Method for preparing silicon carbide membrane support from active coke fly ash

By using activated coke fly ash as a pore-forming agent for the silicon carbide membrane support, combined with sintering aids and sintering processes, the problems of low filtration efficiency and difficult processing of activated coke fly ash in steel plant flue gas purification are solved, and the The preparation of high-performance silicon carbide membrane support is suitable for steel coking, petrochemical and other fields.

WO2024222162A1PCT designated stage expired Publication Date: 2024-10-31NANJING TECH UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/077844
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-02-20
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

When the existing technology uses activated coke fly ash in flue gas purification in steel plants, there are problems such as low filtration efficiency, water waste, pollution and treatment difficulties, and it fails to effectively utilize the high added value of activated coke fly ash.

Method used

Activated coke fly ash is used as a pore-forming agent for the silicon carbide film support, and the silicon carbide film is prepared by ball milling to uniform particle size, combined with sintering aids such as nano-zirconia and alumina, and using mechanical extrusion and muffle furnace sintering processes. Support body.

Benefits of technology

The prepared silicon carbide membrane support has high porosity, high mechanical strength, and excellent gas permeability. It is suitable for high-temperature flue gas purification, and the process is simple and easy for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024077844_31102024_PF_FP_ABST
    Figure CN2024077844_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a silicon carbide membrane support from active coke fly ash. The method comprises using active coke regenerated fly ash as a pore-forming agent, micron-sized silicon carbide powder as a main aggregate, one or more of nano-zirconia, alumina, and magnesium oxide as sintering aids, and an aqueous polyvinyl alcohol solution as a binder, uniformly mixing same to obtain a prefabricated material, extrusion-molding the prefabricated material to obtain a support green body, then putting the support green body into a drying oven for constant-temperature drying, and finally putting the dried support green body into a high-temperature furnace for programmed sintering. The method utilizes active coke fly ash, which is captured by filtration during active coke desulfurization and denitrification and regeneration gas purification in coking plants, as a pore-forming agent, solving the disposal problem of active coke fly ash (which contains trace amounts of heavy metal ions and adsorbs high concentrations of SO2 and NH3) and effectively reducing the preparation cost of silicon carbide ceramic membrane supports. Additionally, the prepared silicon carbide ceramic membrane has relatively high mechanical strength and gas permeability and thus has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing silicon carbide membrane support from activated coke fly ash Technical Field

[0001] The invention belongs to the field of porous ceramic separation membrane preparation and relates to a method for preparing a silicon carbide membrane support body by using activated coke fly ash. Background Art

[0002] High-temperature silicon carbide membranes are materials capable of directly filtering and purifying high-temperature flue gases. They are widely used in high-temperature gas-solid separation units in the fields of steel metallurgy, petrochemicals, coal chemical industry, polysilicon, and waste incineration. High-temperature silicon carbide ceramic membrane technology effectively avoids the waste of water resources and sludge treatment caused by spray cooling, improves energy efficiency, and protects the long-term stability of downstream heat exchangers and catalysts. It is an advanced and efficient gas-solid separation technology. During the preparation process of the high-temperature silicon carbide membrane support, a large amount of pore-forming agent must be added to form a high porosity and uniform pore structure. The composition, particle size distribution, and addition amount of the pore-forming agent have a significant impact on the gas permeability of the silicon carbide membrane.

[0003] Steel plants generate a large amount of high-temperature flue gas during sintering and coal coking processes. Activated coke desulfurization and denitrification technology is used to remove SO2 and mercury from the flue gas and remove nitrogen oxides (NO x ) catalytic reduction, so that SO2 and nitrogen oxides (NO x ) can meet emission standards. The fluidized bed process is then coupled to heat the adsorption saturated activated coke in the regeneration tower for regeneration. The activated coke desorbs a high-concentration SO2 mixed gas in the heating section of the regeneration tower, which contains activated coke fly ash formed by the wear of the activated coke during the fluidization process. The desorbed activated coke particles continue to circulate to the primary and secondary adsorption towers for adsorption, and the cycle repeats for a long time. The high-concentration SO2 mixed gas (containing a large amount of activated coke fly ash) generated by the desorption of activated coke in the heating section of the regeneration tower, if directly entering the downstream process to prepare ammonium sulfate / sulfuric acid, will result in low purity of the ammonium sulfate / sulfuric acid product. The original process uses spray-coupled plate and frame filtration technology, which not only has low filtration efficiency, but also causes a series of problems such as waste of water resources, pollution of the working environment, and difficulty in post-treatment of activated coke sludge. The high-temperature silicon carbide ceramic membrane purification technology developed by Nanjing University of Technology replaces the plate and frame filtration technology, which can efficiently intercept and directly obtain dry activated coke fly ash, while improving the purity of the downstream process of preparing ammonium sulfate / sulfuric acid.

