Negative electrode for power storage element and power storage element

Optimizing the porosity and binder distribution in the negative electrode active material layer of power storage elements using natural graphite particles with specific size and binder content improves the initial input and energy storage efficiency.

WO2024214610A1PCT designated stage expired Publication Date: 2024-10-17GS YUASA INT LTD

Patent Information

Application Number
PCT/JP2024/013738
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-03
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Current power storage elements, such as non-aqueous electrolyte secondary batteries, face challenges in achieving high initial input due to limitations in the porosity and binder distribution of natural graphite particles in negative electrodes, leading to suboptimal binding and conductivity.

Method used

A negative electrode with a negative electrode active material layer containing natural graphite particles and a binder, where the internal porosity is 2% or less, the average particle diameter is between 6 μm and 10 μm, and the binder content is between 0.1% and 2.0% by mass, ensuring effective binding and conductivity by optimizing the ratio of binder to graphite particle diameter.

Benefits of technology

This configuration enhances the initial input of power storage elements by ensuring proper binding and conductivity between natural graphite particles, leading to improved energy storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013738_17102024_PF_FP_ABST
    Figure JP2024013738_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A negative electrode for a power storage element according to one aspect of the present invention has a negative electrode active material layer containing natural graphite particles and a binder. The internal porosity of the natural graphite particles is 2% or less. The average particle diameter of the natural graphite particles is 6 μm to 10 μm. The content of the binder in the negative electrode active material layer is 0.1 mass% to 2.0 mass%. The binder is particulate, and the ratio (B / A) of the average particle diameter B of the binder to the average particle diameter A of the natural graphite particles is 0.015 to 0.0375.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode for energy storage element and energy storage element

[0001] The present invention relates to a negative electrode for an energy storage element and an energy storage element.

[0002] Due to their high energy density, non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc. The non-aqueous electrolyte secondary batteries generally have a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring charge-transporting ions between the electrodes. Other energy storage elements besides non-aqueous electrolyte secondary batteries include capacitors such as lithium ion capacitors and electric double layer capacitors, as well as energy storage elements using electrolytes other than non-aqueous electrolytes.

[0003] A typical energy storage device includes an electrode assembly in which a positive electrode containing a positive electrode active material and a negative electrode containing a negative electrode active material are stacked with a separator interposed therebetween. The electrode assembly is housed in a container together with an electrolyte to form an energy storage device. Carbon materials such as graphite are widely used as the negative electrode active material (see, for example, Patent Document 1).

[0004] Japanese Patent Application Publication No. 2016-085906

[0005] The energy storage element is required to have a large energy (power: W) that can be taken in per unit time during charging, that is, a large input (power) during charging.

[0006] The present invention has been made based on the above circumstances, and aims to provide a negative electrode for a storage element that can increase the initial input of the storage element, and a storage element equipped with such a negative electrode for a storage element.

[0007] A negative electrode for an energy storage device according to one aspect of the present invention has a negative electrode active material layer containing natural graphite particles and a binder, wherein the natural graphite particles have an internal porosity of 2% or less, the natural graphite particles have an average particle size of 6 μm or more and 10 μm or less, the content of the binder in the negative electrode active material layer is 0.1 mass % or more and 2.0 mass % or less, the binder is in a particulate form, and a ratio (B / A) of an average particle size B of the binder to an average particle size A of the natural graphite particles is 0.015 or more and 0.0375 or less. A energy storage device according to another aspect of the present invention includes the negative electrode for an energy storage device according to the one aspect of the present invention.

[0008] The negative electrode for an electric storage device according to one aspect of the present invention can increase the initial input power of the electric storage device. The electric storage device according to another aspect of the present invention has a large initial input power.

[0009] Fig. 1 is a perspective view showing an embodiment of an electric storage element, and Fig. 2 is a schematic view showing an embodiment of an electric storage device configured by assembling a plurality of electric storage elements.

[0010] First, an outline of the negative electrode for an energy storage device and the energy storage device disclosed in this specification will be described.

[0011] [1] A negative electrode for a storage battery element according to one aspect of the present invention has a negative electrode active material layer containing natural graphite particles and a binder, wherein the natural graphite particles have an internal porosity of 2% or less, the natural graphite particles have an average particle size of 6 μm or more and 10 μm or less, the content of the binder in the negative electrode active material layer is 0.1 mass % or more and 2.0 mass % or less, the binder is in a particulate state, and a ratio (B / A) of an average particle size B of the binder to an average particle size A of the natural graphite particles is 0.015 or more and 0.0375 or less.

[0012] The negative electrode for an energy storage device described in [1] above can increase the initial input power of the energy storage device. While the reason for this is unclear, the following reason is presumed. Generally, natural graphite is a material that can easily achieve both low procurement costs and high output performance when used as a negative electrode active material. When natural graphite is used as a negative electrode active material, it is often processed by rolling it into a spherical shape, which makes the natural graphite particles prone to forming internal voids. When such natural graphite particles and a binder are used to prepare a negative electrode mixture, the binder may penetrate into the internal voids of the natural graphite particles, preventing the natural graphite particles from being properly bound together. In contrast, in the negative electrode for an energy storage device described in [1] above, the internal porosity of the natural graphite particles serving as a negative electrode active material is 2% or less, resulting in few internal voids for the binder to penetrate, and the binder can be easily disposed between the natural graphite particles. Furthermore, when the content of the binder is within the above range, the binder appropriately binds the natural graphite particles together without excessively coating the natural graphite particles, making it easier to ensure sufficient conductivity between the natural graphite particles. Furthermore, when the average particle size of the natural graphite particles is within the above range, the internal voids of the natural graphite particles are small, making it difficult for the binder to be trapped in the internal voids. In addition, when the binder is particulate and the ratio (B / A) of the average particle size B of the binder to the average particle size A of the natural graphite particles is within the above range, the binder is difficult to be trapped in the internal voids of the natural graphite particles and can be easily disposed between the natural graphite particles. Furthermore, the natural graphite particles can be well bonded together. That is, in the negative electrode for an energy storage element, the binder is easily disposed between the natural graphite particles without excessively coating the natural graphite particles, making it possible to well bond the natural graphite particles together. Therefore, the negative electrode for an electric storage element described in the above [1] can increase the initial input power of the electric storage element.

