Adhesive film for circuit connection, circuit connection structure, and method for producing same

The adhesive film with fluorene skeleton-containing epoxy resin and conductive particles addresses the need for HAST resistance and stable connections in the display industry, ensuring reliable circuit connections and preventing disconnection in organic LEDs by maintaining conduction and stability under varying pressures.

WO2024214701A1PCT designated stage expired Publication Date: 2024-10-17RESONAC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014419
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-09
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The increasing demand for panel quality reliability in the display industry, particularly in organic LEDs, requires adhesive films for circuit connections that provide sufficient High Accelerated Stress Test (HAST) resistance and stable connection resistance between electrodes, while also preventing circuit disconnection due to deformation of plastic substrates under pressure.

Method used

An adhesive film containing a fluorene skeleton-containing epoxy resin with a specific molecular weight and softening point, combined with conductive particles, is used to ensure HAST resistance and maintain conduction between electrodes, even at low pressures, by suppressing the flow of conductive particles and improving trapping efficiency.

Benefits of technology

The adhesive film achieves stable and reliable circuit connections with sufficient HAST resistance and conduction characteristics, preventing circuit disconnection and ensuring high connection reliability, suitable for both COG and COP mounting techniques.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014419_17102024_PF_FP_ABST
    Figure JP2024014419_17102024_PF_FP_ABST
Patent Text Reader

Abstract

This adhesive film for circuit connection comprises a thermosetting resin component and electroconductive particles. The thermosetting resin component contains a fluorene skeleton-containing epoxy resin represented by general formula (1) and an epoxy resin thermosetting agent. (In formula (1), RE is a skeleton residue derived from an epoxy resin, RP is a skeleton residue derived from a phenol compound having a fluorene skeleton, and n represents the number of repetitions.)
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive film for circuit connection, circuit connection structure and method for manufacturing the same

[0001] The present invention relates to an adhesive film for circuit connection, a circuit connection structure, and a method for producing the same.

[0002] In recent years, the display industry has seen a paradigm shift in display module technology from liquid crystal displays to organic light-emitting diodes (LEDs), and this has led to changes in the materials used to make panels.

[0003] Conventional liquid crystal displays use glass substrates as their substrates, and as circuit materials formed on the glass substrates, metals such as aluminum are used for the underlying circuit layers, and ITO (Indium Tin Oxide) is used for the surface electrodes. On the other hand, organic LEDs use flexible plastic substrates such as polyimide substrates as their substrates, and Ti is commonly used as the circuit material formed on the plastic substrates. Furthermore, a pressure-sensitive adhesive layer and a flexible member such as a polyethylene terephthalate (PET) substrate are usually disposed on the underside of the polyimide substrate to provide flexibility (see, for example, Patent Document 1).

[0004] Incidentally, in liquid crystal displays, from the viewpoints of fine pitch, light weight and thinness, so-called COG (chip on glass) mounting is adopted, in which various electronic components such as driver ICs are directly mounted on the glass substrate of the display panel. Also, as a COG mounting method, for example, a method is used in which a circuit connection structure is obtained by thermocompression bonding a liquid crystal driver IC onto a glass substrate via a circuit connection adhesive film having anisotropic conductivity in which conductive particles are dispersed in the adhesive.

[0005] JP 2016-054288 A

[0006] In recent years, the market has been demanding higher levels of reliability in panel quality. To improve reliability, it is necessary for the mounting assembly to have HAST resistance, which means that the connection resistance is less likely to increase even after severe tests such as HAST (Highly Accelerated Stress Test).

[0007] The main object of the present invention is to provide an adhesive film for circuit connection that can be used to connect circuit components together and can provide a circuit connection structure that has sufficient HAST resistance to stabilize the connection resistance between opposing electrodes.

[0008] In order to solve the above problems, one aspect of the present invention provides an adhesive film for circuit connection, which comprises a thermosetting resin component and conductive particles, wherein the thermosetting resin component contains a fluorene skeleton-containing epoxy resin represented by the following general formula (1), and an epoxy resin thermosetting agent: [In formula (1), R E is a backbone residue derived from an epoxy resin, and R P is a skeleton residue derived from a phenolic compound having a fluorene skeleton, and n represents the number of repetitions.

[0009] This adhesive film for circuit connection can connect circuit components to each other, thereby obtaining a circuit connection structure that has sufficient HAST resistance to stabilize the connection resistance between opposing electrodes. The reason for this effect is not entirely clear, but the inventors speculate as follows. It is believed that the adhesive film for circuit connection contains a fluorene skeleton-containing epoxy resin having the specific structure described above and an epoxy resin thermosetting agent, which ensures sufficient fluidity to fill voids between electrodes when connecting circuit components by thermocompression bonding, and that the rigid structure of the fluorene skeleton allows the elastic modulus of the cured product to be maintained after connection, thereby improving HAST resistance.

[0010] The fluorene skeleton-containing epoxy resin may have a weight average molecular weight of 5,000 to 8,000.

[0011] The fluorene skeleton-containing epoxy resin may have a softening point of 85 to 105°C.

[0012] Meanwhile, organic LEDs are also increasingly adopting COP (chip-on-plastic) mounting, in which a driving IC and other components are directly mounted on a plastic substrate. However, excessive pressure on the plastic substrate can cause problems associated with the deformation of the plastic substrate, such as deformation, cracking, and disconnection of Ti circuits mounted on a polyimide substrate. Therefore, COG mounting using a circuit-connecting adhesive film typically applies an area-equivalent pressure of 50 to 100 MPa to the bump electrodes of the IC chip. However, in COP mounting of organic LEDs, low pressures of, for example, 40 MPa or less are preferred to prevent circuit disconnections. Mounted structures fabricated under such low pressure conditions tend to have high connection resistance between opposing electrodes, making it difficult to obtain sufficient electrical conductivity.

[0013] When the fluorene skeleton-containing epoxy resin has the above-mentioned molecular weight and / or softening point, electrical continuity between opposing electrodes of a circuit connection structure can be easily ensured even when circuit components are connected at low pressure. Furthermore, when the adhesive film for circuit connection is made into a reel product, transferability to circuit components can be improved.

[0014] The conductive particles may be unevenly distributed on one side of the film, which facilitates improving the efficiency of capturing the conductive particles when connecting a circuit.

[0015] Another aspect of the present invention provides an adhesive film for circuit connection, comprising: a first adhesive layer containing conductive particles, a cured product of a photocurable resin component, and a first thermosetting resin component; and a second adhesive layer provided on the first adhesive layer and containing a second thermosetting resin component, wherein the second thermosetting resin component contains a fluorene skeleton-containing epoxy resin represented by the following general formula (1) and an epoxy resin thermosetting agent: [In formula (1), R E is a backbone residue derived from an epoxy resin, and R P is a skeleton residue derived from a phenolic compound having a fluorene skeleton, and n represents the number of repetitions.

[0016] This adhesive film for circuit connection can connect circuit components to obtain a circuit connection structure that has sufficient HAST resistance to stabilize the connection resistance between opposing electrodes. Furthermore, in the above-mentioned adhesive film for circuit connection, the first adhesive layer containing conductive particles contains a cured product of a photocurable resin component, which can suppress the flow of conductive particles during circuit connection, preventing the flowed conductive particles from bridging adjacent circuits and thereby reducing insulation, and further increasing the efficiency of capturing conductive particles.

[0017] In the adhesive film for circuit connection according to the other aspect, the fluorene skeleton-containing epoxy resin may have a weight average molecular weight of 5,000 to 8,000.

[0018] The fluorene skeleton-containing epoxy resin may have a softening point of 85 to 105°C.

[0019] When the fluorene skeleton-containing epoxy resin has the above-mentioned molecular weight and / or softening point, electrical continuity between opposing electrodes of a circuit connection structure can be easily ensured even when circuit components are connected at low pressure. Furthermore, when the adhesive film for circuit connection is made into a reel product, transferability to circuit components can be improved.

[0020] Another aspect of the present invention provides a method for manufacturing a circuit connection structure, comprising the steps of interposing the above-mentioned adhesive film for circuit connection between a first circuit member having a first electrode and a second circuit member having a second electrode, and thermocompression bonding the first circuit member and the second circuit member to electrically connect the first electrode and the second electrode to each other.

[0021] Another aspect of the present invention provides a circuit connection structure comprising: a first circuit member having a first electrode; a second circuit member having a second electrode; and a circuit connection portion disposed between the first circuit member and the second circuit member and electrically connecting the first electrode and the second electrode to each other, wherein the circuit connection portion comprises a cured product of the above-mentioned adhesive film for circuit connection.

[0022] According to the present invention, it is possible to provide an adhesive film for circuit connection that can be used to connect circuit components together and that can provide a circuit connection structure that has sufficient HAST resistance to stabilize the connection resistance between opposing electrodes. Furthermore, according to the present invention, it is possible to provide a circuit connection structure that uses the above-mentioned adhesive film for circuit connection, and a method for producing the same.

[0023] Fig. 1 is a schematic cross-sectional view showing one embodiment of an adhesive film for circuit connection. Fig. 2 is a schematic cross-sectional view showing one embodiment of a circuit connection structure. Fig. 3 is a schematic cross-sectional view showing one embodiment of a method for producing a circuit connection structure. Fig. 3(a) and Fig. 3(b) are schematic cross-sectional views showing each step.

[0024] In this specification, "(meth)acrylate" means at least one of acrylate and its corresponding methacrylate. The same applies to other similar expressions such as "(meth)acryloyl" and "(meth)acrylic acid." The materials exemplified below may be used alone or in combination of two or more, unless otherwise specified. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified. Numerical ranges indicated using "to" indicate a range that includes the numerical values ​​written before and after "to" as the minimum and maximum values, respectively. "A or B" means that either A or B may be present, or both may be present. "Room temperature" means 25°C.

[0025] In the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range may be replaced by the upper or lower limit of another numerical range. In addition, in the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced by a value shown in the examples.

[0026] [Adhesive Film for Circuit Connection] The adhesive film for circuit connection of this embodiment contains a thermosetting resin component and conductive particles, and the thermosetting resin component contains a fluorene skeleton-containing epoxy resin (hereinafter also referred to as a (C-F) component) represented by the following general formula (1), and an epoxy resin thermosetting agent.

[0027] [In formula (1), R E is a backbone residue derived from an epoxy resin, and R P is a skeleton residue derived from a phenolic compound having a fluorene skeleton, and n represents the number of repetitions.

[0028] The conductive particles may be unevenly distributed on one surface of the film. In this case, the adhesive film for circuit connection may include a region P in the thickness direction of the film containing a thermosetting resin component and a cured product of a photocurable resin component, and the conductive particles may be dispersed in this region P (the conductive particles may be arranged at intervals in the direction in which the film extends). The adhesive film for circuit connection may also have a region S adjacent to region P, which contains a thermosetting resin component containing a (C-F) component and an epoxy resin thermosetting agent. Region S may not contain a cured product of a photocurable resin component or conductive particles.

