Method for producing a high-temperature-resistant integral bond
The method of using a completely melted annular element for thermal joining between mineral-insulated cables and connecting parts addresses the challenges of existing methods by creating a cohesive, high-temperature-resistant connection that is media-tight and compliant with standards, ensuring stability and integrity at elevated temperatures.
Patent Information
- Application Number
- PCT/EP2024/060300
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
Existing methods for joining mineral-insulated sheathed cables to connecting parts are prone to gaps, corrosion, and weld seam irregularities due to material property differences, leading to non-media-tight connections and compliance issues at high temperatures.
A method involving a thermal joining process using an annular element that is completely melted to create a cohesive, high-temperature-resistant circular seam connection between the conductor element and the connecting part, which can be achieved through soldering or welding without additional filler materials, ensuring a strong and error-free joint.
The method produces a high-temperature-resistant, media-tight connection that is independent of the geometric and physical properties of the cable and connecting part, reducing the risk of corrosion and compliance issues, and maintaining integrity at temperatures above 380°C.
Smart Images

Figure EP2024060300_24102024_PF_FP_ABST
Abstract
Description
[0001] Method for producing a high-temperature-resistant material-to-material joint
[0002] The invention relates to a method for producing a high-temperature-resistant, in particular temperature-resistant, material-to-material joint between a conductor element and a connecting part. Furthermore, the invention relates to a high-temperature-resistant, in particular temperature-resistant, assembly, particularly temperature-resistant at temperatures of at least 380°C, preferably at least 700°C.
[0003] Field devices in automation technology, especially industrial temperature measuring devices or their process-related components used to record process variables, are designed for high-temperature applications using so-called mineral-insulated sheathed cables (also known as mineral-insulated cables or mineral-insulated wires, or MIL for short). These are specifically designed for high-temperature applications and are typically exposed to corrosive and mechanical stress during normal use. In addition to the aforementioned applications in temperature measurement technology, MIL cables are also used in signaling and / or heating technology.
[0004] MI cables typically comprise a tubular element with an outer sheath, inside which inner conductors (usually 1 to 8) run, particularly parallel to the cylindrical axis of the outer sheath. The outer sheath is typically made of a metal (e.g., stainless steel, nickel-based alloy, copper, etc.) and has an outer diameter in the range of 0.5 to 10.0 mm. The inner conductors are insulated from the outer sheath and, if necessary, from each other by means of a compact insulating material, e.g., by being pressed into a metal oxide powder, especially a highly compressed one, e.g., MgO, Al2O3, SiO2. The inner conductors can have different diameters, depending on the MI cable type. Depending on the powder type, this powder can be of varying hygroscopicity and / or density, have varying grain sizes, have a different degree of dryness, and / or may contain chemically bound (residual) water.
[0005] Such a conductor element is then cut to the required length, for example, when constructing a thermometer measuring insert, and the inner conductors are exposed over a certain length. A corresponding temperature sensor element is then soldered or welded in a two-, three-, or four-wire circuit. The inner conductors are made, for example, of a thermal material (when the MI leads are used as connecting leads for a thermocouple as the temperature sensor element) or of a Cu-Ni or Ni-Cr alloy, Ni-plated copper, Ni, or Cu (when the MI leads are used as connecting leads for a PTC thermistor, e.g., a Pt100, as the temperature sensor element).
[0006] The outer sheath is also often joined to a connecting part, particularly a metal one, using an additional joint. The connecting part has a guide, e.g., designed as a bore, into which the conductor element is inserted. Connecting an Ml cable to the connecting part using the additional joint enables the installation of the Ml cable, e.g., for temperature measurement, in a technical system, especially an automation process system. The technical system typically comprises a container, such as a (pressure) vessel, silo, pipeline, etc., with a medium arranged therein – e.g., a fluid (gas, liquid) or a solid. This (additional) joint therefore serves the purpose of mechanically connecting the conductor element to the connecting part and not (also) electrically contacting the conductor element. The joint should therefore also be designed to be sealed against the medium.
[0007] Various joining techniques are known from the prior art for implementing the aforementioned, particularly non-detachable, joint between a mineral-insulated sheathed cable and a connecting part. The joint is typically force-fit and / or material-fit. A particular challenge, especially for high-temperature applications, is that the components of a mineral-insulated cable (outer sheath, insulation material, inner conductor) and, if applicable, the connecting part are made of different materials and therefore have different physical properties, especially heat capacities and thermal conductivity coefficients.
[0008] Force-locking joints include crimping, for example, in which the connecting part is pushed onto the Ml cable and overlaps it. The connecting part is deformed, particularly pressed, at several points on both joining partners in an overlapping area (also: circumference). In this way, both dissimilar (Ml cable and connecting part consist of different base materials) and similar (Ml cable and connecting part consist of the same or very similar base materials) material combinations can be joined. Such purely force-locking joints have the following disadvantages:
[0009] Depending on the degree / type of deformation at the crimp point, one or more gaps may form, allowing corrosion to occur at the joint upon contact with the process medium. As a result, the joint may no longer be sufficiently media-tight, especially gas-tight.
[0010] During crimping, the connection point is crushed, resulting in deformation of the Ml cable. This can lead to noncompliance with required specifications, especially those according to relevant standards, e.g., IEC 61515 and / or ASTM E585 / E585M, e.g., regarding minimum distances between the inner conductors and / or between the inner conductor and the outer sheath.
[0011] Bonded joints include adhesive bonding, soldering, and welding, with thermal processes typically being preferred. The amount of heat applied during welding is generally significantly greater than during soldering.
[0012] During soldering, the two joining partners usually remain in the solid phase and are not melted. Soldering is primarily based on diffusion processes and requires the addition of a solder whose liquidus temperature is lower than the solidus temperature of the joining partners and has a different chemical composition than the two joining partners. For example, a joining gap is provided between the MI wire and the connecting part, into which the solder can flow during soldering. The solder is usually added as a wire, as a solder preform, or in the form of a paste. This allows both similar and dissimilar material combinations to be joined. Soldering between an MI wire and a connecting part requires special surface preparation, e.g. using a flux, to enable wetting of the surfaces to be wetted with solder.Soldering is used for smaller dimensions of MI cables, especially with dissimilar base material combinations or as an alternative to laser welding of similar base material combinations and small dimensions. The soldering processes known from the prior art for creating a material-to-material connection between an MI cable and a connecting part have the following disadvantages:
[0013] Pore formation: State-of-the-art solder joints often have pores (internal) or pores open towards the surface, which then impair the strength of the joint or lead to leaks.