[0013] "Graphite" refers to a graphite that has an average lattice spacing (d 002) is 0.33 nm or more and less than 0.34 nm. Here, the "discharged state" of the carbon material refers to a state in which the carbon material used as the negative electrode active material is discharged so that charge-transporting ions capable of occluding and releasing during charging and discharging are sufficiently released. For example, in a half-cell using a negative electrode containing the carbon material as the working electrode and metallic Li as the counter electrode, the open-circuit voltage is 0.6 V or more. When preparing a carbon material from an assembled energy storage element for the X-ray diffraction measurement, a sample containing the carbon material in the discharged state can be prepared specifically by the following method. First, the energy storage element is discharged at a constant current of 0.1 C to the discharge end voltage during normal use. Here, normal use refers to the use of the energy storage element under the charge and discharge conditions recommended or specified for the energy storage element. Thereafter, the energy storage element is disassembled, and the negative electrode is removed. A half-cell is assembled using the removed negative electrode as the working electrode and metallic Li as the counter electrode. If the open circuit voltage of this half-cell is less than 0.6 V, the half-cell is discharged at a current of 0.1 C so that the open circuit voltage becomes 0.6 V or higher. Note that discharging the half-cell refers to an oxidation reaction in which charge-transporting ions are released from the carbon material (graphite) serving as the negative electrode active material. The half-cell is disassembled, the negative electrode is removed, and the negative electrode is thoroughly washed with dimethyl carbonate and then dried under reduced pressure at room temperature. Next, a powder of the negative electrode active material layer is collected from the negative electrode. The obtained powder of the negative electrode active material layer is used as a sample containing a carbon material for measuring the X-ray diffraction. Operations from disassembling the energy storage element to collecting the sample containing the carbon material to be measured are carried out, if necessary, in a dry air atmosphere with a dew point of −40°C or lower.

[0014] "Natural graphite" refers to graphite extracted from natural resources. Natural graphite particles whose surfaces are coated with materials other than natural graphite are also considered natural graphite particles. Natural graphite exhibits four peaks in the X-ray diffraction pattern at a diffraction angle 2θ ranging from 40° to 50°. These four peaks are believed to be two peaks derived from the hexagonal crystal structure and two peaks derived from the rhombohedral crystal structure. In the case of artificial graphite, it is generally believed that only two peaks derived from the hexagonal crystal structure are exhibited. In the X-ray diffraction pattern, the ratio of the peak intensity derived from the (012) plane to the peak intensity derived from the (100) plane ((012) / (100)) is preferably 0.3 or more, more preferably 0.4 or more. The peak intensity ratio ((012) / (100)) is preferably 0.6 or less. Here, the (100) plane originates from a hexagonal crystal structure, and the (012) plane originates from a rhombohedral crystal structure.

[0015] The "internal porosity" of natural graphite particles refers to the area ratio of voids within a particle to the total area of ​​the particle in a cross-section (cross-sectional SEM image) of the natural graphite particle observed in an SEM image obtained using a scanning electron microscope (SEM). The "internal porosity (area ratio of voids within a particle to the total area of ​​the particle)" of natural graphite particles can be determined by the following procedure. (1) Preparation of Measurement Sample The negative electrode to be measured is fixed with a thermosetting resin. The cross-section of the negative electrode fixed with the resin is exposed by ion milling to prepare a measurement sample. Note that when the negative electrode to be measured is included in an assembled energy storage element, the negative electrode is prepared by the following procedure, and the same applies hereinafter. The energy storage element is discharged at a constant current of 0.1 C to the discharge end voltage during normal use to enter a discharged state. The discharged energy storage element is disassembled, the negative electrode is removed, and the negative electrode is thoroughly washed with dimethyl carbonate and then dried under reduced pressure at room temperature. The entire process from disassembling the energy storage device to preparing the negative electrode to be measured is carried out in a dry air atmosphere with a dew point of -40°C or below. (2) Obtaining a Cross-Sectional SEM Image A JSM-7001F (manufactured by JEOL Ltd.) scanning electron microscope is used to obtain a cross-sectional SEM image. The cross-sectional SEM image is obtained by observing a secondary electron image. The acceleration voltage is 15 kV. The observation magnification is set so that 3 to 15 natural graphite particles appear in one field of view. The obtained cross-sectional SEM image is saved as an image file. Other conditions, such as spot diameter, working distance, irradiation current, brightness, and focus, are appropriately set so that the contours of the natural graphite particles are clearly visible. (3) Cutting Out the Contours of Natural Graphite Particles The contours of the natural graphite particles are cut out from the obtained cross-sectional SEM image using the image cutout function of the image editing software Adobe Photoshop Elements 11. This contour cutting is performed by using the quick selection tool to select the area outside the contours of the natural graphite particles and editing the area other than the natural graphite particles to a black background. If the contours of less than three natural graphite particles can be cut out at this time, cross-sectional SEM images are acquired again, and this process is repeated until the contours of three or more natural graphite particles can be cut out.(4) Binarization Process The image of the first of the cut-out natural graphite particles is binarized using image analysis software PopImaging 6.00, with a threshold value set to a concentration 20% lower than the concentration at which the intensity is at its maximum. The area of ​​the higher concentration side is calculated through the binarization process, thereby obtaining the "area S1 of voids within the particle." Next, the same image of the first natural graphite particle as above is binarized using a threshold value of 10% concentration. The outer periphery of the natural graphite particle is determined through the binarization process, and the area inside the periphery is calculated as the "area S0 of the entire particle." The calculated S1 and S0 are used to calculate the ratio of S1 to S0 (S1 / S0), thereby calculating the "area ratio R1 of voids within the particle to the area of ​​the entire particle" for the first natural graphite particle. The images of the second and subsequent cut-out natural graphite particles are also binarized as described above, and the areas S1 and S0 are calculated. Based on the calculated areas S1 and S0, the area ratios R2, R3, ... of the intraparticle voids relative to the total particle area for each natural graphite particle are calculated. (5) Determination of Internal Porosity The "internal porosity" of a natural graphite particle is determined by calculating the average value of the area ratios R1, R2, R3, ... of the intraparticle voids relative to the total particle area for all natural graphite particles calculated by the binarization process. Note that instead of the scanning electron microscope used in "obtaining a cross-sectional SEM image", the image editing software used in "cutting out the contours of natural graphite particles", and the image analysis software used in "binarization process", devices, software, etc. capable of equivalent measurement, image editing, and image analysis may be used.

