Polyimide resin precursor, polyimide resin, and polyimide film

A polyimide resin precursor with specific structural units addresses adhesion and heat resistance issues in the semiconductor field by enhancing the properties of polyimide resins, enabling better coating and thermal performance.

WO2024214600A1PCT designated stage expired Publication Date: 2024-10-17MITSUBISHI GAS CHEM CO INC

Patent Information

Application Number
PCT/JP2024/013675
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-01
Filing Date
2024-04-02
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Polyimide resins used in the semiconductor field face challenges with adhesion to silicon-based substrates due to lower surface functional groups and require curing at lower temperatures, while also needing improved heat resistance and solubility in rinsing liquids for coating applications.

Method used

A polyimide resin precursor with specific structural units derived from tetracarboxylic dianhydrides and diamines, such as 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride and 4-aminophenyl-4-aminobenzoate, is developed, which enhances heat resistance, adhesion, and solubility, allowing for better coating properties and thermal imidization.

Benefits of technology

The resulting polyimide resin exhibits excellent heat resistance, improved adhesion to silicon-based substrates, and enhanced solubility in rinsing liquids, making it suitable for semiconductor applications with improved processing conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013675_17102024_PF_FP_ABST
    Figure JP2024013675_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A polyimide resin precursor having a constituent unit A derived from a tetracarboxylic dianhydride and a constituent unit B derived from a diamine, wherein: the constituent unit A contains a constituent unit (A1) derived from a compound represented by formula (a1); and the constituent unit B contains at least one selected from the group consisting of a constituent unit (B1) derived from a compound represented by formula (b1), a constituent unit (B2) derived from a compound represented by formula (b2), and a constituent unit (B3) derived from a compound represented by formula (b3).
Need to check novelty before this filing date? Find Prior Art

Description

Polyimide resin precursor, polyimide resin and polyimide film

[0001] The present invention relates to a polyimide resin precursor, a polyimide resin, and a polyimide film.

[0002] Polyimide resins have excellent heat resistance and mechanical properties, and various applications are being considered in fields such as electrical and electronic components. For example, among electrical and electronic components, polyimide resins with heat resistance and transparency are used in the display field. In the display field, glass is generally used as the supporting substrate. For example, Patent Document 1 discloses a polyimide precursor having a repeating unit derived from 4-aminophenyl-4-aminobenzoate, with the aim of obtaining a polyimide film with improved heat resistance, linear thermal expansion coefficient, and light transmittance, as well as improved adhesion between a laminate of a polyimide film and a glass substrate.

[0003] Patent No. 7235157

[0004] Polyimide resins are used not only in the display field but also as insulating film materials in the semiconductor field. Polyimide resins used in the semiconductor field require not only heat resistance but also adhesion to supporting substrates such as silicon, silicon nitride, and silicon oxide. However, compared to the glass used in the display field, silicon has fewer functional groups on its surface, resulting in poor adhesion to resins, and therefore polyimide resins require higher adhesion. Furthermore, compared to displays, semiconductors require lower curing temperatures because high-temperature processing can affect the supporting substrate depending on the device configuration, and therefore adhesion must be achieved even at lower temperatures. In the semiconductor field, resin varnishes are mainly applied by spin coating, making it necessary to remove varnish that has spread to the periphery and backside of silicon wafers. However, polyimide resins and polyimide resin precursors (polyamic acids) generally have poor solubility in rinse solutions (e.g., propylene glycol monomethyl ether, cyclohexanone) used to remove varnish. Therefore, there is a demand for polyimide resin precursor varnishes with excellent solubility in rinse solutions, or in other words, excellent coatability. The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a polyimide resin precursor that can produce a polyimide resin having excellent heat resistance and adhesion and has excellent coatability, and further to provide a polyimide resin and a polyimide film having excellent heat resistance and adhesion.

[0005] The present inventors have discovered that a polyimide resin precursor having specific structural units, a polyimide film obtained using the precursor, and a polyimide resin can solve the above-mentioned problems, and have thus completed the present invention.

[0006] That is, the present invention relates to the following items [1] to

[15] : [1] A polyimide resin precursor having a structural unit A derived from a tetracarboxylic dianhydride and a structural unit B derived from a diamine, wherein the structural unit A includes a structural unit (A1) derived from a compound represented by the following formula (a1), and the structural unit B includes at least one selected from the group consisting of a structural unit (B1) derived from a compound represented by the following formula (b1), a structural unit (B2) derived from a compound represented by the following formula (b2), and a structural unit (B3) derived from a compound represented by the following formula (b3): [2] The polyimide resin precursor according to [1] above, wherein the proportion of the structural unit (A1) in the structural unit A is 30 to 100 mol %. [3] The polyimide resin precursor according to [1] above or [2] above, wherein the total proportion of the structural unit (B1), the structural unit (B2), and the structural unit (B3) in the structural unit B is 30 to 100 mol %. [4] The polyimide resin precursor according to any one of [1] to [3] above, wherein the polyimide resin precursor is a polyamic acid. [5] The polyimide resin precursor according to any one of [1] to [4] above, wherein the structural unit A further comprises at least one selected from the group consisting of a structural unit (A3) derived from a compound represented by the following formula (a3) ​​and a structural unit (A4) derived from a compound represented by the following formula (a4): [6] The polyimide resin precursor according to any one of [1] to [5] above, wherein the molar ratio of the structural unit (A1) in the structural unit A to the total of the structural units (A3) and (A4), [(A1) / ((A3)+(A4))], is 30 / 70 to 100 / 0. [7] A varnish containing the polyimide resin precursor according to any one of [1] to [6] above and an organic solvent. [8] The varnish according to [7] above, wherein the organic solvent contains at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, and γ-butyrolactone. [9] A polyimide film obtained by applying the varnish according to [7] or [8] above to a support and heating it.

[10] A polyimide resin having a structural unit AI derived from a tetracarboxylic dianhydride and a structural unit BI derived from a diamine, wherein the structural unit AI includes a structural unit (AI1) derived from a compound represented by the following formula (a1), and the structural unit BI includes at least one selected from the group consisting of a structural unit (BI1) derived from a compound represented by the following formula (b1), a structural unit (BI2) derived from a compound represented by the following formula (b2), and a structural unit (BI3) derived from a compound represented by the following formula (b3):

[11] The polyimide resin according to

[10] above, wherein the proportion of the structural unit (AI1) within the structural unit AI is 30 to 100 mol %.

[12] The polyimide resin according to

[10] or

[11] above, wherein the total proportion of the structural unit (BI1), the structural unit (BI2), and the structural unit (BI3) within the structural unit BI is 30 to 100 mol %.

[13] The polyimide resin according to any one of

[10] to

[12] above, wherein the structural unit AI further comprises at least one selected from the group consisting of a structural unit (AI3) derived from a compound represented by the following formula (a3) ​​and a structural unit (AI4) derived from a compound represented by the following formula (a4):

[14] The polyimide resin according to any one of

[10] to

[13] above, wherein the molar ratio of the structural unit (AI1) to the total of the structural units (AI3) and (AI4) within the structural unit AI, [(AI1) / ((AI3)+(AI4)], is 30 / 70 to 100 / 0.

[15] A polyimide film comprising the polyimide resin according to any one of

[10] to

[14] above.

[0007] According to the present invention, a polyimide resin having excellent heat resistance and adhesion can be obtained, and a polyimide resin precursor having excellent coatability can be provided. Furthermore, a polyimide resin and a polyimide film having excellent heat resistance and adhesion can be provided. Because the polyimide resin precursor of the present invention has the above-mentioned properties, it is useful as a raw material in the semiconductor field.

[0008] [Polyimide Resin Precursor] The polyimide resin precursor of the present invention is a polyimide resin precursor having a structural unit A derived from a tetracarboxylic dianhydride and a structural unit B derived from a diamine, in which the structural unit A includes a structural unit (A1) derived from a compound represented by the following formula (a1), and the structural unit B includes at least one selected from the group consisting of a structural unit (B1) derived from a compound represented by the following formula (b1), a structural unit (B2) derived from a compound represented by the following formula (b2), and a structural unit (B3) derived from a compound represented by the following formula (b3).

[0009] The reasons why the polyimide resin precursor of the present invention has excellent coatability and why use of the polyimide resin precursor of the present invention can produce polyimide resins with excellent heat resistance and adhesion are unclear, but are thought to be as follows. The polyimide resin precursor of the present invention contains a structure derived from a specific tetracarboxylic dianhydride component having a highly sterically hindered substituent and a flexible moiety, and a structure derived from a specific diamine having an ester skeleton with high linearity and relatively low water absorption. This is thought to increase the solubility of the polyimide precursor while providing a resin obtained after thermal imidization with excellent heat resistance. Furthermore, by including the above structure, the polyimide resin precursor of the present invention is thought to provide a resin that is less likely to absorb moisture, which inhibits adhesion. As described above, the polyimide resin precursor of the present invention can produce polyimide resins with excellent heat resistance and adhesion, and is thought to provide excellent coatability.

[0010] <Structural Unit A> The structural unit A is a structural unit derived from a tetracarboxylic dianhydride contained in a polyimide resin precursor. The structural unit A includes a structural unit (A1) derived from a compound represented by the following formula (a1). When the structural unit A includes the structural unit (A1), the coatability of the varnish and the adhesion of the polyimide resin can be improved.

