LCP resin composition, preparation method therefor, and use thereof
By adding trace amounts of fully aromatic multifunctional oligomers and glass fibers to the LCP resin to form a micro-branched or micro-crosslinked structure, the problem of poor warpage performance of the liquid crystal polymer is solved and the flexural modulus of the resin composition is achieved. Significant improvement in regulation and warpage properties, suitable for manufacturing precision electronic components.
Patent Information
- Application Number
- PCT/CN2024/087760
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-31
AI Technical Summary
During the injection molding process, liquid crystal polymer molded products warp due to unequal shrinkage in the longitudinal direction and flow direction, which affects the precision of electronic components. Existing improvement methods mainly rely on adding chopped glass fibers and mineral fillers, without starting from the matrix. The angle of the resin is improved.
LCP resin and trace amounts of fully aromatic multifunctional oligomers are used together with glass fibers and fillers to form a micro-branched or micro-cross-linked structure, which destroys the segment regularity of the resin and adjusts the warpage performance and flexural modulus of the resin composition.
The warpage performance of the LCP resin composition is significantly improved, the grain size is reduced, and the bending modulus is adjusted, making it suitable for the manufacturing of precision electronic components.
Smart Images

Figure PCTCN2024087760-FTAPPB-I100001 
Figure PCTCN2024087760-FTAPPB-I100002 
Figure PCTCN2024087760-FTAPPB-I100003
Abstract
Description
A LCP resin composition and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to an LCP resin composition, a preparation method and an application thereof. Background Art
[0002] With the development of information technology, the integration of electronic components is becoming increasingly higher, which requires the materials of components to be smaller and thinner. Thermoplastic liquid crystal polymers (LCPs) have excellent heat resistance, mechanical properties, solvent resistance, and dimensional stability, and are widely used in the electronic and electrical fields. In addition, the main chain segments of liquid crystal polymer molecules are rigid, easily oriented during melt flow, and have good fluidity. Therefore, liquid crystal polymers are very suitable for injection molding small and thin parts. However, products molded from liquid crystal polymers have a unique skin-core structure of liquid crystal polymers, which can have a fiber-reinforced effect. However, due to its unique skin-core structure, when injection molded into precision electronic components, it undergoes unequal shrinkage in the longitudinal direction and the flow direction. There is a shrinkage difference, and the resulting internal stress can cause the plastic part to warp, seriously affecting the precision of the electronic components. This also poses a higher challenge to the warping performance of liquid crystal polymer materials.
[0003] A common method for improving the warpage performance of liquid crystal polymers is to add a certain amount of chopped glass fiber and mineral fillers. For example, the invention patent with publication number CN 105111772A uses a certain amount of alkali-free glass fiber, mica powder, etc. to improve the warpage performance of liquid crystal polymers.
[0004] However, none of the above methods for improving warpage performance are improved from the perspective of the matrix resin.
[0005] Summary of the Invention
[0006] Based on the defects of the prior art, the purpose of the present invention is to provide an LCP resin composition, a preparation method and application thereof, wherein the LCP resin composition is prepared by combining an LCP resin with a trace amount of a fully aromatic multifunctional oligomer to form a micro-branched or micro-crosslinked structure, thereby improving the skin-core structure of the LCP resin and destroying the segment regularity of the LCP resin, thereby improving the warping performance of the LCP resin composition and adjusting the flexural modulus of the LCP resin composition.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] In a first aspect, the present invention provides an LCP resin composition comprising the following raw materials in parts by weight:
[0009] 100 parts of LCP resin, 0.1-1 parts of fully aromatic multifunctional oligomer, 10-60 parts of glass fiber and 20-70 parts of filler;
[0010] The LCP resin comprises repeating units represented by the following structures: -O-Ar1-O-, -OC-Ar2-CO-, -O-Ar3-CO-, -CO-Ar4-CO-;
[0011] wherein -Ar1-, -Ar2-, -Ar3-, and -Ar4- are each independently Any of the following;
[0012] The fully aromatic multifunctional oligomer has the following structure:
[0013] Wherein, R1, R2, and R3 are the structure represented by formula (I) or the structure represented by formula (II):
[0014] Wherein, n is any number among 1, 2, 3, 4, 5, 6, n in R1, R2, R3 are the same or different positive integers, -Ar5- is R4 and R5 are each independently a carboxyl group or an acetoxy group.
