Wet particle emulsifier

The method of producing aqueous suspensions with specific silk fibroin fibers allows for the efficient formation of stable Pickering emulsions at low silk loadings, overcoming previous inefficiencies and toxicity issues, making it suitable for industrial use in cosmetics, pharmaceuticals, and food industries.

WO2024216332A1PCT designated stage expired Publication Date: 2024-10-24DEAKIN UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/AU2024/050365
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current methods for producing stable Pickering emulsions using silk fibroin fibers are inefficient due to long processing times and the use of toxic materials, and require high silk concentrations, making them unsuitable for industrial applications in cosmetics, pharmaceuticals, and food industries.

Method used

A method involving the production of aqueous suspensions containing silk fibroin fibers with a specific aspect ratio and width, achieved through degumming, cutting, partial hydrolysis, and shear homogenization, allowing for the formation of stable Pickering emulsions at low silk loadings and avoiding the use of toxic materials.

Benefits of technology

The method enables the production of stable Pickering emulsions with fine droplets and high viscosity, suitable for industrial applications, using silk fibroin fibers at low concentrations, thus addressing the inefficiencies and toxicity concerns of previous methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure AU2024050365_24102024_PF_FP_ABST
    Figure AU2024050365_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm.
Need to check novelty before this filing date? Find Prior Art

Description

WET PARTICLE EMULSIFIERTechnical Field

[0001] The present invention relates to the preparation and use of aqueous suspensions containing modified silk fibroin fibres which can be used in the preparation of a wide range of oil in water and water in oil Pickering emulsions (PE). The aqueous suspensions containing modified silk fibroin fibres may be used as emulsifiers in the formation of Pickering emulsions useful in a number of applications particularly in the cosmetics, pharmaceutical, biomedical, medtech and food industries given the safety profile of silk as a protein material. The applicants have found that Pickering emulsions produced using the aqueous suspension containing the modified silk fibroin fibres of the present invention are stable and can be produced with quite low loadings of silk compared to the disperse phase which is emulsified. In addition emulsions produced using the silk fibroin fibres of the present invention as emulsifiers are typically have high viscosity and can also form gel like emulsions.Background of Invention

[0002] Emulsions are found in a wide variety of products in everyday use including foods, cosmetics and pharmaceuticals. An emulsion can be understood to be a mixture of two or more liquids in which one of the liquids is present in the form of droplets of microscopic size or finer which are distributed throughout the other liquid. Simple emulsions are either oil droplets distributed in continuous water phase (called an oil in water emulsion (O / W)) or water droplets distributed in continuous oil phase (a water in oil emulsion (W / O)). Merely by way of example milk is an everyday example of an oil in water emulsion in which the fat phase of the milk forms tiny droplets within the water phase. In contrast to this margarine is an example of a water in oil emulsion as it consists of tiny droplets of water dispersed throughout a blend of vegetable oils.

[0003] The presence of emulsions in society and their extensive use in the food, cosmetics and pharmaceutical industry has lead to them being extensively studied in order to be able to provide stable emulsions. Thus it is well known that a simple emulsion can be temporarily produced by subjecting a mixture of oil and water to high shear (such as by rapid mixing). Emulsions of this type are formed in essence bybreaking up the dispersed phase into fine droplets within the continuous phase but require significant energy input to produce the required increase in interfacial area between the two phase. Unfortunately it is also well known that these emulsions are very unstable and tend to break down quite quickly leading to separation of oil and water phases unless an additive is used to stabilise the emulsion.

[0004] In order to stabilise emulsions and extend the life of any products that are in the form of an emulsion there has been significant research conducted into the identification and development of emulsifiers that help stabilise the emulsion once formed. Accordingly, there are now a wide range of natural and synthetic emulsifiers in use in various industries.

[0005] In general emulsifiers work as they create a physical barrier that keeps the droplets from coalescing with each other which would ultimately lead to phase separation. In general, a typical emulsifier consists of a hydrophilic (water loving) head group and a hydrophobic (oil loving) tail group. As such emulsifiers are attracted to both the water phase and the oil phase and when added to a mixture containing both water and oil they tend to congregate at the surface of the droplets in the mixture such that the water loving head group is present in the water phase and the oil loving tail group is present in the oil phase. As such in the case of an oil in water emulsion the emulsifier sits around the oil droplet with the hydrophilic head group extending out into the water phase and the hydrophilic tail group extending around and into the oil droplet.

[0006] Given the broad range of applications of emulsions in food, cosmetics and pharmaceuticals a potential concern is the safety profile of any emulsifier used. Accordingly, in the formation of emulsions there is always a concern that the emulsifier used may be having an unintended effect in the final formulation. As such research is constantly being carried out to identify new emulsifiers.

[0007] Historically most commonly used emulsifiers have been compounds that are soluble in either the dispersed phase or the continuous phase and as a result of their amphiphilic nature accumulate at the interface between the continuous phase and the dispersed phase. In this role they “stabilise” the emulsion as they prevent the droplets of the dispersed phase from coalescing.

[0008] Pickering emulsions have garnered interest in more recent times. A Pickering emulsion is an emulsion which is stabilised by solid particles as the emulsifier rather than by a compound that dissolves in the continuous or dispersed phases. As a result of their unique properties Pickering emulsions have the potential to find application in a number of areas in which emulsions are used.

[0009] Whilst there has been significant research carried out to date most Pickering emulsions are formed using inorganic particles like silica and the like. There are relatively few organic materials that will form insoluble particles that can be used to form Pickering emulsion. Such number is limited as it has been found that it is important for Pickering emulsion particles to have a water contact angle close to 90 deg. Accordingly most organic particles need to be modified to increase or decrease contact angle to form Pickering emulsions.

[0010] One area of research into the identification of potential emulsifiers in the formation of Pickering emulsions is an analysis of naturally occurring materials where these are perceived to be less likely to lead to any undesirable side effects. As such groups have conducted research into naturally occurring biopolymers like cellulose, peptides and proteins to determine if they have the ability to be used as emulsifiers in the formation of Pickering emulsions. An example of a naturally occurring material that has previously been reported to be able to be used in the formation of Pickering emulsions is silk fibre.

[0011] Silk is a naturally occurring fibre that is produced by a wide variety of arthropods with the most commercially significant being silk produced by the Bombyx mori silkworm reared using Mulberry tree leaves. In its natural form, silk is predominantly made up of an insoluble protein known as fibroin which is coated by a smaller amount of a water soluble protective layer known as sericin and it may also contain small amounts of other substances. Whilst the process of silk manufacture varies from country to country almost all processes involve one or more steps in which the silk is treated to remove the sericin leaving the “degummed (sericin free)” fibre made of fibroin protein. This typically involves heating of the fibres in alkali at elevated temperature.

[0012] Silk has been previously reported as an emulsifier in the form of a silk nanofibers. Unfortunately the reported nanofibre production requires a long, chemically intensive process route to convert silk fibre into solution. For example the reported procedure requires at least 72 hours of dialysis to remove toxic materials like Li Br used for dissolution of silk, then a further 24 plus hours for nano particles formation from solution and then a further more than 24 hrs to get self-assembled nanofibres. Accordingly, the produced nanofibers are not commercially attractive due to the time taken to produce the fibres and the use of toxic materials such as LiBr in their manufacture which makes their use problematic in foods, cosmetics and medtech, pharmaceuticals and biopharmaceuticals.

[0013] In a further attempt to use silk in the formation of emulsions it has been reported that emulsions can be formed using ball milled silk particles obtained using a standard silk isolation process in which silk has been treated to remove the water soluble sericin. The reported literature suggests that whilst this material may be used in the formation of emulsions there is a requirement that the emulsion contain at least 10% silk in order to provide a suitable stable emulsion. In addition the reported emulsion contained droplets with a droplet size of 100 micron or higher which is undesirable.

[0014] Many previous processes for the generation of potential emulsifiers have focused on the production of nano scale particles which were believed to be required for the production of a stable emulsion. A skilled worker in the field would generally not have expected to be able to form a strong emulsion with strong stability with micron size particles as it was believed that the presence of nanometre particles was required for the formation of a strong emulsion. The present invention demonstrates that if proper aspect ratio is maintained then micron size particles produced using simple, scalable and short processes are able to produce good emulsions

[0015] Accordingly, it would be desirable to provide alternative silk based emulsifiers that could find application in the preparation of Pickering emulsions in a wide variety of industries due to its consumer acceptance (being a natural product) and its status of being Generally recognised as safe (GRAS) by regulatory bodies such as the FDA.Summary of The Invention

[0016] As a result of the desire to provide alternative silk based emulsifiers, the applicants have identified a relatively straightforward process that can be utilised to modify silk to make it suitable for use as an emulsifier in the preparation of Pickering emulsions that find use in a number of industrial applications.

[0017] The applicants have identified that a specific combination of processing steps when carried out in combination produce silk fibroin fibres with a suitable size and fibre geometry which enables them to be used to form stable Pickering emulsions at relatively low loadings of silk in the final emulsion. In particular the applicants have found that silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm are particularly suitable for use in the formation of stable Pickering emulsions.

[0018] The applicants have found that silk fibroin fibres of this type are useful in the formation of Pickering emulsions but cannot be provided in the form of dry fibre particles as in the drying process the fibres aggregate and tend to stick together and cannot be redispersed easily. As such it is necessary to provide the fibres in the form of an aqueous suspension.

