Automobile skeleton member

The automobile frame member's strategic arrangement of soft, transition, and hard regions addresses the challenge of achieving sufficient plastic work during collisions, enhancing shock absorption by dispersing deformation and ensuring high strength and ductility.

WO2024214730A1PCT designated stage expired Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014506
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Current automobile frame members face challenges in achieving sufficient plastic work during collisions due to increased strength of steel plates, which leads to localized deformation and reduced shock absorption properties, as higher strength results in poor ductility and early rupture.

Method used

The automobile frame member is designed with a strength varying region arranged in the order of soft, transition, hard, transition, and soft regions along the longitudinal direction, dispersing plastic deformation and ensuring sufficient plastic work through controlled Vickers hardness variations.

Benefits of technology

This design effectively disperses plastic deformation across the frame member, enhancing shock absorption properties by preventing early rupture and ensuring high strength while maintaining ductility, thus achieving excellent impact absorption characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014506_17102024_PF_FP_ABST
    Figure JP2024014506_17102024_PF_FP_ABST
Patent Text Reader

Abstract

When the Vickers hardness of this automobile skeleton member is measured along the longitudinal direction thereof, the average Vickers hardness value HVave is 400 to 800 Hv. This automobile skeleton member includes a variable-intensity region in which a soft region, a transition region, a hard region, a transition region, and a soft region are arranged in the stated order along the longitudinal direction, and Lt / H2>{−0.0018×(4.0×HVh−297)+2.54}×Ls / H2+{0.0012×(4.0×HVh−297)−1.96}.
Need to check novelty before this filing date? Find Prior Art

Description

Automotive frame components

[0001] The present invention relates to an automobile frame member. More specifically, the present invention relates to an automobile frame member that has excellent impact absorption properties against impacts from the vehicle's traveling direction. This application claims priority based on Japanese Patent Application No. 2023-064689, filed on April 12, 2023, the contents of which are incorporated herein by reference.

[0002] Automotive frame members are components that form the framework of an automobile and are mainly made from steel sheets. In recent years, further improvements in safety have been required for these automotive frame members from the perspective of passenger protection, and further weight reduction is also required from the perspective of fuel efficiency regulations and achieving carbon neutrality. To meet these demands, efforts are being made to increase the strength of the steel sheets used in automotive frame members.

[0003] Automobile frame members include deformation suppression members that are placed to protect the passenger compartment during a collision, and impact absorbing members that are placed to absorb the energy of a collision and mitigate the impact on the passengers. For example, impact-absorbing automobile frame members are required to exert sufficient plastic work during a collision in order to improve their impact absorption characteristics. In other words, impact-absorbing automobile frame members are required to have high deformation stress in the steel plate during a collision and large plastic strain occurring over a wide area.

[0004] Generally, increasing the strength of steel sheets reduces their ductility. Therefore, if the strength of steel sheets for automotive frame components is increased, the steel sheets will fracture earlier during a collision, making it difficult for plastic strain to occur, making it difficult for the automotive frame components to exert sufficient plastic work during a collision. Currently, there is a demand for automotive frame components that can exert sufficient plastic work during a collision.

[0005] Patent Document 1 discloses a steel plate member having a band-shaped groove and partially reducing the strength of the groove portion in order to enhance the impact absorption characteristics.

[0006] Patent Document 2 discloses a technology for manufacturing a hot-formed press product with partially reduced strength in order to improve impact absorption characteristics. Patent Document 2 discloses a hot-formed press product in which the strength of a flange portion of a B-pillar, for example, is partially reduced by partially moving the die during the time when the hot press is held at the bottom dead center, thereby slowing the cooling rate of that portion.

[0007] Japanese Patent Publication No. 2020-093291 International Publication No. 2021 / 200923

[0008] In order to improve the impact absorption characteristics of a component, it is necessary to increase the deformation stress of the steel plate during a collision and to generate larger plastic strain over a wide area. However, if the strength of the steel plate used in the component is increased, the work hardening capacity of the steel plate decreases, resulting in localized plastic deformation in the component, making it difficult to obtain the desired plastic work.

[0009] Furthermore, the steel plate member disclosed in Patent Document 1 has a band-shaped groove and the strength of the groove portion is partially reduced, so when the member is deformed by collision, the plastic deformation area is localized in the groove portion, and there is a problem that sufficient plastic work cannot be obtained.

[0010] The hot-formed press product disclosed in Patent Document 2 has a soft region only in the flange portion of the B-pillar. Because the flange portion is usually fixed by spot welding or the like, it is unlikely to undergo significant plastic deformation during a collision, and the hot-formed press product disclosed in Patent Document 2 has the problem that a clear increase in the plastic work of the member cannot be expected. Furthermore, the hot-formed press product disclosed in Patent Document 2 has the problem that the amount of reduction in hardness in the soft portion is small, and a clear increase in the plastic work cannot be expected.

[0011] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an automobile frame member having excellent impact absorption properties, particularly an automobile frame member having excellent impact absorption properties against impacts from the direction of travel of the vehicle.

[0012] The gist of the present invention is as follows. (1) An automobile frame member according to one aspect of the present invention is an automobile frame member for absorbing impacts from the traveling direction of a vehicle, wherein the longitudinal length of the automobile frame member is defined as L in mm, the length of the short side of the smallest circumscribing rectangle of the cross section of the member observed from the longitudinal direction is defined as A in mm, the measurement interval when measuring Vickers hardness is defined as X = A / 40 in mm, the minimum number of measurement points when measuring Vickers hardness is the smaller of Y = 100 or Y = L / X, the Vickers hardness is measured at Y or more measurement points at intervals of X mm along the longitudinal direction from an arbitrary position of the automobile frame member, the average value of the Vickers hardness of all measurement points is defined as HVave, the average value of the Vickers hardness of the five measurement points with the largest values ​​among all measurement points is defined as HVmax, and a region where three or more consecutive measurement points have a Vickers hardness of HVmax-33Hv or more among all measurement points is defined as a hard region, HVmin is the average value of the five smallest Vickers hardness values ​​among all the measurement points, a soft region is a region where three or more consecutive measurement points have a Vickers hardness of HVmin+33Hv or less, and a transition region is a region where three or more consecutive measurement points have a Vickers hardness of more than HVmin+33Hv and less than HVmax-33Hv, the HVave is 400Hv or more and 800Hv or less, and a strength change region is included that is arranged along the longitudinal direction in the following order: soft region, transition region, hard region, transition region, and soft region, the average length in the longitudinal direction of the soft region included in the strength change region is defined as Ls in mm, and the average length in the longitudinal direction of the transition region included in the strength change region is defined as Lt in mm, When the length from the longitudinal center position of one of the soft regions included in the strength change region to the longitudinal center position of the other soft region is H2 in mm, the average Vickers hardness of the hard regions included in the strength change region is HVh, and the average Vickers hardness of the soft regions included in the strength change region is HVs, the following (Equation 1) is satisfied.(Formula 1): Lt / H2>{-0.0018×(4.0×HVh-297)+2.54}×Ls / H2+{0.0012×(4.0×HVh-297)-1.96} (2) In the automobile frame member described in (1) above, when ΔHV is the value obtained by subtracting the HVs from the HVh, the following (Formula 2) and (Formula 3) may be satisfied: (Formula 2): Lt / H2>5Ls / H2+{-0.0012×(4.0×ΔHV-297)-0.80} (Formula 3): Ls / H2+Lt / H2<1 (3) In the automobile frame member described in (1) or (2) above, when HVsth is the average Vickers hardness of the strength change region, the HVsth may be 400 Hv or more and 800 Hv or less. (4) In the automobile frame member described in any one of (1) to (3) above, the cross-sectional shape of the member observed from the longitudinal direction may be a single hat shape or a double hat shape.

