Polymeric material suitable for recycling

The use of polymers with a specific sulphide moiety structure enables efficient recycling of thermoset materials by allowing reversible cycloreversion and repolymerization, addressing the challenges of incomplete debonding and material stability in existing photo-reversible systems.

WO2024218505A1PCT designated stage expired Publication Date: 2024-10-24UNIVERSITY OF WARWICK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/GB2024/051021
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current methods for recycling thermoset materials are hindered by their irreversible covalent 3D crosslinked networks, which prevent flow and subsequent recycling upon heating, and existing photo-reversible systems often suffer from incomplete debonding due to competing light absorption and radical side reactions.

Method used

A method involving polymers with a specific sulphide moiety structure that undergoes [2+2] cycloreversion upon heating, allowing for the generation of oligomers or monomers that can be repolymerized, enabling reversible debonding, rebonding, and recycling without significant side reactions.

Benefits of technology

This approach allows for near-quantitative cycloreversion and repolymerization, facilitating the recycling of thermoset materials with high efficiency and minimal material loss, overcoming the limitations of existing photo-reversible systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GB2024051021_24102024_PF_FP_ABST
    Figure GB2024051021_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A cycloreversion process comprising photo-dimerisation of compounds comprising monothiomaleimide moieties and the thermal reversion to the monomer form. Such moieties can be used as crosslinkers in common plastics materials, thus facilitating recycling and reuse.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] POLYMERIC MATERIAL SUITABLE FOR RECYCLING

[0002] This invention relates generally to dimeric and polymeric materials suitable for recycling. More specifically, although not exclusively, the invention relates to dimeric and polymeric materials fabricated from maleimides containing sulphide moieties, and methods suitable for bonding, debonding, re-bonding, reshaping, (re)processing, and recycling the same.

[0003] The sustainability of polymer materials is a global concern. According to Statista, the annual plastic generation per capita in the UK alone is 98.66 kg, and the recycling rate of UK plastic packing waste is just 44.2%. The remaining plastic waste is either incinerated or goes to landfill sites, which causes pollution to the environment. Consequently, there is a need to improve the sustainability of polymeric materials.

[0004] Much research attention has been focused on improving the sustainability of thermoplastics, e.g. PET (polyethylene terephthalate) bottles. This type of polymer comprises physically entangled chains that can melt and be reshaped reversibly at elevated temperatures. However, less research attention has been focused on improving the sustainability of thermoset materials.

[0005] Thermoset materials (e.g. epoxy resins, polyurethanes) provide outstanding durability and thermomechanical robustness, often in combination with low-cost, high-throughput and freedom of design production. However, this type of polymer comprises an irreversible covalent 3D crosslinked network, which prevents flow and subsequent recycling upon heating. This makes it extremely challenging to recycle thermoset materials.

[0006] One proposed solution to the recycling of thermoset materials is the use of dynamic covalent polymer networks. In this type of polymer, the permanent connections within the polymer network of traditional thermosets are replaced with reversible covalent bonds A + B C, which may be debonded upon application of a stimulus. Therefore, the material possesses thermoset properties during use whilst being able to be “healed”, reshaped, or reprocessed in a similar manner to thermoplastics.

[0007] The use of photo-reversible chemistries is an attractive method for reprocessing thermosettype polymers. However, a drawback of some reported systems is that the photo-reversion reaction may be incomplete. For example, most photodynamic systems rely on homolytic chain cleavage (e.g. disulfides) that often inflict other (irreversible) radical side reactions. Alternatively, light-gated dynamic covalent bonding / debonding has been achieved through photo-reversible [2+2] and [4+4] dimerization, for instance of coumarins (Polym. Chern., 2017, 8, 2499-2508) and anthracenes (Macromolecules 2017, 50, 5, 1930-1938). However, these systems typically suffer from incomplete photo-cycloreversion because conjugated scission products of these compounds compete for light absorbance, making photo-reversion incomplete. This incomplete debonding process can be compensated for at low concentrations, but sets practical limitations for thermoset material recycling. Moreover, degradation products are typically formed under the applied harsh UV-conditions (i.e. A < 260 nm). Interestingly, anthracene dimers are known to revert thermally. In contrast to photo-scission, this thermal reversion could provide quantitative debonding although irreversible material damage is often caused by the need of extensive heating (typically > 160 °C).

[0008] It is therefore a first non-exclusive object of the invention to provide new molecules and materials, e.g. polymers, suitable for reprocessing and recycling, which lack the aforementioned issues.

[0009] Accordingly, a first aspect of the invention provides a method for recycling a compound, e.g. a polymer, the method comprising providing a compound, e.g. polymer, the compound, e.g. polymer, comprising a moiety having the general structure (1a) and / or (1 b) or a stereoisomer, enantiomer, racemate, or tautomer thereof:

[0010] (1a)

[0011] (1 b) wherein R1and R2are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1and / or R2is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl; the method comprising heating the compound, e.g. polymer, to a temperature at or above 35°C, e.g. at or above a temperature of 40°C, or at or above a temperature of 45°C, or at or above a temperature of 50°C, or at or above a temperature of 55°C, or at or above a temperature of 60°C, or at or above a temperature of 65°C, or at or above a temperature of 70°C, or at or above a temperature of 75°C, or at or above a temperature of 80°C, or at or above a temperature of 85°C, or at or above a temperature of 90°C, or at or above a temperature of 95°C, or at or above a temperature of 100°C, to generate oligomers or monomers comprising moieties having the general structures (2a) and (2b):

[0012] (2a)

[0013] (2b) wherein R1and R2are defined as above; and at least 50%, e.g. at least 60%, or at least 70%, or at least 80%, or at least 90% of the moieties defined in general structure (1a) and (1b) are converted into the moieties defined in general structure (2a) and (2b).

[0014] The term Cm-n refers to a group with m to n carbon atoms, with m and n being integers and m < n. The term “C1.20 alkyl” refers to a linear or branched hydrocarbon chain containing 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 , 12, 13, 14, 15, 16, 17, 18, 19, or 20 carbon atoms, for example methyl, ethyl, n-propyl, / so-propyl, n-butyl, / so-butyl, sec-butyl, terf-butyl, n-pentyl and n-hexyl, n- heptyl, n-octyl, n-decyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n- pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl, or n-eicosyl, and so on.

[0015] The term “C2-20 alkylene” refers to a divalent alkyl group, which is a linear or branched hydrocarbon chain containing 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 , 12, 13, 14, 15, 16, 17, 18, 19, or 20 carbon atoms. Alkylene groups are divalent alkyl groups and may likewise be linear or branched and have two points of attachment to the remainder of the molecule. Furthermore, an alkylene group may, for example, correspond to one of those alkyl groups listed in this paragraph. For example, C1.6 alkylene may be -CH2-, -CH2CH2-,-CH2CH(CHs)-, - CH2CH2CH2- or -CH2CH(CHS)CH2-. The alkyl and alkylene groups may be unsubstituted or substituted by one or more substituents. Possible substituents are described herein. For example, substituents for an alkyl or alkylene group may be halogen, e.g. fluorine, chlorine, bromine and iodine, OH, C1-C4 alkoxy, -NR’R” amino, wherein R’ and R” are independently H or alkyl, e.g. C1.6 alkyl. Substituents may also be ring systems such as an aromatic ring (e.g. a five or six membered aromatic ring), a saturated ring system (e.g. a five or six membered saturated ring system), a bridged ring system, a spiro bicyclic ring system, or a heterocyclic ring system, or a fused ring system. The ring system may itself be substituted or unsubstituted. Other substituents for the alkyl group may alternatively be used.

[0016] The term “C2-20 alkenyl” refers to a linear or branched hydrocarbon chain containing at least one double bond and having 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 , 12, 13, 14, 15, 16, 17, 18, 19, or 20 carbon atoms. The double bond(s) may be present as the E or Z isomer. The double bond may be at any possible position of the hydrocarbon chain. For example, a “C2-6 alkenyl” may be ethenyl, propenyl, butenyl, butadienyl, pentenyl, pentadienyl, hexenyl and hexadienyl. Alkenylene groups are divalent alkenyl groups and may likewise be linear or branched and have two points of attachment to the remainder of the molecule. Furthermore, an alkenylene group may, for example, correspond to one of those alkenyl groups listed in this paragraph. For example alkenylene may be -CH=CH-, -CH2CH=CH-, - CH(CHs)CH=CH- or -CH2CH=CH-. Alkenyl and alkenylene groups may unsubstituted or substituted by one or more substituents. Possible substituents are described herein. For example, substituents may be those described above as substituents for alkyl groups. The term “C1.20 haloalkyl”, e.g. “C1.4 haloalkyl”, refers to a hydrocarbon chain substituted with at least one halogen atom independently chosen at each occurrence, for example fluorine, chlorine, bromine and iodine. The halogen atom may be present at any position on the hydrocarbon chain. For example, C1.6 haloalkyl may refer to chloromethyl, fluoromethyl, trifluoromethyl, chloroethyl e.g. 1 -chloromethyl and 2-chloroethyl, trichloroethyl e.g. 1 ,2,2- trichloroethyl, 2,2,2-trichloroethyl, fluoroethyl e.g. 1 -fluoromethyl and 2-fluoroethyl, trifluoroethyl e.g. 1 ,2,2-trifluoroethyl and 2,2,2-trifluoroethyl, chloropropyl, trichloropropyl, fluoropropyl, trifluoropropyl. A haloalkyl group may be, for example, -CX3, -CHX2, -CH2CX3,-CH2CHX2or -CX(CH3)CH3wherein X is a halo (e.g. F, Cl, Br or I). A fluoroalkyl group, i.e. a hydrocarbon chain substituted with at least one fluorine atom (e.g. -CF3, -CHF2, -CH2CF3or -CH2CHF2).

[0017] The term “C2.2o alkynyl” includes a branched or linear hydrocarbon chain containing at least one triple bond and having 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 , 12, 13, 14, 15, 16, 17, 18, 19, or 20 carbon atoms. The triple bond may be at any possible position of the hydrocarbon chain. For example, the “C2.6 alkynyl” may be ethynyl, propynyl, butynyl, pentynyl and hexynyl. Alkynylene groups are divalent alkynyl groups and may likewise be linear or branched and have two points of attachment to the remainder of the molecule. Furthermore, an alkynylene group may, for example, correspond to one of those alkynyl groups listed in this paragraph. For example alkynylene may be -C=C-, -CH2C=C-, -CH2C=CCH2-, -CH(CH3)CH C- or - CH2C=CCH3. Alkynyl and alkynylene groups may unsubstituted or substituted by one or more substituents. Possible substituents are described herein. For example, substituents may be those described above as substituents for alkyl groups.

[0018] The term “C3.g cycloalkyl” includes a saturated hydrocarbon ring system containing 3, 4, 5, 6, 7, 8, or 9 carbon atoms. For example, the “C3-Ce cycloalkyl” may be cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, bicyclo[2.1.1]hexane or bicyclo[1.1.1]pentane. Suitably the “C3-Ce cycloalkyl” may be cyclopropyl, cyclobutyl, cyclopentyl or cyclohexyl.

[0019] The term “aromatic” when applied to a substituent as a whole includes a single ring or polycyclic ring system with 4n + 2 electrons in a conjugated TT system within the ring or ring system where all atoms contributing to the conjugated TT system are in the same plane. The term “aryl” includes an aromatic hydrocarbon ring system with or without the presence of ring substitution. The ring system has 4n +2 electrons in a conjugated TT system within a ring where all atoms contributing to the conjugated TT system are in the same plane. For example, the “aryl” may be phenyl and naphthyl. The aryl system itself may be substituted with other groups.

[0020] The term “heteroaryl” includes an aromatic mono- or bicyclic ring incorporating one or more (for example 1-4, particularly 1 , 2 or 3) heteroatoms selected from nitrogen, oxygen or sulfur. The ring or ring system has 4n + 2 electrons in a conjugated TT system where all atoms contributing to the conjugated TT system are in the same plane.

[0021] The term “heterocyclic” includes a non-aromatic saturated or partially saturated monocyclic or fused, bridged, or spiro bicyclic heterocyclic ring system. Monocyclic heterocyclic rings may contain from about 3 to 12 (suitably from 3 to 7) ring atoms, with from 1 to 5 (suitably 1 , 2 or 3) heteroatoms selected from nitrogen, oxygen or sulfur in the ring. Bicyclic heterocycles may contain from 7 to 12-member atoms in the ring. Bicyclic heterocyclic(s) rings may be fused, spiro, or bridged ring systems. The heterocyclyl group may be a 3-12, for example, a 3- to 9- (e.g. a 3- to 7-) membered non-aromatic monocyclic or bicyclic saturated or partially saturated group comprising 1 , 2 or 3 heteroatoms independently selected from O, S and N in the ring system (in other words 1 , 2 or 3 of the atoms forming the ring system are selected from O, S and N). By partially saturated it is meant that the ring may comprise one or two double bonds. This applies particularly to monocyclic rings with from 5 to 7 members. The double bond will typically be between two carbon atoms but may be between a carbon atom and a nitrogen atom. Bicyclic systems may be spiro-fused, i.e. where the rings are linked to each other through a single carbon atom; vicinally fused, i.e. where the rings are linked to each other through two adjacent carbon and / or nitrogen atoms; or they may be share a bridgehead, i.e. the rings are linked to each other through two non-adjacent carbon or nitrogen atoms (a bridged ring system). Examples of heterocyclic groups include cyclic ethers such as oxiranyl, oxetanyl, tetrahydrofuranyl, dioxanyl, and substituted cyclic ethers. Heterocycles comprising at least one nitrogen in a ring position include, for example, azetidinyl, pyrrolidinyl, piperidinyl, piperazinyl, morpholinyl, thiomorpholinyl, tetrahydrotriazinyl, tetrahydropyrazolyl, tetrahydropyridinyl, homopiperidinyl, homopiperazinyl, 2,5-diaza-bicyclo[2.2.1]heptanyl and the like. Typical sulfur containing heterocycles include tetrahydrothienyl, dihydro-1 , 3-dithiol, tetra hydro-2 H- thiopyran, and hexahydrothiepine. Other heterocycles include dihydro oxathiolyl, tetrahydro oxazolyl, tetrahydro-oxadiazolyl, tetrahydrodioxazolyl, tetrahydrooxathiazolyl, hexahydrotriazinyl, tetrahydro oxazinyl, tetrahydropyrimidinyl, dioxolinyl, octahydrobenzofuranyl, octahydrobenzimidazolyl, and octahydrobenzothiazolyl. For heterocycles containing sulfur, the oxidized sulfur heterocycles containing SO or SO2 groups are also included. Examples include the sulfoxide and sulfone forms of tetrahydrothienyl and thiomorpholinyl such as tetrahydrothiene 1 ,1 -dioxide and thiomorpholinyl 1 ,1 -dioxide. A suitable value for a heterocyclyl group which bears 1 or 2 oxo (=0), for example, 2 oxopyrrolidinyl, 2-oxoimidazolidinyl, 2-oxopiperidinyl, 2,5- dioxopyrrolidinyl, 2,5-dioxoimidazolidinyl or 2,6-dioxopiperidinyl. Particular heterocyclyl groups are saturated monocyclic 3 to 7 membered heterocyclyls containing 1 , 2 or 3 heteroatoms selected from nitrogen, oxygen or sulfur, for example azetidinyl, tetrahydrofuranyl, tetrahydropyranyl, pyrrolidinyl, morpholinyl, tetrahydrothienyl, tetrahydrothienyl 1 ,1 -dioxide, thiomorpholinyl, thiomorpholinyl 1 ,1 -dioxide, piperidinyl, homopiperidinyl, piperazinyl or homopiperazinyl. As the skilled person would appreciate, any heterocycle may be linked to another group via any suitable atom, such as via a carbon or nitrogen atom. For example, the term “piperidino” or “morpholino” refers to a piperidin- 1-yl or morpholin-4-yl ring that is linked via the ring nitrogen.

