Steel sheet with temporary double-layered corrosion protection for an optimized coating process
A double-layer corrosion protection system using organic silicon compounds and corrosion protection oil on sheet steel addresses residue issues and environmental concerns, enabling efficient and environmentally friendly painting processes with enhanced corrosion resistance.
Patent Information
- Application Number
- PCT/EP2024/060223
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
Existing sheet steel coatings with temporary corrosion protection often leave residues that interfere with painting processes, leading to uneven application and optical defects, and require additional cleaning steps, which can result in environmental and health hazards due to the use of hazardous materials like chrome and nickel.
A double-layer temporary corrosion protection system for sheet steel, comprising an intermediate layer with organic silicon compounds chemisorbed onto a metallic coating, followed by a corrosion protection oil layer, ensuring complete and uniform coverage without visual disturbances and reducing the need for additional processing steps.
The solution provides effective temporary corrosion protection, ensuring a uniform and clean surface for painting, reducing environmental impact by minimizing hazardous waste and improving corrosion resistance and paint adhesion without the need for phosphating or chromium-containing pretreatments.
Smart Images

Figure IMGF000024_0001
Abstract
Description
[0001] Steel sheet with double-layer temporary corrosion protection for optimized painting
[0002] The invention relates to a temper-rolled steel sheet comprising a steel substrate and a metallic coating consisting of a zinc or aluminum alloy arranged on one or both sides of the steel substrate. The metallic coating comprises a double-layer temporary corrosion protection layer, with an intermediate layer containing organic silicon compounds as the first layer and, arranged thereon, a second layer containing or consisting of a corrosion protection oil. Furthermore, the invention relates to a method for producing such a steel sheet and its use for producing a painted component.
[0003] Sheets made of steel, for example, particularly for use in the automotive sector, are typically coated with a metallic coating, such as a zinc coating with particularly low aluminum content from the melt (Z), a zinc-based coating with aluminum and magnesium content from the melt (ZM), a zinc or zinc-based coating heat-treated after hot-dip coating (ZF), and an electrolytically applied zinc coating (ZE). Alternatively, the steel materials are coated with a metallic coating consisting of an aluminum alloy (hot-dip aluminized sheet fal AS).
[0004] Such sheets are used in particular for the manufacture of automobiles or white goods (such as electric stoves, refrigerators, freezers, washing machines, dryers, and dishwashers). This requires a coating that is free of optical defects such as spots, light-dark coloring, orange peel, etc.
[0005] Since the further steps after metallic coating and skin passing usually take place at different times and / or locations, these sheets are provided with temporary corrosion protection and, if necessary, a functional coating before this (i.e. beneath the temporary corrosion protection). For later painting, the layers arranged on the metallic coating usually have to be removed again. Removal is generally carried out in one or more cleaning steps. It can happen that the cleaning is not complete, i.e. that residues of the coating and / or temporary corrosion protection remain on at least parts of the skin passing steel sheet. Such residues, as well as dirt residues such as chips, dust or other particles as well as oil, which originate, for example, from the equipment used both before and after cleaning, tend to accumulate in the skin passing valleys.Due to the dipole moments of the metal oxides on the surface of the metallic coatings, any polarizable or dipolar compounds or polar ends of amphiphilic molecules applied to them are also more strongly bound to the surface. This impairs the surface's cleaning properties. This negatively impacts pre- and post-treatment processes (such as phosphating and painting), which require a surface free of oil and dirt. In particular, the circumstances described lead to uneven application of further treatment agents. This means that, on the one hand, the application of further agents and / or layers is unevenly thick and, on the other hand, can also exhibit optical defects. Both an uneven primer thickness and optical defects lead to uneven coating, for example, uneven e-coating, and to the associated reduced corrosion resistance.
[0006] The object of the present invention is to provide a skin-passed sheet with a metallic coating which has temporary corrosion protection which, on the one hand, ensures good corrosion protection until further processing of the sheet and, on the other hand, enables further processing without problems. This means that the corrosion protection must no longer exhibit the disadvantages described above in the further process steps up to painting and ultimately completion of the products, nor must it cause any further obstacles. In particular, a painting without optical defects should be achieved with the fewest possible number of work steps. This first requires the application of a complete, uniform and homogeneous temporary corrosion protection; in particular, the strings of pearls / worm structure known to those skilled in the art in the CuSO4 test should no longer be recognizable after coating.Furthermore, the sheet metal treated with temporary corrosion protection should require few, preferably no, new process steps or equipment compared to state-of-the-art processes. The individual components of the temporary corrosion protection must therefore be precisely coordinated. Furthermore, other aspects such as environmental protection, sustainability, and especially health should also be considered.
[0007] Furthermore, the amount of waste should be reduced, with a focus on hazardous waste (as listed in the waste list pursuant to Article 7 of Directive 2008 / 98 / EC of December 30, 2014), particularly chromium and / or nickel compounds. The painted sheet metal, without prior phosphating, should exhibit a visual appearance and / or corrosion resistance similar to that of sheet metal prepared for painting using phosphate and / or chromium-containing pretreatments, particularly tri- / bication zinc phosphating.
[0008] Furthermore, it is an object of the present invention to provide painted components with improved corrosion protection, improved paint adhesion and less infiltration after damage and / or improved stone chip protection compared to the prior art.
[0009] The problem is solved with the features of claim 1.
[0010] The invention relates to a tempered steel sheet comprising a steel substrate and a metallic tempered coating consisting of a zinc or aluminum alloy arranged on one or both sides of the steel substrate, characterized in that the metallic coating has a double-layer temporary corrosion protection, with an intermediate layer containing organic silicon compounds as the first layer and arranged thereabove a second layer containing or consisting of a corrosion protection oil.
[0011] In this context, the term "skin-passed steel sheet" is intended to clarify that, in one alternative, a skin-passed steel sheet has been electrolytically coated with a metallic coating, while, in another alternative, the substrate coated with the metallic coating has been skin-passed. Ultimately, in both alternatives, the steel sheet exhibits a texture created by contact with skin-pass rolls. In the case of electrolytic coating, the resulting coating precisely replicates the skin-passed surface; the coating does not alter the texture. The coating is applied to one or both sides of the steel substrate, preferably both sides.
[0012] The intermediate layer is bonded to the metallic coating by chemisorption, i.e., by chemical bonding. In the broadest sense, chemical bonding can be an ionic bond, a covalent bond, a coordinate bond, or a weak bond via electrostatic attraction or van der Waals forces.
[0013] In one alternative, this intermediate layer is created by the chemical reaction of an aqueous treatment dispersion with the metallic substrate, which chemically alters the adsorbate, i.e., the aqueous treatment dispersion, and / or the adsorbent, i.e., the metallic coating. In another alternative, components of the aqueous dispersion are covalently bonded to components of the metallic coating.