[0013] According to the above-described aspect of the present invention, it is possible to provide an automobile frame member that has excellent impact absorption properties against impacts from the traveling direction of the vehicle.

[0014] Fig. 1 is a schematic diagram of an automobile frame member according to one embodiment of the present invention. Fig. 2 is an analysis result summarizing the deformation state of an automobile frame member subjected to axial compression load. Fig. 3 is a schematic diagram explaining analysis conditions for the finite element method. Fig. 4 is a schematic diagram of a load-displacement curve. Fig. 5 is a cross-sectional schematic diagram of an automobile frame member according to another embodiment of the present invention.

[0015] Preferred embodiments of the present invention will be described in detail below. However, the present invention is not limited to the configurations disclosed in the present embodiments, and various modifications are possible within the scope of the present invention. Furthermore, the drawings used in the following description may clearly show the features of the present embodiments, and the dimensional ratios of each component may not be the same as the actual ones. Furthermore, the numerical ranges described below include the lower and upper limits. Numerical values ​​indicated as "greater than" or "less than" do not include the numerical range. "%" regarding the content of each element means "mass %."

[0016] The present inventors conducted extensive research into the deformation state of automobile frame members when they are subjected to an axial compressive load, with the aim of improving the impact absorption characteristics of automobile frame members against impacts from the vehicle's traveling direction. As a result, they found that even when the strength of steel plates used in automobile frame members is increased on average, if the automobile frame member includes a strength change region that is arranged in the longitudinal direction in this order: soft region, transition region, hard region, transition region, and soft region, and if this strength change region is controlled in a favorable manner, then a large amount of plastic work can be achieved when the automobile frame member is subjected to an axial compressive load.

[0017] Specifically, the automobile frame member according to this embodiment is an automobile frame member for absorbing impacts from the traveling direction of the vehicle, wherein the longitudinal length of the automobile frame member is defined as L in mm, the length of the short side of the smallest circumscribing rectangle of the cross section of the member observed from the longitudinal direction is defined as A in mm, the measurement interval when measuring Vickers hardness is defined as X = 1 / 40A (X = A / 40) in mm, the minimum number of measurement points when measuring Vickers hardness is defined as Y = 100 or Y = L / X, whichever is smaller, the Vickers hardness is measured at Y or more measurement points at intervals of X mm along the longitudinal direction from an arbitrary position on the automobile frame member, the average value of the Vickers hardness of all measurement points is defined as HVave, and the average value of the Vickers hardness of the five largest values ​​of all measurement points is defined as HVmax, a hard region is defined as a region where three or more consecutive measurement points have a Vickers hardness of HVmax-33Hv or more, HVmin is defined as the average of the five smallest Vickers hardness values ​​among all measurement points, a soft region is defined as a region where three or more consecutive measurement points have a Vickers hardness of HVmin+33Hv or less, and a transition region is defined as a region where three or more consecutive measurement points have a Vickers hardness of more than HVmin+33Hv and less than HVmax-33Hv, the HVave is 400Hv or more and 800Hv or less, and a strength change region is included that is arranged along the longitudinal direction in the following order: soft region, transition region, hard region, transition region, and soft region, and the average length in the longitudinal direction of the soft region included in the strength change region is defined as Ls in mm, When the average longitudinal length of the transition region included in the strength change region is Lt in mm, the length from the longitudinal center position of one of the soft regions included in the strength change region to the longitudinal center position of the other soft region is H2 in mm, the average Vickers hardness of the hard regions included in the strength change region is HVh, and the average Vickers hardness of the soft regions included in the strength change region is HVs, the following (Equation 1) is satisfied.(Formula 1): Lt / H2>{-0.0018×(4.0×HVh-297)+2.54}×Ls / H2+{0.0012×(4.0×HVh-297)-1.96}.

[0018] FIG. 1 is a schematic diagram of an automobile frame member according to this embodiment. The automobile frame member 1 according to this embodiment includes a strength change region 11. When subjected to an axial compressive load, plastic deformation in this strength change region 11 begins in the soft region 11a, and the plastic deformation can be dispersed from the soft region 11a to the transition region 11b and hard region 11c. As a result, the region that undergoes plastic deformation during deformation expands, and plastic deformation also occurs in regions (the transition region 11b and the hard region 11c) that are stronger than the soft region 11a, resulting in a large amount of plastic work.

[0019] On the other hand, if an automobile frame member is made of a soft material, it will not be possible to ensure the strength required for an automobile frame member, and sufficient plastic work will not be obtained when subjected to an axial compressive load. On the other hand, if an automobile frame member is made of a hard material, the hard material will have relatively high strength but poor ductility, and will therefore fracture early when subjected to an axial compressive load, preventing sufficient plastic work from being obtained.

[0020] Furthermore, if an automobile frame member does not include the above-mentioned transition region (if it includes only the above-mentioned hard region and soft region), the hard region and the soft region will be in contact with each other at all locations in the longitudinal direction of the member. In this case, when the automobile frame member is subjected to an axial compressive load, deformation will be concentrated at the boundary between the hard region and the soft region at all locations in the longitudinal direction of the automobile frame member, causing early fracture and preventing sufficient plastic work from being obtained.

[0021] On the other hand, if an automobile frame member includes the above-mentioned strength change region in at least one location in the longitudinal direction, when the automobile frame member is subjected to an axial compressive load, the deformation at this location is dispersed from the soft region to the transition region and the hard region, resulting in a large amount of plastic work.

[0022] Specifically, when an automobile frame member includes a soft region, a transition region, and a hard region having a predetermined length in the longitudinal direction, when an axial compressive load is applied, plastic deformation begins in the soft region, but the deformation does not concentrate in the soft region but is dispersed to the transition region located next to the soft region, and further dispersed to the transition region located next to the transition region. As a result, the strength required for an automobile frame member is ensured, early fracture is suppressed, and sufficient plastic work is obtained.

