Glass-ceramic and glass-ceramic product having spinel crystal phase
By optimizing the component proportions and additives of the glass-ceramics, the problem of coloration and transmittance reduction caused by the Ti element introduced by TiO2 is solved, and a glass-ceramic product with excellent light transmittance and mechanical properties is achieved, which is suitable for electronics. equipment and display equipment.
Patent Information
- Application Number
- PCT/CN2024/081696
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-31
AI Technical Summary
In the prior art, the application of prepared glass-ceramics with spinel crystal phase in electronic equipment and display equipment is limited. The Ti element introduced by TiO2 causes coloring and reduced transmittance, and the difference in refractive index reduces the visible light range. transmittance.
By optimizing the component ratio, prepare crystallized glass with SiO2: 40~55%, Al2O3+ZnO: 26~45%, Li2O: 0.1~6%, MgO: 0.1~6%, TiO2: 0.5~7%, combined with P2O5 +ZrO2、 Additives such as Na2O, B2O3, K2O, CaO+BaO+SrO, and Y2O3 control the ratios of Li2O/TiO2, Al2O3/ZnO, SiO2/Al2O3, etc. to form crystallized glass with excellent light transmittance and mechanical properties.
It achieves high transmittance (more than 87.0%) and excellent mechanical properties of glass-ceramics, such as drop resistance, crush resistance and Vickers hardness, making it suitable for electronic equipment and display equipment.
Smart Images

Figure PCTCN2024081696-FTAPPB-I100001 
Figure PCTCN2024081696-FTAPPB-I100002 
Figure PCTCN2024081696-FTAPPB-I100003
Abstract
Description
Glass-ceramics and glass-ceramics products having a spinel crystal phase Technical Field
[0001] The present invention relates to a glass-ceramic, in particular to a glass-ceramic having a spinel crystal phase and a glass-ceramic product. Background Art
[0002] Glass-ceramics are a polycrystalline solid material formed by the controlled crystallization of specific glass components. They combine the structural characteristics and properties of both glass and ceramics, making them a new class of inorganic non-metallic materials undergoing development and promising applications. Glass-ceramics boast excellent properties such as high mechanical strength, low thermal expansion coefficient, excellent corrosion resistance, high hardness, and excellent wear resistance, finding applications in electronics, machinery, aerospace, biomedicine, and other fields.
[0003] Glass-ceramics with a spinel crystal phase are used in display devices and electronic devices, particularly in the front and back covers of portable electronic devices (such as mobile phones, watches, and PADs). Compared to materials like ceramics and sapphire, they offer significant advantages. They have a smooth surface, a completely dense and uniform structure, are resistant to contamination, and feature a relatively simple process, high production capacity, and low cost. Compared to high-aluminum glass, glass-ceramics with a spinel crystal phase exhibit higher mechanical strength, hardness, drop resistance, thermal conductivity, and superior thermal and chemical stability.
[0004] In the prior art, TiO2 is used as a nucleating agent to prepare glass-ceramics with a spinel crystal phase. However, the Ti element introduced by TiO2 is prone to change in valence in the glass, forming TiO2. 3+ Ion. Ti 3+ Ions tend to exist stably in the formed crystalline phase, causing the glass-ceramics to be colored (brown-yellow), thereby reducing the transmittance of the glass-ceramics in the visible light region. In addition, the refractive index of spinel is relatively high (1.83), which is significantly different from the refractive index of the matrix glass. The precipitation of the spinel crystal phase will also reduce the transmittance of the glass-ceramics in the visible light region. The above factors restrict the application of glass-ceramics with a spinel crystal phase in electronic devices and display devices. Therefore, how to improve the transmittance of glass-ceramics with a spinel crystal phase is also an urgent problem to be solved.
[0005] Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a glass-ceramic having a spinel crystal phase and a glass-ceramic product having excellent light transmittance and mechanical properties.
[0007] The technical solution adopted by the present invention to solve the technical problem is:
[0008] (1) Glass-ceramic products with a spinel crystal phase, whose components, expressed in percentage by weight, contain: SiO2: 40-55%; Al2O3+ZnO: 26-45%; Li2O: 0.1-6%; MgO: 0.1-6%; TiO2: 0.5-7%, wherein the Li2O / TiO2 ratio is 0.2-4.5.
[0009] (2) The microcrystalline glass product having a spinel crystal phase according to (1), wherein the components, expressed in percentage by weight, further contain: P2O5+ZrO2: 0-8%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or a clarifier: 0-2%.
[0010] (3) Glass-ceramic products with a spinel crystal phase, whose components contain SiO2, Al2O3, Li2O, ZnO and TiO2, and the light transmittance of the glass-ceramic products with a thickness of less than 1 mm at a wavelength of 550 nm is more than 87.0%.
[0011] (4) A glass-ceramic product having a spinel crystal phase, wherein the components thereof include SiO2, Al2O3, Li2O, ZnO and TiO2, and wherein the drop resistance of the glass-ceramic product is above 1200 mm.
[0012] (5) A glass-ceramic product having a spinel crystal phase, wherein the components thereof include SiO2, Al2O3, and ZnO, and wherein the glass-ceramic product has an anti-compression strength of 400N or more.
[0013] (6) Glass-ceramic products with a spinel crystal phase, with a haze of less than 0.3% for glass-ceramic products with a thickness of less than 1 mm.
[0014] (7) A glass-ceramic product having a spinel crystal phase, wherein the drop ball test height of the glass-ceramic product is greater than 1000 mm.
[0015] (8) Glass-ceramics with a spinel crystal phase, whose components contain SiO2, Al2O3, Li2O, ZnO and TiO2, and the average optical |B| value of the glass-ceramics with a thickness of less than 1 mm at 400 to 800 nm is less than 1.0.
[0016] (9) A glass-ceramic product having a spinel crystal phase, wherein the components thereof include SiO2, Al2O3, Li2O, ZnO and TiO2, and wherein the depth of the ion exchange layer of the glass-ceramic product is greater than 75 μm.
[0017] (10) A glass-ceramic product having a spinel crystal phase, wherein the components thereof include SiO2, Al2O3, and Li2O, and the surface stress of the glass-ceramic product is greater than 200 MPa.
[0018] (11) A glass-ceramic product having a spinel crystal phase, wherein the components thereof include SiO2, Al2O3, ZnO and TiO2, and the grain size of the glass-ceramic product is less than 60 nm.
[0019] (12) Glass-ceramics with a spinel crystal phase, where the light transmittance at a wavelength of 550 nm for a glass-ceramics with a thickness of less than 1 mm is 87.0% or more.
[0020] (13) A glass-ceramic product having a spinel crystal phase, wherein the components thereof include SiO2, Al2O3 and ZnO, and wherein the Vickers hardness of the glass-ceramic product is 650 kgf / mm 2 above.
[0021] (14) A glass-ceramic product having a spinel crystal phase according to any one of (3) to (13), wherein the components thereof, expressed in percentage by weight, comprise: SiO2: 40 to 55%; and / or Al2O3 + ZnO: 26 to 45%; and / or Li2O: 0.1 to 6%; and / or MgO: 0.1 to 6%; and / or TiO2: 0.5 to 7%; and / or P2O5 + ZrO2: 0 to 8%; and / or Na2O: 0 to 6%; and / or B2O3: 0 to 4%; and / or K2O: 0 to 3%; and / or CaO + BaO + SrO: 0 to 5%; and / or Y2O3: 0 to 6%; and / or a clarifier: 0 to 2%.
[0022] (15) A glass-ceramic product having a spinel crystal phase, wherein the components thereof are expressed in percentage by weight and are composed of SiO2: 40-55%; Al2O3+ZnO: 26-45%; Li2O: 0.1-6%; MgO: 0.1-6%; TiO2: 0.5-7%; P2O5+ZrO2: 0-8%; Na2O: 0-6%; B2O3: 0-4%; K2O: 0-3%; CaO+BaO+SrO: 0-5%; Y2O3: 0-6%; and a clarifier: 0-2%.
[0023] (16) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: Li2O / TiO2 is 0.2 to 4.5, preferably Li2O / TiO2 is 0.5 to 3.5, more preferably Li2O / TiO2 is 0.7 to 2.5, and further preferably Li2O / TiO2 is 0.75 to 1.5.
[0024] (17) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: Al2O3 / ZnO is 1.0 to 3.0, preferably Al2O3 / ZnO is 1.2 to 2.8, more preferably Al2O3 / ZnO is 1.25 to 2.5, and further preferably Al2O3 / ZnO is 1.5 to 2.3.
[0025] (18) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: SiO2 / Al2O3 is 1.5 to 3.2, preferably SiO2 / Al2O3 is 1.7 to 3.0, more preferably SiO2 / Al2O3 is 1.8 to 2.8, and further preferably SiO2 / Al2O3 is 2.0 to 2.5.
[0026] (19) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: (TiO2 + ZnO) / Al2O3 is 0.4 to 1.5, preferably (TiO2 + ZnO) / Al2O3 is 0.5 to 1.2, more preferably (TiO2 + ZnO) / Al2O3 is 0.6 to 1.0, and further preferably (TiO2 + ZnO) / Al2O3 is 0.6 to 0.9.
[0027] (20) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: (Li2O+MgO) / TiO2 is 0.3 to 8.0, preferably (Li2O+MgO) / TiO2 is 0.5 to 5.0, more preferably (Li2O+MgO) / TiO2 is 1.0 to 3.0, and further preferably (Li2O+MgO) / TiO2 is 1.2 to 2.5.
[0028] (21) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: Al2O3 / (MgO+TiO2) is 1.3 to 10.0, preferably Al2O3 / (MgO+TiO2) is 1.5 to 8.0, more preferably Al2O3 / (MgO+TiO2) is 2.5 to 6.5, and further preferably Al2O3 / (MgO+TiO2) is 3.0 to 5.5.
[0029] (22) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: (Al2O3+Li2O) / P2O5 is 5.0 to 45.0, preferably (Al2O3+Li2O) / P2O5 is 7.0 to 35.0, more preferably (Al2O3+Li2O) / P2O5 is 8.0 to 30.0, and further preferably (Al2O3+Li2O) / P2O5 is 10.0 to 25.0.
[0030] (23) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: P2O5 / ZrO2 is 0.1 to 5.0, preferably P2O5 / ZrO2 is 0.2 to 3.0, more preferably P2O5 / ZrO2 is 0.5 to 2.0, and further preferably P2O5 / ZrO2 is 0.6 to 1.5.
[0031] (24) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: (SiO2 + Na2O) / ZnO is 2.2 to 6.2, preferably (SiO2 + Na2O) / ZnO is 2.5 to 6.0, more preferably (SiO2 + Na2O) / ZnO is 2.8 to 5.5, and further preferably (SiO2 + Na2O) / ZnO is 3.0 to 5.0.
[0032] (25) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components are expressed in weight percentages, wherein: (Na2O + K2O) / ZnO is less than 0.8, preferably (Na2O + K2O) / ZnO is less than 0.6, more preferably (Na2O + K2O) / ZnO is less than 0.4, and further preferably (Na2O + K2O) / ZnO is less than 0.2.
[0033] (26) The glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the components thereof are expressed in percentage by weight and contain: SiO2: 45-53%, preferably SiO2: 48-52%; and / or Al2O3+ZnO: 30-42%, preferably Al2O3+ZnO: 32-42%, more preferably Al2O3+ZnO: 35-40%; and / or Li2O: 1-5%, preferably Li2O: 2-4%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO2: 1-6%, preferably TiO2: 2 ~5%; and / or P2O5+ZrO2: 0.1~7%, preferably P2O5+ZrO2: 0.5~5%; and / or Na2O: 0~4%, preferably Na2O: 0~2%; and / or B2O3: 0~2%, preferably B2O3: 0~1%; and / or K2O: 0~2%, preferably K2O: 0~1%; and / or CaO+BaO+SrO: 0~4%, preferably CaO+BaO+SrO: 0~2%; and / or Y2O3: 0~4%, preferably Y2O3: 0~2%; and / or clarifier: 0~1%, preferably clarifier: 0~0.5%.
[0034] (27) The microcrystalline glass product having a spinel crystal phase according to any one of (1) to (15), wherein the components thereof, expressed in weight percentage, contain: Al2O3: 15 to 30%, preferably Al2O3: 18 to 25%, more preferably Al2O3: 20 to 23%; and / or ZnO: 9 to 20%, preferably ZnO: 11 to 18%, more preferably ZnO: 12 to 16%; and / or P2O5: 0 to 5%, preferably P2O5: 0.5 to 4%, more preferably P2O5: 1 to 3%; and / or ZrO2: 0 to 5%, preferably ZrO2: 0.5 to 4%, more preferably ZrO2: 1 to 3%.
[0035] (28) According to any one of (1) to (15) of the microcrystalline glass product having a spinel crystal phase, the spinel crystal phase accounts for 20 to 60% by weight of the microcrystalline glass product, preferably the spinel crystal phase accounts for 25 to 50% by weight of the microcrystalline glass product, more preferably the spinel crystal phase accounts for 25 to 45% by weight of the microcrystalline glass product, and further preferably the spinel crystal phase accounts for 30 to 45% by weight of the microcrystalline glass product.
[0036] (29). The glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the glass-ceramic product having a spinel crystal phase contains a quartz crystal phase, preferably the quartz crystal phase accounts for less than 20% by weight of the glass-ceramic product, more preferably the quartz crystal phase accounts for less than 10% by weight of the glass-ceramic product, further preferably the quartz crystal phase accounts for less than 5% by weight of the glass-ceramic product, and further preferably the glass-ceramic product having a spinel crystal phase does not contain a quartz crystal phase.
