Sheet body
The sheet body with controlled adhesive strength and weather-resistant properties addresses the challenges of durability and handling in structure reinforcement, ensuring strong adhesion and ease of use for structure repair.
Patent Information
- Application Number
- PCT/JP2024/015408
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-17
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional sheet materials for structure reinforcement and repair lack durability, weather resistance, and ease of handling, particularly in windy conditions and on complex surfaces, as they tend to wrinkle, detach easily, and require frequent replacement.
A sheet body with a controlled adhesive strength, measured between 1.5 N/25 mm and less than 100% of the maximum tensile elastic region, ensuring strong adhesion while allowing for easy peeling and reattachment, and incorporating a weather-resistant layer to maintain waterproofness and rigidity.
The sheet body provides reliable adhesion, weather resistance, and ease of handling, allowing for successful initial application and reapplication without damage, reducing waste and environmental impact.
Smart Images

Figure JP2024015408_24102024_PF_FP_ABST
Abstract
Description
Sheet body
[0001] The present disclosure relates to a sheet body that is attached to a structure to be used for reinforcing or repairing the structure. More specifically, the present disclosure relates to a sheet body that has excellent adhesiveness to the structure and can be peeled off and reattached at the construction site even after being attached to the structure.
[0002] Various structures, such as ordinary houses and commercial buildings, are known. Examples of roofs for structures include slate roofs, metal roofs, Galvalume steel roofs, and concrete roofs, including flat roofs (also called "rikuyane" or "rokuyane" in Japanese). These structures can develop leaks due to deterioration caused by long-term exposure to wind and rain, or damage caused by disasters such as typhoons. For this reason, emergency repairs are often performed when deterioration or damage occurs to the roof of a structure.
[0003] 23, a commonly known method of emergency repair for a roof is to place a blue tarp 31 to cover the damaged area of a roof 30, and then place multiple sandbags 32 as weights on top of the blue tarp 31 to secure the blue tarp 31. Other methods that can be used as weights include bags filled with water, as disclosed in Patent Documents 1 and 2, for example.
[0004] However, when repairing a roof using a conventional blue tarp 31, it is difficult to prevent wrinkles in the blue tarp 31. Furthermore, the surface of a roof is usually not flat. This causes gaps between the blue tarp 31 and the roof, which can allow water to seep in through these gaps. There is also the problem that the blue tarp 31 can be blown away by strong winds such as those from typhoons. Furthermore, blue tarps 31 usually do not have very high weather resistance and deteriorate within about a year, requiring replacement.
[0005] To address the above-mentioned issues, for example, as disclosed in Patent Document 3, a surface sheet material used for finishing exterior walls formed from ALC panels is known, which comprises a sheet substrate that is a woven fabric formed by weaving glass fibers, waterproof paint, and an intermediate layer formed between the two and composed of a mixture of an inorganic material and a flexible resin material.
[0006] JP 2010-144360 A JP 2000-16886 A Registered Utility Model No. 3009544 A
[0007] According to the facing sheet material disclosed in Patent Document 3, even if cracks occur in the joints of the ALC panels, the joints are covered by the facing sheet material. Therefore, the appearance is not affected. Furthermore, by filling small gaps between adjacent facing sheet materials with a waterproof sealant, it is possible to prevent rainwater from entering. However, although such facing sheet materials are attached to the ALC panels with an adhesive, it is difficult to say that the facing sheet can be stably attached for a long period of time, as it is exposed to various environments.
[0008] In consideration of these conventional problems, the applicant of the present patent application (hereinafter also referred to as "the present applicant") has developed a structure protection sheet comprising a polymer cement layer and a resin layer, with a specifically controlled thickness distribution, as previously disclosed in International Publication No. 2021 / 010456. This structure protection sheet can be used both for preliminary reinforcement of newly constructed structures and for repairing structures that have already deteriorated over time. Furthermore, it can be attached to structures via adhesive, significantly reducing the construction time required to install a protection sheet on the surface of a structure's roof. Furthermore, its excellent strength allows for long-term protection of structures.
[0009] Here, it has been found that while the structure protection sheet can impart excellent weather resistance to a structure, depending on the skill level of the worker applying it to the structure, it may not be applied neatly or evenly to the structure, resulting in wrinkles and the like. When a worker does not apply the sheet neatly or evenly to a structure, there is a demand for the sheet to be peeled off and reapplied. However, conventional structure protection sheets have been developed with the primary aim of increasing adhesive strength when applied to a structure in order to impart adhesiveness to the structure. As a result, once applied, the sheet could not be peeled off and reapplied. More specifically, once peeled off, the structure protection sheet would be damaged, losing its adhesiveness and weather resistance properties, and therefore could not be reapplied. As a result, application at the construction site was not successful the first time, and the peeled structure protection sheet had to be discarded. As such, conventional structure protection sheets had issues with ease of handling at construction sites.
[0010] Therefore, the present disclosure has been made to solve the above-mentioned problems, and its purpose is to provide a sheet body that has excellent adhesion to structures while also improving handleability at construction sites.
[0011] As a result of intensive research, the present inventors have found that, from the viewpoint of ensuring weather resistance, the sheet body of the present disclosure needs to have an adhesive strength of a certain value or more in the 180° peel test described below before being attached to a structure. Furthermore, from the viewpoint of improving handling such as re-attachment, it has been found that it is important to control the adhesive strength of the sheet body before being attached to a structure to a value less than 100% of the maximum test force in the tensile elastic region described below. The present disclosure has been completed based on the above findings.
[0012] A first aspect of the present disclosure is a sheet body that is attached to a structure to be used for reinforcing or repairing the structure, and that, before being attached to the structure, has an adhesive strength that is a measured value of 1.5 N / 25 mm or more in a 180° peel test and is a value that is less than 100% of the maximum test force in the tensile elastic region.
[0013] According to this first aspect, it is possible to improve the ease of handling of the sheet body at the construction site while ensuring excellent adhesive strength of the sheet body to the structure. More specifically, by setting the upper limit of the adhesive strength of the sheet body to a value less than 100% of the maximum test force in the tensile elastic region, the sheet body is less likely to undergo plastic deformation when peeled off after being applied, making the sheet body less likely to be damaged, and making it possible to re-apply the sheet body.
[0014] Furthermore, a second aspect of the present disclosure is based on the first aspect, and has an adhesive strength such that the measured value of the 180° peel strength after a weather load test is 1.5 N / 25 mm or more.
[0015] According to this second aspect, the adhesive strength after the weather load test (details of the test will be explained later) is ensured to be the same as before being attached to the structure, and a sheet body with excellent weather resistance can be provided.
[0016] Furthermore, a third aspect of the present disclosure is based on the first aspect and further has waterproofness such that there is no water leakage in a waterproofness test after a weather load test.
[0017] According to the third aspect, a predetermined waterproof property is ensured even after the weather resistance load test, and a sheet body having excellent weather resistance can be provided.
[0018] Furthermore, a fourth aspect of the present disclosure is based on the first aspect, and when a deformation test is conducted by sequentially performing the operations described in the following items (1), (2), (3), and (4), the energy calculated by the calculation in (4) below is a value of 2.0 mJ or more. (1) A rectangular sheet body having short sides of 50 mm and long sides of 100 mm is prepared as a sample. (2) The sample is curved so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample from the edges of the pair of short sides to a position 15 mm away along the long sides is gripped and fixed with a fixing portion, thereby forming a curved portion with a perimeter of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample arranged parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface having a diameter of 100 mm and a thickness of 10 mm is used, and the pressing tool is brought into contact with the curved portion from above in an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool is moved downward by 20 mm at a test speed of 30 mm / min. (4) The energy required to move the pressing tool is calculated.
[0019] According to this fourth aspect, it is possible to impart appropriate rigidity to the sheet body. Therefore, the sheet body can be easily handled when attached to the surface of a structure. More specifically, it becomes easier to lay the sheet body on the surface of a structure. Note that the "deformation test" referred to in this specification refers to the above-mentioned deformation test.
[0020] According to each of the above-mentioned aspects, the sheet body can have excellent adhesiveness to structures while improving the ease of handling at the construction site. Specifically, even if the sheet body is once attached to a structure and then peeled off, the sheet body can be reattached without being damaged (while maintaining adhesiveness and weather resistance).
[0021] In other words, each of the above-mentioned aspects allows the sheet body to be applied to a structure with excellent adhesive strength while also allowing the sheet body to be re-applied as needed, which are contradictory effects that have been difficult to achieve in the past. Therefore, the sheet body of each of the above-mentioned aspects allows the sheet body to be reliably applied to the target area of a structure, and improves the handling and workability during application work at the construction site. Furthermore, since the sheet body can be reused once peeled off, waste is reduced, which also contributes to environmental protection.
[0022] FIG. 1 is a cross-sectional view schematically showing a sheet body according to a second embodiment, the sheet body having a single adhesive layer and a single weather-resistant layer. FIG. 2 is a cross-sectional view schematically showing a sheet body according to a second embodiment, the sheet body having multiple base layers and multiple weather-resistant layers. FIG. 3 is a schematic diagram showing a state in which a release sheet is peeled from a sheet body according to the present disclosure. FIG. 4 is a schematic diagram showing a state in which the sheet body of FIG. 3 is attached to a structure. FIGS. 5(A), 5(B), 5(C), and 5(D) are schematic diagrams illustrating a method for measuring the rigidity of a sheet body according to the present disclosure. FIG. 6 is a schematic diagram showing an example of a reinforcing material for a sheet body according to the present disclosure. FIG. 7 is a partially enlarged view of the reinforcing material of FIG. 6. FIG. 8 is a schematic diagram showing a 180° peel test method. FIG. 9 is a graph showing how to determine the maximum test force in the tensile elastic region based on a tensile test. FIG. 10 is a graph showing how to determine the maximum test force in the tensile elastic region based on a tensile test. FIG. 11 is a graph showing the relationship between the stroke (mm) of the pressing jig and the test force (N). FIG. 12 is a perspective view of a mount simulating a roof. FIG. 13 is a diagram showing the side and dimensions of the mount of FIG. 12. FIG. 14 is a front view of the mount of FIG. 12. FIG. 15 is a schematic diagram of a method for measuring storage modulus. FIG. 16 is a graph showing an example of measurement of storage modulus. FIG. 17 is a cross-sectional view schematically showing a sheet body according to a third embodiment. FIG. 18 is a cross-sectional view schematically showing a sheet body according to a fourth embodiment. FIG. 19 is a cross-sectional view schematically showing a sheet body according to a fifth embodiment. FIG. 20 is a schematic diagram showing the structure of a supply item containing a sheet body according to the present disclosure. FIG. 21 is a schematic perspective view of a sheet body according to a sixth embodiment and a solar cell unit arranged on top of it. FIG. 22 is a schematic cross-sectional view of the sheet body and solar cell unit of FIG. 21. FIG. 23 is an explanatory diagram of a conventional roof repair method.
[0023] Hereinafter, the sheet body of the present disclosure will be described with reference to the drawings. Note that the present disclosure is not limited to the following description and the forms in the drawings, and various modifications are possible as long as the technical features thereof are maintained.
[0024] The sheet body of the present disclosure is a sheet body that is attached to a structure to reinforce or repair the structure, and has an adhesive strength that, before being attached to the structure, is a value measured in a 180° peel test of 1.5 N / 25 mm or more and is less than 100% of the maximum test force in the tensile elastic region. In other words, before being attached to the structure, the sheet body of the present disclosure has an adhesive strength with a lower limit measured in a 180° peel test of 1.5 N / 25 mm and an upper limit near 100% of the maximum test force in the tensile elastic region (the method for determining the value at which the maximum test force in the tensile elastic region is 100% will be described later). Therefore, the adhesive strength of the sheet body of the present disclosure at 100% of the maximum test force in the tensile elastic region is greater than the adhesive strength at 1.5 N / 25 mm measured in a 180° peel test. Note that the term "adhesion" used herein can also be replaced with the term "bonding."
[0025] [Structure] The structure to which the sheet body of the present disclosure is applied is not particularly limited. Examples of structures include concrete, wooden, and steel structures. From the viewpoint of the sheet body being applied once at the construction site and then peeled off and reapplied, other examples of structures include the roof, wall, eaves, fence, gatepost, gate, gate roof, etc. of a house. Such structures have more complex shapes than large structures such as bridge girders, and there is a risk of wrinkles in the sheet body, for example. For this reason, it is often difficult to apply the sheet body successfully in a single application operation. Therefore, the technical concept of the present disclosure is easily applicable to such structures. Below, the structure will be further explained using a roof as an example.
[0026] Further examples of structures include ordinary houses and large structures such as gymnasiums, hospitals, and public facilities. The sheet body of the present disclosure can be suitably attached to, for example, the roofs of such structures. The shape of the roof is not particularly limited. Examples of roofs include roofs of any shape, such as gable roofs, hip roofs, square roofs, flat roofs, shed roofs, and semi-cylindrical roofs.
[0027] Specific examples of roofs include slate roofs, roofs made of Galvalume Steel Sheets (registered trademark), galvanized steel roofs (roofs made of zinc-plated steel sheets), metal roofs made of painted iron, and concrete roofs, including flat roofs. Slate comprises a cement layer, an inorganic decorative (cement) layer disposed on the cement layer, an inorganic colored stone layer disposed on the inorganic decorative layer, and an inorganic coating disposed on the inorganic colored stone layer. Slate is widely used as a roofing material for ordinary houses due to its simple appearance, wide range of colors, light weight, and low cost. However, slate roofs are more prone to cracking than roofs made of Galvalume Steel Sheets (registered trademark), and have lower durability and waterproofing properties than roofs made of other materials. As a result, they are more susceptible to problems such as breakage. Therefore, slate roofs are particularly suitable as roofs to which the sheet of the present disclosure is attached. In the following description, the roof of a structure will also be referred to as a "slate roof, etc."
[0028] The surface of the roof may have steps similar to those found in a typical slate roof. Here, the sheet body of the present disclosure preferably has, for example, a specific rigidity. When the sheet body is applied to the roof of a structure, even if the roof of the structure has steps such as a slate roof, the formation of gaps can be prevented.
[0029] Furthermore, by applying the sheet member of the present disclosure to the roof of a structure, the sheet member can follow cracks and expansion that occur in the roof of the structure. This has the special effect of preventing deterioration factors such as water and chloride ions from penetrating into the interior of the roof of the structure and allowing moisture inside the roof of the structure to be discharged as water vapor. In particular, for slate roofs and the flat roofs mentioned above, which are materials that tend to accumulate rainwater, the ability to discharge water vapor is highly effective in preventing deterioration of the material.
[0030] [Characteristics of the Sheet Body] The sheet body of the present disclosure is used to reinforce or repair the surface of a structure. Specifically, the surface of a structure is reinforced or repaired by attaching one main surface of the sheet body of the present disclosure to the surface of the structure. Note that the object to which the sheet body of the present disclosure is attached is not limited to structures whose surface has deteriorated or been damaged. By attaching the sheet body of the present disclosure to the surface of a structure in advance, deterioration or damage can be prevented.
[0031] [1] <Adhesive strength of sheet body> The sheet body of the present disclosure has an adhesive strength (initial adhesive strength) of 1.5 N / 25 mm or more measured in a 180° peel test before being attached to a structure. This makes the sheet body less likely to peel off even when exposed to strong winds after being attached to the surface of a structure. Therefore, the sheet body can easily be stably maintained attached to the surface of a structure for a long period of time.
[0032] The measured value in a 180° peel test before application to a structure is, for example, preferably 5 N / 25 mm or more, more preferably 8 N / 25 mm or more. Furthermore, a value of 9 N / 25 mm or more is even more preferable, and a value of 12 N / 25 mm or more is particularly preferable. Furthermore, a value of 15 N / 25 mm or more is most preferable. Setting the measured value within any of the above ranges makes it easier to achieve the effect described in [1] above.
[0033] More specifically, when the measured value is set to 1.5 N / 25 mm or more, a sheet body that can withstand a strong wind range of 15 m / s is easily obtained. Furthermore, when the measured value is set to 5 N / 25 mm or more, a sheet body that can withstand a storm range of 25 m / s is easily obtained. Furthermore, when the measured value is set to 8 N / 25 mm or more, a sheet body that can withstand a storm range of 30 m / s is easily obtained. Furthermore, when the measured value is set to 9 N / 25 mm or more, a sheet body that can withstand a storm range of 45 m / s is easily obtained. Furthermore, when the measured value is set to 12 N / 25 mm or more, a sheet body that can withstand a storm range of 65 m / s is easily obtained. However, the adhesive strength of the sheet body before it is attached to a structure is set to a value less than 100% of the maximum test force in the tensile elastic region, as will be explained later, so that the sheet body can be peeled off and reattached after being attached at the construction site.
