All-resin heat utilizing power generation element
The all-resin heat generation element addresses the limitations of conventional thermoelectric systems by using a semiconductor, electrolyte, and conductive polymer layers without metals, offering flexible, cost-effective, and efficient power generation from geothermal or waste heat.
Patent Information
- Application Number
- PCT/JP2024/015361
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional thermoelectric power generation systems face challenges such as high costs, limited operating temperature range, low conversion efficiency, physical durability issues, and restricted installation locations due to the use of metal semiconductors, which also require cooling and are not suitable for applications with vibrations.
An all-resin heat generation element comprising a semiconductor layer, an electrolyte layer, and a conductive polymer layer without a metal layer, allowing for flexible, miniaturized, and self-supporting designs that can utilize geothermal or waste heat for power generation.
The all-resin design reduces material costs, simplifies manufacturing, enhances durability, and enables installation in diverse locations, including those with vibrations, while improving heat utilization efficiency and power generation capabilities.
Smart Images

Figure 000023 
Figure 000024 
Figure 000025
Abstract
Description
All-resin heat-utilizing power generation element
[0001] The present invention relates to an all-resin thermal power generation element.
[0002] Thermoelectric power generation using the Seebeck effect has been known as a thermal power generation method that utilizes geothermal energy or factory waste heat (Patent Documents 1 and 2, and Non-Patent Document 1), and its practical application is expected to be realized in order to efficiently utilize thermal energy. Thermoelectric power generation using the Seebeck effect is a power generation principle that utilizes the generation of voltage when a temperature gradient is applied to a metal or semiconductor. Specifically, it is a thermoelectric power generation system that converts thermal energy into electrical energy by applying a temperature gradient to a thermoelectric conversion element that combines a p-type semiconductor and an n-type semiconductor.
[0003] However, conventional thermoelectric conversion elements that utilize a temperature gradient have problems such as the high cost of the semiconductors that make up the thermoelectric conversion element, a high operating temperature range, and low conversion efficiency. Furthermore, the physical durability of the joints is poor, making it impossible to install them in places where they are subject to vibration. Furthermore, since a temperature gradient is required for power generation, installation locations are limited, and in some cases, a cooling device for the temperature gradient is required. In particular, because one dimension of the thermoelectric conversion module is used for the temperature gradient, the heat source is utilized in two dimensions, and all surrounding heat cannot be utilized in three dimensions, resulting in low heat utilization efficiency.
[0004] Japanese Patent Application Laid-Open No. 2010-147236 Japanese Patent Application Laid-Open No. 2003-219669 International Publication No. 2017 / 038988 International Publication No. 2020 / 031992
[0005] "Renewable and Sustainable Energy Reviews" (Netherlands), 2014, Vol. 33, p. 371
[0006] A heat-powered battery capable of converting thermal energy into electrical energy has been developed by combining a thermoelectric conversion material that generates thermally excited electrons and holes with an electrolyte (Patent Document 3). The present inventors have developed an even more stable heat-powered battery (Patent Document 4). However, a heat-powered battery that can be used in a wider variety of locations and applications has been anticipated. Therefore, an object of the present invention is to provide a heat-powered battery that can be used in a wider variety of locations and applications.
[0007] The present inventors have conducted extensive research into thermal power generation cells that can be used in a variety of locations and applications, and have surprisingly found that an all-resin thermal power generation element that does not have a metal foil can be used in a variety of applications. The present invention is based on this finding. Therefore, the present invention provides: [1] an all-resin thermal power generation element including a semiconductor layer that generates thermally excited electrons and holes, an electrolyte layer containing a solid electrolyte or electrolyte solution in which charge-transporting ion pairs can move, and a conductive polymer layer containing an electron transport material, wherein no metal layers are present on the outside of either the semiconductor layer or the conductive polymer layer; [2] a laminated all-resin thermal power generation element in which two or more all-resin thermal power generation elements according to [1] are stacked; [3] a laminated all-resin thermal power generation element according to [2], which has metal layers on the outside of one semiconductor layer and on the outside of the other conductive polymer layer of the laminated all-resin thermal power generation element; [4] a thermal power generation element according to any one of [1] to [3], in which the thermally excited electron density of the semiconductor that generates thermally excited electrons and holes in the semiconductor layer is 10 15 / m 3 [5] a thermoelectric power generation device including the heat utilization power generation element according to any one of [1] to [3]; [6] a thermobattery including the thermoelectric power generation element according to any one of [1] to [3]; [7] a thermoelectric power generation module including the thermoelectric power generation element according to any one of [1] to [3]; [8] a thermoelectric power generation method including the steps of installing the thermoelectric power generation module according to [7] at a heat generation location and heating the thermoelectric power generation module with the heat to generate electric power; and [9] the thermoelectric power generation method according to [8], wherein the heat is geothermal heat or exhaust heat.
[0008] The all-resin thermal power generation element of the present invention does not have metal foil, so it can be made lighter in weight. The all-resin thermal power generation element of the present invention does not have metal foil, so it is highly flexible and can be applied to places where bending is required, and it can also be made smaller. The all-resin thermal power generation element of the present invention does not have metal foil, but can be made to stand on its own. The all-resin thermal power generation element of the present invention does not have metal foil, so interfacial resistance can be reduced. The all-resin thermal power generation element of the present invention does not have metal foil, so it is possible to reduce raw material costs, the manufacturing process is simplified, and it can be manufactured in a short time. The all-resin thermal power generation element of the present invention can prevent the risk of internal shots due to cracks in the metal film.