[0022] The term “fused ring system” takes the IIIPAC definition and includes aliphatic and aromatic systems.

[0023] The term “bridged ring systems” includes ring systems in which two rings share more than two atoms, see for example Advanced Organic Chemistry, by Jerry March, 4th Edition, Wiley Interscience, pages 131-133, 1992. Suitably the bridge is formed between two non- adjacent carbon or nitrogen atoms in the ring system. The bridge connecting the bridgehead atoms may be a bond or comprise one or more atoms. Examples of bridged heterocyclyl ring systems include, aza-bicyclo[2.2.1]heptane, 2-oxa-5- azabicyclo[2.2.1]heptane, aza-bicyclo[2.2.2]octane, aza-bicyclo[3.2.1]octane, and quinuclidine.

[0024] The term “spiro bi-cyclic ring systems” includes ring systems in which two ring systems share one common spiro carbon atom, i.e. the heterocyclic ring is linked to a further carbocyclic or heterocyclic ring through a single common spiro carbon atom. Examples of spiro ring systems include 3,8-diaza-bicyclo[3.2.1]octane, 2,5-diaza-bicyclo[2.2.1]heptane, 6-azaspiro[3.4]octane, 2-oxa-6-azaspiro[3.4]octane, 2-azaspiro[3.3]heptane, 2-oxa-6- azaspiro[3.3]heptane, 6-oxa-2-azaspiro[3.4]octane, 2,7-diaza-spiro[4.4]nonane, 2- azaspiro[3.5]nonane, 2-oxa-7-azaspiro[3.5]nonane and 2-oxa-6-azaspiro[3.5]nonane.

[0025] In embodiments, the compound may be or comprise a polymer.

[0026] In embodiments, one or both of R1and R2of general formulae (2a) and / or (2b) may represent or comprise the polymer scaffold or chain. In embodiments, the polymer scaffold or chain may comprise a thermoset material. In embodiments, the polymer scaffold or chain main comprise one or more of polyurethane, polyacrylate, polyacrylamide, polymethacrylamide, polyether, polystyrene, poly(methyl methacrylate), polyethylene oxide), polymethacrylate, copolymer of acrylate, methacrylate, styrene, poly(isobornyl acrylate), polyacrylonitrile, polyether, polyester, polylactic acid, polyamide, polyester, amide, polycarbonate, poly-alpha-olefin, ethylene propylene diene monomer (M-class) rubber (EPDM), ethylene propylene rubber (EPM), hydrogenated or unhydrogenated polybutadienes, acrylonitrile butadiene styrene (ABS), styrene-butadiene rubber (SBR), polysiloxanes, polyisocyanurates (PIR), and / or block, comb and / or star copolymers of those polymers. In embodiments, the polymer scaffold may be bonded to the moiety having the general structure (2a) and (2b) via the nitrogen atom.

[0027] In embodiments, R1and R2may have or comprise the same structure. In embodiments, R1and R2may have or comprise a different structure from one another.

[0028] In embodiments, R1and / or R2may be CH2CH2CH3.

[0029] In a further series of embodiments, R1and / or R2may be a phenyl group (-Ph), methyl benzoate (-PhCOOMe), or methoxybenzene (-PhOMe).

[0030] In embodiments, the method may comprise re-polymerising the oligomers or monomers to form the polymer. In embodiments, re-polymerising the oligomers or monomers may have a yield of greater than 90%, e.g. greater than 95%, or greater than 98%, or greater than 99%, e.g. 100%. In embodiments, repolymerising the oligomers or monomers may comprise irradiating the oligomers or monomers with UV light. In embodiments, irradiating with UV light may comprise using a wavelength from 300 to 600 nm, e.g. from 310 to 500 nm, or from 320 to 450 nm, e.g. from 330 to 420 nm, e.g. from 340 to 410 nm, e.g. from 360 to 400 nm, e.g. 365 nm or 395 nm, and / or a power of 15 mW, and / or for a duration of one hour or more.

[0031] Advantageously, depolymerisation of the polymer into oligomers or monomers according to the method of the invention is reversible upon heating. That is, the polymer may be reverted back to its oligomers or monomers by heating to a temperature at or above 35°C. This is because the moieties (1 a) and (1 b) are able to undergo a formal [2+2] cycloreversion upon heating to generate oligomers or monomers comprising moieties having the general structure (2a) and (2b). The oligomers or monomers may be repolymerised, e.g. via irradiation, to undergo [2+2] cycloadditions to reform the polymer. Consequently, these compounds may find use as sustainable polymers that are able to be recycled. This result is surprising because maleimides not comprising such a sulphide moiety do not exhibit this behaviour. Without wishing to be bound by theory, the inventors believe that the thiol substitution of the olefin of the maleimide, i.e. to form a sulphide bond, modifies the stereoelectronics of the compound which allows quantitative or near quantitative cycloreversion on a repeatable basis.

[0032] Consequently, the method of the invention may be used for debonding, rebonding, reshaping, (re)processing, and recycling the polymer.

[0033] In embodiments, the method may comprise heating the repolymerised polymer to a temperature above 35°C (e.g. at or above a temperature of 40°C, or at or above a temperature of 45°C, or at or above a temperature of 50°C, or at or above a temperature of 55°C, or at or above a temperature of 60°C, or at or above a temperature of 65°C, or at or above a temperature of 70°C, or at or above a temperature of 75°C, or at or above a temperature of 80°C, or at or above a temperature of 85°C, or at or above a temperature of 90°C, or at or above a temperature of 95°C, or at or above a temperature of 100°C) to generate oligomers or monomers comprising moieties having the general structure (2a) and (2b), e.g. and at least 50%, e.g. at least 60%, or at least 70%, or at least 80%, or at least 90% of the moieties defined in general structure (1a) and / or (1 b) are converted into the moieties defined in general structure (2a) and (2b).

[0034] In embodiments, the method may comprise performing n cycles (e.g. 1 , 2, 3, 4, 5, or more) of repolymerisation, e.g. by irradiation, followed by depolymerisation by conversion back to oligomers or monomers, e.g. by heating to a temperature above 35°C, e.g. at or above a temperature of 40°C, or at or above a temperature of 45°C, or at or above a temperature of 50°C, or at or above a temperature of 55°C, or at or above a temperature of 60°C, or at or above a temperature of 65°C, or at or above a temperature of 70°C, or at or above a temperature of 75°C, or at or above a temperature of 80°C, or at or above a temperature of 85°C, or at or above a temperature of 90°C, or at or above a temperature of 95°C, or at or above a temperature of 100°C .

[0035] In embodiments, method comprising heating the polymer to a temperature above 105°C, or above 110°C, or above 115°C, or above 120°C, or above 125°C, or above 130°C, or above 135°C, or above 140°C, or above 145°C, or above 150°C, or above 155°C, or above 160°C. In embodiments, the method may comprise heating the polymer to a temperature between 120 to 160°C, e.g. between 130 to 150°C. Advantageously, the cycloreversion reaction is possible at relatively low temperatures. More advantageously, by using different types of energy to cyclise (i.e. repolymerise) and cyclorevert (i.e. depolymerise) the polymer, the forward reaction to form the polymer does not compete with the backward reaction to cyclorevert the polymer to its oligomers or monomers.

[0036] In embodiments, the polymer may be dissolved or suspended in a solvent. In alternative embodiments, the method may be performed on the bulk polymer, i.e. in the absence of solvent.

[0037] In embodiments, the moieties of the oligomers or monomers having the general structures (2a) and (2b) may be represented by the formulae (2c) and (2d):

[0038] (2c)

[0039] (2d) wherein R1and R2are defined as above; wherein Racomprises an aliphatic or aromatic group, for example Ramay be selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1-20 alkyl, C2-20 alkenyl, C1-20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein Rais optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

[0040] In embodiments, the oligomers may comprise a polymer scaffold or chain. In embodiments, Raof general formulae (2c) and / or (2d) may represent or comprise the polymer scaffold or chain. In embodiments, the polymer scaffold or chain may comprise a thermoset material. In embodiments, the polymer scaffold or chain main comprise one or more of polyurethane, polyacrylate, polystyrene, poly(methyl methacrylate), polyethylene oxide, polymethacrylate, copolymer of acrylate, methacrylate, styrene, poly(isobornyl acrylate), polyacrylonitrile, polyether, polyester, polylactic acid, polyamide, polyester, amide, polycarbonate, poly- alpha-olefin, ethylene propylene diene monomer (M-class) rubber (EPDM), ethylene propylene rubber (EPM), hydrogenated or unhydrogenated polybutadienes, acrylonitrile butadiene styrene (ABS), styrene-butadiene rubber (SBR), polysiloxanes, polyisocyanurates (PIR), and / or block, comb and / or star copolymers of those polymers. In embodiments, the polymer scaffold may be bonded to the moiety having the general structure (2a) and (2b) via the sulphur atom, i.e. to form a sulphide bond.

[0041] In embodiments, the monomers or oligomers may have more than one moiety having the general structure (1a) and / or (1 b), for example, two, three, four, or more, moieties having the general structure (1a) and / or (1b). In embodiments, Ramay comprise a core or hub moiety of the monomer or oligomer. In embodiments, the core or hub may comprise a alkyl chain, for example comprising an ester moiety or a polyethylene glycol moiety. In embodiments, the core or hub moiety may comprise a tertiary or quaternary carbon atom, i.e. a carbon atom which is bonded to three or four other carbon atoms respectively.

[0042] In embodiments, the monomers (2a), (2b), (2c), and / or (2d) may have or comprise the following general structure (11):

[0043] (11) wherein Rcindependently comprises an aliphatic or aromatic group, for example Rcmay be independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein Rcis optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl;

[0044] L is a linker group independently comprising or consisting of C1.10 alkylene; C2-10 alkenylene; C2-ioalkynylene or C6-i2aryl, wherein said Ci- 10 alkylene; C2-10 alkenylene; C2-io alkynylene or C6-i2 aryl optionally comprise one or more heteroatoms within the hydrocarbon chain, wherein said heteroatoms are selected from one or more of O, S and N;

[0045] H is a core or hub moiety, for example comprising a secondary, tertiary, or quaternary carbon atom; and x is an integer of 1 , 2, 3, 4, or more.

[0046] In embodiments, x is an integer of 1 , 2, 3, or 4. That is, the monomer may comprise one, two, three, or four arms, which may be the same or may be different from one another. In embodiments, the linker group (L) may comprise an ester moiety. In embodiments, the - S-L- group may comprise or consist of the formula -S-(CH2)y(C=O)O(CH2)z- wherein y and z are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, y may be 2 and z may be 1 .

[0047] In embodiments, the linker group (L) may comprise a polyethylene glycol moiety and / or an ester group. In embodiments, the -S-L- group may comprise or consist of the formula -S- (CH2)p(C=O)O(CH2CH2O)q(CH2)r- wherein p, q, and r are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, p may be 2 and r may be 1.

[0048] In embodiments, the monomers (2a), (2b), (2c), and / or (2d) may have or comprise the following general structure (12):

[0049] (12) wherein Rdindependently comprises an aliphatic or aromatic group, for example Rdmay be independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein Rdis optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl;

[0050] L is a linker group independently comprising or consisting of C1.10 alkylene; C2-10 alkenylene; C2-ioalkynylene or C6-i2aryl, wherein said Ci- 10 alkylene; C2-10 alkenylene; C2-10 alkynylene or Ce-12 aryl optionally comprise one or more heteroatoms within the hydrocarbon chain, wherein said heteroatoms are selected from one or more of O, S and N; H is a core or hub moiety, for example comprising a secondary, tertiary, or quaternary carbon atom; and y is an integer of 1 , 2, 3, 4, or more.

[0051] In embodiments, y is an integer of 1 , 2, 3, or 4. That is, the monomer may comprise one, two, three, or four arms, which may be the same or may be different from one another.

[0052] In embodiments, the linker group (L) may comprise an ester moiety. In embodiments, the - S-L- group may comprise or consist of the formula -S-(CH2)y(C=O)O(CH2)z- wherein y and z are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, y may be 2 and z may be 1 .

[0053] In embodiments, the linker group (L) may comprise a polyethylene glycol moiety and / or an ester group. In embodiments, the -S-L- group may comprise or consist of the formula -S- (CH2)p(C=O)O(CH2CH2O)q(CH2)r- wherein p, q, and r are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, p may be 2 and r may be 1 .

[0054] In embodiments, the monomers (2a), (2b), (2c), and / or (2d) may have or comprise the following general structure (13):

[0055] (13) wherein L1and L2are linker groups independently comprising or consisting of Ci-w alkylene; C2-10 alkenylene; C2-10 alkynylene or C6-i2 aryl, wherein said Ci- 10 alkylene; C2-10 alkenylene; C2-10 alkynylene or Ce-12 aryl optionally comprise one or more heteroatoms within the hydrocarbon chain, wherein said heteroatoms are selected from one or more of O, S and N;

[0056] H1and H2are core or hub moieties, for example independently comprising a secondary, tertiary, or quaternary carbon atom. In embodiments, the monomers (2a), (2b), (2c), and / or (2d) may have or comprise the following general structure (14): (14) wherein ReRf, R9, Rhindependently comprises an aliphatic or aromatic group, for example Rdmay be independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein ReRf, R9, Rhis optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl; and g, h, i are independently integers of 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10 or more.

[0057] In embodiments, the monomers (2a), (2b), (2c), and / or (2d) may have or comprise the following general structure (3):

[0058] (3) wherein R1and R2are defined as above;

[0059] R3and R4are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R3and / or R4are optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

[0060] In embodiments, R3and R4may be the same or may be different. In embodiments, R3and R4may each represent an alkyl chain, e.g. a Ci-e alkyl chain, for example CH2CH3.

[0061] In embodiments, the monomers (2a), (2b), (2c), or (2d) may have or comprise the following general structure (4):

[0062] (4) wherein R1, R2, R6are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1, R2, R6is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl wherein R5is selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R5is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

[0063] In embodiments, R5represents an alkyl chain, e.g. a Ci-e alkyl chain, for example CH2CH3. In embodiments, the monomers (2a), (2b), (2c), or (2d) may have or comprise the following general structure (5):

[0064] (5) wherein R1, R2, R6, R7are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1, R2, R6, R7is optionally substituted with one or more of H, D, F, Cl, Br, I,

[0065] OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl. In embodiments, the oligomers or monomers according to the method may consists of monomers (3) and / or (4) and / or (5). A further aspect of the invention provides a polymer comprising a backbone and crosslinked bridges, the backbone comprising plural, e.g. two or more, moieties having the general structure (1a) and / or (1 b) or a stereoisomer, enantiomer, racemate, or tautomer thereof:

[0066] (1a)

[0067] (1b) wherein R1and R2are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1and / or R2is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

[0068] In embodiments, the backbone of the polymer further comprises an alkyl group, e.g. an alkyl group comprising ester moieties.

[0069] In embodiments, the backbone of the polymer chain further comprises the following general structure (6):

[0070] (6) wherein Rmand Rnare independently alkyl groups, e.g. C1-20 alkyl, or hydrocarbon chains comprising heteroatoms, e.g. -CH2O(C=O)CH2CH2-.

