[0108] , The determination of the mechanical properties of axial compressive strength and diametrical compressive tensile strength was carried out in the certified laboratory of Falcão Bauer (Technological Center for Quality Control) following the Technical Standards ABNT NBR 7680-1 / 2015 (ASTM C39) and ABNT NBR 7222:2011 (ASTM C496 / C496M), respectively, in test specimens obtained according to the present invention containing the resin dicyclopentadiene (DCPD). The determined axial compressive strength was (70.5 ± 0.2) MPa and the diametrical compressive tensile strength was (6.1 ± 0.1) MPa. A typical embodiment of Portland cement presents axial compressive strength values ranging between 10 and 45 MPa and diametrical compressive tensile strength ranging between 2 and 7 MPa, depending on the mix or water / cement ratio used.Thus, the embodiment of the present invention, using DCPD resin, is more resistant to axial compression than a typical Portland cement embodiment. This same preferred embodiment also has tensile strength by diametrical compression equivalent to that achieved by a typical Portland cement embodiment.
[0109] , Load testing of beams in two preferred embodiments, both with dicyclopentadiene resin, was conducted by a large construction company in its Large Structures Laboratory, according to ABNT NBR 9607:2019 Standard (similar to ACI-318:2002) on beams measuring 50cm x 30cm x 2.87m. A total load of 21.5 tons was loaded on the beams of the two preferred embodiments, and the deflection formed by the load on the beams was measured. No deflection was determined, that is, the deformation suffered by both beams subjected to the load of 21.5 tons was equal to Omm.
[0110] , The determination of the abrasion resistance property was carried out through the abrasion wear test in the certified laboratory of Falcão Bauer (Technological Center for Quality Control), following the ABNT NBR 9781-1 / 2013 (ASTM C936 / C936M 20) standards, on samples of interlocking floors of the same preferred embodiment with dicyclopentadiene resin (DCPD). The abrasion wear value obtained for the material of the present invention was 19.5mm, which, according to the ABNT NBR 9781 (ASTM C936 / C936M 20) standard, classifies the interlocking floor of this material as highly resistant to wear, since the value is less than 20.0mm of abrasion wear.
[0111] , Considering that sleepers are in practice inverted double-supported beams, some evaluations made for these applications may be relevant to the present invention. Among the main evaluations that should be considered are the positive and negative moments, the resistance to repeated loading at the support, and the overload at the rail support for a preferred embodiment with dicyclopentadiene (DCPD) resin.
[0112] , The evaluation of the positive and negative moments, at the supports and at the center, for a preferred embodiment using a dicyclopentadiene resin, was carried out in accordance with ABNT NBR 11709:2015 and AREMA:2019 standards, at the LAEDE (Acoustics and Dynamic and Static Testing Laboratory) certifying laboratory, using loads of 108.93 kN at the negative moment at the supports, 143.21 kN at the positive moment at the supports, 39.66 kN at the negative moment at the center and 27.76 kN at the positive moment at the center. No damage, cracks or fissures were observed at any point of the tested sleeper, which behaves as an inverted double-supported beam.
[0113] , The evaluation of repeated loading on the support, which can also The fatigue test, which can be called a fatigue test, was performed in accordance with ABNT NBR 11709:2015 and AREMA:2019 standards at the LAEDE (Acoustics and Dynamic and Static Testing Laboratory) certification laboratory, employing loads ranging from 14.32 kN to 157.53 kN, which corresponds to a variation of 10 to 110% of the positive moment load on the supports. Furthermore, a frequency of 7 Hz was used for a total of 3 million loading and unloading cycles. No damage, cracks, or fissures were observed at any point on the sleeper, produced from a preferred embodiment using the dicyclopentadiene (DCPD) resin of the present invention.
