Method for selectively extracting lithium from sedimentary lithium-deficient clay, and use thereof

Through the roasting method without the addition of complex sulfate, the calcium source of the sedimentary lithium-poor clay is used to achieve efficient and selective extraction of lithium, which solves the problems of large tons of lithium slag and large consumption of complex sulfate in the existing technology, and reduces the The cost of chemicals and slag rate are reduced, and the lithium grade and leaching rate are improved.

WO2024216537A1PCT designated stage expired Publication Date: 2024-10-24GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
PCT/CN2023/089221
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

When extracting lithium from sedimentary lithium-poor clay, the existing technology has problems such as a large amount of lithium slag per ton, high consumption of composite sulfate/sulfuric acid, high roasting temperature and difficulty in industrial application. It is difficult to meet the lithium resource demand of the power battery industry. .

Method used

Adopting a roasting method without the addition of complex sulfates, through the steps of crushing, screening, sorting, roasting and leaching, the calcium source of the ore itself is fully utilized, the amount of materials entering the smelting is reduced, the lithium grade is improved, and concentrated sulfuric acid and secondary roasting are used to generate Calcium sulfate performs selective leaching of lithium.

Benefits of technology

Efficient and selective extraction of lithium is achieved, with a Li leaching rate >80%, almost no Ca and Al leaching, a slag rate <60%, low chemical cost, and a process that is energy-saving and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023089221_24102024_PF_FP_ABST
    Figure CN2023089221_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a method for selectively extracting lithium from sedimentary lithium-deficient clay, and a use thereof. The method comprises the following steps: 1) crushing and sieving sedimentary lithium-deficient clay minerals ore to obtain oversize products, undersize products, and intermediate size products; 2) sorting the oversize products to obtain calcite and gangue; 3) performing ore blending on the undersize products, the intermediate size products and part of calcite to obtain a feed product, wherein the mass of said part of calcite in step 3) accounts for 7-18% of the mass of calcite in step 2); 4) roasting the feed product to obtain calcine; and 5) leaching the calcine to obtain a lithium-rich leachate and residues. According to the present disclosure, while selective lithium extraction from sedimentary lithium-deficient clay is achieved, calcium sources of the minerals are fully utilized, and no composite sulfate is added as a roasting additive, thereby reducing the agent cost and the residue rate, effectively reducing the amount of feed materials for smelting, and improving the lithium grade of the feed materials.
Need to check novelty before this filing date? Find Prior Art

Description

A method for selectively extracting lithium from sedimentary lithium-deficient clay and its application Technical Field

[0001] The present disclosure belongs to the technical field of lithium extraction from lithium ores, for example, a method for selectively extracting lithium from sedimentary lithium-deficient clay and its application. Background Art

[0002] Thanks to the country's strong support for the new energy industry, the power battery industry has developed rapidly, leading to a rapid expansion in lithium demand. Currently, my country's main lithium resources include spodumene (Xinjiang and Sichuan), lepidolite (Jiangxi), lithium salt lakes (Qinghai and Tibet), and lithium clay (Guizhou and Yunnan). Currently, spodumene, lepidolite, and lithium salt lakes have industrialized, but lithium resources still cannot meet the needs of the power battery industry. Therefore, lithium clay has gradually attracted the attention of domestic researchers.

[0003] Currently, lithium clays are typically directly extracted using hydrometallurgical methods. After leaching, impurity removal and purification, lithium precipitation, and refining, battery-grade lithium carbonate is obtained. Hydrometallurgical methods are suitable for lithium clays with high Li₂O₃ content (≥0.8%). However, for lithium-poor clays, problems such as large lithium slag production per ton and high consumption of composite sulfate / sulfuric acid are encountered. Therefore, direct acid leaching (low-temperature sulfation roasting followed by water leaching) is currently used for sedimentary lithium-poor clays. For example, CN114892024A discloses a method for extracting lithium from lithium-containing clays by low-temperature roasting. The method comprises the following steps: 1. Mixing an acid with the lithium-containing clay and then low-temperature roasting the mixture to obtain a roasted product; 2. Cooling the roasted product and then adding deionized water for water leaching to obtain a mixed solution; and 3. Filtering the mixed solution obtained in step 2 to obtain a filtrate. This technology has the advantages of low energy consumption and saving auxiliary agents, but the acid addition is more than 50% (mass fraction of the ore deposit), and the acid consumption is still high; Or take the composite salt replacement process, for example CN115350806A has adopted the method for composite sulfate roasting-water leaching that adds calcium carbonate, sodium sulfate and potassium sulfate, and makes lithium-rich leachate through grinding-balling-roasting-water leaching, has the advantages that process is simple, cost is low, leachate impurity content is low and lithium leaching rate is high, but there is that the sulfate addition is large, potassium sulfate unit consumption cost is high, roasting temperature is high etc. deficiencies; Or take the technology of microwave roasting, for example CN114959253A adopts the technology of pretreatment-microwave roasting-water leaching, has the advantages such as heating-up time is short, roasting temperature is low, leaching agent is cheap, leaching rate is high, but industrial microwave roasting practice is less, and industrialization may have problems.

