Inner-bag film for semi-solid-state battery, and semi-solid-state battery

The inner bag film with a polyolefin base and adhesive layer addresses the inflexibility and weight issues of metal exterior materials by enabling heat-sealing and gas permeability, enhancing the moldability and performance of semi-solid batteries for diverse applications.

WO2024214636A1PCT designated stage expired Publication Date: 2024-10-17DAI NIPPON PRINTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013991
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional metal exterior materials for power storage devices are inflexible and heavy, making it difficult to accommodate the diverse shapes and weight reduction requirements of modern applications, such as electric vehicles and portable electronics, and semi-solid batteries require a packaging solution that maintains the shape of semi-solid electrodes while allowing for heat-sealing and gas permeability.

Method used

An inner bag film for semi-solid batteries composed of a laminate with a polyolefin base material and an adhesive layer, allowing for easy heat-sealing and excellent moldability, which fixes multiple cells together and provides CO2 permeability without the need for metal layers or holes.

Benefits of technology

The inner bag film enables the creation of lightweight, flexible, and efficient semi-solid batteries with improved moldability and gas release properties, ensuring the stability and performance of semi-solid batteries in various shapes and configurations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000033_0000
    Figure 00000033_0000
  • Figure 00000033_0001
    Figure 00000033_0001
Patent Text Reader

Abstract

Provided is an inner-bag film for a semi-solid-state battery, which is to be placed between an outer case and battery elements of the semi-solid-state battery. The inner-bag film for a semi-solid-state battery comprises a laminate including at least a base and an adhesive layer, wherein the base includes a polyolefin.
Need to check novelty before this filing date? Find Prior Art

Description

Inner bag film for semi-solid battery and semi-solid battery

[0001] The present disclosure relates to an inner bag film for a semi-solid battery and a semi-solid battery.

[0002] Various types of electricity storage devices have been developed, and in all of them, exterior materials are essential components for sealing electricity storage device elements such as electrodes and electrolytes. Conventionally, metal exterior materials have been widely used as exterior materials for electricity storage devices.

[0003] Meanwhile, in recent years, with the increasing performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc., there has been a demand for electricity storage devices to have a variety of shapes as well as to be thinner and lighter in weight. However, the metallic exterior materials for electricity storage devices that have been widely used in the past have the drawbacks of being difficult to keep up with the diversification of shapes and also having limitations on how much they can be made lighter.

[0004] Therefore, a film-like laminate in which a base layer, a barrier layer, an adhesive layer, and a heat-sealable resin layer are laminated in this order has been proposed as an exterior material for an electricity storage device that can be easily processed into various shapes and can be made thinner and lighter (see, for example, Patent Document 1).

[0005] In such an electrical storage device packaging material, a recess is generally formed by cold forming, and electrical storage device elements such as electrodes and electrolyte are placed in the space formed by the recess, and a heat-sealable resin layer is heat-sealed to obtain an electrical storage device in which the electrical storage device elements are housed inside the electrical storage device packaging material.

[0006] JP 2008-287971 A International Publication No. 2019 / 087956

[0007] Semi-solid batteries using semi-solid electrodes are known as power storage devices (see Patent Document 2). Semi-solid batteries use semi-solid electrodes that have fluidity, and the electrodes tend to lose their shape when dried. For this reason, in semi-solid batteries, the battery element is kept in shape by an exterior material (packaging).

[0008] For example, Patent Document 2 discloses a semi-solid battery (electrochemical cell) including a power generating element including a semi-solid positive electrode, a semi-solid negative electrode, a separator located between the positive electrode and the negative electrode, a positive electrode current collector electrically connected to the positive electrode, and a negative electrode current collector electrically connected to the negative electrode, and a packaging body containing the power generating element, the packaging body having holes opening to the inside and outside.

[0009] Similar to general energy storage devices, in semi-solid batteries, multiple cells (single cells) can be connected to form a module (battery assembly), which can then be housed in a package to form a single large semi-solid battery. When a semi-solid battery is modularized, each cell can have its battery element housed in an inner bag, and these cells can then be housed in a package. In such a configuration, if the multiple cells are not fixed in the bag, the cells may move within the package during use, potentially damaging the cells and the package. Therefore, it is desirable to fix the cells together within the package. The inventors of the present invention considered that using an inner bag film to form the inner bag, imparting heat-sealing properties to the substrate that constitutes the outer surface of the inner bag film, and heat-sealing the outer surfaces of the inner bags together would be effective, and set a new goal: to impart heat-sealing properties to the substrate of the inner bag film.

[0010] Furthermore, as described above, in a film-like packaging material for an electricity storage device, recesses are generally formed by cold forming, and electricity storage device elements such as electrodes and an electrolyte are placed in the spaces formed by the recesses, and a heat-sealable resin layer is heat-sealed to obtain an electricity storage device in which the electricity storage device elements are housed inside the packaging material for an electricity storage device. For example, when such a packaging material is applied to a semi-solid battery, the inner bag film also requires excellent formability.

[0011] Under these circumstances, the main object of the present disclosure is to provide a novel inner bag film that is placed between the exterior material and the battery element of a semi-solid battery, which can easily be heat-sealed to the base materials of the inner bag film and has excellent formability.

[0012] The inventors of the present disclosure conducted extensive research to solve the above-mentioned problems. As a result, they discovered that in an inner bag film for a semi-solid battery, which is disposed between the exterior material of the semi-solid battery and the battery element, the inner bag film is composed of a laminate including at least a substrate and an adhesive layer, and the substrate contains polyolefin, so that the substrates of the inner bag film can be easily heat-sealed to each other and have excellent formability. Furthermore, because the substrates of the inner bag film can be easily heat-sealed to each other, they discovered that, for example, by preparing multiple cells containing battery elements of a semi-solid battery in an inner bag formed by the inner bag film and heat-sealing the substrates of the inner bag located on the outside of each cell to each other, the multiple cells can be fixed in the package by heat-sealing.

[0013] The present disclosure has been completed based on these findings and through further investigations. That is, the present disclosure provides the following aspects of the invention: An inner bag film for a semisolid battery, which is disposed between an exterior material of the semisolid battery and a battery element, the inner bag film for a semisolid battery being composed of a laminate including at least a substrate and an adhesive layer, and the substrate containing polyolefin.

[0014] According to the present disclosure, it is possible to provide a novel inner bag film that is disposed between an exterior material of a semi-solid battery and a battery element, the inner bag film being easily heat-sealed to the base materials of the inner bag film and having excellent formability. Furthermore, according to the present disclosure, it is also possible to provide a semi-solid battery using the inner bag film.

[0015] 1 is a schematic diagram showing an example of a cross-sectional structure of a packaging film for a semi-solid battery according to the present disclosure, FIG. 2 is a schematic diagram showing an example of a cross-sectional structure of an exterior material used in a semi-solid battery according to the present disclosure, and FIG. 3 is a schematic diagram showing an example of a cross-sectional structure of a semi-solid battery according to the present disclosure.

[0016] The inner bag film for a semi-solid battery of the present disclosure is an inner bag film for a semi-solid battery that is disposed between the exterior material of the semi-solid battery and the battery element, and is composed of a laminate including at least a substrate and an adhesive layer, and is characterized in that the substrate contains a polyolefin. By having this configuration, the inner bag film for a semi-solid battery of the present disclosure can easily heat-seal the substrates of the inner bag film to each other and has excellent formability.