[0011] The compound represented by formula (a1) is 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA). When the structural unit A contains the structural unit (A1), the resulting polyimide resin has excellent heat resistance, and further, the coatability of the varnish and the adhesion of the polyimide resin can be improved.

[0012] The proportion of the structural unit (A1) within the structural unit A is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, and still more preferably 95 to 100 mol; it may even be 100 mol, and the structural unit A may consist solely of the structural unit (A1). When the proportion of the structural unit (A1) is within the above range, the resulting polyimide resin will have excellent heat resistance, and further, the coatability of the varnish and the adhesion of the polyimide resin can be improved.

[0013] The structural unit A may consist solely of the structural unit (A1), or may include a structural unit other than the structural unit (A1), and preferably further includes, as the structural unit other than the structural unit (A1), at least one selected from the group consisting of the structural unit (A3) derived from a compound represented by the following formula (a3) ​​and the structural unit (A4) derived from a compound represented by the following formula (a4), and more preferably includes the structural unit (A3) derived from a compound represented by the following formula (a3). In other words, the structural unit A includes at least one selected from the group consisting of the structural unit (A3) derived from a compound represented by the formula (a3) ​​and the structural unit (A4) derived from a compound represented by the formula (a4), and the structural unit (A1) derived from a compound represented by the formula (a1), or is composed solely of the structural unit (A1).

[0014] The compound represented by formula (a3) ​​is pyromellitic anhydride (PMDA). When structural unit A contains structural unit (A3), the heat resistance of the polyimide resin can be enhanced while maintaining favorable varnish coatability and polyimide resin adhesion. The compound represented by formula (a4) is 4,4-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl (BP-TME). When structural unit A contains structural unit (A4), the heat resistance of the polyimide resin can be enhanced while maintaining favorable varnish coatability and polyimide resin adhesion.

[0015] The molar ratio of the structural unit (A1) to the total of the structural units (A3) and (A4) in the structural unit A [(A1) / ((A3)+(A4))] is preferably 30 / 70 to 100 / 0, more preferably 40 / 60 to 100 / 0, even more preferably 50 / 50 to 100 / 0, still more preferably 60 / 40 to 100 / 0, even more preferably 60 / 40 to 90 / 10, and still more preferably 60 / 40 to 80 / 20. When the molar ratio of the structural unit (A1) to the total of the structural units (A3) and (A4) is 100 / 0, the structural unit A does not include the structural units (A3) and (A4).

[0016] The molar ratio of the structural unit (A1) to the structural unit (A3) in the structural unit A [(A1) / (A3)] is preferably 30 / 70 to 100 / 0, more preferably 40 / 60 to 100 / 0, even more preferably 40 / 60 to 90 / 10, even more preferably 40 / 60 to 80 / 20, even more preferably 40 / 60 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. When the molar ratio of the structural unit (A1) to the structural unit (A3) is 100 / 0, the structural unit A does not contain the structural unit (A3). By using the structural units constituting the structural unit A in the above molar ratio, it is possible to improve the heat resistance of the polyimide resin while maintaining good varnish coatability and adhesion of the polyimide resin.

[0017] The structural unit A may contain structural units other than the structural unit (A1), the structural unit (A3), and the structural unit (A4). The tetracarboxylic acid dianhydride that provides such a structural unit is not particularly limited, but examples include aromatic tetracarboxylic acid dianhydrides excluding compounds represented by formula (a1), (a3), and (a4), alicyclic tetracarboxylic acid dianhydrides, and aliphatic tetracarboxylic acid dianhydrides. When the structural unit A contains structural units other than the structural unit (A1), the structural unit (A3), and (A4), it is preferable for the structural unit A to contain an aromatic tetracarboxylic acid dianhydride, among tetracarboxylic acid dianhydrides excluding compounds represented by formula (a1), (a3), and (a4). Examples of aromatic tetracarboxylic dianhydrides include 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride (BPF-PA), 2,3,6,7-naphthalene tetracarboxylic 2,3:6,7-dianhydride (NTCDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 9,9-bis(trifluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic dianhydride (6FCDA), 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]hexafluoropropane dianhydride, and 4,4'-oxydiphthalic anhydride (ODPA). Examples of suitable dianhydrides include 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), hydroquinone diphthalic anhydride (HQDEA), ethylene glycol bis(trimellitate) dianhydride (TMEG), and p-phenylene bis(trimellitate) dianhydride (TAHQ). Of these, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) is preferred.Examples of alicyclic tetracarboxylic dianhydrides include cyclohexane-1,2,4,5-tetracarboxylic dianhydride (HPMDA), cyclohexane-1,2,3,4-tetracarboxylic dianhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5',6,6'-tetracarboxylic dianhydride (CpODA), 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopent ... Examples of the aliphatic tetracarboxylic dianhydride include 1,2,4,5-cyclopentanetetracarboxylic dianhydride, 3,3',4,4'-bicyclohexyltetracarboxylic dianhydride, 2,2-propylidene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, and bicyclo[4.4.0]decane-2,3,6,7-tetracarboxylic acid dianhydride. Examples of the aliphatic tetracarboxylic dianhydride include 1,2,3,4-butanetetracarboxylic acid dianhydride. In this specification, "aromatic tetracarboxylic acid dianhydride" refers to a tetracarboxylic acid dianhydride containing one or more aromatic rings, "alicyclic tetracarboxylic acid dianhydride" refers to a tetracarboxylic acid dianhydride containing one or more alicyclic rings but no aromatic rings, and "aliphatic tetracarboxylic acid dianhydride" refers to a tetracarboxylic acid dianhydride containing neither an aromatic ring nor an alicyclic ring. The structural unit A may optionally contain one type of structural unit, or two or more types of structural units.

[0018] <Structural Unit B> The structural unit B is a structural unit derived from a diamine contained in the polyimide resin precursor. The structural unit B includes at least one selected from the group consisting of a structural unit (B1) derived from a compound represented by the following formula (b1), a structural unit (B2) derived from a compound represented by the following formula (b2), and a structural unit (B3) derived from a compound represented by the following formula (b3). When the structural unit B includes one or more of the structural unit (B1), the structural unit (B2), and the structural unit (B3), the coatability of the varnish and the adhesion of the polyimide resin can be improved.

[0019] The compound represented by formula (b1) is 4-aminophenyl-4-aminobenzoate (4-BAAB). When structural unit B contains structural unit (B1), the resulting polyimide resin has excellent heat resistance, and the coatability of the varnish and the adhesion of the polyimide resin can also be improved. The compound represented by formula (b2) is bis(4-aminophenyl)terephthalate (APTP). When structural unit B contains structural unit (B2), the resulting polyimide resin has excellent heat resistance, and the adhesion of the polyimide resin can also be improved. The compound represented by formula (b3) is 1,4-bis(4-aminobenzoyloxy)benzene. When structural unit B contains structural unit (B3), the resulting polyimide resin has excellent heat resistance, and the adhesion of the polyimide resin can also be improved. The structural unit B includes at least one selected from the group consisting of the structural unit (B1), the structural unit (B2), and the structural unit (B3), preferably includes at least one selected from the group consisting of the structural unit (B1) and the structural unit (B2), and more preferably includes the structural unit (B1).

[0020] The total ratio of the structural unit (B1), the structural unit (B2), and the structural unit (B3) in the structural unit B is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the structural unit B may consist of only at least one selected from the group consisting of the structural unit (B1), the structural unit (B2), and the structural unit (B3). The ratio of the structural unit (B1) in the structural unit B is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the structural unit B may consist of only the structural unit (B1). The ratio of the structural unit (B2) within the structural unit B is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and structural unit B may consist solely of the structural unit (B2). The ratio of the structural unit (B3) within the structural unit B is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and structural unit B may consist solely of the structural unit (B3). When the ratios of the structural units (B1), (B2), and (B3) are within the above ranges, the resulting polyimide resin has excellent heat resistance, and furthermore, the coatability of the varnish and the adhesion of the polyimide resin can be improved.

