Preparation method for modified polyethersulfone / polyetherimide polymer alloy

By introducing large dipole moment polar groups into the high Tg polymer molecular chain, and blending modified polyethersulfone and polyetherimide to construct fluorine-containing nanomicrodomains, the problem of polymer-based nanocomposites has been solved. The problems of dielectric performance degradation and high cost at high temperatures have been achieved by increasing the dielectric constant and reducing losses.

WO2024221958A1PCT designated stage expired Publication Date: 2024-10-31SHENZHEN INST OF ADVANCED TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/137601
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2023-12-08
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The dielectric energy storage performance of existing polymer-based nanocomposites deteriorates at high temperatures, and the addition of inorganic fillers weakens the processability and reliability. Moreover, the method of introducing large polar groups through molecular branches is costly and causes dielectric loss. promote.

Method used

By introducing large dipole moment polar groups into the high Tg polymer molecular chain, using the preparation method of modified polyethersulfone, using sulfonyl fluorine-containing chains and difluoro monomers for molecular structure design, combined with polymer alloy technology , constructing fluorine-containing nano-domains to increase the dielectric constant and reduce dielectric loss.

Benefits of technology

It achieves a significant increase in dielectric constant, maintaining high-temperature performance, reducing dielectric loss at low addition amounts, reducing production costs, simple operation, and wide applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137601_31102024_PF_FP_ABST
    Figure CN2023137601_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A preparation method for a modified polyethersulfone / polyetherimide polymer alloy, comprising: blending modified polyethersulfone and a high-Tg polyetherimide polymer, adding the mixture into DMAc according to the solid content of 15%-20%, stirring and dissolving at 80°C, then preparing a thin film on a glass plate by using a spin-coating method, finally, transferring the glass plate into a vacuum drying oven, standing overnight at 55°C, performing heat preservation at 100°C for 3-5 hours, and after performing curing at 180°C for 3-5 hours, obtaining a blended film, wherein the mass fraction of the modified polyethersulfone in the mixture is 1 wt%-30 wt%. A modified polyarylethersulphone polymer fragment of which the side chain is grafted with a large dipole moment polar group is used as an organic filler, and by adding a small amount of the modified polyarylethersulphone polymer fragment, the dielectric loss can be greatly reduced, the operation is simple, the broad spectrum is good, the effect on Tg is very small, and the dispersion and interface problems of an inorganic filler are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

A preparation method of modified polyethersulfone / polyetherimide polymer alloy Technical Field

[0001] The present invention belongs to high dielectric constant (ɛ r ), low dielectric loss (tanδ) composite dielectric materials, specifically a preparation method of a modified polyethersulfone / polyetherimide polymer alloy. Background Art

[0002] Polymer-based dielectric energy storage capacitors have been widely used in modern electronic and power systems due to their advantages such as fast charging and discharging speed and high power density. Especially in recent years, with the rise of the application of polymer-based dielectric energy storage capacitors in new energy vehicles, wind turbines, downhole oil and gas exploration and other fields, higher requirements have been put forward for the high-temperature energy storage performance of dielectric energy storage capacitors, such as operating temperatures as high as 150°C. The biaxially oriented polypropylene (BOPP, continuous operating temperature <85°C)-based dielectric energy storage capacitors that currently occupy the mainstream market are gradually unable to meet the performance requirements of new fields. Therefore, the development of high dielectric constant (ε r ), dielectric polymers with high operating temperature and low dielectric loss (tanδ) are important directions of current related research. Technical issues

[0003] Polymer-based nanocomposites enhance dielectric properties by adding fillers. They have been widely studied because they combine the advantages of high dielectric constant of ceramics and low loss of polymers. However, due to the surface energy difference between inorganic ceramics and polymer matrices, the poor dispersion and compatibility of ceramic fillers in the matrix have always been difficult to effectively solve in industry. Especially at high temperatures, their dielectric energy storage performance deteriorates rapidly. Moreover, the addition of inorganic fillers inevitably weakens the processability of the polymer matrix. Excessive fillers will lead to poor film flexibility, brittle texture, and reduced processability and reliability.

