Simple preparation method for and use of hydrogenation catalyst support

The direct mixing method to prepare ZIFs-derived CN materials solves the problems of high preparation cost and environmental pollution in the existing technology, and achieves efficient and environmentally friendly catalyst preparation and excellent catalytic activity, which is suitable for the hydrogenation of phenol to cyclohexanone reaction.

WO2024212294A1PCT designated stage expired Publication Date: 2024-10-17NANJING TECH UNIV

Patent Information

Application Number
PCT/CN2023/092652
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2023-05-08
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The application of existing ZIFs-derived CN materials in the catalytic field is limited by factors such as high preparation costs, low raw material utilization, unfriendly preparation processes, and low catalyst yields, resulting in limited applications in the catalytic field.

Method used

The direct mixing method is used to mix 2-methylimidazole and cobalt source and then calcined. After pickling and drying, a high-efficiency phenol hydrogenation Pd@CN catalyst is prepared, which avoids the use of organic solvents, simplifies the preparation process, and improves the utilization rate of raw materials. and catalyst yield.

Benefits of technology

It achieves high yield, rich pore structure and high catalytic activity of CN materials, reduces preparation costs and environmental pollution, and is suitable for industrial production. The catalyst shows a phenol conversion rate of 98.6% and a cyclohexane conversion rate of 94.1% in the phenol-cyclohexane system. Hexanone selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023092652_17102024_PF_FP_ABST
    Figure CN2023092652_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of catalytic hydrogenation, and relates to a simple preparation method for and use of a hydrogenation catalyst support. The support is prepared by using a direct mixing method, that is, 2-methylimidazole is directly mixed with different cobalt sources, the mixture is calcined, and then acid pickling is carried out to obtain the support. The method has the advantages of simple preparation process, short preparation period, low raw material cost, high support yield, and the like. A Pd@CN catalyst prepared by the support provided by the present invention has good catalytic activity when applied to a reaction system of hydrogenation of phenol to cyclohexanone.
Need to check novelty before this filing date? Find Prior Art

Description

A simple preparation method and application of hydrogenation catalyst carrier Technical Field

[0001] The invention belongs to the technical field of catalytic hydrogenation catalyst preparation, and relates to a simple preparation method and application of a hydrogenation catalyst carrier. Background Art

[0002] Zeolitic imidazolate frameworks (ZIFs), formed by the coordination of metal ions (such as Zn and Co) and organic ligands (imidazole or its derivatives), are a special class of MOFs (metal-organic frameworks) with advantages such as large surface area, rich pore structure, easy functionalization, and excellent stability (thermal and chemical stability). The rich nitrogen content and inherited pore structure of ZIFs' organic ligands make them ideal precursors for the preparation of CN materials, with wide applications in catalysis.

[0003] The typical preparation process for existing ZIF-67-based CN materials is as follows: using methanol as a solvent, 2-methylimidazole, and a cobalt source as ligands, ZIF-67 is first synthesized, followed by calcination under an Ar atmosphere, and then acid washing to prepare a CN support (e.g., ZL201610912429.7, ZL201710344634.2). These traditional ZIF-derived CN preparation methods require the synthesis of specific ZIFs and utilize large amounts of organic solvents during the synthesis process, which easily wastes uncoordinated raw materials in the solution and results in low raw material utilization. Furthermore, these traditional methods involve complex synthesis steps and significant raw material loss during the synthesis process, resulting in low catalyst yield and high production costs. Furthermore, the use of large amounts of solvents leads to severe environmental pollution during the production process. Therefore, the current application of ZIF-based CN materials in catalysts is hampered by high preparation costs, low raw material utilization, environmentally unfriendly preparation processes, and low catalyst yields, limiting the further application of ZIF-derived CN materials in catalysis.