[0004] Therefore, it is necessary to propose a method for selective lithium extraction from lithium-deficient clay, reduce the amount of materials fed into the smelting, improve the lithium grade of the feed, and achieve selective lithium leaching under the condition of low acid or composite salt usage.

[0005] Summary of the Invention

[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0007] To address the shortcomings of the prior art, the present invention aims to provide a method for selectively extracting lithium from sedimentary lithium-deficient clay and its application. This method selectively extracts lithium from sedimentary lithium-deficient clay while fully utilizing the ore's own calcium source. It eliminates the need for the addition of composite sulfates as roasting additives, resulting in a low reagent cost ratio and a low slag rate. This method effectively reduces the amount of material fed to the smelter and improves the lithium grade of the input material.

[0008] To achieve this goal, the present disclosure adopts the following technical solutions:

[0009] In a first aspect, an embodiment of the present disclosure provides a method for selectively extracting lithium from sedimentary lithium-deficient clay, the method comprising the following steps:

[0010] (1) crushing and screening the sedimentary lithium-poor clay ore to obtain an oversize product, an undersize product and an intermediate particle size product;

[0011] (2) sorting the above-screen product to obtain calcite and gangue;

[0012] (3) blending the undersize product, the intermediate size product, and the calcite to obtain a feed product;

[0013] wherein the mass of the portion of calcite in step (3) accounts for 7-18% of the mass of the calcite in step (2);

[0014] (4) roasting the input product to obtain calcine;

[0015] (5) Leaching the roasted sand to obtain lithium-rich leachate and leach residue.

[0016] The embodiments of the present disclosure provide a method for selective lithium extraction. While achieving selective lithium extraction from sedimentary lithium-deficient clay, the method fully utilizes the ore's own calcium source, does not require the addition of composite sulfate as a roasting additive, has a low reagent cost ratio, a low slag rate, effectively reduces the amount of material fed into the smelter, and improves the lithium grade of the feed.

[0017] In the lithium-rich leachate obtained by the method provided in the embodiment of the present disclosure, the Li leaching rate is >80%, Ca and Al are almost not leached, the leaching rates of Ca and Al are both less than 3%, and the slag rate is <60% (for feed quality), where the feed quality refers to the quality of sedimentary lithium-poor clay ore.

[0018] In one embodiment, the mass of the portion of calcite in step (3) is 7-18% of the mass of the calcite in step (2), for example, it can be 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17% or 18%, etc.

[0019] In the embodiment of the present disclosure, part of the calcite is used to blend with the undersize product and the intermediate particle size product to adjust the calcium content of the smelting material to an appropriate range, so as to generate an appropriate amount of Li + The exchange agent lays a solid foundation. If the mass of calcite used in the ore blending process in step (3) is too much, the calcium content of the smelting material will be too high, which will have little effect on improving the lithium leaching rate and will increase the slag rate. If the mass of calcite used in the ore blending process in step (3) is too little, the calcium content of the smelting material will be too low, which is not conducive to lithium leaching.

[0020] The embodiment of the present disclosure does not limit the screening method of step (1). For example, the screening may be performed using a wet multi-layer vibrating screen.

[0021] In one embodiment, the particle size of the above-sieve product in step (1) is greater than 5 mm and less than 100 mm, for example, it can be 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm or 50 mm.

[0022] In one embodiment, the particle size of the intermediate-grade product in step (1) is in the range of 2-5 mm, for example, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm or 5 mm.

[0023] In one embodiment, the particle size of the undersize product in step (1) is less than 2 mm, for example, it can be 1.5 mm, 1 mm, 0.5 mm or 0.1 mm.

[0024] The embodiments of the present disclosure do not specifically limit the sorting method, and those skilled in the art may select it according to their needs.

[0025] In one embodiment, the sorting in step (2) includes photoelectric sorting.

[0026] It should be noted that photoelectric sorting refers to the use of differences in the optical, magnetic, and conductive properties of the incoming materials to perform sorting. Photoelectric sorting is performed on the screened product on a conveyor belt, using X-rays and images to identify the ore structure, which is then compared with a database to identify calcite. Finally, high-pressure gas is injected into the calcite (or non-calcite ore) at the end of the belt, changing its trajectory and separating the calcite from the non-calcite.

