Poly(ethylene terephthalate) film for vapor deposition and transparent gas-barrier film

By modifying the PET film surface to achieve a C-O-C peak area ratio of 58.5% through corona treatment and depositing aluminum oxide and silicon oxide, the PET film achieves enhanced gas barrier performance and transparency, addressing the insufficiencies of existing PET films in barrier properties.

WO2024214769A1PCT designated stage expired Publication Date: 2024-10-17TOYOBO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014652
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-11
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing PET films used for transparent gas barrier films do not achieve sufficient barrier performance even with inorganic layer deposition due to inadequate surface treatment, leading to insufficient adhesion and barrier properties.

Method used

A polyethylene terephthalate film with a modified surface having a C-O-C peak area ratio of 58.5% or more, achieved through corona treatment, is used for vapor deposition of an inorganic layer, specifically aluminum oxide and silicon oxide, to enhance adhesion and barrier properties without an overcoat.

Benefits of technology

The modified PET film enables the formation of a dense inorganic layer, resulting in improved gas barrier performance and transparency, maintaining barrier properties over time while being cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014652_17102024_PF_FP_ABST
    Figure JP2024014652_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a poly(ethylene terephthalate) film (PET film) for producing a transparent gas-barrier film which is inexpensive, has excellent transparency, can retain barrier properties, and makes it possible to preserve the contents over a long period; and a transparent gas-barrier film which comprises this PET film as a base and has improved barrier performance. This PET film for vapor deposition is for use in applications where an inorganic layer is vapor-deposited, and is characterized by having a modified surface on the side where the inorganic layer is to be vapor-deposited. The PET film is further characterized in that, when O1s peaks obtained from an analysis of the modified surface by X-ray photoelectron spectroscopy (XPS) are subjected to waveform fitting with respect to a C-O-C peak (533.1 eV) and a C=O peak (531.5 eV), then the proportion of the area of the C-O-C peak in the total area is 58.5% or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Polyethylene terephthalate film for vapor deposition and transparent gas barrier film

[0001] The present invention relates to a polyethylene terephthalate film (PET film) that is excellent in transparency, gas barrier properties, printability, and flexibility and is used as a packaging material for foods, medicines, electronic components, etc., which require airtightness, or as a base material for a transparent gas barrier film that has excellent properties as a gas blocking material, and to a transparent gas barrier film using the same.

[0002] Transparent gas barrier films are made by laminating an inorganic material onto a plastic film. Metal oxides are often used as the inorganic material from the viewpoint of transparency. In particular, films made by laminating silicon oxide, aluminum oxide, or mixtures of these metal oxides by vapor deposition or CVD are mainly commercially available (see, for example, Patent Document 1).

[0003] The surface of the PET film on which the inorganic material barrier layer is laminated is subjected to anchor coating to improve the adhesive strength between the barrier layer and the PET film or the barrier properties, or the surface of the PET film is modified with plasma or the like.

[0004] Although not for a PET film used in a transparent gas barrier film, a method has been described in which the surface of a PET film is subjected to atmospheric pressure plasma treatment to adjust the peak derived from a C-C bond in the valence band spectrum determined by X-ray photoelectron spectroscopy (XPS), thereby improving the adhesion of the film (see, for example, Patent Document 2).

[0005] Furthermore, with regard to PET films for battery exteriors other than transparent gas barrier films, polyester films for battery exteriors are known in which the film surface is subjected to a corona treatment or the like to improve the delamination resistance after bonding of aluminum foil (see, for example, Patent Document 3).

[0006] In addition, a method has been described in which the surface of a PET film is subjected to reactive ion etching (RIE), the C1s peak obtained by XPS is separated into three waveforms derived from C-C, C-O, and O-C=O, and the area ratio of the separated waveform of O-C=O is adjusted to 16.2 to 17.8%, thereby improving adhesion (see, for example, Patent Document 4).

[0007] Patent No. 02638797 Publication JP 2010-59308 JP 2012-238491 JP 2018-69477

[0008] However, according to the investigations of the present inventors, it has been found that the PET film described in Patent Document 2 is subjected to atmospheric pressure plasma treatment, and therefore sufficient barrier performance cannot be obtained even if an inorganic layer is vapor-deposited.

[0009] Furthermore, it has been found that the polyester film described in Patent Document 3 does not have a sufficient degree of corona treatment or the like, and therefore, even if an inorganic layer is vapor-deposited, sufficient barrier performance cannot be obtained.

