Thermochromic cholesteric liquid crystal material and preparation method therefor
By mixing parent liquid crystal and chiral agent in cholesteric liquid crystal and adjusting the proportion of liquid crystal monomers, the problem of low color change sensitivity of traditional cholesteric liquid crystal is solved, and a thermochromic effect with high sensitivity and wide color change range is achieved. Suitable for applications such as temperature display and color-changing fabrics.
Patent Information
- Application Number
- PCT/CN2023/097045
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-05-30
- Publication Date
- 2024-10-24
AI Technical Summary
The color change sensitivity of traditional cholesteric liquid crystals with temperature is not high, and the color changing range is narrow, which affects the sensitivity of liquid crystal thermometers.
By mixing the parent liquid crystal and the chiral agent, adjusting the type and proportion of the liquid crystal monomers, and using the molecular arrangement in the system to be highly sensitive to temperature, the periodic changes of the cholesteric liquid crystal are realized, thereby changing the reflected color, and the chiral agent is added to Improved sensitivity and color change range.
It achieves continuous discoloration of the structural color from red to blue in a narrow temperature range. It has high sensitivity and a wide discoloration range. It is suitable for room temperature applications and has huge application potential.
Smart Images

Figure CN2023097045_24102024_PF_FP_ABST
Abstract
Description
A thermochromic cholesteric liquid crystal material and a preparation method thereof
[0001] Cross-references
[0002] This application claims priority to Chinese application No. 202310420834.7 filed on April 19, 2023, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to the technical field of thermochromic materials, and in particular to a thermochromic cholesteric liquid crystal material and a preparation method thereof. Background Art
[0004] The vast majority of plants and animals in nature possess a rich variety of colors, using color to convey information and adapt to their environment. Many colors are produced by certain compounds in plants and animals that absorb or reflect specific wavelengths of light. These colors are called dye colors (or chemical colors), such as the colors of most flowers. In addition to dye colors, colors are also widely found in nature. These colors are produced by physical processes such as interference and diffraction of light caused by the microstructures on the surfaces of plants and animals. These colors are called structural colors (or physical colors), such as the colors of butterfly wings and beetle shells. Furthermore, some plants and animals can change color in response to external stimuli, or they can actively change color to convey information or camouflage themselves, such as chameleons.
[0005] Due to their unique helical structure, cholesteric liquid crystals possess strong optical rotation and selective reflection properties, enabling them to display remarkably vibrant colors. They can also be light-controlled by various external stimuli. Cholesteric liquid crystals selectively reflect different wavelengths at different temperatures, a phenomenon known as the cholesteric thermochromic effect. Compared to other stimuli, thermal stimulation is widely present in nature, is pollution-free, and is easy to operate. Therefore, utilizing the thermochromic effect of cholesteric liquid crystals to control reflected color has gradually attracted the attention of researchers, and corresponding applicable devices have been fabricated, such as liquid crystal thermometers, color-changing fabrics, and infrared detectors. However, the color change sensitivity of cholesteric liquid crystals with temperature is generally low, which affects the sensitivity of liquid crystal thermometers. Therefore, the development of a cholesteric liquid crystal with simple components, minimal processing steps, continuous color change, a wide color change range, high sensitivity, and excellent stability is of great significance for thermochromic cholesteric liquid crystals.
[0006] Summary of the Invention
[0007] The present invention aims to provide a highly temperature-sensitive thermochromic cholesteric liquid crystal material and its preparation method to address the technical issues of conventional cholesteric liquid crystals, such as low sensitivity to temperature-dependent color changes and a narrow color change range. In addition to its high sensitivity, the present thermochromic cholesteric liquid crystal material boasts a color change range that can be controlled near room temperature, enabling it to change color at human body temperature.
[0008] To achieve the above objectives, the present invention provides a thermochromic cholesteric liquid crystal material, which is composed of a mixture of a matrix liquid crystal and a chiral agent. The structural color is obtained by adding the chiral agent, and the temperature range of the cholesteric liquid crystal is adjusted by adjusting the type and proportion of liquid crystal monomers in the matrix liquid crystal. The molecular arrangement in the system is highly sensitive to temperature, and temperature changes cause the periodicity of the cholesteric liquid crystal to change, thereby changing the reflected color.
[0009] Specifically, the mother liquid crystal includes mixture A and mixture B, both of which are hydrogen-bonded liquid crystals. The function of mixtures A and B is to give the liquid crystal a relatively wide temperature range. The mixing ratio of the two is mainly to adjust the covered color change temperature range, and the type and content of the chiral agent selected will have a great influence on the sensitivity of the system.
