Rigid polyurethane foam material and preparation method therefor
By using a combination of multi-functional polyether polyol, polyester polyol, toluene diisocyanate and glass fiber continuous mat, the cross-linking density and foam fineness of polyurethane rigid foam materials are improved, which solves the problem of polyurethane rigid foam materials in cryogenic environments. It eliminates the problem of unstable mechanical properties and improves the mechanical and thermal insulation properties in low-temperature environments, making it suitable for cryogenic thermal insulation fields.
Patent Information
- Application Number
- PCT/CN2023/090107
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-04-23
- Publication Date
- 2024-10-24
AI Technical Summary
Existing polyurethane rigid foam materials have unstable mechanical properties in cryogenic environments, cannot maintain mechanical strength and thermal insulation properties, and are not suitable for cryogenic thermal insulation fields in ultra-low temperature environments.
It is prepared by using raw materials such as multifunctional polyether polyol, multifunctional polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and glass fiber continuous mat through high-pressure mixing and confined space foaming processes. Create a polyurethane rigid foam material with moderate density, improve its cross-linking density and foam fineness, and enhance its compression strength and thermal insulation performance.
The mechanical properties and thermal insulation properties of polyurethane rigid foam materials have been improved in low-temperature environments. The density is 70-210kg/m3, the surface flatness is controlled within 5mm, and the core material utilization rate is increased to more than 85%. It is suitable for cryogenic insulation. field.
Smart Images

Figure CN2023090107_24102024_PF_FP_ABST
Abstract
Description
A polyurethane rigid foam material and preparation method thereof Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more particularly to a polyurethane rigid foam material and a preparation method thereof. Background Art
[0002] Rigid polyurethane foam, also known as rigid polyurethane foam, is second only to soft polyurethane foam in the usage of polyurethane products. Most rigid polyurethane foams have a closed-cell structure and offer excellent properties such as good thermal insulation, light weight, high specific strength, and easy construction. They also offer sound insulation, shock absorption, electrical insulation, and resistance to heat, cold, and solvents. They are widely used in refrigerator and freezer insulation, cold storage, refrigerated trucks, and other insulation materials, as well as in buildings, storage tanks, and pipelines. Smaller amounts are used in non-insulating applications, such as wood imitation and packaging. Generally speaking, lower-density rigid polyurethane foams are primarily used as thermal insulation (heat preservation), while higher-density rigid polyurethane foams can be used as structural materials (imitation wood).
[0003] Ordinary polyurethane rigid foam materials have excellent thermal insulation properties, but they will shrink and crack severely in deep cold environments, resulting in their inability to maintain mechanical strength and thermal insulation properties. To solve this problem, it is usually possible to use a composite with glass fiber continuous mat to enhance the mechanical properties and dimensional stability of polyurethane rigid foam materials at low temperatures, and to improve the flame retardant grade of polyurethane by adding certain flame retardants. For example, Patent 2007101441393 (Publication No. CN101235128A) discloses a continuous fiber reinforced polyurethane with a density of 400-800kg / m 3 The polyurethane foam material is suitable for "bearing structural materials" and cannot be used for heat preservation in ultra-low temperature environments. Patent 200610058849X (publication number CN1834130A) discloses a density of 115-135kg / m 3 , a thermal insulation material with a compressive strength of 1.4-1.7MPa, but the patent does not provide a detailed thermal conductivity coefficient for the thermal insulation performance of the material, and it is unknown what the mechanical properties of the material at low temperatures are.
[0004] In addition, due to the addition of continuous glass fiber mat, the reinforced polyurethane rigid foam material usually adopts a free-style foaming process, and the foaming in a confined space is mostly used to prepare low-density polyurethane sandwich panels. For example, Patent 201810493822.6 (Publication No. CN109096459B) discloses an environmentally friendly low-density polyurethane sandwich panel, which is a polyurethane color steel plate produced by a continuous polyurethane sandwich panel production process. Patent 202011587634.3 (Publication No. CN112694592A) discloses a polyurethane sandwich panel and its preparation method, but the density of these polyurethane materials is 50kg / m 3 The following, and no reinforcing materials are added, are not suitable for the field of deep cold insulation.
[0005] Therefore, how to develop a deep-cold thermal insulation enhanced polyurethane rigid foam material that can be continuously produced in a confined space is an urgent problem that needs to be solved by those skilled in the art.
[0006] Summary of the Invention
[0007] In view of this, an object of the present invention is to provide a polyurethane rigid foam material and a preparation method thereof to address the deficiencies in the prior art.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] A polyurethane rigid foam material comprises the following raw materials in parts by weight: 30-50 parts of multifunctional polyether polyol, 30-50 parts of multifunctional polyester polyol, 50-80 parts of toluene diisocyanate, 50-80 parts of polymethylene polyphenyl polyisocyanate, 15-30 parts of a foaming auxiliary additive composition and 5-20 parts of continuous glass fiber mat.
