Biomass schiff base, biomass schiff base polymer, photo-thermal coating, and preparation method
By combining the biomass Schiff base with the epoxy resin system and multi-layer structure, the problems of wear resistance and self-healing performance of the photothermal anti-icing coating are solved, achieving high wear resistance and excellent anti-icing performance and extending the service life. The coating has a long service life and has a self-cleaning function.
Patent Information
- Application Number
- PCT/CN2023/091236
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2023-04-27
- Publication Date
- 2024-10-24
AI Technical Summary
The existing photothermal anti-icing coating has poor wear resistance, limited number of wear cycles, and does not use biomass raw materials, which affects its superhydrophobic and photothermal properties.
Biomass Schiff base and epoxy resin system are used to build a multi-layer structure through spraying method, combined with micro-nano structure and fluorinated ADP, to prepare a photothermal superhydrophobic anti-icing coating with self-healing properties, using two scales of nitrogen. Titanium oxide (nTiN and μTiN) is used as a filler to enhance the wear resistance and anti-icing performance of the coating.
It achieves high wear resistance and self-healing performance of the coating, extends the freezing time, improves photothermal de-icing efficiency, and has excellent self-cleaning function, significantly extending the service life of the coating.
Smart Images

Figure CN2023091236_24102024_PF_FP_ABST
Abstract
Description
A biomass Schiff base and its polymer, photothermal coating and preparation method Technical Field
[0001] The present invention belongs to polymer material technology, and specifically relates to a biomass Schiff base and its polymer, a photothermal coating and a preparation method. Background Art
[0002] Photothermal superhydrophobic anti-icing coatings are one effective solution to the problem of icing on wind turbine blades. To better absorb external light energy, the coating's photothermal fillers are often distributed on the material's surface. However, in actual use, external factors such as wind and sand can severely abrade the material's surface. This not only affects the material's superhydrophobicity and, in turn, its passive anti-icing properties, but also significantly impacts its photothermal performance. Therefore, wear resistance is particularly important for photothermal anti-icing materials. Existing technologies commonly suffer from the following problems: First, most photothermal anti-icing coatings lose their superhydrophobicity after only about 50 wear cycles, and the loads used in testing are only 50g to 100g. Anti-icing performance is also poor, with a freezing time of only 288s (compared to 57s for a blank sample). Furthermore, sustainable and green development is a key focus in the materials field today. However, no reports have been found using biomass raw materials to prepare wear-resistant photothermal anti-icing coatings. Technical issues
[0003] This paper designed and synthesized a biomass Schiff base monomer HD containing hydroxyl groups at both ends. A biomass epoxy resin system, HD-EP, was prepared through a ring-opening reaction between the hydroxyl groups and the epoxy groups of the epoxy resin TDE-85. The curing behavior and wetting properties of HD-EP were systematically studied. A highly wear-resistant photothermal anti-icing coating (HD-EP@yTiN) was prepared by spraying HD-EP, a mixture of μTiN and nTiN, and a mixture of ADP and FAS layer by layer onto a glass slide using a simple spray coating method. x / FADP z ), a new type of highly wear-resistant photothermal anti-icing coating. Technical Solutions
[0004] The present invention adopts the following technical solutions:
[0005] A biomass Schiff base is ((decane-1,10-diacylbis(nitrene divinylene))bis(methyl divinylene)bis(furan-5,2-diacyl))dimethanol.
[0006] The present invention discloses a method for preparing the above-mentioned biomass Schiff base, comprising the following steps: using 5-hydroxymethylfurfural and 1,10-diaminodecane as raw materials, reacting at 90-120°C for 0.5-3h to obtain the biomass Schiff base; preferably, using 5-hydroxymethylfurfural and 1,10-diaminodecane as raw materials, reacting at a molar ratio of 1:1 at 100-120°C for 0.5-2h to obtain the biomass Schiff base.
[0007] The present invention discloses a biomass Schiff base polymer obtained by curing an epoxy resin with the biomass Schiff base. Specifically, the biomass Schiff base is mixed with the epoxy resin and then cured to obtain the biomass Schiff base polymer. Preferably, the curing temperature is 180-220°C for 5-8 hours, and the curing time is stepwise increased, such as 180°C / 2h + 200°C / 2h + 220°C / 2h.
[0008] The present invention discloses a biomass Schiff base photothermal coating and a preparation method thereof, comprising the following steps: sequentially preparing a biomass Schiff base prepolymer-titanium nitride layer and a biomass Schiff base prepolymer-aluminum dihydrogen phosphate-fluorosilicone layer on a biomass Schiff base prepolymer film, followed by curing to obtain the biomass Schiff base photothermal coating. Preferably, the curing temperature is 180-220°C for 5-8 hours, and the curing time is a stepwise heating cycle, such as 180°C / 2h + 200°C / 2h + 220°C / 2h.
[0009] In the present invention, the titanium nitride in the biomass Schiff base prepolymer-titanium nitride layer comprises micronized titanium nitride and nanometerized titanium nitride. In the biomass Schiff base prepolymer-aluminum dihydrogen phosphate-fluorosilicone layer, the fluorosilicone is tridecafluorooctylsiloxane. Preferably, the mass ratio of micronized titanium nitride to nanometer titanium nitride in the titanium nitride is 1:(0.25-1).