[0010] Therefore, an object of the present invention is to provide a PET film, which is a vapor-deposited raw sheet of a transparent gas barrier film, having an improved surface condition that improves barrier performance, without using an anchor coat in which another resin is laminated on the substrate or an overcoat in which a resin is laminated on the inorganic layer that serves as a barrier layer, in order to improve the gas barrier performance of the transparent gas barrier film having an inorganic substance formed on the PET film.An object of the present invention is also to provide a transparent gas barrier film using the PET film as a substrate, with improved barrier performance.

[0011] The present inventors have conducted extensive research into the optimal surface condition of the PET film used as the raw material in order to improve the barrier properties of a transparent gas barrier film having an inorganic layer laminated thereon, and have discovered a PET film with a surface condition that densifies the inorganic layer, leading to the present invention.

[0012] That is, the present invention includes the following: [1] A polyethylene terephthalate film for vapor deposition used in applications in which an inorganic layer is vapor-deposited, the polyethylene terephthalate film having a modified surface on the side on which the inorganic layer is vapor-deposited, and when the O1s peak obtained by X-ray photoelectron spectroscopy (XPS) of the modified surface is waveform-fitted with a C-O-C peak (533.1 eV) and a C=O peak (531.5 eV), the area ratio of the C-O-C peak to the total area is 58.5% or more. [2] The polyethylene terephthalate film for vapor deposition according to [1], wherein the modified surface is formed by corona treatment. [3] A transparent gas barrier film comprising: a polyethylene terephthalate film having a modified surface, in which, when the O1s peak obtained by X-ray photoelectron spectroscopy (XPS) is waveform-fitted with a C-O-C peak (533.1 eV) and a C=O peak (531.5 eV), the area ratio of the C-O-C peak to the total area is 58.5% or more; and an inorganic layer vapor-deposited on the modified surface. [4] The transparent gas barrier film according to [3], in which the modified surface is formed by corona treatment. [5] The transparent gas barrier film according to [3] or [4], in which the inorganic layer contains aluminum oxide and silicon oxide.

[0013] The present invention provides a PET film for producing a transparent gas barrier film that is inexpensive, has excellent transparency, and can maintain its barrier properties, allowing contents to be stored for a long period of time. It also provides a transparent gas barrier film that uses the PET film as a substrate and has improved barrier properties.

[0014] It is a figure which shows the X-ray spectroscopy spectrum (O1s) of the modified surface of the PET film. It is a cross-sectional view for explaining corona treatment. It is a schematic diagram of an evaporation apparatus of the electron beam heating type.

[0015] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0016] The polyethylene terephthalate film for vapor deposition of the present invention is a polyethylene terephthalate film for vapor deposition used in applications in which an inorganic layer is vapor-deposited, and is characterized in that it has a modified surface on the side on which the inorganic layer is vapor-deposited, and when the O1s peak obtained by X-ray photoelectron spectroscopy (XPS) of the modified surface is waveform-fitted with a C—O—C peak (533.1 eV) and a C═O peak (531.5 eV), the area ratio of the C—O—C peak to the total area is 58.5% or more.

[0017] The O1s peak obtained by X-ray photoelectron spectroscopy (XPS) referred to in the present invention is obtained by analyzing the energy of photoelectrons emitted by exciting the surface of a PET film with Al Kα rays, as shown in FIG. 1, and plotting electrons originating from the 1s orbital of oxygen atoms with the electron binding energy on the horizontal axis and the number (signal intensity) on the vertical axis.

[0018] In addition, although the 1s orbital energy of an oxygen atom is fixed, when it bonds with other atoms, the energy of the electron orbit changes, causing the bond energy peak to shift. The C-O-C peak (533.1 eV) and C=O peak (531.5 eV) referred to in the present invention refer to the C-O-C peak 22 near the bond energy of 533.1 eV and the C=O peak 23 near the bond energy of 531.5 eV observed in a PET film.

[0019] The C—O—C peak 22 near 533.1 eV and the C═O peak 23 near 531.5 eV in the present invention are separated by fitting a function to the actually measured O1s peak 21. The Voigt function is often used as the function for fitting.

[0020] In the present invention, the function shown in Equation 1 is used for ease of calculation.

[0021] f(x, a, b, c, n) = a・(1 / (((x-b) / c) 2 +1)) n (Equation 1) In equation 1, a represents a value proportional to the peak intensity, x represents the binding energy, b represents the peak position on the binding energy, c represents a peak shape parameter (related to the shape of the base of the peak), and n represents a peak shape parameter (related to the attenuation from the peak position).