[0071] In embodiments, one of Rmor Rnis -CH2O(C=O)CH2CH2-. In embodiments, each of Rmand Rnare -CH2O(C=O)CH2CH2-.

[0072] In embodiments, the crosslinked bridges comprise plural, e.g. two or more, moieties having the general structure (1a) and / or (1b) or a stereoisomer, enantiomer, racemate, or tautomer thereof.

[0073] In embodiments, the crosslinked bridges comprise the general structure (6).

[0074] A further aspect of the invention provides a polymer comprising plural, e.g. two or more, moieties having the general structure (1a) and / or (1b) or a stereoisomer, enantiomer, racemate, or tautomer thereof:

[0075] (1a)

[0076] (1b) wherein R1and R2are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1and / or R2is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

[0077] In embodiments, the polymer may comprise a backbone. The backbone may be bonded to the sulphur atom of the moieties shown in general formulae (1a) or (1 b). In embodiments, the backbone may comprise one or more of polyurethane, a polyacrylate, polystyrene, poly(methyl methacrylate), polyethylene oxide), polyacrylamide, polymethacrylamide, polyether, polymethacrylate, copolymer of acrylate, methacrylate, styrene, poly(isobornyl acrylate), polyacrylonitrile, polyether, polyester, polylactic acid, polyamide, polyester, amide, polycarbonate, poly-alpha-olefin, ethylene propylene diene monomer (M-class) rubber (EPDM), ethylene propylene rubber (EPM), hydrogenated or unhydrogenated polybutadienes, acrylonitrile butadiene styrene (ABS), styrene-butadiene rubber (SBR), polysiloxanes, polyisocyanurates (PIR), and / or block, comb and / or star copolymers of those polymers.

[0078] In embodiments, the polymer according to the invention may be that disclosed in Macromolecules 2022, 55 (19), 8495-8504 by the inventors.

[0079] A further aspect of the invention provides a monomer, the monomer comprising three, four, or more moieties, for example wherein the molecular weight is less than 3000 gmol’1, or less than 2000 gmol-1, or less than 1500 gmol-1, having the following general formula (7):

[0080] (7) wherein R1is selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1-20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

[0081] In embodiments, R1represents an alkyl group, e.g. a Ci-e alkyl chain, e.g. CH2CH2CH3.

[0082] In embodiments, the monomer may have or comprise the following general structure (11):

[0083] (11) wherein Rcindependently comprises an aliphatic or aromatic group, for example Rcmay be independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein Rcis optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl;

[0084] L is a linker group independently comprising or consisting of CMO alkylene; C2-10 alkenylene; C2-ioalkynylene or C6-i2aryl, wherein said Ci- 10 alkylene; C2-10 alkenylene; C2-10 alkynylene or Ce-12 aryl optionally comprise one or more heteroatoms within the hydrocarbon chain, wherein said heteroatoms are selected from one or more of O, S and N;

[0085] H is a core or hub moiety, for example comprising a secondary, tertiary, or quaternary carbon atom; and x is an integer of 3, 4, or more.

[0086] In embodiments, x is an integer of 3 or 4. That is, the monomer may comprise three or four arms, which may be the same or may be different from one another. In embodiments, the linker group (L) may comprise an ester moiety. In embodiments, the - S-L- group may comprise or consist of the formula -S-(CH2)y(C=O)O(CH2)z- wherein y and z are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, y may be 2 and z may be 1 .

[0087] In embodiments, the linker group (L) may comprise a polyethylene glycol moiety and / or an ester group. In embodiments, the -S-L- group may comprise or consist of the formula -S- (CH2)p(C=O)O(CH2CH2O)q(CH2)r- wherein p, q, and r are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, p may be 2 and r may be 1 .

[0088] In embodiments, the monomer may have or comprise the following general structure (12):

[0089] (12) wherein Rdindependently comprises an aliphatic or aromatic group, for example Rdmay be independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein Rdis optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl;

[0090] L is a linker group independently comprising or consisting of C1.10 alkylene; C2-10 alkenylene; C2-ioalkynylene or C6-i2aryl, wherein said Ci- 10 alkylene; C2-10 alkenylene; C2-10 alkynylene or Ce-12 aryl optionally comprise one or more heteroatoms within the hydrocarbon chain, wherein said heteroatoms are selected from one or more of O, S and N;

[0091] H is a core or hub moiety, for example comprising a secondary, tertiary, or quaternary carbon atom; and y is an integer of 3 or 4, or more.

[0092] In embodiments, y is an integer of 3 or 4. That is, the monomer may comprise three or four arms, which may be the same or may be different from one another.

[0093] In embodiments, the linker group (L) may comprise an ester moiety. In embodiments, the - S-L- group may comprise or consist of the formula -S-(CH2)y(C=O)O(CH2)z- wherein y and z are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, y may be 2 and z may be 1 .

[0094] In embodiments, the linker group (L) may comprise a polyethylene glycol moiety and / or an ester group. In embodiments, the -S-L- group may comprise or consist of the formula -S- (CH2)p(C=O)O(CH2CH2O)q(CH2)r- wherein p, q, and r are independent integers of 0, 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10. For example, p may be 2 and r may be 1 .

[0095] In embodiments, the monomer may comprise the following general structure (13):

[0096] (13) wherein L1and L2are linker groups independently comprising or consisting of Ci-w alkylene; C2-10 alkenylene; C2-10 alkynylene or C6-i2 aryl, wherein said Ci- 10 alkylene; C2-10 alkenylene; C2-10 alkynylene or Ce-12 aryl optionally comprise one or more heteroatoms within the hydrocarbon chain, wherein said heteroatoms are selected from one or more of O, S and N;

[0097] H1and H2are core or hub moieties, for example independently comprising a secondary, tertiary, or quaternary carbon atom. In embodiments, the monomer may have or comprise the following general structure (14):

[0098] (14) wherein ReRf, R9, Rhindependently comprises an aliphatic or aromatic group, for example Rdmay be independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein ReRf, R9, Rhis optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl; and g, h, i are independently integers of 1 , 2, 3, 4, 5, 6, 7, 8, 9, 10 or more.

[0099] In embodiments, each moiety having the general formula (7) is bonded to a core or hub moiety of the monomer. In embodiments, the core or hub moiety may comprise a tertiary or quaternary carbon atom, i.e. a carbon atom which is bonded to three or four other carbon atoms respectively. In embodiments, the core or hub moiety may comprise the following general structure (8):

[0100] (8) wherein R8and R9are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R8and R9are optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

[0101] In embodiments, the core or hub moiety may comprise the following general structure (9):

[0102] (9) wherein R10is selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R10is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, Ci- 04 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C^ alkynyl.

[0103] In embodiments, R8and / or R9and / or R10may represent an alkyl group, e.g. a Ci-e alkyl chain, for example CH2CH3.

[0104] In embodiments, the core or hub moiety may comprise the following general structure (10):

[0105] (10)

[0106] In embodiments, the monomer has the structure (3), (4) and / or (5) as defined above.

[0107] The monomer according to the invention may be dimerised or polymerised to form a dimer or polymer. Therefore, a further aspect of the invention provides a polymer fabricated from the monomer having the general formula (7) as defined above.

[0108] A yet further aspect of the invention provides a method of polymerising the monomers according to general formula (7) to form a polymer. In embodiments, polymerising the monomers may have a yield of greater than 90%, e.g. greater than 95%, or greater than 98%, or greater than 99%, e.g. 100%. In embodiments, polymerising the monomers may comprise irradiating the monomers with UV light. In embodiments, irradiating with UV light may comprise using a wavelength from 300 to 600 nm, e.g. from 310 to 500 nm, or from 320 to 450 nm, e.g. from 330 to 420 nm, e.g. from 340 to 410 nm, e.g. from 360 to 400 nm, e.g. 365 nm or 395 nm, and / or a power of 15 mW, and / or for a duration of one hour or more, and / or a power of 15 mW, and / or for a duration of one hour or more. In embodiments, the method of the invention may further comprise heating the resulting polymer to a temperature at or above 35°C, e.g. at or above a temperature of 40°C, or at or above a temperature of 45°C, or at or above a temperature of 50°C, or at or above a temperature of 55°C, or at or above a temperature of 60°C, or at or above a temperature of 65°C, or at or above a temperature of 70°C, or at or above a temperature of 75°C, or at or above a temperature of 80°C, or at or above a temperature of 85°C, or at or above a temperature of 90°C, or at or above a temperature of 95°C, or at or above a temperature of 100°C, to regenerate the monomers having general formula (7). In embodiments, at least 50%, e.g. at least 60%, or at least 70%, or at least 80%, or at least 90% of the polymer is converted into the monomers defined in general structure (7).

[0109] In embodiments, the method or the monomer or polymer of the invention may be used in or as an adhesive, a foam, a sealant, a moulded article, a film, a coating, a varnish, a paint, an ink, a composite material, an extruded article, a 3D printed object, a fibre, an elastomer, a polymer-based adhesive, a pharmaceutical, a biomedical product, and / or a self-healing material capable of recovering from structural damage such as scratches.

[0110] In embodiments, the monomers of the invention may be used in 3D printing. Advantageously, this allows for a closed loop recycling process.

[0111] Within the scope of this application it is expressly intended that the various aspects, embodiments, examples and alternatives set out in the preceding paragraphs, in the claims and / or in the following description and drawings, and in particular the individual features thereof, may be taken independently or in any combination. That is, all embodiments and / or features of any embodiment can be combined in any way and / or combination, unless such features are incompatible. For the avoidance of doubt, the terms “may”, “and / or”, “e.g.”, “for example” and any similar term as used herein should be interpreted as non-limiting such that any feature so-described need not be present. Indeed, any combination of optional features is expressly envisaged without departing from the scope of the invention, whether or not these are expressly claimed. The applicant reserves the right to change any originally filed claim or file any new claim accordingly, including the right to amend any originally filed claim to depend from and / or incorporate any feature of any other claim although not originally claimed in that manner. Embodiments of the invention will now be described by way of example only with reference to the accompanying drawings in which:

[0112] Figure 1 is a schematic of the method according to the invention;

[0113] Figure 2a is a scheme for the reversible dimerization of N-propyl monothiohexyl maleimide (MTHM) monomer;

[0114] Figure 2b is a1H NMR spectrum (400 MHz) of the reaction mixture of Figure 2a;

[0115] Figure 2c is a1H NMR spectrum (400 MHz) of the cycloreversion reaction of Figure 2a;

[0116] Figure 2d is a1H NMR spectrum (400 MHz) of the photodimerization product of Figure 2a;

[0117] Figure 2e is a kinetic study of the cycloreversion of photodimer (101) to MTHM monomer (100);

[0118] Figure 2f is an1H NMR study showing the cyclability of polymerisation and depolymerisation via cycloreversion of the MTHM monomer (100);

[0119] Figure 3 is the results of a kinetic study of [2+2] cycloreversion of the thiomaleimide photodimer at different temperatures;

[0120] Figure 4 is kinetic plots for the [2+2] cycloreversion of photodimer shown in Figure 2a at different temperatures;

[0121] Figure 5a is a1H NMR (300 MHz) spectra of the maleimide monomer before and after irradiation according to a Comparative Example;

[0122] Figure 5b is a1H NMR (300 MHz) spectrum of the [2+2] photodimer of maleimide;

[0123] Figure 5c is a 1 H NMR (300 MHz) spectrum of the reaction mixture after prolonged heating of the [2+2] photodimer of maleimide;

[0124] Figure 6 is a synthetic scheme for the synthesis of monothiomaleimides according to the invention;

[0125] Figure 7a and 7b are1H and13C NMR spectra of the compounds made in Figure 6;

[0126] Figure 8 is UV-vis spectrum of a compound according to the invention;

[0127] Figure 9 shows1H NMR spectra showing the cycloaddition of compounds according to the invention;

[0128] Figure 10 shows1H NMR spectra showing the cycloaddition of compounds according to the invention;

[0129] Figure 11a is a series of1H NMR spectra of a monothiomaleimide according to the invention, which has undergone several cycles of photoaddition and cycloreversion; Figure 11 b is a series of1H NMR spectra of a monothiomaleimide according to the invention, which has undergone several cycles of photoaddition and cycloreversion;

[0130] Figure 12 is a graph showing the storage and loss modulus for monomers according to the invention;

[0131] Figure 13 is a graph showing the storage and loss modulus for the photocured monomers of Figure 12 according to the invention;

[0132] Figure 14 shows photo-rheology data for compounds according to the invention;

[0133] Figure 15 is two graphs illustrating isothermal analysis for the uncured and photocured monothiomaleimides according to the invention using thermogravimetric analysis (TGA);

[0134] Figure 16 is shown glass slides bonded together using the polymers of the invention;

[0135] Figure 17 is photographs illustrating strength testing of a compound according to the invention;

[0136] Figure 18 is a graph showing DSC testing for compounds according to the invention;

[0137] Figure 19 shows tensile strength testing of polymers according to the invention;

[0138] Figure 20 is a series of photographs illustrating scratch and heal tests of polymers according to the invention;

[0139] Figure 21 is a schematic illustration of the healing properties of materials, e.g. polymers, according to the invention;

[0140] Figures 22a to 22c are schemes for the creation of monothiomaleimides;

[0141] Figures 23 to 25 are1H NMR spectra showing the cycloaddition of compounds formed in Figures 22a-22c;

[0142] Figures 26a and 26b are the results of a kinetic study of the cycloaddition of compounds formed in Figures 22a-22c under 365nm and 405nm wavelength irradiation;

[0143] Figures 27a to 27c are the results of a kinetic study of the cycloreversion of compounds formed in Figures 22a-22c at 155°C, 140°C, and 125°C;

[0144] Figure 28a is a graph of the photo-rheology of MTM-TC333 during irradiation;

[0145] Figure 28b is a graph of the photodimerization of MTM-TC333,

[0146] Figure 28c is1H NMR spectra showing the cycloreversion and dimerization of MTM- TC333;

[0147] Figures 29a to 31 b show1H NMR spectra of the photodimerization and cyclorevsion of the compounds in Example 6b. ii - iv;

[0148] Figures 32a and 32b shows1H NMR spectra during photodimerization of the compound in Example 7a ii, and a graph showing the conversion against time; Figures 33a and 33b shows1H NMR spectra during thermal cycloreversion and the thermal cycloreversion kinetics of the compound of Example 7a iii.

[0149] Figure 34 shows 1 H NMR spectra during the bonding and de-bonding of the compound in Example 9a ii; And

[0150] Figures 35 to 37 are series of photographs illustrating the reversible crosslinking and gelation of materials according to the invention .

[0151] Referring first to Figure 1 , there is shown a schematic of the method 1 according to the invention. There is shown the monomers M according to the invention. In other embodiments, the monomers may be oligomers. There is shown the polymerised product P after cycloaddition of the monomers. It is shown that the monomers M comprise a monothiolmaleimide moiety (i.e. a maleimide comprising a sulphide moiety), and that the polymer P comprises a [2+2] cycloaddition product of the monothiolmaleimide moieties.

[0152] In the method of the invention, the monomers M are irradiated with UV irradiation at a wavelength from 300 to 600 nm to form the polymer P in a [2+2] cycloaddition reaction. The polymer P may then be heated at a temperature at or above 120 °C to cycloreverse the [2+2] cycloaddition to reform the monomers M. Advantageously, this reaction proceeds without the formation of substantial quantities of side products.

[0153] Examples and Results

[0154] [2+2]-Photocycloaddition reactions were performed using a 365 nm Lumidox II 96-Position LED array set at 45 mW. Irradiance (15 mW cm-2 ) was estimated by using an S142C Integrating Sphere Power Sensor Head with Silicon Detector, connected to a ThorLabs PM400 optical power meter at a wavelength set to 365 nm.