[0027] Calcite with high purity can be separated through sorting, which can be used as a source of lithium and calcium for subsequent extraction, or used as a primary refractory material after simple processing. The gangue obtained through sorting can be used as general building materials.

[0028] In one embodiment, the undersize product in step (3) is first subjected to sedimentation and concentration before being mixed with the intermediate size product and calcite.

[0029] In the disclosed embodiment, the purpose of sedimentation and concentration of the undersize product is to increase the material concentration, which is beneficial to the subsequent grinding operation.

[0030] In one embodiment, the calcite in step (3) is first crushed to a particle size of less than 15 mm before ore blending, for example, it can be 12 mm, 10 mm, 8 mm, 6 mm, 4 mm or 2 mm.

[0031] In one embodiment, after the ore blending in step (3), the ore is ground so that particles with a particle size less than 0.074 mm account for 70-90% of the total number of particles, for example, 70%, 75%, 80%, 85% or 90%.

[0032] In one embodiment, based on the mass of the feed product in step (3), the Ca content in the feed product is 10-15 wt.%, for example, 10 wt.%, 11 wt.%, 12 wt.%, 13 wt.%, 14 wt.% or 15 wt.%.

[0033] In the embodiment of the present disclosure, if the content of Ca is too low, it will be detrimental to lithium leaching; if the content of Ca is too high, it will result in an excessive amount of slag.

[0034] In one embodiment, the roasting in step (4) includes one-stage roasting and two-stage roasting.

[0035] In one embodiment, the specific steps of the first stage roasting include: mixing the feed product with concentrated sulfuric acid, and performing aging roasting to obtain roasted sand I and CO2.

[0036] In the disclosed embodiment, the feed product is mixed with concentrated sulfuric acid. The calcite in the feed product reacts with the added concentrated sulfuric acid to produce calcium sulfate. The calcium sulfate-containing calcine is then subjected to a subsequent secondary roasting step. The CO₂ is absorbed by water to produce a weak acid solution, which can be recycled for lithium leaching.

[0037] In one embodiment, the mixing process is accompanied by stirring.

[0038] In one embodiment, the mass fraction of the concentrated sulfuric acid is 70-80%, for example, 70%, 72%, 74%, 76%, 78% or 80%.

[0039] In one embodiment, based on the mass of the feed product in step (3), the amount of concentrated sulfuric acid used is 15-35 wt.%, for example, it can be 15 wt.%, 18 wt.%, 21 wt.%, 24 wt.%, 27 wt.%, 30 wt.%, 31 wt.%, 32 wt.%, 33 wt.%, 34 wt.% or 35 wt.%, etc.

[0040] In the embodiment of the present disclosure, if the amount of concentrated sulfuric acid used is too little, it is not conducive to the generation of sufficient calcium sulfate and is not conducive to the leaching of lithium; if the amount of concentrated sulfuric acid used is too much, it is easy to react with gangue minerals, resulting in the leaching of other impurity ions, which is not conducive to the purification of the lithium-rich leachate.

[0041] In one embodiment, the temperature of the first stage roasting is 150-280°C, for example, 150°C, 170°C, 190°C, 210°C, 220°C, 240°C, 260°C or 280°C.

[0042] In one embodiment, the calcination time is 0.5-4 hours, for example, 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours or 4 hours.

[0043] In one embodiment, the specific steps of the two-stage roasting include: roasting the roasted sand I in two stages to obtain roasted sand II and acid gas.

[0044] In the disclosed embodiments, during the second-stage roasting process, calcium sulfate, acting as an exchange agent, reacts with the lithium in the lithium clay to form Li₂SO₄, which in turn leaches the lithium. Furthermore, the acid gas is absorbed by water to form a sulfuric acid solution. When the concentration reaches 70-80%, it can be recycled back to the first-stage roasting process, resulting in an energy-efficient and environmentally friendly process.

[0045] In one embodiment, the temperature of the second stage calcination is 350-750°C, for example, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C or 750°C.

[0046] In one embodiment, the second-stage calcination time is 0.5-4 hours, for example, 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours or 4 hours.

[0047] In one embodiment, during the leaching process in step (5), the leaching agent used includes a weak acid solution.

[0048] In one embodiment, the weak acid solution comprises a carbonic acid solution.

[0049] In one embodiment, the solute in the carbonic acid solution is derived from CO2 generated during the first stage roasting process.

[0050] In the disclosed embodiment, the CO2 generated during the first stage roasting process can be recycled, which saves costs and makes the process energy-saving and environmentally friendly.

[0051] In one embodiment, the leaching method in step (5) includes three-stage countercurrent leaching.

[0052] In one embodiment, during the three-stage countercurrent leaching process, the mass ratio of the calcined sand to the leaching agent is 1:(3-6), for example, it can be 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 or 1:6.