[0019] Accordingly, the present invention provides an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm. As stated above these fibres are found to be able to be used in the formation of Pickering emulsions at quite low loadings of silk. The applicants have also developed a process for the production of a suspension containing fibres of this type.

[0020] Accordingly, in yet an even further aspect the present invention provides a method of producing an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm, the method comprising (i) providing degummed silk fibroin fibres, (ii) cutting the degummed silk fibroin fibres to form cut silk fibroin fibres that will pass through a 5 mm grid; (iii) partial hydrolysis of the silk fibroin fibres to form partially hydrolysed silk fibroin fibres, and (iv) shearhomogenisation of the hydrolysed silk fibroin fibres; wherein steps (iii) and (iv) may be carried out sequentially or simultaneously. The process has been found to produce aqueous suspensions containing silk fibroin fibres with the desired properties on a consistent basis and is applicable to industrial scale up relatively easily.

[0021] In yet an even further aspect the present invention provides a method of producing an emulsion the method comprising (a) providing an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm; (b) adding a water immiscible component to the aqueous solution to form a mixture; and (c) subjecting the mixture to high shear to form an emulsion.

[0022] In yet an even further aspect still the present invention provides a formulation in the form of an emulsion comprising (a) silk fibroin fibres wherein 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm; (b) water (c) a water immiscible component and (d) one or more active ingredients.Description of the Drawing

[0023] Figure 1. Shows the process flow of a preferred embodiment for making the aqueous suspensions of silk fibroin fibres of the invention.

[0024] Figure 2. Shows an SEM image of the degummed silk fibre of example 1 .

[0025] Figure 3. Shows SEM image of silk snippets (produced using 4 mm grid)(example 2).

[0026] Figure 4. Shows SEM images of alkali hydrolysed and shear homogenized silk fibres Left: B-1 M-1 ; Right: B-1 M-2 (example 3).

[0027] Figure 5. Shows SEM images of acid hydrolysed and shear homogenized silk fibres Left: 15HS-20; Right: 15-HS-40 (example 5).

[0028] Figure 6. Shows SEM images of acid hydrolysed silk, 30HS-20 and shear homogenized silk fibres (example 5).

[0029] Figure 7. Shows fibre width distribution for 1 M NaOH, treated for 60 min at 25°C along with shear homogenization.

[0030] Figure 8. Shows fibre width distribution for 1 M NaOH, treated for 120 min at 25°C along with shear homogenisation.

[0031] Figure 9. Shows fibre width distribution for 15 wt.% (2.8M) H2SO4, treated at 20°C for 30 min and shear homogenized.

[0032] Figure 10. Shows fibre width distribution for 15 wt.% (2.8M) H2SO4, treated at 40°C for 30 min followed by shear homogenization.

[0033] Figure 11. Shows fibre width distribution for 30 wt% (5.6M) H2SO4, treated at 20°C for 30 min followed by shear homogenization.

[0034] Figure 12. Shows fibre width distribution in line graph format for alkali treated shear homogenised samples.

[0035] Figure 13. Shows fibre width distribution in line graph format for acid treated shear homogenised samples.

[0036] Figure 14. Shows fibre width distribution in line graph format for acid treated shear homogenised then 5 pass high pressure homogenised samples.

[0037] Figure 15. Shows bar graph of weight loss after hydrolysis under various regimes.

[0038] Figure 16. Shows FTIR spectrum of alkali hydrolysis samples versus a control degummed silk.

[0039] Figure 17. Shows FTIR spectrum of acid hydrolysis samples versus a control degummed silk.

[0040] Figure 18. Shows an emulsion produced by the process of the present invention using 0.75% silk and 30% oil.

[0041] Figure 19. Shows a viscosity graph of various emulsions produced by shear homogenisation of silk.

[0042] Figure 20. Shows a viscosity graph of various emulsions produced by shear homogenisation followed by high pressure homogenisation of silk.Detailed Description

[0043] In this specification, a number of terms are used that are well known to a skilled addressee. Nevertheless, for the purposes of clarity, a number of terms will be defined.

[0044] Throughout this specification, unless the context requires otherwise, the word “comprise”, or variations such as “comprises” or “comprising”, will be understood to imply the inclusion of a stated element or integer or group of elements or integers but not the exclusion of any other element or integer or group of elements or integers.

[0045] It is to be noted that where a range of values is expressed, it will be clearly understood that this range encompasses the upper and lower limits of the range, and all numerical values or sub-ranges in between these limits as if each numerical value and sub-range is explicitly recited. The statement "about X% to Y%" has the same meaning as "about X% to about Y%," unless indicated otherwise.

[0046] The term “about” as used in the specification means approximately or nearly and in the context of a numerical value or range set forth herein is meant to encompass variations of + / - 10% or less, + / - 5% or less, + / - 1% or less, or + / - 0.1 % or less of and from the numerical value or range recited or claimed.

[0047] It is also to be noted that, as used herein, the singular forms “a”, “an” and “the” include plural aspects unless the context already dictates otherwise.

[0048] An “emulsion” is a mixture of two or more liquids that are normally immiscible (unmixable or unblendable), with one of the liquids forming the dispersed phase and the other liquid forming the dispersion medium. Two liquids can form a number of different types of emulsions. By way of example, oil and water can form an oil-in-water emulsion where the oil is the dispersed phase and the water is the dispersion medium. Alternatively, they can form a water-in-oil emulsion where water is the dispersed phase and oil is the dispersion medium. Multiple emulsions are also possible such as a water- in-oil-in-water emulsion or an oil-in-water-in-oil emulsion. In circumstances where thereare multiple similar phases in the same emulsion (like the two oil phases in an oil-in- water-in-oil emulsion) each phase may contain a different solute.

[0049] As used herein the term “stable emulsion” refers to an emulsion that in which there is less than a 5% increase in mean droplet size over the first two weeks of storage at ambient temperature.

[0050] As used herein the term “miscibility” and derivations thereof such as “miscible” refers to the property or ability of two substances to mix in all proportions, or put another way, their ability to fully dissolve in each other at any concentration.

[0051] Accordingly as used herein the term “water-immiscible” means that there are certain proportions of the substance where it does not dissolve in water. For example, butanone (methyl ethyl ketone) is significantly soluble in water but is still classed as water-immiscible as these two solvents are not soluble in each other in all proportions.

[0052] As used herein the term “oil” refers to any nonpolar chemical substance that is both hydrophobic and lipophilic, and may include triesters of glycerol and fatty acids. Oils are typically liquids at room temperature.

[0053] The term “aspect ratio” of an object is typically defined as the ratio of its longest dimension to its shortest dimension. For example the aspect ratio of a circle is 1 . In relation to the fibres as there is some natural variation along the length of a fibre the term aspect ratio is defined as the ratio of the length of the fibre to its average width. Determining aspect ratio in this way provides a more accurate assessment of the aspect ratio as it takes into account variations of the width of a fibre along its length as well as removing the anomaly that would be caused by a fibre containing a weak point where it is typically very narrow but which is not representative of the fibre as a whole.

[0054] As used herein the term “average width” refers to the width of a fibre when three or more measurements are taken of the width of the fibre perpendicular to its longitudinal axis and the average of these measurements is determined. The measurements are typically taken at regular points along the longitudinal axis such as 25% of the way along the longitudinal axis, 50% of the way along the longitudinal axis and 75% of the way along the longitudinal axis.

[0055] As would be clear to a skilled worker in the art in describing fibres made by any process there is typically some degree of variation between fibres and within a fibre (where for example the width may vary along its length) as a whole with there generally being a distribution of fibres. Accordingly in describing the fibres of the present invention we have referred to language such as “wherein at least 90% of the fibres have an aspect ratio of at least 40.” For the avoidance of doubt in this and related phrases the 90% refers to the number percentage of the fibres such that 90% of the total number of fibres used for measurements having an aspect ratio at least 40. Put another way for every 100 fibres, 90 will have an aspect ratio of at least 40.

[0056] As discussed above the present invention provides a suspension containing novel silk fibroin fibres, methods for their production, methods for the use of fibres of this type in the formation of emulsions and formulations in the form of an emulsion containing the fibres.Silk Fibroin Fibres of the invention

[0057] As discussed above silk is a naturally occurring fibre that is produced by a wide variety of arthropods. In its natural form silk is predominantly made up of an insoluble protein known as fibroin which is coated by a smaller amount of a water soluble protective layer known as sericin and it may also contain small amounts of other substances. During processing the sericin is removed and the fibroin fibre is used for the textile industry. Whilst this form of silk fibre is well known it cannot readily be used in the formation of emulsion due to size, long length and large diameter. Accordingly a significant amount of research has been conducted in order to identify modifications to silk fibroin fibres that may make them suitable for use in the formation of Pickering emulsions.

[0058] The applicants have found that an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm are particularly suitable as emulsifiers in the formation of Pickering emulsions. As stated previously it is necessary to provide the fibres in the form of an aqueous suspension as of they are dried the fibres tend to agglomerate and are very hard to separate and redisperse.

[0059] In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 45. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 50. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 55. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 60. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 65. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 70. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 100. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 200. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 300. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 400. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 500. In one embodiment at least 90% of the silk fibroin fibres (by number) have an aspect ratio of at least 600.

