Rectangular wire and production method for same
The extrusion molding method using a fluorine-containing copolymer provides a high-productivity, smooth, and adherent insulating coating for rectangular wires, addressing the issues of existing methods by ensuring excellent followability and insulation performance during deformation.
Patent Information
- Application Number
- PCT/JP2024/014823
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
The existing methods for manufacturing rectangular wires with insulating coatings face challenges such as low productivity, poor surface smoothness, and poor followability during bending deformation due to the use of powder coating and baking processes, leading to issues like peeling and wrinkles.
A method involving extrusion molding with a fluorine-containing copolymer, specifically a polyaryletherketone and a fluorine-containing copolymer based on tetrafluoroethylene, is used to form a uniform insulating coating around a rectangular conductor, ensuring excellent adhesion and smoothness, and maintaining insulation properties even during deformation.
The solution results in a rectangular wire with high productivity, excellent surface smoothness, and improved followability during bending, preventing peeling and wrinkles, while maintaining high insulation properties and partial discharge inception voltage.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Flat wire and its manufacturing method
[0001] This application claims priority to Japanese Patent Application No. 2023-064886, filed on April 12, 2023, the contents of which are incorporated herein by reference.
[0002] There is a demand for smaller and lighter vehicle equipment and the like used in automobiles, railways, aircraft, and the like. Therefore, there is a demand for thinner coatings of insulating coating materials for insulated wires of electrical equipment used in such vehicle equipment. Furthermore, as electrical equipment becomes higher in output and voltage, there is a demand for such insulating coating materials to have strong adhesion to conductors as well as excellent insulation properties.
[0003] By using a rectangular conductor for the electric wire, the space factor when coiled is higher than that of a round wire. As a result, the overall space required for the coil can be saved, contributing to the miniaturization of electrical equipment. However, with rectangular conductors, it is more difficult to form a uniform insulating coating than with round wires, and there is a problem in that the insulation cannot be maintained sufficiently.
[0004] Patent Document 1 discloses a method for manufacturing a rectangular wire, in which a powder having an average particle diameter of 0.02 μm or more and 150 μm or less is applied to a rectangular conductor, the powder containing a melt-moldable fluororesin having a melting point of 100°C or more and 325°C or less and at least one functional group selected from the group consisting of a carbonyl group-containing group, a hydroxy group, an epoxy group, and an isocyanate group, thereby forming an insulating coating layer having a thickness of 10 to 150 μm on the outer periphery of the rectangular conductor.
[0005] JP 2017-204410 A
[0006] However, the manufacturing method described in Patent Document 1 requires a powder preparation step and a firing step after the powder coating, resulting in low productivity. Furthermore, the powder coating reduces the surface smoothness of the insulating coating. Furthermore, the insulating coating has poor conformability to the rectangular conductor, resulting in wrinkles in the insulating coating or peeling off from the rectangular conductor when the rectangular wire is bent.
[0007] The present invention aims to provide a rectangular wire that is highly productive and has excellent surface smoothness of the insulating coating film and excellent followability of the insulating coating film to the rectangular conductor during bending deformation, as well as a method for manufacturing the same.
[0008] The present invention has the following aspects: [1] A rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, wherein the insulating coating material has a melt flow rate of 20.0 to 300.0 g / 10 min at a temperature of 372°C and a load of 49 N, the coating of the insulating coating material has an average thickness of 10 to 1000 μm, and the unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the rectangular wire is less than 0.06 mm, and the insulating coating material is polyaryl ether ketone (A [2] A rectangular wire comprising a cross-sectional area of the rectangular conductor of 2.6 mm2 or more, and a fluorine-containing copolymer (B) having a unit based on tetrafluoroethylene, wherein the fluorine-containing copolymer (B) comprises one or more selected from the group consisting of a fluorine-containing resin (B1) and a fluorine-containing elastomer (B2) having a melting point of 260°C or more, wherein the content of the fluorine-containing copolymer (B) relative to the total mass of the polyaryl ether ketone (A) and the fluorine-containing copolymer (B) in the insulating coating material is 5 mass% or more, and the coating of the insulating coating material does not peel off from the rectangular conductor in a winding test in accordance with "5.1.2 Flat Wire of JIS 3216-3:2011." 2 [3] The fluorine-containing resin (B1) is —CH 2 It has an OH group, and the —CH 2 The content of OH groups is 1×10 6[4] The rectangular wire according to any one of [1] to [3], wherein the fluorine-containing elastomer (B2) has iodine atoms, and the content of the iodine atoms is 0.05 mass% or more relative to the total mass of the fluorine-containing elastomer (B2). [5] The rectangular wire according to any one of [1] to [4], wherein the insulating coating material has a partial discharge inception voltage of 600 Vrms or more. [6] A method for producing a rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction and a coating of an insulating coating material formed by extrusion molding and directly covering the entire circumferential direction of the rectangular conductor, the method comprising the steps of: melting a composition containing polyaryl ether ketone (A) and a fluorine-containing copolymer (B) having units based on tetrafluoroethylene using an extruder equipped with a die; and extruding the molten composition from the die around the rectangular conductor to coat the rectangular conductor with the molten composition and form the insulating coating material; and [7] A method for producing a rectangular wire according to [6], wherein the drawdown ratio DDR calculated by the following formula 1 is 0.5 or more and less than 10.0, and the insulating coating has an average thickness of 10 to 1000 μm, and the unbiased standard deviation of the insulating coating thickness in the axial direction of the rectangular wire is less than 0.06 mm, the fluorine-containing copolymer (B) comprises one or more selected from the group consisting of a fluorine-containing resin (B1) and a fluorine-containing elastomer (B2) having a melting point of 260°C or higher, and the content of the fluorine-containing copolymer (B) relative to the total mass of the polyaryletherketone (A) and the fluorine-containing copolymer (B) in the composition is 5 mass% or more, and the insulating coating does not peel off from the rectangular conductor in a winding test in accordance with "JIS 3216-3:2011, 5.1.2 Flat Wire." DDR = (D A -C A ) / (F A -C A ) Formula 1 In the above formula 1, D A is the opening area of the die (mm 2 ) and C Ais the cross-sectional area (mm 2 ) and F A is the cross-sectional area (mm 2 [8] The cross-sectional area of the rectangular conductor is 2.6 mm 2 [9] The method for producing a rectangular wire according to [6] or [7], wherein the fluorine-containing resin (B1) is —CH 2 It has an OH group, and the —CH 2 The content of OH groups is 1×10 6[1A] The method for producing a rectangular wire according to any one of [6] to [8], wherein the number of iodine atoms in the fluorine-containing elastomer (B2) is more than 30, relative to the total mass of the fluorine-containing elastomer (B2).
[10] The method for producing a rectangular wire according to any one of [6] to [9], wherein the fluorine-containing elastomer (B2) has iodine atoms, and the content of the iodine atoms is 0.05 mass% or more relative to the total mass of the fluorine-containing elastomer (B2).
[11] The method for producing a rectangular wire according to any one of [6] to
[10] , wherein the partial discharge inception voltage of the insulating coating material is 600 Vrms or more. [1A] A rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, wherein the insulating coating material has a melt flow rate of 20.0 to 300.0 g / 10 min, 30.0 to 250.0 g / 10 min, 40.0 to 200.0 g / 10 min, or 50.0 to 230.0 g / 10 min at a temperature of 372°C and a load of 49 N, the coating of the insulating coating material has an average thickness of 10 to 1000 μm, 20 to 500 μm, or 50 to 200 μm, and the unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the rectangular wire is less than 0.06 mm, 0.03 mm or less, 0.01 mm or less, 0.001 mm or more but less than 0.06 mm, 0.001 to 0.03 mm, or 0.00 a thickness of 1 to 0.01 mm, the insulating coating material comprising a polyaryl ether ketone (A) and a fluorine-containing copolymer (B) having units based on tetrafluoroethylene, the fluorine-containing copolymer (B) comprising one or more selected from the group consisting of a fluorine-containing resin (B1) and a fluorine-containing elastomer (B2) having a melting point of 260°C or higher, 280°C or higher, 290°C or higher, 260 to 350°C, 280 to 340°C, or 290 to 330°C, the content of the fluorine-containing copolymer (B) relative to the total mass of the polyaryl ether ketone (A) and the fluorine-containing copolymer (B) in the insulating coating material being 5% by mass or higher, 5 to 45% by mass, or 10 to 30% by mass, and the flat wire is such that the coating of the insulating coating material does not peel off from the flat wire in a winding test in accordance with "JIS 3216-3:2011, 5.1.2 Flat wire." [2A] The cross-sectional area of the rectangular conductor is 2.6 mm 2 More than 3.0 mm 2 Above, 2.6 to 15 mm 2 , or 3.0 to 15 mm2 [3A] The fluorine-containing resin (B1) is —CH 2 It has an OH group, and the —CH 2 The content of OH groups is 1×10 6[4A] The flat wire according to any one of [1A] to [3A], wherein the fluorine-containing elastomer (B2) contains iodine atoms, and the content of the iodine atoms is 0.05% by mass or more, 0.1 to 5% by mass, or 0.2 to 1% by mass, relative to the total mass of the fluorine-containing elastomer (B2). [5A] The rectangular wire according to any one of [1A] to [4A], wherein the insulating coating material has a partial discharge inception voltage of 600 Vrms or more, 700 Vrms or more, 800 Vrms or more, 900 Vrms or more, 600 to 5000 Vrms, 700 to 4000 Vrms, 800 to 3000 Vrms, or 900 to 3000 Vrms.[6A] A method for producing a rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, the method comprising: using an extruder equipped with a die to melt a composition containing polyaryl ether ketone (A) and a fluorine-containing copolymer (B) having units based on tetrafluoroethylene; and extruding the molten composition from the die around the rectangular conductor to coat the conductor with the molten composition, thereby forming the insulating coating material; wherein the insulating coating material has a melt flow rate of 20.0 to 300.0 g / 10 min, 30.0 to 250.0 g / 10 min, 40.0 to 200.0 g / 10 min, or 50.0 to 230.0 g / 10 min at a temperature of 372 ° C. and a load of 49 N, and the coating of the insulating coating material has an average thickness of 10 to 1000 μm, 20 to 500 μm. or 50 to 200 μm, the unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the rectangular wire is less than 0.06 mm, 0.03 mm or less, 0.01 mm or less, 0.001 mm or more but less than 0.06 mm, 0.001 to 0.03 mm, or 0.001 to 0.01 mm, and the fluorine-containing copolymer (B) has a melting point of 260°C or more, 280°C or more, 290°C or more, 260 to 350°C, 280 to 340°C, or The method for producing a rectangular wire according to [6A], wherein the rectangular wire comprises one or more selected from the group consisting of a fluorine-containing resin (B1) and a fluorine-containing elastomer (B2) having a temperature of 290 to 330°C, wherein the content of the fluorine-containing copolymer (B) relative to the total mass of the polyaryl ether ketone (A) and the fluorine-containing copolymer (B) in the composition is 5% by mass or more, 5 to 45% by mass, or 10 to 30% by mass, and wherein the coating of the insulating coating material does not peel off from the rectangular conductor in a winding test in accordance with "JIS 3216-3:2011, 5.1.2, Flat Wire." [7A] The method for producing a rectangular wire according to [6A], wherein the drawdown ratio DDR calculated by the following formula 1 is 0.1 or more but less than 10.0, 0.5 or more but less than 10.0, 0.5 to 5, or 0.8 to 1.5. DDR=(D. A -C A ) / (F A -C A ) Formula 1 In the above formula 1, D A is the opening area of the die (mm2 ) and C A is the cross-sectional area (mm 2 ) and F A is the cross-sectional area (mm 2 [8A] The cross-sectional area of the rectangular conductor is 2.6 mm 2 More than 3.0 mm 2 Above, 2.6 to 15 mm 2 , or 3.0 to 15 mm 2 [9A] The method for producing a rectangular wire according to [6A] or [7A], wherein the fluorine-containing resin (B1) is —CH 2 It has an OH group, and the —CH 2 The content of OH groups is 1×10 6 [10A] The method for producing a rectangular wire according to any one of [6A] to [9A], wherein the fluorine-containing elastomer (B2) has iodine atoms, and the content of the iodine atoms is 0.05% by mass or more, 0.1 to 5% by mass, or 0.2 to 1% by mass, relative to the total mass of the fluorine-containing elastomer (B2). [11A] The method for manufacturing a rectangular wire according to any one of [6A] to [10A], wherein the partial discharge inception voltage of the insulating coating material is 600 Vrms or more, 700 Vrms or more, 800 Vrms or more, 900 Vrms or more, 600 to 5000 Vrms, 700 to 4000 Vrms, 800 to 3000 Vrms, or 900 to 3000 Vrms.
