Solid electrolyte including covalent organic framework, and all-solid-state battery including same
The integration of a covalent organic skeletal structure and cross-linked polymer in solid electrolytes addresses chemical instability and conductivity issues, resulting in improved battery performance and lifespan for all-solid-state batteries.
Patent Information
- Application Number
- PCT/KR2024/005065
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
Current solid electrolytes for all-solid-state batteries face challenges such as chemical instability, insufficient ionic conductivity, and interfacial resistance, which hinder the development of high-energy density and safe lithium batteries.
A solid electrolyte with a covalent organic skeletal structure and a cross-linked polymer derived from polyalkylene oxide-based multifunctional monomers, such as 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, and methacrylamide, is developed to enhance chemical stability and ionic conductivity, forming a lithium ion channel for improved battery performance.
The solution achieves high ionic conductivity, extended lifespan, and enhanced rate characteristics, ensuring excellent interfacial compatibility and mechanical strength, thus overcoming the limitations of existing solid electrolytes.
Smart Images

Figure KR2024005065_24102024_PF_FP_ABST
Abstract
Description
Solid electrolyte comprising a covalent organic skeleton structure and an all-solid-state battery comprising the same
[0001] The present invention relates to a solid electrolyte comprising a covalently bonded organic skeleton structure and an all-solid-state battery comprising the same.
[0002] Recently, as the development of lithium batteries with improved energy density and safety has become a necessity, all-solid-state batteries that use solid electrolytes instead of liquid electrolytes are attracting attention as next-generation batteries.
[0003] Solid electrolytes can be classified into polymer solid electrolytes or inorganic solid electrolytes depending on their material. In particular, inorganic solid electrolytes have the advantage of securing high cation transport coefficients and ionic conductivity. However, inorganic solid electrolytes have chemical instability, high interfacial resistance with electrodes, and require high temperature / high pressure conditions during cell manufacturing and operation. In particular, commercialization is difficult due to problems such as dendrite growth through voids caused by grain boundary defects in inorganic solid electrolytes.
[0004] In contrast, polymer solid electrolytes offer advantages over inorganic solid electrolytes in terms of flexibility, lightness, processability, and chemical stability. However, compared to conventional liquid and inorganic solid electrolytes, polymer solid electrolytes have lower ionic conductivity and lithium ion yield at room temperature. Furthermore, their low electrochemical window hinders their combination with high-voltage cathode materials.
[0005] Therefore, to solve the above problems, there is an urgent need for research on solid electrolytes with excellent chemical stability and ionic conductivity and all-solid-state batteries including the same.
[0006] In order to solve the above-described problems, the present invention aims to provide a solid electrolyte having excellent chemical stability and excellent ionic conductivity and lithium ion yield.
[0007] In addition, another object of the present invention is to provide an all-solid-state battery having excellent battery performance, life characteristics, and rate characteristics, including the solid electrolyte.
[0008] In order to achieve the above-described task, the inventors of the present invention have continuously conducted research to produce a solid electrolyte having excellent chemical stability and excellent ionic conductivity, and as a result, they have discovered that a solid electrolyte produced from a slurry composition mixing (i) a covalent organic skeleton structure including a specific repeating unit and (ii) a crosslinkable monomer selected from a polyalkylene oxide-based multifunctional monomer, 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, methacrylamide, and a combination of two or more thereof exhibits excellent ionic conductivity and lithium ion yield, and a battery including the same can realize the effect of significantly improving life characteristics and rate characteristics, thereby completing the present invention.
[0009] The present invention provides a solid electrolyte comprising a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1; and a crosslinked polymer derived from a crosslinkable monomer.
[0010] [Chemical Formula 1]
[0011]
[0012] In the above chemical formula 1, A is a monocyclic or polycyclic ring compound, -X- is a divalent linking group, R1 to R4 are each independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not -H at the same time, and M is Li, Li2 or Li3.
[0013] According to one embodiment of the present invention, in the chemical formula 1, -X- may be any one selected from the group consisting of a direct bond, -NH-, =CH-NH-, -NH-C(=O)-, -CH=CH-NH-, -OC(=O)-NH-, -CH2-C(=O)O-NH-, -B(-O-)2, and -C(=O)NH-N=CH-.
[0014] According to one embodiment of the present invention, the chemical formula 1 may be represented by the following chemical formula 1-1.
[0015] [Chemical Formula 1-1]
[0016]
[0017] In the above chemical formula 1-1, R1 to R4 are the same as defined in the above chemical formula 1.
[0018] According to one embodiment of the present invention, the covalently bonded organic skeleton structure may be a polygonal structure including a repeating unit of the chemical formula 1 on one side and having a pore formed on the inside.
[0019] According to one embodiment of the present invention, the pores of the covalent organic skeleton structure may have a diameter of 1.0 to 8.0 nm.
[0020] According to one embodiment of the present invention, the covalent organic skeleton structure may include a repeating unit represented by the following chemical formula 2.
[0021] [Chemical Formula 2]
[0022]
[0023] In the above chemical formula 2, R1 to R4 are each independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not -H at the same time, and M is Li, Li2 or Li3.
[0024] According to one embodiment of the present invention, the crosslinkable monomer is selected from polyalkylene oxide-based multifunctional monomers, 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, methacrylamide, and combinations of two or more thereof.
[0025] According to a preferred embodiment, the crosslinkable monomer is a polyalkylene oxide-based multifunctional monomer, and when a polyalkylene oxide-based multifunctional monomer is used, it is preferable in that it can facilitate the movement of lithium ions within the organic skeletal structure and maximize ion conductivity.
[0026] The above polyalkylene oxide-based multifunctional monomer may include two or more reactive functional groups selected from the group consisting of an acrylic group, a methacrylic group, a vinyl group, a thiol group, an epoxy group, an isocyanate group, a silanol group, a halogen group, a carboxyl group, a hydroxyl group, and an amine group.
[0027] According to one embodiment of the present invention, the polyalkylene oxide-based multifunctional monomer may have a number average molecular weight of 100 to 10,000 g / mol.
[0028] According to one embodiment of the present invention, the crosslinking polymer may be included in an amount of 1 to 100 parts by weight based on 100 parts by weight of the covalent organic skeleton structure.
[0029] According to one embodiment of the present invention, the thickness of the solid electrolyte may be 0.1 to 100 μm.
[0030] According to one embodiment of the present invention, the lithium ion conductivity of the solid electrolyte is 6.0 x10 -5 It can be more than S / cm.
[0031] The present invention can provide an all-solid-state battery including the above-described solid electrolyte.