[0034] (180° Peel Test) The 180° peel test in this disclosure conforms to JIS Z0237:2022 "Test Methods for Pressure-Sensitive Adhesive Tapes and Sheets" and is carried out as follows. Test Equipment An "Autograph AGX-V 10kN" manufactured by Shimadzu Corporation is used. If this test equipment is difficult to obtain due to discontinuation of production, etc., a successor model of the test equipment or an equipment capable of equivalent measurements can be used. This also applies to other measuring equipment used in this disclosure. Test specimens are prepared as follows, with reference to JIS Z0237:2022 10.1. The materials to be prepared are as follows: Materials for preparing test specimens: (A) Rectangular PET film cut to a size of 25 mm on the short side and 200 mm on the long side (T601E (thickness 50 μm) manufactured by Mitsubishi Chemical Corporation or an equivalent product); (B) Rectangular double-sided adhesive tape cut to a size of 25 mm on the short side and 100 mm on the long side (No. 5015 (25 mm width) manufactured by Nitto Denko Corporation or an equivalent product); (C) Rectangular sheet of the present disclosure cut to a size of 25 mm on the short side and 100 mm on the long side (including a release sheet as described below, but the release sheet may be omitted); (D) Adherend: SUS304 steel plate according to JIS Z0237 10.2.2, with a surface finish of BA finish (hereinafter also referred to as "BASUS plate"); It has an edge size of 75 mm and a long side of 150 mm.
[0035] - Method for preparing 180° peel test specimen (1) The surface of a BASUS plate is cleaned using a nonwoven fabric "Bencott M-3II" (registered trademark) manufactured by Asahi Kasei Corporation or an equivalent product to which MEK (methyl ethyl ketone) has been attached. (2) The adhesive surface of the double-sided adhesive tape of (B) is attached to the side of the sheet body of (C) that does not have a release sheet (the side opposite to the side of the sheet body that will be attached to the structure (the side that will become the outer surface of the sheet-attached structure after the sheet body is attached to the structure) using a tape compression roll (manual type with a load of 2 kg). (3) The release liner of the double-sided adhesive tape of (B) that was attached to the sheet body of (C) in (2) is peeled off. Thereafter, the PET film of (A) is attached to the end of the 25 mm side of the sheet body of (C) and the double-sided adhesive tape of (B) using a tape compression roll (manual type with a load of 2 kg). (4) The release sheet of the sheet (C) with the PET film attached thereto prepared in (3) is peeled off, and the surface of the sheet that will be attached to the surface of the structure is attached to the BASUS plate prepared in (1). When attaching, a tape pressing roll (manual type with a 2 kg load) is moved back and forth twice to attach the sheet. (5) The test specimen prepared in (4) is stored at room temperature and humidity (23±2°C, 50±10% RH) for 24 hours.
[0036] 180° Peel Test Method: This test is performed in accordance with the method described in JIS Z0237 11.5. Specifically, the test method described in 11.5.1 is performed as "a test method in which the tape and sheet of Method 1 are peeled at 180° from a stainless steel test plate." The load cell used is set to 1 kN. The test conditions are set in an environment of a temperature of 23±2°C and a relative humidity of 50±5% RH.
[0037] FIG. 8 is a schematic diagram showing the 180° peel test method. In this test, for example, an apparatus having the configuration shown in FIG. 8 is used. In FIG. 8, the sheet body is shown as a sheet-like object. As shown in FIG. 8, with the lower end of the BASUS plate fixed by a first chuck jig, the end of the PET film is pulled upward by a second chuck jig. At this time, the test speed is set to 300 mm / min and the peel length is set to 100 mm. After the start of measurement, the measured value for the first 30 mm length is ignored. Then, the adhesive strength of the 30 mm length peeled from the test plate is measured multiple times. The multiple measured values are then averaged. The average value obtained is used as the peel adhesive strength value. The adhesive strength of the 180° peel test is measured using the above procedure.
[0038] The sheet body of the present disclosure has an adhesive strength that is less than 100% of the maximum test force in the tensile elastic region before being attached to a structure. This specifies the upper limit of the adhesive strength of the sheet body. This improves the handleability of the sheet body at the construction site.
[0039] Specifically, even after the sheet body has been attached to a structure, if the attachment does not go well (for example, if the sheet body becomes wrinkled), it can be peeled off and reattached. In other words, by setting the upper limit of the adhesive strength to less than 100% of the maximum test force in the tensile elastic region, the sheet body can be peeled off with the maximum tensile force that allows elastic deformation. By configuring the sheet body so that it has an adhesive strength that allows it to be peeled off with a force less than 100% of the maximum test force in the tensile elastic region before being attached to a structure, it is possible to prevent the sheet body from plastically deforming when peeled off, thereby reducing the adhesive strength and weather resistance, and also to make the sheet body easier to reattach and use.
[0040] From the viewpoint of ease of peeling off the sheet body, the maximum test force in the tensile elastic region before being attached to a structure is preferably, for example, 90% or less of the maximum test force in the tensile elastic region, and more preferably 80% or less. More specifically, if the value is 90% or less, the sheet body can be easily peeled off manually without using a jig or machine, for example. Furthermore, if the value is 80% or less, the sheet body can be more easily peeled off manually.
[0041] The maximum test force in the tensile elastic region in this disclosure is calculated by the following method. (Method for calculating the maximum test force in the tensile elastic region) - Sheet test piece size: Adjust to a width of 25 mm and a length of 100 mm. - Test equipment: Shimadzu Corporation's "Autograph AGX-V 10kN" is used. - Equipment setting conditions: When using Shimadzu Corporation's "Autograph AGX-V 10kN," a 1kN load cell and a PFG-1kNA chuck jig are used.
[0042] Test conditions (tensile test conditions), test method: Both short sides of a sheet (test piece) measuring 25 mm wide and 100 mm long were fixed with chuck jigs. The lower chuck jigs fixed the portion of the sheet (test piece) from its bottom end to 25 mm, and the upper chuck jigs fixed the portion of the sheet (test piece) from its top end to 25 mm. The distance between the chucks was set to approximately 50 mm.
[0043] In this state, a preload is applied to the sheet body (test specimen). The preload is performed by moving the upper chuck jig upward at a speed of 5 mm / min until the load applied to the test specimen reaches 0.005 N. The upper chuck jig is then moved upward at a test speed of 200 mm / min. The point at which the maximum test force drops by 50% in one second is recognized as the break point. The control program of the measuring device can also be used when implementing the above preload method. Specifically, the program can be set to "stretch until a preload of 0.005 N is applied" and then "stretch at a test speed of 200 mm / min until the break point is reached." Test environment: The following is performed at 23±2°C and 50±10% humidity.
[0044] Definition of Tensile Elastic Region The tensile elastic region is defined as the stroke from the first maximum point to the minimum point calculated using the following formula (1).
[0045]
[0046] Calculation of the maximum test force in the tensile elastic region. A specific method for calculating the maximum test force in the tensile elastic region will be described below with reference to FIGS. 9 and 10. The graph in FIG. 9 shows the relationship between the stroke (elongation of the test specimen) and the test force when the sheet body (test specimen) is stretched (the upper chuck jig is moved upward). The upper graph in FIG. 10 shows an enlarged view of the region between 0 and 2.5 mm of the stroke on the horizontal axis of the graph in FIG. 9 (the area shown in gray in the graph in FIG. 9). Furthermore, the lower graph in FIG. 10 shows a curve obtained by twice differentiating the upper graph (a graph showing the relationship between the stroke and the test force). The stroke corresponding to the minimum point in the lower graph (the first minimum point in the graph) is then determined, and the test force corresponding to this stroke is calculated from the upper graph. The test force calculated for this stroke is 100% of the maximum test force in the tensile elastic region.
[0047] The sheet body of the present disclosure has an upper limit of adhesive strength before being attached to a structure, which is set to a value less than the maximum test force in the tensile elastic region determined as described above, i.e., a value less than 100% of the maximum test force in the tensile elastic region.
[0048] In the present disclosure, as described above, a sheet body is configured so that, before being attached to a structure, it has an adhesive strength of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% as measured in the maximum test force in the tensile elastic region. To control the adhesive strength to such values, it is important to control the adhesive strength of the attachment surface of the sheet body to be attached to the structure (hereinafter simply referred to as the attachment surface). This control can be achieved, for example, by selecting an adhesive material present on or near the attachment surface of the sheet body, or by controlling the content of the adhesive material in the sheet body on or near the attachment surface.
[0049] More specifically, examples of adhesive materials include adhesives that have a low glass transition temperature, such as acrylic, silicone with siloxane bonds, rubber, and urethane-based adhesives, and utilize van der Waals forces or electrostatic forces. Furthermore, the surface of the sheet to be attached to the structure may be configured to have a microstructure like a gecko's limbs (a structure with a large surface area and capable of utilizing intermolecular forces. For example, a structure with multiple nanometer-sized fine hairs that, when in contact with the target surface, generate van der Waals forces, thereby generating adhesive force to the target surface). Furthermore, a method of using the adhesive in combination with the microstructure may also be considered. Furthermore, a method of controlling the thickness of the adhesive region (adhesive region) to an appropriate thickness that is neither too thick nor too thin is also effective for controlling adhesive force. From the perspective of easily controlling the adhesive force within the range, it is preferable to control the adhesive force by combining the material used for the adhesive and the thickness of the adhesive region.
[0050] Furthermore, in the sheet member of the present disclosure having a laminated structure including multiple layers, the layer having the attachment surface (for example, the adhesive layer described below) can be formed from the adhesive agent described above, or the thickness of this layer, the material constituting the layer, and the surface properties can be controlled (for example, by employing the microstructure described above). More specific methods will be described in detail later.
[0051] [2] <Durability (Weather Resistance) of Sheet Body> The sheet body of the present disclosure preferably has an adhesive strength of 1.5 N / 25 mm or more as measured in a 180° peel test, even after a weather load test, for example. This makes it easier for the sheet body 10 to remain attached to the surface of a structure for a long period of time after being attached to the structure, and makes it less likely to peel off even when exposed to strong winds.
[0052] For example, the measured value in the 180° peel test after the weathering load test is preferably 5 N / 25 mm or more, more preferably 8 N / 25 mm or more. Furthermore, a value of 9 N / 25 mm or more is even more preferable, and a value of 12 N / 25 mm or more is particularly preferable. Furthermore, a value of 15 N / 25 mm or more is most preferable. If the measured value in the 180° peel test after the weathering load test is a value within any of the above ranges, the effect described in [2] above is more easily achieved.
[0053] More specifically, a value of 1.5 N / 25 mm or more makes it easier to obtain a sheet body that can withstand a strong wind range of 15 m / s. A value of 5 N / 25 mm or more makes it easier to obtain a sheet body that can withstand a storm range of 25 m / s. A value of 8 N / 25 mm or more makes it easier to obtain a sheet body that can withstand a storm range of 30 m / s. A value of 9 N / 25 mm or more makes it easier to obtain a sheet body that can withstand a storm range of 45 m / s. A value of 12 N / 25 mm or more makes it easier to obtain a sheet body that can withstand a storm range of 65 m / s.
[0054] (Weather Load Test) The weather load test in the present disclosure is carried out in the following manner. Specifically, UV irradiation, condensation, and showering are repeatedly performed on the sheet body to be tested under the following conditions. Equipment used: Iwasaki Electric Co., Ltd. iSuper UV Tester SUV-W161, a metal halide lamp weather meter. Test time: 300 hours
[0055] Test conditions: The test object was subjected to the following UV irradiation treatment in multiple cycles until 300 hours had elapsed since the start of the test. One cycle of UV irradiation treatment included 4 hours of UV irradiation, a 30-second water shower after the UV irradiation, a 4-hour condensation treatment after the shower, and another 30-second shower after the condensation treatment. UV irradiation conditions: UV irradiation intensity: 120 W / cm 2 Uses a metal halide lamp, irradiation temperature 63°C, irradiation humidity 50% Shower conditions Shower water temperature: 25±3°C Shower duration: 30 seconds Shower water volume: 3.18 L / min to 5.16 L / min Condensation environment After shower irradiation, the temperature of the test environment is raised to 60°C over 30 minutes, and then lowered to 25°C over 3.5 hours. Humidity during testing is controlled at 90±10% RH.
[0056] Furthermore, it is preferable that the sheet body of the present disclosure does not leak water in the waterproofing test before and after the weathering load test. Here, "no leaking water" does not strictly mean that no leaking occurs, but means that no leaking water is confirmed visually from the sheet body in the waterproofing test described below. The inventors of the present application have confirmed that the weather resistance of the sheet body is sufficient if no leaking water is confirmed visually. In the present disclosure, preventing leaking water in the waterproofing test makes it easier to achieve the effects of reinforcing and repairing the surface of a structure.
[0057] (Waterproof Test) In the present disclosure, the waterproof test is performed by the following method. Two rectangular flexible boards with short sides of 50 mm, long sides of 100 mm, and a thickness of 4.0 mm are prepared. The two boards are butted together and fixed so that their long sides are in contact. This produces a square-shaped fixing adherend with one side of 100 mm and a thickness of 4.0 mm.
[0058] A test specimen was prepared by placing a sheet cut into a square shape with sides of 100 mm on one side of the fixation adherend. The adhesive surface of the sheet was then attached to the surface of the fixation adherend. A vinyl chloride pipe with an outer diameter of 42 mm, an inner diameter of 40 mm, and a length of 500 mm was then placed upright on one side of the fixation adherend (the side that would become the outer surface of the sheet-attached structure) and fixed to the fixation adherend. The pipe was then securely fixed to the surface of the sheet to prevent visible leakage of the fluorescent leakage test agent described below from between the pipe and the sheet when the test agent was poured into the pipe.
[0059] Then, 370±0.1 g of liquid fluorescent leak detection agent is poured into the tube through the opening at one end. This state is left to stand for 24 hours in an environment of 23±2°C and 50±10% RH. After leaving it for 24 hours, the back surface of the fixing adherend (the surface on which the sheet body is not superimposed) is irradiated with UV light and visually checked for the presence or absence of bright spots or liquid stains. If bright spots or liquid stains are found as a result of the visual inspection, the sample is judged to have leaked. If no bright spots or liquid stains are found as a result of the visual inspection, it is judged to have no leaks.
[0060] As described above, the sheet body of the present disclosure preferably has an adhesive strength of 1.5 N / 25 mm or more at 180° peel strength after a weathering load test. Furthermore, it preferably has waterproof properties such that no water leakage occurs in a waterproofing test after the weathering load test. These properties relate to the weathering resistance of the sheet body.
[0061] Furthermore, in order to control the weather resistance of the sheet body, it is important to control the weather resistance of the surface opposite to the attached surface of the sheet body (this refers to the surface corresponding to the outer surface of the sheet-attached structure, hereinafter also referred to as the "surface of the sheet body"). This control can be achieved, for example, by selecting the materials used near the surface of the sheet body and controlling the content thereof.
[0062] Furthermore, when the sheet body of the present disclosure has multiple layers, the weather resistance can be controlled by controlling the thickness and surface properties of the layer located on the surface of the sheet body (for example, the weather-resistant layer described below). More specifically, such weather resistance can be controlled, for example, in the case of a sheet body that contains more bonding structures with a bonding energy stronger than ultraviolet light (410 KJ / mol) on the surface or near the surface than in other regions. Examples of bonding structures with such strong bonding energy include siloxane bonds and carbon-fluorine bonds.
[0063] Furthermore, the sheet body of the present disclosure may have a structure in which the number of double bonds is reduced, for example, on the surface or near the surface compared to other regions. In this case, by reducing the number of reaction sites on the surface or near the surface of the sheet body, the chemical stability of the sheet body can be improved. An example of a structure in which the number of double bonds is reduced is a structure in which a non-diene rubber is present in greater amounts on the surface or near the surface of the sheet body than in other regions.
[0064] Furthermore, the sheet body of the present disclosure may have a structure in which, for example, a surface or near the surface has a larger amount of a radical trapping material that traps radicals generated by irradiation with energy rays such as ultraviolet (UV) rays, than in other regions. Alternatively, the sheet body of the present disclosure may have a structure in which, for example, a surface or near the surface has a larger amount of an additive that absorbs UV rays and suppresses the generation of radicals, such as a hindered amine light stabilizer (HALS), than in other regions. Alternatively, the sheet body of the present disclosure may have a structure in which, for example, a surface or near the surface has a larger amount of a phenol-based or thioether-based antioxidant than in other regions.
[0065] Furthermore, when the sheet body of the present disclosure has multiple layers, weather resistance can also be controlled by forming a layer located on the surface of the sheet body (for example, a weather-resistant layer described below) from a predetermined material. This point will be described in detail later.
[0066] [3] <Handling of the sheet body when attached to a structure (rigidity against bending)> The sheet body of the present disclosure preferably has, for example, an appropriate rigidity in order to facilitate improving handling (e.g., ease of attachment) when attached to a structure. This facilitates improving the handling of the sheet body at a construction site (e.g., ease of laying). The rigidity of the sheet body can be confirmed by the following deformation test. Specifically, when a deformation test is conducted on the sheet body by sequentially performing the operations described in items (1), (2), (3), and (4) below, if the energy calculated by the calculation in (4) below is 2.0 mJ or more, the sheet body is considered to have appropriate rigidity. (1) A rectangular sheet body with a short side of 50 mm and a long side of 100 mm is prepared as a sample. (2) The sample is bent so that a pair of short sides overlap, and a pair of regions of the sample extending from the edges of the pair of short sides to a position 15 mm away along the long side are gripped and fixed with a fixing portion, thereby forming a curved portion with a circumference of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample aligned parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface diameter of 100 mm and a thickness of 10 mm is used to contact the curved portion from above under an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool is moved downward 20 mm at a test speed of 30 mm / min. (4) The energy required to move the pressing tool (20 mm movement) is calculated (the integral of the moving distance and the force).
