Raw material composition of foam cement, foam cement and preparation method therefor and use thereof, and battery
By preparing foamed cement with flame retardant, heat-insulating and fire-resistant properties, the problem of fire spread in new energy vehicle battery packs has been solved, and the fire spread and hazard reduction in the battery field have been effectively controlled, while production costs have been reduced.
Patent Information
- Application Number
- PCT/CN2023/088580
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-17
AI Technical Summary
New energy vehicle battery packs are at risk of fire and explosion due to the instability of lithium-ion batteries. Existing insulation materials cannot have both mechanical strength and flame retardant, thermal insulation and fire resistance properties, causing fires to spread rapidly.
The foamed cement raw material composition composed of cement, foaming agent, accelerating setting agent, water reducing agent, etc. is used to prepare foamed cement through synergistic coordination, which has excellent flame retardant, heat insulation and fire resistance properties, and maintains good mechanical properties. strength.
It can effectively control the spread of fire in the battery field, reduce the range of battery fire or explosion, increase the fire resistance time, and reduce production costs.
Smart Images

Figure PCTCN2023088580-FTAPPB-I100001 
Figure PCTCN2023088580-FTAPPB-I100002 
Figure PCTCN2023088580-FTAPPB-I100003
Abstract
Description
Raw material composition of foamed cement, foamed cement, preparation method, application, and battery
[0001] This application claims priority to Chinese patent application No. 2023103819150, filed April 11, 2023. This application incorporates the entirety of the aforementioned Chinese patent application. Technical Field
[0002] The invention relates to a raw material composition of foamed cement, foamed cement, a preparation method, application and a battery. Background Art
[0003] New energy vehicle battery packs and energy storage power station enclosures utilize a large number of lithium-ion batteries. Due to their instability, battery packs present a risk of fire and explosion. This is particularly true when cells are squeezed, overcharged, short-circuited, or exposed to heat. Fires can easily occur when the flames spread to adjacent cells, potentially causing inter-cell explosions. When a large number of cells ignite, the battery pack can burst into flames.
[0004] Currently, new energy vehicle battery packs are lined with sheet materials such as aerogel mats, polymer fire-retardant coatings, high-silica wool felt, mica sheets, and ultra-fine glass wool to isolate heat diffusion and control the spread of fire. While existing technologies can achieve a certain degree of heat isolation and fire control, they still have many shortcomings, such as significantly increasing battery weight and cost. Most importantly, these methods simply aim to delay flames and heat conduction to a certain extent, without inhibiting flame and temperature transmission. This results in a short fire-blocking period and rapid fire spread after the skeleton collapses due to combustion.
[0005] Summary of the Invention
[0006] To overcome the drawback of existing sheet materials used in new energy vehicle battery packs, which lack both mechanical strength and flame retardancy, thermal insulation, and fire resistance, the present invention provides a foamed cement raw material composition, foamed cement, preparation method, application, and battery. The foamed cement produced from the foamed cement raw material composition of the present invention exhibits excellent flame retardancy, thermal insulation, and fire resistance while maintaining good mechanical strength and low production costs.
[0007] The present invention adopts the following technical solutions to solve the above technical problems.
[0008] The present invention provides a raw material composition for foamed cement, which comprises the following components in parts by weight:
[0009] 65-98 parts of cement, 0.01-25 parts of foaming agent, 0.5-6 parts of accelerating agent and 0.5-4 parts of water reducing agent;
[0010] The foaming agent includes one or more of ferrous sulfate, hydrogen peroxide and sodium lauryl sulfate.
