Preparation method for polyimide interlayer toughened fiber composite material, fiber preform, and composite material panel

The polyimide spinning liquid is prepared by electrospinning and sprayed on the surface of fiber cloth, which solves the problem of difficult control of polyimide agglomeration and uniformity in fiber composite materials, and improves the interlaminar fracture toughness and Shear strength, achieving better toughening effect and application potential.

WO2024212474A1PCT designated stage expired Publication Date: 2024-10-17NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI

Patent Information

Application Number
PCT/CN2023/126851
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2023-10-26
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Polyimide particles are prone to agglomeration in fiber composite materials, resulting in a decrease in interlayer shear strength. Existing interlayer particle toughening methods are difficult to ensure the uniformity and controllability of powdering, affecting the repeatability and industrialization of composite materials. application.

Method used

By preparing polyimide spinning liquid and spraying it on the surface of fiber cloth using electrospinning method, the concentration of spinning liquid is adjusted to construct different micro-nano structure morphologies, such as fiber, spherical and bead-like, to ensure the polyimide's Dispersion uniformity and interlayer toughening effect.

Benefits of technology

It effectively avoids the agglomeration of polyimide, improves the interlaminar fracture toughness and shear strength of composite materials, enhances the layered impedance capability of composite materials, and improves the repeatability of experiments and industrial application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023126851_17102024_PF_FP_ABST
    Figure CN2023126851_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method for a polyimide interlayer toughened fiber composite material. The method comprises the following steps: A) preparing a polyimide spinning solution; and B) using an electrostatic spinning method to spray the polyimide spinning solution onto the surface of a fiber cloth or of a prepreg, obtaining a polyimide interlayer toughened fiber composite material; the polyimide spinning solution has different concentrations, and the polyimide interlayer toughened fiber composite material has different polyimide layer micro / nano structural morphology. The present application further provides a fiber preform and a composite material panel. The preparation method of the polyimide interlayer toughened fiber composite material provided in the present application allows for adjusting the concentration of the electrospinning solution to construct different micro / nano structural morphologies, and different structural morphologies trigger different toughening mechanisms, further producing different interlayer toughening effects. The method provided by the present invention does not affect the original forming process of a composite material, the processing method is flexible, and the interlayer toughening effect is remarkable, with immense application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Preparation method of polyimide interlayer toughened fiber composite material, fiber preform and composite material plate Technical Field

[0001] The invention relates to the technical field of fiber composite materials, in particular to a preparation method of a polyimide interlayer toughened fiber composite material, a fiber preform and a composite material plate. Background Art

[0002] Fiber-reinforced plastic (FRP) composites, due to their excellent mechanical properties, are widely used in aircraft, automobiles, sporting goods, building structure reinforcement, and offshore platforms. However, due to the inherent brittleness and layered structure of the resin, their load-bearing capacity through the thickness direction is low, making them prone to delamination damage.

[0003] Interlaminar toughening technology is an effective way to improve the toughness and delamination resistance of FRP composites. This method involves inserting toughening materials into the interlaminar regions of the composite material where delamination is likely to occur, thereby increasing the delamination resistance of the composite material. Compared to the first-generation single-phase matrix composites and the second-generation multi-phase matrix composites, interlaminar toughened composites are also called third-generation composites. Interlaminar toughening methods can be divided into particle toughening, film toughening, and fiber toughening according to the structural morphology of the toughening material. Although continuous films can improve the interlaminar fracture toughness of composite materials, the film thickness is difficult to control and the process performance is poor, making it unsuitable for industrial application. Interlaminar particle toughening and fiber toughening can overcome the above shortcomings and have a higher toughening amplitude, so they have important research and application value.

[0004] Polyimide (PI) is widely used in fiber-reinforced resin-based composites due to its excellent performance. Some researchers have used thermoplastic polyimide (TPI) particles to perform interlaminar toughening modification on phthalonitrile resin composites and found that the introduction of PI particles significantly improves the interlaminar fracture toughness of the composites. However, as the mass fraction of PI increases further, particle agglomeration defects will occur, resulting in a decrease in the interlaminar shear strength of the composites. In addition, the method of achieving interlaminar particle toughening by sprinkling powder into the middle layer does not guarantee the uniformity of the powder sprinkling, and the process is difficult to control, resulting in poor experimental repeatability. Moreover, it is usually difficult to control the size of commercially available PI particles. Therefore, it is of great significance to control the morphology of polyimide as an interlaminar toughening material.