[0037] (30) The glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof are expressed in weight percentage and contain: La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0-5%, preferably La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0-2 %, more preferably La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0~1%, further preferably does not contain La2O3, and / or does not contain Gd2O3, and / or does not contain Yb2O3, and / or does not contain Nb2O5, and / or does not contain WO3, and / or does not contain Bi2O3, and / or does not contain Ta2O5, and / or does not contain TeO2.
[0038] (31) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the grain size of the glass-ceramic product is 60 nm or less, preferably 45 nm or less, more preferably 10 to 30 nm; and / or the depth of the ion exchange layer is 75 μm or more, preferably 80 to 150 μm, more preferably 100 to 125 μm; and / or the surface stress is 200 MPa or more, preferably 250 to 400 MPa, more preferably 300 to 400 MPa; and / or the drop ball test height is 1000 mm or more, preferably 1200 mm or more, more preferably 1500 mm or more; and / or the drop resistance is 1200 mm or more, preferably 1300 mm or more, more preferably 1400 mm or more; and / or the fracture toughness is 1.0 MPa·m 1 / 2 Above, preferably 1.2 MPa·m 1 / 2 More preferably, 1.2 to 1.6 MPa·m 1 / 2 and / or a four-point bending strength of 500 MPa or more, preferably 600 MPa or more, more preferably 700 to 1000 MPa; and / or a compressive strength of 400 N or more, preferably 400 to 550 N, more preferably 450 to 550 N; and / or a Vickers hardness of 650 kgf / mm 2 Above, preferably 660kgf / mm2 More preferably, 680 to 750 kgf / mm 2 .
[0039] (32) The glass-ceramic product having a spinel crystal phase according to any one of (1) to (15), wherein the haze of the glass-ceramic product having a thickness of less than 1 mm is less than 0.3%, preferably less than 0.25%, more preferably 0.05 to 0.2%; and / or the average light transmittance at a wavelength of 400 to 800 nm is greater than 87.0%, preferably greater than 88.5%, more preferably greater than 89.5%; and / or the light transmittance at a wavelength of 550 nm is greater than 87.0%, preferably greater than 88.0%, more preferably greater than 89.0%; and / or the average light |B| value at 400 to 800 nm is less than 1.0, preferably less than 0.8, more preferably 0.3 to 0.6.
[0040] (33) The microcrystalline glass product having a spinel crystal phase according to (32), wherein the thickness of the microcrystalline glass product is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0041] (34) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in percentage by weight, comprise: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.
[0042] (35) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in percentage by weight, comprise: NiO: 0.1 to 4%; and / or Ni2O3: 0.1 to 4%; and / or CoO: 0.05 to 2%; and / or Co2O3: 0.05 to 2%; and / or Fe2O3: 0.2 to 7%; and / or MnO2: 0.1 to 4%; and / or Er2O3: 0.4 to 8%; and / or Nd2O3: 0.4 to 8%; and / or Cu2O: 0.5 to 4%; and / or Pr2O3: 0.4 to 8%; and / or CeO2: 0.5 to 4%.
[0043] (36) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in percentage by weight, comprise: NiO: 0.1 to 3%; and / or Ni2O3: 0.1 to 3%; and / or CoO: 0.05 to 1.8%; and / or Co2O3: 0.05 to 1.8%; and / or Fe2O3: 0.2 to 5%; and / or MnO2: 0.1 to 3%; and / or Er2O3: 0.4 to 6%; and / or Nd2O3: 0.4 to 6%; and / or Cu2O: 0.5 to 3%; and / or Pr2O3: 0.4 to 6%; and / or CeO2: 0.5 to 3%.
[0044] (37) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in weight percentage, contain: NiO: 0.1 to 3%; and / or Ni2O3: 0.1 to 3%.
[0045] (38) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in weight percentage, contain: CoO: 0.05 to 1.8%; and / or Co2O3: 0.05 to 1.8%.
[0046] (39) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in weight percentage, contain: Cu2O: 0.5 to 3%; and / or CeO2: 0.5 to 3%.
[0047] (40) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof are expressed in percentage by weight and contain: Fe2O3: 0.2-5%, CoO: 0.05-0.3%; or Fe2O3: 0.2-5%, CoO: 0.05-0.3%; or Fe2O3: 0.2-5%, CoO: 0.05-0.3%, NiO: 0.1-1%; or Fe2O3: 0.2-5%, Co2O3: 0.05-0.3%, NiO: 0.1-1%.
[0048] (41) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in percentage by weight, comprise: Pr2O3: 0.4 to 6%; or Fe2O3: 0.2 to 5%; or MnO2: 0.1 to 3%; or Er2O3: 0.4 to 6%; or Nd2O3: 0.4 to 6%.
[0049] (42) A glass-ceramic product having a spinel crystal phase according to any one of (1) to (14), wherein the components thereof, expressed in weight percentage, contain: Er2O3: 0.4 to 6%, Nd2O3: 0.4 to 4%, and MnO2: 0.1 to 2%.
[0050] (43) Glass-ceramics with a spinel crystal phase, whose components, expressed in percentage by weight, contain: SiO2: 40-55%; Al2O3+ZnO: 26-45%; Li2O: 0.1-6%; MgO: 0.1-6%; TiO2: 0.5-7%, wherein the Li2O / TiO2 ratio is 0.2-4.5.
[0051] (44) The microcrystalline glass having a spinel crystal phase according to (43), wherein its components, expressed in percentage by weight, further contain: P2O5+ZrO2: 0-8%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or clarifier: 0-2%.
[0052] (45) Glass-ceramics with a spinel crystal phase, the components of which include SiO2, Al2O3, Li2O, ZnO and TiO2, and the light transmittance of the glass-ceramics with a thickness of less than 1 mm at a wavelength of 550 nm is more than 87.0%.
[0053] (46) Glass-ceramics having a spinel crystal phase, wherein the grain size of the glass-ceramics is less than 60 nm.
[0054] (47) Glass-ceramics having a spinel crystal phase, the components of which include SiO2, Al2O3, Li2O, ZnO and TiO2, and the haze of glass-ceramics with a thickness of less than 1 mm is less than 0.3%.
[0055] (48) Glass-ceramics having a spinel crystal phase, the components of which include SiO2, Al2O3, ZnO and TiO2, and the Young's modulus of the glass-ceramics is 80 to 110 GPa.
[0056] (49) Glass-ceramics with a spinel crystal phase, the components of which include SiO2, Al2O3, Li2O and ZnO, and the average optical |B| value of the glass-ceramics with a thickness of less than 1 mm at 400 to 800 nm is less than 1.0.
[0057] (50) Glass-ceramics with a spinel crystal phase, the components of which include SiO2, Al2O3 and ZnO, and the average light transmittance of the glass-ceramics with a thickness of less than 1 mm at a wavelength of 400 to 800 nm is more than 87.0%.
[0058] (51) The glass-ceramics having a spinel crystal phase according to any one of (45) to (50), wherein the components thereof are expressed in percentage by weight and contain: SiO2: 40 to 55%; and / or Al2O3+ZnO: 26 to 45%; and / or Li2O: 0.1 to 6%; and / or MgO: 0.1 to 6%; and / or TiO2: 0.5 to 7%; and / or P2O5+ZrO2: 0 to 8%; and / or Na2O: 0 to 6%; and / or B2O3: 0 to 4%; and / or K2O: 0 to 3%; and / or CaO+BaO+SrO: 0 to 5%; and / or Y2O3: 0 to 6%; and / or clarifier: 0 to 2%.
[0059] (52) Glass-ceramics with a spinel crystal phase, whose components, expressed in percentage by weight, are composed of SiO2: 40-55%; Al2O3+ZnO: 26-45%; Li2O: 0.1-6%; MgO: 0.1-6%; TiO2: 0.5-7%; P2O5+ZrO2: 0-8%; Na2O: 0-6%; B2O3: 0-4%; K2O: 0-3%; CaO+BaO+SrO: 0-5%; Y2O3: 0-6%; and clarifier: 0-2%.
[0060] (53) The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: Li2O / TiO2 is 0.2 to 4.5, preferably Li2O / TiO2 is 0.5 to 3.5, more preferably Li2O / TiO2 is 0.7 to 2.5, and further preferably Li2O / TiO2 is 0.75 to 1.5.
[0061] (54) The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: Al2O3 / ZnO is 1.0 to 3.0, preferably Al2O3 / ZnO is 1.2 to 2.8, more preferably Al2O3 / ZnO is 1.25 to 2.5, and further preferably Al2O3 / ZnO is 1.5 to 2.3.
[0062] (55) The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: SiO2 / Al2O3 is 1.5 to 3.2, preferably SiO2 / Al2O3 is 1.7 to 3.0, more preferably SiO2 / Al2O3 is 1.8 to 2.8, and further preferably SiO2 / Al2O3 is 2.0 to 2.5.
[0063] (56) The microcrystalline glass having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: (TiO2+ZnO) / Al2O3 is 0.4 to 1.5, preferably (TiO2+ZnO) / Al2O3 is 0.5 to 1.2, more preferably (TiO2+ZnO) / Al2O3 is 0.6 to 1.0, and further preferably (TiO2+ZnO) / Al2O3 is 0.6 to 0.9.
[0064] (57) The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: (Li2O+MgO) / TiO2 is 0.3 to 8.0, preferably (Li2O+MgO) / TiO2 is 0.5 to 5.0, more preferably (Li2O+MgO) / TiO2 is 1.0 to 3.0, and further preferably (Li2O+MgO) / TiO2 is 1.2 to 2.5.
[0065] (58) The microcrystalline glass having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: Al2O3 / (MgO+TiO2) is 1.3 to 10.0, preferably Al2O3 / (MgO+TiO2) is 1.5 to 8.0, more preferably Al2O3 / (MgO+TiO2) is 2.5 to 6.5, and further preferably Al2O3 / (MgO+TiO2) is 3.0 to 5.5.
[0066] (59). The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: (Al2O3+Li2O) / P2O5 is 5.0 to 45.0, preferably (Al2O3+Li2O) / P2O5 is 7.0 to 35.0, more preferably (Al2O3+Li2O) / P2O5 is 8.0 to 30.0, and further preferably (Al2O3+Li2O) / P2O5 is 10.0 to 25.0.
[0067] (60). The microcrystalline glass having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: P2O5 / ZrO2 is 0.1 to 5.0, preferably P2O5 / ZrO2 is 0.2 to 3.0, more preferably P2O5 / ZrO2 is 0.5 to 2.0, and further preferably P2O5 / ZrO2 is 0.6 to 1.5.
[0068] (61). The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: (SiO2 + Na2O) / ZnO is 2.2 to 6.2, preferably (SiO2 + Na2O) / ZnO is 2.5 to 6.0, more preferably (SiO2 + Na2O) / ZnO is 2.8 to 5.5, and further preferably (SiO2 + Na2O) / ZnO is 3.0 to 5.0.
[0069] (62) The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components are expressed in weight percentage, wherein: (Na2O+K2O) / ZnO is less than 0.8, preferably (Na2O+K2O) / ZnO is less than 0.6, more preferably (Na2O+K2O) / ZnO is less than 0.4, and further preferably (Na2O+K2O) / ZnO is less than 0.2.
[0070] (63) The glass-ceramics having a spinel crystal phase according to any one of (43) to (52), wherein the components thereof are expressed in weight percentages as follows: SiO2: 45-53%, preferably SiO2: 48-52%; and / or Al2O3+ZnO: 30-42%, preferably Al2O3+ZnO: 32-42%, more preferably Al2O3+ZnO: 35-40%; and / or Li2O: 1-5%, preferably Li2O: 2-4%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO2: 1-6%, preferably TiO2: 2-5%; and / or P2O5+ZrO2: 0.1~7%, preferably P2O5+ZrO2: 0.5~5%; and / or Na2O: 0~4%, preferably Na2O: 0~2%; and / or B2O3: 0~2%, preferably B2O3: 0~1%; and / or K2O: 0~2%, preferably K2O: 0~1%; and / or CaO+BaO+SrO: 0~4%, preferably CaO+BaO+SrO: 0~2%; and / or Y2O3: 0~4%, preferably Y2O3: 0~2%; and / or clarifier: 0~1%, preferably clarifier: 0~0.5%.
[0071] (64). The microcrystalline glass having a spinel crystal phase according to any one of (43) to (52), wherein the components thereof are expressed in weight percentage and contain: Al2O3: 15 to 30%, preferably Al2O3: 18 to 25%, more preferably Al2O3: 20 to 23%; and / or ZnO: 9 to 20%, preferably ZnO: 11 to 18%, more preferably ZnO: 12 to 16%; and / or P2O5: 0 to 5%, preferably P2O5: 0.5 to 4%, more preferably P2O5: 1 to 3%; and / or ZrO2: 0 to 5%, preferably ZrO2: 0.5 to 4%, more preferably ZrO2: 1 to 3%.
[0072] (65). In the glass-ceramic having a spinel crystal phase according to any one of (43) to (52), the weight percentage of the spinel crystal phase in the glass-ceramic is 20 to 60%, preferably the weight percentage of the spinel crystal phase in the glass-ceramic is 25 to 50%, more preferably the weight percentage of the spinel crystal phase in the glass-ceramic is 25 to 45%, and further preferably the weight percentage of the spinel crystal phase in the glass-ceramic is 30 to 45%.