[0017] The inner bag film for a semi-solid battery and the semi-solid battery of the present disclosure are described in detail below. In this disclosure, a numerical range indicated by "to" means "greater than or equal to" or "less than or equal to." For example, 2 to 15 mm means 2 mm or greater and 15 mm or less. In the numerical ranges described in this disclosure in stages, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Separately described upper and lower limits, upper and lower limits, or lower and upper limits may be combined to form a numerical range. In the numerical ranges described in this disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0018] In addition, in this disclosure, "semi-solid" refers to a material that is a mixture of a liquid phase and a solid phase, such as a particle suspension, a colloidal suspension, an emulsion, a gel, or a micelle, and a semi-solid battery uses semi-solid electrodes.

[0019] 1. Inner Bag Film for Semisolid Battery The inner bag film for a semisolid battery of the present disclosure is composed of a laminate including at least a substrate and an adhesive layer. Furthermore, the substrate contains a polyolefin. That is, the inner bag film for a semisolid battery of the present disclosure is a laminate film including at least a substrate containing a polyolefin and an adhesive layer. As shown in the schematic diagram of FIG. 3 , the inner bag film for a semisolid battery 1 of the present disclosure is disposed between the exterior material 3 and the battery element 4 of a semisolid battery 10.

[0020] As described above, in the case of semi-solid batteries, similar to general power storage devices, it is conceivable to connect a plurality of cells (single cells) to form a module (battery assembly) and house this in a package to form a single large semi-solid battery. In such a semi-solid battery module, since a plurality of cells are housed in the package, it is desirable to fix the plurality of cells together.

[0021] Furthermore, as described above, in film-like packaging materials for electricity storage devices, recesses are generally formed by cold forming, and electricity storage device elements such as electrodes and electrolyte are placed in the spaces formed by the recesses, and a heat-sealable resin layer is heat-sealed to obtain an electricity storage device in which the electricity storage device elements are housed inside the packaging material for electricity storage devices. For example, when such packaging materials are applied to semi-solid batteries, the inner bag film also requires excellent formability.

[0022] The inner bag film of the present disclosure uses a polyolefin substrate, which has heat-sealing properties and excellent formability, so that the substrates can be fixed together by heat fusion and has excellent formability.

[0023] In the semi-solid battery 10 of the present disclosure, the battery element 4 is housed in an inner bag formed by an inner bag film 1, and the inner bag housing the battery element 4 is housed in a package formed by an exterior material 3. The battery element 4 preferably has a structure sealed (hermetically sealed) by the inner bag film 1. Furthermore, the battery element 4 and the packaging film 1 preferably have a structure sealed (hermetically sealed) by the exterior material 3. That is, in the semi-solid battery 10, the battery element 4 preferably has a structure doubly sealed by the inner bag film 1 and the exterior material 3.

[0024] The battery element 4 can be sealed in the inner bag by covering the battery element 4 with the inner bag film 1 and heat-sealing the flange portion of the inner bag film 1. Furthermore, the inner bag with the sealed battery element 4 can be covered with the exterior material 3 and heat-sealed the flange portion of the exterior material 3 to seal the inner bag in the package.

[0025] The semi-solid battery 10 may be configured such that a plurality of inner bags each containing a battery element 4 are housed within a package. In this case, at least some of the inner bags each containing a battery element 4 can be fixed together by heat sealing. Specifically, at least two inner bags can be fixed together by heat sealing the base materials 11 of the inner bag film 1 constituting the inner bag together. The location where the packages are heat sealed together is not particularly limited, and examples include the peripheral edge 30a of the inner bag, the top surface of the inner bag, and the bottom surface of the inner bag. Furthermore, while it is not necessary to heat seal all of the inner bags contained within the package, it is preferable to heat seal all adjacent inner bags together from the viewpoint of sufficiently fixing the inner bags.

[0026] For example, as shown in FIG. 3 , in a semi-solid battery 10 according to the present disclosure, a battery element 4 is covered with an inner bag film 1 to form each cell 30. Furthermore, a plurality of cells 30 are covered with an exterior material 3. For example, in FIG. 3 , a flange portion (peripheral edge portion 3 a of the exterior material 3) of the exterior material 3 is formed near the periphery of the inner bag (cell 30) containing the battery element 4. The inner bag is then covered with the exterior material 3, and the flange portion of the exterior material 3 is heat-sealed to form a package containing the inner bag (cell 30). In this manner, in the present disclosure, the inner bag containing the battery element 4 can be the cell 30. Note that the use of the inner bag film 1 according to the present disclosure is not limited to the inner bag of a cell (single battery), and there are no particular limitations on the use of the inner bag film 1 as long as it is disposed between the exterior material 3 and the battery element 4 of the semi-solid battery 10.

[0027] In the semi-solid battery 10 shown in the schematic diagram of Figure 3, two cells 30 are housed in a package formed by an exterior material 3, and in each cell 30, a battery element 4 is housed in an inner bag formed by an inner bag film 1. When the semi-solid battery 10 is used as a module, the number of cells in the package may be two or more, and for example, 2 to 20 cells are housed in the package.

[0028] 3, each inner bag is made up of two inner bag films 1. In each cell 30, the adhesive layers 12 of the two inner bag films 1 are bonded together at the flange portions 30a, thereby sealing the battery element 4 in the inner bag. The inner bag may be made up of one inner bag film, or two or more inner bag films.

[0029] In Figure 3, the cells 30 are fixed together by heat sealing the base material 11 of the inner bag film 1 that forms the outer surface of the inner bag at the flange portion of the inner bag (the peripheral edge portion 30a of the inner bag).

[0030] The inner bag film 1 is used with the adhesive layer 12 (described later) facing inward (the surface in contact with the battery element 4). The exterior material 3 is used with the heat-sealable resin layer 35 (described later) facing inward (the surface in contact with the inner bag film 1).

[0031] As shown in Fig. 3, the metal terminal 2 protrudes outside the exterior packaging material 3. The metal terminal 2 is connected to each of the positive and negative electrodes of the battery element 4. Fig. 3 schematically shows an electrode 40 connected from the battery element 4 to the metal terminal 2. An adhesive film 21 for a metal terminal can be disposed between the metal terminal 2 and the exterior packaging material 3. By disposing the adhesive film 21 for a metal terminal, the adhesion between the metal terminal 2 and the heat-sealable resin layer 35 of the exterior packaging material 3 can be improved.

[0032] As shown in Figure 3, in the semi-solid battery 10, the inner bag film 1 (the adhesive layer 12) can be adhered to the electrode 40 at positions where the electrode 40 is present, and the inner bag films 1 (the adhesive layers 12) can be adhered to each other at positions where the electrode 40 is not present. In order to adhere the inner bag film 1 to the electrode 40, it is preferable that the adhesive layer 12 has adhesive properties to metal. Furthermore, in the semi-solid battery 10, at positions where the metal terminal 2 is present, the exterior material 3 (the heat-sealable resin layer 35) can be adhered to the metal terminal 2 via the adhesive film for metal terminal 21, and at positions where the metal terminal 2 is not present, the exterior material 3 (the heat-sealable resin layer 35) can be adhered to each other.