[0010] Preferably, the composition comprises: 35 parts of multifunctional polyether polyol, 50 parts of multifunctional polyester polyol, 60 parts of toluene diisocyanate, 80 parts of polymethylene polyphenyl polyisocyanate, 15 parts of foaming auxiliary additive composition and 15 parts of glass fiber continuous mat.
[0011] Furthermore, the multifunctional polyether polyol has a molecular weight of 300-500, preferably 350-450, more preferably 400; a hydroxyl value of 500-800 mgKOH / g, preferably 550-650 mgKOH / g, more preferably 600 mgKOH / g; a viscosity of 2000-4000 mPa·s, preferably 2500-3500 mPa·s, more preferably 3000 mPa·s; and a moisture content of less than 0.15%. Furthermore, the multifunctional polyether polyol is at least one of sucrose polyether polyol, sorbitol polyether polyol, pentaerythritol polyether polyol, and polytetramethylene glycol.
[0012] The beneficial effect of adopting the above further technical solution is that the multifunctional polyether polyol selected in the present invention can further increase the crosslinking density of the polyurethane rigid foam material, thereby improving its compressive strength.
[0013] Furthermore, the multifunctional polyester polyol has a molecular weight of 500-800, preferably 550-650, more preferably 600; a hydroxyl value of 200-400 mgKOH / g, preferably 350-400 mgKOH / g, more preferably 380 mgKOH / g; a viscosity of 1000-3000 mPa·s, preferably 1500-2000 mPa·s, more preferably 1800 mPa·s; and a moisture content of less than 0.15%. Furthermore, the multifunctional polyester polyol is at least one of phthalic anhydride polyester polyol, metaphthalic anhydride polyester polyol, and aromatic-aliphatic copolyester.
[0014] The beneficial effect of adopting the above-mentioned further technical solution is that the multifunctional polyester polyol selected by the present invention has better compatibility with the polymethylene polyphenyl polyisocyanate component, which can further increase the foam fineness of the polyurethane rigid foam material, thereby improving its thermal insulation performance.
[0015] Furthermore, the polymethylene polyphenyl polyisocyanate has an isocyanate content of 30-40 wt%, preferably 35-37 wt%, and more preferably 36 wt%; a viscosity of 200-400 mPa·s, preferably 250-350 mPa·s, and more preferably 300 mPa·s; and a functionality of 2.0-3.0, preferably 2.5-3.0, and more preferably 2.8.
[0016] The beneficial effect of adopting the above-mentioned further technical solution is that the polymethylene polyphenyl polyisocyanate selected in the present invention has a moderate viscosity, which is conducive to the uniform mixing of the components; and a high functionality, which can further increase the crosslinking density of the polyurethane rigid foam material, thereby improving its compressive strength.
[0017] Furthermore, the above-mentioned foaming auxiliary additive composition includes the following raw materials in parts by weight: 10-20 parts of polyether-polydimethylsiloxane copolymer, 30-40 parts of pentafluoropropane, 30-40 parts of trans-1-chloro-3,3,3-trifluoropropene, 1-3 parts of small molecule amine catalyst and 1-3 parts of organic tin catalyst; preferably: 13 parts of polyether-polydimethylsiloxane copolymer, 32 parts of pentafluoropropane, 38 parts of trans-1-chloro-3,3,3-trifluoropropene, 1.4 parts of small molecule amine catalyst and 2.2 parts of organic tin catalyst.
[0018] Furthermore, the small molecule amine catalyst is dimethylcyclohexylamine, and the organotin catalyst is dibutyltin dilaurate.
[0019] The beneficial effect of adopting the above further technical solution is that the foaming auxiliary additive composition selected in the present invention includes a foaming agent, a stabilizer and a catalyst, thereby ensuring the mechanical strength and dimensional stability of the polyurethane rigid foam material.
[0020] Furthermore, the apparent density of the above-mentioned glass fiber continuous mat is 500-700 kg / m 2 , preferably 550kg / m 2 ; Organic matter content is 2-3wt%, preferably 2.2wt%; width of each roll is 1-3m, preferably 2.1m; length is 100-150m, preferably 120m.
[0021] The beneficial effect of adopting the above-mentioned further technical solution is that the glass fiber continuous mat selected by the present invention has a high apparent density and high strength, and is coated with a coupling agent component on the surface, which can effectively combine with the polyurethane rigid foam material body, thereby improving its tensile strength.
[0022] A method for preparing a polyurethane rigid foam material specifically comprises the following steps:
[0023] (1) Weighing the raw materials according to the weight of the above-mentioned polyurethane rigid foam material;
[0024] (2) mixing a polyfunctional polyether polyol, a polyfunctional polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition to obtain a mixture;
[0025] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0026] (4) After the semi-finished product is naturally cured, it is cut into sections and cured again to obtain a polyurethane rigid foam material.