[0015] The LCP resin of the present invention comprises four repeating units: -O-Ar1-O-, -OC-Ar2-CO-, -O-Ar3-CO-, -CO-Ar4-CO-, wherein -Ar1-, -Ar2-, -Ar3-, -Ar4- are each independently Any one of the above has good processing performance, and the LCP resin with the above-mentioned repeating unit structure can fully undergo ester exchange reaction with a trace amount of fully aromatic multifunctional oligomer to form a micro-branched or micro-crosslinked structure, reducing the grain size of the LCP resin composition, thereby improving the warpage performance of the resin composition. The amount of the fully aromatic multifunctional oligomer selected by the present invention needs to be strictly controlled. If the amount of the fully aromatic multifunctional oligomer is too little, the degree of crosslinking between the fully aromatic multifunctional oligomer and the LCP resin is too low, resulting in the grain size of the LCP resin composition being too large, which is obviously not conducive to improving the warpage performance of the LCP resin composition, and is also not conducive to adjusting the flexural modulus of the LCP resin composition to an appropriate range; if the amount of the fully aromatic multifunctional oligomer is too much, the degree of crosslinking between the fully aromatic multifunctional oligomer and the LCP resin is too high, and it is easy to form an infusible material, which affects the application of the LCP resin composition.
[0016] As a preferred embodiment of the present invention, the LCP resin has a melting point of 302 to 372° C. and a shear viscosity of 10 to 30 Pa·s.
[0017] As a preferred embodiment of the present invention, in the repeating units of the LCP resin, the molar content of -O-Ar1-O- is 10 to 30%, the molar content of -OC-Ar2-CO- is 8 to 20%, the molar content of -O-Ar3-CO- is 40 to 80%, and the molar content of -OC-Ar4-CO- is 2 to 10%.
[0018] Furthermore, among the components of the LCP resin, the molar content of -O-Ar1-O- is 20-25%, the molar content of -OC-Ar2-CO- is 17-18%, the molar content of -O-Ar3-CO- is 50-60%, and the molar content of -OC-Ar4-CO- is 3-7%.
[0019] Furthermore, -Ar1- is -Ar2- is -Ar3- is -Ar4- is
[0020] As a preferred embodiment of the present invention, the LCP resin is obtained by reacting HO-Ar1-OH, HOOC-Ar2-COOH, HO-Ar3-COOH, HOOC-Ar4-COOH and an acylating agent, wherein the molar ratio of HO-Ar1-OH, HOOC-Ar2-COOH, HO-Ar3-COOH, and HOOC-Ar4-COOH is: HO-Ar1-OH: HOOC-Ar2-COOH: HO-Ar3-COOH: HOOC-Ar4-COOH = (10-30): (8-20): (40-80): (2-10).
[0021] Furthermore, the molar ratio of HO-Ar1-OH, HOOC-Ar2-COOH, HO-Ar3-COOH, and HOOC-Ar4-COOH is: HO-Ar1-OH: HOOC-Ar2-COOH: HO-Ar3-COOH: HOOC-Ar4-COOH = (20-25): (17-18): (50-60): (3-7).
[0022] As a preferred embodiment of the present invention, R4 is a carboxyl group, and R5 is an acetoxy group.
[0023] As a preferred embodiment of the present invention, the fully aromatic multifunctional oligomer is obtained by reacting the following reactants:
[0024] (1) Trimesic acid or pyrogallol;
[0025] (2) at least one of HO-Ar5-COOH, HOOC-Ar5-COOH, and HO-Ar5-OH, wherein -Ar5- is
[0026] (3) Acylation agent.
[0027] Furthermore, the fully aromatic multifunctional oligomer is obtained by reacting the following reactants:
[0028] (1) Trimesic acid or pyrogallol;
[0029] (2) HO-Ar5-COOH, -Ar5- is
[0030] (3) Acylation agent.