[0004] Activated coke fly ash is a porous material that adsorbs high concentrations of SO2, a small amount of NH3, and contains some metal catalysts. According to the national hazardous waste management regulations, it needs to be treated as hazardous waste, which is a complex process and has high treatment costs. Through energy spectrum analysis, the main elements in activated coke fly ash are C, N, O, S, Cu, and Zr. It is suitable as a pore-forming agent for the preparation of silicon carbide membrane supports. At the same time, the metal oxides in activated coke fly ash can serve as sintering aids for silicon carbide membrane supports. After inquiry, there are no relevant literature or patents on the high-value-added utilization of activated coke fly ash. Wuhan University of Science and Technology used rice husk ash as the main raw material and sodium carboxymethyl cellulose and clay as binders and plasticizers to prepare rice husk ash-based porous ceramics with a porosity of 50%-75% and a compressive strength of 2.5-12.5 MPa [Chen Hui et al. Preparation and characterization of rice husk ash-based porous ceramics [J]. Materials Review, 2014, 8(3):122-124.]. Yancheng Institute of Technology uses straw ash, pretreated with water washing and impurity removal, as a silicon source, α-Al2O3 powder as an aluminum source, and rice husk powder as a pore-forming agent to prepare porous mullite ceramics [Jiang Jinhai et al. Preparation of Porous Mullite Ceramics from Straw Ash [J]. Refractories, 2019, 5:450-454]. However, the production of rice husk ash and straw ash is cumbersome, polluting the environment, and their uneven ash particle size distribution limits their use as porous ceramic filter materials. Activated coke fly ash, a recycled hazardous waste, has a uniform particle size distribution and can aid sintering, making it ideal as a raw material for preparing silicon carbide membrane supports.

[0005] Summary of the Invention

[0006] The purpose of the present invention is to provide a method for preparing a silicon carbide membrane support body from activated coke fly ash. By using hazardous waste activated coke fly ash as a pore-forming agent for the silicon carbide membrane support body, it can be applied in the fields of steel coking, petrochemical industry, coal chemical industry, biomass gasification, waste incineration, etc.

[0007] The technical solutions of the present invention are as follows:

[0008] A method for preparing a silicon carbide membrane support from activated coke fly ash, the preparation steps being as follows:

[0009] (1) Silicon carbide aggregate, activated coke fly ash, and sintering aid are configured in a certain proportion and stirred to obtain a mixed powder a;

[0010] (2) adding a certain amount of polyvinyl alcohol aqueous solution to the mixed powder a and stirring evenly to obtain preform b;

[0011] (3) taking a certain amount of preform b, and subjecting the silicon carbide support green body prepared by mechanical extrusion to constant temperature drying for a period of time to obtain a dried support green body c;

[0012] (4) The support body green body c is placed in a muffle furnace for programmed temperature sintering, and after sintering, a silicon carbide membrane support body d is obtained.

[0013] in:

[0014] In step (1), the activated coke fly ash needs to be ball milled for 2-6 hours to obtain a uniform particle size, the ball milling speed is 200-500 r / min, and the ball-to-material ratio is 2-10.

[0015] The average particle size of the silicon carbide aggregate in the mixed powder a in step (1) is in the range of 1-300 μm, and the sintering aid is one or more of nano zirconium oxide, aluminum oxide, and magnesium oxide, with an average particle size in the range of 50-500 nm.

[0016] The mass proportion of the mixed powder a in step (1) is as follows: the activated coke fly ash after ball milling accounts for 5-20wt.%, the sintering aid is one or more of zirconium oxide, aluminum oxide, and magnesium oxide, with a total proportion of 1-10wt.%, and the rest is silicon carbide aggregate.

[0017] The concentration of the polyvinyl alcohol aqueous solution in step (2) is 2.5-10 wt.%, and the amount of the polyvinyl alcohol aqueous solution added is 1-5% of the mass of the mixed powder a.

[0018] In step (3), the drying temperature of the silicon carbide membrane support is 50-100° C., and the drying time is 1-4 hours.

