Low-coercivity wire rod and manufacturing method therefor
Through alloy composition optimization and process control, low coercivity wires with coercivity less than 25A/m were prepared, which solved the problem of high coercivity of electromagnetic pure iron materials, improved the response speed and magnetic properties of electronic components, and is suitable for For high performance fast switching and communication electronic devices.
Patent Information
- Application Number
- PCT/CN2024/088744
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-23
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
The coercive force of existing electromagnetic pure iron materials is high, resulting in slow magnetization and demagnetization speeds, making it difficult to meet the needs for rapid electric energy parameter conversion and response.
By optimizing the design of alloy components and regulating the structure, the content of Fe, C, Si, Mn, Al, O, N, Ca and other elements and the proportion of impurities are controlled to form low coercive force soft magnetic materials, using specific smelting and continuous casting methods. , rough rolling, heating, wire rod rolling, Stelmer fan cooling, wire rod drawing and annealing processes to prepare low coercive force wire rods with a coercive force of less than 25A/m.
It achieves low coercivity of soft magnetic materials, improves the response speed and magnetic properties of electronic components, and meets the needs of high-performance fast switching relays and communication electronic devices.
Smart Images

Figure PCTCN2024088744-FTAPPB-I100001 
Figure PCTCN2024088744-FTAPPB-I100002 
Figure PCTCN2024088744-FTAPPB-I100003
Abstract
Description
Low coercivity wire and manufacturing method thereof Technical Field
[0001] The present invention relates to a steel material and a preparation method thereof, and in particular to a wire material and a preparation method thereof. Background Art
[0002] Soft magnetic materials are materials whose magnetization occurs primarily in magnetic fields with a strength of H no greater than 1000 A / m. They exhibit low coercivity and high permeability. They are easy to magnetize and demagnetize. Electromagnetic pure iron is a typical soft magnetic material. With the rapid development of industries like electronics and telecommunications, the application areas of electromagnetic pure iron are continuously expanding, and demand is growing rapidly.
[0003] The main magnetic properties of electromagnetic pure iron include coercive force, coercive force aging increase, maximum magnetic permeability, and maximum magnetic induction intensity. The maximum magnetic induction intensity depends on the composition of the material. The physical state it corresponds to is the neat arrangement of the magnetization vectors inside the material. It is the number of magnetic lines of force passing through the unit cross-sectional area of the iron core, also known as magnetic flux density. It represents the magnetization ability of the material and its unit is T. Coercive force is a quantity that indicates the ease of magnetization of a material and depends on the material's composition and defects (impurities, stress, etc.). Magnetic permeability is the ratio of B to H corresponding to any point on the hysteresis loop and is closely related to the material structure and device operating state. Coercive force refers to the fact that after a magnetic material is saturated magnetized, when the external magnetic field returns to zero, its magnetic induction intensity B does not return to zero. Only by adding a magnetic field of a certain magnitude in the opposite direction of the original magnetizing field can the magnetic induction intensity return to zero. This magnetic field is called the coercive magnetic field, also known as coercive force. The smaller the coercive force of soft magnetic materials, the easier it is to magnetize and demagnetize. In practical applications, the circuit's electrical energy parameter conversion can be achieved more quickly, improving the response speed. Therefore, it is expected to reduce the coercive force of electromagnetic pure iron materials.
[0004] For example, the Chinese patent document with publication number CN100457385C, publication date February 4, 2009, and titled "A Low Coercive Force and High Permeability Electromagnetic Pure Iron Cold-Rolled Sheet Material" adopts the following composition ratios: C ≤ 0.010%, Si ≤ 0.10%, Mn ≤ 0.20%, P ≤ 0.015%, S ≤ 0.010%, Al = 0.50% to 0.80%, [O] and [N] < 40 ppm, electrolytic inclusions < 60 ppm, and the remainder being Fe, to obtain a DT4C brand product with low coercive force and high permeability.
[0005] Summary of the Invention
[0006] One of the purposes of the present invention is to provide a low coercive force wire, which is obtained by optimizing the alloy composition design and controlling the structure to obtain a soft magnetic material, so that it has low coercive force, is easier to magnetize and demagnetize, and improves the response speed and magnetic properties of electronic components.
[0007] To achieve the above object, the present invention provides a low coercive force wire comprising Fe and unavoidable impurities, and further comprising the following chemical elements in the following mass percentages:
[0008] 0<C≤0.003%;
[0009] Si≤0.01%;
[0010] Mn: 0.1-0.2%;
[0011] Al: 0.30-0.45%;
[0012] O: 0.0015-0.0035%;
[0013] N: 0.001-0.003%;
[0014] Ca: 0.0005-0.0015%.