[0016] The "average particle size" of natural graphite particles refers to the value (median diameter) at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by laser diffraction / scattering in a diluted solution of particles diluted with a solvent in accordance with JIS-Z-8825 (2013). It has been confirmed that the median diameter based on the above measurement is approximately equal to the arithmetic mean value of the circle-equivalent diameters measured by extracting 100 natural graphite particles, while avoiding extremely large and extremely small natural graphite particles, in a cross-sectional SEM image of the negative electrode obtained using a scanning electron microscope (SEM). The cross-sectional SEM image of the negative electrode is obtained by the procedures described in "(1) Preparation of measurement sample" and "(2) Acquisition of cross-sectional SEM image" in the above-mentioned determination of the "internal porosity" of the natural graphite particles.

[0017] [2] In the negative electrode for a storage device according to the above [1], the content of the binder in the negative electrode active material layer may be less than 1.0 mass %.

[0018] In the negative electrode for a storage battery element described in [2] above, the content of the binder in the negative electrode active material layer is less than the upper limit, and therefore the input power retention rate during charge-discharge cycling can be increased. While the reason for this is unclear, the following is presumed. Generally, binders tend to swell when immersed in an electrolyte, for example. On the other hand, by having the content of the binder in the negative electrode active material layer be less than the upper limit, the amount of binder coated on the natural graphite particles can be maintained within an appropriate range even when the binder swells. This reduces the increase in resistance on the surfaces of the natural graphite particles, and allows the input power retention rate during charge-discharge cycling to be increased.

[0019] [3] In the negative electrode for a storage element according to the above [1] or [2], a ratio (B / A) of an average particle size B of the binder to an average particle size A of the natural graphite particles may be 0.018 or more and 0.030 or less.

[0020] In the negative electrode for an energy storage element described in [3] above, the ratio (B / A) of the average particle size B of the binder to the average particle size A of the natural graphite particles is within the above range, so that the binder is less likely to be trapped in the internal voids of the natural graphite particles and can be more easily disposed between the natural graphite particles. In addition, the natural graphite particles can be more effectively bound to each other.

[0021] The "average particle diameter" of the binder refers to the arithmetic mean value of the circle-equivalent diameter measured by extracting 100 particles from a surface SEM image of the negative electrode obtained using a scanning electron microscope (SEM), avoiding extremely large and extremely small binder particles. A JSM-7001F (manufactured by JEOL Ltd.) scanning electron microscope was used to obtain the surface SEM image of the negative electrode. The surface SEM image was obtained by observing a secondary electron image. The acceleration voltage was 5 kV. The observation magnification was set so that 3 to 15 natural graphite particles appeared in one field of view. The obtained surface SEM image was saved as an image file. Other conditions, such as spot diameter, working distance, irradiation current, brightness, and focus, were appropriately set so that the contours of the binder particles were clearly visible.

[0022] [4] In the negative electrode for a storage device according to any one of [1] to [3] above, the binder may have an average particle size of 150 nm or more and 225 nm or less.

[0023] In the negative electrode for an energy storage element described in [4] above, since the average particle size of the binder is within the above range, the binder is less likely to be trapped in the internal voids of the natural graphite particles, and can be more easily disposed between the natural graphite particles. In addition, the natural graphite particles can be more effectively bound to each other.

[0024] [5] In the negative electrode for a storage device according to any one of [1] to [4] above, the binder particles may have an average aspect ratio of 1.5 or less.

[0025] In the negative electrode for a storage battery element described in [5] above, the average aspect ratio of the binder particles is equal to or less than the upper limit, thereby enabling the natural graphite particles to be more effectively bound together. The "average aspect ratio of the binder particles" refers to the arithmetic mean value of the T / Y value, which is the ratio of the longest major axis T of the binder particles to the longest minor axis Y in the direction perpendicular to the major axis T, measured by extracting 10 particles from a surface SEM image of the negative electrode obtained using a scanning electron microscope (SEM), while avoiding extremely large and extremely small binder particles. The surface SEM image of the negative electrode is obtained using the same procedure as for the SEM image used to determine the average particle diameter of the binder.

[0026] [6] An electric storage device according to another aspect of the present invention includes the negative electrode for an electric storage device according to any one of [1] to [5] above.

[0027] The energy storage element according to the above [6] includes the negative electrode for an energy storage element according to any one of the above [1] to [5], and therefore has a large initial input.

[0028] Hereinafter, a negative electrode for an energy storage element, an energy storage element, an energy storage device, a method for manufacturing an energy storage element according to one embodiment of the present invention, and other embodiments will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.

[0029] [Negative electrode for energy storage device] A negative electrode for an energy storage device according to one embodiment of the present invention (hereinafter also simply referred to as "negative electrode") has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The negative electrode is used as the negative electrode of, for example, a nonaqueous electrolyte secondary battery such as a lithium ion secondary battery, other nonaqueous electrolyte energy storage devices, and energy storage devices using an electrolyte other than a nonaqueous electrolyte. The negative electrode is suitable as the negative electrode of a nonaqueous electrolyte energy storage device.

[0030] (Negative electrode substrate) The negative electrode substrate has electrical conductivity. Whether or not it has electrical conductivity is determined by measuring the volume resistivity of the negative electrode substrate in accordance with JIS-H-0505 (1975) at 10 -2The resistance is determined using Ω cm as a threshold value. Metals such as copper, nickel, stainless steel, and nickel-plated steel, or alloys thereof, carbonaceous materials, etc., are used as the material for the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0031] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and also increase the energy density per volume of the energy storage element.

[0032] (Intermediate layer) The intermediate layer is a layer disposed between the negative electrode substrate and the negative electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the negative electrode substrate and the negative electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent. The binder and conductive agent in the intermediate layer may be the same as the binder and conductive agent in the negative electrode active material layer described below.

[0033] (Negative Electrode Active Material Layer) The negative electrode active material layer contains natural graphite particles and a binder, and optionally contains other negative electrode active materials besides the natural graphite particles, a conductive agent, a thickener, a filler, and other optional components, as needed.

[0034] Natural graphite particles are a component that functions as a negative electrode active material. The type of natural graphite particles is not particularly limited, and examples include flake graphite, massive graphite (flake graphite), and earthy graphite. As the type of natural graphite particles, flake graphite or massive graphite is preferred, and flake graphite is more preferred, from the viewpoint of ensuring crystallinity. The natural graphite particles may be graphite particles obtained by spheroidizing flake graphite and then consolidating it. As the natural graphite particles, one type of the natural graphite particles described above may be used alone, or two or more types may be used in combination. The natural graphite particles may be coated on the surface with a carbon material other than natural graphite particles (e.g., non-graphitic carbon). The coating of the carbon material can be achieved, for example, by coating the surface of the natural graphite particles with pitch and firing the resulting mixture.