[0073] (66). The glass-ceramic having a spinel crystal phase according to any one of (43) to (52), wherein the glass-ceramic having a spinel crystal phase contains a quartz crystal phase, preferably the weight percentage of the quartz crystal phase in the glass-ceramic is less than 20%, more preferably the weight percentage of the quartz crystal phase in the glass-ceramic is less than 10%, further preferably the weight percentage of the quartz crystal phase in the glass-ceramic is less than 5%, and further preferably the glass-ceramic having a spinel crystal phase does not contain a quartz crystal phase.
[0074] (67) The glass-ceramics having a spinel crystal phase according to any one of (43) to (51), wherein the components, expressed in weight percentage, contain: La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0-5%, preferably La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0-2 %, more preferably La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0~1%, further preferably does not contain La2O3, and / or does not contain Gd2O3, and / or does not contain Yb2O3, and / or does not contain Nb2O5, and / or does not contain WO3, and / or does not contain Bi2O3, and / or does not contain Ta2O5, and / or does not contain TeO2.
[0075] (68) The glass-ceramic having a spinel crystal phase according to any one of (43) to (52), wherein the glass-ceramic has a grain size of 60 nm or less, preferably 45 nm or less, more preferably 10 to 30 nm; and / or a Young's modulus of 80 to 110 GPa, preferably 85 to 105 GPa, more preferably 90 to 105 GPa; and / or a Vickers hardness of 550 kgf / mm 2 Above, preferably 580kgf / mm 2 More preferably, 600 to 650 kgf / mm 2 .
[0076] (69). According to any one of the microcrystalline glass having a spinel crystal phase described in (43) to (52), the haze of the microcrystalline glass with a thickness of less than 1 mm is less than 0.3%, preferably less than 0.25%, and more preferably 0.05 to 0.2%; and / or the average light transmittance at a wavelength of 400 to 800 nm is greater than 87.0%, preferably greater than 88.5%, and more preferably greater than 89.5%; and / or the light transmittance at a wavelength of 550 nm is greater than 87.0%, preferably greater than 88.0%, and more preferably greater than 89.0%; and / or the average light |B| value at 400 to 800 nm is less than 1.0, preferably less than 0.8, and more preferably 0.3 to 0.6.
[0077] (70). The microcrystalline glass having a spinel crystal phase according to (69), wherein the thickness of the microcrystalline glass is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0078] (71). The microcrystalline glass having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof are expressed in percentage by weight and contain: NiO: 0 to 4%; and / or Ni2O3: 0 to 4%; and / or CoO: 0 to 2%; and / or Co2O3: 0 to 2%; and / or Fe2O3: 0 to 7%; and / or MnO2: 0 to 4%; and / or Er2O3: 0 to 8%; and / or Nd2O3: 0 to 8%; and / or Cu2O: 0 to 4%; and / or Pr2O3: 0 to 8%; and / or CeO2: 0 to 4%.
[0079] (72) The glass-ceramics having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof are expressed in percentage by weight and contain: NiO: 0.1 to 4%; and / or Ni2O3: 0.1 to 4%; and / or CoO: 0.05 to 2%; and / or Co2O3: 0.05 to 2%; and / or Fe2O3: 0.2 to 7%; and / or MnO2: 0.1 to 4%; and / or Er2O3: 0.4 to 8%; and / or Nd2O3: 0.4 to 8%; and / or Cu2O: 0.5 to 4%; and / or Pr2O3: 0.4 to 8%; and / or CeO2: 0.5 to 4%.
[0080] (73) The microcrystalline glass having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof are expressed in percentage by weight and contain: NiO: 0.1 to 3%; and / or Ni2O3: 0.1 to 3%; and / or CoO: 0.05 to 1.8%; and / or Co2O3: 0.05 to 1.8%; and / or Fe2O3: 0.2 to 5%; and / or MnO2: 0.1 to 3%; and / or Er2O3: 0.4 to 6%; and / or Nd2O3: 0.4 to 6%; and / or Cu2O: 0.5 to 3%; and / or Pr2O3: 0.4 to 6%; and / or CeO2: 0.5 to 3%.
[0081] (74) The glass-ceramics having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof, expressed in weight percentage, contain: NiO: 0.1 to 3%; and / or Ni2O3: 0.1 to 3%.
[0082] (75) The glass-ceramics having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof, expressed in weight percentage, contain: CoO: 0.05 to 1.8%; and / or Co2O3: 0.05 to 1.8%.
[0083] (76) The glass-ceramics having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof, expressed in weight percentage, contain: Cu2O: 0.5 to 3%; and / or CeO2: 0.5 to 3%.
[0084] (77) The microcrystalline glass having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof are expressed in percentage by weight and contain: Fe2O3: 0.2 to 5%, CoO: 0.05 to 0.3%; or Fe2O3: 0.2 to 5%, Co2O3: 0.05 to 0.3%; or Fe2O3: 0.2 to 5%, CoO: 0.05 to 0.3%, NiO: 0.1 to 1%; or Fe2O3: 0.2 to 5%, Co2O3: 0.05 to 0.3%, NiO: 0.1 to 1%.
[0085] (78) The microcrystalline glass having a spinel crystal phase according to any one of (43) to (51), wherein its components, expressed in weight percentage, contain: Pr2O3: 0.4 to 6%; or Fe2O3: 0.2 to 5%; or MnO2: 0.1 to 3%; or Er2O3: 0.4 to 6%; or Nd2O3: 0.4 to 6%.
[0086] (79) The microcrystalline glass having a spinel crystal phase according to any one of (43) to (51), wherein the components thereof, expressed in weight percentage, contain: Er2O3: 0.4 to 6%, Nd2O3: 0.4 to 4%, and MnO2: 0.1 to 2%.
[0087] (80) A glass cover comprising a glass-ceramic product having a spinel crystal phase as described in any one of (1) to (42), and / or a glass-ceramic product having a spinel crystal phase as described in any one of (43) to (79).
[0088] (81) Glass components comprising a glass-ceramic product having a spinel crystal phase as described in any one of (1) to (42), and / or a glass-ceramic product having a spinel crystal phase as described in any one of (43) to (79).
[0089] (82) An electronic device comprising a glass-ceramic product having a spinel crystal phase as described in any one of (1) to (42), and / or a glass-ceramic product having a spinel crystal phase as described in any one of (43) to (79), and / or a glass cover as described in (80), and / or a glass component as described in (81).
[0090] (83) A display device comprising a glass-ceramic product having a spinel crystal phase as described in any one of (1) to (42), and / or a glass-ceramic product having a spinel crystal phase as described in any one of (43) to (79), and / or a glass cover as described in (80), and / or a glass component as described in (81).
[0091] (84). A method for manufacturing a glass-ceramic product having a spinel crystal phase as described in any one of (1) to (42), the method comprising the following steps: forming a matrix glass, subjecting the matrix glass to a crystallization process to form a glass-ceramic product having a spinel crystal phase, and then subjecting the glass-ceramic product having a spinel crystal phase to a chemical strengthening process to form a glass-ceramic product having a spinel crystal phase.
[0092] (85). According to the method for manufacturing a microcrystalline glass product having a spinel crystal phase as described in (84), the formation of the matrix glass includes the following steps: mixing the raw materials uniformly according to the component ratio, then placing them in a crucible, and melting them in an electric furnace or a gas furnace at a temperature range of 1350 to 1550°C for 5 to 24 hours, preferably at a melting temperature of 1450 to 1550°C, and then clarifying, homogenizing, forming, and annealing to obtain the matrix glass, wherein the clarifying temperature is greater than 1550°C but less than or equal to 1650°C, and the annealing temperature is 450 to 600°C.
[0093] (86). According to the method for manufacturing a microcrystalline glass product having a spinel crystal phase as described in (84), the crystallization process includes the following steps: heating to a prescribed crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.
[0094] (87) According to the method for manufacturing a microcrystalline glass product having a spinel crystal phase described in (84), the crystallization process includes the following steps: performing a nucleation process at a first temperature and then performing a crystal growth process at a second temperature.
[0095] (88) The method for manufacturing a microcrystalline glass product having a spinel crystal phase according to (87), wherein the crystallization process includes: a first temperature of 600 to 700°C, a second temperature greater than 700°C but less than or equal to 800°C, a holding time at the first temperature of 1 to 6 hours, and a holding time at the second temperature of 2 to 5 hours.
[0096] (89). The method for manufacturing a glass-ceramic product having a spinel crystal phase according to (84), wherein the chemical strengthening process comprises: immersing the glass-ceramic product having a spinel crystal phase in a salt bath of molten Na salt at 350 to 470°C for 1 to 36 hours, preferably in the temperature range of 400 to 460°C, and preferably in the time range of 2 to 15 hours; and / or immersing the glass-ceramic product having a spinel crystal phase in a mixed salt bath of molten K salt and Na salt at 360 to 450°C for 1 to 36 hours, preferably in the time range of 2 to 24 hours.
[0097] (90). A method for manufacturing a microcrystalline glass having a spinel crystal phase as described in any one of (43) to (79), the method comprising the following steps: forming a matrix glass, and then forming a microcrystalline glass having a spinel crystal phase through a crystallization process of the matrix glass.
[0098] (91). According to the method for manufacturing microcrystalline glass having a spinel crystal phase described in (90), the formation of the matrix glass includes the following steps: mixing the raw materials uniformly according to the component ratio, then placing them in a crucible, and melting them in an electric furnace or a gas furnace at a temperature range of 1350 to 1550°C for 5 to 24 hours, preferably at a melting temperature of 1450 to 1550°C, and then clarifying, homogenizing, forming, and annealing to obtain the matrix glass, wherein the clarification temperature is greater than 1550°C but less than or equal to 1650°C, and the annealing temperature is 450 to 600°C.
[0099] (92). According to the method for manufacturing microcrystalline glass having a spinel crystal phase described in (90), the crystallization process includes the following steps: heating to a prescribed crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling. The crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.
[0100] (93) According to the method for manufacturing a microcrystalline glass product having a spinel crystal phase described in (90), the crystallization process includes the following steps: performing a nucleation process at a first temperature and then performing a crystal growth process at a second temperature.
[0101] (94) The method for manufacturing a microcrystalline glass product having a spinel crystal phase according to (93), wherein the crystallization process includes: a first temperature of 600 to 700°C, a second temperature greater than 700°C but less than or equal to 800°C, a holding time at the first temperature of 1 to 6 hours, and a holding time at the second temperature of 2 to 5 hours.
[0102] The beneficial effects of the present invention are as follows: through reasonable component design, the glass-ceramics having a spinel crystal phase or the glass-ceramics products having a spinel crystal phase obtained by the present invention have excellent light transmittance and mechanical properties. DETAILED DESCRIPTION
[0103] The glass-ceramics having a spinel crystal phase and the glass-ceramics products having a spinel crystal phase of the present invention are materials having a crystalline phase (sometimes also referred to as crystals) and a glass phase. The crystalline phase of the glass-ceramics and glass-ceramics products can be identified by the peak angles appearing in the X-ray diffraction pattern obtained by X-ray diffraction analysis and / or measured by TEMEDX.
[0104] After repeated experiments and research, the inventors of the present invention have obtained the glass-ceramics having a spinel crystal phase or glass-ceramics products having a spinel crystal phase of the present invention by specifying the content and content ratio of the specific components constituting the glass-ceramics having a spinel crystal phase and the glass-ceramics products having a spinel crystal phase to specific values and containing a specific crystal phase. In the present invention, the glass-ceramics having a spinel crystal phase is sometimes referred to as simply glass-ceramics, and the glass-ceramics products having a spinel crystal phase are sometimes referred to as simply glass-ceramics.
[0105] The following describes the scope of each component (ingredient) of the matrix glass, microcrystalline glass, and microcrystalline glass products of the present invention. In this specification, unless otherwise specified, the content of each component is expressed as a weight percentage (wt%) relative to the total amount of the matrix glass, microcrystalline glass, or microcrystalline glass product material converted into an oxide composition. Here, the "composition converted into oxides" refers to the case where oxides, composite salts, hydroxides, etc. used as raw materials for the matrix glass, microcrystalline glass, or microcrystalline glass product components of the present invention decompose and transform into oxides when melted, and the total amount of the oxide material is taken as 100%. In addition, in this specification, when it is simply referred to as glass, it is the matrix glass before crystallization (i.e., crystallization process treatment), and the matrix glass after crystallization (i.e., crystallization process treatment) is referred to as microcrystalline glass, and microcrystalline glass products refer to products obtained after chemical strengthening of microcrystalline glass.
[0106] Unless otherwise indicated in specific circumstances, the numerical ranges listed herein include upper and lower limits, and "above" and "below" include the endpoints, as well as all integers and fractions within the range, without limitation to the specific values listed when defining the range. The term "about" as used herein means that the formula, parameters and other quantities and features are not and do not need to be exact, and may be approximate and / or larger or lower if necessary, reflecting tolerances, conversion factors and measurement errors, etc. The term "and / or" herein is inclusive, for example, "A; and / or B" means only A, or only B, or both A and B.
[0107] In some embodiments of the present invention, the spinel crystalline phase in the glass-ceramic or glass-ceramic product having a spinel crystalline phase is preferably a zinc aluminum spinel crystalline phase (ZnAl2O4). In some embodiments, the spinel crystalline phase has a higher weight percentage than other crystalline phases in the glass-ceramic or glass-ceramic product. In some embodiments, the spinel crystalline phase accounts for 20 to 60% by weight of the glass-ceramic or glass-ceramic product, preferably the spinel crystalline phase accounts for 25 to 50% by weight of the glass-ceramic or glass-ceramic product, more preferably the spinel crystalline phase accounts for 25 to 45% by weight of the glass-ceramic or glass-ceramic product, and further preferably the spinel crystalline phase accounts for 30 to 45% by weight of the glass-ceramic or glass-ceramic product. In some embodiments, the spinel crystalline phase accounts for 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, or 60% by weight of the microcrystalline glass or microcrystalline glass article.