[0015] Furthermore, the present invention also provides a low coercive force wire, the mass percentage of each chemical element of which is:
[0016] 0<C≤0.003%;
[0017] Si≤0.01%;
[0018] Mn: 0.1-0.2%;
[0019] Al: 0.30-0.45%;
[0020] O: 0.0015-0.0035%;
[0021] N: 0.001-0.003%;
[0022] Ca: 0.0005-0.0015%;
[0023] The balance is Fe and other inevitable impurities.
[0024] In the low coercivity wire of the present invention, the design principles of the chemical elements are specifically described as follows:
[0025] Carbon (C) is a crucial element used in steel production. During blast furnace ironmaking, converter furnace (BOF), or electric furnace smelting, carbon is retained in the final product. During cooling or annealing of the steel after rolling, carbon precipitates as cementite. The presence of cementite pins magnetic domains, increasing the material's coercivity. Therefore, the present invention limits the carbon content to 0.003% by weight. In some embodiments, the low-coercivity wire of the present invention has a C content of 0.001 to 0.003% by weight.
[0026] Si: Si is a non-metallic element. Excessive Si content in the present invention can reduce the alloy's magnetic properties. However, Si cannot be completely removed during the steelmaking process. Considering both smelting costs and performance, the present invention limits its upper limit to 0.01%. In some embodiments, the low-coercivity wire of the present invention has a Si content of 0.001 to 0.01% by weight.
[0027] Mn: Mn easily combines with the harmful element S to form MnS, reducing its harmful effects. Furthermore, Mn's solid solution in the steel facilitates grain growth during annealing. To fully utilize the Mn element's potential, the present invention controls the Mn content to be greater than or equal to 0.1%. However, excessive Mn content increases the difficulty of controlling the wire's microstructure during cooling and reduces magnetic properties. Therefore, the Mn addition is controlled to be less than or equal to 0.20%.
[0028] Al: Al is often added to steel as a deoxidizing element. The addition of Al affects the alloy phase transformation. Al dissolved in ferrite increases the austenite transformation temperature, but the addition of Mn expands the austenite phase region and reduces the phase transformation temperature. The present invention simultaneously considers the interaction between Al and Mn elements. Through calculation and experimental research, it is found that when the Al addition amount is higher than 0.3%, the phase transformation point of the material alloy can be higher than 930°C, which is beneficial to the growth of equiaxed ferrite grains during the annealing process after wire drawing. However, when the Al content in the steel is too high, Al replacing iron will reduce the magnetic properties of the alloy and promote the growth of oxide size and increase coercivity. Therefore, the Al addition amount is controlled to be less than or equal to 0.45%.
[0029] O: The O element is an essential element in the steelmaking process. In the present invention, O combines with Al in the liquid steel to form alumina precipitates. By adding Al in 2-3 portions during the steelmaking process and in the refining process, the alumina particle size can be controlled to not exceed 3 μm. This provides nucleation points for the solidification of the molten steel during the continuous casting process, promotes the formation of an equiaxed crystal structure, prevents excessive segregation of residual elements due to excessive growth of columnar crystals, and reduces the material's processing performance and magnetic properties, thereby facilitating structural homogenization. Therefore, the present invention controls the O content in the steel to be greater than or equal to 0.0015%. However, excessively high oxygen content will lead to an increase in inclusions and an increase in size in the steel, significantly affecting the material's drawing and magnetic properties. To improve coercivity, it is necessary to control the O content to be less than or equal to 0.0035%.
[0030] N: In the present invention, N, when dissolved in ferrite, lowers the phase transition temperature and magnetic properties. Therefore, its content must be kept below 0.003%. During alloy cooling, N readily combines with Al to precipitate. This, along with residual C, forms carbides with other alloying elements. These small, nanoscale precipitates prevent abnormal grain growth during heating, promote uniform ferrite grain growth, and improve the uniformity of the material's structure and properties. Therefore, to maximize the N's potential, its content is controlled to be greater than or equal to 0.001%.
[0031] Ca: In the present invention, adding Ca element greater than or equal to 0.0005% is beneficial to the dispersion and distribution of alumina particles. However, too much Ca element will increase the difficulty of alloy smelting and increase the cost. Therefore, the Ca content is controlled to be less than or equal to 0.0015%.
[0032] Furthermore, among other inevitable impurities in the low coercivity wire of the present invention: Ti≤0.003%, P≤0.015%, S≤0.008%.