[0029] First, the component (C-F) will be described.

[0030] The component (C--F) can contain a bisphenol fluorene skeleton represented by the following general formula (2).

[0031] [In formula (2), R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, and may contain a cyclic structure.

[0032] The content of the skeleton may be 15 to 70 mol %, 30 to 70 mol %, 20 to 60 mol %, or 30 to 50 mol %. P and R ER having a bisphenol fluorene skeleton P and R E It can also be determined from the types and amounts of raw materials used to produce component (C-F).

[0033] The epoxy equivalent of component (C-F) may be 700 to 1500 g / eq, 750 to 1400 g / eq, 800 to 1200 g / eq, or 900 to 1100 g / eq. Here, the epoxy equivalent is the number of grams (g / eq) of resin containing 1 gram equivalent of epoxy groups, and is measured according to the method specified in JIS K-7236.

[0034] The component (CF) may have a weight average molecular weight of 5,000 to 8,000 from the viewpoint of obtaining HAST resistance even in low-pressure mounting and from the viewpoint of transferability.

[0035] In this specification, the weight-average molecular weight of the fluorene skeleton-containing epoxy resin refers to the weight-average molecular weight measured using gel permeation chromatography (GPC) under the following conditions: Detector: Hitachi High-Tech Science L-2490-RI Column: Gelpack GL-R440+R450+R400M Flow rate: 2.05 ml / min Concentration: 5 mg / ml Injection volume: 200 μl Column temperature: 40° C. Eluent: THF Standard sample: polystyrene

[0036] Furthermore, the component (CF) may have a softening point of 100 to 150° C. from the viewpoint of obtaining HAST resistance even in low-pressure mounting and from the viewpoint of transferability.

[0037] In this specification, the softening point of the fluorene skeleton-containing epoxy resin refers to the softening point measured using a thermomechanical analyzer (TMA) under the following conditions: Thermomechanical analyzer: Hitachi High-Tech Sciences TMA-7100, Penetration (Φ1 mm) mode, Heating rate: 10°C / min, Load: 98.1 mN

[0038] The component (C-F) can be produced by a method of reacting a phenol compound with a difunctional epoxy resin in the presence of a catalyst (see, for example, JP 2015-178592 A).

[0039] The phenol compound used as a raw material may include a fluorene skeleton-containing phenol compound represented by the following general formula (3) (hereinafter, also referred to as "phenol compound 3"). Note that the phenol compound used as a raw material may include other phenol compounds other than phenol compound 3.

[0040] [In formula (3), R 11 , R 12 , R 13 , R 14 and R 15 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, and may contain a cyclic structure.

[0041] The main component of the phenol compound 3 may be a compound in which m is 0 in general formula (3) (hereinafter also referred to as "compound 3-a"), and may contain a minor component in which m is 1 or more. An example of compound 3-a is 9,9-bis(4-hydroxyphenyl)fluorene (BPFL).

[0042] The content of compound 3-a in phenol compound 3 may be 50% by mass or more. The content of the compound in which m is 1 or 2 in phenol compound 3 (hereinafter also referred to as "compound 3-b") may be 0.01 to 1.0 area%, 0.05 to 0.7 area%, or 0.07 to 0.5 area%, when quantified in area% based on absorption at a wavelength of 272 nm by HPLC measurement.

[0043] In general formula (3), R 11 , R 12 , R 13 , R 14 and R 15may each independently be a methyl group, an ethyl group, a tert-butyl group, a cyclohexyl group, a phenyl group, an indanyl group, or an α-methylbenzyl group, or may be a methyl group, a phenyl group, or an α-methylbenzyl group.

[0044] In order to adjust the amount of fluorene skeleton introduced, a phenolic compound other than phenolic compound 3 may be used in combination in an amount of 70% by mass or less relative to the total amount of phenolic compounds. Examples of such phenolic compounds include bisphenol A, bisphenol F, bisphenol S, 4,4'-biphenol, tetramethyl bisphenol A, dimethyl bisphenol A, tetramethyl bisphenol F, dimethyl bisphenol F, tetramethyl bisphenol S, dimethyl bisphenol S, tetramethyl-4,4'-biphenol, dimethyl-4,4'-biphenol, 1-(4-hydroxyphenyl)-2-[4-(1,1-bis-(4-hydroxyphenyl)ethyl)phenyl]propane, 2,2'-methylene-bis(4-methyl-6-tert-butylphenol), 4,4'-butylidene-bis(3-methyl-6-tert-butylphenol), trishydroxyphenylmethane, resorcinol, and dihydric phenol compounds such as hydroquinone. These phenolic compounds can be used alone or in combination of two or more.

[0045] Examples of bifunctional epoxy resins include bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethylbisphenol A, tetramethylbisphenol F, tetramethylbisphenol S, dimethylbisphenol A, dimethylbisphenol F, dimethylbisphenol S, terpene diphenol, thiodiphenol, bisphenol fluorene, biscresol fluorene, bisphenol type epoxy resins obtained from dihydroxydiphenyl ether, etc., biphenol type epoxy resins obtained from biphenol, tetramethylbiphenol, dimethylbiphenol, etc., hydroquinone, methylhydroquinone, dibutylhydroquinone, resorcinol, benzenediol type epoxy resins obtained from methylresorcinol, etc., naphthalene type epoxy resins obtained from dihydroxynaphthalene, etc. These bifunctional epoxy resins can be used alone or in combination of two or more.

[0046] Furthermore, a bifunctional epoxy resin having a fluorene skeleton (hereinafter also referred to as "bifunctional epoxy resin F") may be used as the bifunctional epoxy resin. This allows the fluorene skeleton content in component (C-F) to be adjusted. Examples of bifunctional epoxy resin F include an epoxy resin represented by the following general formula (4) (hereinafter also referred to as "epoxy resin 4").

[0047] In formula (4), X represents a divalent group represented by the following general formula (5), Y represents a divalent group represented by the following general formula (6), and t represents the number of repetitions, and the average value (number average) is 0 to 5. Note that t is preferably 0 to 3, and more preferably 0 to 1. {In formula (5), R 21 represents a hydrogen atom or a methyl group, and s represents an integer of 0 to 3. {In formula (6), R 31 , R 32 , R 33 , and R 34 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, and may contain a cyclic structure.

[0048] The epoxy resin 4 may be an epoxy resin obtained by reacting a bisphenol fluorene with an epihalohydrin, in which s is 0 in the general formula (4).

[0049] The epoxy equivalent of the bifunctional epoxy resin F may be 230 to 500 g / eq, 230 to 400 g / eq, or 230 to 350 g / eq. The epoxy equivalent of the bifunctional epoxy resin F is preferably at least 100 g / eq lower, more preferably at least 400 g / eq lower, than the epoxy equivalent of the target component (C-F).

[0050] The catalyst that can be used in producing component (C-F) can be a known catalyst used in the production of epoxy resins, and examples of such known catalysts include phosphines such as triphenylphosphine and tris(2,6-dimethoxyphenyl)phosphine, quaternary phosphonium salts such as tetrabutylphosphonium benzotriazolate, tetra-n-butylphosphonium hexafluorophosphate, tetra-n-butylphosphonium o,o-diethylphosphorodithioate, methyltributylphosphonium dimethylphosphate, tetra-n-butylphosphonium tetrafluoroborate, n-butyltriphenylphosphonium bromide, and ethyltriphenylphosphonium iodide, imidazoles such as 2-ethyl-4-methylimidazole and 2-phenylimidazole, quaternary ammonium salts such as tetramethylammonium chloride and tetraethylammonium bromide, and tertiary amines such as triethylamine and benzyldimethylamine. Of these, phosphines and quaternary phosphonium salts are preferred. The amount of these catalysts used may be 0.005 to 1 part by mass, or 0.01 to 0.5 parts by mass, per 100 parts by mass of the total amount of phenol compounds.

[0051] A reaction solvent can be used when producing component (C-F). A non-reactive organic solvent can be used as the reaction solvent. Examples of the reaction solvent include aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, and acetone; ketones such as methyl ethyl ketone, methyl butyl ketone, dipropyl ketone, cyclopentanone, and cyclohexanone; and ethers such as dialkyl ethers, 2-ethoxyethyl ethyl ether, tetrahydrofuran, and dioxane. These organic solvents can be used alone or in combination of two or more. Among the above organic solvents, organic solvents having a boiling point of 70 to 170°C at normal pressure are preferred.

[0052] The amount of the organic solvent used may be 100 parts by mass or less relative to 100 parts by mass of the total amount of the phenol compound and the difunctional epoxy resin.

[0053] As the epoxy resin heat curing agent, any known curing agent capable of thermally curing an epoxy resin can be used, such as an amine-based curing agent, an acid anhydride curing agent, or a polyhydric phenol-based curing agent.

[0054] Examples of the amine curing agent include aliphatic and alicyclic amines such as bis(4-aminocyclohexyl)methane, bis(aminomethyl)cyclohexane, m-xylylenediamine, isophoronediamine, and 3,9-bis(3-aminopropyl)-2,4,8,10-tetraspiro[5,5]undecane; aromatic amines such as metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, and diaminoethylbenzene; and tertiary amines such as benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo-(5,4,0)-undecene-7, and 1,5-azabicyclo-(4,3,0)-nonene-7, as well as salts thereof.

[0055] Examples of the acid anhydride curing agent include aromatic acid anhydrides such as phthalic anhydride, trimellitic anhydride, and pyromellitic anhydride; cyclic aliphatic acid anhydrides such as tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyl-endo-methylenetetrahydrophthalic anhydride, dodecenylsuccinic anhydride, and trialkyltetrahydrophthalic anhydride; and carboxylic acid dianhydrides such as 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride and 1,2,3,4-butanetetracarboxylic dianhydride.

[0056] Examples of polyhydric phenol-based curing agents include hydroxybenzenes such as catechol, resorcinol, and hydroquinone, biphenols, binaphthols, bisphenols such as bisphenol F, bisphenol A, and bisphenol S, phenol novolaks, cresol novolaks, novolak compounds of dihydric phenols such as bisphenol A, alkylphenol novolaks, aralkylphenol novolaks, triazine ring-containing phenol novolaks, biphenylaralkylphenols, trishydroxyphenylmethane novolaks, aralkylnaphthalenediols, and dicyclopentadiene polyphenols.

[0057] In this embodiment, the component (C2): a thermal cationic polymerization initiator, which will be described later, can be used.

[0058] The epoxy resin heat curing agent may be used alone or in combination of two or more.

[0059] One embodiment of the adhesive film for circuit connection according to this embodiment is an adhesive film for circuit connection comprising a first adhesive layer (e.g., corresponding to region P) containing conductive particles, a cured product of a photocurable resin component, and a first thermosetting resin component, and a second adhesive layer (e.g., corresponding to region S) provided on the first adhesive layer and containing a second thermosetting resin component. In this adhesive film for circuit connection, the second thermosetting resin component can contain a (C-F) component and an epoxy resin thermosetting agent.