[0004] In order to avoid the above problems, molecular engineering can be used to directly g (Glass transition temperature) The introduction of large polar groups into the polymer molecular chain. However, the introduction of polar groups into the molecular branch chain will cause the matrix T g However, the dipole polarization is still inevitably affected by steric hindrance, which increases the dielectric loss of the film, and the cost of industrial production is high. Technical Solutions

[0005] In order to solve the problem that the introduction of polar groups into the molecular side chains in the prior art will cause the matrix T g In order to reduce the problems of large dielectric loss of dielectric polymers and high industrial production costs, the present invention provides a preparation method of modified polyethersulfone.

[0006] The preparation method of the modified polyether sulfone comprises the following steps:

[0007] Add a solvent, a water-carrying agent, a base, a difluoromonomer mixture and a dihydroxy monomer into a reactor and react at 140° C. for 3-4 hours, remove water, and keep warm at 160° C.-165° C. for 3-4 hours to obtain a dark brown viscous liquid. Pour the dark brown viscous liquid into acid, let it stand, filter and dry to obtain a light yellow solid. The light yellow solid is crushed and boiled in boiling water for 1 hour, and the process is repeated 3-5 times. The mixture is washed until the pH value is 7, and dried to obtain the modified polyethersulfone.

[0008] The difluoro monomer mixture includes difluoro monomers containing sulfonyl fluoride chains and difluoro monomers not containing sulfonyl fluoride chains.

[0009] Furthermore, the mass ratio of the solvent to the water-carrying agent is 5:1;

[0010] The molar ratio of the difluoromonomer mixture, the dihydroxy monomer and the base is 1:1:1.2;

[0011] The molar ratio of the difluoro monomer containing a sulfonyl fluoride chain in the difluoro monomer mixture is 2%-60%.

[0012] Further, the solvent is selected from N,N-dimethylacetamide;

[0013] The water-carrying agent is selected from toluene;

[0014] The base is selected from anhydrous potassium carbonate;

[0015] The difluoromonomer not containing a sulfonyl fluoride chain is selected from one or more of 4,4'-difluorodiphenyl sulfone, 1,3-difluorobenzene, 1,4-difluorobenzene, 4,4'-difluorodiphenylmethane and 4,4'-difluorodiphenyl ether;

[0016] The dihydroxy monomer is selected from one or more of 4,4'-dihydroxydiphenyl sulfone, bisphenol A, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenylmethane, 2,5-dihydroxytoluene, 2,7-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxyfluorene, 1,4-dihydroxybenzene and 1,4-bis(3-hydroxyphenoxy)benzene.

[0017] Furthermore, the difluoro monomer containing a sulfonyl fluoride chain in the preparation method of the modified polyethersulfone is prepared by the following method:

[0018] The 3,5-difluorobenzylamine was added to dichloromethane at a molar ratio of amino group of 3,5-difluorobenzylamine: sulfonyl group of sulfonyl-containing fluorine-containing grafting agent: triethylamine = 1:1:2.5, and the solid content of the mixed solution was 25%-30%.

[0019] Furthermore, the sulfonyl-containing fluorine-containing grafting agent is selected from one or more of 1,1,2,2,3,3,4,4,5,5,6,6,6-trifluorotrifluoro-1-hexanesulfonyl fluoride, perfluorooctanesulfonyl chloride, pentafluorobenzenesulfonyl chloride, trifluoromethanesulfonyl chloride, 1,1,2,2,3,3,4,4,5,5,6,6,7,7,7-pentadecafluoroheptane-1-sulfonyl fluoride, perfluorooctanesulfonyl fluoride, perfluoro-1-butanesulfonyl fluoride and trifluoromethylsulfonyl fluoride.

[0020] The present invention also provides a modified polyethersulfone.

[0021] The modified polyethersulfone is obtained by the preparation method of the modified polyethersulfone as described in any one of the above items.

[0022] Furthermore, the modified polyethersulfone has the following general structural formula:

[0023]

[0024] Wherein, R1 is selected from 、 、 、 、 、 、 、 、 、 and One or more of .

[0025] R2 is selected from 、 、 、 and One or more of .

[0026] R3 is selected from one or more of perfluoro-substituted alkyl groups or perfluoro-substituted aryl groups;

[0027] a and b are selected from any positive integers.