[0010] In the present invention, the biomass Schiff base prepolymer is a mixture of the above-mentioned biomass Schiff base and epoxy resin; and then solidified to obtain a biomass Schiff base polymer. The above-mentioned biomass Schiff base and epoxy resin are mixed in a solvent, and then divided into three parts, namely mixed solution A, mixed solution B, and mixed solution C; the mixed solution B is mixed with titanium nitride in a solvent to obtain a biomass Schiff base-titanium nitride mixed solution; the mixed solution C is mixed with aluminum dihydrogen phosphate and fluorosilicone in a solvent to obtain a biomass Schiff base-aluminum dihydrogen phosphate-fluorosilicone mixed solution; the mixed solution A is dried to obtain a biomass Schiff base prepolymer film; the biomass Schiff base-titanium nitride mixed solution is dried to obtain a biomass Schiff base prepolymer-titanium nitride layer; the biomass Schiff base-aluminum dihydrogen phosphate-fluorosilicone mixed solution is dried to obtain a biomass Schiff base prepolymer-aluminum dihydrogen phosphate-fluorosilicone layer. Preferably, the drying is carried out by keeping the temperature at 70-90°C for 1-5 minutes. The solvent in the solution is a conventional solvent, such as ethanol. Preferably, the solvent is consistent and is ethanol.
[0011] In the present invention, the total volume of mixed liquid A, mixed liquid B, and mixed liquid C is 100%, wherein the volume of mixed liquid B is 20-40%, the volume of mixed liquid C is 15-30%, and the remainder is mixed liquid A; the mass sum of the biomass Schiff base and the epoxy resin is the mass of the resin matrix, and the mass ratio of the resin matrix, titanium nitride, aluminum dihydrogen phosphate, and fluorosilicone is 100:(55-80):(3-9):(30-40).
[0012] The present invention discloses a photothermal anti-icing material, comprising a substrate and a biomass Schiff base photothermal coating on its surface, wherein the biomass Schiff base photothermal coating is the above-mentioned biomass Schiff base photothermal coating.
[0013] The present invention discloses the application of the above-mentioned biomass Schiff base, biomass Schiff base polymer, and biomass Schiff base photothermal coating in the preparation of anti-icing coating; and the application of the above-mentioned photothermal anti-icing material in the preparation of wind turbine blade materials, especially coating materials.
[0014] This study used biomass-based 5-hydroxymethylfurfural and 1,10-diaminodecane as raw materials to synthesize a Schiff base (HD) containing a hydroxymethyl structure via a one-step method. HD was used as a curing agent and combined with a trifunctional epoxy resin (e.g., 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ester, TDE-85) to construct an epoxy resin system. A resin coating (HD-EP) was spray-coated on a glass slide. The HD-EP exhibited a contact angle of 95.7°, indicating a hydrophobic state. The surface energy calculated using the two-liquid method (Owens-Wendt-Kaelble) was 16.66 mN / m. At -20°C, a droplet on a glass slide froze after only 37 seconds, while it took 120 seconds on the HD-EP surface to freeze, a 2.24-fold increase in freezing time.
[0015] The present invention adopts a layer-by-layer spraying method, wherein the first layer is a HD / EP resin solution, the second layer is a HD / EP resin-micron titanium nitride (μTiN) and nano-TiN (nTiN) mixed solution, and the third layer is a HD / EP resin-aluminum dihydrogen phosphate (ADP)-tridecafluorooctylsiloxane (FAS) mixed solution sprayed in sequence to prepare a new resin-based composite coating (denoted as HD-EP@yTiN). x / FADP z ), where HD-EP@cTiN 75FADP7 exhibits excellent superhydrophobicity, with a WCA of 165.5° and a SA of 4°. It also exhibits exceptional wear resistance, maintaining its superhydrophobicity after 100 abrasion cycles on 1200# sandpaper. The coating also exhibits excellent anti-icing properties, with droplets freezing for 446 seconds at -20°C. Frozen droplets completely melt in just 10 seconds under 808nm near-infrared light. This excellent wear resistance is attributed to the synergistic effect of the resin system and the filler protective layer.
[0016] Icing of wind turbine blades has severely hampered the development of wind power, and photothermal super-hydrophobic anti-icing coatings are an important strategy for addressing this issue. However, existing photothermal super-hydrophobic anti-icing coatings generally suffer from low wear resistance. This paper investigates a novel, highly wear-resistant photothermal super-hydrophobic anti-icing resin-based composite coating, improving its wear resistance without compromising its anti-icing performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a schematic diagram of the synthesis of Schiff base HD.
[0018] Figure 2 shows the characterization of HD, where A is the H-NMR spectrum, B is the C-NMR spectrum, and C is the FT-IR spectrum of HMF and HD.
[0019] Figure 3 shows pictures of HD-EP before and after self-repair, where a is before self-repair and b is after self-repair, both magnified 200 times under an ultra-depth-of-field microscope.
[0020] Figure 4 shows the WCA and SA of the coating HD-EP@yTiNx / FADP.
[0021] Figure 5 shows the SEM images of different coatings, where a is HD-EP@μTiN 75 / FADP7, b is HD-EP@dTiN 75 / FADP7, c is HD-EP@cTiN 75 / FADP7, d is HD-EP@bTiN 75 / FADP7, e is HD-EP@aTiN 75 / FADP7 and f are HD-EP@nTiN 75 / FADP7.
[0022] Figure 6 is a schematic diagram of the changes in WCA and SA of the composite coating with wear cycles.
[0023] Figure 7 HD-EP@cTiN 75 HD-EP@cTiN 75 SEM images of / FADP7 before and after 100 wear tests, where a is HD-EP@cTiN 75Before coating wear, b is HD-EP@cTiN 75 After coating wear, c is HD-EP@cTiN 75 / FADP7 coating before wear, d is HD-EP@cTiN 75 / FADP7 coating after wear.
