Leaching method for nickel laterite ore
The iron is removed through the atmospheric pressure hydrochloric acid leaching method and the heating hydrolysis step, combined with the recovery of magnesium oxide from nickel sedimentation slag as a neutralizing agent, which solves the problems of low nickel and cobalt concentration and large amount of neutralizing agent in the laterite nickel ore leaching process, and achieves efficient Nickel and cobalt recovery and hydrochloric acid recycling reduce production costs and equipment investment.
Patent Information
- Application Number
- PCT/CN2023/096913
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-05-29
- Publication Date
- 2024-10-31
AI Technical Summary
The existing laterite nickel ore leaching process has a low concentration of nickel and cobalt elements, a large amount of neutralizer, and the need to add oxidants, resulting in high process costs and large equipment investment, making it difficult to achieve large-scale industrial application.
The atmospheric pressure hydrochloric acid leaching method is used to remove iron through a heating and hydrolysis step, reducing the use of neutralizers. The nickel sedimentation slag is used to recover magnesium oxide as a neutralizer, avoiding the introduction of additional oxidants, achieving efficient recovery of nickel and cobalt and recycling of hydrochloric acid.
It improves the recovery rate of nickel and cobalt, reduces equipment investment and production costs, simplifies the treatment process, and realizes the possibility of large-scale industrial application.
Smart Images

Figure CN2023096913_31102024_PF_FP_ABST
Abstract
Description
A leaching method for laterite nickel ore Technical Field
[0001] The embodiments of the present application relate to the field of metallurgy technology, for example, a method for leaching laterite nickel ore. Background Art
[0002] Nickel and cobalt are widely used in various fields of industry and daily life, including stainless steel, non-ferrous metal alloys, new energy vehicles, electroplating, chemicals, and other fields. With the depletion of nickel sulfide ore resources, the development and utilization of laterite nickel ore, which accounts for over 70% of the world's nickel resources, has attracted much attention. The related wet sulfuric acid pressure leaching process for laterite nickel ore has high reaction temperatures and produces a large amount of sulfur-containing waste slag that cannot be directly utilized. The hydrochloric acid leaching process has the advantages of mild reaction conditions and easy medium regeneration and recycling, and has been widely used. However, due to the low concentration of hydrochloric acid and the fact that most of the iron and magnesium are leached during the leaching process, the subsequent nickel and cobalt concentrations are low, requiring the addition of more neutralizers, requiring large equipment footprints, and complex impurity handling.
[0003] At the same time, the methods disclosed in the related art for leaching laterite nickel ore with hydrochloric acid at normal pressure have many other defects. For example, in the clean production method for leaching laterite nickel ore with hydrochloric acid at normal pressure disclosed in CN 103215446A, hydrochloric acid leaching and high-temperature calcination process are used to treat the laterite nickel ore. The nickel and cobalt concentrations obtained by this process are low, and the leached impurities iron and magnesium cannot be separated from the nickel and cobalt, making subsequent refining difficult and costly. CN 112226630A discloses a method for extracting valuable metal elements from laterite nickel ore using hydrochloric acid leaching and acid-base regeneration cycle. The method uses hydrochloric acid pressure leaching for laterite nickel ore, resulting in high reaction temperature, low nickel and cobalt concentration, and the subsequent separation of iron slag and silicon slag together is more complicated, affecting the process economy. 109457111A discloses a method for extracting nickel and cobalt from laterite nickel ore using hydrochloric acid leaching. The method uses limonite and serpentine laterite nickel ores for leaching, and employs one or more of hydrogen peroxide, sodium peroxide, sodium hypochlorite, air, oxygen, and ozone to oxidize ferrous ions. Consequently, sodium ions are introduced, expensive and highly toxic hydrogen peroxide is used, or the reaction time is long, resulting in high economic costs. The method for treating laterite nickel ore leachate disclosed in CN 109457112A employs a stepwise oxidation-induced iron precipitation scheme, which requires the addition of seed crystals, resulting in a long overall process flow and the addition of numerous reagents.
[0004] Based on the above research, the relevant laterite nickel ore leaching process has problems such as low nickel and cobalt element concentration, large amount of neutralizer, and the need to add oxidant. It is necessary to provide a laterite nickel ore leaching method that is clean and efficient, has a high leaching rate and requires little equipment investment, so that the process has greater economic value and can be applied on a large scale in industry.