[0108] In some embodiments of the present invention, the crystal phase in the glass-ceramic having a spinel crystal phase or the glass-ceramic product having a spinel crystal phase contains a quartz crystal phase (including both quartz and quartz solid solution). Preferably, the quartz crystal phase includes a β-quartz solid solution. In some embodiments, the weight percentage of the quartz crystal phase in the glass-ceramic or the glass-ceramic product is less than 20%, preferably the weight percentage of the quartz crystal phase in the glass-ceramic or the glass-ceramic product is less than 10%, more preferably the weight percentage of the quartz crystal phase in the glass-ceramic or the glass-ceramic product is less than 5%, and further preferably the glass-ceramic or the glass-ceramic product does not contain a quartz crystal phase. In some embodiments, the weight percentage of the quartz crystal phase in the microcrystalline glass or microcrystalline glass article is 0%, greater than 0%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, or 20%.
[0109] SiO2 is a network former in the glass-ceramics and glass-ceramics products of the present invention. SiO2 utilizes the structural components of silicon-oxygen tetrahedra to form a network structure, forming the basic structure of silicates. In some embodiments, SiO2 is also a necessary component for the formation of the quartz crystal phase. If the SiO2 content is too low, the chemical stability of the glass-ceramics and glass-ceramics products will deteriorate. If the SiO2 content is too high, it will significantly increase the viscosity of the glass, raising the melting temperature, making it difficult to smelt the material, and increasing the difficulty of forming the matrix glass. Therefore, the SiO2 content in the present invention is 40-55%, preferably 45-53%, and more preferably 48-52%. In some embodiments, the SiO2 may comprise about 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 48.5%, 49%, 49.5%, 50%, 50.5%, 51%, 51.5%, 52%, 52.5%, 53%, 53.5%, 54%, 54.5%, 55%.
[0110] Al2O3 is beneficial for improving the mechanical properties and chemical stability of the glass-ceramics and glass-ceramics products of the present invention, and is also an essential component for forming the spinel crystal phase of the present invention. Al2O3 can form [AlO4] tetrahedrons, replacing some [SiO4] tetrahedrons to form a network structure. The molecular volume of [AlO4] tetrahedron is 41 cm 3 / mol, the molecular volume of [SiO4] tetrahedron is 27.2 cm 3 / mol, after replacing part of the [SiO4] tetrahedron with [AlO4] tetrahedron, the molecular volume increases and the structural network space expands, which is beneficial to the diffusion of alkali metal ions during chemical strengthening and is also conducive to the acceptance of a large amount of Na + , promoting ion exchange. Too low an Al2O3 content is detrimental to enhancing the strengthening effect and crystal precipitation, resulting in poor mechanical properties and chemical stability of the glass. Too high an Al2O3 content makes glass melting difficult, requires high melting temperatures, and easily causes surface stone precipitation during molding. Therefore, the Al2O3 content is preferably 15-30%, preferably 18-25%, and more preferably 20-23%. In some embodiments, the Al2O3 may include about 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%.
[0111] In some embodiments, controlling the ratio of SiO2 to Al2O3 (SiO2 / Al2O3) within a range of 1.5 to 3.2 is beneficial for increasing the drop ball test height and four-point bending strength of glass-ceramics and glass-ceramics products, and increasing the ion exchange layer depth and surface stress of glass-ceramics products. Therefore, SiO2 / Al2O3 is preferably 1.5 to 3.2, more preferably 1.7 to 3.0, further preferably 1.8 to 2.8, and even more preferably 2.0 to 2.5. In some embodiments, the value of SiO2 / Al2O3 is 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.85, 2.9, 2.95, 3.0, 3.05, 3.1, 3.15, 3.2.
[0112] Li2O can lower the melting point of glass and is also an essential component for participating in chemical strengthening and improving the mechanical properties of glass-ceramics products. On the other hand, Li2O can provide free oxygen and reduce TiO2 coloring. If the Li2O content is too high, the crystals in the glass-ceramics and glass-ceramics products will easily grow, and the crystal growth will be unstable, which will affect the transmittance of the glass-ceramics and glass-ceramics products and deteriorate the chemical stability. Therefore, the content of Li2O is 0.1-6%, preferably 1-5%, and more preferably 2-4%. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, or 6% of Li2O may be included.
[0113] ZnO is an essential component for forming the spinel crystal phase of the present invention. The spinel crystal phase content can be regulated by controlling the content of ZnO and Al2O3, taking into account the transmittance while ensuring mechanical strength. If the ZnO content is low, the crystal phase content in the microcrystalline glass and microcrystalline glass products is low, and the mechanical properties such as Vickers hardness and Young's modulus are poor. If the ZnO content is too high, the residual Zn in the glass phase 2+ It hinders ion exchange during the chemical strengthening process, which is not conducive to obtaining high-performance micro-glass products. Therefore, the content of ZnO is 9-20%, preferably 11-18%, and more preferably 12-16%. In some embodiments, the content of ZnO may be about 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, or 20%.
[0114] In some embodiments, controlling the combined content of Al2O3 and ZnO (Al2O3+ZnO) within the range of 26-45% is beneficial for obtaining a desired content of spinel crystal phase in the glass-ceramics and glass-ceramics products, improving the drop resistance and ball drop test height of the glass-ceramics and glass-ceramics products while preventing deterioration in the surface stress of the glass-ceramics products. Therefore, the Al2O3+ZnO content is preferably 26-45%, more preferably 30-42%, further preferably 32-42%, and even more preferably 35-40%. In some embodiments, the Al2O3 + ZnO is 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5%, 35%, 35.5%, 36%, 36.5%, 37%, 37.5%, 38%, 38.5%, 39%, 39.5%, 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%.
[0115] In some embodiments, controlling the ratio of Al2O3 to ZnO (Al2O3 / ZnO) within a range of 1.0 to 3.0 is beneficial for improving the hardness of the glass-ceramics and glass-ceramics products, optimizing the Young's modulus, and preventing a decrease in transmittance and deterioration in haze of the glass-ceramics and glass-ceramics products. Therefore, Al2O3 / ZnO is preferably 1.0 to 3.0, more preferably 1.2 to 2.8, further preferably 1.25 to 2.5, and even more preferably 1.5 to 2.3. In some embodiments, the Al2O3 / ZnO is 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.85, 2.9, 2.95, 3.0.
[0116] TiO2 is a nucleating agent for the glass-ceramics and glass-ceramics products of the present invention. If the TiO2 content is too high, the glass-ceramics and glass-ceramics products will be severely colored (brown-yellow), and the transmittance of the glass-ceramics and glass-ceramics products in the visible light region will be reduced, and the haze and |B| value will increase. In addition, if the TiO2 content is too high, the glass will easily become milky during molding and crystallization, making the glass opaque. Therefore, the content of TiO2 in the present invention is 0.5-7%, preferably 1-6%, and more preferably 2-5%. In some embodiments, it may contain about 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, or 7% TiO2.
[0117] In some embodiments, controlling the ratio of Li2O content to TiO2 content (Li2O / TiO2) within the range of 0.2 to 4.5 can effectively reduce the Ti content in glass-ceramics and glass-ceramics products. 3+ Ion coloring improves the transmittance of glass-ceramics and glass-ceramics products, and optimizes the haze and |B| value of glass-ceramics and glass-ceramics products. Therefore, the Li2O / TiO2 ratio is preferably 0.2 to 4.5, more preferably 0.5 to 3.5, further preferably 0.7 to 2.5, and even more preferably 0.75 to 1.5. In some embodiments, the Li2O / TiO2 is 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5.
[0118] In some embodiments, controlling the ratio (TiO2+ZnO) / Al2O3 between the combined content of TiO2 and ZnO (TiO2+ZnO) and the content of Al2O3 within the range of 0.4 to 1.5 can optimize the chemical strengthening properties of the glass-ceramics, increase the depth of the ion exchange layer of the glass-ceramics product, and improve the fracture toughness, four-point bending strength, and drop ball test height. Therefore, preferably, (TiO2+ZnO) / Al2O3 is 0.4 to 1.5, more preferably (TiO2+ZnO) / Al2O3 is 0.5 to 1.2, further preferably (TiO2+ZnO) / Al2O3 is 0.6 to 1.0, and even more preferably (TiO2+ZnO) / Al2O3 is 0.6 to 0.9. In some embodiments, (TiO2+ZnO) / Al2O3 is 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5.
[0119] ZrO2 can be used as a nucleating agent for microcrystalline glass and microcrystalline glass products. When used together with TiO2, it can make the microcrystalline glass nuclei as numerous as possible. When there are more nuclei, it is conducive to stable crystal growth and uniform grain size. If the ZrO2 content is too high, the melting of the glass will be more difficult. Therefore, the content of ZrO2 is 0-5%, preferably 0.5-4%, and more preferably 1-3%. In some embodiments, it may contain about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5% ZrO2.
[0120] ZrO2 has a low solubility in the glass system of the present invention. In some embodiments, the solubility of ZrO2 in the glass can be increased by containing a certain amount of P2O5. However, if too much P2O5 is contained, the glass will easily separate during molding, resulting in reduced chemical stability of the microcrystalline glass and microcrystalline glass products. Therefore, the content of P2O5 in the present invention is 0-5%, preferably 0.5-4%, and more preferably 1-3%. In some embodiments, it may contain about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5% P2O5.
[0121] In some embodiments, controlling the ratio of the combined content of Al2O3 and Li2O (Al2O3+Li2O) to the content of P2O5 ((Al2O3+Li2O) / P2O5)) within a range of 5.0 to 45.0 is beneficial for improving the four-point bending strength and drop resistance of the glass-ceramics and glass-ceramics products, and increasing the surface stress of the glass-ceramics products. Therefore, (Al2O3+Li2O) / P2O5 is preferably 5.0 to 45.0, more preferably (Al2O3+Li2O) / P2O5 is 7.0 to 35.0, further preferably (Al2O3+Li2O) / P2O5 is 8.0 to 30.0, and even more preferably (Al2O3+Li2O) / P2O5 is 10.0 to 25.0. In some embodiments, (Al2O3 + Li2O) / P2O5 is 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0, 12.5, 13.0, 13.5, 14.0, 14.5, 15.0, 15.5, 16.0, 16.5, 17.0, 17.5, 18.0, 18.5, 19.0 , 19.5, 20.0, 20.5, 21.0, 21.5, 22.0, 22.5, 23.0, 23.5, 24.0, 24.5, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, 40.0, 41.0, 42.0, 43.0, 44.0, 45.0.
[0122] In some embodiments, controlling the combined content of P2O5 and ZrO2 (P2O5+ZrO2) within the range of 0-8% is beneficial for obtaining uniform grains and smaller grain sizes in the glass-ceramics and glass-ceramics products, thereby optimizing the transmittance of the glass-ceramics and glass-ceramics products. Therefore, the P2O5+ZrO2 content is preferably 0-8%, more preferably 0.1-7%, and even more preferably 0.5-5%. In some embodiments, P2O5+ZrO2 is 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6. %, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9%, 8%.
[0123] In some embodiments, controlling the ratio of P2O5 to ZrO2 (P2O5 / ZrO2) within a range of 0.1 to 5.0 is beneficial for improving the hardness and fracture toughness of glass-ceramics and glass-ceramics products, and preventing deterioration in drop resistance and Young's modulus. Therefore, P2O5 / ZrO2 is preferably 0.1 to 5.0, more preferably 0.2 to 3.0, further preferably 0.5 to 2.0, and even more preferably 0.6 to 1.5. In some embodiments, P2O5 / ZrO2 is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0.
[0124] MgO helps reduce the viscosity of the glass, inhibits glass crystallization during molding, refines grains during crystallization, and also has the effect of improving low-temperature solubility. In some embodiments, MgO has the effect of promoting the formation of a quartz solid solution crystal phase. If the MgO content is too high, a quartz solid solution crystal phase is easily formed during glass crystallization. The quartz solid solution crystal phase has larger grains, which will reduce the transmittance of the micro-ceramic glass and micro-ceramic glass products. Therefore, the MgO content is 0.1-6%, preferably 1-5%, and more preferably 2-4%. In some embodiments, the present invention may comprise about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9% or more. %, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6% MgO.
[0125] In some embodiments, controlling the ratio (Li2O+MgO) / TiO2 of the combined content of Li2O and MgO (Li2O+MgO) to the content of TiO2 within the range of 0.3 to 8.0 can refine the grains, improve the transmittance and drop resistance of the glass-ceramics and glass-ceramics products, and optimize the haze and |B| value of the glass-ceramics and glass-ceramics products. Therefore, (Li2O+MgO) / TiO2 is preferably 0.3 to 8.0, more preferably (Li2O+MgO) / TiO2 is 0.5 to 5.0, further preferably (Li2O+MgO) / TiO2 is 1.0 to 3.0, and even more preferably (Li2O+MgO) / TiO2 is 1.2 to 2.5. In some embodiments, (Li2O+MgO) / TiO2 is 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0.