[0024] Figure 8 shows a glass slide, HD-EP resin coating, and HD-EP@cTiN 75 / Icing delay time test and deicing test of FADP7 coating.
[0025] Figure 9 shows the freezing delay time test of different coatings.
[0026] Figure 10 is a schematic diagram of the surface temperature of different coatings changing with time. The highest temperature of each curve in the figure is taken as the standard. From top to bottom, HD-EP@cTiN 75 / FADP、HD-EP@cTiN 70 / FADP、HD-EP@cTiN 65 / FADP、HD-EP@cTiN 60 / FADP、HD-EP@cTiN 55 / FADP、HD-EP@cTiN 50 / FADP、HD-EP@μTiN 75 / FADP.
[0027] Figure 11 shows HD-EP@cTiN 75 / Photos of FADP7 before and after self-repair.
[0028] Figure 12 shows HD-EP@cTiN 75 / Schematic diagram of the self-cleaning function of FADP7. Modes for Carrying Out the Invention
[0029] A feasible way to increase the service life of anti-icing coatings is to introduce self-repairing properties into the resin coating. The self-repairing properties of anti-icing coatings generally include two meanings. One is that when the coating surface loses its super-hydrophobic properties due to structural damage, oxygen erosion, etc., the super-hydrophobic properties can be restored under certain conditions. The other is that the coating can self-repair surface scratches under certain conditions. At present, there is relatively little public information about self-repairing anti-icing coatings. The self-repairing properties of existing super-hydrophobic anti-icing coatings with self-repairing properties are limited to the recovery of super-hydrophobic properties. This self-repair is achieved by the migration of low surface energy segments to the surface of the material. Other repairs are achieved by melting components with low melting points, which means that the material has poor heat resistance and cannot be used to prepare photothermal anti-icing coatings. In addition, the curing agents containing dynamic covalent bonds used in the existing technologies are all petroleum-based raw materials, and no renewable biomass raw materials are used. The present invention uses biomass raw materials to synthesize a new biomass Schiff base, and uses it as an epoxy resin curing agent to prepare an epoxy resin with self-healing properties for preparing a photothermal superhydrophobic anti-icing coating. First, 5-hydroxymethylfurfural (HMF) and 1,10-diaminodecane (DAD) are used as biomass raw materials to solvent-free synthesize a long alkyl chain Schiff base (HD) with two alcoholic hydroxyl end-capping groups. Then, HD is used to cure the trifunctional epoxy resin TDE-85 to prepare a new self-healing epoxy resin coating HD-EP.
[0030] It is well known that superhydrophobicity, a key performance factor in passive anti-icing, stems from the synergistic effect of the coating material's surface structure and low surface energy. However, in practical applications, the long-term wear and tear of wind and sand on the coating material surface is difficult to ignore, especially for anti-icing coatings on outdoor equipment such as wind turbine blades, which are exposed to wind and sand erosion for a long time. As the surface structure is constantly damaged by wear and tear, the superhydrophobicity of the coating will continue to decrease, significantly affecting the coating's anti-icing performance. In addition, for photothermal anti-icing coatings, in order to better absorb light energy, photothermal fillers are often distributed on the surface of the coating. However, the accumulated wear and tear from wind and sand can cause the photothermal fillers to fall off, affecting the photothermal performance. In summary, wear resistance is an important property that determines whether the anti-icing coating can function properly in practical applications. The existing technology generally has the following problems: First, most photothermal anti-icing coatings have poor wear resistance, losing their superhydrophobicity after only about 50 wear cycles. Moreover, there is no evidence of the material's self-repairing properties. At most, it can be achieved through the melting of beeswax, which is a non-intrinsic self-repairing method and has a limited number of repair cycles. In addition, sustainable green development is the key direction of development in the field of materials today. There are no reports on the use of biomass raw materials as coating raw materials in existing wear-resistant, light-heat and anti-icing coatings.
[0031] This invention discloses a photothermal super-hydrophobic anti-icing resin-based composite coating with both self-healing properties and high wear resistance. The solution uses μTiN and nTiN to construct a surface micro-nanostructure combined with fluorinated ADP. The self-healing epoxy resin prepared above strengthens the adhesion between the filler and the substrate. The resulting coating exhibits excellent structure and performance, including super-hydrophobicity, good wear resistance, and anti-icing properties.
[0032] 1,10-Diaminodecane (DAD) and petroleum ether were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (China), 4,5-epoxytetrahydrophthalic acid diglycidyl ester (TDE-85) and 5-hydroxymethylfurfural (HMF) were purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (China), and anhydrous ethanol was purchased from Yonghua Chemical Co., Ltd. (China). Tridecafluorooctylsiloxane (FAS) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (China), nano-titanium nitride (nTiN, 20-100 nm) and micro-titanium nitride (μTiN, 2-10 μm) were purchased from Shanghai Yuanye Biotechnology Co., Ltd. (China), and aluminum dihydrogen phosphate (ADP) was purchased from Shanghai Adamas Reagent Co., Ltd. (China). All reagents were not subjected to additional treatment. The raw materials used in this invention are existing products, and the specific preparation procedures and testing methods are conventional techniques.
[0033] The nuclear magnetic resonance spectra (HNMR) were recorded using an AVANCE III HD-400 nuclear magnetic resonance spectrometer ( 1 H-NMR) and carbon nuclear magnetic resonance spectroscopy ( 13 C-NMR). Deuterated chloroform (CDCl3) was used as the solvent and tetramethylsilane (TMS) was used as the internal standard.
