Light-emitting element, display device, and method for producing light-emitting element

The integration of a charge functional layer with an inorganic hole transporting material, voids, and organic molecules in light emitting elements addresses the high driving voltage issue, enhancing carrier density and mobility, thereby improving efficiency and reducing voltage requirements.

WO2024218913A1PCT designated stage expired Publication Date: 2024-10-24SHARP DISPLAY TECHNOLOGY CORP

Patent Information

Application Number
PCT/JP2023/015653
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-24

Smart Images

  • Figure JP2023015653_24102024_PF_FP_ABST
    Figure JP2023015653_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A light-emitting element (10) comprises a light-emitting layer (6) and an electric-charge functional layer (4). The electric-charge functional layer (4) includes: an inorganic layer (4U) containing an inorganic hole-transporting material; one or more voids (4Z); and organic molecules (T). The organic molecules (T) each include: a first functional group (K1) capable of binding to the inorganic hole-transporting material; and a second functional group (K2) having electron-withdrawing properties or electron-donating properties.
Need to check novelty before this filing date? Find Prior Art

Description

Light-emitting element, display device, and method for manufacturing light-emitting element

[0001] The present disclosure relates to a light-emitting device and the like.

[0002] Patent Document 1 discloses a light-emitting device having a bipolar layer between a hole transport layer and an active layer.

[0003] U.S. Patent Publication US2013 / 0015424

[0004] Conventional light-emitting elements have a problem in that they require high driving voltage.

[0005] A light-emitting element according to the present disclosure comprises an anode and a cathode, an emitting layer located between the anode and the cathode, and a charge functional layer located between the anode and the emitting layer, the charge functional layer including an inorganic layer containing an inorganic hole transport material, one or more voids, and organic molecules, the organic molecules including a first functional group capable of bonding with the inorganic hole transport material and a second functional group having electron-withdrawing or electron-donating properties.

[0006] The driving voltage of the light emitting element can be reduced.

[0007] FIG. 1 is a cross-sectional view showing a configuration example of a light-emitting element according to the present disclosure. FIG. 2 is a cross-sectional view showing a configuration example of a portion of a light-emitting element. FIG. 3 is a band diagram of an inorganic hole transport material (p-type semiconductor) and a charge functional layer. FIG. 4 is a schematic diagram showing an example of an organic molecule. FIG. 5 is a structural formula showing an example of an organic molecule. FIG. 6 is a flowchart showing an example of a method for manufacturing nanoparticles. FIG. 7 is a flowchart showing an example of a method for manufacturing a light-emitting element. FIG. 8 is a cross-sectional SEM image of a light-emitting element of Example 1. FIG. 9 is a cross-sectional SEM image of a light-emitting element of Example 2. FIG. 10 is a graph showing the voltage (E)-luminance (L) characteristics of the light-emitting elements of Example 1, Example 2, Comparative Example 1, and Comparative Example 2; and FIG. 11 is a graph showing the voltage (E)-current density (J) characteristics of the light-emitting elements of Example 1, Example 2, Comparative Example 1, and Comparative Example 2. FIG. 11 is a flowchart showing an example of a method for manufacturing a light-emitting element. FIG. 12 is a cross-sectional view showing an example of a method for manufacturing a light-emitting element. FIG. 13 is a schematic diagram showing a configuration example of a display device according to the present embodiment.

[0008] Fig. 1 is a cross-sectional view showing an example of the configuration of a light-emitting element according to the present disclosure. Fig. 2 is a cross-sectional view showing an example of the configuration of a portion of a light-emitting element. As shown in Fig. 1, the light-emitting element 10 includes, in order from the lower layer side (pixel circuit substrate 2 side), an anode 3, a charge functional layer 4, a hole transport layer 5, a light-emitting layer 6, an electron transport layer 7, and a cathode 8. The light-emitting layer 6 may be a quantum dot light-emitting layer containing a plurality of quantum dots Q.

[0009] As shown in Figure 2, the light-emitting element 10 includes an emissive layer 6 located between the anode 3 and the cathode 8, and a charge functional layer 4 located between the anode 3 and the emissive layer 6. The charge functional layer 4 includes an inorganic layer 4U containing an inorganic hole transport material, one or more voids 4Z, and organic molecules T. The organic molecules T include a first functional group K1 capable of bonding with the inorganic hole transport material and a second functional group K2 having electron-withdrawing or electron-donating properties. The voids 4Z in the charge functional layer 4 refer to spaces where the inorganic hole transport material and organic molecules are not present. The spaces 4S in the charge functional layer 4 are spaces where the inorganic hole transport material is not present. The voids 4Z and spaces 4S are located within the charge functional layer 4 and the inorganic layer 4U.

[0010] The organic molecule T may have a first functional group K1 including at least one of a carboxyl group, a silanol group, a phosphoryl group, a thiol group, and an amino group, and a second functional group K2 including at least one of a nitro group, a halogen group, an amino group, a methoxy group, and an ethoxy group.

[0011] In the charge functional layer 4 of the light-emitting element 10, the organic molecules T enter the spaces 4S, thereby increasing the carrier density and mobility of the charge functional layer 4 and reducing the driving voltage of the light-emitting element 10. The charge functional layer 4 may be a hole injection layer (HIL).