[0067] Here, the energy in (4) is calculated based on the following formula (2).
[0068]
[0069] In equation (2), E represents the calculated energy (mJ), F represents the test force (N), and s represents the displacement (mm) of the pressing jig. An example of the measurement results is shown in FIG. 11. The graph shown in FIG. 11 shows the relationship between the displacement (stroke) (mm) of the pressing jig and the test force (N) on the vertical axis. The area of the shaded portion in FIG. 11 represents the energy E.
[0070] Here, Figures 5(A), 5(B), 5(C), and 5(D) are schematic diagrams illustrating a method for measuring the rigidity of a sheet body according to the present disclosure. Figure 5(A) is a front view of the sheet body. Figures 5(B), 5(C), and 5(D) show views of the curved sheet body viewed from the thickness direction of the sheet body. Specifically, for example, as shown in Figure 5(A), a rectangular sheet body having short sides of 50 mm and long sides of 100 mm is prepared as sample 19. Then, as shown in Figure 5(B), sample 19 is curved so that a pair of short sides on the same surface overlap each other, and a pair of regions of sample 19 extending from the edges of the pair of short sides to a position 15 mm apart along the long sides are gripped and fixed with fixing portion 18. This forms a curved portion having a perimeter of 70 mm between the pair of regions of sample 19 (as viewed from the thickness direction of sample 19).
[0071] Thereafter, as shown in FIGS. 5(C) and 5(D), with the surfaces of the pair of regions of sample 19 arranged parallel to the vertical direction and with the curved portion facing upward, a disk-shaped pressing jig 17 with a pressing surface having a diameter of 100 mm and a thickness of 10 mm is used to bring the pressing jig 17 into contact with the curved portion from above in an environment of a temperature of 23±2° C. and a humidity of 50±10% RH, and the pressing jig 17 is moved downward by 20 mm at a testing speed of 30 mm / min.
[0072] Here, it is preferable that the energy required to move the pressing jig 17 (to move it downward by 20 mm) be a value of 2.0 mJ or more, which makes it easier to impart appropriate rigidity (for example, appropriate stiffness) to the sheet body.
[0073] From the viewpoint of the handleability of the sheet body described above, the energy required to press and deform the curved portion of the sheet body of the present disclosure is, for example, preferably 2.0 mJ or more, more preferably 3.5 mJ or more, even more preferably 5 mJ or more, even more preferably 10 mJ or more, and even more preferably 20 mJ or more. On the other hand, from the viewpoint of ensuring the handleability, the upper limit of the energy is, for example, 30 mJ or less. If the energy is a value within any of the above ranges, for example, even if the structure is a roof with steps, a sheet body with excellent handleability can be obtained that is easy to apply along the steps.
[0074] For example, the energy can be measured using an autograph (AGX-V (10 kN) manufactured by Shimadzu Corporation) while gripping a sheet (sample 19 in FIG. 5) with a pneumatic flat gripper (PFG-1 kNA) manufactured by Shimadzu Corporation. If the test device is difficult to obtain due to discontinuation of production, a successor model of the test device or a device capable of equivalent measurements can be used.
[0075] In the present disclosure, as described above, in order to improve the handleability of the sheet body when it is attached to a structure, the energy required for a predetermined deformation in the test is preferably, for example, 2.0 mJ or more. This can be achieved by controlling the rigidity of the sheet body. To control the rigidity of the sheet body, it is important to control the internal structure of the sheet body.
[0076] In order to control the internal structure of the sheet body, for example, a reinforcing material may be inserted into the sheet body to be attached to a structure. In this case, the internal structure of the sheet body can be controlled by changing the content of the reinforcing material. Furthermore, when the sheet body has multiple layers, the sheet body may have a reinforcing layer (for example, a reinforcing material described below) disposed inside. In this case, the reinforcing layer imparts a predetermined rigidity to the sheet body, thereby controlling the internal structure of the sheet body.
[0077] When the sheet contains a filler for adjusting strength, specific methods for imparting rigidity to the sheet include, for example, controlling at least one of the filler material, the amount of filler added to the sheet, and the size and shape of the filler particles. In this case, the filler material may be either an inorganic material or an organic material, or a mixture of inorganic and organic materials.
[0078] Nonwoven fabrics can also be used as reinforcing materials. In this case, the nonwoven fabric is not particularly limited as long as it is formed into a sheet shape without weaving fibers. Examples of fibers constituting the nonwoven fabric include at least one of natural fibers and chemical fibers. Examples of chemical fibers include fibers made of polyolefin resins such as polypropylene and polyethylene, polyester resins, polyacrylic resins, and polyamide resins such as nylon, as well as copolymers and modified products of these resins, and synthetic fibers made of combinations of these. Among these, polyester fibers are preferred as fibers with excellent water resistance, heat resistance, dimensional stability, weather resistance, etc.
[0079] As a specific method for imparting rigidity to the sheet body, a mesh or a film may be inserted into the sheet body. In this case, the mesh or film may contain at least one of vinylon, PET, polypropylene (polyolefin), polystyrene, and polyvinylidene fluoride. Furthermore, for example, the film may be a biaxially stretched film.
[0080] As a specific method for imparting rigidity to the sheet body, it is also preferable to insert a mesh or foil containing a metal material such as aluminum or steel into the sheet body. The rigidity of the sheet body can also be controlled by controlling the thickness of the sheet body. Furthermore, in the case of a sheet body including a substrate layer, which will be described later, the rigidity of the sheet body can also be controlled by adjusting the viscoelasticity of the substrate layer. In this case, the viscoelasticity of the substrate layer may be adjusted by adjusting the glass transition temperature (Tg, hereinafter also referred to simply as Tg) of the resin contained in the substrate layer or by changing the degree of crosslinking of the resin. Various methods can be used to control the rigidity of the sheet body, and this will be described in detail later.
[0081] The sheet body of the present disclosure has the above-mentioned rigidity while also having appropriate flexibility. For example, the sheet body has flexibility to the extent that it can be wound into a roll. Here, "roll-shaped winding" refers to winding the sheet body onto a roll core material having a diameter of, for example, several centimeters or more and several tens of centimeters or less (specifically, for example, a diameter of 10 mm or more and 300 mm or less). Even with a thinner roll core material, it is possible to wind the sheet body to several meters by hand winding, etc. Therefore, for example, the sheet body can be managed in roll form. Furthermore, it is also possible to unfold the rolled sheet body at the construction site and quickly prepare and cut sheet bodies to a predetermined size for construction. Therefore, the sheet body can be easily and simply applied to construction targets having a relatively large area.
[0082] [Layer structure of sheet body, etc.] The structure of the sheet body of the present disclosure is not particularly limited as long as it can be attached to the surface of a structure and has the properties (including preferred properties) described above. That is, the sheet body of the present disclosure may be composed of a single layer or multiple layers. Below, a sheet body of the present disclosure (first embodiment) composed of a single layer and a sheet body of the present disclosure (second embodiment) composed of multiple layers will be described separately.
[0083] [1] First Embodiment (Sheet Body of the Present Disclosure Consisting of a Single Layer) When the sheet body of the present disclosure is constituted by a single layer, the sheet body may have, for example, a predetermined adhesiveness on the attachment surface side. The sheet body also preferably has a predetermined weather resistance. In this case, the surface side opposite the attachment surface side of the sheet body may have a predetermined weather resistance. Furthermore, from the viewpoint of ensuring ease of handling when attached to a structure, the sheet body preferably has a predetermined rigidity. In this case, for example, a reinforcing member may be disposed inside the sheet body in order to control the rigidity capable of withstanding bending within a predetermined range. Here, the sheet body 10 in FIG. 3 schematically shows the configuration of the sheet body 10 of the first embodiment. A specific description will be given below.
[0084] [1-1] <Sheet body composed of a single layer having a predetermined adhesiveness on its attachment surface side> In the present disclosure, the adhesiveness of the attachment surface side of the sheet body is controlled from the viewpoint of providing sufficient adhesiveness to a structure while imparting adhesive strength that allows re-attachment at the construction site. Specifically, this can be achieved by selecting an adhesive material present on or near the attachment surface of the sheet body, or by controlling the content of the adhesive material in the sheet body on or near the attachment surface.
[0085] More specifically, examples of adhesive materials include adhesives that have a low glass transition temperature (Tg) and can utilize van der Waals forces or electrostatic forces, such as acrylic, silicone with siloxane bonds, rubber, and urethane. The adhesive surface of the sheet body may also be configured with a microstructure like a gecko's limbs (a structure with a large surface area and capable of utilizing intermolecular forces). Furthermore, adhesives may be used in combination with the microstructure. Furthermore, controlling the thickness of the adhesive region of the sheet body (adhesive region) to an appropriate thickness that is neither too thick nor too thin is also effective in controlling the adhesive strength. From the perspective of easily controlling the adhesive strength within a certain range, it is also preferable to adjust the adhesive material and the thickness of the adhesive region in combination.
[0086] [1-2] <Sheet body composed of a single layer having predetermined weather resistance on the surface side> The sheet body of the present disclosure preferably has predetermined weather resistance. From this viewpoint, for example, it is preferable to control the weather resistance on the surface side of the sheet body. This will be specifically described below.
[0087] The weather resistance of the surface side of the sheet body can be controlled, for example, by selecting and adjusting the content of a material placed on or near the surface of the sheet body. More specifically, examples of such materials include placing a material that can form many bond structures with stronger bond energy than ultraviolet light (410 kJ / mol), such as siloxane bonds or carbon-fluorine bonds, on or near the surface of the sheet body, or increasing the content of such material on or near the surface of the sheet body. Specific examples of such materials include at least one of acrylic silicone, fluororesin, and silicone resin.
[0088] Furthermore, from the viewpoint of reducing the number of reactive sites on or near the surface of the sheet body and thereby chemically stabilizing the sheet body, the sheet body may contain a material having a structure with few double bonds. The presence of a large amount of such a material on or near the surface of the sheet body increases the chemical stability of the surface and near the surface of the sheet body. An example of such a material is a non-diene rubber. Specifically, the non-diene rubber may be at least one of CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), and EPDM (ethylene propylene rubber).
[0089] Examples of methods for forming a large number of the above-mentioned bond structures on or near the surface of the sheet body include a method of unevenly distributing on or near the surface of the sheet body at least one of a radical trapping material that traps radicals generated by irradiation with energy rays such as ultraviolet (UV) rays, an additive such as HALS that absorbs UV rays and suppresses the generation of radicals, and an antioxidant such as a phenolic or thioether-based antioxidant.
[0090] [1-3] <Sheet body composed of a single layer having a predetermined rigidity> From the viewpoint of providing ease of handling when attaching the sheet body to a structure, it is preferable that the sheet body of the present disclosure has a predetermined rigidity that can withstand bending, etc. This will be specifically described below.
[0091] For example, a reinforcing material may be disposed inside the sheet body. For example, the rigidity of the sheet body can be controlled by adjusting the content of the reinforcing material in the sheet body. Further specific examples of methods for controlling the rigidity of the sheet body include adjusting at least one of the amount of strength-adjusting filler (which may be either an inorganic material or an organic material, or a mixture of inorganic and organic materials), the particle size of the filler, and the particle shape of the filler. Furthermore, the sheet body may include a mesh or film (which may be a biaxially oriented film) containing vinylon, PET, polypropylene (polyolefin), polystyrene, polyvinylidene fluoride, etc. as a reinforcing material. Alternatively, the sheet body may preferably include a mesh or foil containing a metal material such as aluminum or steel as a reinforcing material. Furthermore, the rigidity of the sheet body can be controlled by adjusting the thickness of the sheet body. Furthermore, when the sheet body includes a substrate layer described below, the viscoelasticity of the substrate layer can be adjusted by adjusting the Tg of the resin of the substrate layer or by changing the degree of crosslinking of the resin, thereby controlling the rigidity of the sheet body.
[0092] [1-4] <Other Matters Related to the Sheet Body Composed of a Single Layer> The sheet body of the present disclosure may have a configuration in which, for example, the adhesive component is unevenly distributed on the adhesive surface side relative to the surface opposite the adhesive surface. In other words, the sheet body of the present disclosure composed of a single layer may contain an adhesive component unevenly distributed on the second surface side, which is the adhesive surface to be attached to a structure, relative to the first surface side, which is located opposite the structure. This will be specifically described below.
[0093] For example, the physical properties of the sheet body may be adjusted by the energy of the electron beam. Specifically, a method of producing a sheet body using an unvulcanized rubber sheet that can be cured by electron beams can be exemplified. In this method, when irradiating the rubber sheet with electron beams, by adjusting at least one of the thickness of the rubber sheet and the electron beam irradiation dose, a rubber sheet having a single layer structure with different degrees of crosslinking on one side and the other side can be obtained.
[0094] This structure with different cross-linking degrees includes a low-cross-linking degree portion and a high-cross-linking degree portion. The low-cross-linking degree portion has relatively high adhesiveness, and the high-cross-linking degree portion has relatively low adhesiveness. The surface of the sheet that is directly irradiated with electron beams undergoes more cross-linking due to the electron beams than the opposite surface. Therefore, a high-cross-linking degree portion can be arranged on the surface of the sheet that is irradiated with controlled electron beams, and a low-cross-linking degree portion can be arranged on the opposite surface. This results in a sheet with a high-cross-linking degree portion arranged on one surface and a low-cross-linking degree portion arranged on the other surface. Therefore, in principle, the sheet can achieve both adhesiveness and water resistance (weather resistance).
[0095] Examples of rubber that can be used for the rubber sheet include isoprene rubber, SBR (styrene butadiene rubber), CR (chloroprene rubber), NBR (acrylonitrile butadiene rubber), HNBR (hydrogenated acrylonitrile butadiene rubber), CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), and EPDM (ethylene propylene rubber).
[0096] An example of a method for producing rubber is given below. First, raw rubber is masticated to obtain plasticized rubber. This plasticized rubber is kneaded to obtain a compounded rubber. This compounded rubber is crosslinked (vulcanized) to obtain a crosslinked rubber. In the vulcanization process for crosslinking (vulcanizing) this compounded rubber, one side of the compounded rubber is irradiated with an electron beam to vary the degree of crosslinking in the thickness direction of the compounded rubber, thereby producing a rubber (rubber sheet) with a structure having different degrees of crosslinking on one side and the other side. In this way, the sheet body of the present disclosure may contain rubber and have a crosslinked structure of rubber with different degrees of crosslinking on the first side and the second side.
[0097] The sheet may also have a configuration in which the adhesive component is unevenly distributed on the side (first side) opposite the application surface (second side) based on, for example, a solution diffusion method. Specifically, in this case, a sheet may be manufactured by dissolving resins A and B, which have poor compatibility (i.e., different solubility parameters), in a solvent with a solubility parameter intermediate between those of resins A and B to prepare a solution, and then applying and drying the solution. In this case, resins A and B are dissolved in the solvent in the solution state, but phase-separate from each other when the solution is applied and dried. This results in a gradient function that allows the sheet to achieve different properties.
[0098] The combination of resin A and resin B in the sheet body can be, for example, a combination of a resin that exhibits adhesive properties and a resin that exhibits weather resistance and rigidity sufficient to withstand bending. An example of such a combination of resin A and resin B (functionally gradient materials: FGMs) is a combination of acrylic resin and epoxy resin. In this case, the acrylic resin exhibits adhesive properties, and the epoxy resin side is responsible for weather resistance and rigidity. To further enhance the weather resistance properties of the epoxy resin, a radical trapping material, a UV absorbing material, or the like may be added to the material of the sheet body. Furthermore, the rigidity of the sheet body can be improved by increasing the degree of crosslinking of the epoxy resin.
[0099] More specifically, the solution may be, for example, a solution containing an acrylic resin, an epoxy resin, and an MEK solvent, in which the acrylic resin has an SP value (solubility parameter) of approximately 8, the epoxy resin has an SP value of approximately 10, and the MEK solvent has an SP value of 9.3. In this solution, the acrylic resin and the epoxy resin each dissolve in the presence of the solvent, but after the solvent evaporates, the acrylic resin and the epoxy resin form a gradient. Therefore, the sheet body can exhibit a gradient function due to the acrylic resin and the epoxy resin. In this way, the sheet body may contain an acrylic resin and an epoxy resin and have a phase-separated structure due to the acrylic resin and the epoxy resin.
[0100] [2] Second embodiment (sheet body of the present disclosure composed of multiple layers) When the sheet body of the present disclosure is composed of multiple layers, the sheet body may include a layer disposed on the attachment surface side and having a predetermined adhesive property. It is also preferable that the sheet body has a predetermined weather resistance. In this case, for example, it is preferable that the sheet body includes a weather-resistant layer disposed on the surface side opposite to the attachment surface side and having a predetermined weather resistance.
[0101] Furthermore, from the viewpoint of ensuring ease of handling when attached to a structure, it is preferable that the sheet body has a predetermined rigidity. In this case, for example, in order to control the rigidity that can withstand bending within a predetermined range, the sheet body may be configured so that at least one of the first layer arranged on the attachment surface side and the second layer arranged on the opposite side from the attachment surface has a predetermined rigidity. Alternatively, the sheet body may include a first layer arranged on the attachment surface side, a second layer arranged on the opposite side from the attachment surface, and a third layer arranged between the first and second layers, and the third layer is configured to have a predetermined rigidity. Specific explanations will be given below.