[0060] As will be appreciated the applicants have found that the aspect ratio alone does not provide a fibre with the desired properties. The applicants have found that the combination of the aspect ratio and the width of the fibres is important in ensuring adequate fibre performance to form a good stable emulsion.

[0061] As such the silk fibroin fibres are also of a defined width in order to create the required Pickering emulsion. In general the applicants have found that it is necessary that the average width of the fibres is between 100 nm and 1000 nm. In one embodiment the average width of the fibres is between 100 nm and 900 nm. In one embodiment the average width of the fibres is between 100 nm and 800 nm. In one embodiment the average width of the fibres is between 100 nm and 700 nm. In one embodiment the average width of the fibres is between 100 nm and 600 nm. In one embodiment the average width of the fibres is between 100 nm and 500 nm. In one embodiment the average width of the fibres is between 100 nm and 400 nm. In one embodiment the average width of the fibres is between 100 nm and 300 nm. In one embodiment the average width of the fibres is between 100 nm and 200 nm. In one embodiment the average width of the fibres is between 100 nm and 150 nm.

[0062] In order to provide a Pickering emulsion with the desired properties it is desirable that all the silk fibroin fibres have the stated aspect ratio and average width as described above. Nevertheless as will be appreciated by a skilled worker in the field a working emulsion can be produced as long as a sufficient number or percentage of the particles meet this criteria. As such the applicants have typically found that an acceptable emulsion can be formed if at least 90 % of the particles (by number) having an aspect ratio of at least 40 and further wherein the average width of the fibres is less between 100 nm and 1000 nm.

[0063] The silk fibroin particles may be present in the suspension in a wide variety of amounts depending upon the method of manufacture of the suspension. In general the silk fibroin fibres are present in an amount of from 0.1 % % to 7% w / v based on the total amount of the aqueous suspension. In one embodiment the silk fibroin fibres are present in an amount of from 0.3% to 6% w / v based on the total amount of the aqueous suspension. In one embodiment the silk fibroin fibres are present in an amount of from 0.5% to 5% w / v based on the total amount of the aqueous suspension.Formation of a Suspension containing Silk Fibroin Fibres of the invention

[0064] As discussed above the present invention provides a method of producing an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm, the method comprising (i) providing degummed silk fibroin fibres, (ii) cutting the degummed silk fibroin fibres to form cut silk fibroin fibres that will pass through a 5 mm grid; (iii) partial hydrolysis of the silk fibroin fibres to form partially hydrolysed silk fibroin fibres, and (iv) shear homogenisation of the hydrolysed silk fibroin fibres; wherein steps (iii) and (iv) may be carried out sequentially or simultaneously.

[0065] The first step in the method of formation of a suspension containing silk fibroin fibres of the invention is the provision of degummed silk fibroin fibres. The applicants have found that the provision of degummed silk is important in order to ensure that the fibres are able to be adequately separated because of the removal of gummy sericin protein during degumming that glue silk filaments together.

[0066] The method of providing degummed silk fibroin fibres can be done by any way known in the art. In one embodiment the step of providing degummed silk fibroin fibres comprises heating a silk starting material in an alkali solution at a temperature of from 80°C to 120°C. In yet a further embodiment the step of providing degummed silk fibroin fibres comprises heating a silk starting material at a temperature of from 100°C to 120°C. In yet a further embodiment the step of providing degummed silk fibroin fibres comprises subjecting a silk starting material to enzymatic treatment.

[0067] Examples of Silk materials that may be used as starting materials in the present invention include the Shell of Green or stifled Cocoon after removing the pupae, reeled silk filament from silk reeling factory, degummed silk from spun silk industry, waste cut cocoon and reeling waste from the silk reeling sector, degummed silk waste from spun silk industry, and raw silk or degummed silk based silk fabric waste. In one embodiment the silk starting material is raw silk.

[0068] The type of silk starting material can also vary widely. Examples include silk from B. mori (Mulberry), A.assama (Muga silk). S.C / 7c / 7? / (Eri silk) and A. Pemy / (Tasar).

[0069] The amount of starting material present in the alkali solution may vary. In one embodiment the starting material is present in an amount of 10 to 100 g per L of alkali solution. In one embodiment the starting material is present in an amount 20 to 100 g per L of alkali solution. In yet another embodiment the starting material is present in an amount of in an amount of 40 to 100 g per L of alkali solution.

[0070] As will be appreciated the process is a combination of temperature, time and alkali concentration with all three variables interacting with each other. Thus, for example, the higher the temperature the shorter the time that is required in order to provide degummed silk fibroin fibres. A skilled worker will typically modify one or more of these variables based on the equipment available and the desired timeline of the process step.

[0071] Nevertheless as stated above the temperature is typically from 80°C to 120°C. In one embodiment the temperature is from 85°C to 1 15°C. In yet an even further embodiment the temperature is from 90°C to 110°C. In yet an even furtherembodiment the temperature is from 95°C to 1 15°C. In one embodiment the temperature is about 100°C.

[0072] As will be appreciated as the alkali solution is typically an aqueous solution and the temperatures discussed above may exceed the boiling point of the solution the heating step is typically conducted in a sealed vessel. The vessel may be of any suitable type and a skilled worker in the field could easily choose a suitable vessel based on the production parameters they wish to use such as volume and the like.

[0073] The heating is carried out for a time period that is sufficient to provide degummed silk fibroin fibres. In general as discussed above selection of the time will depend upon the other variables used and the starting material used. This may involve some routine experimentation based on the starting material of choice but once determined will be relatively consistent. It is anticipated, however, that the heating will be carried out for from 10 minutes to 240 minutes. Once again it is anticipated that lower temperatures will require a longer heating period whereas higher temperatures will require a shorter heating period.

[0074] In one embodiment the heating is carried out for from 15 minutes to 180 minutes. In one embodiment the heating is carried out for from 20 minutes to 150 minutes. In one embodiment the heating is carried out for from 25 minutes to 120 minutes. In one embodiment the heating is carried out for from 30 minutes to 90 minutes. In one embodiment the heating is carried out for from 45 minutes to 75 minutes. In one embodiment the heating is carried out for from 50 minutes to 70 minutes. In one embodiment the heating is carried out for from 55 minutes to 65 minutes. In one embodiment the heating is carried out for about 60 minutes.

[0075] The alkli solution used may be any suitable alkali solution known in the art. Examples of alkali solutions that may be used include sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium hydroxide and potassium hydroxide. In general, however, it is found to be preferable if the alkali is a mild alkali such as sodium carbonate or sodium bicarbonate. In one embodiment the alkali is sodium carbonate. In one embodiment the alkali is sodium bicarbonate. It is particularly desirable that the alkali is sodium carbonate as this alkali is the alkali of choice for the degumming of silk in the commercial silk industry and so silk processorstypically have ready amounts of sodium carbonate on hand and are also well versed in its use in relation to materials safety and handling.

[0076] In choosing an alkali solution the solution is typically chosen so that the alkali solution has a pH of greater than 8.0. In one embodiment the alkali solution has a pH of greater than 9.0. In one embodiment the alkali solution has a pH of greater than 10.0.A skilled addressee in the field would readily be able to vary the pH of an alkali solution to fall within this range once a suitable alkali was chosen.In table 1 below we outline examples of different alkali at different concentrations.Table 1

[0077] The amount of alkali can vary depending upon the specific alkali source chosen. In circumstances where the alkali is sodium carbonate the amount of alkali in the alkali solution is typically from 0.5g / L to 5g / L. In one embodiment the amount of alkali in the alkali solution is from 0.5 / L to 4g / L. In one embodiment the amount of alkali in the alkali solution is from 0.5g / L to 3g / L. In one embodiment the amount of alkali in the alkali solution is from 0.5g / L to 2g / L.

[0078] It is typical that during the heating step the alkali solution is agitated. This can be carried out in a wide variety of ways depending upon the apparatus chosen. Following completion of the heating step the alkali solution is typically cooled and the degummed silk fibroin fibres washed to remove alkali residues discussed below.

[0079] Following heating the degummed silk fibroin fibres may then be washed to remove any residue from the heating step. As will be appreciated there are a number of potential washing steps that may be used. Washing steps that may be used either alone or in combination may include (a) a warm water washing step (b) a cold water washing step (c) a mild acid washing step to remove basic residue from the heating step. Any washing regime may incorporate one or more of these steps.

[0080] If a warm water washing step is used the water is typically at a temperature of from 40°C to 80°C. In one embodiment the warm water wash is at a temperature of from 40°C to 70°C.

[0081] If a cold water washing step is used the water is typically at a temperature of from 5°C to 20°C. In one embodiment the cold water wash is at a temperature of from 10°C to 20°C. In one embodiment the cold water wash is at a temperature of from 15°C to 20°C.

[0082] If a mild acid washing step is used the wash is typically dilute acetic acid. The dilute acid wash is typically at a temperature is of from 10°C to 30°C. In one embodiment the acid wash is at a temperature of from 15°C to 25°C. In one embodiment the acid wash is at a temperature of about 20°C. If an acid wash is used the silk fibres are typically washed with the dilute acid until the pH of the washing liquor is 7 which indicates that all residual alkali has been removed.

[0083] Once the degummed silk fibroin fibres have been washed after separating sericin, they are then dried prior to subjection to the remaining steps of the process. The drying may be carried out in any way well known in the art although it is typical that the drying is carried out using oven drying typically at a temperature of from 70°C to 80°C or air drying.