[0005] Summary of the Invention

[0006] The technical problem solved by the present invention is to provide a method for preparing a polyimide interlayer toughening fiber composite material. The preparation method provided in this application can improve the dispersion uniformity of polyimide, thereby exerting the interlayer toughening effect.

[0007] In view of this, the present application provides a method for preparing a polyimide interlayer toughened fiber composite material, comprising the following steps:

[0008] A) preparing a polyimide spinning solution;

[0009] B) spraying the polyimide spinning solution onto the surface of a fiber cloth or a prepreg by an electrostatic spinning method to obtain a polyimide interlayer toughened fiber composite material;

[0010] The concentration of the polyimide spinning solution is different, and the micro-nano structure morphology of the polyimide layer of the polyimide interlayer toughening fiber composite material is different.

[0011] Preferably, the micro-nanostructure morphology of the polyimide layer is one or more of fibrous, spherical, beaded and tubular.

[0012] Preferably, the concentration of the polyimide spinning solution is 10-40 wt%.

[0013] Preferably, the solvent of the polyimide in the polyimide spinning solution is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, m-cresol, chloroform and dichloromethane.

[0014] Preferably, the fiber cloth is selected from one or more of carbon fiber, glass fiber, metal fiber, basalt fiber, aramid fiber, carbon nanotube fiber, graphene fiber and plant fiber.

[0015] Preferably, the electrospinning voltage of the electrospinning method is 10-20 kV, the spinning speed is 1-2 ml / h, the receiving distance is 15-20 cm, the temperature is 20-30° C., the humidity is 35-45%, and the time is 24-40 min.

[0016] The present application also provides a fiber preform, comprising multiple layers of stacked fiber cloths and a polyimide interlayer toughening fiber composite material arranged between the fiber cloths, wherein the polyimide interlayer toughening fiber composite material is a polyimide interlayer toughening fiber composite material prepared by the preparation method.

[0017] The present application also provides a composite material plate, comprising a fiber preform and a resin matrix composited in the fiber preform, wherein the fiber preform is the fiber preform described above.

[0018] Preferably, the resin matrix is ​​selected from one or more of epoxy resin, phenolic resin, vinyl resin, bismaleimide resin, polyimide resin and thermoplastic resin.

[0019] The present application also provides a method for preparing the composite material plate, comprising:

[0020] Infusing the resin-based slurry into the fiber preform and then curing it to obtain a composite material board;

[0021] The fiber preform is the fiber preform described above.

[0022] The present application provides a method for preparing a polyimide interlayer toughened fiber composite material, which first prepares a polyimide spinning solution, and then sprays the polyimide spinning solution onto the surface of a fiber cloth or a prepreg by an electrospinning method to obtain a polyimide interlayer toughened fiber composite material; the preparation method provided by the present application prepares a polyimide interlayer toughened fiber composite material by introducing an electrospinning method, thereby ensuring the uniformity of polyimide dispersion and effectively avoiding the occurrence of agglomeration; at the same time, by adjusting the concentration of the electrospinning solution, different micro-nanostructure morphologies such as fiber-like and beaded-like can be constructed, thereby exerting different interlayer toughening effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG1 is a schematic diagram of a polyimide interlayer toughened composite material plate of the present invention;

[0024] FIG2 is a schematic diagram of the layup of a preform provided in Example 1 of the present invention;

[0025] Figure 3 shows the microscopic morphology of PI at different electrospinning solution concentrations;

[0026] FIG4 is a graph showing the double cantilever beam test results of the composite material plates prepared in Example 1 of the present invention and Comparative Example 1;

[0027] FIG5 is an R curve (a curve showing crack propagation resistance versus crack propagation) of the composite material plates prepared in Example 1 of the present invention and Comparative Example 1;

[0028] FIG6 is a graph showing the end delamination flexure (ENF) test results of the composite panels prepared in Example 1 of the present invention and Comparative Example 1;