[0009] Fig. 1 is a diagram showing a conventional thermal power generation element. Fig. 2 is a diagram showing an all-resin thermal power generation element of the present invention. Fig. 3 is a diagram showing a conventional laminated thermal power generation element (A) having a metal layer between thermal power generation elements, and a laminated all-resin thermal power generation element (B or C) of the present invention which does not have a metal layer between the all-resin thermal power generation elements. (B) has a metal layer on the outside of one semiconductor layer and on the outside of the other conductive polymer layer of the laminated all-resin thermal power generation element. Fig. 1 shows (A) the adhesion between a semiconductor layer and metal foil produced by a conventional method, and (B) the adhesion between a semiconductor layer and metal foil produced by the method of the present invention.
[0010] [1] All-resin thermoelectric generator The all-resin thermoelectric generator of the present invention includes a semiconductor layer that generates thermally excited electrons and holes, an electrolyte layer containing a solid electrolyte or electrolyte solution through which charge-transporting ion pairs can migrate, and a conductive polymer layer containing an electron transport material. The all-resin thermoelectric generator of the present invention does not include a metal layer on the outside of either the semiconductor layer or the conductive polymer layer. As used herein, "all-resin" means that the internal active cell structure does not include a metal layer, and the semiconductor layer, electrolyte layer, and conductive polymer layer contain resin. Although no metal is used in the laminate structure, metal current collectors may be used for the positive and negative electrodes. Furthermore, metal wires, carbon sheets, graphene, or conductive fibers can be used as current collectors instead of metal layers.
[0011] <Semiconductor Layer> The semiconductor layer constituting the thermoelectric power generation element of the present invention includes a semiconductor. In this specification, "semiconductor" refers to a material that can generate thermally excited electrons and holes by heat. Specific examples include metal semiconductors, tellurium compound semiconductors, silicon germanium (Si-Ge) compound semiconductors, silicide compound semiconductors, skutterudite compound semiconductors, clathrate compound semiconductors, Heusler compound semiconductors, half-Heusler compound semiconductors, metal oxide semiconductors, organic semiconductors, and other semiconductors. The semiconductor used in the present invention functions as a thermoelectric conversion material.
[0012] Examples of metal semiconductors include Si semiconductors and Ge semiconductors. Examples of tellurium compound semiconductors include Bi-Te compounds (e.g., Bi 2 Te 3 , Sb 2 Te 3 , CsBi 4 Te 6 , Bi 2 Se 3 , Bi 0.4 Sb 1.6 Te 3 , Bi 2 (Se, Te) 3 , (Bi, Sb) 2 (Te, Se) 3 , (Bi, Sb) 2 Te 3 , or Bi 2 Te 2.95 Se 0.05 ), Pb—Te compounds (e.g., PbTe or Pb 1-x Sn x Te), SnTe, Ge-Te, AgSbTe 2 , Ag—Sb—Ge—Te compounds (e.g., GeTe—AgSbTe 2 (TAGS)), Ga 2 Te 3 , (Ga 1-x In x ) 2 Te 3 , Tl 2 Te-Ag 2 Te, Tl 2 Te-Cu 2 Te, Tl 2Te-Sb 2 Te 3 , Tl 2 Te-Bi 2 Te 3 , Ti 2 Te-GeTe, Ag 8 Tl 2 Te 5 , Ag 9 TlTe 5 , Tl 9 BiTe 6 , Tl 9 SbTe 6 , Tl 9 CuTe 5 , Tl 4 SnTe 3 , Tl 4 PbTe 3 , or Tl 0.02 Pb 0.98 Te can be mentioned.
[0013] Silicon germanium (Si-Ge) compound semiconductors include Si x Ge 1-x , or SiGe-GaP.
[0014] Silicide compound semiconductors include β-FeSi 2 Compounds (e.g., β-FeSi 2 , Fe 1-x Mn x Si 2 , Fe 0.95 Mn 0.05 Si (2-y) Al y , FeSi (2-y) Al y , Fe 1-y Co y Si 2 ), Mg 2 Si, MnSi 1.75-x , Ba 8 Si 46 , Ba 8 Ga 16 Si 30 , or CrSi 2 Examples include:
[0015] The skutterudite compound semiconductor includes a compound of the formula TX 3wherein T is a transition metal selected from the group consisting of Co, Fe, Ru, Os, Rh, and Ir, and X is a pnictogen selected from the group consisting of P, As, and Sb; 4 X 12 (wherein R is a rare earth selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu; M is selected from the group consisting of Fe, Ru, Os, and Co; and X is selected from the group consisting of P, As, and Sb), a compound represented by the formula: Yb y Fe 4-x Co x Sb 12 , (CeFe 3 CoSb 12 ) 1-x (MoO 2 ) x or (CeFe 3 CoSb 12 ) 1-x (W.O. 2 ) x Examples include:
[0016] The clathrate compound semiconductor is a compound of the formula M 8 X 46 (M is selected from the group consisting of Ca, Sr, Ba, and Eu, and X is selected from the group consisting of Si, Ge, and Sn), a compound represented by formula (II) 8 (III) 16 (IV) 30 (wherein II is a Group II element, III is a Group III element, and IV is a Group IV element) 8 (III) 16 (IV) 30 Examples of the compound include Ba 8 Ga x Ge 46-x , Ba 8-x (Sr, Eu) x Au 6 Ge 40 , or Ba 8-x EU x Cu 6 Si 40) can be mentioned.