[0022] The O1s peak 21 is measured in a state superimposed on a background 26 by a spectrometer used to measure the wavelength distribution of the exciting X-rays, inelastic scattering of the peak electrons, secondary electrons, multiple scattering, and the kinetic energy of the electrons.

[0023] There are the Shriley method and the Tougaard method for calculating background based on physical assumptions, but in the present application, correction is performed using a straight line method that connects the vicinity of 544 eV and the vicinity of 524 eV, which are distant from the peak position, with a straight line.

[0024] The area ratio of the C—O—C peak 22 during waveform fitting referred to in the present application is calculated as a percentage of the area ratio of the C—O—C peak to the total area of ​​the area surrounded by the background 26 and the C—O—C peak 22 and the area surrounded by the C═O peak 23 and the background 26, with the sum of these areas being set to 100%.

[0025] The area ratio of the C-O-C peak on the modified surface is 58.5% or more, preferably 59.0% or more, and more preferably 60.0% or more. A value of 58.5% or more tends to improve the water vapor transmission rate (WVTR). Even when forming an inorganic layer by vapor deposition, deterioration of the WVTR is minimized even in poor conditions of the vapor deposition apparatus and relatively high pressure. Furthermore, the C-O-C peak area ratio is preferably 62.0% or less. When the area ratio is 62.0% or less, corona strike-through (the phenomenon in which the back side of the treated surface is treated) is less likely to occur, and blocking is less likely to occur when the film is wound into a roll.

[0026] The inorganic layer in the present invention may be made of a metal such as Al, Si, Ti, Zn, Zr, Mg, Sn, Cu, or Fe, or an oxide, nitride, fluoride, or sulfide of these metals. Specific examples include SiOx (x=1.0 to 2.0), alumina, magnesia, zinc sulfide, titania, zirconia, cerium oxide, or a mixture thereof.

[0027] In particular, aluminum oxide, silicon oxide and mixtures thereof are suitable for use as transparent gas barrier films, and the modified surface of the present invention is particularly effective for the binary vapor deposition of aluminum oxide and silicon oxide.

[0028] The PET film referred to in the present invention refers to a film obtained by melt-extruding a PET resin whose main raw material is polyethylene terephthalate obtained by polymerizing ethylene glycol and terephthalic acid, to which other polymers may be mixed to adjust the film properties, or to which known additives such as ultraviolet absorbers, antistatic agents, plasticizers, lubricants, and colorants may be added, and then, as necessary, stretching in the machine direction (MD) and / or the transverse direction (TD), cooling, and heat setting.

[0029] The thickness of the PET film is not particularly limited, but the thickness of the PET film of the present invention is preferably in the range of 5 to 1000 μm, and more preferably in the range of 7 to 25 μm for roll-to-roll vacuum deposition.

[0030] In the present invention, as a preferred condition of the PET film, a corona treatment is preferred as a method for increasing the area ratio of the C—O—C peak to 58.5% or more.

[0031] Although it is preferable that each value is high, the PET film may be processed on surfaces other than the intended surface or may be damaged by heat during the processing process, so the values ​​are set as high as possible within the allowable range of other physical properties.

[0032] Corona treatment is a method of treating the surface of PET with plasma by generating a discharge in the atmosphere. For example, the corona treatment method shown in Figure 2 can be used to corona treat a long PET film. A high AC voltage of 10 to 60 kHz is applied to an electrode 4 in the atmosphere to cause a discharge. The PET film 6 to be treated runs over a dielectric-coated roll 5 covered with silicone rubber or the like, and is treated with plasma generated between the dielectric-coated roll 5 and the electrode 4.

[0033] The degree of treatment, which is related to the area ratio of the C—O—C peak, can be adjusted by adjusting the distance between the electrode 4 and the dielectric-coated roll 5 , the power applied to the electrode 4 and the dielectric-coated roll 5 , and the running speed of the PET film 6 .

[0034] Generally, the gap between the electrode 4 and the dielectric-coated roll 5 is set to 5 mm or less. If the gap is too large, discharge becomes difficult. If the gap is narrowed, the treatment degree increases and the area ratio of the C-O-C peak increases. A narrow gap is preferable, but if it is too narrow, the electrode will deform and the film will flap, causing contact between the film and the electrode and scratches.

[0035] Increasing the power applied to the electrode 4 and the dielectric-coated roll 5 increases the degree of treatment and the area ratio of the C-O-C peak. Simply increasing the power can cause abnormal discharge or the electrodes to heat up and deform, so the number and shape of the electrodes must be selected appropriately.