[0028] The present invention also provides a method for preparing a modified polyethersulfone / polyetherimide polymer alloy.

[0029] The preparation method of the modified polyethersulfone / polyetherimide polymer alloy comprises the following steps:

[0030] The modified polyethersulfone described above is mixed with high T g(210-225℃) polymer polyetherimide blend, the mixture is added to DMAc at a solid content of 15%-20%, stirred and dissolved at 80℃, and then a film is made on a glass plate by a doctor blade method. Finally, the glass plate is transferred to a vacuum oven, and after being heated at 55℃ overnight, kept at 100℃ for 3-5 hours, and cured at 180℃ for 3-5 hours, a blend film is obtained.

[0031] Wherein, the mass fraction of the modified polyethersulfone in the mixture is 1wt%-30wt%.

[0032] Furthermore, the mass fraction of the modified polyethersulfone in the mixture is 2wt%-4wt%. Beneficial effects

[0033] 1. The preparation of difluoromonomers containing sulfonyl fluoride chains can be completed at room temperature.

[0034] 2. Modified polyethersulfone can achieve significant effects at a relatively low addition amount, so it has good dispersibility and little effect on the mechanical properties and Tg of the film, thus maintaining the superior performance of the base material at high temperatures to the greatest extent.

[0035] 3. Modified polyethersulfone can be regarded as a polymer modifier with good industrial compatibility, broad spectrum, simple operation and high application potential. Compared with direct grafting modification on the matrix polymer molecular chain, the production cost is greatly reduced.

[0036] 4. The self-assembly of perfluoroalkyl chains to construct polar nano-microdomains with large dipole moments solves the problem of dielectric materials with large dipole moment groups. r and tanδ, in order to improve the composite material ɛ r while reducing its tanδ purpose. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] FIG1 is a hydrogen spectrum of a difluoromonomer containing a sulfonyl fluoride chain provided in Example 1 (deuterated reagent: deuterated dimethyl sulfoxide (DMSO-d6));

[0038] FIG2 is a fluorine spectrum of a difluoromonomer containing a sulfonyl fluoride chain provided in Example 1 (deuterated reagent: deuterated dimethyl sulfoxide (DMSO-d6));

[0039] FIG3 is a carbon spectrum of a difluoromonomer containing a sulfonyl fluoride chain provided in Example 1 (deuterated reagent: deuterated dimethyl sulfoxide (DMSO-d6));

[0040] FIG4 is a high-resolution mass spectrum (negative mode, hydrogen reduction) of a difluoromonomer containing a sulfonyl fluoride chain provided in Example 1;

[0041] FIG5 is a fluorine spectrum of the modified poly(aryl ether sulfone) provided in Example 1 (deuterated reagent: deuterated dimethyl sulfoxide (DMSO-d6)). [0041.1] [Corrected 29.01.2024 according to Rule 91] FIG6 is a reaction flow chart of the introduction of fluorinated side chains by nucleophilic substitution polymerization of a dihydroxy monomer (HO-R1-OH) and a difluoromonomer mixture (FBA-F and F-R2-F) under alkaline conditions to form the modified poly(arylethersulfone) (PES-F); [0041.2] [Corrected 29.01.2024 according to Rule 91] Figure 7 is a synthetic route for a difluoromonomer containing a sulfonyl fluoride chain (FBA-F). Best Mode for Carrying Out the Invention

[0042] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings, but they should not be understood as limiting the scope of implementation of the present invention.

[0043] The present invention intends to directly in high T g (Glass transition temperature 210℃-225℃) The introduction of large dipole moment polar groups into the polymer molecular chain solves the problems of poor compatibility, low processability, poor reliability and high production cost of dielectric polymers in the existing technology. g Relaxation can also achieve the purpose of improving the dielectric constant of polymers while avoiding a series of problems caused by the introduction of inorganic fillers. Assisted by polymer alloy technology, the advantages of various polymer materials can be combined with each other, which is more conducive to reducing production costs, expanding the scope of use, and lowering the threshold for industrialization. Therefore, it has broad application prospects.