[0084] The degummed silk fibroin fibres in dry form are then cut to form cut silk fibres that will pass through a 5 mm grid. In one embodiment the fibres are cut such that they will pass through a grid between 0.25 and 5.0 mm. In one embodiment the fibres are cut such that they will pass through a grid between 1.0 and 3.0 mm. In one embodiment the fibres are cut such that they will pass through a 4.00 mm grid. In one embodiment the fibres are cut such that they will pass through a 3.00 mm grid. In one embodiment the fibres are cut such that they will pass through a 2.00 mm grid.

[0085] The cutting may be carried out in any way known in the art although typically cutting comprises passing the degummed fibroin fibres through a fibre cutting machine or a cutter mill to form cut silk fibres of the desired dimension if required repeatedly before passing through the grid.

[0086] A cutter mill is piece of equipment that consists of a series of uniformly spaced knives (typically 2 to 12 in number) which are attached to a horizontal rotor (rotating knives) which act against a series of stationary knives that are attached to the casing body of the mill. The bottom of the mill typically has a screen or grid attached which controls the residence time of the material inside the mill head as once the fibre particles are small enough to pass through the grid they fall out the bottom of the mill. As would be appreciated by a skilled worker in the field the size of particles produced by a cutter mill are typically determined by the rotor size, the gap between the sets of knives and the size of the screen or grid. A skilled worker will readily be able to modify these variables to produce cut silk of the required size. As will also be appreciated, however, given that the silk fibroin fibres are typically relatively thin there is the possibility that some of them may contact the screen in a lengthwise fashion and pass through the grid.

[0087] Following cutting as described above the process of the present invention then comprises (iii) partial hydrolysis of the silk fibroin fibres to form partially hydrolysed silk fibroin fibres, and (iv) shear homogenisation of the hydrolysed silk fibroin fibres; wherein steps (iii) and (iv) may be carried out sequentially or simultaneously.

[0088] The partial hydrolysis of the silk fibroin fibres may be carried out using acid hydrolysis, alkali hydrolysis or enzymatic hydrolysis. Accordingly in one embodiment hydrolysis of the silk fibroin fibres comprises subjecting the silk fibroin fibres to acid oralkali treatment to form partially hydrolysed silk fibroin fibres. In one embodiment hydrolysis of the silk fibroin fibres comprises subjecting the silk fibroin fibres to acid treatment to form partially hydrolysed silk fibroin fibres. In one embodiment hydrolysis of the silk fibroin fibres comprises subjecting the silk fibroin fibres to alkali treatment to form partially hydrolysed silk fibroin fibres. In one embodiment hydrolysis of the silk fibroin fibres comprises subjecting the silk fibroin fibres to enzymatic treatment to form partially hydrolysed silk fibroin fibres.

[0089] The acid or alkali treatment typically involves addition of the silk fibroin fibres to an alkali or acid solution to form a suspension of the silk fibroin fibres in the alkali or acid aqueous suspension. The amount of silk fibroin fibres in the aqueous suspension may vary widely but is typically from 0.1 wt% to 6wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.3wt% to 5.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.5wt% to 4.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.7wt% to 3.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.8wt% to 2.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.9wt% to 1 .5.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is about 1 % based on the total weight of the aqueous suspension.

[0090] The alkali solution used may be any suitable alkali solution known in the art. Examples of alkali solutions that may be used include sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium hydroxide and potassium hydroxide. In general, however, it is found to be preferable if the alkali is a strong alkali such as potassium hydroxide or sodium hydroxide. In one embodiment the alkali solution is potassium hydroxide. In one embodiment the alkali solution is sodium hydroxide.

[0091] In choosing an alkali solution the solution is typically chosen so that the alkali solution has a pH of greater than 9.0. In one embodiment the alkali solution has a pH of greater than 10.0. In one embodiment the alkali solution has a pH of greater than 1 1.0. In one embodiment the alkali solution has a pH of greater than 12.0. In one embodiment the alkali solution has a pH of greater than 13.0.

[0092] The concentration of the alkali solution typically varies depending upon the alkali chosen. In one embodiment the alkali is at a concentration of from 0.1 M to 10.0 M. In one embodiment the alkali is at a concentration of from 0.2M to 9.0 M. In one embodiment the alkali is at a concentration of from 0.3M to 8.0 M. In one embodiment the alkali is at a concentration of from 0.4M to 7.0 M. In one embodiment the alkali is at a concentration of from 0.5M to 6.0 M. In one embodiment the alkali is at a concentration of from 0.6M to 5.0 M. In one embodiment the alkali is at a concentration of from 0.7M to 4.0 M. In one embodiment the alkali is at a concentration of from 0.8M to 3.0 M. In one embodiment the alkali is at a concentration of from 0.9M to 2.0 M. In one embodiment the alkali is at a concentration of about 1 .0M.

[0093] If an alkali hydrolysis is conducted the hydrolysis is typically carried out for from 15 minutes to 360 minutes. In one embodiment the hydrolysis is carried out for from 60 minutes to 270 minutes. In one embodiment the hydrolysis is carried out for from 90 minutes to 240 minutes. The hydrolysis is typically conducted at a temperature of from 20°C to 30°C most typically 25°C.

[0094] Following completion of the desired length of alkali hydrolysis the reaction is quenched by addition of dilute acid to neutralise the alkali and achieve a pH of 7.0 in the solution.

[0095] If the hydrolysis is an acid treatment a wide variety of acid may be used although it is preferred that the acid is a strong acid. Examples of suitable acids include sulphuric acid, nitric acid and hydrochloric acid. In one embodiment the acid is sulphuric acid. In one embodiment the acid is nitric acid. In one embodiment the acid is hydrochloric acid.

[0096] In choosing an acid solution the solution is typically chosen so that the acid solution has a pH of lower than 5.0. In one embodiment the acid solution has a pH oflower than 4.0. In one embodiment the acid solution has a pH of lower than 3.0. In one embodiment the acid solution has a pH of lower than 2.0. In one embodiment the acid solution has a pH of lower than 1 .0.

[0097] The concentration of the acid solution typically varies depending upon the acid chosen. In one embodiment the acid is at a concentration of from 0.1 M to 10.0 M. In one embodiment the acid is at a concentration of from 0.2M to 9.0 M. In one embodiment the acid is at a concentration of from 0.3M to 8.0 M. In one embodiment the acid is at a concentration of from 0.4M to 7.0 M. In one embodiment the acid is at a concentration of from 0.5M to 6.0 M. In one embodiment the acid is at a concentration of from 0.6M to 5.0 M. In one embodiment the acid is at a concentration of from 0.7M to 4.0 M. In one embodiment the acid is at a concentration of from 0.8M to 3.0 M. In one embodiment the acid is at a concentration of from 0.9M to 2.0 M. In one embodiment the acid is at a concentration of about 1 .0M.

[0098] Upon completion, the acid treatment is then typically stopped by addition of water followed by centrifugation and washing until the suspension reaches a pH of 7.0.

[0099] In relation to acid or alkali hydrolysis as discussed above the temperature of the acid or alkali solution used may vary although the temperature is typically from 20°C to 40°C. In one embodiment the hydrolysis is carried out at a temperature of from 20°C to 35°C. In one embodiment the hydrolysis is carried out at a temperature of from 20°C to 30°C. In one embodiment the hydrolysis is carried out at a temperature about 25°C.

[0100] The process of the present invention also comprises shear homogenisation of the partially hydrolysed silk fibroin fibres. The shear homogenisation may be carried out either simultaneously with or subsequent to the partial hydrolysis step. In one embodiment the shear homogenisation is carried out simultaneously with the partial hydrolysis step. In one embodiment the shear homogenisation is carried out subsequent to the partial hydrolysis step.

[0101] In circumstances where the partial hydrolysis and the shear homogenisation are carried out simultaneously the partial hydrolysis is conducted along with shear mixing. In circumstances where the partial hydrolysis and the shear homogenisationare carried out sequentially a suspension of the silk fibroin fibres is added to a shear homogeniser.

[0102] The shear homogenisation may be carried out in a number of ways. The shear homogeniser typically has a rotation speed of from 1000 to 30000 rpm. In one embodiment the shear homogeniser has a rotation speed of from 5000 to 25000 rpm. In one embodiment the shear homogeniser has a rotation speed of from 10000 to 20000 rpm. In one embodiment the shear homogeniser has a rotation speed of from 12000 to 18000 rpm. In one embodiment the shear homogeniser has a rotation speed of from 14000 to 16000 rpm. In one embodiment the shear homogeniser has a rotation speed of about 15000 rpm.

[0103] The shear homogenisation is typically carried out for from 15 minutes to 180 minutes. In one embodiment the shear homogenisation is carried out for from 20 minutes to 150 minutes. In one embodiment the shear homogenisation is carried out for from 25 minutes to 120 minutes. In one embodiment the shear homogenisation is carried out for from 30 minutes to 90 minutes. In one embodiment the shear homogenisation is carried out for from 45 minutes to 75 minutes. In one embodiment the shear homogenisation is carried out for from 50 minutes to 70 minutes. In one embodiment the shear homogenisation is carried out for from 55 minutes to 65 minutes. In one embodiment the shear homogenisation is carried out for about 60 minutes.

[0104] In a preferred embodiment of the invention after shear homogenisation as discussed above the suspension of silk fibroin fibres is then subjected to high pressure homogenisation.