[0021] The structural unit B may contain structural units other than the structural unit (B1), the structural unit (B2), and the structural unit (B3). Diamines that provide such structural units are not particularly limited, but include aromatic diamines, alicyclic diamines, and aliphatic diamines excluding the compounds represented by formula (b1), the compounds represented by formula (b2), and the compounds represented by formula (b3). Examples of aromatic diamines include 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (2,2'-TFMB), 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-5,5'-diaminobiphenyl, 2,2-bis(4-aminophenyl)hexafluoropropane (HFDA), 2 , 2-bis(3-amino-4-methylphenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP), 4,4'-diaminodiphenyl ether (4,4'-ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (DDM), 4,4'-diaminodiphenyl sulfone (4,4'-DDS), 3,3'-diaminodiphenyl sulfone (3,3'-DDS ), 4,4'-diamino-2,2'-dimethylbiphenyl (mTB), 9,9-bis(4-aminophenyl)fluorene (BAFL), 4,4'-diaminobiphenyl (benzidine), 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diaminodiphenyl sulfide, 4,4'-diaminobenzophenone, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 5-amino-1,3,3-trimethyl -1-(4-aminophenyl)-indan (5-TMDM), 6-amino-1,3,3-trimethyl-1-(4-aminophenyl)-indan (6-TMDM), 1,3-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,3-bis(4-amino-α,α-dimethylbenzyl)benzene (BisAM), 1,4-bis(4-amino-α,α-dimethylbenzyl)benzene (BisAP), 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl (BODA), 1,1-bis[4-(4-aminophenoxy)phenyl]cyclohexane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 1,4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone [4-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4-diaminobenzanilide, 4-aminobenzoate-4-aminophenyl, 3,4-diaminobenzanilide, and the like. Examples of alicyclic diamines include 1,3-bis(aminomethyl)cyclohexane (1,3-BAC), 1,4-bis(aminomethyl)cyclohexane, 1,3-cyclohexyldiamine, 1,4-cyclohexyldiamine, isophoronediamine, bis(aminomethyl)norbornane, 4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexyl ether, and 2,2-bis(4-aminocyclohexyl)propane. Examples of aliphatic diamines include ethylenediamine and hexamethylenediamine. In this specification, aromatic diamine refers to a diamine containing one or more aromatic rings, alicyclic diamine refers to a diamine containing one or more alicyclic rings but no aromatic rings, and aliphatic diamine refers to a diamine containing neither an aromatic ring nor an alicyclic ring. The structural units other than the structural units (B1), (B2), and (B3) optionally contained in the structural unit B may be one type, or two or more types.

[0022] <Characteristics of Polyimide Resin Precursor> The number-average molecular weight of the polyimide resin precursor is preferably 5,000 to 500,000 from the viewpoint of the mechanical strength of the resulting polyimide film. Furthermore, from the same viewpoint, the weight-average molecular weight (Mw) is preferably 10,000 to 800,000, more preferably 30,000 to 300,000. The number-average molecular weight and weight-average molecular weight of the polyimide resin precursor can be determined from values ​​converted into standard polymethyl methacrylate (PMMA) by gel filtration chromatography measurement.

[0023] The polyimide resin precursor of the present invention is preferably a polyimide resin precursor having a polyamic acid structure, and more preferably a polyamic acid.

[0024] <Method for Producing Polyimide Resin Precursor> The polyimide resin precursor may be produced by any method, but the following production method is preferred. As described above, the polyimide resin precursor is preferably produced by a production method in which a compound (tetracarboxylic acid component) that provides the above-mentioned structural unit A is reacted with a compound (diamine component) that provides the above-mentioned structural unit B to obtain a polyimide resin precursor having a polyamic acid structure. More specifically, a preferred method for producing a polyimide resin precursor is a production method in which a tetracarboxylic acid component containing a compound represented by formula (a1) is reacted with a diamine component containing at least one selected from the group consisting of a compound represented by formula (b1), a compound represented by formula (b2), and a compound represented by formula (b3), to obtain a polyimide resin precursor having a polyamic acid structure.

[0025] The tetracarboxylic acid component used in this production method includes a compound that provides the structural unit (A1), and may also include a tetracarboxylic acid component other than the compound that provides the structural unit (A1), as long as the effects of the present invention are not impaired. The diamine component used in this production method preferably includes at least one selected from the group consisting of a compound that provides the structural unit (B1), a compound that provides the structural unit (B2), and a compound that provides the structural unit (B3), and may also include a diamine component other than the compound that provides the structural unit (B1), the compound that provides the structural unit (B2), and the compound that provides the structural unit (B3), as long as the effects of the present invention are not impaired. The amount of the diamine component relative to the tetracarboxylic acid component is preferably 0.9 to 1.1 moles.

[0026] The method for reacting the tetracarboxylic acid component and the diamine component in this production method is not particularly limited, and known methods can be used. Specific reaction methods include charging a reactor with the tetracarboxylic acid component, the diamine component, a solvent, and, if necessary, an end-capping agent, and stirring the mixture for 1 to 72 hours at a temperature preferably in the range of 0 to 120°C, more preferably 5 to 80°C. When the reaction is carried out at 80°C or below, the molecular weight of the polyimide resin precursor does not vary depending on the temperature history during polymerization, and the progress of thermal imidization can be suppressed, allowing for stable production of a polyimide resin precursor having a polyamic acid structure.

[0027] The above method provides a polyimide resin precursor solution having a polyamic acid structure dissolved in a solvent. The concentration of the polyimide resin precursor in the resulting solution is preferably 1 to 50% by mass, more preferably 3 to 35% by mass, and even more preferably 5 to 30% by mass. Next, the raw materials used in this production method will be described.

[0028] [Tetracarboxylic Acid Component] The tetracarboxylic acid component used as a raw material in the present production method is preferably the tetracarboxylic acid dianhydride described above in the section <Structural Unit (A)>. The tetracarboxylic acid dianhydride used as the tetracarboxylic acid component in the present production method may be in the form of a dianhydride, a tetracarboxylic acid (free acid), or an alkyl ester of a tetracarboxylic acid, but is preferably a dianhydride. The tetracarboxylic acid component used as a raw material in the present production method includes a compound represented by formula (a1) (a compound that provides structural unit (A1)). The ratio of the compound represented by formula (a1) in the tetracarboxylic acid component is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, and even more preferably 95 to 100 mol. It may even be 100 mol, and the tetracarboxylic acid component may consist solely of the compound represented by formula (a1). By ensuring that the ratio of the compound represented by formula (a1) is within the above range, the heat resistance of the resulting polyimide resin is excellent, and the coatability of the precursor varnish and the adhesion of the polyimide resin are also improved.

[0029] The tetracarboxylic acid component may consist solely of the compound represented by formula (a1), or may contain a tetracarboxylic acid component other than the compound represented by formula (a1). As the tetracarboxylic acid component other than the compound represented by formula (a1), preferably, it further contains at least one selected from the group consisting of a compound represented by the following formula (a3) ​​and a compound represented by the following formula (a4), more preferably, it contains a compound represented by the following formula (a3).

[0030] The compound represented by formula (a3) ​​is pyromellitic anhydride (PMDA). When the tetracarboxylic acid component contains a compound represented by formula (a3), the heat resistance of the resulting polyimide resin can be enhanced while maintaining good coatability of the resulting varnish and good adhesion of the polyimide resin. The compound represented by formula (a4) is 4,4-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl (BP-TME). When the tetracarboxylic acid component contains a compound represented by formula (a4), the heat resistance of the resulting polyimide resin can be enhanced while maintaining good coatability of the resulting varnish and good adhesion of the polyimide resin.

[0031] The molar ratio of the compound represented by formula (a1) to the compound represented by formula (a3) ​​and the compound represented by formula (a4) in the structural unit A [(a1) / ((a3)+(a4))] is preferably 30 / 70 to 100 / 0, more preferably 40 / 60 to 100 / 0, even more preferably 50 / 50 to 100 / 0, still more preferably 60 / 40 to 100 / 0, still more preferably 60 / 40 to 90 / 10, and still more preferably 60 / 40 to 80 / 20. When the molar ratio of the compound represented by formula (a1) to the compound represented by formula (a3) ​​and the compound represented by formula (a4) is 100 / 0, the tetracarboxylic acid component does not include the compound represented by formula (a3) ​​and the compound represented by formula (a4).

[0032] The molar ratio [(a1) / (a3)] of the compound represented by formula (a1) to the compound represented by formula (a3) ​​in the tetracarboxylic acid component is preferably 30 / 70 to 100 / 0, more preferably 40 / 60 to 100 / 0, even more preferably 40 / 60 to 90 / 10, still more preferably 40 / 60 to 80 / 20, even more preferably 40 / 60 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. When the molar ratio of the compound represented by formula (a1) to the compound represented by formula (a3) ​​is 100 / 0, the tetracarboxylic acid component does not contain the compound represented by formula (a3). When the tetracarboxylic acids constituting the tetracarboxylic acid component are in the above molar ratio, the heat resistance of the polyimide resin can be enhanced while maintaining good varnish coatability and polyimide resin adhesion.

[0033] The tetracarboxylic acid component may contain a tetracarboxylic acid component other than the compound represented by formula (a1), the compound represented by formula (a3), and the compound represented by formula (a4). Examples of such a tetracarboxylic acid component include, but are not limited to, aromatic tetracarboxylic acid dianhydrides other than the compound represented by formula (a1), the compound represented by formula (a3), and the compound represented by formula (a4), alicyclic tetracarboxylic acid dianhydrides, and aliphatic tetracarboxylic acid dianhydrides. When the tetracarboxylic acid component contains a tetracarboxylic acid component other than the compound represented by formula (a1), the compound represented by formula (a3), and the compound represented by formula (a4), it is preferable to contain an aromatic tetracarboxylic acid dianhydride among tetracarboxylic acid dianhydrides other than the compound represented by formula (a1), the compound represented by formula (a3), and the compound represented by formula (a4). Examples of aromatic tetracarboxylic dianhydrides include 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride (BPF-PA), 2,3,6,7-naphthalene tetracarboxylic 2,3:6,7-dianhydride (NTCDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 9,9-bis(trifluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic dianhydride (6FCDA), 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]hexafluoropropane dianhydride, and 4,4'-oxydiphthalic anhydride (ODPA). Examples of suitable dianhydrides include 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), hydroquinone diphthalic anhydride (HQDEA), ethylene glycol bis(trimellitate) dianhydride (TMEG), and p-phenylene bis(trimellitate) dianhydride (TAHQ). Of these, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) is preferred.Examples of alicyclic tetracarboxylic dianhydrides include cyclohexane-1,2,4,5-tetracarboxylic dianhydride (HPMDA), cyclohexane-1,2,3,4-tetracarboxylic dianhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5',6,6'-tetracarboxylic dianhydride (CpODA), 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopent ... Examples of the aliphatic tetracarboxylic dianhydride include 1,2,4,5-cyclopentanetetracarboxylic dianhydride, 3,3',4,4'-bicyclohexyltetracarboxylic dianhydride, 2,2-propylidene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, and bicyclo[4.4.0]decane-2,3,6,7-tetracarboxylic acid dianhydride. Examples of the aliphatic tetracarboxylic dianhydride include 1,2,3,4-butanetetracarboxylic acid dianhydride. These tetracarboxylic acid dianhydrides may be used alone or in combination of two or more.