[0027] Furthermore, in the above step (2), the mixing equipment is a high-pressure mixing head; the mixing pressure is 50-300 bar, preferably 100-150 bar; the mixing temperature is 15-35°C, preferably 20-30°C; the discharge rate of the high-pressure mixing head is 20-120 kg / min, preferably 50-80 kg / min.
[0028] The beneficial effect of adopting the above-mentioned further technical solution is that the mixing pressure of the high-pressure mixing head selected by the present invention is large, which can improve the mixing effect of the hydroxyl component and the isocyanate component, making the pores of the polyurethane rigid foam material more delicate and having better thermal insulation performance.
[0029] Furthermore, in the above step (3), the upper, lower, left and right sides of the confined space are all composed of high-strength chain plates; the thickness of the chain plates is 5-25 mm, preferably 10-20 mm; the flatness of the chain plates is ±0.5-1 mm, preferably ±0.5-0.7 mm; the temperature of the chain plates is 15-45°C, preferably 30-40°C; the forward speed of the chain plates is 0.5-2.5 m / min; preferably 1.0-1.5 m / min.
[0030] The beneficial effect of adopting the above-mentioned further technical solution is that the polyurethane foam foaming process of the present invention is completed in a confined space, the foam shape and size are regular and controllable, and the utilization rate of the polyurethane foam core material can be improved.
[0031] Furthermore, the above step (3) further includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 90-250g / m 2 , preferably 150-200g / m 2 .
[0032] The beneficial effect of adopting the above further technical solution is that the kraft paper selected in the present invention can isolate the continuous glass fiber mat from the chain plate, thereby avoiding the influence of the chain plate on the foaming process.
[0033] Furthermore, in the above step (4), the natural curing time is 15-35 minutes; and the re-curing time is 48 hours.
[0034] Furthermore, the above steps (2)-(4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 15-35°C, preferably 20-30°C; and the ambient humidity is below 80%, preferably 30%-70%.
[0035] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0036] The density of the deep-cold heat-insulating enhanced polyurethane rigid foam material continuously produced in a confined space of the present invention is 70-210 kg / m 3 On the premise of ensuring the low-temperature mechanical strength and thermal insulation performance of the material, the surface flatness is controlled within 5mm, and the core material utilization rate is increased to more than 85%, which can be widely used in the field of deep cold insulation. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] FIG1 is a schematic diagram of a process flow of a method for preparing a polyurethane rigid foam material according to the present invention;
[0038] FIG2 is a cross-sectional view of a polyurethane rigid foam material prepared in Example 5 of the present invention;
[0039] FIG3 is a cross-sectional view of the polyurethane rigid foam material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0040] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0041] Example 1
[0042] A polyurethane rigid foam material comprises the following raw materials by weight: 30 kg of sucrose polyether polyol, 50 kg of phthalic anhydride polyester polyol, 80 kg of toluene diisocyanate, 50 kg of polymethylene polyphenyl polyisocyanate, 15 kg of a foaming auxiliary additive composition, and 15 kg of a continuous glass fiber mat;
[0043] The sucrose polyether polyol has a molecular weight of 300, a hydroxyl value of 500 mgKOH / g, a viscosity of 2000 mPa·s, and a moisture content of 0.15%.
[0044] The molecular weight of the phthalic anhydride polyester polyol is 500, the hydroxyl value is 200 mgKOH / g, the viscosity is 1000 mPa·s, and the moisture content is 0.15%;
[0045] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 30 wt%, a viscosity of 200 mPa·S, and a functionality of 2.0;
[0046] The foaming auxiliary additive composition includes the following raw materials by weight: 10 kg of polyether-polydimethylsiloxane copolymer, 30 kg of pentafluoropropane, 30 kg of trans-1-chloro-3,3,3-trifluoropropene, 1 kg of dimethylcyclohexylamine and 1 kg of dibutyltin dilaurate;
[0047] The apparent density of glass fiber continuous mat is 500kg / m 2 , organic matter content is 2wt%, each roll is 1m wide and 100m long;
[0048] The preparation method of the above-mentioned polyurethane rigid foam material, as shown in Figure 1, specifically comprises the following steps:
[0049] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0050] (2) adding sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition to a high-pressure mixing head for mixing at a pressure of 50 bar, a temperature of 20° C. and a discharge rate of 30 kg / min to obtain a mixture;
[0051] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0052] The upper, lower, left and right sides of the confined space are all made of high-strength chain plates; the thickness of the chain plates is 5mm, the flatness is ±0.5mm, the temperature is 20℃, and the forward speed is 0.5m / min;
[0053] It also includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 90g / m 2 ;
[0054] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0055] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 15° C. and the ambient humidity is 40%.