[0012] The second functional group K2 in FIG. 2 may have electron-withdrawing properties if the inorganic hole transport material is a p-type semiconductor, and may have electron-donating properties (hole-withdrawing properties) if the inorganic hole transport material is an n-type semiconductor.

[0013] 2, the organic molecules T may be arranged in the space 4S so as to contact the void 4Z. The organic molecules T are self-assembled monomolecules, and an organic film 4F (self-assembled monolayer) containing the self-assembled monomolecules may be arranged in the space 4S so as to contact the void 4Z. The organic film 4F may be arranged on the edge of the space 4S. The void 4Z may be located inside the inorganic layer 4U.

[0014] The porosity of the charge functional layer 4 may be 3.0% to 15.0%. The porosity may be the ratio of the void area to the cross-sectional area of ​​the charge functional layer 4. If the porosity is less than 3%, there may not be enough organic molecules T in the charge functional layer 4, and the carrier density improvement effect may be reduced. On the other hand, if the porosity is more than 15%, the carrier density improvement effect may saturate, and the carrier transport ability of the charge functional layer 4 may decrease due to the small proportion of inorganic hole transport material.

[0015] The average diameter of the voids 4Z may be 5.0 nm to 30.0 nm. The diameter of the voids 4Z can be the longest diameter of the voids 4Z that appear in the cross section of the charge functional layer 4. If the average diameter of the voids 4Z is less than 5.0 nm, organic molecules may not be able to sufficiently enter the spaces where the inorganic hole transport material is not present, which may reduce the effect of improving the carrier density. On the other hand, if the average diameter of the voids 4Z is more than 30 nm, there will be a large amount of space where the inorganic hole transport material is not present, which may reduce the carrier transport ability of the charge functional layer 4.

[0016] The thickness of the organic film 4F may be 0.5 nm to 2.0 nm. If the thickness of the organic film 4F (the size of the organic molecules T) is less than 0.5 nm, the binding strength of the organic molecules T to the inorganic hole transport material may be reduced. If the thickness of the organic film 4F (the size of the organic molecules T) is more than 2.0 nm, the organic molecules T may have difficulty entering the space 4S where no inorganic hole transport material is present.

[0017] The inorganic hole transport material of the charge functional layer 4 may be a metal chalcogenide. The metal chalcogenide may be a metal oxide or a metal compound containing at least one of a CN group, an SCN group, and an SeCN group.

[0018] The second functional group K2 of the organic molecule T may have electron-withdrawing properties, and the metal chalcogenide serving as the inorganic hole transport material may contain at least one of Ni, Cu, Fe, and Co. In this case, the inorganic hole transport material is a p-type semiconductor.

[0019] The second functional group K2 of the organic molecule T may have electron donating properties, and the metal chalcogenide that is the inorganic hole transport material may contain at least one of Mo, V, and W. In this case, the inorganic hole transport material is an n-type semiconductor.

[0020] The inorganic hole transport material of the charge functional layer 4 may be a p-type semiconductor. FIG. 3 is a band diagram of the inorganic hole transport material (p-type semiconductor) and the charge functional layer. As shown in FIG. 3, the Fermi level (Ef) of the charge functional layer 4 may be deeper than the Fermi level (Ef) of the p-type semiconductor (inorganic hole transport material), and the difference between the valence band top (VBM) and the Fermi level (Ef) of the charge functional layer 4 may be smaller than the difference between the valence band top (VBM) and the Fermi level (Ef) of the p-type semiconductor. In this case, the hole transport function of the charge functional layer 4 is enhanced, and the driving voltage of the light-emitting element 10 can be reduced. The valence band top (VBM) of the charge functional layer 4 may be deeper than the valence band top (VBM) of the p-type semiconductor (inorganic hole transport material). In this case, the energy barrier between the charge functional layer 4 and the hole transport layer 5 is reduced, and the driving voltage of the light-emitting element 10 can be further reduced. The p-type semiconductor, which is an inorganic hole transport material, may be nickel oxide. In this case, nickel oxide is chemically stable, making it easier to obtain stable characteristics. The charge functional layer 4 in FIG. 3 contains organic molecules having an electron-withdrawing second functional group. The reference example in FIG. 3 shows a case in which organic molecules without a second functional group are used in the HIL, and it can be seen that in this case, the effect of the charge functional layer 4 is not observed.

[0021] The inorganic hole transport material of the charge functional layer 4 may be an n-type semiconductor. The difference between the conduction band minimum (CBM) and the Fermi level (Ef) of the charge functional layer 4 may be smaller than the difference between the conduction band minimum (CBM) and the Fermi level (Ef) of an n-type semiconductor. In this case, the hole transport function of the charge functional layer 4 is enhanced, and the driving voltage of the light-emitting element 10 can be reduced. In this case, the charge functional layer 4 contains organic molecules having an electron-donating second functional group.

[0022] 2, the charge functional layer 4 may have a plurality of nanoparticles NP containing an inorganic hole transport material. In the charge functional layer 4, by forming a nanoparticle layer containing a plurality of nanoparticles NP as the inorganic layer 4U, spaces 4S and voids 4Z are easily formed in the charge functional layer 4.