[0004] Summary of the Invention

[0005] The present invention proposes a new solution to the problems existing in the preparation process of ZIFs-derived Pd@CN catalysts, namely, a direct mixing method is used to mix 2-methylimidazole with different cobalt sources, and then a high-efficiency phenol hydrogenation Pd@CN catalyst is prepared through calcination, acid washing and loading steps.

[0006] In order to achieve the above object, the present invention is implemented by adopting the following technical solutions:

[0007] The CN support was prepared by a direct mixing method, that is, 2-methylimidazole was directly mixed with a cobalt source and then calcined to obtain Co@CN, which was then acid-washed and dried to obtain the CN support.

[0008] The preparation process of CN vector is as follows. Unless otherwise specified, the concentrations in the instructions are by mass:

[0009] Step 1: Mix 2-methylimidazole with a cobalt source;

[0010] Step 2: The above mixture is calcined under Ar atmosphere to obtain Co@CN;

[0011] Step 3: Add Co@CN to deionized water and concentrated nitric acid solution and stir;

[0012] Step 4: Filter and wash the filtered solid with deionized water several times, and dry to obtain the CN carrier.

[0013] The above method adopts a direct mixing method to directly mix 2-methylimidazole with a cobalt source and then calcine to obtain Co@CN, and then undergo an acid washing step to prepare a CN material with a rich pore structure. This is the first time that a carrier is prepared without the use of an organic solvent. In the process of preparing the carrier, there is no need to separately synthesize a specific ZIFs material. The entire preparation process has the advantages of low raw material cost, high raw material utilization, simple preparation process, green environmental protection, and high carrier yield, providing a new idea for the batch preparation of ZIFs-derived CN materials. After the carrier is prepared by this method, Pd is further loaded by impregnation to obtain an efficient phenol liquid-phase hydrogenation catalyst. It has been verified that the catalyst activity and stability can meet industrial requirements.

[0014] Preferably, in step 1, the cobalt source is any one of cobalt acetate tetrahydrate, cobalt chloride hexahydrate, and cobalt nitrate hexahydrate, and the molar ratio of 2-methylimidazole:cobalt source is (1-12):1.

[0015] Preferably, the calcination in step 2 is carried out in a tubular furnace, the heating rate of the tubular furnace is 1-10°C / min, the calcination temperature is 550-1000°C, and the calcination time is 100-150min;

[0016] Preferably, in step 3, the mass ratio of Co@CN: deionized water: concentrated nitric acid (66%) is 1:(20-30):(20-30), the stirring temperature is 30-90°C, the stirring time is 30-90min, and the stirring rate is 50-300 rpm.

[0017] Preferably, in step 4, the washing times are 2-5 times, the drying temperature is 40-100° C., and the drying time is 3-5 hours.

[0018] The present invention directly mixes 2-methylimidazole with a cobalt source and then calcines the mixture. During the heating process, the cobalt source melts and coats the 2-methylimidazole and reacts to form a transition state ZIF and a small amount of ZIF. During the calcination process, part of the 2-methylimidazole volatilizes to form an alkaline gas that produces an etching effect; Co nanoparticles aggregate and grow; the irregular block structure of the transition state ZIF is retained, and the stacking of the block structure will form a pore structure. The CN material obtained by the present invention has a large specific surface area, rich pore structure, a high proportion of mesopores, and rich defect sites. The large specific surface area and rich defect sites of the carrier are conducive to the anchoring and dispersion of active sites; the rich pore structure and high mesopore ratio are conducive to reducing diffusion resistance, promoting mass transfer, and improving the utilization rate of active sites. This preparation method does not require the synthesis of specific ZIFs and does not require the use of organic solvents. It has the advantages of a simple preparation process, high utilization rate of organic ligands, low raw material costs, high catalyst yield, and environmental friendliness. Different cobalt sources and raw material molar ratios significantly influence catalyst performance and yield. The highest CN support yield was achieved when cobalt acetate tetrahydrate was used as the cobalt source and the ratio of 2-methylimidazole to cobalt acetate tetrahydrate was 4:1. The support's performance met the requirements for catalyst preparation and hydrogenation catalysis, making it suitable for industrial production and use. In a phenol-cyclohexane system, the prepared catalyst achieved a phenol conversion of 98.6% and a cyclohexanone selectivity of 94.1% at a temperature of 100°C, a pressure of 0.1 MPa, a reaction time of 30 minutes, and a catalyst content of 0.03 g.