[0035] The upper limit of the internal porosity of the natural graphite particles is 2%, preferably 1.5%, and more preferably 1%. When the internal porosity of the natural graphite particles is equal to or less than the above upper limit, the binder is easily disposed between the natural graphite particles, allowing for a large initial input. The lower limit of the internal porosity of the natural graphite particles is not particularly limited, but can be set to 0.1% from the viewpoint of manufacturability. The internal porosity of the natural graphite particles may be equal to or greater than any of the above lower limits and equal to or less than any of the above upper limits. The internal porosity of the natural graphite particles can be adjusted by, for example, compacting the natural graphite particles.

[0036] The lower limit of the average particle size of the natural graphite particles is 6 μm, preferably 6.5 μm, and more preferably 7 μm. On the other hand, the upper limit of the average particle size of the natural graphite particles is 10 μm, and in some cases, 9 μm or 8 μm is preferable. When the average particle size of the natural graphite particles is equal to or greater than the lower limit, excessive coating of the surface of the natural graphite particles with the binder can be suppressed, thereby increasing the initial input. When the average particle size of the natural graphite particles is equal to or less than the upper limit, the internal voids of the natural graphite particles are small, making it difficult for the binder to be trapped in these internal voids. In other words, even a small amount of binder can be easily disposed between the natural graphite particles, thereby increasing the initial input. Methods for obtaining natural graphite particles with a predetermined particle size include pulverizing the natural graphite material with a pulverizer, classifier, or the like. Examples of pulverizing methods include methods using a mortar, ball mill, sand mill, vibration ball mill, planetary ball mill, jet mill, counter jet mill, swirling airflow jet mill, or sieve. During pulverization, wet pulverization can be used in the presence of water or an organic solvent such as hexane. As a classification method, a sieve or an air classifier can be used as needed for both the dry and wet methods.

[0037] The content of natural graphite particles in the negative electrode active material layer is preferably 60% by mass to 99.5% by mass, more preferably 80% by mass to 99% by mass, and even more preferably 90% by mass to 99% by mass. By setting the content of natural graphite particles within the above range, it is possible to achieve both high energy density and manufacturability of the negative electrode active material layer, and to further increase the initial input power.

[0038] The negative electrode active material may contain other negative electrode active materials in addition to natural graphite particles. Examples of other negative electrode active materials in addition to natural graphite particles include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li 4 Ti 5 O 12 , LiTiO 2、 TiNb 2 O 7Examples of the "non-graphitic carbon" include titanium-containing oxides such as titanium dioxide, polyphosphate compounds, silicon carbide, and carbon materials such as artificial graphite and non-graphitic carbon. The "non-graphitic carbon" is a material having an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. However, it is preferable that natural graphite particles are the main negative electrode active material. For example, in a cross-sectional SEM image of the negative electrode, the area ratio of natural graphite particles to the area occupied by all negative electrode active materials (area occupied by natural graphite particles / area occupied by all negative electrode active materials) is preferably 90% or more, more preferably 99% or more, and may be substantially 100%. Note that the cross-sectional SEM image of the negative electrode is obtained using the same procedure as for the SEM image used to determine the "internal porosity (area ratio of voids within particles to the area of ​​the entire particle)" of natural graphite particles. The area occupied by the negative electrode active material is the area of ​​the entire particles of the negative electrode active material (area including internal voids). Note that a cross-sectional SEM image containing 10 or more particles of the negative electrode active material in one field of view is used to determine the area ratio of the natural graphite particles to the area occupied by all the negative electrode active materials (area occupied by natural graphite particles / area occupied by all the negative electrode active materials). The content of the natural graphite particles in all the negative electrode active materials contained in the negative electrode active material layer is preferably 90% by mass or more, more preferably 99% by mass or more, and may be substantially 100% by mass. In other words, it is particularly preferable that only natural graphite particles are used as the negative electrode active material. Thus, by using natural graphite particles primarily as the negative electrode active material, the initial input power becomes larger.

[0039] The content of all the negative electrode active materials in the negative electrode active material layer is preferably 60% by mass to 99.5% by mass, more preferably 80% by mass to 99% by mass, and even more preferably 90% by mass to 99% by mass. By setting the content of all the negative electrode active materials within the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.

[0040] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers. Among these, SBR is preferred from the viewpoints of high flexibility and ease of binding natural graphite particles together.

[0041] The binder is particulate. The lower limit of the average particle diameter of the binder is preferably 150 nm, more preferably 160 nm, and even more preferably 170 nm. On the other hand, the upper limit of the average particle diameter of the binder is preferably 225 nm, more preferably 210 nm, and even more preferably 200 nm. When the average particle diameter of the binder is equal to or greater than the above-mentioned lower limit, the binder is less likely to be trapped in the internal voids of the natural graphite particles, and can be more easily arranged between the natural graphite particles. When the average particle diameter of the binder is equal to or less than the above-mentioned upper limit, the binding strength of the binder between the natural graphite particles is easily increased. The average particle diameter of the binder may be equal to or greater than any of the above-mentioned lower limits and equal to or less than any of the above-mentioned upper limits.

[0042] The lower limit of the ratio (B / A) of the average particle size B of the binder to the average particle size A of the natural graphite particles is 0.015, preferably 0.018, more preferably 0.020, and even more preferably 0.022. The upper limit of the ratio (B / A) is 0.0375, preferably 0.035, more preferably 0.030, and even more preferably 0.028. When the ratio (B / A) is equal to or greater than the lower limit, the binder can be more easily arranged between the natural graphite particles. When the ratio (B / A) is equal to or less than the upper limit, the binder can easily be bonded between the natural graphite particles. The ratio (B / A) may be equal to or greater than any of the lower limits and equal to or less than any of the upper limits.

[0043] The average aspect ratio of the binder particles is preferably 1.5 or less, more preferably 1.4 or less, more preferably 1.3 or less, and even more preferably 1.2 or less. By setting the average aspect ratio of the binder particles to the above upper limit or less, it is easy to increase the binding strength of the binder between the natural graphite particles.

