Method for manufacturing a plurality of semiconductor chips
The method simplifies semiconductor chip manufacturing by bonding a functional semiconductor wafer to a carrier wafer, generating channels, and electrochemically etching the sacrificial layer to efficiently remove the growth substrate, addressing the complexity and inefficiency of existing methods and enabling cost-effective batch production.
Patent Information
- Application Number
- PCT/EP2024/057636
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-24
AI Technical Summary
Current semiconductor chip manufacturing methods are complex and inefficient, particularly in removing the growth substrate from the semiconductor layer sequence on a wafer level, which hinders the simplification and cost-effectiveness of the process.
A method involving a functional semiconductor wafer with an epitaxial semiconductor layer sequence and a sacrificial layer grown on a growth substrate, where the wafer is bonded to a carrier wafer, channels are generated through the substrate, and the sacrificial layer is electrochemically etched to facilitate the removal of the growth substrate, allowing for the efficient separation of semiconductor chips.
This method simplifies the semiconductor chip manufacturing process by enabling the batch production of semiconductor chips with reduced process time and complexity, while ensuring mechanical stability and precise control over the substrate removal, suitable for high-hardness materials like GaN.
Smart Images

Figure EP2024057636_24102024_PF_FP_ABST
Abstract
Description
[0001] Description
[0002] METHOD FOR MANUFACTURING A PLURALITY OF SEMICONDUCTOR CHIPS
[0003] A method for manufacturing a plurality of semiconductor chips is provided .
[0004] An improved method for manufacturing a plurality of semiconductor chips is to be provided . Particularly, a simpli fied method for manufacturing a plurality of semiconductor chips is to be provided, wherein a growth substrate is removed from a semiconductor layer sequence on wafer level in a simpli fied manner .
[0005] This obj ect is achieved with the method having the steps of claim 1 .
[0006] Improved embodiments and developments of the method are given in the dependent claims .
[0007] According to an embodiment of the method for manufacturing a plurality of semiconductor chips , a functional semiconductor wafer comprising an epitaxial semiconductor layer sequence with a plurality of chip regions is provided . The epitaxial semiconductor layer sequence is arranged on a growth substrate and a sacri ficial layer is arranged at least between the chip regions and the growth substrate . For example , the epitaxial semiconductor layer sequence is epitaxially grown on the growth substrate . Particularly, the sacri ficial layer and the epitaxial semiconductor layer sequence are both epitaxially grown on the growth substrate above each other . In other words , the sacri ficial layer is first epitaxially grown on the growth substrate and then the epitaxial semiconductor layer sequence is epitaxially grown on the sacri ficial layer . It is also possible that there are further semiconductor layers arranged between the chip regions and the growth substrate . Preferably, such layers are also epitaxially grown . Further, the sacri ficial layer can extend completely over the growth substrate or only partially . For example , the sacri ficial layer is only formed in places over the growth substrate , particularly only between the chip regions and the growth substrate .
[0008] Particularly, the chip regions of the epitaxial semiconductor layer sequence comprise active zones generating electromagnetic radiation during operation of the finished semiconductor chips , the active zones being arranged between an n-doped epitaxial semiconductor layer and a p-doped epitaxial semiconductor layer .
[0009] According to a further embodiment of the method, the epitaxial semiconductor layer sequence comprises or consists of one or several I I I / V compound semiconductor materials , particularly nitride semiconductor compound materials . Nitride semiconductor compound materials are semiconductor compound materials containing nitrogen, such as the materials from the system InxAlyGai-x-yN with 0 < x < 1 , 0 < y < 1 and x+y < 1 .
[0010] According to a further embodiment of the method, a carrier wafer is provided . The carrier wafer is intended to be partially comprised by the finished semiconductor chips for mechanical stabili zation . For example , the carrier wafer comprises or consists of silicon or germanium . The carrier wafer is , for example n-doped . According to a further embodiment of the method, the functional semiconductor wafer is bonded to the carrier wafer such that a wafer compound is achieved . Particularly, the bonding process is a wafer bonding process , wherein a mechanically stable connection between the functional semiconductor wafer and the carrier wafer is achieved by impact of pressure and / or temperature . For example , the carrier wafer and the functional wafer are connected via main surfaces .
[0011] According to a further embodiment of the method, channels are generated between the chip regions through the growth substrate and the sacri ficial layer such that the sacri ficial layer is accessible through the channels . For example , the channels penetrate the functional semiconductor wafer completely and the carrier wafer partially . The channels can have any geometry . For example , the channels have in plan view on the wafer compound a round or circular base area . Preferably, the channels are arranged between the chip regions .
[0012] Further, it is possible that the channels are embodied as grooves extending along a main extension direction along the wafer compound . Particularly, the grooves can extend parallel to each other . For example , the grooves form a grid between the chip regions and correspond at least partially with separation lines along which the semiconductor chips are separated at a later stage . Between two directly adj acent grooves one or more rows of chip regions can be arranged . For example , the rows of chip regions can be separated from each other by mesas not penetrating the growth substrate . The mesas also correspond to the separation lines and / or the grooves , for example . According to a further embodiment of the method, the sacri ficial layer is electrochemically etched . For electrochemical etching an ECE voltage is applied between a first ECE contact on the wafer compound and a second ECE contact arranged within an electrochemical etchant . Particularly, direct voltage is applied as the ECE voltage . For example , the ECE voltage lies between 1 Volt and 50 Volt , limits inclusive .