[0114] The sleeper's overload capacity was assessed by applying a 250.62 kN force to its support at a rate of 50 kN / min. This overload was applied for a period of 5 minutes and then unloaded at the same rate, in accordance with NBR 11709:2015 and AREMA:2019 standards, at the LAEDE (Acoustics and Dynamic and Static Testing Laboratory) certification laboratory. No damage, cracks, or fissures were recorded at any point on the sleeper, which was produced with the same preferred embodiment using dicyclopentadiene (DCPD) resin. Immediately after, the sleeper support was loaded again at the same rate to the breaking point, which reached a load of 318.30 kN.
[0115] , The modulus of elasticity (MOE) and modulus of rupture (MOR) of the same preferred embodiment using dicyclopentadiene resin (DCPD) were tested following the NBR 11709:2015 and AREMA:2019 standards, at the LAEDE (Acoustics and Dynamic and Static Testing Laboratory) certifying laboratory, at a displacement rate of 127 mm / min. When applying a load of 30.8 kN, there was not enough flexion to measure the deflection at the center of the sleeper due to its high stiffness and, based on this result, it is estimated that the MOE is greater than 15 GPa. The modulus of rupture (MOR), determined for the tested sleeper produced with a preferred embodiment, was 21.59 MPa. The value recommended by AREMA:2019 is greater than 17.2 MPa. The modulus of elasticity (MOE) was also tested according to ABNT NBR 8522:2017 (ASTM C469) and determined at 15.7GPa.
[0116] , Another preferred embodiment, using PET monomer resin, was evaluated for its mechanical properties of axial compressive strength and abrasion wear resistance. Furthermore, its water absorption capacity was also evaluated. All tests were carried out in a certified laboratory of Falcão Bauer (Quality Control Technology Center) following the ABNT NBR 9781-1 / 2013 Standards (ASTM C936 / C936M > 20). The results obtained showed an axial compressive strength of (64.9 ± 8.2) MPa, an abrasion wear resistance of 20.5 mm, and a water absorption capacity of (5.4 ± 0.3)%.
[0117] , Having described an example of a preferred embodiment of the present invention, it should be understood that the scope of the present invention encompasses other possible variations of the inventive concept described, being limited only by the content of the appended claims, including possible equivalents.
[0118] , Example 1: Composite material production process.
[0119] , To prepare the composite material, the sand is first dried until it reaches a humidity level of less than or equal to 1%.
[0120] , The components are then weighed in the defined proportions, with an example of a preferred embodiment being composed of 81% sand; 8.35% filler, preferably gypsum, 9.65% resin, preferably DCPC; 0.38% initiator, preferably MEKP and 0.62% vinyltrimethoxysilane additive.
[0121] , After weighing, the dry sand and filler compounds are mixed in a conventional mixer (industrial mixer or concrete mixer) or even manually mixed if the quantity of composite to be produced is small, for approximately 20 minutes, under ambient pressure and temperature conditions, until complete homogenization.
[0122] , The next step is the formation of the organic liquid mixture (called Syrup), which consists of adding the additive (phase compatibilizing agent or flexibilizing agent, which are selected from the group consisting of: vinyltrimethoxysilane, methacryltrimethoxysilane, methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, calcium diacrylate, zinc diacrylate, butylacrylate, butylmethylacrylate, methylmethacrylate, triethyleneglycolmethacrylate, ethylhexylmethacrylate, IT (acrylic acid, methacrylic acid, or combinations thereof) of orthophthalic, isophthalic, and / or terephthalic unsaturated polyester associated with each other or with other components such as dicyclopentadiene (DCPD) or and mix for approximately 20 seconds to ensure homogeneity of the liquid phase. Then, the initiator methyl ethyl ketone peroxide, of medium reactivity, desensitized with dimethyl phthalate, is added to the liquid mixture and homogenized for approximately 20 seconds.
[0123] Finally, the dry mixture is added to a mixer, under which the liquid mixture is added and mixed immediately for 1 to 2 minutes until a homogeneous appearance is obtained.