[0017] Heusler compound semiconductors include Fe 2 Val, (Fe 1-x Re x ) 2 Val or Fe 2 (V 1-x-y Ti x Ta y ) Al can be mentioned.
[0018] Examples of half-Heusler compound semiconductors include compounds represented by the formula MSiSn (wherein M is selected from the group consisting of Ti, Zr, and Hf), compounds represented by the formula MNiSn (wherein M is Ti or Zr), compounds represented by the formula MCoSb (wherein M is selected from the group consisting of Ti, Zr, and Hf), and compounds represented by the formula LnPdX (wherein Ln is selected from the group consisting of La, Gd, and Er, and X is Bi or Sb).
[0019] As the metal oxide semiconductor, In 2 O 3 -SnO 2 , (CaBi)MnO 3 , Ca(Mn,In)O 3 , Na x V 2 O 5 , V 2 O 5 , ZnMnGaO 4 and its derivatives, LaRhO 3 , LaNiO 3 , SrTiO 3 , SrTiO 3 : Nb, Bi 2 Sr 2 Co 2 O y , Na x CoO 2 , NaCo 2 O 4 , CaPd 3 O 4 , formula Ca a M 1 b Co c M 2 d Age O f (In the formula, M 1 is one or more elements selected from the group consisting of Na, K, Li, Ti, V, Cr, Mn, Fe, Ni, Cu, Zn, Pb, Sr, Ba, Al, Bi, Y and rare earth elements, and M 2 is one or two elements selected from the group consisting of Ti, V, Cr, Mn, Fe, Ni, Cu, Mo, W, Nb, Ta and Bi, and 2.2≦a≦3.6, 0≦b≦0.8, 2≦c≦4.5, 0≦d≦2, 0≦e≦0.8, 8≦f≦10), ZnO, Na(Co,Cu) 2 O 4 , ZnAlO, Zn 1-x Al x O or La 1.98 Sr 0.02 CuO 4 Examples include:
[0020] The organic semiconductor may include an organic perovskite, a polyaniline, a polyacetylene, a polythiophene, a polyalkylthiophene, or a polypyrrole.
[0021] Other semiconductors include alloys containing Co and Sb (e.g., CoSb 3 , CeFe 3 CoSb 12 , CeFe 4 CoSb 12 , or YbCo 4 Sb 12 ), alloys containing Zn and Sb (e.g., ZnSb, Zn 3 Sb 2 , or Zn 4 Sb 3 ), alloys containing Bi and Sb (e.g., Bi 88 Sb 12 ), CeInCu 2 , (Cu, Ag) 2 Se, Gd 2 Se 3 , CeRhAs, or CeFe 4 Sb 12 , Li 7.9 B 105 , BaB 6 , SrB 6 , CaB6 , AlPdRe compounds (e.g., Al 71 Pd 20 (Re 1-x Fe x ) 9 ), AlCuFe quasicrystal, Al 82.6-x Re 17.4 Si x 1 / 1-cubic approximation crystal, YbAl 3 , YbMn x Al 3 , β-CuAgSe, B 4 C / Ba 3 C, (Ce 1-x La x ) Ni 2 , or (Ce 1-x La x ) In 3 Examples include:
[0022] The semiconductor layer may contain components other than the semiconductor, as long as the semiconductor can generate a sufficient number of thermally excited electrons and holes for power generation when heated to an appropriate temperature. Examples of such components include, but are not limited to, binders (polyvinyl alcohol, methyl cellulose, acrylic resin, agar, etc.) that bind the thermoelectric conversion material, and sintering aids (magnesium oxide, yttrium oxide, calcium oxide, etc.) that help form the thermoelectric conversion material. Solvents used in the manufacturing process may also remain. The first layer used in the present invention essentially functions as a thermoelectric conversion layer. The semiconductor layer of the present invention contains a resin. Examples of resins include, but are not limited to, the binders described above.