[0013] According to a further embodiment of the method, the growth substrate is thinned prior to the generation of the channels . For example , thinning of the growth substrate takes place by one or a combination of the following methods : grinding, polishing, electrochemical polishing . For example , prior to thinning the growth substrate has a thickness between and including 200 micrometer and 1000 micrometer . Preferably, during thinning material is removed from the growth substrate in a direction perpendicular to a main extension plane of the growth substrate . For example , after thinning the growth substrate has a thickness between and including 10 micrometer and 100 micrometer . A variation of the thickness of the growth substrate over the whole wafer compound lies , for example , between and including + / - 2 micrometer after thinning .
[0014] According to a preferred embodiment , the method comprises the following steps :
[0015] - providing the functional semiconductor wafer comprising the epitaxial semiconductor layer sequence with the plurality of chip regions , wherein the epitaxial semiconductor layer sequence is arranged on the growth substrate and the sacri ficial layer is arranged at least between the chip regions and the growth substrate ,
[0016] - bonding the functional semiconductor wafer to the carrier wafer such that the wafer compound is achieved,
[0017] - generating the channels through the growth substrate and the sacri ficial layer such that the sacri ficial layer is accessible through the channels ,
[0018] - electrochemically etching the sacri ficial layer, wherein
[0019] -the growth substrate is thinned prior to the generating of the channels .
[0020] Particularly, the steps are conducted in the given order . Preferably, the channels are generated after bonding the functional semiconductor wafer to the carrier wafer . Also , thinning preferably takes place after bonding the carrier wafer and the semiconductor wafer .
[0021] According to a further embodiment of the method, the wafer compound is singulated into a plurality of separated semiconductor chips along the separation lines .
[0022] Particularly, the present method takes place as a batch process on wafer level manufacturing a plurality of semiconductor chips in parallel . Particularly, the epitaxial semiconductor layer sequence and the sacri ficial layer are provided as a part of a wafer with a diameter of several inches . Particularly, the sacri ficial layer is at present removed on waver level from the wafer compound . In other words , the sacri ficial layer is removed as part of the wafer compound, which is singulated in separate semiconductor chips at a later stage . A batch process on wafer level particularly has the advantage of reduced process time . According to a further embodiment of the method, a first passivation layer is deposited over a main face of the wafer compound, wherein the first passivation layer comprises first openings . Particularly, the growth substrate is accessible through the first openings . Generating the channels starts preferably from the first openings . Further, the first openings are preferably arranged between the chip regions in plan view . For example , the passivation layer comprises or consists of a dielectric material , such as an oxide or a nitride . Particularly, a thickness of the first passivation layer lies between and including 50 nanometer and 800 nanometer .
[0023] According to a further embodiment of the method, the channels are at least partially formed by reactive ion etching ( short "RIE" ) . Particularly, the channels are completely formed by reactive ion etching . Particularly, it is possible to generate the channels in an ef fective way by reactive ion etching, i f the growth substrate is thinned prior to generating the channels . I f the growth substrate is thinned prior to generating the channels , it is possible to penetrate the growth substrate by the channels formed by reactive ion etching in a short process time . Particularly, in this embodiment of the method, the growth substrate is formed of , or comprises , GaN . GaN is a semiconductor material having a high hardness that is complicated to separate , for example by sawing . Therefore , according to the present method, reactive ion etching is preferably used for generating the channels within the growth substrate . In order to achieve the generation of the channels that completely penetrate through the growth substrate by reactive ion etching in short process times , the growth substrate is preferably thinned prior to the formation of the channels . Further, it is possible that the channels are firstly partially formed by laser grooving and / or sawing, particularly within the growth substrate . Then the channels are , for example , finished by reactive ion etching .
[0024] According to a further embodiment of the method, etch stop elements are arranged between the chip regions . The etch stop elements are particularly preferably configured to stop reactive ion etching, particularly of the channels . Consequently, the channels are preferably formed up to the etch stop element parallel to a growth direction of the epitaxial semiconductor layer sequence . For example , the etch stop elements comprise or consist of at least one of the following materials : SiCy , ZnO, AI2O3.
[0025] According to a further embodiment of the method, an edge of the functional semiconductor wafer is tapered . Tapering the edge of the functional semiconductor wafer is also achieved, for example , by reactive ion etching . For example , the edge of the functional semiconductor wafer is tapered such that a cross-sectional area of the functional semiconductor wafer decreases from the epitaxial semiconductor layer sequence to the growth substrate .
[0026] According to a further embodiment of the method, the carrier wafer has a larger diameter than the functional semiconductor wafer . For example , the functional semiconductor wafer has a diameter between 2 and 6 inches , limits inclusive , while the carrier wafer has a diameter between 6 and 20 inches , limits inclusive . For example , the functional semiconductor wafer has a diameter of 2 inches , while the carrier wafer has a diameter of 4 inches or 6 inches or 8 inches . For example , the diameter of the carrier wafer is as large that more than one functional semiconductor wafer can be bonded to the carrier wafer .