[0014] Many of the solder joints known from the state of the art are unsuitable for use in high-temperature applications, as the reflow temperature of the solder joint often corresponds to the liquidus temperature. In this case, at operating temperatures above the liquidus temperature, the connection between the liquid line and the connecting part can become leaky or even come loose.
[0015] Welding creates permanent, material-tight joints using heat (fusion welding) and / or pressure (pressure welding), with or without the addition of a filler metal. Fusion welding processes are typically used to join micro-leads to a connecting part, particularly arc welding (TIG welding, (micro)plasma welding) and beam welding (laser beam welding). In fusion welding processes, heat is applied from the outside until the base materials and, if applicable, the filler metal melt.
[0016] The welding filler material can facilitate welding or even make it possible in the first place. For similar base material combinations, welding does not necessarily require the use of a welding filler material, whereas for dissimilar base material combinations, a welding filler material is generally used. The selection of the welding filler material is then based on the more noble (higher-alloyed) base material of the two joining partners. The welding filler material for joining MI cables with a connecting part is usually fed into the arc or beam at the welding line in the form of a rod (e.g., manual TIG welding, manual (micro) plasma welding, manual laser beam welding) or a wire (mechanized and automated arc welding processes (e.g., TIG, MIG / MAG), laser beam processes, electron beam processes).The diameter of the welding rod or wire is selected in relation to the wall thicknesses to be welded (MI line and connecting piece) as well as the required weld seam thickness. For smaller wall thicknesses (and diameters), thinner welding consumables (<0.5 mm) must be used for process control and stability reasons. These are either available as special sizes or are not available on the market. The welding consumable can be added to the weld in powder form. It is completely melted, mixes with the two molten areas of the MI line and the connecting piece, and forms a weld pool, which, after solidification (falling below the solidus temperature), forms a weld seam. In the above-mentioned manual welding processes, the two joining partners are not moved (rotated) during welding. In the above-mentionedIn mechanized / automated welding processes, the two joining partners are rotated either mechanically or manually. These welding processes are generally used for medium and larger micro-leads (e.g., diameters >= 5.0 mm), as the welding process can be implemented more stably with these dimensions due to the controlled heat input. When welding micro-leads to a connecting part, in-process control of the heat input (the welding energy) is of utmost importance.
[0017] Fusion welding (arc welding, beam welding) of MI cables with a connecting part (with identical or dissimilar base material combinations, with or without filler metal, manually or automatically) often leads to weld seam irregularities. The weld seam quality can vary and, in extreme cases, even lead to the destruction of the MI cable's outer sheath during welding, burn-through and / or the formation of open pores extending all the way to the surface. The reasons for this are the different properties of MI cables, such as fluctuating outer sheath thicknesses along the entire MI cable length due to the manufacturing process and / or the aforementioned differences in heat capacities and thermal conductivity coefficients. In addition, the properties of the insulating material, such as grain size, density (degree of compaction), powder purity, (residual) water content, vary depending on the insulating material.Dimensions, type, and / or manufacturer of the MI cable. All of these parameters influence the stability of the welding process. Furthermore, MI cables often have to be heated in a furnace before welding to remove the residual water content from the insulating material or to reduce it sufficiently. When joining MI cables and connectors, close tolerance pairing of the two joining partners must therefore be ensured before welding, so that the gap between them is as small as possible to make the welding process more controllable, especially with regard to the locally introduced heat (heat conduction). The air in the gap acts as a thermal insulator. In addition, excessively large gaps can lead to cracks in the root area of the weld; these are unacceptable and should therefore be avoided in principle.When using welding consumables, care must be taken to ensure precise welding consumable feeding (position of the welding consumable relative to the weld line) in order to avoid possible (often unacceptable) irregularities in the weld joint (e.g. lack of fusion, burn-through through the MI conductor, root camber / under-camber in butt welds, excessive weld camber, etc.). In addition, the thickness (diameter) of the welding consumable must be matched to the dimensions of the relatively small MI conductors (small outer diameters, thin sheaths) and the connecting parts, as well as the required weld thickness. The dimensions of the available welding consumables (rods, wires, wire electrodes, etc.) are standardized (EN ISO 544); smaller diameters (<0.5 mm) are either not available at all or only available on request as custom-made products (typically in small quantities and therefore correspondingly more expensive).
[0018] The object of the invention is therefore to provide an improved joining method that eliminates the weaknesses of the aforementioned joining methods or at least significantly reduces them. The joining method should be independent of the geometric and physical properties of the Ml cable and the connecting part and be suitable for both arc welding and beam welding, and in particular for both dissimilar and similar base material combinations and all common weld seam types (fillet welds, butt welds, beaded welds, etc.).
[0019] The problem is solved by a method for producing a high-temperature-resistant material-to-material joint and a high-temperature-resistant assembly with a material-to-material joint between a conductor element and a connecting part.
[0020] With regard to the method, the object is achieved by a method for producing a high-temperature-resistant, in particular a temperature-resistant, material-locking joint between a conductor element and a connecting part, the method comprising the steps:
[0021] Providing the conductor element, the conductor element comprising:
[0022] - a tubular element with an outer casing, in particular a metallic one;
[0023] - at least one inner conductor arranged inside the tubular element, in particular at least two inner conductors;
[0024] - an insulating material arranged inside the tubular element, which serves to electrically insulate at least the tubular element from the at least one inner conductor;
[0025] Providing the connecting part, in particular at least partially metallic, wherein the connecting part has a, in particular cylindrical, guide for receiving the conductor element;
[0026] Providing an annular element; inserting the conductor element into the guide, wherein the conductor element inserted into the guide, the annular element and the connecting part are arranged relative to one another in such a way that the annular element both
[0027] - on a first joining surface of the outer shell, in particular an end face and / or on the shell surface of the outer shell, and
[0028] - rests against a second, in particular metallic, joining surface of the connecting part, in particular an end face or a, in particular at least partially cylindrical, lateral surface of the connecting part; and
[0029] Joining by means of a thermal joining process in which the ring-shaped element is completely melted and a material-locking joint is created between the conductor element and the connecting part, in particular in the form of a ring-shaped circumferential seam.
[0030] The joint produced by means of the method according to the invention serves in particular only for the mechanical connection between the conductor element and the connecting part, and typically not also for the production of an electrical connection between the inner conductors and the connecting element.
[0031] The connecting part is, for example, one of the following: a (threaded) connection, a bracket or fastening, a sleeve.
[0032] The metallic connecting part comprises in particular at least one of the following: a stainless steel, a nickel-based alloy, copper or a copper alloy.