[0014] In one embodiment, the intermediate layer contains or consists of polymers, such as organic polymers based on acrylic acid or derivatives thereof. In an alternative, the intermediate layer contains or consists of:
[0015] - 1 / 4 to 3 parts by weight of a polymer selected from the group consisting of maleic acid / polyacrylic acid copolymer, modified polyacrylic acid or polyacrylic acid,
[0016] - 1 part by weight of a phosphate component and
[0017] - if necessary 1 / 10 to 5 / 10 parts by weight of a metal-containing component selected from the group Zn, Ca, Mg and / or Al.
[0018] In a further alternative, this intermediate layer contains or consists of organic silicon compounds, preferably one or more compounds selected from the group comprising or consisting of: silanes, silanols, siloxanes, alkoxysilanes, derivatives of silanes, siloxanes and / or alkoxysilanes, and polymers and derivatives thereof. Preferred derivatives are one or more compounds selected from the group comprising or consisting of: silanes, siloxanes, alkoxysilanes with functional groups such as -OR with R as H or alkyl, preferably C1 to C7, vinyl, phenyl, benzyl; -NR2 with R as H or alkyl, preferably C1 to C7, vinyl, phenyl, benzyl; condensation products with elimination of water of hydrolyzed alkoxysilanes, i.e. silanols orAlkoxysilanes with hydroxyl groups; at least one silane, silanol and / or siloxane with at least one alkoxy group, with at least one amido group, with at least one amino group, with at least one urea group, as well as condensation products, copolymers and polymers of at least two of the above-mentioned compounds.
[0019] Alternatively or additionally, the above-mentioned silanes, silanols, siloxanes, alkoxysilanes and derivatives thereof are selected from the group comprising or consisting of: bis-tri(m)ethoxysilylalkane, for example bis-triethoxysilylethanes, methyltrimethoxysilane, tetraethoxysilane, aminopropyltriethoxysilane, 4-amino-dialkylalkyldialkoxysilane, 2-aminoethyl-3-amino-propyltrimethoxysilane, 2-aminoethyl-3-amino-propyltriethoxysilane, gamma-aminoalkyltrialkoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-alkylaminoisoalkyltrialkoxysilane, poly(aminoalkyl)alkyldialkoxysilane, aminoalkylaminoalkyltrialkoxysilane, N-(gamma-trialkoxysilylalkyl)dialkylenetriamine;Aminoalkylaminoalkyldialkoxysilane, aminoalkyltrialkoxysilane, bis-aminosilane, bis-diaminosilane, bis-(trialkoxysilylalkyl)amine, such as bis(trimethoxysilylpropyl)amine and / or bis(triethoxysilylpropyl)amine, bis-(trialkoxysilyl)ethane, N-(aminoalkyl)aminoalkyldialkoxysilane, vinyltriacetoxysilane, vinyltrimethoxysilane, ureidopropyl-itrimethoxysilane, gamma-uridoalkyltrialkoxysilane, bis-trimethoxysilylpropylurea;3-[2-(2-Aminoalkylamino)alkylamino]alkyltrialkoxysilane, 3-(2-Aminoethylamino)propyldimethoxymethylsilane, N -(3-(T ria I koxysi ly Da I ky l)al kyl end ia min, N-beta-(aminoalkyl)-gamma-aminoalkyltrialkoxysilane, 4-Amino-dialkylalkyltrialkoxysilane, 3-(trimethoxysilyl)propyl methacrylate, gamma-(trialkoxysilylalkyl)dialkylentriamine, 3-glycidoxypropyltrimethoxysilane, 3-triethoxysilyl-N-(l,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N, N-Bis[3-(trimethoxysilyDpropyllethylenediamine and / or N-2-aminoalkyl-3-aminopropyltrialkoxysilane with alkyl preferably selected from the group comprising or consisting of: methyl, ethyl and / or propyl, such as N-2(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, combinations of at least two of the above-mentioned compounds and / or polymers thereof.;
[0020] For the purposes of the invention, siloxanes are compounds of the formula: R3Si-[O-SiR2]n-O-SiR3, where R is H or alkyl, preferably C1 to C7, and n=0 to 20. Polymers thereof with R=alkyl are referred to as silicones. Alkoxysilanes have the general formula (RO)4-Si, where R is alkyl, preferably C1 to C7.
[0021] Alternatively, the aqueous dispersion may additionally contain inorganic salts, such as salts with cations selected from the group containing or consisting of Zr 4+ , Zn 2+ , Ca 2+ , Mg 2+ , and Al 3+ and preferably copper and anions selected from the group containing or consisting of CF, NO3 _ , SO4 2 ■ and P04 3 '. In one alternative, Cu is present as an oxide. In another alternative, the aqueous dispersion contains no dispersed copper oxalates.
[0022] The intermediate layer is preferably applied as an aqueous dispersion. In this dispersion, at least some of the organic silicon compounds are hydrolyzed or alkoxylated. At least some of the organic silicon compounds react to form polymers, such as polysiloxanes. In the form of the hydrolyzed or alkoxylated organic silicon compounds and / or polysiloxanes, they react with the hydroxyl groups of the metal, releasing water or alcohol, and forming a strong bond with the substrate. Condensation occurs simultaneously and subsequently during drying between the organic silicon compounds, now covalently bonded to the surface, resulting in the formation of a network-like structure that creates a homogeneous intermediate layer evenly distributed over the surface of the coating.
[0023] For the purposes of the invention, the term "aqueous dispersion" encompasses a composition in which particles and / or droplets are dispersed in water, as well as colloidally dispersed and / or molecularly dispersed compositions. Alternatively, the aqueous dispersion contains organic solvents, in particular alcohols, preferably methanol or ethanol, lower ketones, or ethers with up to 7, preferably 5, carbon atoms.
[0024] In one embodiment, the intermediate layer has a Si content of at least 1.0 mg / m2, preferably at least 2.5 mg / m2, particularly preferably at least 5.0 mg / m2, in particular at least 7.5 mg / m2, and a maximum of 100.0 mg / m2 or 75.0 mg / m2, preferably a maximum of 50.0 mg / m2 or 40.0 mg / m2, particularly preferably a maximum of 30.0 or 20.0 mg / m2, in particular a maximum of 15.0 or 12.5 mg / m2. A quantitative determination of the applied layer weight is carried out, for example, by X-ray fluorescence analysis (XRF) or GDOES (Glow Discharge Optical Emission Spectroscopy). The expression that the intermediate layer has a layer weight with a deposit of a certain element in a specified mass per unit area means that the intermediate layer contains the corresponding element (regardless of the form, i.e. elemental, atomic, ionic or oxidic) in the specified mass per unit area.In the event that the Si concentration of the steel sheet, i.e., the steel substrate, interferes with the Si determination in the intermediate layer, thus potentially leading to erroneous results, the expert performs reference or differential measurements at locations on the steel sheet where no intermediate layer is present or where the intermediate layer has been removed for measurement purposes. This information relates to the occurrence of the element Si (silicon), regardless of its form. It therefore does not matter whether this element is present as neutral atoms, as ions, or in compounds such as organic compounds, such as alcohols, esters, polymers or complexes, oxides, salts, hydroxides, or similar.