[0105] In one embodiment the high-pressure homogenisation is carried out at a pressure of from 100 to 4000 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of from 500 to 1500 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of from 500 to 1000 bar In one embodiment the high-pressure homogenisation is carried out at a pressure of about 600 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of about 700 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of about 800 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of about 900 bar.

[0106] In one embodiment the high-pressure homogenisation is carried out at a temperature of from 10°C to 90°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 10°C to 70°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 10°C to 50°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 20°C to 50°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 20°C to 30°C.

[0107] In certain embodiments the high-pressure homogenisation involves multiple passes of the suspension through the homogeniser. In one embodiment the suspension is passed 6 times through the homogeniser. In one embodiment the suspension is passed 5 times through the homogeniser. In one embodiment the suspension is passed 4 times through the homogeniser. In one embodiment the suspension is passed 3 times through the homogeniser. In one embodiment the suspension is passed 2 times through the homogeniser. In one embodiment the suspension is passed a single time through the homogeniser.

[0108] The flow rate of the suspension through the high-pressure homogeniser will be dependent on a number of variables including the exact parameters and scale of the homogeniser equipment, however, the flow rate is typically in the range of from 10 to 28000 L / h. The suspension of silk passing through the high pressure homogenisation is generally from 1 -2% w / V. typically less than 1 %.Use of the suspension containing silk fibroin fibres to form an emulsion

[0109] As stated previously the aqueous suspension containing the silk fibroin fibres of the invention may be used as an emulsifier in the formation of a Pickering emulsion in which the fibres act as an emulsifier. The applicants have found that the fibres can be used in the formation of either an oil in water emulsion or a water in oil emulsion depending upon the way in which the emulsion is formed. As such the fibres are inherently very flexible emulsifiers that can be used in the formulation of a wide variety of emulsions.

[0110] Accordingly the present invention provides a method of producing an emulsion the method comprising (a) providing an aqueous suspension containing silkfibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm; (b) adding a water immiscible component to the aqueous solution to form a mixture; and (c) subjecting the mixture to high shear form an emulsion. In certain embodiments the emulsion is a stable emulsion as specified herein.

[0111] As can be seen the first step in the process is providing an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is less than 1000 nm.

[0112] The amount of silk fibroin fibres in the aqueous suspension may vary widely but is typically from 0.1 wt% 7.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.5wt% to 6.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.6wt% to 5.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.7wt% to 4.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is from 0.8wt% to 3.0wt% based on the total weight of the aqueous suspension. In one embodiment he amount of silk fibroin fibres in the aqueous suspension is from 0.9wt% to 2.0wt% based on the total weight of the aqueous suspension. In one embodiment the amount of silk fibroin fibres in the aqueous suspension is about 1 % based on the total weight of the aqueous suspension.

[0113] The second step in the process is addition of a water immiscible component to the aqueous suspension to form a mixture. The water-immiscible component may take any number of forms with the identity of the water-immiscible component typically being selected on the basis of the desired end-use application of emulsion, the cost, availability, and properties of the material. For example where the emulsion is intended to be used as a food additive it is advantageous to attempt to use a food-grade water- immiscible component. In principle, any water-immiscible component may be used with a water-immiscible liquid being preferred.

[0114] In some embodiments, the water-immiscible component is an oil or a combination of oils. The oil may be an organic oil or a mineral oil. Examples of oils that may be used include Ce-C hydrocarbons, triglycerides, natural oils, petroleum-based oils, and silicone oils. In some embodiments the oil is a natural oil selected from the group consisting of almond oil, apricot kernel oil, avocado oil, coconut oil, olive oil, safflower oil, sesame oil, soybean oil, sunflower oil, rapeseed oil, hemp oil, canola oil, cocoa butter, peanut oil, wheat germ oil, and other vegetable oils. The oil may also be sandalwood oil or an essential oil such as lavender oil, tea tree oil, frankincense oil, peppermint oil, eucalyptus oil, lemon oil, lemongrass oil, orange oil, rosemary oil, bergamot oil, and cedarwood oil.

[0115] In some embodiments the water-immiscible component is a solvent or a combination of solvents. Examples of suitable solvents that may be used include carbon tetrachloride, chloroform, cyclohexane, 1 ,2-dichloroethane, dichloromethane, diethyl ether, dimethyl formamide, ethyl acetate, heptane, hexane, cyclohexane, methyl-tert-butyl ether, pentane, toluene, and 2,2,4-trimethylpentane or a combination thereof. In one embodiment the water-immiscible component is hexane or cyclohexane.

[0116] The amount of water immiscible component in the final emulsion may vary widely from as low as 5% w / w up to 90% w / w based on the total weight of the emulsion. Nevertheless the amount water immiscible component is typically from 10 to 70% w / w and the amount of water immiscible component mixed with the aqueous suspension containing the silk fibroin fibres is selected to achieve this range in the final emulsion. In one embodiment the amount of water immiscible component in the final emulsion is from 10 to 60% w / w. In one embodiment the amount of water immiscible component in the final emulsion is from 10 to 50% w / w. In one embodiment the amount of water immiscible component in the final emulsion is from 10 to 40% w / w. In one embodiment the amount of water immiscible component in the final emulsion is from 20 to 40% w / w. In one embodiment the amount of water immiscible component in the final emulsion is from 25 to 35% w / w. In one embodiment the amount of water immiscible component in the final emulsion is from 28 to 32% w / w. In one embodiment the amount of water immiscible component in the final emulsion is about 30% w / w.

[0117] Following combination of the aqueous suspension containing silk fibroin fibres with the water immiscible component the resulting mixture is subjected to high shear to form the emulsion.

[0118] The applicants have found that the droplets in the final emulsion produced by the methods of the present invention typically are fine droplets which facilitate their use in many formulations. In one embodiment the method produces emulsions wherein 90 % of the droplets in the emulsion are less than 100 .M. In another embodiment the method produces emulsions wherein 90 % of the droplets in the emulsion are less than 70 .M. In another embodiment the method produces emulsions wherein 90 % of the droplets in the emulsion are less than 40 |iM.

[0119] There are a number of known technologies that may be used to subject a liquid mixture to high shear. Examples of techniques for providing high shear that produce the necessary shear forces include high-pressure homogenisation, microfluidisation, hydrodynamic cavitation and ultrasonication.

[0120] In one embodiment of the method of the invention in step (c), the mixture is subjected to high shear by sonication of the aqueous mixture comprising silk fibroin fibres and water immiscible component. The sonication frequency used may vary greatly although it is typically in the range of from 20kHz to 200kHz. In one embodiment the sonication is carried out at a frequency of from 20kHz to 200kHz. In one embodiment the sonication is carried out at a frequency of from 20kHz to 150kHz. In one embodiment the sonication is carried out at a frequency of from 20kHz to 100kHz. In one embodiment the sonication is carried out at a frequency of from 20kHz to 40kHz.

[0121] As will be appreciated by a skilled worker in the field sonication frequency is merely one variable in the sonication process. In general, the threshold energy density is a better way of determining the sonication step.

[0122] The threshold energy density (E) may be defined as:

[0123] E=(P X t) / V;

[0124] Where P = Power input (W), t = time (s) and V (mL) is the processed volume.

[0125] In certain embodiments, the sonication is carried out at an energy density of greater than 20 J / mL. In certain embodiments the sonicator is a 400W sonicator. The sonicator may be operated at various power levels. In certain embodiments the sonicator is operated at a power of from 50% to 100%.

[0126] The sonication may be carried out for any period of time necessary to achieve the desired phase inversion. In one embodiment the sonication is carried out for from 1 second to 600 seconds. In one embodiment the sonication is carried out for from 5 seconds to 300 seconds. In one embodiment the sonication is carried out for from 10 seconds to 200 seconds. In one embodiment the sonication is carried out for from 15 seconds to 100 seconds. In one embodiment the sonication is carried out for from 20 second to 50 seconds. The sonicator may also be pulsed in order to maximise shear. The pulse may vary from 50 to 100. In one embodiment the pulse is 50. In one embodiment the pulse is 60. In one embodiment the pulse is 70. In one embodiment the pulse is 80. In one embodiment the pulse is 90. In one embodiment the pulse is 100.

[0127] In one aspect the sonication is carried out in a continuous fashion whereby the mixture is passed through a sonication zone in order to produce the desired emulsion. In one embodiment the residence time in the sonication zone is 1 second to 600 seconds. In one embodiment the residence time in the sonication zone is 5 seconds to 300 seconds. In one embodiment the sonication is carried out for from 10 seconds to 200 seconds. In one embodiment the sonication is c the residence time in the sonication zone is 15 seconds to 100 seconds. In one embodiment the residence time in the sonication zone is 20 second to 50 seconds.

[0128] In one embodiment the sonication is carried out for about 5 seconds. In one embodiment the sonication is carried out for about 10 seconds. In one embodiment the sonication is carried out for about 15 seconds. In one embodiment the sonication is carried out for about 20 seconds. In one embodiment the sonication is carried out for about 25 seconds. In one embodiment the sonication is carried out for about 30 seconds. In one embodiment the sonication is carried out for about 35 seconds. In one embodiment the sonication is carried out for about 40 seconds. In one embodiment the sonication is carried out for about 45 seconds. In one embodiment the sonication iscarried out for about 50 seconds. In one embodiment the sonication is carried out for about 55 seconds. In one embodiment the sonication is carried out for about 60 seconds.