[0032] The present invention can provide a method for producing a solid electrolyte, comprising the steps of (S1) applying pressure to a slurry composition for producing a solid electrolyte, which comprises (i) a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1 and (ii) a crosslinkable monomer selected from a polyalkylene oxide-based multifunctional monomer, 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, methacrylamide, and a combination of two or more thereof, and (S2) polymerizing the solid electrolyte slurry composition to produce a crosslinked polymer.
[0033] According to one embodiment of the present invention, in the step (S1), a pressure of 5 to 250 MPa may be applied.
[0034] The present invention can provide a slurry composition for preparing a solid electrolyte, comprising (i) a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1 and (ii) a crosslinkable monomer selected from among polyalkylene oxide-based multifunctional monomers, 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, methacrylamide, and combinations of two or more thereof.
[0035] [Chemical Formula 1]
[0036]
[0037] In the above chemical formula 1, A is a monocyclic or polycyclic ring compound, -X- is a divalent linking group, R1 to R4 are each independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not -H at the same time, and M is Li, Li2 or Li3.
[0038] An all-solid-state battery employing a solid electrolyte according to one embodiment of the present invention can simultaneously satisfy excellent battery performance, cycle life characteristics, and rate characteristics. Specifically, the solid electrolyte according to one embodiment can realize high ionic conductivity and energy density at room temperature by forming lithium ion channels between the covalent organic skeleton structure layers of the cross-linked polymer to induce rapid lithium ion movement. Furthermore, it has the advantages of excellent interfacial compatibility with the electrode, mechanical strength, and oxidation stability, and excellent interfacial stability with the lithium metal negative electrode, as well as excellent processability, making it advantageous for commercialization.
[0039] Figure 1 is a Fourier transform infrared spectroscopy (ATR-FT-IR) analysis spectrum of COF-1 and COF-2 according to Manufacturing Examples 1 and 2.
[0040] Figure 2 is an X-ray diffraction (XRD) analysis spectrum of COF-1 and COF-2 according to Manufacturing Examples 1 and 2.
[0041] Figure 3 is a graph showing the surface area analysis results of COF-1 and COF-2 according to Manufacturing Examples 1 and 2.
[0042] Figure 4 is a graph showing the results of pore structure analysis of COF-1 and COF-2 according to Manufacturing Examples 1 and 2.
[0043] Figure 5 is a schematic diagram illustrating a method for manufacturing a solid electrolyte according to one embodiment and an image of the manufactured solid electrolyte. Through this, it was confirmed that a solid electrolyte with excellent flexibility and large-area scalability can be manufactured.
[0044] Figure 6 is an SEM image analyzing a cross-section of a solid electrolyte according to Example 1.
[0045] Figure 7 is a graph showing the charge / decharge behavior over time to evaluate the stability of the lithium metal battery and electrolyte according to Example 6 and Comparative Example 3.
[0046] Figure 8 is a graph analyzing the electrochemical characteristics (charge / discharge voltage profile) of the all-solid-state lithium metal battery of Evaluation Example 4 containing the solid electrolytes of Example 6 and Comparative Example 3. In Figure 8, the descending curve represents the discharge capacity, and the ascending curve represents the charge capacity.
[0047] Figure 9 is a graph showing the results of analyzing the life characteristics (changes in capacity and coulombic efficiency according to the number of charge / discharge cycles) of the all-solid-state lithium metal battery of Evaluation Example 4 including the solid electrolyte of Example 6 and Comparative Example 3.
[0048] Figure 10 is a graph showing the results of analyzing the rate characteristics (change in capacity according to the number of charge / discharge cycles at each current density) of the all-solid-state lithium metal battery of Evaluation Example 4 including the solid electrolyte of Example 6.
[0049] Unless otherwise defined herein, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0050] As used herein, the singular forms may be intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0051] Additionally, the numerical ranges used herein include lower and upper limits and all values within that range, increments logically derived from the shape and width of the defined range, all doubly defined values, and all possible combinations of upper and lower limits of numerical ranges defined in different shapes. Unless otherwise specified herein, values outside the defined numerical range that may arise due to experimental error or rounding of values are also included in the defined numerical range.
[0052] The term "comprises" in this specification is an open-ended description equivalent to expressions such as "includes," "contains," "has," or "characterized by," and does not exclude additional elements, materials, or processes not listed herein.
[0053] In this specification, “substitution” may mean, but is not particularly limited to, that one or more hydrogens in the residue of the compound are substituted with a hydroxy group, a nitro group, a cyano group, an amino group, a carboxyl group, a straight or branched C1 to C6 alkyl group, a C1 to C6 alkylsilyl group, a C3 to C12 cycloalkyl group, a C6 to C12 aryl group, a C2 to C12 heteroaryl group, a C1 to C6 alkoxy group, a halogen group, or a C1 to C6 fluoroalkyl group.
[0054] Hereinafter, a solid electrolyte according to one embodiment of the present invention will be described in more detail.
[0055] One aspect of the present invention provides a solid electrolyte capable of achieving excellent ionic conductivity and electrochemical stability. Specifically, the solid electrolyte comprises a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1; and a crosslinked polymer derived from a polyalkylene oxide-based multifunctional monomer.
[0056] [Chemical Formula 1]
[0057]
[0058] In the above chemical formula 1, A is a monocyclic or polycyclic ring compound, -X- is a divalent linking group, R1 to R4 are each independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not -H at the same time, and M is Li, Li2 or Li3.
[0059] Specifically, in the above chemical formula 1, A may be a monocyclic or polycyclic aromatic or non-aromatic ring compound.
[0060] The monocyclic aromatic ring compound may be, for example, substituted or unsubstituted, benzene, or an aromatic heterocyclic compound. However, the monocyclic aromatic ring compound of the present invention is not limited to the examples described above. As a non-limiting example, the monocyclic aromatic ring compound may be 1,3,5-triazine.
[0061] The polycyclic aromatic ring compound may be a substituted or unsubstituted C3 to C30 polycyclic aromatic ring compound, and for example, may be a bicyclic aromatic ring compound such as substituted or unsubstituted C3 to C30 naphthelene, azulene, etc.; a tricyclic aromatic ring compound such as anthracene, phenanthrene, fluorene, etc.; a four-ring aromatic ring compound such as tetracene, pyrene, etc.; or a combination thereof, and may be a polycyclic aromatic ring compound derived therefrom, and may include one or more heterocycles. However, the polycyclic aromatic ring compound of the present invention is not limited to the examples described above.
[0062] The monocyclic non-aromatic ring compound may be, for example, a substituted or unsubstituted C3 to C12 cycloalkane. However, the monocyclic non-aromatic ring compound of the present invention is not limited to the examples described above.
[0063] The polycyclic non-aromatic ring compound may be, for example, a polycyclic non-aromatic ring compound in which multiple monocyclic non-aromatic ring compounds are joined or unjoined, but is not limited to the above examples.