[0034] [Diamine Component] The diamine component used as a raw material in this production method is preferably the diamine described above in the section <Structural Unit (B)>. The diamine used as the diamine component in this production method may be in the form of either a diamine or a diisocyanate corresponding to the diamine, but is preferably a diamine. The diamine component used as a raw material in this production method includes at least one selected from the group consisting of the compound represented by formula (b1) (a compound that provides structural unit (B1)), the compound represented by formula (b2) (a compound that provides structural unit (B2)), and the compound represented by formula (b3) (a compound that provides structural unit (B3)), preferably at least one selected from the group consisting of the compound represented by formula (b1) and the compound represented by formula (b2), and more preferably the compound represented by formula (b1). The diamine component may include two or three of the compounds represented by formula (b1), (b2), and (b3). The total ratio of the compound represented by formula (b1), the compound represented by formula (b2), and the compound represented by formula (b3) in the diamine component is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the diamine component may consist of only at least one selected from the group consisting of the compound represented by formula (b1), the compound represented by formula (b2), and the compound represented by formula (b3). The ratio of the compound represented by formula (b1) in the diamine component is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the diamine component may consist of only the compound represented by formula (b1). The ratio of the compound represented by formula (b2) in the diamine component is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, and still more preferably 95 to 100 mol, and may be 100 mol, and the diamine component may consist solely of the compound represented by formula (b2).The ratio of the compound represented by formula (b3) in the diamine component is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, and still more preferably 95 to 100 mol, or even 100 mol, and the diamine component may consist solely of the compound represented by formula (b3). When the ratios of the compound represented by formula (b1), the compound represented by formula (b2), and the compound represented by formula (b3) are within the above ranges, the obtained polyimide resin has excellent heat resistance, and further, the coatability of the precursor varnish and the adhesion of the polyimide resin can be improved.

[0035] The diamine component may contain a diamine component other than the compound represented by formula (b1), the compound represented by formula (b2), and the compound represented by formula (b3). Examples of such diamine components include, but are not limited to, aromatic diamines, alicyclic diamines, and aliphatic diamines excluding any of the compounds represented by formula (b1), the compounds represented by formula (b2), and the compounds represented by formula (b3). Examples of aromatic diamines include 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (2,2'-TFMB), 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-5,5'-diaminobiphenyl, 2,2-bis(4-aminophenyl)hexafluoropropane (H FDA), 2,2-bis(3-amino-4-methylphenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP), 4,4'-diaminodiphenyl ether (4,4'-ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (DDM), 4,4'-diaminodiphenyl sulfone (4,4'-DDS), 3,3'-diaminodiphenyl Sulfone (3,3'-DDS), 4,4'-diamino-2,2'-dimethylbiphenyl (mTB), 9,9-bis(4-aminophenyl)fluorene (BAFL), 4,4'-diaminobiphenyl (benzidine), 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diaminodiphenyl sulfide, 4,4'-diaminobenzophenone, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane Benzene, 5-amino-1,3,3-trimethyl-1-(4-aminophenyl)-indan (5-TMDM), 6-amino-1,3,3-trimethyl-1-(4-aminophenyl)-indan (6-TMDM), 1,3-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,3-bis(4-amino-α,α-dimethylbenzyl)benzene (BisAM), 1,4-bis(4-amino-α,α-dimethylbenzyl)benzene (BisAP), 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl (BODA), 1,1-bis[4-(4-aminophenoxy)phenyl]cyclohexane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 1,4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]ketone, bis[ [4-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4-diaminobenzanilide, 4-aminobenzoate-4-aminophenyl, 3,4-diaminobenzanilide, and the like. Examples of alicyclic diamines include 1,3-bis(aminomethyl)cyclohexane (1,3-BAC), 1,4-bis(aminomethyl)cyclohexane, 1,3-cyclohexyldiamine, 1,4-cyclohexyldiamine, isophoronediamine, bis(aminomethyl)norbornane, 4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexyl ether, and 2,2-bis(4-aminocyclohexyl)propane. Examples of aliphatic diamines include ethylenediamine and hexamethylenediamine. One or more diamines may be used.

[0036] [End-capping Agent] In addition to the tetracarboxylic acid component and diamine component described above, an end-capping agent may also be used in the production of the polyimide resin precursor. Monoamines or dicarboxylic acids are preferred as end-capping agents, with monoamines being more preferred. Using monoamines as end-capping agents can improve the heat resistance of the polyimide resin while maintaining good varnish application properties and adhesion to the polyimide resin. The amount of the end-capping agent introduced is preferably 0.0001 to 0.2 mol, more preferably 0.0001 to 0.1 mol, even more preferably 0.001 to 0.06 mol, and even more preferably 0.01 to 0.06 mol, per mol of the tetracarboxylic acid component. From the viewpoint of heat resistance, the amount of the end-capping agent introduced is preferably 0.001 to 0.2 mol, more preferably 0.01 to 0.2 mol, even more preferably 0.06 to 0.2 mol, and even more preferably 0.1 to 0.2 mol, per mol of the tetracarboxylic acid component. Examples of monoamine end-capping agents include methylamine, ethylamine, propylamine, butylamine, benzylamine, 4-methylbenzylamine, 4-ethylbenzylamine, 4-dodecylbenzylamine, 3-methylbenzylamine, 3-ethylbenzylamine, aniline, 3-methylaniline, 4-methylaniline, o-aminophenol (2-aminophenol), m-aminophenol (3-aminophenol), p-aminophenol (4-aminophenol), o-aminobenzoic acid, m-aminobenzoic acid, and p-aminobenzoic acid. Of these, benzylamine, aniline, and p-aminophenol (4-aminophenol) are preferred, with p-aminophenol (4-aminophenol) being more preferred. Examples of dicarboxylic acid end-capping agents include dicarboxylic acids, which may be partially ring-closed. Examples include phthalic acid, phthalic anhydride, 4-chlorophthalic acid, tetrafluorophthalic acid, 2,3-benzophenonedicarboxylic acid, 3,4-benzophenonedicarboxylic acid, cyclopentane-1,2-dicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, etc. Of these, phthalic acid and phthalic anhydride are more preferred.

[0037] [Solvent (Organic Solvent)] The solvent (organic solvent) used in the production of the polyimide resin precursor may be any solvent capable of dissolving the resulting polyimide resin precursor. Examples thereof include aprotic solvents, phenolic solvents, ether solvents, and carbonate solvents, with aprotic solvents being preferred.

[0038] Specific examples of aprotic solvents include amide solvents, lactone solvents, phosphorus-containing amide solvents, sulfur-containing solvents, ketone solvents, and ester solvents, among which amide solvents or lactone solvents are preferred, and amide solvents are more preferred. Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-methylcaprolactam, 1,3-dimethyl-2-imidazolidinone (1,3-dimethylimidazolidinone), tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, etc., and at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone and N-methyl-2-pyrrolidone is preferred, with N-methyl-2-pyrrolidone being more preferred in terms of resin solubility, and 1,3-dimethyl-2-imidazolidinone being more preferred in terms of obtaining a resin with high heat resistance. Examples of the lactone solvent include γ-butyrolactone and γ-valerolactone, and γ-butyrolactone is preferred. Examples of phosphorus-containing amide solvents include hexamethylphosphoric amide and hexamethylphosphine triamide. Examples of sulfur-containing solvents include dimethyl sulfone, dimethyl sulfoxide, and sulfolane. Examples of ketone solvents include acetone, methyl ethyl ketone, cyclohexanone, methylcyclohexanone, and cyclopentanone. Examples of ester solvents include 2-methoxy-1-methylethyl acetate.