[0044] The basic principle of the present invention is: to synthesize a new type of polyarylethersulfone (PES) modified polymer through molecular structure design, graft a fluorine-containing grafting agent with a large dipole moment polar group (-SO2) on the molecular side chain, blend it with a polyetherimide (PEI) polymer with excellent high-temperature performance, and construct a fluorine nano-microregion containing polar groups through the difference in surface energy between the fluorine-containing chain segment and the main chain, and use the "fluorine migration" method to achieve controllable distribution of nano-microregions containing polar groups. This will increase the band gap width of the polymer dielectric film and optimize the high-temperature dielectric energy storage performance. The molecular structure design method avoids the dispersion and interface problems of inorganic fillers. Fluorine is a large-volume atom, which leads to an increase in the free volume in the microregion and the polar group sub-T g Polarization resistance is reduced, achieving the purpose of increasing dielectric constant while reducing dielectric loss. At the same time, a small amount of modified polyarylethersulfone (PES-F) polymer segment with a large dipole moment polar group grafted on the side chain is used as an organic filler to significantly reduce dielectric loss. It is simple to operate, has good broad spectrum, and has a great effect on T gThe impact is small.

[0045] The present invention provides a modified polyarylethersulfone.

[0046] [Corrected 29.01.2024 in accordance with Rule 91] Under alkaline conditions, a dihydroxy monomer (HO-R1-OH) and a difluoromonomer mixture (FBA-F and F-R2-F) undergo nucleophilic substitution polymerization to form the modified poly(arylethersulfone) (PES-F), introducing fluorinated side chains. The reaction flow is shown in Figure 6.

[0047] [Corrected 29.01.2024 in accordance with Article 91]

[0048] The preparation method of modified polyarylethersulfone comprises the following steps:

[0049] First, N,N-dimethylacetamide (DMAc) was added to a three-necked flask at a solids content of 25%-30%. Simultaneously, toluene was added at a mass ratio of DMAc:toluene = 5:1. Finally, a mixture of difluoromonomers (FBA-F and F-R2-F): dihydroxy monomer: anhydrous potassium carbonate was added at a molar ratio of 1:1:1.2. A reaction apparatus was set up and nitrogen purged for 20 minutes while stirring. The temperature was then raised to 140°C for 3-4 hours, during which water produced during the reaction was removed with toluene. This stage is crucial for increasing the molecular weight of the product, with increased molecular weight as the reaction time increases. In the second step, the temperature was raised to 160-165°C and maintained for 3-4 hours, resulting in a dark brown, viscous liquid. While still hot, the liquid was slowly poured into dilute hydrochloric acid and allowed to stand overnight. Filtering, washing, and drying yielded a pale yellow solid. Finally, the product was pulverized and boiled in boiling water for 1 hour, repeated 3-5 times. The solid was then washed until the pH reached 7 and dried to obtain PES-F powder.

[0050] The molar ratio (b / (a+b)) of the difluoromonomer containing a sulfonyl fluoride chain (FBA-F) in the difluoromonomer mixture is 2%-60%, preferably 30%-40%, a and b are the number of repeating structural units, which are any positive integers, and the molecular weight of the modified polyarylethersulfone is between 6000 and 50000.

[0051] The dihydroxy monomer (HO-R1-OH) is selected from one or more of 4,4'-dihydroxydiphenyl sulfone, bisphenol A, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenylmethane, 2,5-dihydroxytoluene, 2,7-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxyfluorene, 1,4-dihydroxybenzene and 1,4-bis(3-hydroxyphenoxy)benzene.

[0052] The difluoromonomer (F-R2-F) not containing a sulfonyl fluoride chain is selected from one or more of 4,4'-difluorodiphenyl sulfone, 1,3-difluorobenzene, 1,4-difluorobenzene, 4,4'-difluorodiphenylmethane and 4,4'-difluorodiphenyl ether.

[0053] [Corrected 29 January 2024, in accordance with Rule 91] A typical aminosulfonylation reaction (also known as the Hinsberg reaction) is used to covalently graft a sulfonyl-containing fluorine chain onto 3,5-difluorobenzylamine (3,5-DFBA). The synthetic route for the difluoromonomer containing a sulfonyl fluoride chain (FBA-F) is shown in Figure 7.