[0124] , Example 2: Production process of beams, precast parts and interlocking flooring
[0125] , The composite material obtained according to example 1 is used for molding beams, pre-molded parts or floors in molds with previously established shapes and prepared with the application of a layer of release agent, which may be petroleum jelly, mineral oil, paraffins of vegetable, animal or petrochemical origin, polymeric solution of linear polymers (polyethylene, polypropylene, polyvinyl alcohol, polyvinyl chloride, polytetrafluoroethylene), polymeric or silicone films or combinations thereof.
[0126] , In the case of the production of larger parts such as beams and precast parts, a pressing force of approximately 20 tons is used for approximately 30 seconds, and for the production of smaller parts such as interlocking flooring, a pressing force of approximately 4 tons is used for approximately 30 seconds. After pressing, the part is sent for pre-curing in an oven at atmospheric pressure at a temperature of approximately 60°C for a period of 120 minutes and a subsequent curing process for a minimum period of 7 days at a pressure and temperature of 25°C.
Claims
CLAIMS 1. Polymeric composite characterized by comprising: - sand; - at least one organic or inorganic load; - at least one polyester resin; - at least one organic peroxide initiator; and - at least one additive.
2. Composite according to claim 1, characterized in that the filler is selected from the group consisting of fly ash or sugarcane bagasse or eucalyptus root or other vegetable or mineral residue, silica, alumina, limestone, foundry sand, talc, crushed stone powder, plaster, lime, dolomite, bentonite, barite, attapulgite, sepiolite, vermiculite, porous magnetite, calcium carbonate, magnesium carbonate, mica, graphite, gypsum, gilsonite and a combination thereof.
3. Composite according to claim 1, characterized in that the polyester resin is selected from the group consisting of orthophthalic, isophthalic and / or terephthalic unsaturated polyester resin associated with each other or with other components such as dicyclopentadiene (DCPD) or neopentyl glycol (NPG), polyethylene terephthalate (PET) monomer being a thermosetting resin and a combination thereof.
4. Composite according to claim 1, characterized in that the organic peroxide initiator is methyl ethyl ketone peroxide, of medium reactivity, desensitized with dimethyl phthalate.
5. Composite according to claim 1, characterized in that the additive is phase compatibilizing additives or flexibilizing additives.
6. Composite according to claim 5, characterized in that the phase compatibilizing additive is selected from the group consisting of by vinyltrimethoxysilane, methacryltrimethoxysilane, methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, calcium diacrylate, zinc diacrylate and combinations thereof; and the flexibilizing additive is selected from the group consisting of butylacrylate, butylmethylacrylate, methylmethacrylate, triethyleneglycolmethacrylate, ethylhexylmethacrylate, acrylic acid, methacrylic acid and combinations thereof.
7. Composite according to claim 3, characterized in that the resin is dicyclopentadiene present in an amount ranging from 4% to 44%, by mass, based on the total mass of the composite.
8. Composite according to claim 3, characterized in that the resin is PET monomer present in an amount ranging from 4% to 44%, by mass, based on the total mass of the composite.
9. Composite according to claim 3, characterized in that the resin is orthophthalic unsaturated polyester resin present in an amount ranging from 4% to 44%, by mass, based on the total mass of the composite.
10. Composite according to claim 3, characterized in that the resin is isophthalic unsaturated polyester resin present in an amount ranging from 4% to 44%, by mass, based on the total mass of the composite.
11. Composite according to claim 3, characterized in that the resin is terephthalic unsaturated polyester resin present in an amount ranging from 4% to 44%, by mass, based on the total mass of the composite.
12. Composite according to claim 3, characterized in that the resin is neopentyl glycol present in an amount ranging from 4% to 44%, by mass, based on the total mass of the composite.
13. Composite according to claim 1, characterized in that the sand is preferably medium-grained sand and is present in the proportion of 30% to 97% by mass, based on the total mass of the composite.