[0039] Examples of phenol-based solvents include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol. Examples of ether-based solvents include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, 1,4-dioxane, and propylene glycol monomethyl ether. Examples of carbonate-based solvents include diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, and propylene carbonate. Among the above solvents, it is preferable to contain at least one selected from the group consisting of amide solvents and lactone solvents, with an amide solvent or a lactone solvent being preferred, and at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, and γ-butyrolactone being preferred. From the viewpoint of resin solubility, at least one selected from the group consisting of N-methyl-2-pyrrolidone and γ-butyrolactone is more preferred, with N-methyl-2-pyrrolidone or γ-butyrolactone being even more preferred, and γ-butyrolactone being even more preferred. Furthermore, from the viewpoint of obtaining a resin with high heat resistance, it is more preferable to contain at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone and γ-butyrolactone, with 1,3-dimethyl-2-imidazolidinone or γ-butyrolactone being even more preferred, and γ-butyrolactone being even more preferred. The above solvents may be used alone or in combination of two or more. In view of the above, the organic solvent preferably contains at least one selected from the group consisting of amide solvents and lactone solvents, more preferably contains at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, and γ-butyrolactone, even more preferably contains at least one selected from the group consisting of N-methyl-2-pyrrolidone and γ-butyrolactone, and still more preferably contains γ-butyrolactone.

[0040] [Varnish] The varnish of the present invention contains the polyimide resin precursor and an organic solvent, that is, the polyimide resin precursor is dissolved in the organic solvent.

[0041] The organic solvent is not particularly limited as long as it dissolves the polyimide resin precursor, but the compounds described above as solvents used in producing the polyimide resin precursor (solvents described in the section [Solvent (organic solvent)]) are preferred, and more preferred solvents are also the same. Specific examples include aprotic solvents, phenolic solvents, ether solvents, and carbonate solvents, with aprotic solvents being preferred.

[0042] Specific examples of the aprotic solvent include amide solvents, lactone solvents, phosphorus-containing amide solvents, sulfur-containing solvents, ketone solvents, and ester solvents, with amide solvents or lactone solvents being preferred, and amide solvents being more preferred. Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-methylcaprolactam, 1,3-dimethyl-2-imidazolidinone (1,3-dimethylimidazolidinone), tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, and 3-butoxy-N,N-dimethylpropanamide, with at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone and N-methyl-2-pyrrolidone being preferred, with N-methyl-2-pyrrolidone being more preferred from the viewpoint of resin solubility. Furthermore, from the viewpoint of obtaining a resin with high heat resistance, 1,3-dimethyl-2-imidazolidinone, which was used in the production of the precursor, is more preferred. Examples of lactone solvents include γ-butyrolactone and γ-valerolactone, with γ-butyrolactone being preferred. Examples of phosphorus-containing amide solvents include hexamethylphosphoric amide and hexamethylphosphine triamide. Examples of sulfur-containing solvents include dimethyl sulfone, dimethyl sulfoxide, and sulfolane. Examples of ketone solvents include acetone, methyl ethyl ketone, cyclohexanone, methylcyclohexanone, and cyclopentanone. Examples of ester solvents include 2-methoxy-1-methylethyl acetate.

[0043] Examples of phenol-based solvents include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol. Examples of ether-based solvents include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, 1,4-dioxane, and propylene glycol monomethyl ether. Examples of carbonate-based solvents include diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, and propylene carbonate. Among the above organic solvents, at least one selected from the group consisting of amide solvents and lactone solvents is preferred, with an amide solvent or a lactone solvent being preferred, at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, and γ-butyrolactone being preferred, at least one selected from the group consisting of N-methyl-2-pyrrolidone and γ-butyrolactone being more preferred, N-methyl-2-pyrrolidone or γ-butyrolactone being even more preferred, and γ-butyrolactone being even more preferred. From the viewpoint of obtaining a resin with high heat resistance, among the above organic solvents, at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone and γ-butyrolactone used in the production of the precursor is more preferred, with 1,3-dimethyl-2-imidazolidinone or γ-butyrolactone being even more preferred, and γ-butyrolactone being even more preferred. The above organic solvents may be used alone or in combination of two or more. In view of the above, the organic solvent preferably contains at least one selected from the group consisting of amide solvents and lactone solvents, more preferably contains at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, and γ-butyrolactone, even more preferably contains at least one selected from the group consisting of N-methyl-2-pyrrolidone and γ-butyrolactone, and still more preferably contains γ-butyrolactone.From the viewpoint of obtaining a resin with high heat resistance, the organic solvent more preferably contains at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone and γ-butyrolactone used in producing the precursor, further preferably contains 1,3-dimethyl-2-imidazolidinone or γ-butyrolactone, and still further preferably contains γ-butyrolactone.

[0044] The varnish of the present invention may be the above-mentioned polyimide resin precursor solution itself after the production of the polyimide resin precursor, or may be a solution obtained by further diluting the polyimide resin precursor solution by mixing it with an organic solvent.

[0045] The varnish of the present invention may further contain an imidization catalyst and a dehydration catalyst from the viewpoint of efficiently promoting the imidization of the polyamic acid moiety of the polyimide resin precursor of the present invention. The imidization catalyst is preferably an imidization catalyst having a boiling point of 40°C or higher. An imidization catalyst having a boiling point of 40°C or higher allows the imidization to proceed sufficiently before volatilization. Examples of imidization catalysts include amine compounds such as pyridine and picoline; imidazole compounds such as imidazole, 1,2-dimethylimidazole, 1-benzylimidazole, 1-benzyl-2-methylimidazole, and benzimidazole; and the like. The above imidization catalysts may be used alone or in combination of two or more. Examples of dehydration catalysts include acid anhydrides such as acetic anhydride, propionic anhydride, n-butyric anhydride, benzoic anhydride, and trifluoroacetic anhydride; and carbodiimide compounds such as dicyclohexylcarbodiimide. These may be used alone or in combination of two or more.

[0046] The polyimide resin precursor contained in the varnish of the present invention is solvent-soluble, allowing for the production of a high-concentration varnish that is stable at room temperature. The varnish of the present invention preferably contains 3 to 40% by mass of the polyimide resin precursor, more preferably 5 to 30% by mass. The viscosity of the varnish is preferably 0.1 to 100 Pa·s, more preferably 0.1 to 20 Pa·s. The viscosity of the varnish is measured at 25°C using an E-type viscometer. The varnish of the present invention may also contain various additives, such as inorganic fillers, adhesion promoters, release agents, flame retardants, UV stabilizers, surfactants, leveling agents, defoamers, fluorescent brighteners, crosslinking agents, polymerization initiators, and photosensitizers, as long as they do not impair the required properties of the resulting polyimide resin and polyimide film. The method for producing the varnish of the present invention is not particularly limited, and known methods can be used. For example, the varnish can be obtained by adjusting the concentration by adding an additional solvent, as needed, to the solution of the polyimide resin precursor obtained by the above-mentioned production method.

[0047] [Polyimide Film and Method for Producing Polyimide Film] The polyimide film of the present invention is preferably produced by using the varnish described above. The polyimide film of the present invention is obtained by imidizing the polyimide resin precursor described above.

[0048] The method for producing a polyimide film using the varnish of the present invention is not particularly limited, and known methods can be used. For example, the varnish of the present invention is applied to a smooth support such as a glass plate, a metal plate, or a plastic plate, or formed into a film, and then the organic solvents contained in the varnish, such as the reaction solvent and dilution solvent, are removed by heating to obtain a polyamic acid film. The polyamic acid in the polyamic acid film is imidized (dehydration ring closure) by heating, and then peeled off from the support to produce a polyimide film. Since the polyimide film of the present invention is suitable for use as an insulating film in the semiconductor field, silicon, silicon nitride, silicon oxide, etc. are preferred as the support, with silicon being more preferred. That is, the polyimide film of the present invention is preferably a film obtained by applying the above-mentioned varnish to a support and heating it, and the method for producing the polyimide film of the present invention is preferably a method in which the above-mentioned varnish is applied to a support and heated.

[0049] The heating temperature when drying a varnish containing a polyimide resin precursor to obtain a polyimide resin precursor (polyamic acid) film is preferably 50 to 150°C. The heating temperature when imidizing the polyimide resin precursor by heating is preferably 300 to 420°C, more preferably 350 to 400°C. The heating time is preferably 1 minute to 6 hours, more preferably 5 minutes to 2 hours, and even more preferably 15 minutes to 1 hour. By using such a temperature and time, the physical properties of the resulting polyimide film are improved. Examples of the heating atmosphere include air gas, nitrogen gas, oxygen gas, hydrogen gas, and a nitrogen / hydrogen mixed gas. However, to suppress discoloration of the resulting polyimide resin, nitrogen gas with an oxygen concentration of 100 ppm or less and a nitrogen / hydrogen mixed gas containing hydrogen at a concentration of 0.5% or less are preferred. The imidization method is not limited to thermal imidization; chemical imidization can also be used.

[0050] The thickness of the polyimide film of the present invention can be appropriately selected depending on the application, etc., but is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 1 μm or more, even more preferably 5 μm or more, and even more preferably 7 μm or more. It is also preferably 250 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, and even more preferably 20 μm or less. A thickness within the above range enables practical use as an insulating film. The thickness of the polyimide film can be easily controlled by adjusting the solids concentration and viscosity of the varnish.

[0051] The polyimide film of the present invention preferably has the following physical properties. When the polyimide film of the present invention satisfies the following physical properties, it has excellent heat resistance. The glass transition temperature (Tg) is preferably 320°C or higher, more preferably 330°C or higher, even more preferably 350°C or higher, and still more preferably 400°C or higher. The 5% weight loss temperature (Td5%) is preferably 500°C or higher, more preferably greater than 500°C. The above-mentioned physical properties in the present invention can be specifically measured by the methods described in the examples.

