Polyamide resin, polymerization method therefor, and use thereof
By adjusting the composition and polymerization method of polyamide resin, the binding force between 1,4-cyclohexanedicarboxylic acid polyamide and silica gel is improved and the water absorption rate is reduced, which solves the application problems in the field of outdoor LED displays and realizes the improvement of polyamide resin Stability and waterproof performance in high temperature and high humidity environments.
Patent Information
- Application Number
- PCT/CN2024/082668
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-20
- Publication Date
- 2024-10-31
AI Technical Summary
The high-temperature-resistant polyamide based on 1,4-cyclohexanedicarboxylic acid has a low binding force with silicone, making it unsuitable for outdoor LED displays. Especially in high-temperature and high-humidity environments, there is a problem of separation of plastic and silicone.
By adjusting the composition of the polyamide resin, including the molar percentages of 2,4-cyclohexanedicarboxylic acid, 1,10-decanediamine, and 1,12-dodecanediamine, the proportion of trans structure is controlled at 77-81% , and uses a specific polymerization method to react in a pressure kettle to form a polyamide resin with high binding force and low water absorption.
It achieves high bonding force and low water absorption between polyamide resin and silicone, which is suitable for outdoor LED display fields and ensures the stability and waterproof performance of lamp beads.
Smart Images

Figure PCTCN2024082668-FTAPPB-I100001 
Figure PCTCN2024082668-FTAPPB-I100002 
Figure PCTCN2024082668-FTAPPB-I100003
Abstract
Description
Polyamide resin, polymerization method and application thereof Technical Field
[0001] The present invention relates to the technical field of polymer materials, in particular to a polyamide resin and a polymerization method and application thereof. Background Art
[0002] Compared to semi-aromatic heat-resistant polyamides derived from terephthalic acid or isophthalic acid, heat-resistant polyamides derived from 1,4-cyclohexanedicarboxylic acid monomers lack benzene rings in their molecular structure and exhibit a weaker electron-withdrawing effect. Therefore, heat-resistant polyamides derived from 1,4-cyclohexanedicarboxylic acid monomers are less likely to acquire electrons during long-term UV aging, resulting in a more stable molecular structure and improved UV aging resistance.
[0003] LED encapsulants primarily include epoxy resin and silicone. Silicone resin boasts excellent mechanical properties, aging resistance, good thermal stability, weather resistance, flexibility, high light transmittance, low internal stress, and low moisture absorption. Compared to epoxy resin, its performance is more suited to the encapsulation requirements of high-power, high-brightness LED products. Consequently, silicone is rapidly replacing epoxy resin as the ideal next-generation LED encapsulation material. With the rapid development of LEDs, LED lamps have begun to be used in outdoor displays. These applications require long periods of exposure to high temperatures and humidity, such as exposure to sunlight or rain. In such environments, polyamides with low water absorption and strong bonding between the polyamide reflector and silicone are essential to prevent moisture from penetrating the lamp and causing failure. However, high-temperature-resistant polyamides based on 1,4-cyclohexanedicarboxylic acid exhibit weak bonding with silicone, resulting in separation between the plastic and silicone, making them unsuitable for outdoor LED displays.
[0004] Therefore, how to improve the bonding strength between high-temperature resistant polyamide based on 1,4-cyclohexanedicarboxylic acid and silicone while ensuring low water absorption to meet the needs of the outdoor LED display field is an urgent problem to be solved in this field.
[0005] Summary of the Invention
[0006] The purpose of the present invention is to provide a polymer having the advantages of high temperature resistance, low water absorption and high bonding strength with silica gel, as well as a polymerization method and application thereof.
[0007] The present invention is achieved through the following technical solutions:
[0008] A polyamide resin comprising the following repeating units, measured by mole percentage:
[0009] Diacid unit: 1,4-cyclohexanedicarboxylic acid;
[0010] The diamine units include 1,10-decanediamine and 1,12-dodecanediamine, wherein the amount of 1,10-decanediamine in the diamines is 66-75%.
[0011] Preferably, the amount of 1,10-decanediamine in the diamine is 69-72%.
[0012] In the high-temperature resistant polyamide resin, the trans structure accounts for 77-81% of the total mass fraction. The testing method involves dissolving 5 mg of the polyamide resin in 10 mg of deuterated trifluoroacetic acid and performing a proton nuclear magnetic resonance (NMR) spectrum on a Bruker DPX400 NMR instrument. In the proton nuclear magnetic resonance (NMR) spectrum, the cis structure peaks at 1.96 ppm, and the trans structure peaks at 1.83 ppm. The trans structure ratio of the resin is determined by NMR integration of these two peaks.
[0013] The melting point of the high-temperature resistant polyamide resin is 305-318°C. The specific testing method is as follows: the melting point of the sample is tested using a Perkin Elmer Dimond DSC analyzer in a nitrogen atmosphere at a flow rate of 50 mL / min. During the test, the temperature is first raised to 350°C at a rate of 20°C / min, held at 350°C for 2 minutes to remove the thermal history of the resin, then cooled to 50°C at a rate of 20°C / min, held at 50°C for 2 minutes, and then raised to 350°C at a rate of 20°C / min. The endothermic peak temperature at this point is defined as the melting point (T).
