Hydrophobic silica wet gel and aerogel

WO2024220696A3PCT designated stage expired Publication Date: 2024-11-28CARDINAL CG CO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/025233
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-16
Filing Date
2024-04-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Silica aerogels have limited applications in windows due to the inability to achieve a combination of mechanical, thermal, and optical properties, with hydrophobic silica aerogels facing issues of lower visible transmission and higher haze when made hydrophobic, and existing methods are costly and detrimental to optical properties.

Method used

A method of synthesizing hydrophobic silica aerogel using alkoxy silanes, such as methyl silicate and tetramethoxy silane, with a controlled molar ratio and aging process, avoiding the use of surfactants and excessive solvents to achieve high visible transmission and low haze, while maintaining mechanical and thermal properties.

Benefits of technology

The method produces hydrophobic silica aerogel with visible transmission of at least 97.8% and haze value of 3% or less, offering improved optical, mechanical, and thermal properties suitable for window applications without excessive processing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024025233_28112024_PF_FP_ABST
    Figure US2024025233_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The invention provides hydrophobic silica wet gel, hydrophobic silica aerogel, and methods that can be used to form an enhanced hydrophobic silica aerogel sheet having an advantageous combination of properties. Some embodiments of the invention provide a hydrophobic silica aerogel having advantageous properties, such as desirable performance on visible transmission, haze, or both.
Need to check novelty before this filing date? Find Prior Art

Description

HYDROPHOBIC SILICA WET GEL AND AEROGELRELATED APPLICATIONS

[0001] This application claims priority to U.S. patent application No. 18 / 636,553, filed April 16, 2024 (which in turn claims priority to U.S. provisional patent application No. 63 / 497,250, filed April 20, 2023) and to U.S. patent application No. 18 / 636,591, filed April 16, 2024 (which in turn claims priority to U.S. provisional patent application No. 63 / 497,251, filed April 20, 2023), the entire contents of each of which are incorporated herein by reference.FIELD OF THE INVENTION

[0002] The present invention relates to hydrophobic silica wet gel and methods of making hydrophobic silica wet gel. The invention also relates to hydrophobic transparent silica aerogel and methods of making hydrophobic transparent silica aerogel. Additionally, the invention relates to hydrophobic transparent silica aerogel sheets and methods of making hydrophobic transparent silica aerogel sheets. Further, the invention relates to an article having a glass sheet and a hydrophobic transparent silica aerogel sheet, and methods of making such an article. Still further, the invention relates to an insulating glazing unit having a hydrophobic transparent silica aerogel sheet between two glass sheets, and methods of making such an insulating glazing unit. Further yet, the invention relates to a laminated glass assembly having a hydrophobic transparent silica aerogel sheet between glass sheets, and methods of making such a laminated glass assembly.BACKGROUND OF THE INVENTION

[0003] Silica aerogels are thermally insulating materials that have applications in a number of different industries. However, silica aerogels have had limited applications in windows because they have not traditionally achieved the right combination of mechanical, thermal and optical properties to be fully acceptable for all such applications. Researchers have experimented with many different precursor recipes and methods in the hope of producing silica aerogel with an optimum combination of mechanical, thermal and optical properties but have been unsuccessful. While some recipes and methods led to certain properties being optimized, other properties were compromised.

[0004] One property desirable for window applications is high visible transmission. When silica aerogel is provided as part of certain windows, it must be transparent to be considered optically acceptable. Another desirable property is low haze. Silica aerogel must have low haze to be ideal for use with many windows. Still another desirable property is moisture resistance. Silica aerogels tend to be hydrophilic and thus prone to deterioration of several different properties when exposed to enough moisture. Too much moisture exposure can cause undesirable optical defects, such as reduction in visible transmission and increase in haze. Since some amount of moisture is often present inside insulating glazing units, it is desirable for silica aerogel to be hydrophobic. Hydrophobic silica aerogel can resist deterioration from moisture, making it particularly advantageous for use in window applications.

[0005] Researchers have attempted to produce transparent hydrophobic silica aerogel. However, while researchers have found certain recipes and methods that produce hydrophobic silica aerogel, the resulting aerogel was characterized by lower visible transmission, too much haze, or both. Moreover, existing methods for making silica aerogel hydrophobic have not been ideal for commercial use. For example, some prior methods involve using hydrophobic agents in the production process. These agents, however, may cause an increase in haze and a reduction in visible transmission. Researchers have tried to mitigate this undesirable effect by adding processing steps. One other mitigation step is to add expensive surfactants to control particle size in the silica wet gel. However, the wet gels then must be subjected to further processing, such as excessive solvent baths using expensive solvents, to remove the surfactants and excess hydrophobic agents. This additional processing is not only expensive, but it can actually cause deterioration in optical properties of the resulting silica aerogel.

[0006] It would be desirable to provide hydrophobic silica aerogel having a desirable combination of mechanical, thermal and / or optical properties. It would be particularly desirable to provide silica aerogel that is hydrophobic in combination with having high visible transmission and low haze, optionally together with certain advantageous mechanical properties. It would also be desirable to provide methods of making high quality hydrophobic silica aerogel that are commercially feasible and do not require expensive or excessive processing.BRIEF DESCRIPTION OF THE DRAWINGS

[0007] FIG. 1 is a flow chart depicting a method of making hydrophobic silica wet gel in accordance with certain embodiments;

[0008] FIG. 2 is a flow chart depicting a method of making hydrophobic silica aerogel in accordance with certain embodiments;

[0009] FIG. 3 is a flow chart depicting a method of making hydrophobic silica wet gel in accordance with certain embodiments;

[0010] FIG. 4 is a flow chart depicting a method of making hydrophobic silica aerogel in accordance with certain embodiments;

[0011] FIG. 5 is a flow chart depicting a method of making hydrophobic silica wet gel in accordance with certain embodiments;

[0012] FIG. 6 is a flow chart depicting a method of making hydrophobic silica aerogel in accordance with certain embodiments;

[0013] FIG. 7 is a schematic, broken-away, cross-sectional side view of an article that includes a glass sheet and a hydrophobic silica aerogel sheet in accordance with certain embodiments;

[0014] FIG. 8 is a schematic, partially broken-away, cross-sectional side view of an insulating glazing unit in accordance with certain embodiments; and

[0015] FIG. 9 is a schematic, partially broken-away, cross-sectional side view of a laminated glass assembly that includes a hydrophobic silica aerogel sheet in accordance with certain embodiments.SUMMARY OF THE INVENTION

[0016] Certain embodiments provide a hydrophobic silica aerogel sheet synthesized from at least two alkoxy silanes and having a visible transmission of at least 97.8% and a haze value of 3% or less. The hydrophobic silica aerogel sheet can also include at least one of the following features (A) through (E):(A) a water contact angle of at least 90°;(B) a thermal conductivity in air of 13.5 mW / m K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 750 m2 / g;(E) an average pore diameter of 30 nm or less.

[0017] The hydrophobic silica aerogel sheet can optionally include at least two of the features (A) through (E), at least three of the features (A) through (E), at least four of the features (A) through (E), or all of the features (A) through (E). Also, in some cases, the visible transmission of the hydrophobic silica aerogel sheet is at least 98.6%, and the haze value is 2.5% or less. In further cases, the visible transmission of the hydrophobic silica aerogel sheet is at least 99%, and the haze value is 2% or less. The water contact angle in feature (A) can optionally be at least 100°, such as at least 110° or at least 120°. The flexural modulus in feature (C) can optionally be 1500 kPa or less. Further, the specific surface area in feature (D) can optionally be at least 800 m2 / g. Even further, the average pore diameter in feature (E) can optionally be 27 nm or less.

[0018] Other embodiments provide a hydrophobic silica aerogel sheet synthesized from at least two alkoxy silanes and having a visible transmission of at least 98% and a haze value of 2% or less. The hydrophobic silica aerogel sheet can also include at least one of the following features (A) through (E):(A) a water contact angle of at least 110°;(B) a thermal conductivity in air of 13 mW / m K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 750 m2 / g;(E) an average pore diameter of 29 nm or less.

[0019] Again, the hydrophobic silica aerogel sheet can optionally include at least two of the features (A) through (E), at least three of the features (A) through (E), at least four of the features (A) through (E), or all of the features (A) through (E).

[0020] Other embodiments provide a hydrophobic silica aerogel sheet synthesized from at least two alkoxy silanes and having a visible transmission of at least 98.6% and a haze value of 1.5% or less. The hydrophobic silica aerogel sheet can also include at least one of the following features (A) through (E):(A) a water contact angle of at least 120°;(B) a thermal conductivity in air of 13 mW / m K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 900 m2 / g;(E) an average pore diameter of 28 nm or less.

[0021] Here too, the hydrophobic silica aerogel sheet can optionally include at least two of the features (A) through (E), at least three of the features (A) through (E), at least four of the features (A) through (E) or all of the features (A) through (E).

[0022] In some embodiments, a first alkoxy silane of the two alkoxy silanes is selected from methyl silicate 51, tetramethoxysilane and tetraethoxy silane, and a second alkoxy silane of the two alkoxysilanes is selected from methyltrimethoxysilane, methyltri ethoxysilane, ethyltrimethoxysilane and propyltrimethoxysilane. In certain embodiments, a first alkoxy silane of the two alkoxy silanes is selected from methyl silicate 51 and tetramethoxy silane, and a second alkoxy silane of the two alkoxy silanes is selected from methyltrimethoxysilane and methyltriethoxysilane. In some cases, the first alkoxysilane is methyl silicate 51 and the second alkoxy silane is methyltrimethoxy silane. Also, in some cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltriethoxysilane. In further cases, the first alkoxysilane is tetramethoxysilane and the second alkoxysilane is methyltrimethoxysilane. In even further cases, the first alkoxysilane is tetramethoxysilane and the second alkoxysilane is methyltriethoxysilane.

[0023] Certain embodiments provide a method of making a hydrophobic silica aerogel, comprising the steps of: synthesizing a hydrophobic silica wet gel from a first alkoxysilane and a second alkoxy silane, wherein the first alkoxy silane is selected from methyl silicate 51 and tetramethoxy silane (also known as tetramethyl orthosilicate), and the second alkoxysilane is methyltrimethoxysilane; aging the hydrophobic silica wet gel for an aging time period; and subjecting the hydrophobic silica wet gel to drying, for example critical point drying, to form a hydrophobic silica aerogel having a shrinkage value of 4% or less, for example 3.5% or less, 3% or less, 2.5% or less, 2% or less or 1.75% or less.

[0024] In some cases, the first alkoxy silane is methyl silicate 51. In other cases, the first alkoxy silane is tetramethoxy silane. The method can further include subjecting thehydrophobic silica wet gel to solvent extraction with an extraction solvent (e.g., methanol) for an extraction time period of less than 24 hours (e.g., less than 20 hours). Also, in some cases, the method can be devoid of using a surfactant. Additionally or alternatively, the method can be devoid of using a hydrophobic agent other than the second alkoxysilane.

[0025] Further, the step of aging the hydrophobic silica wet gel can comprise aging the hydrophobic silica wet gel at room temperature. The aging time period can be at least 7 days (168 hours), at least 8 days (192 hours), at least 9 days (216 hours) or at least 10 days (240 hours). The aging time period can be a time period until which structural changes of the hydrophobic silica wet gel no longer occur. The hydrophobic silica aerogel prepared according to this method can have a visible transmission of at least 97.8% and a haze value of 3% or less, for example a visible transmission of at least 98% and a haze value of 3% or less, a visible transmission of at least 98.6% and a haze value of 2.5 % or less, or a visible transmission of at least 99% and a haze value of 2% or less. Also, the hydrophobic silica aerogel prepared according to this method can have a water contact angle of at least 90%, for example at least 100% or at least 110%.

[0026] Other embodiments provide a method of making a hydrophobic silica aerogel, comprising the steps of: preparing a silica wet gel from a precursor material comprising a first alkoxysilane, solvent, catalyst and water, wherein the first alkoxysilane is selected from methyl silicate 51 and tetramethoxy silane; preparing a hydrophobic treatment solution from a second alkoxysilane and diluent, wherein the second alkoxysilane is selected from methyltrimethoxysilane and methyltri ethoxysilane; exposing the silica wet gel to the hydrophobic treatment solution to form a hydrophobic silica wet gel; aging either the silica wet gel or the hydrophobic silica wet gel for an aging time period; subjecting the hydrophobic silica wet gel to solvent extraction with an extraction solvent for an extraction time period of less than 24 hours (e.g., less than 20 hours); and subjecting the hydrophobic silica wet gel to critical point drying to form a hydrophobic silica aerogel.

[0027] In some cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltrimethoxysilane. In other cases, the first alkoxysilane is tetramethoxy silane and the second alkoxysilane is methyltrimethoxysilane. Also, in other cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltriethoxysilane. In yet other cases, the first alkoxy silane is tetramethoxy silane and the second alkoxy silane is methyltriethoxysilane. The method can further include aging the silica wet gel or the hydrophobic silica wet gel at room temperature. The aging time period can be at least 7 days (168 hours), at least 8 days (192 hours), at least 9 days (216 hours) or at least 10 days (240 hours). The aging time period can be a time period until which structural changes of the hydrophobic silica wet gel no longer occur.

[0028] In some cases, the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel such that less than 1% solvent remains within the hydrophobic silica aerogel. Further, in some cases, the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less, for example 3.5% or less, 3% or less, 2.5% or less, 2% or less or 1.75% or less.

[0029] The method can also be devoid of using a surfactant. Additionally or alternatively, the method can be devoid of using a hydrophobic agent other than the hydrophobic treatment solution. Further, in certain cases, each of the solvent, the diluent and the extraction solvent is methanol.

[0030] The hydrophobic silica aerogel prepared according to this method can have a visible transmission of at least 97.8% and a haze value of 3% or less, for example a visible transmission of at least 98% and a haze value of 3% or less, a visible transmission of at least 98.6% and a haze value of 2.5 % or less, or a visible transmission of at least 99% and a haze value of 2% or less. Also, the hydrophobic silica aerogel prepared according to this method can have a water contact angle of at least 90%, for example at least 100% or at least 110%.

[0031] Other embodiments provide a method of making a hydrophobic silica aerogel, comprising the steps of:preparing a first solution by mixing a first alkoxysilane and solvent, wherein the first alkoxysilane is selected from methyl silicate 51 and tetramethoxysilane; preparing a second solution by mixing solvent, ammonium hydroxide and water; mixing the first solution and the second solution together; allowing components in the first solution and the second solution to react to form a silica wet gel; preparing a third solution by combining methyltnmethoxysilane and diluent; adding the third solution to the silica wet gel; allowing the third solution to react with the silica wet gel to form a hydrophobic silica wet gel; aging either the silica wet gel or the hydrophobic silica wet gel for an aging time period; subjecting the hydrophobic silica wet gel to solvent extraction with an extraction solvent; subjecting the hydrophobic silica wet gel to drying to form a hydrophobic silica aerogel; and wherein the method is devoid of using a surfactant.

[0032] In some cases, the first alkoxy silane is methyl silicate 51. In other cases, the first alkoxy silane is tetramethoxysilane. The step of aging can comprise aging the silica wet gel or the hydrophobic silica wet gel at room temperature. The aging time period can be at least 7 days (168 hours), at least 8 days (192 hours), at least 9 days (216 hours) or at least 10 days (240 hours). The aging time period can be a time period until which structural changes of the hydrophobic silica wet gel no longer occur. Further, in some cases, the step of subjecting the hydrophobic silica wet gel to solvent extraction is performed during an extraction time period of less than 24 hours (e.g., less than 20 hours).

[0033] In certain cases, the step of subjecting the hydrophobic silica wet gel to drying can form the hydrophobic silica aerogel such that less than 1% solvent remains within the hydrophobic silica aerogel. Also, in some cases, the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less, for example 3.5% or less, 3% or less, 2.5% or less, 2% or less or 1.75% or less.

[0034] Also, in some cases, the method can be devoid of using a surfactant. Additionally or alternatively, the method can be devoid of using a hydrophobic agent other than the third solution. Further, in certain cases, each of the solvent, the diluent and the extraction solvent is methanol. The hydrophobic silica aerogel prepared according to this method can have a visible transmission of at least 97.8% and a haze value of 3% or less, for example a visible transmission of at least 98% and a haze value of 3% or less, a visible transmission of at least 98.6% and a haze value of 2.5 % or less, or a visible transmission of at least 99% and a haze value of 2% or less. Also, the hydrophobic silica aerogel prepared according to this method can have a water contact angle of at least 90%, for example at least 100% or at least 110%.

[0035] Other embodiments provide a method of making a hydrophobic silica aerogel, comprising the steps of: preparing a silica wet gel from a precursor material comprising a first alkoxysilane, solvent, catalyst and water, wherein the first alkoxysilane is selected from methyl silicate 51 and tetramethoxy silane; aging the silica wet gel for an aging time period; preparing a hydrophobic treatment solution from a second alkoxysilane, catalyst and diluent, wherein the second alkoxysilane is selected from methyltrimethoxysilane and methyltri ethoxysilane; adding the hydrophobic treatment solution to an extraction solvent to form a solvent exchange solution; subjecting the silica wet gel to the solvent exchange solution for an extraction time period of less than 24 hours and allowing components in the solvent exchange solution to react with the silica wet gel to form a hydrophobic silica wet gel; and subjecting the hydrophobic silica wet gel to drying to form a hydrophobic silica aerogel.

[0036] In some cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltrimethoxysilane. In other cases, the first alkoxysilane is tetramethoxy silane and the second alkoxysilane is methyltrimethoxysilane. Also, in other cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltriethoxysilane. In yet other cases, the first alkoxysilane is tetramethoxysilane and the second alkoxysilane is methyltriethoxysilane. The step of aging can comprise aging the silica wet gel or thehydrophobic silica wet gel at room temperature. The aging time period can be at least 7 days (168 hours), at least 8 days (192 hours), at least 9 days (216 hours) or at least 10 days (240 hours). The aging time period can be a time period until which structural changes of the hydrophobic silica wet gel no longer occur. Further, in some cases, the step of subjecting the hydrophobic silica wet gel to the solvent exchange solution is performed during an extraction time period of less than 24 hours (e.g., less than 20 hours).

[0037] In certain cases, the step of subjecting the hydrophobic silica wet gel to drying can form the hydrophobic silica aerogel such that less than 1% solvent remains within the hydrophobic silica aerogel. Also, in some cases, the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less, for example 3.5% or less, 3% or less, 2.5% or less, 2% or less or 1.75% or less.

[0038] Also, in some cases, the method can be devoid of using a surfactant. Additionally or alternatively, the method can be devoid of using a hydrophobic agent other than the hydrophobic treatment solution. Further, in certain cases, each of the solvent, the diluent and the extraction solvent is methanol. The hydrophobic silica aerogel prepared according to this method can have a visible transmission of at least 97.8% and a haze value of 3% or less, for example a visible transmission of at least 98% and a haze value of 3% or less, a visible transmission of at least 98.6% and a haze value of 2.5 % or less, or a visible transmission of at least 99% and a haze value of 2% or less. Also, the hydrophobic silica aerogel prepared according to this method can have a water contact angle of at least 90%, for example at least 100% or at least 110%.

[0039] Other embodiments provide a method of making a hydrophobic silica aerogel, comprising the steps of: preparing a first solution by mixing a first alkoxysilane and solvent, wherein the first alkoxysilane is selected from methyl silicate 51 and tetramethoxysilane; preparing a second solution by mixing ammonium hydroxide and water; mixing the first solution and the second solution together; allowing components in the first solution and the second solution to react to form a silica wet gel; aging the silica wet gel for an aging time period;preparing a third solution by mixing catalyst and solvent; preparing a fourth solution by mixing a second alkoxysilane, catalyst and diluent, wherein the second alkoxysilane is selected from methyltrimethoxysilane and methyltri ethoxysilane; preparing a solvent exchange solution by mixing the third solution, the fourth solution and an extraction solvent; subjecting the silica wet gel to the solvent exchange solution for an extraction time period of less than 24 hours and allowing components in the solvent exchange solution to react with the silica wet gel to form a hydrophobic silica wet gel; and subjecting the hydrophobic silica wet gel to drying to form a hy drophobic silica aerogel; and wherein the method is devoid of using a surfactant.

[0040] In some cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltrimethoxysilane. In other cases, the first alkoxysilane is tetramethoxy silane and the second alkoxysilane is methyltrimethoxysilane. Also, in other cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltriethoxysilane. In yet other cases, the first alkoxy silane is tetramethoxy silane and the second alkoxy silane is methyltriethoxysilane. The step of aging can comprise aging the silica wet gel or the hydrophobic silica wet gel at room temperature. The aging time period can be at least 7 days (168 hours), at least 8 days (192 hours), at least 9 days (216 hours) or at least 10 days (240 hours). The aging time period can be a time period until which structural changes of the hydrophobic silica wet gel no longer occur. Further, in some cases, the step of subjecting the hydrophobic silica wet gel to the solvent exchange solution is performed during an extraction time period of less than 24 hours (e.g., less than 20 hours).

[0041] In certain cases, the step of subjecting the hydrophobic silica wet gel to drying can form the hydrophobic silica aerogel such that less than 1% solvent remains within the hydrophobic silica aerogel. Also, in some cases, the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less, for example 3.5% or less, 3% or less, 2.5% or less, 2% or less or 1.75% or less.

[0042] Also, the method can be devoid of using a hydrophobic agent other than the second alkoxy silane in the solvent exchange solution. Further, in certain cases, each of the solvent, the diluent and the extraction solvent is methanol. The hydrophobic silica aerogel prepared according to this method can have a visible transmission of at least 97.8% and a haze value of 3% or less, for example a visible transmission of at least 98% and a haze value of 3% or less, a visible transmission of at least 98.6% and a haze value of 2.5 % or less, or a visible transmission of at least 99% and a haze value of 2% or less. Also, the hydrophobic silica aerogel prepared according to this method can have a water contact angle of at least 90%, for example at least 100% or at least 110%.

[0043] Other embodiments provide a method of making a hydrophobic silica aerogel, comprising the steps of: preparing a first solution by mixing a first alkoxysilane and solvent; preparing a second solution by mixing solvent, base catalyst and water; mixing the first solution and the second solution together; allowing components in the first solution and the second solution to react to form a silica wet gel; preparing a third solution by combining a second alkoxysilane and diluent; adding the third solution to the silica wet gel; allowing components in the third solution and the silica wet gel to react to form a hydrophobic silica wet gel; and drying the hydrophobic silica wet gel to form a hydrophobic silica aerogel having a visible transmission of at least 97.8% and a haze value of 3% or less.