[0033] The joining connection can be either of a different type or of the same type.
[0034] The advantage of the method according to the invention is that the controlled and complete melting of the annular element creates an intact and defect-free (annular) joint which at the same time has a high temperature resistance.
[0035] In one embodiment of the method, the joining process comprises soldering, wherein during the soldering the annular element serves as a solder preform, in particular a lead-free one, so that a solder connection is produced as the material-locking joining connection.
[0036] The solder preform is, for example, made of a composite material comprising a first composite component made of a solder alloy, in particular based on indium (In) or tin (Sn), which is arranged in a metallic matrix forming the second composite component. The second composite component is a metal with a high melting temperature, such as copper or silver or the metals mentioned in the scientific article cited below. The solder alloy is arranged in layers / levels in the metallic matrix. During the joining process, the solder preform is preferably oriented such that the layers or levels are arranged essentially parallel to the two joining surfaces of the two joining partners. The solder preform is characterized in that intermetallic phases are formed during soldering, which run along the layers of the solder alloy.Due to the layered structure of the solder preform, the intermetallic phases are distributed essentially evenly in a direction perpendicular to the joining surfaces, which means that the solder joints produced with it exhibit excellent mechanical strength and high temperature resistance. Such a solder preform is described in DE 10 2018 116 410 A1, DE 10 2019 122 611 A1, or the scientific article "Preform-based diffusion soldering for use under conventional soldering process parameters" by HM Daoud et al. (European Microelectronics and Packaging Conference (EMPC) & Exhibition, DOI 10.23919 / EMPC.2017.8346889) and is manufactured and marketed by Pfarr under the name PFDS400®. A solder joint made with the PFDS400® solder preform is high temperature resistant despite the low liquidus temperature of the solder preform of less than 250°C.A solder joint made with a PFDS400® solder preform (a tin-containing solder alloy) has a temperature resistance of at least 400°C, i.e., well above the aforementioned liquidus temperature. Such a solder preform is therefore preferably used in this embodiment to form the annular element.
[0037] In one embodiment of the method, the joining process comprises welding, wherein during the welding the annular element serves as a welding filler material, so that a welded joint is produced as the material-to-material joining connection.
[0038] In this embodiment, it is therefore preferable that no further welding filler material needs to be used, thus avoiding the disadvantages mentioned at the beginning.
[0039] Regardless of whether (soft-Z-hard) soldering or welding is used as the thermal joining process, the annular element produces a well-controllable and intact joint, especially in the form of a circular weld.
[0040] In one embodiment of the method, a single- or multi-core mineral-insulated conductor (MI conductor) is used as the conductor element.
[0041] In one embodiment of the method, the annular element, the first joining surface and the second joining surface are metallic, wherein the annular element is at least as highly alloyed or more highly alloyed as the more highly alloyed of the two joining surfaces, wherein the annular element consists in particular of a nickel-based alloy or a stainless steel. This embodiment is particularly preferred for the joining process comprising welding. In one embodiment of the method, the annular element comprises a base body, wherein the base body is designed as a rotational body in such a way that it can be rotated by an (imaginary) rotation, in particularwith an angle of less than or at most equal to 360°, is formed by an (imaginary) cross-sectional area (QF) around an (imaginary) axis of rotation (RA), wherein the axis of rotation (RA) lies in a plane with the cross-sectional area (QF) and does not intersect the cross-sectional area (QF), wherein a distance (AB) between the axis of rotation (RA) and a center point of the cross-sectional area is greater than a diameter (DM) of the cross-sectional area, and wherein in particular the cross-sectional area is round, elliptical, circular, angular, triangular or rectangular.
[0042] For example, in the case of a circular area as a cross-sectional area and a rotation with an angle of 360°, it is a full torus.
[0043] In one embodiment of the method, the diameter D of the cross-sectional area is at least 0.05 times, in particular 0.1 times, as large as a wall thickness of the outer shell and / or the diameter of the cross-sectional area is at most as large as a wall thickness of the outer shell and in particular less than 0.5 times the wall thickness and / or the distance is at least three times, in particular at least five times, as large as the diameter.
[0044] In one embodiment of the method, the conductor element and the annular element are arranged relative to one another before joining in such a way that the imaginary axis of rotation substantially coincides with a cylinder axis of the conductor element.
[0045] In one embodiment of the method, the annular element is manufactured in the form of a separate element before joining and then provided.
[0046] In one embodiment of the method, the annular element is placed, in particular pushed, onto the outer shell and / or a shell surface of the connecting part before joining.
[0047] In one embodiment of the method, the annular element has at least one, in particular exactly one, projection which extends from an inner surface of the annular element, in particular an inner surface facing the rotation axis, in the direction of the first joining surface and / or the second joining surface, and wherein the projection has a height in the direction of the first joining surface and / or second joining surface which is at most as large as 0.1 times the diameter, in particular 0.05 times the diameter.
[0048] In one embodiment of the method, the base body is designed as a rotational body, which is formed by a rotation through an angle of less than 360°, in particular greater than 315°, preferably greater than 350°, so that the base body has a gap. In one embodiment of the method, this comprises the following steps to be performed before joining:
[0049] Fixing the annular element at a predetermined joining position, in particular on the lateral surface of the outer shell and / or a lateral surface of the connecting part;
[0050] Tacking the annular element at the joining position, wherein during the tacking, the annular element is only melted in some areas and only partially bonded to the conductor element and / or the connecting part, in particular at least at the projection serving as the tacking point.
[0051] If necessary, the ring-shaped element is fixed using a tool before stapling.
[0052] In one embodiment of the method, the annular element sits in a press fit on the lateral surface of the outer shell and / or a lateral surface of the connecting part before joining.
[0053] In one embodiment of the method, the annular element is integrally bonded to the connecting part or the conductor element during the manufacturing process, so that, prior to joining, an assembly comprising the annular element and the connecting part or conductor element integrally bonded thereto is obtained. Unlike previously, the annular element and one of the two joining partners are no longer separate, but rather components of a common assembly that are already integrally bonded to one another. In this case, stapling, for example, can be omitted.
[0054] In a further development of the latter embodiment, the method comprises the following step to be carried out before joining:
[0055] - Providing the annular element by means of an additive manufacturing process, wherein the annular element is applied directly to the connecting part and / or the conductor element at a predetermined joining position by means of the additive manufacturing process during its manufacture, whereby the assembly comprising the annular element and the connecting part or conductor element integrally connected thereto is obtained before joining.