[0011] In the present invention, the cement may be one or more of Portland cement, ordinary Portland cement, composite Portland cement, sulfoaluminate cement, and magnesium oxychloride cement, such as ordinary Portland cement or Portland cement. Portland cement refers to any hydraulic cementing material made by grinding Portland cement clinker primarily composed of calcium silicate, less than 5% limestone or granulated blast furnace slag, and an appropriate amount of gypsum, collectively referred to internationally as Portland cement. Ordinary Portland cement refers to a hydraulic cementing material made by grinding Portland cement clinker, 5%-20% mixed materials, and an appropriate amount of gypsum. Composite Portland cement refers to a hydraulic cementing material made by grinding Portland cement clinker, two or more specified mixed materials, and an appropriate amount of gypsum. Sulphoaluminate cement refers to a hydraulic cementing material made by grinding a clinker containing anhydrous calcium sulfoaluminate and dicalcium silicate as the main mineral components, obtained by calcining raw materials of appropriate composition, and adding varying amounts of limestone and an appropriate amount of gypsum. The magnesium oxychloride cement refers to a hardened cement formed by using light-burned powder obtained by calcining magnesite ore or ash powder (mainly MgO) obtained by low-temperature calcining dolomite as a binder, magnesium chloride hexahydrate (MgCL2·6H2O) and other water-soluble magnesium salts as a blending agent, and then adding water.
[0012] The compressive strength of the ordinary Portland cement is preferably 50MPa-60MPa, for example, 52.5MPa. The model of the ordinary Portland cement is preferably PO52.5. The compressive strength of the Portland cement is preferably 50MPa-60MPa, for example, 52.5MPa. The model of the Portland cement is preferably PI52.5. The compressive strength is tested using the method specified in GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", which is as follows: cement, standard sand and water are mixed in a mass ratio of 1:3.0:0.5 to form a standard test piece of 40mm×40mm×160mm, and the test piece is cured for 28 days under standard curing conditions (20±1 degrees Celsius, relative humidity of 90% or more in air), and its compressive strength is measured.
[0013] In the present invention, the mass fraction of the cement is preferably 80 parts to 95 parts, such as 85 parts, 86 parts or 90 parts.
[0014] In the present invention, the foaming agent is preferably ferrous sulfate and hydrogen peroxide, or sodium lauryl sulfate.
[0015] Wherein, when the foaming agent is ferrous sulfate and hydrogen peroxide, the mass ratio of the ferrous sulfate to the hydrogen peroxide is preferably 1:(1-5), for example, 1:3.
[0016] In the present invention, the mass fraction of the foaming agent is preferably 3 parts to 10 parts, such as 4 parts, 8 parts or 9 parts.
[0017] In the present invention, the accelerating setting agent generally refers to an admixture added to concrete to enable the concrete to set and harden quickly. The accelerating setting agent can be any one of an aqueous solution of aluminum sulfate, sodium aluminate, potassium aluminate, sodium silicate, potassium silicate or other commercially available accelerating setting agents, such as potassium silicate.
[0018] In the present invention, the mass fraction of the quick-setting agent is preferably 0.5 parts to 1.5 parts, for example, 1 part.
[0019] In the present invention, the water reducer generally refers to a concrete admixture that can reduce the amount of mixing water while maintaining the concrete slump substantially unchanged. The water reducer can be conventional in the art, preferably one or more of a polycarboxylate water reducer, a naphthalene-based water reducer, or other commercially available water reducers, such as a polycarboxylate water reducer. The polycarboxylate water reducer is preferably PCV-A, purchased from Jiangsu Subote New Materials Co., Ltd. The water reducer can be in liquid or powder form.
[0020] In the present invention, the mass fraction of the water reducer is preferably 0.5 parts to 1.5 parts, for example 0.8 parts.
[0021] In the present invention, the raw material composition of the foamed cement preferably further comprises a reinforcing resin, wherein the weight percentage of the reinforcing resin is preferably 0-10 parts, for example 8 parts.
[0022] The reinforcing resin may be one or more of water-based acrylic resin, water-based polyester resin, water-based polyurethane resin and water-based epoxy resin, such as water-based acrylic resin. The model of the water-based acrylic resin is preferably W118-45.
[0023] In the present invention, the raw material composition of the foamed cement preferably further comprises a curing agent, wherein the mass fraction of the curing agent is preferably 0-10 parts, for example, 2 parts.
[0024] The curing agent may be one or more of an aziridine curing agent, an isocyanate curing agent, a Wanhua isocyanate and an epoxy curing agent, such as an isocyanate curing agent.