[0044] Further embodiments provide a method of making a hydrophobic silica aerogel, comprising the steps of: preparing a first solution by mixing a first alkoxysilane and solvent; preparing a second solution by mixing base catalyst and water; mixing the first solution and the second solution together; allowing components in the first solution and the second solution to react to form a silica wet gel; preparing a third solution by mixing base catalyst and solvent; preparing a fourth solution by combining a second alkoxysilane and diluent;preparing a solvent mixture by mixing the third solution, the fourth solution and solvent; subjecting the silica wet gel to the solvent mixture and allowing components in the solvent mixture to react with the silica wet gel to form a hydrophobic silica wet gel; and drying the hydrophobic silica wet gel to form a hydrophobic silica aerogel having a visible transmission of at least 97.8% and a haze value of 3% or less.

[0045] In either method, the first alkoxysilane can be selected from methyl silicate 51, tetramethoxy silane and tetraethoxy silane, and the second alkoxysilane can be selected from methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane and propyltrimethoxysilane. In certain cases, the first alkoxysilane is selected from methyl silicate 51 and tetramethoxy silane, and the second alkoxy silane can be selected from methyltrimethoxysilane and methyltriethoxysilane. In some cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltrimethoxysilane. In other cases, the first alkoxysilane is methyl silicate 51 and the second alkoxysilane is methyltriethoxysilane. In further cases, the first alkoxysilane is tetramethoxysilane and the second alkoxysilane is methyltrimethoxysilane. In even further cases, the first alkoxysilane is tetramethoxysilane and the second alkoxysilane is methyltriethoxysilane.

[0046] In some embodiments, the hydrophobic silica aerogel prepared according to either method can further include at least one of the features (A) through (F):(A) a water contact angle of at least 90°;(B) a thermal conductivity in air of 13.5 mW / m-K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 750 m2 / g;(E) an average pore diameter of 30 nm or less;(F) a shrinkage value of less than 3.5%.

[0047] The hydrophobic silica aerogel prepared by either method can optionally include at least two of the features (A) through (F), at least three of the features (A) through (F), at least four of the features (A) through (F), at least five of the features (A) through (F), or all of the features (A) through (F). Also, in some cases, the visible transmission of the hydrophobic silica aerogel sheet is at least 98.6%, and the haze value is 2.5% or less. In further cases, thevisible transmission of the hydrophobic silica aerogel sheet is at least 99%, and the haze value is 2% or less. The water contact angle in feature (A) can optionally be at least 100°, such as at least 110° or at least 120°. The flexural modulus in feature (C) can optionally be 4500 kPa or less. Further, the specific surface area in feature (D) can optionally be at least 800 m2 / g. Even further, the average pore diameter in feature (E) can optionally be 27 nm or less.

[0048] In other embodiments, the hydrophobic silica aerogel prepared according to either method can further include at least one of the features (A) through (F):(A) a water contact angle of at least 110°;(B) a thermal conductivity in air of 13 mW / m K or less;(C) a flexural modulus of 6000 kPa or less;(D) a surface area of at least 750 m2 / g;(E) an average pore diameter of 29 nm or less;(F) a shrinkage value of less than 2%.

[0049] Here too, the prepared hydrophobic silica aerogel can include at least two of the features (A) through (F), at least three of the features (A) through (F), at least four of the features (A) through (F), at least five of the features (A) through (F), or all of the features (A) through (F).

[0050] In further embodiments, the hydrophobic silica aerogel prepared according to either method can have a visible transmission of at least 98.6% and a haze value of 1.5% or less. The hydrophobic silica aerogel can further include at least one of the features (A) through (F):(A) a water contact angle of at least 120°;(B) a thermal conductivity in air of 13 mW / m K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 900 m2 / g;(E) an average pore diameter of 28 nm or less;(F) a shrinkage value of less than 1.75%.

[0051] Again, the prepared hydrophobic silica aerogel can optionally include at least two of the features (A) through (F), at least three of the features (A) through (F), at least four of the features (A) through (F), at least five of the features (A) through (F), or all of the features (A) through (F).

[0052] Other embodiments provide an article comprising a glass substrate and a hydrophobic silica aerogel sheet, the hydrophobic silica aerogel sheet being adhered to the glass substrate. Additional embodiments provide an insulating glazing unit comprising two glass sheets and a between-pane space, the between-pane space being located between the two glass sheets, the insulating glazing unit further comprising a hydrophobic silica aerogel sheet received in the between-pane space. The hydrophobic silica aerogel sheet can optionally be adhered to an interior surface of one of the two glass sheets. Further embodiments provide a laminated glass assembly comprising two glass sheets and a hydrophobic silica aerogel sheet between the two glass sheets. The hydrophobic silica aerogel sheet in these embodiments can have any of the features described herein. In some cases, the hydrophobic silica aerogel sheet has a thickness of between 2 mm and 15 mm.DETAILED DESCRIPTION OF PREFERRED EMBODIMENTS

[0053] The following detailed description is to be read with reference to the drawings, in which like elements in different drawings have like reference numerals. The drawings, which are not necessarily to scale, depict selected embodiments and are not intended to limit the scope of the invention. Skilled artisans will recognize that the examples provided herein have many useful alternatives that fall within the scope of the invention.

[0054] In the present specification, anywhere the terms “comprising” or “comprises” are used, those terms have their ordinary, open-ended meaning. In addition, where appropriate, the disclosure at each such location is to be understood to also disclose that it may, as an alternative, “consist essentially of’ or “consist of.”

[0055] Applicant has developed precursor materials, hydrophobic silica wet gel, hydrophobic silica aerogel and methods of making such materials that can be used to form enhanced silica aerogel sheets. The enhanced silica aerogel sheets can achieve an exceptional, surprising combination of optical, thermal and / or mechanical properties, which makes them highly advantageous for use in window applications.

[0056] The term “silica wet gel” refers to a material that is obtained by allowing components of a precursor material to react to form silica wet gel. The precursor material serves as an intermediate product that is used to form silica wet gel. Also, the term “silica aerogel” refers to material that is obtained by removing liquid from silica wet gel material and replacing the liquid with gas or vacuum. Further, the term “hydrophobic silica wet gel” refers to silica wet gel that resists absorbing moisture. Likewise, the term “hydrophobic silica aerogel” refers to silica aerogel that resists absorbing moisture.

[0057] Certain embodiments provide a precursor material and a hydrophobic agent for synthesizing a hydrophobic silica wet gel. The precursor material serves as an intermediate product that is used to form silica wet gel, which is treated with the hydrophobic agent to form a hydrophobic silica wet gel. The precursor material comprises a first alkoxysilane, and the hydrophobic agent comprises a second alkoxysilane.

[0058] Several reactions take place during silica wet gel synthesis: hydrolysis, condensation, nucleation and growth. These various reactions can have different reaction rates depending on the components used for the precursor material. The reaction rates affect mechanical, thermal and optical properties of a resulting silica aerogel. Thus, the resulting aerogel is extremely sensitive to variations in precursor material components and percentage of components. As an example, the hydrolysis reaction rate is determined by the amount of catalyst in the precursor material. The hydrolysis reaction is also exothermic, so it imparts heat to the precursor material, which in turn accelerates the condensation reaction rate. As a consequence, too much catalyst can accelerate the condensation reaction rate. Accelerated condensation reaction rates are undesirable since they can lead to an accelerated nucleation rate and an accelerated growth rate. Furthermore, if the grow th rate exceeds the nucleation rate, the three-dimensional polymer structure will have unduly large particle sizes. Larger particle sizes create more scattering of light, which in turn leads to undesirable properties such as increased haze and reduced visible transmission. All of these variabilities make silica wet gel and aerogel synthesis unpredictable. Even more unpredictability occurs when hydrophobic agents are added to the synthesis process, since hydrophobic agents may agglomerate and cause increased haze and reduced visible transmission.

[0059] In some embodiments, the precursor material comprises a first alkoxysilane, solvent, water and base catalyst. The hydrophobic agent comprises a second alkoxysilane. Applicant has identified a “sweet spot” of weight percentage ranges for these components along with a molar ratio range of the first alkoxy silane: second alkoxysilane that can be used to form hydrophobic silica wet gel and hydrophobic silica aerogel having a surprising combination of optical, mechanical and / or thermal properties. Particular embodiments using specific methods, weight percentages and molar ratios will be discussed.

[0060] In some cases, the first alkoxysilane is selected from methyl silicate 51 (MS-51) and tetramethyl orthosilicate (also known as tetramethoxy silane) (TMOS). The second alkoxysilane can be an organo-silane selected from methyltnmethoxysilane (MTMS), methyltriethoxysilane (MTES), ethyltrimethoxysilane (ETMS) and propyltnmethoxysilane (PTMS). In certain cases, the first alkoxysilane is MS-51 and the second alkoxysilane is MTMS. In other cases, the first alkoxysilane is MS-51 and the second alkoxysilane is MTES. In further cases, the first alkoxysilane is TMOS and the second alkoxysilane is MTMS. In even further cases, the first alkoxy silane is TMOS and the second alkoxy silane is MTES.In some cases, the precursor material comprises MS-51 as the first alkoxysilane, methanol as the solvent, and ammonium hydroxide as the base catalyst, while the hydrophobic agent comprises MTMS as the second alkoxysilane. In other cases, the precursor material comprises MS-51 as the first alkoxysilane, methanol as the solvent, and ammonium hydroxide as the base catalyst, while the hydrophobic agent comprises MTES as the second alkoxysilane. Also, in some cases, the precursor material comprises TMOS as the first alkoxysilane, methanol as the solvent, and ammonium hydroxide as the base catalyst, while the hydrophobic agent comprises MTMS as the second alkoxysilane. In other cases, the precursor material comprises TMOS as the first alkoxysilane, methanol as the solvent, and ammonium hydroxide as the base catalyst, while the hydrophobic agent comprises MTES as the second alkoxysilane.The hydrophobic agent includes the second alkoxysilane. In some cases, the hydrophobic agent is a solution that includes the second alkoxysilane and diluent. In other cases, the hydrophobic agent is a solvent extraction solution that includes the second alkoxysilane, diluent, catalyst and solvent.

[0061] In some cases, components in a first solution, a second solution, a third solution, a fourth solution and a fifth solution are present within selected weight percentages. Again, Applicant has identified recipe components along with a “sweet spot” of weight percentage ranges that can be used to form hydrophobic silica wet gel and hydrophobic silica aerogel having an exceptional combination of properties. As used herein, “weight percent” refers to weight percent of a component in a single solution used to form hydrophobic wet gel (e.g., in the first solution, the second solution, the third solution, the fourth solution or the fifth solution). Further, as used herein, “total weight percent” refers to total weight percent of a component used to form hydrophobic silica wet gel. For example, if three solutions are used to form the hydrophobic silica wet gel, the total weight percent of a component is the total weight percent of that component in the combination of the first solution, the second solution and the third solution. Similarly, if four solutions are used to form the hydrophobic silica wet gel, the total weight percent of a component is the total weight percent of that component in the combination of the first solution, the second solution, the third solution and the fourth solution. Finally, if five solutions are used to form the hydrophobic silica wet gel, the total weight percent of a component is the total weight percent of that component in the combination of the first solution, the second solution, the third solution, the fourth solution and the fifth solution.

[0062] Some embodiments provide a method of making a hydrophobic silica wet gel. FIG. 1 illustrates a method 200A of preparing a hydrophobic silica wet gel according to certain embodiments. The method 200A includes a step 205 of preparing a first solution by mixing a first alkoxysilane and solvent, a step 210 of preparing a second solution by mixing solvent, catalyst and water, a step 215 of mixing the first solution and the second solution together to form a mixed solution, a step 220 of allowing components in the mixed solution to react to form silica wet gel, a step 225 of aging the silica wet gel for a period of time, a step 230 of preparing a third solution by mixing a second alkoxysilane and diluent, a step 235 of adding the third solution to the silica wet gel before aging is complete, and a step 240 of allowing the third solution to react with the silica wet gel to form hydrophobic silica wet gel.

[0063] In certain cases, step 205 comprises preparing the first solution by mixing a first alkoxysilane and methanol, step 210 comprises preparing a second solution by mixingmethanol, ammonium hydroxide and water, and step 230 comprises preparing a third solution by mixing an organo-silane and methanol. In method 200 A, hydrophobic treatment is performed before the silica wet gel aging is complete.

[0064] In some embodiments of the method 200A, the first alkoxy silane is MS-51. Applicant has found that MS-51 provides desirable results because it is pre-hydrolyzed. As a result, a hydrolysis reaction in the precursor material is absent, which leads to a lower condensation rate and thus a lower nucleation rate. Lower nucleation rates allow the formation of a three- dimensional polymer structure with smaller particle sizes. The resulting silica aerogel therefore has less scattering of light and therefore reduced haze and increased transmissivity. For commercial window applications, aerogel particle size is desirably less than 5 nm to have the lowest possible light scattering and thus acceptable haze and transmissivity. Also, in some cases, the precursor material comprises methanol as the solvent. Applicant has discovered that by using methanol as the solvent, the resulting aerogel material has less haze and less optical distortion than with other solvents. In certain cases, the precursor material comprises ammonium hydroxide as the catalyst. Here too, Applicant has discovered that by using ammonium hydroxide as the catalyst, the resulting aerogel material has less haze and less optical distortion than with other catalysts.

[0065] In some embodiments of method 200A, the first alkoxysilane is MS-51 and the second alkoxysilane is MTMS. In these embodiments, the method 200A makes a hydrophobic silica wet gel having a density of between 100 mg / cc and 200 mg / cc, and the MS-51 and MTMS can be provided in a controlled amount selected to provide a molar ratio ofMS-51:MTMS of greater than or equal to 0.95: 1 and less than or equal to 2.55:1. The molar ratio of MS-51 :MTMS can also be greater than or equal to 0.98: 1 and less than or equal to 1.43 : 1 , or greater than or equal to 1.3 : 1 and less than or equal to 1.7 : 1. In other cases, the density is between 120 mg / cc and 200 mg / cc, and the molar ratio of MS-51 :MTMS is greater than or equal to 1.2:1 and less than or equal to 2.55: 1, for example greater than or equal to 1.25: 1 and less than or equal to 1.43: 1 or greater than or equal to 1.60: 1 and less than or equal to 1.71 : 1. In yet other cases, the density is between 120 mg / cc and 150 mg / cc and the molar ratio of MS-51 :MTMS is greater than or equal to 1.2: 1 and less than or equal to 2: 1 , for example greater than or equal to 1.25 : 1 and less than or equal to 1.29: 1 or greater than or equal to 1.60: 1 and less than or equal to 1.66: 1.

[0066] Also, in some embodiments, the method 200A makes a hydrophobic silica wet gel having a density of between 100 mg / cc and 200 mg / cc, and the MS -51 has a total weight percent of greater than or equal to 10% and less than or equal to 25% and the MTMS has a total weight percent of greater than or equal to 2% and less than or equal to 5%. The total weight percent represents a total weight percent of a component in the first, second and third solutions. Also, in some cases, the density of the hydrophobic silica wet gel is between 120 mg / cc and 150 mg / cc and the total weight percent of the MS-51 is greater than or equal to 13% and less than or equal to 21%, and the total weight percent of the MTMS is greater than or equal to 2% and less than or equal to 4%.

[0067] In additional embodiments, in the method 200A, the first alkoxysilane is MS-51, the second alkoxysilane is MTMS, the solvent and the diluent is methanol and the catalyst is ammonium hydroxide. In some embodiments, the method 200A makes a hydrophobic silica wet gel having a density of between 100 mg / cc and 200 mg / cc, and the MS-51 has a total weight percent of greater than or equal to 10% and less than or equal to 25%, the MTMS has a total weight percent of greater than or equal to 2% and less than or equal to 5%, the methanol has a total weight percent of greater than or equal to 59% and less than or equal to 76%, the water has a total weight percent of greater than or equal to 10% and less than or equal to 14% and the ammonium hydroxide has a total weight percent of greater than or equal to 0.010% and less than or equal to 0.14%. In additional embodiments, the method 200A makes a hydrophobic silica wet gel having a density of between 120 mg / cc and 150 mg / cc, and the MS-51 has a total weight percent of greater than or equal to 13% and less than or equal to 21%, the MTMS has a total weight percent of greater than or equal to 2% and less than or equal to 4%, the methanol has a total weight percent of greater than or equal to 66% and less than or equal to 73%, the water has a total weight percent of greater than or equal to 10% and less than or equal to 12% and the ammonium hydroxide has a total weight percent of greater than or equal to 0.010% and less than or equal to 0. 14%.

[0068] Also, in some embodiments of the method 200 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30% and less than or equal to 56% and methanol at a weight percent of greater than or equal to 44% and less than or equal to 70%, the second solution comprises methanol at a weight percent of greater than or equal to 58%and less than or equal to 68%, water at a weight percent of greater than or equal to 32% and less than or equal to 41%, and ammonium hydroxide at a weight percent of greater than or equal to 0.03% and less than or equal to 0.4%, and the third solution comprises methanol at a weight percent of greater than or equal to 84% and less than or equal to 90% and MTMS at a weight percent of greater than or equal to 10% and less than or equal to 16%.

[0069] In other embodiments of the method 200A, the first solution comprises MS-51 at a weight percent of greater than or equal to 36% and less than or equal to 49% and methanol at a weight percent of greater than or equal to 51% and less than or equal to 64%, the second solution comprises methanol at a weight percent of greater than or equal to 65% and less than or equal to 67%, water at a weight percent of greater than or equal to 32% and less than or equal to 35%, and ammonium hydroxide at a weight percent of greater than or equal to 0.03% and less than or equal to 0.4%, and the third solution comprises methanol at a weight percent of greater than or equal to 86% and less than or equal to 90% and MTMS at a weight percent of greater than or equal to 10% and less than or equal to 14%.Embodiments of Method 200A

[0070] In some cases, the MTMS is provided in a controlled amount to provide a molar ratio of the MS-51 :MTMS of greater than or equal to 0.95: 1 and less than or equal to 2.55: 1. In specific cases, the molar ratio is greater than or equal to 0.95: 1 and less than or equal to 2: 1, such as greater than or equal to 0.95: 1 and less than or equal to 1.2: 1. In further cases, the molar ratio is greater than or equal to 1.2: 1 and less than or equal to 2.55: 1, such as greater than or equal to 1.2: 1 and less than or equal to 2: 1.

[0071] Also, in some cases, the MS-51 has a total weight percent of greater than or equal to 10.775% and less than or equal to 24.032% and the MTMS has a total weight percent of greater than or equal to 2.593% and less than or equal to 3.171%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 10.775% and less than or equal to 20.399% and the MTMS has a total weight percent of greater than or equal to 2.871% and less than or equal to 3. 171%. In other cases, the MS-51 has a total weight percent of greater than or equal to 10.775% and less than or equal to 13.494% and the MTMS has a total weight percent of greater than or equal to 3.12% and less than or equal to 3.171%. In further cases,the MS-51 has a total weight percent of greater than or equal to 13.494% and less than or equal to 24.032% and the MTMS has a total weight percent of greater than or equal to 2.593% and less than or equal to 3.12%. In even further cases, the MS-51 has a total weight percent of greater than or equal to 13.494% and less than or equal to 20.399% and the MTMS has a total weight percent of greater than or equal to 2.871% and less than or equal to 3.12%.

[0072] In certain embodiments of method 200A where the first alkoxysilane is MS-51 and where the second alkoxysilane is MTMS, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 55.56% and methanol at a weight percent of greater than or equal to 44.44% and less than or equal to 69. 16%, the second solution comprises methanol at a weight percent of greater than or equal to 58.63% and less than or equal to 67.54%, water at a weight percent of greater than or equal to 32. 16% and less than or equal to 41%, and ammonium hydroxide at a weight percent of greater than or equal to 0.3% and less than or equal to 0.38%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.775% and less than or equal to 24.032%, MTMS at a total weight percent of greater than or equal to 2.593% and less than or equal to 3.171%, methanol at atotal weight percent of greater than or equal to 59.809% and less than or equal to 74.442%, water at a total weight percent of greater than or equal to 11.506% and less than or equal to 13.442% and ammonium hy droxide at a total weight percent of greater than or equal to 0.096% and less than or equal to 0. 124%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0073] Also, in some embodiments of the method 200 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 51.06% and methanol at a weight percent of greater than or equal to 51.06% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 66.94% and less than or equal to 67.54%, water at a weight percent of greater than or equal to 32. 16% and less than or equal to 32.76%, and ammonium hydroxide at a weight percent of about 0.3%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gelobtained by method 200 A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.775% and less than or equal to 20.399%, MTMS at a total weight percent of greater than or equal to 2.871% and less than or equal to 3.171%, methanol at a total weight percent of greater than or equal to 66.217% and less than or equal to 74.442%, water at a total weight percent of greater than or equal to 10.417% and less than or equal to 11.506% and ammonium hydroxide at a total weight percent of greater than or equal to 0.096% and less than or equal to 0.106%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0074] In certain embodiments of the method 200A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 36.84% and methanol at a weight percent of greater than or equal to 63.16% and less than or equal 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 66.94% and less than or equal to 67.54%, water at a weight percent of greater than or equal to 32. 16% and less than or equal to 32.76%, and ammonium hydroxide at a weight percent of about 0.3%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200 A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.775% and less than or equal to 13.494%, MTMS at a total weight percent of greater than or equal to 3.12% and less than or equal to 3.171 %, methanol at a total weight percent of greater than or equal to 71.961% and less than or equal to 74.442%, water at a total weight percent of greater than or equal to 11.321% and less than or equal to 11.506% and ammonium hydroxide at a total weight percent of greater than or equal to 0.104% and less than or equal to 0.106%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0075] Further, in some embodiments of the method 200 A, the first solution comprises MS- 51 at a weight percent of greater than or equal to 36.84% and less than or equal to 55.56% and methanol at a weight percent of greater than or equal to 44.44% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 58.63% and less than or equal to 66.94%, water at a weight percent of greater than or equal to 32.76% and less than or equal to 41%, and ammonium hydroxide at a weight percent of greater than or equal to 0.3% and less than or equal to 0.38%, and the third solutioncomprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 13.494% and less than or equal to 24.032%, MTMS at a total weight percent of greater than or equal to 2.593% and less than or equal to 3.12%, methanol at a total weight percent of greater than or equal to 59.809% and less than or equal to 71.961%, water at a total weight percent of greater than or equal to 11.321% and less than or equal to 13.442% and ammonium hydroxide at a total weight percent of greater than or equal to 0.096% and less than or equal to 0. 124%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0076] In even further embodiments of the method 200A, the first solution comprises MS-51 at a weight percent of greater than or equal to 36.84% and less than or equal to 48.94% and methanol at a weight percent of greater than or equal to 51.06% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of about 66.94%, water at a weight percent of about 32.76%, and ammonium hydroxide at a weight percent of about 0.3%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200 A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 13.494% and less than or equal to 20.399%, MTMS at a total weight percent of greater than or equal to 2.871% and less than or equal to 3.12%, methanol at a total weight percent of greater than or equal to 66.217% and less than or equal to 71.961%, water at a total weight percent of greater than or equal to 10.417% and less than or equal to 11.321% and ammonium hydroxide at a total weight percent of greater than or equal to 0.096% and less than or equal to 0.104%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 200A

[0077] In additional embodiments of method 200A where the first alkoxy silane is MS-51 and where the second alkoxysilane is MTMS, the MTMS is provided in a controlled amount to provide a molar ratio of the MS-51 : MTMS of greater than or equal to .98:1 and less than or equal to 1.43: 1. In specific cases, the molar ratio is greater than or equal to .98: 1 and less thanor equal to 1.29: 1, such as greater than or equal to .98: 1 and less than or equal to 1.25: 1. In further cases, the molar ratio is greater than or equal to 1.25:1 and less than or equal to 1.43: 1, such as greater than or equal to 1.25: 1 and less than or equal to 1.29:1.

