Artificial leather and preparation method therefor

Through the multi-layer structure of artificial leather, using PHA base material and non-PHA base material, the environmental and performance deficiencies of existing synthetic leather are solved, and the effects of environmental protection, softness, antibacterial and mildew prevention are achieved.

WO2024222728A1PCT designated stage expired Publication Date: 2024-10-31BEIJING PHABUILDER BIOTECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/089511
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing synthetic leather uses petroleum-based materials in the production process, which leads to environmental pollution and health risks. It also has insufficient antibacterial and anti-mildew properties and poor hand feel, making it difficult to meet consumer needs.

Method used

Artificial leather with a multi-layer structure, including base fabric layer, filling layer, foam layer and simulation layer, is mainly composed of PHA base material and non-PHA base material. By adjusting the material proportion and additives, it can achieve environmental protection, softness, antibacterial and mildew resistance , waterproof and breathable performance.

Benefits of technology

It has realized environmentally friendly and degradable artificial leather, which has soft feel, good elasticity, skin-friendly and antibacterial and anti-mildew properties, while avoiding the environmental pollution and health risks of traditional leather.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024089511_31102024_PF_FP_ABST
    Figure CN2024089511_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of leather, in particular to artificial leather and a preparation method therefor. The artificial leather comprises a PHA base material, a non-PHA base material and / or auxiliary materials, and comprises four layers, i.e., a base cloth layer, a filling layer, a foamed layer and a simulation layer, wherein the main materials of the four layers are the same, and the use of an adhesive is avoided. The artificial leather of the present application does not cause damage to the ecological environment, and also has the advantages of being environmentally friendly and degradable and having a high recycling rate.
Need to check novelty before this filing date? Find Prior Art

Description

Artificial leather and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of leather, in particular to artificial leather and a preparation method thereof. Background Art

[0002] Leather is widely used in many modern fields, including automotive interiors, furniture, leather shoes and leather clothing, and decoration. Leather is generally divided into two categories: natural leather and synthetic leather. Due to the condemnation of animal protectionism, natural leather has gradually been replaced by synthetic leather.

[0003] However, the primary components of current synthetic leather are petroleum-based materials such as polyvinyl chloride (PVC), polyurethane (PU), nylon microfiber, acrylic, and spandex. The production process consumes significant amounts of petroleum, generating toxic pollution, and the finished product is difficult to compost in the natural environment. While chemically stable at room temperature and exhibiting excellent physical properties such as abrasion resistance and tear strength, synthetic leather still suffers from poor breathability, a hard feel, poor skin compatibility, a pungent odor, and even the presence of free formaldehyde, making it difficult to meet consumer demand.

[0004] Furthermore, leather also has antibacterial and anti-mite requirements. However, existing antibacterial leathers often have poor elasticity. After prolonged compression or stress, they take a long time to rebound. This is due to the high levels of antibacterial and anti-fungal agents added during production or surface treatment. This results in a hard, less elastic feel, and a less than ideal, comfortable feel.

[0005] Summary of the Invention

[0006] To solve the above-mentioned problems, the present invention provides an artificial leather that is naturally fully degradable, soft to the touch, elastic, skin-friendly, antibacterial, mildew-proof, waterproof, breathable, and easy to dye. No solvents or adhesives are required during the production process, truly achieving environmental friendliness throughout the entire production, use, and disposal process.

[0007] A first aspect of the present invention provides an artificial leather.

[0008] Preferably, the artificial leather comprises a base fabric layer, a filling layer, a foaming layer and / or a simulation layer.

[0009] Preferably, the artificial leather is a laminated structure, wherein the first layer is a base fabric layer, the second layer is a filling layer, the third layer is a foaming layer, and the fourth layer is a simulation layer.

[0010] In a specific embodiment of the present invention, the mass ratio of the base fabric layer to the filling layer + foaming layer + simulation layer is any value from (1:5) to (2:5), for example, 1:5, 1.1:5, 1.2:5, 1.3:5, 1.4:5, 1.5:5, 1.6:5, 1.7:5, 1.8:5, 1.9:5 or 2:5.

[0011] Preferably, the artificial leather comprises a substrate, and the substrate comprises a PHA substrate.

[0012] Preferably, the added mass of the PHA substrate in any one, two, three or four layers of the base fabric layer, the filling layer, the foaming layer or the simulation layer accounts for 50%-80%, preferably 60%-75%, for example, 50%, 55%, 60%, 61%, 61.5%, 61.54%, 61.8%, 61.84%, 61.9%, 61.94%, 62%, 63%, 64%, 64.03%, 64.04%, 64.1%, 64.13%, 64.3%, 64.34%, 64.5%, 64. .51%, 64.6%, 65%, 65.38%, 65.5%, 65.8%, 65.81%, 65.86%, 65.9%, 66%, 66.5%, 66.6%, 66.8%, 67%, 67.3%, 67.37%, 68%, 68.4%, 68.41%, 68.5%, 69%, 69.2%, 69.23%, 69.3%, 69.5%, 69.6%, 69.68%, 70%, 71%, 72%, 73%, 74%, 75% or 80%.

[0013] Preferably, the substrate further includes a non-PHA substrate.

[0014] Further preferably, in any one, two, three or four layers of the base fabric layer, filling layer, foaming layer or simulation layer, the mass ratio of the PHA substrate to the non-PHA substrate is (1-5): 1, preferably any value in (2-4): 1, for example, 1: 1, 1.5: 1, 2: 1, 2.46: 1, 2.5: 1, 2.85: 1, 2.86: 1, 2.88: 1, 3: 1, 3.09: 1, 3.5: 1, 4: 1, 4.5: 1, 5: 1.

[0015] Preferably, the PHA matrix comprises a homopolymer or copolymer of monomers constituting PHA.

[0016] Further preferably, the monomers constituting PHA include but are not limited to one or more of 2-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 3-hydroxypropionic acid, 5-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid or 3-hydroxynonanoic acid, 3-hydroxydecanoic acid, and 3-hydroxydodecanoic acid.

[0017] In a specific embodiment of the present invention, the PHA includes but is not limited to one or more of P(HB-LA), P3HP, PHB, P4HB, PHV, PHO, PHN, PHD, PHBV, P34HB, PHBHHp, PHBHHx, P3HB4HB3HV or P3HB4HB5HV.

[0018] In a specific embodiment of the present invention, any one, two, three or four of the base fabric layer, filling layer, foaming layer or simulation layer include a PHA substrate (preferably including P34HB, and more preferably including non-P34HB PHA). In a specific embodiment of the present invention, the PHA substrate includes a mixed raw material of P34HB and non-P34HB PHA.

[0019] Preferably, the added mass of P34HB in the PHA matrix is ​​any value between 21% and 79%, preferably any value between 25% and 70%, for example, 21%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, and 79%.

[0020] Preferably, the molar content of 4HB in the P34HB is any value between 3% and 30%, preferably any value between 8% and 24%, for example, 3%, 5%, 8%, 10%, 12%, 15%, 16%, 20%, 24%, 25%, and 30%.

[0021] Preferably, the non-PHA substrate includes but is not limited to one or more of PLA, PBAT, PPC, PBS, PGA, black tea fiber, soy protein fiber, mulberry fiber, sugarcane fiber or bamboo fiber.

[0022] In a specific embodiment of the present invention, in the artificial leather, the PHA substrate of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer is PHB and P34HB, and the molar content of 4HB in the P34HB is any value between 3% and 30%, preferably any value between 8% and 24%, for example, 3%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, and preferably the molar content of 4HB in the P34HB is 16%; preferably, in the PHA substrate, the added mass of P34HB is any value between 21% and 79%, preferably any value between 25% and 70%, for example, 21, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 79%. In a specific embodiment of the present invention, In the embodiment, the mass ratio of PHB and P34HB in the PHA substrate is 3:2; the non-PHA substrate in the artificial leather is black tea fiber, mulberry fiber and PBS, and the mass ratio of black tea fiber, mulberry fiber and PBS in the non-PHA substrate of the base fabric layer is 4.5:3:10; the mass ratio of black tea fiber, mulberry fiber and PBS in the non-PHA substrate of the filling layer and / or foaming layer is 6:4:13.3; the mass ratio of black tea fiber, mulberry fiber and PBS in the non-PHA substrate of the simulation layer is 3:2:6.7; the mass ratio of PHA substrate and non-PHA substrate in the substrates of the base fabric layer, filling layer and foaming layer is 2.86:1; the mass ratio of PHA substrate and non-PHA substrate in the simulation layer is 2.85:1.

[0023] In a specific embodiment of the present invention, in the artificial leather, the PHA substrate of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer is PHBV and P34HB, and the molar content of 3HV in the PHBV is any value in the range of 1%-30%, for example, 1%, 5%, 10%, 15%, 20%, 25%, 30%, preferably, the molar content of 3HV in the PHBV is 5%, and the molar content of 4HB in the P34HB is 3%-30%. Any value, preferably any value in the range of 8%-24%, such as 3%, 5%, 10%, 15%, 20%, 25%, 30%, preferably the molar content of 4HB in the P34HB is 12%, preferably, in the PHA matrix, the added mass of P34HB is any value in the range of 21%-79%, preferably any value in the range of 25%-70%, such as 21, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75 , 79%. In a specific embodiment of the present invention, the mass ratio of PHBV and P34HB in the PHA substrate is 1:1; the non-PHA substrate in the artificial leather is soy protein fiber, PLA and PBAT, and the mass ratio of soy protein fiber, PLA and PBAT in the non-PHA substrate in the base fabric layer is 4.5:5:8; the mass ratio of soy protein fiber, PLA and PBAT in the non-PHA substrate in the filling layer and / or foaming layer is 6:6.7:10.7; the mass ratio of soy protein fiber, PLA and PBAT in the non-PHA substrate in the simulation layer is 3:3.3:5.3; the mass ratio of PHA substrate and non-PHA substrate in the substrate of the base fabric layer is 2.86:1; the mass ratio of PHA substrate and non-PHA substrate in the substrate of the filling layer and / or foaming layer is 2.85:1; the mass ratio of PHA substrate and non-PHA substrate in the substrate of the simulation layer is 2.88:1.

[0024] In a specific embodiment of the present invention, in the artificial leather, the PHA substrates of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer are PHB, P34HB and PHBHHx, the molar content of 4HB in the P34HB is any value between 3% and 30%, preferably any value between 8% and 24%, for example, 3%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, preferably the molar content of 4HB in the P34HB is 8%, the molar content of 3HHx in the PHBHHx is any value between 1% and 30%, for example, 1%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, preferably the molar content of 3HHx in the PHBHHx is 20%, preferably, the P In the HA substrate, the added mass of P34HB is any value between 21% and 79%, preferably any value between 25% and 70%, for example, 21, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, and 79%. In a specific embodiment of the present invention, the mass ratio of PHB, P34HB, and PHBHHx in the PHA substrate is 9:5:3; the non-PHA substrate in the artificial leather is sugarcane fiber, PPC, and PGA, and the mass ratio of sugarcane fiber, PPC, and PGA in the non-PHA substrate in the base fabric layer, filling layer, foaming layer, and / or simulation layer is 3:4:4; the mass ratio of the PHA substrate and the non-PHA substrate in the base fabric layer, filling layer, and foaming layer is 3.09:1.

[0025] In a specific embodiment of the present invention, in the artificial leather, the PHA substrate of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer is PHBV, P34HB and PHBHHx, and the molar content of 3HV in the PHBV is any value in the range of 1%-30%, for example, 1%, 5%, 10%, 15%, 20%, 25%, 30%, preferably, the molar content of 3HV in the PHBV is 5%, the molar content of 4HB in the P34HB is 3 %-30%, preferably any value in the range of 8%-24%, such as 3%, 5%, 8%, 10%, 15%, 20%, 24%, 25%, 30%, preferably the molar content of 4HB in the P34HB is 10%, the molar content of 3HHx in the PHBHHx is any value in the range of 1%-30%, such as 1%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, preferably the molar content of 3HHx in the PHBHHx is The molar content of Hx is 8%. Preferably, the mass of P34HB added to the PHA substrate is any value within the range of 21%-79%, preferably any value within the range of 25%-70%, for example, 21, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 79%. In a specific embodiment of the present invention, the mass ratio of PHBV, P34HB and PHBHHx in the PHA substrate is 2:1:1; the non-PHA substrate in the artificial leather is soybean protein fiber, bamboo fiber and PBS, and the mass ratio of soybean protein fiber, bamboo fiber and PBS in the non-PHA substrate of the base fabric layer is 3:6:10.5; the mass ratio of soybean protein fiber, bamboo fiber and PBS in the non-PHA substrate of the filling layer, foaming layer and / or simulation layer is 2:4:7; the mass ratio of the PHA substrate to the non-PHA substrate in the substrate of the base fabric layer, filling layer, foaming layer and / or simulation layer is 2.46:1.

[0026] In a specific embodiment of the present invention, in the artificial leather, the PHA substrate of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer is PHB and P34HB, and the molar content of 4HB in the P34HB is any value in the range of 3%-30%, preferably any value in the range of 8%-24%, for example, 3%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, and preferably the molar content of 4HB in the P34HB is 16%; preferably, in the PHA substrate, the added mass of P34HB is any value in the range of 21%-79%, preferably any value in the range of 25%-70%, for example, 21, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75. 79%. In a specific embodiment of the present invention, the mass ratio of PHB to P34HB in the PHA substrate is 5:4; the non-PHA substrate in the artificial leather is black tea fiber, bamboo fiber and PGA, and the mass ratio of black tea fiber, bamboo fiber and PGA in the non-PHA substrate of the base fabric layer is 9:8:10; the mass ratio of black tea fiber, bamboo fiber and PGA in the non-PHA substrate of the filling layer and / or foaming layer is 6:5.3:6.7; the mass ratio of black tea fiber, bamboo fiber and PGA in the non-PHA substrate of the simulation layer is 3:2.7:3.3; the mass ratio of PHA substrate and non-PHA substrate in the substrates of the base fabric layer, filling layer, foaming layer and simulation layer is 4:1.