[0031] Furthermore, the molar ratio of reactant (1) to reactant (2) is 1:(3-24).
[0032] If trimesic acid, HO-Ar5-COOH and an acylating agent react, the prepared fully aromatic multifunctional oligomer has a structure shown in formula (I); if pyrogallol, HO-Ar5-COOH and an acylating agent react, the prepared fully aromatic multifunctional oligomer has a structure shown in formula (II).
[0033] The study found that the relative molar proportion of the repeating unit -O-Ar3-CO- in the LCP resin repeating unit is controlled at 50-60%, and -Ar5- is When the resin is added, the processing performance of the resin is good, and the repeating unit is close to the side chain monomer structure in the wholly aromatic multifunctional oligomer. The addition of a small amount of oligomer has little effect on other physical properties of the LCP resin composition.
[0034] As a preferred embodiment of the present invention, the molecular weight of the wholly aromatic multifunctional oligomer is 570 to 2370 g / mol.
[0035] As a preferred embodiment of the present invention, the mass ratio of the wholly aromatic multifunctional oligomer to the LCP resin is (0.2-0.8):100.
[0036] As a preferred embodiment of the present invention, the filler is an inorganic flake filler, and the inorganic flake filler is selected from at least one of talc powder and mica powder.
[0037] The mass ratio of the glass fiber, filler and LCP resin is (3-6): (3-5): 10. The present invention selects filler and glass fiber to synergistically improve the warping performance of the LCP resin composition. When the amount of glass fiber and filler meets the above conditions, the warping performance of the LCP resin composition is greatly improved, making the LCP resin composition suitable for electronic components.
[0038] In a second aspect, the present invention provides a method for preparing a low-warpage LCP resin composition as described in the first aspect, comprising the following steps:
[0039] The LCP resin, the wholly aromatic multifunctional oligomer, the glass fiber and the filler are mixed and then blended and extruded through a twin-screw extruder to obtain an LCP resin composition.
[0040] As a preferred embodiment of the present invention, during the blending and extrusion by the twin-screw extruder, the extrusion temperature is Tm-30°C to Tm+30°C, and the screw speed is 200 to 600 rpm, wherein Tm is the melting point of the LCP resin.
[0041] In a third aspect, the present invention provides a use of the low-warpage LCP resin composition as described in the first aspect in the preparation of electronic components.
[0042] Furthermore, the electronic components include thin-walled parts such as memory card slots and computer fans.
[0043] The beneficial effects of the present invention are that the present invention provides a low-warpage LCP resin composition, a preparation method thereof, and an application thereof. The LCP resin composition is prepared by combining a specific LCP resin with a trace amount of a fully aromatic multifunctional oligomer to form micro-branching or micro-crosslinking, thereby improving the skin-core structure of the LCP resin and destroying the segment regularity of the LCP resin, thereby improving the warpage performance and flexural modulus of the LCP resin composition. DETAILED DESCRIPTION
[0044] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples. Its purpose is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise all fall within the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention are all conventional common reagents and instruments unless otherwise specified.
[0045] The materials used in the examples and comparative examples are as follows:
[0046] LCP resin was prepared by the following method:
[0047] (1) Under nitrogen conditions, parahydroxybenzoic acid (HBA), biphenol (BP), terephthalic acid (TA), isophthalic acid (IA) and acetic anhydride are added to a reactor in a certain molar ratio, and an acylation reaction is carried out under the action of acetic anhydride. The reaction temperature is 100°C to 180°C, and the reaction time is 0.5 to 4 hours;
[0048] (2) After the acylation reaction is completed, the pressure in the reactor is maintained at atmospheric pressure, and the temperature is raised to 200°C to 310°C at a rate of 0.1 to 5°C / min, and acetic acid and unreacted acetic anhydride molecules are discharged from the distillation column. When the amount of acetic acid received reaches more than 90 wt% of the theoretical value, the pressure in the reactor is reduced to 5 to 40 kPa. This reduced pressure condition is maintained and the reaction system is heated to 330 to 400°C. When the stirring power reaches the set value, the material is discharged, cooled, and granulated to obtain a prepolymer;
[0049] (3) The prepolymer is subjected to solid-phase polymerization in a solid-phase polymerization container to obtain an LCP resin.