[0078] Also, in some cases, the MS-51 has a total weight percent of greater than or equal to 10.775% and less than or equal to 22.077% and the MTMS has a total weight percent of greater than or equal to 3.12% and less than or equal to 4.467%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 10.775% and less than or equal to 17.105% and the MTMS has a total weight percent of greater than or equal to 3.12% and less than or equal to 3.845%. In other cases, the MS-51 has a total weight percent of greater than or equal to 10.775% and less than or equal to 13.493% and the MTMS has a total weight percent of greater than or equal to 3.12% and less than or equal to 3.171%. In further cases, the MS-51 has a total weight percent of greater than or equal to 13.493% and less than or equal to 22.077% and the MTMS has a total weight percent of greater than or equal to 3. 12% and less than or equal to 4.467%. In even further cases, the MS-51 has a total weight percent of greater than or equal to 13.493% and less than or equal to 17. 105% and the MTMS has a total weight percent of greater than or equal to 3.12% and less than or equal to 3.845%.

[0079] Further, in some embodiments of the method 200 A, the first solution comprises MS- 51 at a weight percent of greater than or equal to 30.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 63.53% and less than or equal to 67.53%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than or equal to 15.41%, and methanol at a weight percent of greater than or equal to 84.6% and less than or equal to 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.775% and less than or equal to 22.077%, MTMS at a total weight percent of greater than or equal to 3. 12% and less than or equal to 4.467%, methanol at a total weight percent of greater than or equal to 62.546% and less than or equal to 74.436%, water at a total weight percent of greater than or equal to 10.896% and less than or equal to 11.603% andammonium hydroxide at a total weight percent of greater than or equal to 0.014% and less than or equal to 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0080] In other embodiments of the method 200 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.37% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 67.53%, water at a weight percent of greater than or equal to 32.43% and less than 34.64%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than or equal to 13.18% and methanol at a weight percent of greater than or equal to 86.82% and less than or equal to 89.17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.775% and less than or equal to 17. 105%, MTMS at a total weight percent of greater than or equal to 3.12% and less than or equal to 3.845%, methanol at a total weight percent of greater than or equal to 67.779% and less than or equal to 74.436%, water at a total weight percent of greater than or equal to 11.256% and less than or equal to 11.603% and ammonium hydroxide at a total weight percent of about 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0081] In other embodiments of the method 200 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 36.84% and methanol at a weight percent of greater than or equal to 63.16% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 67.53% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 33.03%, and ammonium hydroxide at a weight percent of about 0.04%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89.17%. The resulting hydrophobic silica wet gel obtained by method 200 A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.775% and less than or equal to 13.493%, MTMS at a total weight percent of greater than or equal to 3.12% and less than or equal to 3.171 %, methanol at a totalweight percent of greater than or equal to 71.956% and less than or equal to 74.436%, water at a total weight percent of greater than or equal to 11.416% and less than or equal to11.603% and ammonium hydroxide at a total weight percent of about 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0082] Further, in some embodiments of the method 200 A, the first solution comprises MS- 51 at a weight percent of greater than or equal to 36.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 63.53% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than or equal to 15.41% and methanol at a weight percent of greater than or equal to 84.6% and less than or equal to 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 13.493% and less than or equal to 22.077%, MTMS at a total weight percent of greater than or equal to 3. 12% and less than or equal to 4.467%, methanol at a total weight percent of greater than or equal to 62.546% and less than or equal to 71.956%, water at a total weight percent of greater than or equal to 10.896% and less than or equal to 11.416% and ammonium hydroxide at a total weight percent of greater than or equal to 0.014% and less than or equal to 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0083] In even further embodiments of the method 200A, the first solution comprises MS-51 at a weight percent of greater than or equal to 36.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.37% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 34.64%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than orequal to 13.18% and methanol at a weight percent of greater than or equal to 86.82% and less than or equal to 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 13.493% and less than or equal to 17.105%, MTMS at atotal weight percent of greater than or equal to 3. 12% and less than or equal to 3.845%, methanol at a total weight percent of greater than or equal to 67.779% and less than or equal to 71.956%, water at a total weight percent of greater than or equal to 11.256% and less than or equal to 11.416% and ammonium hydroxide at a total weight percent of about 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 200A

[0084] In other embodiments of method 200A where the first alkoxysilane is MS-51 and the second alkoxysilane is MTMS, the MTMS is provided in a controlled amount to provide a molar ratio of the MS-51 :MTMS of greater than or equal to 1.3 : 1 and less than or equal to 1.71 : 1. In specific cases, the molar ratio is greater than or equal to 1.3 : 1 and less than or equal to 1.66: 1, such as greater than or equal to 1.3: 1 and less than or equal to 1.60: 1. In further cases, the molar ratio is greater than or equal to 1.60: 1 and less than or equal to 1.71 : 1 , such as greater than or equal to 1.60:1 and less than or equal to 1.66: 1.

[0085] Also, in some cases, the MS-51 has atotal weight percent of greater than or equal to 10.861% and less than or equal to 22.242% and the MTMS has a total weight percent of greater than or equal to 2.358% and less than or equal to 3.75%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 10.861% and less than or equal to 17.237% and the MTMS has a total weight percent of greater than or equal to 2.358% and less than or equal to 3.1%. In yet other cases, the MS-51 has a total weight percent of greater than or equal to 10.861% and less than or equal to 13.599% and the MTMS has a total weight percent of greater than or equal to 2.358% and less than or equal to 2.397%. In further cases, the MS-51 has a total weight percent of greater than or equal to 13.599% and less than or equal to 22.242% and the MTMS has a total weight percent of greater than or equal to 2.358 % and less than or equal to 3.75%. In even further cases, the MS-51 has a total weightpercent of greater than or equal to 13.599% and less than or equal to 17.237% and the MTMS has a total weight percent of greater than or equal to 2.358% and less than or equal to 3.1%.

[0086] In some embodiments of the method 200A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 63.53% and less than or equal to 67.53%, water at a weight percent of greater than or equal to 32.3973% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 8.35% and less than or equal to 13.18% and methanol at a weight percent of greater than or equal to 86.82% and less than or equal to 91.65%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.861% and less than or equal to 22.242%, MTMS at a total weight percent of greater than or equal to 2.358% and less than or equal to 3.75%, methanol at a total weight percent of greater than or equal to 63.015% and less than or equal to 75.031%, water at a total weight percent of greater than or equal to 10.979% and less than or equal to 11.696% and ammonium hydroxide at a total weight percent of greater than or equal to 0.014% and less than or equal to 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0087] Also, in some embodiments of the method 200 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.34% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 67.53%, water at a weight percent of greater than or equal to 32.3973% and less than or equal to 34.64%, and ammonium hydroxide at a weight percent of about 0.04%, and the third solution comprises MTMS at a weight percent of greater than or equal to 8.35% and less than or equal to 10.83% and methanol at a weight percent of greater than or equal to 89.17% and less than or equal to 91.65%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.861% and less than or equal to 17.237%, MTMS at atotal weight percent of greater than or equal to 2.358% and less than or equal to 3.1%, methanol at a total weight percent of greater than or equal to 68.304% and less than or equal to 75.031%, water at a total weight percent of greater than or equal to 11.344% and less than or equal to 11.696% and ammonium hydroxide at a total weight percent of about 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0088] Further, in some cases, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 36.84% and methanol at a weight percent of greater than or equal to 63.16% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 66.92% and less than or equal to 67.53%, water at a weight percent of greater than or equal to 32.3973% and less than or equal to 33.03%, and ammonium hydroxide at a weight percent of about 0.04%, and the third solution comprises MTMS at a weight percent of about 8.35% and methanol at a weight percent of about 91.65%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 10.861% and less than or equal to 13.599%, MTMS at a total weight percent of greater than or equal 2.358% and less than or equal to 2.397%, methanol at a total weight percent of greater than or equal to 72.521% and less than or equal to 75.031%, water at a total weight percent of greater than or equal to 11.507% and less than or equal to 11.696% and ammonium hydroxide at a total weight percent of about 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0089] Further, in some embodiments of the method 200 A, the first solution comprises MS- 51 at a weight percent of greater than or equal to 36.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 63.53% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 8.35% and less than or equal to 13.18% and methanol at a weight percent of greater than or equal to 86.82% and less thanor equal to 91.65%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 13.599% and less than or equal to 22.242%, MTMS at a total weight percent of greater than or equal to 2.358% and less than or equal to 3.75%, methanol at a total weight percent of greater than or equal to 63.015% and less than or equal to 72.521%, water at a total weight percent of greater than or equal to 10.979% and less than or equal to 11.507% and ammonium hydroxide at a total weight percent of greater than or equal to 0.014% and less than or equal to 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0090] In even further embodiments of the method 200A, the first solution comprises MS-51 at a weight percent of greater than or equal to 36.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.34% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 34.64%, and ammonium hydroxide at a weight percent of about 0.04%, and the third solution comprises MTMS at a weight percent of greater than or equal to 8.35% and less than or equal to 10.83% and methanol at a weight percent of greater than or equal to 89. 17% and less than or equal to 91.65%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 13.599% and less than or equal to 17.237%, MTMS at a total weight percent of greater than or equal to 2.358% and less than or equal to 3.1%, methanol at a total weight percent of greater than or equal to 68.304% and less than or equal to 72.521%, water at a total weight percent of greater than or equal to 11.344% and less than or equal to 11.507% and ammonium hydroxide at a total weight percent of about 0.015%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 200A

[0091] In some embodiments of the method 200A, TMOS is used as the first alkoxy silane.Applicant has found that TMOS provides desirable results because the resulting silica aerogel has less scattering of light and thus reduced haze and increased transmissivity. Forcommercial window applications, aerogel particle size is desirably less than 5 nm to have the lowest possible light scattering and thus acceptable haze and transmissivity. Also, in some cases, the precursor material comprises methanol as the solvent. Applicant has discovered that by using methanol as the solvent, the resulting aerogel material has less haze and less optical distortion than with other solvents. In certain cases, the precursor material comprises ammonium hydroxide as the catalyst. Applicant has discovered that by using ammonium hydroxide as the catalyst, the resulting aerogel material has less haze and less optical distortion than with other catalysts.

[0092] In some embodiments of the method 200A, TMOS is used as the first alkoxy silane and an organo-silane is used as the second alkoxysilane. The step 205 comprises preparing a first solution by mixing TMOS and methanol, step 210 comprises preparing a second solution by mixing methanol, ammonium hydroxide and water, and step 230 comprises preparing a third solution by mixing an organo-silane and methanol. The organo-silane can be MTMS in some embodiments.

[0093] In some cases, the MTMS is provided in a controlled amount to provide a molar ratio ofthe TMOS:MTMS of greater than or equal to 3.7: 1 and less than or equal to 9.2: 1. In specific cases, the molar ratio is greater than or equal to 3.7: 1 and less than or equal to 6.9: 1, such as greater than or equal to 3.7: 1 and less than or equal to 4.6:1. In further cases, the molar ratio is greater than or equal to 4.6: 1 and less than or equal to 9.2: 1, such as greater than or equal to 4.6: 1 and less than or equal to 6.9: 1.

[0094] Also, in some cases, the TMOS has a total weight percent of greater than or equal to 13.821% and less than or equal to 28.368% and the MTMS has a total weight percent of greater than or equal to 2.63% and less than or equal to 3.204%. In certain cases, the TMOS has a total weight percent of greater than or equal to 13.821% and less than or equal to 23.676% and the MTMS has a total weight percent of greater than or equal to 2.927% and less than or equal to 3.204%. In yet other cases, the TMOS has a total weight percent of greater than or equal to 13.821% and less than or equal to 16.915% and the MTMS has a total weight percent of greater than or equal to 3. 137% and less than or equal to 3.204%. In further cases, the TMOS has a total weight percent of greater than or equal to 16.915% and less than or equal to 28.368% and the MTMS has a total weight percent of greater than or equal to2.63% and less than or equal to 3. 137%. In even further cases, the TMOS has a total weight percent of greater than or equal to 16.915% and less than or equal to 23.676% and the MTMS has a total weight percent of greater than or equal to 2.927% and less than or equal to 3.137%.

[0095] In some embodiments of the method 200 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.17% and less than or equal to 62.82% and methanol at a weight percent of greater than or equal to 37.18% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 54.96% and less than or equal to 65.66%, water at a weight percent of greater than or equal to 33.98% and less than or equal to 44.63%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.41%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 13.821% and less than or equal to 28.368%, MTMS at a total weight percent of greater than or equal to 2.63% and less than or equal to 3.204%, methanol at a total weight percent of greater than or equal to 55.244% and less than or equal to 71.246%, water at a total weight percent of greater than or equal to 10.604% and less than or equal to 13.633% and ammonium hydroxide at a total weight percent of greater than or equal to 0.112% and less than or equal to 0. 125%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0096] In other embodiments of the method 200 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.17% and less than or equal to 55. 11% and methanol at a weight percent of greater than or equal to 44.89% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 64.28% and less than or equal to 65.66%, water at a weight percent of greater than or equal to 33.98% and less than or equal to 35.35%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.37%, and the third solution comprises organo-silane at a weight percent of about 10.83% and methanol at a weight percent of about 89.17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to13.821% and less than or equal to 23.676%, MTMS at a total weight percent of greater than or equal to 2.927% and less than or equal to 3.204%, methanol at a total weight percent of greater than or equal to 62.681% and less than or equal to 71.246%, water at a total weight percent of greater than or equal to 10.604% and less than or equal to 11.607% and ammonium hydroxide at a total weight percent of greater than or equal to 0.112% and less than or equal to 0.122%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0097] In further embodiments of the method 200A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.17% and less than or equal to 44.25% and methanol at a weight percent of greater than or equal to 55.75% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 64.28% and less than or equal to 65.66%, water at a weight percent of greater than or equal to 33.98% and less than 34.65%, and ammonium hydroxide at a weight percent of about 0.36%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 13.821% and less than or equal to 16.915%, MTMS at a total weight percent of greater than or equal to 3.137% and less than or equal to 3.204%, methanol at a total weight percent of greater than or equal to 68.464% and less than or equal to 71.246%, water at a total weight percent of greater than or equal to 11.364% and less than or equal to 11.607% and ammonium hydroxide at a total weight percent of greater than or equal to 0.120% and less than or equal to 0.122%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0098] Further, in some embodiments of the method 200A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 62.82% and methanol at a weight percent of greater than or equal to 37. 18% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 54.96% and less than or equal to 64.99%, water at a weight percent of greater than or equal to 34.65% and less than or equal to 44.63%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.41%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weightpercent of about 89.17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 16.915% and less than or equal to 28.368%, MTMS at a total weight percent of greater than or equal to 2.63% and less than or equal to 3.137%, methanol at a total weight percent of greater than or equal to 55.244% and less than or equal to 68.464%, water at a total weight percent of greater than or equal to 10.604% and less than or equal to 13.633% and ammonium hydroxide at a total weight percent of greater than or equal to 0.112% and less than or equal to 0.125%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0099] In even further embodiments of the method 200A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 55. 11% and methanol at a weight percent of greater than or equal to 44.89% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 64.28% and less than or equal to 64.99%, water at a weight percent of greater than or equal to 34.65% and less than or equal to 35.35%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.37%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 16.915% and less than or equal to 23.676%, MTMS at a total weight percent of greater than or equal to 2.927% and less than or equal to 3.137%, methanol at a total weight percent of greater than or equal to 62.681% and less than or equal to 68.464%, water at a total weight percent of greater than or equal to 10.604% and less than or equal to 11.364% and ammonium hydroxide at a total weight percent of greater than or equal to 0.112% and less than or equal to 0. 120%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 200A

[0100] In some embodiments of the method 200A where TMOS is used as the first alkoxysilane and the second alkoxysilane is MTMS, the MTMS is provided in a controlled amount to provide a molar ratio of the TMOS:MTMS of greater than or equal to 3.86: 1 andless than or equal to 6. 11 : 1. In specific cases, the molar ratio is greater than or equal to 3.86: 1 and less than or equal to 5.79: 1, such as greater than or equal to 3.86: 1 and less than or equal to 4.83: 1. In further cases, the molar ratio is greater than or equal to 4.83: 1 and less than or equal to 6. 11 : 1, such as greater than or equal to 4.83:1 and less than or equal to 5.79: 1.

[0101] Also, in some embodiments, the TMOS has a total weight percent of greater than or equal to 13.82% and less than or equal to 30.937% and the MTMS has a total weight percent of greater than or equal to 3. 136% and less than or equal to 4.529%. In certain cases, the TMOS has a total weight percent of greater than or equal to 13.82% and less than or equal to 24.684% and the MTMS has a total weight percent of greater than or equal to 3.136% and less than or equal to 3.814%. In yet other cases, the TMOS has a total weight percent of greater than or equal to 13.82% and less than or equal to 16.914% and the MTMS has a total weight percent of greater than or equal to 3. 136% and less than or equal to 3.203%. In further cases, the TMOS has a total weight percent of greater than or equal to 16.914% and less than or equal to 30.937% and the MTMS has a total weight percent of greater than or equal to 3. 136% and less than or equal to 4.529%. In even further cases, the TMOS has a total weight percent of greater than or equal to 16.914% and less than or equal to 24.684% and the MTMS has a total weight percent of greater than or equal to 3.136% and less than or equal to 3.814%.

[0102] In some embodiments of the method 200A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 68.39% and methanol at a weight percent of greater than or equal to 31.61% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 56.38% and less than or equal to 65.65%, water at a weight percent of greater than or equal to 34.25% and less than or equal to 43.41%, and ammonium hydroxide at a weight percent of greater than or equal to 0.11% and less than or equal to 0.14%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than or equal to 15.41% and methanol at a weight percent of greater than or equal to 84.59% and less than or equal to 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 13.82% and less than or equal to 30.937%, MTMS at a total weight percent of greater than or equal to 3.136% and less than or equal to 4.529%, methanol at a total weight percent ofgreater than or equal to 53.471% and less than or equal to 71.24%. water at a total weight percent of greater than or equal to 11.028% and less than or equal to 11.7% and ammonium hydroxide at a total weight percent of greater than or equal to 0.035% and less than or equal to 0.037%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0103] In other embodiments of the method 200 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 58.38% and methanol at a weight percent of greater than or equal to 41.62% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 61. 14% and less than or equal to 65.65%, water at a weight percent of greater than or equal to 34.25% and less than or equal to 38.73%, and ammonium hydroxide at a weight percent of greater than or equal to 0.11% and less than or equal to 0.12%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than or equal to 13.18% and methanol at a weight percent of greater than or equal to 86.82% and less than or equal to 89. 17%. The resulting hydrophobic silica wet gel obtained by the method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 13.82% and less than or equal to 24.684%, MTMS at a total weight percent of greater than or equal to 3.136% and less than or equal to 3.814%, methanol at a total weight percent of greater than or equal to 60.322% and less than or equal to 71.24%, water at a total weight percent of greater than or equal to 11.145% and less than or equal to 11.7% and ammonium hydroxide at a total weight percent of greater than or equal to 0.035% and less than or equal to 0.037%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0104] In additional embodiments of the method 200 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 44.25% and methanol at a weight percent of greater than or equal to 55.75% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 64.97% and less than or equal to 65.65%, water at a weight percent of greater than or equal to 34.25% and less than or equal to 34.92%, and ammonium hydroxide at a weight percent of about 0.11%, and the third solution comprises MTMS at a weight percent of about 10.83% and methanol at a weight percent of about 89.17%. The resulting hydrophobic silica wet gelis thereby synthesized from TMOS at a total weight percent of greater than or equal to 13.82% and less than or equal to 16.914%, MTMS at a total weight percent of greater than or equal to 3.136% and less than or equal to 3.203%, methanol at a total weight percent of greater than or equal to 68.459% and less than or equal to 71.24%, water at a total weight percent of greater than or equal to 11.455% and less than or equal to 11.7% and ammonium hydroxide at a total weight percent of greater than or equal to 0.036% and less than or equal to 0.037%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0105] Further, in some embodiments of the method 200A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 68.39% and methanol at a weight percent of greater than or equal to 31.61% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 56.38% and less than or equal to 64.97%, water at a weight percent of greater than or equal to 34.92% and less than or equal to 43.41%, and ammonium hydroxide at a weight percent of greater than or equal to 0. 11 % and less than or equal to 0.14%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than or equal to 15.41% and methanol at a weight percent of greater than or equal to 84.59% and less than or equal to 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 16.914% and less than or equal to 30.937%, MTMS at a total weight percent of greater than or equal to 3.136% and less than or equal to 4.529%, methanol at atotal weight percent of greater than or equal to 53.471% and less than or equal to 68.459%, water at a total weight percent of greater than or equal to 11.028% and less than or equal to 11.455% and ammonium hydroxide at a total weight percent of greater than or equal to 0.035% and less than or equal to 0.036%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0106] In even further embodiments of the method 200A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 58.38% and methanol at a weight percent of greater than or equal to 41.62% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 61. 14% and less than or equal to 64.97%, water at a weight percent of greater than or equalto 34.92% and less than or equal to 38.73%, and ammonium hydroxide at a weight percent of greater than or equal to 0.11% and less than or equal to 0.12%, and the third solution comprises MTMS at a weight percent of greater than or equal to 10.83% and less than or equal to 13.18% and methanol at a weight percent of greater than or equal to 86.82% and less than or equal to 89. 17%. The resulting hydrophobic silica wet gel obtained by method 200A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 16.914% and less than or equal to 24.684%, MTMS at a total weight percent of greater than or equal to 3.136% and less than or equal to 3.814%, methanol at a total weight percent of greater than or equal to 60.322% and less than or equal to 68.459%, water at a total weight percent of greater than or equal to 11.145% and less than or equal to 11.455% and ammonium hydroxide at a total weight percent of greater than or equal to 0.35% and less than or equal to 0.36%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.