[0053] It should be noted that the mass ratio of the roasted sand to the leaching agent refers to the ratio of the mass of the roasted sand to the mass of the leaching agent.

[0054] In one embodiment, during the three-stage countercurrent leaching process, the pH of the slurry during leaching is 3-4, for example, it can be 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9 or 4.

[0055] As a preferred technical solution, the method comprises the following steps:

[0056] (1) crushing and screening the sedimentary lithium-poor clay ore to obtain an oversize product, an undersize product and an intermediate particle size product;

[0057] Among them, the particle size of the oversize product is greater than 5mm and less than 100mm, the particle size of the intermediate particle size product is in the range of 2-5mm, and the particle size of the undersize product is less than 2mm;

[0058] (2) performing photoelectric separation on the oversize product of step (1) to obtain calcite and gangue;

[0059] (3) sedimenting and concentrating the undersize product of step (1), and then mixing it with the intermediate-size product of step (1) and the crushed calcite with a particle size of less than 15 mm, blending the ore, and then grinding the ore so that particles with a particle size of less than 0.074 mm account for 70-90% of the total number of particles, to obtain a feed product with a Ca content of 10-15 wt.%;

[0060] wherein the mass of the calcite with a crushed particle size of less than 15 mm accounts for 7-18% of the mass of the calcite in step (2);

[0061] (4) mixing the feed product of step (3) with concentrated sulfuric acid having a mass concentration of 70-80% and stirring, and calcining at 150-280° C. for 0.5-4 h to obtain calcine I and CO2;

[0062] Wherein, based on the mass of the feed product in step (3), the amount of concentrated sulfuric acid used is 15-35wt.%;

[0063] (5) calcining the calcined sand I in step (4) in two stages at 350-750° C. for 0.5-4 h to obtain calcined sand II and acid gas;

[0064] (6) mixing the roasted sand II described in step (5) with a weak acid solution, and performing three-stage countercurrent leaching to obtain a lithium-rich leachate and a leach residue;

[0065] The mass ratio of roasted sand II to weak acid solution is 1:(3-6).

[0066] In a second aspect, an embodiment of the present disclosure provides an application of the method for selectively extracting lithium from sedimentary lithium-deficient clay as described in the first aspect, wherein the method is applied to the selective extraction of lithium from low-grade lithium clay.

[0067] The numerical range described in the present disclosure includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present disclosure no longer exhaustively lists the specific point values ​​included in the range.

[0068] Compared with the prior art, the present disclosure has the following beneficial effects:

[0069] (1) The present disclosure provides a method for selective lithium extraction, which not only realizes the selective extraction of lithium from sedimentary lithium-deficient clay, but also makes full use of the calcium source of the ore itself, does not require the addition of composite sulfate as a roasting additive, has a low reagent cost ratio, a low slag rate, effectively reduces the amount of material fed into the smelting, and improves the lithium grade of the feed.

[0070] (2) In the lithium-rich leachate obtained by the method provided by the present disclosure, the Li leaching rate is >80%, Ca and Al are almost not leached, their leaching rate is <3%, and the slag rate is <60% (relative to the feed mass).

[0071] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of the present disclosure, they are used to explain the technical solution of this article and do not constitute a limitation to the technical solution of this article.

[0073] FIG1 is a process flow chart of selective lithium extraction from sedimentary lithium-deficient clay according to Example 1 of the present disclosure. DETAILED DESCRIPTION

[0074] The technical solution of the present disclosure is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present disclosure and should not be regarded as specific limitations of the present disclosure.

[0075] Example 1

[0076] The sedimentary lithium-deficient clay treated in this embodiment includes 0.52% Li2O, 14.73% Ca and 7.55% Al.

[0077] This embodiment provides a method for selectively extracting lithium from sedimentary lithium-deficient clay. FIG1 shows a process flow chart thereof. The method comprises the following steps:

[0078] (1) crushing the sedimentary lithium-poor clay ore so that the particle size of the crushed product is less than 100 mm, and then screening it with a wet multi-layer vibrating screen to obtain an oversize product, an undersize product and an intermediate particle size product;

[0079] Among them, the particle size of the oversize product is greater than 5mm and less than 100mm, the particle size of the intermediate particle size product is in the range of 2-5mm, and the particle size of the undersize product is less than 2mm;

[0080] (2) performing photoelectric separation on the above-screen product to obtain calcite and gangue;

[0081] (3) the undersize product is sedimented and concentrated, and then mixed with the intermediate particle size product and calcite crushed to a particle size of less than 15 mm, blended, and then ground so that particles with a particle size of less than 0.074 mm account for 70% of the total number of particles, to obtain a feed product with a Ca content of 10.04 wt.%;