[0050] The melting point, crystallization temperature and shear viscosity of LCP resin were tested. The test steps are as follows:
[0051] (1) Melting point and crystallization temperature: measured using a DSC 200F3 manufactured by NETZSCH. The temperature was raised from room temperature to 390°C at a heating rate of 20°C / min, then cooled to room temperature at 20°C / min, and finally heated to 390°C at 20°C / min. The melting point was determined by taking the highest point of the melting peak of the second heating curve, and the crystallization temperature was determined by taking the lowest point of the crystallization peak of the first cooling curve.
[0052] (2) Shear viscosity: tested using a Malvern capillary rheometer at a temperature of 20°C above the melting point and a shear rate of 1000s -1 , measured using a die with an inner diameter of 1 mm and a length of 20 mm.
[0053] The molar ratio of LCP resin 1: HBA, BP, TA, IA and acetic anhydride is HBA: BP: TA: IA: acetic anhydride = 60: 20: 17: 3: 105; the melting point of LCP resin 1 is 362 ° C, the shear viscosity is 15 Pa s, and the repeating unit of LCP resin 1 is: The molar content is 60%, The molar content is 20%, The molar content is 17%, The molar content is 3%.
[0054] The molar ratio of LCP resin 2: HBA, BP, TA, IA and acetic anhydride is HBA:BP:TA:IA:acetic anhydride=50:25:18:7:105; the melting point of LCP resin 2 is 335°C, the shear viscosity is 21 Pa·s, and in the repeating unit of LCP resin 2, The molar content is 50%, The molar content is 25%, The molar content is 18%, The molar content is 7%.
[0055] The molar ratio of LCP resin 3: HBA, BP, TA, IA and acetic anhydride is HBA: BP: TA: IA: acetic anhydride = 40: 30: 20: 10: 105; the melting point of LCP resin 3 is 302 ° C, the shear viscosity is 30 Pa s, and the repeating unit of LCP resin 3 is: The molar content is 40%, The molar content is 30%, The molar content is 20%, The molar content is 10%.
[0056] The molar ratio of LCP resin 4: HBA, BP, TA, IA and acetic anhydride is HBA: BP: TA: IA: acetic anhydride = 80: 10: 8: 2: 105; the melting point of LCP resin 4 is 372 ° C, the shear viscosity is 30 Pa · s, and the repeating unit of LCP resin 4 is: The molar content is 80%, The molar content is 10%, The molar content is 8%, The molar content is 2%.
[0057] The molar ratio of LCP resin 5: HBA, BP, IA and acetic anhydride is HBA: BP: IA: acetic anhydride = 60: 20: 20: 105; the melting point of LCP resin 5 is 322 ° C, the shear viscosity is 27 Pa · s, and the repeating unit of LCP resin 5 is: The molar content is 60%, The molar content is 20%, The molar content is 20%.
[0058] The molar ratio of LCP resin 6: HBA, BP, TA and acetic anhydride is HBA: BP: TA: acetic anhydride = 60: 20: 20: 105; the melting point of LCP resin 6 is 389 ° C, the shear viscosity is 35 Pa · s, and the repeating unit of LCP resin 6 is: The molar content is 60%, The molar content is 20%, The molar content is 20%.
[0059] The fully aromatic multifunctional oligomers were prepared by the following method:
[0060] Prepare a reaction vessel equipped with a stirrer, monomer feed port, reflux condenser, thermometer, and nitrogen inlet. Replace the gas in the reactor with nitrogen and add the reactants separately. Place the reactor in molten salt at 240°C and reflux for 2 hours. Then start to extract acetic acid. When the acetic acid extraction reaches a certain value, stop the reaction, pour out the reactants, cool them, crush them and grind them into powder to obtain a fully aromatic multifunctional oligomer. The infrared spectrum of the product shows a peak at 1735cm -1 There is a stretching vibration peak of lipid C=O at .
