Metal surface micro-texture processing method based on mask biological jet

Through mask biojet technology and high-precision servo control system, microbial culture is used to produce highly oxidizing ion solution to form micro-texture on the metal surface, which solves the high cost and control problems of micro-nano pattern processing in the existing technology, and realizes Low-energy, high-precision micro-texture processing improves the performance and service life of parts.

WO2024212675A1PCT designated stage expired Publication Date: 2024-10-17HUAQIAO UNIVERSITY

Patent Information

Application Number
PCT/CN2024/074431
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-01-29
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing surface texture processing technology has high equipment costs and high processing costs when processing micro-nano patterns. The micro-nano pattern morphology is difficult to control and the process is complex. It is difficult to meet the needs of efficient, low-cost, and precise micro-texture.

Method used

The metal surface micro-texture method based on mask biojet is used to produce highly oxidizing ion solution through microbial culture. The mask jet technology is used to form micro-texture on the metal surface. Combined with a high-precision servo control system, special-shaped micro-nano Processing of structures.

Benefits of technology

It achieves low-energy, green, and low-consumption micro-texture processing, reduces surface damage, improves the mechanical properties and processing accuracy of parts, has strong applicability, and extends the service time of parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024074431_17102024_PF_FP_ABST
    Figure CN2024074431_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A metal surface micro-texture processing method based on mask biological jet, comprising the following steps: (1) microorganism culture: increasing the number and microbial activity of microbial communities, so that the concentration of high-oxidizability ions in a culture solution reaches an expected set; (2) mask preparation: designing and preparing a mask according to a micro-texture requirement; (3) surface pretreatment of a workpiece to be processed; (4) micro-texture processing; and (5) re-oxidizing the culture solution. According to the method in combination with a mask technology and a high-precision servo control system, the surface material of a workpiece is selectively removed, the processing of the texture pattern of a special-shaped workpiece can be achieved, and the applicability is high.
Need to check novelty before this filing date? Find Prior Art

Description

A metal surface micro-texturing processing method based on mask biojet Technical Field

[0001] The invention belongs to the technical field of functional surface processing, and in particular relates to a metal surface micro-texturing processing method based on mask biojet. Background Art

[0002] Surface texturing refers to the creation of a pattern with defined geometric shapes and dimensions, arranged in a regular pattern, on a material's surface. Surface texturing can effectively improve a material's wear resistance, optical properties, biocompatibility, adhesion and release properties, lubricity, and heat dissipation. Parts with micro-textured surfaces are widely used in basic components, implants, medical devices, optical elements, and heat exchangers, and hold significant potential for application in national strategic industries such as aerospace, energy and transportation, and medical rehabilitation.

[0003] The processing technology of surface texture is mainly divided into additive forming, subtractive forming and forced forming. Additive forming of texture mainly adds materials to the surface of the material in an orderly manner through coating, sputtering, spraying, deposition, casting, etc., and processes micro-protrusions on the surface of the material, thereby improving the surface performance of the material. Subtractive forming of texture mainly achieves micro-removal of the material surface through mechanical cutting, high-energy beam processing, chemical etching, electrical discharge machining, electrochemical processing, etc., and processes micro-grooves, micro-pits, bionic patterns, etc. on the surface of the material to improve the surface performance. Forced forming of texture uses the plastic deformation of the material under external constraints to prepare large-area micro-textures. Existing surface texture processing technology faces problems such as high equipment costs, high processing costs, difficult to control the morphology of micro-nano patterns, and complex processes in the process of processing patterns of several microns to tens of microns. Therefore, it is very necessary to develop a new processing method to solve the above problems.

[0004] Summary of the Invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a method for metal surface micro-texturing based on mask biojet.