[0107] FIG. 3 illustrates a method 300 A according to certain embodiments. The method includes a step 305 of preparing a first solution by mixing a first alkoxy silane and solvent, a step 310 of preparing a second solution by mixing solvent, catalyst and water, a step 315 of mixing the first solution and the second solution together to form a mixed solution, a step 320 of allowing components in the mixed solution to react to form silica wet gel, a step 325 of aging the silica wet gel for a period of time, a step 330 of preparing a third solution by mixing a second alkoxysilane and diluent, a step 335 of adding the third solution to the silica wet gel after aging is complete, and a step 340 of allowing the third solution to react with the silica wet gel to form hydrophobic silica wet gel. In the method 300A, the step 335 of adding the third solution to the silica wet gel takes places after the aging step 325 is complete. The third solution serves as a hydrophobic agent. Therefore, the silica wet gel is aged completely before making it hydrophobic.Embodiments of Method 300A

[0108] In some embodiments of the method 300A, the first alkoxysilane is MS-51 and MTMS is used as the organo-silane. The MTMS is provided in a controlled amount to provide a molar ratio of the MS-51 :MTMS of greater than or equal to 0.95: 1 and less than or equal to 2.55: 1. In specific cases, the molar ratio is greater than or equal to 0.95: 1 and lessthan or equal to 2:1, such as greater than or equal to 0.95: 1 and less than or equal to 1.2: 1. In further cases, the molar ratio is greater than or equal to 1.2: 1 and less than or equal to 2.55: 1, such as greater than or equal to 1.2: 1 and less than or equal to 2: 1.

[0109] Also, in some cases, the MS-51 has a total weight percent of greater than or equal to 1.815% and less than or equal to 4.771% and the MTMS has a total weight percent of greater than or equal to 0.515% and less than or equal to 0.534%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 1.815% and less than or equal to 3.729% and the MTMS has a total weight percent of greater than or equal to 0.525% and less than or equal to 0.534%. In yet other cases, the MS-51 has a total weight percent of greater than or equal to 1.815% and less than or equal to 2.304% and the MTMS has a total weight percent of greater than equal to 0.533% and less than or equal to 0.534%. In further cases, the MS-51 has a total weight percent of greater than or equal to 2.304% and less than or equal to 4.771% and the MTMS has a total weight percent of greater than or equal to 0.515% and less than or equal to 0.533%. In even further cases, the MS-51 has a total weight percent of greater than or equal to 2.304% and less than or equal to 3.729% and the MTMS has a total weight percent of greater than or equal to 0.525% and less than or equal to 0.533%.

[0110] In some embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 55.56% and methanol at a weight percent of greater than or equal to 44.44% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 58.63% and less than or equal to 67.54%, water at a weight percent of greater than or equal to 32. 16% and less than or equal to 41%, and ammonium hydroxide at a weight percent of greater than or equal to 0.3% and less than or equal to 0.38%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.815% and less than or equal to 4.771%, MTMS at a total weight percent of greater than or equal to 0.515% and less than or equal to 0.534%, methanol at a total weight percent of greater than or equal to 92.021% and less than or equal to 95.695%, water at a total weight percent of greater than or equal to 1.9% and less than or equal to 2.668% and ammonium hydroxide at a total weight percent of greater than or equal to 0.018% and less than or equal to 0.025%. Theresulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.[OHl] In additional embodiments of the method 300 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 48.93% and methanol at a weight percent of greater than or equal to 51.06% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 66.94% and less than or equal to 67.54%, water at a weight percent of greater than or equal to 32. 16% and less than or equal to 32.76%, and ammonium hydroxide at a weight percent of about 0.3%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.815% and less than or equal to 3.729%, MTMS at atotal weight percent of greater than or equal to 0.525% and less than or equal to 0.534%, methanol at a total weight percent of greater than or equal to 93.823% and less than or equal to 95.695%, water at a total weight percent of greater than or equal to 1.905% and less than or equal to 1.938% and ammonium hydroxide at atotal weight percent of about 0.018%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0112] In specific embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 36.84% and methanol at a weight percent of greater than or equal to 63.16% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 66.94% and less than or equal to 67.54%, water at a weight percent of greater than or equal to 32. 16% and less than or equal to 32.76%, and ammonium hydroxide at a weight percent of about 0.3%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at atotal weight percent of greater than or equal to 1.815% and less than or equal to 2.304%, MTMS at atotal weight percent of greater than or equal to 0.533 and less than or equal to 0.534%, methanol at a total weight percent of greater than or equal to 95.213% and less than or equal to 95.695%, water at a total weight percent of greater than or equal to 1.932% and less than or equal 1.938 andammonium hydroxide at a total weight percent of about 0.018%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0113] Further, in some embodiments of the method 300 A, the first solution comprises MS- 51 at a weight percent of greater than or equal to 36.84% and less than or equal to 55.56% and methanol at a weight percent of greater than or equal to 44.44% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 58.63% and less than or equal to 66.94%, water at a weight percent of greater than or equal to 32.76% and less than or equal to 41%, and ammonium hydroxide at a weight percent of greater than or equal to 0.3% and less than or equal to 0.38%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.304% and less than or equal to 4.771%, MTMS at a total weight percent of greater than or equal to 0.515% and less than or equal to 0.533%, methanol at a total weight percent of greater than or equal to 92.021% and less than or equal to 95.213%, water at a total weight percent of greater than or equal to 1.932% and less than or equal to 2.668% and ammonium hydroxide at a total weight percent of greater than or equal to 0.018% and less than or equal to 0.025%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0114] In even further embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 36.84% and less than or equal to 48.93% and methanol at a weight percent of greater than or equal to 51.06% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of about 66.94%, water at a weight percent of about 32.76%, and ammonium hydroxide at a weight percent of about 0.3%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.304% and less than or equal to 3.729%, MTMS at a total weight percent of greater than or equal to 0.525% and less than or equal to 0.533%, methanol at a total weight percent of greater than or equal to 93.823% and less than or equal to 95.213%,water at a total weight percent of greater than or equal to 1.905% and less than or equal to 1.932% and ammonium hydroxide at a total weight percent of about 0.02%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 300A

[0115] In some embodiments where the first alkoxysilane is MS-51 and MTMS is used as the organo-silane, the MTMS is provided in a controlled amount to provide a molar ratio of the MS-5EMTMS of greater than or equal to .98: 1 and less than or equal to 1.43:1. In specific cases, the molar ratio is greater than or equal to .98: 1 and less than or equal to 1.29:1, such as greater than or equal to .98:1 and less than or equal to 1.25: 1. In further cases, the molar ratio is greater than or equal to 1.25 : 1 and less than or equal to 1.43: 1 , such as greater than or equal to 1.25: 1 and less than or equal to 1.29:1.

[0116] Also, in some cases, the MS-51 has a total weight percent of greater than or equal to 1.815% and less than or equal to 3.917% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.793%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 1.815% and less than or equal to 2.955% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.664%. In yet other cases, the MS-51 has a total weight percent of greater than or equal to 1.815% and less than or equal to 2.304% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.534%. In further cases, the MS- 51 has a total weight percent of greater than or equal to 2.304% and less than or equal to 3.917% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.793%. In even further cases, the MS-51 has a total weight percent of greater than or equal to 2.304% and less than or equal to 2.955% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.664%.

[0117] In some embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equalto 63.53% and less than or equal to 67.59%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.91% and methanol at a weight percent of greater than or equal to 99.39% and less than or equal to 99.09%. The resulting hydrophobic silica wet gel is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.815% and less than or equal to 3.917%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.793%, methanol at a total weight percent of greater than or equal to 93.354% and less than or equal to 95.694%, water at atotal weight percent of greater than or equal to 1.933% and less than or equal to 1.954% and ammonium hydroxide at a total weight percent of greater than or equal to 0.003% and less than or equal to 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0118] In additional embodiments of the method 300 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.37% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 67.59%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 34.64%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.76% and methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.815% and less than or equal to 2.955%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.664%, methanol at a total weight percent of greater than or equal to 94.434% and less than or equal to 95.694%, water at a total weight percent of greater than or equal to 1.94% and less than or equal to 1.954% and ammonium hydroxide at atotal weight percent of greater than or equal to 0.003% and less than or equal to 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0119] In specific embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 36.84% and methanol at a weight percent of greater than or equal to 63.16% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 66.92% and less than or equal to 67.59%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 33.03%, and ammonium hydroxide at a weight percent of about 0.04%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.815% and less than or equal to 2.304%, MTMS at atotal weight percent of greater than or equal to 0.533% and less than or equal to 0.534, methanol at a total weight percent of greater than or equal to 95.212% and less than or equal to 95.694%, water at a total weight percent of greater than or equal to 1.948% and less than or equal to 1.954% and ammonium hydroxide at a total weight percent of greater than or equal to 0.003% and less than or equal to 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0120] Further, in some embodiments of the method 300 A, the first solution comprises MS- 51 at a weight percent of greater than or equal to 36.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 63.13%, the second solution comprises methanol at a weight percent of greater than or equal to 63.53% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.91% and methanol at a weight percent of greater than or equal to 99.09% and less than or equal to 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.304% and less than or equal to 3.917%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.793%, methanol at a total weight percent of greater than or equal to 93.354% and less than or equal to 95.212%, water at a total weight percent of greater than or equal to 1.933% and less than or equal to 1.948% and ammonium hydroxide at a totalweight percent of greater than or equal to 0.003% and less than or equal to 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0121] In even further embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 36.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.37% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 34.64%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.76% and methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.304% and less than or equal to 2.955%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.664%, methanol at a total weight percent of greater than or equal to 94.434% and less than or equal to 95.212%, water at a total weight percent of greater than or equal to 1.944% and less than or equal to 1.948% and ammonium hydroxide at a total weight percent of greater than or equal to 0.003% and less than or equal to 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 300A

[0122] In additional embodiments where MS-51 is provided as the first alkoxysilane and MTMS is provided as the organo-silane, the MTMS is provided in a controlled amount to provide a molar ratio of the MS-51 :MTMS of greater than or equal to 1.31 : 1 and less than or equal to 1.72: 1. In specific cases, the molar ratio is greater than or equal to 1.31: 1 and less than or equal to 1.66: 1. In further cases, the molar ratio is greater than or equal to 1.61: 1 and less than or equal to 1.72: 1 , such as greater than or equal to 1.61: 1 and less than or equal to 1.66: 1.

[0123] Also, in some cases, the MS-51 has a total weight percent of greater than or equal to 1.817% and less than or equal to 3.922% and the MTMS has a total weight percent of greater than or equal to 0.400% and less than or equal to 0.661%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 1.817% and less than or equal to 2.959% and the MTMS has a total weight percent of greater than or equal to 0.400% and less than or equal to 0.532%. In yet other cases, the MS-51 has a total weight percent of greater than or equal to 1.817% and less than or equal to 2.307% and the MTMS has a total weight percent of greater than or equal to 0.400% and less than or equal to 0.401%. In further cases, the MS- 51 has a total weight percent of greater than or equal to 2.307% and less than or equal to 3.922% and the MTMS has a total weight percent of greater than or equal to 0.400% and less than or equal to 0.661%. In even further cases, the MS-51 has a total weight percent of greater than or equal to 2.307% and less than or equal to 2.959% and the MTMS has a total weight percent of greater than or equal to 0.400% and less than or equal to 0.532%.

[0124] In some embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 63.53% and less than or equal to 67.59%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.4016% and less than or equal to 0.76% and methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.54%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.817% and less than or equal to 3.922%, MTMS at a total weight percent of greater than or equal to 0.400% and less than or equal to 0.661%, methanol at a total weight percent of greater than or equal to 93.478% and less than or equal to 95.822%, water at a total weight percent of greater than or equal to 1.936% and less than or equal to 1.957% and ammonium hydroxide at a total weight percent of about 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0125] In additional embodiments of the method 300 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.37% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 67.59%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 34.64%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.4016% and less than or equal to 0.61% and methanol at a weight percent of greater than or equal to 99.39% and less than or equal to 99.54 %. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.817% and less than or equal to 2.959%, MTMS at a total weight percent of greater than or equal to 0.400% and less than or equal to 0.532%, methanol at a total weight percent of greater than or equal to 94.56% and less than or equal to 95.822%, water at a total weight percent of greater than or equal to 1.946% and less than or equal to 1.957% and ammonium hydroxide at a total weight percent of about 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0126] In specific embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 30.84% and less than or equal to 36.84% and methanol at a weight percent of greater than or equal to 63.16% and less than or equal to 69.16%, the second solution comprises methanol at a weight percent of greater than or equal to 66.92% and less than or equal to 67.59%, water at a weight percent of greater than or equal to 32.43% and less than or equal to 33.03%, and ammonium hydroxide at a weight percent of about 0.04%, and the third solution comprises MTMS at a weight percent of about 0.4016% and methanol at a weight percent of about 99.54%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.817% and less than or equal to 2.307%, MTMS at atotal weight percent of greater than or equal to 0.400% and less than or equal to 0.401%, methanol at a total weight percent of greater than or equal to 95.339% and less than or equal to 95.822%, water at a total weight percent of greater than or equal to 1.951 % and less than or equal to 1.957% and ammonium hydroxide at atotal weight percent of about 0.003%. The resultinghydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0127] Further, in some embodiments of the method 300 A, the first solution comprises MS- 51 at a weight percent of greater than or equal to 36.84% and less than or equal to 53.73% and methanol at a weight percent of greater than or equal to 46.27% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 63.53% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 36.42%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.4016% and less than or equal to 0.76% and methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.54%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.307% and less than or equal to 3.922%, MTMS at a total weight percent of greater than or equal to 0.400% and less than or equal to 0.661%, methanol at a total weight percent of greater than or equal to 93.478% and less than or equal to 95.339%, water at a total weight percent of greater than or equal to 1.936% and less than or equal to 1.951% and ammonium hydroxide at a total weight percent of about 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0128] In even further embodiments of the method 300A, the first solution comprises MS-51 at a weight percent of greater than or equal to 36.84% and less than or equal to 44.63% and methanol at a weight percent of greater than or equal to 55.37% and less than or equal to 63.16%, the second solution comprises methanol at a weight percent of greater than or equal to 65.31% and less than or equal to 66.92%, water at a weight percent of greater than or equal to 33.03% and less than or equal to 34.64%, and ammonium hydroxide at a weight percent of greater than or equal to 0.04% and less than or equal to 0.05%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.4016% and less than or equal to 0.61% and methanol at a weight percent of greater than or equal to 99.39% and less than or equal to 99.54%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.307% and less than or equal to 2.959%, MTMS at a total weight percent of greater than orequal to 0.400% and less than or equal to 0.532%, methanol at a total weight percent of greater than or equal to 94.560% and less than or equal to 95.339%, water at a total weight percent of greater than or equal to 1.946 and less than or equal to 1.951% and ammonium hydroxide at a total weight percent of about 0.003%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.

[0129] In other embodiments of the method 300 A, step 305 comprises prepanng a first solution by mixing TMOS and methanol, step 310 comprises preparing a second solution by mixing methanol, ammonium hydroxide and water, and step 330 comprises preparing a third solution by mixing an organo-silane and methanol. The organo-silane can be MTMS in some embodiments.Additional Embodiments of Method 300A

[0130] In some embodiments of the method 300A where TMOS is the first alkoxy silane and MTMS is the organo-silane, the MTMS is provided in a controlled amount to provide a molar ratio of the TMOS:MTMS of greater than or equal to 3.7: 1 and less than or equal to 9.2: 1. In specific cases, the molar ratio is greater than or equal to 3.7: 1 and less than or equal to 6.9: 1, such as greater than or equal to 3.7: 1 and less than or equal to 4.6:1. In further cases, the molar ratio is greater than or equal to 4.6: 1 and less than or equal to 9.2:1, such as greater than or equal to 4.6: 1 and less than or equal to 6.9: 1.

[0131] Also, in some cases, the TMOS has a total weight percent of greater than or equal to 2.308% and less than or equal to 5.643% and the MTMS has a total weight percent of greater than or equal to 0.523% and less than or equal to 0.535%. In certain cases, the TMOS has a total weight percent of greater than or equal to 2.308% and less than or equal to 4.27% and the MTMS has a total weight percent of greater than or equal to 0.528% and less than or equal to 0.535%. In yet other cases, the TMOS has a total weight percent of greater than or equal to 2.308% and less than or equal to 2.875% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.535%. In further cases, the TMOS has a total weight percent of greater than or equal to 2.875% and less than or equal to 5.643% and the MTMS has a total weight percent of greater than or equal to 0.523% and less than or equal to 0.533%. In even further cases, the TMOS has a total weight percent ofgreater than or equal to 2.875% and less than or equal to 4.27% and the MTMS has a total weight percent of greater than or equal to 0.528% and less than or equal to 0.533%.

[0132] In some embodiments of the method 300 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 67.87% and methanol at a weight percent of greater than or equal to 32.13% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 49.4% and less than or equal to 65.66%, water at a weight percent of greater than or equal to 33.98% and less than or equal to 50. 14%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.46%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.308% and less than or equal to 5.643%, MTMS at a total weight percent of greater than or equal to 0.523% and less than or equal to 0.535%, methanol at a total weight percent of greater than or equal to 91.097% and less than or equal to 95. 197%, water at a total weight percent of greater than or equal to 1.94% and less than or equal to 2.712% and ammonium hydroxide at a total weight percent of greater than or equal to 0.020% and less than or equal to 0.025%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0133] In additional embodiments of the method 300 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 55.11% and methanol at a weight percent of greater than or equal to 44.89% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 64.28% and less than or equal to 65.66%, water at a weight percent of greater than or equal to 33.98% and less than or equal to 35.35%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.37%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.308% and less than or equal to 4.27%, MTMS at a total weight percent of greater than or equal to 0.528% and less than or equal to 0.535%, methanol at a total weight percent of greater than orequal to 93.269% and less than or equal to 95.197%, water at a total weight percent of greater than or equal to 1.913% and less than or equal to 1.94% and ammonium hydroxide at a total weight percent of about 0.020%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0134] In specific embodiments of the method 300A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 44.25% and methanol at a weight percent of greater than or equal to 55.75% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 64.99% and less than or equal to 65.66%, water at a weight percent of greater than or equal to 33.98% and less than 34.65%, and ammonium hydroxide at a weight percent of about 0.36%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.308% and less than or equal to 2.875%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.535%, methanol at a total weight percent of greater than or equal to 94.639% and less than or equal to 95. 197%, water at a total weight percent of greater than or equal to 1.933% and less than or equal to 1.94% and ammonium hydroxide at a total weight percent of about 0.020%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0135] Further, in some embodiments of the method 300A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 67.87% and methanol at a weight percent of greater than or equal to 32. 13% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 49.4% and less than or equal to 64.99%, water at a weight percent of greater than or equal to 34.65% and less than or equal to 50. 14%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.46%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.875% and less than or equal to 5.643%, MTMS at a total weight percent of greater than orequal to 0.523% and less than or equal to 0.533%, methanol at a total weight percent of greater than or equal to 91.097% and less than or equal to 94.639%, water at a total weight percent of greater than or equal to 1.933% and less than or equal to 2.712% and ammonium hydroxide at a total weight percent of greater than or equal to 0.020% and less than or equal to 0.025%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0136] In even further embodiments of the method 300A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 55. 11% and methanol at a weight percent of greater than or equal to 44.89% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 64.28% and less than or equal to 64.99%, water at a weight percent of greater than or equal to 34.65% and less than or equal to 35.35%, and ammonium hydroxide at a weight percent of greater than or equal to 0.36% and less than or equal to 0.37%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.875% and less than or equal to 4.27%, MTMS at a total weight percent of greater than or equal to 0.528% and less than or equal to 0.533%, methanol at a total weight percent of greater than or equal to 93.269% and less than or equal to 94.639%, water at a total weight percent of greater than or equal to 1.913% and less than or equal to 1.933% and ammonium hydroxide at a total weight percent of about 0.020%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 300A

[0137] In additional embodiments where the first alkoxysilane is TMOS and the organo- silane is MTMS, the MTMS is provided in a controlled amount to provide a molar ratio of the TMOS:MTMS of greater than or equal to 3.86:1 and less than or equal to 6.11 : 1. In specific cases, the molar ratio is greater than or equal to 3.86: 1 and less than or equal to 5.79: 1, such as greater than or equal to 3.86:1 and less than or equal to 4.83: 1. In further cases, the molar ratio is greater than or equal to 4.83 : 1 and less than or equal to 6. 11 : 1 , such as greater than or equal to 4.83: 1 and less than or equal to 5.79: 1.

[0138] Also, in some cases, the TMOS has a total weight percent of greater than or equal to 2.308% and less than or equal to 5.427% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.795%. In certain cases, the TMOS has a total weight percent of greater than or equal to 2.308% and less than or equal to 4.293% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.663%. In yet other cases, the TMOS has a total weight percent of greater than or equal to 2.308% and less than or equal to 2.875% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.535%. In further cases, the TMOS has a total weight percent of greater than or equal to 2.875% and less than or equal to 5.427% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.795%. In even further cases, the TMOS has a total weight percent of greater than or equal to 2.875% and less than or equal to 4.293% and the MTMS has a total weight percent of greater than or equal to 0.533% and less than or equal to 0.663%.