[0027] According to a further embodiment of the method, the sacri ficial layer comprises or consists of a highly n-doped semiconductor material , particularly of a highly n-doped nitride semiconductor compound material . Particularly, the highly n-doped nitride semiconductor compound material has a higher etching rate in the electrochemical etchant than a lower doped or non-doped nitride semiconductor compound material . Particularly, the active radiation generating zones of the chip regions , are low, non-doped or only unintentionally doped . Therefore , the sacri ficial layer comprising the highly n-doped semiconductor material can be electrochemically etched against the chip regions . Particularly, the highly n-doped semiconductor material has a dopant concentration of at least 1018 / cm3.
[0028] According to a further embodiment of the method, an etch stop layer is arranged between the sacri ficial layer and the chip regions . Particularly, the etch stop layer has a smaller etching rate in the electrochemical etchant than the sacri ficial layer . For example , the etch stop layer has an etching rate in the electrochemical etchant of one magnitude of order smaller than the sacri ficial layer . In such a way the chip regions are protected against material decomposition during electrochemical etching . Preferably, the etch stop layer is in direct contact with the sacri ficial layer . Also , the etch stop layer can be in direct contact with the chip regions . For example , particularly i f the chip regions are based on, or consist of , materials of a nitride semiconductor compound material , the etch stop layer comprises , or consists of , AIN or Al lnN .
[0029] According to a further embodiment of the method, the growth substrate comprises or consists of GaN . Particularly, GaN is suited for epitaxial growth of a nitride semiconductor compound material .
[0030] According to a further embodiment of the method, the growth substrate is removed, for example by li ft of f . For example , the growth substrate is removed from the wafer compound by a tape li ft-of f . During the tape li ft-of f a tape is adhered to a freely accessible main surface of the growth substrate and peeled of f such that the grow substrate adhered to the tape is separated from the wafer compound .
[0031] According to a further embodiment of the method, an etch stop indicator layer is arranged between the growth substrate and the chip regions . Particularly, the etch stop indicator layer is arranged between the growth substrate and a further n- doped semiconductor layer . Particularly, the etch stop indicator layer is arranged between the further n-doped semiconductor layer and an unintentionally doped or low n- doped semiconductor layer . These semiconductor layers are , for example , also epitaxially grown on the growth substrate , for example on an n-doped GaN growth substrate . The etch stop indicator layer may comprise a metal or one of the following materials : AlGaN, for example with an Al content of at least 4 % , InAlN or AIN . Preferably, the etch stop indicator layer is lattice matched to the underlying material , such as an unintentionally or low doped semiconductor layer . The etch stop indicator layer particularly indicates that the growth substrate is penetrated during reactive ion etching . Particularly, the etch stop indicator layer is not removed by thinning the growth substrate . After thinning the growth substrate , the remaining part of the growth substrate has a tolerance of its thickness , for example of 10% due to the thinning process . During generating the channels in the growth substrate particularly with reactive ion etching, the etch stop indicator layer indicates when the channels have penetrated the growth substrate completely and have reached the etch stop indicator layer . This helps to match stopping the reactive ion etching in due time .
[0032] According to a further embodiment of the method, second openings are generated in the first passivation layer . Particularly, the growth substrate is electrically conductively connected with the first ECE contact on the wafer compound through the second openings , preferably by a metallic layer .
[0033] At present the term " first opening" or " second opening" do not indicate an order of formation of the openings . Rather, the first openings are intended and configured to form starting points for the formation of the channels , while the second openings are intended and configured for electrically conductive connection of the growth substrate .
[0034] According to a further embodiment of the method, during bonding of the functional semiconductor wafer to the carrier wafer, a metal layer on or over the carrier wafer is bonded to a continuous p-contact layer on or over the functional semiconductor wafer . For example , the metal layer extends continuously over a central area of the carrier wafer . For example , the metal layer on or over the carrier wafer and the continuous p-contact layer on or over the functional semiconductor wafer comprise or consist of the same material . For example , the metal layer and / or the continuous p-contact layer comprises or consists of one of the following metals : gold, silver, platinum, indium, tin .
[0035] According to a further embodiment of the method, the metal layer is only arranged in the central area of the carrier wafer, while an edge area of the carrier wafer not covered by the functional semiconductor wafer after bonding is free of the metal layer .
[0036] According to a further embodiment of the method, the first passivation layer is deposited over the metal layer on the edge area of the carrier wafer that is not covered by the functional semiconductor wafer after bonding .
[0037] According to a further embodiment of the method, bonding the functional semiconductor wafer to the carrier wafer comprises connecting metallic bond pads over the chip regions to metallic mounting areas on the carrier wafer . Further, the metallic mounting areas over the chip regions can be electrically isolated from each other by the etch stop elements and / or an isolation material . Particularly, the metallic mounting regions of the carrier wafer are electrically isolated from each other, for example by a further isolation material .
[0038] According to a further embodiment of the method, the metallic layer connects the growth substrate electrically conductively with the first ECE contact on the wafer compound through the second openings . For example , the metallic layer forms a conductor track in the edge area of the carrier wafer . A second passivation layer particularly preferably electrically isolates the metallic layer from the electrochemical etchant during electrochemical etching . For example , the second passivation layer is arranged on or over the metallic layer and / or encapsulates the second passivation layer .