[0129] In one embodiment of the process of the invention in step (c) the mixture is subjected to high shear by the subjection of the aqueous mixture comprising silk fibroin fibres and water immiscible component to high-pressure homogenisation.

[0130] In one embodiment the high-pressure homogenisation is carried out at a pressure of from 100 to 2000 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of from 500 to 1500 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of from 500 to 1000 bar In one embodiment the high-pressure homogenisation is carried out at a pressure of about 600 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of about 700 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of about 800 bar. In one embodiment the high-pressure homogenisation is carried out at a pressure of about 900 bar.

[0131] In one embodiment the high-pressure homogenisation is carried out at a temperature of from 10°C to 90°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 10°C to 70°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 10°C to 50°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 20°C to 50°C. In one embodiment the high-pressure homogenisation is carried out at a temperature of from 20°C to 30°C.

[0132] In certain embodiments the high-pressure homogenisation involves multiple passes of the mixture through the homogeniser. In one embodiment the mixture is passed 6 times through the homogeniser. In one embodiment the mixture is passed 5 times through the homogeniser. In one embodiment the mixture is passed 4 times through the homogeniser. In one embodiment the mixture is passed 3 times through the homogeniser. In one embodiment the mixture is passed 2 times through the homogeniser. In one embodiment the is passed a single time through the homogeniser.

[0133] The flow rate of the mixture through the high-pressure homogeniser will be dependent on a number of variables including the exact parameters and scale of the homogeniser equipment, however, the flow rate is typically in the range of from 10 to 28000 L / h.

[0134] The end result of the method of the invention is an emulsion which may be used in a number of industrial formulations.Formulations of the Invention

[0135] The present inventions also pertains to novel formulations that can be produced using the methods of the present invention. Accordingly the present invention provides a formulation in the form of an emulsion comprising (a) silk fibroin fibres wherein 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm; (b) water (c) a water immiscible component and (d) one or more active ingredients.

[0136] The amount of silk fibroin fibres in the formulations of the invention is typically from 0.1 to 5% w / w based on the total weight of the formulation. In one embodiment the amount of silk fibroin fibres in the formulations of the invention is from 0.5 to 4% w / w. In one embodiment the amount of silk fibroin fibres in the formulations of the invention is from 0.5 to 3% w / w. In one embodiment the amount of silk fibroin fibres in the formulations of the invention is from 0.5 to 2.5% w / w. In one embodiment the amount of silk fibroin fibres in the formulations of the invention is from 0.5 to 2.0% w / w. In one embodiment the amount of silk fibroin fibres in the formulations of the invention is from 0.5 to 1 .2% w / w.

[0137] The formulations of the invention also contain a water immiscible component.

[0138] In some embodiments, the water-immiscible component is an oil or a combination of oils. The oil may be an organic oil or a mineral oil. Examples of oils that may be used include Ce-C hydrocarbons, triglycerides, natural oils, petroleum-based oils, and silicone oils. In some embodiments the oil is a natural oil selected from the group consisting of almond oil, apricot kernel oil, avocado oil, coconut oil, olive oil,safflower oil, sesame oil, soybean oil, sunflower oil, rapeseed oil, hemp oil, canola oil, cocoa butter, peanut oil, wheat germ oil, and other vegetable oils. The oil may also be sandalwood oil or an essential oil such as lavender oil, tea tree oil, frankincense oil, peppermint oil, eucalyptus oil, lemon oil, lemongrass oil, orange oil, rosemary oil, bergamot oil, and cedarwood oil.

[0139] In some embodiments the water-immiscible component is a solvent or a combination of solvents. Examples of suitable solvents that may be used include carbon tetrachloride, chloroform, cyclohexane, 1 ,2-dichloroethane, dichloromethane, diethyl ether, dimethyl formamide, ethyl acetate, heptane, hexane, cyclohexane, methyl-tert-butyl ether, pentane, toluene, and 2,2,4-trimethylpentane or a combination thereof. In one embodiment the water-immiscible component is hexane or cyclohexane.

[0140] The amount of water immiscible component in the formulation may vary widely from as low as 5%w / w up to 90%w / w based on the total weight of the formulation. Nevertheless, the amount of water immiscible component is typically from 10%w / w to 70% w / w. In one embodiment the amount of water immiscible component in the formulation is from 10%w / w to 60% w / w. In one embodiment the amount of water immiscible component in the formulation is from 10%w / w to 50% w / w. In one embodiment the amount of water immiscible component in the formulation is from 10%w / w to 40% w / w. In one embodiment the amount of water immiscible component in the formulation is from 20%w / w to 40% w / w. In one embodiment the amount of water immiscible component in the formulation is from 20%w / w to 35% w / w. In one embodiment the amount of water immiscible component in the formulation is from 28%w / w to 32% w / w. In one embodiment the amount of water immiscible component in the formulation is about 30% w / w.

[0141] The amount of water in the formulation may vary widely from as low as 10%w / w up to 90%w / w based on the total weight of the formulation. In one embodiment the amount of water in the formulation is from 20% w / w to 90% w / w. In one embodiment the amount of water in the formulation is from 30% w / w to 90 % w / w. In one embodiment the amount of water in the formulation is from 30% w / w to 80% w / w. In one embodiment the amount of water in the formulation is from 40% w / w to 80% w / w. In one embodiment the amount of water in the formulation is from 50% w / w to 80% w / w. In one embodimentthe amount of water in the formulation is from 60% w / w to 80% w / w. In one embodiment the amount of water in the formulation is from 65% w / w to 75% w / w. In one embodiment the amount of water in the formulation is about 70% w / w.

[0142] The formulations of the present invention also contain one or more active agents. The active agent may be any type of active agent and may include a cosmetic agent, a therapeutic agent or a nutraceutical agent. The active agent may be present in either the dispersed phase or the continuous phase.

[0143] Examples of active agents include anaesthetics, antibiotics (eg, erythromycin and tetracycline), salicylic acid , anti-allergic agents, anti-fungal agents, anti-helminthic anti-irritants, anti-inflammatory agents, antimicrobial agents, antibacterial agents, analgesics, nitric oxide synthase inhibitors, insect repellents, skin cooling Agents, chelating agents, perfumes, vitamins, or any mixture thereof.

[0144] The formulations of the invention may also contain a number of other additives such as preservatives, self-blackening agents, skin penetration enhancers, colorants (including dyes, lakes and pigments, which may be untreated or chemically surface treated to improve wettability or some other property), demulcents, emollients, wetting agents, lubricants, skin protectants, humectants, pH adjusters, preservatives, stabilizers, surfactants, thickeners, plasticizers, viscosity improvers, or any mixture thereof.

[0145] The invention will now be illustrated by way of examples; however, the examples are not to be construed as being limitations thereto.ExamplesMaterials:

[0146] Silk materials of the following forms can be used for particle production including shell of Green or stifled Cocoon after removing the pupae, reeled Silk filament from silk reeling factory, degummed silk from spun silk industry, waste cut cocoon and reeling waste from the silk reeling sector, degummed silk waste of various types from spun silk industry and raw silk or degummed silk based silk fabric waste.

[0147] A wide variety of silk types may be used including silk from B.mori (Mulberry), A.assama (Muga silk) and S.C ricini (Eri silk) and A. Pernyi (Tasar). B.mori was used because it is widely available compared to other type of silk. Silk materials were supplied by Automatic Reeling mill Ramgrah, India and Rudrasagar Silk Mill India.

[0148] Chemicals for emulsion formation were purchased from New Directions Australia Pty Ltd and other chemicals were from Sigma Aldrich Australia and were used as received.Example 1 : Degumming of Silk

[0149] Silk cocoon shells were cut into pieces. In place of cocoon shells, raw silk filaments can also be used. The cocoon pieces / raw silk filaments were degummed to remove sericin gum using an Ahiba dyeing machine. For this 20 g silk and 300 mL alkaline solution (2g / L Sodium carbonate, using deionised water containing 0.5g / L of soap) were used in each beaker. Beakers are closed and air tight. Temperature was 98 deg C, time of treatment 30 min. the heating rate was 4 deg C per min and cooling rate was 2 deg C per min. The breakers were rotated slowly @5 rev / min. The degummed silk was removed once the temperature dropped to 40 deg C. The degummed silk fibres were rinsed with warm water and then with cold water till all residual alkali could be removed and pH of the washed liquor turned to 7. Degummed silk fibres were dried in fume hood or in an oven at 80 deg C till dry and kept for future use.Example 2: Cutter Milling of degummed silk fibroin fibres

[0150] Degummed Bombyx mori silk fibres (BMSF) prepared using the procedure of example 1 were chopped with the help of a cutter mill (Pulverisette 19 from Fritsch GmbH, Germany) to produce silk snippets (SS). Fibres were cut repeatedly between five “V” shaped rotary blades (2888 rpm) fixed on a rotor and three stationary blades until they were small enough to pass through the grid / sieve. A grid of 4 mm was used for all the works. Since silk fibres have a small diameter of 10-20 pm so SS longer than 4 mm can also pass through the grids.Example 3: Alkali hydrolysis of silk fibres in combination with shear homogenising

[0151] 1 wt.% of 4 mm silk snippets cut using the procedure in example 2 were treated with 1 M sodium hydroxide at 25°C from 1 -2 hours along with shear mixing at 15000 rpm with a T 25 digital ULTRA-TURRAX shear mixer (IKA, Australia) with a rotor diameter of 18 mm. Few drops of Foamaster MO 2134 were used as an antifoam to prevent excessive foaming during homogenisation. After the treatment, neutralisation was carried out by using 0.5M HCI to stop hydrolysis and then centrifuged and washed to remove the residual NaCI salt at 7000g until the suspension reached a pH of 7.