[0023] The diameter of the nanoparticles NP may be 4.0 nm to 9.0 nm. If the diameter of the nanoparticles NP is less than 4.0 nm, the conductivity of the nanoparticles P may decrease. On the other hand, if the diameter of the nanoparticles NP is more than 9.0 nm, the irregularities of the inorganic layer 4U may increase, causing contact between the charge functional layer 4 and the light-emitting layer 6 or the electron transport layer 7, which may increase the reactive current.

[0024] The diameter of the plurality of nanoparticles NP may be 5.0 nm ≦ D50 ≦ 40 nm. If D50 is less than 5.0 nm, the conductivity of the nanoparticles may decrease. On the other hand, if D50 is more than 40 nm, the irregularities of the inorganic layer 4U may become large, causing contact between the charge functional layer 4 and the light-emitting layer 6 or the electron transport layer 7, which may increase the reactive current. D50 is the median diameter, which means that the total volume of nanoparticles with a particle size of D50 or less is 50% of the total volume of all nanoparticles. The diameter of the nanoparticles NP when the nanoparticles NP appearing in the cross section of the charge functional layer 4 are deformed into a circular shape with equal volume can be used.

[0025] The diameter of the plurality of nanoparticles NP may be 3.0 nm ≦ (D84 - D16) / 2 ≦ 10 nm. Here, (D84 - D16) is referred to as the particle size deviation. If the particle size deviation (D84 - D16) is less than 3.0 nm, the particle size distribution is narrow, and the inorganic layer 4U may become too dense, potentially reducing the porosity of the charge functional layer 4. On the other hand, if the particle size deviation is greater than 10 nm, the particle size distribution is wide and coarse particles are included, increasing the porosity of the inorganic layer 4U, potentially increasing the porosity of the charge functional layer 4 too much.

[0026] 2, each of the multiple nanoparticles NP may be a nickel oxide nanoparticle. The organic molecule T may have one or two first functional groups K1. In this case, the first functional groups K1 that are not bonded to the inorganic layer 4U are more likely to exist, preventing the hole transport in the charge functional layer 4 from being inhibited. The first functional groups K1 may include a phosphoryl group. In this case, bonding between the inorganic hole transport material and the first functional groups K1 is easily formed, facilitating the formation of the charge functional layer 4.

[0027] As shown in FIG. 2, the inorganic hole transport material is a p-type semiconductor, the inorganic layer 4U is a nanoparticle layer of metal chalcogenide, the second functional group K2 of the organic molecule T is electron-withdrawing, and a self-assembled monolayer (SAM) of the same material as the organic molecule T may be included above and below the upper surface 4J of the inorganic layer.

[0028] FIG. 4 is a schematic diagram showing an example of an organic molecule. FIG. 5 is a structural formula showing an example of an organic molecule. As shown in FIG. 4, the organic molecule T may include a hole-transporting functional group K3 (e.g., a carbazole group, a tetracyano group, a triarylamine group, a fluorene group, a quinonediimide group, a phthalocyanine group, a triphenylene group, a phenylnaphthalene group, etc.). As shown in FIG. 5, the organic molecule T may be Br-2PACz ([2-(3,6-dibromo-9H-carbazol-9-yl)ethyl]phosphonic acid) or 4-nitrobenzoic acid. Other examples of the organic molecule T include a molecule in which Br in Br-2PACz is substituted with any one of the other halogens F, Cl, and I, 4-(trifluoromethyl)benzoic acid, 4-chlorobenzoic acid, etc.

[0029] 2, the driving voltage of the light-emitting element 10 can be reduced by providing organic molecules T in the gaps 4Z of the charge functional layer 4. That is, by bonding an organic film 4F (self-assembled monolayer) having an electron-withdrawing second functional group K2 to an inorganic hole transport material (e.g., nickel oxide) and deepening the VBM (the upper level of the valence band), the energy barrier between the charge functional layer 4 and the hole transport layer 5 is reduced, and the driving voltage can be reduced.

[0030] In this case, it was found that the difference between Ef (Fermi level) and VBM becomes smaller in the charge functional layer 4. For example, when the organic molecule T has electron-withdrawing properties, the organic molecule T attracts electrons from the inorganic hole transport material, increasing the number of holes in the inorganic hole transport material, so that the Fermi level approaches the VBM and the difference between Ef and VBM becomes smaller.

[0031] Therefore, by adsorbing the organic film 4F (self-assembled monolayer) deep into the inorganic layer 4U, it was possible to increase the carrier density and mobility of the inorganic layer 4U. Furthermore, experimental results also revealed that the driving voltage reduction effect of the organic film 4F (self-assembled monolayer) is greater in inorganic layers 4U that are nanoparticle layers with many voids (e.g., nickel oxide nanoparticle layers) than in sol-gel films with few voids. Here, the sol-gel film is a film obtained by applying a precursor solution of an inorganic hole transport material and heating it, and is likely to form a dense film. Here, the precursor solution is a solution in which a salt containing nickel ions, such as nickel acetate, nickel nitrate, or nickel chloride, is dissolved in a solvent such as ethanol, dimethyl sulfoxide, or water in which the salt dissolves. When the solvent is water, it is called a precursor aqueous solution.