[0019] When the heating program described in step (4) is 0-500°C, the heating rate is 1-2°C / min, and the temperature is kept at 500°C for 2-4h. When the temperature is 500-1000°C, the heating rate is 2-4°C / min, and the temperature is raised to a maximum of 1250-1450°C. When the temperature is above 1000°C, the heating rate is 0.5-1°C / min, and the temperature is kept at the highest temperature for 4-6h, and then the temperature is naturally lowered.

[0020] Beneficial effects of the present invention:

[0021] 1. The present invention uses hazardous waste activated coke fly ash as a pore-forming agent for the silicon carbide membrane support. At the same time, the metal oxides in the activated coke fly ash can also play a partial role in assisting sintering. The silicon carbide membrane support prepared by this method has excellent properties such as low cost, high porosity, high mechanical strength, and high gas permeability. This product is suitable for high-temperature flue gas purification in steel coking, petrochemical industry, coal chemical industry, biomass gasification, and waste incineration.

[0022] 2. The activated coke fly ash of the present invention as a pore-forming agent for the silicon carbide membrane support has simple pretreatment steps, is easy to operate, and is convenient for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG1 is a physical picture of the sheet-shaped and strip-shaped silicon carbide membrane support prepared in Example 2.

[0024] FIG2 is a gas flux diagram of the sheet-like silicon carbide ceramic membrane support prepared in Example 3.

[0025] FIG3 is a pore size distribution diagram of the sheet-like silicon carbide ceramic membrane support prepared in Example 3.

[0026] FIG4 is a microscopic morphology of the strip-shaped silicon carbide ceramic membrane support prepared in Example 4.

[0027] FIG5 is a particle size distribution analysis diagram of the activated coke fly ash of Example 4 after ball milling for 3 hours. DETAILED DESCRIPTION

[0028] The present invention will be further explained below with reference to the examples. The following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0029] Example 1

[0030] First, the activated coke fly ash was pretreated as follows: ball milling for 6 hours at a ball milling speed of 500 r / min and a ball-to-material ratio of 2. Then, silicon carbide with an average particle size of 1 μm, zirconium oxide and aluminum oxide with an average particle size of 50 nm, and the activated coke fly ash were mixed in a mass ratio of 94:0.5:0.5:5 and stirred to obtain a mixed powder a. A 2.5 wt.% polyvinyl alcohol aqueous solution was added to the mixed powder a in an amount of 1 wt.%, and stirred to obtain a preform b. ; The silicon carbide support green body prepared by mechanical extrusion method is dried at a constant temperature of 50℃ for 4 hours to obtain a dried silicon carbide membrane support green body c; sintering is carried out by programmed temperature rise. When the temperature rise program is 0-500℃, the heating rate is 1℃ / min, and it is kept at 500℃ for 2 hours. When the temperature rise program is 500-1000℃, the heating rate is 2℃ / min. When the temperature is above 1000℃, the heating rate is 0.5℃ / min. The maximum temperature is raised to 1250℃, and it is kept at the highest temperature for 4 hours, and then the temperature is naturally lowered.

[0031] The average pore size of the silicon carbide membrane support was 450 nm, the porosity was 42.5%, and the gas permeation flux was 32 m 3 ·m -2 ·h -1 KPa, flexural strength is 60MPa.

[0032] FIG1 is a physical picture of the sheet-shaped and strip-shaped silicon carbide membrane support prepared in Example 2;

[0033] Example 2

[0034] First, the activated coke fly ash was pretreated as follows: ball milling for 5 hours at a ball milling speed of 500 r / min and a ball-to-material ratio of 4. Then, silicon carbide with an average particle size of 50 μm, zirconium oxide and aluminum oxide with an average particle size of 100 nm, and the activated coke fly ash were mixed in a mass ratio of 90:1:1:8 and stirred to obtain a mixed powder a. A 3 wt.% polyvinyl alcohol aqueous solution was added to the mixed powder a in an amount of 2 wt.% and stirred to obtain a prefabricated material b. The mechanical The silicon carbide support green body prepared by the extrusion method was dried at a constant temperature of 50°C for 4 hours to obtain a dried silicon carbide membrane support green body c; it was sintered by programmed temperature rise. When the temperature rise program was 0-500°C, the heating rate was 1°C / min, and it was kept at 500°C for 2.5 hours. When the temperature was 500-1000°C, the heating rate was 2.5°C / min, and the heating rate above 1000°C was 0.5°C / min. The maximum temperature was raised to 1300°C, and it was kept at the highest temperature for 4 hours, and then cooled naturally.