[0061] The molecular weight of the fully aromatic multifunctional oligomer 1 is 930 g / mol, and the structural formula is as follows:
[0062] The reactants are trimesic acid, p-hydroxybenzoic acid, and acetic anhydride, and the molar ratio of the reactants is trimesic acid:p-hydroxybenzoic acid:acetic anhydride=1:6:6.3.
[0063] The molecular weight of the fully aromatic multifunctional oligomer 2 is 1692 g / mol, and the structural formula is as follows:
[0064] The reactants are pyrogallol, p-hydroxybenzoic acid, and acetic anhydride, and the molar ratio of the reactants is pyrogallol:p-hydroxybenzoic acid:acetic anhydride=1:12:12.6.
[0065] The reactants are pyrogallol, p-hydroxybenzoic acid, m-hydroxybenzoic acid, and acetic anhydride, and the molar ratio of the reactants is pyrogallol: p-hydroxybenzoic acid, m-hydroxybenzoic acid: acetic anhydride = 1:2:1:6.3.
[0066] The molecular weight of the fully aromatic multifunctional oligomer 3 is 612 g / mol, and the structural formula is as follows:
[0067] The reactants are trimesic acid, hydroquinone, and acetic anhydride, and the molar ratio of the reactants is trimesic acid:hydroquinone:acetic anhydride=1:3:3.15.
[0068] The molecular weight of the fully aromatic multifunctional oligomer 4 is 570 g / mol, and the structural formula is as follows:
[0069] The reactants are pyrogallol, terephthalic acid, and acetic anhydride, and the molar ratio of the reactants is pyrogallol:terephthalic acid:acetic anhydride=1:3:1.05.
[0070] The molecular weight of the fully aromatic multifunctional oligomer 5 is 2370 g / mol, and the structural formula is as follows:
[0071] The reactants are: trimesic acid, p-hydroxybenzoic acid, and acetic anhydride; the molar ratio of the reactants is 1:18:18.9.
[0072] The molecular weight of the fully aromatic multifunctional oligomer 6 is 3090 g / mol, and the structural formula is as follows:
[0073] The reactants are trimesic acid, p-hydroxybenzoic acid, and acetic anhydride, and the molar ratio of the reactants is trimesic acid:p-hydroxybenzoic acid:acetic anhydride=1:24:25.2.
[0074] The molecular weight of the fully aromatic multifunctional oligomer 7 is 612 g / mol, and the structural formula is as follows:
[0075] The reactants are trimesic acid, resorcinol, and acetic anhydride, and the molar ratio of the reactants is trimesic acid:resorcinol:acetic anhydride=1:3:3.15.
[0076] Glass fiber: Model 584, manufactured by China Jushi Co., Ltd.
[0077] Talc powder: GH 903A, manufactured by Guilin Talc Technology Development Co., Ltd.
[0078] Unless otherwise specified, the materials used in the examples and comparative examples of the present invention are all commercially available raw materials, and the raw materials used in each parallel experiment are all of the same kind.
[0079] Examples 1 to 17 and Comparative Examples 1 to 8
[0080] Examples 1 to 17 and Comparative Examples 1 to 8 respectively provide an LCP resin composition and a preparation method thereof. The components of the LCP resin composition are shown in Tables 1 to 3.
[0081] The preparation method of the LCP resin composition comprises the following steps:
[0082] After the raw materials are uniformly mixed, they are blended and extruded through a twin-screw extruder to obtain a low-warpage LCP resin composition;
[0083] During the blending and extrusion of the twin-screw extruder, the extrusion temperature is: Tm-30°C in zone 1, Tm-10°C in zone 2, Tm+30°C in zone 3, Tm-20°C in zone 4, Tm-20°C in zone 5, Tm-20°C in zone 6, Tm-20°C in zone 7, Tm+10°C in zone 8, and Tm+30°C in zone 9; the screw speed is 400 rpm, where Tm is the melting point of the corresponding LCP resin.