[0027] In a specific embodiment of the present invention, in the artificial leather, the PHA substrate of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer is PHB and P34HB, and the molar content of 4HB in the P34HB is any value between 3% and 30%, preferably any value between 8% and 24%, for example, 3%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, and preferably the molar content of 4HB in the P34HB is 16%; preferably, in the PHA substrate, the added mass of P34HB is any value between 21% and 79%, preferably any value between 25% and 70%, for example, 21, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 79%. In a specific embodiment of the present invention, In the embodiment, the mass ratio of PHB and P34HB in the PHA substrate is 17:8; the non-PHA substrate in the artificial leather is mulberry fiber, bamboo fiber and PBAT, and the mass ratio of mulberry fiber, bamboo fiber and PBAT in the non-PHA substrate of the base fabric layer is 9:5:21; the mass ratio of mulberry fiber, bamboo fiber and PBAT in the non-PHA substrate of the filling layer and / or foaming layer is 6:3.4:14; the mass ratio of mulberry fiber, bamboo fiber and PBAT in the non-PHA substrate of the simulation layer is 3:1.7:7; the mass ratio of PHA substrate and non-PHA substrate in the base fabric layer substrate is 2.86:1; the mass ratio of PHA substrate and non-PHA substrate in the substrates of the filling layer, foaming layer and simulation layer is 2.85:1.

[0028] In a specific embodiment of the present invention, in the artificial leather, the PHA substrate of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer is PHB and P34HB, and the molar content of 4HB in the P34HB is any value in the range of 3%-30%, preferably any value in the range of 8%-24%, for example, 3%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, and preferably the molar content of 4HB in the P34HB is 16%; preferably, in the PHA substrate, the added mass of P34HB is any value in the range of 21%-79%, preferably any value in the range of 25%-70%, for example, 21 , 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 79%. In a specific embodiment of the present invention, the mass ratio of PHB to P34HB in the PHA substrate is 33:15; the non-PHA substrate in the artificial leather is black tea fiber, soy protein fiber and PBAT, and the mass ratio of black tea fiber, soy protein fiber and PBAT in the non-PHA substrate of the base fabric layer, filling layer, foaming layer and / or simulation layer is 4:4:5; the mass ratio of PHA substrate to non-PHA substrate in the substrate of the base fabric layer, filling layer, foaming layer and simulation layer is 2.46:1.

[0029] Preferably, the artificial leather further comprises auxiliary materials.

[0030] More preferably, the auxiliary material includes one or both of a filler and an ultraviolet absorber.

[0031] Preferably, any one, two, three or four of the base fabric layer, filling layer, foaming layer or simulation layer comprises a PHA substrate, more preferably a non-PHA substrate, and more preferably a filler and a UV absorber.

[0032] In a specific embodiment of the present invention, any one, two, three or four of the base fabric layer, filling layer, foaming layer or simulation layer comprises a mixed raw material substrate of P34HB and non-P34HB PHA, preferably comprises a non-PHA substrate, and more preferably comprises a filler and a UV absorber.

[0033] More preferably, the filler is a micron-sized filler.

[0034] More preferably, the ultraviolet absorber is a nano-scale inorganic powder.

[0035] Preferably, in the base fabric layer, the mass ratio of the filler to the ultraviolet absorber in the auxiliary material is any value in the range of (3-5):1, such as 3:1, 4:1, or 5:1.

[0036] Preferably, in the filling layer, the mass ratio of the filler to the ultraviolet absorber in the auxiliary material is any value in the range of (5-8):1, such as 5:1, 6:1, 6.5:1, 7:1, or 8:1.

[0037] Preferably, in the simulation layer, the mass ratio of the filler to the ultraviolet absorber in the auxiliary material is any value in the range of (1-3):1, such as 1:1, 1.5:1, 2:1, or 3:1.

[0038] Preferably, in the base fabric layer, the mass ratio of PHA, filler and UV absorber is any value of (35-60):(3-5):1, for example, 35:3:1, 36:4:1, 42:4:1, 45:4:1, 48:4:1, 50:4:1, 54:4:1, 55:4:1, and 60:4:1.

[0039] Preferably, in the filling layer, the mass ratio of PHA, filler and UV absorber is any value of (40-80):(5-8):1, for example, 40:5:1, 45:5:1, 48:6.5:1, 50:8:1, 56:6.5:1, 64:6.5:1, 66.6:6.5:1, 66.7:6.5:1, 70:6.5:72:6.5:1, 75:8:1, and 80:8:1.

[0040] Preferably, in the simulation layer, the mass ratio of PHA, filler and UV absorber is any value of (20-40):(1-3):1, for example, 20:1:1, 24:1.5:1, 25:3:1, 28:1.5:1, 30:3:1, 32:1.5:1, 33.3:1.5:1, 33.4:1.5:1, 36:1.5:1, and 40:3:1.

[0041] Preferably, in the base fabric layer, the mass of the filler added is 0%-10% of the PHA substrate, preferably 0.1%-10%, and more preferably any value in the range of 5%-8%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0042] Preferably, in the filling layer, the mass of the filler added is 0%-11% of the PHA substrate, preferably 0.1%-11%, and more preferably any value in the range of 5%-11%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 9.5%, 9.6%, 9.7%, 9.8%, 10%, 10.1%, 10.2%, 10.5%, and 11%.

[0043] Preferably, fillers are added or not added to the foaming layer. In one embodiment of the present invention, no fillers are added to the foaming layer.

[0044] Preferably, in the simulation layer, the added mass of the filler is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value between 1% and 2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 2.2%, 2.3%, 2.4%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0045] The filler includes but is not limited to one or more of hollow glass microspheres, mica powder or talc powder.

[0046] In a specific embodiment of the present invention, the filler is hollow glass microspheres.

[0047] In a specific embodiment of the present invention, the filler is mica powder.

[0048] In a specific embodiment of the present invention, the filler is talc.

[0049] Preferably, in the base fabric layer, the added mass of the ultraviolet absorber is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.9%, 2%, 2.1%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0050] Preferably, in the filling layer, the added mass of the ultraviolet absorber is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.5%, 1.6%, 2%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0051] Preferably, in the foaming layer, the added mass of the ultraviolet absorber is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.1%, 1.2%, 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0052] Preferably, in the simulation layer, the added mass of the ultraviolet absorber is 0%-10% of the PHA substrate, preferably 0.1%-5%, and further preferably any value between 1% and 2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.47%, 1.48%, 1.49%, 1.5%, 1.56%, 1.6%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0053] Preferably, the ultraviolet absorber includes but is not limited to one or more of nano ZnO, rutile TiO2 or nano CeO2.

[0054] In a specific embodiment of the present invention, the ultraviolet absorbers in the base fabric layer, filling layer, foaming layer and simulation layer are nano ZnO and rutile TiO2, and the mass ratio of the nano ZnO to rutile TiO2 is 2:3.

[0055] In a specific embodiment of the present invention, the ultraviolet absorbers in the artificial leather are rutile TiO2 and nano-CeO2, the mass ratio of rutile TiO2 and nano-CeO2 in the base fabric layer, filling layer and simulation layer is 1:1; the mass ratio of rutile TiO2 and nano-CeO2 in the foaming layer is 7:8.

[0056] In a specific embodiment of the present invention, the ultraviolet absorbers in the base fabric layer, the filling layer, the foaming layer and the simulation layer are nano-ZnO and nano-CeO2, and the mass ratio of the nano-ZnO to nano-CeO2 is 2:3.

[0057] In a specific embodiment of the present invention, the ultraviolet absorbers in the base fabric layer, filling layer, foaming layer and simulation layer are nano ZnO and rutile TiO2, and the mass ratio of the nano ZnO to rutile TiO2 is 2:3.

[0058] Preferably, the auxiliary materials further include but are not limited to one or more of a chain extender, an environmentally friendly plasticizer, an anti-hydrolysis agent, an antioxidant, a heat stabilizer or a foaming agent.

[0059] Preferably, in any one, two or three layers of the base fabric layer, filling layer or simulation layer, the auxiliary material includes one or both of fillers or ultraviolet absorbers, and further preferably also includes one or more of chain extenders, environmentally friendly plasticizers, anti-hydrolysis agents, antioxidants, heat stabilizers or foaming agents.

[0060] Preferably, in the foaming layer, the auxiliary material includes one or both of a filler or an ultraviolet absorber, further preferably also includes one or both of a foaming agent or an environmentally friendly plasticizer, and more preferably also includes one or both of a chain extender, an anti-hydrolysis agent, an antioxidant or a thermal stabilizer.

[0061] Preferably, in the base fabric layer, the added mass of the chain extender is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-3%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.9%, 2%, 2.1%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0062] Preferably, in the filling layer, the added mass of the chain extender is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-3.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 2.2%, 2.3%, 2.4%, 3%, 3.1%, 3.5%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0063] Preferably, in the foaming layer, the added mass of the chain extender is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-4.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 2.9%, 3%, 3.1%, 4%, 4.1%, 4.2%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%.

[0064] Preferably, in the simulation layer, the added mass of the chain extender is 0%-10% of the PHA substrate, preferably 0.1%-5%, and further preferably any value in the range of 1%-3.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 2.2%, 2.3%, 2.4%, 2.5%, 2.9%, 3%, 3.1%, 3.5%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0065] The chain extender includes but is not limited to one or more of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, dimethylolpropionic acid, dimethyldiallylammonium chloride, 1,4-butanediol, BASF ADR 4400 or BASF ADR 4468.

[0066] In a specific embodiment of the present invention, the chain extenders in the base fabric layer, filling layer, foaming layer and / or simulation layer of the artificial leather are sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, dimethylolpropionic acid (DMPA) and BASF ADR 4400, and the mass ratio of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, dimethylolpropionic acid (DMPA) and BASF ADR 4400 is 3:3:4.

[0067] In a specific embodiment of the present invention, the chain extender in the base fabric layer, filling layer, foaming layer and / or simulation layer of the artificial leather is sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 1,4-butanediol and BASF ADR 4468, and the mass ratio of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 1,4-butanediol and BASF ADR 4468 is 3:2:5.

[0068] In a specific embodiment of the present invention, the chain extender in the base fabric layer, filling layer, foaming layer and / or simulation layer of the artificial leather is dimethyldiallyl ammonium chloride (DMDAAC), dimethylolpropionic acid (DMPA) and BASF ADR 4400, and the mass ratio of dimethyldiallyl ammonium chloride (DMDAAC), dimethylolpropionic acid (DMPA) and BASF ADR 4400 is 2:3:5.

[0069] In a specific embodiment of the present invention, the chain extender in the base fabric layer, filling layer, foaming layer and / or simulation layer of the artificial leather is dimethyldiallyl ammonium chloride (DMDAAC), 1,4-butanediol and BASF ADR 4468, and the mass ratio of dimethyldiallyl ammonium chloride (DMDAAC), 1,4-butanediol and BASF ADR 4468 is 2:1:2.

[0070] Preferably, in the base fabric layer, the added mass of the environmentally friendly plasticizer is 0%-10% of the PHA substrate, preferably 0.1%-5%, and further preferably any value in the range of 1%-2.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.9%, 2%, 2.1%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0071] Preferably, in the filling layer, the added mass of the environmentally friendly plasticizer is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.9%, 2%, 2.2%, 2.3%, 2.4%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0072] Preferably, in the foaming layer, the added mass of the environmentally friendly plasticizer is 0%-10% of the PHA substrate, preferably 0.1%-10%, and more preferably any value in the range of 1%-8%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 6.6%, 6.7%, 6.8%, 7%, 7.1%, 8%, 9%, 10%.

[0073] Preferably, in the simulation layer, the added mass of the environmentally friendly plasticizer is 0%-10% of the PHA substrate, preferably 0.1%-5%, and further preferably any value in the range of 1%-3.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 2.9%, 3%, 3.1%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0074] The environmentally friendly plasticizer includes but is not limited to one or both of acetyl tributyl citrate and 2,2,4-trimethyl-1,3-pentanediol diisobutyrate.

[0075] In a specific embodiment of the present invention, the environmentally friendly plasticizer is acetyl tributyl citrate.

[0076] In a specific embodiment of the present invention, the environmentally friendly plasticizer is 2,2,4-trimethyl-1,3-pentanediol diisobutyrate.

[0077] Preferably, in the base fabric layer, the added mass of the anti-hydrolysis agent is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value between 1% and 2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.5%, 1.6%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0078] Preferably, in the filling layer, the added mass of the anti-hydrolysis agent is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.47%, 1.48%, 1.49%, 1.5%, 1.56%, 1.6%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0079] Preferably, in the foaming layer, the added mass of the anti-hydrolysis agent is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.47%, 1.48%, 1.49%, 1.5%, 1.56%, 1.6%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0080] Preferably, in the simulation layer, the added mass of the anti-hydrolysis agent is 0%-10% of the PHA substrate, preferably 0.1%-5%, and further preferably any value between 1% and 2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.47%, 1.48%, 1.49%, 1.5%, 1.56%, 1.6%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0081] Preferably, the anti-hydrolysis agent includes, but is not limited to, one or more of anti-hydrolysis agent HYY-003, bis(2,6-diisopropylbenzene)carbodiimide or anti-hydrolysis agent HD900A.