[0023] <Electrolyte Layer> The electrolyte layer contains a solid electrolyte or an electrolyte solution in which a charge-transporting ion pair can migrate. In this specification, the term "charge-transporting ion pair" refers to two stable ions with different valences, in which one ion is oxidized or reduced to form the other ion, and the ions can transport electrons and holes. They may also be ions of the same element but with different valences. The ion source contained in the solid electrolyte of the present invention is not particularly limited as long as it is a metal ion, and examples thereof include copper ions, iron ions, vanadium ions, manganese ions, nickel ions, tin ions, zinc ions, aluminum ions, calcium ions, potassium ions, magnesium ions, palladium ions, titanium ions, alkali metal ions, and rare earth metal ions. For example, copper ions or iron ions include monovalent copper ions, divalent copper ions, divalent iron ions, and trivalent iron ions. However, copper ions or iron ions are preferably two stable ions with different valences. This is because one ion is oxidized or reduced to form the other ion, and the copper ions or iron ions can transport electrons and holes. Therefore, in the case of copper ions, monovalent copper ions and divalent copper ions are preferred, and in the case of iron ions, divalent iron ions and trivalent iron ions are preferred. As the monovalent copper ions, for example, CuCl, CuBr, copper(I) acetate, copper(I) iodide, or copper(I) sulfate can be used. As the divalent copper ions, CuCl 2 , CuTSFI 2 , copper(II) acetate, copper(II) sulfate, or copper(II) acetylacetonate can be used. As the divalent iron ion, Fe(C 5 H 5 ) 2 (Ferrocene), K 4 [Fe(CN) 6 ], iron(II) acetylacetonate, iron(II) chloride, iron(II) sulfate, or iron(II) acetate can be used. 3 , K. 3 [Fe(CN) 6 ], iron(III) acetylacetonate or iron(III) sulfate can be used.
[0024] The concentration of the ion source is not particularly limited as long as the effects of the present invention can be obtained, but it is preferable to add the ion source so that the concentration is, for example, 0.01 to 98 mol % relative to the polymer, etc. By being in this range, the ion source can efficiently transport electrons and holes.
[0025] (Electrolyte) The electrolyte includes a solid electrolyte or an electrolyte solution. The electrolyte is not particularly limited as long as it can transport two ions of a charge-transporting ion pair. That is, the electrolyte used in the electrolyte layer is not particularly limited as long as its redox potential is in an appropriate position relative to the valence electron charge potential of the thermoelectric conversion material used in the thermoelectric power generation element and the charge-transporting ion pair can move back and forth within the electrolyte. Note that the electrolyte is preferably physically and chemically stable at a temperature at which the thermoelectric conversion material generates a sufficient number of thermally excited electrons and holes for power generation.
[0026] The electrolyte may be a solid electrolyte or an electrolyte solution (liquid electrolyte) depending on its form. Here, the electrolyte may be in the form of an electrolyte solution (liquid electrolyte) or a solid electrolyte depending on the temperature. That is, the compounds contained in the electrolyte solution (liquid electrolyte) and the compounds contained in the solid electrolyte overlap. Furthermore, electrolytes include molten salts, ionic liquids, deep eutectic solvents, and the like. Molten salts refer to salts composed of cations and anions in a molten state. Molten salts with relatively low melting points (e.g., 100°C or less, or 150°C or less) are referred to as ionic liquids. However, in this specification, molten salts in a solid state are referred to as solid electrolytes, and those in a solution state are referred to as electrolyte solutions (liquid electrolytes). Specific examples of electrolyte solutions (liquid electrolytes), solid electrolytes, and molten salts are provided below, but these terms may overlap.
[0027] The electrolyte solution used is in a solution (liquid) state at a temperature at which the semiconductor in the semiconductor layer generates a sufficient number of thermally excited electrons and holes for power generation.Specific examples of the electrolyte solution include, but are not limited to, methoxide ions, hydrogen ions, ammonium ions, pyridinium ions, lithium ions, sodium ions, potassium ions, calcium ions, magnesium ions, aluminum ions, iron ions, copper ions, zinc ions, cobalt ions, fluoride ions, cyanide ions, thiocyanate ions, chloride ions, acetate ions, sulfate ions, carbonate ions, phosphate ions, bicarbonate ions, and bromine ions.
[0028] The solid electrolyte is in a solid state in which charge-transporting ion pairs can move inside at a temperature at which the semiconductor in the semiconductor layer generates a sufficient number of thermally excited electrons and holes for power generation. The use of a high-temperature solid electrolyte allows it to be used in a thermoelectric power generation element that uses a thermoelectric power generation element that generates thermally excited electrons and holes at high temperatures. Specific examples of the solid electrolyte include, but are not limited to, sodium ion conductors, copper ion conductors, lithium ion conductors, silver ion conductors, hydrogen ion conductors, strontium ion conductors, aluminum ion conductors, fluorine ion conductors, chloride ion conductors, and oxide ion conductors. Specific examples of the solid electrolyte include RbAg 4 I 5 , Li 3 N, Na 2 O.11Al 2 O 3 , Sr-β alumina, Al(WO 4 ) 3 , PbF 2 , PbCl 2 , (ZrO 2 ) 0.9 (Y 2 O 3 ) 0.1 , (Bi 2 O 3 ) 0.75 (Y 2 O 3 ) 0.25 , CuZr 2 (P.O. 4 )3 、CuTi 2 (0) 4 ) ) 3 、Cu x b 1-x Ti 1+x (0) 4 ) ) 3 、 ̈ 0.5 Cu 0.5 h 2 (0) 4 ) ) 3 、Cu 1+x Cr x Ti 2-x (0) 4 ) ) 3 、Cu 0.5 TiコrrOO 4 ) ) 3 、CuCr 2 b(b) 4 ) ) 3 、Cu 2 ccZr2OO 4 ) ) 3 、Cuウn 2 (0) 4 ) ) 3 、CuHf 2 (0) 4 ) ) 3 、i 7 La 3 h 2 9 12 、i 7 La 3 h 2-x b x 9 12 、i 7 La 3 h 2-x Taxッ 12 、i 5 La 3 Ta 2 9 12 、i 0.33 La 0.55 4iッ 3 、i 1.5 Al 0.5 Ge 1.5 P 3 9 12 、i 1.3 Al 0.3 Ti 1.7 P 3 9 12 、i 3P.O. 4 (LiPON), Li 4 SiO 4 -Li 3 P.O. 4 , Li 4 SiO 4 , or Li 3 BO 3 Examples include: a molten salt can be used as the solid electrolyte or the electrolyte solution; an ionic liquid can be used in the case of a thermoelectric power generation element used at a relatively low temperature; and a deep eutectic solvent (DES) can be used as the ionic liquid.