[0082] The calcite with a particle size of less than 15 mm accounts for 7.85% of the mass of the calcite in step (2), and the remaining calcite is used as a primary refractory material after simple processing;

[0083] (4) mixing the feed product with concentrated sulfuric acid having a mass concentration of 80% and stirring, stirring evenly, and then calcining at 280° C. for 1 h to obtain calcine I and CO2;

[0084] Wherein, based on the mass of the feed product in step (3), the amount of concentrated sulfuric acid used is 15wt.%;

[0085] (5) The roasted sand I is subjected to a second-stage roasting at 750° C. for 0.5 h to obtain roasted sand II and acid gas. The acid gas is absorbed by water to generate a sulfuric acid solution, which can be reused in the first roasting step when the concentration reaches 80%;

[0086] (6) mixing the roasted sand II and the carbonate solution, and performing three-stage countercurrent leaching, wherein the pH of the slurry during leaching is 3.9, to obtain a lithium-rich leachate and a leach residue;

[0087] The mass ratio of the roasted sand II to the carbonate solution is 1:6, and the solute in the carbonate solution comes from the CO2 described in step (4).

[0088] Example 2

[0089] The sedimentary lithium-deficient clay treated in this embodiment includes 0.52% Li2O, 14.73% Ca and 7.55% Al.

[0090] This embodiment provides a method for selectively extracting lithium from sedimentary lithium-deficient clay, the method comprising the following steps:

[0091] (1) crushing the sedimentary lithium-poor clay ore so that the particle size of the crushed product is less than 100 mm, and then screening it with a wet multi-layer vibrating screen to obtain an oversize product, an undersize product and an intermediate particle size product;

[0092] Among them, the particle size of the oversize product is greater than 5mm and less than 100mm, the particle size of the intermediate particle size product is in the range of 2-5mm, and the particle size of the undersize product is less than 2mm;

[0093] (2) performing photoelectric separation on the above-screen product to obtain calcite and gangue;

[0094] (3) the undersize product is sedimented and concentrated, and then mixed with the intermediate particle size product and calcite crushed to a particle size of less than 15 mm, blended, and then ground so that particles with a particle size of less than 0.074 mm account for 80% of the total number of particles, to obtain a feed product with a Ca content of 12.5 wt.%;

[0095] The calcite with a particle size of less than 15 mm accounts for 12.25% of the mass of the calcite in step (2), and the remaining calcite is used as a primary refractory material after simple processing;

[0096] (4) mixing the feed product with concentrated sulfuric acid having a mass concentration of 75% and stirring, stirring evenly, and then calcining at 230° C. for 1.5 h to obtain calcine I and CO2;

[0097] Wherein, based on the mass of the feed product in step (3), the amount of concentrated sulfuric acid used is 25wt.%;

[0098] (5) The roasted sand I is subjected to a second-stage roasting at 600° C. for 2.5 hours to obtain roasted sand II and acid gas. The acid gas is absorbed by water to generate a sulfuric acid solution, which can be reused in the first roasting step when the concentration reaches 75%;

[0099] (6) mixing the roasted sand II and the carbonate solution, and performing three-stage countercurrent leaching, wherein the pH of the slurry during leaching is 3.5, to obtain a lithium-rich leachate and a leach residue;

[0100] The mass ratio of the roasted sand II to the carbonate solution is 1:4, and the solute in the carbonate solution comes from the CO2 described in step (4).

[0101] Example 3

[0102] The sedimentary lithium-deficient clay treated in this embodiment includes 0.52% Li2O, 14.73% Ca and 7.55% Al.

[0103] This embodiment provides a method for selectively extracting lithium from sedimentary lithium-deficient clay, the method comprising the following steps:

[0104] (1) crushing the sedimentary lithium-poor clay ore so that the particle size of the crushed product is less than 100 mm, and then screening it with a wet multi-layer vibrating screen to obtain an oversize product, an undersize product and an intermediate particle size product;

[0105] Among them, the particle size of the oversize product is greater than 5mm and less than 100mm, the particle size of the intermediate particle size product is in the range of 2-5mm, and the particle size of the undersize product is less than 2mm;

[0106] (2) performing photoelectric separation on the above-screen product to obtain calcite and gangue;

[0107] (3) the undersize product is sedimented and concentrated, and then mixed with the intermediate particle size product and calcite crushed to a particle size of less than 15 mm, blended, and then ground so that particles with a particle size of less than 0.074 mm account for 90% of the total number of particles, to obtain a feed product with a Ca content of 14.99 wt.%;

[0108] The calcite with a particle size of less than 15 mm accounts for 17.85% of the mass of the calcite in step (2), and the remaining calcite is used as a primary refractory material after simple processing;