[0152] This procedure outlined above was utilised to produce two production runs namely (1 ) B-1 M-1 : B. mori silk hydrolysed by 1 M NaOH for 1 hr and (2) B-1 M-2: B. mori silk hydrolysed by 1 M NaOH for 2 hr. The variable modified was the time of hydrolysis.Example 4: Acid hydrolysis of silk fibres

[0153] Acidic pre-treatment of 1 wt.% 4 mm silk snippets (prepared using the procedure in example 2) (10 gm snippets in 1000 mL acid solution) was carried at two different concentrations (15% and 30%) of H2SO4 for 30 min at various temperatures (20°and 40°) under continuous stirring. After the treatment, the reaction was stopped by diluting and mixing with icy water. Washing of the pre-treated silk samples was done by repeated centrifugation with distilled water at 7000g until a neutral pH of 7 was achieved.

[0154] This procedure was followed to produce three batches namely (1 ) 15HS-20: B. mori silk hydrolysed by 15 wt.% (2.8 M) H2SO4 at 20°C for 30 min (2) 15HS-40: B. mori s hydrolysed by 15 wt.% (2.8 M) H2SO4 at 40°C for 30 min and (3) 30HS-20: B. mori silk hydrolysed by 30 wt.% (5.6 M) H2SO4 at 20°C for 30 min. As can be seen there was a variation in hydrolysis temperature and acid concentration.Example 5: Acid hydrolysed silk with shear homogeniser

[0155] 1 wt.% (5 gm in 500 mL water) of acid hydrolysed silk fibres produced using the procedure in example 4 were then shear homogenised with a T 25 digital ULTRA-TURRAX shear mixer (IKA, Australia) with a rotor diameter of 18 mm at 15000 rpm for 30 minutes.Example 6: High-pressure homogenisation of shear homogenized alkali and acid hydrolysed silk

[0156] The sample produced using the procedures of examples 3 or 5 were then passed through a high-pressure homogeniser for the final shear-induced fibrillation. A high-pressure homogeniser (APV 1000, SPX Flow Technology) or a Panda Plus was used with 700 bar for the first pass and 1000 bar for the additional 4 passes.Example ?: Scanning Electron microscopy

[0157] A Zeiss Supra 55VP SEM Scanning Electron Microscopy was used to observe the morphological changes. Silk fibre suspensions were diluted to a concentration of 0.0001% w / w, and a drop of this diluted suspension was placed on a silicon wafer and dried overnight at room temperature. The stubs were gold-coated (thickness ~5 nm) with a Leica ACE600 sputter coater before imaging. Secondary electron detector mode was used to capture images at an accelerating voltage of 5 kV at different magnifications. An SEM mage of the degummed silk of example 1 is shown in figure 2. An SEM mage of the cut silk of example 2 is shown in figure 3. SEM images of two samples of the alkali hydrolysed and shear homogenised silk fibres of example 3 is shown in figure 4. SEM images of three samples of the acid hydrolysed and shear homogenised silk fibres of example 5 is shown in figures 5 and 6.

[0158] Alkali treatment (Fig 4) with NaOH initially swells fibres and helps in loosening the fibre structure. With the introduction of shear homogenisation in the system, these swollen fibres undergo spontaneous fibre splitting along the length without cutting the length significantly mostly within the first hour. After 1 hr, slight fibre shortening is evident.

[0159] Acid treatment (Fig. 5, 6) for only 30 minutes at room temperature and 40C also helped in fibre swelling and partial silk dissolution, which later helped in sufficient fibrillation when subjected to shear homogenisation. Shear homogenising following acid treatment assisted in producing finer fibrils due to the weak interaction between fibrils affected by hydrolysis.Example 8: Optical microscopy

[0160] Morphology and length distribution of silk snippets and after homogenisation were observed with the help of an optical microscope (Olympus DP71 , Japan). Magnifications of 10x and 20x were used by placing a drop of a suspension of very low concentration on a glass slide.Example 9: Determination of fibre and nanofibril size distribution from microscopy

[0161] The images obtained from SEM were analysed for fibre dimension with Image J software. Homogenized fibre width was only measured from images, as the length was virtually impossible to measure due to entanglement. Approximately 100 measurements across the fibril width were taken from each image and plotted to determine the average fibre width.

[0162] 1 M NaOH, treated for 60 min at 25°C (Example 3)

[0163] 1 M NaOH, treated for 120 min at 25°C and simultaneously homogenized(Example 3)

[0164] 15% H2SO4, treated for 30 min at 20°C and subsequently homogenized(Example 5)

[0165] 15% H2SO4, treated for 30 min at 40°C and subsequently homogenized(Example 5)

[0166] 30% H2SO4, treated for 30 min at 20°C and subsequently homogenized (Example 5)

[0167] A bar graph graphical representation of the data is given in figures 7 to 11 and in line graph format in figures 12 and 13.

[0168] 15% H2SO4, treated for 60 min at 40°C subsequently homogenized and then processed by high pressure homogenizer 5 passes (Example 6)

[0169] 15% H2SO4, treated for 120 min at 40°C subsequently homogenized and then processed by high pressure homogenizer, 5 passes (Example 6)

[0170] A line graph representation of this data is shown in figure 14.Example 10: Weight loss analysis of hydrolysed silk

[0171] Weight loss of acid pre-treated silk and shear mixed alkali-hydrolysed silk samples were determined to observe the effect of each treatment on silk and is represented by the amount of silk dissolved while carrying out alkali and acid hydrolysis at different temperatures and conditions. It is calculated from the weight of silk before and after treatments. After alkali (with shear homogenisation) and acid treatment, the samples were centrifuged, washed, and dried overnight at 65°C before taking the final weight.

[0172] Weight loss can be calculated by the following: weiqht of treated silkWeight loss (%) = (1 - — - — - - — — weight of degummed silk

[0173] The results are shown in figure 15. As can be seen alkali assisted shear homogenising with 1 M NaOH did not show significant weight loss over time. When sulfuric acid of lower concentration (15wt.%) was used then weight loss was not prominent and there was less dissolved silk. The weight loss at 30wt.% H2SO4 at 20°C was more or less stable but higher than 15 wt.% at the same temperature. Hydrolysis intensity increased with the increase in temperature and concentration.Example 11 : Chemical structure based on FTIR

[0174] The Fourier transform infrared (FTIR) spectra of degummed silk and treated silk samples was performed by Bruker Vertex 70 spectrometer by Attenuated Total Reflectance (ATR) technique using a scanning resolution of 4 cm-1and 32 scans per sample. Each sample was scanned within a wavelength range of 600 to 4000 cm13 times, and the spectrums were baseline corrected and smoothed with Opus 5.5 software. The results are shown in Figures 16 and 17. The control and silk nanofibres showed characteristic peaks at 1624 cm’1, 1520 cm’1and 1260 cm’1corresponding to amide I, amide II, and amide III respectively of silk II structure. These peaks confirmed the presence of the [3-sheet structure. The absorption peak in amide I is due to the C- O stretching. The silk structure after acid, alkali treatment and shear mixing preserved the [3-sheet structures which were indicated by the presence of strong peaks between 1620-1630 cm-1 . So, these treatments did not change the secondary structure.Example 12: Differential scanning calorimetry

[0175] Differential scanning calorimetry of freeze-dried SNFs was carried out by DSC Q200 (TA Instruments, USA). 6-7mg of samples were placed in an aluminium pan, and a similar empty pan was taken as the reference. Heating was done from room temperature to 350°C at a rate of 10°C / min at 50mL / min nitrogen atmosphere.Example 13: Emulsion formation- Oil In water Formulation

[0176] A silk fibre suspension from example 3 (69.5 parts water 0.5 parts silk) was used to form Oil-in-water (O / W) Pickering emulsion with 30 parts oil. The following mass fraction was used for formation of emulsion.• Silk: 0.5 parts• Oil: Caprylic / Capric Triglyceride: (30 parts)• Water: 69.5

[0017] The mixture was subjected to sonication and an SEM image of the resultant emulsion is shown in figure 18.Example 14: Oil Droplet Size distribution of an emulsion

[0178] A Malvern Instruments Mastersizer 3000, which is a laser diffraction based particle size analyser, was used to measure droplet size of oil in O / W emulsion for a variety of emulsions produced using the procedure of example 13 with variations in the amount of silk. The amount of oil was kept constant at 30% and as the silk was increased the water was decreased such that the amount of silk plus water was 70wt%. The Hydro MV unit was used for the controlled, automated wet dispersion of samples. The dispersion medium was DI water. Two drops of 5% Nonidet P-40 was used to facilitate dispersion. Refractive index of 1.450 and absorbance of 0.001 were used for oil phase as this is required to measure droplet size. After the emulsion drops were put into the MV unit, 30 second was allowed once obscuration was achieved followed by stirring at 1500 RPM for 2 min for stabilization. 10 measurements were made and average readings were taken. The gradual change of readings over 10 measurementswas also used to indicate the stability of the emulsion droplet. The results are shown in the tables below.