[0029] FIG7 is a SEM image of the fracture surface of the composite material plate prepared in Comparative Example 1 of the present invention;

[0030] FIG8 is a SEM image of the fracture surface of the composite material plate prepared in Example 1 of the present invention;

[0031] FIG9 is a SEM image of the fracture surface of the composite material plate prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0032] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0033] In view of the problem of agglomeration of polyimide particles in the prior art, the present application provides a method for preparing a polyimide interlayer toughened fiber composite material. By adjusting the concentration of the polyimide spinning solution, different micro-nanostructure morphologies (such as fibers, spheres, and beads of fibers and microspheres) are constructed. Different structural morphologies trigger different toughening mechanisms, thereby producing different interlayer toughening effects. Specifically, an embodiment of the present invention discloses a method for preparing a polyimide interlayer toughened fiber composite material, comprising the following steps:

[0034] A) preparing a polyimide spinning solution;

[0035] B) spraying the polyimide spinning solution onto the surface of a fiber cloth or a prepreg by an electrostatic spinning method to obtain a polyimide interlayer toughened fiber composite material;

[0036] The concentration of the polyimide spinning solution is different, and the micro-nano structure morphology of the polyimide layer of the polyimide interlayer toughening fiber composite material is different.

[0037] In the preparation method of a polyimide interlayer toughened fiber composite material, the present application first prepares a polyimide spinning solution, specifically, placing a soluble polyimide in an agate mortar, gently grinding it, and then completely dissolving it in a solvent; the preparation process of the soluble polyimide includes but is not limited to the introduction of flexible groups, large side groups, non-coplanar structures, fluorine-containing groups, asymmetric structures, copolymerization, and hyperbranched polyimides on the main chain, that is, the present application has no particular restrictions on the soluble polyimide. The solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, m-cresol, chloroform, and dichloromethane. The dissolution method includes but is not limited to stirring, ultrasound, or heating.

[0038] In the present application, the concentration of the polyimide spinning solution is 10-40 wt %. Specifically, the concentration of the polyimide spinning solution is 12-30 wt %.

[0039] The present application then sprays the polyimide spinning solution onto the surface of a fiber cloth or prepreg by electrospinning to obtain a polyimide interlayer toughened fiber composite material. In the present application, the micro-nanostructure morphology of the polyimide layer varies depending on the concentration of the electrospinning solution, and can be one or more of fibrous, spherical, beaded, and tubular. More specifically, when the concentration of the polyimide spinning solution is 12-20 wt%, the micro-nanostructure morphology of the polyimide layer is spherical, when the concentration of the polyimide spinning solution is 22-26 wt%, the micro-nanostructure morphology of the polyimide layer is tubular or beaded, and when the concentration of the polyimide spinning solution is 30 wt%, the micro-nanostructure of the polyimide layer is fibrous. The fiber cloth is selected from one or more of carbon fiber, glass fiber, metal fiber, basalt fiber, aramid fiber, carbon nanotube fiber, graphene fiber, and plant fiber. In the above process, the electrospinning method is a method well known to those skilled in the art, and this application does not impose any particular restrictions on its specific implementation. The electrospinning voltage of the electrospinning method is 10-20 kV, the spinning speed is 1-2 ml / h, the receiving distance is 15-20 cm, the temperature is 20-30 ° C, and the humidity is 35-45%; specifically, the electrospinning voltage of the electrospinning method is 15 kV, the spinning speed is 1 ml / h, the receiving distance is 15 cm, the temperature is 24 ° C, the humidity is 40%, and the time is 40 min.

[0040] The present application also provides a fiber preform comprising multiple layers of laminated fiber cloth and a polyimide interlayer toughening fiber composite material disposed between the fiber cloths. The polyimide interlayer toughening fiber composite material is prepared by the above-described preparation method. In the fiber preform provided herein, the polyimide interlayer toughening fiber composite material is disposed between the multiple layers of fiber cloth, and the specific location of the polyimide interlayer toughening fiber composite material is not particularly limited in this application. The fiber cloth is not particularly limited in this application and is any fiber cloth familiar to those skilled in the art.

[0041] The present application also provides a composite material board, which includes a fiber preform and a resin matrix composited in the fiber preform, wherein the fiber preform is the fiber preform described in the above embodiment.