[0039] With the described method, for example , semiconductor chips embodied as an edge emitting laser device or a VCSEL ( short for "vertical cavity surface emitting laser" ) can be manufactured . Furthermore , LED chips ( short for " light emitting diode chips" ) , particularly, UV-LED chips can be achieved .
[0040] The semiconductor chips manufactured with the method can be used, for example , in augmented reality applications as well as in a micro-AFS ( short for "microstructured adaptive front lighting system" ) .
[0041] Further advantageous embodiments and developments of the method for manufacturing a plurality of semiconductor chips result from the exemplary embodiment described below in connection with the Figures .
[0042] Figures 1 to 13 show schematic views of stages of a method for manufacturing a plurality of semiconductor chips according to an exemplary embodiment .
[0043] Figure 14 shows a schematic view of a stage of a method for manufacturing a plurality of semiconductor chips according to a further exemplary embodiment . Figures 15 and 16 show schematic views of stages of a method for manufacturing a plurality of semiconductor chips according to a further exemplary embodiment .
[0044] Figures 17 and 18 show schematic views of stages of a method for manufacturing a plurality of semiconductor chips according to a further exemplary embodiment .
[0045] Figures 19 to 21 show schematic views of stages of a method for manufacturing a plurality of semiconductor chips according to a further exemplary embodiment .
[0046] Figures 22 , 23 and 24 show schematic views of stages of methods for manufacturing a plurality of semiconductor chips according to further exemplary embodiments .
[0047] Equal or similar elements as well as elements of equal function are designated with the same reference signs in the Figures . The Figures and the proportions of the elements shown in the Figures are not regarded as being shown to scale . Rather, single elements , in particular layers , can be shown exaggerated in magnitude for the sake of better presentation and / or better understanding .
[0048] According to the method of the exemplary embodiment of Figures 1 to 13 , a functional semiconductor wafer 1 is provided ( Figure 1 ) .
[0049] The functional semiconductor wafer 1 comprises an epitaxial semiconductor layer sequence 2 with a plurality of chip regions 3 , wherein in Figure 1 only two chip regions 3 are exemplarily shown for the sake of clarity . The chip regions 3 are arranged on a growth substrate 4 . At present , the epitaxial semiconductor layer sequence 2 is based on a nitride semiconductor compound material , while the growth substrate 4 comprises or consists of n-doped GaN being electrically conductive . It is also possible that the growth substrate 4 is undoped .
[0050] The chip regions 3 are embodied equally to each other in the present exemplary embodiment . Each chip region 3 comprises an n-doped semiconductor layer 39 and a p-doped semiconductor layer 40 . Between the n-doped semiconductor layer 39 and the p-doped semiconductor layer 40 an active zone 28 is arranged . The active zone 28 is configured to generate electromagnetic radiation in the operation of the finished semiconductor chip .
[0051] The chip regions 3 further comprises a layer of unintentionally doped semiconductor material 41 having, for example , a thickness between and including 200 nanometer and 1000 nanometer . The layer of unintentionally doped semiconductor material 41 is in direct contact with an etch stop layer 42 .
[0052] The chip regions 3 comprises further p-contact layers 43 , at present comprising or consisting of ITO ( short for " indium tin oxide" ) . The p-contact layers 43 are in direct contact with a continuous p-contact layer 54 , which is configured for electrical connection of p-doped layers of the epitaxial semiconductor layer sequence 2 . The continuous p-contact layer 54 comprises or consists of a metal .
[0053] The chip regions 3 further comprises a first mirror layer 46 , particularly a DBR mirror layer ( DBR short for "distributed bragg reflector" ) . The first mirror layer 46 is intended to be part of a vertical resonator of a finished semiconductor chip being a VCSEL .
[0054] Between the chip regions 3 and the growth substrate 4 a sacri ficial layer 5 being highly n-doped is arranged . For example , the sacri ficial layer 5 is based on a nitride semiconductor compound material and has a dopant concentration of at least 1018cm-3. Particularly, the sacri ficial layer 5 extends completely along a main extension plane of the functional semiconductor wafer 1 .
[0055] An etch stop layer 42 is arranged between the sacri ficial layer 5 and the chip regions 3 . The etch stop layer 42 is in direct contact with the sacri ficial layer 5 and the chip regions 3 . The etch stop layer 42 comprises or consists of AIN or Al lnN . A further n-doped semiconductor layer 47 is arranged between the sacri ficial layer 5 and the growth substrate 4 . Between the further n-doped semiconductor layer 47 and the growth substrate 4 a further unintentionally doped semiconductor layer 61 is arranged, which can also be low n- doped .
[0056] The chip regions 3 are electrically isolated to each other by an isolation material 48 . The isolation material 48 is arranged at side faces of the chip regions 3 and extend until the etch stop layer 42 parallel to a growth direction DGof the epitaxial semiconductor layer sequence 2 . Within the isolation material 48 , etch stop elements 60 are arranged . The isolation material 48 laterally surrounds the etch stop elements 60 completely, the etch stop elements 60 are in direct contact with the continuous p-contact layer 54 . The thickness of the etch stop elements 60 in the growth direction DGof the epitaxial semiconductor layer sequence 2 is about 3 micrometer . At present , the etch stop elements 60 are made of SiO2.