[0006] In order to achieve the above objectives, one of the technical solutions of the present invention is: a method for metal surface micro-texturing based on mask biojet, which specifically includes the following steps:

[0007] (1) Microbial culture: providing a suitable culture environment for microbial growth and reproduction, increasing the number and activity of microbial communities by expanding culture, and increasing the concentration of oxidative ions in the culture medium;

[0008] (2) Preparing a mask: Designing a mask pattern based on the shape and arrangement of the micro-nanostructure to be processed, and preparing a mask;

[0009] (3) Pretreatment: Pretreatment of the surface of the workpiece;

[0010] (4) Microtexture processing: According to the specific morphology of the micro-nanostructure to be processed, the spatial position between the culture fluid nozzle, the mask and the workpiece to be processed is adjusted, and the process parameters such as the injection speed and injection angle are adjusted. The microbial culture fluid with a high oxidizing ion concentration is injected through the mask onto the surface of the workpiece to be processed and fully reacts. The oxidizing ions are used to erode and remove the exposed surface of the workpiece to be processed, thereby forming a microtexture surface. The injection speed and injection angle are key factors in the processing of special-shaped curved surfaces and special-shaped microtextures.

[0011] (5) Reoxidation of the culture medium: After erosion, the culture medium is converted into a low-oxidizing solution, which is then transported to the microbial culture vessel and reoxidized by the microorganisms into a high-oxidizing solution, thus achieving a continuous cycle of the entire processing process.

[0012] Microbial culture is to build a culture environment based on the environmental factors that microorganisms need for growth or metabolism, such as oxygen, pH, nutrients, and temperature, and provide raw materials to be converted. By expanding the culture, the number of microbial populations is increased, and the activity of microorganisms and the concentration of highly oxidizing ions in the solution are improved.

[0013] Furthermore, the microorganisms used in step (1) have a corrosive effect on metals. The microorganisms can directly produce ions or participate in ion conversion, including but not limited to Thiobacillus ferrooxidans and Thiobacillus thiooxidans.

[0014] Furthermore, in step (1), during the culture process, the microorganisms are kept at a high activity by monitoring parameters such as the number of microorganisms or the concentration of the product, which are relevant parameters characterizing the conversion efficiency of the microorganisms. When the microbial activity is low, the microbial activity can be gradually increased by using a gradient of different culture medium volumes.

[0015] During the microtexturing process, the oxidizing solution fully contacts and reacts with the metal, thereby achieving material removal. The low-oxidizing solution generated by material removal needs to be oxidized into a high-oxidizing solution by microbial action. Therefore, it is necessary to ensure that the microorganisms are at a high activity during the experiment. Bacteria are usually stored at low temperatures in a refrigerator. The activity of bacteria is low under low temperature conditions, and the activity of microorganisms needs to be improved through gradual cultivation. The activity of microorganisms is determined by the conversion efficiency per unit time. In this method, the amount of product and reactant per unit volume after microbial action is measured using a colorimetric reaction to characterize the microbial activity.

[0016] Furthermore, the culture medium in step (1) is rich in highly oxidizing ions, and the culture medium involved in the microtexture processing can be a highly oxidizing solution containing microorganisms or a highly oxidizing solution without microorganisms.

[0017] The mask has a penetrating texture pattern, and a highly oxidizing solution with a certain kinetic energy passes through the mask to fully contact and react with the surface material of the workpiece to be processed.

[0018] Furthermore, the shape of the micro-texture pattern in step (2) is circular, square, rectangular, or other required shapes.

[0019] Furthermore, the scale of the micro-texture pattern in step (2) is designed to be millimeter, micrometer or nanometer scale according to requirements.

[0020] Furthermore, the mask used in steps (2) and (4) is made of a material that will not be corroded by a highly oxidizing solution, preferably plastic, rubber, ceramic, corrosion-resistant metal, etc.

[0021] Furthermore, in step (2), the mask is processed into the desired shape using various currently suitable processing methods, including but not limited to laser, etching, high-energy beam, water jet, and mechanical processing.

[0022] Furthermore, the main components of the workpiece to be processed in step (3) and step (4) can be corroded by the high-oxidizing solution, and the workpiece to be processed includes but is not limited to pure metal materials, metal alloy materials, metal sintered materials, etc. whose oxidizability is lower than that of trivalent iron ions, such as iron, cobalt, copper, and tin.