[0023] In the automobile frame member according to this embodiment, it is not necessary to provide a transition region between the hard region and the soft region at every location in the longitudinal direction of the member, but it is sufficient to include the strength change region at at least one location in the longitudinal direction. Of course, if two or more strength change regions are included, the plastic work load will be preferably large.

[0024] Note that the automobile frame member according to this embodiment includes a transition region that is greater than HVmin+33Hv and less than HVmax-33Hv, so the value obtained by subtracting HVmin from HVmax (hardness difference) exceeds 66 Hv. If the value obtained by subtracting HVmin from HVmax (hardness difference) is 66 Hv or less, the transition region may not be included, and deformation may concentrate at the boundary between the hard region and the soft region, preventing the deformation from being dispersed.

[0025] In the automobile frame member according to this embodiment, the hard region, transition region, and soft region are divided as described above, on the premise that the value obtained by subtracting HVmin from HVmax (hardness difference) exceeds 66 Hv.

[0026] Specifically, a hard region is defined as a region where, among the Y or more measurement points, there are three or more consecutive measurement points where the Vickers hardness is HVmax-33Hv or more. If there are less than three consecutive measurement points where the Vickers hardness is HVmax-33Hv or more, this is considered to be a measurement singularity. Therefore, in this embodiment, the measurement singularity is ignored to identify the hard region.

[0027] Similarly, a soft region is defined as a region where, among the Y or more measurement points, there are three or more consecutive measurement points where the Vickers hardness is HVmin+33Hv or less. If there are less than three consecutive measurement points where the Vickers hardness is HVmin+33Hv or less, the region is considered to be a measurement singularity. Therefore, in this embodiment, the measurement singularity is ignored to identify the soft region.

[0028] Similarly, the transition region is defined as a region where, among the Y or more measurement points, there are three or more consecutive measurement points where the Vickers hardness is greater than HVmin+33Hv and less than HVmax-33Hv. If there are fewer than three consecutive measurement points where the Vickers hardness is greater than HVmin+33Hv and less than HVmax-33Hv, but not three or more consecutive measurement points, this is considered to be a measurement singularity. Therefore, in this embodiment, the measurement singularity is ignored to identify the transition region. It is preferable that a transition region be included between the hard region and the soft region.

[0029] The automobile frame member according to this embodiment includes a strength change region arranged in the following order along the longitudinal direction of the member: soft region, transition region, hard region, transition region, and soft region. This strength change region is preferably controlled, so that when an axial compressive load is applied, plastic deformation is dispersed from the soft region to the transition region and hard region.

[0030] Furthermore, since the automobile frame member according to this embodiment is premised on having high strength (hardness), the HVave may be 400 Hv or more and 800 Hv or less, and more preferably 450 Hv or more.

[0031] As described above, the value obtained by subtracting HVmin from HVmax (hardness difference) is sufficient as long as it exceeds 66 Hv. This hardness difference is preferably 80 Hv or more, more preferably 100 Hv or more, and even more preferably 150 Hv or more. On the other hand, the upper limit of this hardness difference is not particularly limited, but may be, for example, 400 Hv.

[0032] The HVmax is not particularly limited, but may be 470 Hv or more and 800 Hv or less. The HVmax is preferably 500 Hv or more, more preferably 550 Hv or more, and even more preferably 600 Hv or more.

[0033] Similarly, the above HVmin is not particularly limited, but may be 250 Hv or more and 400 Hv or less, and preferably 350 Hv or less.

[0034] The automobile frame member of this embodiment may include at least one strength change region arranged in the following order: soft region, transition region, hard region, transition region, and soft region when Vickers hardness is measured at the Y or more measurement points at X mm intervals from any position on the member along the longitudinal direction.

[0035] The position of the above-mentioned strength change region in an automobile frame member is not particularly limited, as long as the above-mentioned strength change region is located in a portion where the passenger space is unlikely to be affected even if the member is deformed when the automobile frame member is subjected to an impact in the longitudinal direction. For example, when an automobile frame member is subjected to an axial compressive load, the portions where the passenger space is unlikely to be affected even if the member is deformed are portions known as front side members and rear side members, and the above-mentioned strength change region may be located in these portions.

[0036] Furthermore, it is preferable that high-strength hard regions be arranged at both longitudinal ends of an automobile frame member in which a strength change region is arranged, so as to realize a smooth load path from other components to the automobile frame member when an impact is received from the longitudinal direction. For example, when Vickers hardness is measured at five or more measurement points at intervals of the above X mm along the longitudinal direction from the longitudinal end of the automobile frame member, it is preferable that the Vickers hardness of the longitudinal end of the automobile frame member is equal to or greater than the above-mentioned HVmax-33Hv. In other words, it is preferable that the longitudinal end of the automobile frame member is the above-mentioned hard region. It is also preferable that both longitudinal end of the automobile frame member are the above-mentioned hard region. It is preferable that the above-mentioned strength change region is arranged at a position other than both longitudinal end of the automobile frame member (for example, a middle position).

[0037] The automobile frame member according to this embodiment may include at least one strength change region, but may also include two or more strength change regions. If the automobile frame member includes two or more strength change regions, when the automobile frame member is subjected to an impact and plastically deforms, the deformation is dispersed from the soft region to the transition region and the hard region at more locations within the member, which is preferable.

[0038] Furthermore, in the automobile frame member according to this embodiment, when the average length in the longitudinal direction of the soft region included in the strength change region is Ls (unit: mm), the average length in the longitudinal direction of the transition region included in the strength change region is Lt (unit: mm), the length from the center position in the longitudinal direction of one of the soft regions included in the strength change region to the center position in the longitudinal direction of the other soft region is H2 (unit: mm), the average value of Vickers hardness of the hard region included in the strength change region is HVh (unit: Hv), and the average value of Vickers hardness of the soft region included in the strength change region is HVs (unit: Hv), the following formula 1 is satisfied. (Formula 1): Lt / H2>{-0.0018 x (4.0 x HVh - 297) + 2.54} x Ls / H2 + {0.0012 x (4.0 x HVh - 297) - 1.96}

[0039] Furthermore, in addition to the above formula 1, the automobile frame member according to this embodiment preferably satisfies the following formulas 2 and 3, where ΔHV is the value obtained by subtracting the above HVs from the above HVh: (Formula 2): Lt / H2>5Ls / H2+{-0.0012×(4.0×ΔHV-297)-0.80} (Formula 3): Ls / H2+Lt / H2<1

[0040] Figure 2 shows an example of the analysis results summarizing the deformation state of an automobile frame member when subjected to an axial compressive load. In Figure 2, the vertical axis is Lt / H2 and the horizontal axis is Ls / H2. The straight lines shown in Figure 2 correspond to the above formula 1. In other words, the area indicated by circles and triangles in the figure is the range that satisfies the above formula 1. Note that the area indicated by only circles in the figure corresponds to the range that satisfies the above formulas 1 to 3.