[0009] According to the present invention, it is possible to provide a rectangular wire that is highly productive and has excellent surface smoothness of the insulating coating film and excellent conformability of the insulating coating film to the rectangular conductor during bending deformation, as well as a manufacturing method thereof.
[0010] The melt flow rate is the melt mass flow rate defined in JIS K 7210-1:2014 (corresponding international standard ISO 1133-1:2011). Hereinafter, the melt flow rate will also be referred to as MFR. The melt viscosity can be determined by the method described in the Examples. The average thickness of the coating of the insulating coating material is determined by taking a 5 m rectangular wire, measuring the thickness of the coating of the insulating coating material on the long side of a rectangular cross section perpendicular to the axial direction every 100 mm, and taking the arithmetic average. The unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the rectangular wire is determined by taking a 5 m rectangular wire, measuring the thickness of the coating of the insulating coating material on the long side of a rectangular cross section perpendicular to the axial direction every 100 mm, and using the measured values. -CH in the fluorine-containing resin (B1) 2 The OH group content can be determined by infrared spectroscopy. Specifically, it can be determined by the method described in the Examples. The iodine atom content in the fluorine-containing elastomer (B2) can be determined by ion chromatography. The melting point can be determined as the temperature corresponding to the maximum value of the melting peak measured by differential scanning calorimetry (DSC). The partial discharge inception voltage of the insulating coating material can be determined by the method described in the Examples. The volume of the polyaryl ether ketone (A) or the fluorine-containing copolymer (B) can be determined by multiplying the mass (g) of the polyaryl ether ketone (A) or the fluorine-containing copolymer (B) by its specific gravity (g / cm 3 ) The specific gravity of the polyaryl ether ketone (A) or the fluorine-containing copolymer (B) is a value measured at 23°C by the underwater displacement (suspension) method. The "number average particle size" of the fluorine-containing copolymer (B) is the average value of the maximum diameters of 100 particles randomly selected in optical microscope observation. The storage modulus G' of the fluorine-containing elastomer (B2) is a value measured in accordance with ASTM D6204 under conditions of 100°C and 50 cpm. The Mooney viscosity (ML 1+10, 121°C) is a value measured at 121°C in accordance with JIS K6300-1:2000 (corresponding international standards ISO 289-1:2005, ISO 289-2:1994). The weld strength, thermal expansion coefficient and Izod impact strength of the composition containing the polyaryl ether ketone (A) and the fluorinated copolymer (B) can be determined by the methods described in the examples.
[0011] The term "polymer unit" refers to a portion (polymerized unit) derived from a monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a portion of the unit is converted into a different structure by processing the polymer. In this specification, a unit based on a monomer is also referred to as a "monomer unit."
[0012] <<Rectangular Wire>> This wire comprises a rectangular conductor with a rectangular cross section perpendicular to the axial direction, and an insulating coating formed by extrusion molding that directly covers the entire circumferential surface of the conductor. In a winding test conforming to JIS 3216-3:2011, 5.1.2, "Rectangular Wire," the insulating coating does not peel off from the conductor. If the insulating coating does not peel off from the conductor during the winding test, this indicates improved surface smoothness and conformability to the conductor during bending deformation.
[0013] <Flat conductor> A flat conductor is the core of a flat wire and has a rectangular cross section perpendicular to the axial direction. The material of the flat conductor may be any known material for the core of an electric wire, such as copper, tin, silver, gold, aluminum, or alloys thereof. Among these, copper is preferred because it is easy to form. The thickness of the flat conductor is, for example, 0.5 mm to 3.0 mm. The width of the flat conductor is, for example, 1.0 mm to 5.0 mm. The thickness of the flat conductor is the short side of the rectangular cross section perpendicular to the axial direction. The width of the flat conductor is the long side of the rectangular cross section perpendicular to the axial direction.
[0014] The cross-sectional area of the rectangular conductor is 2.6 mm 2 More than 3.0 mm is preferable. 2The upper limit of the cross-sectional area of the rectangular conductor is not particularly limited, but is, for example, 15 mm 2 The cross-sectional area of the rectangular conductor is 2.6 to 15 mm 2 is preferable, and 3.0 to 15 mm 2 is more preferable. The cross-sectional area of the rectangular conductor is the area of the cross section perpendicular to the axial direction. If the insulating coating film has poor conformability to the rectangular conductor during bending deformation, the larger the cross-sectional area of the rectangular conductor, the more likely it is that wrinkles will occur in the insulating coating film or that the insulating coating film will peel off from the rectangular conductor during bending deformation of the rectangular wire. The rectangular wire of this embodiment has excellent conformability of the insulating coating film to the rectangular conductor during bending deformation, so the larger the cross-sectional area of the rectangular conductor, the more useful it is.
[0015] <Coating of insulating coating material> The average thickness of the coating of the insulating coating material is 10 to 1000 μm, preferably 20 to 500 μm, and more preferably 50 to 200 μm. When the average thickness of the coating is equal to or greater than the lower limit, the tracking resistance is excellent. When the average thickness of the coating is equal to or less than the upper limit, the overall thickness of the rectangular wire can be reduced, which enables the coil to take up less space when coiled, contributing to the miniaturization of electrical equipment.
[0016] The unbiased standard deviation of the thickness of the insulating coating material in the axial direction of the rectangular wire (hereinafter simply referred to as "thickness variation") is less than 0.06 mm, preferably 0.03 mm or less, and more preferably 0.01 mm or less. When the thickness variation of the coating is less than (or equal to) the upper limit, excellent crack resistance and tracking resistance during bending deformation are achieved. The smaller the thickness variation of the coating, the better, and it may even be zero. From the perspective of ease of manufacture and yield, the thickness variation of the coating is preferably 0.001 mm or more. The lower limit and the upper limit can be appropriately combined. Examples of combinations where the thickness variation of the coating is not zero include 0.001 mm or more but less than 0.06 mm, 0.001 to 0.03 mm, and 0.001 to 0.01 mm. To achieve a thickness variation of less than 0.06 mm, it is preferable to form the insulating coating material by extrusion molding so that it directly covers the entire circumferential direction of the rectangular conductor. Other methods, such as powder coating, for forming an insulating coating film are undesirable because thickness variations tend to be large. In particular, when a fluorine-containing resin is used to form an insulating coating film by powder coating, the viscosity is difficult to adjust during melting, which tends to cause large variations, compared to non-fluorine-containing resins such as acrylic resins, epoxy resins, epoxy-acrylic resins, polyurethane resins, polyester resins, polyimide resins, polyamideimide resins, and polyesterimide resins.
[0017] The MFR of the insulating coating material at a temperature of 372°C and a load of 49 N is 20.0 to 300.0 g / 10 min, preferably 30.0 to 250.0 g / 10 min, more preferably 40.0 to 200.0 g / 10 min, and even more preferably 50.0 to 230.0 g / 10 min. The MFR of the insulating coating material is preferably measured after preheating at the measurement temperature (372°C) for 5 minutes. Note that if the MFR is 100.0 g / 10 min or higher, it is preferable to shorten the preheating time. In this case, the preheating time is preferably 30 to 180 seconds.
[0018] When the MFR of the insulating coating material at a temperature of 372°C and a load of 49 N is equal to or greater than the lower limit, the surface smoothness of the coating of the insulating coating material and the ability of the coating of the insulating coating material to conform to the rectangular conductor during bending deformation are improved.When the MFR of the insulating coating material at a temperature of 372°C and a load of 49 N is equal to or less than the upper limit, the strength of the coating of the insulating coating material is improved.
[0019] The partial discharge inception voltage of the insulating coating material is preferably 600 Vrms or more, more preferably 700 Vrms or more, even more preferably 800 Vrms or more, and particularly preferably 900 Vrms or more. The upper limit of the partial discharge inception voltage of the insulating coating material is not particularly limited, but may be, for example, 5000 Vrms or less, 4000 Vrms or less, or 3000 Vrms or less. The partial discharge inception voltage of the insulating coating material is preferably 600 to 5000 Vrms, more preferably 700 to 4000 Vrms, even more preferably 800 to 3000 Vrms, and particularly preferably 900 to 3000 Vrms.
[0020] If there are minute void-like defects in the insulating coating material, an electric field concentrates at that location, causing a weak discharge. This discharge is called partial discharge. If the partial discharge inception voltage is equal to or greater than the lower limit, it means that there are few such defects. If the partial discharge inception voltage of the insulating coating material is equal to or greater than the lower limit, the adhesiveness of the insulating coating material to the rectangular conductor is improved. As a result, the ability of the insulating coating film to conform to the rectangular conductor during bending deformation is improved.
[0021] The insulating coating material contains a polyaryl ether ketone (A) and a fluorinated copolymer (B) having units based on tetrafluoroethylene. The insulating coating material may further contain components other than the polyaryl ether ketone (A) and the fluorinated copolymer (B) as long as the properties of the insulating coating material are not significantly impaired.