[0102] [2-1] <Sheet body provided with a layer arranged on the attachment surface side and having a predetermined adhesiveness> In the present disclosure, from the viewpoint of providing sufficient adhesiveness to a structure to obtain weather resistance while also providing adhesive strength to the extent that it can be reattached at the construction site, it is preferable that the sheet body be provided with a layer arranged on the attachment surface side, having a predetermined adhesiveness, and being attached to the structure (hereinafter this layer will also be referred to as an "adhesive layer").
[0103] The adhesiveness of the adhesive layer can be controlled, for example, by adjusting the thickness, surface properties, and material of the adhesive layer. When controlling the surface properties of the adhesive layer, for example, the microstructure described above can be employed. Furthermore, setting the thickness of the adhesive layer to an appropriate value that is neither too thick nor too thin is also effective for controlling the adhesiveness of the adhesive layer. Furthermore, from the viewpoint of easily controlling the adhesive strength of the adhesive layer within a predetermined range, it is also preferable to adjust the adhesive material and the thickness of the adhesive layer in combination.
[0104] More specifically, examples of materials for the adhesive layer include adhesives that have a low glass transition temperature (Tg) and can utilize van der Waals forces or electrostatic forces, such as acrylic, silicone with siloxane bonds, rubber, and urethane-based adhesives. The adhesive strength of the adhesive layer can be controlled by adjusting the thickness and degree of crosslinking of the adhesive layer. The adhesive surface of the adhesive layer may also be configured with a microstructure like a gecko's limbs (a structure with a large surface area and capable of utilizing intermolecular forces). Furthermore, the adhesive and the microstructure may be used in combination. Details of the adhesive layer will be described further below.
[0105] [2-2] <Sheet body having a layer arranged on the surface side and having predetermined weather resistance> The sheet body of the present disclosure preferably has predetermined weather resistance. From this viewpoint, the sheet body preferably has, for example, a layer arranged on the surface side and having predetermined weather resistance (weather-resistant layer). This will be described in detail below.
[0106] The weather resistance of the weather-resistant layer can be controlled, for example, by adjusting the material of the weather-resistant layer and the content of the material in the weather-resistant layer. More specifically, examples of such materials include disposing a material capable of forming a large number of bond structures, such as siloxane bonds or carbon-fluorine bonds, in the weather-resistant layer, which have a bond energy stronger than that of ultraviolet light (410 kJ / mol), or increasing the content of such a material in the weather-resistant layer. Specific examples of such weather-resistant layer materials include at least one of acrylic silicone, fluororesin, and silicone resin.
[0107] Furthermore, from the viewpoint of reducing the number of reactive sites in the weathering layer and chemically stabilizing the weathering layer, the weathering layer may contain a material having a structure with few double bonds. The presence of a large amount of such a material in the weathering layer increases the chemical stability of the weathering layer. Examples of such materials include non-diene rubbers. Specific examples of such non-diene rubbers include at least one of CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), and EPDM (ethylene propylene rubber).
[0108] Examples of a method for forming many of the above bond structures in the weather-resistant layer include a method of unevenly distributing at least one of a radical trapping material that traps radicals generated by irradiation with energy rays such as ultraviolet (UV) rays, an additive such as HALS that absorbs UV rays and suppresses the generation of radicals, and an antioxidant such as a phenolic or thioether-based antioxidant. Details of such weather-resistant layers will be described later.
[0109] [2-3] <Sheet body having a layer with a predetermined rigidity> From the viewpoint of ensuring ease of handling when attached to a structure, the sheet body of the present disclosure is preferably controlled to have a rigidity that can withstand bending. Therefore, for example, the sheet body may be configured so that at least one of the first layer arranged on the attachment surface side and the second layer arranged on the opposite side of the attachment surface has a predetermined rigidity. Alternatively, the sheet body may be configured so that the first layer arranged on the attachment surface side, the second layer arranged on the opposite side of the attachment surface, and a third layer arranged between the first and second layers, and the third layer has a predetermined rigidity. Specific examples are described below.
[0110] An example of the first layer disposed on the adhesive surface of the sheet body is an adhesive layer. An example of a method for imparting rigidity to the adhesive layer is to configure the adhesive layer to contain an adhesive and a filler. In this case, the adhesive layer contains, for example, an adhesive with a relatively low glass transition temperature (Tg) such as acrylic, silicone with a siloxane bond, rubber, or urethane, which can utilize van der Waals forces or electrostatic forces, and a filler such as silica, alumina, titanium oxide, calcium carbonate, or carbon black. For example, the rigidity of the adhesive layer can be controlled by adjusting at least one of the amount of filler added to the adhesive layer and the particle shape of the filler. Specific examples of filler particle shapes include spherical, acicular, amorphous, and tetrapod-shaped. The rigidity of the sheet body can also be controlled by adjusting the thickness of the weather-resistant layer. The rigidity of the sheet body can also be controlled by adjusting the Tg of the adhesive in the weather-resistant layer.
[0111] An example of the layer disposed on the surface side of the sheet body, i.e., the second layer disposed on the opposite side of the sheet body from the adhesive surface, is a weather-resistant layer. One example of a method for imparting rigidity to the weather-resistant layer is to construct the weather-resistant layer so that it contains a main material and a filler. In this case, the weather-resistant layer contains, for example, a main material such as acrylic silicone, fluororesin, silicone resin, or non-diene rubber, and a filler such as silica, alumina, titanium oxide, calcium carbonate, or carbon black. For example, the rigidity of the weather-resistant layer can be controlled by adjusting at least one of the amount of filler added to the weather-resistant layer and the particle shape of the filler. Specific examples of filler particle shapes include spherical, acicular, amorphous, and tetrapod-shaped. Furthermore, the rigidity of the sheet body can be controlled by adjusting at least one of the thickness of the weather-resistant layer and the Tg of the main material of the weather-resistant layer. In this way, at least one of the adhesive layer and the weather-resistant layer in the sheet body may contain a filler.
[0112] In a sheet body having a first layer (e.g., an adhesive layer) disposed on the side of the adhesive surface, a second layer (e.g., a weather-resistant layer) disposed on the opposite side of the adhesive surface, and a third layer disposed between the first and second layers, where the third layer is configured to have a predetermined rigidity, one method of imparting rigidity to the third layer is, for example, to configure the third layer as a substrate layer (described below) and impart rigidity to the substrate layer, which will be described in detail later.
[0113] [3] <Specific example of second embodiment> Fig. 1 is a cross-sectional view schematically showing a sheet member 10 of a second embodiment having a single adhesive layer and a single weather-resistant layer. Fig. 2 is a cross-sectional view schematically showing a sheet member 10 of a second embodiment having a plurality of base layers and a plurality of weather-resistant layers. Both the first and second embodiments are examples of "a sheet member of the present disclosure composed of a plurality of layers."
[0114] The sheet body 10 of the present disclosure may include at least one base material layer 12 and at least one weather-resistant layer 13. As an example, the sheet body 10 of a second embodiment shown in FIG. 1 includes an adhesive layer 11, a single base material layer 12 disposed over one side of the adhesive layer 11, a single weather-resistant layer 13 disposed over the side of the base material layer 12 opposite the adhesive layer 11 side, and a release sheet 16 disposed over the other side of the adhesive layer 11. The at least one weather-resistant layer 13 is disposed above the adhesive layer 11. The release sheet 16 is disposed on the side of the adhesive layer 11 opposite the weather-resistant layer 13 side. When the release sheet 16 is removed, the sheet body 10 shown in FIG. 1 has a laminated structure consisting of three layers.
[0115] 2 includes an adhesive layer 11, a plurality of (here, two) base layers 12 superimposed on one side of the adhesive layer 11, a plurality of (here, two) weather-resistant layers 13 superimposed on the outermost surface of the base layer 12 opposite the adhesive layer 11, and a release sheet 16 superimposed on the other side of the adhesive layer 11. The base layer 12 is disposed between the adhesive layer 11 and the weather-resistant layer 13. When the release sheet 16 is removed, the sheet 10 shown in FIG. 2 has a laminated structure consisting of five layers. Details of each layer will be described later.
[0116] 2, in the case of a sheet body 10 including a plurality of base material layers 12 and a plurality of weather-resistant layers 13, a laminate structure including a plurality of base material layers 12 directly laminated to one another and a laminate structure including a plurality of weather-resistant layers 13 directly laminated to one another may be laminated. By using each of these laminate structures, it is possible to easily control the overall thickness or properties of each of the base material layers 12 or weather-resistant layers 13 included in the sheet body 10. Therefore, for example, it is possible to easily impart the properties described above to the sheet body 10.
[0117] For example, the sheet body 10 may include another layer disposed between the substrate layer 12 and the weather-resistant layer 13. In other words, the sheet body 10 may include a third layer (another layer) disposed between the first layer (substrate layer 12) and the second layer (weather-resistant layer 13). This makes it easier to control, for example, the adhesiveness of the sheet body 10 and the overall rigidity of the sheet body 10. As shown in FIG. 1 , the sheet body 10 may have a release sheet 16 attached to the surface of the adhesive layer 11. This is preferable because the adhesive layer 11 is protected by the release sheet 16. Furthermore, examples of the laminate structure of the sheet body 10 include a laminate structure including the adhesive layer 11 and the weather-resistant layer 13, as well as a laminate structure in which the adhesive layer 11 and the substrate layer 12, which has been provided with weather resistance, are laminated. In the following description, unless otherwise specified, the "sheet body 10" refers to a sheet body 10 having a three-layer laminate structure in which an adhesive layer 11, a base layer 12, and a weather-resistant layer 13 are provided in this order, as shown in Figure 1.
[0118] (Adhesive layer 11) The adhesive layer 11 is preferably composed of, for example, an acrylic adhesive. Acrylic adhesives allow for easy adjustment of adhesive strength to the roof of a structure or the like, provide a high degree of freedom in material design, and are also excellent in transparency, weather resistance, and heat resistance. This allows the sheet member 10 to more suitably reinforce or repair the surface of a structure. The acrylic adhesive is not particularly limited, and commercially available products can be used. Examples include Orivine (registered trademark) BPS6574, BPS6554, and BPS5565K manufactured by Toyochem Co., Ltd.
[0119] When an acrylic adhesive is used, the material of the adhesive layer 11 preferably contains an isocyanate-based crosslinking agent (curing agent) in an amount of, for example, 1 part by weight or more per 100 parts by weight of the acrylic adhesive. The content of the isocyanate-based crosslinking agent (curing agent) in the material is more preferably, for example, 4 parts by weight or more per 100 parts by weight of the acrylic adhesive. On the other hand, the content of the isocyanate-based crosslinking agent (curing agent) in the material is preferably, for example, 10 parts by weight or less per 100 parts by weight of the acrylic adhesive. The content of the isocyanate-based crosslinking agent (curing agent) in the material is more preferably, for example, 6 parts by weight or less per 100 parts by weight of the acrylic adhesive. This makes it easier to control the adhesiveness of the adhesive layer within the range specified in the present disclosure.
[0120] Furthermore, when an acrylic adhesive is used, the material of the adhesive layer 11 preferably contains, for example, 1 part by weight or more of a tackifier (e.g., a rosin-based, terpene-based, petroleum resin-based, or phenolic resin-based tackifier) per 100 parts by weight of the acrylic adhesive. Meanwhile, the content of the tackifier in the material is more preferably, for example, 20 parts by weight or less, and even more preferably 10 parts by weight or less, per 100 parts by weight of the acrylic adhesive. This makes it easier to control the adhesiveness of the adhesive layer within the range specified in the present disclosure. Furthermore, by configuring the sheet body to have multiple (e.g., two) adhesive layers and varying the ratio of crosslinking agent (curing agent) in each adhesive layer, the adhesive layer 11 can more easily exhibit stable adhesive strength even when subjected to temperature changes.
[0121] The thickness of the adhesive layer 11 is generally 15 μm or more from the viewpoint of exerting sufficient adhesive strength to the surface of the structure. The thickness of the adhesive layer 11 is, for example, preferably 30 μm or more, more preferably 40 μm or more. Furthermore, a value of 50 μm or more is even more preferable, and a value of 70 μm or more is particularly preferable. On the other hand, taking productivity and the like into consideration, the thickness is generally 180 μm or less. The thickness of the adhesive layer 11 is, for example, preferably 170 μm or less, more preferably 160 μm or less. Furthermore, a value of 140 μm or less is even more preferable, and a value of 125 μm or less is most preferable.
[0122] In this way, for example, by appropriately adjusting the thickness of the adhesive layer 11, the initial adhesive strength of the sheet member 10 when attached to the surface of a structure via the adhesive layer 11 and the adhesive strength after a weathering load test can be adjusted to fall within the above-mentioned range. The optimal range for the thickness of the adhesive layer 11 may vary depending on the type of adhesive used. For example, in the examples described below, an acrylic adhesive, Orivine (registered trademark) BPS5565K manufactured by Toyochem Co., Ltd., is used as the adhesive. When this adhesive is used, the thickness of the adhesive layer 11 is preferably, for example, 20 μm or more and 180 μm or less.
[0123] The storage modulus G′ of the adhesive layer 11 at 23±2° C. is, for example, 1×10 3 A value of 1×10 Pa or more is preferable. 4 A value of 1×10 Pa or more is more preferable. 6 A value of 1×10 Pa or less is preferable. 5 A value of 0.1 Pa or less is more preferable. By setting the storage modulus G' at 23±2°C of the adhesive layer 11 to any value within these ranges, for example, it becomes easier to control the adhesive layer 11 to an appropriate softness. Therefore, in the sheet member 10, the adhesive strength can be ensured while the handleability (for example, the sheet member 10 is less likely to slip when attached to a structure) can be easily improved.
[0124] A method for measuring the storage modulus G' will now be described. FIG. 15 is a schematic diagram of the method for measuring the storage modulus G'. A DMAQ850 Rheometer DHR-2 (manufactured by TA Instruments Japan Co., Ltd.) is used as the viscoelasticity measuring device. If the testing device is no longer available due to discontinuation of production, a successor model of the testing device or a device capable of equivalent measurements can be used.
[0125] Sample Preparation and Measurement Methods: First, an adhesive layer 11 with a thickness of approximately 2 mm is prepared. A sample is prepared by punching this adhesive layer 11 into a 5 mm disk shape. Next, as shown in FIG. 15, this punched sample is sandwiched and fixed between a parallel plate and a lower plate. The punched sample is then subjected to vibration at a frequency of 1.0 Hz, and the temperature of the punched sample is changed at 5°C / min within a temperature range of -80°C to 80°C. The storage modulus G' of the punched sample at this time is measured in shear mode. FIG. 16 is a graph showing an example of measuring the storage modulus G'. For convenience, FIG. 16 shows an example in which the upper limit of the sample's temperature range is set to 120°C.
[0126] Specific examples of materials for the adhesive layer 11 include Olivine (registered trademark) BPS5565K manufactured by Toyochem Co., Ltd., which is an acrylic adhesive, and BHS8515 manufactured by Toyochem Co., Ltd., which is an isocyanate-based crosslinking agent (curing agent).
[0127] (Substrate Layer 12) The substrate layer 12 is, for example, a layer that defines the shape of the sheet body 10 of the present disclosure. The substrate layer 12 preferably has the function of maintaining the overall shape of the sheet body 10 and imparting a predetermined rigidity to the sheet body 10. The sheet body 10 may include a single substrate layer 12 as shown in FIG. 1 , or may include multiple substrate layers 12 as shown in FIG. 2 . The number of substrate layers 12 included in the sheet body 10 is determined taking into consideration, for example, the overall thickness of the sheet body 10, the functions imparted to the substrate layer 12, the length of the factory production line, or the production cost of the sheet body 10. For example, if a single substrate layer 12 having a predetermined thickness cannot be obtained due to a short factory production line, a layered structure of multiple substrate layers 12 having a predetermined overall thickness may be formed by applying multiple layers of the material for the substrate layer 12.
[0128] The configuration of the base material layer 12 is not particularly limited. The base material layer 12 preferably contains, for example, a composite material of a resin material and a material that imparts rigidity to the sheet body 10. This makes it easier to impart a predetermined rigidity to the sheet body 10. Examples of the resin material contained in the base material layer 12 include acrylic resin, acrylic silicone resin, fluororesin, and silicone resin.
[0129] Furthermore, a filler can be exemplified as a material contained in the base layer 12 that imparts rigidity to the sheet body 10. In this case, examples of fillers include cement, mortar, silica, alumina, titanium oxide, calcium carbonate, and carbon black. Furthermore, the rigidity of the sheet body 10 can be controlled, for example, by adjusting the particle shape of the filler. Specific examples of the particle shape of the filler include spherical, acicular, amorphous, and tetrapod-shaped.
[0130] Furthermore, the rigidity of the sheet body 10 can be controlled by adjusting the thickness of the base material layer 12. The base material layer 12 is preferably composed of, for example, a resin component containing acrylic and mortar. The base material layer 12 more preferably contains polymer cement. By controlling the ratio of the resin component and mortar, which are the materials of the base material layer 12, the rigidity of the sheet body 10 can be easily controlled and the degree of freedom in material design can be improved. Furthermore, since the thickness of the base material layer 12 can be obtained to an extent that is easy to handle, the sheet body 10 can be used more suitably to reinforce or repair the surface of a structure.