[0056] Example 2
[0057] A polyurethane rigid foam material comprises the following raw materials by weight: 50 kg of sucrose polyether polyol, 30 kg of phthalic anhydride polyester polyol, 50 kg of toluene diisocyanate, 80 kg of polymethylene polyphenyl polyisocyanate, 30 kg of a foaming auxiliary additive composition, and 20 kg of a continuous glass fiber mat;
[0058] The sucrose polyether polyol has a molecular weight of 300, a hydroxyl value of 500 mgKOH / g, a viscosity of 2000 mPa·s, and a moisture content of 0.15%.
[0059] The molecular weight of the phthalic anhydride polyester polyol is 500, the hydroxyl value is 200 mgKOH / g, the viscosity is 1000 mPa·s, and the moisture content is 0.15%;
[0060] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 30 wt%, a viscosity of 200 mPa·S, and a functionality of 2.0;
[0061] The foaming auxiliary additive composition includes the following raw materials by weight: 10 kg of polyether-polydimethylsiloxane copolymer, 30 kg of pentafluoropropane, 30 kg of trans-1-chloro-3,3,3-trifluoropropene, 1 kg of dimethylcyclohexylamine and 1 kg of dibutyltin dilaurate;
[0062] The apparent density of glass fiber continuous mat is 500kg / m 2 , organic matter content is 2wt%, each roll is 1m wide and 100m long;
[0063] The preparation method of the above-mentioned polyurethane rigid foam material, as shown in Figure 1, specifically comprises the following steps:
[0064] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0065] (2) adding sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition to a high-pressure mixing head for mixing at a pressure of 100 bar, a temperature of 25° C., and a discharge rate of 80 kg / min to obtain a mixture;
[0066] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0067] The upper, lower, left, and right sides of the confined space are all made of high-strength chain plates; the thickness of the chain plates is 15mm, the flatness is ±0.5mm, the temperature is 25°C, and the forward speed is 1m / min;
[0068] It also includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 150g / m 2 ;
[0069] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0070] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 20° C. and the ambient humidity is 50%.
[0071] Example 3
[0072] A polyurethane rigid foam material comprising the following raw materials by weight: 40 kg of sorbitol polyether polyol, 40 kg of phthalic anhydride polyester polyol, 60 kg of toluene diisocyanate, 70 kg of polymethylene polyphenyl polyisocyanate, 20 kg of a foaming auxiliary additive composition, and 15 kg of a continuous glass fiber mat;
[0073] The sorbitol polyether polyol has a molecular weight of 350, a hydroxyl value of 550 mgKOH / g, a viscosity of 2500 mPa·s, and a moisture content of 0.10%.
[0074] The molecular weight of the phthalic anhydride polyester polyol is 550, the hydroxyl value is 350 mgKOH / g, the viscosity is 1500 mPa·s, and the moisture content is 0.10%;
[0075] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 35 wt%, a viscosity of 250 mPa·S, and a functionality of 2.5;
[0076] The foaming auxiliary additive composition includes the following raw materials by weight: 10 kg of polyether-polydimethylsiloxane copolymer, 30 kg of pentafluoropropane, 30 kg of trans-1-chloro-3,3,3-trifluoropropene, 1 kg of dimethylcyclohexylamine and 1 kg of dibutyltin dilaurate;
[0077] The apparent density of glass fiber continuous mat is 500kg / m 2 , organic matter content is 2wt%, each roll is 1m wide and 100m long;
[0078] The preparation method of the above-mentioned polyurethane rigid foam material, as shown in Figure 1, specifically comprises the following steps:
[0079] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0080] (2) adding sorbitol polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition into a high-pressure mixing head for mixing at a pressure of 150 bar, a temperature of 30° C. and a discharge rate of 100 kg / min to obtain a mixture;
[0081] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0082] The upper, lower, left, and right sides of the confined space are all made of high-strength chain plates; the thickness of the chain plates is 10mm, the flatness is ±0.5mm, the temperature is 30°C, and the forward speed is 1.5m / min;
[0083] It also includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 180g / m 2 ;
[0084] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0085] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 25° C. and the ambient humidity is 60%.
[0086] Example 4
[0087] A polyurethane rigid foam material comprises the following raw materials by weight: 45 kg of sorbitol polyether polyol, 35 kg of phthalic anhydride polyester polyol, 55 kg of toluene diisocyanate, 70 kg of polymethylene polyphenyl polyisocyanate, 25 g of a foaming auxiliary additive composition, and 5 g of a continuous glass fiber mat;
[0088] The sorbitol polyether polyol has a molecular weight of 350, a hydroxyl value of 550 mgKOH / g, a viscosity of 2500 mPa·s, and a moisture content of 0.10%.