[0054] [Corrected 29.01.2024 in accordance with Article 91]

[0055] The synthesis method of a difluoromonomer containing a sulfonyl fluoride chain (FBA-F) comprises the following steps:

[0056] First, the required amount of dichloromethane solvent is calculated based on the solids content (25%-30%). The mixture is added at a molar ratio of 1:1:2.5:3,5-difluorobenzylamine (amino group of 3,5-difluorobenzylamine): sulfonyl group of the sulfonyl-containing fluorinated grafting agent: triethylamine. The reaction is stirred at room temperature for 1-4 days. The liquid phase is then poured into a prepared treatment solution (a mixture of ether: water: ice: 85% H₃PO₄ = 75:50:25:2 by volume). The mixture is shaken several times, and the aqueous phase is extracted three times with ether. The organic phases are then combined. The organic phases are then washed with deionized water and saturated sodium chloride, dried over anhydrous magnesium sulfate, and the solvent removed by rotary evaporation. Finally, the mixture is vacuum-dried at 60-70°C for 10-15 hours to yield the purified difluoromonomer containing sulfonyl fluoride chains (FBA-F).

[0057] The sulfonyl-containing fluorine-containing grafting agent is selected from one or more of 1,1,2,2,3,3,4,4,5,5,6,6,6-trifluorotrifluoro-1-hexanesulfonyl fluoride, perfluorooctanesulfonyl chloride, pentafluorobenzenesulfonyl chloride, trifluoromethanesulfonyl chloride, 1,1,2,2,3,3,4,4,5,5,6,6,7,7,7-pentadecafluoroheptane-1-sulfonyl fluoride, perfluorooctanesulfonyl fluoride, perfluoro-1-butanesulfonyl fluoride and trifluoromethylsulfonyl fluoride.

[0058] The present invention also provides a method for preparing a modified polyarylethersulfone / polyetherimide polymer alloy. The method for preparing the modified polyarylethersulfone / polyetherimide polymer alloy comprises the following steps:

[0059] The modified polyarylethersulfone (PES-F) synthesized above was mixed with high T gThe polymer polyetherimide was blended and added to DMAc at a solids content of 15%-20%, stirring and dissolving at 80°C. A film was then formed on a glass plate using a doctor blade method. The glass plate was transferred to a vacuum oven and cured at 55°C overnight, 100°C for 3-5 hours, and 180°C for 3-5 hours to produce a blended film.

[0060] The mass fraction of PF in the blend is 1 wt%-30 wt%, more preferably 2 wt%-4 wt%.

[0061] Examples 1-7 were provided according to the above preparation method.

[0062] Example 1

[0063] To a single-necked flask, 3,5-DFBA (0.01 mol), CH2Cl2 (7.2 ml), and triethanolamine (TEA, 0.025 mol) were added in appropriate proportions. A magnetic stirrer was then placed. Perfluorobutylsulfonyl fluoride (PBSF, 0.01 mol) was then slowly added while stirring. After displacing the air in the flask with nitrogen, the reaction was sealed and stirred at room temperature for 4 days to yield a pale yellow, transparent liquid. The liquid phase was then transferred to a separatory funnel, and ether (75 ml), water (50 ml), ice (25 g), and 85% H3PO4 (2 ml) were added. The mixture was shaken several times and allowed to stand for separation into two phases. The aqueous phase was extracted three times with Et2O. The combined organic phases were washed sequentially with 20 ml of deionized water and 20 ml of saturated NaCl, then dried over anhydrous magnesium sulfate and filtered. Finally, the CH2Cl2 solvent was removed by rotary evaporation and the product was dried under vacuum at 65 °C for 10 h to obtain a light yellow solid product N-(3,5-difluorophenyl)-1,1,2,3,3,4,4-non-fluorobutane-1-sulfonamide (FBA-F).