[0131] More specifically, examples of the base layer-forming composition containing an acrylic resin that can be used include Spring Coat (Brush) Admixture manufactured by Kikusui Chemical Industry Co., Ltd. and Aronble Coat A450 Base manufactured by Toagosei Co., Ltd. Furthermore, examples of the mortar used in the base layer 12 that can be used include Spring Coat (Brush) Powder manufactured by Kikusui Chemical Industry Co., Ltd. and Aronble Coat A450 Setter manufactured by Toagosei Co., Ltd. The materials for the base layer-forming composition and the mortar exemplified above may each be used alone or in combination.
[0132] When a resin component and a mortar component are used as the material for the base layer 12, the amount of the resin component relative to the total amount of the mixture of the mortar component and the resin component is preferably, for example, 10 parts by weight or more. The amount of the resin component relative to the total amount of the mixture is more preferably, for example, 20 parts by weight or more, even more preferably, 30 parts by weight or more, and most preferably, 40 parts by weight or more. On the other hand, the amount of the resin component relative to the total amount of the mixture is preferably 90 parts by weight or less, more preferably, 80 parts by weight or less, even more preferably, 70 parts by weight or less, and most preferably, 60 parts by weight or less. This makes it easier to ensure adhesion of the base layer 12 to the weather-resistant layer 13 described below and to impart appropriate rigidity to the sheet body 10.
[0133] Furthermore, a film- or mesh-shaped reinforcing material may be used as a material that provides rigidity. This reinforcing material is disposed, for example, inside the base material layer 12. Examples of the reinforcing material contained in the base material layer 12 include meshes and films (which may be biaxially oriented films) made of vinylon, PET, polypropylene (polyolefin), polystyrene, polyvinylidene fluoride, etc. Furthermore, meshes and foils made of metal materials such as aluminum and steel are also preferred as reinforcing materials contained in the base material layer 12. Thus, the base material layer 12 may include a reinforcing material in the form of a mesh, film, or foil.
[0134] FIG. 6 is a schematic diagram showing an example of the reinforcing material 15 of the sheet body 10 of the present disclosure. FIG. 7 is a partially enlarged view of the reinforcing material 15 of FIG. 6. The reinforcing material 15 shown in FIGS. 6 and 7 is a material used in the base layer 12, and as an example, has a biaxially woven structure in which warp and weft fibers are arranged in a lattice pattern. The shape of the reinforcing material 15 is not particularly limited. Examples of the shape of the reinforcing material 15 include the biaxially woven structure shown in FIGS. 6 and 7, as well as any other shape, such as a triaxially woven structure. Preferred examples of the reinforcing material 15 include mesh materials such as high-strength vinylon mesh (e.g., for civil engineering applications) and cheesecloth made of vinylon (e.g., for agricultural applications), polyester, polyvinyl alcohol, etc. These reinforcing materials 15 can easily widen the elastic range of the sheet body 10. They can also easily impart appropriate rigidity to the sheet body 10. Furthermore, they can improve the handleability of the sheet body 10.
[0135] For example, the line pitch of the reinforcing material 15 is preferably 50 mm or more and 1.2 mm or less. In other words, the line density of the reinforcing material 15 is preferably 0.2 lines / cm or more and 8.0 lines / cm or less. Such a reinforcing material 15 can easily impart rigidity to the sheet body 10 while ensuring the tensile strength of the sheet body 10.
[0136] For example, when the base material layer 12 is viewed in a plane, the reinforcing material 15 may have a size that covers the entire surface of the base material layer 12, or may have a size that is smaller than the base material layer 12. In other words, the area of the reinforcing material 15 when viewed in a plane may be equal to or smaller than the area of the base material layer 12 when viewed in a plane.
[0137] The area of the reinforcing material 15 when viewed in a plane (planar area) is preferably, for example, 60% to 95% of the planar area of the base layer 12. If the planar area of the reinforcing material 15 is 60% or more, for example, it becomes easier to ensure the rigidity of the sheet body 10 and to control the elongation rate of the sheet body 10. It also becomes easier to suppress variations in rigidity in different regions of the sheet body 10. If the planar area of the reinforcing material 15 is 95% or less, for example, when the base layer 12 is formed so as to sandwich the reinforcing material 15 in the thickness direction of the sheet body 10, it becomes easier to ensure the adhesive strength of the reinforcing material 15 to the base layer 12 throughout the entire base layer 12. The planar area of the reinforcing material 15 can be measured by a known method.
[0138] The thickness of the reinforcing material 15 is, for example, 10% or more of the thickness of the base material layer 12. The thickness of the reinforcing material 15 is, for example, preferably 20% or more of the thickness of the base material layer 12, more preferably 30% or more, particularly preferably 40% or more, and most preferably 50% or more. On the other hand, the thickness of the reinforcing material 15 is, for example, 80% or less of the thickness of the base material layer 12. The thickness of the reinforcing material 15 is, for example, preferably 70% or less of the thickness of the base material layer 12, more preferably 60% or less, and particularly preferably 55% or less. Setting the thickness of the base material layer 12 in this manner makes it easier to impart appropriate rigidity to the sheet body 10.
[0139] Furthermore, by setting the thickness of the reinforcing material 15 and the thickness of the base layer 12 to satisfy the above-mentioned relationship, the sheet body 10 of the present disclosure can be configured to have excellent adhesion between the adhesive layer 11 and the base layer 12 and appropriate rigidity. Therefore, excellent handleability is obtained when the sheet body 10 is attached to the roof of a structure or the like, and the structure can be protected for a long period of time by the sheet body 10 without causing wrinkles or gaps with the roof of the structure. For example, the lower limit of the thickness of the reinforcing material 15 relative to the thickness of the base layer 12 is preferably 45%, and the upper limit of this thickness is preferably 55%.
[0140] Furthermore, the rigidity of the sheet body 10 can be controlled by adjusting the Tg of the resin component contained in the base material layer 12. The rigidity of the sheet body 10 can also be controlled by adjusting the amount of voids or the diameter of the voids in the base material layer 12. When the sheet body 10 includes multiple base material layers 12, for example, the sheet body 10 may include a first base material layer 12 including a resin component having a Tg of a predetermined value and a second base material layer 12 including a resin component having a Tg lower than that of the resin component contained in the first base material layer 12.
[0141] From the viewpoint of ensuring the rigidity of the sheet body 10, the thickness of the base material layer 12 is, for example, 100 μm or more. The thickness of the base material layer 12 is, for example, preferably 200 μm or more, more preferably 300 μm or more, and most preferably 350 μm or more. On the other hand, taking into consideration productivity and the like, the thickness of the base material layer 12 is, for example, 1500 μm or less. The thickness of the base material layer 12 is preferably 1200 μm or less, more preferably 1000 μm or less, and most preferably 750 μm or less. In this way, by appropriately adjusting the thickness of the base material layer 12, appropriate rigidity of the sheet body 10 can be obtained.
[0142] When a resin component, a mortar component, and a reinforcing material 15 are used as materials for the base layer 12, as a specific example, a Spring Coat (Brush) admixture manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the resin component. Also, a Spring Coat (Brush) powder manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the mortar component. Also, a vinylon mesh material (cheesecloth (BINEO (registered trademark) "V520") manufactured by Unitika Ltd. can be used as the reinforcing material 15 (mesh component).
[0143] (Weather-resistant layer 13) The weather-resistant layer 13 is a layer disposed on the opposite side of the surface of the structure and exposed to the outside. The sheet body 10 may include a single weather-resistant layer 13, as shown in FIG. 1, or multiple weather-resistant layers 13, as shown in FIG. 2. The number of weather-resistant layers included in the sheet body 10 is determined taking into consideration the overall thickness of the sheet body 10, the functions to be provided (weather resistance, waterproofing, salt protection, neutralization prevention, water vapor permeability, etc.), the length of the factory production line, production costs, etc. For example, if a single weather-resistant layer 13 having a predetermined thickness cannot be obtained due to a short production line, a layered structure of multiple weather-resistant layers 13 having a predetermined overall thickness can be formed by applying multiple layers of the material for the weather-resistant layer 13.
[0144] The weather-resistant layer 13 is preferably, for example, a layer that ensures the weather resistance of the sheet body 10. For example, the weather-resistant layer 13 is preferably formed by applying a paint that is flexible and can conform to cracks and fissures that occur on the roof of the structure, and that can form a weather-resistant layer 13 that is excellent in waterproofing, salt blocking properties, neutralization prevention properties, and water vapor permeability.
[0145] When the weather-resistant layer 13 contains a resin, the resin is preferably a resin having a bond structure with a bond energy stronger than that of ultraviolet light (410 kJ / mol). Examples of such resins include acrylic resins exhibiting rubber properties (e.g., synthetic rubbers primarily composed of acrylic esters), acrylic urethane resins, acrylic silicone resins, fluororesins, flexible epoxy resins, and polybutadiene rubber. Among these, acrylic silicone resins are preferred because they can more easily ensure weather resistance. The resin contained in the weather-resistant layer 13 may be the same as the resin components contained in the base layer 12. The resin contained in the weather-resistant layer 13 is preferably a resin containing an elastic film-forming component, such as rubber. Of these resins, acrylic silicone resins are preferred because they are safe, easy to apply, and are not considered hazardous under the Fire Service Act.
[0146] An example of a method for forming the weather-resistant layer 13 is to prepare a coating liquid by mixing a resin and a solvent, apply the coating liquid to a release sheet, and then dry and remove the solvent from the coating film. The solvent may be water or an aqueous solvent, or may be an organic solvent such as xylene or mineral spirits.
[0147] The weather-resistant layer 13 may also contain a pigment from the viewpoint of providing a wide range of color variations for the sheet member 10. The weather-resistant layer 13 may also contain an inorganic substance. By containing an inorganic substance in the weather-resistant layer 13, scratch resistance can be imparted to the weather-resistant layer 13. The inorganic substance contained in the weather-resistant layer 13 is not particularly limited, and examples thereof include conventionally known materials such as metal oxide particles such as silica, alumina, and titania.
[0148] The weather-resistant layer 13 may also contain a known antifouling agent. The sheet member 10 is typically used to reinforce or repair structures installed outdoors. For this reason, the weather-resistant layer 13 is often soiled, but by containing an antifouling agent in the weather-resistant layer 13, the sheet member 10 can be suitably prevented from being soiled. The antifouling agent contained in the weather-resistant layer 13 is not particularly limited, and for example, known materials can be used. The weather-resistant layer 13 may also contain an additive that can impart various functions to the sheet member 10. Examples of such additives include cellulose nanofibers.
[0149] The weather-resistant layer 13 preferably contains, for example, an acrylic silicone resin. By adjusting the ratio of siloxane bonds, acrylic silicone resins can easily control weather resistance, color, and the degree of resin degradation, allowing for a high degree of freedom in material design. Furthermore, because they have excellent heat and cold resistance, the sheet member 10 can more effectively reinforce or repair the surface of a structure. Examples of acrylic silicone resins contained in the weather-resistant layer 13 include weather-resistant layer-forming compositions containing acrylic resins (e.g., Cool Life SP Black (CB1) P5-0 manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., Bell Earth Elastic Black manufactured by Fujikura Kasei Co., Ltd., Aronble Coat T-1000 manufactured by Toagosei Co., Ltd., Acryset EMN325E manufactured by Nippon Shokubai Co., Ltd., and U-Double EF008 manufactured by Nippon Shokubai Co., Ltd.). Each of these materials may be used alone or in combination.
[0150] When using an acrylic silicone resin, an acrylic silicone resin having a Tg of 0° C. or less and an acrylic silicone resin having a Tg of more than 0° C. may be used. In this case, for example, the acrylic silicone resin having a Tg of more than 0° C. may be added in an amount of 0 parts by weight or more to 100 parts by weight of the acrylic silicone resin having a Tg of 0° C. or less.
[0151] The amount of the acrylic silicone resin having a Tg greater than 0°C added is, for example, more preferably 20 parts by weight or more, even more preferably 50 parts by weight or more, and most preferably 80 parts by weight or more, per 100 parts by weight of the acrylic silicone resin having a Tg of 0°C or less.
[0152] On the other hand, the amount of the acrylic silicone resin with a Tg greater than 0°C added is preferably 200 parts by weight or less, more preferably 180 parts by weight or less, even more preferably 150 parts by weight or less, and most preferably 120 parts by weight or less, per 100 parts by weight of the acrylic silicone resin with a Tg of 0°C or less. By using an acrylic silicone resin with a Tg of 0°C or less and an acrylic silicone resin with a Tg greater than 0°C within any of the above ranges, the weather-resistant layer 13 can maintain its heat resistance, which prevents blocking in the summer, and its cold resistance, which prevents problems such as cracking in the winter. This makes it easier to control the sheet member 10 to achieve the desired performance.
[0153] The thickness of the weather-resistant layer 13 is arbitrarily set depending on, for example, the usage pattern, age, or shape of the roof of a structure. From the viewpoint of ensuring weather resistance, the thickness of the weather-resistant layer 13 is, for example, 10 μm or more. For example, the thickness of the weather-resistant layer 13 is preferably 30 μm or more, more preferably 50 μm or more, even more preferably 70 μm or more, and particularly preferably 90 μm or more. In another example, a value of 100 μm or more is even more preferable. On the other hand, for example, the thickness of the weather-resistant layer 13 is 500 μm or less, taking into consideration productivity, etc. For example, the thickness of the weather-resistant layer 13 is preferably 400 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and most preferably 150 μm or less. If the thickness of the weather-resistant layer 13 is within any of the above ranges, the weather resistance of the sheet member 10 required in the present disclosure can be easily ensured. Furthermore, from the viewpoint of ensuring weather resistance, it is preferable that there is little variation in the thickness of the weather-resistant layer 13. Specifically, it is preferable that the variation in the thickness of the weather-resistant layer 13 is within ±30% of the thickness of the weather-resistant layer 13. Such precision in the thickness of the weather-resistant layer 13 can be easily achieved by manufacturing the sheet member 10 on a factory production line.
[0154] In this way, by appropriately adjusting the thickness of the weather-resistant layer 13 to any value within the above ranges, it is possible to easily adjust the sheet member 10 so that, before being attached to a structure, the sheet member 10 has an adhesive strength of 1.5 N / 25 mm or more measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region. In this case, a specific example of a material for the weather-resistant layer 13 is preferably an acrylic silicone-based material. Examples of the acrylic silicone-based resin contained in the weather-resistant layer 13 include weather-resistant layer-forming compositions containing acrylic resins (e.g., Cool Life SP Black (CB1) P5-0 manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., Bell Earth Elastic Black manufactured by Fujikura Kasei Co., Ltd.).
[0155] (Sheet body 10) The thickness of the sheet body 10 in the present disclosure is, for example, 10 μm or more from the viewpoint of imparting predetermined properties to the sheet body 10. The thickness of the sheet body 10 is, for example, preferably 100 μm or more, more preferably 300 μm or more. Furthermore, a value of 500 μm or more is even more preferable, and a value of 600 μm or more is most preferable. Furthermore, the thickness of the sheet body 10 is, for example, 10 cm or less. The thickness of the sheet body 10 is, for example, preferably 5 cm or less, more preferably 1 cm or less, and even more preferably 5 mm or less. Furthermore, a value of 1 mm or less is particularly preferable, and a value of 800 μm or less is most preferable.
[0156] Furthermore, from the viewpoint of stably imparting predetermined properties to the sheet body 10, the thickness distribution of the sheet body 10 is preferably, for example, a value of ±10% or less of the total thickness of the sheet body 10. When the thickness distribution of the sheet body 10 is within this range, for example, even an unskilled worker can easily provide a layer with little thickness variation on the surface of a structure. Furthermore, by controlling the thickness distribution within this range, it becomes easier to uniformly reinforce the structure.
[0157] The method for manufacturing the sheet body 10 is not particularly limited, but will be exemplified below. First, a coating liquid, which is the material for the weather-resistant layer 13, is applied to a predetermined shape-imparting sheet 14 (see FIG. 19 ), which is a substrate. Thereafter, the solvent in the coating film formed by the application is removed by heating, or the resin in the coating film is cured, or the like. In this way, the weather-resistant layer 13 is formed. Next, a coating liquid, which is the material for the substrate layer 12, is applied to the weather-resistant layer 13. Thereafter, the solvent in the coating film formed by the application is removed by heating, or the resin in the coating film is cured, or the like. In this way, the substrate layer 12 is formed.
[0158] On the other hand, a coating liquid, which is the material for the adhesive layer 11, is applied onto the release sheet 16. Thereafter, the solvent in the coating film formed by the application is removed by heating, or the resin in the coating film is cured, etc., thereby forming the adhesive layer 11. Thereafter, the weather-resistant layer 13 and the base layer 12 are bonded to form a bonded body. The shape-imparting sheet 14 is peeled off from this bonded body, and the adhesive layer 11 is attached to the base layer 12 side. In this manner, the sheet body 10 is manufactured.
[0159] A more specific method for manufacturing the sheet member 10 will be described below. First, a coating liquid, which is the material for the weather-resistant layer 13, is applied to a previously prepared shape-imparting sheet 14. Thereafter, the solvent in the coating film formed by the application is dried and removed, thereby forming the weather-resistant layer 13.