[0032] In the light-emitting element 10, the charge functional layer 4 may have a hole injection function, and a hole transport layer 5 containing an organic material may be disposed between the charge functional layer 4 and the light-emitting layer 6. When the hole transport layer 5 is provided, the light-emitting efficiency of the light-emitting element 10 can be improved. The hole transport layer 5 may have a functional group (third functional group K3) with hole transport properties. In this case, holes are smoothly transported from the charge functional layer 4 to the hole transport layer 5.

[0033] Examples of materials for the hole transport layer 5 include poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl))diphenylamine)] (abbreviated as "TFB"), poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine] (abbreviated as "Poly-TPD"), polyvinylcarbazole (abbreviated as "PVK"), and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (abbreviated as "PTAA") These materials may be used alone or in combination of two or more.

[0034] In the light-emitting layer 6, holes from the anode 3 and electrons from the cathode 8 recombine to emit light. The light-emitting element 10 may be configured so that light emission occurs in the light-emitting layer 6 when a voltage or current is applied between the anode 3 and the cathode 8. The light-emitting layer 6 may include a plurality of light-emitting quantum dots Q. The quantum dots Q refer to dots (particles) having a maximum width of 100 nm or less. The shape of the quantum dots Q is not particularly limited as long as it satisfies the above-mentioned maximum width, and is not limited to a spherical three-dimensional shape (circular cross-sectional shape). For example, the quantum dots may have a polygonal cross-sectional shape, a rod-like three-dimensional shape, a branch-like three-dimensional shape, a three-dimensional shape with an uneven surface, or a combination thereof. The quantum dots are typically semiconductor single crystals and may have a particle size of 1.0 nm to 50 nm. The quantum dots may include a II-VI group semiconductor compound such as MgS, MgSe, MgTe, CaS, CaSe, CaTe, SrS, SrSe, SrTe, BaS, BaSe, BaTe, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, HgS, HgSe, or HgTe, and / or a III-V group semiconductor compound crystal such as GaAs, GaP, InN, InAs, InP, or InSb, and / or a group IV semiconductor compound crystal such as Si or Ge. The quantum dots Q may be, for example, a core-shell type in which the semiconductor crystal described above serves as a core and is overcoated with a shell material having a high band gap, or a shell-less type in which only the core is present. The light-emitting layer 6 may include an organic or inorganic ligand on the surface of the quantum dots Q.

[0035] The light-emitting layer 6 may include an inorganic matrix material 6X filling spaces between the plurality of light-emitting quantum dots Q. The inorganic matrix material 6X refers to a component that contains and holds other substances, and may alternatively be referred to as a base material, a parent material, or a filler. The inorganic matrix material 6X may be a component of the light-emitting layer 6 that contains the plurality of light-emitting quantum dots Q. The inorganic matrix material 6X may be filled into the light-emitting layer 6. The inorganic matrix material 6X may be amorphous. The elemental proportion of carbon in the inorganic matrix material 6X may be 10% or less.

[0036] The inorganic matrix material 6X preferably has a wider band gap than the core material of the quantum dots Q. A semiconductor or an insulator can be used as the inorganic matrix material 6X. The inorganic matrix material 6X may contain at least one of a metal sulfide and a metal oxide. Examples of metal sulfides include zinc sulfide (ZnS), zinc magnesium sulfide (ZnMgS, ZnMgS 2 ), gallium sulfide (GaS, Ga 2 S 3 ), zinc tellurium sulfide (ZnTeS), magnesium sulfide (MgS), zinc gallium sulfide (ZnGa 2 S 4 ), magnesium gallium sulfide (MgGa 2 S 4 Examples of metal oxides include zinc oxide (ZnO), titanium oxide (TiO 2 ), tin oxide (SnO 2 ), tungsten oxide (WO 3 ), zirconium oxide (ZrO 2 ), silicon dioxide (SiO 2 ) can be mentioned.

[0037] The anode 3 supplies holes to the light-emitting layer 6. The cathode 8 supplies electrons to the light-emitting layer 6. The cathode 8 may be located opposite the anode 3. In FIG. 1 , the cathode 8 is located above the anode 3.

[0038] At least one of the anode 3 and the cathode 8 may be formed of a light-transmitting material. Examples of the light-transmitting material include transparent conductive materials. Examples of the transparent conductive material include ITO (indium tin oxide), IZO (indium zinc oxide), SnO2 (tin oxide), and FTO (fluorine-doped tin oxide). These materials have high transmittance for visible light, which improves the luminous efficiency of the light-emitting element 10.

[0039] At least one of the anode 3 and the cathode 8 may be formed of a light-reflective material. Examples of the light-reflective material that can be used include metal materials. Examples of metal materials that can be used include aluminum (Al), silver (Ag), copper (Cu), and gold (Au). These materials have high reflectance for visible light, which improves the luminous efficiency of the light-emitting element 10.

[0040] The electron transport layer 7 is located between the light-emitting layer 6 and the cathode 8. The electron transport layer 7 transports electrons from the cathode 8 to the light-emitting layer 6. Examples of materials for the electron transport layer 7 include zinc oxide (ZnO), zinc magnesium oxide (MgZnO), titanium oxide (TiO2), and strontium oxide (SrTiO3). These materials may be in the form of nanoparticles. As such, the electron transport layer 7 may contain MgZnO. In this case, electron injection is suppressed, which facilitates the carrier balance of the light-emitting element 10 to be regulated, thereby improving luminous efficiency.