[0025] The aziridine curing agent is preferably DSM Crosslinker CX 100. The isocyanate curing agent is preferably Converstro Bayhydur XP 2655 or Aquolin 270. The epoxy curing agent is preferably one or more of Cardolite NX-8502, NX8101, NX8401, NX8402, NX-8501 and NX-8502.
[0026] In the present invention, the raw material composition of the foamed cement preferably further comprises an admixture, wherein the mass fraction of the admixture is preferably 1 to 50 parts, more preferably 5 to 15 parts, for example 10 parts.
[0027] The admixture can be conventional in the art, preferably one or more of quicklime, gypsum, fly ash, silica fume, and corundum, such as fly ash or corundum. The fly ash preferably has a particle size of 300-350 mesh, such as 325 mesh. The corundum is preferably CT016, purchased from Jiangsu Chentu Building Materials Co., Ltd.
[0028] In the present invention, the raw material composition of the foamed cement preferably further comprises an alkali activator, wherein the mass fraction of the alkali activator is preferably 0-5 parts, more preferably 2-4.5 parts, for example 4.2 parts.
[0029] The alkaline activator may be any one of alkaline activators such as sodium hydroxide, calcium hydroxide, water glass, etc., for example, water glass or calcium hydroxide.
[0030] In the present invention, the raw material composition of the foamed cement preferably also includes reinforcing fiber. Reinforcing fiber refers to fiberglass reinforced plastics and other composite materials used in structural materials. It is a commonly used fibrous reinforcing material and can be divided into two categories based on its chemical composition: inorganic fiber and organic fiber. The weight percentage of the reinforcing fiber can be 10 to 60 parts, for example 40 parts.
[0031] The types of the reinforcing fibers may be conventional in the art, and preferably include one or more of glass fibers, basalt fibers, carbon fibers, and the like.
[0032] The length of the reinforcing fibers may be 3 mm to 25 mm, for example, 3 mm, 6 mm, 12 mm or 25 mm.
[0033] In a preferred embodiment of the present invention, the reinforcing fibers are glass fibers with a length of 3 mm, glass fibers with a length of 6 mm, glass fibers with a length of 12 mm, and glass fibers with a length of 20 mm. The mass ratio of the glass fibers with a length of 3 mm, the glass fibers with a length of 6 mm, the glass fibers with a length of 12 mm, and the glass fibers with a length of 20 mm can be 15:10:10:5.
[0034] In the present invention, the raw material composition of the foamed cement preferably does not include a dispersant. The dispersant can be a conventional substance in the art that can play a dispersing role in cement.
[0035] In a preferred embodiment, the raw material composition of the foamed cement includes the following components in parts by weight: 85-90 parts of cement, 4-5 parts of alkali activator, 0.5-1.2 parts of accelerator, 0.5-1 part of water reducer, 4-9 parts of foaming agent, 8-12 parts of admixture, 5-10 parts of reinforcing resin, 1-3 parts of curing agent, and 35-45 parts of reinforcing fiber.
[0036] In a preferred embodiment, the raw material composition of the foamed cement includes the following components in parts by weight: 85 parts of cement, 4.2 parts of alkali activator, 1 part of accelerator, 0.8 part of water reducer, 9 parts of foaming agent, 10 parts of admixture, 8 parts of reinforcing resin, 4 parts of curing agent, and 40 parts of reinforcing fiber.
[0037] The present invention also provides a method for preparing foamed cement, which comprises the following steps: mixing the raw material composition of the foamed cement as described above with water, and foaming and molding the mixture.
[0038] In the present invention, the mass ratio of the raw material composition of the foamed cement to the water may be (0.8-2.0):1, for example, 1.1:1, 1.2:1, 1.22:1 or 1.33:1.
[0039] In the present invention, the method for preparing the foamed cement preferably comprises the following steps: firstly, the cement, the admixture and the foaming agent are pre-mixed uniformly, and then the remaining raw materials are added and stirred uniformly to obtain the foamed cement.