[0041] 2 shows the results of analyzing the deformation state using the finite element method (FEM) and summarizing the deformation state. For example, the FEM analysis conditions are as follows:

[0042] Figure 3 shows a schematic diagram illustrating the FEM analysis conditions. An automobile frame member 1 was used, which had a top plate length of 25 mm, a flange length of 10 mm, and a double-hat cross-sectional shape (cross-sectional shape with the longitudinal direction normal) with a punch shoulder bend angle of 105°. The plate thickness was 1.2 mm and the longitudinal length was 240 mm. The lengths of the soft region 11a, the transition region 11b, and the hard region 11c, as well as the hardness of each region, were varied. An 800 kg weight was collided with this member in the longitudinal direction at a constant speed of 5,000 mm / sec, and the deformation state was analyzed using FEM.

[0043] The above-mentioned member had hard regions at both longitudinal ends of the member, and two soft regions and a transition region surrounding them at a longitudinal midpoint of the member. That is, as shown in Fig. 3, the above-mentioned automobile frame member 1 had a strength change region 11 at a longitudinal midpoint, which was arranged in the following order: soft region 11a, transition region 11b, hard region 11c, transition region 11b, and soft region 11a.

[0044] In the FEM analysis, the length Ls of the soft region was varied from 0 to 32 mm, the length Lh of the hard region was varied from 0 to 50 mm, the length Lt of the transition region was varied from 0 to 24 mm, and the length H2 from the longitudinal center position of one soft region to the longitudinal center position of the other soft region was varied from 38 to 75 mm. In the FEM analysis, the HVh and ΔHV were set to 600 Hv, 250 Hv, 525 Hv, and 125 Hv. Note that HVs is equal to the value obtained by subtracting ΔHV from HVh. Furthermore, as a comparative material, an analysis was also conducted on a component in which the hardness of the entire component was set to HV = 325.

[0045] The solver for the FEM analysis was not particularly limited, but LS-DYNA from Livermore Software Technology Corporation was used. In the FEM analysis, elements were treated as 2 mm square shells, and the elements were divided into three at the R portion of the component. In addition, the material fracture prediction software was not particularly limited, but NSafe-MAT from Nippon Steel Corporation was used. In the analysis, when it was determined that the material had fractured, the element at the location where it was determined that the fracture had occurred was deleted to simulate the fracture state of the material.

[0046] The above-mentioned FEM analysis was performed to confirm the load-displacement curve of a component subjected to an axial compressive load. This load-displacement curve can be used to determine whether a component subjected to an axial compressive load has performed sufficient plastic work. For example, if the load value on the load-displacement curve is large and the displacement increases, but the load does not immediately decrease and continues at a high load, i.e., if the area enclosed by the curve and the X-axis on the load-displacement curve is large, it can be determined that the amount of plastic work is large.

[0047] Schematic diagrams of load-displacement curves are shown in Figures 4(a) to 4(c). The load-displacement curves of the members confirmed by the above-mentioned FEM analysis could be classified into one of the three types of curves shown in Figure 4(a) to 4(c). In Figure 4, the vertical axis represents load F and the horizontal axis represents displacement S.

[0048] Figure 4(a) corresponds to a load-displacement curve in which a component is prone to material fracture immediately after reaching the maximum load when subjected to an axial compressive load. Figure 4(b) corresponds to a load-displacement curve in which a component is unlikely to fracture even after reaching the maximum load when subjected to an axial compressive load, and plastic deformation is likely to be dispersed within the component. Figure 4(c) corresponds to a load-displacement curve in which a component is unlikely to fracture even after reaching the maximum load when subjected to an axial compressive load, and plastic deformation is likely to be dispersed favorably within the component.

[0049] In the load-displacement curve shown in FIG. 4( a), the area enclosed by the curve and the X-axis (plastic work volume) is small, while in the load-displacement curves shown in FIGS. 4( b) and 4( c), the area enclosed by the curve and the X-axis (plastic work volume) is large.

[0050] Specifically, the plastic work load EA (unit: kJ) was defined as the amount of plastic work obtained from the load-displacement curve of the member including the strength change region, where the displacement is within the range of 1.5 × H2 mm. The plastic work load EA obtained from the same displacement range as above on the load-displacement curve of the comparative material (whole member hardness HV = 325) was defined as EA. 0 (unit: kJ), when the above FEM analysis is performed, the load-displacement curve shown in FIG. 4(a) shows EA / EA 0 The value of EA / EA is less than 1.5, but in the load-displacement curves shown in Figures 4(b) and 4(c), 0 The value of is 1.5 or more.

[0051] In this embodiment, based on the load-displacement curve confirmed under the above conditions, EA / EA 0 When the value of is 1.5 or more, it is judged that the plastic deformation is dispersed from the soft region to the transition region and the hard region, and as a result, a sufficient amount of plastic work is obtained.

[0052] The above-mentioned Figure 2 shows the EA / EA 0 2 shows an example of the results of arranging the conditions under which the value of EA / EA is 1.5 or more. Specifically, FIG. 2 shows the results of FEM analysis when HVh is 600 Hv and ΔHV is 250 Hv. In FIG. 2, the areas indicated by circles and triangles are areas where EA / EA 0 This is a region where the value of is 1.5 or more and where the above formula 1 is satisfied.

[0053] As mentioned above, the upper right region of the straight line in Figure 2 is the region that satisfies the above formula 1. In order for a member to obtain sufficient plastic work, it is preferable that the member collapses into a neat bellows shape when subjected to an axial compressive load, and it is preferable that material fracture does not occur. The above formula 1 indicates the boundary of whether material fracture is preferably suppressed or not.

[0054] That is, material fracture is preferably suppressed under conditions that satisfy the above formula 1. On the other hand, under conditions that do not satisfy the above formula 1, material fracture is not suppressed, and the load-displacement curve resembles the curve shown in Figure 4(a).

[0055] 2 shows the results of the FEM analysis when the HVh of the hard region is 600 Hv, and the above formula 1 includes HVh as a variable. For example, if the hardness of a member is lower, the member becomes less likely to break. In other words, if the HVh value is smaller, the values ​​of Ls / H2 and Lt / H2 required to satisfy the above formula 1 become smaller, and as a result, the region in FIG. 2 that satisfies the above formula 1 becomes wider.

[0056] Although not shown in Figure 2, the line separating the circle and triangle regions in Figure 2 corresponds to the above formula 2. Specifically, the region indicated by circles and triangles in the figure is the range that satisfies the above formula 1, and the region indicated by circles only in the figure is the range that satisfies both formulas 1 and 2. In order for a member to perform a sufficient amount of plastic work, it is preferable that when the member is subjected to an axial compressive load, the deformation does not concentrate locally, but is sufficiently dispersed from the soft region to the transition region and the hard region. The above formula 2 indicates the boundary between whether or not the plastic deformation is favorably dispersed.