[0041] Other examples of materials for the electron transport layer 7 include compounds or complexes containing one or more nitrogen-containing heterocycles such as an oxadiazole ring, a triazole ring, a triazine ring, a quinoline ring, a phenanthroline ring, a pyrimidine ring, a pyridine ring, an imidazole ring, or a carbazole ring.

[0042] Further examples of materials for the electron transport layer 7 include 1,10-phenanthroline derivatives such as bathocuproine and bathophenanthroline, benzimidazole derivatives such as 1,3,5-tris(N-phenylbenzimidazol-2-yl)benzene (TPBI), metal complexes such as bis(10-benzoquinolinolato)beryllium complex, 8-hydroxyquinoline Al complex, and bis(2-methyl-8-quinolinato)-4-phenylphenolate aluminum, and 4,4'-biscarbazole biphenyl. Other examples include aromatic boron compounds, aromatic silane compounds, aromatic phosphine compounds such as phenyldi(1-pyrenyl)phosphine, and nitrogen-containing heterocyclic compounds such as bathophenanthroline, bathocuproine, or triazine derivatives. These materials may be used alone or in combination.

[0043] For the charge functional layer 4, a cross-sectional image of the light-emitting element 10 is obtained using SEM (scanning electron microscopy), and the porosity can be calculated from the contrast of the cross-sectional image. Methods for extracting the charge functional layer 4 from the cross-sectional image include primary human visual judgment, secondary computer or AI (artificial intelligence) judgment, and tertiary human judgment assisted by a computer or AI. Specifically, the line passing through the pixels where the pixel luminance distribution changes most sharply is extracted as a candidate contour line for the charge functional layer 4. Next, the boundary of the void 4Z is extracted from the charge functional layer 4 by contrast judgment. Specifically, a luminance histogram is created for all pixels, a threshold is determined using, for example, the maximum entropy method, and pixels in the area above the threshold are whitened. Meanwhile, other pixels in the area within the charge functional layer 4 are blackened. Next, the number of white and black pixels in the area within the charge functional layer 4 is counted to calculate the porosity. Here, porosity = number of white pixels / (number of white pixels + number of black pixels). If it is difficult to determine the threshold value using the above-mentioned method, it may be determined, for example, by the percentile method. The void diameter (pore diameter) can be determined from the cross-sectional image by measuring, for example, the longest diameter of the void 4Z.

[0044] The inorganic hole transport material can be identified by performing elemental analysis on a cross section of the charge functional layer 4 using a combination of SEM and EDX (Energy Dispersive X-ray Spectroscopy). Here, the cross section of the light-emitting element is obtained by FIB (Focused Ion Beam) processing.

[0045] The organic molecule T can be identified by etching down to the charge functional layer 4 using a GCIB (Gas Cluster Ion Beam), and analyzing the charge functional layer 4 using TOF-SIMS (Time-of-Flight Secondary Ion Mass Spectrometry) and MS / MS (Tandem Mass Spectrometry).

[0046] (Examples 1 and 2) Fig. 6 is a flowchart showing an example of a method for producing nanoparticles. As shown in Fig. 6, in step S11, nickel nitrate hexahydrate (Ni(NO 3 ) 2 ・6H 2 0.05 mmol of HCl and 20 mL of pure water are mixed and stirred to prepare a precursor aqueous solution. In step S13, a 10 mol / L aqueous solution of sodium hydroxide is added to the precursor aqueous solution at a rate of 0.4 to 0.5 mg / min (e.g., 0.45 mg / min) until the pH reaches 9 to 11 (e.g., pH 10), yielding a green precipitate. In step S15, a washing step of adding pure water to the green precipitate, centrifuging, and removing the supernatant is repeated three times. In step S17, the washed green precipitate is dried at 60 to 100°C (e.g., 80°C) to yield a green powder. In step S19, the green powder is calcined at 250 to 300°C for 2 to 6 hours (e.g., at 270°C for 2 hours) to yield a black nickel oxide nanoparticle powder.

[0047] The particle size of the nanoparticles can be measured, for example, as follows. Nickel oxide nanoparticles were dispersed in an aqueous solvent, and the solution was passed through a filter with a pore size of 0.45 μm. The particle size distribution was measured using a particle size distribution analyzer (Microtrac-Bell, Nanotrac Wave II), and the obtained results were used as the particle size. Furthermore, the median diameter D50 (nm) of the nanoparticles was calculated from the results. In this example, the particle size was 6.4 to 86 [nm], and D50 was 9.9 nm. Furthermore, the particle size deviation (D84 - D16) in this example was 4.5 [nm].

[0048] The nickel oxide nanoparticles prepared by the above method contain nitrate ions and are highly dispersible in water. If the rate of addition of the sodium hydroxide aqueous solution is outside the above range, particles with a particle size of 100 nm or more will be present, the irregularities of the inorganic layer 4U will increase, and the charge functional layer 4 will come into contact with the light-emitting layer 6 or the electron transport layer 7, which may increase the reactive current.