[0014] The relative viscosity of the high-temperature resistant polyamide resin ranges from 1.8 to 2.8. The test method is to refer to GB12006.1-89 and measure the relative viscosity of the polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
[0015] The polymerization method of the high-temperature resistant polyamide resin of the present invention comprises the following steps: adding reaction monomers, benzoic acid, sodium hypophosphite and deionized water into a pressure autoclave, wherein the amount of benzoic acid is 1.5-3.0% of the amount of the reaction monomers, the weight of sodium hypophosphite is 0.05-0.15% of the weight of other materials except deionized water, and the weight of deionized water is 25-35% of the total weight of the materials; vacuuming and filling with inert gas (which may be high-purity nitrogen) as a protective gas, heating to 215-225° C. within 1.5-2.5 hours, and then reacting within the temperature range for 0.5-1.5 hours; then continuing the reaction at 225-235° C. and a pressure of 2.0-2.4 MPa for 1-3 hours, removing water formed during the reaction, discharging the materials after the reaction is completed, and vacuum drying the prepolymer to obtain a prepolymer product, and solid-phase thickening the prepolymer product for 8-12 hours under the conditions of 240-260° C. and a pressure of 45-55 Pa to obtain a polyamide resin.
[0016] The high-temperature resistant polyamide resin of the present invention is used to prepare translucent LED-related components, such as LED lamp brackets or LED display screens.
[0017] The present invention has the following beneficial effects
[0018] Through experiments, it was found that the cis / trans structure of the polyamide resin comes from 1,4-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid constitutes the diacid unit of the polyamide resin of the present invention. By controlling the composition of the diamine unit in the polyamide, it was unexpectedly found that a polyamide resin with a specific trans structure ratio can be obtained (research has found that the trans structure ratio of the polyamide resin in which 1,4-cyclohexanedicarboxylic acid constitutes the diacid unit is related to the structure and ratio of the diamine monomer. The possible reason is that the longer the diamine monomer molecular chain, the higher the stability of the trans structure, and therefore the higher the ratio of the trans structure). The trans structure of the polyamide resin accounts for 77 to 81% of the amount of the substance of the polyamide resin, so that the polyamide resin of the present invention has strong silicone bonding and maintains low water absorption, and is suitable for the field of outdoor LED display screens. DETAILED DESCRIPTION
[0019] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those skilled in the art, several variations and improvements can be made without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.
[0020] 1,4-Cyclohexanedicarboxylic acid: purity 98%, SKY CHDA, purchased from SK Chemicals;
[0021] 1,10-Decanediamine: purity 97%, D100615, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0022] 1,12-Dodecanediamine: purity 98%, D106441, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0023] 1,6-Hexanediamine: purity 99%, H103910, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0024] 1,14-Tetradecanediamine: purity 95%, SY250668, purchased from Shanghai Shaoyuan Reagent Co., Ltd.;
[0025] Benzoic acid: purity 99.5%, 242381, purchased from Sigma-Aldrich;
[0026] Sodium hypophosphite: purity 98%, S475696, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0027] The preparation method of the high-temperature resistant polyamide resin of the embodiment and the comparative example is as follows: the reaction monomer, benzoic acid, sodium hypophosphite and deionized water are added to the autoclave; the amount of benzoic acid substance is 1.5% of the amount of the reaction monomer substance, the weight of sodium hypophosphite is 0.10% of the weight of other materials except deionized water, and the weight of deionized water is 30% of the total weight of the materials; the autoclave is evacuated and filled with high-purity nitrogen as a protective gas, the temperature is raised to 220°C within about 2 hours, and then the reaction is carried out within this temperature range for 1 hour; the reaction is then continued at 230°C and a pressure of 2.2 MPa for 2 hours, the water formed during the reaction is removed, the material is discharged after the reaction is completed, and the prepolymer is vacuum dried to obtain a prepolymer product, and the prepolymer product is solid-phase thickened for 8-12 hours under the conditions of 250°C and 50 Pa pressure to obtain a polyamide resin.
[0028] Various test methods:
[0029] (1) Polyamide relative viscosity test method: refer to GB12006.1-89, polyamide viscosity number determination method; the specific test method is: measure the relative viscosity of polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
[0030] (2) Polyamide resin melting point test method: refer to ASTM D3418-2003, Standard Test Method for Transition Temperatures of Polymers By Differential Scanning Calorimetry; the specific test method is: use a Perkin Elmer Dimond DSC analyzer to test the melting point of the sample; nitrogen atmosphere, flow rate is 50mL / min; during the test, first increase the temperature to 350℃ at 20℃ / min, maintain at 350℃ for 2min to remove the thermal history of the resin, then cool to 50℃ at 20℃ / min, maintain at 50℃ for 2min, and then increase the temperature to 350℃ at 20℃ / min, and set the endothermic peak temperature at this time as the T melting point.