[0064] In addition, the above A may be a compound in which a monocyclic or polycyclic aromatic ring compound and a monocyclic or polycyclic non-aromatic ring compound are joined or not joined. Preferably, it may be a monocyclic non-aromatic heterocyclic compound having C3 to C50 or C6 to C20. Here, the meaning of hetero refers to a case in which carbon in the ring compound is substituted with one or more heteroatoms selected from B, O, N, C(=O), P, P(=O), S, S(=O)2, and Si atoms.
[0065] According to one embodiment of the present invention, in the chemical formula 1, -X- may be any one selected from the group consisting of a direct bond, -NH-, =CH-NH-, -NH-C(=O)-, -CH=CH-NH-, -OC(=O)-NH-, -CH2-C(=O)O-NH-, -B(-O-)2 and -C(=O)NH-N=CH-, and preferably a direct bond, =CH-NH-, -NH-C(=O)- or -CH=CH-NH-.
[0066] According to one embodiment of the present invention, in the chemical formula 1, R1 to R4 are each independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not -H at the same time, and M is Li, Li2 or Li3. Preferably, R1 to R4 are each independently -H, -SO3M or -PO3M, R1 to R4 are not -H at the same time, and M may be Li, and in the case of a solid electrolyte satisfying this, more improved ionic conductivity and lithium ion yield can be realized.
[0067] According to one embodiment of the present invention, the chemical formula 1 may be represented by the following chemical formula 1-1. The solid compound according to one embodiment may include a covalent organic skeleton structure (hereinafter, COF) containing at least one repeating unit selected from repeating units represented by the following chemical formulas 1-1 to 1-4.
[0068] [Chemical Formula 1-1]
[0069]
[0070] In the above chemical formula 1-1, R1 to R4 are the same as defined in the above chemical formula 1.
[0071] According to another embodiment of the present invention, the chemical formula 1 may be represented by the following chemical formula 1-2.
[0072] [Chemical Formula 1-2]
[0073]
[0074] In the above chemical formula 1-2, R1 to R4 have the same definition as in the above chemical formula 1.
[0075] According to another embodiment of the present invention, the chemical formula 1 may be represented by the following chemical formula 1-2.
[0076] [Chemical Formula 1-3]
[0077]
[0078] In the above chemical formula 1-3, R1 to R4 have the same definition as in the above chemical formula 1.
[0079] According to another embodiment of the present invention, the chemical formula 1 may be represented by the following chemical formula 1-2.
[0080] [Chemical Formula 1-4]
[0081]
[0082] In the above chemical formula 1-4, R1 to R4 have the same definition as in the above chemical formula 1.
[0083] According to one embodiment of the present invention, the covalent organic skeleton structure may be a polygonal structure including a repeating unit of the chemical formula 1 on one side and having a pore formed on the inside. The polygon may include, for example, a regular or irregular triangle, a square, a pentagon, a hexagon, or a combination thereof, and is not particularly limited as long as a pore is formed on the inside. Specifically, the COF may be a hexagonal structure in which the repeating units of the chemical formula 1 are horizontally arranged to form a two-dimensional sheet layer and having a pore formed on the inside, and the pore may function as a lithium ion channel between the COF sheet layers. The solid electrolyte according to one embodiment may have a lower activation energy required for lithium ion dissociation for lithium ions to move between the sheet layers compared to a conventional COF, and thus may realize an effect in which faster ion conductivity and a significantly improved lithium ion yield are achieved.
[0084] According to one embodiment of the present invention, the pores of the covalent organic skeleton structure may have an average diameter (pore size) of 0.1 to 20.0 nm, specifically 1.0 to 8.0 nm, specifically 1.0 to 2.0 nm, but is not limited thereto.
[0085] According to one embodiment of the present invention, the surface area of the covalent organic skeleton structure is 10 to 800 mg 2 / g, specifically 50 to 500 mg 2 / g may be, but is not limited to.
[0086] According to one embodiment of the present invention, the covalent organic skeleton structure may include a repeating unit represented by the following chemical formula 2.
[0087] [Chemical Formula 2]
[0088]
[0089] In the above chemical formula 2, R1 to R4 are each independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not -H at the same time, M is Li, Li2 or Li3, and a specific description is omitted because it is the same as the above chemical formula 1.
[0090] According to one embodiment of the present invention, the covalently bonded organic skeleton structure may be in a powder form, and the average particle diameter may be, but is not limited to, 0.001 to 10 μm, or 0.01 to 5 μm.
[0091] According to one embodiment of the present invention, the polyalkylene oxide-based multifunctional monomer may be a C1 to C7 polyalkylene oxide-based multifunctional monomer, and may specifically be, but is not limited to, a polyethylene oxide-based, a polypropylene oxide-based, or a polyethylene propylene oxide-based monomer.
[0092] According to one embodiment of the present invention, the polyalkylene oxide-based multifunctional monomer may have a number average molecular weight of 20,000 g / mol or less, or 100 to 10,000 g / mol, or 300 to 1,000 g / mol.
[0093] According to one embodiment of the present invention, the polyalkylene oxide-based multifunctional monomer may include two or more reactive functional groups selected from the group consisting of an acrylic group, a methacryl group, a vinyl group, a thiol group, an epoxy group, an isocyanate group, a silanol group, a halogen group, a carboxyl group, a hydroxyl group, and an amine group, and specifically may include the above-described reactive functional groups at both ends. Preferably, the polyalkylene oxide-based multifunctional monomer may include an acrylic group and / or a methacryl group. In addition, when a polyalkylene oxide-based multifunctional monomer is used rather than using other types of functional monomers or multifunctional monomers, lithium ion channels are effectively formed between the layers of the covalent organic skeleton structure, thereby inducing faster movement of lithium ions, thereby realizing very excellent ion conductivity and energy density.
[0094] Examples of polyalkylene oxide-based multifunctional monomers containing an acrylic group include diethylene glycol diacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, dipropylene glycol diacrylate, dipropylene glycol dimethacrylate, ethylene glycol divinyl ether, ethoxylated trimethylolpropane triacrylate, diethylene glycol divinyl ether, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate (PGEDA), and polyethylene glycol dimethacrylate, and specifically, polyethylene glycol diacrylate (PGEDA), polyethylene glycol dimethacrylate, or a mixture thereof may be used, but the present invention is not limited thereto.
[0095] According to one embodiment of the present invention, the crosslinking polymer may be included in an amount of 1 to 100 parts by weight, specifically 5 to 50 parts by weight, or 5 to 40 parts by weight, specifically 10 to 25 parts by weight, based on 100 parts by weight of the covalent organic skeleton structure. When the above weight ratio is satisfied, a solid electrolyte having improved ion conductivity and lithium ion yield can be manufactured.