[0005] Summary of the Invention
[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0007] The embodiments of the present application provide a leaching method for laterite nickel ore, and more particularly, relate to a hydrochloric acid atmospheric pressure leaching method for laterite nickel ore. The leaching method can significantly reduce the solution processing volume, reduce the addition of neutralizing agents and the number of neutralizations, increase the nickel ion concentration in the solution, reduce the overall equipment investment, and reduce production costs.
[0008] In a first aspect, an embodiment of the present application provides a method for leaching laterite nickel ore, the method comprising the following steps:
[0009] (1) mixing laterite nickel ore with hydrochloric acid, and then leaching to obtain leachate and leaching residue;
[0010] (2) heating and hydrolyzing the leachate obtained in step (1) to obtain iron slag and a hydrolyzate;
[0011] (3) neutralizing the hydrolyzate obtained in step (2) and precipitating aluminum to obtain an aluminum precipitation solution;
[0012] (4) subjecting the aluminum precipitation liquid of step (3) to nickel precipitation to obtain nickel precipitation residue and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid;
[0013] The nickel precipitation slag is reused in the neutralization and aluminum precipitation process in step (3).
[0014] The leaching method described in the present application enables laterite nickel ore to be leached at normal pressure to obtain a leachate, avoids the introduction of a large amount of neutralizing agent to generate a substance that is difficult to filter and easily adsorbs iron hydroxide, simplifies the treatment process, reduces the introduction of impurities, and allows the hydrolyzate to contain a higher content of nickel and cobalt, thereby improving the nickel and cobalt recovery rate and significantly reducing equipment investment; and in the subsequent aluminum precipitation process, the present application uses the nickel precipitation slag generated in the nickel precipitation process, utilizes the manganese oxide therein to oxidize and precipitate iron, and minimizes the introduction of other oxidants. Therefore, the overall process of the present application is simple, can greatly reduce production costs and equipment investment, and can be applied on an industrial scale.
[0015] The laterite nickel ore in step (1) of the present application is ground laterite nickel ore powder.
[0016] Preferably, the hydrolyzate of step (2) is also added during the mixing process of step (1).
[0017] Since the present application uses heating hydrolysis to remove iron, no additional neutralizing agent is added and the pH is not adjusted, the iron removal is achieved. Therefore, the obtained hydrolyzate contains residual acid, so that the hydrolyzate can be reused in the leaching step of step (1), saving the amount of acid used and the leaching effect will not be affected.
[0018] Preferably, the concentration of the hydrochloric acid in step (1) is above 30%, for example, it can be 30%, 31%, 33%, 35% or 38%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, after the leaching in step (1), solid-liquid separation is further performed to obtain the leachate and leach residue.
[0020] Preferably, the leached residue in step (1) comprises silicon slag.
[0021] Preferably, the leaching temperature in step (1) is 80-120°C, for example, 80°C, 90°C, 100°C, 110°C or 120°C, and the leaching time is 1-3h, for example, 1h, 2h or 3h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the leaching in step (1) is carried out in a reactor.
[0023] Preferably, the temperature of the heating hydrolysis in step (2) is 130-180°C, for example, 130°C, 150°C, 170°C or 180°C, and the time is 2-5h, for example, 2h, 3h, 4h or 5h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] The temperature of the heating and hydrolysis in step (2) of the present application will affect the removal of iron, etc. If the temperature of the heating and hydrolysis is too high, the production energy consumption will be high and the equipment operability will be worse. If the temperature of the heating and hydrolysis is too low, the iron will not easily undergo hydrolysis reaction and the reaction effect will be poor.
[0025] Preferably, 20-50% of the hydrolyzate in step (2) is recycled to the leaching process in step (1), for example, 20%, 30% or 50%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] Preferably, in the hydrolyzate of step (2), the nickel concentration is 3-10 g / L, for example, 3 g / L, 5 g / L or 10 g / L, and the iron concentration is less than 20 g / L, for example, 18 g / L, 10 g / L or 5 g / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] The hydrolyzate described in the present application contains a relatively high concentration of nickel and a relatively low concentration of iron, which is beneficial to the subsequent preparation of battery-grade nickel compounds and also indicates that the iron removal efficiency of the present application is relatively high.