[0022] The total content of the polyaryl ether ketone (A) and the fluorine-containing copolymer (B) relative to the total mass of the insulating coating material is preferably 50 mass% or more, more preferably 70 mass% or more, and may be 100 mass%.
[0023] The content of the fluorinated copolymer (B) relative to the total mass of the polyaryletherketone (A) and the fluorinated copolymer (B) in the insulating coating material is 5% by mass or more, preferably 5 to 45% by mass, and preferably 10 to 30% by mass. That is, the content of the polyaryletherketone (A) relative to the total mass of the polyaryletherketone (A) and the fluorinated copolymer (B) in the insulating coating material is 95% by mass or less, preferably 55 to 95% by mass or more, and preferably 70 to 90% by mass.
[0024] <Polyaryletherketone (A)> As the polyaryletherketone (A), from the viewpoints of mechanical properties and heat resistance, polyetherketone (hereinafter also referred to as "PEK"), polyetheretherketone (hereinafter also referred to as "PEEK"), or polyetherketoneketone (hereinafter also referred to as "PEKK") is preferred, with PEEK being particularly preferred. Two or more types of polyaryletherketone (A) may be used in combination, but it is preferable to use one type alone.
[0025] As the PEEK, a PEEK having a repeating unit represented by the following formula (I) is preferred.
[0026] (I) In the formula (I), x1 and y1 are independently 0 or 1, and z1 is 0, 1, or 2.
[0027] The melting point of the polyaryl ether ketone (A) is preferably 200 to 430°C, more preferably 250 to 400°C, and even more preferably 280 to 380°C. When the melting point of the polyaryl ether ketone is equal to or higher than the lower limit of the above range, the heat resistance of the insulating coating material is further improved. When the melting point of the polyaryl ether ketone is equal to or lower than the upper limit of the above range, deterioration of the physical properties due to thermal decomposition of the fluorine-containing copolymer (B) during the production of the rectangular wire can be suppressed, and the characteristics of the fluorine-containing copolymer (B) (flexibility, impact resistance, chemical resistance, etc.) can be maintained.
[0028] The melt viscosity of polyaryletherketone (A) is 390°C at a shear rate of 122 sec. -1Under the measurement conditions, the viscosity is preferably 10 to 690 Pa s, more preferably 50 to 500 Pa s, and even more preferably 100 to 400 Pa s. The MFR of the polyaryl ether ketone (A) at a temperature of 372°C and a load of 49 N is preferably 20.0 to 150.0 g / 10 min, and more preferably 21.0 to 200.0 g / 10 min. When the melt viscosity and MFR of the polyaryl ether ketone (A) are within the above ranges, it is easy to adjust the MFR of the insulating coating material to the above range.
[0029] The polyaryletherketone (A) may be commercially available or may be synthesized from various raw materials by various methods. Commercially available PEEK products include, for example, Victrex PEEK (manufactured by Victrex), VESTAKEEP series (manufactured by Daicel-Evonik), and Ketaspire (manufactured by Solvay Specialty Polymers). Commercially available PEKK products include, for example, Kepstan (manufactured by Arkema).
[0030] <Fluorocopolymer (B)> The fluorine-containing copolymer (B) has units based on tetrafluoroethylene (hereinafter also referred to as "TFE") and contains one or more members selected from the group consisting of fluorine-containing resins (B1) and fluorine-containing elastomers (B2), each having a melting point of 260°C or higher.
[0031] (Fluorine-containing resin (B1)) The melting point of the fluorine-containing resin (B1) is 260°C or higher, preferably 280°C or higher, and more preferably 290°C or higher. When the melting point is equal to or higher than the lower limit, the strength of the resulting insulating coating material is excellent. The melting point of the fluorine-containing resin (B1) is preferably 350°C or lower, preferably 340°C or lower, and more preferably 330°C or lower. When the melting point is equal to or lower than the upper limit, the elongation of the resulting insulating coating material is excellent. The lower limit and the upper limit can be combined as appropriate. Examples of combinations include 260 to 350°C, 280 to 340°C, and 290 to 330°C.
[0032] The melt viscosity of the fluorine-containing resin (B1) is 390°C at a shear rate of 122 sec. -1Under the measurement conditions above, the viscosity is preferably 100 to 1400 Pa s, more preferably 300 to 1300 Pa s, and even more preferably 500 to 1200 Pa s. The MFR of the fluororesin (B1) at a temperature of 372°C and a load of 49 N is preferably 10.0 to 300.0 g / 10 min, more preferably 12.0 to 200.0 g / 10 min, even more preferably 15.0 to 150.0 g / 10 min, and particularly preferably 18 to 80 g / 10 min. When the melt viscosity and MFR of the fluororesin (B1) are within the above ranges, it becomes easier to adjust the MFR of the insulating coating material to the above range.
[0033] The fluorine-containing resin (B1) has TFE units and units other than TFE units.
[0034] Examples of other units include a unit u1 based on a fluorine-containing monomer other than a TFE unit, a unit u2 based on a monomer having a functional group (excluding fluorine-containing monomers), and a unit u3 based on a monomer not having fluorine (excluding fluorine-containing monomers).
[0035] The fluorine-containing monomer of unit u1 is preferably a fluorine-containing compound having one polymerizable carbon-carbon double bond. Examples thereof include fluoroolefins (e.g., vinyl fluoride, vinylidene fluoride, trifluoroethylene, hexafluoropropylene (hereinafter also referred to as "HFP"), chlorotrifluoroethylene, hexafluoroisobutylene, etc., excluding TFE), perfluoro(alkyl vinyl ether) (hereinafter also referred to as "PAVE"), CF 2 =CFOR f2 SO 2 X 1 (However, R f2 is a perfluoroalkylene group having 1 to 10 carbon atoms which may contain an oxygen atom between the carbon atoms, and X 1 is a halogen atom or a hydroxyl group.), CF 2 =CFOR f3 CO 2 X 2 (However, R f3 is a perfluoroalkylene group having 1 to 10 carbon atoms which may contain an oxygen atom between the carbon atoms, and X 2is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, CF 2 =CF(CF 2 ) p OCF = CF 2 (wherein p is 1 or 2), fluoroalkylethylene (hereinafter also referred to as "FAE"), fluorine-containing monomers having a ring structure (for example, perfluoro(2,2-dimethyl-1,3-dioxole), 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, perfluoro(2-methylene-4-methyl-1,3-dioxolane)), etc. One type of fluorine-containing monomer may be used alone, or two or more types may be used in combination.
[0036] The fluorine-containing monomer in the unit u1 is preferably at least one selected from the group consisting of HFP, PAVE and FAE, in view of excellent moldability of the composition containing the fluorine-containing resin (B1), and more preferably HFP or PAVE, and particularly preferably PAVE, in view of excellent electrical properties (dielectric constant, dielectric dissipation factor) and heat resistance.
[0037] Examples of PAVE include CF 2 =CFOR f1 (However, R f1 is a perfluoroalkyl group having 1 to 10 carbon atoms which may contain an oxygen atom between the carbon atoms. Specific examples of PAVE include CF 2 = CFOCF 2 CF 3 , C.F. 2 = CFOCF 2 CF 2 CF 3 (hereinafter also referred to as "PPVE"), CF 2 = CFOCF 2 CF 2 CF 2 CF 3 , C.F. 2 = CFO (CF 2 ) 6 F. As the PAVE, PPVE is preferred.
[0038] As the FAE, for example, CH 2 =CX 3 (CF 2 )q X 4 (However, X 3 is a hydrogen atom or a fluorine atom, q is an integer of 2 to 10, and X 4 is a hydrogen atom or a fluorine atom. Specific examples of FAE include CH 2 =CF(CF 2 ) 2 F, CH 2 =CF(CF 2 ) 3 F, CH 2 =CF(CF 2 ) 4 F, CH 2 =CF(CF 2 ) 5 F, CH 2 =CF(CF 2 ) 6 F, CH 2 =CF(CF 2 ) 2 H, CH 2 =CF(CF 2 ) 3 H, CH 2 =CF(CF 2 ) 4 H, CH 2 =CF(CF 2 ) 5 H, CH 2 =CF(CF 2 ) 6 H, CH 2 =CH(CF 2 ) 2 F, CH 2 =CH(CF 2 ) 3 F, CH 2 =CH(CF 2 ) 4 F, CH 2 =CH(CF 2 ) 5 F, CH 2 =CH(CF 2 ) 6 F, CH 2 =CH(CF 2 ) 2 H, CH 2 =CH(CF 2 ) 3 H, CH 2 =CH(CF2 ) 4 H, CH 2 =CH(CF 2 ) 5 H, CH 2 =CH(CF 2 ) 6 H. FAE includes CH 2 =CH(CF 2 ) q1 X 4 (wherein q1 is 2 to 6, preferably 2 to 4), and CH 2 =CH(CF 2 ) 2 F, CH 2 =CH(CF 2 ) 3 F, CH 2 =CH(CF 2 ) 4 F, CH 2 =CF(CF 2 ) 3 H, CH 2 =CF(CF 2 ) 4 H is more preferred, CH 2 =CH(CF 2 ) 4 F, CH 2 =CH(CF 2 ) 2 F is particularly preferred.
[0039] Examples of the monomer having the functional group of the unit u2 include a monomer having a carboxy group (for example, maleic acid, itaconic acid, citraconic acid, undecylenic acid, etc.); a monomer having an acid anhydride group (for example, itaconic anhydride (hereinafter also referred to as "IAH"), citraconic anhydride (hereinafter also referred to as "CAH"), 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH"), maleic anhydride, etc.), a monomer having a hydroxyl group and an epoxy group (for example, hydroxybutyl vinyl ether, glycidyl vinyl ether, etc.). One type of monomer having a functional group may be used alone, or two or more types may be used in combination. The acid anhydride group means a group represented by -C(=O)-O-C(=O)-.
[0040] The monomer having a functional group of unit u2 is preferably a monomer having an acid anhydride group, more preferably one or more selected from the group consisting of IAH, CAH and NAH, more preferably IAH or NAH, and even more preferably NAH. By using one or more selected from the group consisting of IAH, CAH and NAH, a fluororesin (B1) having an acid anhydride group can be easily produced without using a special polymerization method (see JP-A-11-193312), which is required when maleic anhydride is used.
[0041] The fluorine-free monomer of unit u3 is preferably a fluorine-free compound having one polymerizable carbon-carbon double bond, and examples thereof include olefins (e.g., ethylene, propylene, 1-butene, etc.) and vinyl esters (e.g., vinyl acetate, etc.). One type of fluorine-free monomer may be used alone, or two or more types may be used in combination.