[0089] The molecular weight of the phthalic anhydride polyester polyol is 550, the hydroxyl value is 350 mgKOH / g, the viscosity is 1500 mPa·s, and the moisture content is 0.10%;
[0090] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 35 wt%, a viscosity of 250 mPa·S, and a functionality of 2.5;
[0091] The foaming auxiliary additive composition includes the following raw materials by weight: 10 kg of polyether-polydimethylsiloxane copolymer, 30 kg of pentafluoropropane, 30 kg of trans-1-chloro-3,3,3-trifluoropropene, 1 kg of dimethylcyclohexylamine and 1 kg of dibutyltin dilaurate;
[0092] The apparent density of glass fiber continuous mat is 500kg / m 2 , organic matter content is 2wt%, each roll is 1m wide and 100m long;
[0093] The preparation method of the above-mentioned polyurethane rigid foam material, as shown in Figure 1, specifically comprises the following steps:
[0094] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0095] (2) adding sorbitol polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition into a high-pressure mixing head for mixing at a pressure of 300 bar, a temperature of 35° C. and a discharge rate of 100 kg / min to obtain a mixture;
[0096] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0097] The upper, lower, left, and right sides of the confined space are all made of high-strength chain plates; the thickness of the chain plates is 15mm, the flatness is ±0.8mm, the temperature is 35°C, and the forward speed is 2.0m / min;
[0098] It also includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 250g / m 2 ;
[0099] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0100] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 30° C. and the ambient humidity is 60%.
[0101] Example 5
[0102] A polyurethane rigid foam material comprising the following raw materials by weight: 35 kg of sucrose polyether polyol, 50 kg of phthalic anhydride polyester polyol, 60 kg of toluene diisocyanate, 80 kg of polymethylene polyphenyl polyisocyanate, 15 kg of a foaming auxiliary additive composition, and 15 kg of a continuous glass fiber mat;
[0103] The molecular weight of the sucrose polyether polyol is 400, the hydroxyl value is 600 mgKOH / g, the viscosity is 3000 mPa·s, and the moisture content is 0.05%.
[0104] The molecular weight of the phthalic anhydride polyester polyol is 600, the hydroxyl value is 380 mgKOH / g, the viscosity is 1800 mPa·s, and the moisture content is 0.05%;
[0105] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 36 wt%, a viscosity of 300 mPa·S, and a functionality of 2.8;
[0106] The foaming auxiliary additive composition includes the following raw materials by weight: 13 kg of polyether-polydimethylsiloxane copolymer, 32 kg of pentafluoropropane, 38 kg of trans-1-chloro-3,3,3-trifluoropropene, 1.4 kg of dimethylcyclohexylamine, and 2.2 kg of dibutyltin dilaurate;
[0107] The apparent density of glass fiber continuous mat is 550kg / m 2 , organic matter content is 2.2wt%, each roll is 2.1m wide and 120m long;
[0108] The preparation method of the above-mentioned polyurethane rigid foam material, as shown in Figure 1, specifically comprises the following steps:
[0109] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0110] (2) adding sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition to a high-pressure mixing head for mixing at a pressure of 150 bar, a temperature of 25° C., and a discharge rate of 120 kg / min to obtain a mixture;
[0111] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0112] The upper, lower, left and right sides of the confined space are all made of high-strength chain plates; the thickness of the chain plates is 20mm, the flatness is ±0.5mm, the temperature is 40°C, and the forward speed is 2.5m / min;
[0113] It also includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 160g / m 2 ;
[0114] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0115] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 20° C. and the ambient humidity is 70%.
[0116] Example 6
[0117] A polyurethane rigid foam material comprises the following raw materials by weight: 50 kg of polytetramethylene glycol, 45 kg of aromatic-aliphatic copolyester, 60 kg of toluene diisocyanate, 55 kg of polymethylene polyphenyl polyisocyanate, 20 kg of a foaming auxiliary additive composition, and 10 kg of a continuous glass fiber mat;
[0118] Wherein, the molecular weight of polytetrahydrofuran diol is 450, the hydroxyl value is 650mgKOH / g, the viscosity is 3500mPa·s, and the moisture content is 0.10%;
[0119] The aromatic-aliphatic copolyester has a molecular weight of 650, a hydroxyl value of 400 mgKOH / g, a viscosity of 2000 mPa·s, and a moisture content of 0.10%;
[0120] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 37 wt%, a viscosity of 350 mPa·S, and a functionality of 3.0;
[0121] The foaming auxiliary additive composition includes the following raw materials by weight: 20 kg of polyether-polydimethylsiloxane copolymer, 40 kg of pentafluoropropane, 40 kg of trans-1-chloro-3,3,3-trifluoropropene, 3 kg of dimethylcyclohexylamine and 3 kg of dibutyltin dilaurate;
[0122] The apparent density of glass fiber continuous mat is 700kg / m 2 , organic matter content is 3wt%, each roll is 3m wide and 150m long;
[0123] The preparation method of the above-mentioned polyurethane rigid foam material, as shown in Figure 1, specifically comprises the following steps:
[0124] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0125] (2) adding polytetrahydrofuran diol, aromatic-aliphatic copolyester, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and foaming auxiliary additive composition into a high-pressure mixing head and mixing them under a pressure of 150 bar, a temperature of 20° C., and a discharge rate of 75 kg / min to obtain a mixture;
[0126] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0127] The upper, lower, left, and right sides of the confined space are all made of high-strength chain plates; the thickness of the chain plates is 12mm, the flatness is ±0.7mm, the temperature is 30°C, and the forward speed is 1.5m / min;
[0128] It also includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 100g / m 2 ;
[0129] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0130] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 20° C. and the ambient humidity is 50%.