[0028] Preferably, after the heating and hydrolysis in step (2), solid-liquid separation is also performed to obtain the iron slag and hydrolyzate.
[0029] Preferably, the temperature for neutralizing the precipitated aluminum in step (3) is 40-80°C, for example, 40°C, 60°C or 80°C, and the time is 2-5h, for example, 2h, 3h or 5h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] Preferably, after the neutralization and aluminum precipitation in step (3), solid-liquid separation is also performed to obtain the aluminum slag and aluminum precipitation liquid.
[0031] Preferably, the regenerated magnesium oxide in step (4) is reused in the neutralization and aluminum precipitation process in step (3).
[0032] Preferably, the nickel deposition in step (4) includes a primary nickel deposition and a secondary nickel deposition performed sequentially.
[0033] Preferably, the secondary nickel precipitation obtains secondary nickel precipitation slag and the nickel precipitation liquid of step (4), and the secondary nickel precipitation slag is reused as a neutralizing agent in the neutralization aluminum precipitation process of step (3).
[0034] Preferably, the primary nickel precipitation slag obtained by the primary nickel precipitation includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate.
[0035] The two nickel precipitation processes described in this application not only realize the recovery of nickel-cobalt slag, but also can use the secondary nickel precipitation slag as a neutralizer to neutralize the precipitated aluminum. Therefore, the refining of the primary nickel precipitation slag in this application obtains battery-grade nickel compounds, and the secondary nickel precipitation slag is fully recycled, further avoiding the addition of additional oxidants.
[0036] Preferably, the nickel deposition agent used in the primary nickel deposition comprises the regenerated magnesium oxide described in step (4).
[0037] Preferably, the nickel deposition agent used in the secondary nickel deposition includes the regenerated magnesium oxide described in step (4).
[0038] In the nickel precipitation process, the present application uses the regenerated product finally obtained in the present application as a nickel precipitation agent, thereby achieving maximum resource utilization.
[0039] Preferably, the hydrochloric acid in step (4) is reused in the leaching process in step (1).
[0040] The leaching method described in the present application also ultimately produces hydrochloric acid, thereby achieving the recycling of hydrochloric acid.
[0041] Preferably, the pyrolysis temperature in step (4) is 600-800°C, for example, 600°C, 700°C or 800°C, and the time is 1-3h, for example, 1h, 2h or 3h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] As a preferred technical solution of this application, the leaching method comprises the following steps:
[0043] (1) mixing laterite nickel ore, hydrochloric acid and the hydrolyzed solution of step (2), and then leaching at a temperature of 80-120° C. for 1-3 hours, and performing solid-liquid separation after the leaching to obtain a leachate and silicon slag;
[0044] (2) heating and hydrolyzing the leachate from step (1) at a temperature of 130-180° C. for 2-5 hours, and then performing solid-liquid separation to obtain iron slag and hydrolyzate, wherein 20-50% of the hydrolyzate is reused in the leaching process of step (1);
[0045] In the hydrolyzate, the nickel concentration is 3-10 g / L, and the iron concentration is less than 20 g / L;
[0046] (3) neutralizing the remaining hydrolyzed liquid from step (2) at a temperature of 40-80° C. to precipitate aluminum for 2-5 hours, and then performing solid-liquid separation to obtain aluminum slag and aluminum precipitation liquid;
[0047] (4) subjecting the aluminum precipitation liquid of step (3) to a primary nickel precipitation and a secondary nickel precipitation in sequence to obtain a primary nickel precipitation residue, a secondary nickel precipitation residue and a nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid;
[0048] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization and aluminum precipitation process of step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;
[0049] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation and secondary nickel precipitation processes, and is also reused as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the hydrochloric acid obtained by pyrolysis is reused in the leaching process in step (1).