[0060] Fig. 1 is a schematic cross-sectional view showing one embodiment of an adhesive film for circuit connection according to the present embodiment. The adhesive film for circuit connection 10 shown in Fig. 1 (hereinafter sometimes simply referred to as "adhesive film 10") comprises a first adhesive layer 1 containing conductive particles 4 and an adhesive component 5 including a cured product of a photocurable resin component and a (first) thermosetting resin component, and a second adhesive layer 2 provided on the first adhesive layer 1 and containing a (second) thermosetting resin component. In the adhesive film for circuit connection 10, the second thermosetting resin component contained in the second adhesive layer 2 can contain a fluorene skeleton-containing epoxy resin represented by the above-mentioned general formula (1) and an epoxy resin thermosetting agent.

[0061] The adhesive film for circuit connection of this embodiment will be described below with reference to FIG.

[0062] The adhesive film 10 has conductive particles 4 dispersed in the first adhesive layer 1. Therefore, the adhesive film 10 can be an anisotropically conductive adhesive film for circuit connection. The adhesive film 10 can be interposed between a first circuit member having a first electrode and a second circuit member having a second electrode, and can be used to electrically connect the first electrode and the second electrode to each other by thermocompression bonding the first circuit member and the second circuit member.

[0063] <First Adhesive Layer> The first adhesive layer 1 contains conductive particles 4 (hereinafter sometimes referred to as "component (A)"), a cured product of a photocurable resin component (hereinafter sometimes referred to as "component (B)"), and a thermosetting resin component (hereinafter sometimes referred to as "component (C)"). The first adhesive layer 1 can be obtained, for example, by irradiating a composition layer made of a composition containing components (A), (B), and (C) with light energy to polymerize the components contained in component (B) and cure component (B). The first adhesive layer 1 contains component (A), a cured product of component (B), and an adhesive component 5 containing component (C). The cured product of component (B) may be a cured product obtained by completely curing component (B) or a cured product obtained by partially curing component (B). Component (C) is a component that can flow during circuit connection, such as an uncured curable resin component.

[0064] Component (A): Conductive Particles Component (A) is not particularly limited as long as it is a conductive particle, and may be, for example, a metal particle made of a metal such as Au, Ag, Pd, Ni, Cu, or solder, or a conductive carbon particle made of conductive carbon. Component (A) may also be a coated conductive particle having a core containing non-conductive glass, ceramic, or plastic (e.g., polystyrene), and a coating layer containing the metal or conductive carbon that coats the core. Among these, component (A) is preferably a metal particle formed of a heat-fusible metal, or a coated conductive particle having a core containing plastic and a coating layer containing a metal or conductive carbon that coats the core. Such coated conductive particles can easily deform the cured product of the thermosetting resin component by heating or applying pressure, thereby increasing the contact area between the electrodes and component (A) when electrically connecting the electrodes, thereby further improving the conductivity between the electrodes.

[0065] The conductive particles can be palladium-plated to facilitate low resistance in circuits having a Ti surface. In this case, palladium plating can be provided on the outermost surface of the conductive particles. Specifically, conductive particles can be used in which the surface of a plastic core is Ni-plated and the outermost surface is displacement-plated with Pd. These conductive particles may also have insulating fine particles supported on their surfaces to prevent short circuits between the conductive particles. Furthermore, to facilitate low resistance, a ceramic core material of 100 nm to 200 nm in size may be incorporated into the Ni plating process, followed by Pd plating, with insulating fine particles supported as needed.

[0066] Component (A) may be an insulating-coated conductive particle comprising the above-mentioned metal particles, conductive carbon particles, or coated conductive particles, and an insulating layer containing an insulating material such as a resin and coating the surface of the particle. When component (A) is an insulating-coated conductive particle, even if the content of component (A) is high, the particle surface has an insulating layer, which can suppress the occurrence of short circuits due to contact between components (A), and can also improve the insulation between adjacent electrode circuits. Component (A) can be used alone or in combination of two or more of the above-mentioned various conductive particles.

[0067] The maximum particle size of the (A) component must be smaller than the minimum electrode spacing (the shortest distance between adjacent electrodes). From the viewpoint of excellent dispersibility and conductivity, the maximum particle size of the (A) component may be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more. From the viewpoint of excellent dispersibility and conductivity, the maximum particle size of the (A) component may be 20 μm or less, 10 μm or less, or 5 μm or less. In this specification, the particle size of 300 random conductive particles (pcs) is measured by observation using a scanning electron microscope (SEM), and the largest value obtained is defined as the maximum particle size of the (A) component. Note that when the (A) component has protrusions or is not spherical, the particle size of the (A) component is defined as the diameter of a circle circumscribing the conductive particle in the SEM image.

[0068] The average particle size of component (A) may be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more from the viewpoint of excellent dispersibility and conductivity. The average particle size of component (A) may be 20 μm or less, 10 μm or less, or 5 μm or less from the viewpoint of excellent dispersibility and conductivity. In this specification, the particle size of 300 random conductive particles (pcs) is measured by observation using a scanning electron microscope (SEM), and the average value of the obtained particle sizes is defined as the average particle size.

[0069] Component (A) is preferably uniformly dispersed in first adhesive layer 1. From the viewpoint of obtaining a stable connection resistance, the particle density of component (A) in adhesive film 10 is 100 particles / mm 2 More than 1000 pieces / mm 2 More than 3000 pieces / mm 2 or more than 5000 pieces / mm 2 From the viewpoint of improving the insulating properties between adjacent electrodes, the particle density of the component (A) in the adhesive film 10 may be 100,000 particles / mm 2 Below, 70,000 pieces / mm 2 Below, 50,000 pieces / mm 2 or less, or 30,000 pieces / mm 2 It may be the following:

[0070] In the first adhesive layer 1, 80% or more, 90% or more, or 95% or more of the conductive particles may be separated from other conductive particles. The ratio (monodispersion rate) of conductive particles that are separated from adjacent conductive particles (monodispersion state) can be determined by observing the state of the conductive particles in the adhesive layer with a metallurgical microscope at a magnification of 200 times and using the following formula: Monodispersion rate (%) = (0.16 mm 2 Number of monodispersed conductive particles in the 2 (Number of conductive particles in the container) x 100

[0071] The content of the (A) component may be 1 mass% or more, 5 mass% or more, or 10 mass% or more, based on the total mass of the first adhesive layer, from the viewpoint of further improving conductivity. The content of the (A) component may be 60 mass% or less, 50 mass% or less, or 40 mass% or less, based on the total mass of the first adhesive layer, from the viewpoint of easily suppressing short circuits. When the content of the (A) component is within the above range, the effects of the present invention tend to be significantly exhibited. The content of the (A) component in the composition or composition layer (based on the total mass of the composition or composition layer) may be the same as the above range.

[0072] Component (B): Photocurable Resin Component Component (B) is not particularly limited as long as it is a resin component that cures upon irradiation with light, but from the viewpoint of achieving better connection resistance, it may be a resin component having radical curability. Component (B) may contain, for example, a radical polymerizable compound (hereinafter sometimes referred to as "component (B1)") and a photoradical polymerization initiator (hereinafter sometimes referred to as "component (B2)"). Component (B) may be a component consisting of component (B1) and component (B2).

[0073] Component (B1): Radically Polymerizable Compound Component (B1) is a compound that polymerizes by radicals generated from component (B2) upon irradiation with light (e.g., ultraviolet light). Component (B1) may be either a monomer or a polymer (or oligomer) obtained by polymerizing one or more types of monomers. Component (B1) may be used alone or in combination.

[0074] The component (B1) is a compound having a radical polymerizable group that reacts with a radical. Examples of the radical polymerizable group include a (meth)acryloyl group, a vinyl group, an allyl group, a styryl group, an alkenyl group, an alkenylene group, and a maleimide group. The number of radical polymerizable groups (the number of functional groups) contained in the component (B1) may be 2 or more from the viewpoint of easily obtaining a desired melt viscosity after polymerization, further improving the effect of reducing connection resistance, and providing better connection reliability, and may be 10 or less from the viewpoint of suppressing cure shrinkage during polymerization. Furthermore, in order to balance the crosslink density and cure shrinkage, in addition to a compound having the number of radical polymerizable groups within the above range, a compound having the number of radical polymerizable groups outside the above range may also be used.

[0075] From the viewpoint of suppressing the flow of the conductive particles, the component (B1) may contain, for example, a polyfunctional (difunctional or higher) (meth)acrylate. The polyfunctional (difunctional or higher) (meth)acrylate may be a difunctional (meth)acrylate, and the difunctional (meth)acrylate may be a difunctional aromatic (meth)acrylate.

[0076] Examples of polyfunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethoxylated polypropylene glycol di(meth)acrylate, and 1,3-butane. aliphatic (meth)acrylates such as diol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, glycerin di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, and ethoxylated 2-methyl-1,3-propanediol di(meth)acrylate;Aromatic (meth)acrylates such as ethoxylated bisphenol A di(meth)acrylate, propoxylated bisphenol A di(meth)acrylate, ethoxylated propoxylated bisphenol A di(meth)acrylate, ethoxylated bisphenol F di(meth)acrylate, propoxylated bisphenol F di(meth)acrylate, ethoxylated propoxylated bisphenol F di(meth)acrylate, ethoxylated fluorene di(meth)acrylate, propoxylated fluorene di(meth)acrylate, and ethoxylated propoxylated fluorene di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, ethoxylated propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol aliphatic (meth)acrylates such as pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated propoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tetra(meth)acrylate, ethoxylated propoxylated pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetraacrylate, and dipentaerythritol hexa(meth)acrylate; aromatic epoxy (meth)acrylates such as bisphenol-type epoxy (meth)acrylate, phenol novolac-type epoxy (meth)acrylate, and cresol novolac-type epoxy (meth)acrylate;

[0077] From the viewpoint of achieving both the effect of reducing connection resistance and the suppression of particle flow, the content of the polyfunctional (difunctional or higher) (meth)acrylate may be, for example, 40 to 100 mass %, 50 to 100 mass %, or 60 to 100 mass % based on the total mass of the component (B1).