[0035] The average pore size of the silicon carbide membrane support was 15 μm, the porosity was 43.2%, and the gas permeation flux was 250 m 3 ·m -2 ·h -1 KPa, and the flexural strength is 46.5MPa.

[0036] Example 3

[0037] First, the activated coke fly ash was pretreated as follows: ball milling for 4 hours at a ball milling speed of 400 r / min and a ball-to-material ratio of 5. Then, silicon carbide with an average particle size of 100 μm, zirconium oxide and aluminum oxide with an average particle size of 200 nm, and the activated coke fly ash were mixed in a mass ratio of 86:2:2:10 and stirred to obtain a mixed powder a. A 4 wt.% polyvinyl alcohol aqueous solution was added to the mixed powder a in an amount of 2.5 wt.%, and stirred to obtain a mixed powder a. The preform b is obtained after homogenization; the silicon carbide support green body prepared by the mechanical extrusion method is dried at a constant temperature of 80°C for 3 hours to obtain a dried silicon carbide membrane support green body c; sintering is carried out by programmed temperature rise, when the temperature rise program is 0-500°C, the heating rate is 2°C / min, and it is kept at 500°C for 3 hours, 500-1000°C, the heating rate is 3°C / min, and the heating rate above 1000°C is 0.5°C / min, the maximum temperature is raised to 1350°C, and it is kept at the highest temperature for 5 hours, and then the temperature is naturally lowered.

[0038] The average pore size of the silicon carbide membrane support was 15 μm, the porosity was 43.2%, and the gas permeation flux was 700 m 3 ·m -2 ·h -1 KPa, flexural strength is 35.5MPa.

[0039] FIG2 is a gas flux diagram of a sheet-like silicon carbide ceramic membrane support prepared in Example 3;

[0040] FIG3 is a pore size distribution diagram of a sheet-like silicon carbide ceramic membrane support prepared in Example 3;

[0041] Example 4

[0042] First, the activated coke fly ash was pretreated as follows: ball milling for 3 hours at a ball milling speed of 400 r / min and a ball-to-material ratio of 8. Then, silicon carbide with an average particle size of 200 μm, zirconium oxide and aluminum oxide with an average particle size of 1 μm, and the activated coke fly ash were mixed in a mass ratio of 84:2:2:12 and stirred to obtain a mixed powder a. A 6 wt.% polyvinyl alcohol aqueous solution was added to the mixed powder a in an amount of 3.0 wt.%, and stirred to obtain a preform b. ; The silicon carbide support green body prepared by mechanical extrusion method is dried at a constant temperature of 80℃ for 3h to obtain a dried silicon carbide membrane support green body c; sintering is carried out by programmed temperature rise, when the temperature rise program is 0-500℃, the heating rate is 2℃ / min, and it is kept at 500℃ for 4h, 500-1000℃, the heating rate is 4℃ / min, and the heating rate above 1000℃ is 1℃ / min, the maximum temperature is raised to 1400℃, and it is kept at the highest temperature for 5h, and then the temperature is naturally lowered.

[0043] After testing, the average pore size of the silicon carbide membrane support was 32 μm, the porosity was 44.5%, and the gas permeation flux was 1080 m 3 ·m -2 ·h -1 KPa, flexural strength is 28.8MPa.

[0044] FIG4 is a microscopic morphology of a strip-shaped silicon carbide ceramic membrane support prepared in Example 4;

[0045] FIG5 is a particle size distribution analysis diagram of activated coke fly ash after ball milling for 3 hours in Example 4;

[0046] Example 5

[0047] First, the activated coke fly ash was pretreated as follows: ball milling for 2 hours at a ball milling speed of 200 r / min and a ball-to-material ratio of 10. Then, silicon carbide with an average particle size of 300 μm, magnesium oxide and aluminum oxide with an average particle size of 500 nm, and the activated coke fly ash were mixed in a mass ratio of 70:5:5:20 and stirred to obtain a mixed powder a. A 10 wt.% polyvinyl alcohol aqueous solution was added to the mixed powder a in an amount of 5.0 wt.%, and stirred to obtain a preform b. ; The silicon carbide support green body prepared by mechanical extrusion method is dried at a constant temperature of 100℃ for 1h to obtain a dried silicon carbide membrane support green body c; sintering is carried out by programmed temperature rise. When the temperature rise program is 0-500℃, the heating rate is 1℃ / min, and it is kept at 500℃ for 3h. When the temperature rise program is 500-1000℃, the heating rate is 3℃ / min. When the temperature is above 1000℃, the heating rate is 0.5℃ / min. The maximum temperature is raised to 1450℃, and it is kept at the highest temperature for 6h, and then the temperature is naturally lowered.