[0050] Compared with the related art, the embodiments of the present application have the following beneficial effects:
[0051] In response to the problems encountered in the related wet leaching process, the embodiments of the present application treat laterite nickel ore through a method of atmospheric pressure reaction, high temperature hydrolysis, and partial return recycling. Therefore, the application has the following advantages:
[0052] (1) The embodiments of the present application can respectively obtain relatively pure silicon slag, iron slag and aluminum slag, which reduces the pressure of subsequent waste slag treatment and is conducive to the final preparation of iron, aluminum and silicon products;
[0053] (2) The embodiments of the present application can reuse part of the hydrochloric acid, reduce the amount of hydrochloric acid added, and reduce production costs;
[0054] (3) The nickel and cobalt content in the hydrolyzate for subsequent neutralization treatment is high, which can significantly reduce equipment investment;
[0055] (4) Most of the iron is removed by hydrolysis, avoiding the introduction of large amounts of neutralizing agents to generate difficult-to-filter and easily adsorbed iron hydroxide, simplifying the treatment process, reducing the introduction of impurities, and improving the nickel and cobalt recovery rate;
[0056] (5) Using secondary nickel precipitation slag as a neutralizer for aluminum precipitation, and utilizing the manganese oxide therein to oxidize and precipitate iron, thus avoiding the introduction of other oxidants;
[0057] (6) The embodiments of the present application have the advantages of simple process, greatly reducing production costs and equipment investment, and being able to be applied on an industrial scale.
[0058] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0060] FIG1 is a flow chart of the leaching method described in Example 1 of the present application. DETAILED DESCRIPTION
[0061] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0062] Example 1
[0063] This embodiment provides a leaching method for laterite nickel ore. The flowchart of the leaching method is shown in FIG1 . The leaching method comprises the following steps:
[0064] (1) mixing the ground laterite nickel ore powder, 36% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 105° C. for 2 h, and filtering after the leaching to obtain a leachate and silicon slag;
[0065] (2) heating and hydrolyzing the leaching solution of step (1) at a temperature of 130° C. for 5 h, and then filtering to obtain iron slag and hydrolyzed solution, wherein 40% of the hydrolyzed solution is reused in the leaching process of step (1);
[0066] (3) neutralizing the remaining 60% of the hydrolyzed solution from step (2) at 80° C. for 2 h to precipitate aluminum, and then filtering to obtain aluminum slag and aluminum precipitation liquid;
[0067] (4) subjecting the aluminum precipitation liquid of step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation residue, secondary nickel precipitation residue and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 600° C. for 3 h to obtain regenerated magnesium oxide and hydrochloric acid;
[0068] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization and aluminum precipitation process of step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;
[0069] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation and secondary nickel precipitation processes, and is also reused as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the hydrochloric acid obtained by pyrolysis is reused in the leaching process in step (1).
[0070] Example 2
[0071] This embodiment provides a leaching method for laterite nickel ore, which comprises the following steps:
[0072] (1) mixing the ground laterite nickel ore powder, 31% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 120° C. for 3 h, and filtering after the leaching to obtain a leachate and silicon slag;
[0073] (2) heating and hydrolyzing the leachate obtained in step (1) at a temperature of 140° C. for 4 h, and then filtering the leachate to obtain iron slag and a hydrolyzate, wherein 30% of the hydrolyzate is reused in the leaching process in step (1);
[0074] (3) neutralizing the remaining 70% of the hydrolyzed solution from step (2) at 70° C. to precipitate aluminum for 2 hours, and then filtering to obtain aluminum slag and aluminum precipitation liquid;
[0075] (4) subjecting the aluminum precipitation liquid of step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation residue, secondary nickel precipitation residue and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 650° C. for 2.5 hours to obtain regenerated magnesium oxide and hydrochloric acid;
[0076] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization and aluminum precipitation process of step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;
[0077] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation and secondary nickel precipitation processes; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).
[0078] Example 3
[0079] This embodiment provides a leaching method for laterite nickel ore, which comprises the following steps:
[0080] (1) mixing the ground laterite nickel ore powder, 33% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 90° C. for 1 h, and filtering after leaching to obtain a leachate and silicon slag;
[0081] (2) heating and hydrolyzing the leachate obtained in step (1) at a temperature of 180° C. for 3 h, and then filtering the leachate to obtain iron slag and a hydrolyzate, wherein 20% of the hydrolyzate is reused in the leaching process in step (1);
[0082] (3) neutralizing the remaining 80% of the hydrolyzed solution from step (2) at 50° C. to precipitate aluminum for 5 hours, and then filtering to obtain aluminum slag and aluminum precipitation liquid;
[0083] (4) subjecting the aluminum precipitation liquid of step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 700° C. for 2 h to obtain regenerated magnesium oxide and hydrochloric acid;
[0084] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization and aluminum precipitation process of step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;
[0085] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation and secondary nickel precipitation processes; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).