[0096] According to one embodiment of the present invention, the covalent organic framework structure to the crosslinking polymer may satisfy a volume ratio of 100:1 to 200, specifically 100:30 to 150, or 100:40 to 110, specifically 100:70 to 80. The crosslinking polymer may be formed by polymerization after a polyalkylene oxide-based multifunctional monomer is filled into the pores of the covalent organic framework structure during the manufacturing process. Accordingly, the solid electrolyte may have a structure including a member having the covalent organic framework structure as a base material and in which a three-dimensional crosslinking polymer is continuously filled into the pores of the structure. In addition, the volume of the covalent organic framework structure here may mean a pore volume of the covalent organic framework structure. Additionally, the pore volume per unit weight of the covalent organic skeleton structure according to one embodiment may be, but is not limited to, 0.01 to 0.8 cm3 / g, or 0.1 to 0.5 cm3 / g.
[0097] According to one embodiment of the present invention, the solid electrolyte can be formed into a film form through a certain process, and has the advantage of being manufactured as a free-standing film with excellent flexibility and the ability to be manufactured on a large area. In this case, the thickness of the solid electrolyte may be 0.1 to 100 μm or 1 to 50 μm, but can be easily adjusted depending on the field to which it is to be applied.
[0098] According to one embodiment of the present invention, the solid electrolyte includes the covalent organic framework structure and the crosslinking polymer, and thus has superior flexibility compared to a solid electrolyte manufactured solely with the covalent organic framework structure, and has the advantage of being able to manufacture a large-area thin film.
[0099] According to one embodiment of the present invention, the ionic conductivity of the solid electrolyte, specifically the lithium ion conductivity, is 3.0 x10 -5 S / cm or more, 6.0 x10 -5 S / cm or more, 8.0 x10 -5 S / cm or more, or 6.0 x10 -5 1.0 x10 -3 It can exhibit excellent ionic conductivity of S / cm.
[0100] According to one embodiment of the present invention, the activation energy required for dissociation of lithium ions in the solid electrolyte may be 0.2 eV or less, 0.01 to 0.17 eV, or 0.01 to 0.15 eV.
[0101] According to one embodiment of the present invention, the lithium ion yield of the solid electrolyte may be 0.85 or more, or 0.9 or more, or 0.93 or more.
[0102]
[0103] Hereinafter, one aspect of the present invention can provide a method for producing a slurry composition for producing the above solid electrolyte.
[0104] The present invention can provide a slurry composition for producing a solid electrolyte comprising a covalently bonded organic skeletal structure containing a repeating unit represented by the following chemical formula 1 and a polyalkylene oxide-based multifunctional monomer.
[0105] [Chemical Formula 1]
[0106]
[0107] In the above chemical formula 1, A is a monocyclic or polycyclic ring compound, -X- is a divalent linking group, R1 to R4 are each independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not -H at the same time, and M is Li, Li2 or Li3.
[0108] According to one embodiment of the present invention, in the slurry composition for preparing the solid electrolyte, the polyalkylene oxide-based multifunctional monomer may be included in a weight ratio of 1 to 100, specifically 5 to 50, or 5 to 40, specifically 10 to 25, based on 100 parts by weight of the covalent organic skeleton structure. In addition, the covalent organic skeleton structure to the polyalkylene oxide-based multifunctional monomer may satisfy a volume ratio of 100:1 to 200, specifically 100:30 to 150, or 100:40 to 110, specifically 100:70 to 80. Here, the volume of the covalent organic framework structure may refer to the pore volume of the covalent organic framework structure, and the pore volume of the covalent organic framework structure may be obtained by multiplying the pore volume per unit mass of the covalent organic framework structure and the weight of the covalent organic framework structure introduced.
[0109] The slurry composition for producing the above solid electrolyte may further include an initiator as needed, and may further include a photoinitiator or a thermal initiator depending on the curing method. The initiator may be any known initiator without limitation, and examples of the photoinitiator may be selected from, but are not limited to, acetophenone compounds, benzophenone compounds, triazine compounds, benzoin compounds, imidazole compounds, xanthone compounds, phosphine compounds, and oxime compounds. Examples of the thermal initiator may be selected from, but are not limited to, benzoyl peroxide (BPO), dicumyl peroxide (DCP), azobisisobutyronitrile (AIBN), and the like.
[0110] Specific descriptions of the above chemical formula 1, polyalkylene oxide-based multifunctional monomer, and solid electrolyte are the same as those described above, so they are omitted.
[0111]
[0112] Hereinafter, one aspect of the present invention can provide a method for manufacturing the above-described solid electrolyte.
[0113] The present invention can provide a method for producing a solid electrolyte, comprising the steps of (S1) applying pressure to a slurry composition for producing a solid electrolyte, which comprises a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1 and a polyalkylene oxide-based multifunctional monomer, and (S2) polymerizing the solid electrolyte slurry composition to produce a crosslinked polymer. Specific descriptions of the chemical formula 1, the polyalkylene oxide-based multifunctional monomer, and the solid electrolyte are the same as those described above, and therefore are omitted.
[0114] According to one embodiment of the present invention, in the step (S1), a step of leaving the slurry composition for preparing the solid electrolyte under low pressure conditions for a certain period of time (low pressure-driven method) may be further performed. Preferably, as shown in ② of FIG. 5, a vacuum may be applied for 5 minutes or more, or 30 minutes or more, so that the liquid monomer can effectively penetrate into the pores of the covalently bonded organic skeleton structure.
[0115] According to one embodiment of the present invention, in the step (S1), a pressure of 1 to 400 MPa, 5 to 250 MPa, or 100 to 250 MPa may be applied, and a method of applying the pressure may use a commonly used method.
[0116] According to one embodiment of the present invention, in the step (S2), the solid electrolyte slurry composition is a curable composition, and a solid electrolyte can be manufactured through a curing (polymerization) reaction. The curing reaction may be performed by photocuring, thermal curing, or a combination thereof, and may be performed by appropriate modifications depending on the purpose. Preferably, the polymerization may be a photocuring reaction, and may be performed by irradiating a light source in the ultraviolet wavelength range to activate the above-described reactive functional group and thereby perform crosslinking polymerization.
[0117] In addition, the slurry composition for manufacturing the solid electrolyte may further include an initiator or an organic solvent as needed, but is not limited thereto.
[0118]
[0119] Hereinafter, an all-solid-state battery according to one embodiment will be described. However, except for including the solid electrolyte according to one embodiment, the all-solid-state battery can be manufactured in a structure known in the art using a manufacturing method and materials common in the art.
[0120] The present invention can provide an all-solid-state battery comprising the above-described solid electrolyte. The all-solid-state battery comprises a positive electrode layer and a negative electrode layer, and a solid electrolyte layer between the positive electrode layer and the negative electrode layer, wherein the solid electrolyte layer may comprise a solid electrolyte according to one embodiment.