[0025] In one embodiment, the intermediate layer has a Cu content of at least 0.1 mg / m2, preferably of at least 1.0 mg / m2, particularly preferably of at least 2.0 mg / m2 or of at least 3.0 mg / m2, in particular of at least 4.0 mg / m2 and of at most 100.0 mg / m2 or 75.0 mg / m2, preferably of at most 50.0 mg / m2 or 40.0 mg / m2, particularly preferably of at most 30.0 or 20.0 mg / m2, in particular of at most 15.0 or 10.0 mg / m2. A quantitative determination of the applied layer weight is carried out, for example, using X-ray fluorescence analysis (RFA) or GDOES (Glow Discharge Optical Emission Spectroscopy) analogous to Si as described above.
[0026] The second layer of the double-layer temporary corrosion protection contains or consists of a corrosion protection oil, preferably a mineral oil, particularly preferably containing 15 - 60 wt.%, preferably 20 - 50 wt.% of a naphthenic base oil with 1.0 - 10 wt.%, preferably 1.2 - 8 wt.% Na and / or Ca sulfonates from benzenesulfonic acid with mono-C10-16 alkyl derivatives and / or mono-C16-24 alkyl derivatives as organic radicals.
[0027] The intermediate layer not only ensures temporary corrosion protection, but also reduces or prevents, in comparison to a layer structure without the intermediate layer used according to the invention, the adsorption of polarizable or polar molecules to the metallic coating of the corrosion protection.
[0028] An embodiment further relates to the steel sheet according to the invention, characterized in that the intermediate layer contains rheological additives. Since the intermediate layer is applied as an aqueous solution or aqueous dispersion, the rheology, in particular the viscosity of the solution or dispersion, is crucial. The aqueous dispersion, in which the compounds of the subsequent intermediate layer and the rheological additives are located, is a system in which the components are precisely matched to one another and, on the other hand, additionally matched to the substrate. During the matching process, particular consideration is given to the polarity of the composition and the substrate.
[0029] Alternatively, substances from additive classes such as phyllosilicates, associative thickeners, synthetic layered silicates, liquid rheology additives, or enhancers for fumed silica are used. Rheological additives are preferably selected from the group containing or consisting of: acrylate thickeners, carboxymethylcellulose, methylcellulose, polyurea thickeners, polyurethane thickeners, layered silicates, fumed silica, gelatin, alginates, mono- and / or polysaccharides, including xanthan gum, guar ether, and xanthan gum.
[0030] Particularly preferred is the combination of the above-mentioned organic silicon compounds with rheological additives containing or based on polyurethane or polysaccharides or heteropolysaccharides, preferably modified polysaccharides or heteropolysaccharides, such as guar and / or xanthan gum, in particular slow-swelling guar ether or xanthan gum molecules or modified xanthan gum molecules.
[0031] The combination of the composition for the subsequent intermediate layer with the rheology additives ensures complete wetting of the substrate surface. This results in a uniform, homogeneous dry intermediate layer. Homogeneity refers to the property of the layer exhibiting the same macroscopic properties at all points. Furthermore, the rheology additives can reduce the thickness of the intermediate layer compared to the absence of rheology additives.
[0032] In one embodiment, the intermediate layer contains additional additives, either as an alternative or in addition to the rheological additives, such as poly(meth)acrylic acid and derivatives as a polymer that does not dissolve into smaller compounds under alkaline conditions, or aluminum hydroxides as surface additives that physically delay excessive detachment in alkaline solutions. In addition, tribological additives can be added to improve forming behavior.
[0033] The aqueous dispersion containing the compounds of the subsequent intermediate layer, including the rheological additives and any other additives or components, is a composition in which all components are precisely matched to one another and also to the substrate. Attention must be paid to the stability of the aqueous dispersion, for example, the particle density, the separation rate distribution, and the particle size distribution. These and other criteria and methods for determining stability can be determined according to ISO 13318, ISO / TR 13097:2013; and / or ISO / TR 18811:2018. In particular, the aqueous dispersion exhibits no particle sedimentation or separation (at application temperature) for at least 60 minutes, preferably 120 minutes, more preferably 180 minutes, and especially 240 minutes or more without mechanical mixing or stirring.The match to the substrate can be checked, for example, using a CuSO4 test.
[0034] The present invention further relates to the use of the above-mentioned organic silicon compounds as corrosion protection, in particular as a corrosion protection layer. A further subject matter is the use of the above-mentioned organic silicon compounds in combination with the above-mentioned rheology additives as corrosion protection, in particular as a corrosion protection layer. The rheology additives are incorporated into the corrosion protection layer of organic silicon compounds. This is thus a first corrosion protection layer of organic silicon compounds with incorporated rheology additives.
[0035] The intermediate layer described above forms a complete, uniform, and homogeneous layer. This can be verified by the so-called CuSO4 test. For this purpose, the steel sheet is dried after application of the aqueous dispersion, and rinsed if necessary before drying. The oil- or grease-free surface is immersed in a 5 wt% CuSO4 solution for approximately 10 seconds. The surface is then rinsed in demineralized water by gently swirling.
[0036] When immersed in the CuSO4 solution, bare metal areas react with the free copper ions, and metallic copper is deposited in the form of a black or metallic precipitate. In areas with an inerting post-treatment (passivation, sealing, or similar), less or no copper is deposited, and the precipitate is less dark. In the case of inhomogeneously applied layers, this is clearly visible due to the light-dark contrast. The pearl strings / worm-shaped structure known to those skilled in the art forms, i.e. a series of light or dark dots that can have a width of 0.2 to 1.0 mm or more and a length of several centimeters, possibly even a length across the entire sheet width. The sheets coated with the intermediate layer according to the invention do not exhibit any pearl strings or worm-shaped structures in this CuSO4 test.A complete, uniform and homogeneous intermediate layer is defined in the sense of the invention, i.e. a layer which, after deoiling or degreasing in a CuS04 test as described above, does not exhibit any strings of pearls or worm-shaped structures.
[0037] The steel sheet according to the invention may further comprise at least one further functional coating such as an adhesion-promoting layer, a forming aid, a passivation or a combination thereof.
[0038] Alternatively, the intermediate layer or the aqueous dispersion applied thereto does not comprise or contain any epoxy-based adhesive systems.