[0042] As the fluorine-containing resin (B1), for example, a fluorine-containing resin having TFE units and PAVE units (hereinafter also referred to as "PFA"), a fluorine-containing resin having TFE units and HFP units (hereinafter also referred to as "FEP"), or a fluorine-containing resin having TFE units and ethylene units is preferred, and from the viewpoints of electrical properties (dielectric constant, dielectric dissipation factor) and heat resistance, PFA and FEP are preferred, and PFA is particularly preferred.
[0043] The fluorine-containing resin (B1) preferably has at least one functional group selected from the group consisting of a carbonyl group-containing group, a hydroxy group, an epoxy group, and an isocyanate group. The functional group in the fluorine-containing resin (B1) facilitates dispersion in the polyaryl ether ketone (A). Furthermore, the functional group bonds with atoms on the surface of the rectangular conductor, enhancing adhesion of the insulating coating material to the rectangular conductor. As a result, the ability of the insulating coating material to conform to the rectangular conductor during bending deformation is enhanced. The functional group is preferably present in either one or both of the terminal groups and pendant groups of the main chain of the fluorine-containing resin (B1). The term "main chain" refers to the main carbon chain of a chain compound, and refers to the trunk portion with the largest number of carbon atoms.
[0044] From the viewpoint of dispersibility in the polyaryl ether ketone (A), a carbonyl group-containing group is preferred as the functional group. The carbonyl group-containing group is a group having a carbonyl group -C(=O)- in its structure. Examples of the carbonyl group-containing group include a group having a carbonyl group between carbon atoms of a hydrocarbon group, a carbonate group, a carboxy group, a haloformyl group, an alkoxycarbonyl group, and an acid anhydride group. Examples of the hydrocarbon group in the group having a carbonyl group between carbon atoms of a hydrocarbon group include an alkylene group having 2 to 8 carbon atoms. The number of carbon atoms in the alkylene group does not include the carbon atoms constituting the carbonyl group. The alkylene group may be linear or branched. The haloformyl group is represented by -C(=O)-X (where X is a halogen atom). Examples of the halogen atom in the haloformyl group include a fluorine atom and a chlorine atom, with a fluorine atom being preferred. That is, a fluoroformyl group (also known as a carbonyl fluoride group) is preferred as the haloformyl group. The alkoxy group in the alkoxycarbonyl group is preferably an alkoxy group having 1 to 8 carbon atoms, and particularly preferably a methoxy group or an ethoxy group. The alkoxy group may be linear or branched.
[0045] Examples of the fluororesin (B1) having a functional group include the following, depending on the production method. Fluororesin (B1-1): A fluororesin having a functional group derived from at least one selected from the group consisting of a monomer, a chain transfer agent, and a polymerization initiator used in the production of the fluororesin. Fluororesin (B1-2): A fluororesin obtained by introducing a functional group into a fluororesin having no functional group by surface treatment such as corona discharge treatment or plasma treatment. Fluororesin (B1-3): A fluororesin obtained by graft polymerizing a monomer having a functional group onto a fluororesin having no functional group. Of these, the fluororesin (B1-1) is preferred as the functional group-containing fluororesin.
[0046] When the functional group in the fluorine-containing resin (B1-1) is derived from a monomer used in the production of the fluorine-containing resin (B1-1), a monomer having the functional group of the above-mentioned unit u2 may be used as the monomer.
[0047] When the functional group in the fluorine-containing resin (B1-1) is derived from the chain transfer agent used in the production of the fluorine-containing resin (B1-1), the chain transfer agent may be a chain transfer agent having a functional group such as acetic acid, acetic anhydride, methyl acetate, ethylene glycol, propylene glycol, etc. In this case, the functional group is present as a terminal group of the main chain of the fluorine-containing resin (B1-1).
[0048] When the functional group in the fluorine-containing resin (B1-1) is derived from the polymerization initiator used in the production of the fluorine-containing resin (B1-1), the polymerization initiator may be a polymerization initiator having a functional group, such as di-n-propyl peroxydicarbonate, diisopropyl peroxycarbonate, tert-butyl peroxyisopropyl carbonate, bis(4-tert-butylcyclohexyl)peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, etc. In this case, the functional group is present as a terminal group of the main chain of the fluorine-containing resin (B1-1).
[0049] The functional group in the fluorine-containing resin (B1-1) may be derived from two or more of the monomer, chain transfer agent and polymerization initiator used in the production of the fluorine-containing resin (B1-1).
[0050] As the fluorine-containing resin (B1-1), from the viewpoint of easily controlling the content of functional groups, those having functional groups derived from the monomers used in the production of the fluorine-containing resin (B1-1) are preferred. As the fluorine-containing resin (B1-1) having functional groups derived from monomers, from the viewpoint of thermal stability, a fluorine-containing polymer having units u2 based on TFE and a cyclic hydrocarbon monomer having an acid anhydride group (hereinafter also referred to as "acid anhydride group-containing cyclic hydrocarbon monomer"), and units u1 based on a fluorine-containing monomer other than the TFE unit is preferred. The acid anhydride group of the unit u2 corresponds to the functional group.
[0051] The content of functional groups in the fluorine-containing resin (B1) is 1×10 6The functional group content is preferably 10 to 60,000, more preferably 100 to 50,000, even more preferably 100 to 10,000, and particularly preferably 300 to 5,000, per unit area. When the functional group content is equal to or greater than the lower limit, excellent dispersibility is achieved, and when it is equal to or less than the upper limit, excellent thermal stability is achieved. The functional group content can be measured by methods such as nuclear magnetic resonance (NMR) analysis and infrared absorption spectroscopy. For example, as described in JP 2007-314720 A, the proportion (mol %) of units having functional groups in all units constituting the fluorine-containing resin (B1) can be determined using methods such as infrared absorption spectroscopy, and the functional group content can be calculated from this proportion.
[0052] The fluorine-containing resin (B1) has a —CH 2 It is preferable that the alkyl group has an OH group. 2 The content of OH groups is 1×10 6 Preferably, the number is more than 30, more preferably 60 or more, and even more preferably 150 or more. 2 The upper limit of the OH group content is not particularly limited, but may be, for example, 5,000 or less, 3,000 or less, or 1,000 or less. 2 The content of OH groups is 1×10 6 The number of particles is preferably more than 30 and not more than 5,000, more preferably 60 to 3,000, and even more preferably 150 to 1,000.
[0053] -CH of fluorine-containing resin (B1) 2 When the content of OH groups is equal to or greater than the lower limit, —CH 2 The OH groups bond with atoms on the surface of the rectangular conductor, improving the adhesion of the insulating coating to the rectangular conductor, and as a result, the insulating coating film can better conform to the rectangular conductor during bending deformation.
[0054] In addition, -CH 2 By fluorinating the fluorine-containing resin (B1) having an OH group, —CH 2 The amount of OH groups can be reduced. In addition, by controlling the types and amounts of chain transfer agents, polymerization initiators, and monomers, as well as reaction conditions, the amount of -CH 2The amount of OH groups can be controlled.
[0055] The preferred contents and ratios of each unit in the fluororesin (B1) are as follows: The content of TFE units relative to the total amount of structural units in the fluororesin (B1) is preferably from 90.0 to 99.9 mol%, more preferably from 95.0 to 99.5 mol%, and even more preferably from 96.0 to 99.0 mol%.
[0056] When the fluorine-containing resin (B1) contains units u1, the content of units u1 relative to the total amount of structural units of the fluorine-containing resin (B1) is preferably 0.1 to 10.0 mol%, more preferably 0.5 to 5.0 mol%. When the fluorine-containing resin (B1) contains units u2, the content of units u2 relative to the total amount of structural units of the fluorine-containing resin (B1) is preferably 0.01 to 1.0 mol%, more preferably 0.05 to 0.5 mol%. When the fluorine-containing resin (B1) contains units u3, the content of units u3 relative to the total amount of structural units of the fluorine-containing resin (B1) is preferably more than 0 mol% and 1.0 mol% or less. In one embodiment, it is preferred that the fluorine-containing resin (B1) does not contain units u3. When the fluorine-containing resin (B1) contains any one of the units u1 to u3, the total content of the units u1 to u3 relative to the total amount of the structural units of the fluorine-containing resin (B1) is preferably 0.01 to 10.0 mol%, more preferably 0.05 to 5.0 mol%. When the fluorine-containing resin (B1) contains any one of the units u1 to u3, the total content of the TFE units and the units u1 to u3 relative to the total amount of the structural units of the fluorine-containing resin (B1) is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 100 mol%.
[0057] When the content of each unit is within the above range, the surface smoothness of the coating of the insulating coating material in the obtained rectangular wire and the ability of the coating of the insulating coating material to conform to the rectangular conductor during bending deformation are improved.
[0058] The proportion of each unit can be calculated by melt NMR analysis, fluorine content analysis, infrared absorption spectrum analysis, etc. of the fluorine-containing resin (B1).
[0059] The fluororesin (B1) may contain units based on dicarboxylic acids (itaconic acid, citraconic acid, 5-norbornene-2,3-dicarboxylic acid, maleic acid, etc.) corresponding to the acid anhydride group-containing cyclic hydrocarbon monomer as a result of hydrolysis of part of the acid anhydride groups in the units u2. When such units based on dicarboxylic acids are contained, these units are referred to as units u2.
[0060] Preferable specific examples of the fluorine-containing resin (B1) include copolymers of TFE and PAVE, such as TFE / PPVE copolymer and TFE / PAVE / NAH copolymer. Copolymers of TFE and HFP, such as TFE / HFP copolymer and TFE / HFP / PAVE copolymer. Copolymers of TFE and E, such as TFE / E / HFP copolymer and TFE / E / CH. 2 =CH(CF 2 ) 2 F copolymer, TFE / E / CH 2 =CH(CF 2 ) 4 F copolymer, TFE / E / CH 2 =CH(CF 2 ) 2 F / CH 2 =CH(CF 2 ) 4 F copolymer, TFE / E / HFP / IAH copolymer, TFE / E / CH 2 =CH(CF 2 ) 2 F / IAH copolymer, TFE / E / CH 2 =CH(CF 2 ) 4 F / IAH copolymer, TFE / E / CH 2 =CH(CF 2 ) 2 F / CH 2 =CH(CF 2 ) 4 F / IAH copolymer and the like.
[0061] The fluorine-containing resin (B1) may be one produced by a known production method or a commercially available one. Examples of known production methods include the methods described in WO 2015 / 182702, WO 2016 / 006644, and WO 2016 / 017801.
[0062] (Fluorine-containing elastomer (B2)) The fluorine-containing elastomer (B2) is a fluorine-containing elastic copolymer having no melting point and exhibiting a storage modulus G' at 100°C and 50 cpm of 80 or more, and is distinguished from the fluorine-containing resin (B1).