[0057] Further, a carrier wafer 6 is provided . The carrier wafer 6 consists or comprises silicon or germanium, for example . The carrier wafer 6 can be doped, particularly n-doped . At present , the carrier wafer 6 has a larger diameter than the functional semiconductor wafer 1 . On a main surface of the carrier wafer 6 a metal layer 22 is deposited . A back main surface of the carrier wafer 6 oppositely to the main surface is covered at present with a backside contact layer 38 .
[0058] The chip regions 3 can planari zed by a planari zation material prior to bonding to the carrier wafer 6 .
[0059] The functional semiconductor wafer 1 is bonded to the carrier wafer 6 such that a wafer compound 7 is achieved ( Figure 2 ) . Particularly, the metal layer 22 and the continuous p-contact layer 54 are connected to each other by metal-metal bonding .
[0060] Then, the growth substrate 4 is thinned, for example down to a thickness of about 20 micrometer ( Figure 3 ) .
[0061] In a further step, an edge 62 of the functional semiconductor wafer 1 is etched such that the edge 62 is tapered, for example by reactive ion etching . Particularly, a cross- sectional area in plan view of the functional semiconductor wafer 1 decreases from the epitaxial semiconductor layer sequence 2 to the growth substrate 4 ( Figure 4 ) . Furthermore , the metal layer 22 in an edge area 9 of the carrier wafer 6 is covered by a first passivation layer 63 . Adj acent to the edge area 9 of the carrier wafer 6 a central area 23 is arranged . The first passivation layer 63 is also deposited over the functional semiconductor wafer 1 as , for example , shown in Figure 5 . Second openings 64 are generated within the first passivation layer 63 such that the thinned growth substrate 4 is freely accessible through the second openings 64 . The growth substrate 4 is electrically conductively connected with a first ECE contact 8 on the wafer compound 7 through the second openings 64 by a metallic layer 65 . The first ECE contact 8 is arranged in the edge area 9 of the carrier wafer 6 . The metallic layer 65 forms a conductor track 17 , for example , in the edge area 9 of the carrier wafer 6 , the conductor track 17 connecting the first ECE contact 8 and the GaN growth substrate 4 in the central area 23 of the carrier wafer 6 . Then, the metallic layer 65 is covered by a second passivation layer 66 . Preferably, the metallic layer 65 is encapsulated by the second passivation layer 66 unless a part forming the first ECE contact 8 ( Figure 6 ) .
[0062] In a further step, first openings 67 are arranged in the first passivation layer 63 , wherein the first openings 67 are arranged between the chip regions 3 in plan view on the functional semiconductor wafer 1 . Particularly, the first openings 67 are arranged over the etch stop elements 6 seen in plan view on the functional semiconductor wafer 1 ( Figure 7 ) .
[0063] Then, channels 68 are generated within the functional semiconductor wafer 1 starting from the first openings , particularly by reactive ion etching . The channels 68 are generated between two directly adj acent chip regions 3 and penetrate the growth substrate 4 , the sacri ficial layer 5 and the etch stop layer 42 until the etch stop elements 60 are reached ( Figure 8 ) . At present , also the etch stop elements 60 are partially etched by RIE , for example such that a thickness of about 3 micrometer remains . Particularly, the sacri ficial layer 5 is accessible through the channels 68 , but not the n-doped semiconductor layer 39 , the active zone 28 and the p-doped semiconductor layer 40 . The selectivity of reactive ion etching of the GaN growth substrate 4 versus silicon oxide of the etch stop element 60 is about 1 : 8 .
[0064] Then, the wafer compound 7 is introduced into a liquid electrochemical etchant 12 provided in a vessel 13 . Nitric acid is used as an electrochemical etchant 12 , for example . A second ECE contact 14 is also arranged within the electrochemical etchant 12 . In order to electrically isolate the first ECE contact 8 from the second ECE contact 14 , a sealing rim 59 as part of a wafer holder is used that is arranged on the second passivation layer 66 in the edge area 9 of the carrier wafer 6 . Electrochemical etching of the sacri ficial layer 5 is started by applying an ECE voltage V between the first ECE contact 8 and the second ECE contact 14 ( Figure 9 ) .
[0065] The sacri ficial layer 5 is dissolved and finally removed during electrochemical etching ( Figure 10 ) .
[0066] Then, the growth substrate 4 , the further unintentionally doped semiconductor layer 61 and the further n-doped semiconductor layer 47 are removed from the wafer compound 7 , for example by tape li ft-of f ( Figure 11 ) .
[0067] As , for example , shown in Figure 12 , second mirror layers 49 is arranged on the chip regions 3 forming a vertical resonator of the finished semiconductor chips embodied as VCSELs . A metallic material 51 is introduced within an n- doped part of the epitaxial semiconductor layer sequence 2 in order to achieve an electrically conductive connection of the n-doped semiconductor layers 39 . The channels 68 are filled with isolation material 48 .