[0049] The crystallite diameter of nanoparticles can be measured, for example, as follows. The X-ray intensity of nickel oxide nanoparticles was measured with a powder X-ray diffraction (XRD) device (MiniFlex II, manufactured by Rigaku Corporation) versus the diffraction angle 2θ, and the crystallite diameter d (nm) was calculated from the results using the following Scherrer equation: d = 0.89λ / B cos θ, where λ (nm) is the wavelength of the X-ray. In this measurement, CuKα rays with λ = 0.154 (nm) were used. B is the full width at half maximum (FWHM) of the X-ray diffraction peak. In the example, the crystallite diameter d was 4.3 [nm]. FIG. 7 is a flowchart showing an example of a method for manufacturing a light-emitting device. As shown in FIG. 7, in step S20, an anode is formed by forming an ITO film (30 nm thick, 2 mm × 10 mm) on a substrate using a sputtering method. In step S30, 0.1 ml of the nanoparticle dispersion liquid, in which 30 mg of nickel oxide nanoparticles prepared in Fig. 6 were dispersed in 1.0 ml of water and 1.0 ml of 2-methoxyethanol, was spin-coated onto the anode (ITO), dried at 200°C, and the same process (spin-coating and drying) was repeated several times to form an inorganic layer. The inorganic layer had a thickness of 50 nm.

[0050] In step S35, a solution of Br-2PACz dissolved in ethanol to a concentration of 0.01 M (mol / L) is brought into contact with the inorganic layer for 5 seconds or more, followed by drying to form a charge functional layer. In step S35, the inorganic layer may be immersed in a solution of 4-nitrobenzoic acid dissolved in methanol to a concentration of 0.1 M for 1 hour, followed by drying to form a charge functional layer.

[0051] In step S40, 8 mg of TFB was dissolved in 1 ml of chlorobenzene and spin-coated onto the charge-transport functional layer to form an organic hole transport layer. The thickness of the organic hole transport layer was 40 nm. In step S50, 0.05 to 0.1 ml of a quantum dot solution containing InP / ZnS (core / shell) or CdSe / ZnS (core / shell) was spin-coated onto the organic hole transport layer to form an emissive layer. In step S60, an electron transport layer was formed by spin-coating a nanoparticle dispersion of MgZnO or ZnO onto the emissive layer. The thickness of the electron transport layer was 60 nm. In step S70, a cathode was formed by vacuum-depositing an Ag or Al electrode onto the electron transport layer. The thickness of the cathode was 50 nm.

[0052] Example 1 refers to the case where an inorganic layer (nanoparticle layer) is formed in the above-described step S30, and Example 2 refers to the case where, instead of the above-described step S30, 0.248 g of nickel acetate tetrahydrate was dissolved in 5 ml of ethanol, and 0.1 ml of the solution was spin-coated on the ITO (anode) and dried at 230°C to form an inorganic layer (sol-gel layer). Figure 8 is a cross-sectional SEM image of the light-emitting element of Example 1. Figure 9 is a cross-sectional SEM image of the light-emitting element of Example 2. At this time, the porosity of the charge functional layer (Example 1) in Figure 8 was 3.2%, and the porosity of the charge functional layer (Example 2) in Figure 9 was 2.7%.

[0053] The light-emitting devices can be evaluated, for example, as follows. A spectrum measuring device (MCPD7000, manufactured by Otsuka Electronics Co., Ltd.) and a current-voltage characteristic measuring device (2400, manufactured by Keithley) were used to apply an applied voltage V (voltage between the cathode and anode) to each light-emitting device, and the luminance value L of the light emitted from each light-emitting device was measured using the luminance / spectrum measuring device (spectrometer). In addition, the applied voltage V was changed in various ways, and the V-J characteristics were measured.

[0054] Fig. 10 is a graph showing the voltage (V)-luminance (L) characteristics of the light-emitting elements of Example 1, Example 2, Comparative Example 1, and Comparative Example 2. Fig. 11 is a graph showing the voltage (V)-current density (J) characteristics of the light-emitting elements of Example 1, Example 2, Comparative Example 1, and Comparative Example 2. Comparative Example 1 is a case where only a nickel oxide nanoparticle layer (without organic molecules) is formed as the HIL, and Comparative Example 2 is a case where only a nickel oxide sol-gel layer (without organic molecules) is formed as the HIL.

[0055] 10, it can be seen that the voltage-luminance characteristics of Example 1 (graph a) are improved compared to Comparative Example 1 (graph c1). Specifically, Example 1 has a luminance of 1000 cd / m compared to Comparative Example 1, which does not contain organic molecules. 2 The voltage required for the luminance of 1000 cd / m2 (graph b) is reduced by approximately 7.6 V compared to Comparative Example 2 (graph c2) which does not contain organic molecules. 2 The voltage required for this was reduced by approximately 6.3V.

[0056] 11, it can be seen that the voltage-current density characteristics of Example 1 (graph a) are improved compared to Comparative Example 1 (graph c1). Specifically, Example 1 has a 10 mA / cm 2 The voltage required to pass a current of 10 mA / cm was reduced by approximately 7 V. For Example 2 (graph b), the current was 10 mA / cm compared to Comparative Example 2 (graph c2) which did not contain organic molecules. 2 The voltage required to pass the current was reduced by about 4V.

[0057] 10 and 11 also show that Example 1 has better voltage-current density characteristics than Example 2. This is because in Example 1, organic molecules having electron-withdrawing functional groups penetrate into the inorganic layer through voids and are adsorbed onto the surface of the inorganic hole transport material, improving the carrier density of the inorganic hole transport material and increasing the mobility of the charge functional layer.