[0048] The average pore size of the silicon carbide membrane support was 48.8 μm, the porosity was 44.2%, and the gas permeation flux was 1540 m 3 ·m -2 ·h -1 KPa, flexural strength is 25.5MPa.

[0049] Comparative Example 1

[0050] The difference between this embodiment and embodiment 3 is that activated carbon with an average particle size of 25 μm is used instead of activated coke fly ash, and the remaining steps are consistent with embodiment 3.

[0051] From the SEM photos of Comparative Example 1 and Example 3, it can be seen that when the average particle size of 25 μm is used instead of the activated coke fly ash, the average pore size of the obtained silicon carbide membrane support is 17.2 μm, the porosity is 42.2%, and the gas permeation flux is 600 m 3 ·m -2 ·h -1 The gas flux and flexural strength of the silicon carbide membrane support body decreased significantly, mainly because the metal oxides in the activated coke fly ash can play a good sintering role.

Claims

1. A method for preparing a silicon carbide membrane support from activated coke fly ash, characterized in that: The preparation steps are as follows: (1) Silicon carbide aggregate, activated coke fly ash, and sintering aid are configured in a certain proportion and stirred to obtain a mixed powder a; (2) adding a certain amount of polyvinyl alcohol aqueous solution to the mixed powder a, stirring evenly to obtain a preform b; (3) taking a certain amount of preform b, and subjecting the silicon carbide support green body prepared by mechanical extrusion to constant temperature drying for a period of time, to obtain a dried support green body c; (4) The support body green body c is placed in a muffle furnace for programmed temperature sintering, and after sintering, a silicon carbide membrane support body d is obtained.

2. The method for preparing a low-cost silicon carbide membrane support according to claim 1, characterized in that: In step (1), the activated coke fly ash needs to be ball milled for 2-6 hours to obtain a uniform particle size, the ball milling speed is 200-500r / min, and the ball-to-material ratio is 2-10.

3. The method for preparing a low-cost silicon carbide membrane support according to claim 1, characterized in that: In the mixed powder a of step (1), the average particle size of the silicon carbide aggregate is in the range of 1-300 μm, and the sintering aid is one or more of nano zirconium oxide, aluminum oxide, and magnesium oxide, and the average particle size is in the range of 50-500 nm.

4. The method for preparing a low-cost silicon carbide membrane support according to claim 1, characterized in that: The mass proportion of the mixed powder a described in step (1) is as follows: the activated coke fly ash after ball milling accounts for 5-20wt.%, the sintering aid is one or more of zirconium oxide, aluminum oxide, and magnesium oxide, with a total proportion of 1-10wt.%, and the rest is silicon carbide aggregate.

5. The method for preparing a low-cost silicon carbide membrane support according to claim 1, characterized in that: The concentration of the polyvinyl alcohol aqueous solution in step (2) is 2.5-10wt.%, and the amount of the polyvinyl alcohol aqueous solution added is 1-5% of the mass of the mixed powder a.

6. The method for preparing a low-cost silicon carbide membrane support according to claim 1, characterized in that: In step (3), the drying temperature of the silicon carbide membrane support is 50-100° C. and the drying time is 1-4 hours.

7. The method for preparing a low-cost silicon carbide membrane support according to claim 1, characterized in that: The heating program described in step (4) is as follows: when the temperature is from 0 to 500°C, the heating rate is 1 to 2°C / min, and the temperature is kept at 500°C for 2 to 4 hours. When the temperature is from 500 to 1000°C, the heating rate is 2 to 4°C / min, and the maximum temperature is increased to 1250 to 1450°C. When the temperature is above 1000°C, the heating rate is 0.5 to 1°C / min, and the temperature is kept at the highest temperature for 4 to 6 hours, and then the temperature is naturally lowered.

Citation Information

Patent Citations

  • Pure SiC membrane tube support and preparation method thereof

    CN102659446A

  • Method of preparing porous silicon carbide support at low temperature

    CN105884394A

  • High-temperature-resistant corrosion-resistant reaction sintering silicon carbide film support body and preparation method thereof

    CN110698215A

  • Regeneration method of silicon carbide film for active coke regeneration process

    CN113975972A

  • Method for preparing silicon carbide film support from active coke fly ash

    CN116462529A