[0121] According to one embodiment of the present invention, the positive electrode layer may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector.
[0122] According to another embodiment of the present invention, the positive electrode active material layer may be impregnated with a solid electrolyte according to one aspect within the pores, and the positive electrode layer and the solid electrolyte layer may be integrated with each other.
[0123] For example, the thickness of the solid electrolyte layer may be 0.1 to 100 ㎛, 1 to 100 ㎛, or 5 to 50 ㎛, wherein the thickness of the solid electrolyte layer means the thickness of a section where the positive electrode active material layer and the solid electrolyte are not mixed and only the solid electrolyte according to one embodiment exists.
[0124] An all-solid-state battery according to one embodiment may be manufactured by including the steps of (A) applying a cathode material slurry composition to one surface of a cathode current collector, drying, and rolling to manufacture a cathode active material layer having pores; (B) impregnating the cathode active material layer with a slurry composition for manufacturing a solid electrolyte according to one embodiment and polymerizing the slurry composition for manufacturing a solid electrolyte according to one embodiment to manufacture a cathode layer impregnated with a solid electrolyte and a solid electrolyte layer integrated with the cathode layer; and (C) laminating the cathode layer impregnated with the solid electrolyte and the cathode layer.
[0125] Non-limiting examples of the positive electrode current collector may include a foil made of aluminum, nickel, or a combination thereof, and the positive electrode material slurry composition may include a solvent, a binder, a conductive agent, a dispersant, etc., in addition to the positive electrode active material, as needed. The thickness of the positive electrode current collector is not particularly limited, but may be 3 to 500 μm.
[0126] The above cathode active material can be any cathode active material used in this technical field without limitation, as long as it is a material capable of reversible insertion and dissociation of lithium ions, and non-limiting examples thereof include lithium cobalt oxide composite oxide (LiCoO2), spinel crystalline lithium manganate composite oxide (LiMn2O4), lithium manganate composite oxide (LiMnO2), lithium nickelate composite oxide (LiNiO2), lithium iron phosphate (LiFePO4), lithium manganese phosphate (LiMnPO4), lithium cobalt phosphate (LiCoPO4), lithium iron pyrophosphate (Li2FeP2O7), lithium niobate composite oxide (LiNbO2), lithium iron oxide composite oxide (LiFeO2), lithium magnesium oxide composite oxide (LiMgO2), lithium cuprate composite oxide (LiCuO2), lithium zincate composite oxide (LiZnO2), and molybdic acid. Lithium composite oxide (LiMoO2), lithium tantalate composite oxide (LiTaO2), lithium tungstate composite oxide (LiWO2), lithium permanganate nickel cobalt composite oxide (xLi2MnO3(1-x)LiMn1-y-zNiyCozO2), lithium nickel cobalt aluminum composite oxide (LiNi 0.8 Co 0.15 Al 0.05 O2), lithium nickel cobalt manganese composite oxide (LiNi 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.4 Co 0.2 Mn 0.4 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.7 Co 0.15 Mn 0.15 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2), manganese nickel oxide (LiNi 0.5 Mn1.5 O4) but are not limited to these.
[0127] The conductive material may include, but is not limited to, carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, etc.; conductive fibers such as carbon fibers and metal fibers; metal powders such as fluorinated carbon, aluminum, and nickel powders; conductive whiskeys such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives, but is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery.
[0128] The above binder polymer may include one or more selected from the group consisting of nitrile butadiene rubber, polyethylene glycol, polyacrylonitrile, polyvinyl chloride, polymethyl methacrylate, polypropylene oxide, polydimethylsiloxane, polyvinylidene fluoride, polyvinylidene carbonate, and polyvinylpyrrolidinone, and preferably one or more selected from the group consisting of polyvinylidene fluoride, polyvinylidene carbonate, and polyethylene glycol, but is not limited thereto.
[0129] The above negative electrode layer may include a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector.
[0130] Non-limiting examples of the negative electrode current collector may be selected from a foil made of copper, gold, nickel, or a copper alloy or a combination thereof. The negative electrode active material layer may be any one or two or more selected from the group consisting of any one carbon selected from soft carbon, hard carbon, artificial graphite, natural graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, carbon nanotubes, acetylene black, Ketjen black, graphene, fullerene, activated carbon, and meso carbon microbeads; any one metal selected from silicon, tin, lithium, aluminum, silver, bismuth, indium, germanium, lead, platinum, titanium, zinc, manganese, cadmium, cerium, copper, cobalt, nickel, and iron; an alloy comprising two or more of the above metals; and an oxide of one or more of the above metals; and preferably, lithium metal, but is not limited thereto.
[0131] In particular, the solid electrolyte according to one embodiment has excellent interfacial stability with a lithium metal negative electrode and effectively suppresses dendrite growth, thereby overcoming the limitations of conventional solid electrolytes and realizing excellent lifespan characteristics and rate characteristics. Furthermore, the solid electrolyte has a lithium ion channel formed by a combination of a covalent organic skeleton structure and a cross-linking polymer, and thus has the advantage of being capable of operating with excellent performance without the addition of additional lithium salts and solvents.
[0132] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. However, these are provided to enable those skilled in the art to easily implement the present invention. The present invention may be implemented in various different forms, and the spirit of the present invention is not necessarily limited to the embodiments.
[0133] [Manufacturing Example 1] Manufacturing of a covalent organic framework (COF-1, TpPa-SO3Li)
[0134]
[0135] 2,4,6-Triformylphloroglucinol (63 mg, 0.3 mmol) and 2,5-diaminobenzenesulfonic acid (84.7 mg, 0.45 mmol), 1,4-dioxane (1.2 mL, 14.1 mmol), 1,3,5-trimethylbenzene (0.8 mL, 5.75 mol), acetic acid (0.216 mL, 3.6 mmol), and deionized water (0.38 g, 0.021 mmol) were placed in a Pyrex tube, and the mixture was rapidly frozen in liquid nitrogen and degassed by three freeze-pump-thaw cycles. After that, the tube was sealed and reacted at 120°C for 3 days, the precipitate was collected by filtration, washed with dimethylacetamide and acetone, extracted through Soxhlet with tetrahydrofuran for 12 hours, and dried in vacuo at 120°C overnight to obtain TpPa-SO3H (yield: 119.7 mg, 91%).
[0136] The synthesized TpPa-SO3H (200 mg) was added to a lithium acetate solution (5 M, 20 mL) and stirred at room temperature for 3 days. The resulting powder was filtered and washed three times, and dried overnight in a vacuum at 120°C to finally obtain TpPa-SO3Li powder (hereinafter, COF-1) according to Manufacturing Example 1 (yield: 173.5 mg, 85%).