[0064] Next, FBA-F (0.01 mol), 4,4'-difluorodiphenyl sulfone (DOD, 0.015 mol), 4,4'-dihydroxybiphenyl (FPS, 0.025 mol), DMAc (30 g), MB (5 g), and anhydrous potassium carbonate (0.03 mol) were added sequentially to a three-necked flask to set up a reaction apparatus. The mixture was stirred and purged with nitrogen for 20 minutes. The temperature was then raised to 140°C for 4 hours. Water produced during the reaction was removed with toluene. The temperature was then raised to 160-165°C and maintained for 4 hours, yielding a dark brown viscous liquid. This liquid was then slowly poured into dilute hydrochloric acid (1 mol / L) while still hot and allowed to stand overnight. A pale yellow solid was obtained after filtration, washing, and drying. Finally, the product was pulverized and boiled in boiling water for 1 hour. This process was repeated four times until the pH reached 7. The solid was then dried to obtain PES-F powder.

[0065] PES-F (0.2g) and PEI (9.8g) were added to DMAc (50g) and stirred at 80°C until completely dissolved. After cooling, a thin film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain a 2wt% PES-F@PEI blend film. Measured: ɛ r =2.95, tanδ=0.0075 (150℃, 560kHz), T g =216.9℃.

[0066] The hydrogen spectrum, fluorine spectrum, carbon spectrum and high-resolution mass spectrum of the difluoro monomer containing sulfonyl fluoride chain and the fluorine spectrum of the modified polyarylethersulfone were measured. The test results are shown in Figures 1 to 5:

[0067] The hydrogen spectrum results of the difluoro monomer containing sulfonyl fluoride chain in Figure 1 are: 1 H NMR (400 MHz, DMSO) δ 10.31 (s, 1H), 7.19 (t, J = 10.4 Hz, 1H), 7.07 (d, J = 6.5 Hz, 2H), 4.46 (s, 2H);

[0068] The fluorine spectrum results of the difluoro monomer containing sulfonyl fluoride chain in Figure 2 are: 19 F NMR (376 MHz, DMSO) δ -80.37 (t, J = 9.6 Hz, 3F), -109.49 (t, J = 8.7 Hz, 2F), -113.24 (t, J = 13.2 Hz, 2F), -121.21 (dd, J = 10.9, 6.6 Hz, 2F), -125.72 – -125.83 (m, 2F);

[0069] The carbon spectrum results of the difluoro monomer containing sulfonyl fluoride chain in Figure 3 are: 13 C NMR (101 MHz, DMSO) δ 163.89, 163.76, 161.44, 161.31, 141.98, 141.89, 141.80, 118.70, 118.37, 118.04, 115.83, 115.50, 115.17, 114.40, 114.05, 113.70, 110.64, 110.57, 110.45, 110.38, 103.32, 103.07, 102.81, 46.16;

[0070] The fluorine spectrum results of the modified polyarylethersulfone in Figure 5 are: 19F NMR (376 MHz, DMSO) δ -80.31 (t, J = 9.5 Hz, 3F), -109.77 (t, J = 8.2 Hz, 1F), -113.38 (t, J = 13.1 Hz, 2F), -121.15 – -121.27 (m, 2F), -125.75 (dd, J = 14.6, 11.4 Hz, 2F). Modes for Carrying Out the Invention

[0071] Example 2

[0072] PES-F (0.4 g) and PEI (9.6 g) prepared in Example 1 were added to DMAc (50 g) and stirred at 80°C until completely dissolved. After cooling, a thin film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain a 4 wt% PES-F@PEI blend film. The measured value was: ɛ r =3.2, tanδ=0.001 (150℃, 560kHz), T g =214.5℃.

[0073] Example 3

[0074] PES-F (0.6 g) and PEI (9.4 g) prepared in Example 1 were added to DMAc (50 g) and stirred at 80°C until completely dissolved. After cooling, a thin film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain a 6 wt% PES-F@PEI blend film. The measured value was: ɛ r =3.25, tanδ=0.004 (150℃, 560kHz), T g =209.1℃.

[0075] Example 4

[0076] PES-F (0.8 g) and PEI (9.2 g) prepared in Example 1 were added to DMAc (50 g) and stirred at 80°C until completely dissolved. After cooling, a thin film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain an 8 wt% PES-F@PEI blend film. The measured value was: ɛ r =3.3, tanδ=0.004 (150℃, 560kHz), T g =209.2℃.