[0029] Examples of the molten salt include those containing at least one cation selected from the group consisting of imidazolium cation, pyridinium cation, piperidinium cation, pyrrolidinium cation, phosphonium cation, morpholinium cation, sulfonium cation, and ammonium cation, and at least one anion selected from the group consisting of carboxylate anion, sulfonate anion, halogen anion, tetrafluoroborate, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, and bis(fluorosulfonyl)imide. The electrolyte in the present invention functions as a hole transporting material.
[0030] The electrolyte layer is not limited as long as it can transport holes generated in the thermoelectric conversion material, and can contain components other than a solid electrolyte or an electrolyte solution. Examples of such components include, but are not limited to, solvents (water, methanol, toluene, tetrahydrofuran, etc.) that dissolve or disperse the electrolyte when forming the second layer, binders (polyvinyl alcohol, methyl cellulose, acrylic resin, agar, etc.) that bind the electrolyte, and sintering aids (magnesium oxide, yttrium oxide, calcium oxide, etc.) that help form the hole-transporting material. The second layer used in the present invention essentially functions as a hole-transport layer. The electrolyte layer contains a resin. Examples of resins include, but are not limited to, the binder or metal salt (ion source), a separator (made of resin), or an insulating ceramic.
[0031] The electrolyte layer can be formed by, for example, a squeegee method, a screen printing method, a sputtering method, a vacuum deposition method, a sol-gel method, or a spin coating method. 2 (P.O. 4 ) 3 was prepared by the sol-gel method, and the resulting sol was used to prepare a layered electrolyte layer by a squeegee method. Furthermore, when the electrolyte is an electrolyte solution (liquid electrolyte), the second layer is in a liquid phase. When the second layer is in a liquid phase, the second layer in the thermoelectric power generation element is preferably prepared during the fabrication of the thermoelectric power generation device, thermobattery, or thermoelectric power generation module. That is, the second layer can be prepared by providing a tank for holding the electrolyte solution (liquid electrolyte).
[0032] <Conductive Polymer Layer> The conductive polymer layer contains an electron transport material. Examples of the electron transport material include polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyaniline-based conductive polymers, and polypyrrole-based conductive polymers. Specific examples of the electron transport material include polyacetylene, poly(p-phenylene), poly(p-phenylenevinylene), and polyaniline.
[0033] The conductive polymer layer may contain components other than the electron transport material, as long as they can transport thermally excited electrons generated in the thermoelectric conversion material. Examples of such components include, but are not limited to, binders (such as polyvinyl alcohol, methyl cellulose, acrylic resin, and agar) that bind the electron transport material, and sintering aids (such as magnesium oxide, yttrium oxide, and calcium oxide) that help form the electron transport material. Solvents used in the manufacturing process may also remain. The third layer used in the present invention essentially functions as an electron transport layer. In the thermoelectric power generation element of the present invention, the electron conduction potential of the electron transport material is the same as or positive to the conduction potential of the semiconductor in the semiconductor layer. Therefore, the electron transport material can transport thermally excited electrons.
[0034] The conductive polymer layer can be produced by, for example, a squeegee method, a screen printing method, a sputtering method, a vacuum deposition method, a single crystal growth method, or a spin coating method. When using the spin coating method, the conductive polymer layer can be produced by dissolving the oxadiazole derivative in a polar solvent such as acetone and spin coating the solution onto the substrate or the first layer.
[0035] <<Laminated All-Resin Thermal Power Generation Element>> The all-resin thermal power generation element of the present invention can be used as a laminated all-resin thermal power generation element by stacking two or more all-resin thermal power generation elements. Conventional laminated thermal power generation elements have a metal layer between the stacked thermal power generation elements, as shown in FIG. 3A . In contrast, the laminated all-resin thermal power generation element of the present invention does not have a metal layer between the stacked thermal power generation elements, as shown in FIG. 3B or 3C . Furthermore, as shown in FIG. 3B , the laminated all-resin thermal power generation element may have a metal layer as a current collector on the outside of one semiconductor layer and on the outside of the other conductive polymer layer. Furthermore, instead of a metal layer, a metal wire, a carbon sheet, graphene, or a conductive fiber can be used as a current collector.