[0139] In some embodiments of the method 300 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 68.39% and methanol at a weight percent of greater than or equal to 31.61% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 56.38% and less than or equal to 65.65%, water at a weight percent of greater than or equal to 34.25% and less than or equal to 43.48%, and ammonium hydroxide at a weight percent of greater than or equal to 0.11 % and less than or equal to 0. 14%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.91% and methanol at a weight percent of greater than or equal to 99.09% and less than or equal to 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.308% and less than or equal to 5.427%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.795%, methanol at a total weight percent of greater than or equal to 91.838% and less than or equal to 95.196%, water at a total weight percent of greater than or equal to 1.934% and less than or equal to 1.955% and ammonium hydroxide at a total weight percent of about 0.006%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0140] In additional embodiments of the method 300 A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 58.38% and methanol at a weight percent of greater than or equal to 41.66% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 61.15% and less than or equal to 65.65%, water at a weight percent of greater than or equal to 34.25% and less than or equal to 38.73%, and ammonium hydroxide at a weight percent of greater than or equal to 0.11 % and less than or equal to 0. 12%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.76% and methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.308% and less than or equal to 4.293%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.663%, methanol at a total weight percent of greater than or equal to 93. 1% and less than or equal to 95. 196%, water at a total weight percent of greater than or equal to 1.938% and less than or equal to 1.955% and ammonium hydroxide at a total weight percent of about 0.006%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0141] In specific embodiments of the method 300A, the first solution comprises TMOS at a weight percent of greater than or equal to 38.13% and less than or equal to 44.25% and methanol at a weight percent of greater than or equal to 55.75% and less than or equal to 61.87%, the second solution comprises methanol at a weight percent of greater than or equal to 64.97% and less than or equal to 65.65%, water at a weight percent of greater than or equal to 34.25% and less than or equal to 34.92%, and ammonium hydroxide at a weight percent of about 0.11%, and the third solution comprises MTMS at a weight percent of about 0.61% and methanol at a weight percent of about 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.308% and less than or equal to 2.875%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.535%, methanol at a total weight percent of greater than or equal to 94.638% and less than or equal to 95. 196%, water at a total weight percent of greater than or equal to 1.948 and less than or equal to 1.955% and ammonium hydroxide at a total weight percent of about 0.006%. The resultinghydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0142] Further, in some embodiments of the method 300A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 68.39% and methanol at a weight percent of greater than or equal to 31.61% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 56.38% and less than or equal to 64.97%, water at a weight percent of greater than or equal to 34.92% and less than or equal to 43.48%, and ammonium hydroxide at a weight percent of greater than or equal to 0. 11 % and less than or equal to 0.14%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.91% and methanol at a weight percent of greater than or equal to 99.09% and less than or equal to 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.875% and less than or equal to 5.427%, MTMS at a total weight percent of greater than or equal to 0.533% and less than or equal to 0.795%, methanol at a total weight percent of greater than or equal to 91.838% and less than or equal to 94.638%, water at a total weight percent of greater than or equal to 1.934% and less than or equal to 1.948% and ammonium hydroxide at a total weight percent of about 0.006%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0143] In even further embodiments of the method 300A, the first solution comprises TMOS at a weight percent of greater than or equal to 44.25% and less than or equal to 58.38% and methanol at a weight percent of greater than or equal to 41.66% and less than or equal to 55.75%, the second solution comprises methanol at a weight percent of greater than or equal to 61.15% and less than or equal to 64.97%, water at a weight percent of greater than or equal to 34.92% and less than or equal to 38.73%, and ammonium hydroxide at a weight percent of greater than or equal to 0.11 % and less than or equal to 0. 12%, and the third solution comprises MTMS at a weight percent of greater than or equal to 0.61% and less than or equal to 0.76% and methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.39%. The resulting hydrophobic silica wet gel obtained by the method 300A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.875% and less than or equal to 4.293%, MTMS at a total weight percent of greater than or equal to0.533% and less than or equal to 0.663%, methanol at a total weight percent of greater than or equal to 93.1% and less than or equal to 94.638%, water at a total weight percent of greater than or equal to 1.938% and less than or equal to 1.948% and ammonium hydroxide at a total weight percent of about 0.006%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.

[0144] In the method of 200A, the step 235 of adding the third solution to the silica wet gel occurs before aging is complete. In the method of 300A, the step 335 of adding the third solution to the silica wet gel occurs after aging is complete. The aging step includes keeping the silica wet gel (or hydrophobic silica wet gel) in an airtight environment for a selected period of time. Applicant has found that the aging process allows structural transformations to occur in the three-dimensional polymer structure of the silica wet gel (or hydrophobic silica wet gel) that enhance the mechanical strength of the structure. One exemplary significant structural transformation that takes place during aging is a decrease in spherical silica particle diameter. Another exemplary structural transformation is a decrease in pore size. Pore size is a size of pore spaces between spherical silica particles. Pore sizes are often recorded in terms of average pore size. Another exemplary structural transformation is a strengthening of the necking point between two spherical silica particles. The necking point is the point where two adjacent spherical silica particles adjoin.

[0145] FIG. 5 illustrates a method 400 A according to certain embodiments. The method includes a step 405 of preparing a first solution by mixing a first alkoxysilane and solvent, a step 410 of preparing a second solution by mixing solvent, catalyst and water, a step 415 of mixing the first solution and the second solution together to form a mixed solution, a step 420 of allowing components in the mixed solution to react to form silica wet gel, a step 425 of aging the silica wet gel for a period of time, a step 430 of preparing a third solution by mixing catalyst and solvent, a step 435 of preparing a fourth solution by mixing a second alkoxy silane and diluent, a step 440 of preparing a solvent exchange solution by mixing the third solution, the fourth solution and solvent, and a step 445 of subjecting the silica wet gel to the solvent extraction solution to form hydrophobic silica wet gel. In the method 400A, the solvent exchange solution serves as a hydrophobic agent.

[0146] In certain cases, step 405 comprises preparing the first solution by mixing a first alkoxysilane and methanol, step 410 comprises preparing a second solution by mixing methanol, ammonium hydroxide and water, step 430 comprises preparing a third solution by mixing ammonium hydroxide and methanol, step 435 comprises preparing a fourth solution by mixing a second alkoxysilane and methanol and step 440 comprises preparing a solvent exchange solution by mixing the third solution, the fourth solution and methanol. In method 200A, hydrophobic treatment through the solvent exchange solution is performed after the silica wet gel aging is complete.Embodiments of Method 400A

[0147] In some embodiments of the method 400A, the first alkoxy silane is MS-51 and the second alkoxysilane is MTMS. In some cases, the MTMS is provided in a controlled amount to provide a molar ratio of the MS-51 :MTMS of greater than or equal to 1 : 1 and less than or equal to 1.43: 1. In specific cases, the molar ratio is greater than or equal to 1: 1 and less than or equal to 1.29 : 1 , such as greater than or equal to 0.95 : 1 and less than or equal to 1.25 : 1. In further cases, the molar ratio is greater than or equal to 1.25:1 and less than or equal to 1.43: 1, such as greater than or equal to 1.25: 1 and less than or equal to 1.29:1.

[0148] Also, in some cases, the MS-51 has a total weight percent of greater than or equal to 1.811% and less than or equal to 3.909% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.791%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 1.811% and less than or equal to 2.949% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.663%. In yet other cases, the MS-51 has a total weight percent of greater than or equal to 1.811% and less than or equal to 2.302% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.533%. In further cases, the MS-51 has a total weight percent of greater than or equal to 2.302% and less than or equal to 3.909% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.791%. In even further cases, the MS-51 has a total weight percent of greater than or equal to 2.302% and less than or equal to 2.949%, and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.663%.

[0149] In some embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 18.23% and less than or equal to 36.74% and methanol at a weight percent of greater than or equal to 63.26% and less than or equal to 81.77%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 15.24% and less than or equal to 31.1%, methanol at a weight percent of greater than or equal to 53.54% and less than or equal to 68.33%, water at a weight percent of greater than or equal to 15.35% and less than or equal to 16.41% and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 26.7% and methanol at a weight percent of greater than or equal to 73.3% and less than or equal to 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.9%, methanol at a weight percent of greater than or equal to 99.09% and less than or equal to 99.39% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.811% and less than or equal to 3.909%, MTMS at a total weight percent of greater than or equal to 0.532% and less than or equal to 0.791%, methanol at a total weight percent of greater than or equal to 93.36% and less than or equal to 95.695%, water at a total weight percent of greater than or equal to 1.93% and less than or equal to 1.951% and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0150] In other embodiments of the method 400 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 18.23% and less than or equal to 28.73% and methanol at a weight percent of greater than or equal to 71.27% and less than or equal to 81.77%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greaterthan or equal to 15.24% and less than or equal to 24.15%, methanol at a weight percent of greater than or equal to 59.93% and less than or equal to 68.33%, water at a weight percent of greater than or equal to 15.9% and less than or equal to 16.41% and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 23.28% and methanol at a weight percent of greater than or equal to 76.72% and less than or equal to 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.76%, methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.39% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.811% and less than or equal to 2.949%, MTMS at a total weight percent of greater than or equal to 0.52% and less than or equal to 0.663%, methanol at a total weight percent of greater than or equal to 94.438% and less than or equal to 95.695%, water at a total weight percent of greater than or equal to 1.94% and less than or equal to 1.951% and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0151] In further embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 18.23% and less than or equal to 22.83% and methanol at a weight percent of greater than or equal to 77.17% and less than or equal to 81.77%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 15.24% and less than or equal to 19.13%, methanol at a weight percent of greater than or equal to 64.66% and less than or equal to 68.33%, water at a weight percent of greater than or equal to 16. 19% and less than or equal to 16.41% and ammonium hy droxide at a weight percent of about 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of about 19.54% andmethanol at a weight percent of about 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of about 0.6%, methanol at a weight percent of about 99.39% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.811% and less than or equal to 2.302%, MTMS at a total weight percent of about 0.532%, methanol at a total weight percent of greater than or equal to 95.209% and less than or equal to 95.695%, water at a total weight percent of about greater than or equal to 1.947% and less than or equal to 1.951% and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0152] Additionally, in some embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 22.83% and less than or equal to 36.74% and methanol at a weight percent of greater than or equal to 63.26% and less than or equal to 77.17%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 19.13% and less than or equal to 31.1%, methanol at a weight percent of greater than or equal to 53.54% and less than or equal to 64.66%, water at a weight percent of greater than or equal to 15.35% and less than or equal to 16.19% and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 26.7% and methanol at a weight percent of greater than or equal to 73.3% and less than or equal to 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.9%, methanol at a weight percent of greater than or equal to 99.09% and less than or equal to 99.39% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.302% and less than or equal to 3.909%, MTMS at a totalweight percent of greater than or equal to 0.532% and less than or equal to 0.791%, methanol at a total weight percent of greater than or equal to 93.36% and less than or equal to 95.209%, water at a total weight percent of greater than or equal to 1.93% and less than or equal to 1.947% and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0153] In further embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 22.83% and less than or equal to 28.73% and methanol at a weight percent of greater than or equal to 71.27% and less than or equal to 77.17%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 19.13% and less than or equal to 24.15%, methanol at a weight percent of greater than or equal to 59.93% and less than or equal to 64.66%, water at a weight percent of greater than or equal to 15.9% and less than or equal to 16. 19% and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 23.28% and methanol at a weight percent of greater than or equal to 76.72% and less than or equal to 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.76%, methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.39% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.302% and less than or equal to 2.949%, MTMS at a total weight percent of greater than or equal to 0.532% and less than or equal to 0.663%, methanol at a total weight percent of greater than or equal to 94.438% and less than or equal to 95.209%, water at a total weight percent of greater than or equal to 1.94% and less than or equal to 1.947% and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 400A

[0154] In some embodiments of the method 400A, the first alkoxy silane is MS-51 and MTES is used as the second alkoxysilane. In some cases, the MTES is provided in a controlled amount to provide a molar ratio of the MS -51 : MTES of greater than or equal to 1 : 1.82 and less than or equal to 1: 1. In specific cases, the molar ratio is greater than or equal to 1:1.82 and less than or equal to 1 : 1.22, such as greater than or equal to 1 : 1.82 and less than or equal to 1 : 1.43. In further cases, the molar ratio is greater than or equal to 1 : 1.43 and less than or equal to 1: 1, such as greater than or equal to 1: 1.43 and less than or equal to 1: 1.22.

[0155] Also, in some cases, the MS-51 has a total weight percent of greater than or equal to 1.798% and less than or equal to 3.882% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.472%. In certain cases, the MS-51 has a total weight percent of greater than or equal to 1.798% and less than or equal to 2.928% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.357%. In yet other cases, the MS-51 has a total weight percent of greater than or equal to 1.798% and less than or equal to 2.285% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.24%. In further cases, the MS-51 has a total weight percent of greater than or equal to 2.285% and less than or equal to 3.882% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.472%. In even further cases, the MS-51 has a total weight percent of greater than or equal to 2.285% and less than or equal to 2.928% and the MTMS has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.357%.

[0156] In some embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 18.23% and less than or equal to 36.74% and methanol at a weight percent of greater than or equal to 63.26% and less than or equal to 81.77%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 15.24% and less than or equal to 31.1%, methanol at a weight percent of greater than or equal to 53.54% and less than or equal to 68.33%, water at a weight percent ofgreater than or equal to 15.35% and less than or equal to 16.41% and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 40.57% and methanol at a weight percent of greater than or equal to 59.43% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.68%, methanol at a weight percent of greater than or equal to 98.31% and less than or equal to 98.59% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.798% and less than or equal to 3.882%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.472%, methanol at a total weight percent of greater than or equal to 92.719% and less than or equal to 95.014%, water at a total weight percent of greater than or equal to 1.917% and less than or equal to 1.938% and ammonium hydroxide at atotal weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0157] In other embodiments of the method 400 A, the first solution comprises MS-51 at a weight percent of greater than or equal to 18.23% and less than or equal to 28.73% and methanol at a weight percent of greater than or equal to 71.27% and less than or equal to 81.77%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 15.24% and less than or equal to 24.15%, methanol at a weight percent of greater than or equal to 59.93% and less than or equal to 68.33%, water at a weight percent of greater than or equal to 15.9% and less than or equal to 16.41% and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 38.49% andmethanol at a weight percent of greater than or equal to 61.51% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.54%, methanol at a weight percent of greater than or equal to 98.45% and less than or equal to 98.59% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 1.798% and less than or equal to 2.928%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.357%, methanol at a total weight percent of greater than or equal to 93.777% and less than or equal to 95.014%, water at a total weight percent of greater than or equal to 1.928% and less than or equal to 1.938%, and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0158] In further embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 18.23% and less than or equal to 22.83% and methanol at a weight percent of greater than or equal to 77.17% and less than or equal to 81.77%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 15.24% and less than or equal to 19.13%, methanol at a weight percent of greater than or equal to 64.66% and less than or equal to 68.33%, water at a weight percent of greater than or equal to 16. 19% and less than or equal to 16.41% and ammonium hydroxide at a weight percent of about 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of about 36.26% and methanol at a weight percent of about 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of about 1.41%, methanol at a weight percent of about 98.59% and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at atotal weight percent of greater than or equal to 1.798% and less than or equal to 2.285%, MTES at atotal weight percent of greater than or equal to 1.238% and less than or equal to 1.24%, methanolat a total weight percent of greater than or equal to 94.533% and less than or equal to 95.014%, water at a total weight percent of greater than or equal to 1.934% and less than or equal to 1.938%, and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0159] Additionally, in some embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 22.83% and less than or equal to 36.74% and methanol at a weight percent of greater than or equal to 63.26% and less than or equal to 77.17%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 19.13% and less than or equal to 31.1%, methanol at a weight percent of greater than or equal to 53.54% and less than or equal to 64.66%, water at a weight percent of greater than or equal to 15.35% and less than or equal to 16.19%, and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 40.57% and methanol at a weight percent of greater than or equal to 59.43% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.68%, methanol at a weight percent of greater than or equal to 98.31% and less than or equal to 98.59%, and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.285% and less than or equal to 3.882%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.472%, methanol at a total weight percent of greater than or equal to 92.719% and less than or equal to 94.533%, water at a total weight percent of greater than or equal to 1.917% and less than or equal to 1.934%, and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0160] In further embodiments of the method 400A, the first solution comprises MS-51 at a weight percent of greater than or equal to 22.83% and less than or equal to 28.73% and methanol at a weight percent of greater than or equal to 71.27% and less than or equal to 77.17%, and the second solution comprises water at a weight percent of about 99.86% and ammonium hydroxide at a weight percent of about 0. 14%. The first solution and the second solution therefore form a mixed solution that comprises MS-51 at a weight percent of greater than or equal to 19.13% and less than or equal to 24.15%, methanol at a weight percent of greater than or equal to 59.93% and less than or equal to 64.66%, water at a weight percent of greater than or equal to 15.9% and less than or equal to 16. 19% and ammonium hydroxide at a weight percent of greater than or equal to 0.02% and less than or equal to 0.022%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 38.49% and methanol at a weight percent of greater than or equal to 61.51% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.54%, methanol at a weight percent of greater than or equal to 98.45% and less than or equal to 98.59%, and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from MS-51 at a total weight percent of greater than or equal to 2.285% and less than or equal to 2.928%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.357%, methanol at a total weight percent of greater than or equal to 93.777% and less than or equal to 94.533%, water at a total weight percent of greater than or equal to 1.928% and less than or equal to 1.934% and ammonium hydroxide at a total weight percent of about 0.01%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 400A

[0161] In other embodiments of the method 400 A, TMOS is used as the first alkoxy silane and the second alkoxysilane is MTMS. In some cases, the MTMS is provided in a controlled amount to provide a molar ratio of the TMOS:MTMS of greater than or equal to 3.86: 1 andless than or equal to 6. 11 : 1. In specific cases, the molar ratio is greater than or equal to 3.86: 1 and less than or equal to 5.79: 1, such as greater than or equal to 3.86: 1 and less than or equal to 4.83: 1. In further cases, the molar ratio is greater than or equal to 4.83: 1 and less than or equal to 6. 11 : 1, such as greater than or equal to 4.83:1 and less than or equal to 5.79: 1.

[0162] Also, in some cases, the TMOS has a total weight percent of greater than or equal to 2.304% and less than or equal to 5.416% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.793%. In certain cases, the TMOS has a total weight percent of greater than or equal to 2.304% and less than or equal to 4.284% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.662%. In yet other cases, the TMOS has a total weight percent of greater than or equal to 2.304% and less than or equal to 2.869% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.534%. In further cases, the TMOS has a total weight percent of greater than or equal to 2.869% and less than or equal to 5.416% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.793%. In even further cases, the TMOS has a total weight percent of greater than or equal to 2.869% and less than or equal to 4.284% and the MTMS has a total weight percent of greater than or equal to 0.532% and less than or equal to 0.662%.

[0163] In some embodiments of the method 400 A, the first solution comprises TMOS at a weight percent of greater than or equal to 23.55% and less than or equal to 51.96% and methanol at a weight percent of greater than or equal to 48.04% and less than or equal to 76.45%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 19.63% and less than or equal to 43.82%, methanol at a weight percent of greater than or equal to 40.51% and less than or equal to 63.7%, water at a weight percent of greater than or equal to 15.62% and less than or equal to 16.62%, and ammonium hydroxide at a weight percent of about 0.05%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 26.7% and methanol at a weight percent of greater than or equal to 73.3% and less than or equal to 80.46%. The third solution and the fourth solutionare combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.9%, methanol at a weight percent of greater than or equal to 99.09% and less than or equal to 99.39%, and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.304% and less than or equal to 5.416%, MTMS at a total weight percent of greater than or equal to 0.532% and less than or equal to 0.793%, methanol at a total weight percent of greater than or equal to 91.847% and less than or equal to 95.198%, water at atotal weight percent of greater than or equal to 1.930% and less than or equal to 1.95%, and ammonium hydroxide at a total weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0164] In other embodiments of the method 400 A, the first solution comprises TMOS at a weight percent of greater than or equal to 23.55% and less than or equal to 41.23% and methanol at a weight percent of greater than or equal to 58.77% and less than or equal to 76.45%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 19.63% and less than or equal to 34.74%, methanol at a weight percent of greater than or equal to 49.52% and less than or equal to 63.7%, water at a weight percent of greater than or equal to 15.69% and less than or equal to 16.62%, and ammonium hydroxide at a weight percent of about 0.05%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 23.28% and methanol at a weight percent of greater than or equal to 76.72% and less than or equal to 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.76%, methanol at a weight percent of greater than or equal to 99.23% and less than or equal to 99.39%, and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.304% and less than or equal to 4.284%,MTMS at a total weight percent of greater than or equal to 0.532% and less than or equal to 0.662%, methanol at a total weight percent of greater than or equal to 93.106% and less than or equal to 95.198%, water at a total weight percent of greater than or equal to 1.934% and less than or equal to 1.95%, and ammonium hydroxide at a total weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0165] In further embodiments of the method 400A, the first solution comprises TMOS at a weight percent of greater than or equal to 23.55% and less than or equal to 28.41% and methanol at a weight percent of greater than or equal to 71.59% and less than or equal to 76.45%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 19.63% and less than or equal to 23.81%, methanol at a weight percent of greater than or equal to 6% and less than or equal to 63.7%, water at a weight percent of greater than or equal to 16. 13% and less than or equal to 16.62%, and ammonium hydroxide at a weight percent of about 0.05%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of about 19.54% and methanol at a weight percent of about 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of about 0.6%, methanol at a weight percent of about 99.39%, and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.304% and less than or equal to 2.869%, MTMS at a total weight percent of greater than or equal to 0.532% and less than or equal to 0.534%, methanol at a total weight percent of greater than or equal to 94.642% and less than or equal to 95.198%, water at a total weight percent of greater than or equal to 1.943% and less than or equal to 1.95%, and ammonium hydroxide at atotal weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0166] Additionally, in some embodiments of the method 400A, the first solution comprises TMOS at a weight percent of greater than or equal to 28.41% and less than or equal to 51.96% and methanol at a weight percent of greater than or equal to 48.04% and less than or equal to 71.59%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 23.81% and less than or equal to 43.82%, methanol at a weight percent of greater than or equal to 40.51 % and less than or equal to 60%, water at a weight percent of greater than or equal to 15.62% and less than or equal to 16.13%, and ammonium hydroxide at a weight percent of about 0.05%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 26.7% and methanol at a weight percent of greater than or equal to 73.3% and less than or equal to 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.9%, methanol at a weight percent of greater than or equal to 99.09% and less than or equal to 99.39%, and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.869% and less than or equal to 5.416%, MTMS at a total weight percent of greater than or equal to 0.532% and less than or equal to 0.793%, methanol at a total weight percent of greater than or equal to 91.847% and less than or equal to 94.642%, water at atotal weight percent of greater than or equal to 1.930% and less than or equal to 1.943%, and ammonium hydroxide at a total weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0167] In further embodiments of the method 400A, the first solution comprises TMOS at a weight percent of greater than or equal to 28.41% and less than or equal to 41.23% and methanol at a weight percent of greater than or equal to 58.77% and less than or equal to 71.59%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greaterthan or equal to 23.81% and less than or equal to 34.74%, methanol at a weight percent of greater than or equal to 49.52% and less than or equal to 60%, water at a weight percent of greater than or equal to 15.69% and less than or equal to 16. 13%, and ammonium hydroxide at a weight percent of about 0.05%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTMS at a weight percent of greater than or equal to 19.54% and less than or equal to 23.28% and methanol at a weight percent of greater than or equal to 76.72% and less than or equal to 80.46%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTMS at a weight percent of greater than or equal to 0.6% and less than or equal to 0.76%, methanol at a weight percent of greater than or equal to 99.24% and less than or equal to 99.39%, and ammonium hydroxide at a weight percent of about 0.01%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.869% and less than or equal to 4.284%, MTMS at a total weight percent of greater than or equal to 0.532% and less than or equal to 0.662%, methanol at a total weight percent of greater than or equal to 93.106% and less than or equal to 94.642%, water at atotal weight percent of greater than or equal to 1.934% and less than or equal to 1.943%, and ammonium hydroxide at atotal weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.Additional Embodiments of Method 400A

[0168] In additional embodiments of the method 400A, TMOS is used as the first alkoxysilane and MTES is used as the second alkoxysilane. In some cases, the MTES is provided in a controlled amount to provide a molar ratio of the TMOS:MTES of greater than or equal to 2.16: 1 and less than or equal to 4.3:1. In specific cases, the molar ratio is greater than or equal to 2.16: 1 and less than or equal to 3.68: 1, such as greater than or equal to 2. 16: 1 and less than or equal to 2.7 : 1. In further cases, the molar ratio is greater than or equal to 2.7: 1 and less than or equal to 4.3: 1, such as greater than or equal to 2.7: 1 and less than or equal to 3.68: 1.