[0068] Then, the semiconductor chips are singulated along separation lines 27 running between the chip regions 3 through the etch stop elements 60 as well as the isolation material 48 ( Figure 13 ) .
[0069] At present , the etch stop elements 60 are formed of SiCy , while the growth substrate 4 is a GaN growth substrate 4 . The finished semiconductor chips are VCSELs having a vertical cavity with a thickness including the first mirror layer 46 and the second mirror layer 49 of about 2 micrometer to 3 micrometer . Therefore , the etching uncertainty during forming the channels 68 due to variations in the thickness of the GaN growth substrate 4 caused by thinning the GaN growth substrate 4 should, for example , not be beyond 15 micrometer to 25 micrometer across the whole wafer compound 6 for an selectivity of reactive ion etching of 1 : 8 of the SiCy of the etch stop elements 60 versus the GaN growth substrate 4 . A higher selectivity of reactive ion etching can be achieved as described in Frye et al . "Ultrahigh GaN i SiCy etch selectivity by in si tu surface modi fication of SiCy in a C12~Ar plasma" Mater . Res . Lett . , 2021 , Vol . 9 , NO . 2 , 105- 111 .
[0070] Compared to the method of the exemplary embodiment of Figures 1 to 13 , an etch stop indicator layer 69 is arranged within a further unintentionally doped semiconductor layer 61 arranged between a sacri ficial layer 5 and the GaN growth substrate 4 during the method of the exemplary embodiment of Figure 14 . For example , the etch stop indicator layer 69 comprises or consists of a metal or, for example , AlGaN with an Al content of larger than 4 % , InAlN or AIN . Preferably, the etch stop indicator layer 69 is lattice matched to the GaN growth substrate 4 for minimum defects . The etch stop indicator layer 69 can be doped or undoped . With the help of the etch stop indicator layer 69 , it can be indicated when the GaN growth substrate 4 , is etched through . This is helpful since after thinning the GaN growth substrate 4 particularly has a thickness varying over the whole wafer compound 7 .
[0071] Compared to the exemplary embodiment of the method of Figures 1 to 13 during the method of the exemplary embodiment of Figures 15 to 16 , parts 70 of the channels 68 in the growth substrate 4 of the wafer compound 7 between two directly adj acent chip regions 3 is firstly generated by laser grooving or sawing . This is particularly carried out , i f laser grooving or sawing is faster than the generation of the channels 68 by reactive ion etching ( Figure 15 ) .
[0072] As shown in Figure 16 , the functional semiconductor wafer 1 is penetrated within the etch stop element 60 by reactive ion etching in order to finish the channels 68 .
[0073] Then, further process steps are carried out as already described, for example , in connection with Figures 11 to 13 .
[0074] Compared to the exemplary embodiment of the method of Figures 1 to 13 according to the method of the exemplary embodiment of Figures 17 to 18 , the metal layer 22 of the wafer compound 7 is structured by a further isolation material 55 such that metallic mounting areas 33 over the carrier wafer 6 are electrically isolated from each other by the further isolation material 55 ( Figure 17 ) .
[0075] Also , metallic bond pads 24 over the chip regions of the functional semiconductor wafer are electrically isolated from each other by etch stop elements 60 . The carrier wafer 6 and the functional semiconductor wafer 1 are bonded together, particularly via the metallic bond pads 24 over the chip regions 3 of the functional semiconductor wafer 1 and the metallic mounting areas 33 electrically isolated from each other on the carrier wafer 6 . After bonding the etch stop elements 60 electrically isolating the chip regions 3 and the further isolation material 55 electrically isolating the metallic mounting areas 33 are connected to each other . In the present exemplary embodiment , the etch stop elements 60 are for example formed by a dielectric material .
[0076] Channels 68 are formed through the etch stop elements 60 and the further isolation material 55 ( Figure 18 ) . Therefore , etching for forming the channels 68 within the functional semiconductor wafer 1 can performed during a greater time interval such that the channels 68 deeper penetrate into the wafer compound 7 without giving access to a metal material for example of the continuous p-contact layer 54 through the channels 68 avoiding parasitic electrochemical etching . This is particularly advantageous , i f the growth substrate 4 has a higher inhomogeneity of thickness , for example due to thinning . At present , the channels 68 penetrate the wafer compound 7 such that also a part of the carrier wafer 6 is cut through by the channels 68 . Then, further process steps are conducted as already described for example in connection with Figures 11 to 13 such that single semiconductor chips are achieved .
[0077] Compared to the method of the exemplary embodiment of Figures 1 to 13 , during the method of the exemplary embodiment of Figures 19 to 21 electrically isolating elements 71 are arranged at edges 62 of the functional semiconductor wafer 1 . The electrically isolating elements 71 extend from a continuous p-contact layer 54 continuously along the chip regions 3 up to and over the etch stop layer 42 and the sacri ficial layer 5 to a further n-doped semiconductor layer 47 arranged on the GaN growth substrate 4 .
[0078] In this embodiment of the method, the etch stop elements 60 embedded within the electrically isolation material 48 between the chip regions 3 can also extend as far as the electrically isolating elements 71 at the edge 62 of the functional semiconductor wafer 1 .