[0078] The component (B1) may further contain a monofunctional (meth)acrylate in addition to a polyfunctional (difunctional or higher) (meth)acrylate. Examples of the monofunctional (meth)acrylate include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, butoxyethyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octylheptyl (meth)acrylate, and nonyl (meth)acrylate. Decyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, ethoxypolypropylene glycol (meth)acrylate, mono(2-(meth)acryloyloxy) aliphatic (meth)acrylates such as diethyl succinate; benzyl (meth)acrylate, phenyl (meth)acrylate, o-biphenyl (meth)acrylate, 1-naphthyl (meth)acrylate, 2-naphthyl (meth)acrylate, phenoxyethyl (meth)acrylate, p-cumylphenoxyethyl (meth)acrylate, o-phenylphenoxyethyl (meth)acrylate, 1-naphthoxyethyl (meth)acrylate, 2-naphthoxyethyl (meth)acrylate, phenoxypolyether aromatic (meth)acrylates such as ethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, phenoxy polypropylene glycol (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-hydroxy-3-(o-phenylphenoxy)propyl (meth)acrylate, 2-hydroxy-3-(1-naphthoxy)propyl (meth)acrylate, and 2-hydroxy-3-(2-naphthoxy)propyl (meth)acrylate;Examples include (meth)acrylates having an epoxy group such as glycidyl (meth)acrylate, (meth)acrylates having an alicyclic epoxy group such as 3,4-epoxycyclohexylmethyl (meth)acrylate, and (meth)acrylates having an oxetanyl group such as (3-ethyloxetan-3-yl)methyl (meth)acrylate;

[0079] The content of the monofunctional (meth)acrylate may be, for example, 0 to 60 mass %, 0 to 50 mass %, or 0 to 40 mass %, based on the total mass of the component (B1).

[0080] The cured product of component (B) may have, for example, a polymerizable group that reacts by a mechanism other than a radical. The polymerizable group that reacts by a mechanism other than a radical may be, for example, a cationically polymerizable group that reacts by a cation. Examples of the cationically polymerizable group include epoxy groups such as glycidyl groups, alicyclic epoxy groups such as epoxycyclohexylmethyl groups, and oxetanyl groups such as ethyloxetanylmethyl groups. The cured product of component (B) having a polymerizable group that reacts by a mechanism other than a radical can be introduced by using, for example, a (meth)acrylate having a polymerizable group that reacts by a mechanism other than a radical, such as a (meth)acrylate having an epoxy group, a (meth)acrylate having an alicyclic epoxy group, or a (meth)acrylate having an oxetanyl group, as component (B). From the viewpoint of improving reliability, the mass ratio of the (meth)acrylate having a polymerizable group that reacts by means other than radicals to the total mass of the component (B1) (mass (charge amount) of the (meth)acrylate having a polymerizable group that reacts by means other than radicals / total mass (charge amount) of the component (B1)) may be, for example, 0 to 0.7, 0 to 0.5, or 0 to 0.3.

[0081] The component (B1) may contain other radically polymerizable compounds in addition to polyfunctional (difunctional or higher) and monofunctional (meth)acrylates. Examples of other radically polymerizable compounds include maleimide compounds, vinyl ether compounds, allyl compounds, styrene derivatives, acrylamide derivatives, and nadimide derivatives. The content of other radically polymerizable compounds may be, for example, 0 to 40% by mass based on the total mass of the component (B1).

[0082] Component (B2): Photoradical Polymerization Initiator The component (B2) is a photopolymerization initiator that generates radicals upon irradiation with light having a wavelength in the range of 150 to 750 nm, preferably light having a wavelength in the range of 254 to 405 nm, and more preferably light having a wavelength of 365 nm (e.g., ultraviolet light). The component (B2) may be used alone or in combination.

[0083] The component (B2) decomposes when exposed to light to generate free radicals. In other words, the component (B2) is a compound that generates radicals when exposed to external light energy. The component (B2) may be a compound having an oxime ester structure, a bisimidazole structure, an acridine structure, an α-aminoalkylphenone structure, an aminobenzophenone structure, an N-phenylglycine structure, an acylphosphine oxide structure, a benzyl dimethyl ketal structure, an α-hydroxyalkylphenone structure, or the like. The component (B2) may be used alone or in combination with multiple compounds. From the viewpoints of easily obtaining a desired melt viscosity and of achieving a superior effect of reducing connection resistance, the component (B2) may be a compound having at least one structure selected from the group consisting of an oxime ester structure, an α-aminoalkylphenone structure, and an acylphosphine oxide structure.

[0084] Specific examples of the compound having an oxime ester structure include 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-o-benzoyloxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl)oxime, 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(o-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime), and the like.

[0085] Specific examples of compounds having an α-aminoalkylphenone structure include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-morpholinophenyl)-butanone-1, and the like.

[0086] Specific examples of compounds having an acylphosphine oxide structure include bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0087] From the viewpoint of suppressing the flow of the conductive particles, the content of the (B2) component may be, for example, 0.1 to 10 parts by mass, 0.3 to 7 parts by mass, or 0.5 to 5 parts by mass per 100 parts by mass of the (B1) component.

[0088] The content of the cured product of component (B) may be 1% by mass or more, 5% by mass or more, or 10% by mass or more, based on the total mass of the first adhesive layer, from the viewpoint of suppressing the flow of conductive particles. The content of the cured product of component (B) may be 50% by mass or less, 40% by mass or less, or 30% by mass or less, based on the total mass of the first adhesive layer, from the viewpoint of exhibiting low resistance in low-pressure mounting. When the content of the cured product of component (B) is within the above range, the effects of the present invention tend to be significantly exhibited. The content of component (B) in the composition or composition layer (based on the total mass of the composition or composition layer) may be the same as the above range.

[0089] Component (C): Thermosetting Resin Component The component (C) may contain, for example, a cationic polymerizable compound (hereinafter sometimes referred to as "component (C1)") and a thermal cationic polymerization initiator (hereinafter sometimes referred to as "component (C2)"). The component (C) may be a component consisting of components (C1) and (C2). The first thermosetting resin component and the second thermosetting resin component refer to the thermosetting resin components contained in the first adhesive layer and the second adhesive layer, respectively. The types, combinations, and contents of the components contained in the first thermosetting resin component and the second thermosetting resin component (e.g., component (C1), component (C2), etc.) may be the same or different from each other.

[0090] Component (C1): Cationic Polymerizable Compound Component (C1) is a compound that crosslinks by reacting with component (C2) under heat. Component (C1) refers to a compound that does not have a radically polymerizable group that reacts with a radical, and is not included in component (B1). Component (C1) may be a compound having one or more ring-opening polymerizable cyclic ether groups in the molecule, from the viewpoint of further improving the effect of reducing connection resistance and achieving better connection reliability. Component (C1) may be used alone or in combination. The compound having one or more ring-opening polymerizable cyclic ether groups in the molecule may be, for example, at least one selected from the group consisting of oxetane compounds and alicyclic epoxy compounds. Component (C1) preferably contains both at least one oxetane compound and at least one alicyclic epoxy compound, from the viewpoint of easily achieving the desired melt viscosity.

[0091] The oxetane compound as component (C1) can be used without any particular limitation as long as it has an oxetanyl group and no radically polymerizable group. Commercially available oxetane compounds include, for example, ETERNACOLL OXBP (trade name, manufactured by Ube Industries, Ltd.), OXSQ, OXT-121, OXT-221, OXT-101, and OXT-212 (trade names, manufactured by Toagosei Co., Ltd.). These compounds may be used alone or in combination.

[0092] The alicyclic epoxy compound as component (C1) can be any compound that has an alicyclic epoxy group (e.g., an epoxycyclohexyl group) and does not have a radically polymerizable group, and can be used without any particular limitation. Commercially available alicyclic epoxy compounds include EHPE3150, EHPE3150CE, CEL8010, CEL2021P, and CEL2081 (trade names, manufactured by Daicel Corporation). These compounds may be used alone or in combination.

[0093] The first adhesive layer 1, the composition for forming the first adhesive layer 1, and the composition layer may contain the component (C-F) as the component (C1). In this case, the content of the component (C-F) may be 5 to 30 mass%, 8 to 25 mass%, or 11 to 20 mass% based on the total amount of the component (C1).

[0094] Component (C2): Thermal Cationic Polymerization Initiator Component (C2) is a thermal polymerization initiator that generates an acid or the like upon heating to initiate polymerization. Component (C2) may be a salt compound composed of a cation and an anion. Component (C2) can be, for example, BF 4 - , B.R. 4 - (R represents a phenyl group substituted with two or more fluorine atoms or two or more trifluoromethyl groups), PF 6 - , SbF 6 - , AsF 6 - and onium salts such as sulfonium salts, phosphonium salts, ammonium salts, diazonium salts, iodonium salts, and anilinium salts having anions such as those listed above. Furthermore, when component (C1) contains an epoxy resin, the above-mentioned epoxy resin heat curing agents may be used as component (C2). As component (C2), one type may be used alone, or multiple types may be used in combination.

[0095] From the viewpoint of storage stability, the component (C2) is, for example, an anion containing boron as a constituent element, i.e., BF 4 - or BR 4 - (R represents a phenyl group substituted with two or more fluorine atoms or two or more trifluoromethyl groups). An anion containing boron as a constituent element may be a salt compound having BR 4 - and more specifically, tetrakis(pentafluorophenyl)borate.

[0096] The onium salt as component (C2) may be, for example, an anilinium salt, since it is resistant to substances that can inhibit cationic curing. Examples of anilinium salt compounds include N,N-dialkylanilinium salts such as N,N-dimethylanilinium salt and N,N-diethylanilinium salt.

[0097] Component (C2) may be an anilinium salt having an anion containing boron as a constituent element. Commercially available products of such salt compounds include CXC-1821 (trade name, manufactured by King Industries).

[0098] The content of the (C2) component may be, for example, 0.1 to 25 parts by mass, 1 to 20 parts by mass, 3 to 18 parts by mass, or 5 to 15 parts by mass per 100 parts by mass of the (C1) component, from the viewpoint of ensuring the formability and curability of the adhesive film for forming the first adhesive layer.

[0099] The content of the (C) component may be 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more, based on the total mass of the first adhesive layer, from the viewpoint of ensuring the curability of the adhesive film for forming the first adhesive layer. The content of the (C) component may be 70% by mass or less, 60% by mass or less, 50% by mass or less, or 40% by mass or less, based on the total mass of the first adhesive layer, from the viewpoint of ensuring the formability of the adhesive film for forming the first adhesive layer. When the content of the (C) component is within the above range, the effects of the present invention tend to be significantly exhibited. The content of the (C) component in the composition or composition layer (based on the total mass of the composition or composition layer) may be the same as the above range.

[0100] [Other Components] The first adhesive layer 1 may further contain other components in addition to the component (A), the cured product of the component (B), and the component (C). Examples of the other components include a film-forming component (hereinafter sometimes referred to as "component (D)"), a coupling agent (hereinafter sometimes referred to as "component (E)"), and a filler (hereinafter sometimes referred to as "component (F)").

[0101] Examples of the (D) component include phenoxy resin, polyester resin, polyamide resin, polyurethane resin, polyester urethane resin, acrylic rubber, and epoxy resin (solid at 25°C). These may be used alone or in combination. When a composition containing components (A), (B), and (C) further contains component (D), a composition layer (and further the first adhesive layer 1) can be easily formed from the composition. Among these, component (D) may be, for example, a phenoxy resin.

[0102] From the viewpoint of resin removal properties during mounting, the weight average molecular weight (Mw) of component (D) may be, for example, 5,000 to 200,000, 10,000 to 100,000, 20,000 to 80,000, or 40,000 to 60,000. Mw refers to a value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene.