[0169] Also, in some cases, the TMOS has a total weight percent of greater than or equal to 2.287% and less than or equal to 5.379% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.476%. In certain cases, the TMOS has a total weight percent of greater than or equal to 2.287% and less than or equal to 4.254% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.355%. In yet other cases, the TMOS has a total weight percent of greater than or equal to 2.287% and less than or equal to 2.849% and the MTMS has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.242%. In further cases, the TMOS has a total weight percent of greater than or equal to 2.849% and less than or equal to 5.379% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.476%. In even further cases, the TMOS has a total weight percent of greater than or equal to 2.849% and less than or equal to 4.254% and the MTES has a total weight percent of greater than or equal to 1.238% and less than or equal to 1.355%.

[0170] In some embodiments of the method 400 A, the first solution comprises TMOS at a weight percent of greater than or equal to 23.55% and less than or equal to 51.96% and methanol at a weight percent of greater than or equal to 48.04% and less than or equal to 76.45%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 19.63% and less than or equal to 43.82%, methanol at a weight percent of greater than or equal to 40.51% and less than or equal to 63.7%, water at a weight percent of greater than or equal to 15.62% and less than or equal to 16.62%, and ammonium hydroxide at a weight percent of greater than or equal to 0.05% and less than or equal to 0.052. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 40.57% and methanol at a weight percent of greater than or equal to 59.43% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.68%, methanol at a weight percent of greater than or equal to 98.31% and less than or equal to 98.59%, and ammonium hydroxide at a weight percent of about 0.014%. The resulting hydrophobic silica wet gel obtained by themethod 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.287% and less than or equal to 5.379%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.476%, methanol at a total weight percent of greater than or equal to 91.214% and less than or equal to 94.521%, water at a total weight percent of greater than or equal to 1.917% and less than or equal to 1.936%, and ammonium hydroxide at a total weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 200 mg / cc.

[0171] In other embodiments of the method 400 A, the first solution comprises TMOS at a weight percent of greater than or equal to 23.55% and less than or equal to 41.23% and methanol at a weight percent of greater than or equal to 58.77% and less than or equal to 76.45%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 19.63% and less than or equal to 34.74%, methanol at a weight percent of greater than or equal to 49.52% and less than or equal to 63.7%, water at a weight percent of greater than or equal to 15.68% and less than or equal to 16.62%, and ammonium hydroxide at a weight percent of greater than or equal to 0.05% and less than or equal to 0.052%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 38.49% and methanol at a weight percent of greater than or equal to 61.51% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.54%, methanol at a weight percent of greater than or equal to 98.45% and less than or equal to 98.59%, and ammonium hydroxide at a weight percent of about 0.014%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.287% and less than or equal to 4.254%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.355%, methanol at a total weight percent of greater than or equal to 92.457% and less than or equal to 94.521%, water at a total weight percent of greater than or equal to 1.92% and less than or equal to 1.936%, and ammonium hydroxide at a total weight percent of about 0.014%. The resultinghydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 150 mg / cc.

[0172] In further embodiments of the method 400A, the first solution comprises TMOS at a weight percent of greater than or equal to 23.55% and less than or equal to 28.71% and methanol at a weight percent of greater than or equal to 71.59% and less than or equal to 76.45%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 19.63% and less than or equal to 23.81%, methanol at a weight percent of greater than or equal to 60.014% and less than or equal to 63.7%, water at a weight percent of greater than or equal to 16. 13% and less than or equal to 16.62%, and ammonium hydroxide at a weight percent of greater than or equal to 0.05% and less than or equal to 0.052%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of about 36.26% and methanol at a weight percent of about 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of about 1.41%, methanol at a weight percent of about 98.59%, and ammonium hydroxide at a weight percent of about 0.014%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.287% and less than or equal to 2.849%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.242%, methanol at a total weight percent of greater than or equal to 93.97% and less than or equal to 94.521%, water at a total weight percent of greater than or equal to 1.929% and less than or equal to 1.936%, and ammonium hydroxide at a total weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 100 mg / cc and less than or equal to 120 mg / cc.

[0173] Additionally, in some embodiments of the method 400A, the first solution comprises TMOS at a weight percent of greater than or equal to 28.71% and less than or equal to 51.96% and methanol at a weight percent of greater than or equal to 48.04% and less than or equal to 71.59%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution andthe second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 23.81% and less than or equal to 43.82%, methanol at a weight percent of greater than or equal to 40.51% and less than or equal to 60.01%, water at a weight percent of greater than or equal to 15.62% and less than or equal to 16.13%, and ammonium hydroxide at a weight percent of about 0.05%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about 96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 40.57% and methanol at a weight percent of greater than or equal to 59.43% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.68%, methanol at a weight percent of greater than or equal to 98.31% and less than or equal to 98.59%, and ammonium hydroxide at a weight percent of about 0.014%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.849% and less than or equal to 5.379%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.476%, methanol at a total weight percent of greater than or equal to 91.214% and less than or equal to 93.97%, water at a total weight percent of greater than or equal to 1.917% and less than or equal to 1.929%, and ammonium hydroxide at a total weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 200 mg / cc.

[0174] In further embodiments of the method 400A, the first solution comprises TMOS at a weight percent of greater than or equal to 28.71% and less than or equal to 41.23% and methanol at a weight percent of greater than or equal to 58.77% and less than or equal to 71.59%, and the second solution comprises water at a weight percent of about 99.69% and ammonium hydroxide at a weight percent of about 0.31%. The first solution and the second solution therefore form a mixed solution that comprises TMOS at a weight percent of greater than or equal to 23.81% and less than or equal to 34.74%, methanol at a weight percent of greater than or equal to 49.52% and less than or equal to 60.01%, water at a weight percent of greater than or equal to 15.68% and less than or equal to 16. 13%, and ammonium hydroxide at a weight percent of about 0.05%. Further, the third solution comprises ammonium hydroxide at a weight percent of about 3.71% and methanol at a weight percent of about96.29%, and the fourth solution comprises MTES at a weight percent of greater than or equal to 36.26% and less than or equal to 38.49% and methanol at a weight percent of greater than or equal to 61.51% and less than or equal to 63.74%. The third solution and the fourth solution are combined with additional methanol to form the solvent exchange solution, which comprises MTES at a weight percent of greater than or equal to 1.41% and less than or equal to 1.54%, methanol at a weight percent of greater than or equal to 98.45% and less than or equal to 98.59%, and ammonium hydroxide at a weight percent of about 0.014%. The resulting hydrophobic silica wet gel obtained by the method 400A is thereby synthesized from TMOS at a total weight percent of greater than or equal to 2.849% and less than or equal to 4.254%, MTES at a total weight percent of greater than or equal to 1.238% and less than or equal to 1.355%, methanol at a total weight percent of greater than or equal to 92.457% and less than or equal to 93.97%, water at a total weight percent of greater than or equal to 1.92% and less than or equal to 1.929%, and ammonium hydroxide at a total weight percent of about 0.014%. The resulting hydrophobic silica wet gel also has a density of greater than or equal to 120 mg / cc and less than or equal to 150 mg / cc.

[0175] In each of the embodiments discussed herein, the selected time period for aging is a time period in which the aging process reaches saturation. Once saturation has occurred, no further structural transformation of the wet gel occurs. Applicant has discovered that optimal properties are obtained when the selected time period is a time period of at least 7 days (168 hours), at least 8 days (192 hours), at least 9 days (216 hours) or at least 10 days (240 hours). Additionally, warping of the hydrophobic silica wet gel often takes place during subsequent processes. For example, in many cases, silica wet gel shrinks during drying. However, Applicant has found that a time period of at least 7 days helps prevent warping such as shrinking.

[0176] Other embodiments provide a method of making hydrophobic silica aerogel. FIG. 2 illustrates method 200B according to certain embodiments. The method 200B comprises steps 205 through 240 of making hydrophobic silica wet gel as described with regard to method 200A in FIG. 1, in addition to a step 245 of drying the hydrophobic silica wet gel to form hydrophobic silica aerogel. Additionally, FIG. 4 illustrates a method 300B according to certain embodiments. The method 300B comprises steps 305 through 340 of making hydrophobic silica wet gel as described with regard to method 300A in FIG. 3, in addition toa step 345 of drying the hydrophobic silica wet gel to form hydrophobic silica aerogel.Further, FIG. 6 illustrates a method 400B according to certain embodiments. The method 400B comprises steps 405 through 445 of making hydrophobic silica wet gel as described with regard to method 400A in FIG. 5, in addition to a step 450 of drying the hydrophobic silica wet gel to form hydrophobic silica aerogel.

[0177] In many cases, the drying step results in a hydrophobic silica aerogel having a shrinkage value of 4% or less, for example 3.5% or less, 3% or less, 2.5% or less, 2% or less or 1.75% or less. Also, in some cases, the drying step results in hydrophobic silica aerogel having a visible transmission of at least 97.8% and a haze value of 3% or less, for example a visible transmission of at least 98% and a haze value of 3% or less, a visible transmission of at least 98.6% and a haze value of 2.5 % or less, or a visible transmission of at least 99% and a haze value of 2% or less. Further, in some cases, the drying step results in hydrophobic silica aerogel having a water contact angle of at least 90%, for example at least 100% or at least 110%.

[0178] In certain embodiments, the hydrophobic silica wet gel is dried using a conventional aerogel drying method. In many cases, the hydrophobic silica wet gel is placed in either a freeze dryer, a supercritical dryer, or an ambient dryer. In such instances, the step 245 of drying the hydrophobic silica wet gel comprises either a freeze-drying process, a supercritical drying process, or an ambient drying process.

[0179] In some cases, the hydrophobic silica wet gel is dried using a supercritical drying method (also known as a critical point drying method). As is well-known to skilled artisans, supercritical dry ing involves a solvent exchange. Specifically, the water initially inside the hydrophobic silica wet gel is replaced with a suitable organic solvent (e.g., methanol, ethanol, or acetone). The hydrophobic silica wet gel is then placed in a pressure vessel along with liquid carbon dioxide. The pressure vessel may be filled with, and emptied of, liquid carbon dioxide multiple times, so as to remove the organic solvent and leave liquid carbon dioxide in its place. The liquid carbon dioxide is then heated past its critical temperature and pressure and removed, thereby leaving a hydrophobic silica aerogel.

[0180] Applicant has achieved great results when using methanol as the organic solvent in the solvent exchange. By using methanol as the solvent, the resulting aerogel material has less haze and less optical distortion than with other solvents. In certain embodiments, the hydrophobic silica wet gel can be placed in a methanol solvent bath for 8 hours, removed and then placed in another methanol solvent bath for 8 more hours. The total time period in which the hydrophobic silica wet gel is in the solvent bath can be less than 20 hours, such as less than 17 hours. This is desirable as longer solvent processing time can lead to deterioration in optical properties. Additionally, a shorter solvent processing time is advantageous for commercial production.

[0181] In other cases, the hydrophobic silica wet gel is dried using an ambient drying method. As used herein, ambient drying involves drying the hydrophobic silica wet gel under ambient conditions (e.g., at a temperature in a range of from about 50 degrees to about 85 degrees Fahrenheit, and more typically in a range of from 68 degrees to 72 degrees Fahrenheit). The liquid in the hydrophobic silica wet gel is allowed to slowly evaporate under controlled conditions, leaving a hydrophobic silica aerogel. The controlled conditions ensure that the evaporation is slow enough so that the silica network of the gel does not collapse during the drying. With ambient drying, the dryer is configured to establish a controlled environment in its interior. This may involve a controlled temperature, a controlled pressure, a controlled airflow, a controlled humidity, or any combination thereof.

[0182] In still other cases, the hydrophobic silica wet gel is dried using a freeze-drying method. The hydrophobic silica wet gel is frozen and then put into a vacuum chamber. The solvent is then removed to leave a hydrophobic silica aerogel. Any suitable freeze-drying technique known in the art may be used. As non-limiting examples, the hydrophobic silica wet gel can be placed into a household freezer, liquid nitrogen, or in a cryogenic mixture (e.g., a dry-ice / solvent mixture, such as a dry-ice and acetone bath).

[0183] Other fabrication techniques can be used, such as a rapid supercritical extraction technique. Reference is made to U.S. Patent No. 8,080,591, the salient teachings of which are incorporated herein by reference.

[0184] In some cases, the hydrophobic silica aerogel is provided in the form of a hydrophobic silica aerogel sheet. This is in contrast to aerogel in flowable granular or otherwise particulate form. The hydrophobic silica aerogel sheet preferably is self-supporting, i.e., once fully synthesized and formed, the sheet can retain sheet form without being adhered to glass or another support. This can optionally be the case for any embodiment of the present disclosure involving a hydrophobic silica aerogel sheet.

[0185] The hydrophobic silica aerogel sheet is an enhanced sheet having an advantageous combination of properties. First, the hydrophobic silica aerogel sheet desirably has low haze. For any embodiment involving a hydrophobic silica aerogel sheet, the haze can optionally be less than or equal to 4%, such as less than or equal to 3%, e.g., less than or equal to 2.5%, less than or equal to 2%, or less than or equal to 1.75%. In some cases, the hydrophobic silica aerogel sheet has a haze of less than or equal to 1.5%, less than or equal to 1.25%, or even less than or equal to 1%. This preferably is the case for any embodiment involving a hydrophobic silica aerogel sheet. Haze can be measured in well-known fashion, e.g., using a BYK Haze-Gard plus instrument. Reference is made to ASTM D 1003-00: Standard Test method for Haze and Luminous Transmittance of Transparent Plastics, the contents of which are incorporated herein by reference.

[0186] The hydrophobic silica aerogel sheet desirably has high visible transmission. In some cases, the hydrophobic silica aerogel sheet has a visible transmission of at least 97.8%, at least 97.9%, at least 98%, at least 98.1%, at least 98.2%, at least 98.3%, at least 98.4%, at least 98.5%, at least 98.6%, at least 98.7%, at least 98.8%, at least 98.9%, or at least 99%, such as at least 99.1%, at least 99.2%, at least 99.3%, at least 99.4%, or perhaps at least 99.5%. The term “visible transmission” is well known in the art and is used herein in accordance with its well-known meaning to refer to the percentage of all incident visible radiation that is transmitted through an object (e.g., through the hydrophobic silica aerogel sheet). Visible radiation constitutes the wavelength range of between about 380 nm and about 780 nm. Visible transmission, as well as visible reflection, can be determined in accordance with NFRC 300-2017, Standard Test Method for Determining the Solar and Infrared Optical Properties of Glazing Materials and Fading Resistance of Systems. The well-known and commercially available LBNL WINDOW 7.4 computer program can be used in calculating these and other reported optical properties.

[0187] The hydrophobic silica aerogel sheet can also have desirable transmitted color characterized by “a” and “b” color coordinates that are each between -2 and 2. The present discussion of color properties is reported using the well-known color coordinates of “a” and “b.” In more detail, the color coordinates are indicated herein using the subscript h (i.e., ah and bh) to represent the conventional use of the well-known Hunter Lab Color System (Hunter methods / units, Ill. D65, 10 degree observer). The present color properties can be calculated as specified in “Insight on Color,” “Hunter L, a, b Color Scale,” Applications Note, Vol. 8, No. 9, 06 / 08 (2008), the relevant teachings of which are incorporated herein by reference.

[0188] In addition, the hydrophobic silica aerogel sheet can have a low bulk density. In certain embodiments, the hydrophobic silica aerogel sheet has a bulk density of 200 mg / cc or less. In some cases, the hydrophobic silica aerogel sheet has a bulk density of 150 mg / cc or less, such as 140 mg / cc or less, 130 mg / cc or less, or 125 mg / cc or less. In certain embodiments, the hydrophobic silica aerogel sheet has a bulk density of at least 70 mg / cc. In some cases, the hydrophobic silica aerogel sheet has a bulk density of at least 80 mg / cc, such as at least 85 mg / cc or at least 95 mg / cc. In preferred embodiments, the hy drophobic silica aerogel sheet has a bulk density of between 100 mg / cc and 150 mg / cc, such as between 120 mg / cc and 150 mg / cc. In certain cases, the bulk density is 120 mg / cc. The density of the hydrophobic silica aerogel sheet can optionally be in this range for any embodiment of the present disclosure, preferably in combination with visible transmission and haze levels in the ranges noted above (e.g., Tvisof at least 97.8%, at least 98%, at least 98.6% or at least 99%, together with a haze of 3% or less, 2% or less, 1.75% or less, or 1.5% or less). Bulk density can be determined by weighing the hydrophobic silica aerogel sheet and then calculating the volume using the dimensions of the hydrophobic silica aerogel sheet.

[0189] The hydrophobic silica aerogel sheet can also have low thermal conductivity. For example, the hydrophobic silica aerogel sheet can have a thermal conductivity of 14 mW / m*K or less in air, such as 13.5 mW / m*K or less, 13 mW / m*K or less, 12 mW / m*K or less, or 11.5 mW / m*K or less. Furthermore, the hydrophobic silica aerogel sheet can have a thermal conductivity of 10 mW / m*K or less in an inert gas, such as argon. The thermal conductivity of the hydrophobic silica aerogel sheet can optionally be in one or more(optionally all) of these ranges for any embodiment of the present disclosure. Thermal conductivity can be determined using a conventional heat flow meter, such as the well-known TA Instruments Fox 200 heat flow meter, which is commercially available from Waters Corporation (New Castle, Delaware, U.S.A.).

[0190] Further, the hydrophobic silica aerogel sheet can have a flexural modulus of 6000 kPa or less, such as 4500 kPa or less, 2400 kPa or less, 2300 kPa or less, 2000 kPa or less, 1900 kPa or less, 1800 kPa or less, 1700 kPa or less, 1600 kPa or less, 1500 kPa or less, 1400 kPa or less, 1300 kPa or less, 1200 kPa or less, 1100 kPa or less, 1000 kPa or less, 900 kPa or less, 800 kPa or less, 750 kPa or less, or even 700 kPa or less. In some cases, the hydrophobic silica aerogel sheet can have a flexural modulus of between 700 kPa and 6000 kPa, such as between 750 kPa and 6000 kPa, between 800 kPa and 6000 kPa, between 900 kPa and 6000 kPa, between 1000 kPa and 6000 kPa, between 1100 kPa and 6000 kPa, between 1200 kPa and 6000 kPa, between 1300 kPa and 6000 kPa, between 1400 kPa and 6000 kPa, between 1500 kPa and 6000 kPa, between 1600 kPa and 6000 kPa, between 1700 kPa and 6000 kPa, between 1800 kPa and 6000 kPa, between 1900 kPa and 6000 kPa, between 2000 kPa and 6000 kPa, between 2300 kPa and 6000 kPa and between 2400 kPa and 6000kPa.

[0191] The flexural modulus of a material is a mechanical property that measures a material’s stiffness or resistance to bending and is defined as the ratio of stress to strain in flexural deformation. It is determined from the slope of a stress-strain curve produced by a flexural test, such as ASTM D790: Standard Test Methods for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Material, the contents of which are incorporated herein by reference. The higher the flexural modulus of a material, the harder it is to bend. Conversely, the lower the flexural modulus, the easier it is for the material to bend under an applied force.

[0192] Even further, the hydrophobic silica aerogel sheet can have an average pore size of 31 nm or less, such as 30 nm or less, 29 nm or less, 28 nm or less, 27 nm or less, 26 nm or less, 25 nm or less, 24 nm or less, 23 nm or less, 22 nm or less, 21 nm or less, or even 20 nm or less. This can optionally be the case for any embodiment of the present disclosure that involves the silica aerogel sheet. The average pore size can be determined using a Quantachrome “autosorb-iQ” gas absorption analyzer, which is commercially available fromAnton Paar (Graz, Austria) along with calculating average pore size using density functional theory (DFT) calculations.

[0193] The silica aerogel sheet can also have a specific surface area of at least 750 m2 / g, such as at least 800 m2 / g, at least 850 m2 / g, at least 900 m2 / g, at least 950 m2 / g, or at least 1000 m2 / g. This can optionally be the case for any embodiment of the present disclosure that involves the hydrophobic silica aerogel sheet, preferably in combination with an average pore diameter in one or more (optionally all) of the ranges noted in the paragraph above and / or in combination with a density of between 100 mg / cc and 150 mg / cc, optionally in further combination with visible transmission and haze levels in the ranges noted above (e.g., T™ of at least 97.8%, perhaps at least 98%, at least 98.6%, or at least 99%, together with haze of 3% or less, 2% or less, 1.75% or less, or 1.5% or less). The specific surface area can also be determined using a Quantachrome “autosorb-iQ” gas absorption analyzer, which is commercially available from Anton Paar (Graz, Austria) along with calculating specific surface area using density functional theory (DFT) calculations.

[0194] Further, the silica aerogel sheet can have a water contact angle of at least 90°, such as at least 95°, at least 100°, at least 105°, at least 110°, at least 115°, at least 120°, or at least 125°. A Rame-Hart Contact Angle Goniometer (Model No.100-00) was used for the detection of static contact angle measurement. The measurement was performed by using a traditional sessile drop technique.

[0195] The silica aerogel sheet can also have a linear shrinkage (X / Y direction) of 4% or less, 3.5% or less, 3% or less, 2.5% or less, 2% or less, 1.75% or less, or perhaps 1.7% or less. Sample images were taken with a regular camera with known scale. The images were analyzed with image J software and the final length of the aerogel was determined after CPD drying with respect to the known initial length (Initial length- 120mm).