[0063] The melt viscosity of the fluorine-containing elastomer (B2) was 300°C at a shear rate of 122 sec. -1 Under the measurement conditions, the viscosity is preferably 10 to 2500 Pa s, more preferably 100 to 2300 Pa s, and even more preferably 200 to 2000 Pa s. The MFR of the fluorine-containing elastomer (B2) at a temperature of 230°C and a load of 21 N is preferably 0.1 to 300.0 g / 10 min, more preferably 1.0 to 200.0 g / 10 min, and even more preferably 40.0 to 150.0 g / 10 min. When the melt viscosity and MFR of the fluorine-containing elastomer (B2) are within the above ranges, it becomes easier to adjust the MFR of the insulating coating material to the above range.
[0064] The storage modulus G' of the fluorine-containing elastomer (B2) is preferably from 80 to 800 kPa, more preferably from 100 to 800 kPa, and even more preferably from 120 to 600 kPa. A larger storage modulus G' indicates a larger molecular weight of the fluorine-containing elastomer (B2) and a higher density of entanglement of molecular chains. When the storage modulus G' of the fluorine-containing elastomer (B2) is within the above range, the insulating coating material will have even better mechanical properties such as tensile strength.
[0065] The number-average molecular weight of the fluorine-containing elastomer (B2) is preferably 10,000 to 1,500,000, more preferably 20,000 to 1,000,000, even more preferably 20,000 to 800,000, and particularly preferably 50,000 to 600,000. When the number-average molecular weight of the fluorine-containing elastomer (B2) is at least the lower limit of the above range, the insulating coating material has excellent impact resistance and mechanical properties. When the number-average molecular weight of the fluorine-containing elastomer (B2) is at most the upper limit of the above range, the insulating coating material has excellent fluidity and dispersibility in the polyaryl ether ketone (A). As a result, the flexibility is improved. The number-average molecular weight is the polystyrene-equivalent molecular weight measured using GPC with tetrahydrofuran as an eluent and a calibration curve prepared using polystyrene polymers of known molecular weights.
[0066] Mooney viscosity (ML) of fluorine-containing elastomer (B2) 1+10 , 121°C) is preferably 10 to 300, more preferably 20 to 280, and even more preferably 30 to 250. Mooney viscosity is a measure of molecular weight. A larger Mooney viscosity value indicates a larger molecular weight. A smaller Mooney viscosity value indicates a smaller molecular weight. The Mooney viscosity (ML 1+10 When the Mooney viscosity (ML 1+10 , 121°C) is not more than the upper limit of the above range, the flowability and dispersibility in the polyaryl ether ketone (A) are excellent, and as a result, the composition containing the fluorine-containing elastomer (B2) has excellent molding processability.
[0067] The fluorine-containing elastomer (B2) has TFE units and units other than TFE units.
[0068] Examples of other units include units based on the following monomer m1, units based on the monomer m2, and units based on the monomer m3.
[0069] Monomer m1 is at least one monomer selected from the group consisting of HFP, vinylidene fluoride (hereinafter also referred to as "VdF"), and chlorotrifluoroethylene. Monomer m1 may be used alone or in combination of two or more, and it is preferable to use one monomer alone. Also, monomer m1 may not be used at all.
[0070] Monomer m2 is at least one monomer selected from the group consisting of ethylene (hereinafter also referred to as "E"), propylene (hereinafter also referred to as "P"), PAVE, vinyl fluoride (hereinafter also referred to as "VF"), 1,2-difluoroethylene (hereinafter also referred to as "DiFE"), 1,1,2-trifluoroethylene (hereinafter also referred to as "TrFE"), 3,3,3-trifluoro-1-propylene (hereinafter also referred to as "TFP"), 1,3,3,3-tetrafluoropropylene, and 2,3,3,3-tetrafluoropropylene.
[0071] PAVE includes the above-mentioned PPVE and CF 2 = CFOCF 2 CF 2 CF 2 CF 3 , C.F. 2 = CFO (CF 2 ) 6 In addition to F, CF 2 = CFOCF 3 (hereinafter also referred to as "PMVE"). Among them, PMVE and PPVE are preferred as PAVE, and PMVE is more preferred. One type of PAVE may be used alone, or two or more types may be used in combination.
[0072] Monomer m3 is a monomer having any one of an iodine atom, an epoxy group, and an acid anhydride group at the molecular end and copolymerizable with TFE. By using monomer m3, any one of an iodine atom, an epoxy group, and an acid anhydride group can be introduced into the fluorine-containing elastomer (B2). The proportion of monomer m3 units is preferably 20 mol% or less, more preferably 5 mol% or less, and particularly preferably 0 mol%, based on the total units constituting the fluorine-containing elastomer (B2).
[0073] Examples of the monomer m3 having an iodine atom at the molecular end include iodoethylene, 4-iodo-3,3,4,4-tetrafluoro-1-butene, 2-iodo-1,1,2,2-tetrafluoro-1-vinyloxyethane, 2-iodoethyl vinyl ether, allyl iodide, 1,1,2,3,3,3-hexafluoro-2-iodo-1-(perfluorovinyloxy)propane, 3,3,4,5,5,5-hexafluoro-4-iodopentene, iodotrifluoroethylene, and 2-iodoperfluoro(ethyl vinyl ether). One type of monomer m3 having an iodine atom at the molecular end may be used alone, or two or more types may be used in combination.
[0074] Examples of the monomer m3 having an epoxy group at the molecular terminal include glycidyl esters of (meth)acrylic acid such as glycidyl (meth)acrylate and β-methylglycidyl (meth)acrylate; allyl glycidyl ethers such as allyl glycidyl ether and allylmethylglycidyl ether; and alicyclic epoxy group-containing vinyl monomers such as 3,4-epoxycyclohexyl acrylate and 3,4-epoxycyclohexyl methacrylate. One type of monomer m3 having an epoxy group at the molecular terminal may be used alone, or two or more types may be used in combination.
[0075] Examples of the monomer m3 having an acid anhydride group at the molecular terminal include itaconic anhydride, citraconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, and maleic anhydride. The monomer m3 having an acid anhydride group at the molecular terminal may be used alone or in combination of two or more.
[0076] Examples of the fluorine-containing elastomer (B2) include the following two types of fluorine-containing copolymers: A copolymer having TFE units and P units. A copolymer having TFE units and PAVE units (excluding those having P units or VdF units). The total proportion of the units specifically shown in these two types of fluorine-containing elastomers is preferably 50 mol % or more based on all units constituting the fluorine-containing elastomer.
[0077] Examples of copolymers having TFE units and P units include the following: a copolymer consisting of TFE units and P units, a copolymer consisting of TFE units, P units and VF units, a copolymer consisting of TFE units, P units and VdF units, a copolymer consisting of TFE units, P units and E units, a copolymer consisting of TFE units, P units and TFP units, a copolymer consisting of TFE units, P units and PAVE units, a copolymer consisting of TFE units, P units and 1,3,3,3-tetrafluoropropene units, a copolymer consisting of TFE units, P units and 2,3,3,3-tetrafluoropropene units, a copolymer consisting of TFE units, P units and TrFE units, a copolymer consisting of TFE units, P units and DiFE units, a copolymer consisting of TFE units, P units, VdF units and TFP units, a copolymer consisting of TFE units, P units, VdF units and PAVE units. Among them, as the copolymer having TFE units and P units, a copolymer consisting of TFE units and P units is preferred.
[0078] The copolymer that has TFE unit and PAVE unit can be exemplified by the copolymer that is made up of TFE unit and PAVE unit.Among them, the copolymer that is made up of TFE unit and PMVE unit, the copolymer that is made up of TFE unit, PMVE unit and PPVE unit are preferred, and the copolymer that is made up of TFE unit and PMVE unit is more preferred.
[0079] Other examples of the fluorine-containing elastomer (B2) include copolymers comprising TFE units, VdF units and 2,3,3,3-tetrafluoropropylene units.
[0080] As the fluorine-containing elastomer (B2), the copolymer having TFE unit and P unit, the copolymer having TFE unit and PAVE unit are preferred, the copolymer having TFE unit and P unit are more preferred, and the copolymer consisting of TFE unit and P unit are particularly preferred.The copolymer consisting of TFE unit and P unit has good thermal stability during the production of rectangular wire, so that the transportability during the production of rectangular wire is stable.In addition, the coloring and foaming of insulating coating material are reduced.
[0081] The ratio of each unit constituting the fluorine-containing elastomer (B2) is preferably in the following range, since it contributes more easily to the impact resistance of the insulating coating material. The molar ratio of each unit in a copolymer consisting of TFE units and P units (hereinafter referred to as "TFE:P", and other molar ratios are also described similarly) is preferably 30-80:70-20, more preferably 40-70:60-30, and even more preferably 50-60:50-40. In a copolymer consisting of TFE units, P units, and VF units, the ratio of TFE:P:VF is preferably 30-60:60-20:0.05-40. In a copolymer consisting of TFE units, P units, and VdF units, the ratio of TFE:P:VdF is preferably 30-60:60-20:0.05-40. In copolymers comprising TFE units, P units, and E units, the ratio of TFE:P:E is preferably 20-60:70-30:0.05-40. In copolymers comprising TFE units, P units, and TFP units, the ratio of TFE:P:TFP is preferably 30-60:60-30:0.05-20. In copolymers comprising TFE units, P units, and PAVE units, the ratio of TFE:P:PAVE is preferably 40-70:60-29.95:0.05-20. In copolymers comprising TFE units, P units, and 1,3,3,3-tetrafluoropropene units, the ratio of TFE:P:1,3,3,3-tetrafluoropropene is preferably 30-60:60-20:0.05-40. In copolymers comprising TFE units, P units, and 2,3,3,3-tetrafluoropropene units, the ratio of TFE:P:2,3,3,3-tetrafluoropropene is preferably 30-60:60-20:0.05-40. In copolymers comprising TFE units, P units, and TrFE units, the ratio of TFE:P:TrFE is preferably 30-60:60-20:0.05-40. In copolymers comprising TFE units, P units, and DiFE units, the ratio of TFE:P:DiFE is preferably 30-60:60-20:0.05-40. In copolymers comprising TFE units, P units, VdF units, and TFP units, the ratio of TFE:P:VdF:TFP is preferably 30-60:60-20:0.05-40:0.05-20.In the copolymer comprising TFE units, P units, VdF units and PAVE units, the ratio of TFE:P:VdF:PAVE is preferably 30-70:60-20:0.05-40:0.05-20.
[0082] In a copolymer comprising TFE units, VdF units, and HFP units, the ratio of TFE:VdF:HFP is preferably 20-60:1-40:20-60. In a copolymer comprising TFE units, VdF units, HFP units, and TFP units, the ratio of TFE:VdF:HFP:TFP is preferably 30-60:0.05-40:60-20:0.05-20. In a copolymer comprising TFE units, VdF units, HFP units, and PAVE units, the ratio of TFE:VdF:HFP:PAVE is preferably 30-70:60-20:0.05-40:0.05-20.