[0056] The additive manufacturing process (e.g., 3D printing), e.g., according to the DIN EN ISO / ASTM 52900:2022-03 standard, uses selective laser melting, electron beam melting, and / or selective laser sintering. If necessary, the connecting part and the annular element are also manufactured using a combined additive manufacturing process, especially using different starting materials for the annular element and the connecting part.
[0057] In a further development of the latter embodiment, the method comprises the following steps to be carried out before joining: - Providing a starting material for the annular element;
[0058] - Providing a starting material for the connecting part, in particular comprising a stainless steel;
[0059] - Initial welding of the starting material for the annular element with the starting material for the connecting part in a pressure welding process, in particular by means of diffusion welding, wherein the initial welding of the two starting materials forms an initial assembly, wherein the starting material for the annular element has a smaller thickness in a pressing direction, which pressing direction is perpendicular to a welding surface of the pressure welding process, than the thickness of the starting material for the connecting part in the pressing direction, and wherein in particular the thickness of the starting material for the annular element is at most 0.1, in particular at most 0.05, as large as the thickness of the starting material for the connecting part in the pressing direction; and
[0060] - Manufacturing the annular element and the connecting part integrally connected thereto from the initial assembly, in particular by means of a manufacturing process from the main group of separating and / or forming, in particular by means of machining, cutting, turning, drilling, whereby the assembly comprising the annular element and the connecting part integrally connected thereto is obtained from the initial assembly before joining.
[0061] In one embodiment of the method, the circumferential weld between the conductor element and the connecting part is formed as a fillet weld, butt weld or a bead-shaped weld.
[0062] In one embodiment of the method, this comprises the following step, which step is carried out after the conductor element has been inserted into the guide and before joining or before stapling and joining:
[0063] Clamping an arrangement consisting of a conductor element, connecting part and annular element in a clamping device,
[0064] Rotating the assembly in the case that the clamping device is a rotating device or rotating a power source used in welding and / or tacking around the assembly in the case that a movable power source is used during welding and / or tacking.
[0065] In one embodiment of the method, the tacking and / or welding is carried out in a fusion welding process, in particular an arc welding process, in particular using a non-consumable electrode, or in a beam welding process.
[0066] In one embodiment of the method, welding is free from the use of any further welding filler material other than the annular element.
[0067] In one embodiment of the method, the method comprises the following step: using an energy source during welding, wherein the energy source is directed onto an arrangement consisting of a conductor element, a connecting part and the annular element in such a way that energy emitted by the energy source in the direction of the arrangement is absorbed to a large extent, in particular to more than 85%, by the annular element.
[0068] The object is also achieved by a high-temperature-resistant assembly, in particular one that is temperature-resistant at temperatures of at least 380°C, preferably at least 700°C, comprising:
[0069] - a conductor element and a connecting part, wherein a high-temperature-resistant, material-locking joint exists between the conductor element and the connecting part, and wherein the high-temperature-resistant, material-locking joint is produced by means of the method according to the invention.
[0070] The invention is explained in more detail with reference to the following figures, which are not to scale. Like reference numerals denote like features. For reasons of clarity or where otherwise expedient, previously mentioned reference numerals have been omitted in the following figures.
[0071] They show:
[0072] Fig. 1 a) to 1 c) Different views of a conductor element 1 and a connecting part 2 connected thereto according to the prior art;
[0073] Fig. 2a) to 2c) show sectional views of a conductor element 1 and a connecting part 2, during the production of a joint connection 100 according to an embodiment of the method according to the invention;
[0074] Fig. 3a) and b) sectional views of a conductor element 1 and a connecting part 2, during the production of a joint connection 100 according to a further embodiment of the method according to the invention;
[0075] Fig. 4 A perspective view of the annular element 3 as used in an embodiment of the method according to the invention;
[0076] Fig. 5 sectional views of a conductor element 1 and a connecting part 2, during the production of a joint connection 100 according to a further embodiment of the method according to the invention; and
[0077] Fig. 6 A sectional view of a connecting part 2 and a ring-shaped element 3 integrally connected thereto in a further embodiment of the method according to the invention. Fig. 1 a) shows a side view of a typical embodiment of a conductor element 1 and a connected connecting part 2 according to the prior art. The conductor element 1 is inserted into a cylindrical guide 21 of the connecting part 2. The connecting part 2 is a metallic connection with a thread.
[0078] The conductor element 1 is an MI conductor, as shown in more detail in the sectional view in Fig. 1 b). It is a top view of a section of the conductor element 1 along the section line AA, cf. Fig. 1a. The MI conductor comprises the metallic outer sheath 4 and (here: four) inner conductors 5, which run parallel to the outer sheath 4. They are insulated from the outer sheath 4 by means of an insulating material 6 (a highly compressed metal oxide powder, e.g., MgO, Al2O3, SiO2). The conductor element 1 typically has an outer diameter D in the range of 0.5 - 10.0 mm. The wall thickness WM of the outer sheath 4 is typically 5-20%, e.g., 10% of the outer diameter D of the conductor element 1, whereby the wall thickness WM of the outer sheath 4 can vary over the length of the entire MI conductor as a result of the manufacturing and subsequent processes. Fig 1c) shows a detail in area B of Fig 1 a), namely the transition between the conductor element 1 and the connecting part 2.A lateral surface of the conductor element 1 borders on an end face of the connecting part 2 in the region of a joining connection to be produced.
[0079] The inventive method explained in more detail below enables the production of an improved joint in region B. This is illustrated in more detail for a first embodiment of the inventive method in Figs. 2a) to c). The region already shown in Fig. 1c) now contains the annular element 3, which is designed, for example, as a preformed solder or a welding filler material. The annular element 3 is pushed onto a lateral surface of the outer sheath 4 of the MI line up to a defined joining position.
[0080] A cross-section of the pushed-on annular element 3 along the line C—C is shown in Fig. 2b). At the joining position, the annular element 3 borders with its inner surface on the lateral surface of the outer shell 4. In this embodiment, the lateral surface thus forms a first joining surface 41.
[0081] Subsequently, the conductor element 1 with the annular element 3 pushed onto it (see Fig. 2a) is pushed into the guide 21 of the connecting part 2 until the connecting part 2 abuts the annular element 3 with an end face 22. The conductor element 1 is cylindrical, with a cylinder axis ZA of the conductor element 1 coinciding with a longitudinal axis of the guide 21 of the connecting part 2, which is particularly cylindrical in sections.