[0033] The unavoidable impurities in the present invention are primarily phosphorus (P), sulfur (S), and titanium (Ti). Ti easily combines with nitrogen to form coarse TiN, so the Ti content is preferably controlled to no more than 0.003%. Residual P and S in the steel increase its brittleness and reduce its formability. Therefore, the P content is preferably controlled to no more than 0.015%, and the S content to no more than 0.008%.
[0034] Furthermore, in the low coercivity wire described in the present invention, the mass percentage of chemical elements thereof also satisfies at least one of the following conditions: (Al+100Ca) / (Ti+N)≥85; Mn / S≥20; wherein each chemical element is substituted into the value before the percentage sign of the mass percentage of the corresponding chemical element.
[0035] In order to promote the sufficient precipitation of Al nitride and carbon and to give full play to the role of Ca, the present invention further controls the mass percentage of each chemical element in the material to satisfy (Al + 100Ca) / (Ti + N) ≥ 85. In some embodiments, 85 ≤ (Al + 100Ca) / (Ti + N) ≤ 170.
[0036] The Mn element easily combines with the harmful element S to form MnS. To reduce its harm, the present invention controls Mn / S to be ≥ 20. In some embodiments, 20≤Mn / S≤200.
[0037] The microstructure of the low-coercivity wire described in the present invention includes ferrite grains. Furthermore, the ferrite grain size of the low-coercivity wire described in the present invention is 200-800 μm. This structural feature can effectively reduce the material's coercivity, resulting in excellent soft magnetic properties.
[0038] The microstructure of the low-coercivity wire described herein comprises carbon and nitrogen precipitates of aluminum oxide and aluminum. Furthermore, in the low-coercivity wire described herein, the carbon and nitrogen precipitates of aluminum oxide and aluminum are ≤3 μm in size. This structural feature effectively reduces the material's coercivity, imparting excellent soft magnetic properties. In some embodiments, the carbon and nitrogen precipitates of aluminum oxide and aluminum in the low-coercivity wire described herein are 0.1 to 3 μm in size.
[0039] Furthermore, the coercive force of the low-coercive force wire of the present invention is ≤25 A / m. In some embodiments, the coercive force of the low-coercive force wire of the present invention is 5 to 25 A / m, for example, 10 A / m, 15 A / m, or 20 A / m.
[0040] Another object of the present invention is to provide a method for manufacturing a low coercive force wire, which uses a relatively simple processing technology to produce a soft magnetic material wire that meets the low coercive force requirements.
[0041] Based on the above objectives, the present invention also provides a method for manufacturing a low coercive force wire, which comprises the steps of:
[0042] (1) smelting;
[0043] (2) continuous casting;
[0044] (3) initial rolling;
[0045] (4) Heating: heating to 900-1150° C., for example, 950-1150° C., and keeping warm for 1.5-2.5 hours;
[0046] (5) Wire rod rolling;
[0047] (6) Stelmore fan cooling;
[0048] (7) Wire rod drawing;
[0049] (8) Annealing: The annealing heating temperature is 870-910℃, the holding time is 1-2h, and then cooled to below 500℃ at a cooling rate of less than or equal to 50℃ / h.
[0050] In some embodiments, in the initial rolling step of the manufacturing method described in the present invention, smelting can be carried out by electric furnace or converter smelting, followed by LF (Ladle Furnace) furnace refining and VD (Vacuum Degassing) or RH (Ruhrstahl-Heraeus) degassing treatment, and then calcium wire is fed.
[0051] Furthermore, in the initial rolling step of the manufacturing method of the present invention, the billet or slab is heated to 1100-1250° C. and then rolled into a small billet of 140-220 mm.
[0052] Furthermore, in the wire rod rolling step of the manufacturing method described in the present invention, the rolling speed is controlled to be 20-110 m / s.
[0053] Furthermore, in the wire rod rolling step of the manufacturing method of the present invention, the inlet temperature of the finishing mill is controlled to be 900-980°C, the inlet temperature of the sizing mill is controlled to be 900-980°C, and the spinning temperature is controlled to be 890-960°C.
[0054] Furthermore, in the Stelmore blower cooling step of the manufacturing method described in the present invention, the air volume of the F1-F3 fans of the Stelmore blower group is controlled to be 0-50%.
[0055] Furthermore, in the wire rod drawing step of the manufacturing method of the present invention, the drawing reduction ratio is controlled to be 10-30%.
[0056] Furthermore, in the annealing step of the manufacturing method of the present invention, the cooling rate is controlled to be 30-50° C. / h.