[0137] [Manufacturing Example 2] Manufacturing of covalent organic skeleton structure (COF-2, TpPa-(SO3Li)2)
[0138]
[0139] In the above Manufacturing Example 1, the same procedure as Manufacturing Example 1 was performed except that 120.6 mg (0.45 mmol) of 2,5-diaminobenzene-1,4-disulfonic acid was added instead of 2,5-diaminobenzenesulfonic acid, and 40 mL of lithium acetate solution (5 M) was added. Finally, TpPa-(SO3Li)2 powder (hereinafter, COF-2) according to Manufacturing Example 2 was obtained (yield: 169.2 mg, 82%).
[0140] Fourier transform infrared spectroscopy (ATR-FT-IR, Nicolet iS10 FTIR Spectrometer), X-ray diffraction analysis (XRD, X-ray diffraction, using a Kratos Amicus spectrometer equipped with a Ka X-ray source) and surface area / pore structure analysis (Micromeritics) of the covalent organic skeleton structures according to the above manufacturing examples 1 and 2 ASAP 242) was performed, and the results are shown in Figures 1, 2, and 3. Specifically, the surface area of COF-1 was 343 mg 2 / g, COF-2 is 95 mg 2 / g, and the pore size was measured to be 1.2 nm for both COF-1 and COF-2.
[0141] [Manufacturing Example 3] Manufacturing of a covalent organic skeleton structure (COF-3, TpPa-COOLi)
[0142] TpPa-COOH and TpPa-COOLi powders (hereinafter referred to as COF-3) were obtained in the same manner as in Manufacturing Example 1 above, except that 2,5-diaminobenzoic acid having the following structure was used instead of 2,5-diaminobenzenesulfonic acid (yields of 90% and 86%, respectively).
[0143]
[0144] [Manufacturing Example 4] Manufacturing of covalent organic skeleton structure (COF-4, TpPa-(COOLi)2)
[0145] TpPa-(COOLi)2 powder (hereinafter, COF-4) was obtained in the same manner as in Manufacturing Example 2 above, except that 2,5-diamino-1,4-dibenzoic acid (2,5-diamino-1,4-benzenedicarboxylic acid) having the following structure was used instead of 2,5-diaminobenzene-1,4-disulfonic acid (yield: 83%).
[0146]
[0147] [Example 1]
[0148] COF-1 of the above Preparation Example 1, which is a covalent organic framework (COF), and PEGDA (Poly(ethylene glycol) diacrylate, Mn: 545 g / mol), which is a polyalkylene oxide-based multifunctional monomer, were added at a weight ratio of 100:15, and vacuum was applied for 2 hours, thereby producing a slurry composition for producing a solid electrolyte according to Example 1. At this time, a photoinitiator was added in an amount of 1 part by weight per 100 parts by weight of the PEGDA.
[0149] To evaluate the physical properties, the slurry composition for preparing the above solid electrolyte was formed into a film by applying a pressure of 222 MPa (3 tons) at 120°C for 1 hour using a hydraulic press (Hefei Kejing Materials Technology Co., Ltd.). The film was irradiated with a 365 nm UV lamp for 1 minute to ultimately produce a solid electrolyte in the form of a thin film of approximately 30 μm.
[0150] [Example 2]
[0151] In the above Example 1, a solid electrolyte in the form of a thin film was obtained by performing the same procedure as in Example 1, except that a slurry composition for preparing a solid electrolyte containing COF-1 and PEGDA in a weight ratio of 100:24 was used.
[0152] [Example 3]
[0153] In the above Example 1, a solid electrolyte in the form of a thin film was obtained by performing the same procedure as in Example 1, except that a slurry composition for preparing a solid electrolyte containing COF-1 and PEGDA in a weight ratio of 100:32 was used.
[0154] [Example 4]
[0155] In the above Example 1, a solid electrolyte in the form of a thin film was obtained by performing the same procedure as in Example 1, except that a slurry composition for preparing a solid electrolyte containing COF-1 and PEGDA in a weight ratio of 100:40 was used.
[0156] [Example 5]
[0157] In the above Example 1, a solid electrolyte in the form of a thin film was obtained by performing the same procedure as Example 1, except that COF-2 of Preparation Example 2, instead of COF-1, was used.
[0158] [Example 6]
[0159] In the above Example 5, a solid electrolyte in the form of a thin film was obtained by performing the same procedure as in Example 5, except that a slurry composition for preparing a solid electrolyte containing COF-2 and PEGDA in a weight ratio of 100:11 was used.
[0160] [Example 7]
[0161] In the above Example 5, a solid electrolyte in the form of a thin film was obtained by performing the same procedure as Example 5, except that a slurry composition for preparing a solid electrolyte containing COF-2 and PEGDA in a weight ratio of 100:16 was used.
[0162] [Example 8]
[0163] In the above Example 5, a solid electrolyte in the form of a thin film was obtained by performing the same procedure as Example 5, except that a slurry composition for preparing a solid electrolyte containing COF-2 and PEGDA in a weight ratio of 100:21 was used.
[0164] [Example 9]
[0165] A thin film solid electrolyte was obtained in the same manner as Example 1, except that COF-3 (TpPa-COOLi) of Manufacturing Example 3 was used instead of COF-1 (TpPa-COOLi) of Manufacturing Example 1.
[0166] [Example 10]
[0167] A thin film solid electrolyte was obtained in the same manner as in Example 1, except that 11-azido-3,6,9-trioxaundecan-1-amine was used instead of PEGDA.
[0168]
[0169] 11-azido-3,6,9-trioxaundecan-1-amine [Example 11]
[0170] A thin film solid electrolyte was obtained in the same manner as in Example 1, except that acrylonitrile having the following structure was used instead of PEGDA.
[0171]
[0172] [Example 12]
[0173] A thin film solid electrolyte was obtained in the same manner as in Example 1, except that methacrylamide having the following structure was used instead of PEGDA.
[0174]
[0175] [Comparative Example 1]
[0176] Only the covalently bonded organic skeleton structure COF-1 of the above Preparation Example 1 was used to produce a solid electrolyte in the form of a thin film of about 250 μm by applying a pressure of 222 MPa (3 tons) at 120°C for 0.5 hours using a hydraulic press (Hefei Kejing Materials Technology Co., Ltd.). However, an attempt was made to produce a thin film of 30 μm as in the example, but the powder COF-1 alone was not flexible and easily broke during the moving stage, making it difficult to produce a free-standing film. Therefore, a thin film of COF-1 alone was formed on a substrate using a stainless steel foil as a substrate or a pellet-type cell.
[0177] [Comparative Example 2]
[0178] The same procedure as in Comparative Example 1 was followed, except that COF-2 of Manufacturing Example 2, instead of COF-1, was used in Comparative Example 1.