[0040] In the present invention, the method for preparing the foamed cement preferably comprises the following steps:
[0041] When the foamed cement has a single-layer structure, the raw material composition of the foamed cement as described above is mixed with water to obtain cement slurry; the cement slurry is poured into a mold, left to stand for foaming and forming, and then coated.
[0042] Among them, when the foamed cement has a multi-layer structure, the raw material composition of the foamed cement as described above is mixed with water to obtain cement slurry; the cement slurry is poured into a mold, left to stand for foaming and molding, and then coated to obtain a single-layer structure foamed cement; then the cement slurry is continued to be poured into a mold on the surface of the single-layer structure foamed cement as described above, left to stand for foaming and molding, and coated, and the above steps are repeated in sequence.
[0043] The mixing process is generally further stirred. The stirring is generally performed in a blender. The stirring speed may be 100 rpm to 1000 rpm, for example, 500 rpm. The stirring time may be 5 min to 30 min, for example, 10 min.
[0044] The pouring flow rate may be 1 kg / min-3 kg / min, for example 2 kg / min.
[0045] The standing time may be 2 hours to 24 hours, for example 12 hours.
[0046] In the present invention, after coating, when the foamed cement reaches a demoulding strength, the foamed cement can be demoulded and removed. The demoulding strength generally refers to a Barcol hardness greater than 10.
[0047] In the present invention, the coating can be performed by dipping or spraying the coating. After the coating, the thickness of the coating can be 20 μm-200 μm, for example, 25 μm.
[0048] The coatings include water-based paints, solvent-based paints, and light-curing paints. The water-based paints are preferably Interchar 1120HFA120 purchased from Akzo Nobel, STEELGUARD 651 purchased from PPG, or CYB21-GG180 purchased from Dalian Yibang Technology Co., Ltd. The solvent-based paints are preferably the flame-retardant paint HS-LF series and the corresponding curing agent (peroxide) purchased from Changzhou Huake Polymer Co., Ltd., or Interchar 1983 HFA198 purchased from Akzo Nobel. The light-curing paints are preferably 5640, 2606, 3620, or 3910 purchased from Nanxiong Ketian Chemical Co., Ltd.
[0049] The dipping conditions may be conventional in the art, for example, including the following steps: dipping the foamed cement in the coating at 5° C.-40° C. for 5 seconds-30 seconds, and drying.
[0050] The drying temperature may be 5° C.-40° C., for example, 30° C. The drying time may be 5 s-2 h, for example, 1 h.
[0051] The spraying conditions may be conventional in the art, for example, including the following steps: spraying the coating on the surface of the foamed cement board at 5° C.-40° C. and drying.
[0052] The drying temperature may be 5° C. to 40° C. The drying time may be 5 seconds to 2 hours.
[0053] Wherein, when the coating is the light-curing coating, the dipping or spraying is generally carried out under a light-curing light source. The light-curing light source is preferably an ultraviolet lamp or an LED lamp. The light intensity of the light-curing light source can be 200mJ / cm 2 -1000mJ / cm 2 .
[0054] The present invention also provides a foamed cement, which is prepared by the above-mentioned preparation method.
[0055] In the present invention, the foamed cement may be a single-layer structure or a multi-layer structure.
[0056] Wherein, when the foamed cement is a single-layer structure, the single-layer structure is a flat plate. The density of the foamed cement can be 200kg / m 3 -1000kg / m 3 .
[0057] Wherein, when the foamed cement is a multi-layer structure, the number of layers of the multi-layer structure is at least two. The average density of the foamed cement can be 220kg / m 3 -900kg / m 3 .
[0058] In the present invention, the thickness of the foamed cement may be 0.2 mm to 3 mm, for example, 0.5 mm, 1 mm or 2 mm.
[0059] In the present invention, the thermal conductivity of the foamed cement may be ≤0.06 W / (m·K), preferably 0.01-0.06 W / (m·K).
[0060] In the present invention, the compressive strength of the foamed cement may be 0.5 MPa-11 MPa.
[0061] In the present invention, the refractory temperature of the foamed cement may be ≤1300°C.
[0062] The present invention also provides a foamed cement, the components of which include cement, an accelerating setting agent and a water reducing agent, the porosity of which is 40%-71%, and the average pore diameter of which is 200μm-350μm.