[0155] 1. [2+2] Photodimerisation and thermal cycloreversion of model compounds i. Photo-cycloreversion of photodimer (101) of MTHM monomer (100)

[0156] Referring now to Figure 2a, there is shown a scheme for the reversible dimerization of N- propyl monothiohexylmaleimide (MTHM) monomer (100). The feasibility of the reversible nature of this dimerization was investigated.

[0157] The N-propyl monothiohexylmaleimide (MTHM) monomer (100) was synthesised in two steps from bromomaleic anhydride. Propylamine was added to bromomaleic anhydride and the mixture was refluxed for up to 6 hours. The intermediate alkyl maleimide was reacted with hexane-1 -thiol in the presence of sodium acetate in methanol at room temperature for 10 minutes to yield the N-propyl monothiohexylmaleimide (MTHM) monomer (100).

[0158] Initially, N-propyl monothiohexylmaleimide (MTHM) monomer (100) was irradiated at 365nm to provide the photodimer (101).

[0159] The photodimer (101) was irradiated at 254 nm in DMSO-d6 for approximately 16 hours in order to investigate if shorter wavelength irradiation would lead to the [2+2] cycloreversion.

[0160] Referring now to Figure 2b, there is shown a1H NMR spectrum (400 MHz) of the resulting reaction mixture. It is shown that the signal corresponding to the vinyl proton of the MTHM monomer (100) was present. However, only very low conversion was observed (NMR yield ~ 7 %). The [2+2] cycloreversion could be also observed in the region between 2.6 and 3.1 ppm, as the methylene next to the sulfur atom from the MTHM monomer (100) reappeared at 3.0 ppm, with the photodimer (101) still present at 2.65 and 2.95 ppm. However, a triplet peak around 2.7 ppm, that overlapped with the photodimer (101), indicated potential side products being formed due to degradation because of prolonged exposure to high energy light. Although the reappearance of MTHM monomer (100) was a promising finding because it indicates that the MTHM photodimer (101) can be photochemically reverted into the monomer, these conditions seemed to be unsuitable for effective and reversible [2+2] cycloreversion in a polymer context. ii. Thermal cycloreversion of photodimer (101) of MTHM monomer (100)

[0161] The possibility of [2+2] cycloreversion using heat instead of light was investigated. The photodimer (101) was heated in DMSO-d6 at 120 °C for 65 hours.

[0162] Referring now to Figure 2c, there is shown a1H NMR spectrum (400 MHz) of the resulting reaction mixture.

[0163] It is shown that the [2+2] cycloreversion of the photodimer (101) could indeed occur under thermal conditions, as evidenced from the1H NMR resonance peak of the MTHM monomer (100) clearly present at 6.5 ppm. Additionally, the peaks for the cyclobutane ring protons of the photodimer (101) were absent. This analysis suggested that near quantitative cycloreversion had occurred. However, it should be noted that evidence of some new, minor proton environments indicated that trace amounts (approximately 4 to 5%) of unidentified side products were also formed, likely as a result of prolonged heating at 120 °C during the thermal cycloreversion reaction.

[0164] Following the cycloreversion process, the same solution was irradiated with UV light (365 nm, 15 mW. cm-2) for approximately 45 minutes to explore if the [2+2] photocycloaddition could occur again. Referring now to Figure 2d, there is shown a1H NMR (400 MHz) of the resulting reaction, wherein it is shown that the photodimer (101) reached full yield after irradiation by UV light (365 nm, 15 mW) in a second cycle of photodimersation. No side reactions were observed.

[0165] Advantageously, these results show that the MTHM monomer (100) is able to undergo photodimerisation and thermal cycloreversion with complete conversion and no observed loss of material due to side reactions. More advantageously, this chemistry could be introduced into bulk polymer materials for the recycling and reprocessing of crosslinked polymer networks, e.g. thermoset materials.

[0166] Referring now to Figure 2e, there is shown a kinetic study of the cycloreversion of photodimer (101) to MTHM monomer (100).

[0167] Referring also to Figure 2f, there is shown an1H NMR study showing the cyclability of polymerisation and depolymerisation via cycloreversion of the MTHM monomer (100). It is shown that there is very little degradation of the materials over five cycles. iii. Thermal cycloreversion of the photodimer (101) at different temperatures

[0168] The [2+2] cycloreversion of the MTHM monomer (100) was further investigated in more detail at different temperatures (120, 140, and 160 °C).

[0169] Referring now to Figure 3, there is shown the results of a kinetic study of [2+2] cycloreversion of the thiomaleimide photodimer at 120, 140, and 160 °C in DMSO. It is shown that the [2+2] cycloreversion rate varied depending on the temperature applied. It is shown that at 120 °C, only 5% of the photodimer (101) reverted to the MTHM monomer (100) after 60 minutes, whereas at 140°C it is shown that over 40% of the photodimer (101) reverted to the MTHM monomer (100) after the same period of time. It is also shown that heating the solution up to 160°C provided > 90% conversion of the MTHM monomer (100) to the photodimer (101) after 60 minutes, and full conversion was obtained after 90 minutes.

[0170] Referring now to Figure 4, there is shown kinetic plots for the [2+2] cycloreversion of photodimer (101) at different temperatures (120, 140, and 160 °C) (4a, 4b, and 4c respectively). There is also shown a plot (4d) showing the activation energy calculation of the reaction. It was found that the [2+2] cycloreversion of photodimer (101) followed a first order reaction. This is because the plots 4a, 4b, and 4c provided a linear relationship at all temperatures. The resulting Arrhenius plot (4d) allowed for the activation energy (Ea) for cyclobutane ring breakage to be calculated, which was found to be 133.8 ± 0.7 kJ. mol-1.

[0171] Table 1 below shows the experimentally derived kinetics of the thermal reversion of the dimers (i.e. formed after irradiation). kObs is the observed rate coefficient of thermal reversion; ti / 2 is the half life time in hours. These values are also shown on the graphs of Figure 4.

[0172] Table 1

[0173] 2. Comparative Examples: [2+2] cycloreversion of maleimide dimers

[0174] The [2+2] cycloreversion of maleimide dimers absent a sulfide group was investigated. Maleimide (200) was dissolved in DMSO-d6 solvent and the solution was irradiated for 24 hours (365 nm, 15 mW. cm-2). The same UV light source was used as for the photodimerisation of the MTHM monomer (100) shown in Figure 2a.

[0175] Referring now to Figure 5a, there is shown a1H NMR (300 MHz) spectrum of the maleimide monomer (200) before irradiation, the [2+2] photodimerisation of maleimide after exposure of the solution to UV light (365 nm, 15 mW. cm-2) for 24 hours, and the [2+2] photocycloadduct of maleimide after exposure of the solution to UV light after 48 hours in DMSO-d6. Surprisingly, only 89 % of the maleimide photodimer (201) was obtained after 24 hours. In contrast, the MTHM monomer (100) reached full conversion within 45 minutes under the same irradiation conditions. The solution was left for another 24 hours, which resulted in full conversion to the photodimer (201) being achieved after 48 hours in total. Referring now to Figure 5b, there is shown an1H NMR (300 MHz) spectrum of the [2+2] photodimer (201) of maleimide (200) after heating the solution to 160°C for 2 hours. It is shown that the photodimer (201) is stable, with only minor degradation products observed, and no maleimide monomer (200) was produced. This is surprising because these were the same conditions used to completely cycloreverse the photodimer (101) of the MTHM monomer (100).

[0176] Referring now to Figure 5c, there is shown an1H NMR (300 MHz) spectrum of the [2+2] photodimer (201) of maleimide (200) after heating up the solution of Figure 5b to 160 °C for a further 24 hours. However, it is shown that the photodimer (201) began to thermally degrade (side product peaks at 3.2 to 3.6 ppm and the appearance of a second imide proton peak. Cycloreversion to maleimide was not observed.

[0177] Without wishing to be bound by theory, the inventors believe that sulphide substituent of the monothiomaleimides according to the invention, in comparison with maleimide, is responsible for the advantageous effects which enable thermoreversion of the [2+2] cycloaddition products.

[0178] 3. Thermal cycloreversion of multi-functional monothiomaleimides (MTMs)

[0179] The crosslinking and de-crosslinking reactions under irradiation and heating of a diluted solution of monothiomaleimides (MTMs) was investigated. A coating layer was also prepared. i. Synthesis of multi-functional monothiomaleimides (MTMs)

[0180] Referring to Figure 6, there is shown a synthetic scheme (A) for the preparation of a 3- armed MTM (3-MTM), and a synthetic scheme (B) for the preparation of a 4-armed MTM (4-MTM).

[0181] The 3-armed MTM (3-MTM) was prepared from the commercially available starting material trimethylolpropane tris(3-mercaptopropionate (3-SH) (CAS: 33007-83-9) in the following procedure:

[0182] A / -propyl-3-bromomaleimide (7 g, 32.10 mmol) and sodium acetate (2.632 g, 32.10 mmol) were dissolved in 100 mL methanol. Then, trimethylolpropane tris(3- mercaptopropionate) (2.81 g, 7.13 mmol) was added slowly. The reaction mixture was left to stir at ambient temperature for 30 minutes. Subsequently, the solvent was removed under reduced pressure and the crude product was dissolved in 100 mL dichloromethane and washed with water (3 x 100 mL). Then, dichloromethane was evaporated and the crude product was dissolved in a minimum amount of acetone. Then, the viscous product was precipitated in cold isopropanol. Lastly, the brown viscous product was collected and dried in a vacuum oven to obtain 4.0 g (70%).1H NMR (300 MHz, DMSO-d6) 5 (ppm) 0.63 - 0.95 (m, 12 H), 1.28 - 1.59 (m, 8 H), 2.70 - 2.85 (m, 6 H), 3.16 - 3.26 (m, 6 H), 3.28 - 3.50 (m, 6 H), 3.87 - 4.11 (m, 6 H), 6.49 - 6.71 (m, 3 H);13C NMR (75 MHz, CDCh) 6 (ppm) 7.30, 11.16, 21.78, 22.84, 26.12, 32.49, 39.82, 40.98, 63.71 , 117.90, 149.75, 167.75, 169.39, 170.35; UV (Amax = 360 nm).

[0183] The 4-armed MTM (4-MTM) was prepared from the commercially available starting material pentaerythritol tetrakis(3-mercaptopropionate) (4-SH) (CAS: 7575-23-7) in the following procedure:

[0184] A / -propyl-3-bromomaleimide (7 g, 32.10 mmol) and sodium acetate (2.632 g, 32.10 mmol) were dissolved in 100 mL methanol. Then, pentaerythritol tetrakis(3- mercaptopropionate) (2.61 g, 5.35 mmol) was added slowly. The reaction mixture was left at ambient temperature for 30 minutes. Subsequently, the solvent was removed under reduced pressure and the crude product was dissolved in 100 mL dichloromethane and washed with water (3 x 100 mL). Then, dichloromethane was evaporated and the crude product was dissolved in a minimum amount of acetone. Then, the viscous product was precipitated in cold isopropanol. Lastly, the brown viscous product was collected and dried in a vacuum oven to obtain 3.6 g (65%).1H NMR (300 MHz, DMSO-d6) 5 (ppm) 0.68 - 0.89 (m, 12 H), 1.35 - 1.60 (m, 8 H), 2.72 - 2.85 (m, 8 H), 3.16 - 3.27 (m, 8 H), 3.28 - 3.51 (m, 8 H), 4.03 - 4.25 (m, 8 H), 6.51 - 6.70 (m, 4 H);13C NMR (75 MHz, CDCh) 6 (ppm) 11.25, 21.87, 26.17, 32.48, 39.88, 42.43, 61.92, 118.05, 149.64, 167.78, 169.53, 170.20; UV (Amax = 360 nm).

[0185] Referring now to Figure 7a, there is shown a1H NMR spectrum of 3-MTM (A) and 4-MTM (B) in comparison to the starting materials 3-SH and 4-SH respectively. Referring also to Figure 7b, there is shown a13C NMR spectrum of 3-MTM (A) and 4-MTM (B). ii. Photopolymerisation and thermal cycloreversion of MTMs Referring now to Figure 8, there is shown a UV-vis spectrum for 3-MTM and its cycloaddition product (8a), and a UV-vis spectrum for 4-MTM and its cycloaddition product (8b). UV-Vis spectra were recorded on an Agilent Technologies Cary 60 UV-Vis in the range of 200-800 nm using a cuvette with a 10 mm optical path length.

[0186] The cycloaddition products of 3-MTM and 4-MTM were produced by irradiation of a solution of the starting materials (3-MTM and 4-MTM respectively) in DMSO solvent using UV light (365 nm, 15 mW). The maximum wavelength of absorbance Amax for both 3-MTM and 4- MTM was found to be 360 nm. Irradiation for one hour resulted in the total disappearance of the maximum wavelength peak, which led to the conclusion that these molecules were photoactive and had undergone [2+2] photodimerisation of MTM.

[0187] Solutions of 3-MTM and 4-MTM (8 mg / ml) in DMSO-d6 were prepared in an NMR tube. The solutions were irradiated for one hour (365 nm, 15 mW) and analysed using1H NMR spectroscopy. Referring to Figure 9, there is shown the1H NMR (300 MHz) spectrum for the cycloaddition of (A) 3-MTM and (B) 4-MTM in DMSO-d6 solvent. There is shown the spectrum for 3-MTM starting material (9a), the spectrum of the products after irradiation for 1 hour (9b), and the spectrum of the products after heating the irradiated solution at 160 °C for 2 hours (9c). There is also shown the spectrum for 4-MTM starting material (9d), the spectrum of the products after irradiation for 1 hour (9e), and the spectrum of the products after heating the irradiated solution at 160 °C for 2 hours (9f).

[0188] The1H NMR spectra (9b, 9e) of the solutions after irradiation for 1 hour confirmed that the photochemical [2+2] cycloaddition of 3-MTM and 4-MTM respectively had taken place. The MTM peak at 6.60 ppm completely disappeared, indicating that full conversion of MTM monomer to photodimer had been reached. All the signals in1H NMR became broader, and this is attributed to the increase in the molecular weight due to the intermolecular [2+2] photodimerisation of MTMs.

[0189] The1H NMR spectra (9c, 9f) of the irradiated solutions after heating at 160 °C for 2 hours shows that 3-MTM cycloaddition product reverted to 62% while 4-MTM cycloaddition product reverted with 73% conversion. The [2+2] cycloreversion conversion was calculated from the ratio between the ester group at 4.02 ppm and the reappeared peak of the olefinic proton at 6.60 ppm. Pleasingly, there were no side products observed that could be caused by thermal degradation. This finding concluded that these compounds had followed the similar trends as the model compounds.

[0190] Referring now to Figure 10, there is shown an1H NMR spectrum (300 MHz) for the 3-MTM cycloaddition product (A) and the 4-MTM cycloaddition product (B) after heating for 24 hours at 160 °C in DMSO-d6 solvent. It is shown that full [2+2] cycloreversion took place. However, some degradation products were formed due to the elevated temperature.

[0191] Referring now to Figure 11a, there is shown a series of1H NMR spectra showing the products after three cycles of irradiation and heating of 3-MTM. Referring also to Figure 11b, there is shown a series of1H NMR spectra showing the products after three cycles of irradiation and heating of 4-MTM. The photocycloaddition and cycloreversion were monitored by observing the olefinic peak at 6.60 ppm. This was used to calculate the [2+2] cycloreversion by the integration of methyl peak at 0.8 ppm in comparison to the olefinic peak at 6.60 ppm.