[0019] Compared with the prior art, the advantages and positive effects of the present invention are:

[0020] 1. The rich pore structure of the CN material obtained in the present invention is conducive to reducing diffusion resistance, improving mass transfer, and promoting contact between reaction substrates and active sites, making it an ideal carrier.

[0021] 2. Compared with the traditional preparation method of ZIFs-derived CN materials, this method has the advantages of simple process, environmental friendliness, low raw material cost and high catalyst yield.

[0022] 3. The Pd@CN catalyst prepared by Pd loading was used in the phenol hydrogenation to cyclohexanone system and showed excellent catalytic activity comparable to that of ZIFs-derived catalysts, providing new ideas for the batch preparation of ZIFs-derived CN and its further application in the catalytic field. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a comparison of the yields of CN-67 and CN.

[0024] Figure 2 shows the SEM and XRD patterns of CN.

[0025] Figure 3 shows the N2 adsorption and desorption and pore size distribution of CN.

[0026] Figure 4 shows the effects of different cobalt sources on catalyst performance and product quality.

[0027] Figure 5 shows the effects of different molar ratios of cobalt and 2-methylimidazole on catalyst performance and product quality.

[0028] Figure 6 shows the change of Pd@CN reaction with temperature.

[0029] Figure 7 shows the change of Pd@CN reaction over time. DETAILED DESCRIPTION

[0030] In order to more clearly understand the above-mentioned objects, features and advantages of the present invention, the present invention is further described below in conjunction with specific embodiments. It should be noted that, in the absence of conflict, the embodiments of the present application and the features therein can be combined with each other.

[0031] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways than those described herein. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0032] Example 1

[0033] (1) Preparation of Co@CN materials

[0034] First, 4.2 g of 2-methylimidazole was weighed and placed in a 15 mL crucible. Then, 1.8 g of cobalt acetate tetrahydrate was added. The crucible was placed in a tube furnace and calcined under an Ar atmosphere at a heating rate of 5 °C / min. After heating to 800 °C and holding for 120 min, the material was naturally cooled to room temperature to obtain the Co@CN material.

[0035] (2) Preparation of CN vector

[0036] The prepared Co@CN material was placed in a round-bottom flask. 25 times the mass of deionized water and 25 times the mass of concentrated nitric acid solution (66% by mass) were added, respectively. The mixture was stirred in a 60°C water bath at 200 rpm for 1 hour. After stirring, the mixture was washed three times with deionized water and dried in an oven at 70°C for 4 hours to obtain the CN carrier. Weighing yielded 0.65 g of the material.

[0037] (3) Preparation of Pd@CN catalyst

[0038] First, weigh 0.01g Pd(OAc)2 and place it in a round-bottom flask, add 25mL acetone solution to dissolve it, add 0.2g CN carrier after dissolution, stir at 25℃ for 12h, and the stirring rate is 100 rpm. After the stirring is completed, the solvent acetone is removed by rotary evaporation at 70℃ for 30min, and the catalyst is placed in an oven at 70℃ and dried for 4h to obtain the Pd@CN catalyst.

[0039] The Pd@CN catalyst was used in an experiment to hydrogenate phenol to cyclohexanone. The reaction temperature was 100°C, the pressure was 0.1 MPa, the stirring rate was 100 rpm, the solvent was cyclohexane, the phenol concentration was 1 wt%, and the Pd@CN catalyst dosage was 6 g / L. After 30 minutes of reaction, the phenol conversion rate reached 98.6%, with a selectivity of 94.1%.