[0077] Example 5

[0078] PES-F (1 g) and PEI (9 g) prepared in Example 1 were added to DMAc (50 g) and stirred at 80°C until completely dissolved. After cooling, a thin film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain a 10 wt% PES-F@PEI blend film. The measured value was: ɛ r =3.45, tanδ=0.004 (150℃, 560kHz), T g =200.9℃.

[0079] Example 6

[0080] PES-F (1.2 g) and PEI (8.8 g) prepared in Example 1 were added to DMAc (50 g) and stirred at 80°C until completely dissolved. After cooling, a thin film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain a 12 wt% PES-F@PEI blend film. The measured value was: ɛ r =3.5, tanδ=0.0025 (150℃, 560kHz), T g =201.9℃.

[0081] Example 7

[0082] PES-F (3 g) and PEI (7 g) prepared in Example 1 were added to DMAc (50 g) and stirred at 80°C until completely dissolved. After cooling, a thin film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain a 30 wt% PES-F@PEI blend film. The measured value was: ɛ r =3.5, tanδ=0.0125 (150℃, 560kHz), T g =172.8℃. Industrial Applicability

[0083] Comparative Example 1

[0084] PEI (10 g) was added to DMAc (50 g) and stirred at 80°C until completely dissolved. After cooling, a film was formed on a glass plate using a doctor blade method. Finally, the glass plate was transferred to a vacuum oven and heated at 55°C overnight, kept at 100°C for 4 hours, and cured at 180°C for 4 hours to obtain a PEI film. Measured: ɛ r =2.88, tanδ=0.0055 (150℃, 560kHz), T g =227.5℃.

[0085] The electrical properties, physicochemical properties, and mechanical properties of the modified poly(arylethersulfone) / polyetherimide) composite films prepared in Examples 1-7 and Comparative Example 1 were measured, wherein the electrical properties were tested in accordance with the SJ / T 1147-1993 standard, and the mechanical properties were tested in accordance with the GB / T 13022-1991 standard.

[0086] Experimental results:

[0087] Case name Dielectric constant (ɛr) @150℃ Dielectric loss (tanδ) @150℃ Glass transition temperature (Tg / ℃) Breaking strength (Mpa) @25℃ Breaking elongation (%) @25℃ Young's modulus (Mpa) @25℃ Example 12% PES-F@PEI2.95 0.00752 16.91 12.42 16.90 1508 Example 24% PES-F@PEI3.20 0.00102 14.51 10.64 13.52 1487 Example 36% PES-F@PEI3.25 0.0040 209.11 13.75 11.63 1730 Example 48% PES-F@PEI3.30 0.0040 209.211 0.6016.861580Example 510%PES-F@PEI3.450.0040200.9111.0211.941589Example 612%PES-F@PEI3.500.0025201.987.9713.781315Example 730%PES-F@PEI3.500.0125172.881.307.631401Comparative Example 1PEI2.880.0055227.5114.3515.341775

[0088] The preparation method of the modified polyethersulfone / polyetherimide polymer alloy provided by the present invention constructs a large dipole moment polar nano-microdomain through self-assembly of perfluoroalkyl chains, thereby solving the problem of dielectric materials with large dipole moment groups. r and tanδ, in order to improve the composite material ɛ r At the same time, the purpose of reducing its tanδ.

Claims

1. A method for preparing modified polyethersulfone, characterized in that: The following steps are involved: Add a solvent, a water-carrying agent, a base, a difluoro monomer mixture and a dihydroxy monomer into a reactor, react at 140° C. for 3-4 hours, and keep warm at 160° C.-165° C. for 3-4 hours to obtain a dark brown viscous liquid, pour the dark brown viscous liquid into an acid, let it stand, filter and dry to obtain a light yellow solid, crush the light yellow solid and boil it with boiling water for 1 hour, repeat 3-5 times, wash until the pH is 7, and dry to obtain the modified polyether sulfone. The difluoro monomer mixture includes difluoro monomers containing sulfonyl fluoride chains and difluoro monomers not containing sulfonyl fluoride chains.