[0086] Example 4
[0087] This embodiment provides a leaching method for laterite nickel ore, which comprises the following steps:
[0088] (1) mixing the ground laterite nickel ore powder, 36% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 105° C. for 1 hour, and filtering after the leaching to obtain a leachate and silicon slag;
[0089] (2) heating and hydrolyzing the leachate obtained in step (1) at a temperature of 150° C. for 3 h, and then filtering the leachate to obtain iron slag and a hydrolyzate, wherein 50% of the hydrolyzate is reused in the leaching process in step (1);
[0090] (3) neutralizing the remaining 50% of the hydrolyzed solution from step (2) at 40° C. for 2 h to precipitate aluminum, and then filtering to obtain aluminum slag and aluminum precipitation liquid;
[0091] (4) subjecting the aluminum precipitation liquid of step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 750° C. for 1.5 h to obtain regenerated magnesium oxide and hydrochloric acid;
[0092] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization and aluminum precipitation process of step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;
[0093] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation and secondary nickel precipitation processes; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).
[0094] Example 5
[0095] This embodiment provides a leaching method for laterite nickel ore, which comprises the following steps:
[0096] (1) mixing the ground laterite nickel ore powder, 30% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 120° C. for 2 h, and filtering after the leaching to obtain a leachate and silicon slag;
[0097] (2) heating and hydrolyzing the leachate obtained in step (1) at a temperature of 160° C. for 1 hour, and then filtering the leachate to obtain iron slag and a hydrolyzate, wherein 40% of the hydrolyzate is reused in the leaching process in step (1);
[0098] (3) neutralizing the remaining 60% of the hydrolyzed solution from step (2) at 80° C. for 2 h to precipitate aluminum, and then filtering to obtain aluminum slag and aluminum precipitation liquid;
[0099] (4) subjecting the aluminum precipitation liquid of step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 800° C. for 1 hour to obtain regenerated magnesium oxide and hydrochloric acid;
[0100] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization and aluminum precipitation process of step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;
[0101] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation and secondary nickel precipitation processes; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).
[0102] Example 6
[0103] This embodiment provides a leaching method for laterite nickel ore, which comprises the following steps:
[0104] (1) mixing the ground laterite nickel ore powder, 33% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 105° C. for 2 h, and filtering after the leaching to obtain a leachate and silicon slag;
[0105] (2) heating and hydrolyzing the leachate obtained in step (1) at a temperature of 150° C. for 5 h, and then filtering the leachate to obtain iron slag and a hydrolyzate, wherein 40% of the hydrolyzate is reused in the leaching process in step (1);
[0106] (3) neutralizing the remaining 60% of the hydrolyzed solution from step (2) at 60° C. to precipitate aluminum for 4 hours, and then filtering to obtain aluminum slag and aluminum precipitation liquid;
[0107] (4) subjecting the aluminum precipitation liquid of step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 650° C. for 2 h to obtain regenerated magnesium oxide and hydrochloric acid;
[0108] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization and aluminum precipitation process of step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;
[0109] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation and secondary nickel precipitation processes; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).
[0110] Example 7
[0111] This embodiment provides a leaching method for laterite nickel ore. The leaching method is the same as that of Example 1, except that the hydrolyzate of step (2) is not added in step (1) and the hydrolyzate is not recycled but replaced with hydrochloric acid of the same acid concentration.
[0112] Example 8
[0113] This embodiment provides a method for leaching laterite nickel ore. The leaching method is the same as that of Example 1 except that the temperature of the heating hydrolysis in step (2) is 110°C.
[0114] Example 9
[0115] This embodiment provides a method for leaching laterite nickel ore. The leaching method is the same as that of Example 1 except that the temperature of the heating hydrolysis in step (2) is 200°C.
[0116] Example 10
[0117] This embodiment provides a leaching method for laterite nickel ore, which is the same as that of Example 1 except that the nickel precipitation agent used in the first and second nickel precipitations in step (4) is commercial magnesium oxide, and the regenerated magnesium oxide in step (4) is not reused as a nickel precipitation agent.