[0109] (4) mixing the feed product with concentrated sulfuric acid having a mass concentration of 80% and stirring, stirring evenly, and then calcining at 150° C. for 4 h to obtain calcine I and CO2;

[0110] Wherein, based on the mass of the feed product in step (3), the amount of concentrated sulfuric acid used is 35wt.%;

[0111] (5) The roasted sand I is subjected to a second-stage roasting at 350° C. for 4 hours to obtain roasted sand II and acid gas. The acid gas is absorbed by water to generate a sulfuric acid solution, which can be reused in the first roasting step when the concentration reaches 80%;

[0112] (6) mixing the roasted sand II and the carbonate solution, and performing three-stage countercurrent leaching, wherein the pH of the slurry during leaching is 3, to obtain a lithium-rich leachate and a leach residue;

[0113] The mass ratio of the roasted sand II to the carbonate solution is 1:3, and the solute in the carbonate solution comes from the CO2 described in step (4).

[0114] Example 4

[0115] The difference between this embodiment and embodiment 3 is that the undersize product in step (3) is not subjected to sedimentation and concentration.

[0116] The rest of the preparation methods and parameters remained the same as in Example 3.

[0117] Example 5

[0118] The difference between this embodiment and embodiment 3 is that the calcite in step (3) is not crushed before being mixed with the undersize product and the intermediate particle size product.

[0119] The rest of the preparation methods and parameters remained the same as in Example 3.

[0120] Example 6

[0121] The difference between this embodiment and embodiment 3 is that the content of Ca in the feed product in step (3) is 8 wt.%.

[0122] The rest of the preparation methods and parameters remained the same as in Example 3.

[0123] Example 7

[0124] The difference between this embodiment and embodiment 3 is that the content of Ca in the feed product in step (3) is 18 wt.%.

[0125] The rest of the preparation methods and parameters remained the same as in Example 3.

[0126] Comparative Example 1

[0127] The sedimentary lithium-poor clay treated in this comparative example contains 0.52% Li2O, 14.73% Ca and 7.55% Al.

[0128] This comparative example provides a method for selectively extracting lithium from sedimentary lithium-deficient clay, the method comprising the following steps:

[0129] (1) grinding sedimentary lithium-deficient clay so that particles with a particle size of less than 0.074 mm account for 90% of the total number of particles to obtain a feed product;

[0130] (2) mixing the feed product with concentrated sulfuric acid having a mass concentration of 80% and stirring, stirring evenly, and then calcining at 150° C. for 4 h to obtain calcine I and CO2;

[0131] Wherein, based on the mass of the feed product, the amount of concentrated sulfuric acid used is 35wt.%;

[0132] (3) The roasted sand I is subjected to a second-stage roasting at 350° C. for 4 hours to obtain roasted sand II and acid gas. The acid gas is absorbed by water to generate a sulfuric acid solution, which can be reused in the first roasting step when the concentration reaches 80%;

[0133] (4) mixing the roasted sand II and the carbonate solution, and performing three-stage countercurrent leaching, wherein the pH of the slurry during leaching is 3, to obtain a lithium-rich leachate and a leach residue;

[0134] The mass ratio of the roasted sand II to the carbonate solution is 1:3, and the solute in the carbonate solution comes from the CO2 described in step (4).

[0135] Comparative Example 2

[0136] The sedimentary lithium-poor clay treated in this comparative example contains 0.52% Li2O, 14.73% Ca and 7.55% Al.

[0137] This comparative example provides a method for selectively extracting lithium from sedimentary lithium-deficient clay, the method comprising the following steps:

[0138] (1) grinding sedimentary lithium-deficient clay so that particles with a particle size of less than 0.074 mm account for 90% of the total number of particles to obtain a feed product;

[0139] (2) mixing and stirring the feed product and the composite sulfate, stirring evenly, and then calcining at 900° C. for 1 hour to obtain calcine;

[0140] Wherein, based on the mass of the feed product, the composite sulfate comprises 15% calcium sulfate, 12% sodium sulfate and 8% potassium sulfate;

[0141] (3) mixing the calcine and the carbonate solution, and performing three-stage countercurrent leaching, wherein the pH of the slurry during leaching is 3, to obtain a lithium-rich leachate and a leach residue;

[0142] Wherein, the mass ratio of the roasted sand II to the carbonic acid solution is 1:3.

[0143] Comparative Example 3

[0144] The difference between this comparative example and Example 3 is that the concentrated sulfuric acid in step (4) is replaced by a composite sulfate, which includes 15% calcium sulfate, 12% sodium sulfate and 8% potassium sulfate (based on the mass of the feed product).

[0145] The rest of the preparation methods and parameters remained the same as in Example 3.