[0033] Although not shown, in the semi-solid battery 10, the end of the inner bag film 1 (at least a part of the peripheral edge 30a (flange portion) of the inner bag) may be located in the flange portion (peripheral edge 3a of the outer casing 3) of the outer casing 3. Specifically, the inner bag may be arranged so that the end of the inner bag film 1 is located at least in part of the position where the heat-sealable resin layers 35 of the outer casing 3 are heat-sealed to each other and / or at least in part of the position where the heat-sealable resin layer 35 of the outer casing 3 is brought into close contact with the metal terminal 2. Such an arrangement makes it possible to heat-seal the base material 11 of the inner bag film 1 and the heat-sealable resin layer 35 of the outer casing 3, thereby further firmly fixing the inner bag.

[0034] When the inner bag film 1 is located at the flange portion (peripheral edge portion 3a of the packaging material 3) of the packaging material 3, the adhesive layer 12 of the inner bag film 1 preferably has heat-sealing properties. Also, the adhesive layers 12 of the inner bag film 1 preferably have heat-sealing properties to each other. Also, as described above, the adhesive layer 12 of the inner bag film 1 preferably has adhesive properties to metal.

[0035] The inner bag film 1 for a semi-solid battery according to the present disclosure is composed of two or more layers, as shown in Fig. 1. Fig. 1 shows a schematic cross-sectional view of the inner bag film 1 for a semi-solid battery, which is composed of a laminate including a substrate 11 disposed on the exterior material 3 side and an adhesive layer 12 disposed on the battery element 4.

[0036] When the inner bag film 1 is composed of two or more layers, at least one of the two or more layers is a substrate 11 and at least one layer is an adhesive layer 12. The substrate 11 forms one surface of the inner bag film 1, and the adhesive layer 12 forms the other surface of the inner bag film 1. The inner bag film 1 is preferably composed of two to four layers, more preferably two to three layers, and even more preferably two layers.

[0037] Furthermore, in the manufacturing process of a semi-solid battery, gases such as CO2 are generated from the battery element during the initial charge / discharge process, aging process, etc. Furthermore, semi-solid batteries use semi-solid electrodes with fluidity, and the electrodes are prone to losing their shape when dried. For this reason, in semi-solid batteries, the battery element is housed in an exterior material (packaging), and the initial charge / discharge process, aging process, etc. are performed while the battery element maintains its shape. When the initial charge / discharge process and aging process are performed while the battery element is housed in an exterior material (packaging), measures such as providing holes in the packaging to release the generated gas are necessary. However, while providing holes in the packaging allows the gas generated from the battery element to be released during the manufacturing of the semi-solid battery, there is a problem in that after the semi-solid battery is manufactured, water vapor and the like are likely to penetrate through the holes in the packaging.

[0038] In contrast, the polyolefin contained in the base material of the inner bag film of the present disclosure has excellent CO2 permeability, which allows CO2 gas generated from the battery element housed in the inner bag film (more specifically, the battery element housed in the inner bag formed by the inner bag film) to be efficiently released to the outside.

[0039] From the viewpoint of more suitably exhibiting the effects of the present invention, the inner bag film 1 for a semi-solid battery of the present disclosure has a CO permeability of preferably about 6,000 cc / m at a temperature of 23° C. and a relative humidity of 0% RH for 24 hours. 2 More preferably, about 8,000 cc / m 2 More preferably, about 10,000 cc / m 2 The upper limit of the CO2 permeability is, for example, about 30,000 cc / m 2 Approximately 20,000cc / m 2 The preferred range of CO2 permeability is 6,000 to 30,000 cc / m 2 Approximately 6,000 to 20,000cc / m 2 Approximately 8,000 to 30,000cc / m 2 Approximately 8,000 to 20,000cc / m 2 Approximately 10,000~30,000cc / m 2 Approximately 10,000~20,000cc / m2 The degree of

[0040] Furthermore, from the viewpoint of more suitably exerting the effects of the invention of the present disclosure, the thickness (total thickness) of the inner bag film 1 for a semi-solid battery of the present disclosure is preferably 7 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and is preferably 30 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, and preferred ranges include about 7 to 30 μm, about 7 to 25 μm, about 7 to 20 μm, about 10 to 30 μm, about 10 to 25 μm, about 10 to 20 μm, about 15 to 30 μm, about 15 to 25 μm, and about 15 to 20 μm.

[0041] Furthermore, the inner bag film 1 for a semi-solid battery of the present disclosure preferably does not have holes for gas permeation. This is because the inner bag film 1 of the present disclosure has excellent CO permeability, making it unnecessary to provide such holes, and also because holes in the inner bag in the semi-solid battery 10 would allow water vapor to easily penetrate from the outside.

[0042] From the viewpoint of optimally achieving the effects of the present invention, it is preferable that the inner bag film 1 does not have a metal layer. This is because the presence of a metal layer even in a part of the inner bag film 1 inhibits CO2 permeability. The metal layer refers to a layer formed of metal, such as a metal foil or metal plate, with the thickness of the metal foil being, for example, about 10 to 200 μm, and the thickness of the metal plate being, for example, about 200 μm to several mm.

[0043] The inner bag film 1 for a semi-solid battery may contain various plastic compounding agents and additives for the purpose of improving or modifying, for example, processability, heat resistance, weather resistance, mechanical properties, dimensional stability, oxidation resistance, slipperiness, release properties, flame retardancy, mildew resistance, electrical properties, strength, etc. The content of these compounds may be any amount, ranging from trace amounts to several tens of percent, depending on the purpose. Common additives that may be included include, for example, antiblocking agents, lubricants, crosslinking agents, antioxidants, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, modifying resins, etc.

[0044] (Base material 11) The base material 11 included in the inner bag film 1 contains polyolefin. The base material 11 may contain only one type of polyolefin, or two or more types of polyolefin.

[0045] Specific examples of polyolefins include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; ethylene-α-olefin copolymers; polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); propylene-α-olefin copolymers; and ethylene-butene-propylene terpolymers. When the polyolefin resin is a copolymer, it may be a block copolymer or a random copolymer. These polyolefin resins may be used alone or in combination of two or more. Among these, polypropylene is particularly preferred due to its excellent heat-sealing properties, CO2 permeability, and heat resistance.

[0046] Furthermore, from the viewpoint of more suitably exerting the effects of the invention of the present disclosure, the substrate 11 is preferably formed from a polyolefin film such as a polyethylene film or a polypropylene film, more preferably from a stretched polyolefin film such as a stretched polyethylene film or a stretched polypropylene film, and particularly preferably from a stretched polypropylene film.

[0047] The substrate 11 preferably constitutes one surface of the inner bag film 1 (the surface opposite to the adhesive layer 12). The substrate 11 preferably contains polyolefin, and further, the heat-sealable resin layer 35 of the exterior material 3 preferably contains polyolefin. When the heat-sealable resin layer 35 and the substrate 11 contain the same type of resin, polyolefin, the heat-sealable resin layer 35 and the substrate 11 can be suitably heat-sealed. In this way, in the semi-solid battery 10, by arranging the heat-sealable resin layer 35 of the exterior material 3 and the substrate 11 of the inner bag film 1 so that they are in contact with each other, the heat-sealable resin layer 35 of the exterior material 3 and the substrate 11 of the inner bag film 1 can be heat-sealed to fix the inner bag film 1 within the exterior material 3.