[0082] In a specific embodiment of the present invention, the anti-hydrolysis agent in the base fabric layer, the filling layer, the foaming layer and the simulation layer is the anti-hydrolysis agent HYY-003.

[0083] In a specific embodiment of the present invention, the anti-hydrolysis agent in the artificial leather is anti-hydrolysis agent HYY-003 and anti-hydrolysis agent HD900A, and the mass ratio of anti-hydrolysis agent HYY-003 and anti-hydrolysis agent HD900A in the base fabric layer is 1:2; the anti-hydrolysis agent in the filling layer, foaming layer and simulation layer is anti-hydrolysis agent HYY-003 and anti-hydrolysis agent HD900A, and the mass ratio of anti-hydrolysis agent HYY-003 and anti-hydrolysis agent HD900A is 3:7.

[0084] In a specific embodiment of the present invention, the anti-hydrolysis agent in the artificial leather is an anti-hydrolysis agent HYY-003 and bis(2,6-diisopropylbenzene)carbodiimide, and the mass ratio of the anti-hydrolysis agent HYY-003 and bis(2,6-diisopropylbenzene)carbodiimide in the base fabric layer is 1:2. The anti-hydrolysis agent in the filling layer, foaming layer and simulation layer is an anti-hydrolysis agent HYY-003 and bis(2,6-diisopropylbenzene)carbodiimide, and the mass ratio of the anti-hydrolysis agent HYY-003 and bis(2,6-diisopropylbenzene)carbodiimide is 3:7.

[0085] In a specific embodiment of the present invention, the anti-hydrolysis agents in the base fabric layer, filling layer, foaming layer and simulation layer are bis(2,6-diisopropylbenzene)carbodiimide and anti-hydrolysis agent HD900A, and the mass ratio of bis(2,6-diisopropylbenzene)carbodiimide and anti-hydrolysis agent HD900A is 3:2.

[0086] Preferably, in the base fabric layer, the added mass of the antioxidant is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.9%, 2%, 2.1%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0087] Preferably, in the filling layer, the added mass of the antioxidant is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value between 1% and 2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.8%, 1.9%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0088] Preferably, in the foaming layer, the added mass of the antioxidant is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.47%, 1.48%, 1.49%, 1.5%, 1.56%, 1.6%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0089] Preferably, in the simulation layer, the added mass of the antioxidant is 0%-10% of the PHA substrate, preferably 0.1%-5%, and further preferably any value between 1% and 2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.4%, 1.47%, 1.48%, 1.49%, 1.5%, 1.56%, 1.6%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0090] Preferably, the antioxidant includes but is not limited to one or more of antioxidant 2777, tris(2,4-di-tert-butylphenyl) phosphite or antioxidant S-9228.

[0091] In a specific embodiment of the present invention, the antioxidant is antioxidant 2777.

[0092] In a specific embodiment of the present invention, the antioxidant is tris(2,4-di-tert-butylphenyl) phosphite.

[0093] In a specific embodiment of the present invention, the antioxidant is antioxidant S-9228.

[0094] Preferably, in the base fabric layer, the added mass of the heat stabilizer is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-3%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 2.4%, 2.5%, 2.6%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0095] Preferably, in the filling layer, the added mass of the heat stabilizer is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.8%, 1.83%, 1.87%, 1.9%, 1.95%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0096] Preferably, in the foaming layer, the added mass of the heat stabilizer is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.8%, 1.83%, 1.87%, 1.9%, 1.95%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0097] Preferably, in the simulation layer, the added mass of the heat stabilizer is 0%-10% of the PHA substrate, preferably 0.1%-5%, and more preferably any value in the range of 1%-2.5%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 2%, 2.2%, 2.3%, 2.4%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0098] Preferably, the thermal stabilizer includes but is not limited to one or more of stearate, nanocellulose or fumed nanosilica.

[0099] In a specific embodiment of the present invention, the heat stabilizers in the artificial leather are zinc stearate and fumed nano-silica, the mass ratio of zinc stearate and fumed nano-silica in the base fabric layer, filling layer and foaming layer is 2:3; the mass ratio of zinc stearate and fumed nano-silica in the simulation layer is 1:2.

[0100] In a specific embodiment of the present invention, the heat stabilizers in the artificial leather are nanocellulose and fumed nanosilica, the mass ratio of nanocellulose and fumed nanosilica in the base fabric layer, filling layer and foaming layer is 9:16; the mass ratio of nanocellulose and fumed nanosilica in the simulation layer is 1:2.

[0101] In a specific embodiment of the present invention, the heat stabilizers in the base fabric layer, the filling layer, the foaming layer and the simulation layer are calcium stearate and nanocellulose, and the mass ratio of the calcium stearate to the nanocellulose is 3:2.

[0102] In a specific embodiment of the present invention, the heat stabilizers in the artificial leather are zinc stearate and fumed nano-silica, the mass ratio of zinc stearate and fumed nano-silica in the base fabric layer, filling layer and foaming layer is 2:3; the mass ratio of zinc stearate and fumed nano-silica in the simulation layer is 1:2.

[0103] Preferably, the foaming layer of the artificial leather further contains a foaming agent.

[0104] Preferably, in the foaming layer, the added mass of the foaming agent is 0%-10% of the PHA substrate, preferably 0.1%-10%, and more preferably any value in the range of 1%-6%, for example, 0.00001%, 0.1%, 0.2%, 0.5%, 1%, 1.8%, 1.9%, 2%, 3%, 4%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 6%, 7%, 8%, 9%, 10%.

[0105] Preferably, the foaming agent includes but is not limited to one or more of azodicarbonamide, foaming agent SP1000C, leather foaming agent HF-800, sodium bicarbonate or ammonium bicarbonate.

[0106] In a specific embodiment of the present invention, the foaming agent is azodicarbonamide, leather foaming agent HF-800 and sodium bicarbonate, and the mass ratio of azodicarbonamide, leather foaming agent HF-800 and sodium bicarbonate is 15:8:12.

[0107] In a specific embodiment of the present invention, the foaming agent is azodicarbonamide, foaming agent SP1000C and ammonium bicarbonate, and the mass ratio of azodicarbonamide, foaming agent SP1000C and ammonium bicarbonate is 15:12:8.

[0108] Preferably, in the base fabric layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (3-7): (1-3): 1; preferably any value in (4-6): (1.5-2): 1, for example, 3:1:1, 3:1.5:1, 3:2:1, 3:2.5:1, 3:3:1, 4:1:1, 4:1.5:1, 4:2:1, 4:2.5:1, 4:3:1, 4.8:1.95:1, 5:1:1, 5:1.5:1, 5:1.75:1, 5:2:1, 5:2.5:1, 5:3:1, 5.1:1.65:1, 5.4:1.35:1, 6:1:1, 6:1.5:1, 6:2:1, 6:2.5:1, 6:3:1, 7:1:1, 7:1.5:1, 7:2:1, 7:2.5:1, 7:3:1.

[0109] Preferably, in the filling layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (2-6): (1-3): 1; preferably any value of (3-6): (1-2): 1, for example, 2:1:1, 2:1.5:1, 2:2:1, 2:2.5:1, 2:3:1, 3:1:1, 3:1.5:1, 3:2:1, 3:2.5:1, 3:3:1, 4:1:1, 4:1.5: 1, 4:2:1, 4:2.5:1, 4:3:1, 4.57:1.86:1, 4.76:1.66:1, 4.76:1.67:1, 4.86:1.57:1, 5:1:1, 5:1.5:1, 5:2:1, 5:2.5:1, 5:3:1, 5.14:1.29:1, 6:1:1, 6:1.5:1, 6:2:1, 6:2.5:1, 6:3:1.

[0110] Preferably, in the foaming layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (2-6): (1-3): 1; preferably any value of (3-6): (1-2): 1, for example, 2:1:1, 2:1.5:1, 2:2:1, 2:2.5:1, 2:3:1, 3:1:1, 3:1.5:1, 3:2:1, 3:2.5:1, 3:3:1, 4:1:1, 4:1.5: 1, 4:2:1, 4:2.5:1, 4:3:1, 4.57:1.86:1, 4.76:1.66:1, 4.76:1.67:1, 4.86:1.57:1, 5:1:1, 5:1.5:1, 5:2:1, 5:2.5:1, 5:3:1, 5.14:1.29:1, 6:1:1, 6:1.5:1, 6:2:1, 6:2.5:1, 6:3:1.

[0111] Preferably, in the simulation layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (4-10): (1-3): 1; preferably any value in (5-9): (1.5-2.8): 1, for example, 4:1:1, 4:1.5:1, 4:2:1, 4:2.5:1, 4:3:1, 5:1:1, 5:1.5:1, 5:2:1, 5:2.5:1, 5:3:1, 6:1:1, 6:1.5:1, 6:2:1, 6:2.5:1, 6:3:1 :1, 6.4:2.6:1, 6.66:2.34:1, 6.68:2.32:1, 6.8:2.2:17:1:1, 7:1.5:1, 7:2:1, 7:2.5:1, 7:3:1, 8:1:1, 8:1.5:1, 8:2:1, 8:2.5:1, 8:3:1, 9:1:1, 9:1.5:1, 9:2:1, 9:2.25:1, 9:2.8:1, 9:3:1, 10:1:1, 10:2:1, 10:3:1.

[0112] Preferably, the artificial leather can be prepared by any preparation method in the prior art.

[0113] A second aspect of the present invention provides an artificial leather, wherein the raw materials of the artificial leather include a substrate, the substrate includes a PHA substrate; and the artificial leather includes a filling layer.

[0114] Preferably, the artificial leather further comprises one, two or three of a foaming layer, a base fabric layer or a simulation layer.

[0115] Preferably, at least one of the filling layer, foaming layer, base fabric layer or simulation layer comprises a PHA substrate.

[0116] Preferably, the raw materials further comprise a non-PHA substrate.

[0117] Preferably, the raw materials further include auxiliary materials.

[0118] Preferably, the relevant definitions of the raw materials, PHA substrate, non-PHA substrate, auxiliary materials, filling layer, foaming layer, base fabric layer and / or simulation layer of the artificial leather are the same as those in the first aspect of the present invention.

[0119] The third aspect of the present invention provides a method for preparing artificial leather.

[0120] Preferably, the artificial leather comprises a base fabric layer, a filling layer, a foaming layer and / or a simulation layer.

[0121] Further preferably, the raw material of at least one of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer includes a substrate, and more preferably, the substrate includes a PHA substrate.

[0122] Preferably, the substrate further includes a non-PHA substrate.

[0123] More preferably, the raw materials also include auxiliary materials.

[0124] Preferably, the types and addition amounts of the PHA substrate, non-PHA substrate and auxiliary materials are the same as those defined in the first aspect.

[0125] Preferably, the preparation method includes preparing a base fabric layer, a filling layer, a foaming layer and / or a simulation layer.

[0126] The preparation of the base fabric layer comprises:

[0127] A1: Mix the raw materials, melt them, cool them and granulate them to obtain fiber-specific granules;

[0128] A2: The fiber pellets are melt-extruded and then formed into filaments or non-woven fabrics to form the base fabric layer. Preferably, the forming process includes a web reinforcement forming process, which includes various spinnerets, a spinning process, and subsequent drafting and winding, or hydroentanglement, needle punching, etc.

[0129] Preferably, the step A2 further comprises unwinding the filaments and obtaining the base fabric through a knitting or weaving process.

[0130] The preparation of the filling layer comprises:

[0131] B1: Mix the raw materials, melt them, cool them and granulate them to obtain granules for the filling layer;

[0132] B2: The filling layer is obtained by melting the pellets specially used for the filling layer and casting the melt into a film.

[0133] The preparation of the foaming layer comprises:

[0134] C1: Mix the raw materials, plasticize and then calender into a film to obtain a foam layer.

[0135] The preparation of the simulation layer comprises:

[0136] D1: Mix the raw materials, melt them, cool them and granulate them to obtain granules for the simulation layer;

[0137] D2: The special pellets for the simulation layer are melted and cast into a film to obtain the simulation layer.

[0138] Preferably, the raw materials include a PHA substrate, more preferably also include a non-PHA substrate, and more preferably also include auxiliary materials.

[0139] Preferably, the melting described in A1, A2, B1, B2 and / or D1 includes using a twin-screw extruder, and the reaction temperature is 120-230°C, preferably any value in the range of 150-215°C, for example 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 215, 220, 230°C.

[0140] Preferably, the cooling described in A1, B1 and / or D1 includes using water cooling or air cooling.

[0141] Further preferably, the air cooling includes side blowing or annular blowing.

[0142] More preferably, the air cooling is annular air, and the air supply temperature is 15-70°C, preferably any value in the range of 18-65°C, for example, 15, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70°C.

[0143] Preferably, the weight of the base fabric A2 is 20-450g / m 2 ; preferably 30-400g / m 2 any value, such as 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 350, 400, 450 g / m 2 .

[0144] Preferably, the weight of the non-woven fabric in A2 is 20-450 g / m 2 ; preferably 30-400g / m 2 any value, such as 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 350, 400, 450 g / m 2 .

[0145] Preferably, the casting temperature of B2 and D2 is 120-230°C, preferably any value in the range of 150-215°C, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 215, 220, 230°C.

[0146] Preferably, the thickness of the cast film obtained by the cast film forming process B2 is 60-800 μm, preferably any value in the range of 70-700 μm, for example, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, 340, 350, 360, 370, 380, 390, 400, 500, 600, 700, 800 μm.