[0082] The end face 22 of the connecting part 2 serves as the second joining surface 22. With such an arrangement, a circumferential seam 7 is produced in the thermal joining process as a high-temperature-resistant, integral joint 100, which in this embodiment of the method according to the invention has the form of a fillet weld. By means of the high-temperature-resistant, integral joint 100, an assembly 110 consisting of the integrally connected conductor element 1 and the connecting part 2 is obtained. During the thermal joining process, the complete melting of the annular element 3 creates an intact and flawless, integral joint 100 that is resistant to high temperatures. Welding is preferably used as the thermal process, since welded joints generally exhibit good high-temperature strength.Of course, the invention also encompasses soldering processes, whereby in the latter case, appropriate selection of the solder preform must ensure that the resulting joint 100 is high-temperature resistant (this despite a possibly low liquidus temperature of the solder preform; see the composite material solder preform PFDS400® mentioned above in this context). For the sake of simplicity, the method according to the invention will be explained in more detail below in connection with welding processes, whereby the invention naturally also encompasses soldering processes mutatis mutandis.
[0083] For welding, the assembly comprising conductor element 1, annular element s, and connecting part is clamped in a clamping device 11 (not shown here - see Fig. 5), e.g., a rotating device of a welding device, e.g., on the connecting part 2 or the conductor element 1, depending on the joining position. Clamping is achieved, for example, using a three-jaw chuck, collet system, or in another way. The other side of the assembly is supported on the conductor element 1 by means of a support (loosely mounted tailstock, a steady rest, or a similar support system). For shorter lengths of the conductor element 1, work can be carried out without support.
[0084] Welding is performed either with an arc welding process using a non-consumable electrode (e.g., TIG welding, (micro) plasma welding) or with a beam welding process (e.g., laser beam welding), in each case without the use of a conventional welding consumable (i.e., welding consumable in the form of wire or rod) in addition to the annular element 3. The annular element 3 already functions as a welding consumable, so that preferably no additional welding consumable is required.
[0085] An energy source (arc, beam, ionized gas, the latter in the case of plasma welding) is directed at the annular element 3 in such a way that the primary energy absorption occurs by the annular element 3. Furthermore, in arc welding or beam welding processes, the welding position (angular position) and the size of the arc (over the distance and in combination with the electrode diameter) or the beam (focus diameter) are selected so that complete melting of the annular element 3 and the weld seam flanks can occur. In arc welding processes with non-consumable electrodes, the process can be either mechanized / automatic or manual. In beam welding processes, the process is usually mechanized / automatic. Both welding processes can be carried out in pulsed mode or in continuous mode. During welding, the arc or beam can beBeam energy can be modulated.
[0086] The invention further encompasses welding by means of TIG orbital welding, an arc welding process with a non-consumable electrode, in which the assembly to be welded is not moved, but rather the arc (welding torch) moves around the - preferably rotationally symmetrical - assembly. TIG orbital welding has the advantage that, in the case of long MI conductors, they do not have to be unwound from a spool (also: coil, the usual delivery form of MI conductors) and / or completely straightened. This is because simple rotation of the MI conductor is not necessary during TIG orbital welding. The conductor element 1 only needs to be straightened up to a joining position adjacent to the connecting part 2. Furthermore, in TIG orbital welding, the joining process is largely automated, so that this welding process is preferably used in the method according to the invention.
[0087] The assembly prepared for welding (conductor element 1, connecting part 2, annular element 3) is aligned, secured, and closed in a fixed clamping device 11 (not shown here - see Fig. 5) of a TIG orbital welding device (also called a cassette). The welding head of the TIG orbital welding system is inserted into the cassette perpendicular to the welding point. Depending on the design of the welding system, the non-consumable electrode during TIG orbital welding can be positioned perpendicularly or at an angle to the assembly to be joined.
[0088] Fig. 3 a) and b) show a further example of welding between an MI line and a connecting part 2 by means of an annular element 3, in which a joint 100 is produced as a circular seam 7. Unlike in Fig. 2, the annular element 3 is not pushed over the conductor element 1 as previously shown in Fig. 2a) and b). Instead, an end section of the conductor element 1 to be welded, in particular the MI line, is machined flat and the inner conductors 6 are released for other manufacturing steps. The annular element 3 is placed coaxially between the connecting part 2 and the conductor element 1 and clamped in a clamping device 11 (not shown here - see Fig. 5) as described above in connection with Fig. 2.
[0089] The two joining partners 1, 2 are pressed against each other so that the annular element 3 is held in place during welding. The annular element 3 is completely melted during welding and forms a weld pool with the material melted from the two joining partners 1, 2. After the weld pool has solidified, it forms an intact butt weld 7 as a joint 100. If necessary, a shielding gas (supplied from the outside) and / or a forming gas (supplied from the inside of the connecting part 2) is also supplied during welding. The welds shown are single-layer welds. The same welding processes are used as for the fillet weld joints mentioned above (see above in connection with Fig. 2).
[0090] Of course, the invention also encompasses arrangements in which the annular element 3, like a sandwich, encloses both a portion of the connecting part 2 and the conductor element 1 (not shown). In this case, an inner surface of the annular element 3 borders both a lateral surface of the outer shell 4 (the lateral surface is the first joining surface 41) and a lateral surface of the connecting part 2 as the second joining surface 22, so that the circumferential seam 7 is bead-shaped in this case.
[0091] Depending on the type of joint 100, a specific shape of the annular element 3 can be selected. In the embodiments shown in Fig. 2a) and Fig. 3a), the annular element 3 has the shape of a rotational body with a rectangular cross-sectional area QF; further shapes are discussed below in connection with Fig. 4.
[0092] Fig. 4 shows a perspective view of an annular element 3 as used in the method according to the invention. The annular element comprises a base body which is designed as a rotational body. The rotational body is formed by an (imaginary) rotation of a cross-sectional area QF about an (imaginary) axis of rotation RA, wherein the axis of rotation RA lies in a plane with the cross-sectional area (QF) but does not intersect it. A distance AB between the axis of rotation RA and a center point of the cross-sectional area QF is greater than a diameter DM of the cross-sectional area. In the embodiment shown here, the cross-sectional area is round, so that the base body essentially has the shape of a solid torus. The annular element 3 shown in Fig. 2a) and Fig. 3a), on the other hand, has a rectangular cross-sectional area QF of the base body.The cross-sectional area QF can of course also have shapes other than those shown here and can be, for example, elliptical, square, or triangular (not shown).