[0126] In some embodiments, controlling the ratio of the Al2O3 content to the combined content of MgO and TiO2 (MgO+TiO2), Al2O3 / (MgO+TiO2), within a range of 1.3 to 10.0 is beneficial for improving the hardness and drop ball test height of the glass-ceramics and glass-ceramics products, and optimizing the surface stress and haze of the glass-ceramics products. Therefore, Al2O3 / (MgO+TiO2) is preferably 1.3 to 10.0, more preferably 1.5 to 8.0, further preferably 2.5 to 6.5, and even more preferably 3.0 to 5.5. In some embodiments, Al2O3 / (MgO+TiO2) is 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3 , 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10.0.
[0127] B2O3 helps melt glass and improves its melting efficiency. Excessive B2O3 content can weaken the chemical stability of the glass, leading to boron anomaly, where the boron-oxygen tetrahedron structure transforms into a boron-oxygen triangular structure, and lowering the viscosity of the glass. Furthermore, boron volatilization can easily form streaks, making the glass uneven. Therefore, the B2O3 content is preferably 0-4%, preferably 0-2%, and more preferably 0-1%. In some embodiments, the present invention may include about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4% B2O3.
[0128] Na2O can promote glass melting and improve the chemical strengthening properties of microcrystalline glass. However, if too much Na2O is contained in the present invention, it is easy to cause more broken bonds in the glass, reduce the strength of the matrix glass, and affect the strength of the microcrystalline glass and microcrystalline glass products. Therefore, the upper limit of the Na2O content in the present invention is 6%, preferably 4%, and more preferably 2%. In some embodiments, it may contain about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7% , 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6% Na2O.
[0129] In some embodiments, controlling the ratio (SiO2 + Na2O) / ZnO of the combined SiO2 and Na2O contents (SiO2 + Na2O) to the ZnO content within a range of 2.2 to 6.2 can improve the fracture toughness and compressive strength of the glass-ceramics and glass-ceramics products while optimizing the |B| value. Therefore, (SiO2 + Na2O) / ZnO is preferably 2.2 to 6.2, more preferably 2.5 to 6.0, further preferably 2.8 to 5.5, and even more preferably 3.0 to 5.0. In some embodiments, (SiO2 + Na2O) / ZnO is 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2.
[0130] K2O helps lower the glass melting temperature, facilitates chemical strengthening, and increases the depth of the ion exchange layer of microcrystalline glass products. However, if too much K2O is contained, it can easily reduce the chemical stability of the glass and reduce the hardness. Therefore, the content of K2O is 3% or less, preferably 2% or less, and more preferably 1% or less. In some embodiments, the content of K2O may be about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, or 3%.
[0131] In some embodiments, controlling the ratio of the combined content of Na2O and KO to the content of ZnO (Na2O+KO) / ZnO) to be below 0.8 can refine the grains, reduce the grain size of the glass-ceramics and glass-ceramics products, improve the transmittance and compressive strength of the glass-ceramics and glass-ceramics products, and optimize the haze of the glass-ceramics and glass-ceramics products. Therefore, preferably, (Na2O+KO) / ZnO is below 0.8, more preferably, (Na2O+KO) / ZnO is below 0.6, further preferably, (Na2O+KO) / ZnO is below 0.4, and even more preferably, (Na2O+KO) / ZnO is below 0.2. In some embodiments, (Na2O + KO) / ZnO is 0, greater than 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8.
[0132] CaO, BaO and SrO as co-solvents do not participate in the formation of the crystal phase and remain in the residual glass phase of the microcrystalline glass, which is beneficial to lowering the melting temperature and processing temperature. However, too high a content will damage the nucleation and crystallization in the process of the matrix glass being transformed into microcrystalline glass, and have an adverse effect on the chemical stability of the microcrystalline glass. Therefore, the total content of CaO, BaO and SrO CaO+BaO+SrO is 0-5%, preferably 0-4%, and more preferably 0-2%. In some embodiments, CaO+BaO+SrO is 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1% or more. %, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%.
[0133] Y2O3 can promote the melting of ZrO2 and reduce the difficulty of melting glass. When the content is too high, it will make it difficult to form crystals during the crystallization of the glass, and the drop ball test height of the microcrystalline glass and microcrystalline glass products will decrease. Therefore, the upper limit of the Y2O3 content is 6%, preferably 4%, and more preferably 2%. In some embodiments, it may contain about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1 %, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6% Y2O3.
[0134] In some embodiments, the glass, glass-ceramic, or glass-ceramic product may further contain 0-2% of a clarifier to enhance the defoaming ability of the glass, glass-ceramic, or glass-ceramic product. Such clarifiers include, but are not limited to, one or more of Sb2O3, SnO2, SnO, CeO2, F (fluorine) compounds, Cl (chlorine) compounds, and Br (bromine) compounds, with Sb2O3 being preferred. When these clarifiers are present alone or in combination, their content is preferably capped at 2%, more preferably at 1%, and even more preferably at 0.5%. In some embodiments, one or more of the clarifiers is present in an amount of about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, or 2%.
[0135] Other components not mentioned above, such as La2O3, Gd2O3, Yb2O3, Nb2O5, WO3, Bi2O3, Ta2O5, TeO2, etc., may be appropriately added without affecting the properties of the glass, glass-ceramics, or glass-ceramics products of the present invention. However, to maintain the excellent properties of the glass, glass-ceramics, or glass-ceramics products of the present invention, the individual or combined content of La2O3, Gd2O3, Yb2O3, Nb2O5, WO3, Bi2O3, Ta2O5, and TeO2 is preferably 5% or less, more preferably 2% or less, even more preferably 1% or less, and even more preferably, not contained.
[0136] PbO and As2O3 are toxic substances, and even a small amount thereof does not meet the requirements of environmental protection. Therefore, in some embodiments of the present invention, it is preferred that PbO and / or As2O3 are not contained.
[0137] In some embodiments of the present invention, colored matrix glass, glass-ceramics, or glass-ceramics products can be prepared by including a colorant, allowing the matrix glass, glass-ceramics, or glass-ceramics products to exhibit different colors. The colorant includes: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O5: 0-8%; and / or CeO2: 0-4%. The weight percentage content of the colorant and its function are detailed as follows:
[0138] The brown or green matrix glass, glass-ceramic, or glass-ceramic product prepared by the present invention uses NiO, Ni2O3, or Pr2O5 as a colorant. NiO and Ni2O3 are used as colorants to prepare the brown or green matrix glass, glass-ceramic, or glass-ceramic product. The two components can be used alone or in combination. Their respective content is generally 4% or less, preferably 3% or less. If the content exceeds 4%, the colorant will not dissolve well in the matrix glass, glass-ceramic, or glass-ceramic product. The lower limit of their respective content is 0.1% or more. If it is less than 0.1%, the color of the matrix glass, glass-ceramic, or glass-ceramic product will not be obvious. In some embodiments, NiO or Ni2O3 may be included in an amount of about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, or 4.0%. When used in combination, the total amount of NiO and Ni2O3 is generally less than 4%, and the lower limit of the total amount is greater than 0.1%. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% NiO and Ni2O3 may be included. Pr2O5 is used as a colorant for green matrix glass, microcrystalline glass or microcrystalline glass products. It is used alone, and the general content is less than 8%, preferably less than 6%, and the lower limit of the content is above 0.4%. If it is less than 0.4%, the color of the matrix glass, microcrystalline glass or microcrystalline glass products will not be obvious.In some embodiments, the Pr2O5 may be included at about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0%.
[0139] The blue matrix glass, glass-ceramic, or glass-ceramic product prepared by the present invention uses CoO or Co2O3 as a colorant. The two colorant components can be used alone or in combination. The content of each is generally less than 2%, preferably less than 1.8%. If the content exceeds 2%, the colorant cannot be well dissolved in the matrix glass, glass-ceramic, or glass-ceramic product. The lower limit of each content is above 0.05%. If it is less than 0.05%, the color of the matrix glass, glass-ceramic, or glass-ceramic product is not obvious. In some embodiments, the CoO or Co2O3 content can be about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, or 2.0%. When used in combination, the total amount of CoO and Co2O3 does not exceed 2%, and the lower limit of the total amount is above 0.05%. In some embodiments, the amount of CoO and Co2O3 may be about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, or 2.0%.
[0140] The yellow matrix glass, microcrystalline glass or microcrystalline glass products prepared by the present invention use Cu2O or CeO2 as a colorant. The two colorant components are used alone or in combination, and the lower limit of their respective content is above 0.5%. If it is lower than 0.5%, the color of the matrix glass, microcrystalline glass or microcrystalline glass products is not obvious. Cu2O is used alone at a content of less than 4%, preferably less than 3%. If the content exceeds 4%, the matrix glass is likely to crystallize. In some embodiments, the CuO content may be about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, or 4.0%. The CeO content alone is generally less than 4%, preferably less than 3%. If the content exceeds 4%, the matrix glass, glass-ceramics, or glass-ceramics products may have poor gloss. In some embodiments, CeO2 may be included in an amount of about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, or 4.0%. Furthermore, a small amount of CeO2 added to the glass has a degassing effect. CeO2 can also be used as a clarifier in the glass. When used as a clarifier, its content is less than 2%, preferably less than 1%, and more preferably less than 0.5%. If two colorants are mixed, their total amount is generally less than 4%, and the lower limit of the total amount is above 0.5%. In some embodiments, CeO2 and Cu2O may be included in an amount of about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, or 4.0%.
[0141] The black or smoky gray matrix glass, glass-ceramics or glass-ceramics products prepared by the present invention use Fe2O3 alone as a colorant; or use a mixture of Fe2O3 and CoO as a colorant; or use a mixture of Fe2O3 and Co2O3 as a colorant; or use a mixture of Fe2O3, CoO and NiO as a colorant; or use a mixture of Fe2O3, Co2O3 and NiO as a colorant. The colorant used to prepare black and smoky gray matrix glass, glass-ceramics or glass-ceramics products mainly uses Fe2O3 for coloring, with a content of less than 7%, preferably less than 5%, and its lower limit is more than 0.2%. In some embodiments, it may contain about 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6% %, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0% of Fe2O3. CoO and Co2O3 absorb in visible light and can deepen the coloring of the matrix glass, glass-ceramic or glass-ceramic products. Generally, when mixed with Fe2O3, the content of each is less than 0.6%, and the lower limit is above 0.2%. In some embodiments, CoO and / or Co₂O₃ may be included at approximately 0.2%, 0.3%, 0.4%, 0.5%, or 0.6%. NiO absorbs visible light and can enhance the coloration of the matrix glass, glass-ceramics, or glass-ceramics products. Generally, when mixed, its content is less than 1%, with a combined lower limit of 0.2%. In some embodiments, NiO may be included at approximately 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1.0%.
[0142] The purple matrix glass, microcrystalline glass or microcrystalline glass products prepared by the present invention use MnO2 as a colorant, and the content is generally less than 4%, preferably less than 3%, and the lower limit of the content is above 0.1%. If it is less than 0.1%, the color of the matrix glass, microcrystalline glass or microcrystalline glass products is not obvious. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% MnO2 may be included.
[0143] The pink matrix glass, glass-ceramics, or glass-ceramics products prepared by the present invention use Er2O3 as a colorant, with the usage content generally being 8% or less, preferably 6% or less. Due to the low coloring efficiency of the rare earth element Er2O3, a content exceeding 8% does not further deepen the color of the matrix glass, glass-ceramics, or glass-ceramics products, and instead increases costs. The lower limit of Er2O3 is 0.4% or greater. If it is less than 0.4%, the color of the matrix glass, glass-ceramics, or glass-ceramics products is less noticeable. In some embodiments, Er2O3 may be included in an amount of about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0%.
[0144] The purple-red matrix glass, glass-ceramics, or glass-ceramics products prepared by the present invention use Nd2O3 as a colorant, with the usage content generally being 8% or less, preferably 6% or less. Because the rare earth element Nd2O3 has low coloring efficiency, using a content exceeding 8% will not further deepen the color of the matrix glass, glass-ceramics, or glass-ceramics products, but will instead increase costs. The lower limit of the Nd2O3 content is 0.4% or greater. If it is less than 0.4%, the color of the matrix glass, glass-ceramics, or glass-ceramics products will not be noticeable. In some embodiments, the Nd2O3 may be included in an amount of about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0%.
[0145] The red matrix glass, microcrystalline glass or microcrystalline glass products prepared by the present invention use a mixed colorant of Er2O3, Nd2O3 and MnO2. The Er ions in the glass have absorption at 400-500nm, the Mn ions mainly absorb at 500nm, and the Nd ions mainly have strong absorption at 580nm. The mixture of the three substances can be used to prepare red matrix glass, microcrystalline glass or microcrystalline glass products. Since Er2O3 and Nd2O3 are rare earth colorants, their coloring ability is relatively weak. The usage amount of Er2O3 is within 6%, the usage amount of Nd2O3 is within 4%, and the coloring of MnO2 is strong, with a usage amount within the range of 2%. The lower limit of the total amount of the mixed colorants used is above 0.9%.
[0146] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the matrix glass, microcrystalline glass or microcrystalline glass product of the present invention; however, as the raw materials and / or equipment for producing matrix glass, microcrystalline glass or microcrystalline glass products, there will be certain impurities or components that are not intentionally added, which will be contained in small amounts or trace amounts in the final matrix glass, microcrystalline glass or microcrystalline glass product. This situation is also within the scope of protection of the patent of this invention.