[0147] Preferably, the thickness of the cast film obtained by the cast film forming in D2 is 30-500 μm, preferably any value in the range of 35-420 μm, for example, 30, 35, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 175, 180, 190, 200, 300, 400, 420, 500 μm.

[0148] Preferably, the plasticizing described in C1 includes using a twin-screw extruder, and the plasticizing temperature is 100-200°C, preferably any value in the range of 120-195°C, for example, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 195, 200°C.

[0149] Preferably, the foaming temperature described in C1 is 40-150°C, preferably any value in the range of 40-105°C, for example, 40, 50, 60, 70, 80, 90, 100, 105, 110, 120, 130, 140, 150°C.

[0150] The foaming time is 10-50 min, preferably any value between 15-30 min, for example, 10, 15, 20, 25, 30, 35, 40, 45, 50 min.

[0151] Preferably, the thickness of the foamed layer obtained in C1 is 200-3500 μm, preferably any value in the range of 280-3000 μm, for example, 200, 280, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 2000, 2500, 3000, 3500 μm.

[0152] Preferably, the preparation method further comprises laminating the base fabric layer, the filling layer, the foaming layer and / or the simulation layer.

[0153] Preferably, the compounding includes heating, and the heating temperature is 50-150°C, preferably any value in the range of 60-110°C, for example, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150°C.

[0154] In a specific embodiment of the present invention, the preparation method comprises:

[0155] Preparation of base fabric layer:

[0156] A1: 45-90 parts (preferably any value between 50-80 parts, such as 45, 50, 55, 60, 65, 67.5, 70, 75, 80, 85, 90 parts) of base material and 0-20 parts (preferably any value between 8-12 parts, such as 0, 5, 10, 15, 20 parts) of auxiliary material are weighed and mixed, melted and cooled into granules by a twin-screw extruder, wherein the barrel temperature is set to 120-230°C (preferably any value among 150-215 ℃, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 215, 220, 230 ℃), using ring blowing, the air supply temperature is 15-70 ℃ (preferably any value among 18-65 ℃, for example, 15, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70 ℃), to obtain fiber-specific pellets;

[0157] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 20-450g / m 2 (Preferably 30-400g / m 2 any value, such as 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 350, 400, 450 g / m 2 );

[0158] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a weight of 20-450g / m 2 (Preferably 30-400g / m 2any value, such as 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 350, 400, 450 g / m 2 )'s PHA base fabric, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0159] Prepare the filling layer and laminate the filling layer with the base fabric layer:

[0160] B1: 60-120 parts (preferably any value between 80-100 parts, such as 60, 70, 80, 90, 100, 110, 120 parts) of base material and 0-28 parts (preferably any value between 12-16 parts, such as 0, 5, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28 parts) of auxiliary material were weighed and mixed, melted and cooled by a twin-screw extruder to form granules, wherein the barrel temperature was set at 120-23 0°C (preferably any value in the range of 150-215°C, such as 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 215, 220, 230°C), using ring blowing, with an air supply temperature of 15-70°C (preferably any value in the range of 18-65°C, such as 15, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70°C), to obtain special granules for the filling layer;

[0161] B2: The pellets for the filling layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. The film is then tightly compounded with the preheated PHA base fabric layer by a three-roll setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled to be 50-150°C (preferably any value in the range of 60-110°C, such as 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150°C), and the casting temperature is controlled to be 120-230°C (preferably any value in the range of 150-215°C, such as 120, 130, 140, 150, 160, , 300, 310, 320, 330, 340, 350, 360, 370, 380, 390, 400, 500, 600, 700, 800 μm).

[0162] Prepare the foam layer and laminate it with the base fabric layer / filling layer:

[0163] C1: Weigh 60-120 parts (preferably any value between 80-100 parts, such as 60, 70, 80, 90, 100, 110, 120 parts) of base material and 0-28 parts (preferably any value between 12-16 parts, such as 0, 5, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28 parts) of auxiliary material by mass, mix and dry, and inject into a twin-screw extruder with a heating device. Plasticizing, through calendering film forming, is the foaming layer, through the three-roll shaping machine to make it and the pre-heated PHA base cloth / filling layer tightly compounded together, the foaming layer close to the filling layer, because the two layers of main materials are the same, no adhesive is required, and then sent to the foaming furnace for foaming, wherein the plasticizing temperature is 100-200 ° C (preferably any value in the range of 120-195 ° C, for example 100, 110, 120, 130, 140, 150, 1 60, 170, 180, 190, 195, 200°C), the preheating temperature is 50-150°C (preferably any value in the range of 60-110°C, for example, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150°C), the foaming temperature is 40-150°C (preferably any value in the range of 40-105°C, for example, 40, 50, 60, 70, 80, 90 , 100, 105, 110, 120, 130, 140, 150°C), the foaming time is 10-50 min (preferably 15-30 min, for example 10, 15, 20, 25, 30, 35, 40, 45, 50 min), and the final thickness of the foamed layer after expansion and cooling is 200-3500 μm (preferably any value in the range of 280-3000 μm, for example 200, 280, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 2000, 2500, 3000, 3500 μm).

[0164] Prepare the simulation layer and laminate it with the base fabric layer / filling layer / foaming layer:

[0165] D1: 30-60 parts (preferably any value between 40-50 parts, such as 30, 35, 40, 45, 50, 55, 60 parts) of base material and 0-12 parts (preferably any value between 4-8 parts, such as 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 parts) of auxiliary material were weighed and mixed, melted and cooled into granules by a twin-screw extruder, wherein the barrel temperature was set to 120-230°C (preferably any value among 150-215 ℃, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 215, 220, 230 ℃), adopting ring blowing, the air supply temperature is 15-70 ℃ (preferably any value among 18-65 ℃, for example, 15, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70 ℃), to obtain special granules for simulation layer;

[0166] D2: The artificial layer pellets are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The artificial layer is formed by casting. The artificial layer is tightly compounded with the preheated PHA base fabric / filling / foaming layer by a three-roll setting machine. The artificial layer is close to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled to be 50-150°C (preferably any value between 60-110°C, such as 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150°C), and the casting temperature is 120-230°C The casting film thickness is 30-500 μm (preferably any value in the range of 150-215°C, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 215, 220, 230°C), and the casting film thickness is 30-500 μm (preferably any value in the range of 35-420 μm, for example, 30, 35, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 175, 180, 190, 200, 300, 400, 420, 500 μm).

[0167] The fourth aspect of the present invention provides an artificial leather obtained by the above preparation method.

[0168] A fifth aspect of the present invention provides an application of the artificial leather and / or the artificial leather prepared by the above preparation method.

[0169] Preferably, the application includes application in the manufacture of leather products, simulated skin or antibacterial wound dressings; further preferably, the leather products include automobile interiors, leather furniture, leather shoes, and leather clothing.

[0170] The term "include" or "comprising" in the present invention is an open description containing the specified components or steps described, as well as other specified components or steps that do not substantially affect them.

[0171] The term "and / or" in this invention includes all combinations of the items connected by the term, and each combination should be considered to have been listed separately herein. For example, "A and / or B" includes "A," "A and B," and "B." For another example, "A, B and / or C" includes "A," "B," "C," "A and B," "A and C," "B and C," and "A and B and C."

[0172] Beneficial effects of the present invention:

[0173] 1. The artificial leather of the present invention is mainly made of environmentally friendly and degradable PHA. From raw materials to production, use, recycling or disposal, no solvents or adhesives are required and it can be fully degraded in the natural environment, truly achieving environmental friendliness throughout its entire life cycle. It not only avoids the slaughter of animals and damage to the ecological environment caused by traditional leather, but also has the advantages of environmental degradation and high recycling rate that ordinary artificial leather does not have.

[0174] 2. By adjusting the type and ratio of the substrates and leveraging the excellent biophilic, hydrophobic, antibacterial, and dye-friendly properties of PHA, the present invention achieves an artificial leather that is soft to the touch, elastic, and skin-friendly, while also being antibacterial, mildew-resistant, waterproof, breathable, and easily dyeable. In particular, the rational blending of P34HB with other PHA types ensures that the PHA artificial leather combines a soft feel with strong mechanical properties. The dominant role of PHA over other degradable substrates also improves the overall degradation rate and dyeing performance. The preparation process eliminates the need for the addition of fluorine- or silicon-containing hydrophobic treatment agents; the ideal waterproofing effect is achieved solely through the natural hydrophobicity of PHA as an ester.

[0175] 3. The artificial leather of the present invention unexpectedly discovered through experiments that the 4HB content in P34HB and the amount of P34HB added significantly affect the foaming effect. Specifically, within a certain range, reducing the 4HB content or the amount of P34HB added can achieve a lower foam density and a higher expansion coefficient. However, considering that increasing the 4HB content or the amount of P34HB added can improve the softness of artificial leather, the 4HB content in P34HB and the amount of P34HB added have a relatively narrow applicable range. Experiments have shown that both excessively high and low 4HB content or the amount of P34HB added can affect the overall performance of the artificial leather. Furthermore, increasing the expansion coefficient within a certain range can improve sound insulation.

[0176] 4. The artificial leather of the present invention comprises four layers of PHA: a base fabric layer, a filling layer, a foam layer, and a simulation layer. The base fabric layer can be made of non-woven, knitted, or woven fabrics of varying weights, combined with filling and foam layers of varying thicknesses. This allows for a wide range of leather applications, including automotive interiors, furniture, leather shoes and clothing, and decorative items. Because all four layers are primarily made of PHA, the layers are tightly bonded, resulting in high peel strength. This eliminates the need for adhesives, further enhancing environmental friendliness.

[0177] 5. The artificial leather of the present invention adopts a special foaming process. Conventional foaming processes generally require the addition of solvents, even volatile solvents, to produce resins, and the foaming furnace generally performs the majority of the foaming process rather than micro-foaming. The method described in the present invention does not add solvents or use resins containing volatile solvents. Due to the addition of chain extenders, anti-hydrolysis agents, antioxidants, thermal stabilizers, etc., the melt strength is greatly improved, so that the material after plastication has the characteristics of non-open macroporous foaming, and the foam is unlikely to break due to low melt strength. Combined with the microporous foaming caused by the subsequent foaming furnace, the foam layer has a low foam density, a high expansion coefficient, and fine foam pores, ensuring the soft feel, resilience and breathability of the finished artificial leather.

[0178] 6. The artificial leather of the present invention has an appropriate mass ratio of the "base fabric layer (fiber material)" to the "filling layer + foaming layer + simulation layer (elastic material)" within a range of (1:5) to (2:5). If the base fabric ratio is too low, the artificial leather will have a rubber-like quality; if the base fabric ratio is too high, the artificial leather will have a paper-like quality, failing to achieve the desired simulation effect that can replace natural leather.

[0179] 7. The artificial leather of the present invention uses roughly the same raw materials for each layer, but with different proportions. For example, the base fabric layer contains an appropriate amount of natural plant fiber, the filling layer contains more filler, and the foaming layer contains more flexible substances (such as foaming agents and / or environmentally friendly plasticizers, etc.). Only in this way can the layers be tightly and firmly attached to each other while possessing their own characteristics, forming a differentiated structure, and ultimately making the PHA artificial leather product have many excellent properties and functions.

[0180] 8. The artificial leather of this invention, whose raw materials for each layer are primarily PHA, has unexpectedly been found to possess self-healing properties (high folding strength) during use. This means that minor scratches on the surface can be removed by applying grease, wiping, or simply relaxing and storing. This may be related to its inherent degradation properties and lipophilic and biophilic properties, resulting in a longer lifespan and greater cost-effectiveness.

[0181] 9. The artificial leather of the present invention comprises an anti-UV agent compounded with nano-scale inorganic powder, which is more environmentally friendly than organic UV absorbers. Furthermore, the addition of fillers and UV absorbers unexpectedly provides sound insulation, further expanding its application. Analysis suggests this is likely due to the uniform dispersion and interaction of the micron-scale fillers and nano-scale UV absorbers within the base fabric and filling layers, filling gaps and forming a dense sound-insulating structure. Furthermore, the nano-scale UV absorbers, combined with the loose structure of the foaming layer, cause sound to be continuously reflected by the two outermost layers, resulting in sound energy loss and thus achieving the sound-isolating effect.

[0182] The abbreviations and full names of the present invention are shown in Table 1:

[0183] Table 1 BRIEF DESCRIPTION OF THE DRAWINGS

[0184] Figure 1: Schematic diagram of artificial leather, where 1 is the base fabric layer, 2 is the filling layer, 3 is the foaming layer, and 4 is the simulation layer. DETAILED DESCRIPTION

[0185] Performance testing method:

[0186] (1) Softness: A subjective evaluation method was used, and two groups of people were selected as subjects.

[0187] A group of 10 experts or experienced test subjects, with a weight of 1. They are familiar with the scales and descriptive terms used in subjective testing, and are clear about the human sensation corresponding to each level in the terminology. They can quickly and accurately evaluate and quantify the performance of artificial leather;

[0188] The other group consisted of 10 consumers who had undergone simple training, with a weight of 0.5. Before the experiment, these subjects needed to be informed about the performance of artificial leather and the terminology of the evaluation scale to enable them to make accurate evaluations of the performance of artificial leather and ensure the rigor of the results.

[0189] Experimental conditions: temperature 20℃±2℃, relative humidity 65%±2%, wind speed ≤0.1m / s.

[0190] The softness performance evaluation scale and description vocabulary are shown in Table 2.