[0058] 12 is a flowchart showing an example of a method for manufacturing a light-emitting element. In FIG. 12, in step S31, an inorganic layer (nanoparticle layer) containing metal chalcogenide nanoparticles and voids is formed, and in step S32, an organic solution containing organic molecules having a first functional group capable of bonding with the metal chalcogenide and a second functional group with electron-withdrawing properties is brought into contact with the inorganic layer (nanoparticle layer) for a predetermined time, and then the organic solution is dried. This allows the charge functional layer of Example 1 to be formed.

[0059] Example 3 Fig. 13A is a flowchart illustrating an example of a method for manufacturing a light-emitting element. Fig. 13B is a cross-sectional view illustrating an example of a method for manufacturing a light-emitting element. As shown in Figs. 13A and 13B, in step S36, an initial layer 4K including metal chalcogenide and organic particles is formed. Specifically, 0.248 g of nickel acetate tetrahydrate is dissolved in 5 ml of ethanol, and 7 mg of polystyrene nanoparticles (organic particles) YP having a particle size of 20 nm is added to form 0.1 ml of the solution, which is spin-coated onto ITO (anode) and dried at 110°C, to form the initial layer 4K.

[0060] In step S37, the organic particles YP of the initial layer 4K are dissolved to form an inorganic layer 4U including voids 4S. Specifically, the initial layer is immersed in toluene to dissolve the polystyrene nanoparticles YP, and then dried at 230° C. The dissolution of the polystyrene nanoparticles YP allows the formation of an inorganic layer 4U including voids 4S.

[0061] In step S38, an organic solution containing organic molecules having a first functional group capable of bonding with a metal chalcogenide and a second functional group with electron-withdrawing properties is brought into contact with the inorganic layer for a predetermined period of time, and then the organic solution is dried. Specifically, the inorganic layer is immersed for one hour in a solution in which 4-nitrobenzoic acid is dissolved in ethanol to a concentration of 0.01 mol / L, and then the organic solution is dried to form a charge functional layer 4 including voids 4Z and an organic film (self-assembled monolayer) 4F. The charge functional layer 4 had a thickness of 45 nm.

[0062] In Example 3, a charge functional layer 4 with a porosity of 5% was obtained. It was found that the light-emitting element including the charge functional layer obtained in step S38 consumed less power to achieve the same brightness than Example 2 and Comparative Examples 1 and 2. FIG. 14 is a schematic diagram showing an example configuration of a display device according to this embodiment. The display device 70 includes a display unit DA, a first driver circuit X1 (e.g., a data signal line drive circuit) and a second driver circuit X2 (e.g., a scanning signal line drive circuit, a light-emitting control line drive circuit) that drive the display unit DA, and a control circuit CL that controls the first driver circuit X1 and the second driver circuit X2. The display unit DA may include a pixel circuit layer and a light-emitting element layer. The light-emitting element layer may include a red-emitting light-emitting element 10R (10), a green-emitting light-emitting element 10G (10), and a blue-emitting light-emitting element 10B (10), and each of the light-emitting elements 10R, 10G, and 10B may be connected to a pixel circuit PC formed in the pixel circuit layer.

[0063] [Notes] The above-described embodiments are for the purpose of illustration and description, and are not intended to be limiting. Based on these examples and descriptions, it will be apparent to those skilled in the art that many variations are possible.

[0064] 2 (Pixel circuit) substrate 3 Anode 4 Charge functional layer 4U Inorganic layer 4Z Void 4F Organic film (self-assembled monolayer) 5 Hole transport layer 6 Light-emitting layer 7 Electron transport layer 8 Cathode T Organic molecule K1 First functional group K2 Second functional group 10 Light-emitting element 70 Display device

Claims

1. A light-emitting element comprising an anode and a cathode, an emitting layer located between the anode and the cathode, and a charge functional layer located between the anode and the emitting layer, the charge functional layer including an inorganic layer containing an inorganic hole transport material, one or more voids, and organic molecules, the organic molecules including a first functional group capable of bonding with the inorganic hole transport material, and a second functional group having electron-withdrawing or electron-donating properties.

2. A light-emitting element comprising an anode and a cathode, an emitting layer located between the anode and the cathode, and a charge functional layer located between the anode and the emitting layer, the charge functional layer including an inorganic layer containing a metal chalcogenide which is an inorganic hole transport material, one or more voids, and organic molecules, the organic molecules having a first functional group including at least one of a carboxyl group, a silanol group, a phosphoryl group, a thiol group, and an amino group, and a second functional group including at least one of a nitro group, a halogen group, an amino group, a methoxy group, and an ethoxy group.

3. The light-emitting element according to claim 1 or 2, wherein the voids are located inside the inorganic layer.

4. The light-emitting device according to any one of claims 1 to 3, wherein the organic molecules are in contact with the voids.

5. The light-emitting element according to any one of claims 1 to 4, wherein the organic molecules are self-assembled monomolecules, and an organic film containing the self-assembled monomolecules is disposed in the gap.