[0034] The infrared spectrum (FTIR) was tested using a Vertex 70 intelligent Fourier transform infrared spectrometer with a scanning range of 600-4000 cm -1 , with a resolution of 4cm -1 .
[0035] High-resolution mass spectra (HRMS) were obtained using an Ultimate 3000 HPLC in ESI mode. + .
[0036] The reactivity of the resin prepolymer was measured using a Q200 differential scanning calorimeter (DSC) under a nitrogen atmosphere (flow rate: 50 mL min -1 ), the heating rate is 5℃min -1 、10℃min -1 、15℃min -1 and 20℃min -1 About 4 mg of sample was weighed in an aluminum crucible and sealed, and the scanning temperature range was from room temperature to 300 °C.
[0037] An ultra-depth-of-field camera (VHX-7000) was used to record images of scratches before and after self-repair of the coating, with a magnification of 200 times.
[0038] The water contact angle (WCA) and sliding angle (SA) of the coating were measured using an LSA60Pro contact angle meter. The ambient temperature during the test was 25°C, the droplet volume used in the WCA test was 4 μL, and the droplet volume used in the SA test was 6 μL.
[0039] The surface morphology of the coating was analyzed using a Hitachi S-4700 cold field emission scanning electron microscope (SEM).
[0040] The roughness and morphology of the coating surface were analyzed using Dimension Icon’s atomic force microscope (AFM).
[0041] The absorption spectrum of the coating in the wavelength range of 300~1000nm was recorded using an ultraviolet-visible-near-infrared spectrophotometer (UV3600). The absorption spectrum was obtained by the formula A=1-TR, where T is the transmission and R is the reflection.
[0042] The photothermal conversion performance of the coating was measured and recorded using an infrared thermal imager (PI640i). The 808nm near-infrared light used in the measurement process came from an infrared laser (MDL-H-808-5W) with an energy density of 1W / cm 2 .
[0043] The anti-icing performance of the coating was tested on a freezing table with an ambient temperature of 20°C, a humidity of 47%, and a surface temperature of -20°C. The test method is as follows: the coating sample to be tested is placed flat on the freezing table, 10μL of deionized water is added to the coating surface using a pipette, and the passive anti-icing performance of the coating is evaluated by measuring the time when the droplet begins to form a solid-liquid interface and the time when the droplet is completely frozen. Under the same environmental conditions, an energy density of 1W / cm 2 The coating was irradiated vertically with near-infrared light, and the photothermal deicing performance of the coating was evaluated by recording the time it took for a 10 μL completely frozen droplet to turn back into liquid.
[0044] The mechanical durability of the coating was investigated using a sandpaper abrasion test. In this test, the coating was dragged on 1200# sandpaper at a constant speed for 10 cm under a load of 100g. The contact angle and rolling angle after abrasion were measured. The number of cycles before the coating completely lost its superhydrophobic properties was recorded to assess the coating's wear resistance.
[0045] Example 1 Synthesis of Schiff base ((decane-1,10-diacylbis(nitrene divinylene))bis(methyl divinylene)bis(furan-5,2-diacyl)) dimethanol (HD).
[0046] A solvent-free method was used to synthesize the all-bio-based Schiff base curing agent HD. 2.649g HMF was added to a round-bottom flask, and placed in a magnetic stirring oil bath with a water separator and a condensing reflux device installed, and magnetic stirring was turned on. Then 1.721g DAD was evenly added in 5 batches, and the mixture was reacted at 110°C for 1h. After the reaction, 200mL of deionized water and 200mL of petroleum ether were used for washing, and then the water and the remaining reactants were removed by vacuum evaporation at 80°C. After drying, the biomass Schiff base HD was obtained with a yield of 95%. The reaction diagram and the chemical structure of the product are shown in Figure 1. In Figure 2, A is HD 1 H NMR (400 MHz, Chloroform-d) diagram; B in Figure 2 is HD 13 C NMR (101 MHz, Chloroform-d) diagram. In Figure 2, C is the FT-IR spectrum of HMF and HD, where 1686 cm -1 is the stretching vibration peak of C=O in the aldehyde group, and after the reaction, 1686 cm -1 The peak at 1650cm -1 The stretching vibration peak at the C=N imine bond appears, indicating the reaction between the aldehyde group and the amino group. The mass spectrometry of HD showed a molecular mass of 411.2252, which is consistent with the theoretical value of 411.2260 for HD.
[0047] Example 2 HD-EP resin coating.
[0048] 0.304g of TDE-85, 0.396g of HD, and 10mL of anhydrous ethanol were added to a beaker and stirred at room temperature for 30 minutes to obtain resin spray solution A. A 75×25 mm microscope slide was cleaned with deionized water and ethanol to serve as the coating substrate. Spray solution A was sprayed onto the cleaned slide using spray parameters of 2 bar and 15 cm. After each application of 2mL of spray solution A, the solution was maintained at 80°C for 2 minutes to evaporate the solvent. The sprayed coating was cured using a process of 180°C / 2h, 200°C / 2h, and 220°C / 2h to obtain an HD-EP resin coating with a thickness of 30.84μm.
[0049] HD and TDE-85 were mixed in a 1:1 molar ratio and stirred at 180°C for 30 minutes to obtain an HD-EP prepolymer. DSC curves at different heating rates were used to study the curing behavior of the HD-EP prepolymer. Each curve exhibited a distinct curing exothermic peak in the range of 200-250°C. Using the tangent method for the curing exothermic peak, the curing onset temperature (T) of each curve was determined. i ), curing peak temperature (T p ) and the curing end temperature (T f ), as shown in Table 1. Then, the T i 、T p 、T f Linear fitting was performed separately and the obtained straight line was extrapolated to 0℃ / min. It can be seen that the T i 、
[0050] T p 、T f They are 180℃, 198℃ and 222℃ respectively.