[0083] In a copolymer comprising TFE units and PAVE units, the ratio of TFE:PAVE is preferably 40-70:60-30. In a copolymer comprising TFE units and PMVE units, the ratio of TFE:PMVE is preferably 40-70:60-30. In a copolymer comprising TFE units, PMVE units, and PPVE units, the ratio of TFE:PMVE:PPVE is preferably 40-70:3-57:3-57.
[0084] In the copolymer comprising TFE units, VdF units and 2,3,3,3-tetrafluoropropylene units, the ratio of TFE:VdF:2,3,3,3-tetrafluoropropylene is preferably 1-30:30-90:5-60.
[0085] The fluorine-containing elastomer (B2) may be used alone or in combination of two or more kinds, but it is preferable to use one kind alone. The fluorine-containing elastomer (B2) may be a commercially available product or may be synthesized from various raw materials by various methods. The fluorine-containing elastomer (B2) can be synthesized, for example, by polymerizing TFE and one or more of the monomer m1, the monomer m2, and the monomer m3.
[0086] During polymerization, it is preferable to use a radical polymerization initiator. As the radical polymerization initiator, a compound having a half-life of 10 hours at a temperature of 0 to 100°C is preferred, and a compound having a half-life of 20 to 90°C is particularly preferred. Examples of the radical polymerization initiator include azo compounds (azobisisobutyronitrile, etc.), non-fluorine-based diacyl peroxides (isobutyryl peroxide, octanoyl peroxide, benzoyl peroxide, lauroyl peroxide, etc.), peroxydicarbonates (diisopropyl peroxydicarbonate, etc.), peroxyesters (tert-butyl peroxypivalate, tert-butyl peroxyisobutyrate, tert-butyl peroxyacetate, etc.), fluorine-containing diacyl peroxides (compound 1 represented by the following formula F1), and inorganic peroxides (potassium persulfate, sodium persulfate, ammonium persulfate, etc.). (Z(CF 2 ) r COO) 2 Formula F1 In the formula F1, Z is a hydrogen atom, a fluorine atom, or a chlorine atom, and r is an integer of 1 to 10.
[0087] A chain transfer agent may be used during the polymerization. Examples of the chain transfer agent include compound 2 represented by the following formula F2, compound 3 represented by the following formula F3, alcohols (methanol, ethanol, etc.), chlorofluorohydrocarbons (1,3-dichloro-1,1,2,2,3-pentafluoropropane, 1,1-dichloro-1-fluoroethane, etc.), hydrocarbons (pentane, hexane, cyclohexane, etc.), and mercaptans (tert-dodecyl mercaptan, n-octadecyl mercaptan, etc.). R 1 I 2 ...Formula F2 R 2 IBr...Formula F3 In the above formula F2, R 1 is an alkylene group or a polyfluoroalkylene group having two or more carbon atoms. 2 is an alkylene group or polyfluoroalkylene group having 1 to 16 carbon atoms.
[0088] R 1 , R 2In the formula (I), the polyfluoroalkylene group may be linear or branched. 1 , R 2 is preferably a perfluoroalkylene group. Examples of compound 2 include 1,4-diiodoperfluorobutane, 1,2-diiodoperfluoroethane, 1,3-diiodoperfluoropropane, 1,5-diiodoperfluoropentane, and 1,6-diiodoperfluorohexane. Of these, 1,4-diiodoperfluorobutane is preferred. Examples of compound 3 include 1-iodo-4-bromoperfluorobutane, 1-iodo-4-bromoperfluorobutane, 1-iodo-6-bromoperfluorohexane, and 1-iodo-8-bromoperfluorooctane.
[0089] Iodine compounds such as Compound 2 and Compound 3 can function as chain transfer agents. Therefore, when each monomer is copolymerized in the presence of an iodine compound, an iodine atom can be bonded to the main chain terminal of the fluorine-containing elastomer (B2). When a fluorine-containing elastomer (B2) having a branched chain is obtained, an iodine atom can be similarly bonded to the branched chain terminal.
[0090] Examples of polymerization methods include emulsion polymerization, solution polymerization, suspension polymerization, and bulk polymerization. Emulsion polymerization, in which monomers are polymerized in the presence of an aqueous medium and an emulsifier, is preferred because it allows for easy adjustment of the number-average molecular weight and copolymer composition of the fluorine-containing elastomer (B2) and provides excellent productivity. Water-soluble initiators are preferred as radical polymerization initiators for emulsion polymerization. Examples of water-soluble initiators include persulfuric acid, hydrogen peroxide, water-soluble organic peroxides, organic initiators, redox initiators consisting of a combination of persulfuric acid or hydrogen peroxide with a reducing agent, and inorganic initiators in which a small amount of iron, ferrous salt, silver sulfate, or the like is further present in a redox initiator. Examples of persulfuric acid include ammonium persulfate, sodium persulfate, and potassium persulfate. Examples of water-soluble organic peroxides include disuccinic acid peroxide, diglutaric acid peroxide, and tert-butylhydroxyperoxide. Examples of organic initiators include azobisisobutylamidine dihydrochloride. Examples of reducing agents include sodium hydrogen sulfite and sodium thiosulfate. In the emulsion polymerization method, monomers are polymerized in the presence of an aqueous medium, an emulsifier, and a radical polymerization initiator to obtain an elastomer latex. A pH adjuster may be used during the polymerization of the monomers.
[0091] The fluorine-containing elastomer (B2) preferably contains iodine atoms. The content of iodine atoms is preferably 0.05% by mass or more, more preferably 0.1 to 5% by mass, and even more preferably 0.2 to 1% by mass, based on the total mass of the fluorine-containing elastomer (B2).
[0092] When the iodine atom content of the fluorine-containing elastomer (B2) is equal to or greater than the lower limit, the iodine atoms bond with atoms on the surface of the rectangular conductor, improving the adhesion of the insulating coating to the rectangular conductor, thereby improving the conformability of the insulating coating to the rectangular conductor during bending deformation.
[0093] The amount of iodine atoms can be controlled by controlling the type and amount of the chain transfer agent containing iodine atoms and the monomer containing iodine atoms, as well as the reaction conditions.
[0094] <Other Components> Examples of other components include fluorine-containing polymers other than the fluorine-containing copolymer (B), fluorine-free polymers other than the polyaryl ether ketone (A), fillers, pigments, and other additives. Specific examples of fillers include resins and inorganic fillers. Examples of resins include fibrous resins such as aramid fibers and liquid crystal polyester fibers, and powdered resins such as polytetrafluoroethylene. Examples of inorganic fillers include fibrous fillers such as glass fibers, carbon fibers, boron fibers, and stainless steel microfibers; and powdered fillers such as talc, mica, graphite, molybdenum disulfide, calcium carbonate, silica, silica alumina, alumina, and titanium dioxide. Other examples include hydrotalcites and metal oxides, such as zinc oxide, magnesium oxide, titanium oxide, lead oxide, and copper oxide. Metal powders can also be used. Examples include powders of stainless steel, iron-based materials, titanium, copper, and nickel. One type of filler may be used alone, or two or more types may be used in combination. Examples of pigments include color pigments such as organic pigments and inorganic pigments. Specific examples include carbon black (black pigment), iron oxide (red pigment), aluminum cobalt oxide (blue pigment), copper phthalocyanine (blue pigment, green pigment), perylene (red pigment), and bismuth vanadate (yellow pigment). One of the other components may be used alone, or two or more of them may be used in combination.
[0095] <Method for manufacturing a rectangular wire> The rectangular wire described above can be manufactured by using an extruder equipped with a die to melt a composition containing polyaryl ether ketone (A) and a fluorine-containing copolymer (B), and extruding the molten composition from the die around a rectangular conductor to coat the rectangular conductor with the molten composition, thereby forming the insulating coating material. In addition to the fluorine-containing copolymer, the other components described above may be added to the extruder.
[0096] (Composition) The composition contains a polyaryl ether ketone (A) and a fluorinated copolymer (B) having units based on tetrafluoroethylene. The composition may further contain components other than the polyaryl ether ketone (A) and the fluorinated copolymer (B), as long as the properties of the composition are not significantly impaired.
[0097] The total content of the polyaryl ether ketone (A) and the fluorinated copolymer (B) relative to the total mass of the composition is preferably 50 mass% or more, more preferably 70 mass% or more, and may be 100 mass%.
[0098] The content of the fluorinated copolymer (B) relative to the total mass of the polyaryl ether ketone (A) and the fluorinated copolymer (B) in the composition is 5% by mass or more, preferably 5 to 45% by mass, and preferably 10 to 30% by mass. That is, the content of the polyaryl ether ketone (A) relative to the total mass of the polyaryl ether ketone (A) and the fluorinated copolymer (B) in the composition is 95% by mass or less, preferably 55 to 95% by mass, and preferably 70 to 90% by mass.
[0099] The composition preferably has an MFR of 19.0 to 300.0 g / 10 min at a temperature of 372° C. and a load of 49 N, more preferably 25.0 to 250.0 g / 10 min, and even more preferably 50.0 to 200.0 g / 10 min.
[0100] The weld strength of the composition is preferably 50 MPa or more, more preferably 60 MPa or more, and even more preferably 70 MPa or more. When the weld strength is equal to or greater than the lower limit, it becomes easier to obtain a rectangular wire in which the insulating coating film has excellent conformability to the rectangular conductor during bending deformation. The higher the weld strength, the better, and there is no particular upper limit. The upper limit of the weld strength is, for example, 100 MPa. The weld strength of the composition is preferably 50 to 100 MPa, more preferably 60 to 100 MPa, and even more preferably 70 to 100 MPa.
[0101] The thermal expansion coefficient of the composition is preferably 0.48% or less, more preferably 0.45% or less, and even more preferably 0.40% or less. When the thermal expansion coefficient is equal to or less than the upper limit of the above-mentioned range, it becomes easier to obtain a rectangular wire in which the insulating coating film has excellent conformability to the rectangular conductor during bending deformation. The lower the thermal expansion coefficient, the better, and there is no particular limit to the lower limit.
[0102] When the composition is cut into a test piece having a thickness of 4.0 mm, the Izod impact strength at 23°C is preferably 80 J / m or more, more preferably 90 J / m or more, and even more preferably 100 J / m or more. When the Izod impact strength at 23°C is equal to or greater than the lower limit, the insulating coating material has excellent impact resistance at room temperature. The upper limit of the Izod impact strength at 23°C is not particularly limited, and may be, for example, NB (No break).
[0103] The melting (melt-kneading) is preferably carried out so that particles of the fluorocopolymer (B) having a number average particle size of 0.5 to 10 μm are dispersed in the polyaryl ether ketone (A). By appropriately adjusting the melt-kneading temperature, the extrusion shear rate, and the residence time of the material to be melt-kneaded in the melt-kneading apparatus, particles of the fluorocopolymer (B) having a number average particle size of 0.5 to 10 μm can be dispersed in the polyaryl ether ketone (A).