[0023] Furthermore, the surface pretreatment of the workpiece in step (3) includes but is not limited to rust removal, degreasing, polishing, various cleanings, etc., the purpose of which is to remove surface residues and obtain a neat and dry surface.

[0024] According to the processing requirements and the constraints of the processing environment, the relative positions of the nozzle, mask and workpiece, as well as the processing parameters, are appropriately adjusted to ensure that the flow field of the highly oxidizing solution through the mask is less than or equal to the processing scale of the micro-texture on the workpiece surface, thereby achieving the removal of material in the exposed area.

[0025] Furthermore, in step (4), after the culture solution passes through the mask and contacts the material surface, the highly oxidizing ions in the culture solution undergo a replacement reaction with the metal element or metal oxide on the surface to be processed, oxidizing the metal element or oxide on the surface into metal ions that dissolve in the solution, thereby removing the metal material. Simultaneously, the highly oxidizing culture solution involved in material removal is converted into a low-oxidizing culture solution.

[0026] Furthermore, the nozzle outlet cross-section in step (4) is one of circular, square, rectangular, or other special shapes designed according to the requirements of the workpiece surface micro-texture.

[0027] Furthermore, in step (4), the outlet velocity of the nozzle is adjusted to control the impact velocity of the highly oxidizing solution on the workpiece after passing through the mask, thereby adjusting the processing efficiency and processing accuracy of the micro-texture on the workpiece surface.

[0028] Furthermore, in step (4), the pressure of the highly oxidizing solution impacting the workpiece surface can be adjusted by adjusting the spray angle, and the pressure difference of the solution can be used to obtain textured surfaces of different micro-nano scales.

[0029] Furthermore, the step (4) achieves micro-texturing of the entire surface or a part of the workpiece by controlling the relative position of the nozzle and the workpiece.

[0030] The low-oxidizing solution is transported to the microbial culture vessel through a pipeline, and the characteristics of microorganisms are used to accelerate the oxidation process of the low-oxidizing solution to a high-oxidizing solution. After the solution recovers its high oxidizing property, it continues to participate in the processing of the microtexture, realizing the continuous cycle of the entire processing process.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. This invention utilizes the metabolic characteristics of microorganisms to ensure high oxidizability of the culture medium and introduces jet technology to improve the removal efficiency of workpiece surface materials. This method is green and low-cost.

[0033] 2. The present invention uses a low-energy removal method during the micro-texturing process on the material surface, reducing surface damage and improving the mechanical properties of the surface texture, which is of great benefit to improving component performance and extending service life.

[0034] 3. The present invention combines mask technology and a high-precision servo control system to selectively remove material from the workpiece surface, which can realize the processing of micro-nano structures of special-shaped workpieces and has strong applicability. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] FIG1 is a schematic diagram of a metal surface micro-texturing process based on a mask biojet in Example 1;

[0036] FIG2 is a schematic diagram of adjusting the workpiece posture and position to achieve micro-texturing of the entire workpiece surface in Example 1;

[0037] In the figure, 1-microorganism reaction vessel, 2-culture tank, 3-boosting equipment, 4-jet pipeline, 5-nozzle, 6-mask, 7-liquid storage tank, 8-copper sample, 9-reflux pipeline, 10-pump, 11-clamping platform. DETAILED DESCRIPTION

[0038] To make the objectives, technical solutions, and advantages of the present invention more clearly understood, the present invention is described in more detail below with reference to the accompanying drawings and specific embodiments, but the scope of protection of the present invention is not limited to these embodiments. The same reference numerals throughout the text represent the same elements, and similar reference numerals represent similar elements.

[0039] In the description of the present invention, it should be understood that the terms "upper", "lower", "front", "back", "left", "right", "horizontal", "vertical", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the stereoscopic diagrams in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention.