[0131] Example 7
[0132] A polyurethane rigid foam material comprising the following raw materials by weight: 48 kg of polytetramethylene furan diol, 48 kg of aromatic-aliphatic copolyester, 66 kg of toluene diisocyanate, 51 kg of polymethylene polyphenyl polyisocyanate, 18 kg of a foaming auxiliary additive composition, and 8 kg of continuous glass fiber mat;
[0133] Wherein, the molecular weight of polytetrahydrofuran diol is 500, the hydroxyl value is 800mgKOH / g, the viscosity is 4000mPa·s, and the moisture content is 0.10%;
[0134] The aromatic-aliphatic copolyester has a molecular weight of 800, a hydroxyl value of 400 mgKOH / g, a viscosity of 3000 mPa·s, and a moisture content of 0.10%;
[0135] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 40 wt%, a viscosity of 400 mPa·S, and a functionality of 3.0;
[0136] The foaming auxiliary additive composition includes the following raw materials by weight: 20 kg of polyether-polydimethylsiloxane copolymer, 40 kg of pentafluoropropane, 40 kg of trans-1-chloro-3,3,3-trifluoropropene, 3 kg of dimethylcyclohexylamine and 3 kg of dibutyltin dilaurate;
[0137] The apparent density of glass fiber continuous mat is 700kg / m 2 , organic matter content is 3wt%, each roll is 3m wide and 150m long;
[0138] The preparation method of the above-mentioned polyurethane rigid foam material, as shown in Figure 1, specifically comprises the following steps:
[0139] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0140] (2) adding polytetrahydrofuran diol, aromatic-aliphatic copolyester, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and foaming auxiliary additive composition into a high-pressure mixing head and mixing them at a pressure of 80 bar, a temperature of 25° C., and a discharge rate of 105 kg / min to obtain a mixture;
[0141] (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product;
[0142] The upper, lower, left, and right sides of the confined space are all made of high-strength chain plates; the thickness of the chain plates is 9mm, the flatness is ±1mm, the temperature is 30°C, and the forward speed is 1.3m / min;
[0143] It also includes: using kraft paper to isolate the glass fiber continuous mat from the chain plate; the apparent density of the kraft paper is 130g / m 2 ;
[0144] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0145] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 25° C. and the ambient humidity is 80%.
[0146] Comparative Example 1
[0147] A polyurethane rigid foam material comprising the following raw materials by weight: 45 kg of sucrose polyether polyol, 45 kg of phthalic anhydride polyester polyol, 55 kg of toluene diisocyanate, 65 kg of polymethylene polyphenyl polyisocyanate, 20 kg of a foaming auxiliary additive composition, and 11 kg of a continuous glass fiber mat;
[0148] The molecular weight of the sucrose polyether polyol is 400, the hydroxyl value is 600 mgKOH / g, the viscosity is 3000 mPa·s, and the moisture content is 0.05%.
[0149] The molecular weight of the phthalic anhydride polyester polyol is 600, the hydroxyl value is 380 mgKOH / g, the viscosity is 1800 mPa·s, and the moisture content is 0.05%;
[0150] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 36 wt%, a viscosity of 300 mPa·S, and a functionality of 2.8;
[0151] The foaming auxiliary additive composition includes the following raw materials by weight: 13 kg of polyether-polydimethylsiloxane copolymer, 32 kg of pentafluoropropane, 38 kg of trans-1-chloro-3,3,3-trifluoropropene, 1.4 kg of dimethylcyclohexylamine, and 2.2 kg of dibutyltin dilaurate;
[0152] The apparent density of glass fiber continuous mat is 550kg / m 2 , organic matter content is 2.2wt%, each roll is 2.1m wide and 120m long;
[0153] The preparation method of the above-mentioned polyurethane rigid foam material specifically comprises the following steps:
[0154] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0155] (2) adding sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition to a high-pressure mixing head for mixing at a pressure of 95 bar, a temperature of 25° C., and a discharge rate of 95 kg / min to obtain a mixture;
[0156] (3) pouring the mixture onto a flat glass fiber continuous mat, and then foaming and molding it to obtain a semi-finished product;
[0157] It also includes: using kraft paper to isolate the glass fiber continuous mat from the foaming environment; the apparent density of kraft paper is 110g / m 2 ;
[0158] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0159] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 35° C. and the ambient humidity is 40%.