[0044] The lower limit of the binder content in the negative electrode active material layer is 0.1% by mass, preferably 0.3% by mass, and more preferably 0.5% by mass. Meanwhile, the upper limit of the binder content in the negative electrode active material layer is 2.0% by mass, preferably 1.5% by mass, and more preferably 1.0% by mass. When the binder content in the negative electrode active material layer is equal to or greater than the lower limit, natural graphite particles can be easily bound together. Furthermore, when the binder content in the negative electrode active material layer is equal to or less than the upper limit, the natural graphite particles are not excessively coated, which facilitates ensuring electrical conductivity between the natural graphite particles. This means that the initial input power of the energy storage device can be increased. Furthermore, from the viewpoint of increasing the input power retention rate during charge / discharge cycling of the energy storage device, the upper limit of the binder content in the negative electrode active material layer is more preferably less than 1.0% by mass, even more preferably 0.8% by mass, and in some cases, 0.6% by mass is particularly preferred. The binder content in the negative electrode active material layer may be equal to or greater than any of the lower limits and equal to or less than any of the upper limits. The binder content in the negative electrode active material layer is determined from the mass loss when the binder contained in the negative electrode active material layer is thermally decomposed using a thermogravimetric / differential thermal (TG / DTA) analyzer.

[0045] The conductive agent is not particularly limited as long as it is a material that is conductive. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, etc. Carbonaceous materials include graphite, non-graphitic carbon, graphene-based carbon, etc. Non-graphitic carbon includes carbon nanofiber, pitch-based carbon fiber, carbon black, etc. Carbon black includes furnace black, acetylene black, ketjen black, etc. Graphene-based carbon includes graphene, carbon nanotubes (CNT), fullerene, etc. However, the conductive agent does not include natural graphite particles contained in the negative electrode active material layer. The conductive agent may be in the form of powder, fiber, etc. One of these materials may be used alone as the conductive agent, or two or more may be mixed and used. These materials may also be used in combination. For example, a composite of carbon black and CNT may be used. Among these, carbon black is preferred from the viewpoints of electronic conductivity and coatability, and acetylene black is particularly preferred.

[0046] The content of the conductive agent in the negative electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 2% by mass or more and 9% by mass or less. By setting the content of the conductive agent within the above range, the energy density of the energy storage element can be increased. In one embodiment of the present invention, it may be preferable that the conductive agent is not contained in the negative electrode active material layer.

[0047] The thickener is not particularly limited. Examples of thickeners include polymers that can be dissolved or dispersed in aqueous solvents. Examples of such polymers include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. If the thickener has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like. The content of the thickener in the negative electrode active material layer is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.5% by mass or more and 3% by mass or less. In this specification, the term "thickener" refers to an aqueous solution prepared by dissolving or dispersing 1 part by mass of the thickener in 99 parts by mass of water (aqueous solution containing 1% by mass of the thickener) having a viscosity of 400 mPa·s or more. The viscosity is measured using a Brookfield viscometer at a rotation speed of 60 rpm and a temperature of 25°C. Such thickeners are not included in the binder.

[0048] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof. In one embodiment of the present invention, it may be preferable that the negative electrode active material layer does not contain a filler.

[0049] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0050] [Electricity Storage Element] An electric storage element according to one embodiment of the present invention includes an electrode assembly having a positive electrode, a negative electrode, and a separator, an electrolyte, and a container for accommodating the electrode assembly and the electrolyte. The electrode assembly is typically a stacked type in which multiple positive electrodes and multiple negative electrodes are stacked with separators interposed therebetween, or a wound type in which the positive electrode and negative electrode are stacked with separators interposed therebetween and wound. The electrolyte is present in a state contained in the positive electrode, negative electrode, and separator. A lithium ion secondary battery will be described as an example of an electric storage element. Note that the negative electrode included in the electric storage element according to one embodiment of the present invention can be the same as the negative electrode described above. Therefore, the positive electrode, separator, and electrolyte will be described below.

[0051] <Positive Electrode> The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.

[0052] The positive electrode substrate is conductive. Examples of the material for the positive electrode substrate include metals such as aluminum, titanium, tantalum, and stainless steel, as well as alloys thereof. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high conductivity, and cost. Examples of the positive electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, and A1N30, as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).

[0053] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate and also increase the energy density per volume of the energy storage element.

[0054] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.

[0055] The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, and a filler, as needed. The optional components such as the conductive agent, the binder, the thickener, and the filler can be selected from the materials exemplified for the negative electrode described above.

[0056] The positive electrode active material can be appropriately selected from known positive electrode active materials. As the positive electrode active material for a lithium ion secondary battery, a material capable of absorbing and releasing lithium ions is usually used. Examples of the positive electrode active material include α-NaFeO 2 Examples of suitable lithium transition metal composite oxides include those having a α-type crystal structure, those having a spinel type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. 2 As the lithium transition metal composite oxide having a crystalline structure, for example, Li[Li x Ni (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Co (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1−x−γ−β), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O 2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1−x−γ−β), etc. Examples of lithium transition metal composite oxides having a spinel crystal structure include Li x Mn 2 O 4 , Li x Ni γ Mn (2-γ) O 4 Examples of polyanion compounds include LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 Examples of the chalcogen compound include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.

[0057] The positive electrode active material is usually in the form of particles (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above-mentioned lower limit or more, the positive electrode active material is easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above-mentioned upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. Note that when a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. The "average particle size" of the positive electrode active material refers to the value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by laser diffraction / scattering in a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013). The pulverization method and classification method can be selected, for example, from the methods exemplified for the negative electrode described above.

[0058] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% by mass to 99% by mass, more preferably 70% by mass to 98% by mass, and even more preferably 80% by mass to 95% by mass. By setting the content of the positive electrode active material within the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.

[0059] The content of the conductive agent in the positive electrode active material layer is preferably 1% by mass to 10% by mass, more preferably 3% by mass to 9% by mass. By setting the content of the conductive agent in this range, the energy density of the energy storage element can be increased.

[0060] The content of the binder in the positive electrode active material layer is preferably 1% by mass to 10% by mass, more preferably 3% by mass to 9% by mass, by which the positive electrode active material can be stably maintained.

[0061] Examples of thickeners include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, this functional group may be deactivated in advance by methylation or the like.

[0062] The positive electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.