[0052] The polyimide film of the present invention has the excellent properties described above and can be used in a variety of applications, and is particularly suitable as a film for various members of semiconductor components, particularly as an insulating film for semiconductors.

[0053] [Polyimide Resin] The polyimide resin of the present invention is a polyimide resin having a structural unit AI derived from a tetracarboxylic dianhydride and a structural unit BI derived from a diamine, in which the structural unit AI includes a structural unit (AI1) derived from a compound represented by the following formula (a1), and the structural unit BI includes at least one structural unit selected from the group consisting of a structural unit (BI1) derived from a compound represented by the following formula (b1), a structural unit (BI2) derived from a compound represented by the following formula (b2), and a structural unit (BI3) derived from a compound represented by the following formula (b3). The polyimide resin of the present invention constitutes the polyimide film described above, and the polyimide film is made of the polyimide resin of the present invention. The polyimide resin of the present invention may be obtained by any production method, but is preferably obtained by a production method in which the polyimide resin precursor described above is imidized.

[0054] The reason why the polyimide resin of the present invention and the polyimide film containing the polyimide resin have excellent heat resistance and adhesion is unclear, but it is thought to be as follows. The polyimide resin and polyimide film of the present invention are thought to have excellent heat resistance because they contain a structure derived from a specific tetracarboxylic dianhydride component having a highly sterically hindered substituent and a flexible moiety, and a structure derived from a specific diamine having an ester skeleton that is highly linear and exhibits relatively low water absorption. Furthermore, because they contain the above structure, the polyimide resin and polyimide film of the present invention are thought to be less likely to absorb moisture that inhibits adhesion. As described above, it is thought that the polyimide resin and polyimide film of the present invention have excellent heat resistance and adhesion.

[0055] <Structural units of polyimide resin> The structural units constituting the polyimide resin of the present invention are the same as the structural units described in the section [Polyimide resin precursor]. That is, the polyimide resin has a structural unit AI derived from a tetracarboxylic dianhydride and a structural unit BI derived from a diamine. In the polyimide resin, the structural unit AI and the structural unit BI form an imide structure.

[0056] (Structural Unit AI) The structural unit AI includes a structural unit (AI1) derived from a compound represented by the following formula (a1): When the structural unit AI includes the structural unit (AI1), the adhesion of the polyimide resin can be improved.

[0057] The compound represented by formula (a1) is 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA). When the structural unit AI includes the structural unit (AI1), the polyimide resin exhibits excellent heat resistance and can also have improved adhesion.

[0058] The proportion of the structural unit (AI1) within the structural unit AI is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, and still more preferably 95 to 100 mol; it may even be 100 mol, and the structural unit AI may consist solely of the structural unit (AI1). By ensuring that the proportion of the structural unit (AI1) is within the above range, the polyimide resin will have excellent heat resistance and improved adhesion.

[0059] The structural unit AI may consist solely of the structural unit (AI1), or may include a structural unit other than the structural unit (AI1), and preferably further includes at least one structural unit selected from the group consisting of the structural unit (AI3) derived from a compound represented by the following formula (a3) ​​and the structural unit (AI4) derived from a compound represented by the following formula (a4), and more preferably includes the structural unit (AI3) derived from a compound represented by the following formula (a3). That is, the structural unit AI includes at least one selected from the group consisting of the structural unit (AI3) derived from a compound represented by the formula (a3) ​​and the structural unit (AI4) derived from a compound represented by the formula (a4), and the structural unit (AI1) derived from a compound represented by the formula (a1), or is composed solely of the structural unit (AI1).

[0060] The compound represented by formula (a3) ​​is pyromellitic anhydride (PMDA). When the structural unit A contains the structural unit (AI3), the heat resistance of the polyimide resin can be enhanced while maintaining favorable varnish coatability and polyimide resin adhesion. The compound represented by formula (a4) is 4,4-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl (BP-TME). When the structural unit AI contains the structural unit (AI4), the heat resistance of the polyimide resin can be enhanced while maintaining favorable varnish coatability and polyimide resin adhesion.

[0061] The molar ratio of the structural unit (AI1) to the total of the structural unit (AI3) and the structural unit (AI4) in the structural unit AI [(AI1) / ((AI3)+(AI4))] is preferably 30 / 70 to 100 / 0, more preferably 40 / 60 to 100 / 0, even more preferably 50 / 50 to 100 / 0, still more preferably 60 / 40 to 100 / 0, still more preferably 60 / 40 to 90 / 10, and even more preferably 60 / 40 to 80 / 20. When the molar ratio of the structural unit (AI1) to the total of the structural unit (AI3) and the structural unit (AI4) is 100 / 0, the structural unit AI does not include the structural unit (AI3) or the structural unit (AI4).

[0062] The molar ratio of the structural unit (AI1) to the structural unit (AI3) in the structural unit AI [(AI1) / (AI3)] is preferably 30 / 70 to 100 / 0, more preferably 40 / 60 to 100 / 0, even more preferably 40 / 60 to 90 / 10, even more preferably 40 / 60 to 80 / 20, even more preferably 40 / 60 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. When the molar ratio of the structural unit (AI1) to the structural unit (AI3) is 100 / 0, the structural unit AI does not contain the structural unit (AI3). By having the structural units constituting the structural unit AI in the above molar ratio, it is possible to improve the heat resistance of the polyimide resin while maintaining good varnish coatability and polyimide resin adhesion.

[0063] The structural unit AI may contain structural units other than the structural units (AI1), (AI3), and (AI4). The tetracarboxylic acid dianhydride that provides such a structural unit is not particularly limited, and examples include aromatic tetracarboxylic acid dianhydrides excluding compounds represented by formula (a1), (a3), and (a4), alicyclic tetracarboxylic acid dianhydrides, and aliphatic tetracarboxylic acid dianhydrides. When the structural unit AI contains structural units other than the structural unit (AI1), (AI3), and (AI4), it is preferable to include an aromatic tetracarboxylic acid dianhydride among tetracarboxylic acid dianhydrides excluding compounds represented by formula (a1), (a3), and (a4). Examples of aromatic tetracarboxylic dianhydrides include 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride (BPF-PA), 2,3,6,7-naphthalene tetracarboxylic 2,3:6,7-dianhydride (NTCDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 9,9-bis(trifluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic dianhydride (6FCDA), 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]hexafluoropropane dianhydride, and 4,4'-oxydiphthalic anhydride (ODPA). Examples of suitable dianhydrides include 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), hydroquinone diphthalic anhydride (HQDEA), ethylene glycol bis(trimellitate) dianhydride (TMEG), and p-phenylene bis(trimellitate) dianhydride (TAHQ). Of these, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) is preferred.Examples of alicyclic tetracarboxylic dianhydrides include cyclohexane-1,2,4,5-tetracarboxylic dianhydride (HPMDA), cyclohexane-1,2,3,4-tetracarboxylic dianhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5',6,6'-tetracarboxylic dianhydride (CpODA), 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopent ... Examples of the aliphatic tetracarboxylic dianhydride include 1,2,4,5-cyclopentanetetracarboxylic dianhydride, 3,3',4,4'-bicyclohexyltetracarboxylic dianhydride, 2,2-propylidene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, and bicyclo[4.4.0]decane-2,3,6,7-tetracarboxylic acid dianhydride. Examples of the aliphatic tetracarboxylic dianhydride include 1,2,3,4-butanetetracarboxylic acid dianhydride. The structural unit AI may optionally contain one type of structural unit or two or more types of structural units.

[0064] (Structural Unit BI) The structural unit BI is a structural unit derived from a diamine. The structural unit BI includes at least one selected from the group consisting of a structural unit (BI1) derived from a compound represented by the following formula (b1), a structural unit (BI2) derived from a compound represented by the following formula (b2), and a structural unit (BI3) derived from a compound represented by the following formula (b3). When the structural unit BI includes one or more of the structural unit (BI1), the structural unit (BI2), and the structural unit (BI3), the adhesion of the polyimide resin can be improved.

[0065] The compound represented by formula (b1) is 4-aminophenyl-4-aminobenzoate (4-BAAB). When the structural unit BI contains the structural unit (BI1), the resulting polyimide resin has excellent heat resistance and can also have improved adhesion. The compound represented by formula (b2) is bis(4-aminophenyl)terephthalate (APTP). When the structural unit BI contains the structural unit (BI2), the resulting polyimide resin has excellent heat resistance and can also have improved adhesion. The compound represented by formula (b3) is 1,4-bis(4-aminobenzoyloxy)benzene. When the structural unit BI contains the structural unit (BI3), the resulting polyimide resin has excellent heat resistance and can also have improved adhesion. The structural unit BI includes at least one selected from the group consisting of the structural unit (BI1), the structural unit (BI2), and the structural unit (BI3), preferably includes at least one selected from the group consisting of the structural unit (BI1) and the structural unit (BI2), and more preferably includes the structural unit (BI1).