[0093] In the case of a non-circular cross-sectional area QF, the person skilled in the art will use alternative definitions for the diameter DM and / or center point. For example, the center point of a non-circular area corresponds to a geometric center of gravity. For example, the diameter DM of a non-circular area corresponds to a (maximum or minimum) diameter, in particular in the direction of the distance AB between the axis of rotation RA and the cross-sectional area QF, or to a diameter of a circular area corresponding to the cross-sectional area QF, which circular area has the same area as the cross-sectional area. The main dimensions of the annular element 3, such as a diameter DM of a cross-sectional area QF, for example a width and / or height h for the rectangular cross-sectional area QF shown in Fig. 2, an inner diameter and / or outer diameter, as well as other dimensions of the annular element 3 (Fig.4) are designed depending on the material thicknesses to be welded, ie the diameter of the conductor element 1, the connecting part 2, as well as the required thickness of the joint 100 formed as a circular seam 7.
[0094] For example: the diameter DM of the cross-sectional area QF is at least 0.05 times, in particular 0.1 times as large as a wall thickness WM of the outer shell 4 and / or the diameter DM of the cross-sectional area QF is at most as large as a wall thickness WM of the outer shell 4 and in particular less than 0.5 times the wall thickness WM and / or the distance AB is at least three times, in particular at least five times as large as the diameter DM.
[0095] Depending on the diameter of the outer sheath 4 (in the range 0.5 mm to 10.0 mm), the wall thickness WM of the outer sheath 4 is typically in the range 0.05 mm to 1 mm, which results in corresponding restrictions for the dimensions of the annular element 3. For a 3 mm Ml cable, for example, the cross-sectional area QF of the annular element 3 has a diameter of 0.3 mm.
[0096] In the case of a welded joint, the selection of the material for the annular element 3 depends on the base materials of the two joining partners 1, 2. The annular element 3 is at least as highly alloyed or more highly alloyed as the higher-alloyed of the two joining surfaces 41, 22. For example, the annular element 3 consists of a nickel-based alloy, or, if the highest-alloyed of the two joining partners is a stainless steel, of a stainless steel.
[0097] The annular element 3 is manufactured from a strip or sheet metal using a suitable cutting process, depending on its shape, but preferably using laser cutting. Other cutting processes are also possible, including punching, waterjet cutting, etc. The annular element 3 can be manufactured from a tube or rod by machining. For round cross-sectional areas QF, an annular element 3 can be manufactured from a wire joined at both ends by welding. The annular element 3 can also be manufactured using suitable additive manufacturing processes, e.g., according to EN ISO 52900; see also Fig. 6.
[0098] Depending on the shape of the cross-sectional area QF for constructing the base body of the annular element 3, materials that function as welding consumables standardized in welding technology are preferred as the starting material for the annular element 3. These include, for example, solid strip electrodes for submerged arc welding or electroslag welding, solid wires, and solid wire electrodes. For shapes of the cross-sectional area QF that cannot be manufactured from the aforementioned materials, semi-finished products such as tubes, round bars, hexagonal bars, etc. are used. The annular element 3 preferably has good flatness, e.g., an average roughness Rt of at most 16 pm (micrometers) and / or an average roughness Ra of at most 3.5 pm (micrometers). This is to ensure that it lies as flush as possible on the second joining surface 22 (fillet weld as circular weld 7, Fig. 2c) - or on both joining surfaces 22, 41 (butt weld as circular weld, Fig. 3b).In the case of a square cross-sectional area QF, it is also advantageous if the cross-sectional area QF is as close as possible to a rectangular shape, so that, for example, the end faces of the annular element 3 facing the connecting part 2 and the conductor element 1 are more or less parallel to one another. Parallel-similar means, for example, that the end faces are designed such that they deviate from a parallel shape by less than 30% of the diameter DM of the annular element 3, especially in the direction of the rotation axis RA.
[0099] It is advantageous if the arrangement consisting of conductor element 1, connecting part 2 and annular element 3 is fixed before welding, for example in order to facilitate processing in a clamping device 11 (see Fig. 5). The clamping device is, for example, a rotating device or a stationary cassette; the latter in the case of a TIG circular welding system in the aforementioned TIG orbital welding. For this purpose, for example, the annular element 3 sits in a press fit on the conductor element 1 and / or the connecting part 2. This can be achieved, for example, by choosing a sufficiently small distance AB (or inner diameter of the base body) of the annular element 3 and / or providing a gap 9 in the base body (rotation less than 360°, see Fig. 4). The gap 9 and / or the sufficiently small inner diameter (e.g.A maximum of 5% smaller than the outer diameter of the conductor element 1) enables the annular element 3 to be slid onto, for example, the conductor element 1 in a press fit (e.g., by making the inner diameter of the base body smaller, in particular a maximum of 5% smaller, than the outer diameter of the conductor element 1). In this way, the annular element 3 forms a press and / or transition fit with the conductor element 1.
[0100] If necessary, the method also includes the following steps, which must be carried out before joining: fixing the annular element 3 at a predetermined joining position, in particular on the lateral surface of the outer sheath 4 and / or a lateral surface of the connecting part 2; stapling the annular element 3 at the joining position, wherein during the stapling, the annular element 3 is melted only in certain regions and is only partially bonded to the conductor element 1 and / or the connecting part 2.
[0101] The stapling serves to temporarily connect the annular element 3 to the connecting part 2 and / or the conductor element 1. An assembly prepared for stapling comprises the conductor element 1, the connecting part 2, the annular element 3 and a tool 12, this is shown in more detail in Fig. 5. The arrangement shown in Fig. 5 otherwise corresponds to the arrangement already shown in Fig. 2a), in which the annular element 3 is pushed onto a selected point on the conductor element 1. To determine the joining position, an additional tool 12 is used as a stop. The tool 12 is also pushed onto the conductor element 1 and fixed there, e.g. by means of a screw and / or clamp. The tool 12 has the function of defining the position of the annular element 3 before stapling. In addition, the tool 12 ensures a planar, in particular gap-free, contact of the annular element 3 on the joining surfaces 22,41, e.g.on the end face 22 of the connecting part 2, see Fig. 2a).
[0102] The tool 12 has recesses 12a at its tip to enable tacking and to prevent possible sticking of the tool 12 to the annular element 3. Before welding, the assembly comprising conductor element 1, annular element 3, connecting part 2, including the tool 12, is clamped in a clamping device 11, as explained above in connection with welding. This creates a tack point (or tack weld) 15, which is later integrated into the weld (i.e., completely melted). Tack welding is carried out using either an arc or beam welding process, in each case without filler metal. If more than one tack point (tack weld) is planned, the assembly is moved (rotated) between the individual tack positions, either mechanically or manually on the side of the rotating device, or the non-consumable electrode is moved to the next tack position, in the case of TIG orbital welding.After tack welding, the clamping device 11 is opened, and the tool clamped on the conductor element 1 is released and removed. The thus-fixed assembly (conductor element 1 - connecting part 2 - annular element 3) remains in the clamping device 11 of the welding device. The tacked assembly is realigned in the clamping device 11, and the clamping device 11 is closed again to allow the loose support and coaxial positioning of the tacked assembly during subsequent welding (as explained above in connection with Fig. 2).