2. The method for preparing modified polyether sulfone according to claim 1, characterized in that: The mass ratio of the solvent to the water-carrying agent is 5:1; The molar ratio of the difluoro monomer mixture, the dihydroxy monomer and the base is 1:1:1.2; The molar ratio of the difluoro monomer containing a sulfonyl fluoride chain in the difluoro monomer mixture is 2%-60%.

3. The method for preparing modified polyethersulfone according to claim 1, characterized in that: The solvent is selected from N,N-dimethylacetamide; The water-carrying agent is selected from toluene; The base is selected from anhydrous potassium carbonate; The difluoro monomer without a sulfonyl fluoride chain is selected from one or more of 4,4'-difluorodiphenyl sulfone, 1,3-difluorobenzene, 1,4-difluorobenzene, 4,4'-difluorodiphenylmethane and 4,4'-difluorodiphenyl ether; The dihydroxy monomer is selected from one or more of 4,4'-dihydroxydiphenyl sulfone, bisphenol A, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenylmethane, 2,5-dihydroxytoluene, 2,7-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxyfluorene, 1,4-dihydroxybenzene and 1,4-bis(3-hydroxyphenoxy)benzene.

4. The method for preparing the modified polyether sulfone according to any one of claims 1 to 3, characterized in that: The difluoro monomer containing a sulfonyl fluoride chain is prepared by the following method: The amino group of 3, 5-difluorobenzylamine: the sulfonyl group of the sulfonyl-containing fluorine-containing grafting agent: triethylamine are added into dichloromethane in a molar ratio of 1:1:2.5, and the solid content in the mixed solution is 25%-30%.

5. The method for preparing modified polyethersulfone according to claim 4, characterized in that: The sulfonyl-containing fluorine-containing grafting agent is selected from one or more of 1,1,2,2,3,3,4,4,5,5,6,6,6-trifluorotrifluoro-1-hexanesulfonyl fluoride, perfluorooctanesulfonyl chloride, pentafluorobenzenesulfonyl chloride, trifluoromethanesulfonyl chloride, 1,1,2,2,3,3,4,4,5,5,6,6,7,7,7-pentadecafluoroheptane-1-sulfonyl fluoride, perfluorooctanesulfonyl fluoride, perfluoro-1-butanesulfonyl fluoride and trifluoromethylsulfonyl fluoride.

6. A modified polyethersulfone, characterized in that: The modified polyethersulfone is obtained by the preparation method according to any one of claims 1 to 3.

7. The modified polyethersulfone according to claim 6, characterized in that It has the following general structural formula: Wherein R1 is selected from 、 、 、 、 、 、 、 、 、 and One or more of; R2 is selected from 、 、 、 and One or more of; R3 is selected from one or more of perfluoro-substituted alkyl groups or perfluoro-substituted aryl groups; a and b are selected from any positive integers.

8. A method for preparing a modified polyethersulfone / polyetherimide polymer alloy, characterized in that: The following steps are involved: The modified polyethersulfone according to claim 6 is mixed with a high T g The polymer polyetherimide was blended, and the mixture was added to DMAc at a solid content of 15%-20%, stirred and dissolved at 80°C, and then a film was made on a glass plate by a doctor blade method. Finally, the glass plate was transferred to a vacuum oven, and after being heated at 55°C overnight, kept at 100°C for 3-5 hours, and cured at 180°C for 3-5 hours, a blended film was obtained. Wherein, the mass fraction of the modified polyethersulfone in the mixture is 1wt%-30wt%.

9. The method for preparing the modified polyethersulfone / polyetherimide polymer alloy according to claim 8, characterized in that: The mass fraction of the modified polyethersulfone in the mixture is 2wt%-4wt%.

Citation Information

Patent Citations

  • Perfluorooctane-based compound and method for preparing perfluorooctane-containing terminated polyaryl ether sulphone

    CN104496782A

  • Polyetherimide dielectric composite material as well as preparation method and application thereof

    CN115260762A

  • Pollution-resistant polyethersulfone ultrafiltration membrane

    CN115646223A

  • Preparation method of modified polyether sulfone / polyetherimide polymer alloy

    CN116675861A

  • Polyetherimide Compatible Polymer Blends for Capacitor Films

    US20170084394A1