[0057] That is, compared to the condition where the above formula 1 is satisfied but the above formula 2 is not satisfied, the plastic deformation is preferably distributed from the soft region to the transition region and the hard region under the condition where the above formula 1 and the above formula 2 are satisfied. Under the condition where the above formula 1 is satisfied but the above formula 2 is not satisfied, the load-displacement curve resembles the curve shown in Figure 4(b), and under the condition where the above formula 1 and the above formula 2 are satisfied, the load-displacement curve resembles the curve shown in Figure 4(c).

[0058] 2 shows the results of the FEM analysis when ΔHV, which is the value obtained by subtracting HVs from HVh, is 250 HV, but the above equation 2 includes ΔHV as a variable. For example, if the difference in hardness between the hard region and the soft region increases, plastic deformation becomes more likely to be dispersed. In other words, if the value of ΔHV increases, the value of Ls / H2 to satisfy the above equation 2 increases and the value of Lt / H2 decreases, resulting in a wider region in FIG. 2 that satisfies the above equation 2.

[0059] Furthermore, although not shown in FIG. 2, the above formula 3 indicates the geometric condition between Ls and Lt. For example, when the above formula 3 is transformed, the value of H2 is positive, so Ls + Lt < H2. Here, H2 is the length from the center position of one soft region to the center position of the other soft region, Ls is the average length of the soft region, and Lt is the average length of the transition region. Therefore, it is geometrically impossible for the value of Ls + Lt to be equal to or greater than H2. The above formula 3 indicates the boundary that Ls and Lt can geometrically satisfy.

[0060] Strictly speaking, the strength change region is arranged in the following order: soft region, transition region, hard region, transition region, and soft region, and the length from the center position of one soft region in the longitudinal direction to the center position of the other soft region in the longitudinal direction is H2, so Ls + 2 × Lt < H2. Therefore, the above formula 3 may be replaced with Ls / H2 + 2 × Lt / H2 < 1.

[0061] The automobile frame member according to this embodiment includes a strength change region arranged in the longitudinal direction in the following order: soft region, transition region, hard region, transition region, and soft region, and when the above formula 1 is satisfied, plastic deformation is preferably distributed from the soft region to the transition region and the hard region. Furthermore, when the automobile frame member according to this embodiment simultaneously satisfies the above formulas 2 and 3 in addition to the above formula 1, plastic deformation is even more preferably distributed. In these cases, even when the member is subjected to an axial compressive load, the amount of plastic work is sufficiently large, resulting in excellent impact absorption characteristics.

[0062] As mentioned above, the vertical axis of Fig. 2 represents Lt / H2, and the horizontal axis represents Ls / H2. Qualitatively speaking, Lt / H2 represents the ratio of the average length of Lt to the length of H2, and similarly, Ls / H2 represents the ratio of the average length of Ls to the length of H2. In other words, when an automobile frame member has a strength change region that is arranged in the longitudinal direction in the following order: soft region, transition region, hard region, transition region, and soft region, the above formulas 1 to 3 represent the preferred state of existence of the soft region and the transition region in this strength change region.

[0063] Furthermore, since the automobile frame member according to this embodiment is premised on having high strength (hardness), even if the strength change region includes a soft region and a transition region, when the average Vickers hardness of the strength change region is HVsth, this HVsth is preferably 400 Hv or more and 800 Hv or less. This HVsth is preferably 425 Hv or more, and more preferably 450 Hv or more.

[0064] The above formulas 1 to 3 indicate the conditions under which plastic deformation is preferably distributed depending on the characteristics of the member before the member is subjected to an axial compressive load, more specifically, the characteristics of the strength change regions arranged in the longitudinal direction in the order of soft region, transition region, hard region, transition region, and soft region. However, in the automobile frame member according to this embodiment, the conditions under which plastic deformation is preferably distributed can also be indicated depending on the characteristics of the member after the member is subjected to an axial compressive load.

[0065] For example, an automobile frame member according to this embodiment includes strength change regions arranged in the longitudinal direction in the following order: soft region, transition region, hard region, transition region, and soft region; the average length of the soft regions in the longitudinal direction is Ls in mm; the average length of the transition regions in the longitudinal direction is Lt in mm; the average value of Vickers hardness of the hard regions is HVh in Hv; the average value of Vickers hardness of the soft regions is HVs in Hv; and a test is conducted in which a flat impactor is collided with the automobile frame member in the longitudinal direction at an arbitrary speed, and the length between the peak and valley of buckling of the member crushed into an accordion-like shape is H1 in mm, and it is preferable that the following (Equation 4) is satisfied. (Formula 4): Lt / H1>{-0.0018×(4.0×HVh-297)+2.54}×Ls / H1+{0.0012×(4.0×HVh-297)-1.96}

[0066] Furthermore, in addition to the above formula 4, the automobile frame member according to this embodiment preferably satisfies the following formulas 5 and 6, where ΔHV is the value obtained by subtracting the above HVs from the above HVh: (Formula 5): Lt / H1>5Ls / H1+{-0.0012×(4.0×ΔHV-297)-0.80} (Formula 6): Ls / H1+Lt / H1<1

[0067] Furthermore, the structural structure of the steel of the automobile frame member according to this embodiment is not particularly limited, as long as the steel structure of the automobile frame member according to this embodiment includes martensite, tempered martensite, bainite, retained austenite, ferrite, pearlite, and the like.

[0068] However, since the automobile frame member according to this embodiment is premised on high strength (hardness), it is preferable that the steel structure of the hard region be a structure mainly composed of martensite. Furthermore, in the automobile frame member according to this embodiment, plastic deformation is dispersed from the soft region to the transition region and the hard region, so it is preferable that the transition region contains, in addition to martensite, retained austenite, bainite, tempered martensite, etc. On the other hand, it is sufficient that the soft region has a lower hardness than the hard region and transition region, and that it is sufficient that the soft region contains retained austenite, bainite, tempered martensite, ferrite, pearlite, etc.

[0069] Furthermore, in the automobile frame member according to this embodiment, in order to preferably distribute plastic deformation from the soft region to the transition region and the hard region, it is preferable that the work hardening capacity of the transition region is high, specifically, that the work hardening exponent n value is high. When the work hardening capacity of the transition region is high, plastic deformation is preferably distributed from the soft region to the hard region. It is preferable that the transition region contains a large amount of retained austenite, because this causes stress-induced transformation and increases the work hardening capacity.