[0103] For stapling, several projections or exactly one projection 8, which are arranged on an inner surface of the annular element 3 facing the joining surface(s) 22,41, cf. Fig. 4, serve as stapling point.
[0104] In previous embodiments, the annular element 3 was always provided as a separately manufactured element. An alternative variant of the invention is shown in Fig. 6. In this, the annular element 3 is materially bonded directly to the connecting part 2 during its manufacture. Thus, before joining, in particular welding, an assembly 10a; 10b comprising the annular element 3 and the connecting part 2 materially bonded thereto is obtained. In a first embodiment of the latter variant, an assembly 10a is obtained by means of suitable additive manufacturing processes (also: 3D printing), e.g. according to EN ISO 52900. During its manufacture, the annular element 3 is applied (or printed) directly to the connecting part 2 using the additive manufacturing process and is materially bonded directly to the connecting part 2 during its manufacture.a process is used which applies a starting material for the annular element 3 using directed energy input. The starting material is combined in several layers on the end face of the connecting part 2, which serves as the second joining surface 22. Processes with concentrated thermal energy are used to bond the starting material directly to the connecting part 2 at the application site. Laser beam, electron beam, arc, plasma, or friction are used as the energy source, using additional materials such as metals in powder, wire, or rod form. In addition, processes which work with powder bed-based melting according to EN ISO 52900 can be used to apply the annular element 3 to the connecting part 2. For example,One of the following additive manufacturing processes is used: selective laser melting, electron beam melting, or selective laser sintering. If necessary, the connecting part 2 and the annular element 3 are also manufactured using a common additive manufacturing process, e.g., using different materials.
[0105] In a second embodiment of the latter variant, an assembly 10b is produced by welding starting materials for the connecting part 2, in particular comprising a stainless steel, and the annular element s together in a starting welding process. This is done using a pressure welding process, in particular by means of diffusion welding, so that a starting assembly is formed. Here, the starting material for the annular element 3 is thin in a pressing direction, which is perpendicular to a welding surface of the pressure welding process, compared to the starting material for the connecting part 2.
[0106] Subsequently, a manufacturing process from the main group of separating and / or forming, in particular machining, cutting, turning, and drilling, is used, for example, in combination with thermal separation processes such as plasma fusion cutting, laser cutting, and / or with other suitable forming separation processes, such as wire EDM (cutting EDM), to form the assembly 10b from the initial assembly. In this way, the annular element 3 and the connecting part 2 are already firmly bonded to one another before the connecting part 2 and the conductor element 1 are joined. Reference numerals and symbols
[0107] 1 ladder element
[0108] 2 connecting part
[0109] 100 joints
[0110] 110 assembly
[0111] 21 Guide
[0112] 22 second joining surface
[0113] 3 ring-shaped element
[0114] 4 Outer jacket
[0115] 41 first joining surface
[0116] 5 inner conductors
[0117] 6 Insulating material
[0118] 7 Circumferential seam
[0119] 8 lead
[0120] 9 gap
[0121] 10a, 10b assembly
[0122] 11 Clamping device
[0123] 12 tools
[0124] 15 tack points
[0125] D outer diameter of 4
[0126] WM wall thickness of 4
[0127] QF cross-sectional area of 3
[0128] DM diameter of the QF
[0129] RA rotation axis
[0130] ZA cylinder axis
[0131] AB distance
Claims
Patent claims 1. A method for producing a high-temperature-resistant, in particular a temperature-resistant, material-locking joint (100) between a conductor element (1) and a connecting part (2), the method comprising the steps: Providing the conductor element (1), the conductor element (1) comprising: - a tubular element with an outer casing (4), in particular a metallic one; - at least one inner conductor (5) arranged inside the tubular element, in particular at least two inner conductors (5); - an insulating material (6) arranged inside the tubular element, which serves to electrically insulate at least the tubular element from the at least one inner conductor (5); Providing the connecting part (2), in particular a metallic one at least in some areas, wherein the connecting part (2) has a guide (21), in particular a cylindrical guide, for receiving the conductor element (1); Providing an annular element (3); Inserting the conductor element (1) into the guide (21), wherein the conductor element (1) inserted into the guide (21), the annular element (3) and the connecting part (2) are arranged relative to one another in such a way that the annular element (3) both - on a first joining surface (41) of the outer shell (4), in particular an end face and / or on the shell surface of the outer shell (4), and - rests against a second, in particular metallic, joining surface (22) of the connecting part (2), in particular an end face or a, in particular at least partially cylindrical, lateral surface of the connecting part (2); Joining by means of a thermal joining process, in which the annular element (3) is completely melted and a material-locking joint (100) is produced between the conductor element (1) and the connecting part (2), in particular in the form of an annular circumferential seam (7).
2. Method according to at least one of the preceding claims, wherein the joining process comprises soldering and during the soldering the annular element (3) serves as a, in particular lead-free, solder preform, so that a solder connection is produced as the cohesive joining connection (100).
3. Method according to at least one of the preceding claims, wherein the joining process comprises welding and during the welding the annular element (3) serves as a welding filler material, so that a welded connection is produced as the material-to-material joining connection (100).
4. Method according to at least one of the preceding claims, wherein a single- or multi-core mineral-insulated conductor (MIL) is used as the conductor element (1).
5. Method according to at least one of the preceding claims, wherein the annular element (3), the first joining surface (41) and the second joining surface (22) are metallic, and wherein the annular element (3) is at least as highly alloyed or more highly alloyed as the more highly alloyed of the two joining surfaces (41, 22), wherein the annular element (3) consists in particular of a nickel-based alloy or a stainless steel.
6. Method according to at least one of the preceding claims, wherein the annular element (3) comprises a base body, wherein the base body is designed as a rotational body such that it is formed by an (imaginary) rotation of an (imaginary) cross-sectional area (QF) about an (imaginary) axis of rotation (RA), wherein the axis of rotation (RA) lies in a plane with the cross-sectional area (QF) and does not intersect the cross-sectional area (QF), wherein a distance (AB) between the axis of rotation (RA) and a center point of the cross-sectional area (QF) is greater than a diameter (DM) of the cross-sectional area, and wherein in particular the cross-sectional area (QF) is round, elliptical, circular, angular, triangular or rectangular.