[0084] Table 1
[0085] Table 2
[0086] Table 3
[0087] In order to verify the performance of the LCP resin composition of the present invention, the products prepared in each embodiment and comparative example were subjected to the following performance tests, and the specific steps are as follows:
[0088] (1) Warping deformation: For injection molding, a sample with a length of 100 mm and a thickness of 1.5 mm was placed on a marble plate, with its center fixed close to the marble surface. The height difference between the edge of the sample and the center of the sample was measured with a vernier caliper.
[0089] (2) Flexural modulus: A sample with a length of 100 mm and a thickness of 1.5 mm was injected and tested in accordance with GB / T9341-2008 Determination of Flexural Properties of Plastics. The test conditions were: span 64 mm, deflection 10 mm.
[0090] (3) XRD half-peak width: The XRD half-peak width reflects the change in grain size. Grain size affects the warpage performance of the resin. Excessively large or small grain size makes the resin composition too rigid or too soft, which will increase the warpage. X-ray diffraction was used for measurement, and two-dimensional wide-angle XRD was used for testing. The sample was placed on the stage with perpendicular incident light. The experiment was conducted on a Xeuss2.0 device (Xenocs, France) equipped with a Cu Kα X-ray source (λ = 0.154nm). A Pilatus3R 200K-A detector (pixel size 490×400 pixels) was used to collect 2D spectra, and the spectra were integrated along 0-360° using Foxtrot software to obtain 1D XRD curves. The half-peak width was calculated by the software. The distance from the sample to the detector in the experiment was 170nm.
[0091] (4) Unmelted matter: Injection mold 100 plates with a length and width of 10 cm and a thickness of 0.8 mm. Visually inspect the surface for protrusions or white spots. Record the total number of protrusions and white spots in each 100 plates, i.e., the amount of unmelted matter.
[0092] The test results are shown in Tables 4 to 6.
[0093] Table 4
[0094] Table 5
[0095] Table 6
[0096] By comparing the test results of Examples 1 to 4 and Comparative Examples 2 and 5, it can be seen that the filler added in Comparative Example 2 is too little, the measured XRD half-peak width is larger, and the warpage deformation is significantly larger. This is because the amount of glass fiber and talc added is too little. Although the glass fiber and talc can be evenly dispersed in the resin composition, the crystallinity of the resin composition is relatively small, but the warpage performance of the resin composition cannot be effectively improved; the XRD half-peak width measured in Comparative Example 5 is small, which indicates that too much filler is added, agglomeration occurs in the resin composition, the crystallinity of the resin composition is too high, and even infusible materials are produced, which is obviously not conducive to improving the warpage performance of the resin composition, nor is it conducive to controlling the flexural modulus of the resin composition within an appropriate range. In Examples 1 to 4, Examples 1 to 2 and 4 are blended with the LCP resin in an appropriate amount of glass fiber and talc, so that the LCP resin composition maintains an appropriate flexural modulus, and the warpage performance is effectively improved, with a warpage deformation ≤0.10.
[0097] By comparing the test results of Examples 1, 5-6, 10-11, Comparative Examples 1 and Comparative Examples 3-4, it can be seen that with the increase of the fully aromatic multifunctional polymers, the XRD half-peak width shows a downward trend. This is because the increase in the polymers forms a micro-branched and cross-linked structure, which breaks up the regularity of the molecular chain segments. Compared with Examples 1, 5-6 and 10-11, no wholly aromatic multifunctional oligomer was added to the resin composition of Comparative Example 1, and too little wholly aromatic multifunctional oligomer was added to Comparative Example 4. The XRD half-peak widths measured for both were significantly smaller, and the warpage deformation was significantly larger. This shows that the resin crosslinking degree is too low, which makes the crystallinity of the resin composition too large, which is obviously not conducive to improving the warpage performance of the resin composition, and is also not conducive to controlling the flexural modulus of the resin composition within an appropriate range; the XRD half-peak width measured in Comparative Example 3 is significantly larger, which makes the warpage deformation of the LCP resin composition significantly larger, and produces infusible materials; this may be because the amount of wholly aromatic multifunctional oligomer added in Comparative Example 3 is too much, the resin crosslinking degree is too high, which makes the crystallinity of the resin composition too large and produces infusible materials, which is obviously not conducive to improving the warpage performance of the resin composition.