[0103] The content of component (D) may be 1 mass % or more, 5 mass % or more, 10 mass % or more, or 20 mass % or more, and may be 70 mass % or less, 60 mass % or less, 50 mass % or less, or 40 mass % or less, based on the total mass of the first adhesive layer. The content of component (D) in the composition or composition layer (based on the total mass of the composition or composition layer) may be the same as the above range.

[0104] Examples of component (E) include silane coupling agents having organic functional groups such as (meth)acryloyl groups, mercapto groups, amino groups, imidazole groups, and epoxy groups; silane compounds such as tetraalkoxysilanes; tetraalkoxytitanate derivatives; and polydialkyltitanate derivatives. These may be used alone or in combination. By including component (E) in the first adhesive layer 1, adhesion can be further improved. Component (E) may be, for example, a silane coupling agent. The content of component (E) may be 0.1 to 10 mass% based on the total mass of the first adhesive layer. The content of component (E) in the composition or composition layer (based on the total mass of the composition or composition layer) may be within the above-mentioned range.

[0105] Examples of the component (F) include non-conductive fillers (e.g., non-conductive particles). The component (F) may be either an inorganic filler or an organic filler. Examples of inorganic fillers include inorganic fine particles such as metal oxide fine particles such as silica fine particles, alumina fine particles, silica-alumina fine particles, titania fine particles, and zirconia fine particles; and metal nitride fine particles. Examples of organic fillers include organic fine particles such as silicone fine particles, methacrylate-butadiene-styrene fine particles, acrylic-silicone fine particles, polyamide fine particles, and polyimide fine particles. These may be used alone or in combination. The component (F) may be, for example, silica fine particles. The content of the component (F) may be 0.1 to 10% by mass, based on the total mass of the first adhesive layer. The content of the component (F) in the composition or composition layer (based on the total mass of the composition or composition layer) may be the same as the above range.

[0106] [Other Additives] The first adhesive layer 1 may further contain other additives such as an ion scavenger, a softener, an accelerator, an anti-degradant, a colorant, a flame retardant, and a thixotropic agent. The content of the other additives may be, for example, 0.1 to 10 mass % based on the total mass of the first adhesive layer. The content of the other additives in the composition or composition layer (based on the total mass of the composition or composition layer) may be the same as the above range.

[0107] The thickness d1 of the first adhesive layer 1 may be, for example, 5 μm or less. The thickness d1 of the first adhesive layer 1 may be 4.5 μm or less or 4.0 μm or less. By having the thickness d1 of the first adhesive layer 1 be 5 μm or less, conductive particles can be captured more efficiently during circuit connection. The thickness d1 of the first adhesive layer 1 may be, for example, 0.1 μm or more, 0.5 μm or more, or 0.7 μm or more. The thickness d1 of the first adhesive layer 1 can be determined, for example, by sandwiching an adhesive film between two pieces of glass (thickness: approximately 1 mm), casting a resin composition consisting of 100 g of bisphenol A epoxy resin (trade name: jER811, manufactured by Mitsubishi Chemical Corporation) and 10 g of a curing agent (trade name: Epomount Curing Agent, manufactured by Refine Tech Co., Ltd.), polishing the cross section using a polishing machine, and measuring the cross section using a scanning electron microscope (SEM, trade name: SE-8020, manufactured by Hitachi High-Tech Science Corporation). 1, when a portion of the conductive particles 4 is exposed from the surface of the first adhesive layer 1 (for example, protruding toward the second adhesive layer 2), the distance from the surface 2a of the first adhesive layer 1 opposite the second adhesive layer 2 to the boundary S between the first adhesive layer 1 and the second adhesive layer 2, which is located in the space between adjacent conductive particles 4, 4 (the distance indicated by d1 in FIG. 1), is the thickness of the first adhesive layer 1, and the exposed portions of the conductive particles 4 are not included in the thickness of the first adhesive layer 1. The length of the exposed portions of the conductive particles 4 may be, for example, 0.1 μm or more and 5 μm or less.

[0108] <Second Adhesive Layer> The second adhesive layer 2 contains a (C) component. The (C) component in the second adhesive layer 2 (i.e., the second thermosetting resin component) can contain a fluorene skeleton-containing epoxy resin ((C-F) component) represented by the above-mentioned general formula (1) and an epoxy resin thermosetting agent. The (C) component may also contain a (C1) component other than the (C-F) component as the (C1) component. The (C) component may also contain the above-mentioned (C2) component as an epoxy resin thermosetting agent. The (C1) and (C2) components are the same as the (C1) and (C2) components used in the (C) component in the first adhesive layer 1 (i.e., the first thermosetting resin component). The second thermosetting resin component may be the same as or different from the first thermosetting resin component.

[0109] The (C--F) component contained in the second adhesive layer 2 may have a weight-average molecular weight of 5,000 to 8,000 from the viewpoint of obtaining HAST resistance even in low-pressure mounting and from the viewpoint of transferability.

[0110] Furthermore, component (CF) may have a softening point of 85 to 105° C. from the viewpoint of obtaining HAST resistance even in low-pressure mounting and from the viewpoint of transferability.

[0111] From the viewpoint of maintaining fluidity during curing, the second adhesive layer 2 preferably contains at least one oxetane compound as the component (C1) other than the component (CF).

[0112] From the viewpoint of maintaining high reliability, the content of the (C-F) component in the second adhesive layer 2 may be 10 to 40 mass %, 13 to 37 mass %, or 16 to 34 mass %, based on the total mass of the (C-F) component and the (C1) component other than the (C-F) component.

[0113] The content of component (C) may be 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more, based on the total mass of the second adhesive layer, from the viewpoint of maintaining reliability. The content of component (C) may be 70% by mass or less, 60% by mass or less, 50% by mass or less, or 40% by mass or less, based on the total mass of the second adhesive layer, from the viewpoint of preventing resin seepage problems in a reel, which is one embodiment of the supply form.

[0114] The second adhesive layer 2 may further contain other components and other additives than those in the first adhesive layer 1. Preferred aspects of the other components and other additives are the same as those of the first adhesive layer 1.

[0115] The content of component (D) may be 1 mass% or more, 5 mass% or more, or 10 mass% or more, based on the total mass of the second adhesive layer, and may be 80 mass% or less, 60 mass% or less, or 40 mass% or less.

[0116] The content of the component (E) may be 0.1 to 10% by mass based on the total mass of the second adhesive layer.

[0117] The content of component (F) may be 1 mass % or more, 5 mass % or more, or 10 mass % or more, based on the total mass of the second adhesive layer, and may be 70 mass % or less, 50 mass % or less, or 30 mass % or less.

[0118] The content of the other additives may be, for example, 0.1 to 10% by mass based on the total mass of the second adhesive layer.

[0119] The thickness d2 of the second adhesive layer 2 may be appropriately set depending on the height of the electrodes of the circuit components to be bonded. The thickness d2 of the second adhesive layer 2 may be 5 μm or more or 7 μm or more, and 15 μm or less or 11 μm or less, from the viewpoint of being able to sufficiently fill the space between the electrodes and seal the electrodes, thereby obtaining better connection reliability. The thickness d2 of the second adhesive layer 2 can be determined, for example, by a method similar to the method for measuring the thickness d1 of the first adhesive layer 1. Furthermore, when a portion of the conductive particles 4 is exposed from the surface of the first adhesive layer 1 (e.g., protruding toward the second adhesive layer 2), the distance (d2 in FIG. 1 ) from the surface 3 a of the second adhesive layer 2 opposite the first adhesive layer 1 side to the boundary S between the first adhesive layer 1 and the second adhesive layer 2, which is located in the space between adjacent conductive particles 4, 4, is the thickness of the second adhesive layer 2.

[0120] The thickness of the adhesive film 10 (the sum of the thicknesses of all layers constituting the adhesive film 10; in Figure 1, the sum of the thickness d1 of the first adhesive layer 1 and the thickness d2 of the second adhesive layer 2) may be, for example, 5 μm or more or 8 μm or more, and may be 30 μm or less or 20 μm or less.

[0121] When the adhesive film for circuit connection of this embodiment has the above-mentioned regions P and S, the range of region P in the thickness direction of the film can be set in the same manner as the thickness of the first adhesive layer described above. The contents of each component in region P can also be set in the same manner as the first adhesive layer. The range of region S in the thickness direction of the film can be set in the same manner as the thickness of the above-mentioned second adhesive layer. The contents of each component in region S can also be set in the same manner as the second adhesive layer.

[0122] The minimum melt viscosity of the adhesive film 10 is 450 to 1600 Pa·s. The minimum melt viscosity of the adhesive film 10 may be 500 Pa·s or more, 600 Pa·s or more, 700 Pa·s or more, or 800 Pa·s or more. When the minimum melt viscosity of the adhesive film 10 is 450 Pa·s or more, deformation of the plastic substrate during thermocompression bonding can be suppressed, making it possible to prevent circuit breakage. The minimum melt viscosity of the adhesive film 10 may be 1500 Pa·s or less, 1400 Pa·s or less, 1300 Pa·s or less, 1200 Pa·s or less, 1100 Pa·s or less, or 1000 Pa·s or less. When the minimum melt viscosity of the adhesive film 10 is 1600 Pa·s or less, it is possible to suppress a decrease in the removability of the resin during circuit connection, thereby reducing the connection resistance between opposing electrodes of the circuit connection structure and ensuring good conductive properties. The minimum melt viscosity of the adhesive film can be determined, for example, by the following method. (Method for measuring minimum melt viscosity) Each adhesive film is laminated using a laminator to a thickness of 500 μm or more to obtain a laminate. The release-treated PET is peeled from the obtained laminate and cut into a 10.0 mm x 10.0 mm piece to obtain a measurement sample. The minimum melt viscosity of the obtained measurement sample is measured using a viscoelasticity measuring device (trade name: ARES-G2, manufactured by TA Instruments, heating rate: 10°C / min).

[0123] In the adhesive film 10, the second adhesive layer 2 is usually thicker than the first adhesive layer 1. Therefore, the minimum melt viscosity of the adhesive film 10 tends to vary depending on the second adhesive layer 2. The minimum melt viscosity of the adhesive film 10 can be adjusted, for example, by adjusting the type and content of the constituent components (particularly, component (D)) contained in the second adhesive layer 2. The minimum melt viscosity of the adhesive film 10 can also be adjusted, for example, by using a component (F) with a small particle size. The minimum melt viscosity of the adhesive film 10 tends to increase by using a component (F) with a small particle size.

[0124] In the adhesive film 10, conductive particles 4 are dispersed in the first adhesive layer 1. Therefore, the adhesive film 10 is an anisotropically conductive adhesive film having anisotropic conductivity. The adhesive film 10 is interposed between a first circuit member having a first electrode and a second circuit member having a second electrode, and is used to electrically connect the first electrode and the second electrode to each other by thermocompression bonding the first circuit member and the second circuit member.