[0048] The substrate 11 preferably has a CO2 permeability of about 6,000 cc / m2 at a temperature of 23°C and a relative humidity of 0% RH for 24 hours. 2 More preferably, about 8,000 cc / m 2 More preferably, about 10,000 cc / m 2 The upper limit of the CO2 permeability is, for example, about 30,000 cc / m 2 Approximately 20,000cc / m 2 The preferred range of CO2 permeability is 6,000 to 30,000 cc / m 2 Approximately 6,000 to 20,000cc / m 2 Approximately 8,000 to 30,000cc / m 2 Approximately 8,000 to 20,000cc / m 2 Approximately 10,000~30,000cc / m 2 Approximately 10,000~20,000cc / m 2 In addition, polyester film, polyvinylidene chloride, etc. have a CO2 permeability of 2,000 cc / m 2 The following is the result.

[0049] From the viewpoint of more suitably exerting the effects of the invention of the present disclosure, the thickness of the substrate 11 is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and is preferably 30 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, and preferred ranges include about 5 to 30 μm, about 5 to 25 μm, about 5 to 20 μm, about 10 to 30 μm, about 10 to 25 μm, about 10 to 20 μm, about 15 to 30 μm, about 15 to 25 μm, and about 15 to 20 μm.

[0050] (Adhesive Layer 12) The inner bag film 1 includes an adhesive layer 12. The adhesive layer 12 constitutes one surface of the inner bag film 1 and is a layer disposed on the battery element 4 side.

[0051] The adhesive layer 12 has adhesive properties. As described above, the adhesive layer 12 of the inner bag film 1 preferably has heat-sealing properties. The adhesive layers 12 also preferably have heat-sealing properties to each other. As described above, the adhesive layer 12 of the inner bag film 1 preferably has adhesive properties to metal.

[0052] The resin contained in the adhesive layer 12 is not particularly limited, as long as it has adhesive properties. Examples of resins contained in the adhesive layer 12 include resins such as polyolefin, polyamide, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, and phenolic resin, as well as thermoplastic resins such as modified versions of these resins. Among these, polypropylene, ethylene-methacrylic acid copolymer (EMAA), ethylene-methyl methacrylate copolymer (EMMA), and ethylene-methyl acrylate copolymer (EMA) are preferred. Specific examples of polyolefins include those exemplified for the substrate 11. The resin contained in the adhesive layer 12 may be one type only, or two or more types.

[0053] The resin contained in the adhesive layer 12 preferably has excellent CO2 permeability. The adhesive layer 12 preferably has a CO2 permeability of about 100,000 cc / m2 at a temperature of 23°C and a relative humidity of 0% RH for 24 hours. 2 or more, more preferably about 120,000 cc / m 2More preferably, about 150,000 cc / m 2 The upper limit of the CO2 permeability is, for example, about 400,000 cc / m 2 and more preferably about 300,000 cc / m 2 The preferred range of the CO2 permeability is 100,000 to 400,000 cc / m 2 Approximately 100,000~300,000cc / m 2 degree, 120,000~400,000cc / m 2 Approximately 120,000~300,000cc / m 2 Approximately 150,0000~400,000cc / m 2 Approximately 150,000~300,000cc / m 2 The degree of

[0054] From the viewpoint of more suitably exerting the effects of the present invention, the thickness of adhesive layer 12 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, and preferred ranges include about 2 to 20 μm, about 2 to 10 μm, about 2 to 8 μm, about 3 to 20 μm, about 3 to 10 μm, about 3 to 8 μm, about 4 to 20 μm, about 4 to 10 μm, and about 4 to 8 μm.

[0055] (Method for Manufacturing Inner Bag Film for Semisolid Battery) The method for manufacturing the inner bag film 1 is not particularly limited as long as an inner bag film for a semisolid battery can be obtained, and known or conventional film-forming methods and lamination methods can be applied. The inner bag film 1 can be manufactured by known film-forming and / or lamination methods, such as extrusion or co-extrusion, cast molding, T-die molding, cutting, or inflation. For example, films constituting each pre-fabricated layer may be laminated via an adhesive, a molten resin composition may be laminated onto a pre-fabricated layer by extrusion or co-extrusion, multiple layers may be simultaneously fabricated and laminated by melt-press bonding, or one or more resins may be applied and dried to coat other layers.

[0056] Furthermore, to improve adhesion, the surfaces of each layer constituting the inner bag film 1 may be subjected to a desired surface treatment in advance, as necessary. For example, pretreatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas or nitrogen gas, glow discharge treatment, and oxidation treatment using chemicals may be optionally performed to form a corona-treated layer, ozone-treated layer, plasma-treated layer, oxidation-treated layer, etc. Alternatively, various coating layers such as a primer coating layer, undercoat layer, anchor coating layer, adhesive layer, and vapor-deposited anchor coating layer may be optionally formed on the surface to form a surface-treated layer. The various coating layers may be, for example, resin compositions containing, as the main vehicle, isocyanate resins, polyester resins, polyamide resins, polyurethane resins, epoxy resins, phenolic resins, (meth)acrylic resins, polyvinyl acetate resins, polyolefin resins such as polyethylene or polypropylene, or copolymers or modified resins thereof, or cellulose resins.

[0057] Each layer constituting the inner bag film for a semi-solid battery can be further uniaxially or biaxially stretched by a conventionally known method using a tenter system, a tubular system, or the like, as required.

[0058] 2. Semi-Solid Battery In the semi-solid battery 10 of the present disclosure, a battery element 4 including at least a semi-solid positive electrode, a semi-solid negative electrode, and an electrolyte is housed in an inner bag formed by an inner bag film 1 for a semi-solid battery, and the inner bag is further housed in a package formed by an outer packaging material 3. As described above, the inner bag film 1 is composed of a laminate including at least a substrate 11 and an adhesive layer 12, and the substrate 11 contains polyolefin.

[0059] As described above, in the semi-solid battery 10 of the present disclosure, the battery element 4 is covered by the inner bag film 1, which is further covered by the exterior material 3. More specifically, in the semi-solid battery 10 of the present disclosure, the battery element 4 is housed in an inner bag formed by the inner bag film 1, and a plurality of inner bags housing the battery elements 4 are housed in a package formed by the exterior material 3. The battery element 4 preferably has a structure sealed (hermetically sealed) by the inner bag film 1. Furthermore, the battery element 4 and the inner bag film 1 preferably have a structure sealed (hermetically sealed) by the exterior material 3. The battery element 4 preferably has a structure doubly sealed by the inner bag film 1 and the exterior material 3.

[0060] The battery element 4 can be sealed in the inner bag by covering the battery element 4 with the inner bag film 1 and heat-sealing the flange portion of the inner bag film 1. Furthermore, the inner bag with the sealed battery element 4 can be covered with the exterior material 3 and heat-sealed the flange portion of the inner bag film 1 to seal the battery element in the inner bag. The inner bag film 1 is used with the adhesive layer 12 facing inward (the surface in contact with the battery element 4).

[0061] The semi-solid battery 10 may be configured such that a plurality of inner bags each containing a battery element 4 are housed within a package. In this case, at least some of the inner bags each containing a battery element 4 can be fixed together by heat sealing. Specifically, at least two inner bags can be fixed together by heat sealing the base materials 11 of the inner bag film 1 that constitute the inner bags. The position at which the packages are heat sealed together is not particularly limited, but the peripheral edge 30a of the inner bag is preferred. Furthermore, it is not necessary to heat seal all of the inner bags contained in the package together, but from the perspective of sufficiently fixing the inner bags, it is preferable to heat seal all adjacent inner bags together.