[0070] Furthermore, the automobile frame member according to this embodiment is intended to be a member subjected to axial compressive load, and in order to suppress material fracture, it is preferable that the ultimate deformability is high. If the steel structure contains a small number of microvoids that serve as fracture initiation points, the ultimate deformability is increased, which is preferable. Furthermore, if the steel structure does not contain ferrite or pearlite, the concentration of deformation at the interface between the hard structure and the soft structure is suppressed, and the ultimate deformability is increased, which is preferable.

[0071] Furthermore, in the automobile frame member according to this embodiment, the chemical composition of the steel is not particularly limited. The automobile frame member according to this embodiment has, for example, a steel composition, in mass %, of C: 0.08 to 0.70%, Si: 0.100 to 3.000%, Mn: 0.100 to 3.000%, P: 0.1000% or less, S: 0.0100% or less, N: 0.0200% or less, O: 0.1000% or less, Al: 3.0000% or less, B: 0.0005 to 0.0200%, Nb: 0 to 0.100%, Ti: 0 to 0.200%, Cr: 0 to 1.00%, Mo: 0 to 1.00%, Co: 0 to 5.00%, Ni: 0 to 3.00%, Cu: 0 to 3.00%, V: 0 to 3.00%, It is sufficient if the alloy contains W: 0 to 3.00%, Ca: 0 to 1.0000%, Mg: 0 to 1.0000%, REM: 0 to 1.0000%, Sb: 0 to 1.00%, Zr: 0 to 1.00%, Sn: 0 to 1.00%, As: 0 to 1.0000%, with the balance being Fe and impurities.

[0072] Furthermore, the shape of the automobile frame member according to this embodiment is not particularly limited. It may have any shape according to the design of the automobile. For example, the automobile frame member according to this embodiment may have a cross-sectional shape of a single hat or double hat when viewed from the longitudinal direction. As an example, FIG. 5( a) shows a cross-sectional schematic diagram of an automobile frame member having a cross-sectional shape normal to the longitudinal direction that is a single hat, and FIG. 5( b) shows a cross-sectional schematic diagram of an automobile frame member having a cross-sectional shape normal to the longitudinal direction that is a double hat.

[0073] Next, a method for measuring the characteristics of an automobile frame member according to this embodiment will be described.

[0074] The Vickers hardness can be measured in accordance with JIS Z2244:2020. The measurement load can be set appropriately to a load that produces the largest indentation, allowing for more accurate measurement. For example, the measurement load is set to 9.8×10 -5 ~9.8 x 10 0N. In measuring the Vickers hardness, an electron microscope such as a SEM may be used to measure with high accuracy.

[0075] The Vickers hardness is measured along the longitudinal direction of the automobile frame member. For example, the longitudinal direction of the automobile frame member may be the long axis direction of the automobile frame member in the field of view in which the automobile frame member appears longest when viewed from all directions. The Vickers hardness is measured at the center in the horizontal direction (the direction perpendicular to the longitudinal direction). Even when the automobile frame member has a single-hat or double-hat shape, the Vickers hardness is measured along the longitudinal direction of the automobile frame member, but the measurement position may be the center of the top plate surface.

[0076] Vickers hardness can be measured at Y or more measurement points spaced X mm apart along the longitudinal direction from any position on the automotive frame member, where L is the longitudinal length of the automotive frame member in mm, A is the length of the short side of the smallest circumscribed rectangle of the cross section of the member observed from the longitudinal direction, X is the measurement interval X mm = A / 40, and the minimum number of measurement points is the smaller of Y = 100 or Y = L / X. For example, the coordinates of the first of the Y measurement points can be X / 2 mm or more away from the longitudinal end of the automotive frame member. In this case, the Vickers hardness value at the nth measurement point of the Y measurement points can be regarded as a representative value representing the hardness range from -X / 2 mm to less than X / 2 mm, based on the nth measurement point.

[0077] Note that automobile frame components may have holes as part of their component shape. When measuring Vickers hardness at regular intervals along the longitudinal direction of an automobile frame component (line analysis), it is preferable to set the measurement line for the line analysis so as to avoid holes as much as possible. When performing line analysis of Vickers hardness along the longitudinal direction, if the location to be measured is a hole, the Vickers hardness may be measured on a flat portion 2 mm or more away from the hole in a direction perpendicular to the measurement line. When performing line analysis of Vickers hardness along the longitudinal direction, if the location to be measured is a processed portion (bent-molded portion), the Vickers hardness may be measured on a flat portion 2 mm or more away from the processed portion in a direction perpendicular to the measurement line. Vickers hardness may be measured at least once along the longitudinal direction from any position on the automobile frame component according to the above procedure.

[0078] The longitudinal length L of an automobile frame member can be determined by measuring the maximum longitudinal length of the automobile frame member. Furthermore, the minimum circumscribing rectangle of the cross section of the automobile frame member observed from the longitudinal direction can be determined by observing the cross section of the member at the midpoint of the length L. The length A of the short side of this minimum circumscribing rectangle can be measured. The minimum circumscribing rectangle refers to a rectangle that is in contact with the outside of the cross section of the member and has the smallest area.

[0079] The structural structure of the steel may be observed by the following method: The observation surface is a cross section perpendicular to the longitudinal direction, and the observation surface is polished and immersed in an acetylacetone-based electrolyte, electrolytically etched, and then observed at a magnification of 5000 times (for example, at least 625 μm) using a field emission scanning electron microscope equipped with a secondary electron detector. 2 The secondary electron image can be observed in a field of view (field of view) to distinguish between ferrite and pearlite and structures other than ferrite and pearlite. A structure consisting of massive crystal grains that does not contain a substructure such as lath within the structure is considered to be ferrite. A structure consisting of layered ferrite and Fe-based carbides is considered to be pearlite.

[0080] In addition, at the same observation point as above, a magnification of 10,000 times (for example, at least 150 μm 2A secondary electron image can be observed in a field of view (field of view) to distinguish between tempered martensite and bainite. A structure that is an aggregation of lath-shaped crystal grains and contains Fe-based carbides with a major axis of 20 nm or more elongated in different directions within the structure is considered to be tempered martensite. Among structures that are an aggregation of lath-shaped crystal grains and do not contain Fe-based carbides with a major axis of 20 nm or more within the structure, a structure in which Fe-based carbides precipitate between the laths, and a structure in which Fe carbides precipitate within the laths and the Fe-based carbides elongate in the same direction are considered to be bainite.

[0081] Furthermore, at the same observation location as above, the observation surface is re-polished to a mirror finish, strain is removed, and crystal orientation information is obtained by electron backscatter diffraction at measurement intervals of 0.4 μm. Regions with an fcc crystal structure are considered to be retained austenite.

[0082] Furthermore, the region other than ferrite, pearlite, tempered martensite, bainite, and retained austenite obtained by the above-mentioned method is considered to be martensite.