[0160] Comparative Example 2
[0161] A polyurethane rigid foam material comprising the following raw materials by weight: 55 kg of sucrose polyether polyol, 45 kg of phthalic anhydride polyester polyol, 65 kg of toluene diisocyanate, 55 kg of polymethylene polyphenyl polyisocyanate, 10 kg of a foaming auxiliary additive composition, and 10 kg of a continuous glass fiber mat;
[0162] The molecular weight of the sucrose polyether polyol is 400, the hydroxyl value is 600 mgKOH / g, the viscosity is 3000 mPa·s, and the moisture content is 0.05%.
[0163] The molecular weight of the phthalic anhydride polyester polyol is 600, the hydroxyl value is 380 mgKOH / g, the viscosity is 1800 mPa·s, and the moisture content is 0.05%;
[0164] The polymethylene polyphenyl polyisocyanate has an isocyanate content of 36 wt%, a viscosity of 300 mPa·S, and a functionality of 2.8;
[0165] The foaming auxiliary additive composition includes the following raw materials by weight: 13 kg of polyether-polydimethylsiloxane copolymer, 32 kg of pentafluoropropane, 38 kg of trans-1-chloro-3,3,3-trifluoropropene, 1.4 kg of dimethylcyclohexylamine, and 2.2 kg of dibutyltin dilaurate;
[0166] The apparent density of glass fiber continuous mat is 550kg / m 2 , organic matter content is 2.2wt%, each roll is 2.1m wide and 120m long;
[0167] The preparation method of the above-mentioned polyurethane rigid foam material specifically comprises the following steps:
[0168] (1) Weighing each raw material according to the weight of the above-mentioned polyurethane rigid foam material;
[0169] (2) adding sucrose polyether polyol, phthalic anhydride polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition to a high-pressure mixing head for mixing at a pressure of 120 bar, a temperature of 20° C. and a discharge rate of 135 kg / min to obtain a mixture;
[0170] (3) pouring the mixture onto a flat glass fiber continuous mat, and then foaming and molding it to obtain a semi-finished product;
[0171] It also includes: using kraft paper to isolate the glass fiber continuous mat from the foaming environment; the apparent density of kraft paper is 110g / m 2 ;
[0172] (4) After the semi-finished product is naturally cured for 20 minutes, it is cut into sections and cured again for 48 hours to obtain a polyurethane rigid foam material;
[0173] Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 30° C. and the ambient humidity is 60%.
[0174] Performance Testing
[0175] 1. The polyurethane rigid foam materials prepared in Examples 1-7 and Comparative Examples 1-2 were taken, and the raw material amounts and process parameters were shown in Table 1.
[0176] The density, compressive strength, tensile strength, thermal conductivity, closed porosity, surface smoothness and core material utilization were tested respectively. The test results are shown in Table 2.
[0177] Among them, the performance evaluation methods are as follows:
[0178] Product density: Remove the surface of the polyurethane rigid foam material and cut it into cubes, and then test it according to GB / T6343-2009.
[0179] Compression strength: Cut the polyurethane rigid foam material into samples of 50mm×50mm×50mm and test at -160℃ in accordance with GB / T 8813-2008.
[0180] Tensile strength: Cut the polyurethane rigid foam material into dumbbell-shaped specimens and test at -160℃ in accordance with BS ISO 1926-2005.
[0181] Thermal conductivity: Cut the polyurethane rigid foam material into samples of 300mm×300mm×30mm and test at -160℃ in accordance with ISO 8302.
[0182] Closed-cell rate: Cut the polyurethane rigid foam material into samples of 30mm×30mm×50mm and test them at 20℃ in accordance with GB / T 10799-1989.
[0183] Surface flatness: Calculated by measuring the difference between the lowest point and the highest point on the surface of the polyurethane rigid foam material.
[0184] Core material utilization rate: calculated by calculating the ratio of the volume after removing the upper and lower and side skins of the polyurethane rigid foam material to the volume of the polyurethane rigid foam material blank.
[0185] Table 1 Raw material dosage and process parameters of polyurethane rigid foam materials of Examples 1-7 and Comparative Examples 1-2
[0186] Table 2 Performance test results of polyurethane rigid foam materials of Examples 1-7 and Comparative Examples 1-2
[0187] As shown in Table 2, compared with Comparative Examples 1-2, the density, compressive strength, tensile strength, thermal conductivity, closed cell ratio, surface smoothness and core material utilization of the polyurethane rigid foam materials prepared in Examples 1-7 of the present invention are significantly improved.
[0188] 2. Take the polyurethane rigid foam materials prepared in Example 5 and Comparative Example 1, cut them, and see the cross-sectional views shown in Figures 2 and 3, respectively.
[0189] As can be seen from Figures 2-3, compared with Comparative Example 1, the surface flatness of the polyurethane rigid foam material prepared in Example 5 of the present invention is higher.