6. The light-emitting element according to claim 5, wherein the organic film is positioned around the gap.

7. The light-emitting element according to claim 1, wherein the first functional group includes at least one of a carboxyl group, a silanol group, a phosphoryl group, a thiol group, and an amino group.

8. The light-emitting element according to claim 1, wherein the second functional group includes at least one of a nitro group, a halogen group, an amino group, a methoxy group, and an ethoxy group.

9. The light-emitting device according to any one of claims 1 to 8, wherein the porosity of the charge functional layer is 3.0% to 15.0%.

10. The light-emitting device according to any one of claims 1 to 9, wherein the average diameter of the voids is 5.0 nm to 30.0 nm.

11. The light-emitting element according to claim 5, wherein the organic film has a thickness of 0.5 nm to 2.0 nm.

12. The light-emitting device of claim 1, wherein the inorganic hole transport material is a metal chalcogenide.

13. The light-emitting element according to claim 2 or 12, wherein the metal chalcogenide is a metal oxide or a metal compound containing at least one of a CN group, an SCN group, and an SeCN group.

14. The light-emitting element according to claim 12, wherein the second functional group has electron-withdrawing properties, and the metal chalcogenide includes at least one of Ni, Cu, Fe, and Co.

15. The light-emitting element according to claim 12, wherein the second functional group has electron-donating properties, and the metal chalcogenide includes at least one of Mo, V, and W.

16. The light-emitting element according to any one of claims 1 to 15, wherein the inorganic hole transport material is a p-type semiconductor.

17. The light-emitting device according to claim 16, wherein the upper end level of the valence band of the charge functional layer is deeper than the upper end level of the valence band of the p-type semiconductor.

18. The light-emitting device according to claim 16, wherein the Fermi level of the charge functional layer is deeper than the Fermi level of the p-type semiconductor.

19. The light-emitting device according to claim 16, wherein a difference between the upper end level of the valence band and the Fermi level of the charge functional layer is smaller than a difference between the upper end level of the valence band and the Fermi level of the p-type semiconductor.

20. The light-emitting element according to any one of claims 1 to 19, wherein the inorganic layer comprises a plurality of nanoparticles comprising the inorganic hole transport material.

21. The light-emitting element according to claim 20, wherein the diameter of the plurality of nanoparticles satisfies 5.0 nm≦D50≦40 nm.

22. The light-emitting element according to claim 20, wherein the diameter of the plurality of nanoparticles satisfies 3.0 [nm]≦(D84−D16) / 2≦10 [nm].

23. The light-emitting device of claim 20, wherein each of the plurality of nanoparticles is a nickel oxide nanoparticle.

24. The light-emitting element according to any one of claims 1 to 23, wherein the organic molecule has one or two of the first functional groups.

25. The light-emitting element according to claim 7, wherein the first functional group comprises a phosphoryl group.

26. The light-emitting element according to any one of claims 1 to 25, wherein the organic molecules contain a functional group with a hole-transporting property.

27. The light-emitting element according to any one of claims 1 to 26, wherein the organic molecule is Br-2PACz.

28. The light-emitting element according to any one of claims 1 to 27, wherein the charge functional layer has a hole injection function, and a hole transport layer containing an organic material is provided between the charge functional layer and the light-emitting layer.

29. The light-emitting element according to any one of claims 1 to 28, wherein the light-emitting layer comprises a plurality of light-emitting quantum dots and an inorganic matrix material filling spaces between the plurality of quantum dots.

30. The light-emitting element described in claim 1, wherein the inorganic hole transport material is a p-type semiconductor, the inorganic layer is a nanoparticle layer of metal chalcogenide, the second functional groups of the organic molecules are electron-withdrawing, and the inorganic layer contains self-assembled monolayers of the same material as the organic molecules above and below an upper surface of the inorganic layer.

31. A display device comprising the light-emitting element according to any one of claims 1 to 30.

32. A method for manufacturing a light-emitting element, comprising the steps of: forming an inorganic layer containing metal chalcogenide nanoparticles and voids; contacting the inorganic layer with an organic solution containing organic molecules having a first functional group capable of bonding to the metal chalcogenide and a second functional group having electron-withdrawing properties for a predetermined period of time, and then drying the organic solution.

33. A method for manufacturing a light-emitting element, comprising the steps of: forming an initial layer containing a metal chalcogenide and organic particles; dissolving the organic particles of the initial layer to form an inorganic layer containing voids; and contacting the inorganic layer with an organic solution containing organic molecules having a first functional group capable of bonding to the metal chalcogenide and a second functional group having electron-withdrawing properties for a predetermined period of time, and then drying the organic solution.

34. The method for producing a light-emitting element according to claim 32 or 33, wherein the organic molecule includes Br-2PACz or 4-nitrobenzoic acid.

Citation Information

Patent Citations

  • Electroluminescent device

    CN102916097A

  • Electroluminescent device, manufacturing method thereof, and display device comprising the same

    EP3540807A1

  • Quantum dot light-emitting device

    JP2010520603A

  • Electroluminescent device and light-emitting layer and uses thereof

    JP2020530195A

  • Fluorescent material and process for producing the same

    WO2006009124A1

Cited By

  • Display device, method for manufacturing display device, and method for forming plurality of functional layers

    WO2026099986A1

  • Light-emitting element, display device, and quantum dot-containing liquid

    WO2026105169A1