[0191] Table 2: Subjective evaluation scale for softness

[0192] (2) Foam density: the density of the foaming layer after foaming, which can be calculated by the ratio of the mass to volume of the foaming layer after foaming.

[0193] (3) Expansion coefficient: It can be calculated by the ratio of the density of the foaming layer before foaming to the density after foaming.

[0194] Some of the materials used in this invention come from:

[0195] Hollow glass microspheres: purchased from Zhongke Huaxing New Materials Co., Ltd., product number: C30;

[0196] Mica powder: purchased from Shijiazhuang Huabang Mineral Products Co., Ltd., product number: white, 1250 mesh;

[0197] Talc: purchased from Langfang Yinma Pigment Co., Ltd., product number: YM-T160;

[0198] Nano ZnO: purchased from Beijing Dekedaojin Technology Co., Ltd., product number: DK-ZnO-30;

[0199] Rutile TiO2: purchased from Langfang Yinma Pigment Co., Ltd., product number: YMR-505;

[0200] Nano-CeO2: purchased from Beijing Dekedaojin Technology Co., Ltd., product number: DK-CeO2-20;

[0201] Sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., purity: 99%;

[0202] Dimethylolpropionic acid (DMPA): purchased from Mitsui Chemicals (Shandong) Co., Ltd., purity: superior grade, 99%;

[0203] Dimethyldiallylammonium chloride (DMDAAC): purchased from Hubei Shuangyan Chemical Co., Ltd., product number: GY172;

[0204] 2,2,4-Trimethyl-1,3-pentanediol diisobutyrate: purchased from Zhongshan Dixin Chemical Co., Ltd., product number: viscosity reducer TXIB;

[0205] Anti-hydrolysis agent HYY-003: purchased from Shenzhen Heyanyuese Plastic Pigment Additive Co., Ltd.

[0206] Anti-hydrolysis agent HD900A: purchased from Ningbo Hengze Chemical Co., Ltd.

[0207] Bis(2,6-diisopropylbenzene)carbodiimide: purchased from Wuhan Chengtian Fine Chemical Co., Ltd.

[0208] Antioxidant 2777: purchased from Cytec Corporation, USA, product number: Cytec 2777;

[0209] Tris(2,4-di-tert-butylphenyl) phosphite: purchased from Guangzhou Ruishi Biotechnology Co., Ltd.

[0210] Antioxidant S-9228: purchased from Dover Chemical, USA;

[0211] Nanocellulose: purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., product number: CNF, 20-50 nm;

[0212] Fumed nano-silica: purchased from Hubei Huifu Nanomaterials Co., Ltd., product number: HL-200;

[0213] Foaming agent SP1000C: purchased from: Zhejiang Shuntai Rubber and Plastic Technology Co., Ltd.

[0214] Leather foaming agent HF-800: purchased from Yancheng Zhongmai Rubber and Plastic Products Co., Ltd.

[0215] The various PHAs used in the present invention were sourced from Beijing Microstructure Biotechnology Co., Ltd.

[0216] Example 1: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather

[0217] A1: 30 parts by mass of PHB, 20 parts of P34HB (4HB content: 16 mol%), 4.5 parts of black tea fiber, 3 parts of mulberry fiber, 10 parts of PBS, 4 parts of mica powder, 0.3 part of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.3 part of dimethylolpropionic acid (DMPA), 0.4 part of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.4 part of nano-ZnO, 0.6 part of rutile TiO2, 0.75 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 part of zinc stearate, and 0.75 part of fumed nano-silica were mixed, melted, and cooled to form pellets in a twin-screw extruder. The barrel temperature was set at 160-205°C, and an annular blower was used with an air supply temperature of 18-65°C to obtain fiber-specific pellets.

[0218] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 30-400g / m 2 between;

[0219] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a gram weight of 30-400 g / m 2 The PHA base fabric between, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0220] B1: 40 parts by mass of PHB, 26.7 parts of P34HB (with a 4HB content of 16 mol%), 6 parts of black tea fiber, 4 parts of mulberry fiber, 13.3 parts of PBS, 6.5 parts of mica powder, 0.45 parts of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.45 parts of dimethylolpropionic acid (DMPA), 0.6 parts of BASF ADR 4400, 1.5 parts of acetyl tributyl citrate, 0.4 parts of nano-ZnO, 0.6 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1.25 parts of antioxidant 2777, 0.5 parts of zinc stearate, and 0.75 parts of fumed nano-silica were mixed, melted, and granulated by a twin-screw extruder. The barrel temperature was set to 160-205° C., and an annular blower was used with an air supply temperature of 18-65° C. to obtain pellets specifically for the filling layer.

[0221] B2: The special pellets for the filling layer are vacuum-dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. It is then tightly compounded with the preheated PHA base fabric layer through a three-roller setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled at 65-105℃, the casting temperature is 160-205℃, and the cast film thickness is 70-700μm.

[0222] C1: 40 parts by mass of PHB, 26.7 parts of P34HB (4HB content is 16 mol%), 6 parts of black tea fiber, 4 parts of mulberry fiber, 13.3 parts of PBS, 0.6 parts of sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.6 parts of dihydroxymethylpropionic acid (DMPA), 0.8 parts of BASF ADR 4400, 4.5 parts of acetyl tributyl citrate, 0.3 parts of nano-ZnO, 0.45 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 parts of zinc stearate, 0.75 parts of fumed nano-silica, 1.5 parts of azodicarbonamide, 0.8 parts of leather foaming agent HF-800, and 1.2 parts of sodium bicarbonate were weighed, mixed, dried, injected into a twin-screw extruder with a heating device for plastication, and formed into a film by calendaring. The foaming layer is tightly compounded with the preheated PHA base fabric / filling layer through a three-roller shaping machine. The foaming layer is close to the filling layer. Since the two layers are mainly made of the same material, no adhesive is required. Then it is sent to the foaming furnace for foaming. The plasticizing temperature is 120-195℃, the preheating temperature is 65-105℃, the foaming temperature is 45-100℃, and the foaming time is 15-30min. The final thickness of the foaming layer after expansion and cooling is 280-3000μm.

[0223] D1: 20 parts of PHB, 13.3 parts of P34HB (4HB content is 16 mol%), 3 parts of black tea fiber, 2 parts of mulberry fiber, 6.7 parts of PBS and 0.75 parts of mica powder, 0.3 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.3 parts of dihydroxymethyl propionic acid (DMPA), 0.4 parts of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.2 parts of nano ZnO, 0.3 parts of rutile TiO2, 0.5 parts of anti-hydrolysis agent HYY-003, 0.5 parts of antioxidant 2777, 0.25 parts of zinc stearate, and 0.5 parts of fumed nano-silica were mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature was set to 160-205 ° C, annular blowing was used, and the air supply temperature was 18-65 ° C to obtain granules specifically for the simulation layer;

[0224] D2: The special pellets for the simulation layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the simulation layer. It is then tightly compounded with the pre-heated PHA base fabric / filling / foaming layer through a three-roller setting machine. The simulation layer is closely attached to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The pre-heating temperature is controlled at 65-105℃, the casting temperature is 150-215℃, and the cast film thickness is 35-420μm.

[0225] D3: Emboss one side of the simulation layer by a method such as flat plate embossing or roller embossing, and then cool it to obtain a simulation pattern. The simulated leather is then dyed and rolled up to obtain PHA artificial leather.

[0226] The test results of various properties of the obtained artificial leather are shown in Table 3 below, and the schematic diagram of the prepared artificial leather is shown in Figure 1.

[0227] Table 3 Test data of PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather

[0228] Example 2: PHBV / P34HB+soy protein fiber+PLA+PBAT composite artificial leather

[0229] A1: Weigh 25 parts of PHBV (3HV content is 5 mol%), 25 parts of P34HB (4HB content is 12 mol%), 4.5 parts of soy protein fiber, 5 parts of PLA, 8 parts of PBAT and 4 parts of talc, 0.3 parts of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.2 parts of 1,4-butanediol, 0.5 parts of BASF ADR 4468, 1 part of acetyl tributyl citrate, 0.5 part of rutile TiO2, 0.5 part of nano-CeO2, 0.25 part of anti-hydrolysis agent HYY-003, 0.5 part of anti-hydrolysis agent HD900A, 1 part of tris(2,4-di-tert-butylphenyl) phosphite, 0.45 part of nano-cellulose, and 0.8 part of fumed nano-silica are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain fiber-specific granules;

[0230] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 30-400g / m 2 between;

[0231] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a gram weight of 30-400 g / m 2 The PHA base fabric between, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0232] B1: In parts by mass, weigh 33.3 parts of PHBV (3HV content is 5 mol%), 33.3 parts of P34HB (4HB content is 12 mol%), 6 parts of soy protein fiber, 6.7 parts of PLA, 10.7 parts of PBAT and 6.5 parts of talc, 0.45 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.3 parts of 1,4-butanediol, 0.75 parts of BASF ADR 4468, 1.5 parts of acetyl tributyl citrate, 0.5 parts of rutile TiO2, 0.5 parts of nano-CeO2, 0.3 parts of anti-hydrolysis agent HYY-003, 0.7 parts of anti-hydrolysis agent HD900A, 1.25 parts of tris(2,4-di-tert-butylphenyl) phosphite, 0.45 parts of nano-cellulose, and 0.8 parts of fumed nano-silica are mixed, melted and granulated by a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain special granules for the filling layer;

[0233] B2: The special pellets for the filling layer are vacuum-dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. It is then tightly compounded with the preheated PHA base fabric layer through a three-roller setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled at 65-105℃, the casting temperature is 160-205℃, and the cast film thickness is 70-700μm.

[0234] C1: Weigh 33.3 parts of PHBV (3HV content is 5 mol%), 33.3 parts of P34HB (4HB content is 12 mol%), 6 parts of soy protein fiber, 6.7 parts of PLA, 10.7 parts of PBAT and 0.6 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.4 parts of 1,4-butanediol, 1 part of BASF ADR 4468, 4.5 parts of acetyl tributyl citrate, 0.35 parts of rutile TiO2, 0.4 parts of nano CeO2, 0.3 parts of anti-hydrolysis agent HYY-003, 0.7 parts of anti-hydrolysis agent HD900A, 1 part of tris (2,4-di-tert-butylphenyl) phosphite, 0.45 parts of nano cellulose, 0.8 parts of fumed nano silica, 1.5 parts of azodicarbonamide, 1.2 parts of foaming agent SP1000C, 0.8 parts of ammonium bicarbonate were mixed and dried, and injected into a twin-screw extruder with a heating device. After leaving the machine, it is plasticated and formed into a film through calendering, which is the foaming layer. It is then tightly compounded with the pre-heated PHA base fabric / filling layer through a three-roller shaping machine. The foaming layer is close to the filling layer. Since the two layers are mainly made of the same material, no adhesive is required. It is then sent to the foaming furnace for foaming. The plasticating temperature is 120-195℃, the preheating temperature is 65-105℃, the foaming temperature is 45-100℃, and the foaming time is 15-30min. The final thickness of the foaming layer after expansion and cooling is 280-3000μm.

[0235] D1: In parts by mass, weigh 16.7 parts of PHBV (3HV content is 5 mol%), 16.7 parts of P34HB (4HB content is 12 mol%), 3 parts of soy protein fiber, 3.3 parts of PLA, 5.3 parts of PBAT, 0.75 parts of talc, 0.3 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.2 parts of 1,4-butanediol, 0.5 parts of BASF ADR 4468, 1 part of acetyl tributyl citrate, 0.25 part of rutile TiO2, 0.25 part of nano-CeO2, 0.15 part of anti-hydrolysis agent HYY-003, 0.35 part of anti-hydrolysis agent HD900A, 0.5 part of tris(2,4-di-tert-butylphenyl) phosphite, 0.25 part of nanocellulose, and 0.5 part of fumed nano-silica are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain granules specifically for the simulation layer;

[0236] D2: The special pellets for the simulation layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the simulation layer. It is then tightly compounded with the pre-heated PHA base fabric / filling / foaming layer through a three-roller setting machine. The simulation layer is closely attached to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The pre-heating temperature is controlled at 65-105℃, the casting temperature is 150-215℃, and the cast film thickness is 35-420μm.

[0237] D3: Emboss one side of the simulation layer by a method such as flat plate embossing or roller embossing, and then cool it to obtain a simulation pattern. The simulated leather is then dyed and rolled up to obtain PHA artificial leather.

[0238] The test results of various properties of the obtained artificial leather are shown in Table 4 below, and the schematic diagram of the prepared artificial leather is shown in Figure 1.