[0104] (Production Conditions) Examples of the extruder include a twin-screw extruder and a single-screw extruder, with a twin-screw extruder being preferred. The opening surface of the die is rectangular. The cylinder temperature and die temperature of the extruder are set depending on the types of polyaryl ether ketone (A) and fluorocopolymer (B). The cylinder temperature of the extruder is preferably 50 to 450°C, more preferably 80 to 440°C, and even more preferably 90 to 430°C. The die temperature is preferably 100 to 420°C, more preferably 120 to 400°C, and even more preferably 150 to 380°C. When the cylinder temperature and die temperature of the extruder are equal to or higher than the lower limit, the compatibility of the materials by kneading is improved. When the cylinder temperature and die temperature of the extruder are equal to or lower than the upper limit, thermal degradation of the fluorocopolymer (B) is easily suppressed. The residence time in the extruder is preferably 10 seconds to 30 minutes. The screw rotation speed of the extruder is preferably 0.5 to 100 rpm.
[0105] It is preferable to preheat the rectangular conductor. The temperature of the preheated rectangular conductor is preferably 50 to 400° C., more preferably 80 to 250° C. The preheating method is not particularly limited, but examples include light heating, hot air heating, radiant heating, gas burner heating, and induction heating.
[0106] (Drawdown Ratio) In the manufacturing method of the rectangular wire of this embodiment, the drawdown ratio (hereinafter also referred to as "DDR") calculated by the following formula 1 is preferably 0.1 or more and less than 10.0, more preferably 0.5 or more and less than 10.0, even more preferably 0.5 to 5, and particularly preferably 0.8 to 1.5. When the DDR is equal to or more than the lower limit, a rectangular wire having excellent surface smoothness of the insulating coating film is easily obtained. When the DDR is less than (or equal to or less than) the upper limit, a rectangular wire having excellent surface smoothness of the insulating coating film and excellent followability of the insulating coating film to the rectangular conductor during bending deformation is easily obtained.
[0107] DDR = (D A -C A ) / (F A -C A ) Formula 1 In the above formula 1, D A is the opening area of the die (mm 2 ) and C Ais the cross-sectional area (mm 2 ) and F A is the cross-sectional area (mm 2 )
[0108] D A can be calculated from the following formula 2. A =D L ×D S Formula 2 In the formula 2, D L is the inner dimension (mm) of the long side of the rectangular opening of the die, and D S is the inner dimension (mm) of the short side of the rectangular opening surface of the die.
[0109] C A can be calculated from the following formula 3. A =C L ×C S Formula 3 In the formula 3, C L is the long side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular conductor, and C S is the short side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular conductor.
[0110] F A can be calculated from the following formula 4. A =F L ×F S Formula 4 In the formula 4, F L is the long side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular wire, and F S is the short side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular wire.
[0111] In this embodiment, it is preferable to employ a so-called pressure molding method in which the insulating coating material is formed under pressure. By employing the pressure molding method, the DDR is more likely to be less than (or equal to) the upper limit value than in the conventional tube molding method, and as a result, it is easier to obtain a rectangular wire with excellent surface smoothness of the insulating coating material film and excellent conformability of the insulating coating material film to the rectangular conductor during bending deformation.
[0112] (Uses) The rectangular wire of the present invention can be suitably used for, for example, insulating amplifiers, insulating transformers, automobile alternators, hybrid vehicles, electric ships, electric aircraft, electric vertical take-off and landing aircraft, etc. It can also be used as various electric wires (wrapped electric wires, electric wires for automobiles, electric wires for robots) and coil windings (magnet wire).
[0113] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following examples, Examples 1 to 10 are working examples, and Examples 11 to 24 are comparative examples.
[0114] <Evaluation Method> (MFR of Insulating Coating Material) After preheating the insulating coating material at 372°C for 5 minutes, the MFR at 49N was measured in accordance with JIS K 7210-1:2014. The measurement was carried out at 372°C. Note that if the MFR exceeds 100 g / 10 min, the preheating time may be set to 30 to 180 seconds.
[0115] (MFR of polyaryl ether ketone (A) and fluororesin (B1)) MFR at 49N was measured in accordance with JIS K 7210-1:2014. The measurement was carried out at 372°C.
[0116] (MFR of Fluorine-Containing Elastomer (B2)) The MFR at 21 N was measured in accordance with JIS K 7210-1:2014. The measurement was carried out at 230°C.
[0117] (Melt Viscosity of Polyaryletherketone (A) and Fluorine-Containing Copolymer (B)) The melt viscosity of polyaryletherketone (A) and fluorine-containing copolymer (B) was measured using a capillograph (manufactured by Toyo Seiki Seisakusho, capillary length L: 10 mm, capillary inner diameter r: 1.0 mm, piston diameter D: 9.55 mm). For polyaryletherketone (A) and fluorine-containing resin (B1), the melt viscosity was measured at a temperature of 390°C and a shear rate of 122 sec. -1 For the fluorine-containing elastomer (B2), the temperature was 300°C and the shear rate was 122 sec -1 Measurements were carried out.
[0118] (Melting Points of Polyaryl Ether Ketone (A) and Fluororesin (B1)) Using a differential scanning calorimeter (manufactured by Seiko Instruments Inc.), the polyaryl ether ketone (A) or the fluororesin (B1) was heated at a rate of 10°C / min, and the melting peak was recorded, and the temperature corresponding to the maximum value was taken as the melting point.
[0119] (Mooney viscosity (ML) of fluorine-containing elastomer (B2) 1+10 , 121°C)) The measurement was carried out at 121°C using an SMV-201 (manufactured by Shimadzu Corporation) in accordance with JIS K 6300-1:2000 (corresponding international standards ISO 289-1:2005, ISO 289-2:1994).
[0120] (Storage Modulus G' of Fluorine-Containing Elastomer (B2)) Measurement was carried out using RPA2000 (manufactured by Alpha Technologies) in accordance with ASTM D6204 under conditions of 100°C and 50 cpm.
[0121] (-CH of fluorine-containing resin (B1) 2 Pellets of the fluorine-containing resin (B1) were molded by cold pressing to prepare a film having a thickness of 0.25 to 0.30 mm. This film was scanned 40 times by a Fourier transform infrared spectrometer (FT-IR (Spectrum One, manufactured by PerkinElmer)) to obtain infrared absorption spectrum 1. 2 The same procedure was performed on pellets of fluorine-containing resin not having OH groups (however, the film thickness was the same), and infrared absorption spectrum 2 was obtained. Infrared absorption spectrum 2 was subtracted from infrared absorption spectrum 1 to obtain a difference spectrum. -1 From the peak (absorbance) of 6 -CH for individuals 2 The OH group content was determined. -1 The peak is -CH 2 C, a model compound with an OH group 7 H 15 CH 2 This is a peak observed in -OH. 2The molar absorption coefficient of the OH group is 104 (absorbance / cm / mol). N=I×A×t Equation 5 In the above Equation 5, I is absorbance, A is a correction coefficient, and -CH 2 2236 for OH groups, and t is the thickness of the film (mm).
[0122] (Iodine Content of Fluorine-Containing Elastomer (B2)) The iodine content of the fluorine-containing elastomer (B2) was measured using an ion chromatograph (manufactured by Dia Instruments Co., Ltd., an apparatus combining an automatic sample combustion apparatus, ion chromatograph pretreatment device AQF-100 model, and an ion chromatograph).
[0123] (Weld Strength of Composition) A pellet-like composition containing polyaryl ether ketone (A) and fluorine-containing copolymer (B) was pre-dried for 3 hours under heating at 200°C. Next, using an injection molding machine (manufactured by Fanuc Corporation, ROBOSHOT α-50) and an injection molding mold for weld strength measurement, the composition was injection molded under conditions of a cylinder temperature of 380°C and a mold temperature of 170°C, to obtain a test piece having a sample size of 1B in accordance with ISO 527. This test piece was measured in accordance with ISO 527 using a Tensilon universal testing machine RTF-1350 (manufactured by A&D Co., Ltd.).
[0124] (Thermal Expansion Coefficient of Composition) Pellets of the composition were molded using a heat press manufactured by Tester Sangyo Co., Ltd. under conditions of a processing temperature of 370°C, a preheating time of 10 minutes, a pressure of 10 MPa, and a pressing time of 3 minutes to obtain a sheet with a thickness of 0.5 mm. A square sample measuring 4 mm x 4 mm x 0.5 mm was cut from the obtained sheet. A TMA curve (horizontal axis: temperature, vertical axis: deformation amount) was measured for the obtained sample using a TMA device (TMA / SS6100 manufactured by Hitachi High-Tech Science Corporation) in accordance with JIS K 7196:1991 (measurement mode: penetration mode) under the conditions of a temperature setting of 30 to 390°C, a heating rate of 5°C / min, and a load of 100 mN. The maximum dimensional change rate at which the deformation amount value changed the most was determined in the temperature range of 50 to 303°C on the obtained TMA curve, and this was taken as the thermal expansion coefficient. The dimensional change rate was specifically calculated using the following formula: Dimensional change rate (%) = (thickness length after test - thickness length before test) / thickness length before test × 100
[0125] (Preparation of Injection-Molded Article for Evaluation) A pellet-like composition of polyaryl ether ketone (A) and fluorocopolymer (B) was pre-dried for 3 hours under heating at 200° C. Next, the composition was injection-molded using an injection molding machine (manufactured by Fanuc Corporation, ROBOSHOT α-50) under conditions of a cylinder temperature of 380° C. and a mold temperature of 170° C., to obtain an injection-molded article for evaluation having a thickness of 4.0 mm.
[0126] (Izod Impact Strength of Composition) A test piece measuring 80 mm in length and 10 mm in width was cut out from the injection-molded article for evaluation, and a notch was made at a height of 40 mm in the test piece. The Izod impact strength of the test piece was measured using an Izod tester (manufactured by Toyo Seiki Seisakusho, Ltd.) under the following conditions: hammer capacity: 2.75 J, hammer load: 13.97 N, distance from the shaft center to the center of gravity: 10.54 cm, and distance from the shaft center to the impact point: 33.5 cm. The measurement was carried out at 23°C.
[0127] (Number Average Particle Diameter of Fluorocopolymer (B) in Composition) The injection-molded article for evaluation was observed with a scanning electron microscope (S-4800, manufactured by Hitachi, Ltd.), and the maximum diameters of 100 randomly selected particles were measured and the arithmetic average was taken to determine the number average particle diameter of the fluorine-containing copolymer (B) in the composition.