[0036] [2] Manufacturing Method of Semiconductor Layer The all-resin thermal power generation element of the present invention does not have a metal layer. Therefore, in the manufacturing method of the semiconductor layer, the semiconductor layer is peeled off from the metal foil substrate. Conventional manufacturing methods are coating and drying methods, which result in a large adhesive area between the semiconductor layer and the metal foil, as shown in Figure 4A, and a strong adhesive force between the semiconductor film and the metal foil. Therefore, it is difficult to peel off the semiconductor layer from the metal foil. According to the manufacturing method of the semiconductor layer of the present invention, the adhesive area between the semiconductor layer and the metal foil is small, as shown in Figure 4B, and the semiconductor film can be easily peeled off from the metal foil.
[0037] The method for manufacturing a semiconductor layer includes the steps of: (1) mixing a semiconductor material with a binder solution to obtain a semiconductor binder mixture; (2) mixing a solvent that cannot dissolve the binder to obtain a gel mixture; (3) applying the gel mixture to a metal foil and further sandwiching it between the metal foils; (4) applying pressure to the gel mixture sandwiched between the metal foils; and (5) peeling off the metal foils.
[0038] In the mixing step (1), a semiconductor material is mixed with a binder solution. The semiconductor material can be any of the semiconductor materials described in the "Semiconductor Layer" section above, without limitation. Examples of the binder include, but are not limited to, PVDF, PVA, PEC, PEG, PMMA, PA, PE, PPG, PP, PAI, PU, PI, and PPC. Examples of the solvent for dissolving the binder include, but are not limited to, NMP solution, DMSO solution, DMF solution, pyridine solution, toluene solution, acetone solution, and acetonitrile solution.
[0039] In the step (2) of obtaining the semi-solid mixture, a solvent that cannot dissolve the binder is added to obtain a semi-solid mixture. The semi-solid mixture can be obtained by adding a solvent that cannot dissolve the binder. Examples of solvents that cannot dissolve the binder include acetone, alcohol (e.g., methanol, ethanol, propanol, etc.), water, ether, and THF. The amount of solvent that cannot dissolve the binder added is not particularly limited as long as a semi-solid mixture can be obtained, but for example, 1 to 50 parts by volume, preferably 5 to 30 parts by volume, and more preferably 10 to 15 parts by volume can be added, based on 100 parts by volume of the semiconductor binder mixture.
[0040] In the step (3), the semi-solid mixture is applied to a metal foil and then sandwiched between two metal foils. That is, the semi-solid mixture is sandwiched between two metal foils. The metal foil is not particularly limited, but examples thereof include stainless steel foil, copper foil, aluminum foil, titanium foil, gold foil, silver foil, platinum foil, nickel foil, zinc foil, and brass foil. However, without using a metal foil, the semi-solid mixture may be placed in a hydraulic press or the like and pressure may be applied in the following pressure application step (4). Although the hydraulic press or the like may become contaminated by the semi-solid mixture, the present invention can be sufficiently implemented.
[0041] In the pressure application step (4), pressure is applied to the semi-solid mixture. The pressure applied to the semi-solid mixture is not particularly limited as long as the effects of the present invention are obtained, but it is, for example, in the range of 0.01 to 200 MPa, with a preferred range being 0.1 MPa to 20 MPa. However, an even more preferred range is 1 to 10 MPa. The method for applying pressure is not particularly limited, but pressure can be applied using a hydraulic press or a hand press.
[0042] When a metal foil is used in the step (3), the metal foil is peeled off in the metal foil peeling step (5). Specifically, the upper metal foil is slowly peeled off so as not to tear the film, and the film is vacuum dried at, for example, 25°C to 80°C, preferably 50°C to 70°C. After vacuum drying, the lower metal foil is slowly peeled off so as not to tear the free-standing film.
[0043] [3] Method for Producing a Conductive Polymer Layer A conductive polymer dispersion is dropped onto a metal foil. After uniformly dispersing to the required thickness, the resulting mixture is dried at high temperatures. The dried polymer metal foil is left in an inert gas atmosphere. A conductive polymer layer is obtained. The metal foil is not particularly limited, but examples include stainless steel foil, copper foil, aluminum foil, titanium foil, gold foil, silver foil, platinum foil, nickel foil, zinc foil, and brass foil. Examples of the conductive polymer include polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyaniline-based conductive polymers, and polypyrrole-based conductive polymers. Specific examples of electron transport materials include polyacetylene, poly(p-phenylene), poly(p-phenylenevinylene), and polyaniline.
[0044] [4] Power Generation Method The power generation method of the present invention is characterized in that the thermoelectric power generation element is formed by heating the thermoelectric power generation element so that the thermally excited electron density of the semiconductor that generates thermally excited electrons and holes in the semiconductor layer is 10 15 / cm 3 In the power generation method of the present invention, the thermally excited electron density is preferably 10 15 / cm 3 More preferably, 10 18 / cm 3 More preferably, 10 20 / cm 3 More than 10, most preferably 22 / cm 3 That's all. The higher the thermally excited electron density, the higher the power generation efficiency that can be obtained. The temperature applied to the semiconductor can be appropriately selected so that a sufficient number of thermally excited electrons and holes are generated in each semiconductor for power generation. In other words, in the present invention, a voltage can be generated in the thermoelectric power generation element by applying a temperature to the semiconductor at which a sufficient number of thermally excited electrons and holes are generated in the semiconductor for power generation. The number of thermally excited electrons and holes sufficient for power generation is actually expressed as electron density, and may be approximately the same as the number of photoexcited electrons in the semiconductor used in solar cells, for example, 10, which is the number of photoexcited electrons in amorphous silicon used in solar cells. 15 / cm 3That is, in the thermoelectric conversion material used in the present invention, the thermally excited electron density is 10 15 / cm 3 At temperatures above this temperature, it is possible to generate a sufficient number of thermally excited electrons and holes for power generation, and power generation is possible at temperatures above this temperature.