[0179] Acid pre-treated silk

[0180] For silk produced by shear homogenized silk

[0181] For silk produced by Shear Homogenization followed by high pressure homogenization 5 passExample 15: Rheology of Emulsions

[0182] The rheological measurements of emulsion samples were evaluated byDiscovery HR-3 Rheometer (TA instruments) with a 40mm / 2° cone to parallel geometry and a Peltier plate with a fixed gap of 49pm. To determine storage modulus (G’) and loss modulus (G”), the frequency sweep of the suspensions was carried out at 25°c and 0.01<co<100 rad / s with 0.1 % strain. The shear thinning behaviours of an emulsion of the invention is shown in figures 19 and 20.

[0183] The subject headings used herein are included only for the ease of reference of the reader and should not be used to limit the subject matter found throughout thedisclosure or the claims. The subject headings should not be used in construing the scope of the claims or the claim limitations.

[0184] The description provided herein is in relation to several embodiments which may share common characteristics and features. It is to be understood that one or more features of one embodiment may be combinable with one or more features of the other embodiments. In addition, a single feature or combination of features of the embodiments may constitute additional embodiments.

[0185] All methods described herein can be performed in any suitable order unless indicated otherwise herein or clearly contradicted by context. The use of any and all examples, or exemplary language (e.g., "such as") provided herein, is intended merely to better illuminate the example embodiments and does not pose a limitation on the scope of the claimed invention unless otherwise claimed. No language in the specification should be construed as indicating any non-claimed element as essential.

[0186] It will be apparent to the person skilled in the art that while the invention has been described in some detail for the purposes of clarity and understanding, various modifications and alterations to the embodiments and methods described herein may be made without departing from the scope of the inventive concept disclosed in this specification.

[0187] Those skilled in the art will appreciate that the invention described herein is susceptible to variations and modifications other than those specifically described. It is to be understood that the invention includes all such variations and modifications. The invention also includes all of the steps, features, compositions and compounds referred to, or indicated in this specification, individually or collectively, and any and all combinations of any two or more of the steps or features.

[0188] Future patent applications may be filed in Australia or overseas on the basis of the present application, for example by claiming priority from the present application, by claiming a divisional status and / or by claiming a continuation status. It is to be understood that the following provisional claims are provided by way of example only and are not intended to limit the scope of what may be claimed in any such future application. Furthermore, the claims should not be considered to limit the understandingof (or exclude other understandings of) the invention inherent in the present disclosure. Features may be added to or omitted from the provisional claims at a later date, so as to further define the invention.

Claims

Claims:1 . An aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm.

2. An aqueous suspension according to claim 1 wherein 90% of the fibres have an aspect ratio of at least 50.

3. An aqueous suspension according to claim 1 or 2 wherein 90% of the fibres have an aspect ratio of at least 60.

4. An aqueous suspension according to any one of claims 1 to 3 wherein the average width of the fibres is between 100 nm and 500 nm.

5. An aqueous suspension according to any one of claims 1 to 4 wherein the average width of the fibres is between 100 nm and 300 nm.

6. An aqueous suspension according to any one of claims 1 to 5 wherein the average width of the fibres is between 100 nm and 200 nm.

7. An aqueous suspension according to any one of claims 1 to 6 wherein the silk fibroin fibres are present in the aqueous suspension at from 0.5% to 5% w / w based on the total weight of the aqueous suspension.

8. A method of producing an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm, the method comprising:(i) providing degummed silk fibroin fibres,(ii) cutting the degummed silk fibroin fibres to form cut silk fibroin fibres that will pass through a 5 mm grid;(iii) partial hydrolysis of the silk fibroin fibres to form partially hydrolysed silk fibroin fibres, and(iv) shear homogenisation of the hydrolysed silk fibroin fibres; wherein steps (iii) and (iv) may be carried out sequentially or simultaneously.

9. A method according to claim 8 wherein step (i) comprises heating raw silk in an alkali solution at a temperature of from 80°C to 120°C.

10. A method according to claim 8 or claim 9 wherein the heating is carried out for a period of from 30 to 90 minutes.

11. A method according to any one of claim 9 to 10 wherein the alkali solution is a sodium carbonate solution.

12. A method according to claim 11 wherein in step (i) the alkali solution is at a concentration of from 0.5g / L to 3g / L.

13. A method according to any one of claims 8 to 12 wherein in step (ii) cutting the degummed silk fibroin fibres comprises passing the fibres through a fibre cutting machine or a cutter mill to form cut silk fibroin fibres.

14. A method according to any one of claims 8 to 13 wherein the cut silk fibres will pass through a 1 mm to 3 mm grid.

15. A method according to claim 13 to 14 wherein the cut silk fibroin fibres will pass through a 2 mm grid.

16. A method according to any one of claims 8 to 15 wherein hydrolysis of the silk fibroin fibres comprises subjecting the silk fibroin fibres to acid or alkali treatment to form hydrolysed silk fibroin fibres.

17. A method according to any one of claims 8 to 16 wherein step (III) comprises treating the cut silk fibroin fibres with alkali.

18. A method according to any one of claims 8 to 16 wherein step (III) comprises treating the cut silk fibroin fibres with acid.

19. A method according to claim 17 wherein the fibres are simultaneously subjected to shear mixing.

20. A method of producing an emulsion the method comprising:(a) providing an aqueous suspension containing silk fibroin fibres wherein at least 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm;(b) adding a water immiscible component to the aqueous suspension to form a mixture;(c) subjecting the mixture to high shear form an emulsion.21 . A method according to claim 20 wherein 90% of the fibres have an aspect ratio of at least 50.

22. A method according to claim 20 or 21 wherein 90% of the fibres have an aspect ratio of at least 60.

23. A method according according to any one of claims 20 to 22 wherein the average width of the fibres is less than 500 nm.

24. A method according to any one of claims 20 to 23 wherein the average width of the fibres is less than 300 nm.

25. A method according to any one of claims 20 to 24 wherein the silk fibroin fibres are present in the aqueous suspension at from 0.5% to 5% w / w based on the total weight of the aqueous suspension.

26. A method according to any one of claims 20 to 25 wherein the water immiscible component is an oil or organic solvent.

27. A method according to any one of claims 20 to 26 wherein the water immiscible component is an oil.

28. A method according to any one of claims 20 to 27 wherein the emulsion comprises:(a) from 0.1 to 4% w / w of silk fibroin fibres; wherein 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm(b) from 9.9 to 90% w / w water; and(c) from 9.9 to 90 %w / w of the water immiscible component29. A method according to any one of claims 20 to 28 wherein step (c) comprises sonication.

30. A method according to claim 29 wherein the sonication is at a frequency of from 20kHz to 200kHz.31 . A method according to claim 29 or 30 wherein the sonication is carried out for a period of from 1 second to 600 seconds.

32. A method according to any one of claims 20 to 31 wherein 90% of the droplets in the emulsion are less than 100 .M.

33. A method according to any one of claims 20 to 32 wherein 90% of the droplets in the emulsion are less than 60 |iM.

34. A formulation in the form of an emulsion comprising (a) silk fibroin fibres wherein 90% of the fibres having an aspect ratio of at least 40 and further wherein the average width of the fibres is between 100 nm and 1000 nm; (b) water (c) a water immiscible component and (d) one or more active ingredients.

35. A formulation according to claim 34 wherein 90% of the fibres have an aspect ratio of at least 40.

36. A formulation according to claim 34 or 35 wherein 90% of the fibres have an aspect ratio of at least 50.

37. A formulation according according to any one of claims 34 to 36 wherein the average width of the fibres is less than 500 nm.

38. A formulation according to any one of claims 35 to 37 wherein the average width of the fibres is less than 300 nm.

39. A formulation according to any one of claims 34 to 38 wherein the formulation comprises from 0.1 to 4%w / w of silk fibroin fibres.

40. A formulation according to any one of claims 34 to 39 wherein the formulation comprises from 0.5 to 1 .2% w / w of silk fibroin fibres.41 . A formulation according to any one of claims 34 to 40 wherein the formulation comprises from 10 to 70% w / w of a water immiscible component.

42. A formulation according to any one of claims 34 to 41 wherein the formulation comprises from 20 to 40% w / w of a water immiscible component.

43. A formulation according to any one of claims 34 to 42 wherein the formulation comprises from 25 to 35% w / w of a water immiscible component.

44. A formulation according to any one of claims 34 to 43 wherein the formulation comprises from 29.9 to 90% w / w of water.

45. A formulation according to any one of claims 34 to 44 wherein the formulation comprises from 55 to 80% w / w of water.

46. A formulation according to any one of claims 34 to 45 wherein the formulation comprises from 65 to 75% w / w of water.

47. A formulation according to any one of claims 34 to 46 wherein 90% of the droplets in the emulsion are less than 100 |iM.

48. A formulation according to any one of claims 34 to 47 wherein 90% of the droplets in the emulsion are less than 60 |iM.

49. A formulation according to any one of claims 34 to 48 wherein the formulation has a viscosity of at least 1000 Pa s.

50. A formulation according to any one of claims 34 to 49 wherein the formulation has a viscosity of at least 2000 Pa s.

Citation Information

Patent Citations

  • Controllable preparation method of fibroin micro-nano fibers

    CN110257942A

  • Modified tussah silk fibroin 3D printing support and preparation method thereof

    CN110859994A