[0039] The present invention relates to a hot-dip coated and tempered steel sheet comprising a steel substrate and a metallic, tempered coating arranged on one or both sides of the steel substrate, containing, in addition to zinc and unavoidable impurities, aluminum with a content of 0.1 to 8 wt.% and optionally magnesium with a content of 0.1 to 8 wt.%, characterized in that the metallic coating has a double-layer temporary corrosion protection.
[0040] The Z or ZM coating, applied using the hot-dip coating process, comprises a zinc alloy containing, in addition to zinc (balance) and unavoidable impurities, additional elements such as aluminum with a content between 0.1 and 8 wt.% and, optionally, magnesium with a content between 0.1 and 8 wt.%. Elements from the group Si, Sb, Bi, Zr, Ni, Cr, Pb, Ti, Ca, Mn, Sn, La, Ce, Fe, and Cr may be present as impurities in the molten bath, either individually or cumulatively, in amounts of up to 0.5 wt.%, in particular up to 0.4 wt.%, preferably up to 0.3 wt.%. Elements from the group Si, Sb, Bi, Zr, Ni, Cr, Pb, Ti, Ca, Mn, Sn, La, Ce, Fe, and Cr may be present as impurities in the coating in individual or cumulative amounts of up to 0.5 wt.%, in particular up to 0.4 wt.%, preferably up to 0.3 wt.%. Alternatively, the concentration of Fe may be higher due to the diffusion described above. The remainder is zinc.Steel sheets, separated from steel strips or steel sheet components produced therefrom with a zinc-based corrosion protection coating, have very good cathodic corrosion protection and have been used in automotive engineering for years. If improved corrosion protection is required, the coating has aluminum with a content of at least 0.8 wt.%, in particular at least 1.0 wt.%, preferably at least 1.1 wt.% and optionally magnesium with a content of at least 0.8 wt.%, in particular at least 1.0 wt.%. The coating has aluminum with a content of at most 8.0 wt.%, preferably at most 7.0 wt.%, particularly preferably at most 5.0 wt.%, in particular at most 4.0 wt.% and optionally magnesium with a content of at most 8.0 wt.%, preferably at most 7.0 wt.%, particularly preferably at most 5.0 wt.%, in particular at most 4.0 wt.%.Alternatively, these concentrations are determined using wet-chemical methods in accordance with or based on DIN EN ISO 10111:2019 and / or DIN EN ISO 11885:2009.
[0041] In particular, to set a predetermined thickness of the Z or ZM coating, which in the solid state can be between 1 μm and 60 μm per side, the melt applied to the steel strip while still in the liquid state is scraped off. After leaving the molten bath, the steel strip coated with the liquid melt is passed through a scraping device which has means, for example nozzles, in particular slot nozzles, which act on both sides of the steel strip with a gaseous scraping medium to scrape off the liquid melt. This makes it possible to achieve an asymmetric coating, i.e. different coating layers on both sides. The thickness of the Z or ZM coating can be set, in particular, independently of one another, for each side, between at least 4 μm, preferably at least 5 μm and a maximum of 58 μm, preferably between 5 and a maximum of 55 μm.In a particular embodiment, the thickness of the coating is at least 1 μm, preferably at least 2 μm, particularly preferably at least 3 μm, in particular at least 5 μm and a maximum of 25 μm, preferably a maximum of 20 μm, and particularly preferably a maximum of 15 μm, in particular a maximum of 10 μm, independently of one another, per side. Alternatively, the coating thickness is determined gravimetrically by detachment according to DIN EN ISO 10111 and conversion from mass to thickness based on density, or metallographically in a micrograph.
[0042] Below the minimum limits, sufficient cathodic corrosion protection cannot be guaranteed and above the maximum limit, joining problems may occur when connecting the steel sheet according to the invention or a component made from it to another component.
[0043] Alternatively, the Z or ZM coating has a coating weight of 1 to 650 g / m2, i.e., 0.5 to 320 g / m2 per side, particularly preferably 10 to 500 g / m2, i.e., 5 to 250 g / m2 per side. In another alternative, an asymmetric coating is also possible.
[0044] The present invention further relates to a hot-dip coated and temper-rolled steel sheet as described above, wherein the metallic coating contains unavoidable impurities in addition to zinc and 0.1% to 1.0% aluminum, and has been annealed after hot-dip coating (at temperatures above the melting point of zinc). The coating thus treated consists exclusively of iron-zinc compounds; it is a sheet with a so-called ZF coating.
[0045] The present invention further relates to a skin-passed steel sheet as described above, wherein the metallic coating contains, in addition to zinc, unavoidable impurities and optionally 0.001% to 1%, preferably 0.01% to 1% aluminum and has been applied electrolytically to the skin-passed substrate (electrolytically applied zinc coating (ZE)). Such sheets are defined, for example, in DIN EN 10152:2017-06, but the use of hot-rolled strip as the sheet substrate is also possible according to the invention. The present invention further relates to a skin-passed steel sheet as described above, wherein the metallic coating consists of a silicon-containing aluminum alloy. Suitable aluminum alloys typically consist of 0.1 - 15 wt.% Si, preferably more than 1 wt.% Si, optionally 2 - 4 wt.% Fe, optionally up to 5 wt.% alkali or alkaline earth metals, preferably up to 1% wt.% alkali or alkaline earth metals, and optionally up to 15% wt.-% Zn, preferably up to 10 wt.% Zn and optional further components, the total contents of which are limited to a maximum of 2 wt.%, and the remainder consisting of aluminum and unavoidable impurities. In a preferred variant, the Si content is 1.0 - 3.5 wt.% or 7 - 12 wt.%, in particular 8 - 10 wt.% In a preferred variant, the optional content of alkali or alkaline earth metals comprises 0.1 - 1.0 wt.% Mg, in particular 0.1 - 0.7 wt.% Mg, preferably 0.1 - 0.5 wt.% Mg. Furthermore, the optional content of alkali or alkaline earth metals can comprise in particular at least 0.0015 wt.% Ca, in particular at least 0.01 wt.% Ca.
[0046] Such a corrosion protection coating is preferably produced by hot-dip coating the flat steel product. During hot-dip coating, iron diffuses from the steel substrate into the liquid coating, so that the corrosion protection coating of the flat steel product, upon solidification, has, in particular, an alloy layer and an Al base layer. The alloy layer consists of 35–60 wt.% Fe, optionally further components whose total contents are limited to a maximum of 5.0 wt.%, and the remainder is aluminum. The Al base layer consists of 1.0–15 wt.% Si, optionally 2–4 wt.% Fe, optionally up to 5.0 wt.% alkali or alkaline earth metals, optionally up to 10% Zn, and optionally further components whose total contents are limited to a maximum of 2.0 wt.%, and the remainder is aluminum.