[0051]
[0052] The WCA test of HD-EP resin coating was conducted using a contact angle meter. The WCA of water drop on HD-EP surface was 95°, indicating that the coating is hydrophobic. Since the wettability of the coating is closely related to the surface energy of the material, the surface energy of HD-EP was analyzed using a two-liquid method. First, the WCA of water and formamide on the HD-EP surface were tested, which were 95° and 86° respectively. The r d L With r p L According to the Owens-Wendt-Kaelble method, the surface energy of the HD-EP resin coating can be obtained as follows: s =16.660mN / m.
[0053] A scratch was made on the HD-EP resin coating using a scalpel, measuring 65.03 μm wide and 20.18 μm deep. The scratched coating was then heated at 180°C for 30 minutes and re-examined under an ultra-depth microscope. The scratch width had shrunk to 28.93 μm and the depth was 5.65 μm. See Figure 3 for images of the HD-EP self-healing process before and after, magnified 200x under an ultra-depth microscope. The repair efficiency (n) of the HD-EP coating under these conditions is 55.5%, calculated using the following formula: n = (W1 - W2) / W1 × 100%, where W1 is the scratch width before and after repair, and W2 is the scratch width after repair.
[0054] Example 3: Preparation of photothermal coating by layer-by-layer spraying method
[0055] The substrate is a 75×25 mm microscope slide, which is cleaned with deionized water and ethanol in sequence before use and set aside.
[0056] (1) Preparation of μTiN-based coating HD-EP@xTiNy / FADP
[0057] 0.304 g of TDE-85, 0.396 g of HD and 10 mL of anhydrous ethanol were added to a beaker and stirred at room temperature for 30 min to obtain spray liquid A. A portion of the solution was taken out to prepare spray liquids B and C.
[0058] μTiN was added into a beaker, and 5 mL of anhydrous ethanol and 3 mL of spray liquid A were added thereto. The mixture was dispersed in an ultrasonic instrument for 30 minutes to obtain spray liquid B.
[0059] Spray liquid C was obtained by mixing 0.05 g ADP, 0.25 g FAS, 2 mL spray liquid A, and 3 mL anhydrous ethanol.
[0060] Using spray parameters of 2 bar and 15 cm, spray liquid A (the remaining spray liquid A), spray liquid B, and spray liquid C were sprayed layer by layer onto a clean glass slide. After each spray layer, the coating was kept at 80°C for 2 minutes to evaporate the solvent. The sprayed coating was cured using a process of 180°C / 2h + 200°C / 2h + 220°C / 2h to obtain a μTiN-based coating, designated HD-EP@μTiN. x / FADP7, where x is the mass percentage of μTiN relative to HD-EP resin (actually x%, % is omitted in the name for simplicity), and FADP7 means that the mass percentage of ADP relative to HD-EP resin is 7% (% is omitted in the name for simplicity), see Table 2 for details. For example, if the mass of HD-EP resin is 0.7 g and the mass of μTiN is 0.35 g, then x is 50%, abbreviated as 50.
[0061]
[0062] (2) HD-EP@yTiN coating containing two sizes of fillers x / FADP z Preparation
[0063] 0.304 g of TDE-85, 0.396 g of HD and 10 mL of anhydrous ethanol were added to a beaker and stirred at room temperature for 30 min to obtain spray liquid A. A portion of the solution was taken out to prepare spray liquids C and D.
[0064] 0.05 g ADP, 0.25 g FAS, 2 mL spray liquid A, and 3 mL anhydrous ethanol were mixed to obtain spray liquid C, i.e., a biomass Schiff base-aluminum dihydrogen phosphate-fluorosilicone mixed liquid.
[0065] μTiN and nTiN were added to a beaker, and 5 mL of anhydrous ethanol and 3 mL of spray liquid A were added, and dispersed in an ultrasonic instrument for 30 minutes to obtain spray liquid D, that is, a biomass Schiff base-titanium nitride mixed liquid.
[0066] Using the spray parameters of 2 bar and 15 cm, spray liquid A (the remaining spray liquid A), spray liquid D, and spray liquid C were sprayed layer by layer on a clean glass slide. After each layer was sprayed, the temperature was kept at 80°C for 2 minutes to evaporate the solvent. The sprayed coating was cured according to the process of 180°C / 2h + 200°C / 2h + 220°C / 2h. The obtained coating was named HD-EP@yTiN x / FADP z , where y represents the mass ratio of μTiN to nTiN (when μ:n is 1:1, y=a; when μ:n is 1:0.75, y=b; when μ:n is 1:0.5, y=c; when μ:n is 1:0.25, y=d), x represents the mass of the two TiN fillers and their mass percentage relative to the HD-EP resin (actually x%, for simplicity, % is omitted in the name), and z represents the mass percentage of ADP relative to the HD-EP resin (actually z%, for simplicity, % is omitted in the name), see Table 3.
[0067]
[0068] HD-EP@μTiN x / FADP7 coating, HD-EP@μTiN 75 The WCA of / FADP7 is the maximum (125.2°) and the SA is the minimum (21.2°), which does not meet the superhydrophobicity requirement, that is, the coating surface has a WCA greater than 150° and a SA less than 10°. 75 The surface structure of / FADP7 is very fragile, and droplets can easily penetrate into the coating, making the coating non-hydrophobic (WCA less than 90°). Obviously, the composite coating with only μTiN or nTiN added does not have superhydrophobic properties.