[0040] Anything not specifically stated in the subsequent description is consistent with that in Example 1, or is a routine operation.

[0041] Example 2

[0042] (1) Preparation of Co@CN

[0043] First, 1.54 g of 2-methylimidazole was weighed and placed in a 15 mL crucible. Then, 4.46 g of cobalt chloride hexahydrate was added. The crucible was placed in a tube furnace and calcined under an Ar atmosphere at a heating rate of 1 °C / min. After heating to 550 °C and holding for 100 min, the Co@CN material was obtained after natural cooling to room temperature.

[0044] (2) Preparation of CN

[0045] The prepared Co@CN was placed in a round-bottom flask. Twenty times the mass of deionized water and 20 times the mass of concentrated nitric acid were added, respectively. The mixture was stirred in a 30°C water bath at 50 rpm for 90 minutes. After stirring, the mixture was washed twice with deionized water and dried in an oven at 40°C for 5 hours to obtain the CN material. The yield of the prepared carrier was 0.34 g.

[0046] (3) Preparation of Pd@CN catalyst

[0047] First, weigh 0.01g Pd(OAc)2 and place it in a round-bottom flask, add 20mL acetone solution to dissolve it, add 0.2g CN after dissolution, stir at 10℃ for 15h, and stir at a rate of 50 rpm. After stirring, remove the solvent acetone by rotary evaporation at 50℃ for 45min, and place it in an oven at 40℃ and dry it for 5h to obtain Pd@CN catalyst material.

[0048] The Pd@CN catalyst was used in an experiment to hydrogenate phenol to cyclohexanone. The reaction temperature was 100°C, the pressure was 0.1 MPa, the stirring rate was 100 rpm, the solvent was cyclohexane, the phenol concentration was 1 wt%, and the Pd@CN catalyst dosage was 6 g / L. After 30 minutes of reaction, the phenol conversion reached 96.11%, with a selectivity of 94.0%.

[0049] Example 3

[0050] (1) Preparation of Co@CN

[0051] First, 4.64 g of 2-methylimidazole was weighed and placed in a 15 mL crucible. Then, 1.36 g of cobalt nitrate hexahydrate was added. The crucible was placed in a tube furnace and calcined under an Ar atmosphere at a heating rate of 10°C / min. After heating to 1000°C and holding for 150 minutes, the Co@CN material was obtained after natural cooling to room temperature.

[0052] (2) Preparation of CN

[0053] The prepared Co@CN was placed in a round-bottom flask, followed by the addition of 30 times the mass of deionized water and 30 times the mass of concentrated nitric acid. The mixture was stirred in a 90°C water bath at 300 rpm for 30 minutes. After stirring, the mixture was washed five times with deionized water and dried in an oven at 100°C for 3 hours to obtain the CN material. The yield of the prepared carrier was 0.45 g.

[0054] (3) Preparation of Pd@CN catalyst

[0055] First, 0.01 g of Pd(OAc)2 was weighed and placed in a round-bottom flask, 30 mL of acetone solution was added to dissolve it, and 0.2 g of CN was added after dissolution. The mixture was stirred at 40 °C for 9 h at a stirring rate of 300 rpm. After the stirring was completed, the solvent acetone was removed by rotary evaporation at 90 °C for 15 min, and the mixture was placed in an oven and dried at 100 °C for 3 h to obtain the Pd@CN catalyst material.

[0056] The Pd@CN catalyst was used in an experiment to hydrogenate phenol to cyclohexanone. The reaction temperature was 100°C, the pressure was 0.1 MPa, the stirring rate was 100 rpm, the solvent was cyclohexane, the phenol concentration was 1 wt%, and the Pd@CN catalyst dosage was 6 g / L. After 30 minutes of reaction, the phenol conversion reached 91.1% and the selectivity was 95.3%.