[0047] The aluminum alloy-based metallic coating has a thickness of 5–60 μm, particularly 10–40 μm. The coating weight of the corrosion protection coating is particularly 30–360 g / m² for double-sided corrosion protection coatings and 15–180 g / m² for the single-sided version. The coating weight of the metallic coating is preferably 100–200 g / m² for double-sided coatings and 50–100 g / m² for single-sided coatings.
[0048] Hot-dip coating processes are known to those skilled in the art. Hot-dip coating may additionally comprise one or more of the following steps: cleaning the substrate before the hot-dip bath; heating the substrate; wiping the melt using nozzles after the hot-dip bath to achieve the desired coating thickness; cooling the coated substrate to cure the melt; optionally applying a temper coating; optionally applying further functional coatings, such as an adhesion-promoting layer, a forming aid, a passivation layer, or a combination thereof.
[0049] Skin-passing is known to those skilled in the art and is described, for example, in the handbook "Umformen" (Forming), by Günter Spur, ISBN: 978-3-446-43004-4, page 155. The surface of the steel sheet after skin-passing can exhibit a stochastic surface structure. This is created using skin-pass rolls whose surfaces are textured using a so-called EDT process. Alternatively, the surface of the steel sheet after skin-passing can exhibit a deterministic surface structure. This is created using skin-pass rolls whose surfaces are textured using a laser. A surface exhibiting a pseudo-stochastic surface structure after skin-passing is also conceivable. These surface structures have a (guasi-)stochastic appearance, composed of stochastic elements with a recurring structure.
[0050] If necessary, a cleaning step is carried out before the application of the first corrosion protection layer, preferably an alkaline cleaning step, if necessary with detergents, possibly followed by a rinsing and, if necessary, drying step.
[0051] One version features a steel sheet with a Cr-free, double-layer temporary corrosion protection. Cr-free means that Cr is present in a maximum concentration of 1000 ppm, preferably 500 ppm, and especially 100 ppm [according to VdL Guideline 01 "VdL Guideline Declaration of Coating Materials" Guideline for the Declaration of Lacquers, Paints, Glazes, Renders, Leveling Compounds, Primers, and Related Products, as of May 2019 (7th revision) of the German Association of the Paint and Printing Ink Industry].
[0052] According to the invention, the steel substrate to be used is a hot-rolled or cold-rolled strip. These can be obtained by processes known to those skilled in the art. The steel substrate can be used in the form of steel strips, so-called coils, or as so-called blanks, which are preferably obtained by separating pieces from a hot-rolled or cold-rolled strip using suitable processes. In a further embodiment, a steel sheet is used, characterized in that the steel substrate comprises an alloy containing or consisting of the following elements in wt.%:
[0053] - C: 0.0003 to 0.250%,
[0054] - Si: 0.0005 to 0.70%,
[0055] - Mn: 0.0005 to 2.0%,
[0056] - P: up to 0.15%,
[0057] - S: up to 0.050%,
[0058] - N: up to 0.10%,
[0059] - AI: 0.0050 to 1.50%,
[0060] - optionally one or more of the following elements:
[0061] - Nb: up to 0.20%,
[0062] - Ti: 0.20%,
[0063] - V: 0.0050 to 0.10%,
[0064] - B: up to 0.030% and / or
[0065] - Cu: up to 0.80% and / or
[0066] - Cr: up to 0.80% and / or
[0067] - Ni: up to 0.20% and / or
[0068] - Mo: up to 0.150% and / or
[0069] - Sn: up to 0.10%,
[0070] - Residual iron and unavoidable impurities.
[0071] Alternatively, the substrate is a steel sheet made of an interstitial-free alloy according to DIN EN 10346. The IF alloy of the steel substrate contains or consists of the following elements in wt.%:
[0072] - C: 0.0003 to 0.015%, in particular 0.0005 to 0.010%, preferably 0.001 to 0.005%,
[0073] - Si: 0.0005 to 0.50%, in particular 0.0010 to 0.40%, preferably 0.0010 to 0.30%,
[0074] - Mn: 0.0005 to 1.60%, in particular 0.010 to 1.55%, preferably 0.010 to 1.50%,
[0075] - P: up to 0.10%, in particular up to 0.080%, preferably 0.0002 to 0.060%,
[0076] - S: up to 0.050%, in particular up to 0.040%, preferably 0.0003 to 0.030%,
[0077] - N: up to 0.10%, in particular up to 0.080%, preferably 0.0001 to 0.070%, - AI: 0.0010 to 1.0%, in particular 0.0010 to 0.90%, preferably 0.0010 to 0.80%,
[0078] - one or both of the following elements:
[0079] - Nb: 0.0001 to 0.20%, in particular 0.0002 to 0.10%, preferably 0.0003 to 0.050%,
[0080] - Ti: 0.0005 to 0.20%, in particular 0.010 to 0.150%, preferably 0.010 to 0.120%,
[0081] - optionally one or more of the following elements:
[0082] - B: up to 0.0050% and / or Cu up to 0.20% and / or Cr up to 0.20% and / or Ni up to 0.20% and / or Mo up to 0.150% and / or Sn up to 0.10%,
[0083] - Residual iron and unavoidable impurities.
[0084] An IF steel has no interstitial alloying elements, meaning that no iron atoms in the metal lattice are blocked by carbon or nitrogen atoms. This results in a very soft steel with excellent formability. It is primarily used for complex deep-drawn parts in automotive engineering. Steels of this type are available under the standard designations DX52D, DX53D, DX54D, DX55D, DX56D, DX57D, HX160YD, HX180YD, HX220YD, and HX260YD. These are cold-rolled steels.
[0085] Alternatively, the substrate is a steel sheet made of a bake-hardening alloy according to DIN EN 10346. The bake-hardening alloy of the steel substrate contains or consists of the following elements in wt.%:
[0086] - C: 0.0004 to 0.080%, in particular 0.0010 to 0.060%, preferably 0.0010 to 0.040%,
[0087] - Si: 0.0005 to 0.50%, in particular 0.0010 to 0.40%, preferably 0.010 to 0.20%,
[0088] - Mn: 0.0005 to 1.50%, in particular 0.0010 to 1.40%, preferably 0.0020 to 1.20%,
[0089] - P: up to 0.150%, in particular up to 0.10%, preferably 0.0010 to 0.050%,
[0090] - S: up to 0.050%, in particular up to 0.040%, preferably 0.0005 to 0.030%,
[0091] - N: up to 0.050%, in particular up to 0.030%, preferably 0.0002 to 0.010%,
[0092] - AI: 0.0050 to 1.0%, in particular 0.010 to 0.50%, preferably 0.010 to 0.150%,
[0093] - optionally one or more of the following elements:
[0094] - Nb: up to 0.040% and / or Ti up to 0.030% and / or B up to 0.0030% and / or Cu up to 0.20% and / or Cr up to 0.20% and / or Ni up to 0.20% and / or Mo up to 0.150% and / or Sn up to 0.10%,
[0095] - The remainder is iron and unavoidable impurities. BH steels are characterized by a significant increase in yield strength during paint baking (typically at 170 °C for 20 minutes) combined with excellent formability. Furthermore, these steels possess very good dent resistance, which is why they are preferred for exterior body applications. Steels of this type are available under the standard designations HX180BD, HX220BD, HX260BD, and HX300BD. These are cold-rolled steels.