7. The method according to claim 6, wherein the diameter (DM) of the cross-sectional area (QF) is at least 0.05 times, in particular 0.1 times, as large as a wall thickness (WM) of the outer shell (4) and / or wherein the diameter (DM) of the cross-sectional area (QF) is at most as large as a wall thickness (WM) of the outer shell (4) and in particular less than 0.5 times the wall thickness (WM) and / or where the distance (AB) is at least three times, in particular at least five times as large as the diameter (DM).
8. Method according to claim 6 or 7, wherein the conductor element (1) and the annular element (3) are arranged relative to one another before joining in such a way that the imaginary axis of rotation substantially coincides with a cylinder axis (ZA) of the conductor element (1).
9. Method according to at least one of the preceding claims, wherein the annular element (3) is manufactured in the form of a separate element before joining and is subsequently provided.
10. Method according to at least one of the preceding claims, wherein the annular element (3) is placed, in particular pushed, onto the lateral surface of the outer shell (4) and / or the lateral surface of the connecting part (2) before joining.
11. Method according to at least one of the preceding claims, wherein the annular element (3) has at least one, in particular exactly one, projection (8) which extends from an inner surface, in particular an inner surface facing the rotation axis (RA), of the annular element (3) in the direction of the first joining surface (41) and / or the second joining surface (22), and wherein the projection (8) has a height in the direction of the first joining surface (41) and / or second joining surface (22) which is at most as great as 0.1 times the diameter (DM), in particular 0.05 times the diameter (DM).
12. Method according to at least one of the preceding claims 6 to 11, wherein the base body is designed as a rotational body, which rotational body is formed by a rotation through an angle of less than 360°, in particular greater than 315°, preferably greater than 350°, so that the base body has a gap (9).
13. Method according to at least one of the preceding claims, comprising the following steps to be carried out before joining: Fixing the annular element (3) at a predetermined joining position, in particular on the lateral surface of the outer shell (4) and / or a lateral surface of the connecting part (2); Stitching the annular element (3) at the joining position, wherein during the stitching, the annular element (3) is melted only in some areas and is only partially bonded to the conductor element (1) and / or the connecting part (2), in particular at the at least one projection (8) serving as a stitching point.
14. Method according to at least one of the preceding claims, wherein the annular element (3) sits in a press fit on the lateral surface of the outer shell and / or a lateral surface of the connecting part (2) before joining.
15. Method according to at least one of the preceding claims 1 to 8, wherein the annular element (3) is materially connected to the connecting part (2) or the conductor element (1) during the production of the annular element (3), so that an assembly (10a; 10b) comprising the annular element (3) and the connecting part (2) or conductor element (1) materially connected thereto is obtained before the joining.
16. A method according to claim 15, comprising the following step to be carried out before joining: - Providing the annular element (3) by means of an additive manufacturing process, wherein the annular element (3) is applied directly to the connecting part (2) and / or the conductor element (1) at a predetermined joining position by means of the additive manufacturing process during its manufacture, whereby the assembly (10a) comprising the annular element (3) and the connecting part (2) or conductor element (1) integrally connected thereto is obtained before joining.
17. A method according to claim 15, comprising the following steps to be carried out before joining: - providing a starting material for the annular element (3); - Providing a starting material for the connecting part (2), in particular comprising a stainless steel; - Initial welding of the starting material for the annular element (3) with the starting material for the connecting part (2) in a pressure welding process, in particular by means of diffusion welding, wherein during the initial welding of the two starting materials an initial assembly is formed, wherein the starting material for the annular element (3) has a smaller thickness in a pressing direction (PR), which pressing direction is perpendicular to a welding surface of the pressure welding process, than the thickness of the starting material for the connecting part (2) in the pressing direction, and wherein in particular the thickness of the starting material for the annular element is at most 0.1, in particular at most 0.05 times, as large as the thickness of the starting material for the connecting part (2) in the pressing direction; - Manufacturing the annular element (3) and the connecting part (2) integrally connected thereto from the initial assembly, in particular by means of a manufacturing process from the main group of separating and / or forming, in particular by means of machining, cutting, turning, drilling, whereby the assembly (10b) comprising the annular element and the connecting part (2) integrally connected thereto is obtained from the initial assembly before joining.
18. Method according to at least one of the preceding claims, wherein the circumferential seam (7) between the conductor element (1) and the connecting part (2) is formed as a fillet weld, butt weld or a bead-shaped seam.
19. Method according to at least one of the preceding claims, comprising the following step, which step is carried out after the insertion of the conductor element (1) into the guide (21) and before joining or before stapling and joining: Clamping an arrangement consisting of conductor element (1), connecting part (2) and ring-shaped element (3) in a clamping device (11), Rotating the arrangement, in the event that the clamping device (11) is a rotating device or Rotating a power source used in welding and / or tacking around the assembly, in the case where a movable power source is used, during welding and / or tacking.
20. Method according to at least one of the preceding claims, wherein the tacking and / or welding is carried out in a fusion welding process, in particular an arc welding process, in particular using a non-consumable electrode, or in a beam welding process.
21. Method according to at least one of the preceding claims, wherein the welding is free from the use of a further welding filler material different from the annular element (3).
22. Method according to at least one of the preceding claims 3 to 21, comprising the following step: Using an energy source during welding, wherein the energy source is directed onto an arrangement consisting of a conductor element (1), a connecting part (2) and the annular element (3) in such a way that energy emitted by the energy source in the direction of the arrangement is absorbed to a large extent, in particular to more than 85%, by the annular element (3).
23. High-temperature-resistant, in particular a temperature-resistant assembly (110) at temperatures of at least 380°C, preferably at least 700°C, comprising: - a conductor element (1) and a connecting part (2), wherein a high-temperature-resistant, material-locking joint (100) is present between the conductor element (1) and the connecting part (2), and wherein the high-temperature-resistant, material-locking joint (100) is produced by a method according to at least one of claims 1 to 22.
Citation Information
Patent Citations
Method for producing a high-temperature resistant lead-free solder joint and high-temperature resistant lead-free solder joint
DE102018116410A1
SMD solderable component and method for manufacturing an SMD solderable component
DE102019122611A1
Manufacturing method for a connection between a coaxial cable and a coaxial connector and a coaxial cable with a terminating coaxial connector thereof
EP2219267B1
Coupling sleeve for a mineral-insulated cable and connection method