[0239] Table 4 Test data of PHBV / P34HB+soy protein fiber+PLA+PBAT composite artificial leather

[0240] Example 3: PHB / P34HB / PHBHHx+sugarcane fiber+PPC+PGA composite artificial leather

[0241] A1: 27 parts of PHB, 15 parts of P34HB (4HB content is 8 mol%), 9 parts of PHBHHx (3HHx content is 20 mol%), 4.5 parts of sugarcane fiber, 6 parts of PPC, 6 parts of PGA and 4 parts of hollow glass microspheres, 0.2 parts of dimethyldiallylammonium chloride (DMDAAC), 0.3 parts of dihydroxymethylpropionic acid (DMPA), 0.5 parts of BASF ADR 4400, 1 part of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.4 part of nano-ZnO, 0.6 part of nano-CeO2, 0.25 part of anti-hydrolysis agent HYY-003, 0.5 part of bis(2,6-diisopropylbenzene)carbodiimide, 1 part of antioxidant S-9228, 0.75 part of calcium stearate, and 0.5 part of nano-cellulose are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain fiber-specific granules;

[0242] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 30-400g / m 2 between;

[0243] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a gram weight of 30-400 g / m 2 The PHA base fabric between, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0244] B1: 36 parts of PHB, 20 parts of P34HB (4HB content is 8 mol%), 12 parts of PHBHHx (3HHx content is 20 mol%), 6 parts of sugarcane fiber, 8 parts of PPC, 8 parts of PGA and 6.5 parts of hollow glass microspheres, 0.3 parts of dimethyldiallylammonium chloride (DMDAAC), 0.45 parts of dihydroxymethylpropionic acid (DMPA), 0.75 parts of BASF ADR 4400, 1.5 parts of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.4 parts of nano-ZnO, 0.6 parts of nano-CeO2, 0.3 parts of anti-hydrolysis agent HYY-003, 0.7 parts of bis(2,6-diisopropylbenzene)carbodiimide, 1.25 parts of antioxidant S-9228, 0.75 parts of calcium stearate, and 0.5 parts of nano-cellulose are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is adopted, and the air supply temperature is 18-65°C to obtain granules specifically for the filling layer;

[0245] B2: The special pellets for the filling layer are vacuum-dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. It is then tightly compounded with the preheated PHA base fabric layer through a three-roller setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled at 65-105℃, the casting temperature is 160-205℃, and the cast film thickness is 70-700μm.

[0246] C1: 36 parts of PHB, 20 parts of P34HB (4HB content is 8 mol%), 12 parts of PHBHHx (3HHx content is 20 mol%), 6 parts of sugarcane fiber, 8 parts of PPC, 8 parts of PGA and 0.4 parts of dimethyldiallylammonium chloride (DMDAAC), 0.6 parts of dihydroxymethylpropionic acid (DMPA), 1 part of BASF ADR 4400, 4.5 parts of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.3 parts of nano ZnO, 0.45 parts of nano CeO2, 0.3 parts of anti-hydrolysis agent HYY-003, 0.7 parts of bis (2,6-diisopropylbenzene) carbodiimide, 1 part of antioxidant S-9228, 0.75 parts of calcium stearate, 0.5 parts of nano cellulose, 1.5 parts of azodicarbonamide, 1.2 parts of foaming agent SP1000C, and 0.8 parts of ammonium bicarbonate were mixed and dried, and injected into a double screw with a heating device. The rod extruder plasticizes and forms a film through calendering, which is the foaming layer. It is then tightly compounded with the preheated PHA base fabric / filling layer through a three-roller shaping machine. The foaming layer is close to the filling layer. Since the two layers are mainly made of the same material, no adhesive is required. The film is then sent to a foaming furnace for foaming. The plasticizing temperature is 120-195°C, the preheating temperature is 65-105°C, the foaming temperature is 45-100°C, the foaming time is 15-30min, and the final thickness of the foaming layer after expansion and cooling is 280-3000μm.

[0247] D1: 18 parts of PHB, 10 parts of P34HB (4HB content is 8 mol%), 6 parts of PHBHHx (3HHx content is 20 mol%), 3 parts of sugarcane fiber, 4 parts of PPC, 4 parts of PGA and 0.75 parts of hollow glass microspheres, 0.2 parts of dimethyldiallylammonium chloride (DMDAAC), 0.3 parts of dihydroxymethylpropionic acid (DMPA), 0.5 parts of BASF ADR 4400, 1 part of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.2 parts of nano-ZnO, 0.3 parts of nano-CeO2, 0.15 parts of anti-hydrolysis agent HYY-003, 0.35 parts of bis(2,6-diisopropylbenzene)carbodiimide, 0.5 parts of antioxidant S-9228, 0.45 parts of calcium stearate, and 0.3 parts of nano-cellulose are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain granules specifically for the simulation layer;

[0248] D2: The special pellets for the simulation layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the simulation layer. It is then tightly compounded with the pre-heated PHA base fabric / filling / foaming layer through a three-roller setting machine. The simulation layer is closely attached to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The pre-heating temperature is controlled at 65-105℃, the casting temperature is 150-215℃, and the cast film thickness is 35-420μm.

[0249] D3: Emboss one side of the simulation layer by a method such as flat plate embossing or roller embossing, and then cool it to obtain a simulation pattern. The simulated leather is then dyed and rolled up to obtain PHA artificial leather.

[0250] The test results of various properties of the obtained artificial leather are shown in Table 5 below, and the schematic diagram of the prepared artificial leather is shown in Figure 1.

[0251] Table 5 Test data of PHB / P34HB / PHBHHx+sugarcane fiber+PPC+PGA composite artificial leather

[0252] Example 4: PHBV / P34HB / PHBHHx+soy protein fiber+bamboo fiber+PBS composite artificial leather

[0253] A1: Weigh, by mass, 24 parts of PHBV (3HV content: 5 mol%), 12 parts of P34HB (4HB content: 10 mol%), 12 parts of PHBHHx (3HHx content: 8 mol%), 3 parts of soy protein fiber, 6 parts of bamboo fiber, 10.5 parts of PBS, 4 parts of mica powder, 0.4 parts of dimethyldiallylammonium chloride (DMDAAC), 0.2 parts of 1,4-butanediol, and 0.4 parts of BASF ADR 4468, 1 part of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.4 part of nano-ZnO, 0.6 part of rutile TiO2, 0.45 part of bis(2,6-diisopropylbenzene)carbodiimide, 0.3 part of anti-hydrolysis agent HD900A, 1 part of antioxidant 2777, 0.5 part of zinc stearate, and 0.75 part of fumed nano-silica are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain fiber-specific granules;

[0254] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 30-400g / m 2 between;

[0255] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a gram weight of 30-400 g / m 2 The PHA base fabric between, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0256] B1: In parts by mass, weigh 32 parts of PHBV (3HV content is 5 mol%), 16 parts of P34HB (4HB content is 10 mol%), 16 parts of PHBHHx (3HHx content is 8 mol%), 4 parts of soy protein fiber, 8 parts of bamboo fiber, 14 parts of PBS and 6.5 parts of mica powder, 0.6 parts of dimethyldiallylammonium chloride (DMDAAC), 0.3 parts of 1,4-butanediol, 0.6 parts of BASF ADR 4468, 1.5 parts of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.4 parts of nano-ZnO, 0.6 parts of rutile TiO2, 0.6 parts of bis(2,6-diisopropylbenzene)carbodiimide, 0.4 parts of anti-hydrolysis agent HD900A, 1.25 parts of antioxidant 2777, 0.5 parts of zinc stearate, and 0.75 parts of fumed nano-silica are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain granules specifically for the filling layer;

[0257] B2: The special pellets for the filling layer are vacuum-dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. It is then tightly compounded with the preheated PHA base fabric layer through a three-roller setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled at 65-105℃, the casting temperature is 160-205℃, and the cast film thickness is 70-700μm.

[0258] C1: 32 parts of PHBV (3HV content is 5 mol%), 16 parts of P34HB (4HB content is 10 mol%), 16 parts of PHBHHx (3HHx content is 8 mol%), 4 parts of soy protein fiber, 8 parts of bamboo fiber, 14 parts of PBS and 0.8 parts of dimethyldiallylammonium chloride (DMDAAC), 0.4 parts of 1,4-butanediol, 0.8 parts of BASF ADR 4468, 4.5 parts of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.3 parts of nano ZnO, 0.45 parts of rutile TiO2, 0.6 parts of bis(2,6-diisopropylbenzene)carbodiimide, 0.4 parts of anti-hydrolysis agent HD900A, 1 part of antioxidant 2777, 0.5 parts of zinc stearate, 0.75 parts of fumed nano silica, 1.5 parts of azodicarbonamide, 0.8 parts of leather foaming agent HF-800, and 1.2 parts of sodium bicarbonate were mixed and dried, and injected into a container with a heating device. The twin-screw extruder plasticizes and forms a film through calendaring, which is the foaming layer. It is then tightly compounded with the preheated PHA base fabric / filling layer through a three-roller shaping machine. The foaming layer is close to the filling layer. Since the two layers are mainly made of the same material, no adhesive is required. The film is then sent to a foaming furnace for foaming. The plasticizing temperature is 120-195°C, the preheating temperature is 65-105°C, the foaming temperature is 45-100°C, and the foaming time is 15-30 minutes. The final thickness of the foaming layer after expansion and cooling is 280-3000μm.

[0259] D1: In parts by mass, weigh 16 parts of PHBV (3HV content is 5 mol%), 8 parts of P34HB (4HB content is 10 mol%), 8 parts of PHBHHx (3HHx content is 8 mol%), 2 parts of soy protein fiber, 4 parts of bamboo fiber, 7 parts of PBS and 0.75 parts of mica powder, 0.4 parts of dimethyldiallylammonium chloride (DMDAAC), 0.2 parts of 1,4-butanediol, 0.4 parts of BASF ADR 4468, 1 part of 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, 0.2 part of nano-ZnO, 0.3 part of rutile TiO2, 0.3 part of bis(2,6-diisopropylbenzene)carbodiimide, 0.2 part of anti-hydrolysis agent HD900A, 0.5 part of antioxidant 2777, 0.25 part of zinc stearate, and 0.5 part of fumed nano-silica are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain granules specifically for the simulation layer;

[0260] D2: The special pellets for the simulation layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the simulation layer. It is then tightly compounded with the pre-heated PHA base fabric / filling / foaming layer through a three-roller setting machine. The simulation layer is closely attached to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The pre-heating temperature is controlled at 65-105℃, the casting temperature is 150-215℃, and the cast film thickness is 35-420μm.

[0261] D3: Emboss one side of the simulation layer by a method such as flat plate embossing or roller embossing, and then cool it to obtain a simulation pattern. The simulated leather is then dyed and rolled up to obtain PHA artificial leather.

[0262] The test results of various properties of the obtained artificial leather are shown in Table 6 below, and the schematic diagram of the prepared artificial leather is shown in Figure 1.

[0263] Table 6 Test data of PHBV / P34HB / PHBHHx+soy protein fiber+bamboo fiber+PBS composite artificial leather

[0264] Example 5: PHB / P34HB+black tea fiber+bamboo fiber+PGA composite artificial leather

[0265] A1: 30 parts by mass of PHB, 24 parts of P34HB (4HB content: 15 mol%), 4.5 parts of black tea fiber, 4 parts of bamboo fiber, 5 parts of PGA, 4 parts of mica powder, 0.3 part of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.3 part of dimethylolpropionic acid (DMPA), 0.4 part of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.4 part of nano-ZnO, 0.6 part of rutile TiO2, 0.75 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 part of zinc stearate, and 0.75 part of fumed nano-silica were mixed, melted, and granulated using a twin-screw extruder. The barrel temperature was set at 160-205°C, and an annular blower was used with an air supply temperature of 18-65°C to obtain fiber-specific pellets.

[0266] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 30-400g / m 2 between;

[0267] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a gram weight of 30-400 g / m 2 The PHA base fabric between, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0268] B1: 40 parts by mass of PHB, 32 parts of P34HB (with a 4HB content of 15 mol%), 6 parts of black tea fiber, 5.3 parts of bamboo fiber, 6.7 parts of PGA, 6.5 parts of mica powder, 0.45 parts of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.45 parts of dimethylolpropionic acid (DMPA), 0.6 parts of BASF ADR 4400, 1.5 parts of acetyl tributyl citrate, 0.4 parts of nano-ZnO, 0.6 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1.25 parts of antioxidant 2777, 0.5 parts of zinc stearate, and 0.75 parts of fumed nano-silica were mixed, melted, and granulated by a twin-screw extruder. The barrel temperature was set to 160-205° C., and an annular blower was used with an air supply temperature of 18-65° C. to obtain pellets specifically for the filling layer.

[0269] B2: The special pellets for the filling layer are vacuum-dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. It is then tightly compounded with the preheated PHA base fabric layer through a three-roller setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled at 65-105℃, the casting temperature is 160-205℃, and the cast film thickness is 70-700μm.

[0270] C1: 40 parts by mass of PHB, 32 parts of P34HB (4HB content is 15 mol%), 6 parts of black tea fiber, 5.3 parts of bamboo fiber, 6.7 parts of PGA, 0.6 parts of sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.6 parts of dihydroxymethylpropionic acid (DMPA), 0.8 parts of BASF ADR 4400, 4.5 parts of acetyl tributyl citrate, 0.3 parts of nano ZnO, 0.45 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 parts of zinc stearate, 0.75 parts of fumed nano silica, 1.5 parts of azodicarbonamide, 0.8 parts of leather foaming agent HF-800, and 1.2 parts of sodium bicarbonate were weighed, mixed, dried, injected into a twin-screw extruder with a heating device for plastication, and formed into a film by calendaring. The foaming layer is tightly compounded with the preheated PHA base fabric / filling layer through a three-roller shaping machine. The foaming layer is close to the filling layer. Since the two layers are mainly made of the same material, no adhesive is required. Then it is sent to the foaming furnace for foaming. The plasticizing temperature is 120-195℃, the preheating temperature is 65-105℃, the foaming temperature is 45-100℃, and the foaming time is 15-30min. The final thickness of the foaming layer after expansion and cooling is 280-3000μm.