[0057] Some comparative examples of carrier preparation are provided below.

[0058] 1. Comparison of yield and catalytic performance between direct mixing method and traditional solvent method.

[0059] For the convenience of description, the carrier prepared by the direct mixing method is denoted as CN and the carrier prepared by the traditional solvent method is denoted as CN-67.

[0060] The direct mixing method uses the preparation method described in the Examples, which will not be further described here. The traditional solvent method preparation process is as follows: First, prepare 50 mL of a 0.8 mol / L 2-methylimidazole methanol solution and 50 mL of a 0.1 mol / L cobalt nitrate hexahydrate methanol solution. The 2-methylimidazole solution is placed in a 250 mL conical flask and the cobalt nitrate hexahydrate solution is added while stirring at 100 rpm. The mixture is stirred for 5 minutes and allowed to stand for 24 hours. The mixture is centrifuged, washed twice with methanol, and finally dried in an oven at 80°C for 6 hours to obtain ZIF-67. 0.5 g of ZIF-67 is placed in a tube furnace and calcined at 800°C for 2 hours under an Ar atmosphere. The temperature is raised from room temperature to the target temperature at a rate of 1°C / min. The resulting Co@CN is then acid-washed with a 30% nitric acid solution at 60°C and 100 rpm for 3 hours, washed four times with deionized water, and dried at 80°C for 12 hours to obtain CN-67.

[0061] The same 6g cobalt nitrate and 2-methylimidazole mixture, the ZIF-derived CN produced by the direct mixing method of Example 3 is 0.45g, and the ZIF-derived CN produced by the traditional method is 0.21g. Obviously, the preparation process using the direct mixing method is simpler, the carrier yield is higher, it is green and environmentally friendly, and the raw material cost is lower. This is because the traditional synthesis method only retains ZIF crystals, and a large amount of uncoordinated raw materials in the reaction solution are discarded and wasted. The organic solvent is removed by a centrifugation step, and the operation steps are complicated and can cause product loss. However, using the direct mixing method, the raw materials react during the temperature rise process to generate a small amount of ZIF and transition state ZIF, which are then pyrolyzed to form a CN material with rich pore structure. There is no need to synthesize ZIF, no organic solvent is required, and the waste of raw materials is avoided. The preparation process is simple and the process is green and environmentally friendly.

[0062] A Pd@CN catalyst was prepared using CN-67 as a support. First, 0.01 g of Pd(OAc)2 was weighed and placed in a round-bottom flask. 20 mL of acetone was added to dissolve it. After dissolution, 0.2 g of CN-67 was added. The mixture was stirred at 25°C for 12 hours. After stirring, the acetone solvent was removed by rotary evaporation at 60°C for 30 minutes. The catalyst was then dried in an oven at 50°C for 4 hours to obtain the Pd@CN catalyst.

[0063] The Pd@CN catalyst was used in the experiment of hydrogenating phenol to cyclohexanone. Under the reaction conditions of Example 1-3, the phenol conversion rate was 92.5% and the selectivity was 94.8%, and the performance was similar to that of Example 1-3.

[0064] 2. Impact of different cobalt sources

[0065] As shown in FIG4 , cobalt acetate tetrahydrate, cobalt chloride hexahydrate, and cobalt nitrate hexahydrate were used as cobalt sources, respectively. Under the premise that other preparation conditions were consistent with those in Example 1, the prepared products were shown in FIG4 .

[0066] For the convenience of comparison, the prepared support was further prepared into a catalyst, and the catalyst performance was investigated under the same conditions as in Example 1. As shown in Figure 4, different cobalt sources lead to different CN yields and Pd@CN performances. This is due to the charge, ionic radius and relative affinity of the anions of different cobalt sources to Co. 2+ Different interaction forces lead to different micromorphologies and physicochemical properties of the prepared supports. Among them, when cobalt acetate is used as the cobalt source, the CN yield is the highest when the corresponding catalyst has high performance.