[0179] Additionally, in the solid electrolytes manufactured according to Examples 1 to 8 and Comparative Examples 1 and 2, the weight part of PEGDA per 100 weight parts of COF is shown in Table 1 below.
[0180] [Evaluation Example 1] Ionic conductivity (σ Li )
[0181] The solid electrolytes manufactured in the above examples and comparative examples were laminated between two identical stainless steel foils to manufacture an ionic conductivity measurement cell, and the ionic conductivity of the solid electrolyte was measured. Based on EIS (Electrochemical Impedance Spectroscopy) analysis, the impedance was measured at room temperature by applying a frequency range of 0.1 mHz to 5 MHz and an AC amplitude of 10 mV, and the ionic conductivity was calculated according to Equation 1 below. The results are shown in Table 1 below.
[0182] [Formula 1]
[0183]
[0184] (In the above equation 1, l is the thickness of the all-solid-state battery, R is the resistance measured through EIS analysis, and S is the operating area of the electrode.)
[0185] [Evaluation Example 2] Lithium ion mobility
[0186] In order to evaluate the lithium ion mobility of the solid electrolytes manufactured in the above examples and comparative examples, the activation energy (E) for dissociating and moving Li ions in each solid electrolyte was a ) were measured and shown in Table 1 below.
[0187] In addition, a lithium ion yield measurement cell was manufactured by overlapping the solid electrolytes manufactured in the above examples and comparative examples between two identical lithium metal foils, and a direct current voltage of 10 mV was applied at room temperature for 4 hours, and the impedance value before and after the direct current voltage was applied was measured to obtain the lithium ion yield (Li-ion transform number, t Li+ )) was calculated according to the following equation 2. The results are shown in Table 1 below.
[0188] [Formula 2]
[0189]
[0190] (In the above equation 2, ΔV is the polarization voltage, I ss and R ss represents the normal current and resistance values after polarization, and I0 and R0 are the initial current and resistance values)
[0191] PEGDA (weight part) Ionic conductivity (RT) [S / cm] Activation energy [eV] Lithium ion yield (t) Li+ ) Example 1153.8 x10 -5 0.160.92 Example 2244.7 x10 -5 0.150.93 Example 3322.1 x10 -5 0.190.91 Example 4401.6 x10 -5 0.190.91 Example 5117.3 x10 -5 0.130.93 Example 6168.5 x10 -50.110.95 Example 7215.3 x10 -5 0.150.92 Example 826.64.7 x10 -5 0.170.91 Example 9151.8 x10 -5 0.170.93 Example 10152.7 x10 -5 0.160.91 Example 11153.1 x10 -5 0.150.90 Example 12152.6 x10 -5 0.160.92Comparison Example 102.5 x10 -5 0.180.90Comparison example 204.5 x10 -5 0.160.92
[0192] As shown in Table 1 above, it was confirmed that the solid electrolytes of the examples had significantly improved ionic conductivity and lithium ion yield compared to the solid electrolytes of the comparative examples.
[0193] In addition, the solid electrolyte according to one embodiment is π-π * By forming ion channels through interaction, the activation energy for dissociating Li ions is significantly reduced, thereby inducing rapid movement of lithium ions within the anode, and thus, a battery including the same can achieve excellent energy density.
[0194] In addition, the electrical conductivity (Ionic conductance, 1 / resistance) of Example 6 and Comparative Example 1 was measured, and Example 6 showed 38.8 mS and Comparative Example 1 showed 1.3 mS, confirming that the solid electrolyte according to one embodiment can be manufactured into a thin film and shows excellent ionic conductivity.
[0195] - Manufacturing of all-solid-state lithium metal batteries
[0196] A cathode material slurry composition was prepared by adding N-methylpyrrolidone to a cathode material content of 40 wt% in a weight ratio of cathode active material (Me2BBQ) / conductive material (carbon black; Super P) / binder (polyvinylidene fluoride, PVDF) 3 / 6 / 1. The cathode material slurry composition was applied to an aluminum (Al) thin film having a thickness of 18 μm using a doctor blade, and after hot air drying at 80°C and vacuum drying at 120°C for 24 hours, a cathode active material layer having a thickness of 20 μm was formed, thereby preparing a cathode layer.
[0197] Thereafter, the slurry composition for preparing a solid electrolyte of Example 6 was impregnated into the cathode active material layer, and a pressure of 222 MPa (3 tons) was applied at 120°C for 0.5 hours using a hydraulic press (Hefei Kejing Materials Technology Co., Ltd.) to form a film. The film was irradiated with a 365 nm UV lamp for 1 minute, thereby preparing a cathode layer impregnated with a solid electrolyte and a 30 μm thick solid electrolyte layer integrated with the cathode layer.
[0198] Afterwards, a 50 ㎛ thick lithium metal was rolled onto a 9 ㎛ thick copper foil current collector to form an all-solid-state lithium metal battery according to Example 6.
[0199] [Comparative Example 3] Manufacturing of a Liquid Electrolyte Lithium Metal Battery
[0200] In the above method for manufacturing an all-solid-state lithium metal battery, a solid electrolyte layer was not manufactured, and a polyethylene porous polymer separator was interposed between the positive electrode layer and the negative electrode layer, and then an electrolyte solution in which 1 M LiTFSI was dissolved in a solvent in which dimethyl ether (DME) and 1,3-dioxolane (DOL) were mixed in a volume ratio of 1:1 was injected to manufacture a lithium metal battery.
[0201]
[0202] [Evaluation Example 3] Battery Stability Evaluation
[0203] In order to evaluate the stability of the solid electrolyte for the lithium metal negative electrode, the lithium metal charge / discharge behavior was confirmed for the lithium metal batteries according to Example 6 and Comparative Example 3. Specifically, the lithium metal battery was charged / discharged at a current density of 0.05 mA / cm2 for 5 hours to a capacity per area of 0.25 mAh / cm2, and the voltage change was observed while performing a total of 50 charge / discharge cycles for 500 hours, and the results are shown in Fig. 7. Referring to Fig. 7, it was confirmed that Example 6 formed a significantly lower overvoltage than Comparative Example 3, and through this, it was confirmed that when the solid electrolyte according to one embodiment is used, the formation of lithium metal and dendrites can be effectively controlled, thereby manufacturing a battery having excellent stability with the lithium metal negative electrode.
[0204] [Evaluation Example 4] Life Characteristics Evaluation
[0205] The room temperature life characteristics and rate characteristics of the lithium metal batteries manufactured in Example 6 and Comparative Example 3 above were analyzed. The charge / discharge conditions were a 1000-cycle life test conducted at a current density of 50 mA / g at room temperature (25°C) and a voltage range of 1.8 to 3.4 V, and the results are shown in Figs. 8 and 9. In addition, in order to measure the rate characteristics, several cycle tests were conducted by changing the current density to 20, 50, 100, 200, and 500 mA / g in a voltage range of 1.8 to 3.4 V, and the results are shown in Fig. 10.