[0192] In the first cycle, the solutions were exposed to UV light (365 nm, 15 mW) for an hour, which resulted in full conversion of 3-MTM and 4-MTM in each solution. The resulting solutions were heated for 2 hours at 160°C to cause cycloreversion in 67% and 61% for 3-MTM and 4-MTM respectively. In the second cycle, the solutions were irradiated in the same manner as the first cycle to produce the cycloaddition products, and these were heated for 3 hours at 160°C to cause cycloreversion in 76% and 75% for 3-MTM and 4-MTM respectively. In the third cycle, the solutions were irradiated in the same manner as the first cycle to produce the cycloaddition products, and these were heated for 4 hours at 160°C to cause cycloreversion in 47% and 67% for 3-MTM and 4-MTM respectively. It is shown that these materials undergo cycloaddition and cycloreversion without the formation of degradation products. iii. Photo-rheology to measure storage (G’) and loss (G”) modulus during irradiation The photocuring process of 3-MTM and 4-MTM was investigated using photo-rheology to measure the storage (G’) and loss (G”) modulus during irradiation as the cycloaddition products formed.

[0193] Rheological analysis was performed using an Anton Paar MCR 302 rheometer equipped with a P-PTD 200 glass plate with peltier controller and an H-ETD 400 electrically heated temperature hood with compressed air cooling. A parallel plate configuration (25 mm diameter) was used, connected to an Omnicure S2000 linked to an optical probe and fitted with Lumen Dynamics 200W Mercury lamp and bandpass filter (320 - 390 nm) to irradiate the sample through the glass plate from the bottom. Measurements were performed in oscillatory shear strain with an amplitude of 0.1% and frequency of 0.1 Hz under a set normal force of FN = 0 N. The data was analysed using the RheoCompass software.

[0194] Referring now to Figure 12, there is shown a graph for the storage (G’) and loss (G”) modulus measured for (A) 3-MTM and (B) 4-MTM in the dark for 5 minutes. This provides information about the properties of the materials before the irradiation takes place. It is shown that the loss (G”) modulus was found higher than the storage (G’) modulus for both 3-MTM and 4-MTM, which was expected due to the fluid characteristic of the materials. Both materials showed a stable storage (G’) and loss (G”) modulus measurements throughout the experiment.

[0195] Referring now to Figure 13, there is shown a graph for the storage (G’) and loss (G”) modulus obtained by photo-rheology measured for (A) 3-MTM and (B) 4-MTM during irradiation over 24 hours. An Omnicure S2000 UV light source was linked to an optical probe and fitted with Lumen Dynamics 200W Mercury lamp and bandpass filter (A = 320 - 390 nm).

[0196] It is shown that there is a significant increase in the storage (G’) modulus, which is expected due to the increase in solid content as the cycloaddition products are produced to form a covalent network. In each case, as the material fully cured, the increase in storage (G’) modulus slowed down and eventually plateaued.

[0197] For 3-MTM, the crossover point of the storage (G’) and loss (G”) modulus occurred after 2 hours. However, for 4-MTM, the crossover point of the storage (G’) and loss (G”) modulus, wherein it had reached sol-gel transition, occurred after just 34 minutes. This could be due to 4-MTM having 4 arms, which accelerates molecular weight build-up during the photocuring compared to 3-MTM. Nevertheless, both materials had high G’ values (i.e. > 1 Mpa).

[0198] The photo-rheology experiments were repeated with temperature control. The aim for controlling the temperature was to observe whether decrosslinking takes place and thus a reduction in the storage (G’) modulus and loss (G”) modulus due to the [2+2] cycloreversion. Furthermore, the repeatability of the photochemical [2+2] cycloaddition / cycloreversion of 3-MTM could be assessed in bulk. Referring now to Figure 14, there is shown a graph showing the results of three cycles of irradiation and heating for 3-MTM using photo-rheology connected to the temperature controller. The sample was initially held for 30 minutes at 50°C. Irradiation steps were all performed for 6 hours with Amax = 365 nm at 50 °C. Heating steps all comprised heating to and holding the temperature at 160 °C for 12 hours. Cooling was performed from 160 to 50 °C at 1°C / min. The complex viscosity of the sample was recorded throughout the rheology experiment with the value after each step listed in Table 2 below. The significant change in viscosity after heating, and even during cooling, when compared to the irradiated samples facilitate much easier reprocessing and recycling.

[0199] Table 2

[0200] The difference between this experiment and the NMR study shown in Figure 11a and 11 b is that the samples were transformed from a diluted solution to the bulk state, which would be a better representation when used in material applications.

[0201] Firstly, the sample layer was heated up to 50 °C for practical reasons as the interference of a too viscous material complicates sample manipulation. Before irradiation, the loss (G”) modulus was found to be higher than the storage (G’) modulus over a 30 minute time interval in the dark. This was expected due to the fluidic characteristic of the material and the absence of any rigid content associated with covalent crosslinking. When the material was exposed to the UV light (320-390 nm) for 6 hours, the G’ and G” significantly increased from around 10-100 Pa to around 1 ,000,000 Pa for G’ and 100,000 Pa for G”. When the light was switched off and the temperature was set at 160 °C, both the storage and loss modulus displayed a very fast decrease until they reached 0.001-10 Pa. A crossover denoted the transformation of a covalently crosslinked material into a viscous liquid. The moduli remained constant with the temperature being held at 160 °C and were in the same range as G’ and G” before UV-crosslinking. Then, the second cycle for the irradiation was carried out for 6 hours as the first cycle. Similarly, the G’ and G” increased as a result of the reformation of the covalent crosslinking due to the [2+2] photocycloaddition of MTMs as occurred in the first cycle. Similar results were obtained in the third cycle. It should be noted that the G’ and G” values slightly decreased after each photo-curing step, which might be attributed to minor degradation due to the long-term heating, as observed in the model studies. Nonetheless, both the second and third cycles of heating resulted in a significant and to a similar extent reduction in G’ caused by the [2+2] cycloreversion of MTMs and the dissociation of the covalent network.

[0202] Therefore, the materials according to the invention in bulk underwent multi-cycles of irradiation / heat similar to the solution. This finding was encouraging to apply this material in application and exploit the [2+2] cycloreversion of the material in debondable adhesives and self-healable coatings. iv. Thermogravimetric analysis of uncured and cured samples of 3-MTM and 4- MTM

[0203] The uncured and cured samples of 3-MTM and 4-MTM were analysed by thermogravimetric analysis (TGA). Thermogravimetric analysis (TGA) was performed using a TA Instruments SDT 650.

[0204] Referring now to Figure 15, there is shown two graphs illustrating isothermal analysis for the uncured and photo-cured (A) 3-MTM and (B) 4-MTM using thermogravimetric analysis (TGA). Before irradiation is labelled “Bl” and after irradiation is labelled “Al”. The temperature was set at 140 °C for 24 hours. It was found that the wt.% for all the samples dropped at the earlier stage when the temperature reached 39-45 °C, which might be due to the evaporation of residual acetone. After that, when the temperature was held at 140 °C for 24 hours. There was a reduction in the wt.% for all the samples, although this remained below 15 wt.% loss. This small amount of thermal degradation is in agreement with the finding from1H NMR analysis. Interestingly, the photo-cured samples were less susceptible to thermal degradation than the uncured analogues by approximately 4%. v. Preparation and testing of a coating layer on glass using 3-MTM and 4-MTM Referring now to Figure 16, there is shown two glass slides (A) used in the photo-rheology experiments described. The glass slides comprise the photo-cured 3-MTM (P-3-MTM) and the photo-cured 4-MTM (P-4-MTM). There is also shown the glass slides containing the cured 4-MTM sample holding a weight of 500g (B).

[0205] Initially, a small circular interlayer of 3-MTM and 4-MTM was placed between two individual glass slides. The joined glass slides were easy to debond after material application and thus before being exposed to UV light. After irradiation of both samples for 24 hours, the joined glass slides were much more difficult to separate as a result of the photo-cured layer of 3-MTM and 4-MTM. This was a promising result for the photo-cured products to be used as glass surface coatings and for adhesives.

[0206] The joined glass by 4-MTM layer was found capable of holding 500 g weight for approximately 72 hours and no separation between the joined glass slides was observed. This observation suggested that this layer was successfully cured using UV light (365 nm, 15 mW).

[0207] Referring now to Figure 17, there is shown the joined glass slides of Figure 16 adhered by a 4-MTM cured layer. A 50g weight is attached to one of the slides. There is shown the results before (A) and after (B) heating the joined glass slides in the oven at 120°C.

[0208] The covalently joined glass slides were then placed inside the oven, which was set at 120 °C, in order to observe the influence of the temperature on the photo-cured layer of 4-MTM. The joined glass was loaded with only 50 g weights, which is 10 times smaller than the weight used in the previous demonstration. It was revealed that the adhesion of the glass slides failed after being placed in the oven for 1 hour, which indicated a loss in the adhesive forces of the layer likely attributed to the [2+2] cycloreversion upon heating.

[0209] Referring now to Figure 18, there is shown a graph showing the modulated DSC for the photocured 4-MTM sample. The Y axis represents the normalised reversible and non- reversible heat flow, and the X axis represents the temperature ranging from -5 to 250 °C.

[0210] In order to ensure the adhesion glass failure after being placed in the oven was due to the [2+2] cycloreversion and not simply due to overcoming the glass transition temperature of a physically crosslinked system, the photo-cured 4-MTM was characterised using modulated DSC (differential scanning calorimetry). The feature of modulated DSC is that it does separate between the reversible and non-reversible heat flow, which represent the thermal transitions, such as glass transition, and chemical changes, respectively. It was revealed that there was non-reversible "kinetic” component starting at 127 °C, which is in the temperature range used to investigate the [2+2] cycloreversion. In addition, there was reversible transition at 174 °C, which is the glass transition temperature. The assumption to what had happened in the experiment of placing the joined glass slides adhered by a 4- MTM layer in the oven was that the [2+2] cycloreversion had taken placed and some regions of the layer had gained some fluid characteristic due to the loss of crosslinking density, which had led to the glass transition temperature and the loss of the 4-MTM layer strength.

[0211] Referring now to Figure 19, there is shown a graph showing the results of tensile stress testing of the 3-MTM and 4-MTM samples. Tensile stress test is performed using an Instron servohydraulic machine, type 8872, with a 25kN load cell and running Instron Bluehill3 software. The difference in the load resistance between the uncured and cured glass adhesion samples is shown. The Y-axis represents the load applied by the instrument and the X-axis represents the extension of the layer during the test. Figure 19 also shows two photographs illustrating the joined glass slides at the start (A) and end (B) of the test.

[0212] Tensile stress measurements were carried out to quantitatively analyse the load that 3- MTM and 4-MTM samples could hold. This determines the breakage point where the photocured layer loses the resistance against the load applied to it.

[0213] Glass slides joined by the uncured 3-MTM and 4-MTM were tested as reference of physical adhesion. The test revealed that the uncured layers did not show any resistance against the load, with a continuous extension until 5 mm. The maximum load recorded for both uncured layers was 0.8 N, which might be attributed to the viscosity of the samples. On the other hand, the photo-cured layers were holding a load up to 320 N when the breakage point was reached for both samples. Moreover, the extension recorded for both was found to be 0.7-0.8 mm. In comparison to the uncured reference test sample, the exposure of the layers to the UV light thus led to highly strong and adhesive materials due to the photochemical [2+2] cycloaddition of MTMs. Referring now to Figure 20, there is shown photographs illustrating experiments wherein samples of cured 3-MTM underwent three cycles of scratch and heal processes using UV light (365 nm, 15 mW) and a heat gun.

[0214] This experiment was performed to investigate whether the 3-MTM material would heal from the scratches using multiple irradiation and heat cycles. A drop of 3-MTM sample was squeezed forming a circle with 14-15 mm diameter and subsequently irradiated for 1 hour to induce covalent crosslinking. The sample layer was a rigid rather than highly viscous liquid, indicating that the photo-curing had occurred. The sample layer was then scratched and heated using the heat gun for approximately 1-2 minutes. The scratches disappeared and the layer became a liquid. Then, the sample was re-irradiated for the second time for 20 minutes. The sample layer was found to have the same texture as the previous irradiation cycle with a complete disappearance of the scratches being noted. This process was repeated three times and similar results were obtained. In each heat / irradiation step, the scratches disappeared and the initially covered area of the glass was re-obtained with a rigid texture as the first irradiation cycle.

[0215] Referring now to Figure 21 , there is shown a schematic illustration of the healing properties of materials, e.g. polymers, according to the invention.

[0216] 4. Synthesis of hydroxyl-functional monothiomaleimide and 2+2 cycloadduct thereof.

[0217] N-propylbromomaleimide (3.86 g, 17.7 mmol, 1 eq.) and sodium acetate (1.46 g, 17.7 mmol, 1 eq.) were dissolved in methanol (70 mL) and stirred at -78°C. 2-Mercaptoethanol (1.1 mL, 11.8 mmol, 0.6 eq.) was added dropwise and the reaction was left stirring for 30 minutes. The solvent was removed in vacuo and the crude product was purified by flash chromatography (7:3 petroleum ether to ethyl acetate) to give the alcohol-functionalised monothiomaleimide 3-((2-hydroxyethyl)thio)-1-propyl-1 H-pyrrole-2, 5-dione. The resulting monothiomaleimide was dissolved in a minimum amount of methanol and irradiated at 365 nm using an LED array for 5.5 hours. Solvent removal in vacuo gave the divalent alcohol 2+2 cycloadduct as a yellow oil (2.18 g - 43 %).1H NMR (500 MHz, CDCh): 6 (ppm) = 3.8 (CH2OH, m, 4H), 3.6 (NCH2, m, 4H), 3.5 (CSCH, m, 2H), 3.1 (SCH2, m, 4H), 1.7 (CH2CH3, m, 4H), 0.7 (CH3, m, 6H).13C NMR (125 MHz, CDCh): 6 (ppm) = 173 (C=OCS), 172 (C=OCH), 62 (COH), 55 (CSCH2), 45 (CSCH), 42 (NCH2), 35 (SCH2), 21 (CH2CH3), 12 (CH3). LC-MS (m / z): 453.0 [M+Na]+. HR-ESI-MS (m / z): calc.: 453.1118, found: 453.1124 [M+Na]+.

[0218] 5. Additional model compounds i. Synthesis of 3-(hexylthio)-1-phenyl-1 / 7-pyrrole-2, 5-dione

[0219] With reference to Figure 22a, to a solution of bromomaleic anhydride (500) (5.94 g, 33.6 mmol) in acetic acid (250 mL), 1 molar equivalent of aniline (3.13 g, 33.6 mmol) was added dropwise at 130°C. The reaction mixture was stirred at 130°C overnight. The reaction mixture was allowed to cool before the acetic acid was removed by an azeotropic distillation with toluene (3 x 100 mL) to obtain a brown solid. Impurities were removed by dissolving and filtering in methanol (3 x 50 mL), and subsequently, solvent was removed under reduced pressure and the precipitate isolated by filtration to yield 3-bromo-1-phenyl-1 / 7- pyrrole-2, 5-dione (501) (4.2 g, 14.5 mmol) as an off-white powder with a 62.1% yield.