[0042] Furthermore, the present application also provides a method for preparing a composite material plate, comprising:

[0043] Infusing the resin-based slurry into the fiber preform and then curing it to obtain a composite material board;

[0044] The fiber preform is the fiber preform described in the above solution.

[0045] The resin in the resin-based slurry is selected from one or more of epoxy resin, phenolic resin, vinyl resin, bismaleimide resin, polyimide resin and thermoplastic resin. The pouring method can be carried out in a manner well known to those skilled in the art, and there is no particular limitation in this application. A curing agent may also be added to the resin-based slurry as needed. The curing temperature is 50-100°C, the pressure is 1-5 MPa, and the temperature is 100-150°C.

[0046] In order to further understand the present invention, the preparation method of the polyimide interlayer toughened fiber composite material, the fiber preform and the composite material plate provided by the present invention are described in detail below in combination with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0047] Example 1

[0048] This embodiment is a preparation process of a polyimide interlayer toughening fiber composite material prepared by electrospinning, which is specifically as follows:

[0049] S1. Preparation of polyimide electrospinning solution

[0050] 3.6 g of soluble polyimide (ULTEM 1000) was weighed and gently ground in an agate mortar. 16.4 g of N-N dimethylformamide (DMF) was then weighed and heated at 80°C in silicone oil for 3 h to completely dissolve the polyimide into a transparent brown-yellow liquid. No significant changes occurred after 3 h of standing, resulting in an 18 wt% polyimide spinning solution.

[0051] S2. Spray the polyimide spinning solution onto the surface of the carbon cloth through an electrospinning device

[0052] The electrospinning solution obtained in step S1 was transferred to the syringe of the electrospinning equipment and sprayed on the surface of the carbon cloth. The electrospinning voltage was 15 kV, the spinning speed was 1 ml / h, the receiving distance was 15 cm, the temperature was 24 ° C, the humidity was 40%, and the spinning time was 40 min to obtain a microspherical surface layer. Finally, it was placed in a vacuum oven and dried for 1 hour;

[0053] S3. Preparation of fiber preform

[0054] Take carbon fiber bidirectional cloth (Hexcel G0926, 5H Satin, density 370g / m 3 ), cut into 25×25cm cloth pieces, and then lay the fiber preform by hand lamination; specifically, lay 16 layers of carbon cloth at [0°] 16 The stacking arrangement is as shown in FIG2 , wherein the eighth layer is the carbon cloth sprayed with polyimide obtained in step S2 , and a 45 mm long polytetrafluoroethylene film (30 μm thick) is laid in as a pre-crack;

[0055] Note: In the above preparation process, the PTFE film is only laid for the preparation of double cantilever beam specimens for subsequent performance testing. In the actual production process of composite materials, the PTFE film is not laid, that is, the actual composite material product does not contain PTFE film;

[0056] S4. Preparation of composite material board

[0057] Composite panels were prepared using the VARTM method. Specifically, a double-layered flow net was applied to the laid fiber preform, with a release sheet separating the flow net and the fiber preform, and finally sealed with a vacuum bag.

[0058] Prepare epoxy resin-based slurry by pouring 300g of bisphenol F epoxy resin Epon862 into a beaker, then adding 105.6g of curing agent polyetheramine D-230, stirring thoroughly with a glass rod, and then degassing in a vacuum oven at 25°C for 10 minutes to obtain about 405.6g of resin-based slurry;

[0059] The resin-based slurry is evenly introduced into the fiber preform through the negative pressure of a vacuum pump. After the resin-based slurry is completely infused into the carbon fiber cloth, the VARTM platform is moved into a flat-plate vulcanizer. It is first cured at 80°C and 3.6MPa pressure for 2 hours, and then at 120°C for 2 hours. After cooling and demolding, the composite material board is obtained.

[0060] Comparative Example 1

[0061] In this comparative example, a Spanish carbon cloth which is not sprayed with polyimide is inserted into the middle layer, and the remaining steps and parameters are the same as those in Example 1.