[0190] The above experiments 1-2 show that the density of the deep-cold heat-insulating enhanced polyurethane rigid foam material produced continuously in confined space of the present invention is 70-210 kg / m 3 On the premise of ensuring the low-temperature mechanical strength and thermal insulation performance of the material, the surface flatness is controlled within 5mm, and the core material utilization rate is increased to more than 85%, which can be widely used in the field of deep cold insulation.
[0191] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not limited to the embodiments shown herein but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A polyurethane rigid foam material, It is characterized in that The invention comprises the following raw materials in parts by weight: 30-50 parts of multifunctional polyether polyol, 30-50 parts of multifunctional polyester polyol, 50-80 parts of toluene diisocyanate, 50-80 parts of polymethylene polyphenyl polyisocyanate, 15-30 parts of foaming auxiliary additive composition and 5-20 parts of glass fiber continuous felt.
2. A polyurethane rigid foam material according to claim 1, It is characterized in that The invention comprises the following raw materials in parts by weight: 35 parts of multifunctional polyether polyol, 50 parts of multifunctional polyester polyol, 60 parts of toluene diisocyanate, 80 parts of polymethylene polyphenyl polyisocyanate, 15 parts of foaming auxiliary additive composition and 15 parts of glass fiber continuous felt.
3. A polyurethane rigid foam material according to claim 1 or 2, It is characterized in that The multifunctional polyether polyol has a molecular weight of 300-500, a hydroxyl value of 500-800 mgKOH / g, a viscosity of 2000-4000 mPa·S, and a moisture content of less than 0.15%; The multifunctional polyester polyol has a molecular weight of 500-800, a hydroxyl value of 200-400 mgKOH / g, a viscosity of 1000-3000 mPa·S, and a water content of less than 0.15%.
4. A polyurethane rigid foam material according to claim 1 or 2, It is characterized in that The polymethylene polyphenyl polyisocyanate has an isocyanate content of 30-40 wt %, a viscosity of 200-400 mPa·S, and a functionality of 2.0-3.
0.
5. A polyurethane rigid foam material according to claim 1 or 2, It is characterized in that The foaming auxiliary additive composition comprises the following raw materials in parts by weight: 10-20 parts of polyether-polydimethylsiloxane copolymer, 30-40 parts of pentafluoropropane, 30-40 parts of trans-1-chloro-3,3,3-trifluoropropene, 1-3 parts of small molecule amine catalyst and 1-3 parts of organic tin catalyst.
6. A polyurethane rigid foam material according to claim 1 or 2, It is characterized in that The apparent density of the glass fiber continuous mat is 500-700 kg / m 2 , the organic content is 2-3wt%, each roll is 1-3m wide and 100-150m long.
7. A method for preparing a polyurethane rigid foam material, It is characterized in that The specific steps include: (1) Weighing the raw materials according to the weight proportion of the polyurethane rigid foam material according to any one of claims 1 to 6; (2) mixing a multifunctional polyether polyol, a multifunctional polyester polyol, toluene diisocyanate, polymethylene polyphenyl polyisocyanate and a foaming auxiliary additive composition to obtain a mixture; (3) pouring the mixture onto a flat glass fiber continuous mat, and then entering a confined space for foaming and molding to obtain a semi-finished product; (4) After the semi-finished product is naturally cured, it is cut into sections and cured again to obtain the polyurethane rigid foam material.
8. The method for preparing a polyurethane rigid foam material according to claim 7, It is characterized in that In step (2), the mixing equipment is a high-pressure mixing head with a pressure of 50-300 bar, a temperature of 15-35° C., and a discharge rate of 20-120 kg / min.
9. The method for preparing a polyurethane rigid foam material according to claim 7, It is characterized in that In step (3), the upper, lower, left and right sides of the confined space are all composed of high-strength chain plates; the thickness of the chain plates is 5-25 mm, the flatness is ±0.5-1 mm, the temperature is 15-45° C., and the forward speed is 0.5-2.5 m / min; The method also includes: using kraft paper to isolate the glass fiber continuous felt from the chain plate; the apparent density of the kraft paper is 90-250g / m 2 .
10. The method for preparing a polyurethane rigid foam material according to claim 7, It is characterized in that In step (4), the natural curing time is 15-35 minutes; the re-curing time is 48 hours; Steps (2) to (4) are carried out in a constant temperature and humidity environment, wherein the ambient temperature is 15-35° C. and the ambient humidity is below 80%.
Citation Information
Patent Citations
Polyurethane hard foam thermal insulation layer for low-temperature thermal insulation pipeline and preparation method of polyurethane hard foam thermal insulation layer
CN105601883A
High-fire-retardant glass fiber reinforced rigid polyurethane ultralow-temperature heat preserving material and manufacturing method thereof
CN107090074A
Enhanced polyurethane thermal insulation material for LNG liquid cargo containment system and preparation method of enhanced polyurethane thermal insulation material
CN110804149A
Polyurethane composite cryogenic insulation board and preparation method thereof
CN111231484A
Cryogenic insulation composite sandwich board and preparation method thereof