[0220] 1H NMR (400 MHz, DMSO): bH (ppm) 7.59 - 7.64 (s, 1 H), 7.46 - 7.55 (m, 2H), 7.38 - 7.45 (m, 1 H), 7.31 - 7.39 (m, 2H).13C NMR (100 MHz, DMSO): bC (ppm) 126.97, 128.11 , 128.91 , 130.82, 131.44, 162.01 , 164.67, 167.87. MS (m / z) 251.96 ([M + H]+), 273.95 ([M + Na]+), 283.99 ([M + CH3OH + H]+), 305.97 ([M + CH3OH + Na]+).

[0221] Subsequently, to a solution of 3-bromo-1-phenyl-1 / 7-pyrrole-2, 5-dione (501) (300 mg, 1.69 mmol) and sodium acetate (138 mg, 1.7 mmol) in methanol (100 mL) was added 1- hexanethiol (237 pL, 1.69 mmol). After 5 minutes the solvent was removed in vacuo and the sample purified by flash chromatography (30% ethyl acetate in petroleum ether) to provide 3-(hexylthio)-1-phenyl-1 / 7-pyrrole-2, 5-dione (510) as a brown-orange oil (362 mg, 1.42 mmol) with an 84% yield.

[0222] 1H NMR (400 MHz, CDCI3): bH (ppm) 5.99 - 6.07 (s, 1 H), 3.44 - 3.51 (t, 2H, J = 7.35 Hz), 2.86 - 2.94 (t, 2H, J = 7.48 Hz), 1 .69 - 1 .80 (quint., 2H, J = 7.57 Hz), 1.55 - 1 .68 (m, 2H), 1.40 - 1.51 (m, 2H), 1.24 - 1.39 (m, 4H), 0.83 - 0.96 (m, 6H).13C NMR (100 MHz, CDCI3): bC (ppm) 11.20, 13.96, 21.87, 27.69, 31.80, 39.75, 117.09, 151.47, 168.11 , 169.88. FTIR (cm’1) 1274-1381 (C-N, amine), 1509-1576 (C=C, alkene), 1584-1736 (C=O, lactam), 2788- 3026 (C-H, aliphatic). MS (m / z) 278.1 ([M + Na]+). ii. Synthesis of methyl 4-(3-(hexylthio)-2,5-dioxo-2,5-dihydro-1 H-pyrrol-1- yl) benzoate

[0223] With reference to Figure 22b, to a solution of bromomaleic anhydride (500) (10 g, 56.8 mmol) in acetic acid (250 mL), 1 molar equivalent of methyl 4-aminobenzoate (8.58 g, 56.8 mmol) was added dropwise at 130°C. The reaction mixture was stirred at 130°C overnight. The reaction mixture was allowed to cool before the acetic acid was removed by an azeotropic distillation with toluene (3 x 100 mL) to obtain a brown solid. Impurities were removed by dissolving and filtering in methanol (3 x 50 mL), and subsequently, the solvent was removed under reduced pressure. The precipitate was isolated by filtration to yield methyl 4-(3- bromo-2,5-dioxo-2,5-dihydro-1 / 7-pyrrol-1-yl)benzoate (502) (7.46 g, 24.1 mmol) as a yellow powder with 25.6% yield.

[0224] 1H NMR (400 MHz, DMSO): bH (ppm) 8.05 - 8.11 (d, 2H, JHH = 8.95 Hz), 7.63 - 7.67 (s, 1 H), 7.51 - 7.58 (d, 2H JHH = 8.77 Hz), 3.85 - 3.92 (s, 3H).13C NMR (100 MHz, DMSO): bC (ppm) 52.34, 126.46, 128.71 , 129.83, 131.15, 132.84, 135.71 , 164.34, 165.63, 167.49. MS (m / z) 331.95 ([M + Na]+), 341.99 ([M + CH3OH + H]+), 363.98 ([M + CH3OH + Na]+).

[0225] To a solution of methyl 4-(3- bromo-2,5-dioxo-2,5-dihydro-1 / 7-pyrrol-1-yl)benzoate (502) (0.5 g, 1.6 mmol) and sodium acetate (0.3 g, 3.2 mmol) in methanol (250mL) was added 1- hexanethiol (0.2 mL, 1.6 mmol). The reaction was stirred at 60°C for 2 hours, after which the reaction was allowed to cool to room temperature, and the product was isolated by filtration to provide methyl 4-(3-(hexylthio)-2,5-dioxo-2,5-dihydro-1 / 7-pyrrol-1-yl)benzoate (520) as an orange powder (0.2 g, 0.6 mmol) with 36.0% yield.

[0226] 1H NMR (400 MHz, DMSO): bH (ppm) 7.98 - 8.12 (d, 2H, JHH = 8.40 Hz), 7.50 - 7.58 (d, 2H, JHH = 8.60 Hz), 6.75 - 6.81 (s, 1 H), 3.81 - 3.93 (s, 3H), 3.03 - 3.14 (t, 2H, JHH = 7.28 Hz), 1.64 - 1.76 (qui, 2H, JHH = 7.38 Hz), 1.36 - 1.49 (m, 2H), 1.22 - 1.36 (m, 4H), 0.81 - 0.95 (m, 3H).13C NMR (100 MHz, DMSO): bC (ppm) 13.86, 21.96, 27.80, 30.67, 30.93, 52.26, 62.00, 126.13, 129.72, 145.98, 165.92, 167.85. FTIR (cm’1) 1215-1323 (C-O, aromatic ester), 1520-1587 (C=C, aromatic), 1587-1617 (C=C, alkene), 1028-1133 (C-N, amine), 1617-1751 (C=O, lactam), 1848-1994 (C-H, aromatic), 2765-3056 (C-H, aliphatic). MS (m / z) 370.1 ([M + Na]+), 371.1 ([M + H + Na]+), 372.1 ([M + D + Na]+). iii. Synthesis of 3-(hexylthio)-1-(4-methoxyphenyl)-1 / 7-pyrrole-2, 5-dione

[0227] With reference to Figure 22c, to a solution of bromomaleic anhydride (500) (8 g, 45.2 mmol) in acetic acid (250 mL), 1 molar equivalent of p-anisidine (5.62 g, 45.2 mmol) was added dropwise at 130°C. The reaction mixture was stirred at 130°C overnight. The reaction mixture was allowed to cool before the acetic acid was removed by an azeotropic distillation with toluene (3 x 100 mL) to obtain a brown solid. Impurities were removed by dissolving in methanol (3 x 50 mL), and subsequently, solvent was removed under reduced pressure and the precipitate was isolated by filtration to yield 3-bromo-1-(4- methoxyphenyl)-1 / 7-pyrrole- 2,5-dione (503) (3.6g, 11.3mmol) as a yellow powder with 25.0% yield.

[0228] 1H NMR (400 MHz, DMSO): bH (ppm) 7.55 - 7.62 (s, 1 H), 7.22 - 7.29 (d, 2H, JHH = 8.96 Hz), 7.00 - 7.06 (m, 2H, JHH = 8.95 Hz), 3.75 - 3.82 (s, 3H).13C NMR (100 MHz, DMSO): bC (ppm) 55.37, 114.18, 123.92, 128.51 , 130.70, 132.60, 158.90, 164.90, 168.13. MS (m / z) 303.96 ([M + Na]+).

[0229] To a solution of 3-bromo-1-(4-methoxyphenyl)-1 / 7-pyrrole- 2,5-dione (503) (3 g, 10.7 mmol) and sodium acetate (0.9 g, 10.7 mmol) in methanol (250 mL) was added 1 -hexanethiol (1.5 mL, 10.7 mmol). The reaction was stirred at 60°C for 2 hours, after which the reaction was allowed to cool to room temperature, and the product was isolated by filtration to afford 3- (hexylthio)-1-(4-methoxyphenyl)-1 / 7-pyrrole-2, 5-dione (530) as a bright green crystal (2.1 g, 6.4 mmol) with 60.6% yield.

[0230] 1H NMR (400 MHz, DMSO): bH (ppm) 7.20 - 7.30 (d, 2H, JHH = 9.43 Hz), 6.99 - 7.06 (d, 2H, JHH = 8.95 Hz), 6.67 - 6.73 (s, 1 H), 3.74 - 3.85 (s, 3H), 3.01 - 3.14 (t, 2H, JHH = 7.38 Hz), 1.63 - 1.76 (qui, 2H, JHH = 7.42 Hz), 1.37 - 1.49 (m, 2H), 1.22 - 1.36 (m, 4H), 0.82 - 0.94 (m, 3H).13C NMR (100 MHz, DMSO): bC (ppm) 13.87, 21.96, 27.39, 27.81 , 30.67, 30.85, 55.34, 114.11 , 118.39, 128.32, 150.49, 158.66. FTIR (cm’1) 1259-1271 (C-O, alkyl aryl ether), 1271-1338 (C-N, amine), 1584-1647 (C=C, aromatic), 2743-3045 (C-H, aliphatic). MS (m / z) 342.1 ([M + Na]+). iv. Photodimer formation

[0231] With reference to Figure 23, a 49 mM solution of 3-(hexylthio)-1-phenyl-1 / 7-pyrrole-2,5- dione (510) (14.2 mg, 49 nmol) in DMSO-d6 (1 mL) was placed 3 cm from a Lumidox® II LED source at 365 nm. The power was set to 95 mW / cell and the sample was irradiated for the given amount of time to form 3a,3b-bis(hexylthio)-2,5- diphenyltetrahydrocyclobuta[1 ,2- c:3,4-c']dipyrrole-1 ,3,4,6(2H,5H)-tetraone (511). Conversion was measured using 1 H NMR. Figure 23 shows the 1 H NMR spectra recorded during the photodimerisation of 3- (hexylthio)-1-phenyl-1 H-pyrrole-2, 5-dione under 365 nm irradiation.1H N MR (400 MHz, DMSO): 6H (ppm) 7.55 - 7.63 (m, 4H), 7.49 - 7.55 (m, 2H), 7.36 - 7.42 (m, 4H), 3.89 - 3.94 (s, 2H), 3.00 - 3.12 (dt, 2H, JHH = 7.63 Hz), 2.75 - 2.85 (dt, 2H, J = 7.63 Hz), 1.42 - 1.53 (m, 4H), 1.12 - 1.42 (m, 12H), 0.72 - 0.94 (m, 6H).

[0232] With reference to Figure 24, a 49 mM solution of methyl 4-(3-(hexylthio)-2,5-dioxo-2,5- dihydro-1 H-pyrrol-1-yl)benzoate (520) (17.0 mg, 49 nmol) in DMSO-d6 (1 mL) was placed 3 cm from a Lumidox® II LED array at 365 nm. The power was then set to 95 mW / cell and the sample was irradiated for the given amount of time to afford dimethyl 4,4'-(3a,3b- bis(hexylthio)-1 ,3,4,6-tetraoxooctahydrocyclobuta[1 ,2-c:3,4-c']dipyrrole-2,5- diyl)dibenzoate, and conversion was measured using 1 H NMR. Figure 24 shows the 1 H NMR spectra recorded during the photodimerisation of methyl 4-(3-(hexylthio)-2,5-dioxo-

[0233] 2.5-dihydro-1 H-pyrrol-1-yl)benzoate (521) under 365 nm irradiation.

[0234] 1H NMR (400 MHz, DMSO): 5H (ppm) 8.13 - 8.21 (d, 4H, JHH = 8.72 Hz), 7.57 - 7.63 (d, 4H, JHH = 8.69 Hz), 3.96 - 4.00 (s, 2H), 3.89 - 3.93 (s, 6H), 3.00 - 3.14 (m, 2H), 2.75 - 2.86 (dt, 2H, JHH = 7.16 Hz), 1.41 - 1.52 (m, 4H), 1.14 - 1.35 (m, 12H), 0.75 - 0.92 (m, 6H).

[0235] With reference to Figure 25, a 49 mM solution of 3-(hexylthio)-1-(4-methoxyphenyl)-1 / 7- pyrrole-2, 5-dione (530) (15.6 mg, 49 nmol) in DMSO-d6 (1 mL) was placed 3 cm from a Lumidox® II LED array at 365 nm. The power was then set to 95 mW / cell and the sample was irradiated for the given amount of time to afford 3a,3b-bis(hexylthio)-2,5-bis(4- methoxyphenyl) tetrahydrocyclobuta[1 ,2-c:3,4-c']dipyrrole-1 ,3,4,6(2H,5H)-tetraone (531). Conversion was measured using 1 H NMR. Figure 25 shows the 1 H NMR spectra recorded during the photodimerisation of 3-(hexylthio)-1-(4-methoxyphenyl)-1 H-pyrrole-2, 5-dione under 365 nm irradiation.

[0236] 1H NMR (400 MHz, DMSO): 5H (ppm) 7.26 - 7.32 (d, 4H, JHH = 8.93 Hz), 7.08 - 7.14 (d, 4H, JHH = 9.05 Hz), 3.83 - 3.86 (s, 2H), 3.80 - 3.83 (s, 6H), 3.00 - 3.11 (m, 2H), 2.73 - 2.83 (m, 2H), 1.41 - 1.51 (m, 4H), 1.14 - 1.40 (m, 12H), 0.77 - 0.93 (m, 6H).

[0237] Figures 26a and 26b show the photodimerisation kinetics of 49 mM solutions (in DMSO-ds) of 3-(hexylthio)-1-phenyl-1 / 7-pyrrole-2, 5-dione (510), methyl 4-(3-(hexylthio)-2,5-dioxo-2,5- dihydro-1 H-pyrrol-1-yl)benzoate (520), and 3-(hexylthio)-1-(4-methoxyphenyl)-1 H-pyrrole-

[0238] 2.5-dione (530). Figure 26a shows the reaction under 365 nm irradiation (68.5 mW cm-2) and Figure 26b shows the same reaction under 405 nm irradiation (80 mW cm-2). Figures 27a, 27b, and 27c show the thermal cycloreversion kinetics at 155°C, at 140°C and at 125°C respectively of 25 mM solutions (in DMSO-d6) of the photodimer derivatives of 3- (hexylthio)-1-propyl-1 H-pyrrole-2, 5-dione (101), 3-(hexylthio)-1-phenyl-1 H-pyrrole-2, 5- dione (510), methyl 4-(3-(hexylthio)-2,5-dioxo-2,5-dihydro-1 H-pyrrol-1-yl)benzoate (520), and 3-(hexylthio)-1-(4-methoxyphenyl)-1 H-pyrrole-2, 5-dione (530)

[0239] 6. Multi-functional thiomaleimide compounds a. Synthesis i. “Thiocure 333-modified thiomaleimide” (MTM-TC333)

[0240] N-propyl-3-bromomaleimide (10.06g, 46 mmol, 4.5 eq.) and sodium acetate (3.84g, 47 mmol, 4.5 eq.) was dissolved in 200 mL MeOH. Thiocure® 333 (13.61g, 10 mmol, 1 eq.) was diluted in MeOH (20 mL) and slowly dropped into the prepared monobromomaleimide solution. The reaction was performed under ambient temperature with stirring for 30 min. The solvent was removed in vacuo. The dark oil obtained was dissolved in 200 mL DCM and washed with 100 mL water for 4 times. The organic phase was collected and solvent was removed in vacuo. The crude product was dissolved in minimum amount of acetone and precipitated in cold isopropanol. MTM-TC333 was collected as a brown liquid (13.6 g, 80 %). 1 H NMR (400 MHz, CDCI3): 5 (ppm) 0.77-0.95 (m, 12H), 1.40 (m, 2H), 1.61 (sext, 6H), 2.79 (t, J = 7.2 Hz, 6H), 3.20 (t, J = 7.2 Hz, 6H), 3.31 (m, 6H), 3.47 (t, J = 7.2 Hz, 6H), 3.51-3.76 (m, 80H), 4.29 (m, 6H), 6.12 (s, 3H). DSC: Tg = -42 °C. ii. Synthesis of “Dioxyl 2-arm MTM”