[0062] Comparative testing

[0063] The fiber composite materials provided in Example 1 and Comparative Example 1 were subjected to the following tests:

[0064] 1) With reference to ASTM D5528, an evaluation of the mode I interlaminar fracture toughness was performed, and the results are shown in Figures 4 and 5. Figure 4 is a double cantilever beam test result diagram of the composite panels prepared in Example 1 and Comparative Example 1, and Figure 5 is an R curve (crack propagation resistance versus crack propagation curve) diagram of the composite panels prepared in Example 1 and Comparative Example 1. As can be seen from Figures 4 and 5, compared with the reference sample in Comparative Example 1, the mode I interlaminar fracture toughness of the composite panel in Example 1 increased from 1.55 kJ / m 2 Increased to 1.75kJ / m 2 .

[0065] 2) The Mode II interlaminar fracture toughness was evaluated according to ASTM D7905. FIG6 shows the end delamination flexure (ENF) test results of the composite plates prepared in Example 1 and Comparative Example 1. The calculated Mode II interlaminar fracture toughness of Example 1 is 0.61 kJ / m 2 , compared with 0.51kJ / m in Comparative Example 1 2 , an increase of 19%.

[0066] Figures 7 and 8 are SEM photographs of the fracture surfaces of the composite materials prepared in Example 1 and Comparative Example 1, respectively. As can be seen from the figures, the fracture surface of Comparative Example 1 is relatively smooth, while the fracture surface of Example 1 has many polyimide spheres embedded in the resin, and there is shear failure of the polyimide spheres, as well as the microscopic morphology of the polyimide spheres being debonded as a whole to form voids, which makes the fracture surface of the composite material rough.

[0067] Example 2

[0068] S1. Preparation of polyimide electrospinning solution

[0069] 3.6 g of soluble polyimide (ULTEM 1000) was weighed and then placed in an agate mortar and gently ground. 8.4 g of N-N dimethylformamide (DMF) was then weighed and heated at 80°C in silicone oil for 3 h to completely dissolve the polyimide into a transparent brown-yellow liquid. No significant changes were observed after 3 h of standing, resulting in a 30% mass fraction polyimide spinning solution.

[0070] S2. Spray the polyimide spinning solution onto the surface of the carbon cloth through an electrospinning device

[0071] The electrospinning solution obtained in step S1 was transferred to the syringe of the electrospinning equipment and sprayed onto the surface of the carbon cloth. The electrospinning voltage was 15 kV, the spinning speed was 1 ml / h, the receiving distance was 15 cm, the temperature was 24 ° C, the humidity was 40%, and the spinning time was 24 min (ensuring that the PI surface density was the same as that in Example 1) to obtain a fibrous surface layer, which was finally placed in a vacuum oven and dried for 1 h;

[0072] S3. Preparation of fiber preform

[0073] Take carbon fiber bidirectional cloth (Hexcel G0926, 5H Satin, density 370g / m 3 ), cut into 25×25cm cloth pieces, and then lay the fiber preform by hand lamination; specifically, lay 16 layers of carbon cloth at [0°] 16 The eighth layer is the carbon cloth sprayed with polyimide obtained in step S2, and a 45 mm long polytetrafluoroethylene film (30 μm thick) is laid in as a pre-crack;

[0074] S4. Preparation of composite material board

[0075] Composite panels were prepared using the VARTM method. Specifically, a double-layered flow net was applied to the laid fiber preform, with a release sheet separating the flow net and the fiber preform, and finally sealed with a vacuum bag.

[0076] Prepare epoxy resin-based slurry: 300g of bisphenol F epoxy resin Epon862 is poured into a beaker, and then 105.6g of curing agent polyetheramine D-230 is added. The mixture is stirred thoroughly with a glass rod, and then degassed in a vacuum oven at 25°C for 10 minutes to obtain about 405.6g of resin-based slurry. The resin-based slurry is evenly introduced into the fiber preform through the negative pressure of the vacuum pump. After the resin-based slurry is completely infused into the carbon fiber cloth, the VARTM platform is moved as a whole into a flat vulcanizer. It is first cured at 80°C and 3.6MPa pressure for 2h, and then cured at 120°C for 2h. After that, it is cooled and demolded to obtain a composite material plate.