[0118] Example 11
[0119] This embodiment provides a leaching method for laterite nickel ore, which is the same as that of Example 1 except that the hydrochloric acid in step (4) is not recycled to step (1) and the hydrochloric acid in step (1) is commercial hydrochloric acid.
[0120] Comparative Example 1
[0121] This comparative example provides a method for leaching laterite nickel ore. The leaching method is the same as Example 1 except that in step (2), magnesium oxide is added for precipitation to remove iron instead of heating and hydrolysis.
[0122] Comparative Example 2
[0123] This comparative example provides a leaching method for laterite nickel ore, which is the same as Example 1 except that the neutralizing agent used in the neutralization of aluminum precipitation in step (3) is commercial magnesium oxide, and the secondary nickel precipitation slag and regenerated magnesium oxide are not reused.
[0124] The nickel concentration and iron concentration in the hydrolyzed solution in step (2) in the above examples and comparative examples, the iron concentration in the feed solution after neutralization and aluminum precipitation in step (3), and the total nickel recovery rate are shown in the following table:
[0125] Table 1
[0126] From Table 1 we can see that:
[0127] (1) The leaching method described in the present application can obtain a leachate with a higher nickel content, and at the same time, the overall nickel recovery rate is increased, and the problem of the need to add a large amount of neutralizers and oxidants in the related art is overcome; it can be seen from Examples 1 and 7 that the present application removes iron by heating and hydrolysis, and the obtained hydrolyzate can be reused in step (1) without affecting the final result; it can be seen from Examples 1 and 8-9 that the temperature of heating and hydrolysis in the present application will affect the efficiency of iron removal, the nickel concentration and the nickel recovery rate; it can be seen from Examples 1 and 10 that in the first and second nickel precipitation processes of the present application, the final regenerated magnesium oxide is used. Compared with the additionally added commercial magnesium oxide, it can be seen that the use of regenerated magnesium oxide as a nickel precipitation agent will not have a significant impact on the results of the present application.
[0128] (2) It can be seen from Example 1 and Example 11 that when the hydrochloric acid obtained in step (4) is reused in step (1), a good recovery result is still obtained, and the overall process is not affected; it can be seen from Example 1 and Comparative Example 1 that Comparative Example 1 uses a conventional method to remove iron, which will generate difficult-to-filter substances, introduce impurities, and increase the reaction time. In addition, since most of the neutralizer is added in the form of a slurry, it will also reduce the concentration of nickel and cobalt in the solution after iron removal, affecting the recovery effect of the overall process and increasing the cost. However, the present application can avoid the addition of the neutralizer by heating and hydrolysis, and at the same time increase the content of nickel and cobalt in the leachate; it can be seen from Example 1 and Comparative Example 2 that the present application uses secondary nickel precipitation slag as a neutralizer, and can use the manganese oxide therein to oxidize and precipitate iron, thereby avoiding the introduction of other oxidants as much as possible, which not only reduces the cost but also improves the efficiency of the overall process.
[0129] In summary, the present application provides a leaching method for laterite nickel ore, which can significantly reduce the solution processing volume, reduce the addition of neutralizing agent and the number of neutralization times, increase the nickel ion concentration in the solution, reduce the overall equipment investment, and reduce production costs.
[0130] The above description is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Those skilled in the art should understand that any changes or replacements that can be easily thought of by those skilled in the art within the technical scope disclosed in the present application fall within the protection scope and disclosure scope of the present application.
Claims
1. A leaching method for laterite nickel ore, comprising the following steps: (1) mixing laterite nickel ore with hydrochloric acid, and then leaching to obtain leachate and leached residue; (2) heating and hydrolyzing the leaching solution of step (1) to obtain iron slag and hydrolyzate; (3) neutralizing the hydrolyzate obtained in step (2) and precipitating aluminum to obtain aluminum slag and aluminum precipitation liquid; (4) subjecting the aluminum precipitation liquid in step (3) to nickel precipitation to obtain nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid; The nickel precipitation slag is recycled for the neutralization and aluminum precipitation process in step (3).
2. The leaching method according to claim 1, wherein: The hydrolyzate of step (2) is also added during the mixing process of step (1).