[0010] The clearing point of mixture A is 120° C. to 180° C., and the mixture is a mixture of at least two benzoic acid derivatives, the general structural formula of the benzoic acid derivatives being:
[0011] Wherein, R is OCH2 or CH2; n is an integer of 0-17;
[0012] The crystallization point of mixture B is -30°C to 0°C, and it is a mixture of at least two cyclohexanecarboxylic acid derivatives, and the general structural formula of the cyclohexanecarboxylic acid derivative is:
[0013] Wherein, R is OCH2 or CH2; m is an integer of 0-17.
[0014] As a further preferred technical solution of the present invention, the mass ratio of the total mass of the mixture A and the mixture B to the mass of the chiral agent is 9:1 to 1:9.
[0015] As a further preferred technical solution of the present invention, the mass ratio of the mixture A to the mixture B is 9:1 to 1:9.
[0016] As a further preferred technical solution of the present invention, the chiral agent is a commonly used chiral agent, including but not limited to one or more of S811, R811, S1011, R1011, S5011, R5011, BDH1281, and CB15 mixed in any proportion.
[0017] According to another aspect of the present invention, the present invention also provides a method for preparing a thermochromic cholesteric liquid crystal material, which comprises the following steps:
[0018] (1) mixing at least two benzoic acid derivatives to obtain a mixture A having a clearing point of 120° C. to 180° C.;
[0019] (2) mixing at least two cyclohexanecarboxylic acid derivatives to obtain a mixture B having a crystallization point of -30°C to 0°C;
[0020] (3) Mixture A and mixture B are heated to a clear state respectively, then mixed evenly and a chiral agent is added to obtain a cholesteric liquid crystal, i.e., a thermochromic cholesteric liquid crystal material.
[0021] The thermochromic cholesteric liquid crystal material and preparation method of the present invention, by adopting the above-mentioned technical scheme, can achieve the following beneficial effects: having the characteristics of high sensitivity and wide color gamut, can realize continuous color change of structural color from red to blue within a very narrow temperature range, and optimally can realize the change of structural color from red to blue within 3°C to 5°C, which is much more sensitive than traditional cholesteric liquid crystals and has a wide color change range; the temperature range covered by the color change is close to room temperature, and it can be applied to products based on color change at room temperature according to different usage requirements; the thermochromic cholesteric liquid crystal material with high sensitivity and wide color change range obtained by the present invention has great application potential in temperature display, color-changing fabrics, sensors, anti-counterfeiting technology, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0023] FIG1 is a polarization diagram of the cholesteric liquid crystal at different temperatures in Example 1.
[0024] FIG2 is a reflection spectrum diagram of the cholesteric liquid crystal at different temperatures in Example 1.
[0025] FIG3 is a polarization diagram of the cholesteric liquid crystal at different temperatures in Example 2.
[0026] FIG4 is a reflection spectrum diagram of the cholesteric liquid crystal at different temperatures in Example 2.
[0027] FIG5 is a polarization diagram of the cholesteric liquid crystal at different temperatures in Example 3.
[0028] FIG6 is a reflection spectrum diagram of the cholesteric liquid crystal at different temperatures in Example 3.
[0029] FIG7 shows the chemical structural formulas of the material components in Table 1.
[0030] FIG8 shows the chemical structural formulas of the material components in Table 2.
[0031] FIG9 shows the chemical structural formulas of the material components in Table 3.
[0032] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings and in conjunction with the embodiments. DETAILED DESCRIPTION
[0033] The following describes the specific embodiments of the present invention in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.
[0034] Unless otherwise defined, the technical terms used in the following examples have the same meanings as commonly understood by those skilled in the art to which this invention belongs. The experimental reagents used in the following examples, unless otherwise specified, are conventional biochemical reagents; the experimental methods described, unless otherwise specified, are conventional methods.
[0035] Example 1
[0036] Select the materials and mixing ratios shown in Table 1. The chemical structures of the components are shown in Figure 7. Mixtures A and B are heated separately until clear, then mixed thoroughly. A chiral agent is then added to produce cholesteric liquid crystals, also known as thermochromic cholesteric liquid crystal materials. The clearing point of mixture A is 140°C, and the crystallization point of mixture B is -20°C.
[0037] The reflection color and texture of the cholesteric liquid crystal were preliminarily observed using the reflection mode (RL mode) of a polarizing microscope (POM), and the texture of the liquid crystal was further observed using the transmission mode (TL mode) of a polarizing microscope (POM). The test results are shown in Figures 1 and 2.
[0038] The prepared cholesteric liquid crystal has excellent thermochromic ability. Obvious reflected color can be observed from a polarizing microscope. As the temperature increases, the reflected color changes from red to orange, green, and finally to blue at 60°C.