[0036] Furthermore, when the treatment is carried out with the same electric power, if the traveling speed of the PET film 6 is slowed down, the treatment degree increases and the area ratio of the C—O—C peak increases.

[0037] Although it is possible to supply gas such as nitrogen or helium between the discharge electrodes to generate a discharge, it is preferable to use normal atmospheric air containing 78% nitrogen and 21% oxygen. To ensure stable processing, a fixed amount of atmospheric air with a stable temperature and humidity is blown through a filter.

[0038] Corona discharge converts some of the oxygen in the air into ozone, which changes the surface of the PET film. Free release of ozone can have an adverse effect on the human body and also on the degree of surface treatment, so it is preferable to surround the corona treatment area and exhaust the air uniformly.

[0039] The corona treatment can be carried out on a PET film that has already been formed using a rewinder equipped with a corona treatment device or a slitter that changes the width of the film, but it is preferable to carry out the corona treatment on the PET film during film formation.

[0040] That is, it is preferable to melt the PET resin, extrude it through a T-die, stretch it in the MD (film running direction), stretch it in the TD (film width direction), and then treat it through a corona treatment machine.

[0041] By carrying out the treatment in the same step, not only can the treatment be carried out easily, but also the corona treatment can be carried out in a fresher state on the surface of the PET film, which is preferable.

[0042] Furthermore, the transparent gas barrier film of the present invention is a transparent gas barrier film characterized by laminating an inorganic layer on the above-mentioned PET film. That is, the transparent gas barrier film of the present invention is a transparent gas barrier film comprising: a polyethylene terephthalate film having a modified surface in which, when the O1s peak obtained by X-ray photoelectron spectroscopy (XPS) is waveform-fitted with a C—O—C peak (533.1 eV) and a C═O peak (531.5 eV), the area ratio of the C—O—C peak to the total area is 58.5% or more; and an inorganic layer vapor-deposited on the modified surface.

[0043] As a method for laminating an inorganic layer on the PET film of the present invention, a dry process using a vacuum is suitable. Among them, a vapor deposition method is suitable. The vapor deposition method allows for laminating an inorganic layer over a large area at high speed.

[0044] The deposition method can be any of the following: a resistance heating method in which the deposition material is evaporated using a resistance heating boat; an induction heating method in which the deposition material is placed in a carbon crucible and heated by applying a high-frequency electromagnetic field; and an electron beam heating method in which the deposition material is heated using an electron gun.

[0045] A schematic diagram of an electron beam heating type vapor deposition apparatus is shown in Fig. 3. A process for laminating an inorganic layer will be described, but the present invention is not limited to this.

[0046] A PET film having a modified surface with a C—O—C peak area ratio of 58.5% or more according to the present invention (hereinafter referred to as the present PET film) is prepared on the unwinding roll 7 of the vapor deposition device.

[0047] The present PET film 8 is unwound from the unwinding roll 7 and its surface is treated by a plasma treatment device 9. The plasma treatment device 9 has electrodes and is designed to allow gas to be introduced between the electrodes and the present PET film 8. A direct current or alternating current voltage is applied to the electrodes to cause a discharge and generate plasma. The surface is treated by this plasma. The purpose of the plasma treatment is to remove moisture and other substances that adhere to the present PET film when it is stored in the atmosphere. For this purpose, a rare gas such as argon is preferably introduced.

[0048] After passing through the plasma treatment device 9, the present PET film 8 is transferred to a coating roll 10 cooled to −20° C. An electron beam 12 emitted from an electron gun 11 heats a deposition material 13 placed in a crucible, evaporating the material, and an inorganic layer is laminated on the modified surface of the present PET film 8.

[0049] A transparent gas barrier film (hereinafter referred to as the transparent gas barrier film of the present invention) having an inorganic layer laminated on the modified surface of the PET film 8 of the present invention has electrons charged on the surface of the transparent gas barrier film of the present invention removed by a static eliminator 14 before leaving the coating roll 10. The transparent gas barrier film of the present invention is detached from the coating roll 10 and taken up onto a take-up roll 17, but before that the film thickness or film thickness and composition of the laminated inorganic layer are measured using an optical film thickness meter 15, a fluorescent X-ray film thickness meter 16, or both. In order to achieve the target film thickness or film thickness and composition, the measured values ​​are fed back to the electron gun 11, and the intensity and scanning of the electron beam 12 are adjusted to the target values.