[0146] Comparative Example 4

[0147] The difference between this comparative example and Example 3 is that the calcite with a particle size of less than 15 mm added in step (3) accounts for 5% of the mass of the calcite in step (2).

[0148] The rest of the preparation methods and parameters remained the same as in Example 3.

[0149] Comparative Example 5

[0150] The difference between this comparative example and Example 3 is that the calcite with a particle size of less than 15 mm added in step (3) accounts for 20% of the mass of the calcite in step (2).

[0151] The rest of the preparation methods and parameters remained the same as in Example 3.

[0152] Performance Testing

[0153] The lithium-rich leachates and leach residues prepared in Examples 1-7 and Comparative Examples 1-5 were tested for component content using an ICP tester. The test results are shown in Table 1.

[0154] Table 1

[0155] analyze:

[0156] As can be seen from the above table, the method for selectively extracting lithium from sedimentary lithium-deficient clay provided by the present disclosure not only selectively extracts lithium but also makes full use of the calcium source of the ore itself, does not require the addition of composite sulfate as a roasting additive, has a low reagent cost ratio, a low slag rate, effectively reduces the amount of material fed into the smelting, and improves the lithium grade of the feed.

[0157] From the comparison of the data results of Example 3 and Example 4, it can be seen that if the undersize product is not subjected to sedimentation and concentration, the grinding fineness will be low, which is not conducive to the subsequent lithium leaching and reduces the lithium leaching rate.

[0158] From the comparison of the data results of Example 3 and Example 5, it can be seen that if the calcite is not crushed before being mixed with the undersize product and the intermediate particle size product, the reaction between the calcite and the sulfuric acid is incomplete and sufficient Li + The exchange agent CaSO4 reduces the lithium leaching rate.

[0159] From the comparison of the data results of Example 3 and Example 6-7, it can be seen that if the content of Ca in the feed product is too low, the generated Li + If the exchange agent CaSO4 is insufficient, the lithium leaching rate will be reduced; if the Ca content in the feed product is too high, the feed will contain too much calcite, resulting in increased acid consumption and slag rate, which is not conducive to the resource utilization of this part of calcite.

[0160] From the comparison of the data results of Example 3 and Comparative Example 1, it can be seen that the amount of sulfuric acid used in the process provided by Comparative Example 1 is large, the calcium and aluminum leaching rate is higher, and the subsequent lithium-containing leachate purification process is also more complicated; in addition, the leaching residue contains soluble sulfate, which is difficult to utilize as a resource and is generally treated as hazardous waste.

[0161] From the comparison of the data results of Example 3 and Comparative Example 2, it can be seen that the process provided in Comparative Example 2 requires the addition of composite sulfate, especially potassium sulfate with a higher unit price, and the reagent cost is high; in addition, the slag rate is high, and because the leaching slag contains soluble sulfate, resource utilization is difficult and it is generally treated as hazardous waste.

[0162] From the comparison of the data results of Example 3 and Comparative Example 3, it can be seen that if concentrated sulfuric acid is replaced by composite sulfate, the slag rate increases sharply.

[0163] From the comparison of the data results of Example 3 and Comparative Examples 4-5, it can be seen that if the mass of calcite used in the ore blending process in step (3) is too much, the calcium content of the material entering the smelting will be too high, which will have little effect on improving the lithium leaching rate and significantly increase the slag rate; if the mass of calcite used in the ore blending process in step (3) is too little, the calcium content of the material entering the smelting will be too low and the lithium leaching rate will decrease.

Claims

1. A method for selectively extracting lithium from sedimentary lithium-deficient clay, the method comprising the following steps: (1) crushing and screening the sedimentary lithium-poor clay ore to obtain an oversize product, an undersize product and an intermediate particle size product; (2) sorting the above-screen product to obtain calcite and gangue; (3) blending the undersize product, the intermediate size product and part of the calcite to obtain a feed product; Wherein, the mass of the part of calcite in step (3) accounts for 7-18% of the mass of the calcite in step (2); (4) roasting the input product to obtain roasted sand; (5) Leaching the roasted sand to obtain a lithium-rich leaching solution and leaching residue.

2. The method according to claim 1, wherein: The particle size of the product on the sieve in step (1) is greater than 5 mm and less than 100 mm.

3. The method according to claim 1 or 2, wherein: The particle size of the intermediate grade product in step (1) is in the range of 2-5 mm.

4. The method according to any one of claims 1 to 3, wherein: The particle size of the undersize product in step (1) is less than 2 mm.

5. The method according to any one of claims 1 to 4, wherein: The sorting in step (2) includes photoelectric sorting.

6. The method according to any one of claims 1 to 5, wherein: The undersize product in step (3) is first subjected to sedimentation and concentration before being mixed with the intermediate size product and calcite.