[0160] Next, a coating liquid, which is the material for the substrate layer 12, is applied to the upper surface of the weather-resistant layer 13. At this time, a reinforcing material 15 such as a mesh, film, or foil is inserted into the applied coating liquid, if necessary. Thereafter, the solvent in the coating film formed by the above application is dried and removed, thereby forming the coating film for the substrate layer 12.
[0161] On the other hand, a coating liquid, which is a material for the adhesive layer 11, is applied onto the release sheet 16. Thereafter, the solvent in the coating film formed by the above application is dried and removed to form the adhesive layer 11. Thereafter, the adhesive layer 11 is overlaid on the base layer 12 and adhered to it. Thereafter, the shape-imparting sheet 14 is peeled off from the weather-resistant layer 13. In this manner, the sheet body 10 is manufactured.
[0162] When the sheet body 10 of the present disclosure is applied to a structure, a protective structure for the structure is obtained that includes the sheet body 10 and the structure on which the sheet body 10 is disposed. In this case, the sheet body 10 of any of the aspects of the present disclosure described herein is applied to the protective structure.
[0163] The sheet member 10 of the present disclosure may be used in a state in which two or more layers are stacked. In this case, a protective structure for a structure is obtained, which includes a laminate including a plurality of sheet members 10 arranged in the thickness direction and a structure on which the laminate is arranged. In this case, a plurality of sheet members 10 according to any of the aspects of the present disclosure described herein are applied to the laminate.
[0164] In this case, by placing another sheet body 10 on the surface of the structure protected by one sheet body 10, the surface of the structure can be further protected by the sheet body 10. In this laminate, for example, a portion of one sheet body 10 may be placed on at least a portion of another sheet body 10. In other words, for example, an end of one sheet body 10 may be placed on an end of another sheet body 10. Alternatively, for example, the entirety of another sheet body 10 may be placed on the entirety of one sheet body 10. In addition, in the laminate, the multiple sheet bodies 10 may be attached to each other.
[0165] (Release sheet 16) The release sheet 16 is attached to the surface of the adhesive layer 11 opposite to the base layer 12 side. It is preferable that the release sheet 16 be attached to the sheet body 10 for the purpose of protecting the surface of the adhesive layer 11 before use. Here, FIG. 3 is a schematic diagram showing how the release sheet 16 is peeled off from the sheet body 10 of the present disclosure. FIG. 4 is a schematic diagram showing how the sheet body 10 of FIG. 3 is attached to a structure. As shown in FIG. 3, the release sheet 16 is peeled off when the sheet body 10 is attached to the roof of the structure 21. As shown in FIG. 4, the sheet body 10, in which the adhesive layer 11 is exposed by peeling off the release sheet 16, is attached to the roof of the structure 21 by bringing the adhesive layer 11 into contact with the roof of the structure 21.
[0166] The structure of the release sheet 16 is not particularly limited, and an example thereof is a sheet having a support layer and a release layer. Examples of materials constituting the support layer include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, and synthetic resins such as polycarbonate. The support layer may also be formed primarily from paper. Furthermore, the support layer may be a laminate having two or more constituent layers.
[0167] Examples of materials constituting the release layer include silicone resins, melamine resins, and fluorinated polymers. The release layer can be formed, for example, by applying a coating liquid containing the material constituting the release layer and an organic solvent onto the support layer by a known coating method such as gravure coating, roll coating, comma coating, or lip coating, and then drying and curing the coating film formed by the application. In addition, when forming the release layer, the surface of the support layer on which the release layer is to be formed may be previously subjected to corona treatment or easy-adhesion treatment.
[0168] (Shape-imparting sheet 14) The shape-imparting sheet 14 is used as a substrate when the sheet body 10 is manufactured. The shape-imparting sheet 14 may include resin-laminated paper, which is a process paper used in the manufacturing process of the sheet body 10, or a resin film. The resin-laminated paper referred to here may have an olefin resin layer such as polypropylene or polyethylene. Specifically, the shape-imparting sheet 14 may be, for example, a PP laminate sheet (manufactured by, for example, Lintec Corporation). The thickness of this PP laminate sheet is, for example, 50 μm or more and 200 μm or less.
[0169] As described above, the sheet body 10 has flexibility to the extent that it can be wound into a roll. Therefore, by rolling the sheet body 10, a roll body 26 can be formed, for example, as shown in Fig. 20, which will be described later.
[0170] Further configurations of the sheet body 10 will be illustrated below. Fig. 17 is a cross-sectional view schematically illustrating the configuration of a sheet body 10 according to a third embodiment. When the release sheet 16 described above is the first release sheet 16, the sheet body 10 of this embodiment includes a second release sheet 25 arranged on the side of the weather-resistant layer 13 opposite the adhesive layer 11. As an example, the sheet body 10 has the first release sheet 16, adhesive layer 11, base layer 12, weather-resistant layer 13, and second release sheet 25 arranged in this order in the thickness direction.
[0171] The second release sheet 25 is configured so that when the surface 25a exposed to the outside comes into contact with the surface 16a exposed to the outside of the first release sheet 16, the surfaces 25a and 16a are unlikely to stick to each other. Therefore, when the sheet body 10 is unwound from the roll body 26, the first release sheet 16 can be easily separated from the second release sheet 25, and the sheet body 10 can be easily unwound.
[0172] The second release sheet 25 also has a predetermined rigidity. This improves the rigidity of the remaining sheet body 10 after the first release sheet 16 has been peeled off. Therefore, even if the remaining sheet body 10 after the first release sheet 16 and the second release sheet 25 have been peeled off has low rigidity, the sheet body 10 can be easily handled and attached to the surface of a structure. Furthermore, the remaining sheet body 10 after the first release sheet 16 and the second release sheet 25 can be designed to have a relatively low rigidity. Therefore, for example, even if the surface of a structure to which the sheet body 10 is to be attached is not flat due to unevenness or differences in elevation caused by defects, the sheet body 10 can be attached by conforming well to the surface. Furthermore, for example, the anchoring effect on the surface can be improved, thereby sufficiently improving the adhesive strength of the sheet body 10 within an acceptable range.
[0173] The structure of the second release sheet 25 can be set as appropriate. For example, as shown in Fig. 17, the second release sheet 25 has a contact layer 23 that comes into contact with the first release sheet 16 when the sheet body 10 is wound into a roll, and a weak adhesive layer 24 that is disposed on the first release sheet 16 side of the contact layer 23 when the sheet body 10 is placed flat.
[0174] The contact layer 23 may be composed of a single layer or multiple layers. The contact layer 23 may also contain a resin. In other words, the contact layer 23 may be a resin layer. Examples of resins that may be contained in the contact layer 23 include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6 and aramid, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, synthetic resins such as polycarbonate, and urethane.
[0175] Alternatively, the contact layer 23 may be a fiber layer containing a fiber component and a binder component that binds the fiber component. Alternatively, the contact layer 23 may contain paper. In this case, the contact layer 23 may contain paper as a primary component, or may contain paper in addition to a predetermined primary component. When the contact layer 23 contains paper, the contact layer 23 preferably contains paper that is strong enough to prevent the contact layer 23 from being accidentally torn when the sheet body 10 is attached to the application target. When the contact layer 23 contains paper, the contact layer 23 preferably contains, for example, silicone having a siloxane bond in addition to paper. The contact layer 23 has higher rigidity than, for example, the remaining portion of the sheet body 10 from which the release sheet 16 and the second release sheet 25 and the contact layer 23 and the weak adhesive layer 24 are omitted.
[0176] The thickness of the contact layer 23 can be set appropriately, but is, for example, 20 μm to 500 μm. When the contact layer 23 contains polyethylene terephthalate (PET), the thickness of the contact layer 23 is preferably, for example, 20 μm to 50 μm.
[0177] The weak adhesive layer 24 has a relatively low adhesive strength. For example, the adhesive strength of the weak adhesive layer 24 to the weather-resistant layer 13 is lower than the adhesive strength of the adhesive layer 11 to the base layer 12. Furthermore, for example, the adhesive strength of the weak adhesive layer 24 to the contact layer 23 is higher than the adhesive strength of the weak adhesive layer 24 to the weather-resistant layer 13. The weak adhesive layer 24 may be adhered to the weather-resistant layer 13 by, for example, static electricity. The weak adhesive layer 24 may contain a main component whose Tg is substantially 0. The weak adhesive layer 24 may contain, for example, ethylene vinyl acetate (EVA), urethane, silicone having a siloxane bond, acrylic, etc. The second release sheet 25 is not limited to the above-described configuration and may be, for example, the shape-imparting sheet 14.
[0178] 18 is a cross-sectional view schematically illustrating a sheet body 10 according to a fourth embodiment. The sheet body 10 of this embodiment includes a release sheet 29 disposed on the side of the weather-resistant layer 13 opposite the adhesive layer 11. As an example, the sheet body 10 has the adhesive layer 11, base layer 12, weather-resistant layer 13, and release sheet 29 disposed in this order in the thickness direction. The release sheet 16 is omitted from the sheet body 10 of this embodiment.
[0179] The release sheet 29 contains a surface 29a exposed to the outside and a release agent disposed in the vicinity thereof. An example of the release agent is silicone having a siloxane bond. This structure makes it difficult for the surface 29a and the adhesive surface 11a of the adhesive layer 11 to adhere to each other when the surface 29a exposed to the outside of the release sheet 29 comes into contact with the adhesive surface 11a of the adhesive layer 11 in the roll 26. Therefore, when the sheet 10 is unwound from the roll 26, the adhesive layer 11 can be easily peeled from the release sheet 29, allowing the sheet 10 to be unwound easily.
[0180] As described above, in the present disclosure, when unwinding the sheet body 10 from the roll body 26, the sheet body 10 may be preliminarily made easy to unwind from the roll body 26 so that, for example, the portion of the sheet body 10 provided with the adhesive component does not adhere to other portions of the sheet body 10, making it difficult to remove. Furthermore, the release sheet 29 has a predetermined rigidity. Therefore, in this embodiment, even if the release sheet 16 is omitted, the rigidity of the sheet body 10 can be improved. This improves the handleability of the sheet body 10, and the sheet body 10 can be easily attached to the target of attachment on a structure. In this case, the release sheet 29 has a higher rigidity than the remaining sheet body 10 after the release sheet 29 has been peeled off and removed.
[0181] The structure of the release sheet 29 can be set as appropriate. For example, as shown in Fig. 18, the release sheet 29 has a release substrate layer 28 having a surface 29a that contacts the attachment surface 11a of the adhesive layer 11 when the sheet body 10 is wound into a roll, and a weak adhesive layer 24 that is arranged on the adhesive layer 11 side of the release substrate layer 28 when the sheet body 10 is arranged flat. The release substrate layer 28 may have a similar structure to the contact layer 23, except that it contains, for example, a release agent. The release sheet 29 may also have a release agent layer arranged over the surface 29a.
[0182] 19 is a cross-sectional view schematically illustrating a sheet member 10 according to a fifth embodiment. The sheet member 10 of this embodiment includes a shape-imparting sheet 14 that is arranged on the opposite side of the weather-resistant layer 13 from the adhesive layer 11 when the sheet member 10 is placed flat. The shape-imparting sheet 14 is a sheet that is used when forming the weather-resistant layer 13 described above. The sheet member 10 of this embodiment includes the shape-imparting sheet 14, which is not peeled off even after the weather-resistant layer 13 is formed.
[0183] As an example, the sheet body 10 has a release sheet 16, an adhesive layer 11, a base layer 12, a weather-resistant layer 13, and a shape-imparting sheet 14 arranged in this order in the thickness direction. The surface 14a exposed to the outside of the shape-imparting sheet 14 and the surface 16a exposed to the outside of the release sheet 16 are configured to be less likely to adhere to each other when they come into contact with each other. This allows the sheet body 10 to be easily unwound from the roll 26. The shape-imparting sheet 14 also has a predetermined rigidity. In this case, the shape-imparting sheet 14 has a higher rigidity than the remaining sheet body 10 after the release sheet 16 and the shape-imparting sheet 14 have been peeled and removed. Therefore, the shape-imparting sheet 14 can improve the rigidity of the remaining sheet body 10 after the release sheet 16 has been peeled and removed. Therefore, even if the rigidity of the remaining sheet body 10 after the first release sheet 16 and the shape-imparting sheet 14 have been peeled off is low, the handleability of the sheet body 10 can be improved and the sheet body 10 can be easily attached to the target object of the structure.
[0184] The shape-imparting sheet 14 may contain resin-laminated paper having pseudo-adhesion, which means that two components attached to each other cannot be re-adhered once they are peeled off. In this case, for example, the shape-imparting sheet 14 may contain resin-laminated paper in which a resin layer and paper are laminated together, and the resin layer and the paper are bonded to each other by pseudo-adhesion within the resin-laminated paper. According to this configuration, when the paper in the resin-laminated paper is peeled off from the resin layer while the resin layer is attached to the weather-resistant layer 13, only the paper is peeled off and removed, and the resin layer remains attached to the weather-resistant layer 13 of the sheet body 10.
[0185] Next, in the third to fifth embodiments, an example of an application method for reinforcing or repairing a structure by attaching a sheet 10 to the structure is described. In this application method, a worker unrolls the required length of the sheet 10 from the roll 26. Next, in the third and fifth embodiments, the worker peels off the release sheet 16 from the sheet 10 and applies the exposed adhesive surface 11a of the adhesive layer 11 to the surface of the structure to which the sheet is to be attached. At this time, the worker may peel off the release sheet 16 from the sheet 10 little by little, and apply the exposed adhesive surface 11a of the adhesive layer 11 to the surface of the structure to which the sheet is to be attached. On the other hand, in the fourth embodiment, the worker applies the adhesive surface 11a of the adhesive layer 11 of the sheet 10 to the surface of the structure to which the sheet is to be attached.
[0186] Then, in the third to fifth embodiments, after the worker has attached the sheet body 10 to the object to be attached, he or she peels and removes the corresponding second peel-off sheet 25, release sheet 29, or shape-imparting sheet 14 from the sheet body 10.
[0187] That is, the present application methods according to the third to fifth embodiments include a preparation step of preparing a roll 26 in which the sheet body 10 is wound into a roll, a payout step of paying out the sheet body 10 from the roll 26, and an attachment step of peeling the first release sheet 16 from the paid-out sheet body 10 and attaching the exposed attachment surface to the surface of a structure. Here, in the preparation steps of the third and fifth embodiments, the roll 26 is prepared using a sheet body 10 whose attachment surface 11 a is covered with the first release sheet 16.
[0188] In this application method, the sheet body 10 of the roll body 26 prepared in the preparation step has a laminated structure including a weather-resistant layer 13 and an adhesive layer 11, and a cover sheet is disposed on the side of the weather-resistant layer 13 opposite to the adhesive layer 11. The sheet body 10 including this cover sheet is wound into a roll in the roll body 26, and the cover sheet may be peeled off and removed during or after the attachment step. This cover sheet may be any of the second release sheet 25, the release sheet 29, and the shape-imparting sheet 14.
[0189] Furthermore, in the construction method of the fourth embodiment, the sheet body 10 of the roll body 26 prepared in the preparation step has a laminated structure including the weather-resistant layer 13 and the adhesive layer 11, and has a release sheet 29 that is arranged on the opposite side of the weather-resistant layer 13 from the adhesive layer 11 and is separate from the peel-off sheet 16, and in the preparation step, the roll body 26 in which the sheet body 10 is wound into a roll shape may be prepared so that the release sheet 29 comes into contact with the adhesive layer 11.
[0190] When using the sheet body 10 of the present disclosure, for example, a supply item 38 shown below can be used. FIG. 20 is a schematic diagram showing the structure of a supply item 38 containing the sheet body 10 of the present disclosure. FIG. 17 shows a sheet body 10 including a release sheet 16 as an example. The supply item 38 shown in FIG. 20 includes a roll 26 around which a strip-shaped sheet body 10 is wound, and a container 27 having a storage space 27a for storing the roll 26. The container 27 has a supply port 27b that can unwind and supply the sheet body 10 from the roll 26 stored in the storage space 27a to the outside. The supply port 27b has a width dimension equal to or greater than the width dimension of the sheet body 10 in the axial direction of the roll 26.
[0191] For example, a worker can carry the supply item 38 to a construction site, unwind the required length of sheet 10 from the supply item 38, and use the sheet 10 for construction. Therefore, the supply item 38 allows the sheet 10 to be stored in the form of a roll 26 suitable for storage. Furthermore, when using the sheet 10, only the required amount can be unwound from the supply item 38. This improves work efficiency.
[0192] Furthermore, when unwinding the sheet body 10 from the supply port 27b, the worker can unwind the sheet body 10 while applying uniform tension to the entire widthwise area of the sheet body 10 by, for example, pressing the entire widthwise area of the sheet body 10 against the periphery of the opening of the supply port 27b. This allows the sheet body 10 to be applied to the surface of the structure 21 with uniform tension. Therefore, it is possible to prevent the sheet body 10 from unexpectedly shrinking or expanding after application due to uneven tension acting on the sheet body 10 after application. Note that in order to apply uniform tension to the entire widthwise area of the sheet body 10, a separate member such as a long member that extends in the widthwise direction of the sheet body 10 and comes into contact with the sheet body 10 may be disposed, for example, around the periphery of the opening of the supply port 27b.
[0193] Furthermore, the sheet body provided in the supply item 38 may be any sheet body of the present disclosure, for example, the sheet body 10 of any of the third to fifth embodiments, or the sheet body 10 of other embodiments.