[0066] The total ratio of the structural unit (BI1), the structural unit (BI2), and the structural unit (BI3) in the structural unit BI is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the structural unit BI may consist of only at least one selected from the group consisting of the structural unit (BI1), the structural unit (BI2), and the structural unit (BI3). The ratio of the structural unit (BI1) in the structural unit BI is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the structural unit BI may consist of only the structural unit (BI1). The ratio of the structural unit (BI2) within the structural unit BI is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the structural unit BI may consist solely of the structural unit (BI2). The ratio of the structural unit (BI3) within the structural unit BI is preferably 30 to 100 mol, more preferably 70 to 100 mol, even more preferably 90 to 100 mol, still more preferably 95 to 100 mol, or even 100 mol, and the structural unit BI may consist solely of the structural unit (BI3). When the ratios of the structural units (BI1), (BI2), and (BI3) are within the above ranges, the resulting polyimide resin has excellent heat resistance and the adhesion of the polyimide resin can also be improved.

[0067] The structural unit BI may contain structural units other than the structural units (BI1), (BI2), and (BI3). Diamines that provide such structural units are not particularly limited, but include aromatic diamines, alicyclic diamines, and aliphatic diamines excluding the compounds represented by formula (b1), (b2), and (b3). Examples of aromatic diamines include 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA), 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (2,2'-TFMB), 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-5,5'-diaminobiphenyl, 2,2-bis(4-aminophenyl)hexafluoropropane (HFDA), 2 , 2-bis(3-amino-4-methylphenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP), 4,4'-diaminodiphenyl ether (4,4'-ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (DDM), 4,4'-diaminodiphenyl sulfone (4,4'-DDS), 3,3'-diaminodiphenyl sulfone (3,3'-DDS ), 4,4'-diamino-2,2'-dimethylbiphenyl (mTB), 9,9-bis(4-aminophenyl)fluorene (BAFL), 4,4'-diaminobiphenyl (benzidine), 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diaminodiphenyl sulfide, 4,4'-diaminobenzophenone, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 5-amino-1,3,3-trimethyl -1-(4-aminophenyl)-indan (5-TMDM), 6-amino-1,3,3-trimethyl-1-(4-aminophenyl)-indan (6-TMDM), 1,3-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,3-bis(4-amino-α,α-dimethylbenzyl)benzene (BisAM), 1,4-bis(4-amino-α,α-dimethylbenzyl)benzene (BisAP), 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl (BODA), 1,1-bis[4-(4-aminophenoxy)phenyl]cyclohexane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 1,4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone [4-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4-diaminobenzanilide, 4-aminobenzoate-4-aminophenyl, 3,4-diaminobenzanilide, and the like. Examples of alicyclic diamines include 1,3-bis(aminomethyl)cyclohexane (1,3-BAC), 1,4-bis(aminomethyl)cyclohexane, 1,3-cyclohexyldiamine, 1,4-cyclohexyldiamine, isophoronediamine, bis(aminomethyl)norbornane, 4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexyl ether, and 2,2-bis(4-aminocyclohexyl)propane. Examples of aliphatic diamines include ethylenediamine and hexamethylenediamine. The structural units other than the structural units (BI1), (BI2), and (BI3) optionally contained in the structural unit BI may be of one type or two or more types.

[0068] The polyimide resin of the present invention may contain a structure other than a polyimide chain (a structure formed by imide bonding between the structural unit AI and the structural unit BI) as long as it does not impair the present invention. Examples of structures other than polyimide chains that can be contained in the polyimide resin include structures containing amide bonds. The polyimide resin of the present invention preferably contains a polyimide chain (a structure formed by imide bonding between the structural unit AI and the structural unit BI) as its main structure. Therefore, the proportion of polyimide chains in the polyimide resin of the present invention is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and even more preferably 100% by mass.

[0069] The polyimide resin of the present invention preferably has the following physical properties. When the polyimide resin of the present invention satisfies the following physical properties, it has excellent heat resistance. The glass transition temperature (Tg) is preferably 400°C or higher, more preferably 410°C or higher, even more preferably 420°C or higher, still more preferably 430°C or higher, still more preferably 440°C or higher, and still more preferably 450°C or higher. The 5% weight loss temperature (Td5%) is preferably 500°C or higher, more preferably greater than 500°C. The above-mentioned physical properties in the present invention can be specifically measured by the methods described in the examples.

[0070] The polyimide resin of the present invention has the excellent properties described above and can be used in various applications, and is particularly suitable as a resin for various members of semiconductor components, particularly as an insulating film for semiconductors.

[0071] [Polyimide Film Made from Polyimide Resin] The present invention also includes a polyimide film made from the polyimide resin of the present invention. As described above, the polyimide film made from the polyimide resin of the present invention is preferably obtained by a production method involving imidizing the polyimide resin precursor. The thickness of the polyimide film made from the polyimide resin of the present invention can be appropriately selected depending on the application, etc., but is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 1 μm or more, still more preferably 5 μm or more, and even more preferably 7 μm or more. It is also preferably 250 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, and even more preferably 20 μm or less. A thickness within the above range enables practical use as an insulating film. The thickness of the polyimide film can be easily controlled by adjusting the solids concentration and viscosity of the varnish. The preferred physical properties of the polyimide film made from the polyimide resin of the present invention are as follows. By satisfying the following physical properties, the polyimide film has excellent heat resistance. The glass transition temperature (Tg) is preferably 400°C or higher, more preferably 410°C or higher, even more preferably 420°C or higher, still more preferably 430°C or higher, still more preferably 440°C or higher, and still more preferably 450°C or higher. The 5% weight loss temperature (Td5%) is preferably 500°C or higher, more preferably greater than 500°C. The above-mentioned physical property values ​​in the present invention can be specifically measured by the method described in the Examples. Because of the excellent properties described above, the polyimide film made of the polyimide resin of the present invention can be used for various applications, and is particularly suitable as a film for various members of semiconductor components. In particular, it is particularly suitable for use as an insulating film for semiconductors.

[0072] The present invention will be specifically described below with reference to examples, although the present invention is not limited to these examples in any way.

[0073] <Physical Properties and Evaluation of Varnish and Polyimide Film> The physical properties and evaluation of the varnishes and polyimide films obtained in the Examples and Comparative Examples were performed using the methods described below. (1) Rinsing Suitability (Evaluation of Coating Suitability) PGME (propylene glycol monomethyl ether), cyclohexanone, or cyclopentanone, a rinse solvent, was added to the varnishes obtained in the Examples and Comparative Examples, and the presence or absence of precipitation of the polyimide resin precursor was visually evaluated. The ratio of varnish to rinse solvent (varnish / rinse solvent) used in the evaluation was 1 / 99 (volume / volume). A homogeneous solution in which the polyimide resin precursor dissolved was rated as having rinsing suitability, while a non-uniform dispersion in which the polyimide resin precursor precipitated was rated as not having rinsing suitability. Rinsing suitability indicates excellent coatability. Furthermore, rinsing suitability with a wider range of solvents indicates better coatability. (2) Film Thickness Film thickness was measured using a digital gauge SA-S110 / 03N manufactured by Citizen Finedevices Co., Ltd. (3) Glass Transition Temperature (Tg) (Evaluation of Heat Resistance) Using a Hitachi High-Tech Science Corporation thermomechanical analyzer "TMA 7100C," TMA measurements were performed using a sample size of 4 mm x 20 mm, tension mode, a load of 50 mN, and a heating rate of 10°C / min, raising the temperature from 40°C to 500°C. The point at which an inflection point was observed was extrapolated to determine the glass transition temperature (Tg). The higher the glass transition temperature (Tg), the better the heat resistance. (4) 5% Weight Loss Temperature (Td5%) (Evaluation of Heat Resistance) Measurements were performed using a Hitachi High-Tech Science Corporation thermogravimetric and differential thermal analyzer "NEXTA STA200RV." The sample was heated from 40 to 150°C at a heating rate of 10°C / min, held at 150°C for 30 minutes to remove moisture, and then heated to 500°C. The temperature at which the weight decreased by 5% compared to the weight after holding at 150°C for 30 minutes was defined as the 5% weight loss temperature. The higher the weight loss temperature, the better the heat resistance. In Table 1, ">500" indicates that when the temperature was raised to 500°C, the weight loss did not reach 5% and the 5% weight loss temperature exceeded 500°C. (5) Cross-cut test (evaluation of adhesion) A cross-cut test was performed under the following conditions in accordance with ASTM D3359 to evaluate adhesion.A polyimide layer (polyimide film) was obtained on a 4-inch silicon wafer by the method described in the Examples. Using a cutter knife, the polyimide layer was cut into a grid of 100 squares (each square being 1 mm x 1 mm), which served as the grid portion (cross-cut portion). Tape (Cellotape (registered trademark), CT-24, manufactured by Nichiban Co., Ltd.) was applied to the entire surface of the grid portion (cross-cut portion). The applied tape was peeled off within 0.5 to 1 second. Thereafter, the number of squares of the polyimide layer remaining in the grid portion was counted. The greater the number of squares of the polyimide layer remaining after peeling off the tape, the better the adhesion.