[0063] <Separator> The separator can be appropriately selected from known separators. Examples of separators that can be used include separators consisting of only a substrate layer and separators in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, porous resin films are preferred from the viewpoint of strength, and nonwoven fabrics are preferred from the viewpoint of electrolyte retention. Materials for the substrate layer of the separator are preferably polyolefins such as polyethylene and polypropylene from the viewpoint of shutdown function, and polyimide and aramid from the viewpoint of oxidative decomposition resistance. A composite material of these resins may also be used for the substrate layer of the separator.

[0064] The heat-resistant particles contained in the heat-resistant layer preferably exhibit a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably exhibit a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials exhibiting a mass loss of a predetermined value or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, as well as artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be used in combination. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the energy storage device.

[0065] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.

[0066] The separator may be a polymer gel composed of a polymer and an electrolyte. Examples of polymers include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of a polymer gel has the effect of suppressing leakage. The separator may be a combination of the porous resin film or nonwoven fabric described above and a polymer gel.

[0067] <Electrolyte> The electrolyte may be a non-aqueous electrolyte, such as a non-aqueous electrolytic solution, which contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.

[0068] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of non-aqueous solvents include cyclic carbonates, chain carbonates, carboxylic acid esters, phosphate esters, sulfonic acid esters, ethers, amides, and nitriles. Non-aqueous solvents in which some of the hydrogen atoms contained in these compounds have been substituted with halogens may also be used.

[0069] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Of these, EC is preferred.

[0070] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferred.

[0071] It is preferable to use a cyclic carbonate or a chain carbonate as the non-aqueous solvent, and it is more preferable to use a cyclic carbonate and a chain carbonate in combination. The use of a cyclic carbonate can promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. The use of a chain carbonate can reduce the viscosity of the non-aqueous electrolyte. When a cyclic carbonate and a chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is preferably in the range of, for example, 5:95 to 50:50.

[0072] The electrolyte salt can be appropriately selected from known electrolyte salts, such as lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Of these, lithium salts are preferred.

[0073] The lithium salt is LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2 inorganic lithium salts such as lithium oxalate salts, lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); 3 CF 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) (SO2 C 4 F 9 ), LiC(SO 2 CF 3 ) 3 , LiC(SO 2 C 2 F 5 ) 3 Among these, inorganic lithium salts are preferred, and LiPF 6 is more preferred.

[0074] The content of the electrolyte salt in the non-aqueous electrolyte solution is 0.1 mol / dm at 20°C and 1 atmosphere. 3 2.5mol / dm or more 3 It is preferably 0.3 mol / dm or less. 3 2.0mol / dm or more 3 It is more preferable that it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3 It is more preferable that it is 0.7 mol / dm or less. 3 1.5mol / dm or more 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the non-aqueous electrolyte can be increased.

[0075] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additives include halogenated carbonates such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC); oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, and silyl. Aromatic compounds such as cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, and the like. Carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1 ,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. These additives may be used alone or in combination of two or more.

[0076] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass, based on the total mass of the non-aqueous electrolyte. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and further improve safety.

[0077] The non-aqueous electrolyte may be a solid electrolyte, or a non-aqueous electrolytic solution and a solid electrolyte may be used in combination.

[0078] The solid electrolyte can be selected from any material that has ionic conductivity of lithium, sodium, calcium, etc. and is solid at room temperature (e.g., 15° C. to 25° C.). Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.

[0079] As the sulfide solid electrolyte, in the case of a lithium ion secondary battery, for example, Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 S 5 , Li 10 Ge-P 2 S 12 etc.

[0080] The shape of the energy storage element of this embodiment is not particularly limited, and examples thereof include cylindrical batteries, prismatic batteries, flat batteries, coin batteries, and button batteries. FIG. 1 shows an energy storage element 1 as an example of a prismatic battery. Note that this figure is a see-through view of the inside of the container. An electrode body 2 having a positive electrode and a negative electrode wound with a separator sandwiched between them is housed in a prismatic container 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51.

[0081] [Electricity Storage Device] The energy storage element of the present embodiment can be mounted as an energy storage unit (battery module) configured by assembling a plurality of energy storage elements in an automobile power source such as an electric vehicle (EV), a hybrid electric vehicle (HEV), or a plug-in hybrid electric vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source. In this case, the technology of the present invention may be applied to at least one energy storage element included in the energy storage unit. FIG. 2 shows an example of an energy storage device 30 in which energy storage units 20, each of which is an assembly of two or more electrically connected energy storage elements 1, are further assembled. The energy storage device 30 may include a bus bar (not shown) that electrically connects the two or more energy storage elements 1, a bus bar (not shown) that electrically connects the two or more energy storage units 20, or the like. The energy storage unit 20 or the energy storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more energy storage elements.

[0082] [Method for Manufacturing Energy Storage Element] The method for manufacturing the energy storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode assembly, preparing an electrolyte, and housing the electrode assembly and the electrolyte in a container. Preparing the electrode assembly includes preparing a positive electrode and a negative electrode, and forming the electrode assembly by stacking or winding the positive electrode and the negative electrode with a separator interposed therebetween.

[0083] The method for placing the electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the electrolyte, the non-aqueous electrolyte solution may be poured into the container through an inlet formed in the container, and the inlet may then be sealed.

[0084] [Other Embodiments] The energy storage device of the present invention is not limited to the above-described embodiments, and various modifications may be made without departing from the spirit of the present invention. For example, the configuration of one embodiment can be added to the configuration of another embodiment, and part of the configuration of one embodiment can be replaced with the configuration of another embodiment or well-known technology. Furthermore, part of the configuration of one embodiment can be deleted. Also, well-known technology can be added to the configuration of one embodiment.

[0085] In the above embodiment, the case where the energy storage element is used as a chargeable and dischargeable lithium ion secondary battery has been described, but the energy storage element may be of any type, shape, size, capacity, etc. The present invention can also be applied to various secondary batteries, non-aqueous electrolyte energy storage elements such as capacitors such as electric double layer capacitors and lithium ion capacitors, or energy storage elements using electrolytes other than non-aqueous electrolytes.

[0086] In the above embodiment, the electrode assembly in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode assembly may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode.

[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0088] [Example 1] <Preparation of Negative Electrode> Natural graphite particles were used as the negative electrode active material. These natural graphite particles were spherical graphite particles obtained by spheroidizing flake graphite and then subjecting it to a compaction treatment. The natural graphite particles had an average particle size A of 10.0 μm and an internal porosity of 1%.