[0194] [4] Sixth Embodiment (Sheet Body of the Present Disclosure in Which a Separate Entity is Overlaid on the Side Opposite to the Structure Side) An object separate from the sheet body 10 may be placed (attached) on the upper surface of the sheet body 10 attached to the structure 21. An example of such an object is a solar cell unit 33. FIG. 21 shows a schematic perspective view of the sheet body 10 and the solar cell unit 33 overlaid thereon. FIG. 22 shows a schematic cross-sectional view of the sheet body 10 and the solar cell unit 33 of FIG. 21. FIG. 22 is a cross-sectional view taken along the arrow XXI-XXI in FIG. 21. In FIGS. 21 and 22, the solar cell unit 33 is shown as an example of an object 33 separate from the sheet body 10.
[0195] In this embodiment, as shown in FIGS. 21 and 22 , the solar cell unit includes multiple power generation units 33a-33c arranged side by side and connected by electrical wiring. As an example, the solar cell unit 33 is fixed by adhesive or other means to the surface of the sheet member 10 opposite the structure 21. The roof 30, which is the structure 21, includes multiple plate members 35-37 arranged with portions of the plate members 35-37 overlapping each other. As a result, steps 30a are formed between adjacent plate members 35-37 in a plan view of the roof 30. The sheet member 10 is attached to the roof 30 so as to conform to the plate surfaces of the plate members 35-37 and the surfaces of the steps 30a. The multiple power generation units 33a-33c are arranged corresponding to the plate surfaces of the plate members 35-37. This prevents the power generation units 33a-33c from being affected by the steps 30a and restricting the angle of their outer surfaces relative to the horizontal.
[0196] The structure of the solar cell unit 33 is not limited and may be a known structure. For example, a thin or lightweight structure is preferable. The type of solar cell is also not limited. Examples of types of solar cells include amorphous silicon solar cells, crystalline silicon solar cells, cadmium telluride solar cells, copper indium gallium selenide solar cells, organic thin-film solar cells, perovskite solar cells, and gallium arsenide solar cells. Furthermore, for example, flexible amorphous silicon solar cells, cadmium telluride solar cells, copper indium gallium selenide solar cells, organic thin-film solar cells, and perovskite solar cells are suitable for combination with the sheet body 10 of the present disclosure.
[0197] 21 and 22 show a sheet-body-attached solar cell unit 40 including a sheet body 10 that is attached to a structure 21 to reinforce or repair the structure 21, and a solar cell unit 33 attached directly or indirectly to the sheet body 10. The sheet body 10 included in the sheet-body-attached solar cell unit 40 has an adhesive strength such that the measured value in a 180° peel test is 1.5 N / 25 mm or more and the maximum test force in the tensile elastic region is 100% or less, before being attached to the structure 21. In this embodiment as well, the various effects of the sheet body 10 of the present disclosure are achieved.
[0198] Furthermore, solar cell units are typically fixed to structures such as roofs and mounting frames by various methods, such as by bonding with adhesives or fastening with fastening members, after being adjusted to a position and angle suitable for power generation. To ensure this fixation, solar cell units are fixed to structures by various methods. Depending on the method of fixing the solar cell units and the conditions of the construction site, the solar cell units may not be easy to handle, increasing the workload of workers. Furthermore, when it becomes necessary to remove the solar cell units, they cannot be easily removed from the structure, increasing the workload of removal. Furthermore, deterioration of the structure also easily leads to deterioration of the solar cell units.
[0199] In contrast, in the present embodiment, for example, if the solar cell unit 33 is attached to the sheet body 10 in advance, when the sheet body 10 is attached to the structure, the solar cell unit 33 can be appropriately fixed to the structure 21 together with the sheet body 10. Furthermore, because the sheet body 10 can be reattached, the solar cell unit 33 can be removed from the structure 21 together with the sheet body 10 without undue strain. As a result, the solar cell unit 33 can be reliably attached to the structure 21 while reducing the workload of the worker through simple construction, and when removing the solar cell unit 33 from the structure 21, the solar cell unit 33 can be easily removed together with the sheet body 10.
[0200] For example, perovskite solar cells and copper indium gallium selenide solar cells are required to have higher durability than other solar cells. If the sheet body 10 of the present disclosure is applied to a solar cell unit 33 including a solar cell that is required to have such high durability, the sheet body 10 can reliably fix the solar cell unit 33 to the structure 21. Furthermore, deterioration of the solar cell unit 33 due to deterioration of the structure 21 is less likely to occur, making it easier to achieve high durability for the solar cell unit 33. Furthermore, the solar cell unit 33 can generate stable power with high conversion efficiency.
[0201] 21 and 22 , even if the surface shape of the structure 21 to which the sheet body 10 is to be attached is not flat due to differences in height caused by irregularities or defects, the sheet body 10 can be attached by conforming well to the surface. Therefore, the sheet body 10 can be suitably applied. However, this is not limited to this, and even if the surface shape of the structure 21 to which the sheet body 10 is to be attached is flat, applying the sheet body 10 is preferable because it makes it easier to obtain high durability of the solar cell unit 33 and enables the solar cell unit 33 to generate stable power with high conversion efficiency.
[0202] Furthermore, the sheet member 10 of this embodiment has an adhesive strength of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region before being attached to the structure 21, and exhibits excellent weather resistance. Therefore, the solar cell unit 33 can be fixed to the structure 21 while protecting the structure 21 with the sheet member 10 for a long period of time. Therefore, the solar cell unit 33 can be used stably while suppressing deterioration of the solar cell unit 33 due to deterioration of the structure 21.
[0203] Furthermore, the sheet member 10 of this embodiment has waterproof properties that do not cause water leakage in a waterproofing test after a weather load test before being attached to the structure 21, and therefore can secure the solar cell unit 33 to the structure 21 over a long period of time while protecting the structure 21 from deterioration due to water leakage. Therefore, the solar cell unit 33 can be used stably while suppressing deterioration of the solar cell unit 33 that accompanies deterioration of the structure 21.
[0204] Furthermore, when a deformation test is conducted on the sheet body 10 of this embodiment in which the operations described in (1), (2), (3), and (4) are performed in sequence, the energy calculated in (4) is 2.0 mJ or more. Therefore, the sheet body 10 has appropriate rigidity. This makes it easier for workers to install the solar cell units 33 on the structure 21.
[0205] Furthermore, when a plurality of sheet bodies 10 with solar cell units 33 attached thereto are attached to the surface of a structure 21, even if gaps occur between the sheet bodies 10 and the surface of the structure 21 is exposed to the outside, the surface of the structure 21 can be easily covered by separately attaching a sheet body 10 of the present disclosure to the surface of the structure 21 corresponding to the gap. In this case, for example, a sheet body 10 having a long shape (for example, a strip shape) can be used to match the shape of the gap.
[0206] Furthermore, since the sheet body 10 has flexibility to the extent that it can be wound up into a roll, when a solar cell unit 33 having a predetermined flexibility is attached to the sheet body 10, flexibility is ensured for the entire sheet-attached solar cell unit 40. Therefore, the sheet-attached solar cell unit 40 can be easily installed and placed on various structures 21. It is also possible to manage the sheet-attached solar cell unit 40 in a rolled-up state. Furthermore, for example, the sheet-attached solar cell unit 40 can be transported to the installation site in a rolled-up state and installed easily on a relatively large installation surface.
[0207] In this way, the sheet body 10 equipped with the solar cell unit 33 of the present disclosure can be suitably attached to various structures 21, such as an outdoor building structure 21, a mounting structure 21 installed on land, or a window that is installed as a structure 21 integral with building materials.
[0208] (Application of Sheet Body to Structure) The application of the sheet body of the present disclosure to a structure 21 will be described below. The sheet body 10 of the present disclosure has excellent adhesive strength. Therefore, when attached to the surface of the structure 21, such as the roof, the sheet body 10 can be attached without gaps even to the surface of the structure 21 that has steps. By attaching the sheet body 10, it is possible to prevent water from entering the structure 21 from the outside and to prevent the intrusion of deteriorating factors such as salt water and oxygen that cause rust, for decades. Therefore, it is possible to appropriately suppress deterioration of the structure 21. Furthermore, the sheet body 10 can be installed simply by attaching it to the surface of the structure 21. Therefore, installation can be performed without relying on the skill of the worker, thereby shortening the construction period and reducing labor costs.
[0209] When applying the sheet body of the present disclosure, a primer layer containing a curable resin material may be formed in advance on the surface of the structure 21. Examples of properties required of the primer layer include excellent initial adhesion to the structure protection sheet to be applied, long-term adhesion allowing for long-term storage, sealing properties that firmly adhere the coating film to the deteriorated structure surface and prevent harmful substances from scattering from the deteriorated structure when it is reapplied, curability that allows for quick curing, a pot life that ensures fluidity for a certain period of time, and paint workability that does not require strict blending work at the work site.
[0210] The material for the primer layer is not particularly limited as long as it can provide the physical properties required for the primer layer. For example, there is no particular limitation on the material as long as it has the property of being cured by moisture curing, heat curing, photocuring, or other methods to form a resin. Examples of such materials include acrylic, polyester, urethane, epoxy, and silicone resins. For example, a material containing a reaction product of a polymer containing a (meth)acrylic acid alkyl ester monomer unit in the main chain and raw material compounds containing an epoxy compound and an aminosilane compound is preferred.
[0211] The primer layer is generally used as an undercoat material for the structure 21. In the present disclosure, the primer may be applied to the surface of the structure 21. The undercoat material can be applied by a conventional method. For example, the primer layer, which is an undercoat material, is obtained by applying a paint to the surface of the structure 21 by a conventional method such as applying it with a brush or roller, or spraying it with a spray gun, and forming a coating film.
[0212] The thickness of the primer layer is not particularly limited. For example, the thickness of the primer layer in a wet state is 20 g / m 2 The thickness of the primer layer is, for example, 30 g / m in a wet state. 2 A value of 50 g / m or more is preferable. 2 More preferably, the value is 100 g / m or more. 2 More preferably, the value is 200 g / m 2 The above values are particularly preferred.
[0213] On the other hand, the thickness of the primer layer is, for example, 800 g / m in a wet state. 2 The thickness of the primer layer is, for example, 700 g / m in a wet state. 2 The following values are preferred: 600 g / m 2 The following values are more preferred: 2 The following values are more preferable. In particular, the thickness of the primer layer is, for example, 400 g / m in a wet state. 2 The following values are preferable because they can stabilize the adhesive strength of the sheet 10 to the surface of a structure in various states. The "wet state" referred to here refers to the state before the coating liquid dries, and the above numerical values indicating the wet state refer to the coating weight.
[0214] Several examples and several comparative examples according to the present disclosure were prepared. The several examples and several comparative examples according to the present disclosure will be specifically described. (Example 1) A 130 μm thick shaped sheet 14, which was a PP laminate sheet manufactured by Lintec Corporation, was prepared. A weather-resistant layer-forming composition containing an acrylic resin (a mixture of Cool Life SP Black (CB1) P5-0 manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd. and FC Coat Water-Based Silicone Elastic Black manufactured by Fujikura Kasei Co., Ltd. in a weight ratio of 50:50) was applied onto this shaped sheet 14. The formed coating was dried to form a single-layer weather-resistant layer having a thickness of 110 μm.
[0215] Next, a mixture was prepared by mixing the cement and admixture of a composition for forming a base layer (manufactured by Kikusui Chemical Co., Ltd., Spring Coat (trowel)) in a ratio of 60:40. This mixture was applied to the weather-resistant layer. A vinylon-based mesh material (manufactured by Kuraray Co., Ltd., cheesecloth "Cremona", #600 (600 grit, thickness 230 μm)) was placed so as to press against the surface of the coating film of this mixture. This caused the coating film to harden, and a base layer with a thickness of 450 μm after hardening was formed on the weather-resistant layer.
[0216] Separately, 100 parts by weight of an acrylic adhesive (Olivine (registered trademark) BPS5565K) manufactured by Toyochem Co., Ltd. was mixed with 5 parts by weight of an isocyanate-based crosslinking agent (curing agent) (BHS8515) manufactured by Toyochem Co., Ltd. to prepare an adhesive mixture. This adhesive mixture was applied to the surface of a release sheet and dried to form an adhesive layer with a thickness of 100 μm. The adhesive layer was then superimposed on and adhered to a base layer to form the sheet member 10 according to Example 1. The adhesive (main adhesive) contained in the adhesive layer of Example 1 was "BPS5565K."
[0217] Example 2 A sheet member 10 according to Example 2 was fabricated in the same manner as in Example 1, except that the thickness of the adhesive layer in Example 1 was changed to 30 μm.
[0218] (Example 3) In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 20 parts by weight, and the thickness of the adhesive layer was set to 100 μm. In addition, the reinforcing material 15 was made of a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. The rest of the settings were the same as in Example 1, and a sheet body 10 according to Example 3 was constructed.
[0219] (Example 4) In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 50 parts by weight, and the thickness of the adhesive layer was set to 50 μm. In addition, the reinforcing material 15 was omitted. The rest of the configuration was the same as in Example 1, and a sheet body 10 according to Example 4 was constructed.
[0220] (Example 5) In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 50 parts by weight, and the thickness of the adhesive layer was set to 50 μm. In addition, the reinforcing material 15 was made of polyester nonwoven fabric (ELTAS (registered trademark) "E01012") manufactured by Asahi Kasei Corporation. The rest of the settings were the same as in Example 1, and a sheet body 10 according to Example 4 was constructed.
[0221] Example 6 In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 12 parts by weight, and the thickness of the adhesive layer was set to 100 μm. In addition, the reinforcing material 15 was made of a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. The rest of the settings were the same as in Example 1, and a sheet body 10 according to Example 6 was constructed.
[0222] (Example 7) In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 6 parts by weight, and the thickness of the adhesive layer was set to 100 μm. In addition, the reinforcing material 15 was made of a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. The rest of the settings were the same as in Example 1, and a sheet body 10 according to Example 7 was constructed.
[0223] Comparative Example 1 A sheet member according to Comparative Example 1 was fabricated in the same manner as in Example 1, except that the thickness of the adhesive layer in Example 1 was changed to 10 μm.
[0224] Comparative Example 2 A sheet member according to Comparative Example 2 was fabricated in the same manner as in Comparative Example 1, except that the thickness of the adhesive layer in Comparative Example 1 was changed to 200 μm.
[0225] (Comparative Example 3) A sheet body according to Comparative Example 3 was constructed in the same manner as Comparative Example 1, except that the thickness of the adhesive layer of Comparative Example 1 was changed to 100 μm and the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to a two-component curing acrylic adhesive (Olivine (registered trademark) BPS6617) manufactured by Toyochem Co., Ltd.
[0226] (Comparative Example 4) The thickness of the adhesive layer of Comparative Example 1 was changed to 50 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) was set to 50 parts by weight. In addition, the material of the reinforcing fiber, which is the reinforcing material, was set to a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Ltd. The rest was set in the same way as in Comparative Example 1, and a sheet body according to Comparative Example 4 was constructed.
[0227] (Comparative Example 5) In the adhesive layer of Comparative Example 1, the adhesive (main adhesive agent) was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the thickness of the adhesive layer was changed to 100 μm, and the curing agent ratio (crosslinking agent ratio) of the adhesive layer of Comparative Example 1 was changed to 11 parts by weight. In addition, the reinforcing material was composed of polyester nonwoven fabric (ELTAS (registered trademark) "E01012") manufactured by Asahi Kasei Corporation. The rest of the settings were the same as in Comparative Example 1, and a sheet body according to Comparative Example 5 was constructed.
[0228] (Comparative Example 6) The thickness of the adhesive layer was changed to 100 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) of the adhesive layer was set to 6 parts by weight. In addition, the reinforcing material was omitted. The rest of the settings were the same as those of Comparative Example 1, and a sheet body according to Comparative Example 6 was constructed.
[0229] (Comparative Example 7) The thickness of the adhesive layer of Comparative Example 1 was changed to 100 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) of the adhesive layer was changed to 6 parts by weight. In addition, the reinforcing material was composed of a polyester nonwoven fabric (ELTAS (registered trademark) "E01012") manufactured by Asahi Kasei Corporation. The rest of the settings were the same as those of Comparative Example 1, and a sheet body according to Comparative Example 7 was constructed.
[0230] (Comparative Example 8) The thickness of the adhesive layer of Comparative Example 1 was changed to 50 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) of the adhesive layer was changed to 50 parts by weight. In addition, the base material layer and reinforcing material were omitted. The rest of the settings were the same as those of Comparative Example 1, and a sheet body according to Comparative Example 8 was constructed.
[0231] For the sheet bodies 10 according to Examples 1 to 7 and the sheet bodies according to Comparative Examples 1 to 8, a 180° peel test (adhesive strength (N / 25 mm)), measurement of tensile elasticity (maximum test force in the tensile elastic region (N / 25 mm)), calculation of adhesive strength / tensile elasticity (%) before the weathering load test, evaluation of rework (re-adhesion) before the weathering load test, overlapping waterproof test (waterproofness test), and deformation test were performed before and after the weathering load test. In addition, the following air and water spray test was performed on the sheet bodies 10 according to Examples 1 to 7 and the sheet bodies according to Comparative Examples 1 to 8 before and after the weathering load test.