[0045] [5] Thermoelectric Generator, Thermobattery, and Thermoelectric Generation Module The thermoelectric generator of the present invention includes the thermoelectric generation element of the present invention, preferably including a positive electrode and / or a negative electrode. The thermobattery of the present invention includes the thermoelectric generation element of the present invention, preferably including a positive electrode and / or a negative electrode. The thermoelectric generation module of the present invention includes the thermoelectric generation element of the present invention, preferably including a positive electrode and / or a negative electrode. As used herein, the term "thermobattery" refers to a battery that includes the thermoelectric generation element of the present invention and generates electricity by applying a temperature sufficient to generate thermally excited electrons and holes to the semiconductor (thermoelectric conversion material) of the thermoelectric generation element. In other words, a thermobattery is a "battery that generates electricity when there is a heat source" and is different from conventional "batteries that generate electricity using high-temperature and low-temperature regions."
[0046] <Electrodes> The positive and negative electrodes are not limited as long as they can transport electrons. Examples include titanium, gold, platinum, silver, copper, tin, tungsten, niobium, tantalum, stainless steel, aluminum, graphene, molybdenum, indium, vanadium, rhodium, niobium, chromium, nickel, carbon, alloys thereof, and combinations thereof. The same material may be used for the positive and negative electrodes. The positive and negative electrodes may be provided in the form of conductors or as positive electrode layers or negative electrode layers. The positive and negative electrode layers may be manufactured by vacuum deposition, spin coating, or the like. By providing a negative electrode on the third layer side of the thermoelectric power generation element and a positive electrode on the second layer side, electrons can move from the negative electrode to the positive electrode, generating electricity.
[0047] [6] Thermoelectric Power Generation Method The thermoelectric power generation method of the present invention includes the steps of placing the thermoelectric power generation module at a heat generation location, and heating the thermoelectric power generation module with heat to generate electric power.
[0048] <<Thermoelectric Power Generation Module Installation Step>> In the thermoelectric power generation module installation step, the thermoelectric power generation module of the present invention is installed at a heat generation location. The heat generation location is not particularly limited, as long as it generates heat at a temperature equal to or higher than the temperature at which the thermoelectric conversion material generates a sufficient number of excited electrons and holes for power generation. However, a relatively high-temperature location is preferable because it allows for efficient power generation. Therefore, examples of heat generation locations include geothermal generation locations and waste heat generation locations such as factories. Geothermal energy is not limited to heat in the soil but also includes hot water or steam heated by geothermal energy. Furthermore, geothermal energy includes hot water or steam heated by geothermal energy from oceans, lakes, rivers, etc. The waste heat is not particularly limited, but examples include waste heat from steel furnaces, waste incinerators, substations, subways, automobiles, etc. In particular, waste heat from steel furnaces and waste incinerators, which have large amounts of energy, is released without being utilized, and it is preferable to reuse this energy using the thermoelectric power generation method of the present invention.
[0049] In the power generation step, the thermoelectric power generation module of the present invention is heated to generate electric power. The heat generated from the heat generation location heats the thermoelectric conversion material of the thermoelectric power generation module to a temperature at or above which a sufficient number of excited electrons and holes are generated for power generation, thereby enabling the thermoelectric power generation module to generate electric power.
[0050] The present invention will be specifically described below with reference to examples, but these examples are not intended to limit the scope of the present invention.
[0051] Example 1 (Preparation of a free-standing PEDOT:PSS film) A conductive polymer layer was prepared. 1 mL of PEDOT / PSS dispersion was applied and dispersed onto a mirror-finished copper foil and dried at 120°C. The resulting film was then left in an argon gas atmosphere for several hours, and the free-standing PEDOT / PSS film was peeled off.
[0052] (Electrolyte Preparation) An electrolyte layer was prepared. 5% polyvinylidene fluoride (PVDF) was dissolved in N-methyl-2-pyrrolidone (NMP) by heating at 60°C to prepare a PVDF (5%) solution. 166 mg of lithium chloride (LiCl) was dissolved in 8 g of this solvent by heating at 60°C. 68 mg of copper chloride (I) and 94 mg of copper chloride (II) were added and dissolved by heating at 60°C. The obtained electrolyte solution was added dropwise to the separator. Once the separator was immersed in the electrolyte solution, it was heated at 60°C and vacuum dried.