[0147] The grain size and crystalline phase type of the glass-ceramics or glass-ceramics products of the present invention affect the haze and light transmittance of the glass-ceramics or glass-ceramics products. Smaller grains increase light transmittance, and lower haze indicates higher light transmittance. In some embodiments, the haze of a glass-ceramics product or glass-ceramics with a thickness of less than 1 mm is 0.3% or less, preferably 0.25% or less, and more preferably 0.05-0.2%. In some embodiments, the grain size of the glass-ceramics product or glass-ceramics is 60 nm or less, preferably 45 nm or less, and more preferably 10-30 nm.
[0148] In some embodiments, the crystalline phase content and refractive index of the glass-ceramics or glass-ceramics products of the present invention affect the |B| value of the glass-ceramics or glass-ceramics products. When observed in the visible light range, the glass-ceramics or glass-ceramics products appear bluish or yellowish, affecting the optical properties of the product, which is indicated by the |B| value in LAB (chromaticity value of material color). The glass-ceramics or glass-ceramics products of the present invention exhibit low |B| values in the visible light range. In some embodiments, the average optical |B| value of a glass-ceramics product or glass-ceramics with a thickness of less than 1 mm at 400-800 nm is less than 1.0, preferably less than 0.8, and more preferably 0.3-0.6.
[0149] In some embodiments, the glass-ceramics or glass-ceramics products of the present invention exhibit high transparency in the visible light range (i.e., the glass-ceramics or glass-ceramics products are transparent). Glass-ceramics or glass-ceramics products exhibit high transmittance in the visible light range. In some embodiments, the average light transmittance of glass-ceramics products with a thickness of less than 1 mm or glass-ceramics at 400 to 800 nm is preferably 87.0% or more, more preferably 88.5% or more, and further preferably 89.5% or more. In some preferred embodiments, the light transmittance of glass-ceramics products with a thickness of less than 1 mm or glass-ceramics at 550 nm is preferably 87.0% or more, more preferably 88.0% or more, and further preferably 89.0% or more.
[0150] In some embodiments, antimicrobial components may be added to the matrix glass, glass-ceramic, or glass-ceramic product. The glass-ceramic or glass-ceramic products described herein may be used in applications such as kitchen or dining countertops, where exposure to harmful bacteria is likely. Antimicrobial components contained in the matrix glass, glass-ceramic, or glass-ceramic product include, but are not limited to, Ag, AgO, Cu, CuO, Cu2O, and the like. In some embodiments, the content of these antimicrobial components, alone or in combination, is 2% or less, preferably 1% or less.
[0151] The matrix glass, the glass-ceramics having a spinel crystal phase, and the glass-ceramics products having a spinel crystal phase of the present invention can be produced and manufactured by the following method:
[0152] Generating the matrix glass: The raw materials (oxides, hydroxides, composite salts, etc.) are uniformly mixed according to the component ratio, then placed in a crucible (e.g., platinum or quartz crucible). Depending on the melting difficulty of the glass composition, the glass is melted in an electric furnace or gas furnace at a temperature range of 1350-1550°C for 5-24 hours, preferably 1450-1550°C. The matrix glass is then clarified, homogenized, formed, and annealed to obtain the matrix glass. The clarification temperature is preferably greater than 1550°C but less than or equal to 1650°C, and the annealing temperature is preferably 450-600°C.
[0153] The matrix glass of the present invention can be formed by a well-known method.
[0154] The matrix glass of the present invention is crystallized by a crystallization process after forming or forming processing, and crystals are uniformly separated out inside the glass to make glass-ceramics. The crystallization process can be carried out in one stage or in two stages, and preferably in two stages. The two stages of crystallization are carried out as a process of carrying out a nucleation process at a first temperature and then a process of carrying out a crystal growth process at a second temperature. The crystallization process carried out at the first temperature is referred to as the first crystallization process, and the crystallization process carried out at the second temperature is referred to as the second crystallization process.
[0155] In order to obtain the desired physical and chemical properties of glass-ceramics, the preferred crystallization process is:
[0156] The above-mentioned single-stage crystallization process allows for continuous nucleation and crystal growth. Specifically, the temperature is raised to a predetermined crystallization temperature, maintained at that temperature for a predetermined period of time, and then cooled. The crystallization temperature is preferably 600-800°C, more preferably 650-750°C to precipitate the desired crystalline phase. The holding time at the crystallization temperature is preferably 1-10 hours, more preferably 3-6 hours.
[0157] When the crystallization treatment is carried out in two stages, the first temperature is preferably 600-700°C, the second temperature is preferably greater than 700°C but less than or equal to 800°C, the holding time at the first temperature is preferably 1-6 hours, and the holding time at the second temperature is preferably 2-5 hours.
[0158] In some embodiments, the matrix glass or glass-ceramics described herein can be manufactured into formed bodies, including but not limited to sheets, by various processes, including but not limited to slot drawing, float glass, roller pressing, and other sheet-forming processes known in the art. Alternatively, the matrix glass or glass-ceramics can be formed by float or roller pressing methods known in the art. Formed bodies described herein also include lenses, prisms, and the like.
[0159] The matrix glass or glass-ceramics of the present invention can be used to manufacture a sheet glass molded body or glass-ceramics molded body by grinding or polishing, but the method of manufacturing the glass molded body or glass-ceramics molded body is not limited to these methods.
[0160] The matrix glass or glass-ceramics of the present invention can be prepared into glass formed bodies or glass-ceramics formed bodies of various shapes by using a hot bending process or a press process at a certain temperature, but is not limited to these methods.
[0161] In some embodiments, a glass or glass-ceramic formed body can be formed using a heat bending process. The heat bending process involves placing 2D or 2.5D glass or glass-ceramic in a mold and performing a series of steps in a heat bending machine, including preheating, pressurizing, and cooling, to produce a 3D curved glass or glass-ceramic formed body.
[0162] In some embodiments, a glass-ceramic body has a 2.5D or 3D configuration, i.e., the glass-ceramic body has a non-planar configuration. As used herein, "non-planar configuration" means that, within a 2.5D or 3D shape, at least a portion of the glass-ceramic body extends outward or at an angle relative to a plane defined by the original, laid-out configuration of the 2D matrix glass. A 2.5D or 3D glass-ceramic body formed from a matrix glass may have one or more protrusions or curves.
[0163] The matrix glass, the glass-ceramic having a spinel crystalline phase, and the glass-ceramic article having a spinel crystalline phase described in the present invention can have any reasonably useful thickness.
[0164] In addition to improving mechanical properties by crystallization, the glass-ceramics having a spinel crystal phase of the present invention can also obtain more excellent mechanical properties by forming a compressive stress layer, thereby manufacturing a glass-ceramics product having a spinel crystal phase.
[0165] In some embodiments, the matrix glass or glass-ceramics can be processed into sheets and / or shaped (such as punching, hot bending, etc.), polished and / or smoothed after shaping, and then chemically strengthened through a chemical strengthening process.
[0166] The chemical strengthening described in this invention is an ion exchange process. During the ion exchange process, smaller metal ions in the matrix glass or glass-ceramics are replaced or "exchanged" with larger metal ions of the same valence located near the matrix glass or glass-ceramics. The replacement of smaller ions with larger ions builds up compressive stress in the matrix glass or glass-ceramics, forming a compressive stress layer.
[0167] In some embodiments, the metal ion is a monovalent alkali metal ion (e.g., Na + , K+ , Rb + 、Cs + Ion exchange is performed by immersing the matrix glass or glass-ceramic in a salt bath containing at least one molten salt of a larger metal ion, which is used to replace the smaller metal ions in the matrix glass. Alternatively, other monovalent metal ions such as Ag + 、Tl + 、Cu + The one or more ion exchange processes used to chemically strengthen the matrix glass or glass-ceramic may include, but are not limited to, immersing it in a single salt bath, or immersing it in multiple salt baths of the same or different compositions with washing and / or annealing steps between immersions.
[0168] In some embodiments, the matrix glass or glass-ceramic can be ion-exchanged by immersing it in a bath of molten Na salt (e.g., NaNO3) at a temperature of about 350-470°C for about 1-36 hours, preferably in the temperature range of 400-460°C, and for a time range of 2-15 hours. In this embodiment, the Na ions replace some of the Li ions in the matrix glass or glass-ceramic, thereby forming a surface compressive layer and exhibiting high mechanical properties. In some embodiments, the matrix glass or glass-ceramic can be ion-exchanged by immersing it in a mixed salt bath of molten K salt and Na salt at a temperature of about 360-450°C for about 1-36 hours, preferably in the time range of 2-24 hours.
[0169] The glass-ceramics with spinel crystal phases disclosed herein have high-efficiency low-temperature ion exchange performance. In some embodiments, at a lower ion exchange temperature and a shorter exchange time, the exchange layer depth of Na ions can reach more than 75 μm. After ion exchange, the hardness of the glass-ceramics product with spinel crystal phase is significantly improved. The main reason is that the ion exchange forms a higher compressive stress on the surface of the glass-ceramics product with spinel crystal phase through the "crowding effect", which increases the deformation resistance of the glass-ceramics product with spinel crystal phase and improves the hardness. In some embodiments, after chemical strengthening of the glass-ceramics with spinel crystal phases of the present invention, the Vickers hardness of the obtained glass-ceramics product can reach 650 kgf / mm 2 above.
[0170] The various performance indicators of the glass-ceramics having a spinel crystal phase and / or the glass-ceramics products having a spinel crystal phase of the present invention are tested using the following methods:
[0171] [Haze]
[0172] A haze tester, Minolta CM3600A, was used to prepare samples with a thickness of less than 1 mm and the test was performed according to the GB2410-80 standard.
[0173] [Grain size]
[0174] The SEM scanning electron microscope was used for measurement. The microcrystalline glass was surface treated in HF acid, and then the surface of the microcrystalline glass was sprayed with gold. The surface was scanned under the SEM scanning electron microscope to determine the size of its grains.
[0175] [Light transmittance]
[0176] The light transmittance described in this article is external transmittance, sometimes referred to as transmittance.
[0177] The sample was processed to a thickness of less than 1 mm and the opposite surfaces were parallel-polished. The average light transmittance at 400 to 800 nm was measured using a Hitachi U-41000 spectrophotometer.
[0178] The sample was processed to a thickness of less than 1 mm and the opposite surfaces were parallel-polished. The light transmittance at 550 nm was measured using a Hitachi U-41000 spectrophotometer.
[0179] [Depth of ion exchange layer]
[0180] The depth of the ion exchange layer was measured using a glass surface stress meter SLP-2000.
[0181] The calculation was performed under the measurement conditions that the refractive index of the sample was 1.56 and the photoelastic constant was 29 [(nm / cm) / Mpa].
[0182] [Surface stress]
[0183] The surface stress was measured using a glass surface stress meter SLP-2000.
[0184] The calculation was performed under the measurement conditions that the refractive index of the sample was 1.56 and the photoelastic constant was 29 [(nm / cm) / Mpa].
[0185] [Drop resistance]
[0186] The drop resistance test was carried out using a directional drop tester WH-2101. By loading glass products of the same specifications on 2D glass-ceramic products (each weighing 20g, with 2 pieces loaded), laying 60-80 mesh sandpaper on the base, and letting it fall freely from a specified height, the sample hits the sandpaper directly, and the height at which it can withstand the impact without breaking is the drop resistance. Specifically, the test is carried out from a height of 600mm. Without breaking, the height is changed in sequence through 700mm, 800mm, 900mm, 1000mm and above. For the embodiments with "drop resistance", glass-ceramic products are used as test objects. The test data recorded as 1000mm in the embodiment indicates that even if the glass-ceramic product with a load is dropped from a height of 1000mm, it will withstand the impact without breaking. The maximum experimental height of the drop tester WH-2101 is 2000mm.
[0187] [Drop ball test height]
[0188] A sample of a microcrystalline glass product of 145mm×67mm×0.7mm is placed on a glass supporting fixture, and a 132g steel ball is dropped from a specified height, with the landing point being the center point of the sample. The maximum drop ball test height at which the sample can withstand the impact without breaking is defined. Specifically, the drop ball test height starts at 400mm, and the ball is dropped once at each height. If the sample does not break, the test is continued by successively rising 100mm until the sample breaks. For the embodiments with a "drop ball test height", the microcrystalline glass product is used as the test object. The test data recorded as 1700mm in the embodiment indicates that the microcrystalline glass product can withstand the impact without breaking even if the steel ball is dropped from a height of 1700mm. The drop ball test height in the present invention is sometimes referred to as the drop ball height.
[0189] [Fracture toughness]
[0190] The method of directly measuring the size of the indentation-extended crack was used. The sample size was 2mm×4mm×20mm. After chamfering, grinding and polishing, the sample was prepared. A Vickers hardness indenter was used to apply a force of 49N to the sample and maintain it for 30s. After the indentation was made, the fracture strength was measured using the three-point bending method.
[0191] [Four-point bending strength]
[0192] A microcomputer-controlled electronic universal testing machine CMT6502 was used, and the sample specification was 1 mm or less in thickness (preferably 0.7 mm in thickness), and the test was conducted according to ASTM C 158-2002. In the present invention, the four-point bending strength is sometimes referred to as the bending strength.
[0193] [Vickers hardness]
[0194] The load (N) when a diamond square pyramid indenter with an angle of 136° between the opposing faces presses a pyramid-shaped depression into the test surface is divided by the surface area (mm2) calculated from the length of the depression. 2 ) value. The test load was set to 100 (N) and the holding time was set to 15 (seconds). In the present invention, Vickers hardness may be simply referred to as hardness.