[0069] Figure 4 shows HD-EP@yTiN 0.75 / FADP7's WCA and SA. It can be seen that when the micro-nano ratio gradually decreases, the WCA of the coating shows a trend of first increasing and then decreasing, while the SA shows the opposite trend. When the micro-nano ratio is 1:0.25, the WCA and SA of the coating are 153° and 7.5°, respectively, and it has superhydrophobic properties. When the micro-nano ratio reaches 1:0.5, the coating has the best superhydrophobic properties, with WCA reaching 165.5° and SA reaching 4°. Continuing to increase the content of nTiN to make the micro-nano ratio reach 1:0.75, the WCA and SA show a trend of decreasing and increasing, respectively, reaching 151° and 9°. When the micro-nano ratio reaches 1:1, the WCA and SA of the coating are 128.2° and 26.4°, respectively, and the coating no longer has superhydrophobic properties.
[0070] The surface SEM characterization of the coating was carried out (Figure 5). At a magnification of 2.5K, it can be found that the coating HD-EP@μTiN 0.75 / FADP7's structure does not meet the conditions for super-hydrophobicity, and the tested contact angle is only 125.2°. When the micro-nano ratio changes from 1:0 to 1:0.25, many tiny nano-scale protrusions can be observed on the micron-scale protrusion structure. When the micro-nano ratio reaches 1:0.5, the structure of the coating surface becomes more complicated, and many gully-like cracks appear. At this time, the coating has the best super-hydrophobic properties. After continuing to increase the content of nTiN to make the micro-nano ratio reach 1:0.75 and 1:1, the super-hydrophobic properties continue to decrease with the increase of nTiN content, and even lose the super-hydrophobic properties. For the coating HD-EP@nTiN containing only nTiN 0.75 / FADP7, the surface structure of the coating is very fragile at this time, and the droplets will penetrate into the scratches after the coating is repaired, making the coating lose its superhydrophobic properties.
[0071] Traditional methods for improving coating wear resistance primarily involve adding epoxy resins, polysiloxanes, and other materials to enhance the adhesion between fillers and substrates and create unique surface structures, such as embedded structures. However, these methods only prevent fillers from falling off during wear but cannot prevent damage to the surface structure caused by wear. This invention utilizes aluminum dihydrogen phosphate (ADP) as a protective shell for the surface structure. Through the synergistic effect of ADP and the resin system, the coating's wear resistance is enhanced.
[0072] The wear resistance of the coating was tested by sandpaper polishing. Figure 6 is HD-EP@cTiN 75 / FADP zSchematic diagram of the change of WCA and SA with the increase of wear test cycles. It can be found that with the increase of the number of cycles, the WCA of the coating gradually shows a downward trend, and the SA shows an upward trend. When the mass fraction of ADP reaches 7%, even if the wear cycle reaches 100 times, the coating HD-EP@cTiN 75 The WCA and SA of / FADP7 are still 152.1° and 7.6°. This shows that the coating has excellent wear resistance. After increasing the ADP content to 9 wt%, although the change in wettability before and after wear is smaller than that of other components, the superhydrophobicity before wear is reduced, and the WCA and SA are 155° and 6.5° respectively. 75 When the number of wear times reaches 30, SA is greater than 10°; when the number of wear times exceeds 50, WCA is also less than 150°.
[0073] Figure 7 is HD-EP@cTiN 75 HD-EP@cTiN 75 SEM images of / FADP7 before and after wear test. 75 Before wear, the coating surface had distinct light and dark areas due to its obvious ups and downs, which means it had a high roughness. However, after 100 wear cycles, the micro-nanostructure of the coating surface was severely damaged, and a large area of flat area appeared in the field of view. 75 / FADP7 has a high-low, dense surface. After 100 wear tests, the surface structure composed of obvious protrusions and grooves can still be observed. AFM was used to observe the surface of HD-EP@cTiN 75 HD-EP@cTiN 75 / FADP7 roughness before and after wear test was characterized. After 100 wear cycles, HD-EP@cTiN 75 The structure of HD-EP@cTiN was severely damaged, and the roughness was greatly reduced from 539nm to 178nm. 75 The roughness of / FADP7 only decreased from 534 nm to 467 nm after 100 wear cycles, indicating that the coating has excellent wear resistance.
[0074] Compared with the prior art photothermal super hydrophobic anti-icing coating involving wear resistance, the coating HD-EP@cTiN 75 / FADP7 has relatively better wear resistance and comprehensive performance, and the number of wear cycles is greater than that of most existing technologies. It solves the problem that existing coatings have good wear cycle performance but poor anti-icing performance and short freezing time, making them difficult to use as surface coatings for wind turbine blades.
[0075] The anti-icing and de-icing performance of the coating. The passive anti-icing performance of the coating was studied by measuring the ice delay time. 75 The three groups of test samples of / FADP7 were placed on a -20℃ freezer. 10μL of deionized water was added to the sample surface, and the freezing process of the droplet was observed and recorded. As shown in Figure 8, the contact angles of the droplet on the glass slide and the resin coating were all less than 90°, while on the HD-EP@cTiN 75 / FADP7 surface is greater than 150°, showing a relatively complete spherical shape, indicating that the coating still has super hydrophobic properties even at a low temperature of -20°C. In order to record the time when the droplet freezes on the sample surface, the time when a clear solid-liquid interface appears inside the droplet is selected as the starting freezing time of the droplet, and the time when the liquid phase is completely frozen into the solid phase is the freezing end time. The results show that the starting freezing time and the ending freezing time of the blank component slide are 4s and 37s respectively, HD-EP are 91s and 120s, and HD-EP@cTiN 75 / FADP7 is 289s and 446s, and even if completely frozen, the droplets on the coating still maintain a spherical shape. 75 The freezing time of the FADP7 coating was extended by 12 times compared with the blank sample, which shows that it has good passive anti-icing ability.