[0040] Example 1

[0041] A method for metal surface microtexturing based on mask biojet comprises the following steps:

[0042] 1. Microbial culture: The microorganism used in the embodiment is Thiobacillus ferrooxidans. The activity of the strain stored at low temperature is low, and direct participation in texturing processing will lead to low processing efficiency. When conducting the experiment, different culture solution volumes are used (set to 100ml, 500ml, 2000ml, and 10000ml respectively) to gradually increase the activity of the microorganism to ensure that the microorganism is in a high activity when participating in the reaction. The liquid culture solution includes 3g / L ammonium sulfate, 0.5g / L magnesium sulfate heptahydrate, 0.1g / L dipotassium hydrogen phosphate, 0.01g / L potassium nitrate 24hydrate, and 24.83g / L ferrous sulfate heptahydrate. The pH of the culture solution is adjusted to 1.8 using dilute sulfuric acid. The Thiobacillus ferrooxidans strain is inoculated into the culture solution and oxygen is introduced and cultured in a constant temperature shaker for 20 hours at a temperature of 30°C and a shaker speed of 180rpm. Fe is converted to ferrous sulfate by the action of microorganisms. 2+ Converted to Fe 3+ , determination of Fe in the culture medium 2+ with Fe 3+ The relative content of Fe 3+ The solution is used as a highly oxidizing solution to participate in the processing of surface microtexture. After the action of microorganisms, Fe 2+ The content is almost 0, and most of the iron ions are Fe 3+ According to Fe 2+ with Fe 3+ The color development characteristics in different solutions are used to determine whether the conversion is complete by titration.

[0043] 2. Mask processing: As shown in Figure 1-2, the micro pattern of the mask 6 is a matrix of circular holes designed by experience. Micro-nano laser cutting technology is used to process a 9x9 matrix of circular holes with a diameter of 50μm on a 301 stainless steel sheet, and it is mechanically clamped to fit tightly with the copper sample 8.

[0044] 3. Pretreatment of the workpiece: Copper is selected as the workpiece to be processed. A sample with a diameter of φ = 15 mm and a thickness of h = 3 mm is cut from the copper plate and embedded in the resin. The sample is ground and polished using a grinding and polishing machine. After cleaning and drying, a flat and clean copper block sample 8 is obtained.

[0045] 4. Microtexturing: As shown in Figures 1-2, a booster device 3 is used as a jet power source to increase the pressure of the culture medium. The highly oxidizing culture medium in the culture tank 2 is transported to the nozzle 5 via the jet line 4. The highly oxidizing culture medium is ejected from the nozzle 5 outlet, passes through the mask 6, and reacts with the exposed surface of the copper sample 8. Adjusting the position of the clamping platform 11 can achieve microtexturing of the entire workpiece surface, removing the surface material of the copper block. After the reaction, the culture medium is converted into a low-oxidizing solution and returned to the liquid storage tank 7. In this bio-jet microtexturing process, the nozzle outlet cross-section is circular with a diameter of 12 mm, the distance d between the nozzle outlet and the mask is 5 mm, the flow rate is 0.14 L / s, and the nozzle axis is perpendicular to the mask plane, that is, α = 90° and θ = 90°. After etching for 5 minutes, a microtexture is machined on the surface of the copper sample 8.

[0046] 5. Re-oxidize the culture fluid by utilizing the metabolic characteristics of microorganisms: As shown in FIG1 , the low-oxidizing solution in the liquid storage tank 7 is returned to the microbial reaction vessel 1 through the reflux line 9 and the pump 10 . The low-oxidizing solution is re-oxidized into a high-oxidizing solution by utilizing the characteristics of microorganisms and stored in the culture tank 2 , thereby realizing the recycling of the culture fluid.