[0050] The inorganic layer of the transparent gas barrier film of the present invention preferably has a thickness of 5 nm to 30 nm. If it is too thin, the film will not be uniform and the barrier properties will not be maintained. If it is too thick, the inorganic layer will crack when the transparent gas barrier film of the present invention is deformed, resulting in a decrease in the barrier properties.

[0051] As described above, aluminum oxide, silicon oxide, and mixtures thereof are suitable for the inorganic layer of the transparent gas barrier film of the present invention. A mixture of aluminum oxide and silicon oxide is particularly suitable. In particular, in the mixture of aluminum oxide and silicon oxide, the aluminum oxide content is preferably 20 to 60 mass %. When the aluminum oxide content is 20 mass % or more, the barrier properties are improved. When the content is 60 mass % or less, the inorganic layer does not become too hard, and it is possible to prevent the inorganic layer from cracking and the barrier properties from decreasing when the transparent gas barrier film is deformed.

[0052] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The physical properties and characteristics in the examples were measured or evaluated by the following methods.

[0053] (1) Area ratio of C-O-C peaks The O1s peak by X-ray photoelectron spectroscopy (XPS) was measured using a K-Alpha+ manufactured by Thermo Fisher Scientific. The measurement conditions are as follows: Excitation X-ray: Monochromated AlKa ray X-ray output: 12 kV, 6 mA Photoelectron escape angle: 90° Spot size: 400 μmφ Pass energy: 50 eV Step: 0.1 eV The peak position was corrected by setting the peak derived from the aromatic ring in the C1s spectrum at 284.8 eV.

[0054] The measured O1s peak 21 was subjected to background correction using the linear method, and was assumed to consist of a C—O—C peak (533.1 eV) 22, a C═O peak (531.5 eV) 23, peak 1 (535.5 eV) 24, and peak 2 (538.5 eV) 25. Equation 1 was applied to each peak and the peaks were separated using least-squares fitting.

[0055] The obtained peaks were numerically integrated to determine the area of ​​each peak, and the area ratio (%) of the C—O—C peak to the total area was determined, assuming that the total area of ​​the C—O—C peak and the C═O peak was 100%.

[0056] (2) Water Vapor Transmission Rate (WVTR) Water vapor transmission rate (WVTR) was measured in accordance with JIS K7129 Method B using a water vapor transmission rate measuring device (MOCON PRMATRAN-W3 / 34G, USA) under the measurement conditions of a temperature of 40° C. and a humidity of 90% RH.

[0057] Example 1: PET resin was melted, extruded through a T-die, stretched in the MD, and then stretched in the TD. The PET film surface was then treated with a corona treatment device. Using data obtained by analyzing PET films with previously altered treatment conditions using XPS, the distance between the PET film and the electrodes and the power applied to the electrodes were adjusted to adjust the conditions so that the C-O-C (533.1 eV) at the O1s peak was 58.5%. After corona treatment, the film was wound up on a take-up roll. The PET film had a thickness of 12 μm.

[0058] The wound PET film was slit to a width suitable for processing in an electron beam deposition apparatus, and the PET film was placed in an electron beam deposition apparatus as shown in Figure 3. Alumina and silica with a purity of 99% or higher were placed in a crucible. After evacuating the deposition apparatus, the placed PET film was withdrawn from the unwinding roll and passed through an argon gas plasma. A mixed film of alumina and silica was laminated as an inorganic layer on a coating roll cooled to -20°C. After laminating the alumina-silica film, the film was neutralized and peeled from the coating roll. The film thickness and composition were measured using a fluorescent X-ray film thickness meter. The electron gun was controlled to achieve a film thickness of 13 nm and an aluminum oxide content of 45% by mass. After winding the transparent gas barrier film on the winding roll and opening it to the atmosphere, a sample was taken of the film and its WVTR was measured. The results are shown in Table 1. Furthermore, the remaining PET film remaining on the unwinding roll was sampled to confirm the contact angle, and the area ratio of the C-O-C peak was measured. The results are shown in Table 1.

[0059] (Examples 2 to 5) PET films were produced in the same manner as in Example 1. The treatment conditions of the corona treatment device were changed to obtain PET films with the C-O-C peak area ratios shown in Table 1. An alumina-silica inorganic layer was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 1.

[0060] (Example 6) A PET film was produced in the same manner as in Example 2. The treatment conditions of the corona treatment device were changed to obtain a PET film with the dynamic contact angle shown in Table 1. Furthermore, a transparent gas barrier film was produced under the same conditions as in Example 2, except that instead of laminating an inorganic layer of alumina-silica, only alumina with a purity of 99% or more was laminated, and the WVTR was measured. The results are shown in Table 1.