[0083] The chemical composition of the steel may be measured by a general steel analysis method. For example, the chemical composition may be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). C and S may be measured using a combustion-infrared absorption method, N may be measured using an inert gas fusion-thermal conductivity method, and O may be measured using an inert gas fusion-non-dispersive infrared absorption method.

[0084] Next, a method for manufacturing an automobile frame member according to this embodiment will be described.

[0085] The manufacturing method of the automobile frame member according to this embodiment is not particularly limited. For example, the automobile frame member according to this embodiment may be manufactured by the manufacturing method described below. The manufacturing method described below is one example for manufacturing the automobile frame member according to this embodiment, and is a suitable example of the manufacturing method of the automobile frame member according to this embodiment.

[0086] For example, the automobile frame member according to this embodiment may be manufactured by any one of the following methods (A) to (C).

[0087] (A) Heating Control in Hot Stamping Process When the automobile frame member according to this embodiment is manufactured by hot stamping, heating may be controlled in the hot stamping process.

[0088] For example, when heating a workpiece before hot stamping, the region that is ultimately desired to be in the soft region can be covered with a thicker insulating material, the region that is ultimately desired to be in the transition region can be covered with a thinner insulating material, and the region that is ultimately desired to be in the hard region can be painted black with heat-resistant paint. This method allows the heating temperature of the region covered with the thicker insulating material to be controlled to less than Ac3, the heating temperature of the region covered with the thinner insulating material to be controlled to close to Ac3, and the heating temperature of the region painted black with heat-resistant paint to be controlled to Ac3 or higher. Note that Ac3 refers to the temperature at which ferrite completes its transformation to austenite during heating. The workpiece that has undergone the above heating control can then be hot stamped.

[0089] In an automobile frame component subjected to the above-described heating control, the hard region mainly contains martensite, the transition region contains martensite and retained austenite, and the soft region contains martensite, retained austenite, ferrite, and the like.

[0090] (B) Cooling Control in Hot Stamping Process When the automobile frame member according to this embodiment is manufactured by hot stamping, cooling control may be performed in the hot stamping process.

[0091] For example, when cooling the formed material after hot stamping, a material with low thermal conductivity can be used for the mold in the region that is ultimately desired to be controlled to the soft region, a material with medium thermal conductivity can be used for the mold in the region that is ultimately desired to be controlled to the transition region, and a material with high thermal conductivity can be used for the mold in the region that is ultimately desired to be controlled to the hard region. A material with medium thermal conductivity refers to a material that is intermediate between the material with low thermal conductivity for the soft region and the material with high thermal conductivity for the hard region. By this method, the cooling rate in the region where the mold uses a material with low thermal conductivity can be controlled to less than Vc90, the cooling rate in the region where the mold uses a material with medium thermal conductivity can be controlled to close to Vc90, and the cooling rate in the region where the mold uses a material with high thermal conductivity can be controlled to Vc90 or higher. Vc90 refers to the critical cooling rate (°C / sec) for obtaining a martensitic structure with a volume fraction of 90% or more. The formed material after hot stamping can be cooled by performing the above cooling control. The cooling rate can be controlled in three stages as described above by imparting an uneven shape to the mold.

[0092] In an automobile frame component that has undergone the above-described cooling control, the hard region mainly contains martensite, the transition region contains martensite, bainite, retained austenite, etc., and the soft region contains martensite, bainite, retained austenite, ferrite, pearlite, etc.

[0093] (C) Tempering Control After Hot Stamping Process When the automobile frame member according to this embodiment is manufactured by hot stamping, tempering can be controlled after the hot stamping process.

[0094] For example, when tempering the formed material after the hot stamp forming process, the region that is ultimately to be controlled to the above-mentioned soft region can be locally tempered by controlling the output of the laser irradiation to heat it to a higher temperature, and the region that is ultimately to be controlled to the above-mentioned transition region can be locally tempered by controlling the output of the laser irradiation to heat it to a lower temperature, while the region that is ultimately to be controlled to the above-mentioned hard region can be left untempered.

[0095] In an automobile frame member that has undergone the above-described tempering control, the hard region mainly contains martensite, the transition region contains tempered martensite and the like, and the soft region contains tempered martensite and the like.

[0096] The effects of one aspect of the present invention will be explained in more detail using examples. However, the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved. The present invention will be explained in more detail below by illustrating examples and comparative examples.

[0097] The deformation state of automobile frame members having the shapes and hardness shown in Tables 3 to 17 when subjected to an axial compressive load was analyzed using FEM. The axial compressive load was applied by impacting an 800 kg weight from the longitudinal direction of the member at a constant speed of 5000 mm / s.

[0098] In the automobile frame member used in the analysis, the strength was changed at each location within the member. Specifically, at the midpoint in the longitudinal direction of the member (a position other than both ends), the strength was changed in the following order from the front end of the vehicle: soft region (I), transition region (II), hard region (III), transition region (IV), and soft region (V), as shown in Tables 3 to 7. When strength changes were repeated, the adjacent (V) closer to the front end and the (I) closer to the rear end were considered to be the same. At the front end of the vehicle, the strength was changed from the front end to (III) and (IV), and at the rear end of the vehicle, the strength was changed from the rear end to (III) and (II).

[0099] Here, when the average value of the Vickers hardness of all the measurement points is defined as HVave, the average value of the Vickers hardness of the five largest values ​​among all the measurement points is defined as HVmax, and the average value of the Vickers hardness of the five smallest values ​​among all the measurement points is defined as HVmin, the soft region (I) and soft region (V) correspond to regions where the Vickers hardness is HVmin+33Hv or less, the transition region (II) and transition region (IV) correspond to regions where the Vickers hardness is more than HVmin+33Hv and less than HVmax-33Hv, and the hard region (III) corresponds to regions where the Vickers hardness is HVmax-33Hv or more.

[0100] The shapes of automobile frame members other than those shown in Tables 3 to 17 were as shown in Figure 5(a) when the cross-sectional shape of the member was indicated as "single hat," and as shown in Figure 5(b) when the cross-sectional shape of the member was indicated as "double hat." In the examples in the tables, when the cross-sectional shape of the member was "double hat," the outer and inner members had the same shape, with a top plate length of 25 mm, a vertical wall length of 22.5 mm, a bending angle of the punch shoulder of 105°, and a thickness of 1.2 mm. When the cross-sectional shape of the member was "single hat," the outer member had a top plate length of 90 mm, a vertical wall length of 120 mm, a bending angle of the punch shoulder of 95°, and a thickness of 1.4 mm, and the inner member had a thickness of 1.4 mm.

[0101] The hardness characteristics of the automotive frame members other than those shown in Tables 3 to 17 were that both ends in the longitudinal direction of the member were hard regions. Furthermore, the strength change region was included in the middle position in the longitudinal direction of the member (a position other than both ends). The above hardness values ​​of the automotive frame members were set assuming the use of steel types with the chemical compositions shown in Tables 1 and 2. Furthermore, the Vickers hardness values ​​shown in the tables are hardness values ​​based on the above method, assuming measurements were taken at a measurement interval of X mm and at Y or more measurement points along the longitudinal direction of the automotive frame member and at the center of the horizontal direction on the top plate surface.