[0096] Alternatively, the substrate is a steel sheet made of a multiphase alloy according to DIN EN 10346. The multiphase alloy of the steel substrate contains or consists of the following elements in wt.%:
[0097] - C: 0.050 to 0.250%, in particular 0.060 to 0.250%, preferably 0.070 to 0.250%,
[0098] - Si: 0.020 to 0.50%, in particular 0.020 to 0.40%, preferably 0.020 to 0.30%,
[0099] - Mn: 1.30 to 2.0%, in particular 1.40 to 1.90%, preferably 1.50 to 1.80%,
[0100] - P: up to 0.10%, in particular up to 0.080%, preferably up to 0.060%,
[0101] - S: up to 0.050%, in particular up to 0.040%, preferably up to 0.030%,
[0102] - N: up to 0.10%, in particular up to 0.050%, preferably up to 0.030%,
[0103] - AI: 0.010 to 0.150%, in particular 0.010 to 0.10%, preferably 0.010 to 0.090%,
[0104] - optionally one or more of the following elements:
[0105] - Cu: up to 0.80% and / or Cr up to 0.70% and / or Nb up to 0.10% and / or Ti up to 0.20%;
[0106] - Residual iron and unavoidable impurities.
[0107] Examples of steels of this type are available under the standard designations HCT490X, HCT590X, or HCT780X. These are cold-rolled steels.
[0108] Alternatively, the substrate is a steel sheet made of a micro-alloyed alloy according to DIN EN 10268. The alloy of the steel substrate contains or consists of the following elements in wt.%:
[0109] - C: 0.020 to 0.20%, in particular 0.020 to 0.150%, preferably 0.020 to 0.140%,
[0110] - Si: 0.010 to 0.70%, in particular 0.010 to 0.60%, preferably 0.010 to 0.50%,
[0111] - Mn: 0.020 to 2.0%, in particular 0.020 to 1.90%, preferably 0.020 to 1.80%,
[0112] - P: up to 0.070%, in particular up to 0.060%, preferably up to 0.050%, - S: up to 0.050%, in particular up to 0.040%, preferably up to 0.030%,
[0113] - N: up to 0.080%, in particular up to 0.060%, preferably up to 0.040%,
[0114] - AI: 0.010 to 1.0%, in particular 0.010 to 0.50%, preferably 0.010 to 0.10%,
[0115] - at least one of the following elements:
[0116] - Nb: 0.010 to 0.150%, in particular 0.010 to 0.120%, preferably 0.010 to 0.10% and / or
[0117] - Ti: 0.010 to 0.20%, in particular 0.010 to 0.180%, preferably 0.010 to 0.150% and / or
[0118] - V: 0.0050 to 0.10%, in particular 0.0060 to 0.10%, preferably 0.0090 to 0.10% and / or
[0119] - optionally one or more of the following elements:
[0120] - B: up to 0.0050% and / or Cu up to 0.40% and / or Cr up to 0.50%,
[0121] - Residual iron and unavoidable impurities.
[0122] A microalloyed steel exhibits a fine-grained microstructure, which gives it high fatigue strength, optimal weldability, and high yield strengths. It is primarily used for complex deep-drawn parts in automotive engineering. Examples of steels of this type are available under the standard designations HC260LA, HC300LA, HC340LA, HC380LA, HC420LA, HC460LA, HC500LA, and HC550LA. These are cold-rolled steels.
[0123] The present invention also relates to a method for producing a skin-passed steel sheet as described above, comprising the following steps: a) providing a skin-passed steel sheet having a metallic coating as described above as a steel substrate, b) applying a first layer as an intermediate layer to the steel sheet from step a, c) applying a second layer to the intermediate layer from step b containing or consisting of corrosion protection oil.
[0124] In step a, a steel sheet as described above is used as the steel substrate.
[0125] In step b, the first intermediate layer is applied to the skin-passed steel sheet in the form of an aqueous dispersion. Application is carried out by spraying, dipping, or coating, preferably using a roll coater or chem-coater, at an ambient temperature of 10–50 °C, preferably 20–40 °C.
[0126] The aqueous dispersion contains polymers or organic silicon compounds as described above, in a concentration based on Si as an element of at least 0.002 wt%, preferably of at least 0.02 wt%, particularly preferably of at least 0.08 wt% or 0.12 wt%, in particular of at least 0.16 wt% and of at most 25.0 wt% or 5.0 wt%, preferably of at most 2.5 wt% or 1.25 wt%, particularly preferably of at most 0.75 wt%, in particular of at most 0.60 wt%.
[0127] Alternatively, based on at least one organic silicon compound, the aqueous dispersion contains at least 0.0002 wt.%, preferably at least 0.002 wt.%, particularly preferably at least 0.02 wt.% or 0.050 wt.%, in particular at least 0.08 wt.% and at most 25.0 wt.% or 5.0 wt.%, preferably at most 2.5 wt.% or 0.5 wt.%, particularly preferably at most 0.375 wt.%, in particular at most 0.30 wt.% of at least one of the above-mentioned organic silicon compounds.
[0128] In one embodiment, the aqueous dispersion contains one or more of the rheology additives described above.
[0129] The rheology additives are present in a concentration of active ingredient of at least 0.01 wt%, preferably at least 0.025 wt%, particularly preferably at least 0.05 wt%, in particular at least 0.075 wt% and of at most 5.0 wt% or 2.5 wt%, preferably of at most 1.0 wt%, particularly preferably of at most 0.75 or 0.5 wt%, in particular of at most 0.25 or 0.15 wt%.
[0130] In an alternative, the aqueous dispersion is an alkaline aqueous dispersion having a pH of at least 8.0, preferably at least 9.0, particularly preferably at least 9.5, in particular at least 10.0 and at most 13.0, preferably at most 12.5, particularly preferably at most 12.0 or 11.0, in particular at most 10.5.
[0131] In a further alternative, the aqueous dispersion has a density at 20 °C of at least 0.90 g / cm3, preferably at least 0.95 g / cm3, more preferably at least 1.00 g / cm3 and at most 1.30 g / cm3, preferably at most 1.20 g / cm3, more preferably at most 1.10 g / cm3 and in particular at most 1.0 g / cm3. In a further alternative, the aqueous dispersion has a dynamic viscosity at 20 °C in mPa*s of at least 0.6, preferably at least 0.75, more preferably at least 0.9, in particular at least 1.0 and at most 2.0, preferably at most 5.0, more preferably at most 10.0, in particular at most 15.0.