[0077] The plate was cut into 21 mm wide strips and subjected to hinged double cantilever beam (DCB) test and end delamination flexure (ENF) test respectively to measure the mode I interlaminar fracture toughness (G IC ) is 1.88kJ / m 2 , Mode II interlaminar fracture toughness (G IIC ) is 0.81kJ / m 2 .

[0078] FIG9 is an SEM photograph of the fracture surface of the composite material plate prepared in this embodiment. As can be seen from FIG9 , the polyimide fiber structure is more obvious between layers and the surface is rough. The deformation of the fibers and resin under stress plays a toughening role.

[0079] Figure 3 shows microscopic morphology photographs of the polyimide layer at different electrospinning solution concentrations, where 18 wt% and 30 wt% are microscopic morphology photographs of the polyimide layers prepared in Example 1 and Example 2, respectively. The preparation method of the other polyimide layers is the same as that in Example 1, with the only difference being that in step S1, the concentration of the polyimide spinning solution is shown in Figure 3. As can be seen from Figure 3, in this application, as the spinning solution concentration changes, the microstructure of the polyimide layer also changes accordingly.

[0080] The above embodiments are only intended to help understand the method and core concept of the present invention. It should be noted that, without departing from the principles of the present invention, a number of improvements and modifications may be made to the present invention by those skilled in the art, and such improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0081] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not limited to the embodiments shown herein but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a polyimide interlayer toughened fiber composite material, comprising the following steps: A) preparing a polyimide spinning solution; B) spraying the polyimide spinning solution onto the surface of the fiber cloth or prepreg by electrostatic spinning to obtain a polyimide interlayer toughened fiber composite material; The concentration of the polyimide spinning solution is different, and the micro-nano structure morphology of the polyimide layer of the polyimide interlayer toughened fiber composite material is different.

2. The preparation method according to claim 1, characterized in that: The polyimide layer micro-nano structure morphology is one or more of fiber, sphere, bead and tube.

3. The preparation method according to claim 1, characterized in that: The concentration of the polyimide spinning solution is 10-40 wt %.

4. The preparation method according to claim 1, characterized in that: The solvent of the polyimide in the polyimide spinning solution is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, m-cresol, chloroform and dichloromethane.

5. The preparation method according to claim 1, characterized in that: The fiber cloth is selected from one or more of carbon fiber, glass fiber, metal fiber, basalt fiber, aramid fiber, carbon nanotube fiber, graphene fiber and plant fiber.

6. The preparation method according to claim 1, characterized in that: The electrospinning method has an electrospinning voltage of 10-20 kV, a spinning speed of 1-2 ml / h, a receiving distance of 15-20 cm, a temperature of 20-30° C., a humidity of 35-45%, and a time of 24-40 min.

7. A fiber preform, comprising multiple layers of laminated fiber cloth and a polyimide interlayer toughening fiber composite material arranged between the fiber cloths, wherein the polyimide interlayer toughening fiber composite material is a polyimide interlayer toughening fiber composite material prepared by the preparation method according to any one of claims 1 to 6.

8. A composite material plate, comprising a fiber preform and a resin matrix composited in the fiber preform, wherein the fiber preform is the fiber preform according to claim 7.

9. The composite material plate according to claim 8, characterized in that: The resin matrix is ​​selected from one or more of epoxy resin, phenolic resin, vinyl resin, bismaleimide resin, polyimide resin and thermoplastic resin.

10. The method for preparing the composite material plate according to claim 8, comprising: Infusing the resin-based slurry into the fiber preform and then curing it to obtain a composite material board; The fiber preform is the fiber preform according to claim 7.

Citation Information

Patent Citations

  • Toughening material of composite material and preparation method toughening material

    CN102505355A

  • Preparation method of ultrafine fibrous membrane-toughened prepreg of thermoplastic resin

    CN103552331A

  • Manufacturing method of reinforced fiber fabric with di-function of nonwoven fabric forming-toughening

    CN104309235A

  • Preparation method of polyimide interlayer toughened fiber composite material, fiber preform and composite material plate

    CN116355246A

  • Nonwoven interlayers made using polymer-nanoparticle polymers

    US20150283788A1

Cited By

  • Self-repairing fiber reinforced composite material based on 3D printing vessel network and preparation method thereof

    CN119974544A