[0053] (Preparation of a free-standing semiconductor film) A semiconductor layer was prepared. 200 mg of Ge was placed in a mortar and crushed. 2.0 g of binder solution (PVDF in NMP) was added and stirred. Next, 1 mL of acetone, a solvent that cannot dissolve the binder, was added to make the semiconductor mixture semi-solid. A stainless steel foil was placed on top of the semiconductor mixture and sandwiched between another piece of stainless steel foil. The mixture was clamped in a vice (universal angle vise, Palmgren) at room temperature for 1 hour at a pressure of 2 MPa. The mixture was removed from the pressure machine, the upper and lower stainless steel foils were peeled off, and the mixture was vacuum dried at 60°C to obtain a free-standing semiconductor film.
[0054] The "conductive polymer layer," "electrolyte layer," and "semiconductor layer" obtained in the above steps were laminated as follows to obtain the all-resin thermal power generation element of the present invention. The power generation unit of the all-resin thermal power generation element was obtained by stacking the "conductive polymer layer" (positive electrode) / "electrolyte layer" / "semiconductor layer" (negative electrode) in this order (Figure 2). Furthermore, multiple units described above can be stacked to produce an all-resin thermal power generation element.
[0055] In this example, the procedure of Example 1 was repeated to obtain an all-resin thermal power generation element of the present invention, except that PVA was used instead of PVDF as the binder. In producing a free-standing semiconductor film, the stainless steel foil was easily peeled off from the semiconductor layer.
[0056] Example 3 In this example, the procedure of Example 1 was repeated to obtain an all-resin thermal power generation element of the present invention, except that PEC was used instead of PVDF as the binder. In producing a free-standing semiconductor film, the stainless steel foil was easily peeled off from the semiconductor layer.
[0057] Comparative Example 1 In this example, a thermoelectric power generation element with a metal layer was fabricated according to a conventional method. (Preparation of a PEDOT:PSS film) A conductive polymer layer was fabricated. 1 mL of PEDOT / PSS dispersion was applied and dispersed onto a mirror-finished copper foil and dried at 120°C. The foil was then left to stand for several hours under an argon gas atmosphere. A PEDOT / PSS film with a mirror-finished copper foil was obtained.
[0058] (Electrolyte Preparation) An electrolyte layer was prepared. 5% polyvinylidene fluoride (PVDF) was dissolved in N-methyl-2-pyrrolidone (NMP) by heating at 60°C to prepare a PVDF (5%) solution. 166 mg of lithium chloride (LiCl) was dissolved in 8 g of this solvent by heating at 60°C. 68 mg of copper chloride (I) and 94 mg of copper chloride (II) were added and dissolved by heating at 60°C. The obtained electrolyte solution was added dropwise to the separator. Once the separator was immersed in the electrolyte solution, it was heated at 60°C and vacuum dried.
[0059] (Preparation of Semiconductor Layer with Metal Foil) A semiconductor layer was prepared. 200 mg of Ge was placed in a mortar and ground. 2.0 g of binder solution (PVDF in NMP) was added and stirred. The mixture was dropped onto a stainless steel foil, and a film was prepared using an applicator. The coated metal foil was dried in a vacuum at 60°C. The metal foil could not be peeled off from the semiconductor layer.
[0060] The "conductive polymer layer," "electrolyte layer," and "semiconductor layer" obtained in the above steps were stacked as follows to obtain a conventional thermal power generation element. The power generation unit of the conventional thermal power generation element was obtained by stacking the "conductive polymer layer" (positive electrode), "electrolyte layer," and "semiconductor layer" (negative electrode) in this order (Figure 1).
[0061] The all-resin heat-utilizing power generation element of the present invention is highly flexible because it does not have metal foil, and can be applied to places where bending is required, and can also be made smaller.
Claims
1. An all-resin thermal power generation element comprising: a semiconductor layer that generates thermally excited electrons and holes; an electrolyte layer that contains a solid electrolyte or electrolyte solution in which charge-transporting ion pairs can move; and a conductive polymer layer that contains an electron transport material, wherein the all-resin thermal power generation element does not contain any metal layers on the outside of either the semiconductor layer or the conductive polymer layer.
2. A laminated all-resin heat-utilizing power generation element comprising two or more laminated all-resin heat-utilizing power generation elements as described in claim 1.
3. The laminated all-resin heat-utilizing power generating element according to claim 2, which has a metal layer on the outside of one of the semiconductor layers and on the outside of the other conductive polymer layer of the laminated all-resin heat-utilizing power generating element.
4. The thermal energy generating element according to claim 1 is configured such that the thermally excited electron density of the semiconductor that generates thermally excited electrons and holes in the semiconductor layer is 10 15 / m 3 This method generates electricity by placing the device in an environment where the temperature is above the limit.
5. A thermoelectric power generation device comprising the heat utilization power generation element according to claim 1.
6. A thermobattery comprising the thermoelectric generating element according to claim 1.
7. A thermoelectric power generation module comprising the thermoelectric power generation element according to claim 1.
8. A thermoelectric power generation method comprising the steps of: placing the thermoelectric power generation module according to claim 7 at a heat generation location; and heating the thermoelectric power generation module with heat to generate electric power.
9. The thermoelectric power generation method according to claim 8, wherein the heat is geothermal heat or exhaust heat.
Citation Information
Patent Citations
Power generation module utilizing heat and thermoelectric power generation device including the same
JP2021005649A
Thermoelectric power generating element, thermoelectric power generating battery, and power generation stabilizing method
WO2022191101A1