[0241] N-propyl-3-bromomaleimide (5.00g, 22.93 mmol, 3 eq.) and sodium acetate (1.88g, 22.93 mmol, 3 eq.) were dissolved in 85 mL methanol. 2,2'-(ethylenedioxy)diethanethiol (1.39g, 7.64 mmol, 1 eq.) was mixed with 5 mL methanol and added dropwise into the reaction system while stirring. The reaction was performed at room temperature for 30 minutes. Subsequently, the solvent was removed under reduced pressure and the crude resultant was dissolved in 100 mL dichloromethane (DCM) and washed with 100 mL deionised water for 3 times. The DCM fraction was collected and the solvent was removed under reduced pressure. Minimum amount of acetone was added, and the solid product precipitated in cold isopropanol (I PA) and more crystal product precipitated out after being left overnight at room temperature. The final product (3.1 g) was collected and dried in a vacuum oven with a yield of 83%.1H NMR (400 MHz, CDCh) 5 (ppm) 0.90 (6H, t, J = 7.5 Hz), 1.57-1.66 (4H, m, J = 7.3 Hz), 3.15 (4H, t, J = 6.2 Hz), 3.48 (4H, t, J = 7.3 Hz), 3.66 (4H, s), 3.80 (4H, t, J = 6.2 Hz), 6.16 (2H, s).13C NMR (100MHz, CDCh) 11.17, 21.83, 31.68, 39.76, 68.64, 70.63, 117.84, 150.69, 167.97, 169.72 HR-ESI-MS [M+Na]+m / z 479.1279 iii. Synthesis of “Glycol 2-arm MTM”

[0242] N-propyl-3-bromomaleimide (5.00g, 22.93 mmol, 3 eq.) and sodium acetate (1.88g, 22.93 mmol, 3 eq.) were dissolved in 85 mL methanol. Ethylene glycol bis(3-mercaptopropionate) (1.82g, 7.64 mmol, 1 eq.) was mixed with 5 mL methanol and added dropwise to the bromomaleimide solution while stirring. The reaction was performed at room temperature for 30 minutes. An off-white powder precipitated out from the solution, which was collected by filtration. Subsequently, the product was washed with methanol then dried in a vacuum oven. 3.3 g of “glycol 2-arm MTM” was obtained as a powder with a yield of 85 %.1H NMR (400 MHz, CDCh) 5 (ppm) 0.9 (6H, t, J = 7.4 Hz), 1.57-1.66 (4H, m, J = 7.3 Hz), 2.81 (4H, t, J = 7 Hz), 3.22 (4H, t, J = 7 Hz), 3.48 (4H, t, J = 7.2 Hz), 4.37 (4H, s), 6.14 (2H, s).13C NMR (100 MHz, CDCh) 11.17, 21.82, 26.20, 32.51 , 39.83, 62.62, 149.93, 167.82, 169.46, 170.48 [M+Na]+m / z 535.1174 iv. Synthesis of Isocyanurate-derived thiomaleimide (“isocyanurate 3-arm MTM”)

[0243] N-propyl-3-bromomaleimide (5.00g, 22.93 mmol, 4.5 eq.) and sodium acetate (1.88g, 22.93 mmol, 4.5 eq.) were dissolved in 85 mL methanol. Tris[2-(3-mercaptopropionyloxy)ethyl] isocyanurate (2.68g, 5.10 mmol, 1 eq.) was mixed with 5 mL methanol and added dropwise into the bromomaleimide solution under fast stirring. The reaction was set up at room temperature and reacted for 30 minutes. Brown viscous product formed at the bottom of the reaction flask. The solvent was decanted carefully and the resisdue was washed with isopropanol. The product was dried in a vacuum oven to give 4.03 g of isocyanurate 3-arm MTM as a yellow brown viscous liquid (yield of 84%).1H NMR (400 MHz, CDCh) 6 (ppm) 0.9 (9H, t, J = 7.4 Hz), 1.56-1.66 (6H, m), 2.73 (6H, t, J = 7.2 Hz), 3.18 (6H, t, J = 7.2 Hz), 3.46 (6H, t, 7.2 Hz), 4.21 (6H, m), 4.39 (6H, m), 6.16 (3H, s).13C NMR (100MHz, CDCh) 11.5, 21.80, 26.02, 32.43, 39.80, 42.18, 61.90, 117.70, 149.02, 150.00, 167.82, 169.51 , 170.74 [M+Na]+m / z 959.2237 b. Reversible (de)polymerisation and (de)crosslinking of i. Thiocure 333-modified thiomaleimide (MTM-TC333)

[0244] The MTM-TC333 was dropped on a glass slide and irradiated from the bottom with a Lumidox II® 365 nm UV-light (95 mW / well) for 60 min to give a crosslinked material. DSC: Tg = -34 °C.

[0245] A solution of MTM-TC333 in DMSO-d6 was prepared in an NMR tube. The solution was then irradiated with 365 nm UV LED light (Lumidox® II array, 45 mW / well) and1H NMR spectra were recorded every 5 minutes. As shown in Figure 28b and 28c, the 1 H NMR resonance peak at 6.56 ppm completely disappeared after exposing for approximately 40 min, representing the full conversion of MTM-TC333 from monomeric into photodimer product. The thermal cycloreversion of the MTM-TC333 photodimer was investigated by placing the test tube in a pre-heated oil bath (160°C). A 1 H NMR spectrum was recorded every 5 minutes. The intense singlet at 6.56 ppm referring to maleimide C=CH reappeared, indicative for the successful reversion and reformation of the dioxyl 2-arm MTM. As shown in Figure 28c, after approximately 35 minutes, the polymeric signals reduced with over 99% of starting thiomaleimide monomer being re-formed.

[0246] Figure 28a shows the photo-rheology of MTM-TC333 during irradiation with an Omnicure S2000 broad emitting lamp with bandpass filter A = 320-390 nm. ii. Reversible (de)polymerisation and (de)crosslinking of Dioxyl 2-arm MTM

[0247] A solution of dioxyl 2-arm MTM (50mM) in DMSO-d6 was prepared in an NMR tube. The solution was then irradiated with 365 nm UV LED light and 1 H NMR spectra were recorded every 30 minutes. The colour of the solution changed from colourless to light brown during UV irradiation. As shown in Figure 29a, the 1 H NMR resonance peak at 6.56 ppm completely disappeared after exposing for 120 min, representing the full conversion of dioxyl 2-arm MTM from monomeric into photodimer product. The thermal cycloreversion of the dioxyl 2-arm MTM photodimer was investigated by placing the test tube in a pre-heated oil bath (160°C). A 1 H NMR spectrum was recorded after 1 and 2 h of heating, as shown in Figure 29b. The bottom spectrum of Figure 29b shows the spectrum of the photodimer formed after 150 minutes of 365nm irradiation. The intense singlet at 6.56 ppm referring to maleimide C=CH reappeared, indicative for the successful reversion and reformation of the dioxyl 2-arm MTM. After 1 hour, approximately 87% cycloreversion occurred. Later, at 2 h, the polymeric signals reduced with over 99% of starting thiomaleimide monomer being reformed. iii. Reversible (de)polymerisation and (de)crosslinking of Glycol 2-arm MTM

[0248] A solution of glycol 2-arm MTM (50mM) in DMSO-de was prepared in an NMR tube. The solution was then irradiated with 365 nm UV LED light and1H NMR spectra were recorded every 30 minutes. As shown in Figure 30a, full conversion into the [2+2] photo-cycloaddition product was observed after exposure under 365 nm UV light for 120 minutes.

[0249] The thermal cycloreversion of the glycol 2-arm MTM photodimer was carried out at 160 °C in a pre-heated oil bath. The bottom spectrum of Figure 30b shows the spectrum of the photodimer formed after 150 minutes of 365nm irradiation. 89% of the monomeric starting glycol 2-arm MTM compound was re-generated after heating for 1 h, and over 96% reversion was achieved after 2h heating. iv. Reversible (de)polymerisation and (de)crosslinking of Isocyanurate-derived thiomaleimide (isocyanurate 3-arm MTM)

[0250] A solution of isocyanurate 3-arm MTM in DMSO-d6 was prepared in an NMR tube. The solution was then irradiated with 365 nm UV LED light and 1 H NMR spectra were recorded every 30 minutes. As shown in Figure 31a, full conversion into the [2+2] photo-cycloaddition product was observed after exposure under 365 nm UV light for 120 minutes.

[0251] The thermal cycloreversion of isocyanurate 3-arm MTM photodimers was carried out at 160 °C in a pre-heated oil bath. The bottom spectrum of Figure 31b shows the spectrum of the photodimer formed after 150 minutes of 365nm irradiation. The cycloreversion was fully completed after 2h, with minor product degradation found that can be attributed to the isocyanate trimer core.

[0252] 7. Functional Thiomaleimide Compounds a. Synthesis i. Hydroxyl-containing Thiomaleimide, ‘Hydroxy-MTM’:

[0253] N-propyl-3-bromomaleimide (11 .21 g, 51 mmol, 1 eq.) was dissolved in methanol (150 mL). Sodium acetate (NaOAc) (2.65 g, 32 mmol, 0.63 eq.) was added into the solution while stirring. When all solids were fully dissolved, the dark-brown solution was purged by nitrogen for 15 min. Afterwards, the solution was placed in an ice-bath while stirring, and 2- mercaptoethanol (4 mL, 56 mmol, 1.01 eq.) was added in dropwise. After 2h, the solution was removed from the ice bath and left to stir overnight at room temperature. The resulting mixture was evaporated in vacuo and the obtained crude dark brown oil was purified by column chromatography (silica, 30 % ethyl acetate and 70 % petroleum ether) to give the Hydroxy-MTM as a dark-red oil with 65 % yield (7.14 g, 33 mmol).

[0254] 1 H NMR (400 MHz, CDCI3): 5 (ppm) = 6.16 (s, 1 H), 3.95 (t, 2H), 3.47 (t, 2H), 3.15 (t, 2H), 1.61 (t, 2H), 0.89 (t, 3H). 13C NMR (100 MHz, CDCI3): 5 (ppm) = 169.7, 168.0, 150.4, 118.0, 60.0, 39.8, 34.4, 21.8, 11.2. ii. Di-hydroxyl-containing TM 1 :

[0255] Hydroxy-MTM (1.01 g, 4 mmol) was dissolved in methanol (20 mL) to produce a yellow-red solution. The solution was placed 1 cm away from a 365 nm Lumidox II LED array (95 mW / well) and irradiated for 3 h, which resulted in a yellow solution. The solvent was removed in vacuo to give the di-hydroxyl-containing TM-1 as a dark yellow oil (1.00 g, 2 mmol) with 100 % conversion of the hydroxy-MTM. Figure 32a shows the 1 H NMR spectra (400 MHz, DMSO-d6) recorded during the photodimerization indicating the full conversion to the photodimer. Figure 32b shows the conversion of the Hydroxy-MTM against time. The experimentally observed rate coefficient was kObs = 0.29 min-1and the half-life time was ti / 2 = 2.4 min. Photodimerization was also carried out successfully using 405 nm (110 mW / well) LED irradiation with a similar time required for complete reaction.

[0256] 1 H-NMR (500 MHz, CDCI3): 5 (ppm) = 4.01 - 3.69 (m, 4H), 3.65 - 3.50 (m, 4H), 3.50 - 3.45 (m, 2H), 3.14 - 2.02 (m, 6H), 2.22 (broad s, 2H), 1.77 - 1.45 (m, 4H), 1.03 - 0.80 (m, 6H). 13C-NMR (125 MHz, CDCI3): 5 (ppm) = 173.08, 172.84, 61.44, 54.97, 45.35, 41.60, 34.62, 20.89, 11.30. LR-ESI-MS (m / z): 453.0 [M+Na]+. HR-ESI-MS (m / z): calc.: 453.1118, found: 453.1124 [M+Na]+. iii. Di-hydroxyl-containing TM 2:

[0257] To a solution of N-propyl-3-bromomaleimide (0.15 g, 0.7 mmol, 1 eq.) in methanol (14 mL), NaOAc (0.7 mmol, 1 eq.) was added followed by 1 -thioglycerol (59 pL, 0.7 mmol, 1 eq.). The reaction was stirred at room temperature for ca. 17 hours before the solvent was removed in vacuo. The reaction mixture was dried in vacuo and the crude Di-hydroxyl- containing TM-2 product purified by flash column chromatography (silica; EtOAc 100%). LR-ESI-MS (m / z): 268.0 [M+Na]+. Table 3 below shows the experimentally derived kinetics of the thermal reversion of the dimers (i.e. formed after irradiation). kObs is the observed rate coefficient of thermal reversion; ti / 2 is the half life time in hours. Figure 33a shows the 1 H NMR spectra (400 MHz, DMSO-d6) recorded during the thermal cycloreversion of Hydroxy-TM2 photodimer at 160

[0258] °C. Figure 33b shows the thermal cycloreversion kinetics of Hydroxy-TM2 photodimer (0.03

[0259] M, DMSO-d6) at 160, 140 and 120 °C, determined by 1 H NMR.

[0260] Table 3

[0261] 8. Thiomaleimide crosslinker compounds a. Synthesis i. TM crosslinker 1 :

[0262] Di-hydroxyl-containing TM-1 (1.1 g, 2.6 mmol, 1 eq.), 2,2,5-trimethyl-1 ,3-dioxane-5- carboxylic acid (0.98 g, 5.6 mmol, 2.2 eq.) and 4-Dimethylaminopyridine (0.25 g, 2.0 mmol, 0.77 eq.) were dissolved in dichloromethane (50 mL) and placed under a nitrogen atmosphere at room temperature. To this, a solution of N,N'-dicyclohexylcarbodiimide (1.32 g, 6.40 mmol, 2.5 eq.) in dichloromethane (10 mL) was added dropwise. The reaction was left to stir for 4 days before it was concentrated in vacuo and the salts were filtered off. The resulting filtrate was diluted with dichloromethane (40 mL), washed with deionised water (2 x 20 mL) and dried over MgSO4. The solvent was removed in vacuo and the product was purified by flash chromatography (SiO2; dichloromethane:methanol - 95:5) to give ((1 ,3,4,6-tetraoxo-2,5-dipropyloctahydrocyclobuta[1 ,2-c:3,4-c']dipyrrole-3a,3b- diyl)bis(sulfanediyl))bis(ethane-2,1-diyl) bis(2,2,5-trimethyl-1 ,3-dioxane-5-carboxylate) (0.28 g - 15 %). LR-ESI-MS (m / z): 765.2 [M+Na]+.

[0263] To ((1 ,3,4,6-tetraoxo-2,5-dipropyloctahydrocyclobuta[1 ,2-c:3,4-c']dipyrrole-3a,3b- diyl)bis(sulfanediyl))bis(ethane-2,1-diyl) bis(2,2,5-trimethyl-1 ,3-dioxane-5-carboxylate) (0.28 g, 1 eq.) was added THF (10 mL) and HCI (1M, 1 mL). The reaction mixture was stirred at room temperature overnight and the formation of the target product was monitored by ESI-MS. Dichloromethane (10 mL) was added to the reaction mixture and the resulting mixture was washed with deionised water (6 mL) followed by sodium bicarbonate solution (4 mL) and brine (10 mL). Solvent removal in vacuo resulted in a crude mixture containing the TM crosslinker 1. LR-ESI-MS (m / z): 685.2 [M+Na]+. ii. TM crosslinker 2:

[0264] Di-hydroxyl-containing TM-1 (3.61 g, 8 mmol, 1 eq.) was dissolved into dichloromethane (70 mL). Triethylamine (TEA) (4.48 g, 42 mmol, 1 eq.) was added and the resulting dark solution obtained was purged by nitrogen for 15 min. The solution was cooled in an icebath and acryloyl chloride (3.62g, 40 mmol, 5 eq.) was slowly added dropwise. The ice-bath was removed, and the orange-red solution was allowed to be stir overnight at room temperature. 30 mL of water was added to quench the reaction. The solution was washed with saturated sodium hydrogen bicarbonate (NaHCCh) until the aqueous phase turned colourless. The organic phase was separated and dried in vacuo. The crude product was purified by column chromatography (silica, 40 % ethyl acetate and 60 % petroleum ether, RF (40 % ethyl acetate: 60 % petroleum ether) = 0.7) to give the diacrylate TM crosslinker 2 (3.02 g, 6 mmol) as an orange oil in 75 % yield.