[0196] Certain embodiments provide a hydrophobic silica aerogel sheet synthesized from at least two alkoxy silanes and having a visible transmission of at least 97.8% and a haze value of 3% or less. A first alkoxy silane of the two alkoxy silanes is selected from methyl silicate 51 and tetramethoxy silane, and a second alkoxysilane of the two alkoxysilanes is selected frommethyltrimethoxysilane and methyltriethoxysilane. The hydrophobic silica aerogel sheet can also include at least one of the following features (A) through (E):(A) a water contact angle of at least 90°;(B) a thermal conductivity in air of 13.5 mW / m K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 750 m2 / g;(E) an average pore diameter of 30 nm or less.

[0197] The hydrophobic silica aerogel sheet can optionally include at least two of the features (A) through (E), at least three of the features (A) through (E), at least four of the features (A) through (E), or all of the features (A) through (E). Also, in some cases, the visible transmission of the hydrophobic silica aerogel sheet is at least 98.6%, and the haze value is 2.5% or less. In further cases, the visible transmission of the hydrophobic silica aerogel sheet is at least 99%, and the haze value is 2% or less. The water contact angle in feature (A) can optionally be at least 100°, such as at least 110° or at least 120°. The flexural modulus in feature (C) can optionally be 4500 kPa or less. Further, the specific surface area in feature (D) can optionally be at least 800 m2 / g. Even further, the average pore diameter in feature (E) can optionally be 27 nm or less.

[0198] Other embodiments provide a hydrophobic silica aerogel sheet synthesized from at least two alkoxy silanes and having a visible transmission of at least 98% and a haze value of 2% or less. The hydrophobic silica aerogel sheet can also include at least one of the follow ing features (A) through (E):(A) a water contact angle of at least 110°;(B) a thermal conductivity in air of 13 mW / m-K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 750 m2 / g;(E) an average pore diameter of 29 nm or less.

[0199] Again, the hydrophobic silica aerogel sheet can optionally include at least two of the features (A) through (E), at least three of the features (A) through (E), at least four of the features (A) through (E), or all of the features (A) through (E).

[0200] Other embodiments provide a hydrophobic silica aerogel sheet synthesized from at least two alkoxy silanes and having a visible transmission of at least 98.6% and a haze valueof 1.5% or less. The hydrophobic silica aerogel sheet can also include at least one of the following features (A) through (E):(A) a water contact angle of at least 120°;(B) a thermal conductivity in air of 13 mW / m K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 900 m2 / g;(E) an average pore diameter of 28 nm or less.

[0201] Here too, the hydrophobic silica aerogel sheet can optionally include at least two of the features (A) through (E), at least three of the features (A) through (E), at least four of the features (A) through (E) or all of the features (A) through (E).Examples

[0202] Exemplary hydrophobic silica aerogel sheets (Examples #1-#12) were prepared using MS-51 and MTMS at densities of 100 mg / cc, 120 mg / cc, 150 mg / cc, and 200 mg / cc. In these examples, a hydrophobic silica wet gel sheet was formed before a step of aging was completed. Properties obtained for hydrophobic silica aerogel sheets from these examples were measured using methods described herein and are tabulated in Tables 1-3.Example #1 (MS-51 / MTMS at .95:1 ratio at 100 mg / cc)

[0203] Example #1 was prepared according to the following steps:A. Preparing a first solution by mixing 5.5 mL MS-51 and 18.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 30.84% and methanol at a weight percent of 69.16%.B. Preparing a second solution by mixing 18.5 mL methanol, 0.07 mL ammonium hydroxide and 6.93 mL water. The weight percent of the second solution included methanol at a weight percent of 67.54%, water at a weight percent of 32. 16%, and ammonium hydroxide at a weight percent of 0.3%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 15.24%, methanol at a weight percent of 68.34%, water at a weight percent of 16.27%, and ammonium hydroxide at a weight percent of 0.15%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5EMTMS was .95: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the hydrophobic silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #1 is listed in Table 1.J. Removing the hydrophobic silica wet gel sheet from the mold.K. Placing the hydrophobic silica wet gel sheet in a first methanol bath and allowing solvent exchange to take place for 8 hours.L. Placing the hydrophobic silica wet gel sheet in a second methanol bath and allowing solvent exchange to take place for 8 more hours.M. Placing the hydrophobic wet gel sheet in a dryer and performing critical point drying with a complete CO2 exchange to obtain a hydrophobic silica aerogel sheet.Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #1 are shown in Table 1.Example #2 (MS-51 / MTMS at 1.2:1 ratio at 120 mg / cc)

[0204] Example #2 was prepared according to the following steps:A. Preparing a first solution by mixing 7 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 36.84% and methanol at a weight percent of 63.16%.B. Preparing a second solution by mixing 18 mL methanol, 0.07 mL ammonium hydroxide and 6.93 mL water. The weight percent of the second solution included methanol at a weight percent of 66.94%, water at a weight percent of 32.76%, and ammonium hydroxide at a weight percent of 0.3%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 18.96%, methanol at a weight percent of 64.99%, water at a weight percent of 15.90%, and ammonium hydroxide at a weight percent of 0.15%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5EMTMS was 1.2: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #2 is listed in Table 1.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #2 are shown in Table 1.Example #3 (MS-51 / MTMS at 2:1 ratio at 150 mg / cc)

[0205] Example #3 was prepared according to the following steps:A. Preparing a first solution by mixing 11.5 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 48.94% and methanol at a weight percent of 51.06%.B. Preparing a second solution by mixing 18 mL methanol, 0.07 mL ammonium hydroxide, and 6.93 mL water. The weight percent of the second solution included methanol at a weight percent of 66.94%, water at a weight percent of 32.76%, and ammonium hydroxide at a weight percent of 0.3%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 27.76%,methanol at a weight percent of 57.93%, water at a weight percent of 14.18%, and ammonium hydroxide at a weight percent of 0.13%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5EMTMS was 2: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #3 is listed in Table 1.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #3 are shown in Table 1.Example #4 (MS-51 / MTMS at 2,55: 1 ratio at 200 mg / cc)

[0206] Example #4 was prepared according to the following steps:A. Preparing a first solution by mixing 15 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 55.56% and methanol at a weight percent of 44.44%.B. Preparing a second solution by mixing 18 mL methanol, 0.1 mL ammonium hydroxide, and 9.9 mL water. The weight percent of the second solution included methanol at a weight percent of 58.63%, water at a weight percent of 40.99%, and ammonium hydroxide at a weight percent of 0.38%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 31.6%, methanol at a weight percent of 50.56%, water at a weight percent of 17.68%, and ammonium hydroxide at a weight percent of 0.16%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5EMTMS was 2.55: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #4 is listed in Table 1.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #4 are shown in Table 1.Table 1Example #5 (MS-51 / MTMS at .98:1 ratio at 100 mg / cc)

[0207] Example #5 was prepared according to the following steps:A. Preparing a first solution by mixing 5.5 mL MS-51 and 18.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 30.84% and methanol at a weight percent of 69.16%.B. Preparing a second solution by mixing 18.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 67.53%, water at a weight percent of 32.43%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 15.24%, methanol at a weight percent of 68.33%, water at a weight percent of 16.41%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 MTMS was .98: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the hydrophobic silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #5 is listed in Table 2.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #5 are shown in Table 2.Example #6 (MS-51 / MTMS at 1.25: 1 ratio at 120 mg / cc)

[0208] Example #6 was prepared according to the following steps:A. Preparing a first solution by mixing 7 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 36.84% and methanol at a weight percent of 63.16%.B. Preparing a second solution by mixing 18 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 66.93%, water at a weight percent of 33.03%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 18.96%, methanol at a weight percent of 64.98%, water at a weight percent of 16.04%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 MTMS was 1.25: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #6 is listed in Table 2Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #6 are shown in Table 2.Example #7 (MS-51 / MTMS at 1.29: 1 ratio at 150 mg / cc)

[0209] Example #7 was prepared according to the following steps:A. Preparing a first solution by mixing 9 mL MS-51 and 16.75 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 44.63% and methanol at a weight percent of 55.37%.B. Preparing a second solution by mixing 16.75 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 65.31%, water at a weight percent of 34.64%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 24. 15%, methanol at a weight percent of 59.93%, water at a weight percent of 15.9%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2.5 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS- 5LMTMS was 1.29: 1. The weight percent of the third solution included MTMS at a weight percent of 13.18% and methanol at a weight percent of 86.82%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #7 is listed in Table 2.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #7 are shown in Table 2.Example #8 (MS-51 / MTMS at 1.43: 1 ratio at 200 mg / cc)

[0210] Example #8 was prepared according to the following steps:A. Preparing a first solution by mixing 12 mL MS-51 and 15.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 53.73% and methanol at a weight percent of 46.27%.B. Preparing a second solution by mixing 15.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 63.53%, water at a weight percent of 36.42%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 31.09%, methanol at a weight percent of 53.54%, water at a weight percent of 15.35%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 3 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 MTMS was 1.43: 1. The weight percent of the third solution included MTMS at a weight percent of 15.40% and methanol at a weight percent of 84.6%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #8 is listed in Table 2.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #8 are shown in Table 2.Table 2Example #9 (MS-51 / MTMS at 1.3:1 ratio at 100 mg / cc)

[0211] Example #9 was prepared according to the following steps:A. Preparing a first solution by mixing 5.5 mL MS-51 and 18.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 30.84% and methanol at a weight percent of 69. 16%.B. Preparing a second solution by mixing 18.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 67.53%, water at a weight percent of 32.43%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 15.24%,methanol at a weight percent of 68.33%, water at a weight percent of 16.41%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 1.5 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS- 5EMTMS was 1.3: 1. The weight percent of the third solution included MTMS at a weight percent of 8.35% and methanol at a weight percent of 91.65%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #9 is listed in Table 3.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #9 are shown in Table 3.Example #10 (MS-51 / MTMS at 1,66: 1 ratio at 120 mg / cc)

[0212] Example #10 was prepared according to the following steps:A. Preparing a first solution by mixing 7 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 36.84% and methanol at a weight percent of 63.16%.B. Preparing a second solution by mixing 18 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 66.92%, water at a weight percent of 33.03%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 18.96%, methanol at a weight percent of 64.98%, water at a weight percent of 16.04%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 1.5 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS- 5EMTMS was 1.66:1. The weight percent of the third solution included MTMS at a weight percent of 8.35% and methanol at a weight percent of 91.65%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #10 is listed in Table 3.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #10 are shown in Table 3.Example #11 (MS-51 / MTMS at 1.6: 1 ratio at 150 mg / cc)

[0213] Example #11 was prepared according to the following steps:A. Preparing a first solution by mixing 9 mL MS-51 and 16.75 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 44.63% and methanol at a weight percent of 55.34%.B. Preparing a second solution by mixing 16.75 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 65.31%, water at a weight percent of 34.64%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 24. 15%, methanol at a weight percent of 59.93%, water at a weight percent of 15.9%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 :MTMS was 1.6: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #11 is listed in Table 3.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #11 are shown in Table 3.Example #12 (MS-51 / MTMS at 1.71: 1 ratio at 200

[0214] Example #12 was prepared according to the following steps:A. Preparing a first solution by mixing 12 mL MS-51 and 15.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 53.73% and methanol at a weight percent of 46.27%.B. Preparing a second solution by mixing 15.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 63.53%, water at a weight percent of 36.42%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 31.09%, methanol at a weight percent of 53.54%, water at a weight percent of 15.35%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2.5 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 :MTMS was 1.7: 1. The weight percent of the third solution included MTMS at a weight percent of 13. 18% and methanol at a weight percent of 86.82%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #12 is listed in Table 3.Steps J through M were repeated as performed in Example #1. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #12 are shown in Table 3.Table 3

[0215] Exemplaty hydrophobic silica aerogel sheets (Examples # 13- 24) were prepared using MS-51 and MTMS at densities of 100 mg / cc, 120 mg / cc, 150 mg / cc, and 200 mg / cc. In these examples, a hydrophobic silica wet gel sheet was formed after aging was completed. Properties obtained for hydrophobic silica aerogel sheets in these examples were also measured using methods described herein and tabulated in Tables 4-6.Example #13 (MS-51 / MTMS at 0.95 ratio at 100 mg / cc)

[0216] Example #13 was prepared according to the following steps:A. Preparing a first solution by mixing 5.5 mL MS-51 and 18.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 30.84% and methanol at a weight percent of 69.16%.B. Preparing a second solution by mixing 18.5 mL methanol, 0.07 mL ammonium hydroxide, and 6.93 mL water. The weight percent of the second solution included methanol at a weight percent of 67.54%, water at a weight percent of 32. 16%, and ammonium hydroxide at a weight percent of 0.3%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 15.24%, methanol at a weight percent of 68.34%, water at a weight percent of 16.27%, and ammonium hydroxide at a weight percent of 0.15%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 MTMS was 0.95: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #13 is listed in Table 4.J. Removing the hydrophobic silica wet gel sheet from the mold.K. Placing the hydrophobic silica wet gel sheet in a first methanol bath and allowing solvent exchange to take place for 8 hours.L. Placing the hydrophobic silica wet gel sheet in a second methanol bath and allowing solvent exchange to take place for 8 more hours.M. Placing the hydrophobic wet gel sheet in a dryer and performing critical point drying with a complete CO2 exchange to obtain a hydrophobic silica aerogel sheet.Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #13 are shown in Table 4.Example #14 (MS-51 / MTMS at 1.2: 1 ratio at 120 mg / cc)

[0217] Example #14 was prepared according to the following steps:A. Preparing a first solution by mixing 7 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 36.84% and methanol at a weight percent of 63.16%.B. Preparing a second solution by mixing 18 mL methanol, 0.07 mL ammonium hydroxide, and 6.93 mL water. The weight percent of the second solution included methanol at a weight percent of 66.94%, water at a weight percent of 32.76%, and ammonium hydroxide at a weight percent of 0.3%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 18.95%, methanol at a weight percent of 65%, water at a weight percent of 15.9%, and ammonium hydroxide at a weight percent of 0.15%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 MTMS was 1.2: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #14 is listed in Table 4.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #14 are shown in Table 4.Example #15 (MS-51 / MTMS at 2: 1 ratio at 150 mg / cc)

[0218] Example #15 was prepared according to the following steps:A. Preparing a first solution by mixing 11.5 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 48.94% and methanol at a weight percent of 51.06%.B. Preparing a second solution by mixing 18 mL methanol, 0.07 mL ammonium hydroxide, and 6.93 mL water. The weight percent of the second solution included methanol at a weight percent of 66.94%, water at a weight percent of 32.76%, and ammonium hydroxide at a weight percent of 0.3%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 27.76%, methanol at a weight percent of 57.93%, water at a weight percent of 14. 18%, and ammonium hydroxide at a weight percent of 0.13%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-51 MTMS was2: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #15 is listed in Table 4.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #15 are shown in Table 4.Example #16 (MS-51 / MTMS at 2,55: 1 ratio at 200

[0219] Example #16 was prepared according to the following steps:A. Preparing a first solution by mixing 15 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 55.56% and methanol at a weight percent of 44.44%.B. Preparing a second solution by mixing 18 mL methanol, 0.1 mL ammonium hydroxide, and 9.9 mL water. The weight percent of the second solution included methanol at a weight percent of 58.63%, water at a weight percent of 40.99%, and ammonium hydroxide at a weight percent of 0.38%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 31.6%, methanol at a weight percent of 50.56%, water at a weight percent of 17.68%, and ammonium hydroxide at a weight percent of 0.16%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5LMTMS was 2.55: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #16 is listed in Table 4.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #16 are shown in Table 4.Table 4Example #17 (MS-51 / MTMS at 0,98: 1 ratio at 100 mg / cc)

[0220] Example #17 was prepared according to the following steps:A. Preparing a first solution by mixing 5.5 mL MS-51 and 18.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 30.84% and methanol at a weight percent of 69.16%.B. Preparing a second solution by mixing 18.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 67.53%, water at a weight percent of 32.43%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 15.24%, methanol at a weight percent of 68.33%, water at a weight percent of 16.41%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5LMTMS was 0.98: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #17 is listed in Table 5.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #17 are shown in Table 5.Example #18 (MS-51 / MTMS at 1.25: 1 ratio at 120 mg / cc)

[0221] Example #18 was prepared according to the following steps:A. Preparing a first solution by mixing 7 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 36.84% and methanol at a weight percent of 63.16%.B. Preparing a second solution by mixing 18 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 66.92%, water at a weight percent of 33.04%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 18.96%, methanol at a weight percent of 64.98%, water at a weight percent of 16.04%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5LMTMS was 1.25: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #18 is listed in Table 5.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #18 are shown in Table 5.Example #19 (MS-51 / MTMS at 1.29: 1 ratio at 150 mg / cc)

[0222] Example #19 was prepared according to the following steps:A. Preparing a first solution by mixing 9 mL MS-51 and 16.75 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 44.63% and methanol at a weight percent of 55.37%.B. Preparing a second solution by mixing 16.75 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 65.31%, water at a weight percent of 34.64%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 24. 15%, methanol at a weight percent of 59.93%, water at a weight percent of 15.9%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2.5 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS- 5LMTMS was 1.29: 1. The weight percent of the third solution included MTMS at a weight percent of 0.76% and methanol at a weight percent of 99.24%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #19 is listed in Table 5.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #19 are shown in Table 5.Example #20 (MS-51 / MTMS at 1.43: 1 ratio at 200 mg / cc)

[0223] Example #20 was prepared according to the following steps:A. Preparing a first solution by mixing 12 mL MS-51 and 15.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 53.73% and methanol at a weight percent of 46.27%.B. Preparing a second solution by mixing 15.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 63.53%, water at a weight percent of 36.42%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 31.09%, methanol at a weight percent of 53.54%, water at a weight percent of 15.35%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 3 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5LMTMS was 1.43: 1. The weight percent of the third solution included MTMS at a weight percent of 0.91% and methanol at a weight percent of 99.09%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #20 is listed in Table 5.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #20 are shown in Table 5.Table 5Example #21 (MS-51 / MTMS at 1.31: 1 ratio at 100 mg / cc)

[0224] Example #21 was prepared according to the following steps:A. Preparing a first solution by mixing 5.5 mL MS-51 and 18.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 30.84% and methanol at a weight percent of 69. 16%.B. Preparing a second solution by mixing 18.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 67.53%, water at a weight percent of 32.43%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 15.24%,methanol at a weight percent of 68.33%, water at a weight percent of 16.41%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 1.5 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS- 5EMTMS was 1.31: 1. The weight percent of the third solution included MTMS at a weight percent of 0.46% and methanol at a weight percent of 99.54%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #21 is listed in Table 6.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #21 are shown in Table 6.Example #22 (MS-51 / MTMS at 1.67: 1 ratio at 120 m» / cc)

[0225] Example #22 was prepared according to the following steps:A. Preparing a first solution by mixing 7 mL MS-51 and 18 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 36.84% and methanol at a weight percent of 63.16%.B. Preparing a second solution by mixing 18 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 66.92%, water at a weight percent of 33.04%, and ammonium hydroxide at a weight percent of 0.04%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 18.96%, methanol at a weight percent of 64.98%, water at a weight percent of 16.04%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 1.5 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS- 5EMTMS was 1.67: 1. The weight percent of the third solution included MTMS at a weight percent of 0.46% and methanol at a weight percent of 99.54%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #22 is listed in Table 6.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #22 are shown in Table 6.Example #23 (MS-51 / MTMS at 1.61: 1 ratio at 150 m» / cc)

[0226] Example #23 was prepared according to the following steps:A. Preparing a first solution by mixing 9 mL MS-51 and 16.75 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 44.63% and methanol at a weight percent of 55.37%.B. Preparing a second solution by mixing 16.75 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 65.31%, water at a weight percent of 34.64%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 24. 15%, methanol at a weight percent of 59.93%, water at a weight percent of 15.9%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS-5EMTMS was 1.61: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #23 is listed in Table 6.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #23 are shown in Table 6.Example #24 (MS-51 / MTMS at 1.72: 1 ratio at 200 mg / cc)

[0227] Example #24 was prepared according to the following steps:A. Preparing a first solution by mixing 12 mL MS-51 and 15.5 mL methanol. The weight percent of the first solution included MS-51 at a weight percent of 53.73% and methanol at a weight percent of 46.27%.B. Preparing a second solution by mixing 15.5 mL methanol, 0.01 mL ammonium hydroxide, and 6.989 mL water. The weight percent of the second solution included methanol at a weight percent of 63.53%, water at a weight percent of 36.42%, and ammonium hydroxide at a weight percent of 0.05%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included MS-51 at a weight percent of 31.09%, methanol at a weight percent of 53.54%, water at a weight percent of 15.35%, and ammonium hydroxide at a weight percent of 0.02%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.I l lF. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2.5 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the MS- 51:MTMS was 1.72: 1. The weight percent of the third solution included MTMS at a weight percent of 0.76% and methanol at a weight percent of 99.24%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #24 is listed in Table 6.Steps J through M were repeated as performed in Example #13. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #24 are shown in Table 6.Table 6

[0228] Exemplar)' hydrophobic silica aerogel sheets (Examples #25-#32) were prepared using TMOS and MTMS at densities of 100 mg / cc, 120 mg / cc, 150 mg / cc, and 200 mg / cc. In these examples, a hydrophobic silica wet gel sheet was formed before aging was completed. Properties obtained for hydrophobic silica aerogel sheets obtained for these examples were also measured using methods described herein and tabulated in Tables 7-8.Example #25 (TMOS / MTMS at 3,7: 1 ratio at 100 mg / cc)

[0229] Example #25 was prepared according to the following steps:A. Preparing a first solution by mixing 8 mL TMOS and 17 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 38.13% and methanol at a weight percent of 61.87%.B. Preparing a second solution by mixing 17 mL methanol, 0.08 mL ammonium hydroxide, and 6.92 mL water. The weight percent of the second solution included methanol at a weight percent of 65.66%, water at a weight percent of 33.98%, and ammonium hydroxide at a weight percent of 0.36%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 19.63%, methanol at a weight percent of 63.71%, water at a weight percent of 19.49%, and ammonium hydroxide at a weight percent of 0.17%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 3.7: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83%, and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #25 is listed in Table 7.J. Removing the hydrophobic silica wet gel sheet from the mold.K. Placing the hydrophobic silica wet gel sheet in a first methanol bath and allowing solvent exchange to take place for 8 hours.L. Placing the hydrophobic silica wet gel sheet in a second methanol bath and allowing solvent exchange to take place for 8 more hours.M. Placing the hydrophobic wet gel sheet in a dryer and performing critical point drying with a complete CO2 exchange to obtain a hydrophobic silica aerogel sheet.Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #25 are shown in Table 7.Example #26 (TMOS / MTMS at 4,6: 1 ratio at 120 mg / cc)