[0057] The low coercivity wire of the present invention has the following advantages and beneficial effects:
[0058] The low-coercivity wire of the present invention has a uniform microstructure, a ferrite grain size of 200-800 μm, a coercivity of less than or equal to 25 A / m, and excellent magnetic properties. It can meet the processing requirements of high-performance, fast-switching relay cores and communication electronic device parts, and has broad application prospects. DETAILED DESCRIPTION
[0059] The low coercivity wire and the preparation method thereof according to the present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an undue limitation to the technical solution of the present invention.
[0060] Examples 1-10 and Comparative Examples 1-3
[0061] The low coercivity wires of Examples 1-10 were all prepared by the following steps:
[0062] (1) After smelting in an electric furnace, the steel is subjected to LF furnace refining and RH degassing treatment to control the P content in the steel to be less than or equal to 0.015%, the S content to be less than or equal to 0.008%, and the Ti content to be less than or equal to 0.003%. At the same time, the O content in the steel is controlled to be 0.0015-0.0035%, and the N content to be 0.001-0.003%. After refining, calcium wire is fed to control the Ca content in the steel to be 0.0005-0.0015%.
[0063] (2) A bloom continuous casting machine was used for casting under argon protection to obtain continuous casting blooms or slabs. The bloom size was ≤450 mm and the slab thickness was ≤400 mm. The casting speed, cooling and end soft reduction parameters were adjusted during the continuous casting process to achieve uniform distribution of precipitates and reduce element segregation in the core of the billet. The chemical composition of the bloom or slab is shown in Table 1.
[0064] (3) The slabs were longitudinally cut into billets ≤ 400 mm in size. Examples 6-7 were cut into 400 mm billets, Examples 8-9 were cut into 350 mm billets, and Example 10 was cut into 250 mm billets. The continuously cast blooms or billets cut from slabs were heated to 1100-1250°C and then rolled into 140-220 mm billets. The billets were subjected to eddy current testing, magnetic particle testing, grinding wheel re-molding, additional magnetic particle testing, and grinding to remove surface defects such as cracks and pits. The depth of the defects was ≤ 0.5 mm.
[0065] (4) Heat the billet to 900-1150°C, for example, 950-1150°C, and keep it at this temperature for 1.5-2.5 hours.
[0066] (5) Wire rod rolling: the rolling speed is controlled at 20-110 m / s, the inlet temperature of the finishing mill is controlled at 900-980°C, the inlet temperature of the sizing mill is controlled at 900-980°C, the spinning temperature is controlled at 890-960°C, and the size of the wire rod obtained by rolling is controlled at Φ5.5-16 mm.
[0067] (6) Stelmore fan cooling: The air volume of F1-F3 fans is 0-50%, and 27 3m insulation covers are set on the Stelmore line, of which 1-5# insulation covers are open and 6-27# insulation covers are closed.
[0068] (7) The hot-rolled wire rod is subjected to single-pass drawing, and the drawing reduction ratio is controlled to be 10-30%.
[0069] (8) Annealing: The annealing heating temperature is 870-910℃, the holding time is 1-2h, and then cooled to below 500℃ at a cooling rate of less than or equal to 50℃ / h.
[0070] The comparative wires of Comparative Examples 1-3 were also prepared by the above-mentioned steps, but their chemical compositions and specific process parameters in each step failed to meet the design requirements of the present invention.
[0071] Table 1 lists the mass percentages of the chemical elements in the low coercive force wires of Examples 1-10 and the comparative wires of Comparative Examples 1-3.
[0072] Table 1. (wt%, the balance is Fe and other inevitable impurities except P, S, and Ti)
[0073] Note: In the above formulas (Al+100Ca) / (Ti+N) and Mn / S, substitute the values before the percentage sign of the corresponding chemical element mass percentage.
[0074] Table 2-1 and Table 2-2 list the specific process parameters of the low coercive force wires of Examples 1-10 and the comparative wires of Comparative Examples 1-3 in the above steps.
[0075] Table 2-1.
[0076] Table 2-2.
[0077] The wire rods of Examples 1-10 and the comparative wire rods of Comparative Examples 1-3 were sampled, and the microstructure (ferrite grain size, size of alumina and carbon and nitrogen precipitates of aluminum) of the steel plate samples of each example was observed and analyzed using the metal microstructure inspection method of GB / T 13298-2015. The relevant observation and analysis results are listed in Table 3 below.
[0078] In addition, the wires of Examples 1-10 and the comparative wires of Comparative Examples 1-3 obtained through the above process steps were sampled again, and the coercive force was tested according to the magnetic permeability and saturation magnetic induction ring sample method and the permeometer method in accordance with GB / T 13012-2008, measurement methods of DC magnetic properties of soft magnetic materials. The test results are listed in Table 3.