[0079] In a next step, the carrier wafer 6 and the functional semiconductor wafer 1 are bonded together by a metal-metal bond between a metal layer 22 on a main surface of the carrier wafer 6 and a continuous p-contact layer 54 over the chip regions 3 of the functional semiconductor wafer 1 ( Figure 20 ) . The electrically isolating elements 71 separate the channels 68 and the edge 62 of the functional semiconductor wafer 1 from the sacri ficial layer 5 and the layers of the chip regions 3 arranged between the first mirror layer 46 and the sacri ficial layer 5 at a later stage . Thus , the edge 62 of the functional semiconductor wafer 1 is protected . Then, a first passivation layer 63 is applied over an edge area 9 of the carrier wafer 6 ( Figure 21 ) . However, the first passivation layer 63 does not extend over the edge 62 of the functional semiconductor wafer 1 as for example shown in Figure 5 , since the electrically isolating element 71 isolates the chip regions 3 and particularly the sacri ficial layer 5 adj acent to the edge 62 of the functional semiconductor wafer 1 against an electrical current applied to the metal elements of the wafer compound during electrochemical etching at a later stage .
[0080] A metallic layer 65 is applied on the first passivation layer 63 electrically conductively connecting a first ECE contact 8 on the edge area 9 of the carrier wafer 6 and the electrically conductive GaN growth substrate 4 . The metallic layer 65 forming a conductive track 17 on the edge area 9 of the carrier wafer 6 electrically conductively connected to the first ECE contact 8 , is covered by a second passivation layer 66 .
[0081] In the method according to the exemplary embodiment of Figure 22 , a functional semiconductor wafer 1 is provided, wherein the chip regions 3 are not separated from each other by an isolation material 48 . However, etch stop elements 60 are arranged between the first mirror layers 46 being embedded in the isolation material 48 . The etch stop element 60 are , for example , made of a metal or a dielectric material .
[0082] At an edge 62 of the functional semiconductor wafer 1 , electrically isolating elements 71 are arranged, which extend from a continuous p-contact layer 54 to a further n-doped semiconductor layer 47 arranged between the sacri ficial layer 5 and the GaN growth substrate 4 . In this exemplary embodiment , there are only small variations of height caused by the first mirror layers 46 of about 1 micrometer to 2 micrometer, limits inclusive , to be planari zed .
[0083] Further, an edge area 9 of the wafer carrier 6 is free of the metal layer 22 before thinning the GaN growth substrate 4 .
[0084] Particularly, the carrier wafer 6 can also be non-doped or only unintentially doped . In this case , the electrically connection of the p-doped semiconductor layer 40 has to be established after the removal of the growth substrate 4 from the wafer compound 7 .
[0085] Figure 23 shows a plan view of a wafer compound 7 after bonding a functional semiconductor wafer 1 to a carrier wafer 6 , which might be generated during a method according to a further exemplary embodiment .
[0086] The carrier wafer 6 has a larger diameter than the functional semiconductor wafer 1 . The functional semiconductor wafer 1 is arranged centered in a central area 23 of the carrier wafer 6 . In an edge area 9 of the carrier wafer 6 surrounding the central area 23 , a first ECE contact 8 is applied electrically conductively connected to the functional semiconductor wafer 1 , for example by a conductor track 17 .
[0087] The functional semiconductor wafer 1 comprises channels 68 which at present are formed as grooves 10 with a rectangular base area seen in plan view . The grooves 10 extend parallel to each other within a main extension plane of the functional semiconductor wafer 1 . For example , a distance between two directly adj acent grooves 10 can be twice a width of one chip region 3 or a further integral multiple of the width of one chip region 3 . The first ECE contact 8 is particularly electrically conductively connected to each column 72 of the functional semiconductor wafer 1 , the column being limited by two directly adj acent grooves 10 .
[0088] Figure 24 shows a plan view of a wafer compound 7 generated during a method according to a further exemplary embodiment after bonding a functional semiconductor wafer 1 to a carrier wafer 6 .
[0089] As shown in Figure 24 , the channels 68 can have a base area with arbitrary geometry, for example round or circular . This particularly possible , i f the channels 68 are formed by reactive ion etching and not by sawing .
[0090] The present application claims priority of the German application DE 102023109868 . 3 , the disclosure content of which is inserted herein by reference .