[0067] 3. Influence of molar ratios of different substances

[0068] As shown in Figure 5, while the total mass of 2-methylimidazole and cobalt acetate tetrahydrate remains constant, the support / catalyst yield initially increases and then decreases with varying molar ratios of 2-methylimidazole:cobalt acetate tetrahydrate. Different molar ratios affect the reaction degree of the raw materials, thereby affecting CN yield and Pd@CN performance. When the relative 2-methylimidazole content is high, it prevents sufficient contact with the cobalt source, forming a transitional ZIF. The CN pore structure derived from the transitional ZIF is more developed, resulting in better performance. When the relative 2-methylimidazole content is low, the raw materials react fully, forming a partial ZIF, but the CN pore structure derived from the ZIF is reduced, leading to lower performance. Excessive 2-methylimidazole volatilization increases costs. When the 2-methylimidazole:cobalt acetate tetrahydrate ratio is 4:1, Pd@CN exhibits high catalytic activity and the highest CN support yield.

[0069] Explanation of other figures: Figure 1 is a yield diagram of CN and CN-67. It can be seen from the figure that the yield of CN prepared by direct mixing method is 0.45g, and the yield of CN-67 prepared by traditional method is 0.21g. The yield of CN prepared by direct mixing method is higher. Figure 2 is the SEM and XRD diagram of CN. It can be seen from the XRD diagram that the materials prepared with different molar ratios are all CN materials containing Co nanoparticles. It can be seen from the SEM diagram that CN all present irregular block structures, with carbon nanotubes on the surface and developed pore structures. Figure 3 is a N2 adsorption and desorption curve diagram and a pore size distribution diagram. It can be seen from the figure that CN prepared with different molar ratios all have rich pore structures. Figure 4 shows the effect of different cobalt sources on catalyst performance. It can be seen from the figure that different cobalt sources will affect the yield and performance of the catalyst. Figure 5 shows the effect of different molar ratios on catalyst performance. It can be seen from the figure that the molar ratio has a significant effect on the yield and performance of the catalyst. Figure 6 shows the effect of reaction temperature on reaction performance. As can be seen, with increasing reaction temperature, phenol conversion initially increases and then remains constant, while cyclohexanone selectivity initially remains constant and then decreases. At a reaction temperature of 100°C, both phenol conversion and cyclohexanone selectivity are high. Figure 7 shows the effect of reaction time on reaction performance. As can be seen, longer reaction times increase conversion, reaching 99% phenol conversion. Further increases in reaction time result in no change in phenol conversion, while cyclohexanone selectivity decreases continuously with increasing reaction time. At a reaction time of 30 minutes, both phenol conversion and selectivity are high, fully meeting the catalyst requirements for industrial production.

[0070] In summary, the preparation method of the ZIF-derived CN material provided by the present invention has the advantages of simple process, short preparation cycle, high utilization rate of organic ligands, high catalyst yield, and environmental friendliness. By loading Pd, a Pd@CN catalyst is prepared, and the Pd@CN catalyst is applied to the phenol hydrogenation to cyclohexanone system with significant catalytic effect. This is because Pd@CN has a large specific surface area, rich pore structure, high mesoporosity, and rich defect sites. The large specific surface area and rich defect sites are conducive to the anchoring and dispersion of Pd, thereby improving the utilization rate of Pd atoms; the rich pore structure and high mesoporosity are conducive to reducing diffusion resistance, promoting mass transfer and improving the utilization rate of active sites, thereby improving the activity of the catalyst. This method provides a new idea for the batch preparation of ZIF-derived CN materials and the further application of ZIF-derived CN in the field of catalysis.