[0079] Table 3 lists the microstructure characteristics and coercivity test results of the wires of Examples 1-10 and the comparative wires of Comparative Examples 1-3.
[0080] Table 3.
[0081] As shown in Table 3, the ferrite grain size of the wires in Examples 1-10 ranged from 200 to 800 μm, while the ferrite grain size of the comparative examples was smaller than that of the wires in the present invention. Furthermore, the size of the alumina and aluminum carbon and nitrogen precipitates in the wires in Examples 1-10 of the present invention was ≤ 3 μm.
[0082] It can also be seen from Table 3 that the coercive forces of the wires of Examples 1-10 of the present invention are all lower than 25 A / m, while the coercive force of Comparative Examples 1-3 is as low as 41 A / m.
[0083] In addition, the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.
[0084] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily conceived by those skilled in the art based on the disclosure of the present invention are intended to fall within the scope of protection of the present invention.
Claims
1. A low coercive force wire material containing Fe and unavoidable impurities, characterized in that: It also contains the following chemical elements in the following mass percentages: 0<C≤0.003%; Si≤0.01%; Mn: 0.1-0.2%; Al: 0.30-0.45%; O: 0.0015-0.0035%; N:0.001-0.003%; Ca: 0.0005-0.0015%.
2. The low coercivity wire according to claim 1, characterized in that The mass percentage of each chemical element is: 0<C≤0.003%; Si≤0.01%; Mn: 0.1-0.2%; Al: 0.30-0.45%; O: 0.0015-0.0035%; N: 0.001-0.003%; Ca: 0.0005-0.0015%; the balance is Fe and other inevitable impurities.
3. The low coercive force wire according to claim 1, characterized in that Among other inevitable impurities: Ti≤0.003%, P≤0.015%, S≤0.008%.
4. The low coercivity wire according to claim 3, characterized in that The mass percentage of chemical elements also satisfies at least one of the following conditions: (Al+100Ca) / (Ti+N)≥85; Mn / S≥20; In the formula, each chemical element is substituted into the value before the percentage sign of the corresponding chemical element mass percentage content.
5. The low coercive force wire according to claim 1, characterized in that: The size of the ferrite grains in the low coercive force wire is 200-800 μm.
6. The low coercive force wire according to claim 1, characterized in that: The size of the carbon and nitrogen precipitates of aluminum oxide and aluminum in the low coercivity wire is ≤3 μm.
7. The low coercive force wire according to claim 1, characterized in that: Its coercive force is ≤25A / m.
8. The method for manufacturing a low coercive force wire according to any one of claims 1 to 7, characterized in that: It includes the steps of: (1) Smelting; (2) Continuous casting; (3) initial rolling; (4) Heating: heating to 900-1150°C, keeping warm for 1.5-2.5h; (5) Wire rod rolling; (6) Stelmore fan cooling; (7) Wire rod drawing; (8) Annealing: The annealing heating temperature is 870-910°C, the holding time is 1-2h, and then cooled to below 500°C at a cooling rate of less than or equal to 50°C / h.
9. The manufacturing method according to claim 8, characterized in that: In the initial rolling step, the billet or slab is heated to 1100-1250°C and then rolled into a 140-220 mm billet.
10. The manufacturing method according to claim 8, characterized in that: In the wire rod rolling step, the rolling speed is controlled to be 20-110 m / s.
11. The manufacturing method according to claim 8, characterized in that: In the wire rod rolling step, the inlet temperature of the finishing mill is controlled at 900-980°C, the inlet temperature of the sizing mill is controlled at 900-980°C, and the spinning temperature is controlled at 890-960°C.
12. The manufacturing method according to claim 8, characterized in that: In the Stelmore blower cooling step, the air volume of the F1-F3 blowers of the Stelmore blower group is controlled to be 0-50%.
13. The manufacturing method according to claim 8, characterized in that: In the wire rod drawing step, the drawing reduction ratio is controlled to be 10-30%.
Citation Information
Patent Citations
Method for manufacturing electromagnetic pure iron cold-rolled sheet material with low coercive force and high magnetoconductivity
CN100457385C
Low-coercivity cold-rolled electromagnetic pure iron plate strip continuous annealing method
CN106555034A
Method for manufacturing electromagnetic pure iron cold-rolled sheet material with low coercive force and high magnetoconductivity
CN1775466A
A method for manufacturing cold rolled steel sheet forbraun tube mask frame with superior magnetic property
KR1020020042099A
Steel
SU1261970A1
Cited By
Heat treatment process for soft magnetic stainless steel with high magnetic conductivity and ultralow coercive force
CN120272678A