[0265] 1 H NMR (500 MHz, CDCb) 6 6.42 (dd, J=17.4, 2H), 6.09 (dd, J=17.3 Hz, 2H), 5.85 (dd, J=10.5 Hz, 2H), 4.33 (m, 4H), 3.57 (t, =7.4 Hz, 4H), 3.48 (dt, J=12.8 Hz, 2H), 3.20 (dt, J=12.9 Hz, 2H), 2.99 (s, 2H), 1.68 (m, =7.4 Hz, 4H), 0.96 (t, =7.5 Hz, 6H); 13C NMR (500 MHz, CDCb) 5 11. 06 (CHs), 20.61 (CH2), 30.09 (CH2), 41.36 (CH), 44.19 (CH2), 54.35 (C- S), 62.35 (CH2), 127.55 (CH2), 130.94 (CH2). 131.19 (CH), 165.36 (C=O), 172.29 (C=O). 172.54 (C=O); MS (ESI) m / z [M+Na+] Calc, for C24H3oNaN208S2561.134; Found m / z 561.1.

[0266] 9. Polyurethane-containinq TM-dimers a.TM-containing polyurethane (PU) synthesis i. PU-TM 1 :

[0267] Hydroxy-MTM2 (0.064 g, 0.149 mmol, -0.1 eq.) was added to a large vial followed by PPG2000 (2.66 g, 1.33 mmol, ~0.9 eq.). The mixture was then stirred under a nitrogen atmosphere before IPDI (0.31 mL, 1.46 mmol, 1 eq.) and DBDTL (ca. 5-6 drops, cat.) were added via syringe. The reaction was heated up to <100 °C and stopped stirring due to high viscosity after ca. 1 hour. Product obtained as a yellow viscous liquid.

[0268] SEC (THF, PMMA Standards): Mn = 6.46 kg mol-1 , D = 2.00. ii. PU-TM 2:

[0269] Hydroxy-MTM2 (0.083 g) was dissolved in anhydrous THF (4 mL) and put under nitrogen, where it was stirred for several hours. To this, IPDI (ca. 0.04 mL) was added via a syringe and then DBTDL (ca. 5 drops, cat.) was added. The mixture was then put under reflux at 700C for an hour and then left open to air to allow volatiles to evaporate. The product was obtained as an orange solid. Figure 34 shows 1 H NMR spectra (400 MHz, DMSO-d6) for PU-TM-2; (A) before heating, (B) after heating (ca. 160 °C, ca. 1 hour), and (C) after irradiating (365 nm, 95 mW well-1 , 2 h), indicative of polymeric de-bonding and re-bonding. SEC (DMF, PMMA Standards): Mn = 920 g mol-1 , D = 2.49 iii. PU-TM 3:

[0270] To PPG2000 / NCO (1.04 g, 0.45 mmol) in a sealed flask was added Hydroxy-MTM2 (193 mg, 0.45 mmol) in anhydrous THF (ca. 3 mL). DBTDL (7-8 drops, cat.) was added and the reaction was stirred at ca. 700C under reflux for ca. 21 hours.

[0271] SEC (THF, PMMA Standards): Mn = 12,300, D = 2.81.

[0272] 10. Recycling of MTM materials:

[0273] Figure 35 shows the reversible crosslinking of 3-arm MTM-TC333 in bulk during consecutive irradiation and heating. The material is initially liquid, then solidifies after 1 hour of irradiation using 365nm UV light. After 1hour of heating at 160°C, the composition is returned to its liquid starting state. A further round of irradiation of the now liquid sample again results in a solid material.

[0274] Figure 36 shows the results of consecutive alternate rounds of irradiation and heating in a reversible gelation experiment of 3-arm MTM. Figure 37 shows the same result is achievable with consecutive alternate rounds of irradiation and heating for a 4-arm MTM.

[0275] These tests shows the intrinsic recyclability of the material, even in the absence of any solvent or additive. These results demonstrate clearly the usefulness of the present invention, especially with respect to the recyclability of the compositions. It would be understood that the reversion of the compound to a low viscosity and / or liquid monomer form permits simple handling and reforming of the compound, thus allowing the compound to be easily re-used for a new purpose. Being able to achieve this in the bulk material (i.e. in the absence of solvents, or even additives and catalysts) reduces the cost and potential environmental impact e.g. compared to a system effective only when in solution, or which requires complex and expensive catalysts.

[0276] In conclusion, it has been shown that: • 3-MTM and 4-MTM compounds according to the invention exhibit thermoreversible [2+2] cycloaddition at different elevated temperatures (e.g. 120, 140, and 160 °C);

[0277] • The rate of the [2+2] cycloreversion reaction of 3-MTM and 4-MTM cycloaddition products depends on the temperature applied and the full conversion to the monomer from its [2+2] cycloaddition product could be obtained;

[0278] • In Comparative Examples of the invention, maleimide photodimers did not revert into the maleimide monomer after heating at 160 °C for 2 hours, and instead, thermal degradation products were formed after 24 hours;

[0279] • The photocured material according to the invention has been shown be capable of holding a load of up to 320 N. Thus, the material according to the invention may be exploited as an adhesive;

[0280] • [2+2] cycloreversion has been demonstrated in bulk. Thus, the material according to the invention may be exploited as a debondable adhesive or in healable surface coatings;

[0281] • Multiple cycles of irradiation for [2+2] cycloaddition, and heating for [2+2] cycloreversion may be performed on the material according to the invention, without significant degradation. Thus, the material according to the invention may be exploited in recyclable applications;

[0282] • The material according to the invention has self-healing properties, as demonstrated by the scratch and heal tests in Figure 20;

[0283] • The thiol and N-imide groups are excellent handles for incorporation of the monothiomaleimide compounds according to the invention in a range of polymer materials (e.g. polyacrylates, polyurethanes, polyisocyanurates). Moreover, these can be exploited for adding more properties and functionality to the polymer. Hence, a library of functional materials can be synthesised with an increased number of properties being introduced in a single polymeric scaffold;

[0284] • The thiomaleimide materials exhibit excellent reversibility and recyclability. They are capable of regenerating the initial monomeric compounds without the need of additives such as catalysts and solvents;

[0285] • The thiomaleimide materials are thermally reversible and the dimers can be formed using irradiation X > 400 nm;

[0286] • The temperature at which the reversion to the monomer / oligomer form is achieved can be tuned through structural modification of the thiomaleimide e.g. through substitution of the thiol and / or N-imide groups. It will also be appreciated by those skilled in the art that any number of combinations of the aforementioned features and / or those shown in the appended drawings provide clear advantages over the prior art and are therefore within the scope of the invention described herein.

Claims

CLAIMS1 . A method for recycling a compound, e.g. a polymer, the method comprising providing a compound, e.g. polymer, the compound, e.g. polymer, comprising a moiety having the general structure (1a) and / or (1 b) or a stereoisomer, enantiomer, racemate, or tautomer thereof:(1a)(1b)wherein R1and R2are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1and / or R2is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl; the method comprising heating the compound, e.g. polymer, to a temperature at or above 35°C to generate oligomers or monomers comprising moieties having the general structures (2a) and (2b):(2a)(2b)wherein R1and R2are defined as above; and at least 50%, e.g. at least 60%, or at least 70%, or at least 80%, or at least 90% of the moieties defined in general structure (1a) and (1 b) are converted into the moieties defined in general structure (2a) and (2b).

2. A method according to Claim 1 , wherein the compound is a polymer.

3. A method according to any preceding Claim, wherein the method comprises repolymerising the oligomers or monomers to form the repolymerised polymer, e.g. in a yield of greater than 90%, for example by irradiating with UV light.

4. A method according to Claim 3, the method further comprising heating the repolymerised polymer, e.g. to a temperature at or above 35°C, e.g. at or above 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100°C, to generate oligomers or monomers comprising moieties having the general structure (2a) and (2b), e.g. in a yield of at least 50%.

5. A method according to any preceding Claim, further comprising performing n cycles (e.g. 1 , 2, 3, 4, 5, or more) of repolymerisation, e.g. by irradiation, followed by depolymerisation by conversion back to oligomers or monomers, e.g. by heating to a temperature of at or above 35°C e.g. above 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100°C.

6. A method according to any preceding Claim, wherein the method comprises heating the compound, e.g. polymer, to a temperature above 105°C, or above 110°C, or above 115°C, or above 120°C, or above 125°C, or above 130°C, or above 135°C, or above 140°C, or above 145°C, or above 150°C, or above 155°C, or above 160°C, to generate oligomers or monomers comprising moieties having the general structures (2a) and (2b).

7. A method according to any preceding Claim, wherein the moieties of the oligomers or monomers having the general structures (2a) and (2b) may be represented by the formulae (2c) and (2d):(2c)(2d)wherein R1and R2are defined as in Claim 1 ; and wherein Racomprises an aliphatic or aromatic group, e.g. an alkyl chain comprising an ester moiety, for example Ramay be selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein Rais optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, C1.6 alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

8. A method according to Claim 7, wherein Racomprises a tertiary or quaternary carbon atom.

9. A method according to Claim 7 or 8, wherein Racomprises a polymer scaffold or chain.

10. A method according to any preceding Claim, wherein Racomprises a further one, two, three, or more, moieties according to the general formulae (2a) and (2b).

11. A method according to any preceding Claim, wherein the monomers have the general structure (3):wherein R1and R2are defined as in Claim 1 ;R3and R4are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R3and / or R4are optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

12. A method according to any preceding Claim, wherein the monomers have the general structure (4):wherein R1, R2, R6are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1, R2, R6is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, C1-6 alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl wherein R5is selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R5is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, ORX, NHRy, NRyRzand Rx, Ry, and Rzare independently selected from H, C1-6 alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

13. A method according to any preceding Claim, wherein the monomers have the general structure (5):(5)wherein R1, R2, R6, R7are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1, R2, R6, R7is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

14. A method according to any of Claims 11 to 13, wherein the oligomers or monomers consist of monomers according to general formulae (3) and / or (4) and / or (5).

15. A polymer comprising a backbone and crosslinked bridges, the backbone comprising plural, e.g. two or more, moieties having the general structure (1a) and / or (1 b) or a stereoisomer, enantiomer, racemate, or tautomer thereof:(1a)(1 b)wherein R1and R2are independently selected from C1-20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1and / or R2is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

16. A polymer according to Claim 15, wherein the backbone of the polymer further comprises an alkyl group, e.g. an alkyl group comprising ester moieties.

17. A polymer according to Claim 15 or 16, wherein the backbone of the polymer chain further comprises the following general structure (6):(6)wherein Rm and R- are independently alkyl groups, e.g. C1-20 alkyl, or hydrocarbon chains comprising heteroatoms, e.g. -CH2O(C=O)CH2CH2-.

18. A polymer according to any of Claims 15 to 17, wherein the crosslinked bridges comprise plural, e.g. two or more, moieties having the general structure (1a) and / or (1 b) or a stereoisomer, enantiomer, racemate, or tautomer thereof, and / or the general structure (6).

19. A monomer, the monomer comprising three or four or more moieties having the following general formula (7) and wherein the molecular weight is less than 3000 gmol’1, or less than 2000 gmol’1, or less than 1500 gmol’1(7)wherein R1is selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1-20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

20. A monomer according to Claim 19, wherein each moiety having the general formula (7) is bonded to a core or hub moiety of the monomer, e.g. wherein the core or hub moiety may comprise a tertiary or quaternary carbon atom, for example bonded to the sulphur atom of one or more moieties having the general formula (7).

21. The monomer of Claim 19 or 20, wherein the monomer comprises the following general structure (11):(11)wherein Rcindependently comprises an aliphatic or aromatic group, for example Rcmay be independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein Rcis optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl;L is a linker group independently comprising or consisting of C1.10 alkylene; C2-10 alkenylene; C2-ioalkynylene or C6-i2aryl, wherein said Ci- 10 alkylene; C2-10 alkenylene; C2-10 alkynylene or Ce-12 aryl optionally comprise one or more heteroatoms within the hydrocarbon chain, wherein said heteroatoms are selected from one or more of O, S and N;H is a core or hub moiety, for example comprising a secondary, tertiary, or quaternary carbon atom; and x is an integer of 3, 4, or more.

22. In embodiments, the linker group (L) comprises an ester moiety, e.g. the -S-L- group comprises or consists of the formula -S-(CH2)y(C=O)O(CH2)z- wherein y is 2 and z is 1 , and / or the linker group (L) comprises a polyethylene glycol moiety, e.g. the -S-L- group comprises or consists of the formula -S-(CH2)P(C=O)O(CH2CH2O)q(CH2)r- wherein p is 2 and r is 1.

23. A monomer according to any of Claims 19 to 22, wherein the core or hub moiety comprises one of the following general structures (8), (9), or (10):(8)wherein R8and R9are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R8and R9are optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.wherein R10is selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1-20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R10is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1- C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, ORX, NHRy, NRyRzand Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl. (10)24. A monomer according to any of Claims 19 to 23, having one of the structures (3), (4), or (5):(3)wherein R1and R2are defined as above;R3and R4are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-garyl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R3and / or R4are optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.wherein R1, R2, R6are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1, R2, R6is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl wherein R5is selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, C3-9 aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R5is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl, ORX, NHRy, NRyRzand Rx, Ry, and Rzare independently selected from H, C1-6 alkyl, C2-6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.(5)wherein R1, R2, R6, R7are independently selected from alkyl, substituted alkyl, aryl or substituted aryl groups, for example C1.20 alkyl, C2-20 alkenyl, C1.20 haloalkyl, C2-20 alkynyl, C3-9 cycloalkyl, Cs-g aryl, C3-9 heteroaryl, Cs-g heterocyclyl; wherein R1, R2, R6, R7is optionally substituted with one or more of H, D, F, Cl, Br, I, OH, C1-C4 alkoxy, C^alkenyl, Ci-e haloalkyl, C^alkynyl, Ci-e carboxyl, COORW, ORX, NHRy, NRyRzand Rw, Rx, Ry, and Rzare independently selected from H, Ci-e alkyl, C2- 6 alkenyl, Ci-e haloalkyl, C2-6 alkynyl.

25. A polymer fabricated from the monomer of any of Claims 19 to 24, e.g. for use as an adhesive, a foam, a sealant, a moulded article, a film, a coating, a varnish, a paint, an ink, a composite material, an extruded article, a 3D printed object, a fibre, an elastomer, a polymer-based adhesive, a pharmaceutical, a biomedical product, and / or a self-healing material capable of recovering from structural damage such as scratches.

Citation Information

Patent Citations

  • Dye fluorescence intensity improvement linear polymer and preparation method and application thereof

    CN104910312A