[0061] Comparative Example 1 A PET film was produced in the same manner as in Example 1. The treatment conditions of the corona treatment device were changed to obtain a PET film having the C-O-C peak area ratio shown in Table 1. An alumina-silica inorganic layer was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 1.

[0062] Comparative Example 2 A PET film was produced in the same manner as in Example 1. However, the corona treatment device was stopped from operating. An inorganic layer of alumina-silica was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 1.

[0063] Comparative Example 3 A transparent gas barrier film was produced under the same conditions as in Example 1 of the present application using a PET film that had been subjected to a corona treatment under the same conditions as in Example 1 of JP 2012-238491 A, and the WVTR was measured. That is, a PET film was produced in the same manner as in Example 1 of the present application, and then a corona discharge treatment was applied to the upper surface of the film with an E value of 30 and the film was taken up to obtain a polyester film. The results are shown in Table 1. The E value is the corona discharge treatment intensity, and is a function of the applied voltage (Vp), applied current (Ip), treatment speed (S), and treatment width (Wt), where E = (Vp × Ip) / (S × Wt).

[0064] Comparative Example 4 A transparent gas barrier film was produced under the same conditions as in Example 1 of the present application using a PET film that had been subjected to a corona treatment under the same conditions as in Example 3 of JP 2012-238491 A, and the WVTR was measured. That is, a PET film was produced in the same manner as in Example 1 of the present application, and then the upper surface of the film was subjected to a corona discharge treatment with an E value of 60 and taken up to obtain a polyester film. The results are shown in Table 1.

[0065]

[0066] As the results in Table 1 show, in Examples 1 to 6, the area ratio of the C-O-C peak was 58.5% or more, and therefore the WVTR of the transparent gas barrier films using those PET films was small. This is thought to be because a dense inorganic layer could be formed, and as can be seen from a comparison between Examples 2 and 6, this effect was particularly remarkable when an alumina-silica inorganic layer was formed. In contrast, in Comparative Examples 1 to 4, the area ratio of the C-O-C peak was smaller than 58.5%, and therefore the WVTR of the transparent gas barrier films using those PET films was large.

[0067] The present invention can provide a PET film that is a substrate for producing a transparent gas barrier film that has excellent properties as a gas barrier material, and can also provide a transparent gas barrier film that uses the substrate and has excellent properties as a gas barrier material.

[0068] 4: Electrode 5: Dielectric-coated roll 6: PET film 7: Unwinding roll 8: PET film of the present invention 9: Plasma treatment device 10: Coating roll 11: Electron gun 12: Electron beam 13: Vapor deposition material 14: Static neutralizer 15: Optical film thickness meter 16: Fluorescent X-ray film thickness meter 17: Winding roll 21: O1s spectrum 22: C-O-C peak 23: C=O peak 24: Peak 1 25: Peak 2 26: Background

Claims

1. A polyethylene terephthalate film for deposition used in applications in which an inorganic layer is deposited, the polyethylene terephthalate film having a modified surface on the side on which the inorganic layer is deposited, and when an O1s peak obtained by X-ray photoelectron spectroscopy (XPS) of the modified surface is waveform-fitted with a C-O-C peak (533.1 eV) and a C=O peak (531.5 eV), the area ratio of the C-O-C peak to the total area is 58.5% or more.

2. The polyethylene terephthalate film for deposition according to claim 1, wherein the modified surface is formed by corona treatment.

3. A transparent gas barrier film comprising: a polyethylene terephthalate film having a modified surface in which, when the O1s peak obtained by X-ray photoelectron spectroscopy (XPS) is waveform-fitted with a C-O-C peak (533.1 eV) and a C=O peak (531.5 eV), the area ratio of the C-O-C peak to the total area is 58.5% or more; and an inorganic layer vapor-deposited on the modified surface.

4. The transparent gas barrier film according to claim 3, wherein the modified surface is formed by corona treatment.

5. The transparent gas barrier film according to claim 3 or 4, wherein the inorganic layer contains aluminum oxide and silicon oxide.

Citation Information

Patent Citations

  • Vapor deposited film

    JP1987077453A

  • Polyester-based film for vapor deposition

    JP1991126860A

  • Gas barrier laminated film and its manufacturing method

    JP2007210208A

  • Vapor-deposited polyester film

    JP2017065264A