[0076] In order to study the photothermal deicing performance of the coating, a 1W / cm 2 The energy density of 808nm laser is used to simulate sunlight, which is vertically irradiated onto the frozen droplets on the coating surface to observe and record the melting phenomenon of the droplets. As shown in Figure 8, HD-EP@cTiN 75 The ice on the surface of the FADP7 coating melted rapidly within 10 seconds of irradiation, and the melted droplets still maintained a spherical shape. However, even after irradiation for 100 seconds, the droplets on the glass slide and the resin coating showed no signs of melting. The above results show that HD-EP@cTiN 75 / FADP7 coating has excellent photothermal deicing performance and can completely melt frozen droplets on the surface in a short time.
[0077] In addition, HD-EP@aTiN was also tested 75 / FADP7、HD-EP@bTiN 75 / FADP7, HD-EP@dTiN 75 / FADP7 and HD-EP@μTiN 75 / FADP7 freezing time, as shown in Figure 9, the coating HD-EP@dTiN 75The initial freezing time and final freezing time of FADP7 are 285s and 375s respectively. 75 / FADP7 were 262s and 364s respectively, while the coating HD-EP@aTiN 75 / FADP7、HD-EP@μTiN 75 / FADP7 does not have superhydrophobic properties, so its passive anti-icing performance is also poor. The former is 146s and 253s, while the latter is 116s and 194s.
[0078] Using infrared thermal imaging to study HD-EP@cTiN 75 / FADP7 at 1W / cm 2 As shown in Figure 10, when the near-infrared laser irradiates the sample surface, the surface temperature of all component samples rises rapidly in a short period of time. 75 / FADP7 coating reached 97.4℃; it is worth noting that the single-scale coating HD-EP@μTiN x / FADP7 even with dual-scale coating HD-EP@cTiN x / FADP7 has the same mass fraction, and its temperature after 50s of illumination is only 67.9℃.
[0079] Figure 11 is the coating HD-EP@cTiN 75 / Super-depth microscopic images of FADP7 surface scratches before and after repair. The coating surface was scratched with a scalpel to create a 71.05μm wide and 29.85μm deep scratch. Then, an energy density of 2W / cm 2 The scratched area was irradiated with 808nm near-infrared light for 30 minutes, and then pictures of the scratched area after repair were taken. After 30 minutes of coating repair, it can be observed that the scratch on the resin is no longer obvious, and the middle of the scratch has healed after repair. It is not a continuous scratch. This is because the resin on both sides of the scratch drives the migration of nTiN, μTiN and ADP bonded to the resin during the self-repair process, so that the damaged surface structure is repaired to a certain extent. The width of the scratch after repair is 45.76μm and the depth is 13.58μm. The calculated repair efficiency is 35.7%. Although HD-EP@cTiN 75 The repair efficiency of / FADP7 is lower than that of HD-EP, but the coating HD-EP@cTiN 75 / FADP7 has good light-to-heat conversion function, so it can convert the energy-intensive thermal self-repair into energy-saving and regionally controllable light self-repair.
[0080] Many surfaces in everyday life eventually become contaminated due to the accumulation of dust and dirt. For photothermal coatings, dust accumulation significantly reduces the coating's light absorption efficiency. This wastes significant capital, labor, and energy during the cleaning process. Self-cleaning superhydrophobic coatings offer a promising solution to this problem. Liquid droplets roll off the tilted coating, trapping dust within the droplets and achieving self-cleaning functionality.
[0081] Figure 12 is the coating HD-EP@cTiN 75 Schematic diagram of the self-cleaning function of FADP7. 1g of sand was sprinkled on the surface of the coating, and the coating was placed in a culture dish at an angle of about 10°. 3mL of deionized water was then dripped onto the coating with a dropper. It can be observed that the sand on the surface of the coating was removed from the coating as the droplet rolled down and eventually flowed into the culture dish. After the 3mL of deionized water was dripped, it was found that there was basically no sand left on the coating, indicating that HD-EP@cTiN 75 / FADP7 has good self-cleaning function.
[0082] Compared with other anti-icing technologies, photothermal anti-icing coatings have the advantages of energy saving and high efficiency. They are the most promising representatives of anti-icing materials, and their applications cover many fields such as aerospace, energy industry, and civil transportation. However, wear resistance has always been one of the most important properties of photothermal anti-icing coating materials. Therefore, the research and development of resin-based photothermal anti-icing coatings with high wear resistance is of great significance. The icing problem of wind turbine blades has seriously hindered the development of wind power energy, and photothermal superhydrophobic anti-icing coatings are an important strategy to solve this problem. However, existing photothermal superhydrophobic anti-icing coatings generally have the problem of low wear resistance.