14. Composite according to either of claims 1 or 2, characterized in that it contains at least one filler in the proportion of 4% to 38%, by mass, based on the total mass of the composite.
15. Composite according to claim 1, characterized by comprising a reaction accelerator system; ground rubber and / or glass or metal fibers.
16. Composite according to claim 15, characterized in that the glass or metal fibers are short and uniformly distributed in the matrix or long and aligned in a single direction.
17. Composite according to claim 1, characterized in that it further comprises metallic or polymeric screens and frames in layers or structures.
18. Composite according to either of claims 1 or 13, characterized in that the sand comprises silica particles and may contain other minerals such as: feldspar, mica, zircon, magnetite, ilmenite, monazite and cassiterite.
19. Composite according to claim 2, characterized in that the ash comprises silicon dioxide (silica), aluminum oxide (alumina) and iron oxide (hematite).
20. Process for preparing the polymer composite as defined in any one of claims 1 to 19, characterized by comprising the following steps: (i) Sand drying; (ii) Weighing of the solid materials that make up the composite; (iii) Mixing of solid and dry materials, including sand and at least one load, for a period of 20 minutes, until completely homogenized; (iv) Weighing of the liquid materials that make up the composite; (v) Mixing at least one liquid additive, being a compatibilizing or flexibilizing agent, to a resin and complete homogenization for a period of 1 to 2 minutes, to obtain the organic mixture, also called syrup; (vi) Addition of the initiator to the organic mixture or syrup and homogenization for 1 to 2 minutes; (vii) Addition of the prepared organic mixture to the mixture of dry components; (viii) Homogenization of the formed mass, for a period of 1 to 3 minutes.
21. Use of a polymeric composite as described in any one of claims 1 to 19, characterized in that it is for the production of artifacts selected from beams, columns, precast tiles, sleepers, crosspieces, purlins, precast gutters, interlocking floors, precast civil construction panels, posts, poles, artificial stone for countertops and floors, paving slabs used in bridges, precast slabs, covering plates and / or cobogós.
22. Use of a polymer composite prepared by the process as defined in claim 20, characterized in that it is for the preparation of an artifact selected from beams, columns, precast tiles, sleepers, crosspieces, purlins, precast gutters, interlocking floors, precast civil construction panels, posts, poles, artificial stone for countertops and floors, paving slabs used in bridges, precast slabs, covering plates and / or cobogós.
23. Use according to claim 21, characterized in that the artifact is a beam, precast piece or interlocking floor.
24. Production process of beams, precast parts and interlocking flooring characterized by comprising the following steps: (i) Sand drying; (ii) Weighing of the solid materials that make up the composite; (iii) Mixing of solid and dry materials, including sand and at least one load, for a period of 20 minutes, until completely homogenized; (iv) Weighing of the liquid materials that make up the composite; (v) Mixing at least one liquid additive, being a compatibilizing or flexibilizing agent, to a resin and complete homogenization for a period of 1 to 2 minutes, to obtain the organic mixture, also called syrup; (vi) Addition of the initiator to the organic mixture or syrup and homogenization for 1 to 2 minutes; (vii) Addition of the prepared organic mixture to the mixture of dry components; (viii) Homogenization of the formed mass, for a period of 1 to 3 minutes; (ix) Molding of beams, precast parts or floors in molds with previously established shapes and prepared with the application of a layer of release agent, (x) Pressing of around 20 tons of pressure for larger parts, such as beams and precast parts, and at least 4 tons of pressure for smaller parts such as interlocking flooring. (xi) pre-curing in an oven at atmospheric pressure at a temperature of approximately 60°C for a period of 120 minutes; (xii) curing process for a minimum period of 7 days at room pressure and temperature at a temperature of approximately
Citation Information
Patent Citations
Resin Composition for Engineered Stone and Engineered Stone Formed Therefrom
US20200123057A1
Polymer composite, use of said composite in preparing articles, process of preparing said composite and articles comprising said composite
US20210317284A1