[0063] In the present invention, the components of the foamed cement preferably further include one or more of a reinforcing resin, a curing agent, an admixture, an alkali activator, and a reinforcing fiber, for example, a reinforcing resin, a curing agent, an admixture, an alkali activator, and a reinforcing fiber. The types and proportions of the reinforcing resin, curing agent, admixture, alkali activator, and reinforcing fiber can be as described above.
[0064] In the present invention, the porosity of the foamed cement is preferably 40.5%-70.5%, for example, 40.9%, 41.1%, 41.6%, 42.2%, 43.2%, 49.6%, 64.2%, 66.9%, 67.1%, 67.2%, 68.9% or 70.3%, more preferably 45%-67%.
[0065] In the present invention, the average pore size of the foamed cement is preferably 205 μm-345 μm, for example 207 μm, 215 μm, 216 μm, 218 μm, 220 μm, 235 μm, 290 μm, 305 μm, 313 μm, 330 μm or 340 μm, more preferably 220 μm-330 μm.
[0066] The present invention also provides an application of the foamed cement as described above in the field of batteries.
[0067] The present invention also provides a battery pack, which includes the foamed cement as described above.
[0068] On the basis of conforming to the common sense in this field, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0069] The reagents and raw materials used in the present invention are commercially available.
[0070] The positive progress effect of the present invention is:
[0071] The present invention uses cement as the primary gelling material, along with a foaming agent, an accelerator, and a water reducer, to produce foamed cement. This foamed cement not only possesses excellent mechanical properties but also boasts superior fireproofing, heat insulation, and barrier properties. Its compressive strength can range from 5.0 MPa to 7.4 MPa, its thermal conductivity can range from 0.023 W / (m·K) to 0.059 W / (m·K), and it can burn for at least 7 minutes at 1300°C. Its application in the battery field can limit the scope of battery fires or explosions and reduce hazards. DETAILED DESCRIPTION
[0072] The present invention is further illustrated by way of examples below, but the present invention is not limited to the scope of the examples. Experimental methods in the following examples where specific conditions are not specified were performed according to conventional methods and conditions, or selected according to the product specifications.
[0073] The raw materials used for the foamed cement in the following examples and comparative examples can all be obtained commercially. The commercial sources of the main raw materials are shown in Table 1 below:
[0074] Table 1
[0075] The formulas of the foamed cements of Examples 1 to 12 and Comparative Examples 1 and 2 are shown in Table 2 below:
[0076] Table 2
[0077] The preparation method of the foamed cement of Example 1 to Example 12 and Comparative Example 1 to Comparative Example 2 comprises the following steps:
[0078] Cement, admixtures and foaming agent were stirred in a mixer at a speed of 500 rpm for 10 minutes and mixed evenly. The remaining raw materials were then added to obtain cement slurry. The cement slurry was poured into a mold at a flow rate of 2 kg / min and allowed to stand for 12 hours for foaming to obtain foamed cement. When the Barcol hardness was greater than 10, the foamed cement was removed from the mold and immersed in a coating (Interchar 1120 HFA120) at 5-40°C for 5-30 seconds. After drying at 30°C for 1 hour, the coating had a thickness of 25 μm. A single-layer structure of foamed cement with a thickness of 0.2-3 mm was obtained, and its density was 500 kg / m 3 .
[0079] Effect embodiment
[0080] The foamed cements obtained in Examples 1 to 12 and Comparative Examples 1 and 2 were tested for the following indicators according to the following standards. The test results are shown in Table 3:
[0081] Porosity: Test standard is ASTM C948-81 (2016);
[0082] Average pore size: Use a cross-sectional optical microscope to observe 5-10 points of the foamed cement at a scale of 500nm to determine its pore size, and then calculate the average value to obtain the average pore size.
[0083] Compressive strength: GB / T 15231-2008;
[0084] Density: GB / T 15231-2008;
[0085] Thermal conductivity: GB / T 10294-2008;
[0086] Flame temperature resistance burning time: Use the test method of HB 7068.2-1994 standard, burn at 700℃ or 1300℃ respectively until the foamed cement burns through, and measure the burning time.