[0132] In one embodiment, the aqueous dispersion is Cr-free. For the term Cr-free (chromium-free), see above. In one embodiment, the dispersion contains Cu (ionic or oxide) in a concentration such that the dried interlayer contains 1.0 to 100 mg / m² of copper, as described above.
[0133] A further embodiment relates to the process described above, wherein the steel sheet is rinsed after application of the aqueous dispersion and then dried, preferably without prior rinsing, in the so-called no rinse process.
[0134] If necessary, further functional coatings are applied, such as an adhesion-promoting layer, a forming aid, a passivation or a combination thereof.
[0135] Furthermore, the present invention relates to the use of a steel sheet according to the invention provided with the temporary corrosion protection described above for producing a painted component.
[0136] The present invention also further provides a method for producing a painted component comprising the following steps: d) providing a steel sheet according to the invention described above or a steel sheet produced by the method described above, e) cleaning the steel sheet so that an intermediate layer with a coating of Si of at least 0.2 mg / m2 Si remains and f) coating with a layer containing Si and / or Zr.
[0137] Step e of the process according to the invention is preferably carried out by treating the steel sheet from step d with at least one cleaning agent. According to the invention, the cleaning agent can be acidic, neutral, or alkaline. In a preferred embodiment, an alkaline cleaning agent is used. In one alternative, the alkaline cleaning agent is an alkaline aqueous dispersion with a pH of at least 8.0, preferably at least 9.0, particularly preferably at least 10.0, in particular 11.0 and at most 14.0, preferably at most 13.0, particularly preferably at most 12.0, in particular at most 11.5. The cleaning-active substances, for example surfactants, are preferably present in an amount that appears suitable to the person skilled in the art. According to the invention, further components of the cleaning agent are preferred, for example selected from the group consisting of sodium hydroxide or potassium hydroxide and mixtures thereof.Step e can also be carried out using mechanical energy, for example by brushing the surfaces to be cleaned or by applying water and / or cleaning agents to the surface under high pressure. Step g of the process according to the invention is preferably carried out at a temperature of 20 to 80°C.
[0138] In step e, the second temporary corrosion protection layer containing or consisting of a corrosion protection oil and part of the intermediate layer containing the organic silicon compounds are removed. A homogeneous intermediate layer remains on the sheet, evenly distributed over the surface of the metallic coating, with a lower layer weight than before cleaning in step e. This remaining intermediate layer has a Si content of at least 0.5 mg / m2, preferably of at least 5.0 mg / m2, more preferably of at least 7.5 mg / m2, in particular of at least 10.0 mg / m2 or at least 11.0 mg / m2 and of at most 80.0 mg / m2 or 50.0 mg / m2, preferably of at most 40.0 mg / m2 or 30.0 mg / m2, more preferably of at most 25.0 or 20.0 mg / m2, in particular of at most 15.0 or 12.5 mg / m2.
[0139] In one embodiment, the remaining intermediate layer has a Cu content of at least 0.05 mg / m2, preferably of at least 1.0 mg / m2 or of at least 2.5 mg / m2, particularly preferably of at least 3.0 mg / m2 or of at least 3.5 mg / m2, in particular of at least 4.0 mg / m2 and of at most 80.0 mg / m2 or 50.0 mg / m2, preferably of at most 40.0 mg / m2 or 30.0 mg / m2, particularly preferably of at most 20.0 or 15.0 mg / m2, in particular of at most 12.5 or 10.0 mg / m2.
[0140] A quantitative determination of the remaining layer weight is carried out, for example, by X-ray fluorescence analysis (XRF) or GDOES (Glow Discharge Optical Emission Spectroscopy) with respect to Si and / or Cu as described above, in particular by commercially available XRF handheld devices.
[0141] In step f, in one embodiment, a further layer is applied as an aqueous dispersion, analogous to the intermediate layer as described above. This layer contains organic silicon compounds selected from the organic silicon compounds described above. A layer containing 0.1 mg / m2, preferably at least 0.5 mg / m2 or 1.0 mg / m2, particularly preferably at least 5.0 mg / m2, in particular at least 10.0 mg / m2 and a maximum of 500.0 mg / m2 or 300.0 mg / m2, preferably a maximum of 200.0 mg / m2 or 100.0 mg / m2, particularly preferably a maximum of 75.0 or 50.0 mg / m2, in particular a maximum of 25.0 mg / m2 of Si is applied.
[0142] Additionally or alternatively, a layer containing 0.5 mg / m2, preferably at least 1.0 mg / m2 or 2.0 mg / m2, particularly preferably at least 5.0 mg / m2, in particular at least 10.0 mg / m2 and at most 200.0 mg / m2 or 100.0 mg / m2, preferably at most 50.0 mg / m2, particularly preferably at most 30.0 mg / m2, in particular at most 25.0 mg / m2 Zr is applied, likewise as an aqueous dispersion.
[0143] In an alternative, the aqueous dispersion containing organic silicon compounds additionally contains zirconium (Zr), and is applied in such a way that Zr is present in the layer in concentrations as stated above.
[0144] In a further alternative, the dispersion containing organic silicon compounds and optionally Zr contains Cu and is applied such that the layer has a Cu content of at least 0.1 mg / m2, preferably of at least 1.0 mg / m2, particularly preferably of at least 2.0 mg / m2 or of at least 3.0 mg / m2, in particular of at least 4.0 mg / m2 and of at most 500.0 mg / m2 or 200.0 mg / m2, preferably of at most 100.0 mg / m2 or 50.0 mg / m2, particularly preferably of at most 30.0 or 20.0 mg / m2, in particular of at most 15.0 or 10.0 mg / m2. A quantitative determination of the applied layer weight is carried out, for example, by X-ray fluorescence analysis (RFA) or GDOES (Glow Discharge Optical Emission Spectroscopy) analogous to Si as described above.
[0145] The application of the layer(s) is also carried out as described above, observing the respective concentration specifications. A further embodiment of the above-described process involves rinsing and subsequent drying after application of the aqueous dispersion. Preferably, drying occurs without prior rinsing, in the so-called no-rinse process.
[0146] In one embodiment, the method comprises at least one of the further steps, preferably selected from the group containing or consisting of:
[0147] Cutting the steel sheet from step d,
[0148] Forming the board,
[0149] Joining the formed blank with other parts, preferably made of metal, in particular steel, to form a component.
[0150] After cleaning and coating as described above in steps e and f, painting follows, preferably by means of a KT painting.
[0151] In one version, all layers applied to the metallic coating are free of chromium, nickel and / or manganese.