[0047] Example 2

[0048] 1. Microbial culture: The microorganism used in the embodiment is Thiobacillus ferrooxidans. The activity of the strain stored at low temperature is low, and direct participation in texturing processing will lead to low processing efficiency. When conducting the experiment, different culture solution volumes are used (set to 100ml, 500ml, 2000ml, and 10000ml respectively) to gradually increase the activity of the microorganism to ensure that the microorganism is in a high activity when participating in the reaction. The liquid culture solution includes 3g / L ammonium sulfate, 0.5g / L magnesium sulfate heptahydrate, 0.1g / L dipotassium hydrogen phosphate, 0.01g / L potassium nitrate 24hydrate, and 24.83g / L ferrous sulfate heptahydrate. The pH of the culture solution is adjusted to 1.8 using dilute sulfuric acid. The Thiobacillus ferrooxidans strain is inoculated into the culture solution and oxygen is introduced and cultured in a constant temperature shaker for 20 hours at a temperature of 30°C and a shaker speed of 180rpm. Fe is converted to ferrous sulfate by the action of microorganisms. 2+ Converted to Fe 3+ , determination of Fe in the culture medium 2+ with Fe 3+ The relative content of Fe 3+ The solution is used as a highly oxidizing solution to participate in the processing of surface microtexture. After the action of microorganisms, Fe 2+ The content is almost 0, and most of the iron ions are Fe 3+ According to Fe 2+ with Fe 3+ The color development characteristics in different solutions are used to determine whether the conversion is complete by titration.

[0049] 2. Mask processing: As shown in Figure 1-2, the micro pattern of the mask 6 is a matrix of circular holes designed by experience. Micro-nano laser cutting technology is used to process a 9x9 matrix of circular holes with a diameter of 50μm on a 301 stainless steel sheet, and it is mechanically clamped to fit tightly with the copper sample 8.

[0050] 3. Pretreatment of the workpiece: Copper is selected as the workpiece to be processed. A sample with a diameter of φ = 15 mm and a thickness of h = 3 mm is cut from the copper plate and embedded in the resin. The sample is ground and polished using a grinding and polishing machine. After cleaning and drying, a flat and clean copper block sample 8 is obtained.

[0051] 4. Microtexturing: As shown in Figures 1-2, a booster device 3 is used as a jet power source to increase the pressure of the culture medium. The highly oxidizing culture medium in the culture tank 2 is transported to the nozzle 5 via the jet line 4. The highly oxidizing culture medium is ejected from the nozzle 5 outlet, passes through the mask 6, and reacts with the exposed surface of the copper sample 8. Adjusting the position of the clamping platform 11 can achieve microtexturing of the entire workpiece surface, removing the surface material of the copper block. After the reaction, the culture medium is converted into a low-oxidizing solution and returned to the liquid storage tank 7. In this bio-jet microtexturing process, the nozzle outlet cross-section is circular with a diameter of 12mm. The distance d between the nozzle outlet and the mask is 5mm. The flow rate is 0.17L / s. The nozzle axis is perpendicular to the mask plane, that is, α = 90° and θ = 90°. After etching for 5 minutes, a microtexture is machined on the surface of the copper sample 8.

[0052] 5. Re-oxidize the culture fluid by utilizing the metabolic characteristics of microorganisms: As shown in FIG1 , the low-oxidizing solution in the liquid storage tank 7 is returned to the microbial reaction vessel 1 through the reflux line 9 and the pump 10 . The low-oxidizing solution is re-oxidized into a high-oxidizing solution by utilizing the characteristics of microorganisms and stored in the culture tank 2 , thereby realizing the recycling of the culture fluid.