3. The leaching method according to claim 1 or 2, wherein: The concentration of the hydrochloric acid in step (1) is above 30%.
4. The leaching method according to any one of claims 1 to 3, wherein: After the leaching in step (1), solid-liquid separation is also performed to obtain the leaching solution and leaching residue.
5. The leaching method according to any one of claims 1 to 4, wherein: The leached slag in step (1) includes silicon slag.
6. The leaching method according to any one of claims 1 to 5, wherein: The leaching temperature in step (1) is 80-120° C. and the leaching time is 1-3 h; Preferably, the leaching in step (1) is carried out in a reactor.
7. The leaching method according to any one of claims 1 to 6, wherein: The heating and hydrolysis in step (2) is carried out at a temperature of 130-180° C. and a time of 2-5 h; Preferably, 20-50% of the hydrolyzate in step (2) is recycled to the leaching process in step (1).
8. The leaching method according to any one of claims 1 to 7, wherein: In the hydrolyzate of step (2), the concentration of nickel is 3-10 g / L, and the concentration of iron is less than 20 g / L; Preferably, after the heating and hydrolysis in step (2), solid-liquid separation is also performed to obtain the iron slag and the hydrolyzate.
9. The leaching method according to any one of claims 1 to 8, wherein: The temperature of neutralizing the aluminum precipitation in step (3) is 40-80°C and the time is 2-5h; Preferably, after the neutralization of aluminum precipitation in step (3), solid-liquid separation is also performed to obtain the aluminum slag and aluminum precipitation liquid.
10. The leaching method according to any one of claims 1 to 9, wherein: The regenerated magnesium oxide in step (4) is reused in the neutralization and aluminum precipitation process in step (3).
11. The leaching method according to any one of claims 1 to 10, wherein: The nickel deposition in step (4) includes a primary nickel deposition and a secondary nickel deposition performed sequentially; Preferably, the secondary nickel precipitation obtains secondary nickel precipitation slag and the nickel precipitation liquid of step (4), and the secondary nickel precipitation slag is used as a neutralizing agent back to the neutralization aluminum precipitation process of step (3); Preferably, the primary nickel precipitation slag obtained by the primary nickel precipitation includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate.
12. The leaching method according to claim 11, wherein: The nickel precipitation agent used in the first nickel precipitation comprises the regenerated magnesium oxide described in step (4); Preferably, the nickel deposition agent used in the secondary nickel deposition comprises the regenerated magnesium oxide described in step (4).
13. The leaching method according to any one of claims 1 to 12, wherein: The hydrochloric acid in step (4) is reused in the leaching process in step (1); Preferably, the pyrolysis temperature in step (4) is 600-800° C. and the time is 1-3 h.
14. The leaching method according to any one of claims 1 to 13, comprising the following steps: (1) mixing laterite nickel ore, hydrochloric acid and the hydrolyzate of step (2), and then leaching at a temperature of 80-120° C. for 1-3 hours, and performing solid-liquid separation after the leaching to obtain a leachate and silicon slag; (2) heating the leaching solution of step (1) at a temperature of 130-180° C. for 2-5 hours, and then performing solid-liquid separation to obtain iron slag and hydrolyzate, wherein: 20-50% of the hydrolyzate is reused in the leaching process of step (1); In the hydrolyzate, the concentration of nickel is 3-10 g / L, and the concentration of iron is less than 20 g / L; (3) neutralizing the remaining hydrolyzate of step (2) at a temperature of 40-80° C. for 2-5 hours to precipitate aluminum, and then performing solid-liquid separation to obtain aluminum slag and aluminum precipitate liquid; (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid; The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate; The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process, and is also reused as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the hydrochloric acid obtained by pyrolysis is reused in the leaching process in step (1).
Citation Information
Patent Citations
Method for processing nickel cobalt extracted from laterite-nickel ore by chloride cycle desiliconisation ferrous process
CN101328548A
Comprehensive method for processing laterite nickel ore to produce electrolytic nickel through full wet method
CN102329955A
Method for removing iron and aluminum from mixed nickel cobalt hydroxide leaching solution
CN111500862A
Method for producing high-grade nickel hydroxide through leaching liquor of laterite nickel ore
CN111549238A
Method for treating iron-removed and aluminum-removed liquid
WO2018077241A1