[0031] (3) Polyamide cis-trans ratio test method: 5 mg of polyamide resin was dissolved in 10 mg of deuterated trifluoroacetic acid and the sample was tested by H NMR spectroscopy using a Bruker DPX400 NMR spectrometer. In the H NMR spectrum, the cis peak is at 1.96 ppm, and the trans peak is at 1.83 ppm. The trans ratio of the resin can be obtained by integrating the two peaks.
[0032] (4) Polyamide water absorption: Injection mold the sample into a 20 mm × 20 mm × 2 mm piece, and record its weight as a0. Then, place the piece in 95°C water for 240 hours, and weigh it as a1. Water absorption = (a1 - a0) / a0 * 100%. A water absorption of no more than 1.5% is considered to meet the requirements.
[0033] (5) Silicone bonding strength: The high-temperature resistant polyamide resin sample was injection molded, and the sample size was 80×20×2.0mm. Test method: After uniformly mixing silicone glue A and silicone glue B in a mass ratio of 1:4, take 0.02g and drop it on one end of the surface of a sample, use one end of another sample to press the silicone, and fix it with a clamp. Then put the sample into an oven, pre-cure it at 80℃ for 1h, then heat it to 150℃ and continue curing for 4h before finishing. The cured sample was subjected to a tensile test with a tensile speed of 10mm / min, and the breaking force was recorded. The present invention characterizes the bonding strength of polyamide and silicone by breaking force. When the breaking force is not less than 500N, it is considered to meet the use requirements.
[0034] Table 1: Molar percentage content of each unit of polyamide resin in the embodiment and test results
[0035] As can be seen from Examples 1-6, when 1,10-decanediamine accounts for 69-72% of the total amount of diamine, the water absorption rate is lower and the bonding strength with silica gel is better.
[0036] Table 2: Molar percentage content of each unit of the comparative polyamide resin and test results
[0037] It can be seen from Comparative Example 1 that the molar content of 1,12-dodecanediamine is too high and the trans structure content is too low. Although the water absorption rate is low, the silica gel bonding strength is poor.
[0038] It can be seen from Comparative Example 2 that the trans structure content is not within the scope of the present invention, the binding force with silica gel is low, and the water absorption rate is high.
[0039] As can be seen from Comparative Examples 3-5, it is difficult for other types of monomers to achieve a trans structure ratio within the scope of the present invention, and it is difficult to simultaneously achieve the characteristics of low water absorption and high bonding strength with silica gel.
[0040] The water absorption rate of the polyamide resin of the present invention is less than or equal to 1.4%, and the breaking force in the test of silica gel bonding strength is greater than 500N.
Claims
1. A polyamide resin, characterized in that: In terms of mole percentage, it comprises the following repeating units: Diacid unit: 1,4-cyclohexanedicarboxylic acid; Diamine units: 1,10-decanediamine and 1,12-dodecanediamine, wherein the amount fraction of 1,10-decanediamine in the diamine substance is 66-75%.
2. The polyamide resin according to claim 1, characterized in that The amount fraction of 1,10-decanediamine in the diamine substance is 69-72%.
3. The polyamide resin according to claim 1, characterized in that In the polyamide resin, the trans structure ratio is 77-81%.
4. The polyamide resin according to claim 1, characterized in that The melting point of the polyamide resin is in the range of 305-318°C.
5. The polyamide resin according to claim 1, characterized in that The relative viscosity of the polyamide resin is in the range of 1.8-2.
8. The test method is to refer to GB12006.1-89 and measure the relative viscosity of the polyamide with a concentration of 0.25 g / dl in 98% concentrated sulfuric acid at 25±0.01°C.
6. The method for polymerizing a polyamide resin according to any one of claims 1 to 5, characterized in that: The following steps are involved: Add reaction monomers, benzoic acid, sodium hypophosphite and deionized water into a pressure autoclave; the amount of benzoic acid is 1.5-3.0% of the total amount of reaction monomers, the weight of sodium hypophosphite is 0.05-0.15% of the weight of other materials except deionized water, and the weight of deionized water is 25-35% of the total weight of materials; evacuate and fill with inert gas as protective gas, heat to 215-225° C. within 1.5-2.5 hours under stirring, then react within the temperature range for 0.5-1.5 hours, then continue to react at 225-235° C. and 2.0-2.4 MPa for 1-3 hours, remove water formed during the reaction, discharge after the reaction is completed, and obtain a prepolymer product after vacuum drying. The prepolymer product is solid-phase thickened for 8-12 hours under the conditions of 240-260° C. and 45-55 Pa pressure to obtain a polyamide resin.
7. Use of the polyamide resin according to any one of claims 1 to 5, characterized in that: Used to prepare translucent LED related components.
8. Application of the polyamide resin obtained by the preparation method of claim 6, characterized in that: Used to prepare translucent LED related components.
Citation Information
Patent Citations
Polyamide resin and polyamide molded body using same
CN105814115A
Polyamide resin, polyamide composition and preparation methods
CN113929901A
Polyamide as well as preparation method and application thereof
CN114507343A
Polyamide molding composition as well as preparation method and application thereof
CN115678268A
Polyamide resin and polymerization method and application thereof
CN116769156A