[0195] [Compression strength]
[0196] A microcomputer-controlled electronic universal testing machine CMT6502 is used to place a 145mm×67mm×0.7mm microcrystalline glass product sample on a glass supporting fixture. The extrusion rod adopts a mushroom head design with a diameter of ¢10mm and a downward pressing speed of 5mm / min until the sample is broken. Calibration with a fixture is required before the test, and the test point is at the center. Click the test button until the microcrystalline glass product sample is squeezed and broken, and record the pressure (N) when the sample breaks. For embodiments with "anti-extrusion strength", microcrystalline glass products are used as test objects. The test data recorded as 500N in the embodiment indicates that the maximum extrusion force that the microcrystalline glass product can withstand before breaking is 500N.
[0197] [|B|value]
[0198] A Minolta CM-700d was used for B-value testing. Samples were 1mm or less thick. The instrument was zero-calibrated and white-plate-calibrated using the supplied calibration tube and short tube, respectively. After calibration, the long tube was used to perform an air test to determine the stability and reliability of the instrument's calibration (B ≤ 0.05). After the instrument passed calibration, the product was placed on the zero-calibrated long tube for testing.
[0199] The |B| value is the absolute value of the B value.
[0200] [Young's modulus]
[0201] Young's modulus (E) is calculated using the following formula using ultrasonic testing of its longitudinal wave velocity and shear wave velocity. G=V S 2 ρ
[0202] Where: E is Young's modulus, Pa;
[0203] G is the shear modulus, Pa;
[0204] V T is the shear wave velocity, m / s;
[0205] V S is the longitudinal wave velocity, m / s;
[0206] ρ is the density of glass, g / cm 3 .
[0207] The glass-ceramic product having a spinel crystal phase of the present invention has the following properties:
[0208] 1) In some embodiments, the crystal size of the glass-ceramic product having the spinel crystal phase is 60 nm or less, preferably 45 nm or less, and more preferably 10 to 30 nm.
[0209] 2) In some embodiments, the ion exchange layer of the glass-ceramic article having a spinel crystal phase has a depth of 75 μm or more, preferably 80 to 150 μm, and more preferably 100 to 125 μm.
[0210] 3) In some embodiments, the surface stress of the glass-ceramic product having a spinel crystal phase is greater than 200 MPa, preferably 250 to 400 MPa, and more preferably 300 to 400 MPa.
[0211] 4) In some embodiments, the drop ball test height of the glass-ceramic product having a spinel crystal phase is greater than 1000 mm, preferably greater than 1200 mm, and more preferably greater than 1500 mm.
[0212] 5) In some embodiments, the drop resistance of the glass-ceramic product having the spinel crystal phase is greater than 1200 mm, preferably greater than 1300 mm, and more preferably greater than 1400 mm.
[0213] 6) In some embodiments, the fracture toughness of the glass-ceramic article having the spinel crystal phase is 1.0 MPa·m 1 / 2 Above, preferably 1.2 MPa·m 1 / 2 More preferably, 1.2 to 1.6 MPa·m 1 / 2 .
[0214] 7) In some embodiments, the four-point bending strength of the glass-ceramic product having the spinel crystal phase is 500 MPa or more, preferably 600 MPa or more, and more preferably 700-1000 MPa.
[0215] 8) In some embodiments, the compressive strength of the glass-ceramic product having the spinel crystal phase is greater than 400N, preferably 400-550N, and more preferably 450-550N.
[0216] 9) In some embodiments, the Vickers hardness (H v ) is 650kgf / mm 2 Above, preferably 660kgf / mm 2 More preferably, 680 to 750 kgf / mm 2 .
[0217] 10) In some embodiments, the haze of a glass-ceramic article having a spinel crystal phase with a thickness of 1 mm or less is 0.3% or less, preferably 0.25% or less, and more preferably 0.05-0.2%. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, further preferably 0.5-0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0218] 11) In some embodiments, a glass-ceramic article having a spinel crystal phase and having a thickness of 1 mm or less has an average light transmittance of 87.0% or greater, preferably 88.5% or greater, and more preferably 89.5% or greater, at a wavelength of 400 to 800 nm. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0219] 12) In some embodiments, a glass-ceramic article having a spinel crystal phase and having a thickness of 1 mm or less has a light transmittance at a wavelength of 550 nm of 87.0% or greater, preferably 88.0% or greater, and more preferably 89.0% or greater. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0220] 13) In some embodiments, a glass-ceramic article having a spinel crystal phase and having a thickness of 1 mm or less has an average optical |B| value of 1.0 or less, preferably 0.8 or less, and more preferably 0.3 to 0.6, at 400 to 800 nm. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, even more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0221] The glass-ceramics having a spinel crystal phase of the present invention has the following properties:
[0222] 1) In some embodiments, the crystal size of the glass-ceramics having the spinel crystal phase is 60 nm or less, preferably 45 nm or less, and more preferably 10 to 30 nm.
[0223] 2) In some embodiments, the haze of the spinel crystal glass-ceramics with a thickness of 1 mm or less is 0.3% or less, preferably 0.25% or less, and more preferably 0.05-0.2%. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, further preferably 0.5-0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0224] 3) In some embodiments, the average light transmittance of a spinel crystal glass-ceramic having a thickness of 1 mm or less at a wavelength of 400 to 800 nm is 87.0% or greater, preferably 88.5% or greater, and more preferably 89.5% or greater. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0225] 4) In some embodiments, a glass-ceramic having a spinel crystal phase and having a thickness of 1 mm or less has a light transmittance of 87.0% or greater, preferably 88.0% or greater, and more preferably 89.0% or greater, at a wavelength of 550 nm. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0226] 5) In some embodiments, for glass-ceramics having a spinel crystal phase and a thickness of 1 mm or less, the average optical |B| value at 400-800 nm is 1.0 or less, preferably 0.8 or less, and more preferably 0.3-0.6. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, even more preferably 0.5-0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0227] 6) In some embodiments, the Young's modulus (E) of the glass-ceramics having a spinel crystal phase is 80 to 110 GPa, preferably 85 to 105 GPa, and more preferably 90 to 105 GPa.
[0228] 7) In some embodiments, the Vickers hardness (H v ) is 550kgf / mm 2 Above, preferably 580kgf / mm 2 More preferably, 600 to 650 kgf / mm 2 .
[0229] The microcrystalline glass, microcrystalline glass products, matrix glass, glass forming bodies, and microcrystalline glass forming bodies of the present invention can be widely made into glass cover plates or glass components due to their above-mentioned excellent properties; at the same time, the microcrystalline glass, microcrystalline glass products, matrix glass, glass forming bodies, and microcrystalline glass forming bodies of the present invention can be applied to electronic devices or display devices, such as mobile phones, watches, computers, touch screen displays, etc., for manufacturing protective glass for mobile phones, smart phones, tablet computers, laptop computers, PDAs, televisions, personal computers, MTA machines or industrial displays, or for manufacturing touch screens, protective windows, car windows, train windows, aircraft machinery windows, touch screen protective glass, or for manufacturing hard disk substrates or solar cell substrates, or for manufacturing white household appliances, such as for manufacturing refrigerator parts or kitchen utensils.
[0230] Example
[0231] To further illustrate and describe the technical solutions of the present invention, the following non-limiting examples are provided. While every effort has been made to ensure the accuracy of the numerical values (e.g., amounts, temperatures, etc.) in the present examples, some errors and deviations must be taken into account. The compositions themselves are given in wt % based on the oxides and are normalized to 100%.
[0232] <Glass-ceramics Example with Spinel Crystal Phase>
[0233] This embodiment uses the above-mentioned method for manufacturing glass-ceramics having a spinel crystal phase to obtain glass-ceramics having a spinel crystal phase and having the compositions shown in Tables 1 to 4. Furthermore, the properties of each glass-ceramic were measured using the testing method described in the present invention, and the measurement results are shown in Tables 1 to 4. In the following embodiments, the test sample thickness for haze, average light transmittance at wavelengths of 400 to 800 nm, light transmittance at a wavelength of 550 nm, and average light |B| value at wavelengths of 400 to 800 nm was 0.7 mm.
[0234] Table 1.
[0235] Table 2.
[0236] Table 3.
[0237] Table 4.
[0238] <Example of glass-ceramic product having spinel crystal phase>
[0239] This example employs the above-described method for manufacturing a glass-ceramic product having a spinel crystal phase to produce glass-ceramic products having a spinel crystal phase and having the compositions shown in Tables 5 to 8. Furthermore, the properties of each glass-ceramic product having a spinel crystal phase were measured using the testing methods described herein, and the results are presented in Tables 5 to 8. In the following examples, the test samples for haze, average light transmittance at wavelengths of 400 to 800 nm, light transmittance at a wavelength of 550 nm, and average light |B| values at wavelengths of 400 to 800 nm were 0.7 mm thick.
[0240] Table 5.
[0241] Table 6.
[0242] Table 7.
[0243] Table 8.
Claims
1. A glass-ceramic product having a spinel crystal phase, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 40-55%; Al2O3+ZnO: 26-45%; Li2O: 0.1-6%; MgO: 0.1~6%; TiO2: 0.5-7%, of which Li2O / TiO2 is 0.2-4.
5.
2. The glass-ceramic product having a spinel crystal phase according to claim 1, characterized in that: Its components, expressed in weight percentage, also contain: P2O5+ZrO2: 0-8%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or clarifier: 0-2%.
3. A glass-ceramic product having a spinel crystal phase, characterized in that: Its components include SiO2, Al2O3, Li2O, ZnO and TiO2. The light transmittance of the microcrystalline glass product with a thickness of less than 1 mm at a wavelength of 550 nm is more than 87.0%.
4. The glass-ceramic product having a spinel crystal phase according to claim 3, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 40-55%; and / or Al2O3+ZnO: 26-45%; and / or Li2O: 0.1-6%; and / or MgO: 0.1-6%; and / or TiO2: 0.5-7%; and / or P2O5+ZrO2: 0-8%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or clarifier: 0-2%.
5. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: Its components, expressed in weight percentage, meet one or more of the following 10 conditions: 1) Li2O / TiO2 is 0.5 to 3.5, preferably Li2O / TiO2 is 0.7 to 2.5, and more preferably Li2O / TiO2 is 0.75 to 1.5; 2) Al2O3 / ZnO is 1.0 to 3.0, preferably Al2O3 / ZnO is 1.25 to 2.5, and more preferably Al2O3 / ZnO is 1.5 to 2.3; 3) SiO2 / Al2O3 is 1.5 to 3.2, preferably SiO2 / Al2O3 is 1.8 to 2.8, and more preferably SiO2 / Al2O3 is 2.0 to 2.5; 4) (TiO2+ZnO) / Al2O3 is 0.4-1.5, preferably (TiO2+ZnO) / Al2O3 is 0.6-1.0, and more preferably (TiO2+ZnO) / Al2O3 is 0.6-0.9; 5) (Li2O+MgO) / TiO2 is 0.3 to 8.0, preferably (Li2O+MgO) / TiO2 is 1.0 to 3.0, and more preferably (Li2O+MgO) / TiO2 is 1.2 to 2.5; 6) Al2O3 / (MgO+TiO2) is 1.3 to 10.0, preferably Al2O3 / (MgO+TiO2) is 2.5 to 6.5, and more preferably Al2O3 / (MgO+TiO2) is 3.0 to 5.5; 7) (Al2O3+Li2O) / P2O5 is 5.0 to 45.0, preferably (Al2O3+Li2O) / P2O5 is 8.0 to 30.0, and more preferably (Al2O3+Li2O) / P2O5 is 10.0 to 25.0; 8) P2O5 / ZrO2 is 0.1 to 5.0, preferably P2O5 / ZrO2 is 0.5 to 2.0, and more preferably P2O5 / ZrO2 is 0.6 to 1.5; 9) (SiO2+Na2O) / ZnO is 2.2 to 6.2, preferably (SiO2+Na2O) / ZnO is 2.8 to 5.5, and more preferably (SiO2+Na2O) / ZnO is 3.0 to 5.0; 10) (Na2O+K2O) / ZnO is less than 0.8, preferably (Na2O+K2O) / ZnO is less than 0.4, and more preferably (Na2O+K2O) / ZnO is less than 0.
2.
6. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: The components thereof are expressed by weight percentage, and contain: SiO2: 45-53%, preferably SiO2: 48-52%; and / or Al2O3+ZnO: 30-42%, preferably Al2O3+ZnO: 35-40%; and / or Li2O: 1-5%, preferably Li2O: 2-4%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO2: 1-6%, preferably TiO2: 2-5%; and / or P2O5+ZrO2: 0.1-7%, preferably P2 O5+ZrO2: 0.5~5%; and / or Na2O: 0~4%, preferably Na2O: 0~2%; and / or B2O3: 0~2%, preferably B2O3: 0~1%; and / or K2O: 0~2%, preferably K2O: 0~1%; and / or CaO+BaO+SrO: 0~4%, preferably CaO+BaO+SrO: 0~2%; and / or Y2O3: 0~4%, preferably Y2O3: 0~2%; and / or clarifier: 0~1%, preferably clarifier: 0~0.5%.
7. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: Its components, expressed in weight percentage, contain: Al2O3: 15-30%, preferably Al2O3: 18-25%; and / or ZnO: 9-20%, preferably ZnO: 12-16%; and / or P2O5: 0.5-4%, preferably P2O5: 1-3%; and / or ZrO2: 0.5-4%, preferably ZrO2: 1-3%.
8. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: The weight percentage of the spinel crystal phase in the glass-ceramic product is 20-60%, preferably 25-45%, and more preferably 30-45%.
9. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: The microcrystalline glass product having a spinel crystal phase contains a quartz crystal phase, wherein the weight percentage of the quartz crystal phase in the microcrystalline glass product is less than 20%, preferably the weight percentage of the quartz crystal phase in the microcrystalline glass product is less than 10%, and more preferably the weight percentage of the quartz crystal phase in the microcrystalline glass product is less than 5%.
10. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: Its components, expressed in weight percentage, contain: La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0~5%, preferably does not contain La2O3, and / or does not contain Gd2O3, and / or does not contain Yb2O3, and / or does not contain Nb2O5, and / or does not contain WO3, and / or does not contain Bi2O3, and / or does not contain Ta2O5, and / or does not contain TeO2.
11. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: The microcrystalline glass product has a grain size of 60 nm or less, preferably 10 to 30 nm; and / or an ion exchange layer depth of 75 μm or more, preferably 100 to 125 μm; and / or a surface stress of 200 MPa or more, preferably 300 to 400 MPa; and / or a drop ball test height of 1000 mm or more, preferably 1500 mm or more; and / or a drop resistance of 1200 mm or more, preferably 1400 mm or more; and / or a fracture toughness of 1.0 MPa·m 1 / 2 Above, preferably 1.2 to 1.6 MPa·m 1 / 2 ; and / or a four-point bending strength of 500 MPa or more, preferably 700 to 1000 MPa; and / or an extrusion strength of 400 N or more, preferably 450 to 550 N; and / or a Vickers hardness of 650 kgf / mm 2 Above, preferably 680 to 750 kgf / mm 2 .
12. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: The haze of microcrystalline glass products with a thickness of less than 1 mm is less than 0.3%, preferably 0.05-0.2%; and / or the average light transmittance at a wavelength of 400-800 nm is greater than 87.0%, preferably greater than 89.5%; and / or the light transmittance at a wavelength of 550 nm is greater than 87.0%, preferably greater than 89.0%; and / or the average light |B| value at 400-800 nm is less than 1.0, preferably 0.3-0.
6.
13. The glass-ceramic product having a spinel crystal phase according to claim 12, characterized in that: The thickness of the microcrystalline glass product is 0.2-1 mm, preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm or 0.75 mm.
14. The glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 4, characterized in that: Its components, expressed in weight percentage, include: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.
15. Glass-ceramics having a spinel crystal phase, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 40-55%; Al2O3+ZnO: 26-45%; Li2O: 0.1-6%; MgO: 0.1~6%; TiO2: 0.5~7%, of which Li2O / TiO2 is 0.2~4.
5.
16. The glass-ceramic having a spinel crystal phase according to claim 15, characterized in that: Its components, expressed in weight percentage, also contain: P2O5+ZrO2: 0-8%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or clarifier: 0-2%.
17. Glass-ceramics having a spinel crystal phase, characterized in that: Its components include SiO2, Al2O3, Li2O, ZnO and TiO2. The light transmittance of the microcrystalline glass with a thickness of less than 1 mm at a wavelength of 550 nm is more than 87.0%.
18. The glass-ceramic having a spinel crystal phase according to claim 17, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 40-55%; and / or Al2O3+ZnO: 26-45%; and / or Li2O: 0.1-6%; and / or MgO: 0.1-6%; and / or TiO2: 0.5-7%; and / or P2O5+ZrO2: 0-8%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or clarifier: 0-2%.
19. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: Its components, expressed in weight percentage, meet one or more of the following 10 conditions: 1) Li2O / TiO2 is 0.5 to 3.5, preferably Li2O / TiO2 is 0.7 to 2.5, and more preferably Li2O / TiO2 is 0.75 to 1.5; 2) Al2O3 / ZnO is 1.0 to 3.0, preferably Al2O3 / ZnO is 1.25 to 2.5, and more preferably Al2O3 / ZnO is 1.5 to 2.3; 3) SiO2 / Al2O3 is 1.5 to 3.2, preferably SiO2 / Al2O3 is 1.8 to 2.8, and more preferably SiO2 / Al2O3 is 2.0 to 2.5; 4) (TiO2+ZnO) / Al2O3 is 0.4-1.5, preferably (TiO2+ZnO) / Al2O3 is 0.6-1.0, and more preferably (TiO2+ZnO) / Al2O3 is 0.6-0.9; 5) (Li2O+MgO) / TiO2 is 0.3 to 8.0, preferably (Li2O+MgO) / TiO2 is 1.0 to 3.0, and more preferably (Li2O+MgO) / TiO2 is 1.2 to 2.5; 6) Al2O3 / (MgO+TiO2) is 1.3 to 10.0, preferably Al2O3 / (MgO+TiO2) is 2.5 to 6.5, and more preferably Al2O3 / (MgO+TiO2) is 3.0 to 5.5; 7) (Al2O3+Li2O) / P2O5 is 5.0 to 45.0, preferably (Al2O3+Li2O) / P2O5 is 8.0 to 30.0, and more preferably (Al2O3+Li2O) / P2O5 is 10.0 to 25.0; 8) P2O5 / ZrO2 is 0.1 to 5.0, preferably P2O5 / ZrO2 is 0.5 to 2.0, more preferably P2O5 / ZrO2 0.6~1.5; 9) (SiO2+Na2O) / ZnO is 2.2 to 6.2, preferably (SiO2+Na2O) / ZnO is 2.8 to 5.5, and more preferably (SiO2+Na2O) / ZnO is 3.0 to 5.0; 10) (Na2O+K2O) / ZnO is less than 0.8, preferably (Na2O+K2O) / ZnO is less than 0.4, and more preferably (Na2O+K2O) / ZnO is less than 0.
2.
20. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: The components thereof are expressed by weight percentage, and contain: SiO2: 45-53%, preferably SiO2: 48-52%; and / or Al2O3+ZnO: 30-42%, preferably Al2O3+ZnO: 35-40%; and / or Li2O: 1-5%, preferably Li2O: 2-4%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO2: 1-6%, preferably TiO2: 2-5%; and / or P2O5+ZrO2: 0.1-7%, preferably P2 O5+ZrO2: 0.5~5%; and / or Na2O: 0~4%, preferably Na2O: 0~2%; and / or B2O3: 0~2%, preferably B2O3: 0~1%; and / or K2O: 0~2%, preferably K2O: 0~1%; and / or CaO+BaO+SrO: 0~4%, preferably CaO+BaO+SrO: 0~2%; and / or Y2O3: 0~4%, preferably Y2O3: 0~2%; and / or clarifier: 0~1%, preferably clarifier: 0~0.5%.
21. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: Its components, expressed in weight percentage, contain: Al2O3: 15-30%, preferably Al2O3: 18-25%; and / or ZnO: 9-20%, preferably ZnO: 12-16%; and / or P2O5: 0.5-4%, preferably P2O5: 1-3%; and / or ZrO2: 0.5-4%, preferably ZrO2: 1-3%.
22. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: The weight percentage of the spinel crystal phase in the glass-ceramics is 20-60%, preferably the weight percentage of the spinel crystal phase in the glass-ceramics is 25-45%, and more preferably the weight percentage of the spinel crystal phase in the glass-ceramics is 30-45%.
23. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: The microcrystalline glass having a spinel crystal phase contains a quartz crystal phase, wherein the weight percentage of the quartz crystal phase in the microcrystalline glass is less than 20%, preferably the weight percentage of the quartz crystal phase in the microcrystalline glass is less than 10%, and more preferably the weight percentage of the quartz crystal phase in the microcrystalline glass is less than 5%.
24. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: Its components, expressed in weight percentage, contain: La2O3+Gd2O3+Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2: 0~5%, preferably does not contain La2O3, and / or does not contain Gd2O3, and / or does not contain Yb2O3, and / or does not contain Nb2O5, and / or does not contain WO3, and / or does not contain Bi2O3, and / or does not contain Ta2O5, and / or does not contain TeO2.
25. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: The crystal size of the microcrystalline glass is less than 60 nm, preferably 10 to 30 nm; and / or the Young's modulus is 80 to 110 GPa, preferably 90 to 105 GPa; and / or the Vickers hardness is 550 kgf / mm 2 Above, preferably 600 to 650 kgf / mm 2 .
26. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: The haze of microcrystalline glass with a thickness of less than 1 mm is less than 0.3%, preferably 0.05-0.2%; and / or the average light transmittance at a wavelength of 400-800 nm is greater than 87.0%, preferably greater than 89.5%; and / or the light transmittance at a wavelength of 550 nm is greater than 87.0%, preferably greater than 89.0%; and / or the average light |B| value at 400-800 nm is less than 1.0, preferably 0.3-0.
6.
27. The glass-ceramic having a spinel crystal phase according to claim 26, characterized in that: The thickness of the microcrystalline glass is 0.2-1 mm, preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm or 0.75 mm.
28. The glass-ceramics having a spinel crystal phase according to any one of claims 15 to 18, characterized in that: Its components, expressed in weight percentage, include: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.
29. A glass cover plate, characterized in that: A glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 14, and / or a glass-ceramic product having a spinel crystal phase according to any one of claims 15 to 28.
30. A glass component, characterized in that: A glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 14, and / or a glass-ceramic product having a spinel crystal phase according to any one of claims 15 to 28.
31. An electronic device, characterized in that A glass-ceramic product having a spinel crystal phase as claimed in any one of claims 1 to 14, and / or a glass-ceramic product having a spinel crystal phase as claimed in any one of claims 15 to 28, and / or a glass cover plate as claimed in claim 29, and / or a glass component as claimed in claim 30.
32. A display device, characterized in that A glass-ceramic product having a spinel crystal phase as claimed in any one of claims 1 to 14, and / or a glass-ceramic product having a spinel crystal phase as claimed in any one of claims 15 to 28, and / or a glass cover plate as claimed in claim 29, and / or a glass component as claimed in claim 30.
33. The method for manufacturing a glass-ceramic product having a spinel crystal phase according to any one of claims 1 to 14, characterized in that: The method comprises the following steps: forming a matrix glass, subjecting the matrix glass to a crystallization process to form a microcrystalline glass having a spinel crystal phase, and then subjecting the microcrystalline glass having a spinel crystal phase to a chemical strengthening process to form a microcrystalline glass product having a spinel crystal phase.
34. The method for manufacturing a glass-ceramic product having a spinel crystal phase according to claim 33, characterized in that: The forming of the matrix glass comprises the following steps: The raw materials are mixed uniformly according to the component ratio, then put into a crucible, and melted in an electric furnace or a gas furnace at a temperature range of 1350 to 1550° C. for 5 to 24 hours, preferably at a melting temperature of 1450 to 1550° C., and then clarified, homogenized, formed, and annealed to obtain a matrix glass, wherein the clarification temperature is greater than 1550° C. but less than or equal to 1650° C., and the annealing temperature is 450 to 600° C.
35. The method for manufacturing a glass-ceramic product having a spinel crystal phase according to claim 33, characterized in that: The crystallization process includes the following steps: heating to a prescribed crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.
36. The method for manufacturing a glass-ceramic product having a spinel crystal phase according to claim 33, characterized in that: The crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature, wherein the first temperature is 600-700°C, the second temperature is greater than 700°C but less than or equal to 800°C, the holding time at the first temperature is 1-6 hours, and the holding time at the second temperature is 2-5 hours.
37. The method for manufacturing a glass-ceramic product having a spinel crystal phase according to claim 33, characterized in that: The chemical strengthening process includes: immersing the microcrystalline glass having a spinel crystal phase in a salt bath of molten Na salt at 350-470°C for 1-36 hours, preferably in the temperature range of 400-460°C, and preferably in the time range of 2-15 hours; and / or immersing the microcrystalline glass having a spinel crystal phase in a mixed salt bath of molten K salt and Na salt at 360-450°C for 1-36 hours, preferably in the time range of 2-24 hours.
38. The method for producing glass-ceramics having a spinel crystal phase according to any one of claims 15 to 28, characterized in that: The method comprises the following steps: forming a matrix glass, and then forming a microcrystalline glass having a spinel crystal phase through a crystallization process.
39. The method for manufacturing glass-ceramics having a spinel crystal phase according to claim 38, characterized in that: The forming of the matrix glass comprises the following steps: The raw materials are mixed uniformly according to the component ratio, then put into a crucible, and melted in an electric furnace or a gas furnace at a temperature range of 1350 to 1550° C. for 5 to 24 hours, preferably at a melting temperature of 1450 to 1550° C., and then clarified, homogenized, formed, and annealed to obtain a matrix glass, wherein the clarification temperature is greater than 1550° C. but less than or equal to 1650° C., and the annealing temperature is 450 to 600° C.
40. The method for manufacturing glass-ceramics having a spinel crystal phase according to claim 38, characterized in that: The crystallization process includes the following steps: heating to a prescribed crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.
41. The method for manufacturing a glass-ceramic product having a spinel crystal phase according to claim 38, characterized in that: The crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature, wherein the first temperature is 600-700°C, the second temperature is greater than 700°C but less than or equal to 800°C, the holding time at the first temperature is 1-6 hours, and the holding time at the second temperature is 2-5 hours.
Citation Information
Patent Citations
Crystallized glass substrate for information recording medium and method of producing the same
CN101905952A
Microcrystalline glass, microcrystalline glass product and manufacturing method thereof
CN111807705A
Preparation method of chemically strengthened glass, chemically strengthened glass and raw material glass
CN112645609A
Glass ceramic, glass ceramic product and manufacturing method thereof
CN114907014A
Tempered glass, microcrystalline glass and preparation method and application thereof
CN115286251A
Cited By
High-hardness microcrystalline glass and preparation method thereof
CN120622811A