[0053] Example 3

[0054] 1. Microbial culture: The microorganism used in the embodiment is Thiobacillus ferrooxidans. The activity of the strain stored at low temperature is low, and direct participation in texturing processing will lead to low processing efficiency. When conducting the experiment, different culture solution volumes are used (set to 100ml, 500ml, 2000ml, and 10000ml respectively) to gradually increase the activity of the microorganism to ensure that the microorganism is in a high activity when participating in the reaction. The liquid culture solution includes 3g / L ammonium sulfate, 0.5g / L magnesium sulfate heptahydrate, 0.1g / L dipotassium hydrogen phosphate, 0.01g / L potassium nitrate 24hydrate, and 24.83g / L ferrous sulfate heptahydrate. The pH of the culture solution is adjusted to 1.8 using dilute sulfuric acid. The Thiobacillus ferrooxidans strain is inoculated into the culture solution and oxygen is introduced and cultured in a constant temperature shaker for 20 hours at a temperature of 30°C and a shaker speed of 180rpm. Fe is converted to ferrous sulfate by the action of microorganisms. 2+ Converted to Fe 3+ , determination of Fe in the culture medium 2+ with Fe 3+ The relative content of Fe 3+ The solution is used as a highly oxidizing solution to participate in the processing of surface microtexture. After the action of microorganisms, Fe 2+ The content is almost 0, and most of the iron ions are Fe 3+ According to Fe 2+ with Fe 3+The color development characteristics in different solutions are used to determine whether the conversion is complete by titration.

[0055] 2. Mask processing: As shown in Figure 1-2, the micro pattern of the mask 6 is a matrix of circular holes designed by experience. Micro-nano laser cutting technology is used to process a 9x9 matrix of circular holes with a diameter of 100μm on a 301 stainless steel sheet, and it is mechanically clamped to make it fit tightly with the copper sample 8.

[0056] 3. Pretreatment of the workpiece: Copper is selected as the workpiece to be processed. A sample with a diameter of φ = 15 mm and a thickness of h = 3 mm is cut from the copper plate and embedded in the resin. The sample is ground and polished using a grinding and polishing machine. After cleaning and drying, a flat and clean copper block sample 8 is obtained.

[0057] 4. Microtexturing: As shown in Figures 1-2, a booster device 3 is used as a jet power source to increase the pressure of the culture medium. The highly oxidizing culture medium in the culture tank 2 is transported to the nozzle 5 via the jet line 4. The highly oxidizing culture medium is ejected from the nozzle 5 outlet, passes through the mask 6, and reacts with the exposed surface of the copper sample 8. Adjusting the position of the clamping platform 11 can achieve microtexturing of the entire workpiece surface, removing the surface material of the copper block. After the reaction, the culture medium is converted into a low-oxidizing solution and returned to the liquid storage tank 7. In this bio-jet microtexturing process, the nozzle outlet cross-section is circular with a diameter of 12 mm, the distance d between the nozzle outlet and the mask is 5 mm, the flow rate is 0.14 L / s, and the nozzle axis is perpendicular to the mask plane, that is, α = 90° and θ = 90°. After etching for 5 minutes, a microtexture is machined on the surface of the copper sample 8.

[0058] 5. Re-oxidize the culture fluid by utilizing the metabolic characteristics of microorganisms: As shown in FIG1 , the low-oxidizing solution in the liquid storage tank 7 is returned to the microbial reaction vessel 1 through the reflux line 9 and the pump 10 . The low-oxidizing solution is re-oxidized into a high-oxidizing solution by utilizing the characteristics of microorganisms and stored in the culture tank 2 , thereby realizing the recycling of the culture fluid.

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or make equivalent replacements for some of the technical features therein. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention. Industrial Applicability

[0060] The present invention belongs to the technical field of functional surface processing and specifically discloses a method for microtexturing a metal surface based on a mask biojet, comprising the following steps: (1) microbial cultivation: increasing the number and activity of microbial communities so that the concentration of highly oxidizing ions in the culture medium reaches a desired setting; (2) mask preparation: designing and preparing a mask according to microtexturing requirements; (3) pre-treating the surface of the workpiece to be processed; (4) microtexturing processing; and (5) re-oxidizing the culture medium. The present invention combines mask technology with a high-precision servo control system to selectively remove material from the workpiece surface, enabling the processing of textured patterns on irregularly shaped workpieces. The method has strong applicability and industrial practicality.