[0089] A negative electrode mixture paste containing the above-mentioned negative electrode active material, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener in a mass ratio (solid content equivalent) of 97.0:2.0:1.0, and containing water as a dispersion medium, was prepared. Note that when preparing a negative electrode mixture paste by changing the binder content in the following examples or comparative examples, the total content (solid content equivalent) of the negative electrode active material and binder in the negative electrode mixture paste was adjusted to 99.0 mass%. The above-mentioned negative electrode mixture paste was applied to both sides of copper foil as a negative electrode substrate, dried, and pressed to prepare a negative electrode in which a negative electrode active material layer was disposed on the negative electrode substrate. The average particle diameter B of the binder was 200 nm, and the aspect ratio was 1.0.

[0090] <Preparation of Energy Storage Element> (Preparation of Positive Electrode) α-NaFeO 2 It has a LiNi type crystal structure 0.6 Co 0.2 Mn 0.2 O2 A lithium transition metal composite oxide represented by the formula (I) was used. A positive electrode mixture paste containing the above positive electrode active material, acetylene black (AB) as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder in a mass ratio (solid content equivalent) of 93.0:4.0:3.0, and containing N-methylpyrrolidone (NMP) as a dispersion medium, was prepared. The above positive electrode mixture paste was applied to both sides of aluminum foil serving as a positive electrode substrate, dried, and then pressed to produce a positive electrode in which a positive electrode active material layer was disposed on the positive electrode substrate.

[0091] (Preparation of non-aqueous electrolyte) LiPF was dissolved in a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 30:35:35. 6 to 1.0 mol / dm 3 (20° C., 1 atmosphere) to prepare a non-aqueous electrolyte solution.

[0092] (Fabrication of Energy Storage Element) The positive electrode and the negative electrode were stacked with a polyolefin microporous film separator interposed therebetween to fabricate an electrode assembly, which was then housed in a container made of a metal resin composite film, the nonaqueous electrolyte solution was poured into the container, and the container was then sealed by heat welding to obtain the energy storage element of Example 1.

[0093] [Comparative Example 1, Examples 2 to 5] Energy storage elements of Comparative Example 1 and Examples 2 to 5 were obtained in the same manner as in Example 1, except that the content of the binder (SBR) in the negative electrode active material layer was set as shown in Table 1. The content of CMC in each example was fixed at 1 mass %, and the total of the content of the negative electrode active material, the content of SBR, and the content of CMC was adjusted to 100 mass %. The same applies hereinafter.

[0094] [Comparative Examples 2 to 6] Natural graphite particles different from those used in Example 1 were used as the negative electrode active material. These natural graphite particles were spherical graphite particles obtained by spheroidizing flake graphite and not subjecting it to a compaction treatment. The natural graphite particles had an average particle size A of 9.7 μm and an internal porosity of 10%. Using the negative electrode active material, energy storage elements of Comparative Examples 2 to 6 were obtained in the same manner as in Example 1, except that the binder (SBR) content in the negative electrode active material layer was set as shown in Table 1.

[0095] [Example 6] Natural graphite particles different from those used in Example 1 were used as the negative electrode active material. These natural graphite particles were spherical graphite particles obtained by spheroidizing flake graphite and then subjecting it to a consolidation treatment. The natural graphite particles had an average particle size A of 8.1 μm and an internal porosity of 1%. Using this negative electrode active material, an energy storage element of Example 6 was obtained in the same manner as in Example 1, except that the content of the binder (SBR) in the negative electrode active material layer was set as shown in Table 2.

[0096] [Comparative Example 7] As the negative electrode active material, artificial graphite particles having an average particle diameter A of 2.8 μm and an internal porosity of 1% were used. Using this negative electrode active material, an energy storage element of Comparative Example 7 was obtained in the same manner as in Example 1, except that the content of the binder (SBR) in the negative electrode active material layer was set as shown in Table 2.

[0097] [Comparative Example 8] Natural graphite particles different from those used in Example 1 were used as the negative electrode active material. These natural graphite particles were spherical graphite particles obtained by spheroidizing flake graphite and then subjecting it to a consolidation treatment. The natural graphite particles had an average particle size A of 15.0 μm and an internal porosity of 1%. Using this negative electrode active material, an energy storage element of Comparative Example 8 was obtained in the same manner as in Example 1, except that the content of the binder (SBR) in the negative electrode active material layer was set as shown in Table 2.

[0098] Comparative Example 9 An electricity storage element of Comparative Example 9 was obtained in the same manner as in Example 6, except that the average particle diameter B of the binder (SBR) in the negative electrode active material layer was set as shown in Table 2.

[0099] Examples 7 to 9 Energy storage elements of Examples 7 to 9 were obtained in the same manner as in Example 1, except that the content of the binder (SBR) in the negative electrode active material layer was set as shown in Table 3.

[0100] [Evaluation] (Initial charge / discharge) Each energy storage device was initially charged / discharged at 25°C in the following manner. Constant-current / constant-voltage charging was performed with a charging current of 0.2 C and a charge cut-off voltage of 4.1 V. The charge was terminated until the charging current reached 0.02 C. A rest period of 10 minutes was then provided. Subsequently, constant-current discharge was performed with a discharge current of 0.2 C and a discharge cut-off voltage of 3.0 V. The discharge capacity at this time was designated the "initial discharge capacity."

[0101] (Measurement of Initial Input Power) After the initial charge and discharge, the initial input power was measured as follows. A constant current charge of 1.0 C was performed in a thermostatic chamber at 25°C, and the SOC was adjusted to 50%. After storing the battery in a thermostatic chamber at -30°C for 4 hours, the battery was charged for 10 seconds at a constant current of 5 C, 10 C, 15 C, 20 C, or 25 C. "SOC" (State of Charge) refers to the state of charge of the battery, measured in the voltage range in which the battery is normally used, based on the rated capacity. In this example, the rated capacity was the initial discharge capacity. After each charge, a constant current discharge of 1.0 C was performed to adjust the SOC to 50%. The resistance value was calculated from the slope of the current during each charge and the voltage 1 second after the start of charge, and the initial input power was calculated as "{the difference between the voltage before charge and the upper limit voltage (4.3 V)} / resistance value×upper limit voltage (4.3 V)." The input is the energy (power) that can be taken in per unit time. The measurement results of the initial input are shown in Tables 1 and 2 as "initial input."