[0206] Referring to FIGS. 8 to 10, it can be seen that the all-solid-state lithium metal battery using the solid electrolyte of Example 6 exhibits superior performance compared to the battery using the liquid electrolyte, and specifically, it exhibits an excellent capacity retention rate of more than 80% even after 1000 cycles. In the case of Comparative Example 3, the organic electrode of more than 50 wt% is dissolved in 100 cycles due to the liquid electrolyte, and it can no longer function as an active material, resulting in very poor life characteristics. In contrast, in the case of Example 6, the electrode is not dissolved even after 200 cycles, and accordingly, it can be seen that the solid electrolyte has high ionic conductivity that can be operated at room temperature, low activation energy required for the movement of lithium ions, enabling rapid ion movement, and excellent interfacial stability with high-capacity positive electrode materials such as Me2BBQ or lithium metal negative electrodes, so that the life characteristics and rate characteristics will be excellent.
[0207] In addition, when using the solid electrolyte according to one embodiment, various functional groups can be attached to it to achieve the desired properties, so that it can be widely used in various battery systems. In addition, because the solid electrolyte according to one embodiment has a low density, it can exhibit a significantly high capacity per weight, and can easily realize an improvement in energy density, and thus can be utilized in a wide range of fields such as industrial fields requiring high energy density, such as electric vehicles, drones, and airplanes.
[0208] As described above, the present invention has been described by limited embodiments, but these are provided only to help a more general understanding of the present invention, and the present invention is not limited to the above embodiments, and those skilled in the art to which the present invention pertains can make various modifications and variations based on this description.
[0209] Therefore, the idea of the present invention should not be limited to the described embodiments, and all things that are equivalent or equivalent to the claims described below as well as the claims are considered to fall within the scope of the idea of the present invention.
Claims
1. A solid electrolyte comprising a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1; and a crosslinked polymer derived from a crosslinkable monomer. [Chemical Formula 1] In the above chemical formula 1, A is a monocyclic or polycyclic cyclic compound, -X- is a divalent linker, R1 to R4 are independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not simultaneously -H, and M is Li, Li2 or Li3.
2. In paragraph 1, A solid electrolyte in which -X- in the above chemical formula 1 is any one selected from the group consisting of a direct bond, -NH-, =CH-NH-, -NH-C(=O)-, -CH=CH-NH-, -OC(=O)-NH-, -CH2-C(=O)O-NH-, -B(-O-)2, and -C(=O)NH-N=CH-.
3. In paragraph 1, The above chemical formula 1 is a solid electrolyte represented by the following chemical formula 1-1. [Chemical Formula 1-1] In the above chemical formula 1-1, R1 to R4 are the same as defined in the above chemical formula 1.
4. In paragraph 1, The above covalent bond organic skeleton structure is a solid electrolyte having a polygonal structure including a repeating unit of the above chemical formula 1 on one side and a pore formed on the inside.
5. In paragraph 4, A solid electrolyte having a pore diameter of 1.0 to 8.0 nm in the above covalent organic skeleton structure.
6. In paragraph 1, The above covalent organic skeleton structure is a solid electrolyte comprising a repeating unit represented by the following chemical formula 2. [Chemical Formula 2] In the above chemical formula 2, R1 to R4 are independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not simultaneously -H, and M is Li, Li2 or Li3.
7. In paragraph 1, The above crosslinkable monomer is selected from polyalkylene oxide-based multifunctional monomers, 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, methacrylamide, and combinations of two or more thereof. A solid electrolyte wherein the polyalkylene oxide-based multifunctional monomer contains two or more reactive functional groups selected from the group consisting of an acrylic group, a methacrylic group, a vinyl group, a thiol group, an epoxy group, an isocyanate group, a silanol group, a halogen group, a carboxyl group, a hydroxyl group, and an amine group.
8. In paragraph 7, The above polyalkylene oxide-based multifunctional monomer is a solid electrolyte having a number average molecular weight of 100 to 10,000 g / mol.
9. In paragraph 1, A solid electrolyte in which the crosslinking polymer is included in an amount of 1 to 100 parts by weight based on 100 parts by weight of the covalent organic skeleton structure.
10. In paragraph 1, A solid electrolyte having a thickness of 0.1 to 100 μm.
11. In paragraph 1, The lithium ion conductivity of the above solid electrolyte is 6.0 x10 -5 Solid electrolyte with a density of S / cm or more.
12. An all-solid-state battery comprising any one solid electrolyte selected from claims 1 to 10. 13.(S1) A step of applying pressure to a slurry composition for preparing a solid electrolyte, comprising (i) a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1 and (ii) a crosslinkable monomer selected from among a polyalkylene oxide-based multifunctional monomer, a polyalkylene oxide-based multifunctional monomer, 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, methacrylamide, and a combination of two or more thereof; and (S2) A method for producing a solid electrolyte, comprising a step of polymerizing the above solid electrolyte slurry composition to produce a crosslinked polymer.
14. In paragraph 13, A method for manufacturing a solid electrolyte, wherein in the above step (S1), a pressure of 5 to 250 MPa is applied.
15. A slurry composition for producing a solid electrolyte, comprising a covalently bonded organic skeleton structure containing a repeating unit represented by the following chemical formula 1 and a crosslinkable monomer selected from among polyalkylene oxide-based multifunctional monomers, 11-azido-3,6,9-trioxaundecan-1-amine, acrylonitrile, methacrylamide, and combinations of two or more thereof. [Chemical Formula 1] In the above chemical formula 1, A is a monocyclic or polycyclic cyclic compound, -X- is a divalent linker, R1 to R4 are independently -H, -COOM, -SM, -SO2M, -SO3M, -PO3M or -PO4M, R1 to R4 are not simultaneously -H, and M is Li, Li2 or Li3.
Citation Information
Patent Citations
Lithiation covalent organic framework composite polymer electrolyte as well as preparation and application thereof
CN112786960A
Novel COF modified gel electrolyte of lithium battery and preparation method of novel COF modified gel electrolyte
CN115882058A
Solid polymer electrolyte and Li ion battery comprising the same
KR1020170060225A
Solid electrolytes for rechargeable power sources that include single-ion conducting covalent organic frameworks with immobilized anion groups
KR102172038B1
Cited By
Organic covalent material and preparation method thereof, composite adsorption film and preparation method and application thereof
CN119751784A
Organic covalent materials and their preparation methods, composite adsorption membranes and their preparation methods and applications
CN119751784B
Preparation method for in-situ polymerization of sodium polyacrylate hydrogel containing covalent organic framework material
CN119978434A