[0087] Flame retardant grade: GB / T 8624-2012.
[0088] Table 3
[0089] It can be seen from Table 3 that, relative to Examples 1-12, when the mass fraction of cement in Comparative Example 1 is smaller, the refractory time of the obtained foamed cement is shorter.
[0090] When the amount of foaming agent in Comparative Example 2 is small, the porosity of the obtained foamed cement is small, the thermal conductivity is large, and the fire resistance time is short.
[0091] Although the above describes specific embodiments of the present invention, it should be understood by those skilled in the art that these are merely illustrative and that various changes or modifications may be made to these embodiments without departing from the principles and essence of the present invention. Therefore, the scope of protection of the present invention is defined by the appended claims.
Claims
1. A raw material composition for foamed cement, characterized in that: It includes the following components in parts by mass: 65-98 parts of cement, 0.01-25 parts of foaming agent, 0.5-6 parts of accelerating agent and 0.5-4 parts of water reducing agent; The foaming agent includes one or more of ferrous sulfate, hydrogen peroxide and sodium lauryl sulfate.
2. The raw material composition of foamed cement according to claim 1, characterized in that: The raw material composition of the foamed cement meets one or more of the following conditions: (a) the foaming agent is ferrous sulfate and hydrogen peroxide, or sodium lauryl sulfate; (b) the cement is one or more of Portland cement, ordinary Portland cement, composite Portland cement, sulphoaluminate cement and magnesium oxychloride cement, such as ordinary Portland cement or Portland cement; the compressive strength of the ordinary Portland cement is preferably 50MPa-60MPa, such as 52.5MPa; the compressive strength of the Portland cement is preferably 50MPa-60MPa, such as 52.5MPa; (c) the quick-setting agent is an aqueous solution of aluminum sulfate, sodium aluminate, potassium aluminate, sodium silicate or potassium silicate, such as potassium silicate; (d) The water reducer is a polycarboxylate water reducer and / or a naphthalene-based water reducer, for example, a polycarboxylate water reducer.
3. The raw material composition of foamed cement according to claim 1 or 2, characterized in that: The raw material composition of the foamed cement meets one or more of the following conditions: (e) the mass fraction of the foaming agent is 3 parts to 10 parts, for example 4 parts, 8 parts or 9 parts; Wherein, when the foaming agent is ferrous sulfate and hydrogen peroxide, the mass ratio of the ferrous sulfate to the hydrogen peroxide is preferably 1:(1-5), for example 1:3; (f) the mass fraction of the cement is 80 parts to 95 parts, for example 85 parts, 86 parts or 90 parts; (g) the mass fraction of the accelerating setting agent is 0.5 parts to 1.5 parts, for example, 1 part; (h) The mass fraction of the water reducing agent is 0.5 parts to 1.5 parts, for example 0.8 parts.
4. The raw material composition for foamed cement according to at least one of claims 1 to 3, characterized in that: The raw material composition of the foamed cement meets one or more of the following conditions: (i) the raw material composition of the foamed cement further comprises one or more of a reinforcing resin, a curing agent, an admixture, an alkali activator and a reinforcing fiber; Among them, the mass fraction of the reinforcing resin is preferably 0-10 parts, for example, 8 parts; the mass fraction of the curing agent is preferably 0-10 parts, for example, 2 parts; the mass fraction of the admixture is preferably 1-50 parts, more preferably 5-15 parts, for example, 10 parts; the mass fraction of the alkali activator is preferably 0-5 parts, more preferably 2-4.5 parts, for example, 4.2 parts; the mass fraction of the reinforcing fiber is preferably 10-60 parts, for example, 40 parts; Wherein, the reinforcing resin is preferably one or more of water-based acrylic resin, water-based polyester resin, water-based polyurethane resin and water-based epoxy resin, such as water-based acrylic resin; the model of the water-based acrylic resin is preferably W118-45; Wherein, the curing agent is preferably one or more of aziridine curing agent, isocyanate curing agent, Wanhua isocyanate and epoxy curing agent, such as isocyanate curing agent; the aziridine curing agent is preferably DSM Crosslinker CX 100; the isocyanate curing agent is preferably Converstro Bayhydur XP 2655 or Aquolin 270; the epoxy curing agent is preferably one or more of Cardolite NX-8502, NX8101, NX8401, NX8402, NX-8501 and NX-8502; Wherein, the admixture is preferably one or more of quicklime, gypsum, fly ash, silica fume and corundum, such as fly ash or corundum; Wherein, the alkaline activator is preferably sodium hydroxide, calcium hydroxide or water glass, such as water glass or calcium hydroxide; The type of the reinforcing fiber preferably includes one or any combination of glass fiber, basalt fiber and carbon fiber; the length of the reinforcing fiber is preferably 3 mm-25 mm, such as 3 mm, 6 mm, 12 mm or 25 mm; (j) The raw material composition of the foamed cement does not include a dispersant.