Claims

1. A method for metal surface microtexturing based on mask biojet, characterized in that: The steps include: (1) Microbial culture: Providing a culture environment for the growth and reproduction of microorganisms. The culture medium contains oxidizing ions or ions to be oxidized. By expanding the culture, the number of microbial communities and the activity of microorganisms are increased, and the concentration of oxidizing ions in the culture medium is increased; (2) Preparing a mask: designing a mask pattern according to the shape and arrangement of the micro-nano structure to be processed, and preparing a mask; (3) Pretreatment: pretreatment of the surface of the workpiece; (4) Microtexturing: According to the specific morphology of the micro-nanostructure of the surface to be processed, the spatial position between the culture fluid nozzle, the mask and the workpiece to be processed is adjusted, and the injection speed and injection angle are adjusted so that the culture fluid is sprayed onto the surface of the workpiece through the mask, and the surface of the workpiece to be processed is eroded and removed to form a microtextured surface; (5) Reoxidation of the culture solution by microorganisms: The culture solution eroded in step (4) is transported to the microbial culture in step (1), where the microorganisms reoxidize it into an oxidizing solution.

2. The metal surface microtexturing method according to claim 1, characterized in that: The microorganisms used in the step (1) have a corrosive effect on metals, can directly generate ions or participate in ion conversion, and the microorganisms include Thiobacillus ferrooxidans and Thiobacillus thiooxidans.

3. The metal surface microtexturing method according to claim 1, characterized in that: In the step (1), the number of microorganisms or the concentration of products are monitored to keep the microorganisms participating in the texturing process at a higher activity.

4. The metal surface microtexturing method according to claim 1, characterized in that The oxidizing ion in step (1) is Fe 3+ , the ion to be oxidized is Fe 2+ .

5. The metal surface microtexturing method according to claim 1, characterized in that: The shape of the micro-texture pattern in step (2) is one of circular, square, rectangular or other required shapes, and the scale of the micro-texture pattern is designed to be millimeter, micrometer or nanometer scale according to requirements.

6. The metal surface microtexturing method according to claim 1, characterized in that: In the steps (2) and (4), the mask is made of a material that is not corroded by an oxidizing solution, and the mask has a penetrating mask pattern.

7. The metal surface microtexturing method according to claim 1, characterized in that: The processing methods of the mask in step (2) include laser, etching, high-energy beam, water jet, and mechanical processing.

8. The metal surface microtexturing method according to claim 1, characterized in that: In the steps (3) and (4), the main components of the workpiece to be processed can be corroded by the oxidizing solution, and the workpiece to be processed includes iron, cobalt, copper, tin, and pure metal materials, metal alloy materials, and metal sintered materials whose oxidizability is lower than that of trivalent iron ions.

9. The metal surface microtexturing method according to claim 1, characterized in that: The surface pretreatment of the workpiece to be processed in step (3) includes rust removal, degreasing, polishing, and various cleanings.

10. The metal surface microtexturing method according to claim 1, characterized in that: The nozzle outlet cross-section in step (4) is one of circular, square, rectangular, or other special shapes designed according to the requirements of the workpiece surface micro-texture.

11. The metal surface microtexturing method according to claim 1, characterized in that The step (4) controls the impact speed of the oxidizing solution on the workpiece after passing through the mask by adjusting the outlet speed of the nozzle, adjusts the pressure of the oxidizing solution impacting the workpiece surface by adjusting the injection angle, and realizes micro-texturing processing of the entire surface or a part of the workpiece by controlling the relative position of the nozzle and the workpiece.

Citation Information

Patent Citations

  • Double-face etching method for metal product

    CN103352224A

  • Auxiliary jet flow processing method for mask

    CN109968206A

  • Metal polishing solution and metal polishing method

    CN113403622A

  • Metal surface micro-texture machining method based on mask biological jet

    CN116445912A

  • Etching method, production of ink jet head, ink jet head and ink jet recorder

    JP2000328266A

Cited By

  • Method for producing microtextured metal surfaces by biojet and thermal transfer

    JP2026090214A