[0074] The tetracarboxylic acid components and diamine components used in the examples and comparative examples, as well as their abbreviations, are as follows: <Tetracarboxylic acid components> DSDA: 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (manufactured by ChinaTech Chemical (Tianjin) Co., Ltd.; compound represented by formula (a1)) PMDA: pyromellitic anhydride (compound represented by formula (a3)) 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (manufactured by Daikin Industries, Ltd.) s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride (manufactured by Mitsubishi Chemical Corporation) ODPA: 4,4'-oxydiphthalic anhydride (manufactured by Manac Corporation) <Diamine components> 4-BAAB: 4-aminophenyl-4-aminobenzoate (manufactured by Nihon Junryo Pharmaceutical Co., Ltd.; compound represented by formula (b1)) <End-capping agent> 4-aminophenol

[0075] The abbreviations for the solvents used in the examples and comparative examples are as follows: NMP: N-methyl-2-pyrrolidone (manufactured by Tokyo Pure Chemical Industries, Ltd.) GBL: γ-butyrolactone (manufactured by Mitsubishi Chemical Corporation) DMI: 1,3-dimethyl-2-imidazolidinone (manufactured by Mitsui Chemicals, Inc.)

[0076] Example 1: 22.825 g (0.100 mol) of 4-BAAB and 187.690 g of NMP were added to a 500 mL five-neck round-bottom flask equipped with a stainless steel half-moon stirring blade, a nitrogen inlet tube, a Dean-Stark condenser, a thermometer, and a glass end cap. The mixture was stirred at 200 rpm under a nitrogen atmosphere at a system temperature of 50°C to obtain a solution. 35.828 g (0.100 mol) of DSDA and 46.922 g of NMP were added all at once to this solution, and the mixture was stirred for 3 hours while maintaining the temperature at 50°C using a mantle heater to obtain a polyamic acid (polyimide resin precursor) varnish with a solids concentration of 20% by mass. The resulting polyamic acid varnish was then applied to a supporting substrate (a 4-inch silicon wafer), held at 80°C for 20 minutes on a hot plate, and then heated to 400°C at a rate of 5°C / min in a nitrogen atmosphere in a hot air dryer, and heated at 400°C for 60 minutes to evaporate the solvent and thermally imidize the film, yielding a polyimide film. The evaluation results of the varnish and film are shown in Table 1.

[0077] Examples 2 to 8 and Comparative Example 3 A polyamic acid (polyimide resin precursor) varnish having a solids concentration of 20% by mass was obtained in the same manner as in Example 1, except that the types of tetracarboxylic acid component, diamine component, and solvent were changed as shown in Table 1. Further, a polyimide film was obtained in the same manner as in Example 1. In Examples 6 and 7, 4-aminophenol was added as an end-capping agent in the amount shown in Table 1 simultaneously with the tetracarboxylic acid component. The evaluation results of the varnish and film are shown in Table 1.

[0078] Comparative Example 1: 22.825 g (0.100 mol) of 4-BAAB and 167.190 g of NMP were added to a 500 mL five-neck round-bottom flask equipped with a stainless steel half-moon stirring blade, a nitrogen inlet tube, a Dean-Stark tube equipped with a condenser, a thermometer, and a glass end cap. The mixture was stirred at 200 rpm under a nitrogen atmosphere at a system temperature of 50°C to obtain a solution. 29.422 g (0.100 mol) of s-BPDA and 41.798 g of NMP were added all at once to this solution, and the mixture was stirred for 3 hours while maintaining the temperature at 50°C using a mantle heater. NMP was then added and the mixture was stirred until homogeneous, yielding a polyamic acid (polyimide resin precursor) varnish with a solids concentration of 10% by mass. The resulting polyamic acid varnish was then applied to a supporting substrate (a 4-inch silicon wafer), held at 80°C for 20 minutes on a hot plate, and then heated to 400°C at a rate of 5°C / min in a nitrogen atmosphere in a hot air dryer, and heated at 400°C for 60 minutes to evaporate the solvent and thermally imidize the film, yielding a polyimide film. The evaluation results of the varnish and film are shown in Table 1.

[0079] Comparative Example 2: 22.825 g (0.100 mol) of 4-BAAB and 172.307 g of NMP were added to a 500 mL five-neck round-bottom flask equipped with a stainless steel half-moon stirring blade, a nitrogen inlet tube, a Dean-Stark tube equipped with a condenser, a thermometer, and a glass end cap, and the mixture was stirred at 200 rpm under a nitrogen atmosphere at a system temperature of 50°C to obtain a solution. 31.021 g (0.100 mol) of ODPA and 43.077 g of NMP were added all at once to this solution, and the mixture was stirred for 3 hours while maintaining the temperature at 50°C using a mantle heater. NMP was then added and the mixture was stirred until homogenous, yielding a polyamic acid (polyimide resin precursor) varnish with a solids concentration of 15% by mass. The resulting polyamic acid varnish was then applied to a supporting substrate (a 4-inch silicon wafer), held at 80°C for 20 minutes on a hot plate, and then heated to 400°C at a rate of 5°C / min in a nitrogen atmosphere in a hot air dryer, and heated at 400°C for 60 minutes to evaporate the solvent and thermally imidize the film, yielding a polyimide film. The evaluation results of the varnish and film are shown in Table 1.

[0080]

[0081] As shown in Table 1, the polyimide resin precursor varnishes of the Examples have good rinsability and therefore excellent coatability. Furthermore, the polyimide films (polyimide resins) obtained from the polyimide resin precursors of the Examples have high glass transition temperatures and 5% weight loss temperatures, indicating excellent heat resistance. Furthermore, they also have excellent adhesion to silicon wafers. From these results, it can be seen that the polyimide resin precursor of the present invention can produce polyimide resins and polyimide films with excellent coatability, heat resistance, and adhesion, and is useful as a raw material in the semiconductor field.

Claims

1. A polyimide resin precursor having a structural unit A derived from a tetracarboxylic dianhydride and a structural unit B derived from a diamine, wherein the structural unit A comprises a structural unit (A1) derived from a compound represented by the following formula (a1), and the structural unit B comprises at least one selected from the group consisting of a structural unit (B1) derived from a compound represented by the following formula (b1), a structural unit (B2) derived from a compound represented by the following formula (b2), and a structural unit (B3) derived from a compound represented by the following formula (b3).

2. The polyimide resin precursor according to claim 1, wherein the ratio of the structural unit (A1) in the structural unit A is 30 to 100 mol %.

3. A polyimide resin precursor according to claim 1 or 2, wherein the total of the proportion of the structural unit (B1), the proportion of the structural unit (B2) and the proportion of the structural unit (B3) in the structural unit B is 30 to 100 mol %.

4. The polyimide resin precursor according to any one of claims 1 to 3, which is a polyamic acid.

5. The polyimide resin precursor according to any one of claims 1 to 4, wherein the structural unit A further comprises at least one selected from the group consisting of a structural unit (A3) derived from a compound represented by the following formula (a3) ​​and a structural unit (A4) derived from a compound represented by the following formula (a4):

6. The polyimide resin precursor according to any one of claims 1 to 5, wherein the molar ratio of the structural unit (A1) to the total of the structural unit (A3) and the structural unit (A4) in the structural unit A, [(A1) / ((A3)+(A4)], is 30 / 70 to 100 / 0.

7. A varnish comprising the polyimide resin precursor according to any one of claims 1 to 6 and an organic solvent.

8. The varnish according to claim 7, wherein the organic solvent contains at least one selected from the group consisting of 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, and γ-butyrolactone.

9. A polyimide film obtained by applying the varnish according to claim 7 or 8 onto a support and heating the applied varnish.

10. A polyimide resin having a structural unit AI derived from a tetracarboxylic dianhydride and a structural unit BI derived from a diamine, wherein the structural unit AI includes a structural unit (AI1) derived from a compound represented by the following formula (a1), and the structural unit BI includes at least one selected from the group consisting of a structural unit (BI1) derived from a compound represented by the following formula (b1), a structural unit (BI2) derived from a compound represented by the following formula (b2), and a structural unit (BI3) derived from a compound represented by the following formula (b3).

11. The polyimide resin according to claim 10, wherein the ratio of the structural unit (AI1) in the structural unit AI is 30 to 100 mol %.

12. The polyimide resin according to claim 10 or 11, wherein the total of the proportion of the structural unit (BI1), the proportion of the structural unit (BI2) and the proportion of the structural unit (BI3) in the structural unit BI is 30 to 100 mol %.

13. The polyimide resin according to any one of claims 10 to 12, wherein the structural unit AI further includes at least one selected from the group consisting of a structural unit (AI3) derived from a compound represented by the following formula (a3) ​​and a structural unit (AI4) derived from a compound represented by the following formula (a4):

14. The polyimide resin according to any one of claims 10 to 13, wherein the molar ratio of the structural unit (AI1) to the sum of the structural units (AI3) and (AI4) in the structural unit AI, [(AI1) / ((AI3)+(AI4)], is 30 / 70 to 100 / 0.

15. A polyimide film comprising the polyimide resin according to any one of claims 10 to 14.

Citation Information

Patent Citations

  • Polyimide precursor composition, polyimide film, and polyimide film / substrate laminate

    JP7235157B1

  • Resin composition, polyimide, and method for producing polyimide film

    JP2021109908A

  • Resin composition, polyimide, and method for producing polyimide film

    JP2021109910A

  • Polyimide precursor and resin composition including the same, polyimide resin film, resin film, and method for producing the same

    JP2021175790A

  • Polyimide precursor composition

    WO2018143314A1

Cited By