[0125] The adhesive film 10 can ensure sufficient electrical continuity between opposing electrodes of a circuit connection structure and maintain sufficient insulation between adjacent circuits, even when connecting circuit components with low pressure. Furthermore, the adhesive film 10 can provide a circuit connection structure with sufficient HAST resistance to stabilize the connection resistance between opposing electrodes. Such an adhesive film for circuit connection can be suitably used for COP mounting. More specifically, it can be suitably used for connecting a plastic substrate on which circuit electrodes are formed in an organic EL display to an IC chip such as a driver IC.

[0126] Although the adhesive film of this embodiment has been described above, the present invention is not limited to the above embodiment.

[0127] The adhesive film may be, for example, composed of two layers, a first adhesive layer and a second adhesive layer, or may be composed of three or more layers including two layers, a first adhesive layer and a second adhesive layer. The adhesive film may further include, for example, a third adhesive layer provided on the side of the first adhesive layer opposite to the second adhesive layer.

[0128] The third adhesive layer contains component (C). The components (C1) and (C2) used in component (C) (i.e., the third thermosetting resin component) in the third adhesive layer are similar to the components (C1) and (C2) used in component (C) (i.e., the first thermosetting resin component) in the first adhesive layer 1, and therefore detailed description thereof will be omitted here. The third thermosetting resin component may be the same as or different from the first thermosetting resin component. The third thermosetting resin component may be the same as or different from the second thermosetting resin component.

[0129] The third thermosetting resin component may contain the component (C-F) as the component (C1). In this case, the content of the component (C-F) may be 5 to 30 mass%, 8 to 27 mass%, or 11 to 24 mass% based on the total amount of the component (C1).

[0130] The content of the (C) component may be 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more, based on the total mass of the third adhesive layer, from the viewpoint of imparting good transferability and peel resistance. The content of the (C) component may be 70% by mass or less, 60% by mass or less, 50% by mass or less, or 40% by mass or less, based on the total mass of the third adhesive layer, from the viewpoint of imparting good half-cut property and blocking resistance (suppression of resin bleeding from the reel).

[0131] The third adhesive layer may further contain other components and other additives than those in the first adhesive layer 1. Preferred aspects of the other components and other additives are the same as those of the first adhesive layer 1.

[0132] The content of component (D) may be 10% by mass or more, 20% by mass or more, or 30% by mass or more, based on the total mass of the third adhesive layer, and may be 80% by mass or less, 70% by mass or less, or 60% by mass or less.

[0133] The content of the component (E) may be 0.1 to 10% by mass based on the total mass of the third adhesive layer.

[0134] The content of component (F) may be 1 mass% or more, 3 mass% or more, or 5 mass% or more, based on the total mass of the third adhesive layer, and may be 50 mass% or less, 40 mass% or less, or 30 mass% or less.

[0135] The content of the other additives may be, for example, 0.1 to 10% by mass based on the total mass of the third adhesive layer.

[0136] The thickness of the third adhesive layer may be appropriately set depending on the minimum melt viscosity of the adhesive film, the height of the electrodes of the circuit components to be bonded, etc. The thickness of the third adhesive layer is preferably smaller than the thickness d2 of the second adhesive layer 2. The thickness of the third adhesive layer may be 0.2 μm or more and 3.0 μm or less, from the viewpoint of being able to sufficiently fill the space between the electrodes and seal the electrodes, thereby obtaining better connection reliability. The thickness of the third adhesive layer can be determined, for example, by a method similar to the method for measuring the thickness d1 of the first adhesive layer 1.

[0137] The adhesive film for circuit connection in the above embodiment may be an anisotropically conductive adhesive film, or may be a conductive adhesive film without anisotropic conductivity.

[0138] <Method of Manufacturing an Adhesive Film for Circuit Connection> A method of manufacturing an adhesive film for circuit connection in one embodiment may include, for example, a step of irradiating a composition layer made of a composition containing components (A), (B), and (C) (first thermosetting resin component), and optionally other components, with light to form a first adhesive layer (first step), and a step of laminating a second adhesive layer containing component (C) (second thermosetting resin component) and optionally other components on the first adhesive layer (second step). The manufacturing method may further include a step of laminating a third adhesive layer containing component (C) (third thermosetting resin component) and optionally other components on the layer of the first adhesive layer opposite the second adhesive layer (third step). In this case, either the second step or the third step may be performed first. When the third step is performed first, the third adhesive layer is laminated on the side of the first adhesive layer opposite the side on which the second adhesive layer will be laminated.

[0139] In the first step, for example, a composition containing components (A), (B), and (C), as well as other components added as needed, is first dissolved or dispersed in an organic solvent by stirring, mixing, kneading, or the like to prepare a varnish composition (a first adhesive composition in a varnish form). The varnish composition is then applied to a release-treated substrate using a knife coater, roll coater, applicator, comma coater, die coater, or the like, and the organic solvent is then volatilized by heating to form a composition layer composed of the composition on the substrate. The thickness of the final first adhesive layer (first adhesive film) can be adjusted by adjusting the amount of varnish composition applied. Subsequently, the composition layer composed of the composition is irradiated with light to cure component (B) in the composition layer, thereby forming a first adhesive layer on the substrate. This first adhesive layer can be referred to as a first adhesive film.

[0140] The organic solvent used in preparing the varnish composition is not particularly limited as long as it has the property of being able to uniformly dissolve or disperse each component. Examples of such organic solvents include toluene, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, propyl acetate, butyl acetate, etc. These organic solvents can be used alone or in combination of two or more. The stirring, mixing, or kneading in preparing the varnish composition can be performed using, for example, a mixer, a kneading machine, a three-roll mill, a ball mill, a bead mill, a homodisper, etc.

[0141] The substrate is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent. Examples of such substrates include substrates (e.g., films) made of oriented polypropylene (OPP), polyethylene terephthalate (PET), polyethylene naphthalate, polyethylene isophthalate, polybutylene terephthalate, polyolefin, polyacetate, polycarbonate, polyphenylene sulfide, polyamide, polyimide, cellulose, ethylene-vinyl acetate copolymer, polyvinyl chloride, polyvinylidene chloride, synthetic rubber, liquid crystal polymer, etc.

[0142] The heating conditions for volatilizing the organic solvent from the varnish composition applied to the substrate can be appropriately set depending on the organic solvent used, etc. The heating conditions may be, for example, 40 to 120°C for 0.1 to 10 minutes.

[0143] A portion of the solvent may remain in the first adhesive layer without being removed. The content of the solvent in the first adhesive layer may be, for example, 10 mass % or less based on the total mass of the first adhesive layer.

[0144] For the light irradiation in the curing step, it is preferable to use irradiation light (e.g., ultraviolet light) having a wavelength in the range of 150 to 750 nm. Light irradiation can be carried out using, for example, a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a metal halide lamp, an LED light source, or the like. The integrated light amount of light irradiation can be set as appropriate, but is, for example, 500 to 3000 mJ / cm. 2 It may be.

[0145] The second step is a step of laminating a second adhesive layer on the first adhesive layer. In the second step, for example, a second adhesive layer is first formed on a substrate in the same manner as the first step, except that component (C) and other components added as needed are used and light irradiation is not performed, thereby obtaining a second adhesive film. Next, the first adhesive film and the second adhesive film are bonded together to laminate the second adhesive layer on the first adhesive layer. In addition, in the second step, for example, a varnish composition (varnish-like second adhesive composition) obtained using component (C) and other components added as needed can be applied to the first adhesive layer, and the organic solvent can be volatilized to laminate the second adhesive layer on the first adhesive layer.

[0146] Examples of methods for bonding the first adhesive film and the second adhesive film include hot pressing, roll lamination, vacuum lamination, etc. Lamination can be performed, for example, under temperature conditions of 0 to 80°C.

[0147] A portion of the solvent may remain in the second adhesive layer without being removed. The content of the solvent in the second adhesive layer may be, for example, 10 mass % or less based on the total mass of the second adhesive layer.

[0148] The third step is a step of laminating a third adhesive layer on the layer of the first adhesive layer opposite the second adhesive layer. In the third step, for example, a third adhesive layer is first formed on a substrate in the same manner as in the second step to obtain a third adhesive film. Next, the third adhesive layer can be laminated on the layer of the first adhesive layer opposite the second adhesive layer by laminating the third adhesive film on the side of the first adhesive film opposite the second adhesive layer. In the third step, for example, a varnish composition (a varnish-like third adhesive composition) can also be applied to the layer of the first adhesive layer opposite the second adhesive layer, and the organic solvent can be volatilized, similar to the second step, to laminate the third adhesive layer on the first adhesive layer. The lamination method and conditions are the same as in the second step.

[0149] A portion of the solvent may remain in the third adhesive layer without being removed. The content of the solvent in the third adhesive layer may be, for example, 10 mass % or less based on the total mass of the third adhesive layer.

[0150] <Circuit Connection Structure and Manufacturing Method Thereof> Hereinafter, a circuit connection structure using the above-described adhesive film for circuit connection 10 as the circuit connecting material and a manufacturing method therefor will be described.

[0151] Fig. 2 is a schematic cross-sectional view showing one embodiment of a circuit connection structure. As shown in Fig. 2, a circuit connection structure 20 includes a first circuit board 11 and a first circuit member 13 having a first electrode 12 formed on a main surface 11a of the first circuit board 11, a second circuit board 14 and a second circuit member 16 having a second electrode 15 formed on a main surface 14a of the second circuit board 14, and a circuit connection portion 17 disposed between the first circuit member 13 and the second circuit member 16 and electrically connecting the first electrode 12 and the second electrode 15 to each other.

[0152] The first circuit member 13 and the second circuit member 16 may be the same or different. The first circuit member 13 and the second circuit member 16 may be a glass or plastic substrate on which circuit electrodes are formed; a printed wiring board; a ceramic wiring board; a flexible wiring board; an IC chip such as a driving IC; or the like. The first circuit board 11 and the second circuit board 14 may be formed from an inorganic material such as a semiconductor, glass, or ceramic; an organic material such as polyimide or polycarbonate; or a composite material such as glass / epoxy. The first circuit board 11 may be a plastic substrate. The first circuit member 13 may be, for example, a plastic substrate (a plastic substrate made of an organic material such as polyimide, polycarbonate, polyethylene terephthalate, or cycloolefin polymer) on which circuit electrodes are formed, and the second circuit member 16 may be, for example, an IC chip such as a driving IC. The plastic substrate on which electrodes are formed may be a plastic substrate on which a display area is formed by, for example, a pixel driving circuit such as an organic TFT or a plurality of organic EL elements R, G, and B are regularly arranged in a matrix.