[0271] D1: 20 parts of PHB, 16 parts of P34HB (4HB content is 15 mol%), 3 parts of black tea fiber, 2.7 parts of bamboo fiber, 3.3 parts of PGA and 0.75 parts of mica powder, 0.3 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.3 parts of dihydroxymethyl propionic acid (DMPA), 0.4 parts of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.2 parts of nano ZnO, 0.3 parts of rutile TiO2, 0.5 parts of anti-hydrolysis agent HYY-003, 0.5 parts of antioxidant 2777, 0.25 parts of zinc stearate, and 0.5 parts of fumed nano-silica were mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature was set to 160-205 ° C, annular blowing was used, and the air supply temperature was 18-65 ° C to obtain granules specifically for the simulation layer;

[0272] D2: The special pellets for the simulation layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the simulation layer. It is then tightly compounded with the pre-heated PHA base fabric / filling / foaming layer through a three-roller setting machine. The simulation layer is closely attached to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The pre-heating temperature is controlled at 65-105℃, the casting temperature is 150-215℃, and the cast film thickness is 35-420μm.

[0273] D3: Emboss one side of the simulation layer by a method such as flat plate embossing or roller embossing, and then cool it to obtain a simulation pattern. The simulated leather is then dyed and rolled up to obtain PHA artificial leather.

[0274] The test results of various properties of the obtained artificial leather are shown in Table 7 below, and the schematic diagram of the prepared artificial leather is shown in Figure 1.

[0275] Table 7 Test data of PHB / P34HB+black tea fiber+bamboo fiber+PGA composite artificial leather

[0276] Example 6: PHB / P34HB+Mulberry fiber+Bamboo fiber+PBAT composite artificial leather

[0277] A1: 34 parts of PHB, 16 parts of P34HB (4HB content: 20 mol%), 4.5 parts of mulberry fiber, 2.5 parts of bamboo fiber, 10.5 parts of PBAT, 4 parts of mica powder, 0.3 part of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.3 part of dimethylolpropionic acid (DMPA), 0.4 part of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.4 part of nano-ZnO, 0.6 part of rutile TiO2, 0.75 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 part of zinc stearate, and 0.75 part of fumed nano-silica were mixed, melted, and cooled to form pellets in a twin-screw extruder. The barrel temperature was set at 160-205°C, and an annular blower was used with an air supply temperature of 18-65°C to obtain fiber-specific pellets.

[0278] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 30-400g / m 2 between;

[0279] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a gram weight of 30-400 g / m 2The PHA base fabric between, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0280] B1: 45.3 parts of PHB, 21.3 parts of P34HB (4HB content is 20 mol%), 6 parts of mulberry fiber, 3.4 parts of bamboo fiber, 14 parts of PBAT and 6.5 parts of mica powder, 0.45 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.45 parts of dihydroxymethyl propionic acid (DMPA), 0.6 parts of BASF ADR 4400, 1.5 parts of acetyl tributyl citrate, 0.4 parts of nano ZnO, 0.6 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1.25 parts of DMPA, ... 1. Part of antioxidant 2777, 0.5 part of zinc stearate, and 0.75 part of fumed nano-silicon dioxide are mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature is set to 160-205°C, annular blowing is used, and the air supply temperature is 18-65°C to obtain granules specifically for the filling layer;

[0281] B2: The special pellets for the filling layer are vacuum-dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. It is then tightly compounded with the preheated PHA base fabric layer through a three-roller setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled at 65-105℃, the casting temperature is 160-205℃, and the cast film thickness is 70-700μm.

[0282] C1: 45.3 parts of PHB, 21.3 parts of P34HB (4HB content is 20 mol%), 6 parts of mulberry fiber, 3.4 parts of bamboo fiber, 14 parts of PBAT and 0.6 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.6 parts of dihydroxymethyl propionic acid (DMPA), 0.8 parts of BASF ADR 4400, 4.5 parts of acetyl tributyl citrate, 0.3 parts of nano ZnO, 0.45 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 parts of zinc stearate, 0.75 parts of fumed nano silica, 1.5 parts of azodicarbonamide, 0.8 parts of leather foaming agent HF-800, and 1.2 parts of sodium bicarbonate were weighed, mixed and dried, injected into a twin-screw extruder with a heating device for plastication, and formed into a film by calendaring. The foaming layer is tightly compounded with the preheated PHA base fabric / filling layer through a three-roller shaping machine. The foaming layer is close to the filling layer. Since the two layers are mainly made of the same material, no adhesive is required. Then it is sent to the foaming furnace for foaming. The plasticizing temperature is 120-195℃, the preheating temperature is 65-105℃, the foaming temperature is 45-100℃, and the foaming time is 15-30min. The final thickness of the foaming layer after expansion and cooling is 280-3000μm.

[0283] D1: 22.6 parts of PHB, 10.7 parts of P34HB (4HB content is 20 mol%), 3 parts of mulberry fiber, 1.7 parts of bamboo fiber, 7 parts of PBAT and 0.75 parts of mica powder, 0.3 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.3 parts of dihydroxymethyl propionic acid (DMPA), 0.4 parts of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.2 parts of nano ZnO, 0.3 parts of rutile TiO2, 0.5 parts of anti-hydrolysis agent HYY-003, 0.5 parts of antioxidant 2777, 0.25 parts of zinc stearate, and 0.5 parts of fumed nano-silica were weighed and mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature was set to 160-205 ° C, annular blowing was used, and the air supply temperature was 18-65 ° C to obtain granules specifically for the simulation layer;

[0284] D2: The special pellets for the simulation layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the simulation layer. It is then tightly compounded with the pre-heated PHA base fabric / filling / foaming layer through a three-roller setting machine. The simulation layer is closely attached to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The pre-heating temperature is controlled at 65-105℃, the casting temperature is 150-215℃, and the cast film thickness is 35-420μm.

[0285] D3: Emboss one side of the simulation layer by a method such as flat plate embossing or roller embossing, and then cool it to obtain a simulation pattern. The simulated leather is then dyed and rolled up to obtain PHA artificial leather.

[0286] The test results of various properties of the obtained artificial leather are shown in Table 8 below, and the schematic diagram of the prepared artificial leather is shown in Figure 1.

[0287] Table 8 Test data of PHB / P34HB+mulberry fiber+bamboo fiber+PBAT composite artificial leather

[0288] Example 7: PHB / P34HB+black tea fiber+soy protein fiber+PBAT composite artificial leather

[0289] A1: 33 parts by mass of PHB, 15 parts of P34HB (4HB content: 24 mol%), 6 parts of black tea fiber, 6 parts of soy protein fiber, 7.5 parts of PBAT, 4 parts of mica powder, 0.3 part of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.3 part of dimethylolpropionic acid (DMPA), 0.4 part of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.4 part of nano-ZnO, 0.6 part of rutile TiO2, 0.75 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 part of zinc stearate, and 0.75 part of fumed nano-silica were mixed, melted, and granulated using a twin-screw extruder. The barrel temperature was set at 160-205°C, and an annular blower was used with an air supply temperature of 18-65°C to obtain fiber-specific pellets.

[0290] A2: The fiber-specific pellets are vacuum-dried and injected into an extruder equipped with a heating device to melt. The PHA filaments or PHA non-woven fabrics are obtained by using different spinnerets, spinning processes, and subsequent drawing and winding or spunlace, needle punching and other fiber web reinforcement molding processes. The weight of the PHA non-woven fabric is 30-400g / m 2 between;

[0291] A3: Unwind the PHA filament obtained in A2 and knit or weave it to obtain a filament with a gram weight of 30-400 g / m 2 The PHA base fabric between, the PHA base fabric or the PHA non-woven fabric obtained by A2 are all PHA base fabric layers.

[0292] B1: 44 parts of PHB, 20 parts of P34HB (4HB content is 24 mol%), 8 parts of black tea fiber, 8 parts of soy protein fiber, 10 parts of PBAT, 6.5 parts of mica powder, 0.45 parts of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 0.45 parts of dihydroxymethylpropionic acid (DMPA), 0.6 parts of BASF ADR 4400, 1.5 parts of acetyl tributyl citrate, 0.4 parts of nano-ZnO, 0.6 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1.25 parts of antioxidant 2777, 0.5 parts of zinc stearate, and 0.75 parts of fumed nano-silica were weighed and mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature was set to 160-205°C, annular blowing was used, and the air supply temperature was 18-65°C to obtain granules specifically for the filling layer;

[0293] B2: The special pellets for the filling layer are vacuum-dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the filling layer. It is then tightly compounded with the preheated PHA base fabric layer through a three-roller setting machine. Since the two layers are mainly made of the same material, no adhesive is required. The preheating temperature is controlled at 65-105℃, the casting temperature is 160-205℃, and the cast film thickness is 70-700μm.

[0294] C1: 44 parts of PHB, 20 parts of P34HB (4HB content is 24 mol%), 8 parts of black tea fiber, 8 parts of soy protein fiber, 10 parts of PBAT and 0.6 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.6 parts of dihydroxymethyl propionic acid (DMPA), 0.8 parts of BASF ADR 4400, 4.5 parts of acetyl tributyl citrate, 0.3 parts of nano ZnO, 0.45 parts of rutile TiO2, 1 part of anti-hydrolysis agent HYY-003, 1 part of antioxidant 2777, 0.5 parts of zinc stearate, 0.75 parts of fumed nano silica, 1.5 parts of azodicarbonamide, 0.8 parts of leather foaming agent HF-800, and 1.2 parts of sodium bicarbonate were weighed, mixed and dried, injected into a twin-screw extruder with a heating device for plastication, and formed into a film by calendaring. The foaming layer is tightly compounded with the preheated PHA base fabric / filling layer through a three-roller shaping machine. The foaming layer is close to the filling layer. Since the two layers are mainly made of the same material, no adhesive is required. Then it is sent to the foaming furnace for foaming. The plasticizing temperature is 120-195℃, the preheating temperature is 65-105℃, the foaming temperature is 45-100℃, and the foaming time is 15-30min. The final thickness of the foaming layer after expansion and cooling is 280-3000μm.

[0295] D1: 22 parts of PHB, 10 parts of P34HB (4HB content is 24 mol%), 4 parts of black tea fiber, 4 parts of soy protein fiber, 5 parts of PBAT and 0.75 parts of mica powder, 0.3 parts of sodium N, N-bis (2-hydroxyethyl) -2-aminoethanesulfonate, 0.3 parts of dihydroxymethyl propionic acid (DMPA), 0.4 parts of BASF ADR 4400, 1 part of acetyl tributyl citrate, 0.2 parts of nano ZnO, 0.3 parts of rutile TiO2, 0.5 parts of anti-hydrolysis agent HYY-003, 0.5 parts of antioxidant 2777, 0.25 parts of zinc stearate, and 0.5 parts of fumed nano-silica were mixed, melted and cooled into granules through a twin-screw extruder, wherein the barrel temperature was set to 160-205 ° C, annular blowing was used, and the air supply temperature was 18-65 ° C to obtain granules specifically for the simulation layer;

[0296] D2: The special pellets for the simulation layer are vacuum dried and injected into a twin-screw extruder with a heating device to melt. The film is formed by casting to form the simulation layer. It is then tightly compounded with the pre-heated PHA base fabric / filling / foaming layer through a three-roller setting machine. The simulation layer is closely attached to the foaming layer. Since the two layers are mainly made of the same material, no adhesive is required. The pre-heating temperature is controlled at 65-105℃, the casting temperature is 150-215℃, and the cast film thickness is 35-420μm.

[0297] D3: Emboss one side of the simulation layer by a method such as flat plate embossing or roller embossing, and then cool it to obtain a simulation pattern. The simulated leather is then dyed and rolled up to obtain PHA artificial leather.

[0298] The test results of various properties of the obtained artificial leather are shown in Table 9 below, and the schematic diagram of the prepared artificial leather is shown in Figure 1.

[0299] Table 9 Test data of PHB / P34HB+black tea fiber+soy protein fiber+PBAT composite artificial leather

[0300] Control Example 1: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather with too high P34HB addition

[0301] Compared with Example 1, the amount of P34HB added was too high, and the amount of PHB added was reduced accordingly.

[0302] Among them, A1 contains 10 parts of PHB and 40 parts of P34HB (4HB content is 16 mol%); B1 contains 13.3 parts of PHB and 53.4 parts of P34HB (4HB content is 16 mol%); C1 contains 13.3 parts of PHB and 53.4 parts of P34HB (4HB content is 16 mol%); D1 contains 6.7 parts of PHB and 26.6 parts of P34HB (4HB content is 16 mol%); the mass fractions of other substances and the parameters during the processing are the same as those in Example 1.

[0303] Because the amount of P34HB added in Control Example 1 is too high, the expansion coefficient (15.6), sound insulation (24.5dB), tensile load (warp: 403; weft: 311), tear load (warp: 16.2; weft: 15.8), peel load (warp: 17.4; weft: 17.2) and waterproofness (level 4) of the prepared artificial leather are worse than those in Example 1.

[0304] Control Example 2: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather with too low P34HB addition

[0305] Compared with Example 1, the amount of P34HB added was too low, and the amount of PHB added was increased accordingly.

[0306] Among them, A1 contains 40 parts of PHB and 10 parts of P34HB (4HB content is 16 mol%); B1 contains 53.4 parts of PHB and 13.3 parts of P34HB (4HB content is 16 mol%); C1 contains 53.4 parts of PHB and 13.3 parts of P34HB (4HB content is 16 mol%); D1 contains 26.7 parts of PHB and 6.6 parts of P34HB (4HB content is 16 mol%); the mass fractions of other substances and the parameters during the processing are the same as those in Example 1.

[0307] Since the amount of P34HB added in Control Example 2 is too low, the softness (grade 4.1), expansion coefficient (17.6), sound insulation (25.3), elongation at break (warp: 5.7; weft: 5.6), surface color fastness (grade 4), dyeing uniformity (grade 4) and folding fastness (cracks on the surface after 30,000 times) of the prepared artificial leather are worse than those in Example 1.