[0102] In addition, the "longitudinal length L" shown in the table represents the maximum longitudinal length of the automobile frame member, and the "short side A of the minimum circumscribing rectangle" shown in the table represents the short side of the minimum circumscribing rectangle that contacts the outside of the member cross section at the midpoint of the length L.

[0103] In addition, the "presence or absence of an intensity change region" shown in the table indicates whether or not an intensity change region is present, which is arranged in the following order along the longitudinal direction: soft region, transition region, hard region, transition region, and soft region. In addition, the values ​​of "average length of soft region Ls," "average length of transition region Lt," and "length of hard region Lh" shown in the table are rounded to one decimal place.

[0104] Furthermore, the "length H2 between soft regions (length between soft regions)" shown in the table indicates the length H2 between the centers of two soft regions when a strength change region is present, but indicates the length between the centers of the soft regions (I) and (V) whose strength is changed in the member when a strength change region is not present. Furthermore, the "average hardness HVh of hard regions (average hardness of hard regions)" shown in the table indicates the average hardness HVh of the hard regions when a strength change region is present, but indicates the average hardness of the hard region (III) whose strength is changed in the member when a strength change region is not present. Furthermore, the "average hardness HVs of soft regions (average hardness of soft regions)" shown in the table indicates the average hardness HVs of the soft regions when a strength change region is present, but indicates the average hardness of the soft regions (I) and (V) whose strength is changed in the member when a strength change region is not present.

[0105] Furthermore, the "suitability of formula 1" shown in the table indicates whether the conditions set for the analysis satisfy Lt / H2 > {-0.0018 x (4.0 x HVh - 297) + 2.54} x Ls / H2 + {0.0012 x (4.0 x HVh - 297) - 1.96}, the "suitability of formula 2" shown in the table indicates whether the conditions set for the analysis satisfy Lt / H2 > 5Ls / H2 + {-0.0012 x (4.0 x ΔHV - 297) - 0.80}, and the "suitability of formula 3" shown in the table indicates whether the conditions set for the analysis satisfy Ls / H2 + Lt / H2 < 1.

[0106] Other various conditions, the FEM analysis solver, and the material fracture prediction software are as described above.

[0107] The above-mentioned FEM analysis was carried out to confirm the load-displacement curve of the member subjected to axial compression load. Tables 1 to 17 show the analysis conditions and evaluation results.

[0108] The "plastic work EA / EA" shown in the table 0 The value of EA / EA was calculated based on the above method. 0 When the value is 1.5 or more, it is judged that sufficient plastic work is obtained and the shock absorbing properties against the shock from the longitudinal direction of the member are excellent.

[0109] As can be seen from Tables 1 to 17, among Example Nos. 1 to 73, the inventive examples obtained sufficient plastic work and had excellent impact absorption properties. In contrast, among Example Nos. 1 to 73, the comparative examples did not obtain sufficient plastic work and had poor impact absorption properties.

[0110]

[0111]

[0112]

[0113]

[0114]

[0115]

[0116]

[0117]

[0118]

[0119]

[0120]

[0121]

[0122]

[0123]

[0124]

[0125]

[0126]

[0127] According to the above-described aspects of the present invention, an automobile frame member having excellent impact absorption properties against impacts from the longitudinal direction of the member can be provided, and therefore has high industrial applicability.

[0128] REFERENCE SIGNS LIST 1 automobile frame member 11 strength change region 11a soft region 11b transition region 11c hard region

Claims

1. An automobile frame member for absorbing impacts from the traveling direction of a vehicle, wherein the longitudinal length of the automobile frame member is L in mm, the length of the short side of the smallest circumscribing rectangle of the cross section of the member observed from the longitudinal direction is A in mm, the measurement interval when measuring Vickers hardness is X = A / 40 in mm, the minimum number of measurement points when measuring Vickers hardness is Y = 100 or Y = L / X, whichever is smaller, Vickers hardness is measured at Y or more measurement points at intervals of X mm from an arbitrary position of the automobile frame member along the longitudinal direction, the average Vickers hardness of all measurement points is HVave, the average Vickers hardness of the five largest values ​​of all measurement points is HVmax, and a region where three or more consecutive measurement points have a Vickers hardness of HVmax-33Hv or more is defined as a hard region, the average value of the Vickers hardness of the five smallest values ​​among all the measurement points is defined as HVmin, a region where three or more consecutive measurement points have a Vickers hardness of HVmin+33Hv or less is defined as a soft region, and a region where three or more consecutive measurement points have a Vickers hardness of more than HVmin+33Hv and less than HVmax-33Hv is defined as a transition region, the HVave is 400Hv or more and 800Hv or less, and a strength change region is included in which the soft region, the transition region, the hard region, the transition region, and the soft region are arranged in this order along the longitudinal direction, the average length in the longitudinal direction of the soft regions included in the strength change region is defined as Ls, and the average length in the longitudinal direction of the transition regions included in the strength change region is defined as Lt, an automobile skeleton member characterized in that, when the length from the longitudinal center position of one of the soft regions included in the strength change region to the longitudinal center position of the other of the soft regions is H2 (unit: mm), the average Vickers hardness of the hard regions included in the strength change region is HVh, and the average Vickers hardness of the soft regions included in the strength change region is HVs, the following Equation 1 is satisfied.(Formula 1): Lt / H2>{-0.0018×(4.0×HVh-297)+2.54}×Ls / H2+{0.0012×(4.0×HVh-297)-1.96}.

2. The automobile frame member according to claim 1, characterized in that, when the value obtained by subtracting the HVs from the HVh is taken as ΔHV, the following (formula 2) and (formula 3) are satisfied. (Formula 2): Lt / H2>5Ls / H2+{-0.0012×(4.0×ΔHV-297)-0.80} (Formula 3): Ls / H2+Lt / H2<1 3. An automobile frame member according to claim 1 or 2, characterized in that, when the average value of Vickers hardness of the strength change region is HVsth, the HVsth is 400 Hv or more and 800 Hv or less.

4. An automobile frame member according to claim 1 or 2, characterized in that the cross-sectional shape of the member observed from the longitudinal direction is a single hat type or a double hat type.

5. An automobile frame member according to claim 3, characterized in that the cross-sectional shape of the member observed from the longitudinal direction is a single hat type or a double hat type.

Citation Information

Patent Citations

  • Novel vehicle body side collision structure based on sliding door vehicle type

    CN214057454U

  • Automobile column

    US20110233966A1

  • Structural member for automobile body

    WO2015198867A1