[0153] The first electrode 12 and the second electrode 15 may be electrodes containing metals such as gold, silver, tin, ruthenium, rhodium, palladium, osmium, iridium, platinum, copper, aluminum, molybdenum, and titanium, or oxides such as indium tin oxide (ITO), indium zinc oxide (IZO), and indium gallium zinc oxide (IGZO). The first electrode 12 and the second electrode 15 may be electrodes formed by laminating two or more of these metals, oxides, and the like. An electrode formed by laminating two or more of these metals, oxides, and the like may have two or more layers, or may have three or more layers. When the first circuit member 13 is a plastic substrate, the first electrode 12 may be an electrode having a titanium layer on the outermost surface. The first electrode 12 and the second electrode 15 may be circuit electrodes or bump electrodes. At least one of the first electrode 12 and the second electrode 15 may be a bump electrode. In FIG. 2, the first electrode 12 is a circuit electrode, and the second electrode 15 is a bump electrode.

[0154] The circuit connection portion 17 includes a cured product of the adhesive film 10. The circuit connection portion 17 may be made of a cured product of the adhesive film 10. The circuit connection portion 17 has, for example, a first region 18 located on the first circuit member 13 side in the direction in which the first circuit member 13 and the second circuit member 16 face each other (hereinafter referred to as the "facing direction") and made of a cured product of the component (B) and a cured product of the component (C) and the like other than the conductive particles 4 in the first adhesive layer, a second region 19 located on the second circuit member 16 side in the facing direction and made of a cured product of the component (C) and the like in the second adhesive layer, and conductive particles 4 interposed at least between the first electrode 12 and the second electrode 15 to electrically connect the first electrode 12 and the second electrode 15 to each other. As shown in FIG. 2 , the circuit connection portion 17 does not have to have two distinct regions between the first region 18 and the second region 19, but may have a single region formed by a mixture of the cured material derived from the first adhesive layer and the cured material derived from the second adhesive layer.

[0155] Examples of circuit connection structures include flexible organic electroluminescent color displays (organic EL displays) in which a plastic substrate on which organic EL elements are regularly arranged is connected to a drive circuit element that is a driver for displaying images, and touch panels in which a plastic substrate on which organic EL elements are regularly arranged is connected to a position input element such as a touchpad.The circuit connection structure can be applied to various monitors such as smartphones, tablets, televisions, vehicle navigation systems, and wearable devices; furniture; home appliances; and daily necessities.

[0156] 3A and 3B are schematic cross-sectional views showing one embodiment of a method for manufacturing a circuit connection structure. 3A and 3B are schematic cross-sectional views showing each step. As shown in FIG. 3A, the method for manufacturing a circuit connection structure 20 includes the steps of: interposing the above-described adhesive film 10 between a first circuit member 13 having a first electrode 12 and a second circuit member 16 having a second electrode 15; and thermocompression bonding the first circuit member 13 and the second circuit member 16 to electrically connect the first electrode 12 and the second electrode 15 to each other.

[0157] Specifically, as shown in FIG. 3( a), first, a first circuit member 13 including a first circuit board 11 and a first electrode 12 formed on the main surface 11 a of the first circuit board 11, and a second circuit member 16 including a second circuit board 14 and a second electrode 15 formed on the main surface 14 a of the second circuit board 14 are prepared.

[0158] Next, the first circuit member 13 and the second circuit member 16 are arranged so that the first electrode 12 and the second electrode 15 face each other, and the adhesive film 10 is placed between the first circuit member 13 and the second circuit member 16. For example, as shown in FIG. 3( a), the adhesive film 10 is laminated onto the first circuit member 13 so that the first adhesive layer 1 faces the main surface 11a of the first circuit board 11. Next, the second circuit member 16 is placed on the first circuit member 13 to which the adhesive film 10 has been laminated so that the first electrode 12 on the first circuit board 11 and the second electrode 15 on the second circuit board 14 face each other.

[0159] 3(b), the first circuit member 13 and the second circuit member 16 are heated while being pressed against each other in the thickness direction, thereby thermocompression-bonding the first circuit member 13 and the second circuit member 16. During this process, as indicated by the arrows in FIG. 3(b), the second adhesive layer 2 contains a flowable, uncured thermosetting component, and therefore flows to fill the gaps between the second electrodes 15 and is cured by the heating. As a result, the first electrode 12 and the second electrode 15 are electrically connected to each other via the conductive particles 4, and the first circuit member 13 and the second circuit member 16 are bonded to each other, thereby obtaining the circuit connection structure 20 shown in FIG. 2. In the manufacturing method of the circuit connection structure 20 of this embodiment, the first adhesive layer 1 can be said to be a layer in which a portion of it has been hardened by light irradiation, so that the flow of the conductive particles in the first adhesive layer 1 is suppressed, the first adhesive layer 1 hardly flows during the thermocompression bonding, and the conductive particles are efficiently captured between the opposing electrodes, thereby reducing the connection resistance between the opposing first electrode 12 and second electrode 15. Furthermore, if the thickness of the first adhesive layer is 5 μm or less, the conductive particles tend to be captured even more efficiently during circuit connection.

[0160] The heating temperature for thermocompression bonding can be set appropriately, but may be, for example, 50 to 190°C. The pressure to be applied is not particularly limited as long as it is within a range that does not damage the adherend, but in the case of COP mounting, for example, the area-equivalent pressure at the bump electrode may be 0.1 to 50 MPa, may be 40 MPa or less, or may be 0.1 to 40 MPa. In addition, in the case of COG mounting, for example, the area-equivalent pressure at the bump electrode may be 10 to 100 MPa. The heating and pressurizing time may be in the range of 0.5 to 120 seconds.

[0161] The present invention also relates to the following: [1] An adhesive film for circuit connection, comprising a thermosetting resin component and conductive particles, wherein the thermosetting resin component contains a fluorene skeleton-containing epoxy resin represented by the following general formula (1), and an epoxy resin thermosetting agent: [In formula (1), R E is a backbone residue derived from an epoxy resin, and RP is a skeletal residue derived from a phenolic compound having a fluorene skeleton, and n represents the number of repetitions.] [2] The adhesive film for circuit connection according to [1], wherein the weight-average molecular weight of the fluorene skeleton-containing epoxy resin is 5,000 to 8,000. [3] The adhesive film for circuit connection according to [1] or [2], wherein the fluorene skeleton-containing epoxy resin has a softening point of 85 to 105°C. [4] The adhesive film for circuit connection according to any of [1] to [3], wherein the conductive particles are unevenly distributed on one surface of the film. [5] An adhesive film for circuit connection comprising: a first adhesive layer containing conductive particles, a cured product of a photocurable resin component, and a first thermosetting resin component; and a second adhesive layer provided on the first adhesive layer and containing a second thermosetting resin component, wherein the second thermosetting resin component contains a fluorene skeleton-containing epoxy resin represented by the following general formula (1) and an epoxy resin thermosetting agent: [In formula (1), R E is a backbone residue derived from an epoxy resin, and R P is a skeletal residue derived from a phenolic compound having a fluorene skeleton, and n represents the number of repetitions.] [6] The adhesive film for circuit connection according to [5], wherein the weight-average molecular weight of the fluorene skeleton-containing epoxy resin is 5,000 to 8,000. [7] The adhesive film for circuit connection according to [5] or [6], wherein the fluorene skeleton-containing epoxy resin has a softening point of 85 to 105°C. [8] A method for producing a circuit connection structure, comprising the steps of: interposing the adhesive film for circuit connection according to any one of [1] to [7] between a first circuit member having a first electrode and a second circuit member having a second electrode; and thermocompression-bonding the first circuit member and the second circuit member to electrically connect the first electrode and the second electrode to each other. [9] A circuit connection structure comprising: a first circuit member having a first electrode; a second circuit member having a second electrode; and a circuit connection portion disposed between the first circuit member and the second circuit member and electrically connecting the first electrode and the second electrode to each other, wherein the circuit connection portion comprises a cured product of the adhesive film for circuit connection according to any one of [1] to [7].

[0162] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0163] [Preparation of Conductive Particles] The surfaces of polystyrene particles were plated with Ni, and then the outermost surface was plated with Pd to prepare conductive particles having an average particle size of 3.2 μm.

[0164] [Preparation of First Adhesive Layer and Second Adhesive Layer] The materials shown below were used in preparing the first adhesive layer and the second adhesive layer.

[0165] Component (A): Conductive particles A-1: ​​Conductive particles prepared as above

[0166] Component (B): Photocurable resin component Component (B1): Radical polymerizable compound B1-1: A-BPEF-70T (ethoxylated fluorene-type di(meth)acrylate (bifunctional), product name of Shin-Nakamura Chemical Co., Ltd.), diluted with toluene to a non-volatile content of 70% by mass B1-2: Lipoxy VR-90 (bisphenol A-type epoxy (meth)acrylate (bifunctional) (vinyl ester resin), product name of Showa Denko K.K.)

[0167] Component (B2): Photoradical polymerization initiator B2-1: Irgacure OXE-02 (ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(0-acetyloxime), product name, manufactured by BASF), diluted with MEK to a nonvolatile content of 10% by mass.

[0168] Component (C): Thermosetting resin component Component (C1): Cationic polymerizable compound C1-1: ETERNACOLL OXBP (3-ethyl-3-hydroxymethyloxetane, product name, manufactured by Ube Industries, Ltd.) C1-2: EHPE3150 (1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, product name, manufactured by Daicel Corporation) C1-3: OX-SQ TX-100 (poly({3-[(3-ethyl-3-oxetanyl)methoxy]propyl}silsesquioxane) derivative, product name, manufactured by Toagosei Co., Ltd.) C1-4: CELLOXIDE 2021P (3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, product name, manufactured by Daicel Corporation) C1-5: YL980 (bisphenol A type epoxy resin, epoxy equivalent: 180-190, weight average molecular weight: 362, product name of Mitsubishi Chemical Corporation) C1-6: jER1007 (epoxy resin, epoxy equivalent: 180-190, weight average molecular weight: 10,000, product name of Mitsubishi Chemical Corporation), diluted with an organic solvent to a non-volatile content of 70% by mass C1-7: jER1010 (bisphenol A type solid epoxy resin, epoxy equivalent: 3000-5000, weight average molecular weight: 40000, product name of Mitsubishi Chemical Corporation)

[0169] Component (C-F): fluorene skeleton-containing epoxy resin represented by the above general formula (1) C-F-1: TOPR-300 (high Tg type epoxy resin, epoxy equivalent: 900 to 1,000, weight average molecular weight: 6700, softening point: 91°C, product name, manufactured by Nippon Steel Chemical & Material Co., Ltd.), diluted with MEK to a non-volatile content of 60% by mass

[0170] Component (C2): Thermal cationic polymerization initiator (epoxy resin heat curing agent) C2-1: CXC-1821 (trade name, manufactured by King Industries)

[0171] Component (D): Film-forming component D-1: FX293 (fluorene skeleton-containing phenoxy resin, weight average molecular weight: 32,000, glass transition temperature: 152°C, product name, manufactured by Nippon Steel Chemical & Material Co., Ltd.), diluted with MEK to a nonvolatile content of 35% by mass.