[0062] For example, as shown in FIG. 3 , in a semi-solid battery 10 according to the present disclosure, a battery element 4 is covered with an inner bag film 1 to form each cell 30. Furthermore, a plurality of cells 30 are covered with an exterior material 3. For example, in FIG. 3 , a flange portion (peripheral edge portion 3 a of the exterior material 3) of the exterior material 3 is formed near the periphery of the inner bag (cell 30) containing the battery element 4. The inner bag is then covered with the exterior material 3, and the flange portion of the exterior material 3 is heat-sealed to form a package containing the inner bag (cell 30). In this manner, in the present disclosure, the inner bag containing the battery element 4 can be the cell 30. Note that the use of the inner bag film 1 according to the present disclosure is not limited to the inner bag of a cell (single battery), and there are no particular limitations on the use of the inner bag film 1 as long as it is disposed between the exterior material 3 and the battery element 4 of the semi-solid battery 10.

[0063] In the semi-solid battery 10 shown in the schematic diagram of Figure 3, two cells 30 are housed in a package formed by an exterior material 3, and in each cell 30, a battery element 4 is housed in an inner bag formed by an inner bag film 1. When the semi-solid battery 10 is used as a module, the number of cells in the package may be two or more, and for example, 2 to 20 cells are housed in the package.

[0064] 3, each inner bag is made up of two inner bag films 1. In each cell 30, the adhesive layers 12 of the two inner bag films 1 are bonded together at the flange portions 30a, thereby sealing the battery element 4 in the inner bag. The inner bag may be made up of one inner bag film, or two or more inner bag films. When making an inner bag from a single inner bag film, the inner bag film 1 is folded in half, and the battery element 4 is sandwiched between the inner bag film 1 and sealed.

[0065] In Figure 3, the cells 30 are fixed together by heat sealing the base material 11 of the inner bag film 1 that forms the outer surface of the inner bag at the flange portion of the inner bag (the peripheral edge portion 30a of the inner bag).

[0066] The inner bag film 1 is used with the adhesive layer 12 facing inward (the surface in contact with the battery element 4). The exterior material 3 is used with the heat-sealable resin layer 35, which will be described later, facing inward (the surface in contact with the inner bag film 1).

[0067] As shown in Fig. 3, the metal terminal 2 protrudes outside the exterior packaging material 3. The metal terminal 2 is connected to each of the positive and negative electrodes of the battery element 4. Fig. 3 also shows a schematic diagram of an electrode 40 connected from the battery element 4 to the metal terminal 2. An adhesive film 21 for a metal terminal can be disposed between the metal terminal 2 and the exterior packaging material 3. By disposing the adhesive film 21 for a metal terminal, the adhesion between the metal terminal 2 and the heat-sealable resin layer 35 of the exterior packaging material 3 can be improved.

[0068] As shown in Figure 3, in the semi-solid battery 10, the inner bag film 1 (the adhesive layer 12) can be adhered to the electrode 40 at positions where the electrode 40 is present, and the inner bag films 1 (the adhesive layers 12) can be adhered to each other at positions where the electrode 40 is not present. In order to adhere the inner bag film 1 to the electrode 40, it is preferable that the adhesive layer 12 has adhesive properties to metal. Furthermore, in the semi-solid battery 10, at positions where the metal terminal 2 is present, the exterior material 3 (the heat-sealable resin layer 35) can be adhered to the metal terminal 2 via the adhesive film for metal terminal 21, and at positions where the metal terminal 2 is not present, the exterior material 3 (the heat-sealable resin layer 35) can be adhered to each other.

[0069] Although not shown, in the semi-solid battery 10, the end of the inner bag film 1 (at least a portion of the peripheral edge 30a (flange portion) of the inner bag) may be located at the flange portion of the exterior packaging material 3 (the peripheral edge 3a of the exterior packaging material 3). Specifically, the inner bag may be arranged so that the end of the inner bag film 1 is located at at least a portion of the position where the heat-sealable resin layers 35 of the exterior packaging material 3 are heat-sealed to each other and / or at least a portion of the position where the heat-sealable resin layer 35 of the exterior packaging material 3 is in close contact with the metal terminal 2. This arrangement allows the substrate 11 of the inner bag film 1 to be heat-sealed to the heat-sealable resin layer 35 of the exterior packaging material 3, thereby further firmly fixing the inner bag. Furthermore, the upper and lower surfaces of the inner bag may be heat-sealed to the thermoplastic resin 35 of the exterior packaging material 3. This allows the inner bag and the exterior packaging material to be fixed together, eliminating the need to form a flange portion on the inner bag, and also achieving the effect of miniaturizing (saving space) the semi-solid battery 10.

[0070] The semi-solid battery to which the inner bag film 1 of the present disclosure is applied is not particularly limited. In the semi-solid battery, the positive electrode and the negative electrode are electrochemically active semi-solids. The positive electrode and the negative electrode may have, for example, an active material and an electrolyte. The electrolyte may be, for example, a solvent or a solvent mixture to which a salt has been added. The positive electrode and the negative electrode may contain an additive. The positive and negative electrodes may include, for example, the active materials, compositions, and semi-solid suspensions described in U.S. Provisional Patent Application No. 61 / 787,382, entitled "Semi-Solid Electrodes Having High Rate Capability," and U.S. Provisional Patent Application No. 61 / 787,372, entitled "Asymmetric Battery Having a Semi-Solid Cathode and High Energy Density Anode."

[0071] The thickness of each of the positive electrode and the negative electrode can be, for example, about 250 to 2000 μm.

[0072] In a semi-solid battery, a separator is positioned between the positive and negative electrodes to separate the positive and negative sides of the battery element. The separator reduces the possibility of short circuits within the battery element. The separator is an insulator. The separator may be made of, for example, a ductile and elastic polymer. The separator may be made of, for example, polyolefin, polyvinyl chloride, nylon, fluorocarbon, or polystyrene.

[0073] [Packaging Material 3] In the present disclosure, for example, a metal can can be used as the packaging material 3. Meanwhile, as described above, a packaging material having a laminate structure including at least a substrate layer 31, a barrier layer 33, and a heat-sealable resin layer 35 in this order is also suitable as a packaging material 3 that can achieve a thinner and lighter body. FIG. 2 shows an example of the cross-sectional structure of such a packaging material 3, in which the substrate layer 31, an optional adhesive layer 32, the barrier layer 33, an optional adhesive layer 34, and the heat-sealable resin layer 35 are laminated in this order. In the packaging material 3, the substrate layer 31 is the outer layer, and the heat-sealable resin layer 35 is the innermost layer. During assembly of the semi-solid battery, the battery element 4 is sealed by bringing the heat-sealable resin layers 35 located on the periphery of the battery element 4 into contact with each other and heat-sealing them to seal the battery element 4. 3 illustrates the semi-solid battery 10 using an embossed exterior material 3 formed by embossing or the like, but the exterior material 3 may be an unformed pouch type. Pouch types include three-sided seal, four-sided seal, and pillow type, and any of these types may be used.