[0152] In general, several methods can be used to apply the treatment solutions or dispersions described above. For flat strip products and smaller quantities, the solutions or dispersions can be applied by hand, spray coating, or roller application. In the automotive industry, dipping and spraying processes, or a combination of the two, are most commonly used, as they have no limitations on the quantity, shape, and size of the surfaces to be coated and / or painted and enable high throughput. Oil can also be applied electrostatically.
[0153] The present invention therefore further relates to painted components, preferably components with a KT coating and optionally additional paint layers, manufactured as described above, which exhibit improved corrosion protection, improved paint adhesion, reduced infiltration after damage, and improved stone chip protection compared to components manufactured using steel sheets without a uniform and continuous intermediate layer. Within the scope of the invention, all of the aforementioned different embodiments or alternatives can be combined.
[0154] Examples:
[0155] 1. Preparation of samples:
[0156] To test the effectiveness of the invention, blanks were cut from conventionally produced IF steel strip as samples RF (reference), ZW1, ZW2, and ZW3. The steel substrate in each case consisted of a commercially available steel sold under the designation M3A33, the composition of which is given in Table 1.
[0157] Table 1
[0158] Rest iron and unavoidable impurities, contents in wt.%
[0159] The steel strip from which the samples were taken had a Zn-Al-Mg coating (“ZM coating”) applied to its surfaces by conventional hot-dip coating and consisting of 1.6 wt% Al, 1.2 wt% Mg, and the remainder Zn and unavoidable impurities.
[0160] For further tests, blanks were cut from this ZM coated steel strip and further processed at a pilot plant scale.
[0161] The boards were coated with a dispersion using a chem-coater after hot-dip coating, as follows:
[0162] RF: ZM without intermediate layer, without further treatment;
[0163] ZW1: ZM + intermediate layer, applied as an aqueous dispersion with organic silicon compounds with a Si element content of 0.2 wt.%; ZW2: ZM + intermediate layer; applied as an aqueous dispersion with organic silicon compounds with a Si element content of 0.2 wt.% + 0.5 wt.% polyurethane thickener Agocel AG 6240;
[0164] ZW3: ZM + intermediate layer; applied as an aqueous dispersion with organic silicon compounds with a Si element content of 0.2 wt.% + 5 wt.% polyurethane thickener Agocel AC 6240.
[0165] The boards were oiled with ANTICORIT PL 3802 39 S using a roll coater.
[0166] 2. CuSO4 test:
[0167] The circuit boards were deoiled or degreased with benzine or n-heptane and immersed in a 5 wt% CuSO4 solution for approximately 6 s. They were then rinsed in demineralized water by gentle swirling and visually inspected.
[0168] In all samples treated with the intermediate layer (ZW1, ZW2, ZW3), no deep dark precipitate was visible, as is typical for non-treated surfaces, whereas on the reference RF, light-dark contrasts in the form of strings of pearls or worm-shaped structures were clearly visible.
[0169] The results demonstrate that the sheets according to the invention fulfill the stated objectives and, in particular, provide excellent temporary corrosion protection, which enables painting without optical defects.
Claims
Patent claims 1. A temper-rolled steel sheet comprising a steel substrate and a metallic coating consisting of a zinc or aluminum alloy arranged on one or both sides of the steel substrate, characterized in that the metallic coating has a double-layer temporary corrosion protection, with an intermediate layer containing organic silicon compounds as the first layer and, arranged thereover, a second layer containing or consisting of a corrosion protection oil.
2. Steel sheet according to claim 1, characterized in that the intermediate layer has a layer weight with a coating of at least 1.0 mg / m2 and a maximum of 100 mg / m2 Si.
3. Steel sheet according to one of the preceding claims, characterized in that the intermediate layer contains rheological additives.
4. Steel sheet according to one of the preceding claims, characterized in that the intermediate layer contains organic silicon compounds, one or more compounds selected from the group comprising or consisting of: silanes, silanols, siloxanes, alkoxysilanes, derivatives of silanes, silanols, siloxanes and / or alkoxysilanes and polymers and derivatives thereof.
5. Steel sheet according to one of the preceding claims, characterized in that the intermediate layer has a coating weight with a coating of 1 to 100 mg / m2 copper.
6. Steel sheet according to one of the preceding claims, characterized in that the metallic coating consists of zinc or a zinc alloy comprising, in addition to zinc and unavoidable impurities, also aluminum with a content of 0.001 to 8 wt.% and optionally magnesium with a content of 0.1 to 8 wt.%.
7. Steel sheet according to one of claims 1 to 6, characterized in that the metallic coating consists of a silicon-containing aluminum alloy.
8. Steel sheet according to one of the preceding claims, characterized in that the steel substrate comprises an alloy containing or consisting of the following elements in wt.%: C: 0.0003 to 0.250%; Si: 0.0005 to 0.70%; Mn: 0.0005 to 2.0%; P: up to 0.15%; S: up to 0.050%; N: up to 0.10%; AI: 0.0050 to 1.50%; optionally one or more of the following elements: Nb: up to 0.20%; Ti: 0.20%; V: 0.0050 to 0.10% B: up to 0.030% and / or Cu: up to 0.80% and / or Cr: up to 0.80% and / or Ni: up to 0.20% and / or Mo: up to 0.150% and / or Sn: up to 0.10%; Rest iron and unavoidable impurities.
9. A method for producing a skin-rolled steel sheet according to one of claims 1 to 8, comprising the following steps: a providing a skin-rolled, metallically coated steel sheet, b applying a first intermediate layer to the steel sheet from step a, c applying a second corrosion protection layer to the intermediate layer.
10. The method according to claim 9, characterized in that the first intermediate layer is applied as an aqueous, alkaline dispersion and is optionally dried without prior rinsing.
11. Use of a steel sheet according to one of claims 1 to 7 or a steel sheet produced according to one of claims 8 to 10 for producing a painted component.
12. A method for producing a painted component comprising the following steps: d providing a steel sheet according to any one of claims 1 to 7 or a steel sheet produced according to any one of claims 8 to 10; e cleaning the steel sheet so that an intermediate layer with a coating weight in a coating with Si of at least 0.2 mg / m2 Si remains and f applying a layer containing Si and / or Zr to the cleaned steel sheet from step e.
13. The method according to claim 12, wherein in step f a layer is produced with 0.1 to 500 mg / m2 Si, and / or 0.5 to 200 mg / m2 Zr.
14. Method according to claim 12 or 13, comprising at least one of the further steps: Cutting the steel sheet into blanks, Forming the board, Joining the formed blank with other parts, preferably made of metal, in particular steel, to form a component.
15. Method according to one of claims 12 to 14, characterized in that in a step g the steel sheet from step f is painted.
Citation Information
Patent Citations
Coated steel strip or sheet having advantageous properties
EP2888385B1
Activation treatment of coated steel substrates
WO2015124322A1