[0172] Component (E): Coupling agent E-1: KBM-303 (ethyltrimethoxysilane, product name, manufactured by Shin-Etsu Chemical Co., Ltd.)

[0173] Component (F): Filler F-1: ADMAFINE SE2050 (silica fine particles, manufactured by Admatechs Co., Ltd., trade name)

[0174] The weight-average molecular weights of the fluorene skeleton-containing epoxy resin and the fluorene skeleton-containing phenoxy resin were measured using gel permeation chromatography (GPC) under the following conditions: Detector: Hitachi High-Tech Science L-2490-RI Column: Gelpack GL-R440+R450+R400M Flow rate: 2.05 ml / min Concentration: 5 mg / ml Injection volume: 200 μl Column temperature: 40°C Eluent: THF Standard sample: Polystyrene

[0175] The softening point of the fluorene skeleton-containing epoxy resin was measured using a thermomechanical analyzer (TMA) under the following conditions: Thermomechanical analyzer: Hitachi High-Tech Sciences TMA-7100, Penetration (φ1 mm) mode, Heating rate: 10°C / min, Load: 98.1 mN

[0176] <Preparation of First Adhesive Layer> A composition was obtained by mixing the materials shown in Table 1 in the composition ratios shown in Table 1 (the values ​​in Table 1 indicate the non-volatile content), and then the composition was coated onto a release-treated PET (polyethylene terephthalate) film while applying a magnetic field. The organic solvent and the like were dried with hot air at 70°C for 5 minutes, thereby obtaining composition layers each made of a composition containing each component. The composition layers were coated so that their thickness after drying would be 3 to 4 μm. Thereafter, the composition layers were irradiated with light (UV irradiation: metal halide lamp, cumulative light amount: 1000 to 3000 mJ / cm). 2), a first adhesive layer in which conductive particles were dispersed was prepared, the thickness of which was measured using a contact thickness meter.

[0177]

[0042] If the thickness of the layer or adhesive layer made of the first adhesive composition is smaller than the thickness (diameter) of the conductive particles, measuring the layer thickness using a contact thickness meter will reflect the thickness of the conductive particles, and the thickness of the region where the conductive particles are present will be measured. Therefore, after producing a two-layer adhesive film in which the first adhesive layer and the second adhesive layer are laminated, the thickness of the first adhesive layer located in the space between adjacent conductive particles was measured using a scanning electron microscope according to the method described above (paragraph 0106).

[0178]

[0179] <Preparation of Second Adhesive Layer> A composition was obtained by mixing the materials shown in Table 2 in the composition ratios shown in Table 2 (the values ​​in Table 2 indicate the non-volatile content), and then the composition was coated on a release-treated PET (polyethylene terephthalate) film. The organic solvent and the like were dried with hot air at 70°C for 5 minutes to prepare second composition layers each consisting of a composition containing each component. The composition layers were coated so that the thickness after drying would be 8 to 9 μm. The thickness here was measured using a contact thickness meter. In this way, a second adhesive layer was prepared on the PET film.

[0180]

[0181] (Examples 1 to 3 and Comparative Examples 1 to 5) [Preparation of Adhesive Films] Adhesive films having the configurations shown in Table 3 were prepared using the first adhesive layer and second adhesive layer prepared above. For example, in the adhesive film of Example 1, the first adhesive layer formed from Composition P-1 was attached to the second adhesive layer formed from Composition S-1 while applying a temperature of 50 to 60°C, thereby obtaining the adhesive film of Example 1. For the adhesive films of Examples 2 to 3 and Comparative Examples 1 to 5, adhesive films having the configurations shown in Table 3 were prepared in the same manner as in Example 1.

[0182] The projected particle density of the adhesive films obtained in Examples 1 to 3 and Comparative Examples 1 to 5 was measured, and was found to be approximately 18,000 particles / mm2 It was.

[0183] [Evaluation of Circuit Connection Structure] <Fabrication of Circuit Connection Structure> As a first circuit member, an IC chip (0.9 mm × 20.3 mm, thickness: 0.3 mm, bump electrode size: 70 μm × 12 μm, space between bump electrodes: 12 μm, bump electrode thickness: 9 μm) was prepared, in which bump electrodes were arranged in two staggered rows. Furthermore, as a second circuit member, a polyimide substrate (manufactured by DuPont-Toray Co., Ltd., 200H) (38 mm × 28 mm, thickness: 0.05 mm) was prepared, in which a wiring pattern of Ti: 50 nm / Al: 400 nm (pattern width: 17 μm, space between electrodes: 7 μm) was formed on the surface.

[0184] Circuit connection structures were produced using each of the adhesive films of Examples 1 to 3 and Comparative Examples 1 to 5. The adhesive film was cut to a width of 2.0 mm, and the adhesive film was placed on the first circuit member so that the first adhesive layer and the first circuit member were in contact. Using a thermocompression bonding device (BS-17U, manufactured by Ohashi Manufacturing Co., Ltd.) consisting of a stage made of a ceramic heater and a tool (8 mm x 50 mm), the adhesive film was heated at 70°C and 0.98 MPa (10 kgf / cm 2 The adhesive film was attached to the first circuit member by heating and pressing for 2 seconds under the conditions of 180°C and 25 MPa equivalent area pressure on the bump electrode, and the release film on the side of the adhesive film opposite the first circuit member was peeled off. Next, the bump electrode of the first circuit member was aligned with the wiring pattern of the second circuit member, and then the second adhesive layer of the adhesive film was attached to the second circuit member by heating and pressing for 5 seconds using an 8 mm x 45 mm heat tool with 50 μm thick Teflon (registered trademark) as a buffer material, under the conditions of 180°C connection and 25 MPa equivalent area pressure on the bump electrode, to produce each circuit connection structure.

[0185] (Evaluation of connection resistance) The initial connection resistance (conduction resistance) of the fabricated circuit connection structure was measured by the four-terminal method. A multimeter (7461A, manufactured by ADC Corporation) was used for the measurement. The potential difference was measured at 14 random points, and the average value was calculated. The average potential difference was converted into a connection resistance value and evaluated according to the following criteria. The results are shown in Table 3. A: Connection resistance value less than 1.0 Ω B: Connection resistance value 1.0 Ω or more but less than 3.0 Ω C: Connection resistance value 3.0 Ω or more

[0186] The fabricated circuit connection structures were subjected to a high temperature and high humidity test in which they were stored at 110°C and 85% RH for 32 hours, and then the connection resistance was calculated in the same manner as above and evaluated according to the following criteria. The results are shown in Table 3. A: Connection resistance less than 1.0Ω B: Connection resistance 1.0Ω or more but less than 3.0Ω C: Connection resistance 3.0Ω or more

[0187] [Evaluation of Backside Transfer Resistance of Adhesive Film] (Preparation of Reel Body of Adhesive Film (Tape)) The adhesive film (first adhesive layer / second adhesive layer / PET film) obtained above was cut to a width of 0.6 mm using a roll-to-roll slitting machine, and the adhesive tape was wound up to a length of 100 m around a reel part (core outer diameter: 66 mm, plastic molded product). At this time, it was wound up so that the first adhesive layer faced the core side (inside) and the PET film faced outward. Reel side plates (thickness 2.0 mm) were provided on both sides of the core, and the gap distance between these reel side plates and the wound body of the adhesive tape was within the range of approximately 0.1 mm to 0.5 mm on each side.

[0188] [Evaluation of Back Transfer Resistance] The reel was fixed in a vertical position, a 75 g weight was hung from the tip, and the reel was left in a thermostatic chamber at 30°C (relative humidity 40 to 60%) for 6 hours. Thereafter, using a Tensilon (trade name, manufactured by A&D Co., Ltd.), the adhesive tape was pulled out from the reel at a rate of 1 m / min and observed under a microscope to evaluate the back transfer resistance according to the following criteria: OK: No back transfer of the adhesive film (peel between the second adhesive layer and the PET film) of 5 mm or more was observed over a length of 100 m. NG: Back transfer of the adhesive film of 5 mm or more was observed over a length of 100 m.

[0189]

[0190] 1...first adhesive layer, 2...second adhesive layer, 4...conductive particles, 5...adhesive component, 10...adhesive film for circuit connection (adhesive film), 11...first circuit board, 12...first electrode (circuit electrode), 13...first circuit member, 14...second circuit board, 15...second electrode (bump electrode), 16...second circuit member, 17...circuit connection portion.

Claims

1. An adhesive film for circuit connection comprising a thermosetting resin component and conductive particles, wherein the thermosetting resin component contains a fluorene skeleton-containing epoxy resin represented by the following general formula (1) and an epoxy resin heat curing agent. [In formula (1), R E is a backbone residue derived from an epoxy resin, and R P is a skeleton residue derived from a phenolic compound having a fluorene skeleton, and n represents the number of repetitions.

2. The adhesive film for circuit connection according to claim 1, wherein the weight average molecular weight of the fluorene skeleton-containing epoxy resin is 5,000 to 8,000.

3. The adhesive film for circuit connection according to claim 1, wherein the fluorene skeleton-containing epoxy resin has a softening point of 85 to 105°C.

4. The adhesive film for circuit connection according to claim 1, wherein the conductive particles are unevenly distributed on one surface of the film.

5. An adhesive film for circuit connection comprising: a first adhesive layer containing conductive particles, a cured product of a photocurable resin component, and a first thermosetting resin component; and a second adhesive layer containing a second thermosetting resin component provided on the first adhesive layer, wherein the second thermosetting resin component contains a fluorene skeleton-containing epoxy resin represented by the following general formula (1) and an epoxy resin thermosetting agent. [In formula (1), R E is a backbone residue derived from an epoxy resin, and R P is a skeleton residue derived from a phenolic compound having a fluorene skeleton, and n represents the number of repetitions.

6. The adhesive film for circuit connection according to claim 5, wherein the weight average molecular weight of the fluorene skeleton-containing epoxy resin is 5,000 to 8,000.

7. The adhesive film for circuit connection according to claim 5, wherein the fluorene skeleton-containing epoxy resin has a softening point of 85 to 105°C.

8. A method for producing a circuit connection structure, comprising the steps of: interposing an adhesive film for circuit connection according to any one of claims 1 to 7 between a first circuit member having a first electrode and a second circuit member having a second electrode; and thermocompressing the first circuit member and the second circuit member to electrically connect the first electrode and the second electrode to each other.

9. A circuit connection structure comprising: a first circuit member having a first electrode; a second circuit member having a second electrode; and a circuit connection portion disposed between the first circuit member and the second circuit member and electrically connecting the first electrode and the second electrode to each other, wherein the circuit connection portion comprises a cured product of the adhesive film for circuit connection according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Adhesive for circuit-member connection, and semiconductor device using the same

    JP2011165758A

  • Adhesive composition, and connection structure for circuit member

    WO2008015852A1

  • Filmy adhesive for circuit connection

    WO2008152711A1

  • Adhesive film for circuit connection, and circuit connection structure and manufacturing method therefor

    WO2021251386A1