[0098] By comparing the test results of Examples 5, 7, 13 to 16 and Comparative Example 6, it can be seen that the XRD half-peak width of Comparative Example 6 is too small, while the bending modulus and warpage deformation are too large, which indicates that the molecular weight of the fully aromatic multifunctional oligomer added in Comparative Example 6 is too large, cross-linked with the LCP resin, and the degree of branching and cross-linking is low, which has little effect on the crystallinity of the resin composition; the difference between Example 13 and Example 16 is that the side chains of the oligomer in Example 13 contain para-phenyl groups, and the side chains of the oligomer used in Example 16 contain meta-phenyl groups, and the warpage deformation of Example 13 is smaller.
[0099] Compared with Example 5, the LCP resins of Comparative Examples 7 to 9 have only three repeating unit structures, and the warpage performance of the resin compositions is significantly worse.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A LCP resin composition, characterized in that The composition comprises the following components in parts by weight: 100 parts of LCP resin, 0.1-1 parts of fully aromatic multifunctional oligomer, 10-60 parts of glass fiber and 20-70 parts of filler; The LCP resin comprises repeating units of the following structure: -O-Ar1-O-, -OC-Ar2-CO-, -O-Ar3-CO-, -OC-Ar4-CO-; Wherein, -Ar1-, -Ar2-, -Ar3-, -Ar4- are each independently Any of the following: The fully aromatic multifunctional oligomer has the following structure: Wherein, R1, R2, and R3 are the structures shown in formula (I) or (II): Wherein, n is any number among 1, 2, 3, 4, 5, and 6, n in R1, R2, and R3 are the same or different positive integers, and -Ar5- is R4 and R5 are each independently a carboxyl group or an acetoxy group.
2. The LCP resin composition according to claim 1, characterized in that The LCP resin has a melting point of 302-372° C. and a shear viscosity of 10-30 Pa·s.
3. The LCP resin composition according to claim 1, wherein In the repeating units of the LCP resin, the molar content of -O-Ar1-O- is 10-30%, the molar content of -OC-Ar2-CO- is 8-20%, the molar content of -O-Ar3-CO- is 40-80%, and the molar content of -OC-Ar4-CO- is 2-10%.
4. The LCP resin composition according to claim 1, wherein -Ar1- is -Ar2- is -Ar3- is -Ar4- is 5. The LCP resin composition according to claim 1, characterized in that The mass ratio of the wholly aromatic multifunctional oligomer to the LCP resin is (0.2-0.8):
100.
6. The LCP resin composition according to claim 1, characterized in that The mass ratio of the glass fiber, filler and LCP resin is (3-6): (3-5):
10.
7. The LCP resin composition according to claim 1, characterized in that The filler is an inorganic flake filler, and the inorganic flake filler is selected from at least one of talc powder and mica powder.
8. A method for preparing the LCP resin composition according to any one of claims 1 to 7, characterized in that: The steps include: The LCP resin, the wholly aromatic multifunctional oligomer, the glass fiber and the filler are mixed and then blended and extruded through a twin-screw extruder to obtain a low-warpage LCP resin composition.
9. The method for preparing the LCP resin composition according to claim 8, wherein: During the blending and extrusion by the twin-screw extruder, the extrusion temperature is Tm-30°C to Tm+30°C, and the screw speed is 200 to 600 rpm, wherein Tm is the melting point of the LCP resin.
10. Use of the LCP resin composition according to any one of claims 1 to 7 in the preparation of electronic components.
Citation Information
Patent Citations
Low-warping liquid crystal polyester composite, preparation method and application thereof
CN106633679A
Low-warpage liquid crystal polymer and preparation method thereof
CN111073224A
LCP (Liquid Crystal Polymer) resin composition as well as preparation method and application thereof
CN114672144A
LCP (Liquid Crystal Polymer) resin composition as well as preparation method and application thereof
CN114685957A
LCP (Liquid Crystal Polymer) resin composition as well as preparation method and application thereof