[0091] The invention is not limited to the description of the exemplary embodiments . Rather, the invention comprises each new feature as well as each combination of features , particularly each combination of features of the claims , even i f the feature or the combination of features itsel f is not explicitly given in the claims or the exemplary embodiments . References
[0092] 1 functional semiconductor wafer
[0093] 2 epitaxial semiconductor layer sequence
[0094] 3 chip region
[0095] 4 growth substrate
[0096] 5 sacri ficial layer
[0097] 6 carrier wafer
[0098] 7 wafer compound
[0099] 8 first ECE contact
[0100] 9 edge area
[0101] 10 groove
[0102] 12 electrochemical etchant
[0103] 13 vessel
[0104] 14 second ECE contact
[0105] 17 conductor track
[0106] 20 boundary region
[0107] 21 central region
[0108] 22 metal layer
[0109] 23 central area
[0110] 24 metallic bond pad
[0111] 27 separation line
[0112] 28 active zone
[0113] 33 metallic mounting area
[0114] 38 backside contact layer
[0115] 39 n-doped semiconductor layer
[0116] 40 p-doped semiconductor layer
[0117] 41 layer of unintentionally doped semiconductor material
[0118] 42 etch stop layer
[0119] 43 p-contact layer
[0120] 44 p-contact
[0121] 45 n-contact
[0122] 46 first mirror layer 47 further n-doped semiconductor layer
[0123] 48 isolation material
[0124] 49 second mirror layer
[0125] 51 metallic material
[0126] 54 continuous p-contact layer
[0127] 55 further isolation material59 sealing rim
[0128] 60 etch stop element
[0129] 61 further unintentionally doped semiconductor layer
[0130] 62 edge
[0131] 63 first passivation layer
[0132] 64 second opening
[0133] 65 metallic layer
[0134] 66 second passivation layer
[0135] 67 first opening
[0136] 68 channel
[0137] 69 etch stop indicator layer
[0138] 70 part
[0139] 71 electrically isolating element
[0140] 72 column
[0141] V ECE voltage
[0142] DGgrowth direction
Claims
Claims1. Method for manuf cturing a plurality of semiconductor chips, comprising the steps:- providing a functional semiconductor wafer (1) comprising an epitaxial semiconductor layer sequence (2) with a plurality of chip regions (3) , wherein the epitaxial semiconductor layer sequence (2) is arranged on a growth substrate (4) and a sacrificial layer (5) is arranged at least between the chip regions (3) and the growth substrate(4) ,- bonding the functional semiconductor wafer (1) to a semiconductor carrier wafer (6) such that a wafer compound (7) is achieved,- generating channels (68) through the growth substrate (4) and the sacrificial layer (5) such that the sacrificial layer(5) is accessible through the channels (68) ,- electrochemically etching the sacrificial layer (5) , wherein- the growth substrate (4) is thinned prior to the generating of the channels (68) .
2. Method according to the previous claim, wherein- a first passivation layer (63) over a main face of the wafer compound (7) is deposited,- the first passivation layer (63) comprises first openings (67) ,- generating the channels (68) starts from the first openings (67) .
3. Method according to any of the previous claims, wherein the channels (68) are at least partially formed by reactive ion etching.
4. Method according to any of the previous claims, wherein etch stop elements (60) are arranged between the chip regions (3) .
5. Method according to any of the previous claims, wherein an edge (62) of the functional semiconductor wafer (1) is tapered .
6. Method according to any of the previous claims, wherein- the carrier wafer (6) has a larger diameter than the functional semiconductor wafer (1) , and- a first ECE contact (8) is arranged on a part of the carrier wafer 6 not covered by the functional semiconductor wafer ( 1 ) .
7. Method according to any of the previous claims, wherein the sacrificial layer (5) comprises a highly n-doped semiconductor material.
8. Method according to any of the previous claims, wherein an etch stop layer (42) is arranged between the sacrificial layer (5) and the chip regions (3) .
9. Method according to any of the previous claims, wherein the growth substrate (4) comprises GaN.
10. Method according to any of the previous claims, wherein the growth substrate (4) is removed by lift off.
11. Method according to any of the previous claims, wherein an etch stop indicator layer (69) is arranged between the growth substrate (4) and the chip regions (3) .
12. Method according to any of the previous claims, further comprising the steps:- generating second openings (64) in the first passivation layer ( 63 ) ,- connecting the growth substrate (4) electrically conductively with a first ECE contact (8) on the wafer compound (7) through the second openings (64) .
13. Method according to any of the previous claims, wherein during bonding the functional semiconductor wafer (1) to the carrier wafer (6) a metal layer (22) on the carrier wafer (6) is bonded to a continuous p-contact layer (54) on the functional semiconductor wafer (1) .
14. Method according to the previous claim, wherein the metal layer (22) is only arranged in a central area (23) of the carrier wafer (6) , while an edge area (9) of the carrier wafer (6) is not covered by the functional semiconductor wafer (1) after bonding is free of the metal layer ( 22 ) .
15. Method according to any of claims 13 to 14, wherein the first passivation layer (63) is deposited over the metal layer (22) on the carrier wafer (6) in the edge area (9) not covered by the functional semiconductor wafer (1) .
16. Method according to any of claims 1 to 14, wherein- bonding the functional semiconductor wafer (1) to the carrier wafer (6) comprises connecting metallic bond pads (24) over the chip regions (3) to metallic mounting areas(33) on the carrier wafer (6) , and- the metallic mounting areas (33) on the carrier wafer (6) are electrically isolated from each other.
17. Method according to any of the previous claims, wherein a second passivation layer (66) is deposited on a metallic layer (65) connecting the growth substrate (4) electrically conductively with a first ECE contact (8) on the wafer compound (7) through the second openings (64) .
Citation Information
Patent Citations
Micro-resonant cavity LED chip with substrate removed through chemical erosion and preparation method thereof
CN107369746A
Wafer level packaging of light emitting diodes (LEDS)
US20170229431A1
Process for fabricating at least one semiconductor structure comprising a step of separation relative to the growth substrate
US20200020527A1
DE102023109868A
Cited By
Method for manufacturing a plurality of semiconductor chips
WO2025176467A1