[0074] The thickness of the laminate constituting the exterior material 3 is not particularly limited, but from the viewpoint of cost reduction, improvement of energy density, etc., it may be, for example, about 210 μm or less, preferably about 190 μm or less, about 180 μm or less, about 155 μm or less, or about 120 μm or less. Furthermore, from the viewpoint of maintaining the function of the exterior material for a semi-solid battery, which is to protect the battery element, the thickness of the laminate constituting the exterior material for a semi-solid battery 3 is preferably about 35 μm or more, about 45 μm or more, or about 60 μm or more. Further, preferred ranges of the laminate constituting the semi-solid battery outer casing material 3 include, for example, about 35 to 210 μm, about 35 to 190 μm, about 35 to 180 μm, about 35 to 155 μm, about 35 to 120 μm, about 45 to 210 μm, about 45 to 190 μm, about 45 to 180 μm, about 45 to 155 μm, about 45 to 120 μm, about 60 to 210 μm, about 60 to 190 μm, about 60 to 180 μm, about 60 to 155 μm, and about 60 to 120 μm. In particular, when making the semi-solid battery lightweight and thin, about 60 to 155 μm is preferred, and when improving formability, about 155 to 190 μm is preferred.

[0075] (Substrate Layer 31) In the packaging material 3, the substrate layer 31 is a layer that functions as a substrate of the packaging material, and is a layer that forms the outermost layer side.

[0076] The material for forming the substrate layer 31 is not particularly limited, as long as it has insulating properties. Examples of materials for forming the substrate layer 31 include polyester, polyamide, epoxy, acrylic resin, fluororesin, polyurethane, silicone resin, phenol, polyetherimide, polyimide, and mixtures or copolymers thereof. Polyesters such as polyethylene terephthalate and polybutylene terephthalate have the advantage of being highly resistant to electrolyte and being less susceptible to whitening due to adhesion of electrolyte, and are therefore preferably used as materials for forming the substrate layer 31. Furthermore, polyamide film has excellent stretchability and can prevent whitening due to resin cracking of the substrate layer 31 during molding, and is therefore preferably used as materials for forming the substrate layer 31.

[0077] The base layer 31 may be formed of a uniaxially or biaxially stretched resin film or an unstretched resin film. Among them, a uniaxially or biaxially stretched resin film, especially a biaxially stretched resin film, is preferably used as the base layer 31 because its heat resistance is improved by oriented crystallization.

[0078] Among these, the resin film forming the base layer 31 is preferably nylon or polyester, and more preferably biaxially oriented nylon or biaxially oriented polyester.

[0079] The base material layer 31 may be formed by laminating resin films made of different materials to improve pinhole resistance and insulation when used as a package for a semi-solid battery. Specific examples include a multilayer structure in which a polyester film and a nylon film are laminated together, or a multilayer structure in which a biaxially oriented polyester film and a biaxially oriented nylon film are laminated together. When the base material layer 31 has a multilayer structure, the resin films may be bonded together via an adhesive, or may be directly laminated together without an adhesive. When bonding without an adhesive, examples of methods that bond the films in a hot-melt state include coextrusion, sand lamination, and thermal lamination.

[0080] The base layer 31 may be made low-friction to improve formability. When making the base layer 31 low-friction, the coefficient of friction of the surface is not particularly limited, but may be, for example, 1.0 or less. To make the base layer 31 low-friction, for example, matte treatment, formation of a thin film layer of a slip agent, or a combination thereof may be used.

[0081] The thickness of the base layer 31 is, for example, about 10 to 50 μm, and preferably about 15 to 30 μm.

[0082] (Adhesive Layer 32) In the packaging material 3, the adhesive layer 32 is a layer that is disposed on the base material layer 31 as necessary in order to impart adhesion to the base material layer 31. That is, the adhesive layer 32 is provided between the base material layer 31 and the barrier layer 33.

[0083] The adhesive layer 32 is formed of an adhesive capable of bonding the base material layer 31 and the barrier layer 33. The adhesive used to form the adhesive layer 32 may be a two-component curing adhesive or a one-component curing adhesive. The bonding mechanism of the adhesive used to form the adhesive layer 32 is not particularly limited, and may be any of a chemical reaction type, a solvent volatilization type, a hot melt type, a hot pressure type, or the like.

[0084] The resin component of the adhesive that can be used to form the adhesive layer 32 is preferably a polyurethane-based two-component curing adhesive; polyamide, polyester, or a blend resin of these with modified polyolefin, from the viewpoint of having excellent ductility, durability under high humidity conditions, yellowing prevention, and thermal degradation prevention during heat sealing, and of effectively suppressing a decrease in the laminate strength between the base material layer 31 and the barrier layer 33 and preventing delamination.

[0085] Furthermore, the adhesive layer 32 may be multi-layered with different adhesive components. When the adhesive layer 32 is multi-layered with different adhesive components, it is preferable to select a resin that has excellent adhesion to the base material layer 31 as the adhesive component disposed on the base material layer 31 side, and an adhesive component that has excellent adhesion to the barrier layer 33 as the adhesive component disposed on the barrier layer 33 side, from the viewpoint of improving the laminate strength between the base material layer 31 and the barrier layer 33. When the adhesive layer 32 is multi-layered with different adhesive components, specifically, the adhesive component disposed on the barrier layer 33 side is preferably an acid-modified polyolefin, a metal-modified polyolefin, a mixed resin of polyester and acid-modified polyolefin, a resin containing a copolymer polyester, or the like.

[0086] The thickness of the adhesive layer 32 is, for example, about 2 to 50 μm, and preferably about 3 to 25 μm.

[0087] (Barrier Layer 33) In the exterior packaging material 3, the barrier layer 33 is a layer that not only improves the strength of the exterior packaging material but also has the function of preventing water vapor, oxygen, light, and the like from penetrating into the semi-solid battery. The barrier layer 33 is preferably a metal layer, i.e., a layer formed of a metal. Specific examples of metals constituting the barrier layer 33 include aluminum, stainless steel, and titanium, and aluminum is preferred. The barrier layer 33 can be formed, for example, from a metal foil, a metal vapor deposition film, an inorganic oxide vapor deposition film, a carbon-containing inorganic oxide vapor deposition film, or a film provided with any of these vapor deposition films. It is preferably formed from a metal foil, and more preferably from an aluminum foil. From the viewpoint of preventing the occurrence of wrinkles or pinholes in the barrier layer 33 during the production of the exterior packaging material, the barrier layer is more preferably formed from a soft aluminum foil such as annealed aluminum (JIS H4160:1994 A8021H-O, JIS H4160:1994 A8079H-O, JIS H4000:2014 A8021P-O, JIS H4000:2014 A8079P-O).

[0088] The thickness of the barrier layer 33 is preferably about 10 to 200 μm, more preferably about 20 to 100 μm, about 20 to 45 μm, about 45 to 65 μm, or about 65 to 85 μm, from the viewpoint of making the exterior material thinner while making it less likely to develop pinholes during molding.

[0089] Furthermore, it is preferable that at least one surface, and preferably both surfaces, of the barrier layer 33 be chemically treated in order to stabilize adhesion, prevent dissolution and corrosion, etc. Here, chemical treatment refers to a treatment for forming a corrosion-resistant film on the surface of the barrier layer.

[0090] (Adhesive Layer 34) In the packaging material 3, the adhesive layer 34 is a layer that is provided as needed between the barrier layer 33 and the heat-sealable resin layer 35 in order to firmly bond the heat-sealable resin layer 35.