7. The method according to any one of claims 1 to 6, wherein: In step (3), the calcite is first crushed to a particle size less than 15 mm before ore blending.

8. The method according to any one of claims 1 to 7, wherein: After the ore blending in step (3), the ore is ground so that particles with a particle size less than 0.074 mm account for 70-90% of the total number of particles.

9. The method according to any one of claims 1 to 8, wherein: Based on the mass of the feed product in step (3), the Ca content in the feed product is 10-15wt.%.

10. The method according to any one of claims 1 to 9, wherein: The roasting in step (4) includes a first stage roasting and a second stage roasting.

11. The method according to claim 10, wherein: The specific steps of the first stage roasting include: mixing the input product with concentrated sulfuric acid, performing aging roasting, and obtaining roasted sand I and CO2.

12. The method according to claim 11, wherein: The mixing process is accompanied by stirring.

13. The method according to claim 11 or 12, wherein: The mass fraction of the concentrated sulfuric acid is 70-80%; Optionally, based on the mass of the feed product in step (3), the amount of concentrated sulfuric acid used is 15-35wt.%.

14. The method according to any one of claims 11 to 13, wherein: The temperature of the first stage roasting is 150-280°C; Optionally, the calcination time is 0.5-4h.

15. The method according to any one of claims 10 to 14, wherein: The specific steps of the two-stage roasting include: roasting the roasted sand I in two stages to obtain roasted sand II and acid gas; Optionally, the temperature of the second stage roasting is 350-750°C; Optionally, the second-stage roasting time is 0.5-4h.

16. The method according to any one of claims 1 to 15, wherein: In the leaching process of step (5), the leaching agent used includes a weak acid solution; Optionally, the weak acid solution comprises a carbonic acid solution.

17. The method according to claim 16, wherein: The solute in the carbonic acid solution comes from the CO2 generated during the first stage roasting process.

18. The method according to any one of claims 1 to 17, wherein: The leaching method in step (5) includes three-stage countercurrent leaching; Optionally, during the three-stage countercurrent leaching process, the mass ratio of the roasted sand to the leaching agent is 1:(3-6); Optionally, during the three-stage countercurrent leaching process, the pH of the slurry during leaching is 3-4.

19. The method according to any one of claims 1 to 18, wherein: The method comprises the following steps: (1) crushing and screening the sedimentary lithium-poor clay ore to obtain an oversize product, an undersize product and an intermediate particle size product; Among them, the particle size of the oversize product is greater than 5mm and less than 100mm, the particle size of the intermediate particle size product is in the range of 2-5mm, and the particle size of the undersize product is less than 2mm; (2) performing photoelectric separation on the product on the screen of step (1) to obtain calcite and gangue; (3) the undersize product of step (1) is subjected to sedimentation and concentration, and then mixed with the intermediate particle size product of step (1) and the calcite with a crushed particle size of less than 15 mm, and then ground so that particles with a particle size of less than 0.074 mm account for 70-90% of the total number of particles, to obtain a feed product with a Ca content of 10-15 wt.%; The mass of the calcite with a particle size less than 15 mm after crushing accounts for 7-18% of the mass of the calcite in step (2); (4) mixing the feed product of step (3) with concentrated sulfuric acid having a mass concentration of 70-80% and stirring, and calcining at 150-280° C. for 0.5-4 h to obtain calcined sand I and CO2; Wherein, based on the mass of the feed product in step (3), the amount of concentrated sulfuric acid used is 15-35wt.%; (5) calcining the roasted sand I in step (4) in two stages at 350-750° C. for 0.5-4 h to obtain roasted sand II and acid gas; (6) Mixing the roasted sand II described in step (5) with the weak acid solution and performing three-stage countercurrent leaching to obtain a rich Lithium leachate and leaching residue; Among them, the mass ratio of roasted sand II and weak acid solution is 1:(3-6).

20. An application of the method for selectively extracting lithium from sedimentary lithium-deficient clay as claimed in any one of claims 1 to 19, wherein the method is applied to selectively extracting lithium from low-grade lithium clay.

Citation Information

Patent Citations

  • Method for preparing lithium carbonate through two-stage conversion of lithium ore

    CN107089673A

  • Method of selectively leaching low grade sedimentary lithium ores

    CN110042262A

  • Method for extracting lithium from lithium chinastone mineral by roasting with mixed sulfate method

    CN113999970A

  • Method for extracting lithium ions from clay-type lithium ore with extremely low lithium grade by ion substitution

    CN115976337A

  • Extraction of lithium from lithium-containing materials

    US4588566A

Cited By

  • Method for extracting lithium from amblygonite

    CN120230923A

  • Method for preparing lithium carbonate from lithium ore

    CN121228025A