[0071] The above description is merely a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any person skilled in the art may utilize the technical contents disclosed above to change or modify them into equivalent embodiments with equivalent changes for application in other fields. However, any simple modification, equivalent change, and modification of the above embodiments made in accordance with the technical essence of the present invention without departing from the technical solution of the present invention shall still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A simple method for preparing a hydrogenation catalyst carrier, characterized in that: The 2-methylimidazole is mixed with a cobalt source, calcined, and then acid-washed to prepare the product.

2. Use of the carrier prepared by the method of claim 1 in a hydrogenation catalyst.

3. The method for preparing the hydrogenation catalyst carrier according to claim 1, characterized in that: Here are the steps: Step 1: mixing 2-methylimidazole with a cobalt source to obtain a mixture; Step 2: The mixture in step 1 is calcined under Ar atmosphere to obtain Co@CN; Step 3: Add deionized water and concentrated nitric acid solution to Co@CN and stir evenly; Step 4: Filter and wash the filtered solid with deionized water for several times, and dry to obtain the CN carrier.

4. The method for preparing a hydrogenation catalyst carrier according to claim 3, characterized in that: In step 1, the cobalt source is any one of cobalt acetate tetrahydrate, cobalt chloride hexahydrate, and cobalt nitrate hexahydrate, and the molar ratio of 2-methylimidazole:cobalt source is (1-12):

1.

5. The method for preparing a hydrogenation catalyst carrier according to claim 3, characterized in that: In step 2, the calcination is carried out in a tubular furnace, the heating rate of the tubular furnace is 1-10°C / min, the calcination temperature is 550-1000°C, and the constant temperature time is 100-150min.

6. The method for preparing a catalyst carrier for hydrogenation according to claim 3, characterized in that: In step 3, the mass fraction of the concentrated nitric acid solution is 66%, the mass ratio of Co@CN: deionized water: concentrated nitric acid solution is 1:(20-30):(20-30), the stirring temperature is 30-90°C, the stirring rate is 50-300 rpm, and the stirring time is 30-90 min.

7. The method for preparing a catalyst carrier for hydrogenation according to claim 3, characterized in that: In step 4, the washing times are 2-5 times, the drying temperature is 40-100° C., and the drying time is 3-5 hours.

8. A catalyst for preparing cyclohexanone by hydrogenating phenol, characterized in that: The carrier is prepared by the method of any one of claims 3 to 7.

9. The method for preparing the catalyst according to claim 8, characterized in that: Pd(OAc)2 is dispersed in acetone to obtain solution A; the support obtained by any one of claims 3 to 7 is added to solution A and stirred and impregnated; the acetone is then removed by rotary evaporation; and the Pd@CN catalyst is obtained by drying.

10. The method for preparing the catalyst according to claim 9, characterized in that: The mass ratio of Pd(OAc)2: carrier: acetone is 1:20:(2000-3000), the stirring temperature is 10-40°C, the stirring time is 9-15h, the stirring rate is 50-300 rpm, the rotary evaporation temperature is 50-90°C, the rotary evaporation time is 15-45min, the drying temperature is 40-100°C, and the drying time is 3-5h.

Citation Information

Patent Citations

  • Cobalt-based catalyst for generating ester by alcohol oxidation, and preparation method and application of cobalt-based catalyst

    CN104069883A

  • Preparation method of supported palladium catalyst

    CN106423251A

  • Preparation method of N-doped porous carbon coated nano-particles of Co-Ir core-shell structure and application of N-doped porous carbon coated nano-particles of Co-Ir core-shell structure to catalytic water splitting

    CN108048866A

  • Carbon quantum dots-ZIF-67 adsorption-photocatalytic agent and preparation method thereof

    CN108686705A

  • Magnetic micropore-rich carbon-based cobalt catalyst based on space confinement effect as well as preparation method and application of magnetic micropore-rich carbon-based cobalt catalyst

    CN114192146A

Cited By

  • Mesoporous cobalt-zinc bimetallic monatomic catalyst as well as preparation method and application thereof

    CN119657192A

  • Synthetic method of avibactam sodium