[0230] Example #26 was prepared according to the following steps:A. Preparing a first solution by mixing 10 mL TMOS and 16.5 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 44.25% and methanol at a weight percent of 55.75%.B. Preparing a second solution by mixing 16.5 mL methanol, 0.08 mL ammonium hydroxide, and 6.92 mL water. The weight percent of the second solution included methanol at a weight percent of 64.99%, water at a weight percent of 34.65%, and ammonium hydroxide at a weight percent of 0.36%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 23.81%, methanol at a weight percent of 60.02%, water at a weight percent of 16%, and ammonium hydroxide at a weight percent of 0.17%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 4.6: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #26 is listed in Table 7.Steps J through M were repeated as performed in Example #25. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #26 are shown in Table 7.Example #27 (TMOS / MTMS at 6,9: 1 ratio at 150 mg / cc)

[0231] Example #27 was prepared according to the following steps:A. Preparing a first solution by mixing 15 mL TMOS and 16 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 55. 11% and methanol at a weight percent of 44.89%.B. Preparing a second solution by mixing 16 mL methanol, 0.08 mL ammonium hydroxide, and 6.92 mL water. The weight percent of the second solution included methanol at a weight percent of 64.28%, water at a weight percent of 35.35%, and ammonium hydroxide at a weight percent of 0.37%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 32.45%, methanol at a weight percent of 52.87%, water at a weight percent of 14.53%, and ammonium hydroxide at a weight percent of 0.15%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 6.9: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83%, and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #27 is listed in Table 7.Steps J through M were repeated as performed in Example #25. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #27 are shown in Table 7.Example #28 (TMOS / MTMS at 9,2: 1 ratio at 200 mg / cc)

[0232] Example #28 was prepared according to the following steps:A. Preparing a first solution by mixing 20 mL TMOS and 15.5 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 62.82% and methanol at a weight percent of 37.18%.B. Preparing a second solution by mixing 15.5 mL methanol, 0.1 mL ammonium hydroxide, and 9.9 mL water. The weight percent of the second solution included methanol at a weight percent of 54.96%, water at a weight percent of 44.63%, and ammonium hydroxide at a weight percent of 0.41%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 37.47%, methanol at a weight percent of 44.35%, water at a weight percent of 18%, and ammonium hydroxide at a weight percent of 0.17%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 9.2: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #28 is listed in Table 7.Steps J through M were repeated as performed in Example #25. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #28 are shown in Table 7.Table 7Example #29 (TMOS / MTMS at 3,86: 1 ratio at 100 mg / cc)

[0233] Example #29 was prepared according to the following steps:A. Preparing a first solution by mixing 8 mL TMOS and 17 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 38.13% and methanol at a weight percent of 61.87%.B. Preparing a second solution by mixing 17 mL methanol, 0.024 mL ammonium hydroxide, and 6.98 mL water. The weight percent of the second solution included methanol at a weight percent of 65.65%, water at a weight percent of 34.24%, and ammonium hydroxide at a weight percent of 0.11%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 19.63%, methanol at a weight percent of 63.7%, water at a weight percent of 16.62%, and ammonium hydroxide at a weight percent of 0.05%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 3.86: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #29 is listed in Table 8.Steps J through M were repeated as performed in Example #25. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #29 are shown in Table 8.Example #30 (TMOS / MTMS at 4,83: 1 ratio at 120 mg / cc)

[0234] Example #30 was prepared according to the following steps:A. Preparing a first solution by mixing 10 mL TMOS and 16.5 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 44.25% and methanol at a weight percent of 55.75%.B. Preparing a second solution by mixing 16.5 mL methanol, 0.024 mL ammonium hydroxide, and 6.98 mL water. The weight percent of the second solution included methanol at a weight percent of 64.97%, water at a weight percent of 34.92%, and ammonium hydroxide at a weight percent of 0.11%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 23.81%, methanol at a weight percent of 60.01%, water at a weight percent of 16. 13%, and ammonium hydroxide at a weight percent of 0.05%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was4.83: 1. The weight percent of the third solution included MTMS at a weight percent of 10.83% and methanol at a weight percent of 89. 17%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel sheet in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #30 is listed in Table 8.Steps J through M were repeated as performed in Example #25. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #30 are shown in Table 8.Example #31 (TMOS / MTMS at 5,79: 1 ratio at 150

[0235] Example #31 was prepared according to the following steps:A. Preparing a first solution by mixing 15 mL TMOS and 14 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 58.38% and methanol at a weight percent of 41.62%.B. Preparing a second solution by mixing 14 mL methanol, 0.024 mL ammonium hydroxide, and 6.98 mL water. The weight percent of the second solution included methanol at a weight percent of 61.15%, water at a weight percent of 38.73%, and ammonium hydroxide at a weight percent of 0.12%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 34.74%, methanol at a weight percent of 49.52%, water at a weight percent of 15.69%, and ammonium hydroxide at a weight percent of 0.05%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 2.5 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 5.79: 1. The weight percent of the third solution included MTMS at a weight percent of 13.18% and methanol at a weight percent of 86.82%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #31 is listed in Table 8.Steps J through M were repeated as performed in Example #25. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #31 are shown in Table 8.Example #32 (TMOS / MTMS at 6, 11 : 1 ratio at 200 mg / cc)

[0236] Example #32 was prepared according to the following steps:A. Preparing a first solution by mixing 19 mL TMOS and 11.5 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 68.39% and methanol at a weight percent of 31.61%.B. Preparing a second solution by mixing 11.5 mL methanol, 0.024 mL ammonium hydroxide, and 6.89 mL water. The weight percent of the second solution included methanol at a weight percent of 56.38%, water at a weight percent of 43.48%, and ammonium hydroxide at a weight percent of 0.14%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 43.82%, methanol at a weight percent of 50.51%, water at a weight percent of 15.62%, and ammonium hydroxide at a weight percent of 0.05%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel having dimensions of 5 inches by 5 inches by 3.5 mm.F. Preparing a third solution by mixing 3 mL MTMS and 20 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 6. 11 : 1. The weight percent of the third solution included MTMS at a weight percent of 15.41% and methanol at a weight percent of 84.59%.G. Begin aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.H. Adding the third solution to the silica wet gel in the mold before aging is complete.I. Allowing the third solution to react with the silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #32 is listed in Table 8.Steps J through M were repeated as performed in Example #25. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #32 are shown in Table 8.Table 8Additional exemplary hydrophobic silica aerogel sheets (Examples #33-#40) were prepared using TMOS and MTMS at densities of 100 mg / cc, 120mg / cc, 150 mg / cc, and 200 mg / cc. In these examples, a hydrophobic silica wet gel sheet was formed after aging was completed. Properties obtained for hydrophobic silica aerogel sheets in these examples were also measured using methods described herein and tabulated in Tables 9-10.Example #33 (TMOS / MTMS at 3,7: 1 ratio at 100 mg / cc)

[0237] Example #33 was prepared according to the following steps:A. Preparing a first solution by mixing 8 mL TMOS and 17 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 38.13% and methanol at a weight percent of 61.87%.B. Preparing a second solution by mixing 17 mL methanol, 0.08 mL ammonium hydroxide and 6.92 mL water. The weight percent of the second solution included methanol at a weight percent of 65.66%, water at a weight percent of 33.98%, and ammonium hydroxide at a weight percent of 0.36%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 19.63%, methanol at a weight percent of 63.71%, water at a weight percent of 16.49%, and ammonium hydroxide at a weight percent of 0.17%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 3.7: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #33 is listed in Table 9.J. Removing the hydrophobic silica wet gel sheet from the mold.K. Placing the hydrophobic silica wet gel sheet in a first methanol bath and allowing solvent exchange to take place for 8 hours.L. Placing the hydrophobic silica wet gel sheet in a second methanol bath and allowing solvent exchange to take place for 8 more hours.M. Placing the hydrophobic wet gel sheet in a dryer and performing critical point drying with a complete CO2 exchange to obtain a hydrophobic silica aerogel sheet.Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #33 are shown in Table 9.Example #34 (TMOS / MTMS at 4,6: 1 ratio at 120

[0238] Example #34 was prepared according to the following steps:A. Preparing a first solution by mixing 10 mL TMOS and 16.5 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 44.25% and methanol at a weight percent of 55.75%.B. Preparing a second solution by mixing 16.5 mL methanol, 0.08 mL ammonium hydroxide, and 6.92 mL water. The weight percent of the second solution included methanol at a weight percent of 64.99%, water at a weight percent of 34.65%, and ammonium hydroxide at a weight percent of 0.36%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 23.81%, methanol at a weight percent of 60.02%, water at a weight percent of 16%, and ammonium hydroxide at a weight percent of 0.17%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 4.6: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #34 is listed in Table 9.Steps J through M were repeated as performed in Example #33. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #34 are shown in Table 9.Example #35 (TMOS / MTMS at 6,9: 1 ratio at 150 mg / cc)

[0239] Example #35 was prepared according to the following steps:A. Preparing a first solution by mixing 15 mL TMOS and 16 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 55. 11% and methanol at a weight percent of 44.89%.B. Preparing a second solution by mixing 16 mL methanol, 0.08 mL ammonium hydroxide, and 6.92 mL water. The weight percent of the second solution included methanol at a weight percent of 64.28%, water at a weight percent of 35.35%, and ammonium hydroxide at a weight percent of 0.37%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 32.45%, methanol at a weight percent of 52.87%, water at a weight percent of 14.53%, and ammonium hydroxide at a weight percent of 0.15%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 397 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 6.9: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #35 is listed in Table 9.Steps J through M were repeated as performed in Example #33. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #35 are shown in Table 9.Example #36 (TMOS / MTMS at 9,2: 1 ratio at 200 mg / cc)

[0240] Example #36 was prepared according to the following steps:A. Preparing a first solution by mixing 20 mL TMOS and 12.4 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 67.87% and methanol at a weight percent of 32.13%.B. Preparing a second solution by mixing 12.4 mL methanol, 0.1 mL ammonium hydroxide, and 9.9 mL water. The weight percent of the second solution included methanol at a weight percent of 49.4%, water at a weight percent of 50.14%, and ammonium hydroxide at a weight percent of 0.46%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 41.12%, methanol at a weight percent of 38.94%, water at a weight percent of 19.76%, and ammonium hydroxide at a weight percent of 0.18%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 9.2: 1. The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #36 is listed in Table 9.Steps J through M were repeated as performed in Example #33. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #36 are shown in Table 9.Table 9Example #37 (TMOS / MTMS at 3,86: 1 ratio at 100 mg / cc)

[0241] Example #37 was prepared according to the following steps:A. Preparing a first solution by mixing 8 mL TMOS and 17 mL methanol. The weight percent of the first solution included TMOS at a weight percent of 38.13% and methanol at a weight percent of 61.87%.B. Preparing a second solution by mixing 17 mL methanol, 0.024 mL ammonium hydroxide, and 6.976 mL water. The weight percent of the second solution included methanol at a weight percent of 65.64%, water at a weight percent of 34.25%, and ammonium hydroxide at a weight percent of 0.11%.C. Mixing the first solution and second solution together to form a mixed solution. The weight percent of the mixed solution included TMOS at a weight percent of 19.63%, methanol at a weight percent of 63.7%, water at a weight percent of 16.62%, and ammonium hydroxide at a weight percent of 0.05%.D. Depositing the mixed solution into a mold having interior dimensions of 5 inches by 5 inches by 3.5 mm. Sealing the mold to provide an airtight environment.E. Allowing components in the mixed solution to react to form a silica wet gel sheet having dimensions of 5 inches by 5 inches by 3.5 mm.F. Aging the silica wet gel sheet in the mold at room temperature for a time period of 240 hours.G. Preparing a third solution by mixing 2 mL MTMS and 398 mL methanol. The MTMS was provided in a controlled amount such that a molar ratio of the TMOS:MTMS was 3.86: 1, The weight percent of the third solution included MTMS at a weight percent of 0.61% and methanol at a weight percent of 99.39%.H. Adding the third solution to the aged silica wet gel sheet in the mold after aging is complete.I. Allowing the third solution to react with the aged silica wet gel sheet to form a hydrophobic silica wet gel sheet. The total weight percent of all components used to form the hydrophobic silica wet gel sheet of Example #37 is listed in Table 10.Steps J through M were repeated as performed in Example #33. Properties obtained for the resulting hydrophobic silica aerogel sheet of Example #37 are shown in Table 10.Example #38 (TMOS / MTMS at 4,83: 1 rat...

Claims

WHAT IS CLAIMED IS:

1. An article comprising a glass substrate and a hydrophobic silica aerogel sheet, the hydrophobic silica aerogel sheet being adhered to the glass substrate and being synthesized from at least two alkoxysilanes and having a visible transmission of at least 97.8% and a haze value of 3% or less.

2. The article of claim 1 wherein the hydrophobic silica aerogel sheet further includes at least one of the following features (A) through (E):(A) a water contact angle of at least 90°;(B) a thermal conductivity in air of 13.5 mW / m- K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 750 m2 / g;(E) an average pore diameter of 30 nm or less.

3. The article of claim 2 wherein the hydrophobic silica aerogel sheet includes at least two of the features (A) through (E).

4. The article of claim 3 wherein the hydrophobic silica aerogel sheet includes at least three of the features (A) through (E).

5. The article of claim 4 wherein the hydrophobic silica aerogel sheet includes at least four of the features (A) through (E).

6. The article of claim 5 wherein the hydrophobic silica aerogel sheet includes all of the features (A) through (E).

7. The article of claim 1 wherein the first alkoxy silane is methyl silicate 51 and the second alkoxysilane is methyltrimethoxysilane.

8. The article of claim 1 wherein the first alkoxy silane is methyl silicate 51 and the second alkoxysilane is methyltriethoxysilane.

9. The article of claim 1 wherein the first alkoxy silane is tetramethoxy silane and the second alkoxysilane is methyltrimethoxysilane.

10. The article of claim 1 wherein the first alkoxy silane is tetramethoxy silane and the second alkoxysilane is methyltriethoxysilane.

11. The article of claim 1 wherein the hydrophobic silica aerogel sheet has a thickness of between 2 mm and 5 mm.

12. The article of claim 1 wherein the visible transmission of the hydrophobic silica aerogel sheet is at least 98.6%, and the haze value is 2.5% or less.

13. The article of claim 12 wherein the visible transmission of the hydrophobic silica aerogel sheet is at least 99%, and the haze value is 2% or less.

14. The article of claim 2 wherein the water contact angle is at least 100°.

15. The article of claim 2 wherein the flexural modulus is 4500 or less.

16. The article of claim 2 wherein the specific surface area is at least 800 m2 / g.

17. The article of claim 2 wherein the average pore diameter is 27 nm or less.

18. An insulating glazing unit comprising two glass sheets and a between-pane space, the between-pane space being located betw een the two glass sheets, the insulating glazing unit further comprising a hydrophobic silica aerogel sheet received in the between-pane space, the hydrophobic silica aerogel sheet being formed from at least two alkoxysilanes and having a visible transmission of at least 97.8% and a haze value of 3% or less.

19. The insulating glazing unit of claim 18 wherein the hydrophobic silica aerogel sheet further includes at least one of the following features (A) through (E):(A) a water contact angle of at least 90°;(B) a thermal conductivity in air of 13.5 mW / m- K or less;(C) a flexural modulus of 6000 kPa or less;(D) a specific surface area of at least 750 m2 / g;(E) an average pore diameter of 30 nm or less.

20. The insulating glazing unit of claim 19 wherein the hydrophobic silica aerogel sheet includes at least two of the features (A) through (E).

21. The insulating glazing unit of claim 20 wherein the hydrophobic silica aerogel sheet further includes at least three of the features (A) through (E).

22. The insulating glazing unit of claim 21 wherein the hydrophobic silica aerogel sheet includes at least four of the features (A) through (E).

23. The insulating glazing unit of claim 22 wherein the hydrophobic silica aerogel sheet includes all of the features (A) through (E).

24. The insulating glazing unit of claim 18 wherein the first alkoxy silane is methyl silicate 51 and the second alkoxy silane is methyltrimethoxysilane.

25. The insulating glazing unit of claim 18 wherein the first alkoxysilane is methyl silicate 51 and the second alkoxy silane is methyltriethoxysilane.

26. The insulating glazing unit of claim 18 wherein the first alkoxy silane is tetramethoxysilane and the second alkoxysilane is methyltrimethoxysilane.

27. The insulating glazing unit of claim 18 wherein the first alkoxy silane is tetramethoxysilane and the second alkoxysilane is methyltriethoxysilane.

28. The insulating glazing unit of claim 18 wherein the visible transmission of the hydrophobic silica aerogel sheet is at least 98.6%, and the haze value is 2.5% or less.

29. The insulating glazing unit of claim 28 wherein the visible transmission of the hydrophobic silica aerogel sheet is at least 99%, and the haze value is 2% or less.

30. A method of making a hydrophobic silica aerogel, comprising the steps of: preparing a silica wet gel from a precursor material comprising a first alkoxysilane, solvent, catalyst and water, wherein the first alkoxysilane is selected from methyl silicate 51 and tetramethoxy silane; preparing a hydrophobic treatment solution from a second alkoxysilane and diluent, wherein the second alkoxysilane is selected from methyltrimethoxysilane and methyltri ethoxysilane; exposing the silica wet gel to the hydrophobic treatment solution to form a hydrophobic silica wet gel; aging either the silica wet gel or the hydrophobic silica wet gel for an aging time period; subjecting the hydrophobic silica wet gel to solvent extraction with an extraction solvent for an extraction time period of less than 24 hours; and subjecting the hydrophobic silica wet gel to drying to form a hydrophobic silica aerogel.

31. The method of claim 30 wherein the aging time period is at least 7 days (168 hours).

32. The method of claim 30 wherein the step of aging comprises aging the silica wet gel or the hydrophobic silica wet gel at room temperature.

33. The method of claim 30 wherein the step of aging comprises aging either the silica wet gel or the hydrophobic silica wet gel for an aging time period until structural changes of the silica wet gel or the hydrophobic silica wet gel no longer occur.

34. The method of claim 30 wherein the method is devoid of using a surfactant.

35. The method of claim 30 wherein the method is devoid of using a hydrophobic agent other than the hydrophobic treatment solution.

36. The method of claim 30 wherein each of the solvent, the diluent and the extraction solvent is methanol.

37. The method of claim 30 wherein the extraction time period is less than 20 hours.

38. The method of claim 30 wherein the hydrophobic silica aerogel is formed having a water contact angle of at least 90°.

39. The method of claim 30 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel such that less than 1% solvent remains within the hydrophobic silica aerogel.

40. The method of claim 30 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less.

41. The method of claim 30 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a visible transmission of at least 97.8% and a haze value of 3% or less.

42. A method of making a hydrophobic silica aerogel, comprising the steps of: preparing a first solution by mixing a first alkoxysilane and solvent, wherein the first alkoxysilane is selected from methyl silicate 51 and tetramethoxysilane; preparing a second solution by mixing solvent, ammonium hydroxide and water; mixing the first solution and the second solution together; allowing components in the first solution and the second solution to react to form a silica wet gel; preparing a third solution by combining methyltnmethoxysilane and diluent; adding the third solution to the silica wet gel;allowing the third solution to react with the silica wet gel to form a hydrophobic silica wet gel; aging either the silica wet gel or the hydrophobic silica wet gel for an aging time period; subjecting the hydrophobic silica wet gel to solvent extraction with an extraction solvent; subjecting the hydrophobic silica wet gel to drying to form a hydrophobic silica aerogel; and wherein the method is devoid of using a surfactant.

43. The method of claim 42 wherein the method is devoid of using a hydrophobic agent other than the third solution.

44. The method of claim 42 wherein the aging time period is at least 7 days (168 hours).

45. The method of claim 42 wherein the step of aging either the silica wet gel or the hydrophobic silica wet gel is performed at room temperature.

46. The method of claim 42 wherein the step of aging comprises aging either the silica wet gel or the hydrophobic silica wet gel for an aging time period until structural changes of the silica wet gel or the hydrophobic silica wet gel no longer occur.

47. The method of claim 42 wherein the step of subjecting the hydrophobic silica wet gel to solvent extraction is performed during an extraction time period of less than 24 hours.

48. The method of claim 42 wherein each of the solvent, the diluent and the extraction solvent is methanol.

49. The method of claim 42 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less.

50. The method of claim 42 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with less than 1% solvent remaining within the hydrophobic silica aerogel.

51. The method of claim 42 wherein the hydrophobic silica aerogel is formed having a water contact angle of at least 90°.

52. The method of claim 42 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a visible transmission of at least 97.8% and a haze value of 3% or less.

53. A method of making a hydrophobic silica aerogel, comprising the steps of: preparing a first solution by mixing a first alkoxysilane and solvent, wherein the first alkoxysilane is selected from methyl silicate 51 and tetramethoxysilane; preparing a second solution by mixing ammonium hydroxide and water; mixing the first solution and the second solution together; allowing components in the first solution and the second solution to react to form a silica wet gel; aging the silica wet gel for an aging time period; preparing a third solution by mixing catalyst and solvent; preparing a fourth solution by mixing a second alkoxysilane, catalyst and diluent, wherein the second alkoxysilane is selected from methyltrimethoxysilane and methyltri ethoxysilane; preparing a solvent exchange solution by mixing the third solution, the fourth solution and an extraction solvent; subjecting the silica wet gel to the solvent exchange solution for an extraction time period of less than 24 hours and allowing components in the solvent exchange solution to react with the silica wet gel to form a hydrophobic silica wet gel; andsubjecting the hydrophobic silica wet gel to drying to form a hydrophobic silica aerogel; and wherein the method is devoid of using a surfactant.

54. The method of claim 53 wherein the method is devoid of using a hydrophobic agent other than the second alkoxysilane in the solvent exchange solution.

55. The method of claim 53 wherein the aging time period is at least 7 days (168 hours).

56. The method of claim 53 wherein the step of aging the silica wet gel is performed at room temperature.

57. The method of claim 53 wherein the step of aging comprises aging the silica wet gel for an aging time period until structural changes of the silica wet gel no longer occur.

58. The method of claim 53 wherein the method is devoid of using a surfactant.

59. The method of claim 53 wherein each of the solvent, the diluent and the extraction solvent is methanol.

60. The method of claim 53 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less.

61. The method of claim 53 wherein the hydrophobic silica aerogel is formed having a water contact angle of at least 90°.

62. The method of claim 53 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with less than 1% solvent remaining within the hydrophobic silica aerogel.

63. The method of claim 53 wherein the step of subjecting the hydrophobic silica wet gel to drying forms the hydrophobic silica aerogel with a shrinkage value of 4% or less.

Citation Information

Patent Citations

  • Polymer aerogel for window glazings

    US20180093456A1

  • Optically-transparent, thermally-insulating nanoporous coatings and monoliths

    US20210207428A1