[0232] (Air and Water Spray Test) The air and water spray test (strong wind resistance test) was conducted in accordance with JSTM J6403:2020 [Method for testing water leakage from metal roofs], a group standard of the Japan Testing Center for Building Materials. Specifically, the large-scale water spray test equipment owned by the Japan Testing Center for Building Materials was used. A plurality of strip-shaped sheet bodies 10 according to the present disclosure were prepared as test specimens. Here, FIG. 12 is a perspective view of a stand simulating a roof. FIG. 13 is a diagram showing the side and dimensions of the stand in FIG. 12. FIG. 14 is a front view of the stand in FIG. 12. For this test, the stands shown in FIGS. 12 to 14 were also prepared.
[0233] The prepared sheet bodies 10 of the example were lined up in the width direction, and each sheet body 10 was attached to a stand simulating a roof that had been pre-coated with a primer, with a portion of the width direction of each sheet body 10 overlapping the adjacent sheet body 10. Thereafter, an air and water spray test was carried out under the following test conditions, and it was visually confirmed whether or not the sheet body 10 had peeled off from the stand. Note that the same procedure was followed for the comparative example as well, and the same visual confirmation was carried out.
[0234] The test conditions were as follows: roof slope of the rack 4 sun, wind speed level 9 (lower limit wind speed: 38±2 m / min, upper limit wind speed: 62±2 m / min), water spray rate 4 L / min・m 2 The air and water spray holding time was set to 15 minutes.
[0235] The test specimens were attached to the surface of the stand by first applying a primer to the surface. Then, multiple sheets were placed on top of the primer so as to overlap each other, forming an overlap of 15 mm in the width direction. The multiple sheets were then attached to the top of the primer so as to cover the entire surface of the stand. The wind direction relative to the stand was set so as to blow air from the eaves toward the ridge.
[0236] The specifications for each example and each comparative example are shown in Table 1. Tables 2 and 3 also show the test results of the 180° peel test (adhesive strength (N / 25 mm)), tensile elasticity (maximum test force in the tensile elastic region (N / 25 mm)), adhesive strength / tensile elasticity (%) before the weathering load test, whether or not the film could be reworked (re-pasted) before the weathering load test, the overlap waterproof test (waterproofness test), and the deformation test before and after the weathering load test.
[0237]
[0238]
[0239]
[0240] First, we will describe representative Examples 1 and 2 and representative Comparative Examples 1 to 3. The measured values of the 180° peel test and the maximum test force in the tensile elastic region before the weathering load test were measured immediately after the sheet body was attached to the structure and before any substantial load was applied to the sheet body, and therefore are considered to be values that are close to the measured values of the 180° peel test and the maximum test force in the tensile elastic region before the sheet body was attached to the structure.
[0241] As shown in Tables 2 and 3, the sheet body 10 according to Example 1 had a 180° peel test measurement value of 17.6 N / 25 mm and a maximum test force in the tensile elastic region of 20 N / 25 mm before the weathering load test. Furthermore, when the sheet body 10 according to Example 1 was attached to a structure (a folded roof) at a construction site and then peeled off, no plastic deformation was observed in the sheet body 10, and it could be reattached.
[0242] Furthermore, the measured value of the 180° peel test after the weathering load test for the sheet member 10 according to Example 1 was 41.4 N / 25 mm. The reason why the adhesive strength in the 180° peel test was higher than that before the weathering load test is presumed to be that the adhesive layer softened under high heat of 70°C or higher and 80°C or lower, increasing the contact area and improving the adhesive strength due to the anchor effect.
[0243] Furthermore, in the results of the waterproofing test after the weather load test for the sheet body 10 of Example 1, no bright spots or water stains were found on the back surface of the fixing adherend (the surface on which the sheet body was not overlapped) when visually inspected, and it was determined that there was no water leakage.
[0244] Furthermore, in a deformation test, the sheet body 10 according to Example 1 required 23.0 mJ of energy to move the pressing jig downward by 20 mm at a test speed of 30 mm / min. The sheet body 10 according to Example 1, which has such rigidity, was easy to lay at the construction site and had excellent handleability. In addition, the sheet body 10 according to Example 1 did not peel off even after an air and water spray test.
[0245] The sheet body 10 according to Example 2 had a measured value of 3 N / 25 mm in a 180° peel test and a maximum test force in the tensile elastic region of 20 N / 25 mm. When the sheet body 10 according to Example 2 was attached to a structure (a steel roof) at a construction site and then peeled off, no plastic deformation was observed in the sheet body 10, and it could be reattached.
[0246] Furthermore, the sheet body 10 according to Example 2 had a measured value of 5 N / 25 mm in a 180° peel test after the weathering load test. Furthermore, in the results of the waterproofing test after the weathering load test, no bright spots or water stains were found by visual inspection on the back surface of the fixing adherend (the surface on which the sheet body was not overlapped), and it was determined that there was "no water leakage."
[0247] Furthermore, in a deformation test, the sheet body 10 according to Example 2 required 18.7 mJ of energy to move the pressing jig 20 mm at a test speed of 30 mm / min. The sheet body 10 according to Example 2, which has such rigidity, was easy to lay at the construction site and had excellent handleability. In addition, the sheet body 10 according to Example 2 did not peel off even after an air and water spray test.
[0248] Furthermore, as shown in Tables 1 and 3, the sheet body according to Comparative Example 1 had a measured value of 0.25 N / 25 mm in the 180° peel test, and peeling occurred after the air-spray and water-spray test. On the other hand, the sheet body according to Comparative Example 1 had a maximum test force in the tensile elastic region of 20 N / 25 mm. When the sheet body according to Comparative Example 1 was applied to a structure (a folded roof) at a construction site and then peeled off, no plastic deformation was observed in the sheet body, and it could be reapplied.
[0249] Furthermore, the sheet body according to Comparative Example 1 had a measured value of 1.0 N / 25 mm in a 180° peel test after a weathering load test. Furthermore, peeling occurred in an air-spray and water-spray test after the weathering load test. Furthermore, in the waterproofing test results after the weathering load test, the back surface of the fixing adherend (the surface on which the sheet body was not overlapped) was visually inspected, and no bright spots or water stains were observed, and the sheet body according to Comparative Example 1 was judged to have "no water leakage." Furthermore, in the deformation test, the energy required to move the pressing jig 20 mm at a test speed of 30 mm / min for the sheet body according to Comparative Example 1 was 16 mJ. The sheet body according to Comparative Example 1, which had such rigidity, was easy to install even at the construction site and had excellent handleability.
[0250] The sheet body according to Comparative Example 2 had a measured value of 25 N / 25 mm in a 180° peel test. Furthermore, no peeling occurred after the air-spray and water-spray test. Meanwhile, the maximum test force in the tensile elastic region of the sheet body according to Comparative Example 2 was 20 N / 25 mm. When the sheet body according to Comparative Example 2 was applied to a structure (a folded-height roof) at a construction site and then peeled off, plastic deformation was observed in the peeled sheet body, and it could not be reapplied, so it had to be discarded.
[0251] Furthermore, the sheet body according to Comparative Example 2 had a measured value of 60 N / 25 mm in a 180° peel test after the weathering load test. Furthermore, no peeling occurred in the air-spray and water-spray test after the weathering load test. Furthermore, in the waterproofing test results for the sheet body according to Comparative Example 2 after the weathering load test, no bright spots or water stains were observed on the back surface of the fixing adherend (the side on which the sheet body was not overlapped) by visual inspection, and it was determined to be "water-free." In addition, in the deformation test for the sheet body according to Comparative Example 2, the energy required to move the pressing jig 20 mm at a test speed of 30 mm / min was 25 mJ. The sheet body according to Comparative Example 2, which had such rigidity, was easy to install even at the construction site and had excellent handleability.
[0252] The sheet body according to Comparative Example 3 had a measured value of 0.2 N / 25 mm in a 180° peel test. Furthermore, peeling occurred after an air and water spray test. Meanwhile, the maximum test force in the tensile elastic region of the sheet body according to Comparative Example 3 was 20 N / 25 mm. When the sheet body according to Comparative Example 3 was applied to a structure (a folded-half roof) at a construction site and then peeled off, no plastic deformation was observed in the sheet body, and it could be reapplied.
[0253] Furthermore, the sheet according to Comparative Example 3 had a measured value of 1.3 N / 25 mm in a 180° peel test after the weathering load test. Also, peeling occurred in an air and water spray test after the weathering load test.
[0254] Furthermore, in the waterproofing test results after the weathering load test for the sheet body according to Comparative Example 3, no bright spots or water stains were found on the back surface of the fixing adherend (the surface on which the sheet body was not overlapped) when visually inspected, and it was judged to be "water-leak-free." In addition, in the deformation test for the sheet body according to Comparative Example 3, the energy required to move the pressing jig 20 mm at a test speed of 30 mm / min was 22 mJ. The sheet body according to Comparative Example 3, which had such rigidity, was easy to lay even at the construction site and had excellent handleability.
[0255] Additionally, as shown in Tables 2 and 3, it was confirmed that all of the sheet bodies 10 according to Examples 3 to 7 had performance comparable to or better than that of Examples 1 and 2. In contrast, it was confirmed that in Comparative Examples 4 to 8, the measured value of the 180° peel test before the weathering load test was less than 1.5 N / 25 mm (Comparative Example 4), or the adhesive strength before the weathering load test was 100% or more of the maximum test force in the tensile elastic region (Comparative Examples 5 to 7). As a result, it is considered difficult for any of Comparative Examples 3 to 8 to achieve, compared to Examples 1 to 7, the effect of ensuring excellent adhesion to structures while also achieving the effect of improving handleability so as to enable reapplication of the sheet body at the construction site.
[0256] Furthermore, as shown in Table 3, the deformation test results for all of Examples 1 to 7 were favorable (the energy required to move the pressing jig 17 was at least 2.0 mJ), confirming their excellent durability. Therefore, it is believed that Examples 1 to 7 can be adequately used to reinforce or repair structures even after re-application. Comparative Example 8 had low rigidity, making it impossible to measure the deformation test. Furthermore, in an air and water spray test conducted on the sheet bodies 10 according to Examples 1 to 7 and the sheet bodies according to Comparative Examples 1 to 8 before and after the weathering load test, no significant differences were observed between Examples 1 to 7 and Comparative Examples 1 to 8.
[0257] (Disclosure Items) The following items disclose preferred embodiments of the sheet body of the present disclosure.
[0258] [Item 1] A sheet body that is attached to a structure to be used for reinforcing or repairing the structure, wherein, before being attached to the structure, the sheet body has an adhesive strength of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region.
[0259] According to the above configuration, the sheet body has an adhesive strength of 1.5 N / 25 mm or more measured in a 180° peel test before being attached to a structure, thereby ensuring excellent adhesive strength of the sheet body to the structure. This allows the structure to be appropriately repaired or restored. Furthermore, the sheet body has an adhesive strength of 100% or less in the tensile elastic region maximum test force before being attached to the structure, thereby improving the handleability of the sheet body at the construction site. In other words, once the sheet body is attached, it is less likely to undergo plastic deformation when peeled off, making it less likely to be damaged and allowing it to be reattached. This allows the sheet body to have excellent adhesive strength to the structure while improving the handleability of the sheet body at the construction site.
[0260] [Item 2] The sheet member according to item 1, further having an adhesive strength such that the measured value of the 180° peel strength after a weathering load test is 1.5 N / 25 mm or more.
[0261] According to the above-mentioned configuration, it is ensured that the adhesive strength after the weathering load test is the same as that before being attached to the structure, and therefore a sheet body with excellent weather resistance can be provided.
[0262] [Item 3] The sheet member according to item 1 or 2, further having waterproofness such that no water leakage occurs in a waterproofing test after a weathering load test.
[0263] According to the above-described configuration, the predetermined waterproof property of the sheet body is ensured even after the weather load test, and therefore, a sheet body with excellent weather resistance can be provided.
[0264] [Item 4] The sheet body according to any one of Items 1 to 3, wherein, when a deformation test is conducted in which the operations described in Items (1), (2), (3), and (4) below are performed in sequence, the energy calculated by the calculation in (4) below is a value of 2.0 mJ or more. (1) A rectangular sheet body having short sides of 50 mm and long sides of 100 mm is prepared as a sample. (2) The sample is curved so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample from the edges of the pair of short sides to a position 15 mm apart along the long sides is gripped and fixed with a fixing portion, thereby forming a curved portion with a perimeter of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample arranged parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface having a diameter of 100 mm and a thickness of 10 mm is used, and the pressing tool is brought into contact with the curved portion from above in an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool is moved downward by 20 mm at a test speed of 30 mm / min. (4) The energy required to move the pressing tool is calculated.
[0265] According to the above-mentioned configuration, it is possible to impart appropriate rigidity to the sheet body, which makes it easy to handle when applying the sheet body to the surface of a structure. More specifically, it makes it easy to lay the sheet body on the surface of a structure.
[0266] [Item 5] The sheet member according to any one of items 1 to 4, comprising: an adhesive layer attached to the structure; and at least one weather-resistant layer disposed above the adhesive layer.
[0267] [Item 6] The sheet member according to item 5, further comprising a substrate layer disposed between the adhesive layer and the weather-resistant layer.
[0268] [Item 7] The sheet body according to Item 6, wherein the base material layer includes a reinforcing material.
[0269] [Item 8] The sheet member according to item 6 or 7, wherein at least one of the adhesive layer and the weather-resistant layer contains a filler.
[0270] [Item 9] The sheet member according to any one of items 5 to 7, further comprising: a release sheet disposed on the surface of the adhesive layer opposite to the weather-resistant layer side.
[0271] [Item 10] The sheet body according to any one of items 1 to 4, which is constituted by a single layer and contains an adhesive component that is unevenly distributed on the second surface side, which is the attachment surface to be attached to the structure, compared to the first surface side, which is located opposite the structure.
[0272] [Item 11] The sheet member according to item 10, which contains rubber and has a crosslinked structure of the rubber with a different degree of crosslinking on the first surface side and the second surface side.
[0273] [Item 12] The sheet member according to item 10 or 11, comprising an acrylic resin and an epoxy resin, and having a phase-separated structure between the acrylic resin and the epoxy resin.
[0274] The configurations of the present disclosure are not limited to the above-described embodiments and examples, and the configurations and methods can be changed, added, or deleted without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification.
[0275] REFERENCE SIGNS LIST 10 Sheet body 11 Adhesive layer 12 Base layer 13 Weather-resistant layer 15 Reinforcing material 16 Release sheet 17 Pressing jig 18 Fixing part 19 Sample 21 Structure 30 Roof 31 Blue tarp 32 Sandbag
Claims
1. A sheet body to be attached to a structure to reinforce or repair said structure, which, prior to being attached to said structure, has an adhesive strength of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region.
2. The sheet according to claim 1, further having an adhesive strength such that the measured 180° peel strength after a weather load test is 1.5 N / 25 mm or more.
3. The sheet member according to claim 1, further having waterproofness such that there is no water leakage in a waterproofness test after a weather load test.
4. The sheet body according to claim 1, in which, when a deformation test is carried out by sequentially carrying out the operations described in the following items (1), (2), (3), and (4), the energy calculated by the calculation in the following (4) is a value of 2.0 mJ or more. (1) The rectangular sheet body with short sides of 50 mm and long sides of 100 mm is prepared as a sample. (2) The sample is curved so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample from the edges of the pair of short sides to a position 15 mm away along the long sides is gripped and fixed with a fixing part to form a curved part with a circumference of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample arranged parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface of 100 mm in diameter and 10 mm in thickness is used to contact the curved portion from above in an environment of a temperature of 23±2° C. and a humidity of 50±10% RH, and the pressing tool is moved downward by 20 mm at a test speed of 30 mm / min. (4) The energy required to move the pressing tool is calculated.
5. A sheet member according to any one of claims 1 to 4, comprising: an adhesive layer attached to the structure; and at least one weather-resistant layer disposed above the adhesive layer.
6. The sheet member according to claim 5, further comprising a substrate layer disposed between the adhesive layer and the weather-resistant layer.
7. The sheet member according to claim 6, wherein the base layer includes a reinforcing material.
8. The sheet member according to claim 6, wherein at least one of the adhesive layer and the weather-resistant layer contains a filler.
9. The sheet member according to claim 5, further comprising a release sheet disposed on the surface of the adhesive layer opposite the weather-resistant layer.
10. The sheet according to any one of claims 1 to 4, which is constituted by a single layer and contains an adhesive component that is biased toward the second surface side, which is the attachment surface to be attached to the structure, rather than toward the first surface side, which is located opposite the structure.
11. The sheet member according to claim 10, which contains rubber and has a crosslinked structure of the rubber with a different degree of crosslinking on the first surface side and the second surface side.
12. The sheet according to claim 10, comprising an acrylic resin and an epoxy resin, and having a phase-separated structure between the acrylic resin and the epoxy resin.
Citation Information
Patent Citations
Sheet and method for repairing and reinforcing concrete structure
JP2002256707A
Coating film protective sheet
JP2011084655A
Method of repairing or reinforcing target structure and tacky adhesive sheet used for the same
JP2016169576A
Foamable adhesive sheet and method for manufacturing article
JP7204971B1
Fall-preventing transparent sheet and fall-preventing transparent sheet manufacturing method
WO2020116450A1