[0083] This paper uses green biomass raw materials and a solvent-free method to synthesize a biomass Schiff base, which is then reacted with epoxy resin TDE-85 to prepare an epoxy resin HD-EP with self-healing function. Using resin HD-EP as a coating adhesive, two sizes of TiN (nTiN and μTiN) as fillers and surface micro-nanostructure building materials, and fluorinated ADP, a photothermal superhydrophobic anti-icing coating HD-EP@yTiN with high wear resistance and self-healing performance is prepared by a layer-by-layer spraying method. x / FADP z The coating has excellent super-hydrophobic properties, with a WCA of 165.5° and a SA of 4°. The coating has good wear resistance and can maintain super-hydrophobic properties after 100 sandpaper wear tests. The coating HD-EP@cTiN 75 / FADP7 has good anti-icing performance. Its freezing time at -20℃ is extended to 446s, which is 12 times longer than that of the glass substrate. In addition, under near-infrared light, it only takes 10s to completely melt the ice. Especially the HD-EP@cTiN coating 75 / FADP7 has a certain light self-repair ability, and can achieve a repair rate of 35.7% within 30 minutes under 808nm near-infrared light irradiation; in addition, the coating has excellent self-cleaning function and can complete the self-cleaning function of 1g of sand with 3mL of deionized water.
Claims
1. A biomass Schiff base, which is ((decane-1,10-diacylbis(nitrene divinylene))bis(methyl divinylene)bis(furan-5,2-diacyl))dimethanol.
2. The method for preparing the biomass Schiff base according to claim 1, characterized in that: The method comprises the following steps: taking 5-hydroxymethylfurfural and 1,10-diaminodecane as raw materials, reacting at 90-120° C. for 0.5-3 hours to obtain a biomass Schiff base.
3. A biomass Schiff base polymer, characterized in that: Obtained by curing the epoxy resin with the biomass Schiff base as claimed in claim 1.
4. A method for preparing a biomass Schiff base photothermal coating, characterized in that: The method comprises the following steps: sequentially preparing a biomass Schiff base prepolymer-titanium nitride layer and a biomass Schiff base prepolymer-aluminum dihydrogen phosphate-fluorosilicone layer on a biomass Schiff base prepolymer film, and then curing the layers to obtain a biomass Schiff base photothermal coating; the biomass Schiff base prepolymer is a mixture of the biomass Schiff base and epoxy resin described in claim 1.
5. The method for preparing the biomass Schiff base photothermal coating according to claim 4, characterized in that: The curing temperature is 180-220°C, the time is 5-8 hours, and the curing adopts step-by-step temperature increase; in the biomass Schiff base prepolymer-titanium nitride layer, the titanium nitride is composed of micron titanium nitride and nano titanium nitride in a mass ratio of 1: (0.25-1); in the biomass Schiff base prepolymer-aluminum dihydrogen phosphate-fluorosilicone layer, the fluorosilicone is tridecafluorooctylsiloxane.
6. The method for preparing the biomass Schiff base photothermal coating according to claim 4, characterized in that: The biomass Schiff base described in claim 1 is mixed with epoxy resin in a solvent, and then divided into three parts, namely, mixed solution A, mixed solution B, and mixed solution C; the mixed solution B is mixed with titanium nitride in a solvent to obtain a biomass Schiff base-titanium nitride mixed solution; the mixed solution C is mixed with aluminum dihydrogen phosphate and fluorosilicone in a solvent to obtain a biomass Schiff base-aluminum dihydrogen phosphate-fluorosilicone mixed solution; the mixed solution A is dried to obtain a biomass Schiff base prepolymer film; the biomass Schiff base-titanium nitride mixed solution is dried to obtain a biomass Schiff base prepolymer-titanium nitride layer; the biomass Schiff base-aluminum dihydrogen phosphate-fluorosilicone mixed solution is dried to obtain a biomass Schiff base prepolymer-aluminum dihydrogen phosphate-fluorosilicone layer.
7. The method for preparing the biomass Schiff base photothermal coating according to claim 6, characterized in that: The total volume of mixed liquid A, mixed liquid B and mixed liquid C is 100%, wherein the volume of mixed liquid B is 20-40%, the volume of mixed liquid C is 15-30%, and the remainder is mixed liquid A; the mass of the resin matrix is the sum of the masses of the biomass Schiff base and the epoxy resin, and the mass ratio of the resin matrix, titanium nitride, aluminum dihydrogen phosphate and fluorosilicone is 100: (55-80): (3-9): (30-40).
8. The biomass Schiff base photothermal coating prepared according to the method for preparing the biomass Schiff base photothermal coating according to claim 4.
9. A photothermal anti-icing material, comprising a substrate and a biomass Schiff base photothermal coating on its surface, characterized in that: The biomass Schiff base photothermal coating is the biomass Schiff base photothermal coating according to claim 8.
10. Use of the biomass Schiff base described in claim 1, the biomass Schiff base polymer described in claim 3, or the biomass Schiff base photothermal coating described in claim 8 in the preparation of an anti-icing coating; or use of the photothermal anti-icing material described in claim 9 in the preparation of a fan blade coating material.
Citation Information
Patent Citations
Bio-acrylic acid ester based on schiff base structure and preparation method and application thereof
CN106916083A
Ultra-thin silicon steel surface insulating coating and preparation method thereof
CN108659584A
Bio-based phosphaphenanthrene flame retardant curing agent and preparation method thereo
CN110105396A
Self-repairable epoxy resin material as well as preparation method and application thereof
CN111286009A
Syringaldehyde group epoxy resin with Schiff base structure and preparation method of syringaldehyde group epoxy resin
CN115093544A
Cited By
High-strength insulating Schiff base degradable epoxy resin material and preparation method thereof
CN119684573A
Self-repairing photo-thermal deicing liquid coating and preparation method thereof
CN120329855A
A self-repairing photothermal deicing liquid coating and its preparation method
CN120329855B