[0102] (Charge-Discharge Cycle Test) After measuring the initial input, the energy storage elements of Examples 7 to 9 were subjected to a charge-discharge cycle test in the following manner. In a thermostatic chamber at 60°C, constant-current charging was performed with a charging current of 8 C and a charge cut-off voltage of 3.9 V. Subsequently, constant-current discharging was performed with a discharging current of 8 C and a discharge cut-off voltage of 3.5 V. This charge-discharge cycle was repeated for 1000 hours.

[0103] (Measurement of input power after charge-discharge cycle test) After the above charge-discharge cycle test, the input power after the charge-discharge cycle test was measured in the same manner as the measurement of the initial input power. The percentage of the input power after the charge-discharge cycle test to the initial input power for the energy storage elements of Examples 7 to 9 is shown in Table 3 as the "input power maintenance rate after cycling."

[0104]

[0105]

[0106]

[0107] As shown in Table 1, in all of Examples 1 to 5 and Comparative Examples 1 to 6, the average particle size of the natural graphite particles was 6.0 μm or more and 10.0 μm or less, but the initial input was less than 500 W in Comparative Examples 1 to 6, and 500 W or more in Examples 1 to 5. Comparing Comparative Example 1 with Examples 1 to 5, it is believed that the SBR content in Examples 1 to 5 was 0.1 mass% or more and 2.0 mass% or less, which prevented the natural graphite particles from being excessively coated, resulting in a large initial input. Furthermore, comparing Examples 1 to 5 with Comparative Examples 2 to 6, it is believed that in Comparative Examples 2 to 6, the SBR was trapped in the internal voids of the natural graphite particles, weakening the bonding between the natural graphite particles, whereas in Examples 1 to 5, the internal porosity was 2% or less, which prevented the SBR from being trapped in the internal voids of the natural graphite particles, resulting in a distribution that ensured sufficient conductivity between the natural graphite particles.

[0108] Furthermore, in Comparative Examples 2 to 6, the initial input did not increase even when the SBR content was 2.0% by mass or less, whereas the initial input increased when the SBR content was 0.1% by mass or more and 2.0% by mass or less in Examples 1 to 5. That is, it is presumed that in Comparative Examples 2 to 6, when the SBR content was 0.1% by mass or more and 2.0% by mass or less, the effect of optimizing the coating of the natural graphite particle surfaces with SBR was canceled out by the effect of weakening the binding between the natural graphite particles, whereas in Examples 1 to 5, even when the SBR content was 0.1% by mass or more and 2.0% by mass or less, the effect of optimizing the coating of the natural graphite particle surfaces with SBR was effectively achieved while maintaining the binding between the natural graphite particles.

[0109] As shown in Table 2, Example 6, in which the average particle size of the natural graphite particles was 6 μm or more and 10 μm or less, had a higher initial input power than Comparative Example 7, in which the average particle size of the natural graphite particles was less than 6 μm, and Comparative Example 8, in which the average particle size of the natural graphite particles was more than 10 μm. This suggests that by maintaining the average particle size of the natural graphite particles within an appropriate range, the SBR is likely to be arranged to improve the binding between the natural graphite particles. Furthermore, Example 6, in which the ratio (B / A) of the average particle size B of the binder to the average particle size A of the natural graphite particles was 0.015 or more and 0.0375 or less, had a higher initial input power than Comparative Example 7, in which the ratio (B / A) exceeded 0.0375, and Comparative Examples 8 and 9, in which the ratio (B / A) was less than 0.015. This suggests that by maintaining the ratio (B / A) of the average particle size B of the binder to the average particle size A of the natural graphite particles within an appropriate range, the SBR is likely to be arranged to improve the binding between the natural graphite particles.

[0110] From the above, it is believed that the synergistic effects of the internal porosity of the natural graphite particles being 2% or less, the binder (SBR) content being 0.1% by mass or more and 2.0% by mass or less, the average particle size of the natural graphite particles being 6 μm or more and 10 μm or less, and the ratio (B / A) of the average particle size B of the binder to the average particle size A of the natural graphite particles being 0.015 or more and 0.0375 or less, allow the binder to be easily disposed between the natural graphite particles without excessively coating them, thereby enabling the natural graphite particles to be well bound together.

[0111] As shown in Table 3, the input power retention rate after charge-discharge cycling could be increased by setting the SBR content to less than 1.0 mass %. It is believed that setting the binder content to less than 1.0 mass % allowed the amount of binder coating on the natural graphite particles to be maintained within an appropriate range.

[0112] The present invention can be applied to electric storage elements used as power sources for electronic devices such as personal computers and communication terminals, and automobiles.

[0113] REFERENCE SIGNS LIST 1 Energy storage element 2 Electrode body 3 Container 4 Positive electrode terminal 41 Positive electrode lead 5 Negative electrode terminal 51 Negative electrode lead 20 Energy storage unit 30 Energy storage device

Claims

1. A negative electrode for a storage element, comprising a negative electrode active material layer containing natural graphite particles and a binder, wherein the natural graphite particles have an internal porosity of 2% or less, the natural graphite particles have an average particle diameter of 6 μm or more and 10 μm or less, the content of the binder in the negative electrode active material layer is 0.1% by mass or more and 2.0% by mass or less, the binder is in particulate form, and a ratio (B / A) of an average particle diameter B of the binder to an average particle diameter A of the natural graphite particles is 0.015 or more and 0.0375 or less.

2. The negative electrode for a storage element according to claim 1, wherein the content of the binder in the negative electrode active material layer is less than 1.0 mass %.

3. The negative electrode for a storage element according to claim 1 or 2, wherein the ratio (B / A) of the average particle size B of the binder to the average particle size A of the natural graphite particles is 0.018 or more and 0.030 or less.

4. The negative electrode for a storage element according to claim 1 or 2, wherein the average particle size of the binder is 150 nm or more and 225 nm or less.

5. The negative electrode for a storage element according to claim 1 or 2, wherein the average aspect ratio of the binder particles is 1.5 or less.

6. An electric storage element comprising the negative electrode for an electric storage element according to claim 1 or 2.

Citation Information

Patent Citations

  • Electrode for electrochemical element and method for manufacturing the same

    JP2008251965A

  • Negative electrode plate, lithium-ion secondary battery, and manufacturing method for the negative electrode plate

    JP2022154005A

  • Power storage element

    WO2022259724A1

  • Power storage element

    WO2023286718A1

Cited By

  • Negative electrode for nonaqueous electrolyte power storage element, and nonaqueous electrolyte power storage element

    WO2026211345A1