[0039] Table 1. Sample formula of cholesteric liquid crystal material in Example 1
[0040] Example 2
[0041] The materials and mixing ratios shown in Table 2 were selected, and the chemical structures of the components are shown in Figure 8. Mixtures A and B were heated separately until clear, then mixed evenly. A chiral agent was then added to obtain a cholesteric liquid crystal, i.e., a thermochromic cholesteric liquid crystal material. The clearing point of mixture A was 138°C, and the crystallization point of mixture B was -15°C.
[0042] The reflection color and texture of the cholesteric liquid crystal were preliminarily observed using the reflection mode (RL mode) of a polarizing microscope (POM), and the texture of the liquid crystal was further observed using the transmission mode (TL mode) of a polarizing microscope (POM). The test results are shown in Figures 3 and 4.
[0043] The prepared cholesteric liquid crystal exhibits excellent thermochromic properties. A distinct reflection color can be observed under a polarizing microscope. The color is bright and uniform, and the color change sensitivity is high. The reflection wavelength of the color can cover a range of 674nm to 450nm. At 30°C, the initial center wavelength of the cholesteric liquid crystal is 674nm, and its color is red. When the temperature rises to 32°C, the color changes from red to orange. The increase in temperature causes a blue shift in the reflection band gap. When the temperature rises to 36°C and 44°C, the corresponding reflection colors are green and blue, respectively.
[0044] Table 2. Sample formula of cholesteric liquid crystal material in Example 2
[0045] Example 3
[0046] As a good choice for the technical solution of the present invention, the materials and mixing ratios shown in Table 3 are selected. The chemical structures of the components are shown in Figure 9. Mixtures A and B are heated separately until clear, then mixed uniformly, and a chiral agent is added to obtain cholesteric liquid crystal, i.e., thermochromic cholesteric liquid crystal material. The clearing point of mixture A is 120°C, and the crystallization point of mixture B is -10°C.
[0047] The reflection color and texture of the cholesteric liquid crystal were initially observed using a polarizing microscope (POM) in reflection mode (RL mode), and the texture was further observed using a polarizing microscope (POM) in transmission mode (TL mode). The test results are shown in Figures 5 and 6. At room temperature, the cholesteric liquid crystal exhibits an oily streak texture with bright structural colors.
[0048] At 27°C, the initial central wavelength of cholesteric liquid crystal is approximately 690nm. When the temperature rises from 27°C to 28°C, the reflection band gap of the cholesteric liquid crystal shifts from 680nm to 590nm. The temperature increase causes a blue shift in the reflection band gap. Ultimately, the cholesteric liquid crystal turns green at 29°C and turns blue at 30°C. This fully demonstrates that the present invention has obtained a highly sensitive thermochromic cholesteric liquid crystal material, which can control the color change range near room temperature.
[0049] Table 3. Sample formula of cholesteric liquid crystal material in Example 3
[0050] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.
Claims
1. A thermochromic cholesteric liquid crystal material, which is composed of a mixture of a matrix liquid crystal and a chiral agent, characterized in that: The mother liquid crystal comprises a mixture A and a mixture B, wherein: The clearing point of mixture A is 120°C to 180°C, and it is a mixture of at least two benzoic acid derivatives, and the general structural formula of the benzoic acid derivative is: Wherein, R is OCH2 or CH2, and n is an integer of 0-17; The crystallization point of mixture B is -30°C to 0°C, and it is a mixture of at least two cyclohexanecarboxylic acid derivatives, and the general structural formula of the cyclohexanecarboxylic acid derivative is: Wherein, R is OCH2 or CH2, and m is an integer of 0-17.
2. The thermochromic cholesteric liquid crystal material according to claim 1, characterized in that: The mass ratio of the total mass of the mixture A and the mixture B to the mass of the chiral agent is 9:1 to 1:
9.
3. The thermochromic cholesteric liquid crystal material according to claim 1, characterized in that: The mass ratio of the mixture A to the mixture B is 9:1 to 1:
9.
4. The thermochromic cholesteric liquid crystal material according to claim 1, characterized in that: The chiral agent is a mixture of one or more of S811, R811, S1011, R1011, S5011, R5011, BDH1281, and CB15.
5. A method for preparing the thermochromic cholesteric liquid crystal material according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) mixing at least two benzoic acid derivatives to obtain a mixture A having a clearing point of 120° C. to 180° C.; (2) mixing at least two cyclohexanecarboxylic acid derivatives to obtain a mixture B having a crystallization point of -30°C to 0°C; (3) The mixture A and the mixture B are heated to a clear state respectively, then mixed evenly and a chiral agent is added to obtain a thermochromic cholesteric liquid crystal material.
Citation Information
Patent Citations
Thermochromic cholesteric liquid crystal material and preparation method thereof
CN116396743A
Liquid crystal composition
JP1994057252A
Nematic liquid crystal composition
JP1996259948A
Liquid crystal composition and liquid crystal display element
JP1997059634A
Liquid crystal composition and liquid crystal display element
JP1997059635A