[0091] The adhesive layer 34 is formed of an adhesive capable of bonding the barrier layer 33 and the heat-sealable resin layer 35. The composition of the adhesive used to form the adhesive layer is not particularly limited, and examples include resin compositions containing acid-modified polyolefins. Acid-modified polyolefins are polymers modified by block or graft polymerization of polyolefins with an acid component. Examples of acid-modified polyolefins include the above-mentioned polyolefins, copolymers of the above-mentioned polyolefins with polar molecules such as acrylic acid or methacrylic acid, and polymers such as cross-linked polyolefins. Examples of acid components used for acid modification include carboxylic acids or anhydrides thereof, such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride. The acid-modified polyolefin may also be an acid-modified cyclic polyolefin. Acid-modified cyclic polyolefins are polymers obtained by copolymerizing a portion of the monomers constituting a cyclic polyolefin with an acid component, or by block or graft polymerization of an acid component with a cyclic polyolefin. The acid-modified cyclic polyolefins are the same as those described above. The acid component used for the acid modification is the same as the acid component used for the modification of the polyolefin.

[0092] Preferred acid-modified polyolefins include polyolefins modified with carboxylic acid or its anhydride, polypropylenes modified with carboxylic acid or its anhydride, maleic anhydride-modified polyolefins, and maleic anhydride-modified polypropylenes.

[0093] The thickness of the adhesive layer 34 is, for example, about 1 to 40 μm, and preferably about 2 to 30 μm.

[0094] (Heat-sealable resin layer 35) In the exterior packaging material 3, the heat-sealable resin layer 35 corresponds to the innermost layer, and is a layer that seals the battery element by heat-sealing the heat-sealable resin layers together when assembling the semi-solid battery.

[0095] The resin component used in the heat-sealable resin layer 35 is not particularly limited as long as it is heat-sealable, and examples thereof include polyolefin and cyclic polyolefin. By forming the heat-sealable resin layer 35 from polyolefin, good adhesion is achieved when the inner bag film 1 and the exterior material 3 are heat-sealed.

[0096] Specific examples of the polyolefin include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); and ethylene-butene-propylene terpolymers. Among these polyolefins, polyethylene and polypropylene are preferred.

[0097] The cyclic polyolefin is a copolymer of an olefin and a cyclic monomer, and examples of the olefin constituting the cyclic polyolefin include ethylene, propylene, 4-methyl-1-pentene, butadiene, and isoprene. Examples of the cyclic monomer constituting the cyclic polyolefin include cyclic alkenes such as norbornene; specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornadiene. Among these polyolefins, preferred are cyclic alkenes, and more preferred are norbornene. Another example of the constituting monomer is styrene.

[0098] Among these resin components, preferred are crystalline or amorphous polyolefins, cyclic polyolefins, and blend polymers thereof; more preferred are polyethylene, polypropylene, copolymers of ethylene and norbornene, and blend polymers of two or more of these.

[0099] The heat-sealable resin layer 35 may be formed of a single resin component alone, or may be formed of a blend polymer combining two or more resin components. The heat-sealable resin layer 35 may be formed of only one layer, or may be formed of two or more layers of the same or different resin components. It is particularly preferred that the adhesive layer 12 of the inner bag film 1 and the heat-sealable resin layer 35 use the same resin, as this improves adhesion between these layers.

[0100] The thickness of the heat-sealable resin layer 35 is not particularly limited, but may be about 2 to 2000 μm, preferably about 5 to 1000 μm, and more preferably about 10 to 500 μm. The thickness of the heat-sealable resin layer 35 is, for example, about 100 μm or less, preferably about 85 μm or less, and more preferably about 15 to 85 μm. For example, when the thickness of the adhesive layer 34 is 10 μm or more, the thickness of the heat-sealable resin layer 35 is preferably about 85 μm or less, and more preferably about 15 to 45 μm. For example, when the thickness of the adhesive layer 34 is less than 10 μm or when the adhesive layer 34 is not provided, the thickness of the heat-sealable resin layer 35 is preferably about 20 μm or more, and more preferably about 35 to 85 μm.

[0101] The present disclosure will be described in detail below with reference to examples and comparative examples, but the present disclosure is not limited to the examples.

[0102] <Production of Inner Bag Film for Semi-Solid Battery> (Examples 1 and 2) A two-layer inner bag film for a semi-solid battery (total thickness 20 μm) was produced by extrusion molding an adhesive layer (4 μm thick) of polypropylene (PP) or ethylene-methacrylic acid copolymer (EMAA) onto one side of an oriented polypropylene film (OPP) as a substrate (thickness 16 μm) to form the laminate structure shown in Table 1. The CO permeability of the substrate shown in Table 1 is the CO permeability at a temperature of 25°C and a relative humidity of 65% RH for 24 hours, and is the value described in "For Functional Food Packaging Materials, Kosuke Ishikawa, CMC Publishing Co., Ltd., Publication Date: April 2005, p. 73."

[0103] Comparative Example 1 A two-layer inner bag film for a semi-solid battery (total thickness 20 μm) was produced by extrusion molding an ethylene-methacrylic acid copolymer (EMAA) as an adhesive layer (thickness 8 μm) on a polyethylene terephthalate film as a substrate (thickness 12 μm) to obtain the laminated structure shown in Table 1. The CO permeability of the substrate shown in Table 1 is the CO permeability at a temperature of 25°C and a relative humidity of 65% RH for 24 hours, and is the value described in "For Functional Food Packaging Materials, Kosuke Ishikawa, CMC Publishing Co., Ltd., Publication Date: April 2005, p. 73."

[0104] <Evaluation of Heat-Sealing Properties of Inner Bag Film for Semi-Solid Battery> The heat-sealing properties between the substrates of the inner bag film for semi-solid battery were evaluated using the following method. The results are shown in Table 1. The substrates of the inner bag film for semi-solid battery were heat-sealed to each other, and the peel strength at 25°C was measured as follows. A sample was cut out from the inner bag film for semi-solid battery into a strip measuring 80 mm in length in the MD and 15 mm in width in the TD. The sample was folded in the MD with the substrate side facing inward, and heated and pressurized using a heat sealer (heat seal bar width: 7 mm) to prepare a measurement sample (40 mm in length in the MD). Next, the measurement sample was attached to a tensile tester, and the peel strength between the substrates was measured at a tensile speed of 50 mm / min and a gauge length of 50 mm. The maximum strength (N / 15 mm) at the time of peeling was used. The average value of three measurements was used. The heat sealing conditions for the measurement were fixed at a temperature of 170°C, a surface pressure of 0.4 MPa, and a pressing time of 0.3 seconds. The sealability evaluation criteria are as follows: A+: The peel strength between the substrates exceeded 1.0 N / 15 mm. A: The peel strength between the substrates was 0.1 N / 15 mm or more and 1.0 N / 15 mm or less. C: The peel strength between the substrates was less than 0.1 N / 15 mm, or the substrates were not heat-sealed.