5. A method for preparing foamed cement, characterized in that: The method comprises the following steps: mixing the raw material composition of the foamed cement according to any one of claims 1 to 4 with water, and foaming and molding the mixture; The mass ratio of the raw material composition of the foamed cement to the water is preferably (0.8-2.0):1, such as 1.1:1, 1.2:1, 1.22:1 or 1.33:
1.
6. The method for preparing foamed cement according to claim 5, characterized in that: The preparation method of the foamed cement comprises the following steps: when the foamed cement is a single-layer structure, mixing the raw material composition of the foamed cement according to any one of claims 1 to 4 with water to obtain cement paste; pouring the cement paste into a mold, standing it for foaming and forming, and coating it; When the foamed cement is a multi-layer structure, the raw material composition of the foamed cement as described in any one of claims 1 to 4 is mixed with water to obtain cement slurry; the cement slurry is poured into a mold, left to stand for foaming and forming, and coated to obtain a single-layer structure foamed cement; the cement slurry is then poured into a mold on the surface of the single-layer structure foamed cement as described above, left to stand for foaming and forming, and coated, and the above steps are repeated in sequence.
7. A foamed cement, characterized in that: It is prepared by the method for preparing foamed cement as claimed in claim 5 or 6; Preferably, the foamed cement is a single-layer structure or a multi-layer structure; When the foamed cement is a single-layer structure, the single-layer structure is a flat plate; the density of the foamed cement is preferably 200 kg / m 3 -1000kg / m 3 ; Wherein, when the foamed cement is a multi-layer structure, the number of layers of the multi-layer structure is at least two; the average density of the foamed cement is preferably 220 kg / m 3 -900kg / m 3 ; Preferably, the thickness of the foamed cement is 0.2 mm-3 mm, for example 0.5 mm, 1 mm or 2 mm; Preferably, the thermal conductivity of the foamed cement is ≤0.06 W / (m·K), preferably 0.023-0.059 W / (m·K); Preferably, the compressive strength of the foamed cement is 5.0MPa-7.4MPa; Preferably, the refractory temperature of the foamed cement is ≤1300°C.
8. A foamed cement, characterized in that: Its porosity is 40%-71% and its average pore size is 200μm-350μm.
9. Use of the foamed cement as claimed in claim 7 or 8 in the field of batteries.
10. A battery pack, characterized in that: It comprises the foamed cement as described in claim 7 or 8.
Citation Information
Patent Citations
Light-weight foamed fire-proof plate and preparation method thereof
CN102001850A
Desulfurized ash residue mixed dry mortar
CN102659365A
Light-weight concrete, multifunctional protective plate adopting concrete, and preparation method
CN103922668A
Inorganic foaming thermal-insulation mortar and preparation method thereof
CN103922789A
Chemical foamed concrete and preparation method thereof
CN104250071A
Cited By
Inorganic quick-setting filling material and preparation method thereof
CN119504220A
Fly ash-based foam concrete as well as preparation method and application thereof
CN121293008A
Composite thermal insulation material suitable for A-grade fire prevention and preparation method thereof
CN121318337A