[0128] (Partial Discharge Inception Voltage of Insulating Coating Material) A coating of insulating coating material was cut out from the rectangular conductor of a rectangular wire and press-molded (350°C, preheating for 5 minutes, and applying pressure for 2 minutes) to obtain a measurement sample of 130 mm x 130 mm x 0.12 mm thick. Using the obtained measurement sample, the partial discharge inception voltage of the insulating coating material was measured under the following measurement conditions (low frequency method). The voltage when a discharge charge of 10 pC was detected was obtained as the partial discharge inception voltage. Note that the measurement was performed on five measurement samples, and the average of these was taken as the partial discharge inception voltage. In Tables 1 to 3, the partial discharge inception voltage is represented as PDIV. [Measurement Conditions] Measurement device: Partial Discharge Detector A-006, manufactured by Fujikura Dia Cable Co., Ltd. Electrode: An electrode conforming to JIS C 2110-1 was used. Test voltage: Set up to a maximum of 20 kVrms (50 Hz), and reduced after detecting a discharge charge of 100 pC. Voltage rise / fall rate: 100 V / sec. Other conditions: In the atmosphere, temperature: 18°C, relative humidity: 30%.
[0129] (Average thickness and thickness variation of coating) A 5 m length of rectangular wire was taken, and the thickness of the coating of the insulating coating material on the long side of the rectangular cross section perpendicular to the axial direction was measured every 100 mm (only on the side that contacts the upper inner surface of the die during molding). The arithmetic mean of the measured values (mm) was taken as the average thickness. The unbiased standard deviation of the measured values (mm) was taken as the thickness variation.
[0130] (Winding test) The rectangular wires were evaluated by a winding test in accordance with "JIS3216-3:2011 5.1.2 Rectangular wire." The cross section of the rectangular wire was visually inspected and evaluated according to the following criteria: A: No peeling of the insulating coating from the rectangular conductor. B: Peeling of the insulating coating from the rectangular conductor.
[0131] (Conformability) The rectangular wire was bent edgewise and flatwise at a bending angle of 90±10°. The surface of the insulating coating film at the bent and deformed portion and the cross section of the rectangular wire were then visually observed, and conformability was evaluated according to the following criteria: A: No wrinkles were generated on the surface of the insulating coating film during bending, and no peeling of the insulating coating film from the rectangular conductor occurred. B: Wrinkles were generated on the surface of the insulating coating film during bending, or the insulating coating film peeled from the rectangular conductor.
[0132] (Surface Smoothness) The surface roughness (Ra) of the rectangular wire was measured using a digital microscope (HRX-1, manufactured by Hirox Co., Ltd.). The measurement was carried out at a magnification of 80 times and a measurement length of 4 mm. A: Surface roughness is 45 μm or less B: Surface roughness is more than 45 μm
[0133] <Materials Used> (Polyaryletherketone (A)) Polyaryletherketone (A1): PEEK (manufactured by Daicel-Evonik, product name "VESTAKEEP2000G", melting point: 340°C, MFR: 64g / 10min, melt viscosity: 290Pa.s, specific gravity: 1.32). Polyaryletherketone (A2): PEEK (manufactured by Daicel-Evonik, product name "VESTAKEEP1000G", melting point: 340°C, MFR: 140g / 10min, melt viscosity: 178Pa.s, specific gravity: 1.32). Polyaryletherketone (A3): PEEK (manufactured by Daicel-Evonik, product name "VESTAKEEP3300G", melting point: 340°C, MFR: 21 g / 10 min, melt viscosity: 700 Pa / s, specific gravity: 1.32).
[0134] Fluorine-containing copolymer (B) Fluorine-containing resin (B1): a fluororesin having a molar ratio of TFE units:PPVE units:NAH units=97.9:2.0:0.1 (melting point: 300°C, specific gravity: 2.13, MFR: 16 g / 10 min, melt viscosity: 1120 Pa s, number of main chain carbon atoms: 1×10 6 -CH for individuals 2Content of OH groups: 303. Fluorine-containing elastomer (B2-1): A fluorine-containing elastomer having a molar ratio of TFE units:P units of 56:44 and containing 0.4% by mass of iodine atoms relative to the mass of the fluorine-containing elastomer, MFR: difficult to measure (<150 g / 10 min), melt viscosity: <300 Pa s, specific gravity: 1.55, Mooney viscosity (ML 1+10 , 121°C): 50, storage modulus G': 250 kPa. Fluorine-containing elastomer (B2-2): a fluorine-containing elastomer having a molar ratio of TFE units:P units of 56:44 and containing no iodine atoms, MFR: 11 g / 10 min, melt viscosity: 270 Pa·s, specific gravity: 1.55, Mooney viscosity (ML 1+10 , 121°C): 100, storage modulus G': 390 kPa).
[0135] (Example 1) A rectangular wire was produced by extrusion molding the composition having the formulation shown in Table 1 under the following conditions. The DDR was set to 1. The wire extrusion molding employed a so-called pressure molding method, in which the insulating coating is formed under pressure. Die temperature: 390°C. Cylinder temperature: 320-390°C. Rectangular conductor: rectangular copper wire with a thickness of 1.473 mm and a width of 2.278 mm. Rectangular conductor preheat temperature: 180°C. Coating thickness (set value): 0.12 mm.
[0136] (Examples 2 to 24) Rectangular wires were produced in the same manner as in Example 1, except that the compositions shown in Tables 1 to 3 were used. However, in Examples 11 to 24, the DDR was set to 15, and the insulating coating material was formed substantially under normal pressure, a so-called tube molding method.
[0137] The insulating coating material and rectangular wire of each example were evaluated as described above. The results are shown in Tables 1 to 3.
[0138]
[0139]
[0140]
[0141] Examples 1 to 10 had excellent surface smoothness of the insulating coating film and excellent conformability of the insulating coating film to the rectangular conductor during bending deformation. Examples 11 and 12, which did not contain fluorine-containing copolymer (B), were inferior in surface smoothness of the insulating coating film and excellent conformability of the insulating coating film to the rectangular conductor during bending deformation. Examples 13 to 16, in which the insulating coating material had an MFR of less than 20.0 g / 10 min at 372°C and a load of 49 N, were inferior in surface smoothness of the insulating coating film and excellent conformability of the insulating coating film to the rectangular conductor during bending deformation. Examples 17 to 24, which contained fluorine-containing copolymer (B), had an MFR of 20.0 to 300.0 g / 10 min at 372°C and a load of 49 N, and had a DDR of 15, were inferior in surface smoothness of the insulating coating film and excellent conformability of the insulating coating film to the rectangular conductor during bending deformation.
Claims
1. A rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and an insulating coating film formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, wherein the insulating coating has a melt flow rate of 20.0 to 300.0 g / 10 min at a temperature of 372°C and a load of 49 N, the insulating coating film has an average thickness of 10 to 1000 μm, and the unbiased standard deviation of the thickness of the insulating coating film in the axial direction of the rectangular wire is less than 0.06 mm, The insulating coating material comprises a polyaryletherketone (A) and a fluorine-containing copolymer (B) having a unit based on tetrafluoroethylene, the fluorine-containing copolymer (B) comprising one or more selected from the group consisting of a fluorine-containing resin (B1) and a fluorine-containing elastomer (B2) having a melting point of 260°C or higher, the content of the fluorine-containing copolymer (B) relative to the total mass of the polyaryletherketone (A) and the fluorine-containing copolymer (B) in the insulating coating material is 5 mass% or more, and the rectangular wire is a flat wire in which a coating of the insulating coating material does not peel off from the flat conductor in a winding test in accordance with "JIS3216-3:2011, 5.1.2 Flat wire".
2. The cross-sectional area of the rectangular conductor is 2.6 mm 2 The rectangular wire according to claim 1 .
3. The fluorine-containing resin (B1) is —CH 2 It has an OH group, and the -CH 2 The content of OH groups is 1×10 6 The rectangular wire according to claim 1 or 2, wherein the number of the first and second wires is more than 30.
4. The rectangular wire according to claim 1 or 2, wherein the fluorine-containing elastomer (B2) contains iodine atoms, and the content of the iodine atoms is 0.05 mass% or more relative to the total mass of the fluorine-containing elastomer (B2).
5. The rectangular wire according to claim 1 or 2, wherein the partial discharge inception voltage of the insulating coating material is 600 Vrms or more.
6. A method for producing a rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, the method comprising: melting a composition containing polyaryletherketone (A) and a fluorine-containing copolymer (B) having units based on tetrafluoroethylene using an extruder equipped with a die; and extruding the molten composition from the die around the rectangular conductor to coat the rectangular conductor with the molten composition to form the insulating coating material; wherein the insulating coating material has a melt flow rate of 20.0 to 300.0 g / 10 min at a temperature of 372°C and a load of 49 N, an average thickness of the coating of the insulating coating material is 10 to 1000 μm, and an unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the rectangular wire is less than 0.06 mm; The method for producing a rectangular wire, wherein the fluorine-containing copolymer (B) comprises one or more selected from the group consisting of a fluorine-containing resin (B1) and a fluorine-containing elastomer (B2) having a melting point of 260°C or higher, the content of the fluorine-containing copolymer (B) relative to the total mass of the polyaryl ether ketone (A) and the fluorine-containing copolymer (B) in the composition is 5 mass% or higher, and the rectangular wire is such that a coating of the insulating coating material does not peel off from the rectangular conductor in a winding test based on "JIS3216-3:2011, 5.1.2, Rectangular wire".
7. The method for producing a rectangular wire according to claim 6, wherein the drawdown ratio DDR calculated by the following formula 1 is 0.5 or more and less than 10.
0. A -C A ) / (F A -C A In the above formula 1, D A is the opening area of the die (mm 2 ) and C A is the cross-sectional area (mm 2 ) and F A is the cross-sectional area (mm 2 ).
8. The cross-sectional area of the rectangular conductor is 2.6 mm 2 The method for producing a rectangular wire according to claim 6 or 7, wherein 9. The fluorine-containing resin (B1) is —CH 2 It has an OH group, and the -CH 2 The content of OH groups is 1×10 6 The method for producing a rectangular wire according to claim 6 or 7, wherein the number of the wires is more than 30.
10. A method for producing a rectangular wire as described in claim 6 or 7, wherein the fluorine-containing elastomer (B2) contains iodine atoms, and the content of the iodine atoms is 0.05 mass% or more relative to the total mass of the fluorine-containing elastomer (B2).
11. The method for manufacturing a rectangular wire according to claim 6 or 7, wherein the partial discharge inception voltage of the insulating coating material is 600 Vrms or more.
Citation Information
Patent Citations
Fluororesin and coated electric wire
WO2005052015A1
Magnet wire and coil
WO2020218205A1
Resin composition, molded body, composite body, and application of same
WO2022034903A1
Cited By
Flat wire and method for manufacturing same
WO2026127018A1
Flat wire and method for manufacturing same
WO2026127022A1