[0105] <Moldability Evaluation> The moldability of the inner bag film for a semi-solid battery was evaluated by the following method. The results are shown in Table 1. The inner bag film for a semi-solid battery was cut into a rectangle with a length (MD direction) of 90 mm and a width (TD direction) of 150 mm to prepare a test sample. This sample was placed in a 25°C environment in a rectangular molding die (female die, the surface of which had a maximum height roughness (nominal value of Rz) of 3.2 μm as specified in Table 2 of the surface roughness standard for comparison in JIS B 0659-1:2002, Annex 1 (Reference), corner R2.0 mm, ridge R1.0 mm) with a bore of 31.6 mm (MD) x 54.5 mm (TD) and a corresponding molding die (male die, the surface of the ridgeline had a maximum height roughness (nominal value of Rz) of 1.6 μm as specified in Table 2 of the surface roughness standard for comparison in JIS B 0659-1:2002, Annex 1 (Reference), corner R2.0 mm, ridgeline R1.0 mm). The maximum height roughness (nominal Rz value) of the comparative surface roughness standard specimen, as specified in Table 2, is 3.2 μm. Using a corner R2.0 mm, ridge R1.0 mm, and a pressing pressure (surface pressure) of 0.25 MPa, the molding depth was changed in 0.5 mm increments from 0.5 mm, and cold molding (single-stage drawing) was performed on 10 samples each. The test sample was placed on a female mold so that the heat-sealable resin layer was positioned on the male mold side. The clearance between the male and female molds was 0.3 mm. After cold molding, the samples were irradiated with a penlight in a darkroom to check for pinholes or cracks in the inner bag film for semi-solid batteries through light transmission. The deepest molding depth at which no pinholes or cracks occurred in the inner bag film for semi-solid batteries in any of the 10 samples was defined as A mm, and the number of samples at which pinholes or the like occurred in the inner bag film for semi-solid batteries at the shallowest molding depth was defined as B. The value calculated using the following formula was rounded to two decimal places to determine the limit molding depth of the inner bag film for semi-solid batteries: Limit molding depth = A mm + (0.5 mm / 10 samples) × (10 samples - B samples).

[0106] <Heat Resistance Evaluation> The heat resistance of the inner bag film for semi-solid batteries was evaluated using the following method. The results are shown in Table 1. Peel strength in an 80°C environment was measured as follows. A sample was cut out from the inner bag film for semi-solid batteries into a 15 mm wide strip in the TD direction, folded with the adhesive layer facing inward, and bonded using a heat sealer (heat seal bar width: 7 mm) to prepare a measurement sample. Next, the measurement sample was attached to a tensile tester, and the adhesive layer-to-adhesive layer adhesive strength (peel strength) was measured at a tensile speed of 50 mm / min and a gauge length of 50 mm. The maximum strength (N / 15 mm) at the time of peeling was used. This was the average value of three measurements. The heat sealing conditions were fixed at a temperature of 150°C, a surface pressure of 0.4 MPa, and a pressing time of 0.3 seconds. The heat resistance evaluation criteria were as follows: A: Peel strength of 1.0 (N / 15 mm) or more; B: Peel strength of less than 1.0 (N / 15 mm).

[0107]

[0108] As described above, the present disclosure provides the following aspects of the invention. Item 1. An inner bag film for a semisolid battery, disposed between an exterior material of the semisolid battery and a battery element, the inner bag film for a semisolid battery being composed of a laminate including at least a substrate and an adhesive layer, the substrate containing polyolefin. Item 2. The inner bag film for a semisolid battery according to Item 1, wherein the substrate is composed of a stretched polypropylene film. Item 3. The inner bag film for a semisolid battery according to Item 1 or 2, wherein the adhesive layer has adhesive properties to metal. Item 4. The inner bag film for a semisolid battery according to any one of Items 1 to 3, wherein the thickness of the substrate is 5 μm or more and 30 μm or less. Item 5. The inner bag film for a semisolid battery according to any one of Items 1 to 4, wherein the thickness of the adhesive layer is 2 μm or more and 20 μm or less. Item 6. Item 7. The inner bag film for a semi-solid battery according to any one of items 1 to 5, wherein the inner bag film for a semi-solid battery does not have a metal layer formed of a metal. Item 7. The substrate has a CO2 permeability of 6000 cc / m2 or less at a temperature of 23°C and a relative humidity of 0% RH for 24 hours. 2The inner bag film for a semisolid battery according to any one of Items 1 to 6, wherein the outer casing is composed of a laminate including at least a base material layer, a barrier layer, and a heat-sealable resin layer laminated in this order. Item 9. The inner bag film for a semisolid battery according to any one of Items 1 to 8, wherein the inner bag film is not provided with holes for allowing gas to pass through. Item 10. A semisolid battery in which a battery element including at least a semisolid positive electrode, a semisolid negative electrode, and an electrolyte is housed in an inner bag formed by an inner bag film for a semisolid battery, and the inner bag is further housed in a packaging body formed by an outer casing, wherein the inner bag film for a semisolid battery is composed of a laminate including at least a base material and an adhesive layer, and the base material contains polyolefin. Item 11. The semisolid battery according to Item 10, wherein a plurality of the inner bags each housing the battery element are housed in the packaging body. Item 12. Item 12. The semi-solid battery according to item 11, wherein at least some of the inner bags housing the battery elements are fixed together by thermal fusion.

[0109] REFERENCE SIGNS LIST 1 Semisolid battery inner bag film 2 Metal terminal 3 Exterior material 3a Peripheral edge of exterior material 4 Battery element 10 Semisolid battery 11 Substrate 12 Adhesive layer 21 Metal terminal adhesive film 30 Cell 30a Peripheral edge of inner bag 31 Substrate layer 32 Adhesive layer 33 Barrier layer 34 Adhesive layer 35 Heat-sealable resin layer 40 Electrode

Claims

1. An inner bag film for a semi-solid battery, which is disposed between an exterior material of the semi-solid battery and a battery element, the inner bag film for a semi-solid battery being composed of a laminate including at least a substrate and an adhesive layer, the substrate including a polyolefin.

2. The inner bag film for a semi-solid battery according to claim 1, wherein the substrate is made of a stretched polypropylene film.

3. The inner bag film for a semi-solid battery according to claim 1 or 2, wherein the adhesive layer has adhesiveness to metal.

4. The inner bag film for a semi-solid battery according to claim 1 or 2, wherein the thickness of the substrate is from 5 μm to 30 μm.

5. The inner bag film for a semi-solid battery according to claim 1 or 2, wherein the thickness of the adhesive layer is from 2 μm to 20 μm.

6. The inner bag film for a semi-solid battery according to claim 1 or 2, wherein the inner bag film for a semi-solid battery does not have a metal layer formed of a metal.

7. The substrate has a CO2 permeability of 6000 cc / m2 at a temperature of 23°C and a relative humidity of 0% RH for 24 hours. 2 The inner bag film for a semi-solid battery according to claim 1 or 2.

8. The inner bag film for a semi-solid battery according to claim 1 or 2, wherein the exterior material is composed of a laminate having at least a base material layer, a barrier layer, and a heat-sealable resin layer laminated in this order.

9. The inner bag film for a semi-solid battery according to claim 1 or 2, wherein the inner bag film has no holes for allowing gas to pass therethrough.

10. A semi-solid battery in which a battery element having at least a semi-solid positive electrode, a semi-solid negative electrode, and an electrolyte is housed in an inner bag formed by an inner bag film for a semi-solid battery, and the inner bag is further housed in a packaging body formed by an exterior material, wherein the inner bag film for a semi-solid battery is composed of a laminate having at least a base material and an adhesive layer, and the base material contains polyolefin.

11. The semi-solid battery according to claim 10, wherein a plurality of the inner bags each containing the battery element are contained in the packaging body.

12. The semi-solid battery according to claim 11, wherein at least a portion of the inner bags housing the battery elements are fixed together by thermal fusion.

Citation Information

Patent Citations

  • Packaging material for battery, manufacturing method therefor, and battery

    WO2018066671A1

  • Adhesive film for metal terminals of all-solid-state batteries, metal terminal with adhesive film for metal terminals, all-solid-state battery using said adhesive film for metal terminals, and method for producing all-solid-state battery

    WO2022014718A1