[0308] Comparative Example 3: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather without preheating process

[0309] Compared with Example 1, no preheating process was performed and the composite was directly prepared. The mass fractions of other substances and the parameters during the processing were the same as those in Example 1.

[0310] Since the method described in Comparative Example 3 does not have a preheating step, the peeling load (warp: 13.8; weft: 12.4) and water resistance (grade 4) of the artificial leather prepared therefrom are inferior to those in Example 1.

[0311] Comparative Example 4: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather without filling layer

[0312] Compared with Example 1, no filling layer is included. The mass fractions of other substances and the parameters during the processing are the same as those in Example 1.

[0313] Since the artificial leather prepared in Control Example 4 does not have a filling layer, the sound insulation (24.8), tensile load (warp: 246; weft: 235), tear load (warp: 15.3; weft: 14.8), peel load (warp: 13.9; weft: 13.2), light resistance (level 4), and water resistance (level 2) of the artificial leather prepared therefrom are all worse than those in Example 1.

[0314] Comparative Example 5: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather with too low 4HB molar content

[0315] Compared with Example 1, the molar content of 4HB in P34HB was too low, namely 1 mol%. The mass fractions of other substances and the processing parameters were the same as those in Example 1.

[0316] Since the molar content of 4HB in P34HB in Control Example 5 is too low, the softness (3.9), expansion coefficient (15.4), sound insulation (26.7), elongation at break (warp: 4.5; weft: 5.2), surface color fastness (grade 4), and folding fastness (cracks on the surface after 20,000 times) of the artificial leather prepared therefrom are inferior to those in Example 1.

[0317] Comparative Example 6: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather with too high 4HB molar content

[0318] Compared with Example 1, the molar content of 4HB in P34HB was too high, namely 35 mol%. The mass fractions of other substances and the processing parameters were the same as those in Example 1.

[0319] Since the molar content of 4HB in P34HB in Control Example 6 is too high, the expansion coefficient (5.1), sound insulation (17.7), tensile load (warp: 389; weft: 292), tear load (warp: 15.4; weft: 15.3), peel load (warp: 16.1; weft: 15.7), and waterproofness (4 levels) of the artificial leather prepared therefrom are inferior to those in Example 1.

[0320] Comparative Example 7: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather without filler

[0321] Compared with Example 1, no filler was added to each layer. The mass fractions of other substances and the parameters during the processing were the same as those in Example 1.

[0322] Since no filler was added in Control Example 7, the sound insulation of the artificial leather prepared therefrom (18.3) was worse than that of Example 1.

[0323] Comparative Example 8: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather without adding UV absorber

[0324] Compared with Example 1, no ultraviolet absorber was added to each layer. The mass fractions of other substances and the parameters during the processing were the same as those in Example 1.

[0325] Since no ultraviolet absorber was added in Control Example 8, the sound insulation (22.7) and light resistance (grade 2) of the artificial leather prepared therefrom were inferior to those in Example 1.

[0326] Comparative Example 9: PHB / P34HB+black tea fiber+mulberry fiber+PBS composite artificial leather without adding filler and UV absorber

[0327] Compared with Example 1, no filler or ultraviolet absorber was added to each layer. The mass fractions of other substances and the parameters during the processing were the same as those in Example 1.

[0328] Since no filler and ultraviolet absorber were added in Control Example 9, the sound insulation (14.3) and light resistance (grade 2) of the artificial leather prepared therefrom were inferior to those in Example 1.

[0329] Control Example 10: PLA / PBAT+black tea fiber+mulberry fiber+PBS composite artificial leather without PHA

[0330] Compared with Example 1, PHA is not used in each layer, PHB in Example 1 is replaced by PLA, and P34HB is replaced by PBAT. The mass fractions of other substances and the parameters during the processing are the same as those in Example 1.

[0331] Since no PHA was added to the control example 10, the expansion coefficient (6.8), sound insulation (18.2), peel load (warp: 20.5; weft: 19.7), surface color fastness (level 3), dyeing uniformity (level 2), light fastness (level 4), folding fastness (cracks on the surface after 30,000 times), and water resistance (level 3) of the artificial leather prepared therefrom were worse than those in Example 1.

[0332] Control Example 11: P34HB + black tea fiber + mulberry fiber + PBS composite artificial leather with only P34HB and 4HB in a moderate ratio

[0333] Compared with Example 1, only P34HB was added to each layer, and PHB was not added.

[0334] Among them, the content of P34HB (4HB content is 16 mol%) in A1 is 50 parts; the content of P34HB (4HB content is 16 mol%) in B1 is 66.7 parts; the content of P34HB (4HB content is 16 mol%) in C1 is 66.7 parts; and the content of P34HB (4HB content is 16 mol%) in D1 is 33.3 parts; PHB is not added in each step, and the mass fractions of other substances and the parameters during the processing are the same as those in Example 1.

[0335] Since only P34HB was added to the control example 11, the expansion coefficient (12.9), sound insulation (20.3), tensile load (warp: 350; weft: 262), tear load (warp: 14.3; weft: 13.0), peel load (warp: 15.4; weft: 14.1) and waterproofness (level 3) of the artificial leather prepared therefrom are worse than those in Example 1.

[0336] Control Example 12: PHB+black tea fiber+mulberry fiber+PBS composite artificial leather without P34HB

[0337] Compared with Example 1, no P34HB was added to each layer, and only PHB was added.

[0338] Among them, the amount of PHB in A1 is 50 parts; the amount of PHB in B1 is 66.7 parts; the amount of PHB in C1 is 66.7 parts; the amount of PHB in D1 is 33.3 parts; P34HB is not added in each step, and the mass parts of other substances and the parameters during the processing are the same as those in Example 1.

[0339] Since P34HB is not added to the control example 12, the softness (grade 3.2), expansion coefficient (9.8), sound insulation (11.4), elongation at break (warp: 3.0; weft: 2.7), peeling load (warp: 12.9; weft: 12.6), surface color fastness (grade 3), dyeing uniformity (grade 4) and folding fastness (cracks on the surface after 10,000 times) of the artificial leather prepared therefrom are worse than those in Example 1.

[0340] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. An artificial leather, characterized in that: The artificial leather comprises a base fabric layer, a filling layer, a foaming layer and / or a simulation layer. The raw materials of the base fabric layer, the filling layer, the foaming layer and / or the simulation layer comprise a substrate, and the substrate comprises a PHA substrate.

2. An artificial leather, characterized in that: The raw materials of the artificial leather include a substrate, and the substrate includes a PHA substrate; the artificial leather includes a filling layer; Preferably, the artificial leather further comprises one, two or three of a foaming layer, a base fabric layer or a simulation layer.

3. The artificial leather according to claim 2, characterized in that: At least one of the filling layer, the foaming layer, the base fabric layer or the simulation layer comprises a PHA substrate.

4. The artificial leather according to any one of claims 1 to 3, characterized in that: The artificial leather is a laminated structure, wherein the first layer is a base fabric layer, the second layer is a filling layer, the third layer is a foaming layer, and the fourth layer is a simulation layer.

5. The artificial leather according to any one of claims 1 to 4, characterized in that: The PHA substrate comprises a homopolymer or copolymer of monomers constituting PHA, Preferably, the monomers constituting PHA include one or more of 2-hydroxypropionic acid, 3-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 5-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid, and 3-hydroxydodecanoic acid; Preferably, the PHA comprises one or more of P(HB-LA), P3HP, PHB, P4HB, PHV, PHO, PHN, PHD, PHBV, P34HB, PHBHHp, PHBHHx, P3HB4HB3HV or P3HB4HB5HV; Further preferably, the molar content of 4HB in the P34HB is 3%-30%, preferably 8%-24%.

6. The artificial leather according to any one of claims 1 to 5, characterized in that: The PHA substrate includes a mixed raw material of P34HB and non-P34HB PHA.

7. The artificial leather according to claim 6, characterized in that In the PHA substrate, the added mass of P34HB is 21%-79%, preferably 25%-70%.

8. The artificial leather according to any one of claims 1 to 7, characterized in that: The substrate also includes a non-PHA substrate; Preferably, the non-PHA substrate includes one or more of PLA, PBAT, PPC, PBS, PGA, black tea fiber, soybean protein fiber, mulberry fiber, sugarcane fiber or bamboo fiber.

9. The artificial leather according to claim 8, characterized in that The mass ratio of PHA substrate to non-PHA substrate is (1-5):1; Preferably, the mass ratio of the PHA substrate to the non-PHA substrate is (2-4):

1.

10. The artificial leather according to any one of claims 1 to 9, characterized in that: The artificial leather further comprises auxiliary materials, wherein the auxiliary materials include one or both of fillers and ultraviolet absorbers; Preferably, the filler is a micron-sized filler; Preferably, the ultraviolet absorber is a nano-scale inorganic powder.

11. The artificial leather according to claim 10, characterized in that The filler includes one or more of hollow glass microspheres, mica powder or talc powder.

12. The artificial leather according to claim 10 or 11, characterized in that: The ultraviolet absorber includes nano oxides, preferably one or more of nano ZnO, rutile TiO2 or nano CeO2.

13. The artificial leather according to any one of claims 10 to 12, characterized in that: The auxiliary materials also include one or more of a chain extender, an environmentally friendly plasticizer, an anti-hydrolysis agent, an antioxidant, a heat stabilizer or a foaming agent.

14. The artificial leather according to claim 13, characterized in that The chain extender includes one or more of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, dimethylolpropionic acid, dimethyldiallylammonium chloride, 1,4-butanediol, BASF ADR 4400 or BASF ADR 4468; Preferably, the environmentally friendly plasticizer includes one or both of acetyl tributyl citrate or 2,2,4-trimethyl-1,3-pentanediol diisobutyrate; Preferably, the anti-hydrolysis agent includes one or more of anti-hydrolysis agent HYY-003, bis(2,6-diisopropylbenzene)carbodiimide or anti-hydrolysis agent HD900A; Preferably, the antioxidant includes one or more of antioxidant 2777, tris(2,4-di-tert-butylphenyl)phosphite or antioxidant S-9228; Preferably, the heat stabilizer includes one or more of stearate, nanocellulose or fumed nanosilica; Preferably, the foaming agent includes one or more of azodicarbonamide, foaming agent SP1000C, leather foaming agent HF-800, sodium bicarbonate or ammonium bicarbonate.

15. The artificial leather according to any one of claims 1 to 14, characterized in that: The artificial leather comprises a base fabric layer, a filling layer, a foaming layer and / or a simulation layer; the base fabric layer, the filling layer, the foaming layer and / or the simulation layer comprise a PHA substrate, a non-PHA substrate and auxiliary materials; Preferably, in the base fabric layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (3-7): (1-3): 1; Preferably, in the filling layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (2-6): (1-3): 1; Preferably, in the foaming layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (2-6): (1-3): 1; Preferably, in the simulation layer, the mass ratio of the PHA substrate, the non-PHA substrate and the auxiliary material is (4-10):(1-3):

1.

16. A method for preparing the artificial leather according to any one of 1 to 15, characterized in that: The preparation method includes preparing a base fabric layer, a filling layer, a foaming layer and / or a simulation layer, wherein the raw material of at least one of the base fabric layer, the filling layer, the foaming layer or the simulation layer includes a substrate, and the substrate includes a PHA substrate.

17. The preparation method according to claim 16, characterized in that: The method for preparing the base fabric layer comprises: A1: Mix the raw materials, melt them, cool them and granulate them to obtain fiber-specific granules; A2: Melting and extruding the fiber-specific pellets to obtain filaments or non-woven fabrics through a molding process to obtain a base fabric layer. Preferably, the step A2 further comprises unwinding the filaments and obtaining the base fabric through a knitting or weaving process; Preferably, the preparation of the filling layer comprises: B1: Mix the raw materials, melt them, cool them and granulate them to obtain granules for the filling layer; B2: Melting the special granular material for the filling layer and casting it into a film to obtain the filling layer; Preferably, the preparation of the foaming layer comprises: C1: Mix the raw materials, plasticize, calender into a film, and then heat and foam to obtain a foaming layer; Preferably, the preparation of the simulation layer comprises: D1: Mix the raw materials, melt them, cool them and granulate them to obtain granules for the simulation layer; D2: The special pellets for the simulation layer are melted and cast into a film to obtain the simulation layer.

18. The preparation method according to claim 16 or 17, characterized in that: The preparation method further comprises laminating and compounding the base fabric layer, the filling layer, the foaming layer and / or the simulation layer to prepare the artificial leather; Preferably, the compounding comprises heating, Preferably, the heating temperature is 50-150°C.

19. An application of the artificial leather according to any one of claims 1 to 15 and / or the artificial leather prepared by the preparation method according to any one of claims 16 to 18, characterized in that: The applications include use in manufacturing leather products, simulated skin or antibacterial wound dressings; Preferably, the leather products include one, two or more of automobile interior, leather furniture, leather shoes and / or leather clothing.

Citation Information

Patent Citations

  • Vacuum grain sucking leather and preparation method thereof

    CN107245888A

  • Anti-yellowing PVC synthetic leather for PU sponge compounding and composite material

    CN113529430A

  • Artificial leather and preparation method thereof

    CN116641241A

  • PHA compositions and methods for their use in the production of PHA films

    US20020061944A1

  • Polyhydroxyalkanoate copolymer and polylactic acid polymer compositions for laminates and films

    US20020143136A1